Resin composition
The resin composition with polyarylene ether ketone and untreated carbon fibers addresses the interfacial shear strength issue by enhancing bonding through radical interactions, achieving superior adhesion and strength.
Patent Information
- Application Number
- JP2023053516
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional resin compositions with aromatic polyether and carbon fiber lack sufficient interfacial shear strength at their interface.
A resin composition comprising a specific aromatic polyether, such as polyarylene ether ketone, and carbon fibers without a surface treatment agent, with a controlled radical content, enhances interfacial bonding through radical interactions.
The composition achieves excellent interfacial shear strength and maintains processability by optimizing radical content and using untreated carbon fibers, leading to improved adhesion and strength.
Smart Images

Figure 2024141721000001 
Figure 2024141721000002 
Figure 2024141721000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition. Specifically, the present invention relates to a resin composition which contains an aromatic polyether and carbon fibers and has excellent interfacial shear strength at the interface between the aromatic polyether and the carbon fibers. [Background technology]
[0002] Patent Document 1 discloses that a specific aromatic polyether produced by causing a component having a specific polymerization catalytic activity to be present in a reaction system is mixed with a reinforcing material or filler such as glass fiber, carbon fiber, aramid fiber, calcium carbonate, or calcium silicate and then used. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 64-065129 Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the conventional techniques including Patent Document 1, there was found to be room for further improvement in terms of improving the interfacial shear strength at the interface between the aromatic polyether and the carbon fiber.
[0005] An object of the present invention is to provide a resin composition which contains an aromatic polyether and carbon fibers and has excellent interfacial shear strength at the interface between the aromatic polyether and the carbon fibers. [Means for solving the problem]
[0006] As a result of extensive research, the inventors have found that a resin composition containing a specific aromatic polyether and specific carbon fiber has excellent interfacial shear strength at the interface between the aromatic polyether and the carbon fiber, and have completed the present invention. According to the present invention, the following resin composition can be provided. The amount of radicals at 1.25°C is 4.5×10 15 ~100×10 15 A resin composition comprising an aromatic polyether (A) having a molecular weight of 1.0 or more per gram and carbon fiber (B) having no surface treatment agent. 2. The resin composition according to 1, wherein the aromatic polyether (A) is a polyarylene ether ketone. 3. The resin composition according to 1 or 2, wherein the aromatic polyether (A) comprises one or more selected from the group consisting of polyether ether ketone (PEEK), polyether ketone ketone (PEKK) and polyether ketone (PEK). 4. The resin composition according to any one of 1 to 3, comprising 0.01 to 500 parts by mass of the carbon fiber (B) not containing a surface treatment agent per 100 parts by mass of the aromatic polyether (A). 5. The resin composition according to any one of 1 to 4, wherein the carbon fiber (B) comprises at least one selected from the group consisting of PAN-based carbon fiber, pitch-based carbon fiber, thermosetting carbon fiber, phenol-based carbon fiber, vapor-grown carbon fiber, and recycled carbon fiber (RCF). Effect of the Invention
[0007] According to the present invention, it is possible to provide a resin composition which contains an aromatic polyether and carbon fibers and has excellent interfacial shear strength at the interface between the aromatic polyether and the carbon fibers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The resin composition of the present invention will be described in detail below. In this specification, "x to y" represents a numerical range of "not less than x and not more than y." The upper and lower limit values described in relation to the numerical ranges can be combined in any combination. In addition, among the individual embodiments of the aspects of the present invention described below, it is possible to combine two or more embodiments that are not mutually contradictory, and an embodiment combining two or more embodiments is also an embodiment of the aspects of the present invention.
[0009] The resin composition according to one embodiment of the present invention has a radical amount of 4.5×10 at 25° C. 15 ~100×10 15 The carbon fiber (B) contains an aromatic polyether (A) having a molecular weight of 1.0 to 1.0 carbon atoms / g and no surface treatment agent. According to the resin composition of this embodiment, the amount of radicals in the aromatic polyether (A) at 25° C. is 4.5×10 15 ~100×10 15 Since the aromatic polyether (A) has a molecular weight of 1.0 to 1.0 carbon fibers / g, it exhibits excellent adhesion (interfacial shear strength) to the surface of the carbon fiber (B) that does not have a surface treatment agent. Therefore, the resin composition exhibits excellent strength. The reason why such an effect is exhibited is not necessarily clear, but it is speculated that the radicals abundantly contained in the aromatic polyether (A) interact with the surface of the bare carbon fiber (B) or form chemical bonds.
[0010] (Aromatic polyether (A)) The amount of radicals in aromatic polyether (A) at 25°C is 4.5×10 15 When the number of radicals in the aromatic polyether (A) is 100×10 / g or more, the interfacial shear strength at the interface between the aromatic polyether and the carbon fiber is improved. 15 By keeping the content at or less than 1 / g, the generation of crosslinked structures due to reactions between radicals can be suppressed, and the deterioration of moldability and the generation of foreign matter can be suitably suppressed. In one embodiment, the aromatic polyether (A) has a radical amount of 4.5×10 at 25° C. 15 pcs / g or more, 5.0×10 15 pcs / g or more, 7.0×10 15 pcs / g or more, 10×10 15 pcs / g or more, 15×10 15 pcs / g or more, 20×10 15 pcs / g or more, 25×10 15 pcs / g or more, 30×10 15 Pieces / g or more or 35 x 10 15 pcs / g or more, and 100×10 15 pcs / g or less, 90×1015 pcs / g or less, 80×10 15 pcs / g or less, 70×10 15 pcs / g or less, 60×10 15 pcs / g or less, 50×10 15 pcs / g or less, 45×10 15 Pieces / g or less or 40 x 10 15 It is less than 1 / g. In one embodiment, the aromatic polyether (A) has a radical amount of 5.0×10 at 25° C. 15 ~90×10 15 pieces / g, 10×10 15 ~80×10 15 pieces / g, 20×10 15 ~70×10 15 Pieces / g or 30 x 10 15 ~60×10 15 Pieces / g. The amount of radicals in the aromatic polyether (A) at 25°C can be increased, for example, by using a monomer containing a chlorine atom as a reactive group (e.g., 4,4'-dichlorobenzophenone, etc.) as a monomer when synthesizing (polymerizing) the aromatic polyether (A). The radical amount of the aromatic polyether at 25° C. is a value measured by the method described in the Examples.
[0011] In one embodiment, the aromatic polyether (A) is a polyarylene ether ketone. In one embodiment, the aromatic polyether (A) comprises one or more selected from the group consisting of polyetheretherketone (PEEK), polyetherketoneketone (PEKK) and polyetherketone (PEK). In one embodiment, the aromatic polyether (A) comprises polyetheretherketone (PEEK).
[0012] In one embodiment, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, 99% by mass or more, 99.5% by mass or more, or substantially 100% by mass of the aromatic polyether (A) is one or more selected from the group consisting of polyetheretherketone (PEEK), polyetherketoneketone (PEKK), and polyetherketone (PEK). In this specification, the term "substantially 100 mass %" means that unavoidable impurities may be included.
[0013] In one embodiment, at least 50% by weight, at least 60% by weight, at least 70% by weight, at least 80% by weight, at least 90% by weight, at least 95% by weight, at least 97% by weight, at least 99% by weight, at least 99.5% by weight, or substantially 100% by weight of the aromatic polyether (A) is polyetheretherketone (PEEK).
[0014] In one embodiment, the aromatic polyether (A) contains a structural unit represented by the following formula (1) and a structural unit represented by the following formula (2). [ka]
[0015] In one embodiment, the aromatic polyether (A) contains a repeating unit represented by the following formula (3): [ka]
[0016] The structural unit represented by formula (3) is a linkage between a structural unit represented by formula (1) and a structural unit represented by formula (2).
[0017] In one embodiment, the aromatic polyether (A) does not contain any other structure than the structural units represented by formula (1) and formula (2).
[0018] In one embodiment, the aromatic polyether (A) contains structures other than the structural units represented by formula (1) and formula (2) within a range that does not impair the effects of the present invention.
[0019] In one embodiment, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, 99% by mass or more, 99.5% by mass or more, or substantially 100% by mass of the aromatic polyether (A) is a structural unit represented by formula (1) and a structural unit represented by formula (2), or a repeating unit represented by formula (3).
[0020] In one embodiment, in the aromatic polyether, the molar ratio of the structural unit represented by formula (1) to the structural unit represented by formula (2) (structural unit represented by formula (1) : structural unit represented by formula (2)) is 47.5:52.5 to 52.5:47.5, 48.0:52.0 to 52.0:48.0, 48.5:51.5 to 51.5:48.5, 49.0:51.0 to 51.0:49.0, or 49.5:50.5 to 50.5:49.5. The number of moles of the structural unit represented by formula (1) may be larger than, smaller than, or the same as the number of moles of the structural unit represented by formula (2).
[0021] The terminal structure of the main chain of the aromatic polyether (A) is not particularly limited. In one embodiment, the structural unit represented by formula (1) is disposed at one or more ends of the main chain of the aromatic polyether (A). In this case, the end structure bonded to the structural unit may be a halogen atom. The halogen atom may be, for example, a chlorine atom (Cl) or a fluorine atom (F). In one embodiment, the structural unit represented by formula (2) is disposed at one or more ends of the main chain of the aromatic polyether (A). In this case, the end structure bonded to the structural unit may be, for example, a hydrogen atom (H) or the like (when the end structure is a hydrogen atom (H), a hydroxyl group is formed together with the oxygen atom (O) in the structural unit). The terminal structure of the aromatic polyether (A) may be, for example, a structure in which the above-mentioned halogen atom or hydroxyl group is replaced with a hydrogen atom (H), etc. The terminal structure may have a structure other than those exemplified above.
[0022] The melt flow rate of the aromatic polyether (A) is not particularly limited. In one embodiment, the melt flow rate of the aromatic polyether (A) is 1500 g / 10 min or less, 1000 g / 10 min or less, 500 g / 10 min or less, 300 g / 10 min or less, 200 g / 10 min or less, 100 g / 10 min or less, 80 g / 10 min or less, or 60 g / 10 min or less, and is 0.0001 g / 10 min or more, 0.0005 g / 10 min or more, or 0.001 g / 10 min or more. The aromatic polyether (A) has a melt flow rate of, for example, 0.0001 to 1500 g / 10 min, preferably 0.0005 to 500 g / 10 min, and more preferably 0.001 to 100 g / 10 min. The melt flow rate of the aromatic polyether (A) is a value measured by the method described in the Examples.
[0023] (Carbon fiber without surface treatment (B)) Conventionally, carbon fibers coated with a surface treatment agent are usually used as carbon fibers blended to reinforce resins. Examples of the surface treatment agent include sizing agents and resins for promoting dispersion of carbon fibers in resins. In contrast, the present invention uses carbon fibers (B) that are free of a surface treatment agent. This allows the radicals abundantly contained in the aromatic polyether (A) to interact with the surface of the bare carbon fibers (B) and form chemical bonds, thereby providing excellent adhesion (interfacial shear strength).
[0024] The carbon fiber (B) is not particularly limited as long as it is free of a surface treatment agent. The term "carbon fiber (B) free of a surface treatment agent" means that the carbon surface of the carbon fiber itself is not covered with a surface treatment agent. In one embodiment, the carbon fiber (B) includes at least one selected from the group consisting of PAN-based carbon fiber, pitch-based carbon fiber, thermosetting carbon fiber, phenol-based carbon fiber, vapor-grown carbon fiber, and recycled carbon fiber (RCF).
[0025] In one embodiment, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, 99% by mass or more, 99.5% by mass or more, or substantially 100% by mass of the carbon fiber (B) is one or more types selected from the group consisting of PAN-based carbon fiber, pitch-based carbon fiber, thermosetting carbon fiber, phenol-based carbon fiber, vapor-grown carbon fiber, and recycled carbon fiber (RCF).
[0026] (Other ingredients) In one embodiment, the resin composition includes components other than the aromatic polyether (A) and the carbon fibers (B) that are free of a surface treatment agent. The other components are not particularly limited, and examples thereof include other resins other than the aromatic polyether (A). Examples of the other resins include fluororesins such as polytetrafluoroethylene. As the other components, one type may be used alone, or two or more types may be used in combination. In one embodiment, the resin composition does not contain any other components than the aromatic polyether (A) and the carbon fibers (B) that are free of a surface treatment agent.
[0027] (Composition) In the resin composition, the contents of the aromatic polyether (A) and the carbon fiber (B) without a surface treatment agent are not particularly limited and can be appropriately set according to the application of the resin composition, etc. Regardless of the contents of each of these, as long as the aromatic polyether (A) and the carbon fiber (B) without a surface treatment agent are at least in contact with each other in the resin composition, excellent adhesion (interfacial shear strength) is exhibited at the contact portion, and the effects of the present invention are exhibited. In one embodiment, the resin composition contains 0.01 to 500 parts by mass of carbon fibers (B) without a surface treatment agent based on 100 parts by mass of the aromatic polyether (A). The amount of the carbon fiber (B) without a surface treatment agent relative to 100 parts by mass of the aromatic polyether (A) is, for example, 1 to 400 parts by mass, preferably 10 to 300 parts by mass, and more preferably 20 to 200 parts by mass.
[0028] In one embodiment, 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, 95% by weight or more, 97% by weight or more, 99% by weight or more, 99.5% by weight or more, or substantially 100% by weight of the resin composition is Aromatic polyether (A) and carbon fiber (B) free of a surface treatment agent, The components are aromatic polyether (A), carbon fiber without a surface treatment agent (B), and the other components described above.
[0029] (Method of producing resin composition) In one embodiment, the resin composition is produced by mixing the aromatic polyether (A) and the carbon fiber (B) without a surface treatment agent. The mixing method is not particularly limited as long as the aromatic polyether (A) and the carbon fiber (B) without a surface treatment agent are at least brought into contact with each other. Specific examples of the mixing method include a method of kneading the aromatic polyether (A) and the carbon fiber (B) without a surface treatment agent, and a method of impregnating an aggregate of the carbon fiber (B) without a surface treatment agent with the aromatic polyether (A). The aromatic polyether (A) can be produced, for example, by polymerizing hydroquinone and 4,4'-dichlorobenzophenone. As the carbon fiber (B) without a surface treatment agent, carbon fiber having no surface treatment agent attached to its surface may be used, or carbon fiber from which the surface treatment agent attached to the surface has been removed by cleaning or the like may be used.
[0030] (Application) The use of the resin composition of this embodiment is not particularly limited, and can be widely applied to various uses requiring strength. The resin composition is suitable for use as a metal substitute material, particularly for uses requiring heat resistance, solvent resistance, and durability. More specifically, it is suitable for use as a bearing, gasket, structural material, etc. EXAMPLES
[0031] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0032] Example 1 In a 300 ml separable flask, 0.1600 mol of hydroquinone and 0.1622 mol of 4,4'-dichlorobenzophenone were added as monomers. In addition, 0.0003202 mol of 4-phenoxyphenol was added. In the separable flask, potassium carbonate (K 2 CO 3 0.1860 mol of ) was added, and 140 g of diphenyl sulfone was added as a solvent. A ribbon heater was wrapped around the top of the separable flask, and glass wool was wrapped around it to keep it warm. The entire bottom of the separable flask was also wrapped in a mantle heater. Under nitrogen (flow rate: 0.1 L / min), the reaction mixture in the separable flask was heated and stirred using a mechanical stirrer. The ribbon heater was set to 150°C and the mantle heater to 165°C, and the mixture was heated for 30 minutes while stirring at a stirring speed of 100 rpm. The stirring speed was then changed to 210 rpm, and the reaction mixture was heated to 200°C over 30 minutes. After the temperature was increased, the temperature was kept at 200°C for 1 hour, and then increased again to 250°C over 30 minutes. After the temperature was maintained at 250°C for 1 hour, the stirring speed was changed to 250 rpm and the temperature was raised to 300°C over 30 minutes. After the temperature was raised, the temperature was kept at 300°C for 2 hours, after which the reaction was terminated and the mother liquid was taken out. The recovered product was pulverized and washed with acetone and water to obtain a polymer (aromatic polyether (A)).
[0033] <Evaluation method> Melt Flow Rate Measurement The melt flow rate of the resulting aromatic polyether (A) was measured in accordance with JIS K 7210-1:2014 (ISO 1133-1:2011). The results are shown in Table 1. [Melt flow rate measurement conditions] Equipment: Melt indexer (Tateyama Scientific Co., Ltd. L-220) ·Measurement temperature: 380℃ Measurement load (including piston mass): 2.16 kg Cylinder inner diameter: 9.550mm Die inner diameter: 2.095mm Die length: 8.000mm Piston head length: 6.35mm Piston head diameter: 9.474mm (Piston mass: 110.0g) Procedure: The sample was dried at 150°C for at least 2 hours in advance. The sample was placed in a cylinder, the piston was inserted, and preheated for 6 minutes. A load was applied, the piston guide was removed, and the molten sample was extruded from the die. The sample was cut out at a specified range of piston movement and at a specified time (t [s]), and its mass was measured (m [g]). The MI was calculated using the following formula: MI[g / 10min]=600 / t×m
[0034] Measurement of radical amount The amount of radicals per unit weight of aromatic polyether was measured by ESR (electron spin resonance) method under the following conditions and procedures. [ESR measurement conditions] ESR device: Bruker Japan "ESR5000" ·ESR sample tube diameter: 5mm Microwave Power: 0.5mW Modulation: 0.1mT Modulation Frequency: 100kHz ·SweepTime:60 seconds B Range: 330~345mT ·Measurement temperature: Room temperature (25℃) Number of times: 4 [procedure] First, CuSO 4 5H 2The ESR measurement of O was performed, and the peak integral value was calculated. Then, the ESR measurement of the actual sample (aromatic polyether) was performed, and the peak integral value of the actual sample was calculated. CuSO 4 5H 2 The amount of radicals per unit weight of the actual sample was calculated using the spin amount and peak integral value of O and the peak integral value of the actual sample.
[0035] Measurement of interfacial shear strength (microdroplet method) In order to evaluate the interfacial shear strength between the aromatic polyether and the carbon fiber, the following test was carried out by the microdroplet method. The "microdroplet method" is a method for evaluating the interfacial adhesion between a single fiber and a resin by attaching a resin particle (droplet) to a single fiber, fixing the droplet, and then performing a pull-out test of the single fiber from the droplet. In the microdroplet method, the interfacial shear strength is calculated from the following formula. τ=F / (πDL) In the formula, τ is the interfacial shear strength [MPa], F is the maximum pull-out load [mN], L is the length of the single fiber embedded in the droplet [μm], and D is the fiber diameter [μm]. In this example, droplets were prepared in a nitrogen atmosphere at a temperature of 370°C using a "MODEL HM410" manufactured by Toei Sangyo Co., Ltd., and then cooled to room temperature (25°C), with a pulling speed of 0.12 mm / min and a maximum load of 1 N on the load cell. The carbon fiber used was "IM7" manufactured by Hxcel Co., Ltd. (fiber diameter 5.2 μm, non-sized product) without a surface treatment agent. The test was performed 20 times, and the interfacial shear strength [MPa] was calculated from the average value.
[0036] Comparative Example 1 A commercially available aromatic polyether ("151G" manufactured by Victrex plc) was evaluated in the same manner as in Example 1, and the results are shown in Table 1.
[0037] Comparative Example 2 A commercially available aromatic polyether ("KT880FP" manufactured by Solvay SA) was evaluated in the same manner as in Example 1, and the results are shown in Table 1.
[0038] Comparative Example 3 A commercially available aromatic polyether ("2000P" manufactured by Evonik Industries AG) was evaluated in the same manner as in Example 1, and the results are shown in Table 1.
[0039] [Table 1]
[0040] <Evaluation> From Table 1, the amount of radicals per unit mass of aromatic polyether is 4.5 × 10 15 ~100×10 15 It was found that a density of 1000 particles / g ensures excellent adhesion to carbon fiber, i.e., excellent interfacial shear strength.
Claims
1. The amount of radicals at 25°C is 4.5 x 10 15 ~100 x 10 15 A resin composition comprising an aromatic polyether (A) having a molecular weight of 1.0 to 1.0 carbon fibers per gram and carbon fibers (B) not containing a surface treatment agent.
2. The resin composition according to claim 1 , wherein the aromatic polyether (A) is a polyarylene ether ketone.
3. The resin composition according to claim 1 or 2, wherein the aromatic polyether (A) comprises one or more selected from the group consisting of polyether ether ketone (PEEK), polyether ketone ketone (PEKK) and polyether ketone (PEK).
4. The resin composition according to claim 1 or 2, comprising 0.01 to 500 parts by mass of the carbon fiber (B) without a surface treatment agent per 100 parts by mass of the aromatic polyether (A).
5. The carbon fiber (B) comprises at least one selected from the group consisting of PAN-based carbon fiber, pitch-based carbon fiber, thermosetting carbon fiber, phenol-based carbon fiber, vapor-grown carbon fiber, and recycled carbon fiber (RCF). The resin composition according to claim 1 or 2.