Production method of cement clinker and cement production method using the same
By using aluminum-containing and alkali-rich raw materials with no thermal history to form a protective clinker coating on kiln bricks, the method addresses brick wear and tear issues, improving cement clinker production efficiency and quality.
Patent Information
- Application Number
- JP2023053143
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods for producing cement clinker fail to adequately suppress wear and tear of bricks in the firing zone of rotary kilns, leading to inefficiencies in cement production.
Incorporating cement raw materials with a high content of aluminum-containing components and no thermal history, along with specific alkali components, to form a thick clinker coating layer on the bricks during the firing process, thereby reducing heat transmission and extending brick replacement intervals.
The method effectively suppresses brick wear and tear, enhancing the efficiency and quality of cement clinker production by maintaining the integrity of the kiln bricks.
Smart Images

Figure 2024141467000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing cement clinker and a method for producing cement using the same. [Background technology]
[0002] Cement clinker is produced by introducing cement raw materials into a rotary kiln, which has bricks inside a cylindrical steel shell, and burning the raw cement raw materials. At this time, the cement raw materials are burned at high temperatures of 1450°C or higher, which can cause the bricks to be worn down. When the bricks are worn down, they become thinner, and the cylindrical shell around the bricks can be heated and melted. Therefore, various proposals have been made to avoid such a situation.
[0003] For example, Patent Document 1 listed below proposes providing an injection pipe adjacent to the main burner and injecting a powder with a chemical composition that is likely to produce a coating toward the inner wall of the shell in a range of 0 to 5 m from the downstream end of the rotary kiln toward the upstream side, thereby producing a coating that effectively protects the bricks in the range from the firing zone exit to the cooling zone, without increasing NOx in the exhaust gas or increasing the energy consumption rate, thereby preventing thermal damage to the bricks. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-7925 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the method for producing cement clinker described in Patent Document 1 above has the following problems.
[0006] That is, the method for producing cement clinker described in Patent Document 1 above still has room for improvement in terms of suppressing wear of bricks in the firing zone.
[0007] An object of the present disclosure is to provide a method for producing cement clinker that can suppress wear of bricks in a firing zone, and a method for producing cement using the same. [Means for solving the problem]
[0008] The inventors of the present disclosure have conducted intensive research to solve the above problems. As a result, the inventors of the present disclosure have come to the conclusion that a coating layer may be effectively formed in the calcination zone by including raw materials with no thermal history in the cement raw materials introduced into the rotary kiln. Then, the inventors of the present disclosure have conducted further intensive research and have found that the above problems can be solved by the following disclosure.
[0009] That is, one aspect of the present disclosure provides a method for producing cement clinker, including a cement raw material introducing step of introducing a cement raw material into a rotary kiln having bricks arranged inside a cylindrical shell, and a firing step of obtaining a fired body by firing the cement raw material, wherein the cement raw material introducing step includes a first step of introducing the cement raw material into the rotary kiln such that a content of a first raw material that contains an aluminum-containing component and has no thermal history is 7 mass% or more. According to the above-mentioned method for producing cement clinker, the cement raw material introduction step includes a first step of introducing the cement raw materials into the rotary kiln such that the content of the first raw material, which contains an aluminum-containing component and has no thermal history, is 7% by mass or more. This makes it easier for a thick clinker coating layer to be formed on the bricks in the firing zone where the fired body is formed when the cement raw materials are fired in the firing step. Therefore, even if the inside of the rotary kiln becomes hot, the clinker coating layer makes it difficult for the heat to be transmitted to the bricks, and wear of the bricks due to heat is suppressed. This eliminates the need to replace bricks for a long period of time, improving the production efficiency of cement clinker.
[0010] In the above method for producing cement clinker, it is preferable that the content of the alkali component in the first raw material is 1.0 mass % or more. When the content of the alkali component in the first raw material is 1.0% by mass or more, the clinker coating layer is more likely to adhere to the bricks, and the clinker coating layer can be more easily formed thickly.
[0011] In the above-mentioned method for producing cement clinker, it is preferable that the cement raw material introduction step further includes, after the first step, a second step of introducing the cement raw material into the rotary kiln such that a content of the first raw material is less than 7 mass%. In this case, since a thick clinker coating layer has already been formed on the inside of the rotary kiln in the first step to protect the bricks, the objective of protecting the bricks can be achieved even if the content of the first raw material in the cement raw materials becomes less than 7 mass% in the second step. In addition, there is a tendency for the quality of the cement clinker to be further improved.
[0012] In the above-mentioned method for producing cement clinker, the first raw material may be construction waste soil.
[0013] Another aspect of the present disclosure provides a method for producing cement, comprising the step of producing cement clinker by the method for producing cement clinker described above. According to the above-mentioned method for producing cement, wear of bricks in the firing zone can be suppressed, and therefore the production efficiency of cement clinker can be improved, thereby improving the production efficiency of cement. Effect of the Invention
[0014] According to the present disclosure, there is provided a method for producing cement clinker that can suppress wear of bricks in a firing zone, and a method for producing cement using the same. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic diagram showing a main part of a cement clinker production facility used in a cement clinker production method according to the present disclosure. [Diagram 2] 4 is a graph showing the relationship between the thickness of the coating layer in Example 1 and the distance from the downstream end face of the rotary kiln. [Diagram 3] 4 is a graph showing the relationship between the thickness of the coating layer in Comparative Example 1 and the distance from the downstream end face of the rotary kiln. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, embodiments of the present disclosure will be described in detail.
[0017] <Manufacturing method of cement clinker> First, an embodiment of the method for producing cement clinker according to the present disclosure will be described with reference to Fig. 1. Fig. 1 is a schematic diagram showing the main parts of a cement clinker production facility used in the method for producing cement clinker according to the present disclosure.
[0018] The cement clinker production facility 100 shown in FIG. 1 includes a rotary kiln 10 and a burner 20 as main components.
[0019] The rotary kiln 10 comprises a cylindrical shell 11 and bricks 12 provided inside the cylindrical shell 11. The central axis C of the shell 11 is inclined with respect to the horizontal plane, and the rotary kiln 10 is rotatable about the central axis C of the cylindrical shell 11. The bricks 12 are laid so as to cover the entire inner surface of the shell 11 in order to protect the shell 11.
[0020] The tip of the burner 20 may be disposed at a position coinciding with the downstream end face of the rotary kiln 10 as shown in Fig. 1, but may also be disposed inside the rotary kiln 10. Reference numeral 21 denotes a flame ejected from the tip of the burner 20.
[0021] The method for producing cement clinker in this embodiment includes a cement raw material introduction step of introducing the cement raw material into the rotary kiln 10, and a firing step of firing the cement raw material by ejecting a flame 21 formed by a burner 20 to the upstream side of the rotary kiln 10 while rotating the rotary kiln 10 about the central axis C of the shell 11, thereby obtaining a fired body. Here, the cement raw material introduction step includes a first step of introducing the cement raw material into the rotary kiln 10 such that the content of the first raw material, which contains an aluminum-containing component and has no thermal history, is 7 mass% or more. The method for producing cement clinker may further include a cooling step of cooling the fired body obtained in the firing step to obtain cement clinker.
[0022] According to the above-mentioned method for producing cement clinker, the cement raw material introduction step includes a first step of introducing the cement raw materials into the rotary kiln 10 such that the content of the first raw material containing an aluminum-containing component and having no thermal history is 7% by mass or more. This makes it easier for a thick coating layer 30 to be formed on the bricks 12 in the firing zone where the fired body is formed when the cement raw materials are fired in the firing step. Therefore, even if the inside of the rotary kiln 10 becomes hot, the heat is not easily transferred to the bricks 12 by the coating layer 30, and wear of the bricks 12 due to heat is suppressed. This eliminates the need to replace the bricks 12 for a long period of time, improving the production efficiency of the cement clinker.
[0023] Next, the cement clinker production facility 100, the cement raw material introduction step, and the burning step will be described in detail.
[0024] (Cement clinker manufacturing facility) The material from which the shell 11 of the rotary kiln 10 is made is not particularly limited, but is typically made of steel. As the bricks 12, firebricks are usually used.
[0025] The burner 20 is disposed so as to be substantially coaxial with the central axis C of the shell 11, and is adapted to eject a flame 21 from its tip when fuel is supplied thereto.
[0026] The manufacturing equipment 100 may further include a cement raw material introduction section (not shown) connected to the upstream end of the rotary kiln 10, and a fired body receiving section (not shown) connected to the downstream end of the rotary kiln 10. The cement raw material introduction section is a container that stores the cement raw material to be introduced into the rotary kiln 10. A preheater that preheats the cement raw material before it is introduced into the rotary kiln 10 may be installed in the cement raw material introduction section. The fired body receiving section is a container that receives the fired body discharged from the rotary kiln 10. A burner 20 is installed in the fired body receiving section. A cooler that cools the fired body may also be installed in the fired body receiving section.
[0027] (Cement raw material introduction process) The cement raw material introduction step includes a first step of introducing the cement raw material into the rotary kiln 10 so that the content of the first raw material, which contains an aluminum-containing component and has no thermal history, is 7 mass % or more.
[0028] Regarding the first raw material, "no thermal history" means that when the first raw material is heated from room temperature to 1000°C using a thermogravimetric differential thermal analyzer (TG-DTA) and held at 1000°C for one hour, no heat generation due to the combustion of unburned carbon, etc. is observed and the weight change is 2.0% by mass or more. Note that whether or not heat generation due to the combustion of unburned carbon, etc. is observed can be determined by the presence or absence of an exothermic peak in the DTA curve.
[0029] The aluminum-containing component in the first raw material is a component that contains aluminum, and examples of the aluminum-containing component include clay minerals.
[0030] The content of the aluminum component (Al2O3 component) in the first raw material is not particularly limited, but may be, for example, 10 mass% or more, or 13 mass% or more. The content of the aluminum component in the first raw material may be, for example, 20 mass% or less, or 17 mass% or less.
[0031] The content of the first raw material in the cement raw material may be 7% by mass or more, and may be 8% by mass or more, 10% by mass or more, or 15% by mass or more. The content of the first raw material in the cement raw material may be 25% by mass or less, or may be 20% by mass or less.
[0032] The content of the first raw material in the cement raw materials can be adjusted by changing the mixing ratio of the first raw material without thermal history and the second raw material with thermal history. The second raw material is not particularly limited as long as it is a raw material with a thermal history, and examples of the second raw material include coal ash and slag. These can be used alone or in combination of two or more.
[0033] The first raw material may further contain an alkali component (R2O component) in addition to the aluminum component. Examples of the alkali component include K2O and Na2O. The content of the alkali component (R2O component) in the first raw material is not particularly limited, but is preferably 1.0 mass% or more, and more preferably 2.0 mass% or more. When the content of the alkali component in the first raw material is 1.0 mass% or more, the coating layer 30 is easily attached to the brick 12, and the coating layer 30 can be easily formed thick. The content of the alkaline component in the first raw material may be 5.0% by mass or less, or 3.0% by mass or less. The content of the alkali component (R2O component) in the first raw material is calculated by the following formula. R2O = Na2O + 0.658 × K2O (In the above formula, RO represents the content (mass%) of the alkali component (RO component) in the first raw material, NaO represents the content (mass%) of sodium oxide in the first raw material, and KO represents the content (mass%) of potassium oxide in the first raw material.)
[0034] Examples of the first raw material that has no thermal history include construction waste soil, construction sludge, and purified water cake generated at a water purification plant.
[0035] The cement raw material introduction step may be composed of only the first step, or may further include a second step after the first step in which the first raw material is introduced into the rotary kiln 10 so that the content R2 of the first raw material is less than 7 mass%, but it is preferable to further include the second step after the first step. In this case, since the coating layer 30 has already been formed thickly on the inside of the rotary kiln 10 in the first step to protect the bricks 12, the purpose of protecting the bricks 12 can be achieved even if R2 is less than 7 mass%. In addition, there is a tendency that the quality of the cement clinker can be further improved.
[0036] When R2 is less than 7 mass%, R2 may be 2 mass% or more, or 3 mass% or more, and may be 5 mass% or less, or 4 mass% or less.
[0037] The cement raw materials are generally preheated before being introduced into the rotary kiln 10, but do not necessarily have to be preheated.
[0038] (Firing process) In the firing process, the cement raw materials are fired. The cement raw materials can be fired by heating them at a high temperature of 1450°C or higher using a burner 20. In this firing process, the cement raw materials undergo gradual chemical changes, becoming cement clinker, which is a collection of hydraulic compounds. In the firing process, a coating layer 30, which is a molten cement clinker, is also produced, and this coating layer 30 covers the bricks 12 in the firing zone, gradually increasing in thickness. As a result, wear of the bricks 12 due to the heat from the flame 21 from the burner 20 is suppressed. This coating layer 30 is more likely to be produced in areas with higher temperatures, and therefore tends to be thicker in areas with higher temperatures. The firing zone depends on the size of the flame 21, but is usually a region of about 3 to 20 m from the downstream end face of the shell 11 toward the upstream side in the rotary kiln 10.
[0039] In the firing step, the rotation speed of the rotary kiln 10 is not particularly limited, but may be, for example, 1 to 3 rpm. The flame 21 of the burner 20 is adjusted so as to heat the cement raw materials to a high temperature of 1450° C. or more.
[0040] <Cement manufacturing method> A method for producing cement according to another aspect of the present disclosure includes a clinker production step of producing cement clinker by the above-mentioned method for producing cement clinker.
[0041] According to the above-mentioned method for producing cement, wear of the bricks 12 in the firing zone can be suppressed, and therefore the production efficiency of cement clinker can be improved, thereby improving the production efficiency of cement.
[0042] The method for producing cement may further include a grinding step of grinding the cement clinker to obtain cement after the clinker production step. In the above-mentioned grinding process, the cement clinker is mixed with gypsum and other additives, and then finely ground to form cement. The grinding is carried out by a finishing mill etc. Specifically, balls, cement clinker, gypsum, etc. are ground in a cylindrical drum while colliding with each other due to the rotation of the drum.
[0043] The outline of this disclosure is as follows. [1] A method for producing cement clinker, comprising: a step of introducing a cement raw material into a rotary kiln having a cylindrical shell with bricks on the inside; and a step of calcining the cement raw material to obtain a calcined body, The cement raw material introduction step includes: The method includes a first step of introducing the cement raw material into the rotary kiln so that a content of the first raw material having no heat history is 7% by mass or more; The method for producing cement clinker, wherein the first raw material contains aluminum. [2] The method for producing cement clinker according to [1], wherein the content of the alkali component in the first raw material is 1.0 mass% or more. [3] The method for producing cement clinker according to [1] or [2], wherein the cement raw material introduction step further includes a second step of introducing the cement raw materials into the rotary kiln after the first step so that the content of the first raw material is less than 7 mass%. [4] The method for producing cement clinker according to any one of [1] to [3], wherein the first raw material is construction waste soil. [5] A method for producing cement, comprising a step of producing cement clinker by the method for producing cement clinker according to any one of [1] to [4]. EXAMPLES
[0044] The contents of the present disclosure will be described more specifically below with reference to examples, but the present disclosure is not limited to the following examples.
[0045] Example 1 A cement raw material was prepared by mixing the first raw material without thermal history with the second raw material with thermal history so that the content of the first raw material was 7 mass%. The first raw material was prepared by mixing brand 1A and brand 1B shown in Table 1 in a ratio of 1:1 (mass ratio). The contents of the aluminum component (Al2O3) and the alkali component (R2O) in the first raw material were 16.45 mass% and 2.63 mass%, respectively. On the other hand, the second raw material was used by mixing brands 2A, 2B, 2C, 2D, and 2E shown in Table 2 in a ratio of 1:1:1:1:1 (mass ratio). Table 1 shows the compositions (contents of chemical components) of grades 1A and 1B, with the units of values being mass %. Grade 1A is construction generated soil, and grade 1B is construction sludge. Table 2 shows the compositions (contents of chemical components) of brands 2A to 2E. The contents of chemical components are values measured with coal ash (hereinafter also referred to as "dry ash") obtained by drying incoming coal ash at 40°C as the standard (100% by mass). The units of values are % by mass. Brands 2A to 2E are coal ash or sludge ash. In Table 2, the moisture content is the moisture content obtained by drying the incoming coal ash at 40°C, and the moisture content value is the content measured based on the total mass of the incoming coal ash (100% by mass). The unit of values is mass%, and blank spaces indicate 0% by mass. Unburned C (carbon) is unburned C contained in dry ash, and the value of unburned C is the content measured separately from the chemical components, with the total mass of brands 2A to 2E (dry ash) as the standard (100 mass%). The unit of the value is mass%, and a blank space indicates 0 mass%.
[0046] The cement raw material obtained as described above was preheated to about 1000°C, and then introduced into a rotary kiln 10 of a cement clinker manufacturing facility 100, where the cement raw material was fired to obtain a fired body. The fired body was then cooled to obtain cement clinker. At this time, the configuration of the cement clinker production equipment and the burning conditions were as follows. (Configuration of cement clinker manufacturing facilities) Material of the shell 11 of the rotary kiln 10: steel Thickness of shell 11 of rotary kiln 10: 3~10cm Length of shell 11 of rotary kiln 10: 99.8m Bricks: 23cm thick firebricks (manufactured by Yotai Co., Ltd., Shinagawa Refractories Co., Ltd., etc.) Position of the tip of the burner 20: 0.05 m upstream from the downstream end face of the shell 11 (Firing conditions) Rotary kiln speed: 1.9 rpm Maximum temperature inside rotary kiln 10: 1,300~1,400℃
[0047] After 5 days had elapsed since the cement clinker was obtained as described above, the content of the first raw material in the cement raw materials introduced into the rotary kiln was reduced to 3 mass%, and the production of cement clinker was continued for 165 days.
[0048] In this manner, cement clinker was produced.
[0049] Comparative Example 1 A first raw material with no thermal history was mixed with a second raw material with a thermal history so that the content of the first raw material was 3 mass % to prepare a cement raw material. The contents of the aluminum component (Al2O3) and the alkali component (R2O) in the first raw material were set to 16.45 mass % and 2.63 mass %, respectively, the same as in Example 1. The second raw material was used by mixing brands 2F, 2G, 2H, and 2I shown in Table 3 in a ratio of 1:1:1:1 (mass ratio). Except for this, the content of the first raw material in the cement raw material was not changed during the process, and cement clinker was obtained in the same manner as in Example 1. Table 3 shows the compositions (contents of chemical components) of brands 2F to 2I, and the contents of chemical components are values measured with coal ash (dry ash) obtained by drying incoming coal ash at 40°C as the standard (100% by mass), and the units of values are mass%. Brands 2F to 2I are coal ash or sludge ash. In Table 3, the moisture content is the moisture content obtained by drying the incoming coal ash at 40°C, and the moisture content value is the content measured based on the total mass of the incoming coal ash (100% by mass). The unit of values is mass%, and blank spaces indicate 0% by mass. Unburned C (carbon) is the unburned C contained in the dry ash, and the value of unburned C is the content measured separately from the chemical components, with the total mass of brands 2F to 2I (dry ash) as the standard (100 mass%). The unit of the value is mass%, and a blank space indicates 0 mass%.
[0050] [Table 1] [Table 2] [Table 3]
[0051] For Example 1 and Comparative Example 1, the thickness distribution of the coating layer 30 formed along the central axis C of the shell 11 inside the rotary kiln 10 was measured from the size of the coating when the coating was dismantled. The results are shown in Figures 2 and 3, respectively. Figure 2 is a graph showing the relationship between the thickness of the coating layer in Example 1 and the distance from the downstream end face of the rotary kiln, and Figure 3 is a graph showing the relationship between the thickness of the coating layer in Comparative Example 1 and the distance from the downstream end face of the rotary kiln. The horizontal axis shows the distance from the downstream end face of the rotary kiln 10 toward the upstream side.
[0052] 2 and 3, in Example 1, a coating layer was formed up to a region 45 m from the downstream end face of the rotary kiln, and the thickness of the coating layer was 250 to 300 mm in the region (calcination zone) 11 to 19 m from the downstream end face of the shell where the cement raw materials are calcined. In contrast, in Comparative Example 1, the coating layer was formed up to a region 37 m from the downstream end face of the rotary kiln, and the thickness of the coating layer in the calcination zone was 200 mm. Thus, it was found that the thickness of the coating layer in the firing zone was greater in Example 1 than in Comparative Example 1. Therefore, it is considered that when the cement raw materials are fired in the firing process, the clinker coating layer makes it difficult for high-temperature heat to be transmitted to the bricks, thereby suppressing wear of the bricks due to heat. [Explanation of symbols]
[0053] 10...rotary kiln, 11...shell, 12...brick, 20...burner, 100...cement clinker manufacturing equipment.
Claims
1. A method for producing cement clinker, comprising: a step of introducing a cement raw material into a rotary kiln having a cylindrical shell with bricks disposed inside; and a step of calcining the cement raw material to obtain a calcined body, The cement raw material introduction step includes: A method for producing cement clinker, comprising: a first step of introducing the cement raw material into the rotary kiln such that a content of a first raw material that contains an aluminum-containing component and has no thermal history is 7 mass% or more.
2. The method for producing cement clinker according to claim 1, wherein the content of the alkali component in the first raw material is 1.0 mass% or more.
3. 2. The method for producing cement clinker according to claim 1, wherein the cement raw material introduction step further comprises a second step of introducing the cement raw material into the rotary kiln after the first step so that the content of the first raw material is less than 7 mass%.
4. The method for producing cement clinker according to claim 1, wherein the first raw material is construction waste soil.
5. A method for producing cement, comprising a clinker production step of producing cement clinker by the method for producing cement clinker according to claim 1.
Citation Information
Patent Citations
Rotary kiln
JP1998029839A
Execution of brick for cement rotary kiln
JP1998182198A
Sintered substance and method of manufacturing the same
JP2006256910A
Cement admixture
JP2009234809A
Cement admixture and cement composition
JP2010037119A