Composition, manufacturing method therefor, and cement manufacturing method

A cement composition using cement clinker and fine powder, optimized by the ratio Y≦0.225X+2.09, addresses safety and workability issues in geopolymer and alkali-activated concrete by eliminating high alkalinity, achieving comparable strength and fluidity.

JP2024141561APending Publication Date: 2024-10-10TAIHEIYO CEMENT CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023053289
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing hardened materials like geopolymer and alkali-activated concrete face safety issues due to high alkalinity, leading to viscosity-related deterioration and construction challenges, while requiring alkaline stimulants for strength development.

Method used

A composition comprising cement clinker fine aggregate and fine powder, specifically formulated to exclude highly alkaline materials, with a ratio defined by the equation Y≦0.225X+2.09, enhancing safety and workability.

Benefits of technology

The composition achieves improved safety and workability by eliminating the need for high alkaline materials, ensuring superior fluidity and strength comparable to conventional cement concrete without using alkaline stimulants.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a composition excellent in safety and workability.SOLUTION: A composition includes a cement clinker fine aggregate and fine powder. The fine powder includes at least blast furnace slag fine powder and satisfies equation 1: Y≤0.225X+2.09. In equation 1, X indicates a fineness modulus of the cement clinker fine aggregate, and Y indicates a mass ratio of a content of the cement clinker fine aggregate to a content of the fine powder.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition and a method for producing the same, and to a method for producing cement. [Background technology]

[0002] Patent Document 1 discloses preparing a dry mortar containing ordinary Portland cement clinker and ground granulated blast furnace slag, and producing mortar from this dry mortar (see Example 2 of Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2004-51398 A Summary of the Invention [Problem to be solved by the invention]

[0004] Hardened bodies such as geopolymer concrete and alkali-activated concrete are said to have superior acid resistance and heat resistance compared to general-purpose cement concrete. However, issues have been raised regarding safety due to the use of highly alkaline materials, as well as construction issues such as poor filling properties due to high viscosity.

[0005] In recent years, research has been conducted on geopolymer concrete and alkali-activated concrete, which use industrial by-products such as ground granulated blast furnace slag and coal fly ash as substitute powders for cement, and some of these concretes have been put to practical use, taking advantage of their characteristics such as acid resistance and heat resistance. However, these materials require alkaline activators with high alkaline concentrations to increase their strength, which poses safety issues.

[0006] In view of the above, an object of one aspect of the present invention is to provide a composition that is excellent in safety and workability. [Means for solving the problem]

[0007] In the course of their investigations, the inventors have noticed that a composition containing fine aggregate of cement clinker together with ground granulated blast furnace slag is excellent in safety because it does not require the use of highly alkaline materials or alkaline stimulants with high alkaline concentrations. As a result of further intensive investigations, they have newly discovered that a composition containing fine aggregate of cement clinker together with ground granulated blast furnace slag and which satisfies the following formula 1 has high fluidity and excellent workability.

[0008] One aspect of the present invention is as follows. [1] Contains fine aggregate and fine powder of cement clinker, The fine powder contains at least ground granulated blast furnace slag, and Formula 1 below: Y≦0.225X+2.09 (In formula 1, X represents the coarse particle ratio of the cement clinker fine aggregate, and Y represents the mass ratio of the content of the cement clinker fine aggregate to the content of the fine powder.) A composition that satisfies the above. [2] The fine powder further comprises limestone fine powder; and The composition according to [1], wherein the content of the limestone fine powder is 10% by mass or less, with the total amount of the fine powder being 100% by mass. [3] The fine powder further comprises limestone fine powder and gypsum fine powder; and The composition according to [1] or [2], wherein the total content of the limestone fine powder and the gypsum fine powder is 10% by mass or less, with the total amount of the fine powders being 100% by mass. [4] The composition according to any one of [1] to [3], wherein the cement clinker fine aggregate has a coarse particle ratio X of 3.50 or less. [5] The composition according to any one of [1] to [4], wherein a mass ratio Y of the content of the cement clinker fine aggregate to the content of the fine powder is 1.50 or more and 3.50 or less. [6] The fine powder further comprises limestone fine powder; and The content of the limestone fine powder is 10% by mass or less, based on the total amount of the fine powder being 100% by mass; The coarse aggregate ratio X of the above-mentioned cement clinker fine aggregate is 3.50 or less, and The composition according to any one of [1] to [5], wherein a mass ratio Y of a content of the cement clinker fine aggregate to a content of the fine powder is 1.50 or more and 3.50 or less. [7] The fine powder further includes limestone fine powder and gypsum fine powder; The total amount of the fine powder is 100% by mass, and the total content of the limestone fine powder and the gypsum fine powder is 10% by mass or less. The coarse aggregate ratio X of the above-mentioned cement clinker fine aggregate is 3.50 or less, and The composition according to any one of [1] to [5], wherein a mass ratio X of a content of the cement clinker fine aggregate to a content of the fine powder is 1.50 or more and 3.50 or less. [8] The composition according to any one of [1] to [7], which further contains water and is cured to form a hardened product. [9] A method for producing the composition according to any one of [1] to [7], The above-mentioned production method includes mixing a cement clinker fine aggregate having a coarse particle ratio that satisfies the above formula 1 with a fine powder in a ratio that satisfies the mass ratio of Y in the above formula 1.

[10] A method for producing cement, comprising grinding the composition described in [8]. Effect of the Invention

[0009] According to one aspect of the present invention, a composition excellent in safety and workability can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Composition] One aspect of the present invention relates to a composition comprising a cement clinker fine aggregate and a fine powder, the fine powder including at least ground granulated blast furnace slag, and satisfying the following formula 1:

[0011] Formula 1: Y≦0.225X+2.09 (In formula 1, X represents the coarse particle ratio of the cement clinker fine aggregate, and Y represents the mass ratio of the content of the cement clinker fine aggregate to the content of the fine powder.)

[0012] In the present invention and the present specification, the term "composition" includes a dry composition to which no water has been added and a wet composition to which water has been added. The composition can be, for example, a mortar composition or a cement composition. The term "composition" also includes a composition in an unhardened form and a composition in a hardened form (i.e., a hardened body).

[0013] The above composition will now be described in more detail.

[0014] <Cement clinker fine aggregate> The composition includes a cement clinker fine aggregate. In the present invention and this specification, "cement clinker" refers to a material obtained by crushing and mixing a CaO raw material, an Al2O3 raw material, a Fe2O3 raw material, and a SiO2 raw material, and then firing the mixture in a rotary kiln or the like. "Fine aggregate" refers to a fine aggregate defined in JIS A 0203:2019.

[0015] Examples of the cement clinker include ordinary Portland cement clinker, high-early-strength Portland cement clinker, low-heat Portland cement clinker, moderate-heat Portland cement clinker, and ecocement clinker.

[0016] Cement clinker can contain calcium silicate represented by 3CaO·SiO2 (hereinafter referred to as alite (C3S) or simply alite) or 2CaO·SiO2 (hereinafter referred to as belite (C2S) or simply belite), calcium aluminoferrite represented by 4CaO·Al2O3·Fe2O3 (hereinafter referred to as ferrite (C4AF) or simply ferrite), calcium aluminate represented by 3CaO·Al2O3 (hereinafter referred to as aluminate (C3A) or simply aluminate), etc. The content of each mineral can be calculated using the Borg formula from the results of chemical analysis according to JIS R 5202:2015 or JIS R 5204:2019, or by powder X-ray diffraction (XRD) Rietveld analysis.

[0017] Among them, the cement clinker preferably contains 50-70 mass% alite (C3S), 5-30 mass% belite (C2S), 3-15 mass% aluminate (C3A), and 5-20 mass% ferrite (C4AF) when calculated by the Bogue formula, and more preferably contains 55-65 mass% alite (C3S), 10-20 mass% belite (C2S), 5-12 mass% aluminate (C3A), and 7-15 mass% ferrite (C4AF).The use of fine aggregate of cement clinker having such mineral composition is preferable from the viewpoint of improving the strength of the hardened body.

[0018] The bone dry density of cement clinker fine aggregate is, for example, 2.40 g / cm 3 More than 3.00g / cm 3 The bone dry density of the cement clinker fine aggregate shall be the value obtained in accordance with JIS A 1109:2020.

[0019] The fine aggregate contained in the composition may be only the cement clinker fine aggregate. Alternatively, the composition may contain one or more other fine aggregates in addition to the cement clinker fine aggregate. When the other fine aggregates are contained, the content of the cement clinker fine aggregate relative to the total amount of the fine aggregates (100% by mass) is preferably 75% by mass or more.

[0020] <Fine powder> (Grained blast furnace slag) The composition includes one or more types of fine powder. The composition includes at least ground granulated blast furnace slag as the fine powder. In the present invention and this specification, the term "fine powder" refers to a powder that is finer than inorganic aggregate among admixtures defined in JIS A 0203:2019. The term "ground granulated blast furnace slag" refers to ground granulated blast furnace slag as defined in JIS A 6206:2013.

[0021] One index of particle size is the Blaine specific surface area. The "Blaine specific surface area" is the specific surface area measured by the Blaine method, and is calculated according to 8.1 of JIS R 5201. For example, ground granulated blast furnace slag has a Blaine specific surface area of ​​3000 cm. 2 / g or more 8000cm 2 / g or less of ground granulated blast furnace slag can be used. 2 / g or more 6000cm 2 It is preferable to use ground granulated blast furnace slag having an activity index of 75 or more or 85 or more at 28 days old. The use of such ground granulated blast furnace slag is preferable from the viewpoint of workability and improvement of the strength of the hardened body. The activity index is calculated according to JIS A 6206:2013.

[0022] (Other fine powders) In one embodiment, the fine powder contained in the composition may be only ground granulated blast furnace slag. In another embodiment, the composition may contain one or more other fine powders in addition to the ground granulated blast furnace slag. Examples of such fine powders include limestone fine powder, gypsum fine powder, and the like.

[0023] The limestone fine powder may be waste concrete fine powder, carbonate of fresh concrete sludge, etc. The Blaine specific surface area of ​​the limestone fine powder is, for example, 3000 cm 2 / g or more 8000cm 2 / g or less, and 2 / g or more 6000cm 2 It is preferable that the molecular weight is not more than 1 / g.

[0024] Examples of the gypsum fine powder include fine powders of gypsum dihydrate, α-type hemihydrate, β-type hemihydrate, anhydrous gypsum, etc. The Blaine specific surface area of ​​the gypsum fine powder is, for example, 3000 cm 2 / g or more 15000cm 2 / g or less.

[0025] The mixing ratio of the cement clinker fine aggregate and various fine powders will be described later.

[0026] <Expression 1> The inventors of the present invention have conducted extensive research into the mixing ratio of cement clinker fine aggregate and ground granulated blast furnace slag to improve workability, specifically, fluidity evaluated by the flow value measured by the flow test described in JIS R 5201:2015. As a result, they have found that there is a correlation between the mixing ratio of cement clinker fine aggregate and ground granulated blast furnace slag and the coarse aggregate ratio of the cement clinker fine aggregate, and that fluidity is improved when formula 1 is satisfied. In the present invention and this specification, the "coarse aggregate ratio" is determined by the method described in JIS A 1102:2014. The coarse aggregate ratio is determined by dividing the sum of the mass fractions (%) retained on sieves of 80 mm, 40 mm, 20 mm, 10 mm, 5 mm, 2.5 mm, 1.2 mm, 0.6 mm, 0.3 mm, and 0.15 mm by 100.

[0027] Formula 1 is "Y≦0.225X+2.09". In Formula 1, X represents the coarse particle ratio of the cement clinker fine aggregate. Y represents the mass ratio of the cement clinker fine aggregate content to the fine powder content (the total content when multiple types of fine powder are included).

[0028] From the viewpoint of further improving the fluidity, the composition preferably satisfies the following formula 1-1, and more preferably satisfies the following formula 1-2. Formula 1-1: Y≦0.175X+2.02 Formula 1-2: Y≦0.2X+1.83

[0029] For each of the formulas 1, 1-1, and 1-2, the value on the right side, which has been rounded off to two decimal places, is compared with Y on the left side to determine whether the formula is satisfied.

[0030] X and Y in the above composition may satisfy formula 1. In one embodiment, the coarse particle ratio X of the cement clinker fine aggregate is preferably 3.50 or less, more preferably 3.00 or less, and even more preferably 2.80 or less. In one embodiment, Y is preferably 1.90 or more, and more preferably 1.95 or more. In one embodiment, the mass ratio Y of the content of the cement clinker fine aggregate to the content of the fine powder is preferably 3.50 or less, more preferably 2.70 or less, and even more preferably 2.30 or less. In one embodiment, X is preferably 1.50 or more, more preferably 1.75 or more, and even more preferably 1.95 or more.

[0031] <Mixing ratio of fine powder> The composition contains at least ground granulated blast furnace slag as the fine powder. In one embodiment, the fine powder contained in the composition can be ground granulated blast furnace slag only (i.e., the entire amount of the fine powder is ground granulated blast furnace slag). In another embodiment, the composition can contain ground granulated blast furnace slag and one or more other fine powders. Specific examples of the other fine powders are as described above.

[0032] From the viewpoint of suppressing drying shrinkage of the hardened body, the composition preferably contains, as the fine powder, limestone fine powder and / or gypsum fine powder in addition to the ground granulated blast furnace slag.

[0033] When the composition contains limestone fine powder, the content of the limestone fine powder is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 4% by mass or more, with the total amount of the fine powder being 100% by mass. In the above case, the content of the limestone fine powder is preferably 10% by mass or less, more preferably 8% by mass or less, with the total amount of the fine powder being 100% by mass. In the above case, the fine powder other than the ground granulated blast furnace slag can be only limestone fine powder in one embodiment, and can be two types of fine powder, limestone fine powder and gypsum fine powder, in another embodiment.

[0034] When the composition contains limestone fine powder and gypsum fine powder, the total content of the limestone fine powder and gypsum fine powder is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 4% by mass or more, with the total amount of the fine powder being 100% by mass. In the above case, the total content of the limestone fine powder and gypsum fine powder is preferably 10% by mass or less, and more preferably 8% by mass or less, with the total amount of the fine powder being 100% by mass. In the above case, the fine powder other than the blast furnace slag ground powder can be two types of fine powder, limestone fine powder and gypsum fine powder, in one embodiment, and can further contain one or more types of fine powder.

[0035] When the composition contains the limestone fine powder and the gypsum fine powder, the mixing ratio thereof by mass (limestone fine powder:gypsum fine powder) can be 1:9 to 9:1, and is preferably 2:8 to 8:2.

[0036] The composition may be composed of only the above-mentioned various components, or may further contain one or more other components. Examples of the other components include admixtures. Examples of the admixtures include AE ​​agents, water-reducing agents, expansion agents, foaming agents, waterproofing agents, rust inhibitors, shrinkage reducing agents, water retention agents, setting retarders, accelerators, quick-setting agents, separation reducing agents, foaming agents, foaming agents, antifreeze agents, cold resistance accelerators, water repellents, efflorescence inhibitors, and fibers.

[0037] In one embodiment, the composition may contain one or more mineral fine powders such as cement, fly ash, silica powder, silica fume, etc., as fine powders other than those mentioned above. In this case, the content of the mineral fine powder is preferably 10% by mass or less relative to 100% by mass of the total amount of the fine powders.

[0038] The composition can be prepared by mixing various components with a commonly used mixing tool and / or kneading tool. The tool is not particularly limited, and for example, a hand mixer, a tilting mixer, a pan mixer, a twin-shaft mixer, etc. can be used. Mixing may be performed in a water-free state in advance, or may be performed when mixing water or coarse aggregate, which will be described later.

[0039] The composition may contain water and may be cured by a known method to form a hardened body. The hardened body thus obtained has a compressive strength at 28 days as specified in JIS R 5201:2015 of 50 N / mm 2 It is preferable that the resistance is 55N / mm or more. 2 More preferably, it is 60N / mm 2 More preferably, the content is 30 parts by mass or more or less. Various components can also be mixed with water to prepare a paste. Examples of water include tap water as specified in JIS A 5308:2019 Appendix C, water other than tap water (e.g., river water, lake water, well water, groundwater, industrial water), and recycled water. The content of water relative to 100 parts by mass of fine powder is preferably 30 parts by mass or more and 70 parts by mass or less, more preferably 30 parts by mass or more and 65 parts by mass or less, and even more preferably 40 parts by mass or more and 60 parts by mass or less.

[0040] The composition may also contain coarse aggregate. The coarse aggregate is not particularly limited, and examples thereof include river gravel, mountain gravel, land gravel, sea gravel, crushed stone, limestone coarse aggregate, slag coarse aggregate, lightweight coarse aggregate, clinker coarse aggregate, glass aggregate, and recycled aggregate. Among these, clinker coarse aggregate, limestone coarse aggregate, and slag coarse aggregate are preferred in that they can recycle a large amount of used composition without separating a large amount of coarse aggregate in the manufacturing method of cement or cement clinker described below.

[0041] The composition can be used to manufacture various structures, for example, ready mixed concrete, precast concrete products, premix products, and the like.

[0042] [Method of producing the composition] One aspect of the present invention relates to a method for producing the composition, comprising mixing a cement clinker fine aggregate having a coarse particle ratio that satisfies formula 1 with fine powder in a ratio that satisfies the mass ratio of Y in formula 1.

[0043] For details of the above-mentioned manufacturing method, the above description of the composition can be referred to. Incidentally, the above-mentioned JP-A-2004-51398 (Patent Document 1) discloses a manufacturing method of dry mortar including mixing hydraulic clinker, gypsum and admixture and simultaneously grinding them (see claim 7 of JP-A-2004-51398, etc.). In contrast, in the above-mentioned manufacturing method, a cement clinker fine aggregate having a coarse grain ratio satisfying the formula 1 is prepared, and this cement clinker fine aggregate is mixed with fine powder at a ratio satisfying the mass ratio of Y in the formula 1. Therefore, it is preferable not to perform a grinding process on the mixture of the cement clinker fine aggregate and the fine powder after mixing.

[0044] [Method of manufacturing recycled materials] As described above, in one embodiment, the composition can be a hardened body. One aspect of the present invention relates to a method for producing cement, which includes crushing the hardened body to obtain a recovered material. The recovered material usually contains a large amount of clinker aggregate that has not reacted with water. The clinker aggregate and ground slag powder that have reacted with water become pozzolans, and can be used as cement because they have hydraulic properties as a whole when crushed. The recovered material can also be used as a cement clinker raw material, and cement clinker can be obtained by burning the recovered material as necessary, and cement or cement clinker fine aggregate can be obtained by crushing the cement clinker fine aggregate. The cement clinker fine aggregate thus obtained can also be mixed with ground blast furnace slag or the like to prepare a composition that satisfies formula 1 again. When a coarse aggregate with a low calcium content is used in the hardened body, the coarse aggregate may be separated to recycle more of the used hardened body. EXAMPLES

[0045] The present invention will be further described below based on examples, although the present invention is not limited to the embodiments shown in the examples.

[0046] Table 1 shows details of the samples used in the examples and comparative examples. The ignition loss shown in Table 1 is a value determined by the method described in item 5 of JIS A 5202:2010. The chemical compositions shown in Table 1 were determined by quantitative analysis using an X-ray fluorescence analyzer (Rigaku Corporation, ZSX PrimusII) in accordance with JIS R 5204:2019. The density of the fine powder shown in Table 1 was determined in accordance with JIS R 5201:2015, and the bone dry density of the cement clinker fine aggregate was determined in accordance with JIS A 1109:2020.

[0047] Table 2 shows the mineral composition of the cement clinker. The mineral composition was analyzed by the Rietveld method using an X-ray diffractometer (D8 ADVANCE manufactured by Bruker Japan) and analysis software (DIFFRAC plus TOPAS (Ver5.0) manufactured by Bruker Japan). Specifically, the theoretical profiles of various minerals were fitted to the measured profiles obtained from the results of powder X-ray diffraction to determine the content of each crystalline phase. The mineral composition shown in Table 2 is in mass%.

[0048] [Table 1]

[0049] [Table 2]

[0050] In the examples and comparative examples, the cement clinker fine aggregate shown in Table 3 was used. The cement clinker fine aggregate shown in Table 3 is a cement clinker fine aggregate obtained by combining crushing, classification and mixing of the cement clinkers shown in Tables 1 and 2 so as to have the coarse particle ratio shown in Table 3.

[0051] [Examples 1 to 26, Comparative Examples 1 and 2] A mortar composition was prepared in accordance with JIS R 5201:2015, except that the aggregate and fine powder shown in Table 3 were charged into the mixer in a mixing ratio satisfying Y in Table 3. The prepared mortar compositions were evaluated for the various items shown in Table 3.

[0052] In Table 3, the values ​​shown in the "fluidity" column are flow values ​​measured by the flow test described in JIS R 5201:2015.

[0053] In Table 3, the value shown in the "Initial setting" column is the initial setting time of concrete measured according to the method described in JIS A 1147:2019 (when the penetration resistance is 3.5 N / mm 2 The value shown in the "Final" column is the final time (the time until the penetration resistance value reaches 28.0 N / mm) measured by the method described in the same JIS. 2 (the time it takes for the

[0054] In Table 3, the values ​​shown in the "Strength" column are compressive strengths at an age of 28 days (28 days or more ±8 hours) measured by the method described in JIS R 5201:2015.

[0055] In Table 3, the values ​​shown in the "Shrinkage" column are values ​​obtained using the "Test method for free shrinkage strain due to drying of mortar and concrete" described in Appendix A (reference) of JIS A 1129-1:2010.

[0056] [Table 3]

[0057] As shown in Table 3, the mortar compositions of Examples 1 to 20, in which cement clinker fine aggregate and blast furnace slag powder were mixed to satisfy Formula 1, showed superior fluidity evaluation results compared to the mortar compositions of Comparative Examples 1 and 2, which did not satisfy Formula 1. Furthermore, from the evaluation results of "strength" shown in Table 3, it can be confirmed that by mixing cement clinker fine aggregate and blast furnace slag powder so as to satisfy formula 1, a hardened body with strength equal to or greater than that obtained when ordinary Portland cement and standard sand manufactured by the Cement Association were used (reference example) was obtained, without the use of highly alkaline materials or alkaline irritants with high alkaline concentrations, the safety of which is difficult to ensure. From the evaluation results of "setting" shown in Table 3, it can be confirmed that by mixing cement clinker fine aggregate and ground granulated blast furnace slag so as to satisfy formula 1, a mortar composition that is fully usable for practical purposes was obtained.

[0058] Comparing Examples 15 and 26 with Examples 21 to 25 shown in Table 3, it can be seen that by using limestone fine powder (Example 21) or limestone fine powder and gypsum fine powder (Examples 22 to 25) in combination with blast furnace slag fine powder in a specified ratio, it is possible to suppress the drying shrinkage and expansion of the hardened body. [Industrial Applicability]

[0059] One aspect of the present invention is useful in the field of manufacturing cement, concrete, and the like.

Claims

1. Cement clinker fine aggregate and fine powder, The fine powder contains at least ground granulated blast furnace slag, and The following formula 1: Y≦0.225X+2.09 (In formula 1, X represents the coarse particle ratio of the cement clinker fine aggregate, and Y represents the mass ratio of the content of the cement clinker fine aggregate to the content of the fine powder.) A composition that satisfies the above.

2. The fine powder further comprises limestone fine powder; and The composition according to claim 1 , wherein the content of said limestone fine powder is 10% by mass or less, based on 100% by mass of the total amount of said fine powders.

3. The fine powder further comprises limestone fine powder and gypsum fine powder; and The composition according to claim 1, wherein the total amount of the fine powders is 100% by mass, and the total content of the limestone fine powder and the gypsum fine powder is 10% by mass or less.

4. 2. The composition according to claim 1, wherein the cement clinker fine aggregate has a coarseness ratio X of 3.50 or less.

5. The composition according to claim 1 , wherein a mass ratio Y of the content of the cement clinker fine aggregate to the content of the fine powder is 1.50 or more and 3.50 or less.

6. The fine powder further comprises limestone fine powder; and The content of the limestone fine powder is 10% by mass or less, based on the total amount of the fine powder being 100% by mass; The coarse aggregate ratio X of the cement clinker fine aggregate is 3.50 or less, and The composition according to claim 1 , wherein a mass ratio Y of the content of the cement clinker fine aggregate to the content of the fine powder is 1.50 or more and 3.50 or less.

7. The fine powder further includes limestone fine powder and gypsum fine powder, The total amount of the fine powder is 100% by mass, and the total content of the limestone fine powder and the gypsum fine powder is 10% by mass or less. The coarse aggregate ratio X of the cement clinker fine aggregate is 3.50 or less, and The composition according to claim 1, wherein a mass ratio X of the content of the cement clinker fine aggregate to the content of the fine powder is 1.50 or more and 3.50 or less.

8. The composition according to any one of claims 1 to 7, which further contains water and is cured to form a hardened product.

9. A method for producing the composition according to any one of claims 1 to 7, comprising the steps of: The method for producing the present invention includes mixing a cement clinker fine aggregate having a coarse particle ratio satisfying the formula 1 with a fine powder in a ratio satisfying the mass ratio of Y in the formula 1.

10. A method for producing cement comprising grinding the composition of claim 8.

Citation Information

Patent Citations

  • High-strength dry mortar and its preparation process

    JP2004051398A