Polyethylene-based resin formed sheet
A polyethylene resin foam sheet with an ionomer type antistatic agent and controlled density and resistivity addresses dust adsorption and tearing issues, ensuring flexibility and strength for packaging applications.
Patent Information
- Application Number
- JP2023053249
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polyethylene resin foam sheets require improved antistatic properties to reduce dust adsorption due to static electricity accumulation, while maintaining flexibility and resistance to tearing.
A polyethylene resin foam sheet with a foam layer containing 1.0 to 5.0 parts by mass of an ionomer type antistatic agent per 100 parts by mass of polyethylene resin, achieving a surface resistivity of 5.0×10^14 Ω to 9.0×10^16 Ω and an apparent density of 40 mg/cm^3 or less, ensuring flexibility and high tear strength.
The sheet effectively reduces dust adsorption and maintains flexibility and tear resistance, making it suitable for packaging and transporting large items without tearing or staining.
Smart Images

Figure 2024141535000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyethylene resin foam sheet. [Background technology]
[0002] Patent Document 1 discloses an extruded polyethylene resin foam sheet made of a resin composition containing a polyethylene resin and an ionomer resin antistatic agent. From the viewpoint of stably exhibiting the antistatic properties desired for use as an interleaf for glass plates, this extruded polyethylene resin foam sheet has an apparent density of 15 to 200 kg / m 3 (15-200mg / cm 3 ) and has a volume resistivity of 1×10 13 It is essential that the resistivity be Ω·cm or less. Patent Document 1 explains that when the content of the ionomer resin antistatic agent in the extruded polyethylene resin foam sheet is 5 to 50% by weight relative to 100% by weight of the total of the polyethylene resin and the ionomer resin antistatic agent, the sheet is excellent in flexibility and can stably exhibit antistatic properties, which is preferable. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2021-134258 A Summary of the Invention [Problem to be solved by the invention]
[0004] On the other hand, polyethylene resin foam sheets are not required to have high antistatic properties as described in Patent Document 1, and it is considered that in some cases it is sufficient to have antistatic properties to the extent that they can reduce the adhesion of dust due to the accumulation of static electricity. In some cases, it is considered that rather than antistatic properties, it is more desirable to have physical properties that are difficult to tear and flexible.
[0005] Therefore, an object of the present invention is to provide a polyethylene resin foamed sheet which is tear-resistant, flexible, and has antistatic properties to such an extent that dust adsorption can be reduced. [Means for solving the problem]
[0006] In order to solve the above-mentioned problems, a polyethylene-based resin foamed sheet according to one embodiment is a polyethylene-based resin foamed sheet having a foam layer and a sheet surface constituted by a polyethylene-based resin composition containing a polyethylene resin, the polyethylene-based resin composition containing 1.0 part by mass or more and 5.0 parts by mass or less of an ionomer-type antistatic agent relative to 100 parts by mass of the polyethylene resin, and the apparent density of the foamed layer is 40 mg / cm. 3 The surface resistivity of the sheet surface is 5.0×10 or less. 14 Ω or more 9.0×10 16 Ω or less.
[0007] According to the polyethylene resin foam sheet, the sheet surface is constituted by a polyethylene resin composition containing a polyethylene resin and an ionomer type antistatic agent in the above-mentioned ratio of parts by mass, and therefore the sheet surface has a relatively high tear strength and a surface resistivity of 5.0×10 14 Ω or more 9.0×10 16 The foam layer tends to have antistatic properties to a degree that can reduce the adhesion of dust, that is, within the range of Ω or less. In addition, the foam layer has an apparent density of 40 mg / cm 3 The following tends to make it more flexible: Effect of the Invention
[0008] As described above, the present invention can provide a polyethylene resin foamed sheet that is tear-resistant, flexible, and has antistatic properties to such an extent that dust adsorption can be reduced. [Brief description of the drawings]
[0009] [Figure 1]FIG. 1 is a schematic cross-sectional view showing the structure of a polyethylene resin foam sheet according to one embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing the structure of a polyethylene resin foam sheet according to another embodiment. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing the structure of a polyethylene resin foam sheet according to still another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. One embodiment shown in FIG. 1 is a resin foam sheet 10a having only a foam layer 11 made of a polyethylene resin composition (hereinafter also referred to as "the resin composition"). Since it has a single-layer structure only with the foam layer 11, both sheet surfaces (15a, 16a) of the resin foam sheet 10a are each made of the resin composition. Such a single-layer structure can be formed, for example, by an extrusion foaming method. For example, the resin foam sheet 10a can be produced by a method in which the resin composition as a raw material is melt-kneaded together with a foaming agent inside an extruder, and the resulting melt-kneaded product is extruded into a sheet shape from a die attached to the extruder and foamed.
[0011] From the viewpoint of increasing the strength of the outermost layer to make it difficult to tear, as shown in FIG. 2, the resin foam sheet 10b may have a two-layer structure including a foamed layer 11 and a first non-foamed layer 21 laminated on one surface of the foamed layer 11. In the resin foam sheet 10b, the first non-foamed layer 21 constitutes one sheet surface 15b as the outermost layer, and the foamed layer 11 constitutes the other sheet surface 16a. Since the foamed layer 11 and the first non-foamed layer 21 are each made of the resin composition, each sheet surface (15b, 16a) is made of the resin composition. Similarly, from the viewpoint of increasing the strength of the outermost layer to make it difficult to tear, as shown in FIG. 3, the resin foam sheet 10c may have a three-layer structure including, in order, a first non-foamed layer 21, a foamed layer 11, and a second non-foamed layer 22 made of the resin composition. In the resin foam sheet 10c, the sheet surface 15b on one side is made of the resin composition in the first non-foamed layer 21, the foamed layer 11 is disposed in the center in the sheet thickness direction, and the sheet surface 16b on the other side is made of the resin composition in the second non-foamed layer 22. Each non-foamed layer (21, 22) is a layer that does not substantially have air bubbles. As shown in Figs. 2 and 3, each resin foam sheet (10b, 10c) having a laminated structure can be manufactured, for example, by a method of laminating a polyethylene-based resin film to be the non-foamed layer (21, 22) after once producing a resin foam sheet 10a having only the foamed layer 11, or a method of co-extruding a foamed layer and a non-foamed layer from a die of an extruder. Thus, the resin foam sheet according to the present invention is not limited to a single-layer structure.
[0012] Hereinafter, one embodiment will be described mainly based on the resin foam sheet 10a shown in Fig. 1. The foam layer 11 of the resin foam sheet 10a is made of the resin composition (polyethylene-based resin composition) containing a polyethylene resin and an ionomer-type antistatic agent.
[0013] The polyethylene resin contained in the resin composition is produced, for example, by a catalytic method (medium-low pressure polymerization method), has almost no branching in its molecular structure, and has a modulus of 942 kg / m 3The polyethylene resin contained in the resin composition is produced by a catalytic method (medium-low pressure polymerization method) and has a density of 910 kg / m or more by introducing a comonomer. 3 More than 925kg / m 3 The polyethylene resin contained in the resin composition may be a medium density polyethylene resin (PE-MD) or the like, which is prepared to have a density between the linear low density polyethylene resin (PE-LLD) and the high density polyethylene resin (PE-HD). The resin composition may contain a very low density polyethylene resin (PE-VLD) as the polyethylene resin. The polyethylene resin contained in the resin composition may be, for example, a low density polyethylene resin (PE-LD) prepared by a high pressure polymerization method and having long chain branches in the molecular structure. The polyethylene resin contained in the resin composition may be a polyethylene resin derived from fossil fuels from the viewpoint of easy procurement of raw materials, or may be a polyethylene resin derived from plants from the viewpoint of reducing environmental load.
[0014] For polyethylene resins, the number of molecular ends increases as the number of branches increases even if the molecular weight is the same. Therefore, even between polyethylene resins with the same average molecular weight, a polyethylene resin with more branches (lower melt mass flow rate value) tends to have a somewhat bulkier molecular structure and tends to have a moderately low melt mass flow rate. The melt mass flow rate (MFR) of the polyethylene resin is preferably 7.0 g / 10 min or less, more preferably 6.0 g / 10 min or less, and even more preferably 5.0 g / 10 min or less. From the viewpoint of reducing the equipment load when producing the resin foam sheet 10a (foam layer 11) by the extrusion foaming method, the melt mass flow rate (MFR) of the polyethylene resin is preferably 0.1 g / 10 min or more, more preferably 0.2 g / 10 min or more, and even more preferably 0.3 g / 10 min or more.
[0015] The melt mass flow rate (MFR) can be measured according to JIS K7210:1999 "Plastics - Test method for melt mass flow rate (MFR) and melt volume flow rate (MVR) of thermoplastic plastics". The melt mass flow rate (MFR) can be measured according to "b) Method for measuring the time it takes for a piston to move a specified distance" described in Method B of the same standard. Specifically, the melt mass flow rate (MFR) can be measured using, for example, "Semi-Auto Melt Indexer 2A" manufactured by Toyo Seiki Seisakusho Co., Ltd.
[0016] The measurement conditions for the melt mass flow rate (MFR) can be as follows. (Melt mass flow rate measurement method) Sample: 3-8g Preheat: 270 seconds Load Hold: 30 seconds Test temperature: 190℃ Test load: 21.18N Piston travel distance (interval): 25mm The test is performed on a sample three times, and the average of the three tests can be used as the melt mass-flow rate (g / 10 min).
[0017] From the viewpoint of easy foaming, the resin composition constituting the foamed layer 11 may be a resin composition (hereinafter also referred to as "first resin composition") in which a virgin polyethylene resin and an ionomer type antistatic agent are mixed. From the viewpoint of promoting material recycling, the resin composition constituting the foamed layer 11 is preferably a resin composition in which a first resin composition and a recycled polyethylene resin are mixed. In other words, in this case, it can be said that a part of the polyethylene resin contained in the resin composition constituting the foamed layer 11 is recycled polyethylene resin. In this case, the content of the ionomer type antistatic agent decreases as the mixed amount of the recycled polyethylene resin increases relative to the amount of the first resin composition. The ionomer type antistatic agent is mixed so that it is contained in the resin composition at a content described below.
[0018] From the viewpoint of promoting material recycling, it is also preferable that the resin composition constituting the foam layer is a recycled resin composition containing a polyethylene resin and an ionomer resin (second resin composition: hereinafter also referred to as "recycled resin composition"). From the same viewpoint, it is also preferable that the resin composition constituting the foam layer is a resin composition obtained by mixing a virgin polyethylene resin and a recycled resin composition. In other words, in these cases, it can be said that a part or all of the polyethylene resin contained in the resin composition constituting the foam layer 11 is a recycled polyethylene resin. In general, compared with so-called low molecular weight antistatic agents such as cationic surfactants and anionic surfactants, ionomer type antistatic agents have a large molecular weight and are therefore difficult to disperse in the resin composition. On the other hand, compared with the first resin composition, the recycled resin composition is a composition in which the polyethylene resin contained therein is repeatedly melt-kneaded and contains many molecular chains with relatively small molecular weights, so it is considered that the ionomer type antistatic agent is easily dispersed homogeneously in the resin composition, and is also preferable from the viewpoint that antistatic properties are easily exhibited even when the content of the ionomer type antistatic agent is small.
[0019] The recycled resin composition is preferably derived from a resin product (resin molded product) made of a resin composition containing a polyethylene resin and an ionomer type antistatic agent. Examples of resin products that can be used as starting materials for the recycled resin composition include disused resin foam sheets (resin foam sheets that are no longer expected to be used, resin foam sheets after being used as packaging materials, etc.). For example, the recycled resin composition can be prepared by melt-kneading such resin products.
[0020] From the viewpoints of promoting material recycling, facilitating obtaining high tear strength, and dispersibility described below, it is more preferable that the resin composition constituting the foamed layer 11 is a resin composition obtained by mixing a first resin composition and a recycled resin composition (a second resin composition). Regarding dispersibility, the recycled resin composition has a lower average molecular weight of the polymer than the state before it is used to manufacture a resin product due to ultraviolet degradation that occurs during the use of the resin product that is the starting material, and thermal degradation during the manufacture and recycling of the resin product. Therefore, the melting point of the recycled resin composition is lower and the melt mass flow rate value is higher than before it is used. A recycled resin composition that has a lower melting point and a higher melt mass flow rate value than the first resin composition shows good dispersibility with respect to the first resin composition.
[0021] The melting point of the recycled resin composition (second resin composition) may be 1°C or more lower than the melting point of the first resin composition, 2°C or more lower than the melting point of the first resin composition, or 5°C or more lower than the melting point of the first resin composition. The melt mass flow rate value of the recycled resin composition may be 0.1g / 10min or more higher, 0.2g / 10min or more higher, or 0.5g / 10min or more higher than the melting point of the first resin composition. The recycled resin composition (second resin composition), which can be said to be a polyethylene-based recycled resin composition recovered and recycled from a resin product, is particularly effective when there is a large gap between the melt mass flow rate value of the ionomer-type antistatic agent and the melt mass flow rate value of the polyethylene resin. The difference with the melt mass flow rate value of the ionomer-type antistatic agent may be 3g / 10min or more, 5g / 10min or more, or 7g / 10min or more. The difference from the melt mass flow rate value of the ionomer type antistatic agent is preferably 20 g / 10 min or less.
[0022] When the first resin composition and the recycled resin composition (second resin composition) are mixed to prepare the resin composition, the recycled resin composition may have a lower or higher content of an ionomer type antistatic agent than the first resin composition. When the virgin polyethylene or the first resin composition and the recycled resin composition (second resin composition) are mixed to prepare the resin composition, a resin product having a relatively high content of an ionomer type antistatic agent can be recycled as a starting material for the recycled resin composition. An example of such a resin product is a polyethylene-based resin foam sheet for interleaving a glass substrate, which contains an ionomer type antistatic agent as an antistatic agent. For example, a recycled resin composition (second resin composition) is prepared using a resin foam sheet used as an interleaving sheet for a glass substrate as a starting material, and the recycled resin composition is mixed with the first resin composition to prepare the resin composition, and the resin foam sheet 10a (foam layer 11) can be manufactured by an extrusion foaming method. In this case, by using a first resin composition having a low content of ionomer-type antistatic agent as the first resin composition to be mixed with the recycled resin composition (second resin composition), it is possible to produce a resin foam sheet 10a (foam layer 11) having a lower content of ionomer-type antistatic agent than the resin foam sheet used as the starting material. This method of production is preferable from the viewpoint of producing the resin foam sheet 10a at low cost by effectively recycling the ionomer-type antistatic agent, which is expensive compared to so-called low-molecular-weight antistatic agents.
[0023] The ionomer type antistatic agent contained in the resin composition is a kind of polymer type antistatic agent, and is a high molecular weight compound having carboxylate and / or sulfonate in the molecule. Compared with so-called low molecular weight antistatic agents, the ionomer type antistatic agent can prevent the migration of low molecular weight surfactant molecules to the sheet surface (15a, 16a) by bleeding out. Therefore, when the resin foam sheet 10a is used for packaging an article, it has an advantage that it is easy to prevent the bleed-out surfactant from adhering to the packaged article (hereinafter also referred to as "packaged article") and causing the packaged article to be soiled. In addition, compared with other types of polymer type antistatic agents (for example, polyalkylene oxide type antistatic agents which are copolymers of olefin blocks and hydrophilic blocks such as ethylene oxide or propylene oxide), the ionomer type antistatic agent is effective in preventing lithium ions or sodium ions from migrating to the sheet surface (15a, 16a) when the resin composition contains these ions, and is considered to easily exhibit antistatic properties even in a relatively small amount.
[0024] The salt contained in the molecular structure of the ionomer type antistatic agent may be a carboxylate or a sulfonate. The ionomer type antistatic agent is preferably a copolymer containing ethylene and an unsaturated carboxylic acid as a constituent unit. The copolymer may be a random copolymer, a block copolymer, or a graft copolymer.
[0025] As the ethylene-unsaturated carboxylic acid copolymer, for example, one having a structure in which a part or all of the carboxyl groups are neutralized with an alkali metal or the like can be used. As the unsaturated carboxylic acid, for example, acrylic acid, methacrylic acid, maleic anhydride, monomethyl maleate, monoethyl maleate, etc. can be mentioned. As the unsaturated carboxylic acid, acrylic acid or methacrylic acid is preferable. In the ethylene-unsaturated carboxylic acid copolymer, examples of other monomers that can be structural units in addition to ethylene and unsaturated carboxylic acid include vinyl esters such as vinyl acetate, unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, isobutyl acrylate, n-butyl acrylate, isooctyl acrylate, and methyl methacrylate, and carbon monoxide.
[0026] The ethylene-unsaturated carboxylic acid random copolymer may contain, for example, an ethylene component in a ratio of 60% by mass or more and 90% by mass or less. The ratio of the ethylene component may be 70% by mass or more and 88% by mass or less. The ethylene-unsaturated carboxylic acid random copolymer may contain, for example, an unsaturated carboxylic acid component in a ratio of 10% by mass or more and 40% by mass or less. The ratio of the unsaturated carboxylic acid component may be 12% by mass or more and 30% by mass or less. The ethylene-unsaturated carboxylic acid random copolymer may contain, for example, another unsaturated monomer component in a content of 30% by mass or less. The content of the other unsaturated monomer component is preferably 20% by mass or less. The ethylene-unsaturated carboxylic acid random copolymer is preferably an ethylene-methacrylic acid random copolymer.
[0027] The ion source of the ionomer is preferably an alkali metal (i.e., lithium, sodium, potassium, rubidium or cesium), more preferably potassium. The content of the alkali metal cation in the ionomer is desirably in the range of 0.4 mol to 4.0 mol, preferably 0.6 mol to 2.0 mol, per 1.0 kg of the ionomer type antistatic agent.
[0028] From the viewpoint of easily dispersing the ionomer type antistatic agent homogeneously in the resin composition, the melt mass flow rate of the ionomer type antistatic agent is preferably 10 g / 10 min or more, more preferably 11 g / 10 min or more. The melt mass flow rate of the ionomer type antistatic agent may be, for example, 25 g / 10 min or less, 20 g / 10 min or less, or 15 g / 10 min or less.
[0029] An ionomer type antistatic agent having a small melt mass-flow rate may be used from the viewpoint of increasing the melt viscosity of the resin composition and making it easier to suppress the variation in bubble expansion in the surface layer portion of the foamed layer 11. The ionomer type antistatic agent used for such a purpose may have a melt mass-flow rate of, for example, less than 10 g / 10 min, 8.0 g / 10 min or less, 6.0 g / 10 min or less, or 5.0 g / 10 min or less, and can be, for example, 1.0 g / 10 min or more.
[0030] From the viewpoint of easily dispersing the ionomer type antistatic agent homogeneously in the resin composition and preventing the variation in bubble expansion from becoming too large, the melt mass flow rate of the ionomer type antistatic agent is preferably 25 g / 10 min or less or 20 g / 10 min or less, more preferably 15 g / 10 min or less. From the viewpoint of easily suppressing the variation in bubble expansion in the surface layer portion of the foamed layer 11, the melt mass flow rate of the ionomer type antistatic agent is preferably 1.0 g / 10 min or more or 2.0 g / 10 min or more, more preferably 3.0 g / 10 min or more.
[0031] The resins contained in the resin composition include a polyethylene resin as a base resin and an ionomer type antistatic agent. The resin composition may contain other resins. The total amount of the polyethylene resin and the ionomer type antistatic agent in the resins contained in the resin composition may be, for example, 85% by mass or more, and may be 90% by mass or more, 95% by mass or more, or 98% by mass or more.
[0032] The resin contained in the resin composition may be only a polyethylene resin and an ionomer type antistatic agent. Alternatively, the content of the resin other than the polyethylene resin and the ionomer type antistatic agent among the resins contained in the resin composition may be, for example, less than 15 mass%, or may be less than 10 mass%, less than 5 mass%, or less than 2 mass%, or may be substantially zero. The content of the polyethylene resin in the resin composition may be, for example, 75 mass% or more, or may be 80 mass% or more, or 85 mass% or more.
[0033] The content of the ionomer type antistatic agent in the resin composition is 1.0 part by mass or more, preferably 1.5 parts by mass or more, and may be 2.5 parts by mass or more, based on 100 parts by mass of the polyethylene resin contained in the resin composition, from the viewpoint of reducing the adsorption of dust due to the accumulation of static electricity. From the same viewpoint, the content of the ionomer type antistatic agent in the resin composition may be, for example, 1.0% by mass or more, preferably 1.5% by mass or more, and may be 2.4% by mass or more. If the content of the ionomer type antistatic agent in the resin composition is less than 1.0 part by mass with respect to 100 parts by mass of the polyethylene resin, problems such as the adsorption of dust to impair cleanliness and aesthetics due to the possibility of accumulation of static electricity are likely to become apparent.
[0034] On the other hand, if the content of the ionomer-type antistatic agent in the resin composition constituting the foam layer 11 is too high, the polyethylene resin becomes insufficient, resulting in a loss of flexibility unique to polyethylene resin, or the resin composition becomes difficult to foam, resulting in an insufficient thickness of the foam layer 11, and the tear strength of the resin foam sheet 10a (foam layer 11) is likely to decrease. In addition, when the resin foam sheet 10a is used as a cushioning material for packaging and transporting a large and hard article (packaged item) such as an automobile bumper, if the tear strength of the foam layer is insufficient, the foam layer may tear during transportation, failing to fully exert its cushioning effect, and the packaged item may be damaged. For this reason, from the viewpoint of imparting sufficient tear strength to the foamed layer 11, when the content of the polyethylene resin in the resin composition is taken as 100 parts by mass, the content of the ionomer type antistatic agent in the resin composition is 5.0 parts by mass or less, preferably 4.5 parts by mass or less, more preferably 4.0 parts by mass or less or 3.5 parts by mass or less, even more preferably 3.0 parts by mass or less, and may be 2.0 parts by mass or less. From the same viewpoint, the content of the ionomer type antistatic agent in the resin composition may be, for example, 4.8% by mass or less, preferably 4.3% by mass or less, more preferably 3.8% by mass or less or 3.4% by mass or less, even more preferably 2.9% by mass or less, and may be 2.0% by mass or less.
[0035] When a resin foam sheet 10a (foam layer 11) is produced using a resin composition obtained by mixing a virgin polyethylene resin or the first resin composition described above with the recycled resin composition (second resin composition) described above, if the content of the ionomer type antistatic agent in the recycled resin composition is within a certain range, it is preferable because the content of the ionomer type antistatic agent in the resin composition can be easily adjusted to be within an appropriate range later. From this viewpoint, in the polyethylene resin composition constituting the recycled resin composition (second resin composition) or the resin product that is the starting material thereof, the content of the ionomer type antistatic agent per 100 parts by mass of polyethylene resin is preferably 2.0 parts by mass or more and 15 parts by mass or less, more preferably 3.0 parts by mass or more and 10 parts by mass or less.
[0036] When at least a part of the resin composition is the above-mentioned recycled resin composition (second resin composition), from the viewpoint of promoting material recycling and from the viewpoint of easily imparting strength and flexibility to the resin foam sheet 10a (foam layer 11), the mass ratio of the recycled resin composition to the resin composition (mass of recycled resin composition / mass of polyethylene resin composition) may be, for example, 0.10 or more, preferably 0.20 or more, more preferably 0.30 or more, and may be 0.40 or more, 0.50 or more, or 0.60 or more. When at least a part of the resin composition is a recycled resin composition, from the viewpoint of easily preparing the resin composition having an appropriate content of the ionomer type antistatic agent, the mass ratio of the recycled resin composition to the resin composition (mass of recycled resin composition / mass of polyethylene resin composition) may be, for example, 0.90 or less, preferably 0.80 or less or 0.70 or less, more preferably 0.60 or less, and may be 0.50 or less or 0.40 or less.
[0037] The resin composition may contain not only the polyethylene resin and the ionomer type antistatic agent, but also other additives as necessary. Examples of the other additives include lubricants, weather resistance stabilizers, light stabilizers, antioxidants, antibacterial agents, deodorants, pigments, and inorganic fillers. The content of the other additives in the resin composition is, for example, 5.0% by mass or less, and may be 2.0% by mass or less, 1.0% by mass or less, or may be substantially zero.
[0038] In the resin foam sheet (10a, 10b) shown in Fig. 1 or Fig. 2, at least one side of the foam layer 11 is exposed so as to form the sheet surface (15a, 16a). When the resin foam sheet (10a, 10b) is used so that the foam layer 11 comes into direct contact with an article to be packaged (not shown), the resin composition constituting the foam layer 11 preferably does not contain a fatty acid compound used as a lubricant or surfactant, from the viewpoint of preventing contamination of the article to be packaged due to migration of components to the sheet surface (15a, 16a). Examples of fatty acid compounds that are preferably not contained include fatty acids, fatty acid metal salts, fatty acid amides, and fatty acid esters.
[0039] Specific examples of fatty acids include saturated fatty acids such as lauric acid, palmitic acid, stearic acid, and behenic acid, unsaturated fatty acids such as oleic acid, erucic acid, linoleic acid, and linolenic acid, and further, in addition to these monocarboxylic acids, dicarboxylic acids such as dimer acid, etc. Examples of metals constituting fatty acid metal salts include calcium, magnesium, aluminum, zinc, etc.
[0040] The fatty acid amide is an acid amide derived from a fatty acid. For example, the fatty acid amide may be derived from an aliphatic amine. Specific examples of the fatty acid amide include stearic acid amide, palmitic acid amide, oleic acid amide, erucic acid amide, methylene bisstearic acid amide, ethylene bisstearic acid amide, ethylene bisoleic acid amide, and ethylene bishydroxystearic acid amide.
[0041] Specific examples of fatty acid esters include butyl stearate, stearic acid monoglyceride, oleic acid monoglyceride, behenic acid monoglyceride, linoleic acid monoglyceride, ricinoleic acid monoglyceride, hydroxystearic acid triglyceride, sorbitan fatty acid esters, polyoxyethylene (5) glycerin monostearate, polyoxyethylene (20) glycerin monostearate, polyoxyethylene (5) monooleate, pentaerythritol tetrastearate, polyadipate pentaerythritol stearate, stearyl stearate, 1,2-oxystearic acid, and hydrogenated castor oil.
[0042] From the viewpoint of avoiding contamination of the packaged item, the total content of fatty acid compounds in the resin composition constituting the foamed layer 11 is preferably 10,000 ppm or less, more preferably 1,000 ppm or less, even more preferably 100 ppm or less, and even more preferably 10 ppm or less. The total content of fatty acid compounds in the resin composition constituting the foamed layer 11 may be, for example, 7 ppm or less or 5 ppm or less. The total content of fatty acid compounds in the resin composition constituting the foamed layer 11 may be, for example, 1 ppm or more or 3 ppm or more, and may be 5 ppm or more, 10 ppm or more, or 100 ppm or more, as necessary.
[0043] When the resin foam sheet 10a is used as a cushioning material for packaging and transporting a relatively large article (packaged object) such as an automobile bumper, it is desirable for the resin foam sheet 10a to be flexible in order to efficiently package such a large packaged object. From the viewpoint of imparting such flexibility to the resin foam sheet 10a, the thickness of the resin foam sheet 10a (foam layer 11) may be, for example, 5.0 mm or less or 4.0 mm or less, preferably 3.0 mm or less, and more preferably 2.5 mm or less. From the viewpoint of imparting a certain degree of mechanical strength to the resin foam sheet 10a, the thickness of the resin foam sheet 10a (foam layer 11) may be, for example, 0.40 mm or more, preferably 0.60 mm or more, and more preferably 1.0 mm or more.
[0044] The thickness of the resin foam sheet 10a (foam layer 11) can be measured by the following method. The measurement is performed using a constant pressure thickness measuring device (stand type, manufactured by Teclock, digital indicator PC series model number "PC-440J") and a cylindrical weight. The measurement was performed on a circular surface with a diameter of 3.0 cm (area: 7.1 cm 2 ) with a load of 95 g (including its own weight) applied to the foam layer. Measurements are then taken at 50 points every 5 cm in the width direction, and the arithmetic mean value of the measurements is taken as the thickness of the resin foam sheet (foam layer). If it is not possible to obtain measurements at 50 points, measure as many as possible and use the arithmetic mean of the measurements as the thickness. In the resin foam sheet (10b, 10c) shown in Figures 2 and 3, when determining the thickness of only the non-foamed layers (21, 22), a test piece from which the foamed layer 11 has been removed may be used, and when determining the thickness of only the foamed layer 11, a test piece from which the non-foamed layers (21, 22) have been removed may be used.
[0045] From the viewpoint of imparting the above-mentioned flexibility to the resin foam sheet 10a, the apparent density of the foam layer 11 is 40 mg / cm 3 For example, 35 mg / cm 3 or less, preferably 30 mg / cm 3 More preferably, 25 mg / cm 3 From the viewpoint of easily imparting a certain degree of mechanical strength to the resin foam sheet 10a, the apparent density of the foam layer 11 is, for example, 1.0 mg / cm 3 or more, preferably 5.0 mg / cm 3 More preferably, 10 mg / cm 3 That's all.
[0046] The apparent density of the resin foam sheet (foam layer) can be determined by the following method. (Method of measuring apparent density) The apparent density of the resin foam sheet (foam layer) is determined by the thickness (T: mm) of the resin foam sheet (foam layer) obtained as described above and the basis weight (Y: g / m 2 ) can be calculated using the following formula: Apparent density (mg / cm 3 )=Y / T In the resin foam sheet (10b, 10c) shown in Figures 2 and 3, when the apparent density of only the non-foamed layers (21, 22) is to be determined, a test piece from which the foamed layer 11 has been removed can be used, and when the apparent density of only the foamed layer 11 is to be determined, a test piece from which the non-foamed layers (21, 22) have been removed can be used.
[0047] The basis weight of the resin foam sheet (foam layer) can be determined by the following method. (Method of measuring basis weight) A strip-shaped test piece 20 cm wide is taken from the resin foam sheet (foam layer). The test pieces are taken, for example, so that the direction perpendicular to the extrusion direction is the length direction. The mass W (g) and area S (cm 2 ) and calculate the basis weight using the following formula. Basis weight (g / m 2 )=W / S×10000 If it is difficult to cut a test piece with a width of 20 cm in the direction perpendicular to the extrusion direction, cut it into a rectangle of the possible size, and calculate its mass W (g) and area S (cm 2 ) and calculate the basis weight using the above formula. In the resin foam sheet (10b, 10c) shown in Figures 2 and 3, when determining the basis weight of only the non-foamed layers (21, 22), a test piece from which the foamed layer 11 has been removed can be used, and when determining the basis weight of only the foamed layer 11, a test piece from which the non-foamed layers (21, 22) have been removed can be used.
[0048] The surface resistivity of at least one sheet surface (15a, 16a) of the resin foam sheet 10a is 9.0×10 16 Ω or less, preferably 5.0×10 16 Ω or less, more preferably 1.0×10 16 Ω or less. If the surface resistivity is 9.0×10 16 If it is larger than Ω, static electricity may accumulate, which may cause problems such as dust attraction.
[0049] On the other hand, when the resin foam sheet 10a is used as a cushioning material for packaging an object, if the antistatic property of the resin foam sheet (foam layer) is higher than necessary compared to the antistatic property of the object, a problem may arise in which dust is more likely to adhere to the object while avoiding the cushioning material (resin foam sheet). This problem occurs when the object is a resin molded product (e.g., an automobile bumper) that does not have substantial antistatic properties, or the like, and the surface resistivity of the object is high (e.g., 1.0×10 17This tends to become evident when the resin composition contains too much antistatic agent so that the resin foam sheet (foam layer) has an antistatic property higher than necessary. In addition, when the resin composition contains too much antistatic agent, the resin foam sheet (foam layer) has an insufficient polyethylene resin content, which may cause a problem that the flexibility, foamability, and strength unique to polyethylene resin are impaired. In order to avoid these problems, the surface resistivity of at least one sheet surface (15a, 16a) of the resin foam sheet 10a is 5.0×10 14 Ω or more, preferably 8.0×10 14 Ω or more, and even more preferably 1.0×10 15 It is greater than or equal to Ω.
[0050] When the resin foam sheet 10a is used as a cushioning material, both sheet surfaces (15a and 16a) of the resin foam sheet 10a may have the above-mentioned surface resistivity. When only one sheet surface (15a or 16a) of the resin foam sheet 10a contacts the packaged object, only the sheet surface (15a or 16a) on the contacting side may have the above-mentioned surface resistivity. In the resin foam sheet 10b shown in FIG. 2, when the sheet surface 16a composed of the foam layer 11 contacts the packaged object, only the surface layer portion of the foam layer 11 may have the above-mentioned surface resistivity, or when only the sheet surface 15b composed of the first non-foam layer 21 contacts the packaged object, only the surface layer portion of the first non-foam layer 21 may have the above-mentioned surface resistivity, or each surface layer portion of the foam layer 11 and the first non-foam layer 21 may have the above-mentioned surface resistivity. In the resin foam sheet 10c shown in Fig. 3, when the sheet surface 15b composed of the first non-foamed layer 21 contacts the packaged article, the surface layer portion of the first non-foamed layer 21 may have the above-mentioned surface specific resistivity, or when the sheet surface 16b composed of the second non-foamed layer 22 contacts the packaged article, the surface layer portion of the second non-foamed layer 22 may have the above-mentioned surface specific resistivity, or each of the surface layers of the first non-foamed layer 21 and the second non-foamed layer 22 may have the above-mentioned surface specific resistivity. In the resin foam sheet 10c, the foamed layer 11 does not constitute the sheet surfaces (15b, 16b), but may have the above-mentioned surface specific resistivity at the bonding surface with the non-foamed layers (21, 22).
[0051] The surface resistivity of the resin foam sheet can be measured as follows. (Method of measuring surface resistivity) The surface resistivity can be measured by the method described in JIS K6911:1995 "General testing methods for thermosetting plastics." The test equipment used may be a digital ultra-high resistance / microcurrent meter, model number "R3840", and a resistivity chamber, model number "R12702A", manufactured by Advantest Corporation. The surface resistivity can be calculated by the following formula: electrodes are attached to a test piece taken from a resin foam sheet with a load of about 30 N, the resistance value is measured after charging at 500 V for 1 minute, and the surface resistivity is calculated by the following formula. ρs = (π(D+d) / (Dd)) × Rs ρs: Surface specific resistivity (MΩ) D: inner diameter of the surface ring electrode (cm) d: outer diameter of the inner circle of the surface electrode (cm) Rs: Surface resistance (MΩ) The test piece is 100 mm wide x 100 mm long x thickness T (the thickness of the resin foam sheet as is). The measurement is carried out after conditioning the test specimen for at least 24 hours in an environment of a temperature of 20±2°C and a relative humidity of 65±5% RH. The test environment shall be a temperature of 20±2°C and a relative humidity of 65±5%RH. The number of test pieces (n) shall be five, and in principle, both the front and back sides of each shall be measured.
[0052] When the resin foam sheet 10a is used as a cushioning material for packaging and transporting an object to be packaged, the tear strength in the machine direction (MD) of the resin foam sheet 10a (foam layer 11) may be, for example, 20 N / cm or more, preferably 22 N / cm or more, and more preferably 24 N / cm or more, from the viewpoint of easily preventing the resin foam sheet 10a from tearing during transportation. When packaging an object to be packaged using the resin foam sheet 10a, from the viewpoint of easily allowing a user to cut the resin foam sheet 10a to a size suitable for packaging according to the size of the object to be packaged, the tear strength in the MD of the resin foam sheet 10a (foam layer 11) may be, for example, 40 N / cm or less, preferably 35 N / cm or less, and more preferably 30 N / cm or less.
[0053] The tear strength of the resin foam sheet is determined by the following method. (Method of measuring tear strength) The tear strength of the resin foam sheet is measured in accordance with the method described in JIS K6772:1994 "Vinyl Leather Cloth". Specifically, the test piece is kept in an environment of 23±2°C temperature and 50±5% relative humidity for at least 24 hours, and then the measurement is performed in an environment of 23±2°C temperature and 50±5% relative humidity. The test is carried out using a Tensilon universal testing machine (manufactured by Orientec Co., Ltd., product name "UCT-10T") and universal testing machine data processing software (manufactured by Softbrain Co., Ltd., product name "UTPS-237S"). The test pieces were cut into rectangles with short sides of 40 mm and long sides of 150 mm in the machine direction (MD) and transverse direction (TD) of the resin foam sheet, respectively, and three pieces were prepared with a 75 mm long cut made in the center of one of the two short sides (20 mm from the corner) parallel to the long side. That is, the test piece used is bifurcated at the center in the longitudinal direction. The tensile tester is set so that the distance between the grips is 50 mm, and each end of the bifurcated portion is fixed to a grip. In this state, the test piece is torn apart under the condition that the grippers are separated at a speed of 200 mm / min, and the maximum load until the test piece breaks is measured. The arithmetic mean value of the maximum point loads of each test piece is determined as the tear strength of the resin foam sheet. In the resin foam sheet (10b, 10c) shown in Figures 2 and 3, when the tear strength of only the non-foamed layers (21, 22) is to be measured, a test piece from which the foamed layer 11 has been removed can be used, and when the tear strength of only the foamed layer 11 has been measured, a test piece from which the non-foamed layers (21, 22) have been removed can be used.
[0054] The matters disclosed in this specification include the following. (1) A polyethylene-based resin foamed sheet having a foam layer and a sheet surface constituted by a polyethylene-based resin composition containing a polyethylene resin, the polyethylene resin composition contains 1.0 parts by mass or more and 5.0 parts by mass or less of an ionomer-type antistatic agent relative to 100 parts by mass of the polyethylene resin, The apparent density of the foam layer is 40 mg / cm 3 is as follows: The surface resistivity of the sheet surface is 5×10 14 Ω or more 9×10 16 A polyethylene resin foam sheet having a hardness of Ω or less. (2) The polyethylene-based resin foamed sheet according to the above (1), which has a laminated structure and has a non-foamed layer composed of the polyethylene-based resin composition as an outermost layer. (3) The polyethylene resin foam sheet according to the above (1) or (2), wherein the foam layer has a thickness of 0.6 mm or more and 3.0 mm or less. (4) The polyethylene-based resin foam sheet according to any one of the above (1) to (3), wherein at least a part of the polyethylene-based resin composition is a recycled resin composition comprising the polyethylene resin and the ionomer-type antistatic agent.
[0055] The present invention is not limited to the above-described embodiments, and may be implemented in various forms with improvements, modifications, or variations based on the knowledge of a person skilled in the art without departing from the spirit of the present invention. The present invention may be implemented in a form in which any particular feature is replaced with another technique within a range in which the same action or effect is achieved. For example, in the resin foam sheet (10b, 10c) shown in FIG. 2 or FIG. 3, the non-foamed layer (21, 22) made of the resin composition containing a polyethylene resin and an ionomer-type antistatic agent exerts antistatic properties on the sheet surface (15b, 16b), so that the polyethylene resin composition constituting the foam layer 11 may not contain an ionomer-type antistatic agent. EXAMPLES
[0056] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0057] (Prototype of recycled pellet R1) As a virgin polyethylene resin derived from fossil fuels, model number "LD400" (resin density 919 kg / m 3, MFR 2.0 g / 10 min, melt tension 5.2 cN) were prepared. As an ionomer type antistatic agent, model number "SD100" manufactured by Dow Mitsui Polychemicals Co., Ltd. (ethylene-methacrylic acid random copolymer containing potassium as an ion source, melting point 92°C, MFR 12g / 10min) was prepared. As the foam control agent master batch, a product named "CellMike MB1023" (azodicarbonamide-containing master batch) manufactured by Sanyo Chemical Industries, Ltd. was prepared. In a tandem extruder in which two extruders were connected in the extrusion direction, a first extruder and a second extruder, in that order, a circular die A with an outlet diameter of 222 mm (slit width 0.04 mm) was attached to the tip of the second extruder.
[0058] A mixture was prepared by blending 100 parts by mass of virgin polyethylene resin "LD400", 6 parts by mass of ionomer type antistatic agent "SD100", and 0.15 parts by mass of foam control agent master batch "CellMike MB1023". This mixture was fed into the first extruder (cylinder diameter: φ90 mm) of a tandem extruder, and melt-kneaded so that the maximum temperature reached in the first extruder was 210°C. Mixed butane (isobutane / normal butane = 70 / 30 (molar ratio)) was injected as a foaming agent midway through the first extruder, and further melt-kneading was performed. The amount of the mixed butane injected was adjusted so that the ratio was 18 parts by mass relative to 100 parts by mass of the polyethylene resin. After the melt-kneading in the first extruder, the melt-kneaded product was cooled to a temperature range suitable for foaming (111°C) in a second extruder (cylinder diameter: φ150 mm) connected to the first extruder, and extruded and foamed from the circular die A described above into the atmosphere. The resin temperature at that time was 112°C. The extruded tubular foam was cooled by blowing air onto it, then cooled by placing it on a cooling mandrel with a diameter of 770 mm and a length of 650 mm. The tubular foam was cut along the extrusion direction with a cutter attached to the rear side of the cooling mandrel, and wound up at a speed of 40 m / min to produce a long, strip-shaped resin foam sheet.
[0059] In addition to the above-mentioned tandem extruder, an extruder was prepared having a strand production die B (16 holes, each hole having a diameter of φ2 mm) attached to its tip. The above-mentioned resin foam sheet was put into this extruder (cylinder diameter: φ150 mm) and melted, and the molten resin with a resin temperature of 250°C was extruded into the atmosphere from each hole of the above-mentioned strand production die B at a discharge rate of 80 kg / hour to form a strand resin. This strand resin was immersed in cooling water to be quenched, and then cut into pellets (φ2 mm × length 3 mm) with a pelletizer. In this way, a recycled pellet R1 composed of a recycled polyethylene resin composition containing an ionomer-type antistatic agent was experimentally produced.
[0060] Example 1 In the above-mentioned tandem extruder, the above-mentioned circular die A was removed from the tip of the second extruder, and instead, a circular die C having an outlet diameter of 145 mm (slit width 0.15 mm) was attached to the tip of the second extruder. As a virgin low-density polyethylene resin derived from fossil fuels, Ube Maruzen Polyethylene Co., Ltd.'s model number "B128" (resin density 928 kg / m 3 , MFR 1.0 g / 10 min, melt tension 6.2 cN) were prepared. A mixture was prepared by blending 50 parts by mass of virgin polyethylene resin "B128", 50 parts by mass of recycled pellets R1, and 0.3 parts by mass of air bubble regulator "Cellmike MB1023". This mixture was fed into the first extruder (cylinder diameter: φ90 mm) of a tandem extruder, and melt-kneaded so that the maximum temperature reached in the first extruder was 210°C. Mixed butane (isobutane / normal butane = 70 / 30 (molar ratio)) was injected as a foaming agent midway through the first extruder, and further melt-kneading was performed. The amount of the mixed butane injected was adjusted so that the ratio was 18 parts by mass relative to 100 parts by mass of the polyethylene resin. After the melt-kneading in the first extruder, the melt-kneaded product was cooled to a temperature range suitable for foaming (111°C) in a second extruder (cylinder diameter: φ150 mm) connected to the first extruder, and extruded and foamed from the circular die C described above into the atmosphere. The resin temperature at that time was 112°C. The extruded tubular foam was cooled by blowing air onto it, and then cooled by placing it on a cooling mandrel with a diameter of 515 mm and a length of 650 mm. The tubular foam was cut along the extrusion direction with a cutter attached to the rear side of the cooling mandrel, and taken up at a speed of 25 m / min to produce a long, strip-shaped resin foam sheet having a single-layer structure consisting only of a foam layer (the resin foam sheet of Example 1).
[0061] The formulations at the time of trial production for the above-mentioned Example 1 and other examples described later are summarized in Table 1 below. [Table 1]
[0062] (Examples 2 to 6) In each of Examples 2 to 6, compared to the above-mentioned Example 1, the blending ratio of the virgin polyethylene resin "B128" and the recycled pellets R1 was changed as shown in Table 1 above, and a resin foam sheet having a single-layer structure consisting of only a foam layer was produced in the same manner as in Example 1.
[0063] Example 7 In Example 7, compared to the above-mentioned Example 1, the recycled pellets R1 were not blended, and the blending ratio of the virgin polyethylene resin "B128" and the ionomer-type antistatic agent "SD100" was changed as shown in Table 1 above. Except for this, a resin foam sheet having a single-layer structure consisting of only a foam layer was produced in the same manner as in Example 1.
[0064] (Comparative Examples 1 and 2) In each of Comparative Examples 1 and 2, compared to the above-mentioned Example 1, the blending ratio of the virgin polyethylene resin "B128", the recycled pellets R1, and the ionomer-type antistatic agent "SD100" was changed as shown in Table 1 above, and a resin foam sheet having a single-layer structure consisting of only a foam layer was produced in the same manner as in Example 1.
[0065] (Prototype of recycled pellet R2) Compared to the prototype of the recycled pellet R1 described above, the following two changes were made. As the first change, a polyalkylene oxide type antistatic agent, trade name "PELLECTRON LMP" (a block copolymer of polyether and polyolefin, melting point 115°C, MFR 30g / 10min) manufactured by Sanyo Chemical Industries, Ltd., was prepared. As the second change, a mixture was prepared by blending 100 parts by mass of virgin polyethylene resin "LD400", 6 parts by mass of polyalkylene oxide type antistatic agent "Plectron LMP", and 0.15 parts by mass of foam control agent master batch "CellMike MB1023", and this mixture was supplied into the first extruder of the tandem extruder. Apart from the two changes mentioned above, a recycled pellet R2 composed of a recycled polyethylene resin composition containing a polyalkylene oxide type antistatic agent was produced in the same manner as the above-mentioned recycled pellet R1.
[0066] (Comparative Examples 3 and 4) In each of Comparative Examples 3 and 4, compared to the above-mentioned Example 1, the above-mentioned recycled pellets R2 were blended instead of the recycled pellets R1, and the blending ratio of the virgin polyethylene resin "B128" and the recycled pellets R2 was changed as shown in Table 1 above. Except for this, a resin foam sheet having a single-layer structure consisting of only a foam layer was produced in the same manner as in Example 1.
[0067] Comparative Example 5 In Comparative Example 5, the following two points were changed compared to the above-mentioned Example 1. The first change was to prepare an ionomer-type antistatic agent, trade name "Entira MK400" (containing potassium as an ion source, melting point 93°C, MFR 1.5g / 10min) manufactured by Dow Mitsui Polychemicals Co., Ltd. As the second change, in Comparative Example 5, the recycled pellets R1 were not mixed, and a mixture was prepared by blending 100 parts by mass of virgin polyethylene resin "B128", 5 parts by mass of ionomer type antistatic agent "Entira MK400", and 0.3 parts by mass of bubble control agent master batch "CellMike MB1023", and this mixture was supplied into the first extruder of the tandem extruder. Other than the above-mentioned two changes, a resin foam sheet having a single-layer structure consisting of only a foam layer was produced in the same manner as in Example 1.
[0068] For each of the resin foam sheets prepared as described above, the thickness, basis weight, apparent density, tear strength in MD, and surface resistivity of the sheet were measured by the above-mentioned method. Based on these measured values, the functionality of each resin foam sheet was evaluated according to the following criteria.
[0069] (Evaluation criteria for strength of resin foam sheet) Evaluation : The tear strength is 24 N / cm or more, and when observed with the naked eye after being used twice as a cushioning material for packaging and transporting automobile bumpers, the resin foam sheet shows no particular cracks. Evaluation: Good: The tear strength is 22 N / cm or more and less than 24 N / cm, and when observed with the naked eye after one use as a cushioning material for packaging an automobile bumper, no particular cracks are found in the resin foam sheet. Evaluation △: The tear strength is 20 N / cm or more and less than 22 N / cm. When observed with the naked eye after one use as a cushioning material for packaging an automobile bumper, the resin foam sheet may have small, inconspicuous tears. Rating: ×: The tear strength is less than 20 N / cm, and when observed with the naked eye after one use as a cushioning material for packaging an automobile bumper, the resin foam sheet often has noticeable large cracks.
[0070] (Evaluation criteria for flexibility of resin foam sheet) Evaluation ◎: Apparent density is 30mg / cm 3 Since the resin foam sheet has a thickness of less than or equal to 100 mm and is highly flexible, when used to package automobile bumpers, the resin foam sheet can be easily packaged without generating creases or tears. Evaluation: Apparent density is 30mg / cm 3 More than 40mg / cm 3 or less and has some flexibility, when a resin foam sheet is used to package an automobile bumper, no cracks (cracks penetrating the sheet) will occur in the resin foam sheet, but creases may occur. Evaluation ×: apparent density is 40 mg / cm 3 Because the strength of the foam is higher and less flexible than that of the conventional foam, when a foam sheet is used to package automobile bumpers, the foam sheet is prone to frequent creases and cracks (cracks that penetrate the sheet).
[0071] (Evaluation criteria for antistatic properties of resin foam sheets) ◎: Surface resistivity is 1.0×10 16 It has antistatic properties within the range of Ω or less, and when the resin foam sheet is used as a cushioning material for packaging and transporting automobile bumpers, even when the surface of the sheet is closely observed with the naked eye, no fine dust is found and the surface appears clean. Evaluation: Surface resistivity is 1.0×10 16 Higher than Ω 5.0×10 16 The resin foam sheet has antistatic properties within the range of Ω or less, and when it is used as a cushioning material for packaging and transporting automobile bumpers, there is no dust that is visible at first glance on the surface of the sheet, but fine dust can be found if the surface of the sheet is observed closely with the naked eye. Evaluation △: Surface resistivity is 5.0×10 16 Higher than Ω 9.0×10 16The resin foam sheet has low antistatic properties in the range of Ω or less, and when used as a cushioning material for packaging and transporting automobile bumpers, dust is visible on the sheet surface at a glance, but the dust can be easily removed from the sheet surface by picking it up with the fingertips. Rating ×: Surface resistivity is 9.0×10 16 Therefore, when a resin foam sheet is used as a cushioning material for packaging and transporting automobile bumpers, dust is visible at a glance on the sheet surface, and the dust is adhered to the sheet surface and is difficult to remove from the sheet surface by picking it up with the fingertips.
[0072] (Criteria for overall evaluation of functionality of resin foam sheets) Overall rating ◎: Only rating of ◎ was given in all three categories of strength, flexibility and antistatic properties. Overall rating: Good: All three items of strength, flexibility and antistatic property were rated as ◎ or Good. Overall rating △: There were no × ratings in the three categories of strength, flexibility and antistatic properties. Overall rating: ×: At least one rating of × was given in the three categories of strength, flexibility and antistatic property (lacking in practicality).
[0073] For each of the prototype resin foam sheets (foam layers), the composition of the polyethylene resin composition calculated from the blending amounts shown in Table 1 above, the measured values of the sheet thickness, basis weight, apparent density, MD tear strength and surface resistivity, and the evaluation results of functionality are shown in Table 2 below.
[0074] [Table 2]
[0075] As is clear from Table 2, it was suggested that Examples 1 and 5, which contained an ionomer-type antistatic agent (recycled pellets R1), had higher tear strength and lower surface resistivity of the resin foam sheet (foam layer) than Comparative Examples 3 and 4, which contained a polyalkylene oxide-type antistatic agent (recycled pellets R2) (i.e., it is easier to achieve both strength and antistatic properties).
[0076] In Comparative Examples 1, 2, and 5, in which the content of the ionomer type antistatic agent per 100 parts by mass of the polyethylene resin is in the range of more than 5.0 parts by mass, the tear strength is 20 N / cm or more and the compressibility is 40 mg / cm or more. 3 In other words, in Comparative Examples 1 and 2, the foaming ratio was slightly higher to achieve an apparent density of 31 mg / cm3. 3 In Comparative Example 5, when the foaming ratio was adjusted to be low so as to increase the tear strength, the apparent density was increased to 50 mg / cm. 3 This resulted in a lack of flexibility.
[0077] On the other hand, in Examples 1 to 7, the content of the ionomer type antistatic agent relative to 100 parts by mass of the polyethylene resin was in the range of 1.0 parts by mass or more and 5.0 parts by mass or less, and the tear strength was 20 N / cm or more and the elastic modulus was 40 mg / cm or more. 3 It was suggested that the apparent density below can be achieved simultaneously (strength and flexibility can be achieved simultaneously). In addition, when the above-mentioned Tables 1 and 2 are taken into consideration together, it was suggested that, unexpectedly, Example 1, which was prototyped from a mixture of virgin polyethylene resin and recycled pellets R1, had a higher tear strength and a lower surface resistivity (excellent in both strength and antistatic properties) compared to Example 7, which was prototyped from a mixture of virgin polyethylene resin and ionomer-type antistatic agent. [Explanation of symbols]
[0078] 10a, 10b, 10c: resin foam sheet, 11: foam layer, 15a, 15b: sheet surface on one side, 16a, 16b: sheet surface on the other side, 21: first non-foam layer, 22: second non-foam layer
Claims
1. A polyethylene-based resin foamed sheet having a foam layer and a sheet surface constituted by a polyethylene-based resin composition containing a polyethylene resin, the polyethylene resin composition contains 1.0 parts by mass or more and 5.0 parts by mass or less of an ionomer-type antistatic agent relative to 100 parts by mass of the polyethylene resin, The apparent density of the foam layer is 40 mg / cm 3 is as follows: The surface resistivity of the sheet surface is 5×10 14 Ω or more 9×10 16 A polyethylene resin foam sheet having a hardness of Ω or less.
2. 2. The polyethylene resin foamed sheet according to claim 1, which has a laminated structure, and has a non-foamed layer constituted of the polyethylene resin composition as an outermost layer.
3. 3. The polyethylene resin foam sheet according to claim 1, wherein the foam layer has a thickness of 0.6 mm or more and 3.0 mm or less.
4. 3. The polyethylene-based resin foam sheet according to claim 1, wherein at least a part of the polyethylene-based resin composition is a recycled resin composition comprising the polyethylene resin and the ionomer-type antistatic agent.
Citation Information
Patent Citations
Production method of extruded foam sheet of polyethylene-based resin, and extruded foam sheet of polyethylene-based resin
JP2021134258A