Production method of polystyrene resin extrusion expanded material

By using alkyl chlorides and water with an acid neutralizer in the foam composition, the method addresses equipment corrosion and maintains high heat insulation and large thickness in polystyrene resin foam production.

JP2024141462APending Publication Date: 2024-10-10KANEKA CORP

Patent Information

Application Number
JP2023053136
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

The use of alkyl chlorides and water as blowing agents in polystyrene resin foam production leads to equipment corrosion due to the generation of corrosive gases, compromising the production of foams with high heat insulation properties and large thickness.

Method used

Incorporating an acid neutralizer, such as alkali metal carbonates or bicarbonates, into the foam composition to neutralize the corrosive gases generated by the reaction between alkyl chlorides and water, while maintaining high heat insulation properties and large thickness.

Benefits of technology

The method effectively suppresses equipment corrosion and maintains excellent heat insulation and large thickness in the polystyrene resin foam, ensuring stable production and improved durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141462000001
    Figure 2024141462000001
  • Figure 2024141462000002
    Figure 2024141462000002
Patent Text Reader

Abstract

To suppress corrosion of a facility caused by corrosive gas, when producing a polystyrene resin extrusion expanded body using, alkyl chloride and water, as an expanded material.SOLUTION: There is provided a production method of a polystyrene resin extrusion expanded body configured to: melt and knead a composition including a polystyrene resin and an expanded material, then extrude the composition to a low pressure region and mold the same in foam molding. The expanded material includes at least water and alkyl chloride. The composition includes, in addition to the polystyrene resin and the expanded material, an acid neutralization agent, and in the composition, an amount of the acid neutralization agent to the amount of the alkyl chloride, is preferably 0.003 times or more, in a molar ratio.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an extruded polystyrene resin foam. [Background technology]

[0002] Because of its high insulating properties, extruded polystyrene resin foams are used as insulating materials for houses and buildings, as well as for refrigerators, etc. Extruded polystyrene resin foams are produced by melt-kneading a composition containing a polystyrene resin and a foaming agent in an extruder, and then extruding the mixture through a die slit or the like into a low-pressure region.

[0003] As a method for improving the thermal insulation of extruded polystyrene resin foam, the use of alkyl chlorides such as methyl chloride and ethyl chloride as a blowing agent has been proposed (for example, Patent Documents 1 to 3). By using a gas with low thermal conductivity (high thermal insulation) such as an alkyl chloride as a blowing agent, the low thermal conductivity gas is enclosed in the bubbles of the foam, thereby improving the thermal insulation of the foam. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-330351 A [Patent Document 2] JP 2019-108416 A [Patent Document 3] JP 2019-189811 A Summary of the Invention [Problem to be solved by the invention]

[0005] By using an alkyl chloride as a blowing agent, a foam with high thermal insulation properties can be obtained. Also, by using water as a blowing agent, a foam with large thickness can be easily obtained. However, when an alkyl chloride and water are used in combination as a blowing agent, corrosion of equipment is likely to progress. In view of such problems, the present invention aims to provide a method for producing an extruded polystyrene resin foam with excellent thermal insulation properties and large thickness while suppressing corrosion of equipment. [Means for solving the problem]

[0006] One embodiment of the present invention is a method for producing an extruded polystyrene resin foam, which comprises melt-kneading a composition containing a polystyrene resin and a foaming agent, and extruding the composition into a low pressure region to form a foam. The foaming agent contains at least an alkyl chloride and water. The amount of the alkyl chloride per 100 parts by weight of the polystyrene resin in the composition may be 1 to 8 parts by weight.

[0007] The composition further contains an acid neutralizer in addition to the polystyrene resin and the blowing agent. The amount of the acid neutralizer relative to the alkyl chloride in the composition is preferably 0.003 times or more in molar ratio. The amount of the acid neutralizer relative to 100 parts by weight of the polystyrene resin in the composition may be 0.02 parts by weight or more.

[0008] The acid neutralizing agent includes an alkali metal salt. The acid neutralizing agent may be an alkali metal carbonate or bicarbonate.

[0009] The acid neutralizing agent may be water-soluble. The water-soluble acid neutralizing agent may be dissolved in water as a foaming agent to form an aqueous solution, and the aqueous solution may be mixed with the polystyrene-based resin to prepare the composition.

[0010] The foam may have a thickness of 10 mm or more. The foam may have a thermal conductivity of less than 0.0284 W / mK. Effect of the Invention

[0011] By using alkyl chloride and water as the blowing agent, it is possible to provide an extruded polystyrene resin foam with high heat insulation, large thickness, and beautiful surface. In addition, by containing a predetermined amount of acid neutralizer in the composition used for producing the foam, it is possible to suppress the generation and diffusion of corrosive gases caused by the reaction between alkyl chloride and water, and to prevent deterioration of equipment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention relates to a method for producing an extruded polystyrene resin foam, comprising melt-kneading a composition containing a polystyrene resin and a foaming agent, and extruding the composition in a low pressure region to form an extrusion molded product.

[0013] [Composition] A foamable melt composition is prepared by blending a foaming agent into a resin composition containing a polystyrene resin and melt-kneading the mixture. That is, the foamable melt composition contains at least a polystyrene resin and a foaming agent. Hereinafter, the foamable melt composition is simply referred to as a "composition," and a composition not containing a foaming agent is referred to as a "resin composition."

[0014] Each component contained in the composition will be described in detail below. Unless otherwise specified, each component described below may be used alone or in combination of two or more.

[0015] <Polystyrene resin> The polystyrene resin includes a styrene polymer. Examples of the styrene polymer include a homopolymer of a styrene monomer (polystyrene); a copolymer of two or more kinds of styrene monomers; and a copolymer of a styrene monomer and another monomer. When the styrene polymer is a copolymer, the amount of the styrene monomer in the total monomer is preferably 60% by weight or more, more preferably 70% by weight or more. The polymer sequence of the copolymer is not particularly limited, and may be either a random copolymer or a block copolymer. The copolymer may be a graft copolymer. The styrene polymer may be a polymer having a branched structure.

[0016] Examples of styrene-based monomers include styrene, methylstyrene, dimethylstyrene, ethylstyrene, diethylstyrene, isopropylstyrene, bromostyrene, dibromostyrene, tribromostyrene, chlorostyrene, dichlorostyrene, trichlorostyrene, vinyltoluene, vinylxylene, etc. Examples of other monomers include polyfunctional vinyl compounds such as divinylbenzene; acrylic acid, methacrylic acid; (meth)acrylic acid ester compounds such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, and butyl methacrylate; cyanide vinyl compounds such as (meth)acrylonitrile; diene compounds such as butadiene; unsaturated carboxylic acid anhydrides such as maleic anhydride and itaconic anhydride; and N-alkyl-substituted maleimide compounds such as N-methylmaleimide, N-butylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-(2)-chlorophenylmaleimide, N-(4)-bromophenylmaleimide, and N-(1)-naphthylmaleimide.

[0017] As the styrene-based polymer, from the viewpoints of being relatively inexpensive and suitable for extrusion foam molding, polystyrene, styrene-acrylonitrile copolymer, styrene-(meth)acrylic acid copolymer, styrene-maleic anhydride copolymer, styrene-diene compound copolymer (high-impact polystyrene, for example, styrene-butadiene copolymer), and the like are preferred.

[0018] The polystyrene-based resin may be a blend containing a polymer other than a styrene-based polymer, as long as it does not adversely affect the effects of the present invention. For example, the polystyrene-based resin may be a rubber-reinforced polystyrene (diene-based rubber-reinforced polystyrene, acrylic-based rubber-reinforced polystyrene, etc.). The polystyrene-based resin may be a mixture of a styrene-based polymer and another polymer. Examples of polymers other than a styrene-based polymer include polyolefins such as polypropylene and polyethylene, acrylic polymers, polyesters such as polyethylene terephthalate, polyphenylene ether, etc.

[0019] When the polystyrene resin contains a polymer other than the styrene polymer, the content thereof is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, even more preferably 5 parts by weight or less, and may be 3 parts by weight or less or 1 part by weight or less, relative to 100 parts by weight of the styrene polymer. The content of the styrene polymer in the polystyrene resin is preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, and may be 97% by weight or more, 99% by weight or more, or 100% by weight.

[0020] The polystyrene resin may be a mixture of two or more polymers with different copolymerization components, molecular weights, molecular weight distributions, branched structures, melt flow rates, etc., for the purpose of adjusting the melt viscosity, melt flow rate, melt tension, etc., during molding. The polystyrene resin may be a commercially available polystyrene resin (so-called virgin resin), or a recycled polystyrene resin (for example, recycled polystyrene resin recycled using a recycling extruder or the like after being used in the manufacture of foams, and recycled polystyrene resin recycled from food trays and fish boxes collected in the market). Virgin resin and recycled polystyrene resin may be mixed.

[0021] The polystyrene resin preferably has a melt flow rate (MFR) of 50 g / 10 min or less as measured according to JIS K7210. If the MFR is 50 g / 10 min or less, the foaming agent is easily uniformly dispersed in the polystyrene resin during melt kneading, and extrusion and foam molding can be stably performed, improving production stability. The MFR of the polystyrene resin may be 0.5 to 40 g / 10 min, or 1 to 30 g / 10 min.

[0022] <Foaming agent> In the production method of the present invention, an alkyl chloride and water are used as the blowing agent.

[0023] As the alkyl chloride, methyl chloride or ethyl chloride is preferred since it has a low thermal conductivity in the gas state and contributes greatly to improving the heat insulation.

[0024] The amount of alkyl chloride used is preferably 1 to 8 parts by weight, more preferably 2 to 7 parts by weight, and even more preferably 2.5 to 5 parts by weight, per 100 parts by weight of polystyrene resin. The amount of alkyl chloride in the foam is preferably 0.1 to 1 mol, and may be 0.2 to 8 mol or 0.25 to 7 mol, per 1 kg of foam. When the amount of alkyl chloride is small, the effect of improving heat insulation by alkyl chloride may not be fully exhibited. On the other hand, when the amount of alkyl chloride is excessively large, the plasticizing effect on polystyrene resin is large, which may cause a decrease in heat resistance and strength of the foam.

[0025] By using water as a foaming agent, the surface tension is increased, and bubbles having a relatively large diameter are easily formed, so that a foam having a large thickness can be formed. The amount of water used is preferably 0.1 to 3 parts by weight, more preferably 0.3 to 2 parts by weight, and even more preferably 0.4 to 1.5 parts by weight, based on 100 parts by weight of the polystyrene resin. If the amount of water is small, it may be difficult to obtain a foam having a large thickness. On the other hand, if the amount of water is excessively large, coarse bubbles are easily formed, and pores are generated, which may cause a poor appearance of the foam and a decrease in heat insulation.

[0026] In addition to alkyl chloride and water, other blowing agents that can function as blowing agents may be used. For example, by using hydrofluoroolefin and / or hydrochlorofluoroolefin as a blowing agent, the thermal insulation of the extruded foam tends to be further improved.

[0027] As the hydrofluoroolefin, tetrafluoropropene is preferred because it has a low thermal conductivity of gas and is highly safe. Specific examples of tetrafluoropropene include 1,3,3,3-tetrafluoropropene (HFO-1234ze) and 2,3,3,3-tetrafluoropropene (HFO-1234yf). As the hydrochlorofluoroolefin, hydrochlorotrifluoropropene is preferred because it has a low thermal conductivity of gas and is highly safe. Specific examples of hydrochlorotrifluoropropene include 1-chloro-3,3,3-trifluoropropene (HCFO-1233zd).

[0028] When hydrofluoroolefin and / or hydrochlorofluoroolefin are used as the blowing agent, the amount (total of hydrofluoroolefin and hydrochlorofluoroolefin) used is preferably 0.1 to 10 parts by weight, and may be 0.5 to 7 parts by weight or 1 to 5 parts by weight, based on 100 parts by weight of polystyrene resin, from the viewpoint of improving the heat insulating property of the foam. The more the amount of hydrofluoroolefin and hydrochlorofluoroolefin used, the more the heat insulating property of the foam tends to improve. On the other hand, even if the amount of hydrofluoroolefin and hydrochlorofluoroolefin used is excessively increased, a significant improvement in heat insulating property cannot be expected. In addition, if the amount of hydrofluoroolefin and hydrochlorofluoroolefin used is excessively large, the blowing agent may separate from the resin melt, causing spot holes on the surface of the foam, or the closed cell ratio may decrease, resulting in impaired heat insulating property.

[0029] Examples of blowing agents other than those mentioned above include saturated hydrocarbons having 3 to 5 carbon atoms, such as propane, normal butane, isobutane, normal pentane, isopentane, and opentane; alcohols having 1 to 4 carbon atoms, such as ethanol, methanol, propyl alcohol, isopropyl alcohol, butyl alcohol, isobutyl alcohol, and t-butyl alcohol; dimethyl ether, diethyl ether, methyl ethyl ether, isopropyl ether, n-butyl ether, diisopropyl ether, furan, furfural, 2-methylfuran, tetrahydrofuran, and tetrahydropi ethers such as dimethyl ketone, methyl ethyl ketone, diethyl ketone, methyl-n-propyl ketone, methyl-n-butyl ketone, methyl-i-butyl ketone, methyl-n-amyl ketone, methyl-n-hexyl ketone, ethyl-n-propyl ketone, ethyl-n-butyl ketone, and the like; organic blowing agents represented by carboxylic acid esters such as methyl formate, ethyl formate, propyl formate, butyl formate, amyl formate, methyl propionate, ethyl propionate, and the like; inorganic blowing agents such as carbon dioxide, and chemical blowing agents such as azo compounds and tetrazole.

[0030] Among these exemplified foaming agents, saturated hydrocarbons having 3 to 5 carbon atoms have a plasticizing effect on polystyrene resins and an effect of increasing the fluidity of the molten composition, and therefore can contribute to reducing the load on the extruder. From the viewpoint of foamability, propane, normal butane, and isobutane are preferred among the saturated hydrocarbons having 3 to 5 carbon atoms, and from the viewpoint of the heat insulating properties of the foam, normal butane and isobutane are particularly preferred.

[0031] When using a saturated hydrocarbon having 3 to 5 carbon atoms as a foaming agent, from the viewpoint of improving the heat insulating properties of the foam, the amount of the saturated hydrocarbon having 3 to 5 carbon atoms used is preferably 0.3 parts by weight or more, more preferably 0.5 parts by weight or more, even more preferably 0.7 parts by weight or more, and may be 0.9 parts by weight or more or 1 part by weight or more relative to 100 parts by weight of the polystyrene-based resin. On the other hand, from the viewpoint of suppressing molding defects such as bubble bursting, the amount of the saturated hydrocarbon having 3 to 5 carbon atoms used is preferably 5 parts by weight or less, more preferably 4.5 parts by weight or less, and may be 4 parts by weight or less or 3.5 parts by weight or less relative to 100 parts by weight of the polystyrene-based resin.

[0032] The amount of the foaming agent used (total amount of all foaming agents) is preferably 2 to 20 parts by weight, more preferably 3 to 15 parts by weight, further preferably 4 to 12 parts by weight, and may be 5 to 10 parts by weight, based on 100 parts by weight of the polystyrene resin. When the amount of the foaming agent used is within the above range, the foaming power of the composition is ensured, and a polystyrene resin foam having a desired thickness is easily and stably obtained.

[0033] <Acid neutralizer> In the present invention, the composition contains a polystyrene-based resin, an alkyl chloride as a blowing agent, water, and an acid neutralizing agent.

[0034] The acid neutralizer may be either organic or inorganic as long as it is a compound capable of neutralizing an acid, and examples of organic substances include amines. Examples of inorganic substances include oxides, hydroxides, carbonates, hydrogencarbonates, silicates, etc. of alkali metals or alkaline earth metals. Among these, inorganic substances are preferred because they have little effect on foamability and the physical properties of the foam.

[0035] As described later, it is preferable that the acid neutralizer is dissolved in water as a foaming agent and added to the composition. Therefore, it is preferable that the acid neutralizer is water-soluble, and it is preferable that it is soluble in water at room temperature by 1% by weight or more. As the acid neutralizer, an alkali metal salt is preferable because it has high water solubility and excellent acid neutralization. Among them, carbonates or hydrogen carbonates are preferable because the salt is unlikely to remain and has little effect on foaming property and physical properties of the foam. Examples of alkali metal carbonates include lithium carbonate, sodium carbonate, and potassium carbonate. Examples of alkali metal hydrogen carbonates include lithium hydrogen carbonate, sodium hydrogen carbonate, and potassium hydrogen carbonate. Among them, alkali metal carbonates such as sodium carbonate and potassium carbonate are particularly preferable because they are easy to handle and have a high acid neutralizing effect.

[0036] When alkyl chloride and water are used in combination as a blowing agent, when the alkyl chloride and water come into contact with each other and are mixed inside the extruder during or after the blowing agent is injected, acidic gases such as hydrogen chloride are generated. These acidic gases can corrode metals such as the extruder and piping. By adding an acid neutralizer to the composition, the acidic gases can be neutralized, thereby suppressing corrosion of the equipment.

[0037] The amount of the acid neutralizer is preferably 0.003 times or more, more preferably 0.005 times or more, even more preferably 0.008 times or more, and particularly preferably 0.01 times or more, in terms of molar ratio, relative to the alkyl chloride used as the foaming agent. The amount of the acid neutralizer is preferably 0.02 parts by weight or more, more preferably 0.04 parts by weight or more, even more preferably 0.05 parts by weight or more, and may be 0.06 parts by weight or more, relative to 100 parts by weight of the polystyrene resin. The more the amount of the acid neutralizer is, the more the generation of corrosive gas tends to be suppressed, and the more the corrosion prevention effect of the equipment tends to be enhanced.

[0038] On the other hand, if the amount of acid neutralizer is excessively large, the residue of the acid neutralizer may affect the foaming property and the physical properties of the foam. Therefore, the amount of acid neutralizer is preferably 1 or less by molar ratio to the alkyl chloride, more preferably 0.5 or less, even more preferably 0.1 or less, and may be 0.07 or less, 0.05 or less, or 0.03 or less. The amount of acid neutralizer is preferably 2 parts by weight or less, more preferably 1 part by weight or less, even more preferably 0.5 parts by weight or less, and may be 0.3 parts by weight or less, 0.2 parts by weight or less, or 0.15 parts by weight or less, based on 100 parts by weight of polystyrene resin.

[0039] <Additives> As described above, the composition includes the polystyrene resin and the blowing agent, as well as the acid neutralizer. The composition may further include other additives.

[0040] Examples of additives include water absorbents, heat radiation inhibitors, flame retardants, flame retardant assistants, flame retardant adjusters (iron oxide, iron complexes, diphenylalkanes, diketones, etc.), lubricants (sodium stearate, calcium stearate, etc.), cell size adjusters (talc, etc.), stabilizers (epoxy compounds, polyhydric alcohol ester compounds, phenolic antioxidants, phosphite antioxidants, etc.), processing aids (fatty acid metal salts, fatty acid amides, fatty acid esters, liquid paraffin, olefin waxes, etc.), antistatic agents, surfactants, colorants (pigments, dyes, etc.), ultraviolet absorbers, fluorescent brighteners, plasticizers, fillers, and the like.

[0041] (Water absorbent) When water is used as a foaming agent, the composition preferably contains a water absorbing agent. Water has low solubility in polystyrene resins, and if undissolved water is present in the composition, coarse bubbles are likely to form, which may cause the bubbles to burst. By containing a water absorbing agent in the composition, the solubility of water in the composition is increased and the water is uniformly dispersed, so that molding defects such as the generation of coarse bubbles and the bursting of bubbles are suppressed, and extrusion foam molding can be stably performed.

[0042] Examples of water absorbents include water-absorbing minerals (smectite, zeolite, etc.), silica, and hydrophilic organic substances. Examples of smectite include natural bentonite, purified bentonite, organified bentonite, and hectorite. Examples of zeolites include natural zeolites, artificial zeolites, and synthetic zeolites. Examples of silica include anhydrous silica, modified silica having a hydroxyl group on the surface, and porous silica. Examples of hydrophilic organic substances include polyacrylate-based polymers, starch-acrylic acid graft copolymers, polyvinyl alcohol-based polymers, vinyl alcohol-acrylate-based copolymers, ethylene-vinyl alcohol-based copolymers, polyacrylonitrile-methyl methacrylate-butadiene-based copolymers, polyethylene oxide-based copolymers and derivatives thereof, polyvinylpyrrolidone, sodium carboxymethylcellulose, hydroxyethylcellulose, polyhydric alcohols, and melamine.

[0043] The amount of the water absorbing agent used may be adjusted appropriately depending on the amount of water used, etc. The amount of the water absorbing agent in the composition is about 0.01 to 5 parts by weight, preferably 0.1 to 3 parts by weight, more preferably 0.2 to 2.5 parts by weight, and may be 0.3 to 2 parts by weight or 0.5 to 1.5 parts by weight, relative to 100 parts by weight of the polystyrene resin. The ratio (weight ratio) of the water absorbing agent to the water in the composition is about 0.05 to 5, preferably 0.1 to 4.5, and may be 0.2 to 4 or 0.3 to 3.

[0044] (Heat radiation suppressant) A heat radiation inhibitor may be added to the composition in order to improve the heat insulating property of the foam. The heat radiation inhibitor refers to a substance that has the property of reflecting, scattering, and absorbing electromagnetic waves in the near infrared or infrared region. By including the heat radiation inhibitor, the heat insulating property of the foam tends to be further improved.

[0045] Examples of the heat radiation inhibitor include white particles such as graphite, titanium oxide, barium sulfate, zinc oxide, aluminum oxide, and antimony oxide. Among these, graphite is particularly preferred because of its large heat radiation suppression effect. Among the white particles, titanium oxide is particularly preferred.

[0046] Specific examples of graphite include scaly (flake) graphite, amorphous graphite, spherical graphite, and artificial graphite. Among these, graphite containing scaly (flake) graphite as the main component is preferred because it has a high heat radiation suppression effect. The fixed carbon content of graphite is preferably 80% or more, and more preferably 85% or more.

[0047] The average particle size of the graphite is preferably 15 μm or less, more preferably 10 μm or less. The smaller the average particle size, the larger the specific surface area, and the higher the probability of collision with thermal radiation, resulting in a higher thermal radiation suppression effect. The average particle size of the graphite is the particle size (volume average particle size) when the cumulative volume of the total particle volume is 50% when the particle size distribution is measured and analyzed using a laser diffraction scattering method based on the Mie theory in accordance with ISO13320:2009 and JIS Z8825:2013.

[0048] When using a heat radiation inhibitor such as graphite, the amount of the heat radiation inhibitor in the composition is preferably 0.1 to 6 parts by weight, more preferably 0.5 to 5 parts by weight, and may be 0.8 to 4 parts by weight or 1 to 3.5 parts by weight, based on 100 parts by weight of the polystyrene resin. When the amount of the heat radiation inhibitor is small, a sufficient heat radiation suppression effect cannot be obtained. On the other hand, when the amount of the heat radiation inhibitor is excessively large, the dispersibility in the composition is poor, and it is difficult to obtain a heat radiation suppression effect corresponding to the content. In addition, when the content of a solid additive such as a heat radiation inhibitor increases, the number of nucleation points increases, so that it tends to be difficult to give a beautiful surface to the foam or to obtain a foam with a large thickness in order to make the bubbles of the foam finer. In addition, the solid additive such as a heat radiation inhibitor may be added to the composition as a master batch in which it is dispersed in the polystyrene resin in advance.

[0049] (Flame retardants and flame retardant synergists) As the flame retardant, a bromine-based flame retardant is preferably used. Specific examples of the bromine-based flame retardant include brominated bisphenol-based compounds such as tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl)ether and tetrabromobisphenol A-bis(2,3-dibromopropyl)ether; aliphatic bromine-containing polymers such as brominated styrene-butadiene block copolymers, brominated styrene-butadiene random copolymers, and brominated styrene-butadiene graft copolymers; tetrabromocyclooctane; hexabromocyclododecane; tris(2,3-dibromopropyl)isocyanurate; and the like. The amount of the flame retardant used is about 0.1 to 10 parts by weight, and may be 0.5 to 8 parts by weight or 1 to 5 parts by weight, relative to 100 parts by weight of the polystyrene resin.

[0050] Examples of the flame retardant auxiliary include radical generators such as 2,3-dimethyl-2,3-diphenylbutane and poly-1,4-diisopropylbenzene; phosphoric acid esters; and phosphine oxides.

[0051] [Method of manufacturing foam] For the production of polystyrene-based resin extruded foam, an extrusion foaming device is used in which a melt kneading section and a foam molding section having a die are arranged in this order from the upstream side to the downstream side in the extrusion direction of the composition. The melt kneading section and the foam molding section are connected. A cooling section for lowering the temperature of the composition may be arranged between the melt kneading section and the foam molding section. A polystyrene-based resin extruded foam is produced by melt kneading a resin composition containing a polystyrene-based resin and a foaming agent (melt kneading step), and extruding the foamable molten composition into a low pressure region and foam molding (foaming step).

[0052] In the melt-kneading step, a resin composition containing a polystyrene resin and additives is supplied to a melt-kneading section and kneaded. Examples of methods for blending various additives into a polystyrene resin include a method of adding various additives to a polystyrene resin and mixing them by dry blending; a method of adding various additives to a molten polystyrene resin from a supply section provided in the melt-kneading section; a method of preparing a master batch in which various additives are contained in a high concentration in a polystyrene resin using an extruder, kneader, Banbury mixer, roll, etc., and mixing the master batch and a polystyrene resin by dry blending.

[0053] The melt-kneading section may be, for example, an extruder using a screw. As the extruder using a screw, a single screw extruder or a twin screw extruder may be used. The screw rotation direction of the twin screw extruder may be the same or different. The heating temperature in the melt-kneading section may be equal to or higher than the temperature at which the polystyrene resin melts, and is preferably about 150°C to 260°C from the viewpoint of suppressing deterioration of the resin. The melt-kneading time may be appropriately set according to the type of polystyrene resin and the extrusion amount per unit time.

[0054] In the melt kneading step, a foaming agent is mixed (pressed) into the resin composition under high pressure conditions to prepare a foamable molten composition. The timing of mixing the foaming agent is not particularly limited, and the foaming agent may be mixed at any stage of the melt kneading step, such as before the resin composition is heated and melted, during the resin composition is heated and melted, or after the resin composition is heated and melted. The pressure at which the foaming agent is pressed into the resin composition may be higher than the internal pressure of the melt kneading section.

[0055] In the melt-kneading step, in addition to the polystyrene resin, additives, and foaming agent, the acid neutralizer is blended into the resin composition. The blending method and timing of the acid neutralizer are not particularly limited, and the acid neutralizer may be dry-blended before the resin composition is heated and melted, or the acid neutralizer may be mixed into the melt during or after the resin composition is heated and melted. The timing of mixing the acid neutralizer may be before the foaming agent is pressed in, at the same time as the foaming agent is pressed in, or after the foaming agent is pressed in.

[0056] In a preferred embodiment, an acid neutralizer is dissolved in water as a blowing agent to prepare an aqueous solution in advance, and the aqueous solution of the acid neutralizer is injected into the resin composition as a blowing agent. In this method, whether the alkyl chloride and water as a blowing agent are injected simultaneously, or the alkyl chloride and water are injected separately at different stages, the acid neutralizer is already dissolved in water at the stage of mixing the alkyl chloride and water, so that the generation of corrosive gas due to the reaction between the alkyl chloride and water can be efficiently suppressed.

[0057] When the acid neutralizer is used as an aqueous solution, the concentration of the acid neutralizer in the aqueous solution may be appropriately adjusted taking into consideration the amount of water added to the composition as a foaming agent and the amount of the acid neutralizer added. The concentration of the acid neutralizer in the aqueous solution is, for example, about 0.1 to 30% by weight, and may be 0.5 to 20% by weight, 1 to 15% by weight, or 2 to 10% by weight.

[0058] In the melt-kneading step, the resin composition and the foaming agent are melt-kneaded, and then the foamable molten composition to be supplied to the foaming step may be cooled within a temperature range in which the composition does not solidify. For example, the composition may be cooled in a cooling section disposed between the melt-kneading section and the foam molding section. When the composition is cooled, the temperature of the composition at the outlet of the cooling section is preferably 105°C to 140°C, and may be 110°C to 130°C.

[0059] In the foaming step, the foamable molten composition is extruded from the die of the foam molding section into a low pressure region (eg, an atmospheric pressure region), whereby the volume of the foaming agent increases rapidly to form an extruded polystyrene resin foam.

[0060] The foam molding section may be equipped with a molding plate connected to the downstream side of the die in order to foam mold the foamable molten composition extruded from the die immediately after pressure is released. The molding plate is composed of two plates, one above the other, and the composition extruded from the die slit, which is a linear opening in the die, into a low pressure region is foamed in the space between the two molding plates, thereby obtaining a plate-shaped foam having a certain thickness. The two plates, one above the other, may be arranged parallel to the extrusion direction, or may be arranged so that the gap between them gradually expands from the inlet (upstream side) to the outlet (downstream side).

[0061] The foaming pressure of the extrusion foaming (the pressure applied to the foamable melt immediately before being extruded from the die slit) is, for example, about 2.5 to 15 MPa, and may be 3 to 10 MPa, or 3.5 to 8 MPa. If the foaming pressure is 2.5 MPa or more, the foaming agent can be sufficiently dissolved in the composition, and therefore problems such as the foaming agent being ejected as a gas from the die slit can be suppressed. If the foaming pressure is 15 MPa or less, the discharge amount of the composition can be increased, and therefore productivity can be ensured. The foaming pressure can be adjusted to a desired range by adjusting the supply speed of the composition (discharge amount per unit time), the opening of the die slit, the temperature of the die slit, and the like.

[0062] [Physical properties of foam] The foam is formed, for example, in a plate shape. The thickness of the plate-shaped foam is not particularly limited and is appropriately selected depending on the application. For example, the foam obtained by the above method can be used as an insulating material for houses, buildings, and cold storages. The foam used as these insulating materials preferably has a thickness of 10 mm or more in order to impart high insulation and high compressive strength. The thickness of the foam may be 20 mm or more, 30 mm or more, 40 mm or more, 50 mm or more, or 60 mm or more. The thickness of the foam may be 150 mm or less, 130 mm or less, or 120 mm or less.

[0063] In the case of polystyrene resin extruded foam, after giving the shape by extrusion foam molding, the surface layer (skin layer) that was in contact with the mold may be removed by about 5 mm in the thickness direction to produce the final product, but the above thickness is the thickness of the foam before the skin layer is removed.

[0064] Considering the use as a building insulation material or a refrigerator insulation material, the thermal conductivity of the foam is preferably 0.0284 W / mK or less, more preferably 0.0244 W / mK or less, and may be 0.0240 W / mK or less or 0.0235 W / mK or less. As mentioned above, the composition contains an alkyl chloride as a foaming agent, so that the thermal insulation property tends to be improved (thermal conductivity becomes smaller). From the viewpoint of thermal insulation, the smaller the thermal conductivity, the better, but the thermal conductivity of the polystyrene resin extruded foam is generally 0.020 W / mK or more.

[0065] In order to achieve both light weight and strength, the apparent density of the foam is 20 to 60 kg / m 3 is preferable, and 25 to 40 kg / m 3 The apparent density of the foam is calculated from the volume and mass of a foam cut into a rectangular parallelepiped.

[0066] The closed cell ratio of the foam is preferably 90% or more, and more preferably 95% or more. The higher the closed cell ratio, the better the thermal insulation property tends to be. The closed cell diameter of the foam is calculated by the true volume V1 of the foam (the apparent volume minus the volume of the non-closed cell portion), the apparent volume V2 of the foam, the mass W of the foam, and the true density ρ (approximately 1.05 g / cm in the case of polystyrene resin). 3 ) is calculated based on the following formula: Closed cell ratio (%)=100×(V1-W / ρ) / (V2-W / ρ)

[0067] The average cell diameter of the foam is preferably 0.05 to 0.5 mm, and may be 0.07 to 0.4 mm or 0.1 to 0.3 mm. If the average cell diameter is too small, the distance between the cell walls of the foam is small, so that the range of movement of the cells during foam molding is narrow, making deformation difficult, and it tends to be difficult to impart a beautiful surface to the extruded foam or to increase the thickness of the foam. On the other hand, if the average cell diameter is large, the heat insulating property tends to decrease.

[0068] When the expansion ratio is large (e.g., 20 times or more) and the closed cell ratio is large as described above, the thickness of the cell wall is negligibly small compared to the cell diameter, so the average cell diameter can be roughly calculated from the number of cells per unit length. The average cell diameter of a foam is a value calculated based on the following formula by drawing three straight lines 2 mm long in the thickness direction at any point on the enlarged cross-sectional image of the foam, and using the number a of cells that intersect or come into contact with the straight lines. Average bubble diameter = 2 × 3 / a

[0069] As described above, in the present invention, by using alkyl chloride and water as a blowing agent, it is possible to provide an extruded polystyrene resin foam having high heat insulation, large thickness, and beautiful surface. In addition, by containing a predetermined amount of acid neutralizer in the composition used for preparing the foam, it is possible to suppress the generation and diffusion of corrosive gases caused by the reaction between alkyl chloride and water, and to prevent deterioration of equipment. As shown in the following examples, even when an acid neutralizer is added, the above-mentioned features are maintained, so that the foam obtained by the present invention can be suitably used as an insulating material for houses, buildings, refrigerators, etc. EXAMPLES

[0070] The following examples are provided to further explain the present invention, but the present invention is not limited to these examples.

[0071] [Preparation of graphite master batch] 48 parts by weight of polystyrene resin A (PS Japan "PSJ-Polystyrene GPPS 680", MFR: 7.0g / 10min), 50 parts by weight of graphite (Marutoyo Foundry Manufacturing "M-885"; flake graphite, average particle size 5.5μm, fixed carbon content 89%), and 2 parts by weight of stearic acid monoglyceride (Rikemal S-100P, Riken Vitamin) were charged into a Banbury mixer and melt-kneaded for 20 minutes without heating or cooling under a pressure of 0.49MPa. The resin temperature during kneading was 190°C. The kneaded product was fed into a ruder, and the strand-shaped resin extruded through a die attached to the tip of the ruder at a discharge rate of 250kg / hr was cooled and solidified in a water bath at 30°C, and then cut to obtain a graphite masterbatch.

[0072] [Preparation of resin mixture] Resin mixtures 1 to 4 (hereinafter referred to as "GP1", "GP2", "GP3", and "GP4") were prepared by dry blending polystyrene resin, the above graphite master batch, flame retardant, flame retardant assistant, lubricant, flame retardant, flame retardant assistant, cell size regulator, stabilizer, lubricant, and absorbent in the formulation shown in Table 1. The amount of graphite master batch was 5 parts by weight per 97.6 parts by weight of polystyrene resin B (PS Japan "PSJ-Polystyrene GPPS G9401", MFR: 2.1g / 10min) and styrene-methacrylic acid copolymer (PS Japan "PSJ-Polystyrene G9001", methacrylic acid content: 8% by weight, MFR: 1.5g / 10min).

[0073] Polystyrene resin A, graphite, and stearic acid monoglyceride in Table 1 are components derived from the graphite master batch. The amount of each component in Table 1 is the blending amount (parts by weight) relative to a total of 100 parts by weight of the polystyrene resin.

[0074] [Table 1]

[0075] [Example 1] Extrusion foam molding was performed using a manufacturing apparatus equipped with an extruder in which a first extruder (single-screw extruder, aperture 150 mm), a second extruder (single-screw extruder, aperture 200 mm), a cooler, and a slit die (mouthpiece gap 5 mm) were connected in series in this order, two upper and lower molding plates connected downstream of the slit die of the extruder, and a molding roll located downstream of the molding plates.

[0076] GP1 was fed from the raw material feeder to the first extruder at 800 kg / hr, melt-kneaded in the first extruder at a temperature of 250 ° C., and the amount of foaming agent shown in Table 2 was injected near the downstream end of the first extruder. Thereafter, the composition was cooled while being kneaded in the second extruder connected to the first extruder, and further cooled to the foaming temperature shown in Table 2 in a cooler connected to the second extruder. The cooled composition was entered into a die slit, extruded from the die slit into the atmosphere at a foaming pressure of 4 MPa, and foamed. The composition was molded into a plate by passing through a molding plate and a molding roll in sequence, to obtain a plate-shaped extruded foam having a cross section of 60 mm thick and 1000 mm wide.

[0077] [Examples 2 to 7, Comparative Examples 1 to 4] The type of resin mixture, the type and amount of foaming agent, and the foaming temperature were changed as shown in Table 2. Except for that, extrusion foam molding was carried out in the same manner as in Example 1 to obtain an extruded foam.

[0078] Details of the foaming agents shown in Table 2 are as follows: In Examples 1 to 7 and Comparative Example 2, an aqueous solution of sodium hydrogen carbonate prepared to a predetermined concentration by dissolving sodium carbonate in water was used. Ethyl chloride: Nippon Specialty Chemical Industry Co., Ltd. Water: Tap water from Settsu City, Osaka Prefecture HFO-1234ze: 1,3,3,3-tetrafluoropropene, manufactured by Honeywell Japan HCFO-1233zd: 1-chloro-3,3,3-trifluoropropene, manufactured by Honeywell Japan Dimethyl ether: Iwatani Corporation Isobutane: Mitsui Chemicals Normal butane: Iwatani Corporation

[0079] [Corrosion test using foaming agent] A mixture having the same composition as the foaming agent used in Examples 1 to 7 and Comparative Examples 1 to 4 was sealed in a stainless steel pressure vessel together with a pre-weighed iron piece (approximately 320 mg) measuring 2 cm square and 0.1 mm thick. The pressure vessel was heated at 140°C for 5 hours, after which the iron piece was removed, its appearance was observed, its weight was measured, and its corrosiveness was evaluated according to the following criteria. A: The weight loss of the iron piece is less than 1 mg, and there is no change in the appearance of the iron piece. B: The weight of the iron piece has decreased by 1 mg or more but less than 10 mg, and there is no change in the appearance of the iron piece. C: The weight of the iron piece has decreased by 10 mg or more, or discoloration of the iron piece has been observed.

[0080] [Evaluation of foam] <Residual amount of foaming agent> The foam (without scraping off the surface layer (skin layer) that had been in contact with the mold) was left to stand for one week in standard atmosphere class 3 (temperature 23±5°C, relative humidity 40-70%) of JIS K 7100:1999 to condition it, and then about 1.2g of sample was cut out from the center in the width direction and thickness direction, placed in a sealable glass container with a capacity of about 130cc, and the air in the container was removed using a vacuum pump. The container was then heated at 170°C for 10 minutes, and the foaming agent in the foam was taken out into the container. After cooling to room temperature, helium was introduced into the container to return it to atmospheric pressure, and 40μL of gas was collected using a microsyringe, and gas chromatography analysis was performed under the following conditions, and the remaining amount of the foaming agent (ethyl chloride, HFO-1234ze, HCFO-1234zd, isobutane, and normal butane) in the foam was determined based on a calibration curve created in advance.

[0081] Equipment used: Shimadzu Gas Chromatograph GC-2014 Column: Chemicals Evaluation and Research Institute "G-Column G-950 25UM" Inlet temperature: 65℃ Column temperature: 80℃ Detector temperature: 100℃ Carry gas: High purity helium Carry gas flow rate: 30mL / min Detector:TCD Current: 120mA

[0082] <Apparent density> A rectangular specimen measuring 100 mm wide x 100 mm long was cut from the center of the width of the foam (without the skin layer scraped off). The apparent density (mass / volume) was calculated from the apparent volume calculated from the outer dimensions of the specimen measured using a caliper (Mitutoyo, M-type standard caliper N30) and the mass of the specimen.

[0083] <Independent bubble diameter> Test pieces measuring 40 mm thick × 25 mm long × 25 mm wide were cut out from three locations, namely, the central portion A in the width direction of the foam, and points B and C 150 mm from each end in the width direction, and the closed cell ratio of each sample was determined, and the average closed cell ratio of the three test pieces was calculated. The closed cell ratio was calculated by calculating the true volume V1 (apparent volume minus the volume of the portion that is not closed cell) of the test piece measured using an air comparison specific gravity meter (Tokyo Science Model 1000) according to procedure C of ASTM-D2856-70, the apparent volume V2 calculated from the outer dimensions of the test piece measured using a vernier caliper, the mass W of the test piece, and the true density ρ of the test piece (density of polystyrene resin, 1.05 g / cm 3 The calculation was based on the following formula: Closed cell ratio (%)=100×(V1-W / ρ) / (V2-W / ρ)

[0084] <Average bubble diameter> Similar to the evaluation of the above-mentioned independent bubble diameter, test pieces were cut out from three locations A, B, and C in the width direction, and 100-times magnified photographs of the cross-sections in the width direction and the cross-sections in the length direction of each test piece were taken using a microscope (Keyence's "DIGITAL MICROSCOPE VHX-900"). At an arbitrary location of each magnified photograph, three straight lines with a length of 2 mm in the thickness direction were drawn, and the total number a of bubbles intersecting or touching the three straight lines was obtained. The average bubble diameter in the thickness direction (= 2×3 / a) in the cross-section was calculated. The average value of the average bubble diameters in the thickness direction obtained from each of the six cross-section magnified photographs (two cross-section magnified photographs were taken for each of the three test pieces) was taken as the average bubble diameter of the foam.

[0085] <Thermal conductivity> In accordance with JIS A 9521:2017, a test piece with a thickness of 50 mm × length (extrusion direction) of 300 mm × width of 300 mm was cut out from the central part in the width direction of the foam immediately after production, and was left standing in the standard atmosphere class 3 of JIS K 7100:1999 for one week for conditioning. In an environment with an average temperature of 23°C, the thermal conductivity of the conditioned test piece was measured using a thermal conductivity measuring device (Eihiro Seiki's "HC-074").

[0086] <JIS flammability> In accordance with JIS A 9521:2017, a test piece with a thickness of 10 mm × length (extrusion direction) of 200 mm × width of 25 mm was cut out from the central part in the width direction of the foam immediately after production, and was left standing in the standard atmosphere class 3 of JIS K 7100:1999 for one week for conditioning. When the flammability of the conditioned sample was evaluated, the samples of Examples 1 to 7 and Comparative Examples 1 to 4 all met the criterion of "the flame goes out within 3 seconds, there is no remaining char, and it does not burn beyond the combustion limit indication line".

[0087] <Appearance> The appearance of the foam without the skin layer scraped off (before cutting) and the foam with the skin layer on both the top and bottom sides removed by 5 mm in the thickness direction (after cutting) was visually evaluated. In all of the samples of Examples 1 to 7 and Comparative Examples 1 to 4, the foam before cutting was not corrugated and was plate-like, and no surface abnormalities such as flow marks or scratches were observed either before or after cutting, and the foam had a good appearance.

[0088] Table 2 shows the type of resin mixture used in each Example and Comparative Example, the amount of foaming agent injected (weight relative to 100 parts by weight of polystyrene resin and molar amount per 1 kg of foam), the evaluation results of corrosiveness due to the foaming agent, the foaming temperature, and the evaluation results of the foam. Although sodium carbonate does not act as a foaming agent, Table 2 shows the amount of sodium carbonate contained in the sodium carbonate aqueous solution. The molar ratio of sodium carbonate to ethyl chloride is also shown.

[0089] [Table 2]

[0090] The foams of Examples 1 to 3 and Comparative Examples 1 and 2 using GP1 as the resin mixture had almost the same characteristics, regardless of the concentration of sodium carbonate dissolved in water as a foaming agent or the amount of sodium carbonate aqueous solution injected, and achieved both excellent appearance and heat insulation. In Examples 1 to 3, in which the foaming agent contains sodium carbonate as a neutralizing agent, the metal corrosiveness caused by the foaming agent was low, whereas in Comparative Example 1, in which the foaming agent does not contain sodium carbonate, metal corrosion caused by the foaming agent was observed. In Comparative Example 2, in which the amount of sodium carbonate was small, metal corrosion caused by the foaming agent was observed similarly to Comparative Example 1. From the comparison between Examples 1 to 3 and Comparative Examples 1 and 2, it can be seen that the larger the molar ratio of the acid neutralizing agent to the alkyl chloride in the foaming agent, the more the metal corrosion caused by the foaming agent tends to be suppressed.

[0091] Comparison of Example 4 using GP2 as the resin mixture with Comparative Example 3, and comparison of Examples 5 and 6 using GP3 as the resin mixture with Comparative Example 4, shows that by including sodium carbonate as an acid neutralizer in the foaming agent, it is possible to obtain a foam that has both excellent appearance and heat insulation, while suppressing metal corrosion caused by the foaming agent, just like when no acid neutralizer is used. The foam obtained in Example 7 using GP4 as the resin mixture also had excellent appearance and heat insulation.

Claims

1. A method for producing an extruded polystyrene-based resin foam, comprising melt-kneading a composition containing a polystyrene-based resin and a foaming agent, and extruding the composition in a low pressure region to form an extrusion molded product, comprising the steps of: The blowing agent includes at least an alkyl chloride and water; The composition further comprises an acid neutralizing agent; In the composition, the amount of the acid neutralizer relative to the alkyl chloride is 0.003 times or more in terms of molar ratio. A method for producing an extruded polystyrene resin foam.

2. The method for producing an extruded polystyrene resin foam according to claim 1 , wherein the acid neutralizing agent is an alkali metal salt.

3. The method for producing an extruded polystyrene resin foam according to claim 2, wherein the neutralizing agent is an alkali metal carbonate or hydrogen carbonate.

4. The method for producing an extruded polystyrene resin foam according to any one of claims 1 to 3, wherein the acid neutralizing agent is water-soluble.

5. The method for producing an extruded polystyrene resin foam according to claim 4 , wherein the acid neutralizing agent is dissolved in the water of the foaming agent, and the acid neutralizing agent is mixed with the polystyrene resin and melt-kneaded.

6. The method for producing an extruded polystyrene resin foam according to any one of claims 1 to 3, wherein the amount of the acid neutralizer in the composition is 0.02 parts by weight or more per 100 parts by weight of the polystyrene resin.

7. The method for producing an extruded polystyrene resin foam according to any one of claims 1 to 3, wherein the amount of alkyl chloride in the composition is 1 to 8 parts by weight per 100 parts by weight of the polystyrene resin.

8. The method for producing an extruded polystyrene resin foam according to any one of claims 1 to 3, wherein the foam has a thermal conductivity of 0.0284 W / mK or less.

9. The method for producing an extruded polystyrene resin foam according to any one of claims 1 to 3, wherein the foam has a thickness of 10 mm or more.

Citation Information

Patent Citations

  • Styrenic resin extrusion foaming product and its production method

    JP2005330351A

  • Styrenic resin extrusion foamed body and manufacturing method thereof

    JP2019108416A

  • Styrenic resin extrusion expanded material

    JP2019189811A

Cited By

  • Polystyrene resin extruded foam and method for producing the same

    JP2026165276A