Manufacturing method of polarizer plate

The method addresses structural defects and peeling issues in polarizing plate manufacturing by using a heated easy-slip film with a polyurethane and particle-based slippery layer, ensuring smooth conveyance and adhesion, thereby enhancing the quality and efficiency of the polarizing plate production process.

JP2024141468APending Publication Date: 2024-10-10SUMITOMO CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023053144
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

The existing methods for manufacturing polarizing plates face challenges in preventing structural defects in resin films due to blocking during unwinding, which can lead to issues like minute irregularities and wrinkles, and also result in the peeling of the slippery layer, causing foreign matter in the polarizing plate.

Method used

A method involving a heating process with specific temperature and guide roll configurations to soften the easy-slip film, combined with a slippery layer composed of polyurethane and particles, is used to eliminate structural defects and prevent peeling, ensuring smooth conveyance and adhesion.

Benefits of technology

This method effectively eliminates structural defects and prevents peeling of the slippery layer, resulting in a higher quality polarizing plate with reduced defects and improved manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141468000001_ABST
    Figure 2024141468000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of polarizer plate which eliminates structural defect of a resin film due to blocking and inhibiting an easy-slip film covering the surface of the resin film from being peeled.SOLUTION: A manufacturing method of polarizer plate utilizes an easy-slip film 1. The easy-slip film 1 includes a first resin film 2 and an easy-slip layer 3 covering the surface of the first resin film 2. The easy-slip film 1 unwound from a resin roll R1 is conveyed through a plurality of guide rolls in a heating oven 4. The easy-slip film 1 passing through the heating oven 4 is bonded to the surface of a polarizer film 6 via a first adhesive 5a. Atmospheric temperature in the heating oven 4 is 80°C or higher and 120°C or lower. A guide roll A of the plurality of guide rolls comes in direct contact with the surface of the easy-slip layer 3. Holding angle α between the guide roll A and the easy-slip film 1 is 80° or more and 170° or less. Arithmetic average roughness Ra of the surface of the guide roll A is 0.06 μm or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a polarizing plate. [Background technology]

[0002] Polarizing plates are used in image display devices (such as liquid crystal displays or organic EL displays) in televisions, computers, mobile phones (smartphones), smart watches, portable game consoles, and vehicle instrument panels.

[0003] In the manufacturing method of the polarizing plate, the resin film is bonded to the surface of the polarizer film via an adhesive. Before the resin film is bonded to the surface of the polarizer film, the resin film is unwound from a resin roll (cylindrical roll) made of a wound long resin film. Since the surface of the resin film is flat, the overlapping resin films in the resin roll are in close contact with each other. Due to the weight of the resin roll, long-term storage of the resin roll, heating of the resin roll, and the like, a phenomenon occurs in which the resin films in close contact with each other in the resin roll are difficult to peel off from each other. This phenomenon is called blocking. Due to blocking, structural defects occur in the resin film unwound from the resin roll. For example, structural defects of the resin film are fine irregularities formed on the surface of the resin film, wrinkles of the resin film, and the like. The structural defects of the resin film caused by blocking may be rephrased as deformation of the resin film caused by blocking.

[0004] Patent Document 1 below discloses a method of heating a resin film at 80 to 120° C. in a heating furnace before bonding the resin film to the surface of a polarizer film in order to eliminate structural defects of the resin film caused by blocking. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-205722 A Summary of the Invention [Problem to be solved by the invention]

[0006] Blocking is suppressed to some extent by covering the surface of the resin film before it is wound with a lubricating layer. For example, the lubricating layer is a layer containing a polymer such as polyurethane and a large number of particles such as silica. Due to the large number of particles contained in the lubricating layer, the surface of the lubricating layer becomes rougher than the surface of the resin film. Therefore, the resin films overlap each other in the resin roll via the lubricating layer, and direct adhesion between the resin films is suppressed. The "slippery film" described below means a laminate consisting of a long resin film and a lubricating layer covering the surface of the resin film.

[0007] It is difficult to completely prevent structural defects of the resin film caused by blocking with the easy-slip layer. Therefore, in order to eliminate structural defects of the resin film caused by blocking, it is desirable to heat the easy-slip film in a heating furnace before laminating it on the surface of the polarizer film. The easy-slip film is transported in the heating furnace using multiple guide rolls (freely rotating cylinders). However, a part of the easy-slip layer peels off from the surface of the resin film and adheres to the surface of the guide roll in the heating furnace. The fragments of the easy-slip layer that adhere to the surface of the guide roll adhere to the surface of the easy-slip film that is transported from the upstream. As a result, the fragments of the easy-slip layer are mixed into the polarizing plate as foreign matter, resulting in defects of the polarizing plate.

[0008] An object of one aspect of the present invention is to provide a method for manufacturing a polarizing plate that easily eliminates structural defects in the resin film that constitutes the polarizing plate (structural defects in the resin film due to blocking) and suppresses peeling of the easy-slip layer that covers the surface of the resin film. [Means for solving the problem]

[0009] For example, as described in the following [1] to [5], one aspect of the present invention relates to a method for producing a polarizing plate.

[0010] [1] A method for producing a polarizing plate using a polarizer film and a slippery film, comprising the steps of: The slippery film is composed of a long resin film and a slippery layer covering the surface of the resin film. The method for producing a polarizing plate includes the following steps: A heating step of conveying the lubricating film unwound from a resin roll of the lubricating film through a plurality of guide rolls installed in a heating furnace; a coating step of coating an adhesive on the surface of the slippery film that has passed through the heating furnace; a lamination step of laminating the slippery film onto a surface of the polarizer film via an adhesive; Including, The temperature of the atmosphere in the heating furnace is 80°C or higher and 120°C or lower. The plurality of guide rolls includes at least one guide roll A that is in direct contact with the surface of the slippery layer, The embrace angle between the guide roll A and the slippery film is 80° or more and 170° or less, The arithmetic mean roughness Ra of the surface of the guide roll A is 0.06 μm or less. A method for manufacturing a polarizing plate.

[0011] [2] In the lamination process, a resin film different from the resin film is laminated to the back surface of the front surface of the polarizer film via an adhesive. A method for producing the polarizing plate according to [1].

[0012] [3] The slip layer includes a polymer and a plurality of particles. The plurality of particles are at least one type of particles selected from the group consisting of inorganic particles and organic particles. A method for producing the polarizing plate according to [1] or [2].

[0013] [4] The slip layer comprises polyurethane. The method for producing a polarizing plate according to any one of [1] to [3].

[0014] [5] The arithmetic mean roughness Ra is 0.01 μm or more and 0.06 μm or less. The method for producing a polarizing plate according to any one of [1] to [4]. Effect of the Invention

[0015] According to one aspect of the present invention, there is provided a method for manufacturing a polarizing plate that easily eliminates structural defects in the resin film that constitutes the polarizing plate (structural defects in the resin film due to blocking) and suppresses peeling of the easy-slip layer covering the surface of the resin film. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic diagram illustrating a method for producing a polarizing plate according to one embodiment of the present invention. [Diagram 2] FIG. 2 shows a schematic cross-section of a slippery film and a number of guide rolls in a heating furnace, and the cross-sections of the slippery film and the number of guide rolls in FIG. 2 are parallel to the thickness direction of the slippery film and perpendicular to the rotation axis (center axis) of each guide roll. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings. In the drawings, the same components are designated by the same reference numerals. The present invention is not limited to the following embodiments.

[0018] (Outline of manufacturing method of polarizing plate) As shown in FIG. 1, the method for producing a polarizing plate according to the present embodiment uses a polarizer film 6 and a slippery film 1. As shown in FIG. 2, the slippery film 1 is composed of a long resin film (first resin film 2) and a slippery layer 3 covering one surface (main surface) of the first resin film 2. The slippery layer 3 may cover a part or the whole surface of the first resin film 2. For example, the slippery layer 3 may contain a polymer and a plurality of particles. The plurality of particles contained in the slippery layer 3 may be at least one type of particle selected from the group consisting of inorganic particles and organic particles. As shown in FIG. 1, in the method for producing a polarizing plate according to the present embodiment, a resin film (second resin film 7) other than the first resin film 2 may be used. The slippery film 1, the polarizer film 6, and the second resin film 7 are stacked to form a laminate 8. The MD (Machine Direction) in FIG. 1 and FIG. 2 is the direction in which the slippery film 1, the polarizer film 6, the second resin film 7, or the laminate 8 is transported.

[0019] The method for producing a polarizing plate includes a heating step, a coating step, and a bonding step. As shown in FIG. 1, in the heating step, the lubricating film 1 unwound from a resin roll R1 made of a wound lubricating film 1 is transported through a plurality of guide rolls (g1, g2, g3, g4, and g5) installed in a heating furnace 4. That is, the lubricating film 1 is transported in the heating furnace 4 while the surface of the first resin film 2 or the lubricating layer 3 constituting the lubricating film 1 contacts the surfaces of the first guide roll g1, the second guide roll g2, the third guide roll g3, the fourth guide roll g4, ​​and the fifth guide roll g5 in this order. However, the number of guide rolls installed in the heating furnace 4 is not limited to five.

[0020] The temperature of the atmosphere in the heating furnace 4 is 80°C or more and 120°C or less. Since the temperature of the atmosphere in the heating furnace 4 is 80°C or more and 120°C or less, the slippery film 1 is moderately softened, and structural defects of the slippery film 1 (first resin film 2 and slippery layer 3) caused by blocking are easily eliminated. That is, in the heating furnace 4, the surfaces of the first resin film 2 and the slippery layer 3 constituting the slippery film 1 are flattened. If the temperature of the atmosphere in the heating furnace 4 is lower than 80°C, the slippery film 1 is not softened sufficiently, and structural defects of the slippery film 1 caused by blocking are difficult to eliminate. If the temperature of the atmosphere in the heating furnace 4 is higher than 120°C, the slippery layer 3 constituting the slippery film 1 is excessively softened, and the slippery layer 3 is easily peeled off from the surface of the first resin film 2. For example, the atmosphere in the heating furnace 4 may be air. The temperature of the atmosphere in the heating furnace 4 may be controlled by a heater. Hot air at a temperature of 80° C. or more and 120° C. or less may be continuously supplied into the heating furnace 4.

[0021] The multiple guide rolls installed in the heating furnace 4 include at least one guide roll A that is in direct contact with the surface of the lubricity layer 3. The multiple guide rolls installed in the heating furnace 4 may include multiple guide rolls A. In the heating furnace 4 shown in Fig. 2, the first guide roll g1, the third guide roll g3, and the fifth guide roll g5 are each a guide roll A. However, the number of guide rolls A is not limited to three. The multiple guide rolls installed in the heating furnace 4 may include at least one guide roll B that is in direct contact with the surface of the first resin film 2, not with the lubricity layer 3. The multiple guide rolls installed in the heating furnace 4 may include multiple guide rolls B. In the heating furnace 4 shown in Fig. 2, the second guide roll g2 and the fourth guide roll g4 are each a guide roll B. However, the number of guide rolls B is not limited to two.

[0022] The embrace angle α between the guide roll A and the slippery film 1 (slippery layer 3) is 80° or more and 170° or less. In a cross section perpendicular to the rotation axis ax (center axis) of the guide roll A and including the guide roll A and the easy-to-slip film 1 (easy-to-slip layer 3), the easy-to-slip layer 3 contacts the surface of the guide roll A at two contact points (first contact point a1 and second contact point a2). The line segment that has a length of 1 / 2 the diameter (thickness) of the guide roll A and connects the first contact point a1 and the rotation axis ax is referred to as the "first line segment La1". The line segment that has a length of 1 / 2 the diameter (thickness) of the guide roll A and connects the second contact point a2 and the rotation axis ax is referred to as the "second line segment La2". The angle between the first line segment La1 and the second line segment La2 corresponds to the embrace angle α between the guide roll A and the easy-to-slip film 1 (easy-to-slip layer 3). The embrace angle α between each guide roll A and the slippery film 1 (slippery layer 3) is 80° or more and 170° or less, which easily prevents the slippery layer 3 from peeling off from the surface of the first resin film 2. For the same reason, the embrace angle α between the guide roll A and the slippery film 1 (slippery layer 3) may be 80° or more and 165° or less. If the embrace angle α is smaller than 80°, the slippage of the lubricious film 1 on the surface of the guide roll A is likely to occur, the lubricious layer 3 is likely to peel off, or scratches are likely to form on the surface of the lubricious layer 3. If the embrace angle α is greater than 170°, the gripping force of the slippery film 1 increases, and the slippery layer 3 becomes more likely to peel off.

[0023] In a cross section perpendicular to the rotation axis ax (center axis) of the guide roll B and including the guide roll B and the easy-slip film 1 (first resin film 2), the first resin film 2 may be in contact with the surface of the guide roll B at two contact points (first contact point b1 and second contact point b2). A line segment having a length of 1 / 2 the diameter (thickness) of the guide roll B and connecting the first contact point b1 and the rotation axis ax is referred to as a "first line segment Lb1". A line segment having a length of 1 / 2 the diameter (thickness) of the guide roll B and connecting the second contact point b2 and the rotation axis ax is referred to as a "second line segment Lb2". The angle between the first line segment Lb1 and the second line segment Lb2 corresponds to the embrace angle β between the guide roll B and the easy-slip film 1 (first resin film 2). The embrace angle β between each guide roll B and the slippery film 1 (first resin film 2) is not limited. For example, the embrace angle β between each guide roll B and the slippery film 1 (first resin film 2) may be greater than 0° and equal to or less than 180°. In a cross section perpendicular to the rotation axis ax (central axis) of the guide roll B and including the guide roll B and the slippery film 1 (first resin film 2), the first resin film 2 may contact the surface of the guide roll B at only one contact point.

[0024] As long as at least one guide roll A in direct contact with the surface of the lubricating layer 3 is installed in the heating furnace 4 and the embrace angle α between the guide roll A and the lubricating film 1 (lubricating layer 3) is 80° or more and 170° or less, the positions and the number of the guide rolls A and B in the heating furnace 4 are not limited. In the heating furnace 4 shown in FIG. 2, the lubricating film 1 first comes into contact with the guide roll A (first guide roll g1), but in other embodiments, the lubricating film 1 may first come into contact with the guide roll B. In other words, the order of arrangement of the guide rolls A and B is not limited.

[0025] The arithmetic mean roughness Ra of the surface of each guide roll A is 0.06 μm or less. Since the arithmetic mean roughness Ra of the surface of each guide roll A is 0.06 μm or less, friction between the surface of each guide roll A and the lubricating layer 3 is suppressed, and peeling of the lubricating layer 3 from the surface of the first resin film 2 is easily suppressed. When the arithmetic mean roughness Ra of the surface of each guide roll A is greater than 0.06 μm, the lubricating layer 3 is easily peeled off from the surface of the first resin film 2 due to friction between the surface of each guide roll A and the lubricating layer 3. In other words, when the arithmetic mean roughness Ra of the surface of each guide roll A is greater than 0.06 μm, the fine protrusions formed on the surface of each guide roll A are easily embedded in the lubricating layer 3, and the lubricating layer 3 is easily cut.

[0026] The arithmetic mean roughness Ra of the surface of each guide roll A may be 0.01 μm or more and 0.06 μm or less. When the arithmetic mean roughness Ra of the surface of each guide roll A is 0.01 μm or more, the adhesion between the surface of each guide roll A and the lubricious layer 3 is suppressed to a certain degree. As a result, the peeling of the lubricious layer 3 from the surface of the first resin film 2 is easily suppressed, and the lubricious film 1 is easily transported smoothly. For the same reason, the arithmetic mean roughness Ra of the surface of each guide roll A may be 0.02 μm or more and 0.05 μm or less, or 0.03 μm or more and 0.04 μm or less.

[0027] For example, the method of measuring the arithmetic mean roughness Ra of the surface of the guide roll A may conform to the Japanese Industrial Standards (JIS 1994). For example, the arithmetic mean roughness Ra of the surface of the guide roll A may be measured by a small surface roughness measuring instrument (SURFTEST SJ-310) manufactured by Mitutoyo Corporation. A stylus provided in the measuring instrument is brought into contact perpendicularly with the surface of the guide roll A. Furthermore, the measured profile curve R of the surface of the guide roll A is measured by scanning the surface of each guide roll A with the stylus along a straight line parallel to the rotation axis ax of the guide roll A. Noise in the measured profile curve R may be removed by a Gaussian filter. In other words, the measured profile curve R may be smoothed by a Gaussian filter. The roughness curve of the surface of the guide roll A is obtained by removing the waveform (waviness curve) having a wavelength longer than the long wavelength cutoff value λc (0.8 mm) from the measured profile curve R. On the other hand, it is not necessary to remove noise based on the short wavelength cutoff value λs (waveform with a wavelength shorter than λs) from the measured profile curve R. From the roughness curve of the surface of the guide roll A, the arithmetic average roughness Ra of the surface of the guide roll A may be calculated.

[0028] The arithmetic mean roughness Ra of the surface of each guide roll A may be freely adjusted by polishing the surface of each guide roll A. For example, the arithmetic mean roughness Ra of the surface of each guide roll A may be adjusted based on the material and grain size of the grindstone used to polish the surface of each guide roll A. For example, when the surface of each guide roll A is polished with a buff, the arithmetic mean roughness Ra of the surface of each guide roll A may be adjusted based on the material of the buff, and the material and grain size of the abrasive interposed between the surface of each guide roll A and the buff.

[0029] For example, each guide roll A may be manufactured from a metal having high thermal conductivity. That is, the surface of each guide roll A may be made of a metal. For example, the surface of each guide roll A may be treated by hard chrome plating. For example, the length of each guide roll A in a transverse direction (TD) perpendicular to the MD may be equal to or greater than the width of the slippery film 1 in the TD. That is, the length of each guide roll A in a direction parallel to the rotation axis ax of each guide roll A may be equal to or greater than the width of the slippery film 1 in the TD. For example, the diameter (thickness) of each guide roll A may be 5 cm or more and 30 cm or less. Each guide roll A itself may have a heating mechanism. The material of each guide roll B may be approximately the same as that of each guide roll A. The arithmetic mean roughness Ra of the surface of each guide roll B may be approximately the same as that of each guide roll A. The dimensions of each guide roll B may be approximately the same as that of each guide roll A. Each guide roll B itself may have a heating mechanism.

[0030] For example, the total length of the slippery film 1 (first resin film 2) constituting the resin roll R1 (that is, the total length of the slippery film 1 in MD) may be 500 m or more and 5000 m or less. For example, the width of the slippery film 1 in TD may be 500 mm or more and 3000 mm or less. For example, the conveying time required for conveying the slippery film 1 in the heating furnace 4 may be 10 seconds or more and 60 seconds or less. For example, the thickness of the first resin film 2 contained in the slippery film 1 may be 5 μm or more and 200 μm or less. For example, the thickness of the slippery layer 3 contained in the slippery film 1 may be 0.01 μm or more and 3 μm or less. By satisfying each of the above numerical conditions, the structural defects of the slippery film 1 caused by blocking are easily eliminated, and the peeling of the slippery layer 3 from the surface of the first resin film 2 is easily suppressed.

[0031] The slippery film 1 that has passed through the heating furnace 4 is transported via a guide roll g6 or the like to a facility for carrying out a coating step.

[0032] In the coating step, an adhesive is applied to the surface of the lubricious film 1 that has passed through the heating furnace 4. For example, the first adhesive 5a may be directly applied to the surface of the lubricious layer 3 that constitutes the lubricious film 1 by the first gravure coater c1. Since the surface of the lubricious layer 3 that constitutes the lubricious film 1 is rougher than the surface of the first resin film 2 that constitutes the lubricious film 1, the first adhesive 5a is more likely to adhere to the surface of the lubricious layer 3 than to the surface of the first resin film 2. However, in other embodiments, the first adhesive 5a may be directly applied to the surface of the first resin film 2 that constitutes the lubricious film 1 by the first gravure coater c1.

[0033] The easy-slip film 1 that has been subjected to the coating step is transported via a guide roll g7 or the like to a facility for carrying out a lamination step.

[0034] In the lamination step, the slippery film 1 is laminated to the surface of the polarizer film 6 via the first adhesive 5a, to form a laminate 8. For example, the slippery film 1 and the polarizer film 6 are supplied between a pair of lamination rolls r1 and r2, and the slippery film 1 and the polarizer film 6 are sandwiched between the pair of lamination rolls r1 and r2. As a result, the slippery film 1 is laminated to the surface (first main surface) of the polarizer film 6 via the first adhesive 5a. In the lamination step, the surface of the slippery layer 3 constituting the slippery film 1 may be laminated to the surface of the polarizer film 6 via the first adhesive 5a. In another embodiment, the surface of the first resin film 2 constituting the slippery film 1 may be laminated to the surface of the polarizer film 6 via the first adhesive 5a. The total length of the polarizer film 6 in the MD may be approximately the same as the total length of the slippery film 1 in the MD. The width of the polarizer film 6 in the TD may be approximately the same as the width of the slippery film 1 in the TD. For example, the thickness of the polarizer film 6 may be not less than 1 μm and not more than 50 μm.

[0035] In the lamination step, a resin film (second resin film 7) other than the first resin film 2 constituting the easy-slip film 1 may be laminated to the back surface of the polarizer film 6 via an adhesive. For example, before the lamination step, the second adhesive 5b may be directly applied to the surface of the second resin film 7 by the second gravure coater c2. The second resin film 7 to which the second adhesive 5b is applied may be supplied between a pair of lamination rolls r1 and r2 via a guide roll g8 or the like. That is, the easy-slip film 1, the polarizer film 6, and the second resin film 7 may be simultaneously sandwiched between a pair of lamination rolls r1 and r2. As a result, the second resin film 7 may be laminated to the back surface (second main surface) of the polarizer film 6 via the second adhesive 5b. That is, the easy-slip film 1 and the second resin film 7 may be simultaneously laminated to the polarizer film 6. When the second resin film 7 is attached to the back surface of the polarizer film 6, the slippery film 1, the first adhesive 5a, the polarizer film 6, the second adhesive 5b, and the second resin film 7 may be stacked in this order to form a laminate 8. The total length of the second resin film 7 in the MD may be approximately the same as the total length of the polarizer film 6 in the MD. The width of the second resin film 7 in the TD may be approximately the same as the width of the polarizer film 6 in the TD. For example, the thickness of the second resin film 7 may be 5 μm or more and 200 μm or less.

[0036] When at least one of the first adhesive 5a and the second adhesive 5b is an active energy ray curable resin (ultraviolet ray curable resin or the like), the laminate 8 may be irradiated with active energy rays (ultraviolet ray or the like) by the irradiation device L. The laminate 8 that has passed through the irradiation device L may be transported to a facility for carrying out a post-process via a guide roll g9 or the like.

[0037] (First resin film 2, and second resin film 7) For example, each of the first resin film 2 and the second resin film 7 may be a thermoplastic resin having light-transmitting properties. For example, each of the first resin film 2 and the second resin film 7 may be a transparent thermoplastic resin. For example, each of the first resin film 2 and the second resin film 7 may be a cyclic olefin polymer-based resin (Cyclo Olefine Polymer-based resin), a chain polyolefin-based resin, a cellulose ester-based resin, a polyester-based resin, a polycarbonate-based resin, a (meth)acrylic-based resin, a polystyrene-based resin, or a mixture or copolymer thereof. When the first resin film 2 is a cyclic olefin polymer-based resin (COP-based resin) and the surface of the first resin film 2 is not covered with the easy-slip layer 3, blocking of the first resin film 2 is likely to occur. However, even when the first resin film 2 is a cyclic olefin polymer-based resin, blocking is easily suppressed by covering the surface of the first resin film 2 with the easy-slip layer 3. The composition of the first resin film 2 may be the same as the composition of the second resin film 7. The composition of the first resin film 2 may be different from the composition of the second resin film 7.

[0038] For example, the cyclic olefin polymer resin may be a ring-opening (co)polymer of a cyclic olefin, or an addition polymer of a cyclic olefin. For example, the cyclic olefin polymer resin may be a copolymer (e.g., a random copolymer) of a cyclic olefin and a chain olefin. For example, the chain olefin constituting the copolymer may be ethylene or propylene. For example, the cyclic olefin polymer resin may be a graft polymer obtained by modifying the above-mentioned polymer with an unsaturated carboxylic acid or a derivative thereof, or a hydrogenated product thereof. For example, the cyclic olefin polymer resin may be a norbornene resin using a norbornene monomer such as norbornene or a polycyclic norbornene monomer.

[0039] For example, the linear polyolefin resin may be a homopolymer of a linear olefin such as a polyethylene resin or a polypropylene resin, or a copolymer of two or more types of linear olefins.

[0040] For example, the cellulose ester resin may be cellulose triacetate (triacetyl cellulose (TAC)), cellulose diacetate, cellulose tripropionate, cellulose dipropionate, or a copolymer thereof. For example, the cellulose ester resin may be a cellulose ester resin in which some of the hydroxyl groups have been modified with other substituents. For example, the second resin film 7 may be saponified cellulose triacetate.

[0041] Each of the first resin film 2 and the second resin film 7 may be a polyester resin other than a cellulose ester resin. For example, the polyester resin may be a polycondensation product of a polycarboxylic acid or a derivative thereof and a polyhydric alcohol. For example, the polycarboxylic acid or a derivative thereof may be a dicarboxylic acid or a derivative thereof. For example, the polycarboxylic acid or a derivative thereof may be terephthalic acid, isophthalic acid, dimethyl terephthalate, or dimethyl naphthalenedicarboxylate. For example, the polyhydric alcohol may be a diol. For example, the polyhydric alcohol may be ethylene glycol, propanediol, butanediol, neopentyl glycol, or cyclohexanedimethanol.

[0042] For example, the polyester-based resin may be polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polytrimethylene terephthalate, polytrimethylene naphthalate, polycyclohexane dimethyl terephthalate, or polycyclohexane dimethyl naphthalate.

[0043] For example, the polycarbonate-based resin may be a polymer in which polymerization units (monomers) are bonded via carbonate groups. For example, the polycarbonate-based resin may be a modified polycarbonate having a modified polymer backbone. For example, the polycarbonate-based resin may be a copolymer polycarbonate.

[0044] For example, the (meth)acrylic resin may be a poly(meth)acrylic acid ester (e.g., polymethyl methacrylate (PMMA)); a methyl methacrylate-(meth)acrylic acid copolymer; a methyl methacrylate-(meth)acrylic acid ester copolymer; a methyl methacrylate-acrylic acid ester-(meth)acrylic acid copolymer; a methyl (meth)acrylate-styrene copolymer (e.g., MS resin); or a copolymer of methyl methacrylate and a compound having an alicyclic hydrocarbon group (e.g., a methyl methacrylate-cyclohexyl methacrylate copolymer, or a methyl methacrylate-norbornyl (meth)acrylate copolymer, etc.).

[0045] (Easy layer 3) As described above, the lubrication layer 3 may contain a polymer and a plurality of particles. The plurality of particles contained in the lubrication layer 3 may be at least one type of particle selected from the group consisting of inorganic particles and organic particles. The surface of the lubrication layer 3 containing a plurality of particles is rougher than the surface of the first resin film 2, and therefore has excellent slipperiness. Due to the slipperiness of the lubrication layer 3, blocking of the lubrication film 1 is suppressed, and structural defects of the lubrication film 1 caused by blocking are also suppressed.

[0046] The lubricity layer 3 may contain polyurethane as a polymer. Polyurethane is likely to be firmly adhered to the surface of the first resin film 2 containing a cyclic olefin polymer resin. Therefore, because the lubricity layer 3 contains polyurethane, peeling of the lubricity layer 3 from the surface of the first resin film 2 is likely to be suppressed. Polyurethane is likely to be softened at a temperature of 80°C or higher and 120°C or lower. Therefore, because the lubricity layer 3 contains polyurethane, the lubricity film 1 is likely to be appropriately softened in the heating furnace 4, and structural defects of the lubricity film 1 caused by blocking are likely to be eliminated.

[0047] For example, polyurethane may be synthesized by the reaction of component (i) containing two or more active hydrogens on average in one molecule with polyvalent isocyanate component (ii). For example, in the production of polyurethane, a prepolymer may be synthesized from the above components (i) and (ii). The molecular chain of the prepolymer may be extended using a chain extender. Water may be added to the extended polymer to disperse the polymer in water. That is, water in which polyurethane is dispersed may be used as the raw material of the easy-slip layer 3. As the prepolymer, a prepolymer containing an isocyanate group may be synthesized by a urethane reaction of the above components (i) and (ii) under reaction conditions in which the isocyanate group is in excess. The urethane reaction of the above components (i) and (ii) may be carried out in an organic solvent having excellent affinity with water. Before extending the molecular chain of the prepolymer, the prepolymer obtained by the urethane reaction may be neutralized. The polyurethane may contain an acid structure. A part or all of the acid structure of the polyurethane may be neutralized.

[0048] Polyurethane dispersed in water is commercially available. For example, commercially available polyurethanes include the "ADEKA BONTITAR" series manufactured by Asahi Denka Kogyo Co., Ltd., the "OLESTAR" series manufactured by Mitsui Toatsu Chemicals Co., Ltd., the "BONDIC" series and "HYDRAN" series manufactured by Dainippon Ink and Chemicals, Inc., the "IMPLANIL" series manufactured by Bayer, the "SOFRANATE" series manufactured by Nippon Soflan Co., Ltd., the "POISE" series manufactured by Kao Corporation, the "SANPRENE" series manufactured by Sanyo Chemical Industries, Ltd., the "ISELAX" series manufactured by Hodogaya Chemical Co., Ltd., the "SUPERFLEX" series manufactured by Daiichi Kogyo Seiyaku Co., Ltd., and the "NEOREZ" series manufactured by Zeneca.

[0049] For example, the inorganic particles contained in the easy-slip layer 3 may be at least one type of particles selected from the group consisting of silica, titania, alumina, zirconia, calcium carbonate, talc, clay, calcined kaolin, calcined calcium silicate, hydrated calcium silicate, aluminum silicate, magnesium silicate, and calcium phosphate. For example, the organic particles contained in the easy-slip layer 3 may be at least one type of particles selected from the group consisting of silicone resin, fluororesin, and (meth)acrylic resin. The easy-slip layer 3 may contain multiple types of particles.

[0050] For example, the lubricity layer 3 may contain polyurethane as a polymer and silica as a plurality of particles. Silica (particularly amorphous colloidal silica) is easy to suppress structural defects (wrinkles, etc.) of the lubricity film 1, has excellent transparency, and is easy to be stably dispersed in polyurethane.

[0051] For example, the average particle size D50 of the multiple particles contained in the lubrication layer 3 may be 1 nm or more, 5 nm or more, or 10 nm or more, and 500 nm or less, 300 nm or less, or 200 nm or less. The average particle size D50 is the particle size at which the volume accumulated from the origin reaches 50% in the particle size distribution measured by a laser diffraction method. When the average particle size D50 is equal to or more than the above lower limit, the slipperiness of the lubrication layer 3 is likely to be improved. When the average particle size D50 is equal to or less than the upper limit, the falling off of particles from the lubrication layer 3 is likely to be suppressed.

[0052] For example, the mass of the particles contained in the lubricating layer 3 may be 0.5 parts by mass or more, 5 parts by mass or more, or 8 parts by mass or more, and 20 parts by mass or less, 18 parts by mass or less, or 15 parts by mass or less, relative to 100 parts by mass of the polymer contained in the lubricating layer 3. When the mass of the particles contained in the lubricating layer 3 is equal to or more than the above lower limit, the slipperiness of the lubricating layer 3 is easily improved. As a result, structural defects (wrinkles, etc.) of the lubricating film in the resin roll R1 are easily suppressed, the lubricating film 1 is less likely to adhere to each guide roll in the heating furnace 4, and the lubricating film 1 is easily transported in the heating furnace 4. When the mass of the particles contained in the lubricating layer 3 is equal to or less than the above upper limit, the clouding of the lubricating layer 3 and the polarizing plate is easily suppressed.

[0053] The easy-slip layer 3 may further contain an optional component other than the polymer and the plurality of particles. For example, the optional component may be at least one component selected from the group consisting of a crosslinking agent, a heat stabilizer, a weather stabilizer, a leveling agent, a surfactant, an antioxidant, an antistatic agent, a slip agent, an antiblocking agent, an antifogging agent, a lubricant, a dye, a pigment, a natural oil, a synthetic oil, and a wax.

[0054] For example, in the step of forming the lubrication layer 3, a resin composition containing a polymer, particles, a solvent (water, etc.), and other optional components may be prepared. For example, the resin composition may be an epoxy compound (epoxy resin). A resin layer made of the resin composition may be formed by applying the resin composition to the surface of the first resin film 2. The lubrication layer 3 may be formed by curing the resin layer. For example, the resin layer may be cured by irradiation with light such as ultraviolet light or by heating. A surface treatment (activation treatment, etc.) may be performed on the first resin film 2, and the lubrication layer 3 may be formed on the surface that has been subjected to the surface treatment.

[0055] (Polarizer film 6) The polarizer film 6 may include a polyvinyl alcohol resin. For example, the polarizer film 6 made of a polyvinyl alcohol resin may be produced by processes such as stretching, dyeing, and crosslinking the polyvinyl alcohol resin. The polarizer film 6 may include a polymer of a polymerizable liquid crystal compound and a dichroic dye. The polarizer film 6 containing a polymer of a polymerizable liquid crystal compound and a dichroic dye may be produced by a process of forming a coating film by applying a raw material containing a polymerizable liquid crystal compound, a dichroic dye, and a solvent to the surface of an alignment layer, and a process of polymerizing the polymerizable liquid crystal compound in the coating film. For example, the alignment layer is a film containing a polymer compound and may have a function of aligning the polymerizable liquid crystal compound constituting the polarizer film 6 in a desired direction. For example, the alignment layer may be a type of alignment film selected from the group consisting of an alignment film made of an alignable polymer, a photoalignment film, and a groove alignment film.

[0056] (First adhesive 5a and second adhesive 5b) Each of the first adhesive 5a and the second adhesive 5b may be an active energy ray-curable adhesive (active energy ray-curable resin) or a water-based adhesive. The composition of the first adhesive 5a may be the same as the composition of the second adhesive 5b. The composition of the first adhesive 5a may be different from the composition of the second adhesive 5b.

[0057] The active energy ray curable resin is a resin that is cured by irradiation with active energy rays. For example, the active energy rays may be ultraviolet rays, visible light, electron beams, or X-rays. For example, the active energy ray curable resin may be an ultraviolet ray curable resin.

[0058] The active energy ray-curable resin may be one type of resin or may contain multiple types of resins. For example, the active energy ray-curable resin may contain a cationic polymerizable curable compound or a radical polymerizable curable compound. The active energy ray-curable resin may contain a cationic polymerization initiator or a radical polymerization initiator for initiating the curing reaction of the curable compound.

[0059] The cationic polymerizable curable compound may be, for example, an epoxy-based compound (a compound having at least one epoxy group in the molecule) or an oxetane-based compound (a compound having at least one oxetane ring in the molecule). The radically polymerizable curable compound may be, for example, a (meth)acrylic-based compound (a compound having at least one (meth)acryloyloxy group in the molecule). The radically polymerizable curable compound may be a vinyl-based compound having a radically polymerizable double bond.

[0060] The active energy ray-hardenable resin may contain, as necessary, a cationic polymerization accelerator, an ion trapping agent, an antioxidant, a chain transfer agent, a tackifier, a thermoplastic resin, a filler, a flow adjuster, a plasticizer, an antifoaming agent, an antistatic agent, a leveling agent, a solvent, or the like.

[0061] For example, the aqueous adhesive may be at least one of an aqueous solution of a polyvinyl alcohol resin and an aqueous solution of a urethane resin. For example, the polyvinyl alcohol resin contained in the aqueous adhesive may be at least one modified polyvinyl alcohol resin selected from the group consisting of partially saponified polyvinyl alcohol resin, fully saponified polyvinyl alcohol resin, carboxyl group-modified polyvinyl alcohol, acetoacetyl group-modified polyvinyl alcohol, methylol group-modified polyvinyl alcohol, and amino group-modified polyvinyl alcohol. For example, the aqueous solution of the urethane resin may be a two-liquid urethane emulsion adhesive.

[0062] (Other processes) The method for producing a polarizing plate may further include a step of directly or indirectly attaching (laminating) one or more other resin films (resin layers) to the surface of the easy-slip film 1 or the polarizer film 6. For example, the other resin film (resin layer) may be at least one selected from the group consisting of a protective film, an optical compensation film, a retardation film, a release film, a reflective polarizing film, a film with an antiglare function, a film with a surface antireflection function, a reflective film, a semi-transmissive reflective film, a window film, a pressure-sensitive adhesive layer, an adhesive layer, a hard coat layer, a touch sensor layer, an antistatic layer, and an antifouling layer.

[0063] The method for producing a polarizing plate may further include a step of processing the laminate formed by the above steps according to the size and shape of the image display device. For example, the laminate may be processed by cutting, grinding, and polishing. For example, the processing means for the laminate may be a rotary blade, an end mill, a laser, or the like.

[0064] For example, the thickness of the finished polarizing plate may be from 10 μm to 300 μm.

[0065] The present invention is not necessarily limited to the above-described embodiment. Various modifications of the present invention are possible without departing from the spirit of the present invention, and these modifications are also included in the present invention. EXAMPLES

[0066] The present invention will be described in detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples.

[0067] Example 1 A liquid aqueous resin composition was prepared by mixing water in which polyurethane (ester polyurethane resin containing a carboxyl group) was dispersed, an epoxy compound (polyglycerol polyglycidyl ether), sebacate dihydrazide, silica powder (a large number of particles made of silica), and water. The aqueous resin composition is a raw material for the slippery layer 3. The mass ratio of polyurethane was adjusted to 100 parts by mass, the mass ratio of the epoxy compound was adjusted to 20 parts by mass, the mass ratio of sebacate dihydrazide was adjusted to 5 parts by mass, and the mass ratio of silica powder was adjusted to 8 parts by mass. The content of solids in the aqueous resin composition was adjusted to 5% by mass. The average particle size D50 of the silica powder was 100 nm. Superflex 210 manufactured by Daiichi Kogyo Seiyaku Co., Ltd. was used as the water in which polyurethane was dispersed. Denacol EX-521 manufactured by Nagase ChemteX Corporation was used as the epoxy compound.

[0068] A corona discharge treatment was applied to one surface (main surface) of a long first resin film 2. The first resin film 2 was a cycloolefin resin. ZF14 manufactured by Zeon Corporation was used as the first resin film 2. The total length of the first resin film 2 in MD was 2000 m. The width of the first resin film 2 in TD was 1330 mm. The thickness of the first resin film 2 was 23 μm. The output of the corona discharge treatment was 800 W.

[0069] The above-mentioned aqueous resin composition was applied to the entire one surface of the first resin film 2 that had been subjected to the corona discharge treatment. A die coater was used to apply the aqueous resin composition. The aqueous resin composition applied to the first resin film 2 was dried at 140° C. for 40 seconds to form the lubricious layer 3 on the entire one surface of the first resin film 2. That is, the lubricious film 1 consisting of the first resin film 2 and the lubricious layer 3 covering the surface of the first resin film 2 was produced. The thickness of the dried lubricious layer 3 was 0.5 μm. The lubricious film 1 was wound around a roll core to form a resin roll R1. The total length of the lubricious film 1 constituting one resin roll R1 (the total length of the lubricious film 1 in MD) was 2000 m. A total of five resin rolls R1 were prepared. Each resin roll R1 was stored for one month.

[0070] After storing the resin roll R1 for one month, the following heating process was carried out.

[0071] The first guide roll g1, the second guide roll g2, the third guide roll g3, the fourth guide roll g4, ​​and the fifth guide roll g5 were installed in the heating furnace 4 as shown in FIG. 2. In the heating step, the slippery film 1 unwound from the resin roll R1 was transported through the five guide rolls installed in the heating furnace 4. The surface of each of the five guide rolls was made of metal. The slippery film 1 was transported while being in contact with the surfaces of the first guide roll g1, the second guide roll g2, the third guide roll g3, the fourth guide roll g4, ​​and the fifth guide roll g5 in this order.

[0072] Each of the first guide roll g1, the third guide roll g3, and the fifth guide roll g5 was a guide roll A that was in direct contact with the surface of the lubricity layer 3. The embrace angle α between each guide roll A and the lubricity film 1 (lubricity layer 3) was adjusted to the value shown in Table 1 below. The arithmetic mean roughness Ra of the surface of each guide roll A was adjusted to the value shown in Table 1 below.

[0073] The second guide roll g2 and the fourth guide roll g4 were guide rolls B that were in direct contact with the surface of the first resin film 2.

[0074] The temperature of the atmosphere in the heating furnace 4 was maintained at 105° C. The transport time required for transporting the slippery film 1 in the heating furnace 4 was maintained at 20 seconds. In other words, the time from when any portion X of the slippery film 1 was introduced into the heating furnace 4 to when the any portion X left the heating furnace 4 was maintained at 20 seconds.

[0075] The heating process was completed when the total length (MD length) of the lubricating film 1 passing through the heating furnace 4 reached 10,000 m. After the heating process was completed, the surfaces of the guide rolls A were observed. If the lubricating layer 3 was peeled off from the surface of the first resin film 2, fragments of the lubricating layer 3 should adhere to the surface of each guide roll A. However, fragments of the lubricating layer 3 did not adhere to any of the surfaces of the first guide roll g1, the third guide roll g3, and the fifth guide roll g5. In other words, the lubricating layer 3 that was in direct contact with the surfaces of the first guide roll g1, the third guide roll g3, and the fifth guide roll g5 did not peel off from the surface of the first resin film 2.

[0076] In the easy-to-slip film 1 that had been subjected to the heating step, the structural defect of the easy-to-slip film 1 caused by blocking had been eliminated.

[0077] Example 2 In the case of Example 2, the arithmetic mean roughness Ra of the surface of each of the first guide roll g1, the third guide roll g3, and the fifth guide roll g5 was adjusted to the value shown in the following Table 1. The heating step of Example 2 was carried out in the same manner as in Example 1, except for the arithmetic mean roughness Ra of the surface of each guide roll A.

[0078] Even in the heating step of Example 2, the lubricity layer 3 in direct contact with the surfaces of the first guide roll g1, the third guide roll g3, and the fifth guide roll g5 did not peel off from the surface of the first resin film 2. Even in the lubricity film 1 that had been subjected to the heating step of Example 2, the structural defect of the lubricity film 1 due to blocking was eliminated.

[0079] Comparative Example 1 In the case of Comparative Example 1, the arithmetic mean roughness Ra of the surface of each of the first guide roll g1, the third guide roll g3, and the fifth guide roll g5 was adjusted to the value shown in the following Table 1. The heating step of Comparative Example 1 was carried out in the same manner as in Example 1, except for the arithmetic mean roughness Ra of the surface of each guide roll A.

[0080] In the heating process of Comparative Example 1, a portion of the lubrication layer 3 that was in direct contact with the surface of each of the first guide roll g1, the third guide roll g3, and the fifth guide roll g5 peeled off from the surface of the first resin film 2 and adhered to the surface of each guide roll A.

[0081] [Table 1] [Industrial Applicability]

[0082] For example, a polarizing plate manufactured by the polarizing plate manufacturing method according to one aspect of the present invention may be used in image display devices (liquid crystal displays, organic EL displays, etc.) such as televisions, computers, mobile phones (smartphones), smart watches, portable game consoles, or vehicle instrument panels. [Explanation of symbols]

[0083] 1...slippery film, 2...first resin film, 3...slippery layer, 4...heating furnace, 5a...first adhesive, 5b...second adhesive, 6...polarizer film, 7...second resin film, 8...laminate, A...guide roll A, ax...rotation axis of guide roll, c1...first gravure coater, c2...second gravure coater, g1...first guide roll, g2...second guide roll, g3...third guide roll, g4...fourth guide roll, g5...fifth guide roll, g6, g7, g8, g9...guide roll, L...active energy ray irradiation device, R1...resin roll, r1, r2...lamination roll, α, β...holding angle.

Claims

1. A method for producing a polarizing plate using a polarizer film and a slippery film, comprising the steps of: The slippery film comprises a long resin film and a slippery layer covering the surface of the resin film, The method for producing the polarizing plate includes the steps of: A heating step of conveying the slippery film unwound from a resin roll of the slippery film through a plurality of guide rolls installed in a heating furnace; a coating step of coating an adhesive on the surface of the easy-slip film that has passed through the heating furnace; a bonding step of bonding the easy-slip film to a surface of the polarizer film via the adhesive; Equipped with The temperature of the atmosphere in the heating furnace is 80° C. or higher and 120° C. or lower, The plurality of guide rolls includes at least one guide roll A that is in direct contact with the surface of the lubricious layer, The embrace angle between the guide roll A and the slippery film is 80° or more and 170° or less, The arithmetic average roughness Ra of the surface of the guide roll A is 0.06 μm or less. A method for manufacturing a polarizing plate.

2. In the bonding step, a resin film different from the resin film is bonded to a rear surface of the front surface of the polarizer film via an adhesive. A method for producing the polarizing plate according to claim 1 .

3. The slippery layer includes a polymer and a plurality of particles. The plurality of particles are at least one type of particles selected from the group consisting of inorganic particles and organic particles. A method for producing the polarizing plate according to claim 1 .

4. The slippery layer comprises polyurethane. A method for producing the polarizing plate according to claim 1 .

5. The arithmetic average roughness Ra is 0.01 μm or more and 0.06 μm or less. A method for producing the polarizing plate according to claim 1 .

Citation Information

Patent Citations

  • Method for manufacturing polarizing plate

    JP2013205722A