Charging roll for electro-photographic apparatus

The charging roll design optimizes charging performance by using a specific rubber and resin composition to minimize discharge and harmful substance generation, ensuring effective and environmentally friendly charging in electrophotographic equipment.

JP2024141437AActive Publication Date: 2024-10-10SUMITOMO RIKO CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023053091
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Charging rolls in electrophotographic equipment face issues with excessive discharge leading to environmental and image deterioration due to the generation of harmful substances like ozone and NOx, while insufficient discharge results in image deterioration from inadequate charging.

Method used

A charging roll design incorporating a shaft with an elastic layer containing non-polar rubber, polar rubber, and carbon black, and a surface layer made of fluororesin and (meth)acrylic resin, with specific dielectric constants and resistance values, to optimize charging performance and reduce discharge.

Benefits of technology

The design reduces harmful substance generation and ensures effective charging even with reduced discharge, maintaining image quality and environmental safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141437000001_ABST
    Figure 2024141437000001_ABST
Patent Text Reader

Abstract

To provide a charging roll for electro-photographic apparatuses, the roll having an excellent charging property even if the discharge amount is decreased.SOLUTION: A charging roll 10 for electro-photographic apparatuses includes a shaft body 12, an elastic body layer 14 formed on the outer peripheral surface of the shaft body 12, and a surface layer 16 formed on the outer peripheral surface of the elastic body layer 14. The elastic body layer 14 contains non-polar rubber, polar rubber, and carbon black, a dielectric constant thereof is 7 to 29, and a resistance value thereof is 6.0×104 Ω to 5.0×106 Ω, and the surface layer 16 contains fluororesin and (meth) acrylic resin, a dielectric constant thereof is 10 to 22, and a resistance value thereof is 1.2×104 Ω to 8.8×105 Ω.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a charging roll for electrophotographic equipment, which is suitably used in electrophotographic equipment such as copying machines, printers, and facsimiles that employ an electrophotographic system. [Background technology]

[0002] A charging roll for an electrophotographic device is known to have a configuration including a shaft body made of a core metal or the like, an elastic layer formed on the outer peripheral surface of the shaft body, and a surface layer formed on the outer peripheral surface of the elastic layer. The elastic layer is made of a rubber material such as isoprene rubber, and the surface layer is made of a resin material such as acrylic resin. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2003-140442 A Summary of the Invention [Problem to be solved by the invention]

[0004] The charging rolls of electrophotographic devices often use a charging system that charges the photoconductor by discharging from the charging roll to the photoconductor, but if the amount of discharge is increased in order to fully charge the photoconductor, harmful substances such as ozone and NOx are generated in large amounts, which may cause environmental degradation and image deterioration.On the other hand, if the amount of discharge is small, the amount of charge is insufficient and there is a risk of image deterioration.

[0005] An object of the present invention is to provide a charging roll for electrophotographic equipment which has excellent charging properties even when the amount of discharge is small. [Means for solving the problem]

[0006] The electrostatic charging roll for electrophotographic equipment according to the present invention comprises a shaft body, an elastic layer formed on the outer peripheral surface of the shaft body, and a surface layer formed on the outer peripheral surface of the elastic layer, the elastic layer containing a non-polar rubber, a polar rubber, and carbon black, and having a relative dielectric constant of 7 to 29 and a resistance value of 6.0×10 4 Ω or more 5.0×10 6 Ω or less, the surface layer contains a fluororesin and a (meth)acrylic resin, has a relative dielectric constant of 10 to 22, and has a resistance of 1.2×10 4 Ω or more 8.8×10 5 It is less than Ω.

[0007] The area ratio of the non-polar rubber to the polar rubber on the surface of the elastic layer may be non-polar rubber:polar rubber=9:1 to 7:3. The non-polar rubber may be isoprene rubber or natural rubber, and the polar rubber may be nitrile rubber or hydrin rubber. The carbon black may have an average particle size of 36 nm to 80 nm, and a product of DBP absorption and specific surface area of ​​1728 to 5445. The content of the carbon black may be 15 parts by mass to 50 parts by mass with respect to 100 parts by mass of the total of the non-polar rubber and the polar rubber. The elastic layer may be composed of a composition that does not contain an ion conductive agent. The content ratio of the fluororesin to the (meth)acrylic resin may be fluororesin:(meth)acrylic resin=9.5:0.5 to 7:3 by mass. The fluororesin may have a relative dielectric constant of 8 to 10 and a volume resistivity of 1.0×10 13 Ω cm or more 1.0×10 14The fluororesin may be polyvinylidene fluoride. The difference in volume resistivity between the fluororesin and the (meth)acrylic resin may be 0.2 log Ω or less. The indentation Young's modulus of the fluororesin may be 0.65 GPa or more and 0.75 GPa or less, and the elastic recovery rate may be 40% or more and 50% or less, and the indentation Young's modulus of the (meth)acrylic resin may be 0.65 GPa or more and 0.75 GPa or less, and the elastic recovery rate may be 45% or more and 50% or less. The difference in indentation Young's modulus between the fluororesin and the (meth)acrylic resin may be 0.1 GPa or less, and the difference in elastic recovery rate may be 5% or less. The tensile strength of the fluororesin may be 28 MPa or more and 40 MPa or less. The difference in relative dielectric constant between the fluororesin and the (meth)acrylic resin may be 2 or less. The surface layer may further contain roughness-forming particles. The roughness-forming particles may be porous particles.

[0008] (1) The electrostatic charging roll for an electrophotographic device according to the present invention comprises a shaft, an elastic layer formed on the outer peripheral surface of the shaft, and a surface layer formed on the outer peripheral surface of the elastic layer, the elastic layer containing a non-polar rubber, a polar rubber, and carbon black, and having a relative dielectric constant of 7 to 29 and a resistance value of 6.0×10 4 Ω or more 5.0×10 6 Ω or less, the surface layer contains a fluororesin and a (meth)acrylic resin, has a relative dielectric constant of 10 to 22, and has a resistance of 1.2×10 4 Ω or more 8.8×10 5 It is less than Ω.

[0009] (2) In the above item (1), the area ratio of the non-polar rubber to the polar rubber on the surface of the elastic layer may be non-polar rubber:polar rubber=9:1 to 7:3.

[0010] (3) In the above (1) or (2), the non-polar rubber may be isoprene rubber or natural rubber, and the polar rubber may be nitrile rubber or hydrin rubber.

[0011] (4) In any one of the above (1) to (3), the carbon black may have an average particle size of 36 nm or more and 80 nm or less, and a product of DBP absorption amount and specific surface area of ​​1728 or more and 5445 or less.

[0012] (5) In any one of the above (1) to (4), the content of the carbon black may be 15 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the total of the nonpolar rubber and the polar rubber.

[0013] (6) In any one of the above (1) to (5), the elastic layer may be made of a composition that does not contain an ion conductive agent.

[0014] (7) In any one of the above (1) to (6), the content ratio of the fluororesin to the (meth)acrylic resin may be, in terms of mass ratio, fluororesin:(meth)acrylic resin=9.5:0.5 to 7:3.

[0015] (8) In any one of the above (1) to (7), the fluororesin has a relative dielectric constant of 8 to 10 and a volume resistivity of 1.0×10 13 Ω cm or more 1.0×10 14 It is preferable that the resistivity is Ω·cm or less.

[0016] (9) In any one of the above (1) to (8), the fluororesin may be polyvinylidene fluoride.

[0017] (10) In any one of the above (1) to (9), the difference in volume resistivity between the fluororesin and the (meth)acrylic resin may be 0.2 log Ω or less.

[0018] (11) In any one of the above (1) to (10), the fluororesin may have an indentation Young's modulus of 0.65 GPa or more and 0.75 GPa or less and an elastic recovery rate of 40% or more and 50% or less, and the (meth)acrylic resin may have an indentation Young's modulus of 0.65 GPa or more and 0.75 GPa or less and an elastic recovery rate of 45% or more and 50% or less.

[0019] (12) In any one of the above (1) to (11), the difference in indentation Young's modulus between the fluororesin and the (meth)acrylic resin may be 0.1 GPa or less, and the difference in elastic recovery rate between the fluororesin and the (meth)acrylic resin may be 5% or less.

[0020] (13) In any one of the above (1) to (12), the tensile strength of the fluororesin may be 28 MPa or more and 40 MPa or less.

[0021] (14) In any one of the above (1) to (13), the difference in relative dielectric constant between the fluororesin and the (meth)acrylic resin may be 2 or less.

[0022] (15) In any one of the above (1) to (14), the surface layer may further contain particles for providing roughness.

[0023] (16) In the above item (15), the roughness-imparting particles may be porous particles. Effect of the Invention

[0024] According to the charging roll for electrophotographic equipment of the present invention, the elastic layer contains non-polar rubber, polar rubber, and carbon black, and has a relative dielectric constant of 7 to 29 and a resistance value of 6.0×10 4 Ω or more 5.0×10 6 Ω or less, the surface layer contains fluororesin and (meth)acrylic resin, the relative dielectric constant is 10 to 22, and the resistance is 1.2×10 4 Ω or more 8.8×10 5 Since the resistance is Ω or less, the amount of discharge from the charging roll to the photoconductor is reduced, suppressing the generation of harmful substances such as ozone and NOx, thereby suppressing the deterioration of the environment and the deterioration of images. In addition, the above-mentioned configuration makes it easier for charges to move between the charging roll and the grounded portion of the photoconductor, and the photoconductor can be charged to the desired charge amount by injecting charges from the charging roll into the photoconductor. This results in excellent charging properties even with a small amount of discharge.

[0025] Here, when the area ratio of the non-polar rubber to the polar rubber on the surface of the elastic layer is non-polar rubber:polar rubber=9:1 to 7:3, the relative dielectric constant of the elastic layer is easily within a specific range.

[0026] When the non-polar rubber is isoprene rubber or natural rubber and the polar rubber is nitrile rubber or hydrin rubber, the relative dielectric constant of the elastic layer is easily kept within a specific range.

[0027] When the carbon black has an average particle size of 36 nm or more and 80 nm or less and a product of DBP absorption amount and specific surface area of ​​1728 or more and 5445 or less, the carbon black can be made to have a desired dielectric constant, making it easier to bring the relative dielectric constant of the elastic layer into a specific range.

[0028] When the content of the carbon black is 15 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the total of the non-polar rubber and the polar rubber, the resistance value and the relative dielectric constant of the elastic layer are easily kept within the specific range.

[0029] When the elastic layer is made of a composition that does not contain an ionic conductive agent, the relative dielectric constant of the elastic layer does not increase too much, and it is easy to keep the relative dielectric constant of the elastic layer within a specific range.

[0030] When the content ratio of the fluororesin to the (meth)acrylic resin is, in mass ratio, fluororesin:(meth)acrylic resin=9.5:0.5 to 7:3, the relative dielectric constant of the surface layer is easily kept within a specific range.

[0031] The fluororesin has a relative dielectric constant of 8 to 10 and a volume resistivity of 1.0×10 13 Ω cm or more 1.0×10 14 At Ω·cm or less, fluororesin has a relatively high dielectric constant and low resistance, so it is easy to make the surface layer high dielectric constant and low resistance. At this time, the electrostatic effect of the fluororesin is also easy to maintain.

[0032] When the fluororesin is polyvinylidene fluoride, it has a relatively high dielectric constant and low resistance, so that the surface layer can be easily made to have a high dielectric constant and low resistance, and the electrostatic effect of the fluororesin can be easily maintained.

[0033] When the difference in volume resistivity between the fluororesin and the (meth)acrylic resin is 0.2 log Ω or less, the unevenness of charge injection from the charging roll to the photoconductor is reduced.

[0034] Furthermore, when the fluororesin has an indentation Young's modulus of 0.65 GPa or more and 0.75 GPa or less and an elastic recovery rate of 40% or more and 50% or less, and the (meth)acrylic resin has an indentation Young's modulus of 0.65 GPa or more and 0.75 GPa or less and an elastic recovery rate of 45% or more and 50% or less, the deformation of the charging roll in response to the pressure received from the photosensitive member during rotation becomes uniform, and local stress concentration is less likely to occur.

[0035] When the difference in indentation Young's modulus between the fluororesin and the (meth)acrylic resin is 0.1 GPa or less and the difference in elastic recovery is 5% or less, cracking of the surface layer due to physical stress from the photoreceptor is easily suppressed, thereby improving durability.

[0036] When the tensile strength of the fluororesin is 28 MPa or more and 40 MPa or less, the strength of the surface layer is improved, and the durability is improved.

[0037] When the difference in relative dielectric constant between the fluororesin and the (meth)acrylic resin is 2 or less, unevenness in discharge from the charging roll to the photoconductor is reduced.

[0038] When the surface layer further contains roughness-forming particles, a suitable discharge space can be formed between the photoconductor and the charging roll. In this case, when the roughness-forming particles are porous particles, the binder resin of the surface layer and the roughness-forming particles are more integrated, making the surface layer less likely to crack. In addition, the resistance can be integrated to make the injected charge uniform. [Brief description of the drawings]

[0039] [Figure 1] 1A is a schematic external view of a charging roll for an electrophotographic device according to one embodiment of the present invention, and FIG. 1B is a cross-sectional view taken along line AA thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0040] The charging roll for electrophotographic equipment according to the present invention (hereinafter, simply referred to as the charging roll) will be described in detail. Fig. 1 is a schematic external view (a) of the charging roll for electrophotographic equipment according to one embodiment of the present invention, and its AA line cross-sectional view (b).

[0041] The electrostatic charge roll 10 includes a shaft 12, an elastic layer 14 formed on the outer peripheral surface of the shaft 12, and a surface layer 16 formed on the outer peripheral surface of the elastic layer 14. The elastic layer 14 is a layer (base layer) that serves as the base of the electrostatic charge roll 10. The surface layer 16 is a layer that appears on the surface of the electrostatic charge roll 10.

[0042] The shaft body 12 is not particularly limited as long as it is conductive. Specific examples include a core bar made of a solid or hollow body made of a metal such as iron, stainless steel, or aluminum. An adhesive, primer, or the like may be applied to the surface of the shaft body 12 as needed. In other words, the elastic layer 14 may be bonded to the shaft body 12 via an adhesive layer (primer layer). The adhesive, primer, or the like may be made conductive as needed.

[0043] The elastic layer 14 contains non-polar rubber, polar rubber, and carbon black, and has a dielectric constant of 7 to 29, and a resistance value of 6.0×10 4 Ω or more 5.0×10 6 It is less than Ω.

[0044] Examples of non-polar rubbers for the elastic layer 14 include isoprene rubber (IR), hydrogenated isoprene rubber, natural rubber (NR), butadiene rubber (BR), styrene-butadiene rubber (SBR), butyl rubber (IIR), ethylene-propylene rubber (EPM), ethylene-propylene-diene terpolymer rubber (EPDM), silicone rubber (Q), etc. These may be used alone as the non-polar rubber for the elastic layer 14, or two or more of them may be used in combination. Among these, isoprene rubber and natural rubber are preferred from the viewpoints of high resistance and excellent effect as a dielectric phase.

[0045] Examples of the polar rubber of the elastic layer 14 include nitrile rubber (NBR), hydrin rubber, urethane rubber (U), acrylic rubber (a copolymer of acrylic acid ester and 2-chloroethyl vinyl ether, ACM), and chloroprene rubber (CR). Examples of the hydrin rubber include epichlorohydrin homopolymer (CO), epichlorohydrin-ethylene oxide binary copolymer (ECO), epichlorohydrin-allyl glycidyl ether binary copolymer (GCO), and epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer (GECO). These may be used alone as the polar rubber of the elastic layer 14, or two or more of them may be used in combination. Among these, nitrile rubber (NBR) and hydrin rubber are preferred from the viewpoints of lower resistance and higher relative dielectric constant.

[0046] As a combination of non-polar rubber and polar rubber, from the viewpoint of making it easier to keep the relative dielectric constant of the elastic layer 14 within a specific range, it is preferable that the non-polar rubber is isoprene rubber or natural rubber, and the polar rubber is nitrile rubber or hydrin rubber.

[0047] The content ratio of the non-polar rubber to the polar rubber depends on the mixing method, but from the viewpoint of easily setting the area ratio of the non-polar rubber to the polar rubber in a specific range on the surface of the elastic layer 14, the content ratio of the non-polar rubber to the polar rubber is preferably non-polar rubber:polar rubber=8:2 to 6:4 by mass, and more preferably non-polar rubber:polar rubber=8:2 to 7:3.

[0048] The area ratio of the non-polar rubber to the polar rubber is preferably 9:1 to 7:3 on the surface of the elastic layer 14. This makes it easier to keep the relative dielectric constant of the elastic layer 14 within a specific range. From this viewpoint, the area ratio is more preferably 9:1 to 8:2.

[0049] The carbon black in the elastic layer 14 contributes to adjusting the resistance value and dielectric constant of the elastic layer 14. From the viewpoint of easily keeping the resistance value and dielectric constant of the elastic layer 14 within a specific range, it is preferable that the carbon black in the elastic layer 14 has an average particle size of 36 nm to 80 nm and a product of DBP absorption (oil absorption) and specific surface area of ​​1728 to 5445. The product of DBP absorption and specific surface area is related to the amount of functional groups such as carbonyl groups and hydroxyl groups in the carbon black, and is related to the resistance value and dielectric constant of the carbon black. The average particle size of the carbon black is expressed as an arithmetic mean diameter obtained by observing the carbon black with an electron microscope. The DBP absorption amount of the carbon black is calculated from the amount of DBP (dibutyl phthalate) absorbed by 100 g of carbon black in accordance with JIS K6221. The specific surface area of ​​the carbon black is a value measured by the BET method.

[0050] The carbon black in the elastic layer 14 has a good balance between the resistance value and the relative dielectric constant, and the DBP absorption amount is set to 69 cm 3 / 100g or more 121cm 3 The carbon black in the elastic layer 14 is preferably 45 mm / 100 g or less, because the contact area with the rubber is just right, the tolerance for variation in the amount of addition is high, and it is easy to control the target resistance value and dielectric constant. 2 / g or more 58m 2 / g or less is preferable.

[0051] In the elastic layer 14, the carbon black content is preferably 15 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the non-polar rubber and the polar rubber in total, from the viewpoint of easily keeping the resistance value and the relative dielectric constant of the elastic layer 14 within a specific range, more preferably 20 parts by mass or more and 45 parts by mass or less, and even more preferably 25 parts by mass or more and 40 parts by mass or less.

[0052] The elastic layer 14 is preferably made of a composition that does not contain an ionic conductive agent. When the elastic layer 14 is made of a composition that does not contain an ionic conductive agent, the relative dielectric constant of the elastic layer 14 does not increase too much, and it is easy to keep the relative dielectric constant of the elastic layer 14 within a specific range.

[0053] If necessary, various additives may be appropriately added to the elastic layer 14. Examples of the additives include a lubricant, a vulcanization accelerator, an antioxidant, a light stabilizer, a viscosity modifier, a processing aid, a flame retardant, a plasticizer, a foaming agent, a filler, a dispersant, an antifoaming agent, a pigment, and a mold release agent.

[0054] The thickness of the elastic layer 14 is not particularly limited, and may be appropriately set within a range of 0.1 to 10 mm depending on the application.

[0055] The surface layer 16 contains fluororesin and (meth)acrylic resin, has a relative dielectric constant of 10 to 22, and a resistance value of 1.2×10 4 Ω or more 8.8×10 5 It is less than Ω.

[0056] The fluororesin preferably has a relatively high dielectric constant and low resistance. The relative dielectric constant of the fluororesin is preferably 8 or more and 10 or less. The volume resistivity of the fluororesin is preferably 1.0×10 13 Ω cm or more 1.0×10 14 It is preferable that the dielectric constant and volume resistivity of the fluororesin are within the above ranges. Since the fluororesin has a relatively high dielectric constant and low resistance, it is easy to make the surface layer 16 have a high dielectric constant and low resistance. In this case, the electrostatic effect of the fluororesin is also easily maintained.

[0057] The fluororesin is preferably polyvinylidene fluoride. Since the fluororesin has a relatively high dielectric constant and low resistance, it is easy to make the surface layer have a high dielectric constant and low resistance. In this case, the electrostatic effect of the fluororesin is also easy to maintain.

[0058] Here, if the relative dielectric constant of the fluororesin is set to be larger than the above range, the relative dielectric constant of the surface layer 16 can be set to a desired value even if the fluororesin is used alone. However, in order to set the relative dielectric constant of the fluororesin to be larger than the above range, the fluororesin needs to be modified. Since the effect of using the fluororesin is reduced by modification, it is difficult to set the relative dielectric constant of the surface layer 16 to a desired value using the fluororesin alone. Therefore, in the surface layer 16, a (meth)acrylic resin is used together with the fluororesin in order to set the relative dielectric constant of the surface layer 16 to a desired value. Note that if the resin component of the surface layer 16 is only the (meth)acrylic resin, the relative dielectric constant is too high, making it difficult to set the relative dielectric constant of the surface layer 16 to a desired value.

[0059] The (meth)acrylic resin is a resin selected from an acrylic resin and a methacrylic resin. The (meth)acrylic resin includes a polymer (homopolymer or copolymer) of a (meth)acrylate. The (meth)acrylate may be either monofunctional or polyfunctional.

[0060] Examples of monofunctional (meth)acrylates include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isoamyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate, cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate. alkoxyalkyl (meth)acrylates such as methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and the like; phenoxyalkyl (meth)acrylates such as phenoxyethyl acrylate, nonylphenoxyethyl (meth)acrylate, and the like; and alkoxyalkylene glycol (meth)acrylates such as ethoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, and the like.

[0061] Examples of polyfunctional (meth)acrylates include alkyl diol di(meth)acrylates such as 1,9-nonanediol di(meth)acrylate, polyethylene glycol di(meth)acrylates such as diethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylates such as dipropylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, glycerol tri(meth)acrylate, and polyvalent (meth)acrylates obtained by addition reaction of ethylene glycol diglycidyl ether with a compound having an ethylenically unsaturated bond and active hydrogen such as an unsaturated carboxylic acid or an unsaturated alcohol, polyvalent (meth)acrylates obtained by addition reaction of an unsaturated epoxy compound such as glycidyl (meth)acrylate with a compound having active hydrogen such as a carboxylic acid or an amine, polyvalent (meth)acrylamides such as methylene bis(meth)acrylamide, and polyvalent vinyl compounds such as divinylbenzene.

[0062] The (meth)acrylic resin is more preferably a methacrylic resin from the viewpoints of the dielectric constant, volume resistivity, indentation Young's modulus, elastic recovery rate, etc. Also, the (meth)acrylic resin is more preferably an alkyl (meth)acrylate or a cycloalkyl (meth)acrylate from the viewpoints of the dielectric constant, volume resistivity, indentation Young's modulus, elastic recovery rate, etc.

[0063] The content ratio of the fluororesin and the (meth)acrylic resin is preferably fluororesin:(meth)acrylic resin=9.5:0.5 to 7:3 by mass, which makes it easier to keep the relative dielectric constant of the surface layer 16 within a specific range. The content ratio is more preferably fluororesin:(meth)acrylic resin=9:1 to 7:3, and even more preferably fluororesin:(meth)acrylic resin=8:2 to 7:3.

[0064] In addition, the difference in relative dielectric constant between the fluororesin and the (meth)acrylic resin is preferably 2 or less. This reduces unevenness in discharge from the charging roll 10 to the photoconductor. In addition, the difference in volume resistivity between the fluororesin and the (meth)acrylic resin is preferably 0.2 log Ω or less. This reduces unevenness in injection of charge from the charging roll 10 to the photoconductor.

[0065] Here, it is preferable that the indentation Young's modulus of the fluororesin is 0.65 GPa or more and 0.75 GPa or less, and the elastic recovery rate is 40% or more and 50% or less, and that the indentation Young's modulus of the (meth)acrylic resin is 0.65 GPa or more and 0.75 GPa or less, and the elastic recovery rate is 45% or more and 50% or less. This makes the deformation of the charging roll 10 against the pressure received from the photoconductor during rotation uniform, and local stress concentration is unlikely to occur. In addition, it is preferable that the difference in the indentation Young's modulus between the fluororesin and the (meth)acrylic resin is 0.1 GPa or less, and the difference in the elastic recovery rate is 5% or less. This makes it easier to suppress cracking of the surface layer 16 due to physical stress received from the photoconductor, and improves durability. The indentation Young's modulus can be measured from a sheet-shaped sample using a microindentation hardness tester. The elastic recovery rate can be measured from a sheet-shaped sample using a tensile tester.

[0066] The fluororesin preferably has a tensile strength of 28 MPa or more and 40 MPa or less, which improves the strength and durability of the surface layer 16. The tensile strength of the fluororesin can be measured by the elongation at break of a sheet sample using a tensile tester.

[0067] The surface layer 16 may contain roughness-forming particles. The roughness-forming particles are particles for imparting roughness to the surface of the surface layer 16. In other words, the particles are particles for imparting unevenness to the surface of the surface layer 16. The surface unevenness of the surface layer 16 forms a discharge space between the photoconductor and the charging roll 10.

[0068] The roughness-forming particles may be resin particles, inorganic particles, or the like. The roughness-forming particles may be solid particles or porous particles. When the roughness-forming particles are porous particles, the fluororesin or (meth)acrylic resin, which is the binder resin of the surface layer 16, and the roughness-forming particles are more integrated, making the surface layer 16 less likely to crack. In addition, the resistance can be integrated to make the injected charge uniform.

[0069] Examples of the material of the roughness-forming particles include urethane resin, polyamide resin, (meth)acrylic resin, (meth)acrylic silicone resin, silicone graft (meth)acrylic polymer, (meth)acrylic graft silicone polymer, urethane rubber, silica, etc. Among these, (meth)acrylic resin is more preferable from the viewpoint of affinity with the binder resin of the surface layer 16, integration, etc.

[0070] The size of the roughness-forming particles is not particularly limited, but from the viewpoint of easily ensuring uniform charging properties, the average particle diameter is preferably 3.0 μm or more and 50 μm or less. More preferably, the average particle diameter is 5.0 μm or more and 30 μm or less. The average particle diameter of the roughness-forming particles is expressed as the average of any 20 points when the surface of the surface layer 16 is observed with a laser microscope, and the diameter of the roughness-forming particles visible during surface observation is taken as the particle diameter.

[0071] The content of the roughness-forming particles in the surface layer 16 is not particularly limited, but from the viewpoint of easily ensuring uniform electrostatic properties, it is preferably 3 parts by mass or more and 50 parts by mass or less relative to 100 parts by mass of the binder resin in the surface layer 16. More preferably, it is 5 parts by mass or more and 30 parts by mass or less.

[0072] Various additives may be added to the surface layer 16 as necessary.

[0073] The thickness of the surface layer 16 is not particularly limited, and may be set in the range of 0.1 to 3.0 μm. The thickness of the surface layer 16 can be measured by observing the cross section using a laser microscope (such as Keyence's "VK-9510"). For example, the distance from the surface of the elastic layer 14 to the surface of the surface layer 16 is measured at five arbitrary positions, and the thickness can be expressed as the average.

[0074] The charging roll 10 can be produced by forming an elastic layer 14 on the outer peripheral surface of a shaft body, and then forming a surface layer 16 on the outer peripheral surface of the elastic layer 14 .

[0075] The elastic layer 14 can be formed, for example, as follows: First, the shaft 12 is coaxially placed in the hollow portion of a roll molding die, and an uncrosslinked composition for forming an elastic layer is injected and heated and cured (crosslinked), and then the composition is demolded, or the uncrosslinked composition for forming an elastic layer is extruded onto the surface of the shaft 12 to form the elastic layer 14 on the outer periphery of the shaft.

[0076] A surface layer forming composition is used to form the surface layer 16. The surface layer forming composition contains the above-mentioned main material and other additives which are contained as necessary.

[0077] The composition for forming the surface layer may appropriately contain a solvent such as an organic solvent such as methyl ethyl ketone, toluene, acetone, ethyl acetate, butyl acetate, methyl isobutyl ketone (MIBK), THF, or DMF, or a water-soluble solvent such as methanol or ethanol, in order to adjust the viscosity.

[0078] The surface layer 16 can be formed by a method such as coating a surface layer-forming composition on the outer peripheral surface of the elastic layer 14. As the coating method, various coating methods such as roll coating, dipping, spray coating, etc. The coated surface layer 16 may be irradiated with ultraviolet light or heat treated as necessary.

[0079] In the charging roll 10 having the above configuration, the elastic layer 14 contains non-polar rubber, polar rubber, and carbon black, and has a relative dielectric constant of 7 to 29, and a resistance value of 6.0×10 4 Ω or more 5.0×10 6 Ω or less, the surface layer 16 contains a fluororesin and a (meth)acrylic resin, the relative dielectric constant is 10 to 22, and the resistance value is 1.2×10 4 Ω or more 8.8×10 5 Ω or less. This reduces the amount of discharge from the charging roll 10 to the photoconductor, suppressing the generation of harmful substances such as ozone and NOx, and thus preventing environmental deterioration and image deterioration. In addition, the above-mentioned configuration facilitates charge transfer between the charging roll 10 and the grounded portion of the photoconductor, and the photoconductor can be charged to a desired charge level by injecting charge from the charging roll 10 to the photoconductor. This provides excellent charging performance even with a reduced amount of discharge.

[0080] If the dielectric constant of the surface layer 16 or the elastic layer 14 is higher than the specific range, too much charge is stored, making it difficult for charge to move from the charging roll 10 to the photoconductor at the contact portion. On the other hand, if the dielectric constant is lower than the specific range, discharge from the charging roll 10 to the photoconductor increases, resulting in increased generation of harmful substances such as ozone and NOx. Also, if the resistance value of the surface layer 16 or the elastic layer 14 is higher than the specific range, charge does not move easily at the contact portion from the charging roll 10 to the photoconductor. On the other hand, if the resistance value is lower than the specific range, discharge from the charging roll 10 to the photoconductor increases, resulting in increased generation of harmful substances such as ozone and NOx.

[0081] From the above viewpoints, the relative dielectric constant of the elastic layer 14 is more preferably not less than 10, and not less than 15. Also, it is more preferably not more than 25, and not more than 20. The resistance value of the elastic layer 14 is more preferably not more than 8.0×10 4 Ω or more, 1.0×10 5 Ω or more. Also, 1.0×10 6 Ω or less, 5.0×10 5Similarly, the relative dielectric constant of the surface layer 16 is more preferably 12 or more, more preferably 14 or more, and is 20 or less, more preferably 18 or less. The resistance value of the surface layer 16 is more preferably 2.0×10 4 Ω or more, 5.0×10 4 Ω or more. Also, 8.0×10 5 Ω or less, 5.0×10 5 It is less than Ω.

[0082] In order to set the dielectric constant and resistance value of the elastic layer 14 within the above range, it is recommended to use a small amount of polar rubber based on non-polar rubber and to select carbon black. A suitable combination of non-polar rubber and polar rubber can be selected from those listed above. Since non-polar rubber and polar rubber have low compatibility, the surface area ratio is important as the content ratio. By setting the area ratio within the above specific range, it is easy to set the dielectric constant of the elastic layer 14 within the specific range. The average particle size and the product of DBP absorption and specific surface area are important factors for carbon black, and it is particularly recommended to select a suitable product of DBP absorption and specific surface area, which is an index of the dielectric constant of carbon black.

[0083] In order to set the dielectric constant and resistance value of the surface layer 16 within the above range, it is advisable to select a fluororesin with a relatively high dielectric constant and low resistance as a base, and to use a small amount of (meth)acrylic resin with a higher dielectric constant than the fluororesin. The fluororesin is preferably one having the above-mentioned specific dielectric constant and volume resistivity. By setting the content ratio of the fluororesin and the (meth)acrylic resin within the above-mentioned specific range, it is easy to set the dielectric constant of the surface layer 16 within the specific range. By selecting a fluororesin and a (meth)acrylic resin with similar indentation Young's modulus and elastic recovery rate, cracking of the surface layer 16 due to physical stress from the photoconductor is suppressed, and durability is improved. EXAMPLES

[0084] The present invention will be described in detail below using examples and comparative examples.

[0085] (Examples 1-7, Comparative Examples 1-10) <Preparation of Composition for Forming Elastic Layer> The polar rubber, non-polar rubber, and carbon black were blended in the blending ratios (parts by mass) shown in the table, and a peroxide crosslinking agent, vulcanization aid, and catalyst were blended. These were then stirred and mixed using a stirrer to prepare a composition for forming an elastic layer.

[0086] <Preparation of Elastic Layer> A core bar (diameter 8 mm) was set in a molding die (pipe-shaped), the composition for forming the elastic layer was injected, and the die was heated at 180°C for 30 minutes. The die was then cooled and demolded to form an elastic layer 1.9 mm thick around the outer periphery of the core bar.

[0087] <Preparation of Composition for Forming Surface Layer> A composition for forming a surface layer was prepared by blending fluororesin, (meth)acrylic resin, carbon black, and particles for forming roughness in the blending ratio (parts by mass) shown in the table, diluting with methyl ethyl ketone (MEK), and mixing and stirring at a predetermined stirring speed.

[0088] <Preparation of surface layer> While continuing to stir the surface layer-forming composition, the composition was roll-coated on the outer peripheral surface of the elastic layer and heat-treated to form a surface layer having a thickness of 1.0 μm on the outer periphery of the elastic layer, thereby producing a charging roll.

[0089] As materials for the elastic layer forming composition, the following materials were prepared. (Polar rubber) Polar rubber <1> (NBR): "Nipol 1041" made by Nippon Zeon Polar rubber <2> (ECO): "Hydrin H1100" made by Zeon Corporation Polar rubber <3> (CR): Denka "Denka Chloroprene DCR-107" (Non-polar rubber) Non-polar rubber <1> (IR): "Nipol IR2200" manufactured by Nippon Zeon Non-polar rubber <2> (NR): Maxell Kureha "GW540N" Non-polar rubber <3> (BR): UBE Elastomer "UBEPOL BR130B" (Carbon Black) Carbon black <1> Mitsubishi Chemical "Mitsubishi Carbon Black #25", average particle size 47 nm, oil absorption (DBP absorption) 69 cm 3 / 100g, specific surface area 55m 2 / g Carbon black <2> : Mitsubishi Chemical "Mitsubishi Carbon Black #20", average particle size 50 nm, oil absorption (DBP absorption) 121 cm 3 / 100g, specific surface area 45m 2 / g Carbon black <3> : Tokai Carbon "TOKABLACK♯7270SB", average particle size 36nm, oil absorption (DBP absorption) 62cm 3 / 100g, specific surface area 58m 2 / g Carbon black <4> : Mitsubishi Chemical's "Diablack G", average particle size 80 nm, oil absorption (DBP absorption) 84 cm 3 / 100g, specific surface area 28m 2 / g Carbon black <5> : Nippon Steel Carbon "HTC♯SSRF", average particle size 68nm, oil absorption (DBP absorption) 72cm 3 / 100g, specific surface area 24m 2 / g Carbon black <6> : "Asahi #70L" made by Asahi Carbon, average particle size 25nm, oil absorption (DBP absorption) 85cm 3 / 100g, specific surface area 75m 2 / g

[0090] As materials for the surface layer forming composition, the following materials were prepared. (Fluorine resin) Fluorine resin <1> (PVDF): Arkema "Kynar 711", volume resistivity 1.0 x 10 14 Ω·cm, relative dielectric constant 8, indentation Young's modulus 0.65GPa, elastic recovery 40% Fluorine resin <2> (PVDF): Arkema "Kynar HSV900", volume resistivity 1.0 x 10 13 Ω cm, relative dielectric constant 10, indentation Young's modulus 0.75 GPa, elastic recovery 50% Fluorine resin <3> (PTFE+PFA): Daikin Industries "Neoflon PFA AP-230AS", volume resistivity 1.4×10 13 Ω·cm, relative dielectric constant 8.2, indentation Young's modulus 0.71GPa, elastic recovery 48% Fluorine resin <4> (PVDF): Kureha "KF Polymer #1000", volume resistivity 2.1 x 10 14 Ω·cm, relative dielectric constant 7.6, indentation Young's modulus 0.72GPa, elastic recovery 40% ((Meth)acrylic resin) (Meth)acrylic resin <1> (PMMA): Mitsubishi Chemical's "Dianal BR107", dielectric constant 10, indentation Young's modulus 0.65GPa, elastic recovery 50% (Meth)acrylic resin <2> (PMMA): Mitsubishi Chemical's "Acrypet IRH50001", dielectric constant 11, indentation Young's modulus 0.75GPa, elastic recovery 40% (Carbon Black) Carbon black: TOKUSHIKI "9027BLACK" (Roughness forming particles) ·Grains for roughness formation <1> (PMMA): "Techpolymer MBP-8" manufactured by Sekisui Kasei, average particle size 8 μm, porous particles ·Grains for roughness formation <2> (PMMA): Soken Chemical's "Chemisnow MZ-8HN", average particle size 8μm, solid particles

[0091] (Sample preparation method) Resin (fluororesin or acrylic resin) was added to a mixed solvent of acetone and water (9:1) to make a 5 wt% solution, which was then dissolved by impeller stirring for 24 hours. The solution was then cast in an environment of 28°C and 60% RH, and then baked at 100°C for 30 minutes to produce measurement samples (sheet-shaped) made of each resin.

[0092] (Method of measuring physical properties of samples) (Volume resistivity) The volume resistivity of the obtained sheet sample was measured in accordance with JIS K7194 using a resistance meter RM3545 manufactured by HIOKI and a four-point probe RM9010-01 manufactured by HIOKI.

[0093] (Dielectric constant) The obtained sheet sample was measured in accordance with JIS C2138 by applying 10 kHz using a precision LCR meter E4980A (Agilent Technologies).

[0094] (Indentation Young's Modulus) The indentation Young's modulus of the obtained sheet-like sample was measured using an ultra-microindentation hardness tester (nanoindentation tester: ENT-1100a manufactured by Elionik Co., Ltd.) based on the nanoindentation method.

[0095] (Elastic recovery rate) The elastic recovery rate of the obtained sheet-like sample was measured using a tensile tester (AE-F Strograph, manufactured by Toyo Seiki Seisakusho) in accordance with JIS K6251.

[0096] (Tensile strength) The resulting sheet-like sample was subjected to measurement of elongation at break using a tensile tester (AE-F Strograph, manufactured by Toyo Seiki Seisakusho) in accordance with JIS K6251.

[0097] (relative dielectric constant of elastic layer) The elastic layer before the formation of the surface layer was cut into a sample piece of 1 cm x 1 cm x 0.3 cm, and the obtained sheet-like sample was measured by applying 10 kHz using a precision LCR meter E4980A (Agilent Technologies) in accordance with JIS C2138.

[0098] (Surface dielectric constant) The composition for forming the surface layer was cast in an environment of 28°C x 60% RH, and then baked at 100°C for 30 minutes to prepare a measurement sample (sheet-shaped) made of the composition for forming the surface layer. The obtained sheet-shaped sample was measured by applying 10 kHz using a precision LCR meter E4980A (manufactured by Agilent Technologies) in accordance with JIS C2138.

[0099] (Resistance value of elastic layer) The elastic layer before the formation of the surface layer was cut into a sample piece of 1 cm × 1 cm × 0.3 cm, and the resistance value of the obtained sheet-like sample was measured using a HIOKI resistance meter RM3545 and a HIOKI 4-point probe RM9010-01 in accordance with JIS K7194.

[0100] (Surface resistance value) The composition for forming a surface layer was cast in an environment of 28°C x 60% RH, and then baked at 100°C for 30 minutes to prepare a measurement sample (sheet-shaped) made of the composition for forming a surface layer. The resistance value of the obtained sheet-shaped sample was measured using a HIOKI resistance meter RM3545 and a HIOKI 4-point probe RM9010-01 in accordance with JIS K7194.

[0101] (Rubber surface area ratio) The elastic layer before the surface layer was formed was cut into a sample piece measuring 11 cm x 1 cm x 0.3 cm, which was stained with Os staining method and then observed under a scanning electron microscope at a magnification of 2000. The areas of dark and light colored areas by Os staining respectively indicated the presence of rubber, and the occupied areas were measured.

[0102] (Evaluation / Judgment Method) The manufactured charging roll was attached to the unit (black) of an actual machine (RICOH "IM C8000"), and images were output at 25% density halftone in a 10℃ x 10% RH environment, and an evaluation was performed after 1 million sheets were printed.

[0103] (Black and white dots): Charging property (amount of discharge) Images with no white or black spots were rated as very good (◎), images with a few spots but with low density and within the acceptable range were rated as good (○), and images with many spots and high density were rated as unacceptable (×).

[0104] (Fog): Charging property (amount of charge) Images with no fog were rated as very good (◎), images with a few spots but low density and within the acceptable range were rated as good (◯), and images with many spots and high density were rated as unacceptable (×).

[0105] (Unevenness): Anti-stain Images with no unevenness were rated as very good (A), images with slight unevenness but within the acceptable range were rated as good (O), and images with strong unevenness were rated as unacceptable (X).

[0106] (Crack): Durability A roll having no cracks on the surface was rated as very good (A), and a roll having a few cracks but not affecting the image was rated as good (O).

[0107] [Table 1]

[0108] [Table 2]

[0109] In Comparative Example 1, the area ratio of the polar rubber on the surface of the elastic layer is too small, and the relative dielectric constant of the elastic layer is too small. As a result, the amount of discharge is too large, and image deterioration due to black and white dots occurs. In Comparative Example 3, the area ratio of the polar rubber on the surface of the elastic layer is too large, and the relative dielectric constant of the elastic layer is too large. As a result, image deterioration due to fogging occurs due to insufficient charging. In Comparative Example 2, the carbon black content of the elastic layer is low, and the resistance value of the elastic layer is too high. As a result, image deterioration due to fogging occurs due to insufficient charging. In Comparative Example 4, the carbon black content of the elastic layer is high, and the resistance value of the elastic layer is too low. As a result, the amount of discharge is too large, and image deterioration due to black and white dots occurs.

[0110] In Comparative Example 5, the content of fluororesin in the surface layer is too high, and the relative dielectric constant of the surface layer is too low. As a result, the amount of discharge is too high, and image deterioration due to black and white dots occurs. In Comparative Example 7, the content of fluororesin in the surface layer is too low, and the relative dielectric constant of the surface layer is too high. As a result, image deterioration due to fogging occurs due to insufficient charging. In Comparative Example 6, the content of carbon black in the surface layer is low, and the resistance value of the surface layer is too high. As a result, image deterioration due to fogging occurs due to insufficient charging. In Comparative Example 8, the content of carbon black in the surface layer is high, and the resistance value of the surface layer is too low. As a result, the amount of discharge is too high, and image deterioration due to black and white dots occurs.

[0111] In Comparative Example 9, the product of the oil absorption amount and the specific surface area of ​​the carbon black in the elastic layer is large, and the relative dielectric constant of the elastic layer is too large. As a result, insufficient charging causes image deterioration due to fog. In addition, the resistance value of the elastic layer is too small. As a result, the amount of discharge becomes too large, causing image deterioration due to black and white spots. In Comparative Example 10, the relative dielectric constant of the fluororesin in the surface layer is small at 7.6, and the relative dielectric constant of the surface layer is too small. As a result, the amount of discharge becomes too large, causing image deterioration due to black and white spots. In addition, the volume resistivity is 2.1×10 14 The surface resistance is high at Ω·cm, which causes insufficient charging and leads to image deterioration due to fogging.

[0112] In contrast, in the example, the elastic layer contains non-polar rubber, polar rubber, and carbon black, and has a relative dielectric constant of 7 to 29, and a resistance value of 6.0×10 4 Ω or more 5.0×10 6 Ω or less, the surface layer contains fluororesin and (meth)acrylic resin, the relative dielectric constant is 10 to 22, and the resistance is 1.2×10 4 Ω or more 8.8×10 5 Ω or less. Therefore, the discharge amount is reduced, and image deterioration due to black and white dots is suppressed. In addition, the above-mentioned configuration makes it easier for charges to move, and the charging property is excellent even if the discharge amount is reduced. Therefore, image deterioration due to fogging caused by insufficient charging is also suppressed.

[0113] Although the embodiments and examples of the present invention have been described above, the present invention is not limited to the above-mentioned embodiments and examples, and various modifications are possible without departing from the spirit and scope of the present invention. [Explanation of symbols]

[0114] 10. Charging roll 12 Axial body 14 Elastic layer 16 Surface layer

Claims

1. The shaft body includes an elastic layer formed on an outer peripheral surface of the shaft body, and a surface layer formed on the outer peripheral surface of the elastic layer, The elastic layer contains non-polar rubber, polar rubber, and carbon black, has a relative dielectric constant of 7 to 29, and a resistance value of 6.0×10 4 Ω or more 5.0×10 6 Ω or less, The surface layer contains a fluororesin and a (meth)acrylic resin, has a relative dielectric constant of 10 to 22, and a resistance value of 1.2×10 4 Ω or more 8.8×10 5 Ω or less for electrophotographic equipment.

2. 2. The charging roll for electrophotographic equipment according to claim 1, wherein an area ratio of said non-polar rubber to said polar rubber on the surface of said elastic layer is from 9:1 to 7:

3.

3. 3. The charging roll for an electrophotographic apparatus according to claim 1, wherein the non-polar rubber is an isoprene rubber or a natural rubber, and the polar rubber is a nitrile rubber or a hydrin rubber.

4. 3. The charging roll for an electrophotographic apparatus according to claim 1, wherein the carbon black has an average particle size of 36 nm or more and 80 nm or less, and a product of DBP absorption amount and specific surface area of ​​1,728 or more and 5,445 or less.

5. 3. The charging roll for an electrophotographic device according to claim 1, wherein the content of the carbon black is 15 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the total of the non-polar rubber and the polar rubber.

6. 3. The charging roll for an electrophotographic device according to claim 1, wherein said elastic layer is made of a composition that does not contain an ion conductive agent.

7. 3. The charging roll for electrophotographic equipment according to claim 1, wherein a content ratio of the fluororesin to the (meth)acrylic resin is, in terms of mass ratio, fluororesin:(meth)acrylic resin=9.5:0.5 to 7:

3.

8. The fluororesin has a relative dielectric constant of 8 to 10 and a volume resistivity of 1.0×10 13 Ω・cm or more 1.0×10 14 3. The charging roll for electrophotographic equipment according to claim 1, wherein the surface roughness is Ω·cm or less.

9. 3. The charging roll for an electrophotographic device according to claim 1, wherein the fluororesin is polyvinylidene fluoride.

10. 3. The charging roll for electrophotographic equipment according to claim 1, wherein the difference in volume resistivity between the fluororesin and the (meth)acrylic resin is 0.2 log Ω or less.

11. 3. The charging roll for electrophotographic equipment according to claim 1, wherein the fluororesin has an indentation Young's modulus of 0.65 GPa or more and 0.75 GPa or less and an elastic recovery rate of 40% or more and 50% or less, and the (meth)acrylic resin has an indentation Young's modulus of 0.65 GPa or more and 0.75 GPa or less and an elastic recovery rate of 45% or more and 50% or less.

12. 3. The charging roll for electrophotographic equipment according to claim 1, wherein the difference in indentation Young's modulus between said fluororesin and said (meth)acrylic resin is 0.1 GPa or less and the difference in elastic recovery rate between said fluororesin and said (meth)acrylic resin is 5% or less.

13. 3. The charging roll for an electrophotographic device according to claim 1, wherein the tensile strength of the fluororesin is from 28 MPa to 40 MPa.

14. 3. The charging roll for electrophotographic equipment according to claim 1, wherein the difference in relative dielectric constant between the fluororesin and the (meth)acrylic resin is 2 or less.

15. 3. The charging roll for an electrophotographic device according to claim 1, wherein the surface layer further contains particles for providing roughness.

16. 16. The charge roll for an electrophotographic device according to claim 15, wherein the roughness-forming particles are porous particles.

17. an area ratio of the non-polar rubber to the polar rubber on the surface of the elastic layer is non-polar rubber:polar rubber=9:1 to 7:3; The non-polar rubber is isoprene rubber or natural rubber, and the polar rubber is nitrile rubber or hydrin rubber; The carbon black has an average particle size of 36 nm or more and 80 nm or less, and a product of DBP absorption amount and specific surface area of ​​1728 or more and 5445 or less, The content of the carbon black is 15 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of the total of the non-polar rubber and the polar rubber, the elastic layer is made of a composition that does not contain an ion conductive agent, a content ratio of the fluororesin to the (meth)acrylic resin is, in terms of mass ratio, fluororesin:(meth)acrylic resin=9.5:0.5 to 7:3; The fluororesin has a relative dielectric constant of 8 to 10 and a volume resistivity of 1.0×10 13 Ω・cm or more 1.0×10 14 Ω cm or less, The fluororesin is polyvinylidene fluoride, a difference in volume resistivity between the fluororesin and the (meth)acrylic resin is 0.2 log Ω or less; the fluororesin has an indentation Young's modulus of 0.65 GPa or more and 0.75 GPa or less and an elastic recovery rate of 40% or more and 50% or less, the (meth)acrylic resin has an indentation Young's modulus of 0.65 GPa or more and 0.75 GPa or less and an elastic recovery rate of 45% or more and 50% or less, a difference in indentation Young's modulus between the fluororesin and the (meth)acrylic resin is 0.1 GPa or less, and a difference in elastic recovery between the fluororesin and the (meth)acrylic resin is 5% or less; The tensile strength of the fluororesin is 28 MPa or more and 40 MPa or less, a difference in relative dielectric constant between the fluororesin and the (meth)acrylic resin is 2 or less; The surface layer further contains roughness-forming particles, 2. The charging roll for an electrophotographic device according to claim 1, wherein the roughness-imparting particles are porous particles.

Citation Information

Patent Citations

  • Charging member and charging device

    JP2003140442A

  • Conductive rubber member

    JP2007164147A

  • Charging roll and method of producing the same

    JP2010266844A

  • Conductive member for electrophotographic apparatus

    JP2012047871A

  • Charging member

    JP2015045788A