Method for producing water-soluble film
By controlling the mixing conditions of polyvinyl alcohol resin and starch dispersion, the method achieves uniform dispersion and prevents agglomeration, producing a crack-free water-soluble film with improved blocking resistance for packaging.
Patent Information
- Application Number
- JP2023053160
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods for producing water-soluble films using polyvinyl alcohol resin and starch face challenges in uniformly dispersing fillers, leading to agglomeration, which results in cracks, reduced productivity, and poor blocking resistance, causing leaks and ink bleeding during printing.
A manufacturing method that controls the mixing conditions of an aqueous solution containing polyvinyl alcohol resin and an aqueous dispersion with starch, using specific ratios and temperatures to suppress starch agglomeration, ensuring uniform dispersion and excellent blocking resistance.
The method effectively prevents starch agglomeration, resulting in a crack-free water-soluble film with enhanced blocking resistance, suitable for packaging applications.
Smart Images

Figure 2024141478000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a water-soluble film containing a polyvinyl alcohol resin and starch, more specifically, to a method for producing a water-soluble film that is free from cracks and has excellent blocking resistance by suppressing aggregation of starch contained in the raw material of the water-soluble film. [Background technology]
[0002] Water-soluble films have traditionally been used in a wide range of fields, and water-soluble films using polyvinyl alcohol-based resins in particular have been widely used for individual packaging (unit packaging) of pharmaceuticals such as pesticides and detergents, and for food packaging.
[0003] As a method for producing such a water-soluble film, a method is known in which a polyvinyl alcohol-based resin is usually dissolved or dispersed in a solvent such as water, mixed, and degassed to prepare a mixture (film-forming raw material), and the film-forming raw material is then discharged from a die and cast onto a casting surface such as the metal surface of an endless belt or a drum roll, or the surface of a plastic substrate, and dried to produce a water-soluble film.
[0004] In the method for producing such a water-soluble film, it is known to incorporate various fillers into the film-forming raw materials in order to prevent blocking between films or between individual packages, but the fillers incorporated into the film-forming raw materials tend to aggregate, and it may be difficult to uniformly disperse the fillers. When the fillers aggregate and are not uniformly dispersed, it is difficult to impart excellent blocking resistance to the film. In addition, the filler aggregates tend to clog filters, the film breaks during film formation, and productivity decreases, and when the obtained film is used to make a package, cracks originating from the aggregates tend to cause bags to break or the contents to leak. Furthermore, when printing is performed on the film, ink bleeds tend to occur.
[0005] From the viewpoint of suppressing such aggregation of the filler, Patent Document 1 proposes a method for producing a water-soluble film, which includes a step of preparing an aqueous solution containing a polyvinyl alcohol-based resin and an aqueous dispersion containing a filler, and mixing the two at a temperature of 90°C or lower. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2005-194295 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, according to the study by the present inventors, it has been found that it is difficult to sufficiently suppress the aggregation of the filler by simply specifying the temperature conditions in the step of mixing an aqueous solution containing a polyvinyl alcohol resin with an aqueous dispersion containing a filler, as in the manufacturing method of Patent Document 1. In particular, it is difficult to uniformly disperse a filler that is particularly prone to aggregation, such as raw starch that has the property of gelatinizing when heated in the presence of water.
[0008] Under these circumstances, the present invention provides a production method capable of sufficiently suppressing starch aggregation, and capable of obtaining a water-soluble film free from cracks and excellent in blocking resistance. [Means for solving the problem]
[0009] In view of such circumstances, the present inventor, in the course of intensive research, focused on the step of mixing an aqueous solution containing a polyvinyl alcohol resin with an aqueous dispersion containing starch, and sought to determine the cause of the occurrence of aggregation. In the course of this research, the present inventor found that, in addition to the temperature conditions in the mixing step, each condition such as the solid content ratio of the aqueous solution containing a polyvinyl alcohol resin, the gelatinization temperature of starch, and the content ratios of starch and plasticizers in the aqueous dispersion containing starch have a certain correlation. Based on this knowledge, the present inventor, as a result of further research, found that by adopting a production method that satisfies certain conditions, it is possible to effectively suppress the aggregation of starch, and arrived at the present invention.
[0010] That is, the gist of the present invention is as follows. [1] A step of preparing an aqueous solution (I) containing a polyvinyl alcohol-based resin; Preparing an aqueous dispersion (II) comprising starch (S) and optionally further comprising a plasticizer (AP); A mixing step of mixing the aqueous solution (I) and the aqueous dispersion (II), A method for producing a water-soluble film, wherein the mixing step satisfies the condition shown in the following formula (1): (Formula){[(D' / S') AP' ]×(D T / T)×S R}≦0.50 (1) D': Solid content in the aqueous solution (I) (D S ) and the total amount of the aqueous solution (I) (D S / I). S': mass ratio (S / II) of the starch (S) contained in the aqueous dispersion (II) to the total amount of the aqueous dispersion (II). AP': The solid content of the plasticizer (AP) contained in the aqueous dispersion (II) S ) to the total amount of the aqueous dispersion (II) (AP S / II). If the aqueous dispersion (II) does not contain a plasticizer (AP), the value is 0. S R: Starch (S) contained in the aqueous dispersion (II) and the total amount of the aqueous dispersion (II) excluding the starch (S) (II -S ) and the mass ratio (S / II -S ). D T : Temperature of the aqueous solution (I) [℃]. T: Gelatinization temperature of starch (S) [℃]. [2] The method for producing a water-soluble film according to [1], wherein the mixing step satisfies the condition shown in the following formula (1'). (Formula){[(D' / S') AP' ]×(D T / T)×S R}≦0.35 (1') [3] The method for producing a water-soluble film according to [1] or [2], wherein the step of preparing the aqueous dispersion (II) is a step of preparing an aqueous dispersion (II) containing starch (S) and a plasticizer (AP). [4] The method for producing a water-soluble film according to any one of [1] to [3], wherein the step of preparing the aqueous solution (I) is a step of preparing an aqueous solution (I) containing a polyvinyl alcohol-based resin and a surfactant. [5] The starch (S) has a gelatinization temperature (T) of 50 to 95°C, and the aqueous solution (I) has a temperature (D T ) is 15 to 35° C. The method for producing a water-soluble film according to any one of [1] to [4]. Effect of the Invention
[0011] According to the method for producing a water-soluble film of the present invention, it is possible to effectively suppress aggregation of starch, and therefore to provide a water-soluble film that is free from cracks and has excellent blocking resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be specifically described below. In this specification, the term "solid content" refers to non-volatile content, and refers to the remainder excluding volatile content such as water. For example, the solid content of a PVA-based resin refers to the remainder excluding volatile content (e.g., water, methyl alcohol, methyl acetate, etc.) such as reaction products generated in the production process of the PVA-based resin or residues of raw materials used in the production thereof, and specifically, for example, the remainder excluding volatile content measured by the method specified in JIS K 6726. In this specification, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably greater than X" or "preferably smaller than Y". In addition, "X and / or Y (X and Y are optional configurations)" means at least one of X and Y, and means the following three cases: X only, Y only, and X and Y.
[0013] A method for producing a water-soluble film according to one embodiment of the present invention (hereinafter, may be referred to as "this production method") includes a step of preparing an aqueous solution (I) containing a polyvinyl alcohol-based resin, a step of preparing an aqueous dispersion (II) containing starch (S) and which may optionally further contain a plasticizer (AP), and a mixing step of mixing the aqueous solution (I) and the aqueous dispersion (II), wherein the mixing step satisfies the condition shown in the following formula (1). (Formula){[(D' / S') AP' ]×(D T / T)×S R}≦0.50 (1) D': Solid content in the aqueous solution (I) (D S ) and the total amount of the aqueous solution (I) (D S / I). S': mass ratio (S / II) of the starch (S) contained in the aqueous dispersion (II) to the total amount of the aqueous dispersion (II). AP': The solid content of the plasticizer (AP) contained in the aqueous dispersion (II) S ) to the total amount of the aqueous dispersion (II) (AP S / II). If the aqueous dispersion (II) does not contain a plasticizer (AP), the value is 0. SR : Starch (S) contained in the aqueous dispersion (II) and the total amount of the aqueous dispersion (II) excluding the starch (S) (II -S ) and the mass ratio (S / II -S ). D T : Temperature of the aqueous solution (I) [℃]. T: Gelatinization temperature of starch (S) [℃].
[0014] In the present production method, the above-mentioned formula (1) "{[(D' / S') AP' ]×(D T / T)×S R}" (hereinafter, this value is referred to as the "starch aggregation index (S ID By controlling the coagulation ratio (sometimes referred to as "coagulation ratio") to 0.50 or less, it is possible to effectively suppress the aggregation of starch in the film-forming raw materials, and therefore the water-soluble film obtained by this production method does not crack and has excellent blocking resistance.
[0015] In the present production method, in order to further suppress the aggregation of starch in the film-forming raw material and improve the crack resistance and blocking resistance, the starch aggregation index (S ID ) is preferably 0.35 or less, more preferably 0.30 or less. ID The lower limit of is not particularly limited, but is, for example, 0.01 or more, preferably 0.02 or more. (Formula){[(D' / S') AP' ]×(D T / T)×S R}≦0.35 (1')
[0016] In the present production method, when the aqueous dispersion (II) does not contain a plasticizer (AP), the power (D' / S') of formula (1) is AP' " index " AP' " will be 0, and "(D' / S') AP' " will have a value of 1.
[0017] The present production method will now be described in more detail. Incidentally, hereinafter, in the formula (1) and the like, "D'" is referred to as "solid content concentration (D')", "S'" is referred to as "starch concentration (S')", "AP'" is referred to as "plasticizer concentration (AP')", and "S R " may be referred to as "starch ratio (S R ))".
[0018] <<Method for Producing Water-Soluble Film>> This production method includes at least a step of preparing an aqueous solution (I) containing a polyvinyl alcohol-based resin (hereinafter sometimes referred to as "PVA-based resin"), a step of preparing an aqueous dispersion (II) containing starch (S) and optionally further containing a plasticizer (AP), and a mixing step of mixing the aqueous solution (I) and the aqueous dispersion (II).
[0019] <Step of Preparing Aqueous Solution (I) Containing PVA-Based Resin> This step is a step of dissolving a PVA-based resin or the like in water or the like to prepare an aqueous solution (I) that constitutes the main component of the film-forming raw material. The aqueous solution (I) containing the PVA-based resin contains at least the PVA-based resin and water, and optionally contains optional components such as a surfactant as necessary.
[0020] 〔PVA-Based Resin〕 The PVA-based resin contained in the aqueous solution (I) is a resin in which vinyl alcohol units are the main unit components in the repeating units constituting the polymer. The main unit component means a unit component that occupies 50 mol% or more and 100 mol% or less in the resin. Examples of such PVA-based resins include unmodified PVA and modified PVA-based resins.
[0021] The average saponification degree of the PVA-based resin is preferably 80 mol% or more, particularly preferably 82 to 99.9 mol%, more preferably 85 to 98.5 mol%, and especially preferably 90 to 97 mol%. Also, when using unmodified PVA as the PVA-based resin, its average saponification degree is preferably 80 mol% or more, particularly preferably 82 to 99 mol%, and more preferably 85 to 90 mol%. In addition, when a modified PVA resin is used as the PVA resin, the average saponification degree is preferably 80 mol% or more, particularly 85 to 99.9 mol%, and more preferably 90 to 98 mol%. In addition, when an anionic group-modified PVA resin is used as the PVA resin, the average saponification degree is preferably 85 mol% or more, particularly 88 to 99 mol%, more preferably 90 to 97 mol%, and especially preferably 91 to 94 mol%. If the average saponification degree is too small, the solubility of the water-soluble film in water tends to decrease over time, depending on, for example, the pH of the drug to be packaged. In addition, if the average saponification degree is too large, the solubility in water tends to decrease significantly.
[0022] The degree of polymerization of a PVA-based resin can generally be indicated by the viscosity of an aqueous solution, and the viscosity of a 4 mass % aqueous solution at 20° C. is preferably 5 to 50 mPa·s, more preferably 13 to 45 mPa·s, and particularly preferably 17 to 40 mPa·s. Furthermore, when unmodified PVA is used as the PVA resin, the viscosity of a 4 mass % aqueous solution of the unmodified PVA at 20° C. is preferably 5 to 50 mPa·s, more preferably 13 to 45 mPa·s, and particularly preferably 17 to 45 mPa·s. Furthermore, when a modified PVA resin is used as the PVA resin, the viscosity of a 4 mass % aqueous solution of the modified PVA resin at 20°C is preferably 5 to 50 mPa·s, more preferably 13 to 40 mPa·s, and particularly preferably 17 to 35 mPa·s. If the viscosity is too low, for example, the mechanical strength of the water-soluble film used as a packaging material tends to decrease, whereas if the viscosity is too high, the viscosity of the film-forming raw material tends to increase, resulting in decreased productivity.
[0023] The average degree of saponification is measured in accordance with JIS K 6726 3.5, and the viscosity of a 4% by mass aqueous solution is measured in accordance with JIS K 6726 3.11.2.
[0024] When a modified PVA resin is used as the PVA resin, the modification amount is preferably 1 to 10 mol%, more preferably 1.5 to 8 mol%, particularly preferably 2 to 6 mol%, and especially preferably 2 to 5 mol%. If the modification amount is too small, the solubility in water tends to decrease, whereas if it is too large, the productivity of the PVA resin tends to decrease, the biodegradability tends to decrease, and blocking tends to occur easily.
[0025] In the present production method, the PVA-based resins can be used alone, or unmodified PVA and modified PVA-based resins can be used in combination, or two or more types with different saponification degrees, viscosities, modified species, and amounts can be used in combination. Among these, in water-soluble films for packaging medicines (particularly for packaging laundry detergents), the PVA-based resin preferably contains a modified PVA-based resin in terms of solubility, and particularly preferably contains an anionic group-modified PVA-based resin. Examples of the anionic group include a carboxy group, a sulfonic acid group, and a phosphoric acid group, and in terms of solubility in water and resistance to medicines, the carboxy group and sulfonic acid group are preferred, and the carboxy group is particularly preferred.
[0026] The carboxy group of the carboxy group-modified PVA is derived from a monomer having a carboxy group, and examples thereof include carboxy group-containing unsaturated compounds such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, fumaric acid, and itaconic acid, and compounds in which the carboxy group is completely or partially neutralized with a base such as an alkali compound (e.g., sodium hydroxide, potassium hydroxide, etc.), and monoalkyl esters of the carboxy group-containing unsaturated compounds such as methyl acrylate, ethyl acrylate, methyl methacrylate, monomethyl fumarate, and monomethyl maleate, and dialkyl esters of the carboxy group-containing unsaturated compounds such as diethyl fumarate and diethyl maleate. The carbon number of these esters is usually 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms, and particularly preferably 1 to 4 carbon atoms, from the viewpoints of economy and practicality. Among these, maleic acid compounds are preferred, and monomethyl maleate is more preferred.
[0027] The PVA-based resin can be produced by a conventionally known method, for example, the method described in JP-A-2017-95679.
[0028] 〔water〕 The water contained in the aqueous solution (I) is not particularly limited, but it is preferable to use ion-exchanged water or RO water.
[0029] [Surfactant] The surfactant is contained for the purpose of improving the peelability from the cast surface during film production, and usually includes nonionic surfactants, cationic surfactants, and anionic surfactants. For example, polyoxyethylene nonylphenyl ether, polyoxyethylene octylnonyl ether, polyoxyethylene dodecylphenyl ether, polyoxyethylene alkyl allyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyalkylene alkyl ether phosphate monoethanolamine salt, polyoxyethylene lauryl amino ether, polyoxyethylene stearyl amino ether and other polyoxyethylene alkyl amino ethers, sorbitan monopalmitate, sorbitan monostearate, glycerin stearate, sucrose fatty acid esters, etc. can be mentioned. These can be used alone or in combination of two or more. Among them, polyoxyalkylene alkyl ether phosphate monoethanolamine salt and polyoxyethylene lauryl amino ether are preferred in terms of production stability. These can be used alone or in combination of two or more. Among them, it is also preferable to use a nonionic surfactant and an anionic surfactant in combination.
[0030] In addition, the aqueous solution (I) may contain solvents other than water, fragrances, rust inhibitors, colorants, extenders, defoamers, ultraviolet absorbers, liquid paraffins, fluorescent brighteners, bitter components (e.g., denatonium benzoate, etc.), antioxidants (e.g., sulfites such as sodium sulfite, sodium thiosulfate, etc.), dispersion extenders, plasticizers described below, etc., within the scope of not impairing the object of the present invention. These may be used alone or in combination of two or more. However, the content of these components is preferably less than 30% by mass, more preferably less than 25% by mass, and even more preferably less than 20% by mass, based on the total amount (100% by mass) of the aqueous solution (I).
[0031] Examples of the solvent include ethanol, methanol, propanol, isopropanol, acetone, methyl ethyl ketone, acetic acid, methyl acetate, ethyl acetate, butyl acetate, benzene, toluene, etc. These can be used alone or in combination of two or more kinds.
[0032] [Preparation of aqueous solution (I)] The aqueous solution (I) is obtained by dissolving each component, such as the PVA resin, in water. A high-temperature dissolution method or a pressure dissolution method is appropriately adopted because it has little undissolved matter and is highly productive.
[0033] Specifically, but not limited to, for example, water is charged into a dissolution tank equipped with an agitator, and a PVA-based resin or the like is charged while stirring the water, and water vapor is blown into the tank under normal pressure, followed by stirring and heating, to prepare an aqueous solution (I) of a desired concentration.
[0034] The dissolution temperature (temperature inside the dissolution tank) is usually 80 to 100° C., preferably 90 to 100° C., and more preferably 92 to 100° C. The dissolution time may be appropriately adjusted depending on the dissolution temperature, the pressure during dissolution, and the like, and is usually 1 to 20 hours, preferably 2 to 15 hours, and particularly preferably 3 to 10 hours. If the dissolution time is too short, undissolved materials tend to remain, and if it is too long, productivity tends to decrease.
[0035] The aqueous solution (I) can be prepared as described above. In this production method, it is important to adjust the solids concentration (D') in order to prevent the remaining undissolved matter and the aggregation of starch. In the above formula (1) (hereinafter, when written as "formula (1)", (1') is also included), the solid content concentration (D') is preferably 0.15 to 0.50, more preferably 0.30 to 0.45, from the viewpoint of suppressing the remaining undissolved matter and the aggregation of starch.
[0036] For example, in one embodiment of the present production method, when the solid content contained in the aqueous solution (I) is only solid content derived from the PVA-based resin, the solid content concentration (D') in the formula (1) is the mass ratio of the solid content in the PVA-based resin to the total amount of the aqueous solution (I) (mass of solid content in the PVA-based resin / total mass of the aqueous solution (I)).
[0037] Furthermore, for example, when the components constituting the aqueous solution (I) are a PVA-based resin, water, and other components, the solid content concentration (D') in the formula (1) is the mass ratio of the total amount of solids in the PVA-based resin and solids in the other components to the total amount of the aqueous solution (I), that is, the solid content concentration (D') is "[mass of solids in the PVA-based resin + mass of solids in the other components] / [total mass of the aqueous solution (I): mass of water + mass of the PVA-based resin + mass of the other components]".
[0038] A representative example of the other components is a surfactant. In this case, the solid content concentration (D') in the formula (1) is the mass ratio of the total amount of the solid content in the PVA resin and the solid content in the surfactant to the total amount of the aqueous solution (I), that is, the solid content concentration (D') is "[the mass of the solid content in the PVA resin + the mass of the solid content in the surfactant] / [the total mass of the aqueous solution (I): the mass of water + the mass of the PVA resin + the mass of the surfactant]".
[0039] In addition, in the case where a surfactant and a component other than the surfactant are used in combination as the other component, the solid content concentration (D') in the formula (1) is the mass ratio of the total amount of the solid content in the PVA-based resin, the solid content in the surfactant, and the solid content in the other components to the total amount of the aqueous solution (I), that is, the solid content concentration (D') is "[mass of the solid content in the PVA-based resin + mass of the solid content in the surfactant + mass of the solid content of the other components] / [total mass of the aqueous solution (I): mass of water + mass of the PVA-based resin + mass of the surfactant + mass of the other components]".
[0040] In one example of a preferred embodiment of the present production method, the content of solids derived from the PVA resin in the total amount of solids contained in the aqueous solution (I) (100 mass%) is 50 to 100 mass%, preferably 55 to 95 mass%, and more preferably 10 to 90 mass%. In one example of a preferred embodiment of the present production method, the content of solid contents derived from other components contained in the aqueous solution (I) relative to 100 parts by mass of solid contents derived from the PVA-based resin contained in the aqueous solution (I) is 0 to 45 parts by mass, preferably 5 to 40 parts by mass, and more preferably 10 to 35 parts by mass.
[0041] In one example of a preferred embodiment of the present production method, the content of the PVA resin relative to the total amount (100 mass%) of the aqueous solution (I) is 15 to 40 mass%, preferably 18 to 38 mass%, and more preferably 20 to 36 mass%.
[0042] In one example of a preferred embodiment of the present production method, the content of water relative to the total amount (100 mass%) of the aqueous solution (I) is 35 to 85 mass%, preferably 40 to 70 mass%, and more preferably 40 to 60 mass%.
[0043] In one example of a preferred embodiment of the present production method, the content of the surfactant relative to the total amount (100 mass%) of the aqueous solution (I) is 3 to 12 mass%, preferably 4 to 10 mass%, and more preferably 5 to 8 mass%.
[0044] In one example of a preferred embodiment of the present production method, the total content of the PVA resin, water, and surfactant relative to the total amount (100 mass%) of the aqueous solution (I) is 85 mass% or more, preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 98 to 100 mass%.
[0045] <Step of preparing aqueous dispersion (II) containing starch (S)> This process is a process in which starch (S), a plasticizer (AP), etc. are dissolved in water etc. to prepare an aqueous dispersion (II) which constitutes a part of the film-forming raw material. The aqueous dispersion (II) containing starch (S) contains at least starch (S) and water, and may contain other optional components such as a plasticizer (AP) as necessary.
[0046] [Starch (S)] Examples of the starch (S) used in the present production method include raw starches (corn starch, potato starch, sweet potato starch, wheat starch, kissaba starch, sago starch, tapioca starch, sorghum starch, rice starch, bean starch, kudzu starch, bracken starch, lotus starch, water chestnut starch, etc.), physically modified starches (α-starch, fractionated amylose, moist heat treated starch, etc.), enzyme modified starches (hydrolyzed dextrin, enzymatically decomposed dextrin, amylose, etc.), chemically decomposed modified starches (acid treated starch, hypochlorite oxidized starch, dialdehyde starch, etc.), chemically modified starch derivatives (esterified starch, etherified starch, cationized starch, crosslinked starch, etc.), etc. These may be used alone or in combination of two or more kinds. Of these, it is preferable to use raw starch, particularly corn starch and rice starch, from the standpoints of biodegradability, availability, economy, and environmental conservation.
[0047] The gelatinization temperature (T) of starch (S) is measured, for example, by an amylograph, and is not particularly limited, but from the viewpoint of suppressing starch aggregation, it is preferably 50 to 95° C., more preferably 53 to 93° C., and particularly preferably 55 to 90° C. The gelatinization temperature (T) can be measured, for example, by the method described on pages 194 to 197 of “Encyclopedia of Starch Science” (edited by Fuwa et al., Asakura Publishing Co., Ltd., 2003).
[0048] The average particle size of the starch is preferably 3 to 50 μm, particularly preferably 5 to 40 μm, and further preferably 8 to 35 μm. If the average particle size is too small, the blocking resistance of the film tends to decrease, whereas if it is too large, the starch particles tend to aggregate with each other, decreasing dispersibility and tending to form pinholes when the film is stretched during molding. The average particle size is a value measured by a laser diffraction particle size distribution measuring device, and is calculated from the D50 value (particle size at 50% of the cumulative size) of the obtained cumulative volume distribution.
[0049] [Plasticizer (AP)] Examples of the plasticizer (AP) include glycerols such as glycerin, diglycerin, and triglycerin, alkylene glycols such as diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, and dipropylene glycol, and sugar alcohols such as trimethylolpropane, sorbitol, xylitol, and maltitol. These may be used alone or in combination of two or more. Among these, glycerin, diglycerin, propylene glycol, polyethylene glycol, and sorbitol are preferred.
[0050] By blending a specific ratio of plasticizer (AP) with aqueous dispersion (II), it tends to be possible to effectively suppress the aggregation of starch. The reason why blending a specific ratio of plasticizer (AP) with aqueous dispersion (II) can effectively suppress the aggregation of starch is not necessarily clear, but it is presumed that the viscosity of aqueous dispersion (II) can be increased, and the frequency of contact between starches contained in aqueous dispersion (II) is reduced, resulting in the suppression of aggregation. Alternatively, starch is mainly composed of amylopectin that forms the skeleton of the particle and amylose contained within the particle, and it is presumed that aggregation is caused when amylose, which tends to flow out at the start of gelatinization, ages, and the plasticizer has a syneresis suppressing effect and a particle association suppressing effect, resulting in the suppression of aggregation.
[0051] When such a plasticizer (AP) is blended in the aqueous dispersion (II), it is preferable to use a polyhydric alcohol having a melting point of 50° C. or less in terms of productivity and mechanical properties of the resulting film, and more preferably a compound that is liquid at about room temperature, and a compound having a melting point of 30° C. or less, particularly preferably 20° C. or less. The lower limit of the melting point is usually −95° C., preferably −60° C., particularly preferably −40° C., even more preferably −15° C., and especially preferably −5° C. Specifically, glycerin, polyethylene glycol, propylene glycol, and the like are preferably used. In addition, when two or more kinds are used in combination, it is preferable to use a polyhydric alcohol having a melting point of 50° C. or less and a polyhydric alcohol having a melting point of 80° C. or more in combination.
[0052] 〔water〕 The water contained in the aqueous dispersion (II) is not particularly limited, but it is preferable to use ion-exchanged water or RO water.
[0053] In addition, the aqueous dispersion (II) may contain solvents other than water, fragrances, rust inhibitors, colorants, extenders, defoamers, ultraviolet absorbers, liquid paraffins, fluorescent brighteners, bitter components (e.g., denatonium benzoate, etc.), surfactants, fillers other than starch (S), etc., within the scope of not impairing the object of the invention. These may be used alone or in combination of two or more. However, the content of these components is preferably less than 65% by mass, more preferably less than 60% by mass, and even more preferably less than 55% by mass, and may be less than 10% by mass, less than 5% by mass, or less than 3% by mass, based on the total amount (100% by mass) of the aqueous dispersion (II).
[0054] Examples of fillers other than starch (S) include organic fillers other than starch and inorganic fillers. These can be used alone or in combination of two or more. The organic filler refers to particulate matter (primary particles) made of organic compounds and having any shape, such as needle-like / rod-like, layered, scaly, or spherical, or an aggregate of such particulate matter (secondary particles). Such organic fillers are mainly selected from polymer compounds, and examples include melamine-based resins, polymethyl (meth)acrylate-based resins, polystyrene-based resins, and biodegradable resins such as polylactic acid.
[0055] [Preparation of aqueous dispersion (II)] The aqueous dispersion (II) is obtained by dispersing each component such as the above-mentioned starch (S), plasticizer (AP), etc., in water. In this process, although not limited thereto, water, starch, etc. are charged into a predetermined dispersion tank and stirred under normal pressure, whereby the aqueous dispersion (II) of a desired concentration can be prepared.
[0056] The temperature during stirring (temperature inside the tank) is not particularly limited, but is, for example, 15 to 35° C., preferably 18 to 30° C., and more preferably 20 to 26° C. The stirring time may be appropriately adjusted, but is usually 1 to 12 hours, preferably 2 to 10 hours, and particularly preferably 2 to 8 hours.
[0057] The aqueous dispersion (II) can be prepared as described above. In the present production method, the starch concentration (S'), the plasticizer concentration (AP'), and the starch ratio (S R It is important to adjust
[0058] [Starch concentration (S')] When the components constituting the aqueous dispersion (II) are starch (S) and water, the starch concentration (S') in the above formula (1) is the mass ratio of starch to the total amount of the aqueous dispersion (II), that is, "mass of starch (S) / [total mass of aqueous dispersion (II):mass of water+mass of starch (S)]". Furthermore, when the components constituting the aqueous dispersion (II) are starch (S), plasticizer (AP), and water, the starch concentration (S') in the above formula (1) is the mass ratio of starch (S) to the total amount of the aqueous dispersion (II), that is, "mass of starch (S) / [total mass of aqueous dispersion (II): mass of water + mass of starch (S) + mass of plasticizer (AP)]". Furthermore, when the components constituting the aqueous dispersion (II) in the present production method include starch (S), plasticizer (AP), water, and other components, the starch concentration (S') in the above formula (1) is the mass ratio of starch (S) to the total amount of the aqueous dispersion (II), that is, "mass of starch (S) / [total mass of aqueous dispersion (II): mass of water + mass of starch (S) + mass of plasticizer (AP) + mass of other components]".
[0059] In the present production method, the starch concentration (S') in the formula (1) is, for example, 0.10 to 0.80, preferably 0.10 to 0.60, and more preferably 0.15 to 0.50, from the viewpoint of suppressing aggregation by suppressing heat conduction to starch, etc.
[0060] [Plasticizer concentration (AP')] When the components constituting the aqueous dispersion (II) are starch (S), a plasticizer (AP), and water, the plasticizer concentration (AP') in the above formula (1) is the solid content (AP) in the plasticizer relative to the total amount of the aqueous dispersion (II). S ), that is, the mass ratio of the solid content in the plasticizer (AP S ) / [total mass of aqueous dispersion (II): mass of water + mass of starch + mass of plasticizer]. In addition, when the components constituting the aqueous dispersion (II) in the present production method include starch (S), plasticizer (AP), water, and other components, the plasticizer concentration (AP') in the formula (1) is the solid content (AP) of the plasticizer relative to the total amount of the aqueous dispersion (II). S ), that is, the mass ratio of the solid content in the plasticizer (AP S ) / [Total mass of aqueous dispersion (II): mass of water + mass of starch (S) + mass of plasticizer (AP) + mass of other components]. In addition, when the aqueous dispersion (II) does not contain the plasticizer (AP), the plasticizer concentration (AP') is 0, and the power of the formula (1) "(D' / S') AP' " (index = 0) will have the value "1".
[0061] In the present production method, the plasticizer concentration (AP') in the formula (1) is, for example, 0 to 0.85, preferably 0 to 0.80, and more preferably 0 to 0.75, from the viewpoint of suppressing aggregation by suppressing heat conduction to the starch (S).
[0062] [Starch ratio (S R )] When the components constituting the aqueous dispersion (II) are starch (S) and water, in the formula (1), the starch ratio (S R ) is the total amount of the aqueous dispersion (II) excluding starch (S) (II -S ), that is, “mass of starch (S) / [total mass of aqueous dispersion (II) excluding starch (S):mass of water]”. In addition, when the components constituting the aqueous dispersion (II) are starch (S), plasticizer (AP), and water, in the formula (1), the starch ratio (S R ) is the total amount of the aqueous dispersion (II) excluding starch (S) (II -S ), that is, “mass of starch (S) / [total mass of aqueous dispersion (II) excluding starch (S):mass of water+mass of plasticizer]”. In addition, when the components constituting the aqueous dispersion (II) in the present production method include starch (S), plasticizer (AP), water, and other components, the starch ratio (S R ) is the total amount of the aqueous dispersion (II) excluding starch (S) (II -S ), i.e., "mass of starch (S) / [total mass of aqueous dispersion (II): mass of water + mass of plasticizer (AP) + mass of other components]".
[0063] In this production method, the starch ratio (S R) is, for example, 0.05 to 0.80, preferably 0.10 to 0.70, and more preferably 0.15 to 0.60, from the viewpoint of suppressing aggregation by suppressing heat conduction to starch, etc.
[0064] In one example of a preferred embodiment of the present production method, the content of starch (S) relative to the total amount (100 mass%) of the aqueous dispersion (II) is 10 to 35 mass%, preferably 15 to 35 mass%, and more preferably 15 to 30 mass%.
[0065] In one example of a preferred embodiment of the present production method, the content of the plasticizer (AP) relative to the total amount (100 mass%) of the aqueous dispersion (II) is 0 to 85 mass%, preferably 0 to 80 mass%, and more preferably 0 to 75 mass%.
[0066] In one example of a preferred embodiment of the present production method, the solid content (AP) of the plasticizer relative to the total amount (100 mass%) of the aqueous dispersion (II) is S The content of ) is 0 to 65 mass %, preferably 0 to 60 mass %, and more preferably 0 to 55 mass %.
[0067] In one example of a preferred embodiment of the present production method, the content (mass %) of water relative to the total amount (100 mass %) of the aqueous dispersion (II) is 15 to 90 mass %, preferably 20 to 85 mass %, and more preferably 25 to 85 mass %.
[0068] In one example of a preferred embodiment of the present production method, the total content of starch and water, or the total content of starch, plasticizer, and water, relative to the total amount (100 mass%) of the aqueous dispersion (II) is 85 mass% or more, preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 98 to 100 mass%.
[0069] <Mixing step of mixing the aqueous solution (I) and the aqueous dispersion (II)> This step is a step of mixing the aqueous solution (I) and the aqueous dispersion (II). For example, the aqueous dispersion (II) is added to a dissolution tank containing the aqueous solution (I) and stirred under normal pressure, thereby preparing a membrane-forming raw material (III) having a desired concentration.
[0070] In this process, the temperature in the dissolution tank before the aqueous dispersion (II) is added, i.e., the temperature of the aqueous solution (I) (D T It is important to adjust (for example, lower) the temperature of the aqueous solution (I) in the above formula (1). T ) is preferably, for example, 90°C or lower, for example, 80 to 90°C, from the viewpoint of suppressing aggregation of starch.
[0071] In addition, in this step, the temperature inside the dissolution tank after the aqueous dispersion (II) is charged, i.e., the temperature of the mixture of the aqueous solution (I) and the aqueous dispersion (II), is preferably, for example, 90°C or lower, e.g., 75 to 88°C, from the viewpoint of suppressing aggregation of starch.
[0072] In this step, the time for mixing the aqueous solution (I) and the aqueous dispersion (II) may be appropriately adjusted depending on the temperature conditions, etc., but is usually 30 seconds to 1 hour, preferably 1 to 30 minutes, and particularly preferably 5 to 20 minutes.
[0073] In this step, the mixing ratio of the aqueous solution (I) and the aqueous dispersion (II) is, for example, preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, and even more preferably 3 to 10 parts by mass of the aqueous dispersion (II) per 100 parts by mass of the aqueous solution (I), from the viewpoint of suppressing aggregation of starch and from the viewpoint of preventing the temperature of the aqueous solution (I) from decreasing too much.
[0074] [Defoaming / filtration process] This step is a step in which the membrane-forming raw material (III) is defoamed and filtered. Examples of such defoaming methods include static defoaming, vacuum defoaming, and twin-screw extrusion defoaming. Of these, static defoaming and twin-screw extrusion defoaming are preferred. The static defoaming temperature is usually 50 to 100°C, preferably 70 to 95°C, and the defoaming time is usually 2 to 30 hours, preferably 5 to 20 hours. Examples of filtration methods include filtration using a disc filter. The disc filter preferably has a mesh size of 10 to 100 μm, and multiple disc filters with different mesh sizes may be used.
[0075] The solid content of the film-forming raw material (III) obtained through the above steps is preferably 10 to 60% by mass, particularly preferably 15 to 50% by mass, and further preferably 20 to 40% by mass. If the concentration is too low, the productivity of the film tends to decrease, while if the concentration is too high, the viscosity becomes too high, which may require a long time to degas the film-forming raw material or may cause die lines during film formation.
[0076] [Film forming process] In the film-forming step, the film-forming raw material (III) is shaped into a film, and a drying treatment is performed as necessary to obtain a water-soluble film. For film formation, for example, a melt extrusion method or a casting method can be adopted, and the casting method is preferred in terms of the accuracy of the film thickness. In carrying out the casting method, for example, the film-forming raw material is extruded from a slit such as a T-shaped slit die, cast onto a casting surface such as an endless belt or a metal surface of a drum roll, a polyethylene terephthalate film, or a plastic substrate such as polypropylene, and then dried to produce a water-soluble film. Specifically, the temperature of the film-forming raw material at the discharge section of the film-forming raw material such as a T-shaped slit die is preferably 60 to 98° C., and particularly preferably 70 to 95° C. If the temperature is too low, the viscosity of the film-forming raw material increases, tending to reduce the productivity of the water-soluble film, whereas if the temperature is too high, foaming and the like tend to occur. After casting, the casting surface, such as the metal surface of an endless belt or drum roll, is heated to dry the film. The surface temperature of the casting surface is preferably 50 to 100° C., and more preferably 70 to 95° C. If the surface temperature is too low, the film tends to have a high moisture content due to insufficient drying, and blocking resistance tends to decrease, whereas if the surface temperature is too high, the film-forming raw material tends to foam, resulting in poor film formation. In addition, in the drying process during film formation, drying with a heated roll, drying by blowing hot air onto the film using a floating dryer, drying with a far-infrared device, a dielectric heating device, or the like can be used in combination.
[0077] After drying the film-forming raw material to a moisture content of 15% by mass or less in the above-mentioned drying process, the water-soluble film is peeled off from the casting surface to obtain a water-soluble film. The water-soluble film peeled off from the casting surface (or the drying heat roll) is conveyed while being cooled in an environment of 10 to 35°C.
[0078] In the film-forming process, the water-soluble film peeled off from the cast surface after drying is transported and wound up around a core tube to prepare a film roll. The obtained film roll can be supplied as a product as it is, but it can also be preferably supplied as a film roll slit into a film width of a desired size.
[0079] In this manner, a water-soluble film can be produced.
[0080] <<Water-soluble film>> The water-soluble film obtained by this manufacturing method is a water-soluble film mainly composed of a PVA-based resin. Here, "mainly composed of a PVA-based resin" means that the PVA-based resin is usually contained in an amount of 50% by mass or more, preferably 55% by mass or more, and particularly preferably 60% by mass or more, based on the entire water-soluble film. If the content is too low, the solubility in water and the mechanical properties of the film tend to decrease. The upper limit of the content is usually 99% by mass or less, preferably 95% by mass or less, and particularly preferably 90% by mass or less, from the viewpoint of shape stability over time when used as a liquid detergent package.
[0081] The term "water-soluble film" refers to a film that dissolves in water at room temperature (20°C). In the present invention, the solubility of a film can be evaluated as follows: A water-soluble film is cut to a size of 3 cm x 5 cm, placed in a 1-liter beaker containing water (1 liter) and fixed with a jig, and stirred with a stirrer (rotor length 3 cm, rotation speed 750 rpm) while maintaining the water temperature at 20°C. The film is deemed dissolved when no dispersion of insoluble fine particles with a diameter of 1 mm or more is visually observed.
[0082] The thickness of the water-soluble film obtained by the present production method is appropriately selected depending on the application, etc., but is preferably 10 to 130 μm, particularly preferably 15 to 110 μm, and further preferably 20 to 100 μm. If the thickness is too thin, the mechanical strength of the film tends to decrease, while if the thickness is too thick, the dissolution rate in water tends to decrease and the film formation efficiency also tends to decrease.
[0083] The width of the water-soluble film is appropriately selected depending on the application, etc., but is preferably 300 to 5000 mm, particularly preferably 500 to 4000 mm, and further preferably 600 to 3000 mm. If the width is too narrow, production efficiency tends to decrease, and if it is too wide, slackness and control of the film thickness tend to become difficult.
[0084] The length of the water-soluble film is appropriately selected depending on the application, etc., but is preferably 100 to 20,000 m, particularly preferably 800 to 15,000 m, and further preferably 1,000 to 10,000 m. If the length is too short, switching the film tends to be troublesome, while if it is too long, the film tends to become too heavy or have a poor appearance due to tight winding.
[0085] In addition, the surface of the water-soluble film may be smooth, but from the standpoint of blocking resistance, slipperiness during processing, reduced adhesion between products, and appearance, it is also preferable to apply an embossed pattern, a fine uneven pattern, a special engraved design, or other uneven surface finish to one or both sides of the film.
[0086] In addition, the water content of the water-soluble film is preferably 3 to 15% by mass, particularly preferably 5 to 10% by mass, and further preferably 6 to 8% by mass, in terms of mechanical strength and heat sealability. If the water content is too low, the film becomes too hard, which tends to reduce the formability when made into a package and the impact resistance of the package, or to cause poor sealing, while if the water content is too high, blocking tends to occur. The water content can be adjusted to this level by appropriately setting the drying conditions and humidity control conditions. The moisture content is measured in accordance with JIS K 6726 3.4, and the obtained value of the volatile matter is regarded as the moisture content.
[0087] (Application) Water-soluble films are useful for various packaging applications, such as unit packaging applications for pharmaceuticals such as pesticides and detergents, (hydraulic) transfer films, sanitary products such as napkins and paper diapers, waste disposal products such as ostomy bags, medical products such as blood-absorbing sheets, temporary base materials such as seedling sheets, seed tapes, and embroidery base fabrics, etc. They are particularly suitable for use in unit packaging applications for pharmaceuticals such as laundry detergents and dishwashing detergents.
[0088] [Drug packaging] The drug package is a package made of a water-soluble film that contains a drug or the like. The individual package maintains the shape containing the drug or the like during storage. When used, the package is placed in water and the individual package (water-soluble film) dissolves when it comes into contact with water, and the drug or the like dissolves or disperses from the individual package in the water, exerting the effects of the drug.
[0089] Examples of the drug to be encapsulated include pesticides such as insecticides, fungicides, and herbicides, fertilizers, and detergents, and detergents such as laundry detergent and dishwashing detergent are particularly preferred. The drug may be in the form of a liquid, solid, or gel, and in the case of a liquid, it is in the form of a liquid, and in the case of a solid, it may be in the form of a granule, tablet, or powder. The drug is preferably one that is dissolved or dispersed in water and used, and is particularly useful for packaging liquid detergents. The pH of the drug may be alkaline, neutral, or acidic.
[0090] The liquid detergent preferably has a pH value of 6 to 12, particularly preferably 6.5 to 11, and further preferably 7 to 8. The liquid detergent also preferably has a water content of 15% by mass or less, particularly preferably 0.1 to 10% by mass, and further preferably 0.1 to 7% by mass. Within this range, the water-soluble film will not gel or become insoluble, and will have excellent water solubility. The pH value is measured in accordance with JIS K 3362 8.3, and the water content is measured in accordance with JIS K 3362 7.21.3. The viscosity of the liquid detergent is not particularly limited as long as it is a liquid agent that is fluid and changes shape to fit the container, but is preferably 10 to 200 mPa s. The viscosity of such a liquid agent is measured with a B-type rotational viscometer at room temperature.
[0091] When using a water-soluble film to package a drug such as a liquid detergent to produce a drug package, a known method can be used. For example, a method for producing a drug package using two or more water-soluble films includes a method for vacuum-molding a first water-soluble film with a mold, pouring a drug into the first water-soluble film formed by the vacuum molding, and bonding the formed first water-soluble film to another second water-soluble film to package the drug to produce a drug package. EXAMPLES
[0092] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are based on mass.
[0093] First, the following materials were prepared: ·PVA resin (1): A carboxyl-modified PVA resin (volatile content 5% by mass) with a viscosity of 22 mPa s in a 4% by mass aqueous solution at 20°C, an average degree of saponification of 94% by mole, and a modification amount of 2.2% by mole with monomethyl maleate. ·PVA resin (2): Unmodified PVA resin with a viscosity of 22 mPa s in a 4% by weight aqueous solution at 20°C and an average degree of saponification of 88 mol% (volatile content: 5% by weight) ·Starch (S): Cornstarch (gelatinization temperature: 67℃, average particle size: 20μm) Plasticizer (AP): Glycerin (solid content 87.5% by mass) Surfactants: Polyoxyalkylene alkyl ether phosphate monoethanolamine salt (solid content 91.3% by mass)
[0094] <Example 1> Water was added to a dissolution tank equipped with an agitator, and while stirring the water (temperature 15-20°C), PVA resin (1) and surfactant were added to the tank. Steam was then blown in under normal pressure to raise the temperature in the tank to 95°C or higher, and the mixture was stirred and heated at the same temperature for 2-3 hours to obtain an aqueous solution (I). The solid content (D') in the prepared aqueous solution (I) is shown in Table 1. On the other hand, water was poured into a dispersion tank equipped with an agitator, and while stirring the water (water temperature 15 to 20°C), starch (S) was poured into the tank. The water was stirred for 1 to 2 hours under the condition that the temperature inside the tank was 30°C or less, and an aqueous dispersion (II) was obtained. The starch concentration (S') and starch ratio (S R ) and plasticizer concentration (AP') are shown in Table 1. Next, the temperature of the aqueous solution (I) in the dissolution tank (D T ) was adjusted to 82°C, and 10 parts by mass of the aqueous dispersion (II) were added to 100 parts by mass of the aqueous solution (I), and the aqueous solution (I) and the aqueous dispersion (II) were mixed by stirring to prepare a membrane-forming raw material (III).
[0095] Using the film-forming raw material (III), a film was formed by casting at a speed of 10 m / min using a belt film-forming machine equipped with a stainless steel endless belt whose surface temperature was adjusted to 80°C, and the film was dried at a temperature of 110°C to obtain a water-soluble film with a moisture content of 9% (film width: 1300 mm, film length: 1000 m, film thickness: 90 μm).
[0096] [Cohesion evaluation] The water-soluble film obtained using the film-forming material (III) was cut into a size of 30 cm x 30 cm, and starch aggregates were confirmed using a digital microscope. The results are shown in Table 1. [Evaluation Criteria] No aggregates with a maximum length of 200 μm or more were observed. △: Aggregates with a maximum length of 200 μm or more and less than 300 μm were observed. × Aggregates with a maximum length of 300 μm or more were observed.
[0097] <Examples 2 to 7, Comparative Examples 1 to 2> The composition and amounts of the PVA resin (1), starch, surfactant, and plasticizer were appropriately adjusted, and the film-forming raw materials (III) and water-soluble films shown in Table 1 were obtained according to the manufacturing method of Example 1. The obtained water-soluble films were evaluated in the same manner as above. The results are shown in Table 1.
[0098] <Examples 8 and 9> The PVA resin (1) was replaced with the PVA resin (2), and the composition and amounts of the PVA resin (2), starch, surfactant, and plasticizer were appropriately adjusted to obtain the film-forming raw material (III) and water-soluble films shown in Table 1 according to the manufacturing method of Example 1. The obtained water-soluble films were evaluated in the same manner as above. The results are shown in Table 1.
[0099] In Comparative Examples 1 and 2 and Examples 1, 4, 5, 8, and 9, the aqueous solution (I) contains a PVA resin and a surfactant, the aqueous dispersion (II) contains starch, and no plasticizer. In Examples 2, 3, 6, and 7, the aqueous solution (I) contains a PVA resin and a surfactant, and the aqueous dispersion (II) contains starch and a plasticizer.
[0100] [Table 1]
[0101] As shown in Table 1, the starch aggregation index (S ID In Comparative Examples 1 and 2, where the difference in the particle diameter was more than 0.50, it was confirmed that the starch was not uniformly dispersed and large aggregates were present. On the other hand, the starch aggregation index (S ID In the examples of the present application in which the ratio of the starch content to the total content is 0.50 or less, it was confirmed that the starch is uniformly dispersed and no large aggregates are present. Therefore, a film having no cracks and excellent blocking resistance can be obtained, and is particularly suitable for packaging applications since it does not break or leak contents when used as a package. [Industrial Applicability]
[0102] According to the film-forming raw material for the water-soluble film and the manufacturing method for the water-soluble film of the present invention, it is possible to obtain a water-soluble film having excellent crack resistance and blocking resistance. Such a water-soluble film can be suitably used for various packaging applications, and is particularly useful for unit packaging applications for medicines, etc.
Claims
1. A step of preparing an aqueous solution (I) containing a polyvinyl alcohol-based resin; preparing an aqueous dispersion (II) comprising starch (S) and optionally a plasticizer (AP); A mixing step of mixing the aqueous solution (I) and the aqueous dispersion (II), The method for producing a water-soluble film, wherein the mixing step satisfies the condition shown in the following formula (1): (Formula) {[(D' / S') AP' ]×(D T / T) x S R}≦0.50 ... (1) D': solid content contained in the aqueous solution (I) (D S ) to the total amount of the aqueous solution (I) (D S / I). S': mass ratio (S / II) of the starch (S) contained in the aqueous dispersion (II) to the total amount of the aqueous dispersion (II). AP': solid content (AP) of the plasticizer (AP) contained in the aqueous dispersion (II) S ) to the total amount of the aqueous dispersion (II) (AP S / II). When the aqueous dispersion (II) does not contain a plasticizer (AP), it is 0. S R : Starch (S) contained in the aqueous dispersion (II) and the total amount of the aqueous dispersion (II) excluding the starch (S) (II -S ) and the mass ratio (S / II -S ). D T : Temperature of the aqueous solution (I) [°C]. T: Gelatinization temperature of starch (S) [°C].
2. The method for producing a water-soluble film according to claim 1 , wherein the mixing step satisfies the condition shown in the following formula (1′): (Formula) {[(D' / S') AP' ]×(D T / T) x S R}≦0.35 ... (1')
3. 3. The method for producing a water-soluble film according to claim 1 or 2, wherein the step of preparing the aqueous dispersion (II) is a step of preparing an aqueous dispersion (II) containing starch (S) and a plasticizer (AP).
4. 3. The method for producing a water-soluble film according to claim 1, wherein the step of preparing the aqueous solution (I) is a step of preparing an aqueous solution (I) containing a polyvinyl alcohol-based resin and a surfactant.
5. The gelatinization temperature (T) of the starch (S) is 50 to 95° C., and the temperature (D T 3. The method for producing a water-soluble film according to claim 1, wherein the temperature is 15 to 35° C.
Citation Information