Rubber composition, vulcanization molded body and rubber roll

The rubber composition addresses the issue of inadequate water and alkali resistance in conventional vulcanized products by formulating chloroprene polymers with specific additives, resulting in products with enhanced durability for industrial applications.

JP2024141772AInactive Publication Date: 2024-10-10DENKA CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023053595
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional rubber compositions lack adequate water resistance and alkali resistance in vulcanized products, limiting their effectiveness in harsh environments.

Method used

A rubber composition formulation is developed, where the hardness and heat generation of vulcanized molded products are adjusted to satisfy specific relationships, incorporating chloroprene polymers, organic peroxides, vulcanizing agents, and other additives to enhance water and alkali resistance.

Benefits of technology

The composition achieves vulcanized products with excellent water and alkali resistance, suitable for applications in acid and alkali cleaning lines, and other industrial uses requiring durability in harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141772000001
    Figure 2024141772000001
  • Figure 2024141772000002
    Figure 2024141772000002
  • Figure 2024141772000003
    Figure 2024141772000003
Patent Text Reader

Abstract

To provide a rubber composition capable of obtaining a vulcanization molded body having excellent water resistance and alkali resistance.SOLUTION: There is provided a rubber composition comprising a rubber component, wherein when the hardness of a laminate obtained by laminating a vulcanization molded body 1 for testing of the rubber composition until the thickness is 6.0 mm or more as measured by a type A durometer based on JIS K 6253-3:2023 is defined as X and the heat generation determined by evaluating a vulcanization molded body 2 for testing of the rubber composition by a constant strain flexometer test under the conditions of 40°C, a strain of 0.175 inch, a load of 55 pounds and a frequency of 1800 times per minute based on JIS K 6265:2018 is defined as Y, the hardness X and heat generation T satisfy the following expression (1), the vulcanization molded body 1 for testing is a sheet-like vulcanization molded body having a thickness of 2 mm obtained by press-vulcanizing the rubber composition under the conditions of 170°C and 20 minutes based on JIS K 6299:2012 and the vulcanization molded body 2 for testing is a cylindrical vulcanization molded body having a diameter of 15 mm and a height of 25 mm obtained by press-vulcanizing the rubber composition under the conditions of 170°C and 20 minutes. 1.4X-Y>20.0 (1)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition, a vulcanized molded article, and a rubber roll. [Background technology]

[0002] Rubber products are widely used as materials for general industrial transmission belts and conveyor belts, automotive air springs, vibration-proof rubber, hoses, wipers, immersion products, sealing parts, adhesives, boots, rubber-coated cloth, rubber rolls, etc.

[0003] For example, Patent Document 1 discloses an invention relating to a sulfur-modified chloroprene rubber composition comprising a sulfur-modified chloroprene rubber, a vulcanization accelerator, zinc oxide, and magnesium oxide, in which the blending amount of the vulcanization accelerator is 0.1 to 5 parts by weight, and the blending amounts of zinc oxide and magnesium oxide are specified by a predetermined relational expression between each blending amount and the Mooney scorch time t. Furthermore, Patent Document 2 discloses an invention relating to a copolymer of a chloroprene monomer and an unsaturated nitrile compound, which has a Mooney viscosity ML(1+4)100°C of 20 to 80 and has a functional group with a specific structure. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-209522 [Patent Document 2] International Publication No. 2020 / 044899 Summary of the Invention [Problem to be solved by the invention]

[0005] However, conventional rubber compositions have room for improvement in terms of water resistance and alkali resistance of vulcanized molded articles of the compositions.

[0006] The present invention has been made in view of the above circumstances, and has an object to provide a rubber composition which can give a vulcanized molded article having excellent water resistance and alkali resistance. [Means for solving the problem]

[0007] According to the present invention, there is provided a rubber composition containing a rubber component, wherein a laminate obtained by stacking test vulcanized molded products 1 of the rubber composition to a thickness of 6.0 mm or more has a hardness measured with a type A durometer based on JIS K 6253-3:2023 of X, and a test vulcanized molded product 2 of the rubber composition is evaluated in a constant strain flexometer test based on JIS K 6265:2018 under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute, and the hardness X and the heat generation Y satisfy the following formula (1), and the test vulcanized molded product 1 is obtained by stacking test vulcanized molded products 1 of the rubber composition to a thickness of 6.0 mm or more, and the hardness X and the heat generation Y satisfy the following formula (1), The rubber composition is provided as a sheet-like vulcanized molded product having a thickness of 2 mm, which is obtained by press-vulcanizing the rubber composition at 170°C for 20 minutes based on JIS C 6299:2012, and the test vulcanized molded product 2 is a cylindrical vulcanized molded product having a diameter of 15 mm and a height of 25 mm, which is obtained by press-vulcanizing the rubber composition at 170°C for 20 minutes. 1.4XY>20.0 (1)

[0008] As a result of intensive research, the present inventors have found that by adjusting the formulation of a rubber composition so that a specific relationship is satisfied between the hardness X of a test vulcanized molded product 1 of the rubber composition and the heat generation Y of a test vulcanized molded product 2 of the rubber composition, a rubber composition can be obtained that can give a vulcanized molded product having excellent water resistance and alkali resistance, and have completed the present invention.

[0009] Various embodiments of the present invention will be described below. The embodiments described below can be combined with each other.

[0010] [1] A rubber composition containing a rubber component, wherein a laminate obtained by stacking test vulcanized molded products 1 of the rubber composition to a thickness of 6.0 mm or more has a hardness measured with a type A durometer based on JIS K 6253-3:2023 of X, and a test vulcanized molded product 2 of the rubber composition is evaluated in a constant strain flexometer test based on JIS K 6265:2018 under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute, Y, where the hardness X and heat generation Y satisfy the following formula (1), and the test vulcanized molded product 1 is obtained by stacking test vulcanized molded products 1 of the rubber composition to a thickness of 6.0 mm or more based on JIS K The test vulcanized molding 1 is a cylindrical vulcanized molding having a diameter of 15 mm and a height of 25 mm, obtained by press-vulcanizing the rubber composition at 170°C for 20 minutes in accordance with 6299:2012. 1.4XY>20.0 (1) [2] The rubber composition according to [1], wherein the hardness X is 40 or more and 98 or less. [3] The rubber composition according to [1] or [2], wherein the rubber component contains a chloroprene-based polymer. [4] The rubber composition according to [3], wherein the chloroprene polymer contains 70 to 85 mass % of chloroprene monomer units relative to 100 mass % of the chloroprene polymer. [5] A vulcanized molded article of the rubber composition according to any one of [1] to [4]. [6] A rubber roll comprising a core and a surface layer provided on the peripheral surface of the core, the surface layer including the vulcanized molded article according to [5], and used in at least one of an acid washing line and an alkali washing line. [7] A vulcanized molded product containing a rubber component, wherein when the vulcanized molded product is used as a test vulcanized molded product 1' having a thickness of 6.0 mm or more, the hardness measured with a type A durometer based on JIS K 6253-3:2023 is X', and when the vulcanized molded product is used as a cylindrical test vulcanized molded product 2' having a diameter of 15 mm and a height of 25 mm, the heat generation determined by evaluation in a constant strain flexometer test under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute based on JIS K 6265:2018 is Y', the hardness X' and heat generation Y' satisfy the following formula (2). 1.4X'-Y'>20.0 (2) Effect of the Invention

[0011] According to the rubber composition of the present invention, a vulcanized molded article having excellent water resistance and alkali resistance can be obtained. In addition, since the vulcanized molded article of the present invention has excellent water resistance and alkali resistance, these properties can be utilized to use it as various members requiring water resistance and / or alkali resistance, such as a rubber roll. The rubber roll according to one embodiment of the present invention has excellent water resistance and alkali resistance, and can be used, for example, as at least one of the rubber rolls in an acid washing line and an alkali washing line. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below by illustrating the embodiments of the present invention. The present invention is not limited by these descriptions. The features of the embodiments of the present invention described below can be combined with each other. In addition, each feature can be an invention independently.

[0013] 1. Rubber composition The rubber composition according to the present invention contains a rubber component.

[0014] 1.1 Rubber components The rubber component according to the present invention may contain at least one selected from chloroprene rubber, natural rubber (NR), hydrogenated acrylonitrile butadiene rubber (H-NBR), acrylonitrile butadiene rubber (NBR), and chlorosulfonated polyethylene (CSM). The rubber component preferably contains at least one selected from chloroprene rubber and natural rubber (NR), and the rubber composition according to one embodiment of the present invention preferably contains chloroprene rubber, i.e., preferably contains a chloroprene polymer.

[0015] 1.1.1 Chloroprene rubber The chloroprene rubber according to the present invention refers to a rubber containing a chloroprene polymer having chloroprene (2-chloro-1,3-butadiene) as a monomer unit (monomer unit = structural unit). Examples of the chloroprene polymer include a chloroprene homopolymer and a chloroprene copolymer (a copolymer of chloroprene and a monomer copolymerizable with chloroprene). The polymer structure of the chloroprene polymer is not particularly limited.

[0016] In addition, commercially available 2-chloro-1,3-butadiene may contain a small amount of 1-chloro-1,3-butadiene as an impurity. 2-chloro-1,3-butadiene containing such a small amount of 1-chloro-1,3-butadiene can also be used as the chloroprene monomer of this embodiment.

[0017] The chloroprene polymer according to one embodiment of the present invention may have a monomer unit derived from a monomer other than the chloroprene monomer. The monomer other than the chloroprene monomer is not particularly limited as long as it is copolymerizable with the chloroprene monomer, and examples of the monomer other than the chloroprene monomer include unsaturated nitriles, esters of (meth)acrylic acid (methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc.), hydroxyalkyl (meth)acrylates (2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc.), 2,3-dichloro-1,3-butadiene, 1-chloro-1,3-butadiene, butadiene, isoprene, ethylene, styrene, and sulfur. The chloroprene polymer according to one embodiment of the present invention may contain at least one monomer unit selected from 2,3-dichloro-1,3-butadiene and an unsaturated nitrile monomer. The chloroprene-based polymer according to an embodiment of the present invention may include an unsaturated nitrile monomer unit.

[0018] In the chloroprene polymer according to one embodiment of the present invention, when the chloroprene polymer is taken as 100 mass%, the content of the unsaturated nitrile monomer unit can be 15 to 30 mass%, and more preferably 20 to 25 mass% or less. The content of the unsaturated nitrile monomer unit in the chloroprene rubber according to one embodiment of the present invention is, for example, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30 mass%, and may be within a range between any two of the numerical values ​​exemplified here. By making the content of the unsaturated nitrile monomer unit in the rubber composition equal to or less than the above upper limit, the water resistance and cold resistance of the vulcanized molded product of the rubber composition are further improved. In addition, by including the unsaturated nitrile monomer unit, the oil resistance of the vulcanized molded product of the rubber composition is improved.

[0019] Examples of the unsaturated nitrile include acrylonitrile, methacrylonitrile, ethacrylonitrile, and phenylacrylonitrile. The unsaturated nitrile may be used alone or in combination of two or more. The unsaturated nitrile preferably contains acrylonitrile from the viewpoint of easily obtaining excellent moldability and from the viewpoint of easily obtaining excellent breaking strength, breaking elongation, hardness, tear strength, and oil resistance in the vulcanized molded product.

[0020] The content of unsaturated nitrile monomer units contained in chloroprene rubber can be calculated from the content of nitrogen atoms in the chloroprene rubber. Specifically, the content of nitrogen atoms in 100 mg of chloroprene rubber can be measured using an elemental analyzer (Sumigraph 220F: manufactured by Sumika Chemical Analysis Center Co., Ltd.), and the content of structural units derived from unsaturated nitrile monomers can be calculated. Elemental analysis can be performed under the following conditions. For example, the electric furnace temperatures are set to 900°C for the reactor, 600°C for the reduction furnace, 70°C for the column, and 100°C for the detector, and oxygen is flowed at 0.2 mL / min as the combustion gas and 80 mL / min as the carrier gas. A calibration curve can be created using aspartic acid (10.52%) with a known nitrogen content as a standard substance.

[0021] The chloroprene polymer according to one embodiment of the present invention may contain 70% by mass or more of chloroprene monomer units, preferably 70 to 85% by mass, when the chloroprene polymer is taken as 100% by mass. The content of the chloroprene monomer units in the chloroprene polymer may be, for example, 70, 75, 80, 85, 90, 95, 99, or 100% by mass, and may be within a range between any two of the numerical values ​​exemplified here. By setting the content of the chloroprene monomer units within the above numerical range, a rubber composition can be obtained that can give a molded article having an excellent balance of hardness, tensile strength, and cold resistance.

[0022] The chloroprene polymer according to one embodiment of the present invention may contain 0 to 20 mass% of monomer units other than chloroprene monomer units and unsaturated nitrile monomer units when the chloroprene polymer is taken as 100 mass%. The content of monomer units other than chloroprene monomer units and unsaturated nitrile monomer units in the chloroprene polymer may be, for example, 0, 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20 mass%, and may be within a range between any two of the numerical values ​​exemplified here. By adjusting the copolymerization amount of monomers other than chloroprene monomers and unsaturated nitrile monomers to the above range, the effect of copolymerizing these monomers can be expressed without impairing the properties of the obtained rubber composition.

[0023] The chloroprene-based rubber according to one embodiment of the present invention may include at least one polymer selected from a chloroprene homopolymer, a copolymer containing a chloroprene monomer unit and an unsaturated nitrile monomer unit, and a copolymer containing a chloroprene monomer unit and a 2,3-dichloro-1,3-butadiene monomer unit.

[0024] The rubber component according to the present invention may use one type of chloroprene rubber alone or two or more types of chloroprene rubber in combination. When the rubber composition according to one embodiment of the present invention contains two or more chloroprene-based rubbers, it is preferable that the content based on the total amount of each monomer unit contained in the two or more chloroprene-based polymers is within the above numerical range relative to 100 mass% of the total of the two or more chloroprene-based polymers contained in the rubber composition.

[0025] The chloroprene polymer (such as a chloroprene homopolymer or a chloroprene copolymer) contained in the chloroprene rubber according to the present invention may be a sulfur-modified chloroprene polymer, a mercaptan-modified chloroprene polymer, a xanthogen-modified chloroprene polymer, a dithiocarbonate-based chloroprene polymer, a trithiocarbonate-based chloroprene polymer, a carbamate-based chloroprene polymer, or the like.

[0026] 1.1.2 Chloroprene rubber manufacturing method The method for producing the chloroprene rubber according to the present invention is not particularly limited, but the rubber can be obtained by a production method including an emulsion polymerization step of emulsion-polymerizing raw material monomers including a chloroprene monomer. In the emulsion polymerization step according to one embodiment of the present invention, a chloroprene monomer or a raw material monomer containing a chloroprene monomer and other monomers is emulsion-polymerized using an appropriate amount of an emulsifier, a dispersant, a catalyst, a chain transfer agent, etc., and when the target final conversion rate is reached, a polymerization terminator is added to obtain a latex containing a chloroprene-based polymer containing a chloroprene monomer unit. Next, unreacted monomers can be removed from the polymerization liquid obtained by the emulsion polymerization step. The method is not particularly limited, and examples of the method include a steam stripping method. Thereafter, the pH is adjusted, and a chloroprene rubber containing a chloroprene-based polymer is obtained through conventional processes such as freeze coagulation, water washing, and hot air drying.

[0027] The polymerization initiator used in emulsion polymerization is not particularly limited, and any known polymerization initiator generally used in emulsion polymerization of chloroprene can be used. Examples of the polymerization initiator include organic peroxides such as potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, and t-butyl hydroperoxide.

[0028] The emulsifier used in emulsion polymerization is not particularly limited, and any known emulsifier generally used in emulsion polymerization of chloroprene can be used. Examples of the emulsifier include alkali metal salts of saturated or unsaturated fatty acids having 6 to 22 carbon atoms, alkali metal salts of rosin acid or disproportionated rosin acid (e.g., potassium rosinate), and alkali metal salts of formalin condensates of β-naphthalenesulfonic acid (e.g., sodium salt).

[0029] The molecular weight regulator used in emulsion polymerization is not particularly limited, and any known molecular weight regulator generally used in emulsion polymerization of chloroprene can be used, such as mercaptan compounds, xanthogen compounds, dithiocarbonate compounds, trithiocarbonate compounds, and carbamate compounds. As the molecular weight regulator for the chloroprene rubber according to one embodiment of the present invention, xanthogen compounds, dithiocarbonate compounds, trithiocarbonate compounds, and carbamate compounds can be suitably used.

[0030] The polymerization temperature and the final conversion rate of the monomer are not particularly limited, but the polymerization temperature may be, for example, 0 to 50° C. or 10 to 50° C. The polymerization may be carried out so that the final conversion rate of the monomer falls within the range of 40 to 95% by mass. In order to adjust the final conversion rate, a polymerization terminator that terminates the polymerization reaction may be added to terminate the polymerization when the desired conversion rate is reached.

[0031] The polymerization terminator is not particularly limited, and any known polymerization terminator generally used in emulsion polymerization of chloroprene can be used. Examples of the polymerization terminator include phenothiazine (thiodiphenylamine), 4-t-butylcatechol, 2,2-methylenebis-4-methyl-6-t-butylphenol, etc.

[0032] The chloroprene rubber according to one embodiment of the present invention can be obtained, for example, by removing unreacted monomers by a steam stripping method, adjusting the pH of the latex, and then passing through conventional steps such as freeze coagulation, water washing, and hot air drying.

[0033] Chloroprene rubbers are classified into mercaptan-modified, xanthogen-modified, sulfur-modified, dithiocarbonate-based, trithiocarbonate-based and carbamate-based types depending on the type of molecular weight modifier.

[0034] 1.2 Organic peroxides The rubber composition according to the present invention may contain an organic peroxide, and one or more organic peroxides may be freely selected and used.

[0035] Examples of organic peroxides include dicumyl peroxide, benzoyl peroxide, 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, diisobutyryl peroxide, cumyl peroxy neodecanoate, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxy neodecanoate, di(4-t-butylcyclohexyl) peroxydicarbonate, and di(2-ethylhexyl) peroxydicarbonate. peroxydicarbonate, t-hexyl peroxyneodecanoate, t-butyl peroxyneodecanoate, t-butyl peroxyneoheptanoate, t-hexyl peroxypivalate, t-butyl peroxypivalate, di(3,5,5-trimethylhexanoyl)peroxide, dilauroyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, disuccinic acid peroxide, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, t-hexyl peroxypivalate, dilauroyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, disuccinic acid peroxide, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, Peroxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, t-butylperoxy-2-ethylhexanoate, di(3-methylbenzoyl)peroxide, benzoyl(3-methylbenzoyl)peroxide, dibenzoylperoxide, 1,1-di(t-butylperoxy)-2-methylcyclohexane, 1,1-di(t-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, 2, 2-Di(4,4-di-(t-butylperoxy)cyclohexyl)propane, t-hexylperoxyisopropyl monocarbonate, t-butylperoxymaleic acid, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, t-butylperoxyisopropyl monocarbonate, t-butylperoxy2-ethylhexyl monocarbonate, t-hexylperoxybenzoate, 2,5-di-methyl-2,5-di(benzoylperoxy)hexane, t-butylperoxyacetate, 2,2-di-(t-butylperoxy)butane, t-butyl peroxybenzoate, n-butyl 4,4-di-(t-butylperoxy)valerate, 1,4-bis[(t-butylperoxy)isopropyl]benzene, di-t-hexyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, t-butylcumyl peroxide, di-t-butyl peroxide, p-menthane hydroperoxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3, diisopropylbenzene hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide. Among these, at least one selected from dicumyl peroxide, 1,4-bis[(t-butylperoxy)isopropyl]benzene, t-butyl-α-cumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, and 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3 is preferred, and 1,4-bis[(t-butylperoxy)isopropyl]benzene is particularly preferred.

[0036] From the viewpoint of ensuring processing safety and obtaining a good vulcanized molded product, the rubber composition according to the present invention preferably contains 0 to 5 parts by mass of organic peroxide relative to the rubber component contained in the rubber composition. The content of the organic peroxide is, for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here. In addition, the rubber composition according to one embodiment of the present invention does not contain an organic peroxide, and by adjusting the types and amounts of other components, it is also possible to adjust the hardness X and heat generation Y, and the relationship between the hardness X and heat generation Y.

[0037] 1.3 Vulcanizing agent The rubber composition according to the present invention may contain a vulcanizing agent. The type of vulcanizing agent is not particularly limited as long as it does not impair the effects of the present invention. The vulcanizing agent is preferably a vulcanizing agent that can be used for vulcanizing chloroprene-based rubber. One or more vulcanizing agents may be freely selected and used. An example of the vulcanizing agent is zinc oxide.

[0038] From the viewpoint of ensuring processing safety and being able to obtain a sufficiently vulcanized molded product, the rubber composition according to the present invention preferably contains 1 to 15 parts by mass of a vulcanizing agent relative to the rubber component contained in the rubber composition. The content of the vulcanizing agent is, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass relative to 100 parts by mass of the rubber component contained in the rubber composition, and may be within a range between any two of the numerical values ​​exemplified here.

[0039] 1.4 Acid acceptor The rubber composition according to one embodiment of the present invention may contain an acid acceptor. The acid acceptor may contain at least one selected from the group consisting of hydrotalcite compounds, magnesium-aluminum solid solutions, magnesium oxide, lead oxide, trimead tetroxide, iron trioxide, titanium dioxide, and calcium oxide, and may contain at least one selected from the group consisting of hydrotalcite compounds, magnesium-aluminum solid solutions, and magnesium oxide, and preferably contains magnesium oxide. The acid acceptors may be used alone or in combination of two or more.

[0040] As the hydrotalcite, one represented by the following formula can be used. [M 2+ 1-x M 3+ x (OH)2] x+ [A n-x / n mH2O] x-

[0041] In the above formula, M 2+ :Mg 2+ , Zn2+ At least one divalent metal ion selected from M 3+ :Al 3+ , Fe 3+ At least one trivalent metal ion selected from the following: A n- :Co3 2- , Cl ― , NO3 2- At least one n-type anion selected from the following: X:0 <X≦0.33とすることができる。

[0042] Hydrotalcite is Mg 4.3 Al2(OH) 12.6 CO3·3.5H2O, Mg3ZnAl2(OH) 12 CO3·3H2O, Mg 4.5 Al2(OH) 13 CO3 3.5H2O, Mg 4.5 Al2(OH) 13 CO3, Mg4Al2(OH) 12 CO3·3.5H2O, Mg6Al2(OH) 16 CO3·4H2O, Mg5Al2(OH) 14 CO3·4H2O, Mg3Al2(OH) 10 CO3·1.7H2O, etc., and particularly preferred is Mg 4.3 Al2(OH) 12.6 CO3·3.5H2O, Mg3ZnAl2(OH) 12 CO3·3H2O.

[0043] The amount of the acid acceptor added may be 0.1 to 15 parts by mass relative to 100 parts by mass of the rubber component contained in the rubber composition, and may be, for example, 0.1, 0.2, 0.3, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass, or may be within a range between any two of the numerical values ​​exemplified here.

[0044] 1.5 Maleimide compounds The rubber composition according to one embodiment of the present invention may contain a maleimide compound. The maleimide compounds may be used alone or in combination of two or more.

[0045] The maleimide compound can contribute to the vulcanization of the rubber composition as a co-crosslinking agent. Examples of the maleimide compound include N,N'-o-phenylene bismaleimide, N,N'-m-phenylene bismaleimide, N,N'-p-phenylene bismaleimide, N,N'-(4,4'-diphenylmethane) bismaleimide, 2,2-bis-[4-(4-maleimidophenoxy)phenyl]propane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, and 1,6'-bismaleimide-(2,2,4-trimethyl)hexane. From the viewpoint of improving the heat resistance of the resulting vulcanizate and vulcanized molded article, it is particularly preferable to use N,N'-m-phenylene bismaleimide (also known as m-phenylene dimaleimide).

[0046] The rubber composition according to one embodiment of the present invention may contain 0 to 10 parts by mass of the maleimide compound per 100 parts by mass of the rubber component. The content of the maleimide compound may be, for example, 0, 0.1, 0.2, 0.3, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here. By making the content of the maleimide compound equal to or more than the above lower limit, the vulcanization of the obtained rubber composition proceeds more sufficiently, and a vulcanized molded product having good mechanical properties and heat resistance can be obtained. In addition, by making the content of the maleimide compound equal to or less than the above upper limit, the rubber elasticity of the obtained vulcanized molded product can be sufficiently maintained. In addition, the rubber composition according to one embodiment of the present invention may not contain a maleimide compound, and the hardness X and heat generation Y, as well as the relationship between the hardness X and heat generation Y, may be adjusted by adjusting the types and amounts of other components.

[0047] 1.6 Filling material The rubber composition according to an embodiment of the present invention may contain a filler and may contain carbon black. Examples of carbon black include furnace carbon black such as SAF, ISAF, HAF, EPC, XCF, FEF, GPF, HMF, and SRF, modified carbon black such as hydrophilic carbon black, channel black, lamp black, thermal carbon such as FT and MT, acetylene black, and ketjen black.

[0048] The rubber composition according to the present invention may contain 0 parts by mass or more and less than 100 parts by mass of carbon black per 100 parts by mass of the rubber component. The carbon black content is, for example, 0, 1, 2, 3, 4, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 99 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0049] The rubber composition according to the present invention may contain fillers other than carbon black, provided that the effects of the present invention are not impaired. Examples of fillers other than carbon black include silica such as wet silica filler (hydrated silicic acid), dry silica filler (anhydrous silicic acid), and colloidal silica filler, clay, talc, and calcium carbonate. These may be used alone or in combination of two or more.

[0050] In the rubber composition according to one embodiment of the present invention, when the rubber component is taken as 100 parts by mass, the total amount of carbon black and fillers (reinforcing materials) other than carbon black contained in the rubber composition is preferably 0 to 100 parts by mass. In the rubber composition according to one embodiment of the present invention, when the total amount of carbon black and fillers (reinforcing materials) other than carbon black contained in the rubber composition is taken as 100 mass%, the content of fillers / reinforcing materials other than carbon black can be 50 mass% or less. The content of fillers / reinforcing materials other than carbon black is, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50 mass%, and may be within a range between any two of the numerical values ​​exemplified here. The rubber composition according to one embodiment of the present invention may not contain fillers (reinforcing materials) other than carbon black. In addition, the rubber composition according to one embodiment of the present invention may not contain carbon black and fillers other than carbon black, and the hardness X and heat generation Y, as well as the relationship between hardness X and heat generation Y, can be adjusted by adjusting the types and amounts of other components without blending carbon black and fillers other than carbon black.

[0051] 1.7 Silane coupling agents When the rubber composition according to one embodiment of the present invention contains silica as a filler, it may contain a silane coupling agent. The silane coupling agent is not particularly limited, and those used in commercially available rubber compositions can be used, such as vinyl coupling agents, epoxy coupling agents, styryl coupling agents, methacrylic coupling agents, acrylic coupling agents, amino coupling agents, polysulfide coupling agents, and mercapto coupling agents. In particular, from the viewpoint of scorch resistance and reinforcing effect, vinyl coupling agents, methacrylic coupling agents, and acrylic coupling agents that start reacting under high temperature conditions during crosslinking are preferred.

[0052] The rubber composition according to one embodiment of the present invention may contain 0.5 to 10 parts by mass of a silane coupling agent relative to 100 parts by mass of silica contained in the rubber composition. The content of the silane coupling agent may be, for example, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass relative to 100 parts by mass of silica, and may be within a range between any two of the numerical values ​​exemplified here. Silica may be used alone or in combination of two or more. By containing the above-mentioned silane coupling agent and setting the content of the silane coupling agent within the above numerical range, the dispersibility of the silica filler in the rubber and the reinforcing effect between the rubber and the silica filler can be improved, and the occurrence of scorch can be suppressed.

[0053] 1.8 Lubricants and processing aids The rubber composition according to the present invention may further contain a lubricant and / or a processing aid. The lubricant and processing aid are mainly added to improve processability, such as making the rubber composition easier to peel off from rolls, molding dies, extruder screws, etc. Examples of the lubricant and processing aid include fatty acids such as stearic acid, paraffin-based processing aids such as polyethylene, fatty acid amides, vaseline, factice, etc. These may be used alone or in combination of two or more. The rubber composition according to the present invention may contain 0.1 to 15 parts by mass of the lubricant and processing aid, or may be 1 to 10 parts by mass, based on 100 parts by mass of the rubber component. The content of the lubricant and processing aid may be, for example, 0.1, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0054] 1.9 Vulcanization accelerator The rubber composition according to the present invention may contain a vulcanization accelerator, and may contain 0 to 5.0 parts by mass of the vulcanization accelerator when the rubber composition contained in the composition is 100 parts by mass. The content of the vulcanization accelerator is, for example, 0, 0.1, 0.2.0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here. The rubber composition according to the present invention may also not contain a vulcanization accelerator. The rubber composition according to one embodiment of the present invention may not contain a vulcanization accelerator, and may adjust the types and amounts of other components to adjust the hardness X, heat generation Y, and the relationship between hardness X and heat generation Y.

[0055] The type of vulcanization accelerator is not particularly limited as long as it does not impair the effects of the present invention. The vulcanization accelerator is preferably a vulcanization accelerator that can be used for vulcanization of chloroprene rubber. The vulcanization accelerator can be freely selected and used as one or more types. Examples of the vulcanization accelerator include sulfur, thiuram-based vulcanization accelerators, dithiocarbamate-based vulcanization accelerators, thiourea-based vulcanization accelerators, guanidine-based vulcanization accelerators, xanthogenate-based vulcanization accelerators, and thiazole-based vulcanization accelerators.

[0056] Examples of thiuram vulcanization accelerators include tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and dipentamethylenethiuram tetrasulfide. Examples of dithiocarbamate vulcanization accelerators include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, ferric dimethyldithiocarbamate, and tellurium diethyldithiocarbamate. Examples of the thiourea-based vulcanization accelerator include thiourea compounds such as ethylene thiourea, diethyl thiourea (N,N'-diethyl thiourea), trimethyl thiourea, diphenyl thiourea (N,N'-diphenyl thiourea), and 1,3-trimethylene-2-thiourea. Examples of the guanidine vulcanization accelerator include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salts of dicatechol borate. Examples of the xanthogenate-based vulcanization accelerator include zinc butylxanthogenate and zinc isopropylxanthogenate. Examples of the thiazole-based vulcanization accelerator include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, cyclohexylamine salt of 2-mercaptobenzothiazole, 2-(4'-morpholinodithio)benzothiazole, and N-cyclohexylbenzothiazole-2-sulfenamide. These may be used alone or in combination of two or more.

[0057] 1.10 Other In addition to the above-mentioned components, the rubber composition according to the present invention may further contain components such as an antiaging agent, an antioxidant, a flame retardant, and a vulcanization retarder, as long as the effects of the present invention are not impaired. Examples of the antiaging agent and the antioxidant include ozone antiaging agents, phenolic antiaging agents, amine antiaging agents, acrylate antiaging agents, imidazole antiaging agents, carbamic acid metal salts, waxes, phosphorus antiaging agents, and sulfur antiaging agents. Examples of the imidazole antiaging agents include 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole, and zinc salts of 2-mercaptobenzimidazole. The rubber composition according to the present invention may contain 0.1 to 10 parts by mass of the antiaging agent and the antioxidant in total, relative to 100 parts by mass of the rubber component contained in the rubber composition.

[0058] In the rubber composition according to one embodiment of the present invention, by configuring the types and contents of the components in the rubber composition as described above, the hardness X of a test vulcanization molded product 1 of the rubber composition and the heat generation Y of a test vulcanization molded product 2 of the rubber composition tend to satisfy the relationship of formula (1).

[0059] 2. Method for producing rubber composition The rubber composition according to one embodiment of the present invention can be obtained by kneading the rubber component and other necessary components at a temperature equal to or lower than the vulcanization temperature. A method for producing the rubber composition according to one embodiment of the present invention can include a mixing step of mixing the rubber component and other necessary components at a temperature equal to or lower than the vulcanization temperature.

[0060] A production method according to one embodiment of the present invention can include a first mixing step, a standing step, and a second mixing step. In the first mixing step, raw materials including a rubber component and compounding ingredients for the first mixing step are mixed to obtain a rubber composition precursor, and in the standing step, the rubber composition precursor is stood at 23°C or less for 12 hours or more, and in the second mixing step, the compounding ingredients for the second mixing step are added to the rubber composition precursor after standing and mixed to obtain a rubber composition.

[0061] In the first mixing step, raw materials including a rubber component and a compounding component for the first mixing step are mixed to obtain a rubber composition precursor. The compounding components for the first mixing step may not include a vulcanizing agent, a vulcanization accelerator, an organic peroxide, or a maleimide compound. It is preferable that the compounding components for the first mixing step do not include a component that contributes to vulcanization and crosslinking. The compounding components for the first mixing step may include at least one, two, three, four, five, or six of carbon black, lubricant, processing aid, plasticizer, acid acceptor, and antioxidant, or may include all of these.

[0062] In the standing step, the rubber composition precursor is left standing at 23° C. or lower for 12 hours or more. The standing temperature can be, for example, 5 to 23° C., and may be 5, 8, 11, 14, 17, 20, or 23° C., or may be within a range between any two of the numerical values ​​exemplified here. The standing time can be, for example, 12 to 24 hours, and may be, for example, 12, 14, 16, 18, 20, 22, or 24 hours, or may be within a range between any two of the numerical values ​​exemplified here. In one embodiment of the present invention, the hardness X and heat generation Y can be adjusted by undergoing a standing process.

[0063] In the second mixing step, the compounding components for the second mixing step are added to the rubber composition precursor after standing and mixed to obtain a rubber composition. The compounding components for the second mixing step may include a vulcanizing agent, a vulcanization accelerator, an organic peroxide, and a maleimide compound. The compounding components for the second mixing step may also include carbon black, a lubricant, a processing aid, a plasticizer, an acid acceptor, an anti-aging agent, and the like.

[0064] In each mixing step, examples of the device for kneading the raw material components include conventionally known kneading devices such as a mixer, a Banbury mixer, a kneader mixer, and an open roll.

[0065] 3. Characteristics of rubber composition In one embodiment of the rubber composition, when a laminate obtained by stacking test vulcanized molded products 1 of the rubber composition to a thickness of 6.0 mm or more is measured using a type A durometer based on JIS K 6253-3:2023, X is the hardness of the laminate, and when a test vulcanized molded product 2 of the rubber composition is evaluated using a constant strain flexometer test based on JIS K 6265:2018 under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute, Y is the heat generation determined by the evaluation. The hardness X and heat generation Y satisfy the following formula (1). 1.4XY>20.0 (1)

[0066] Here, the test vulcanized molded article 1 is a sheet-like vulcanized molded article having a thickness of 2 mm obtained by press-vulcanizing a rubber composition at 170° C. for 20 minutes in accordance with JIS K 6299:2012. The test vulcanized molded article 2 was a cylindrical vulcanized molded article having a diameter of 15 mm and a height of 25 mm, which was obtained by press-vulcanizing the rubber composition at 170° C. for 20 minutes.

[0067] The rubber composition according to the present invention is a rubber composition capable of producing a vulcanized molded article having excellent water resistance and alkali resistance by adjusting the hardness X and heat generation Y of the vulcanized molded article of the rubber composition so that the hardness X and heat generation Y satisfy the relationship of formula (1). The hardness X can be controlled by adjusting the manufacturing conditions described later, for example, by the amount of the filler and the plasticizer. The heat generation Y can be controlled by adjusting the manufacturing conditions described later, for example, by the type and amount of the filler, the crosslink density of the obtained vulcanized molded body, and the type and amount of the plasticizer. It is considered that the heat generation Y increases when the amount of the filler is increased, the heat generation Y decreases when the crosslink density becomes dense, and the heat generation Y increases when the amount of the plasticizer is increased. Here, it is presumed that by adjusting the relationship between the hardness X and the heat generation Y to satisfy the formula (1), the amount of the filler, the amount of the plasticizer, the crosslink density, etc. at the hardness X can be adjusted, and thus a rubber composition capable of obtaining a vulcanized molded body having excellent water resistance and alkali resistance can be obtained. The value of (1.4XY) can be greater than 20.0 and equal to or less than 50.0, and can be equal to or less than 45.0. The value of (1.4XY) can be, for example, 20.5, 20.0, 22.0, 24.0, 26.0, 28.0, 30.0, 32.0, 34.0, 36.0, 38.0, 40.0, 42.0, 44.0, 46.0, 48.0, or 50.0, or can be within a range between any two of the values ​​exemplified here.

[0068] In the rubber composition according to one embodiment of the present invention, a laminate in which test vulcanized molded articles 1 of the rubber composition are stacked to a thickness of 6.0 mm or more has a hardness X measured with a type A durometer according to JIS K 6253-3:2023 of preferably 40 to 98. The hardness X is, for example, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 98, and may be within a range between any two of the numerical values ​​exemplified here.

[0069] The hardness X can be controlled by adjusting the manufacturing method of the rubber composition, for example, the presence or absence, the type and the amount of each component blended in the rubber composition, particularly the type and the amount of a filler and a plasticizer, and the manufacturing conditions of the rubber composition (particularly the presence or absence, temperature, and time of a standing process).

[0070] In the rubber composition according to one embodiment of the present invention, the heat generation Y determined by evaluating a vulcanized molded test article 2 of the rubber composition in a constant strain flexometer test under conditions of 40° C., strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute based on JIS K 6265:2018 is preferably 85° C. or less. The heat generation Y may be, for example, 1, 2, 3, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100° C., or may be within a range between any two of the values ​​exemplified here.

[0071] The heat generation Y can be controlled by adjusting the manufacturing method of the rubber composition, in particular the presence or absence, type and amount of each component blended into the rubber composition, such as the presence or absence, type and amount of fillers and components that contribute to vulcanization and crosslinking, as well as the manufacturing conditions of the rubber composition (in particular the presence or absence, temperature and time of a standing process).

[0072] The hardness X and heat generation Y can be specifically evaluated by the method described in the Examples.

[0073] In the rubber composition according to one embodiment of the present invention, when a test vulcanization molding 1 and / or a test vulcanization molding 2 of the rubber composition is immersed in water at 70° C. for 144 hours, the volume change rate ΔV calculated based on JIS K 6258 is preferably less than 9%, more preferably less than 6%. The volume change rate ΔV when immersed in water at 70° C. for 144 hours is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8% or less than 9%, and may be within a range between any two of the numerical values ​​exemplified here.

[0074] In the rubber composition according to one embodiment of the present invention, when a test vulcanization molding 1 and / or a test vulcanization molding 2 of the rubber composition is immersed in 10% sodium hydroxide at 70° C. for 144 hours, the volume change rate ΔV calculated based on JIS K 6258 is preferably less than 10%, more preferably less than 7%. When immersed in water at 70° C. for 144 hours, the volume change rate ΔV is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9% or less than 10%, and may be within a range between any two of the numerical values ​​exemplified here.

[0075] The water resistance and alkali resistance of the vulcanized molded article of the rubber composition can be specifically measured by the method described in the Examples.

[0076] 6. Unvulcanized molded bodies, vulcanized bodies and vulcanized molded bodies The unvulcanized molded body according to one embodiment of the present invention uses the rubber composition according to one embodiment of the present invention, and is a molded body (molded product) of the rubber composition (unvulcanized state) according to one embodiment of the present invention. The manufacturing method of the unvulcanized molded body according to one embodiment of the present invention includes a step of molding the rubber composition (unvulcanized state) according to one embodiment of the present invention. The unvulcanized molded body according to one embodiment of the present invention is made of the rubber composition (unvulcanized state) according to one embodiment of the present invention.

[0077] A vulcanizate according to one embodiment of the present invention is a vulcanizate of the rubber composition according to one embodiment of the present invention. A method for producing a vulcanizate according to one embodiment of the present invention includes a step of vulcanizing the rubber composition according to one embodiment of the present invention.

[0078] The vulcanized molded article according to one embodiment of the present invention is a vulcanized molded article of the rubber composition according to one embodiment of the present invention. The vulcanized molded article according to one embodiment of the present invention uses the vulcanizate according to one embodiment of the present invention, and is a molded article (molded product) of the vulcanizate according to one embodiment of the present invention. The vulcanized molded article according to one embodiment of the present invention is made of the vulcanizate according to one embodiment of the present invention.

[0079] The vulcanized molded article according to one embodiment of the present invention can be obtained by molding a vulcanized product obtained by vulcanizing the rubber composition (unvulcanized state) according to one embodiment of the present invention, and can also be obtained by vulcanizing a molded product obtained by molding the rubber composition (unvulcanized state) according to one embodiment of the present invention. The vulcanized molded article according to one embodiment of the present invention can be obtained by vulcanizing the rubber composition according to one embodiment of the present invention after molding or during molding. The method for producing the vulcanized molded article according to one embodiment of the present invention includes a step of molding the vulcanized product according to one embodiment of the present invention, or a step of vulcanizing the unvulcanized molded article according to one embodiment of the present invention.

[0080] In one embodiment of the present invention, the vulcanized molded product has a hardness of X', measured with a type A durometer based on JIS K 6253-3:2023 when the vulcanized molded product is made into a test vulcanized molded product 1' having a thickness of 6.0 mm or more, and Y', measured with a constant strain flexometer test under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute when the vulcanized molded product is made into a cylindrical test vulcanized molded product 2' having a diameter of 15 mm and a height of 25 mm, based on JIS K 6265:2018. It is preferable that the hardness X' and the heat generation Y' satisfy the following formula (2). 1.4X'-Y'>20.0 (2) The test vulcanized molded body 1' having a thickness of 6.0 mm or more may be a laminate of a plurality of vulcanized molded bodies having a thickness of less than 6.0 mm. The test vulcanized molded body 1' has a thickness of 6.0 mm or more and can be 7.0 mm or less.

[0081] The value of (1.4X'-Y') is greater than 20.0, for example, 20.5, 21.0, 22.0, 24.0, 26.0, 28.0, 30.0, 32.0, 34.0, 36.0, 38.0, 40.0, 42.0, 44.0, 46.0, 48.0, 50.0, and may be within a range between any two of the values ​​exemplified herein.

[0082] The hardness X' of the test vulcanized molded body 1' according to one embodiment of the present invention is, for example, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 98, and may be within a range between any two of the numerical values ​​exemplified here.

[0083] The heat generation Y' of the test vulcanized molded body 2' according to one embodiment of the present invention may be, for example, 1, 2, 3, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100°C, or may be within a range between any two of the values ​​exemplified here.

[0084] The vulcanized molded product according to one embodiment of the present invention has a volume change rate ΔV of preferably less than 9%, more preferably less than 6%, when immersed in water at 70° C. for 144 hours, as calculated based on JIS K 6258. The volume change rate ΔV when immersed in water at 70° C. for 144 hours may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8%, or less than 9%, and may be within a range between any two of the values ​​exemplified here.

[0085] The vulcanized molded product according to one embodiment of the present invention has a volume change rate ΔV calculated based on JIS K 6258 when immersed in 10% sodium hydroxide at 70° C. for 144 hours, which is preferably less than 10%, more preferably less than 7%. The volume change rate ΔV when immersed in water at 70° C. for 144 hours is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9%, or less than 10%, and may be within a range between any two of the numerical values ​​exemplified here.

[0086] The hardness, heat generation, water resistance, and alkali resistance of the vulcanized molded product can be specifically measured by the method described in the Examples. The hardness, heat generation, water resistance, and alkali resistance of the vulcanized molded product can be controlled by adjusting the manufacturing method of the rubber composition, for example, the presence or absence, type, and amount of each component blended in the rubber composition, particularly the presence or absence, type, and amount of a filler or a component that contributes to vulcanization and crosslinking, and the manufacturing conditions of the rubber composition (particularly the presence or absence, temperature, and time of a standing process).

[0087] The unvulcanized molded product, vulcanized product, and vulcanized molded product according to one embodiment of the present invention can be used as rubber parts in various industrial fields such as buildings, structures, ships, railways, coal mines, and automobiles. The rubber composition according to the present invention has excellent water resistance and alkali resistance, and can be used as various members where these properties are required. The rubber composition, vulcanized product, and vulcanized molded product according to one embodiment of the present invention can be used as rubber parts in various industrial fields such as buildings, structures, ships, railways, coal mines, and automobiles, and can be used for rubber parts such as automotive rubber members (e.g., automotive seal materials), hose materials, rubber molded products, gaskets, rubber rolls, industrial cables, industrial conveyor belts, and sponges. In particular, they can be used as transmission belts, conveyor belts, hoses, wipers, immersion products, seal parts, adhesives, boots, rubber-coated cloths, rubber rolls, anti-vibration rubber, or sponge products.

[0088] (Rubber parts for automobiles) Rubber components for automobiles include gaskets, oil seals, and packings, which are components that prevent liquids and gases from leaking and dirt and foreign objects such as rainwater and dust from entering machines and equipment. Specifically, there are gaskets used for fixed applications and oil seals and packings used for moving parts and movable parts. For gaskets where the sealing part is fixed with bolts, various materials are used according to the purpose, as opposed to soft gaskets such as O-rings and rubber sheets. In addition, packings are used for rotating parts such as the shafts of pumps and motors, moving parts of valves, reciprocating parts such as pistons, connecting parts of couplers, water stop parts of water faucets, etc. The rubber composition of the present invention can improve water resistance and alkali resistance. This makes it possible to manufacture automobile parts with excellent oil resistance, which was difficult to do with conventional rubber compositions.

[0089] (Hose material) Hose materials are flexible pipes, and specific examples include high- and low-pressure hoses for water, oil, air, steam, and hydraulic applications. The rubber composition of the present invention can enhance the water resistance and alkali resistance of the hose material while maintaining the processability of the unvulcanized product. This makes it possible to manufacture, for example, a hose material with excellent water resistance and alkali resistance, which was difficult to achieve with conventional rubber compositions.

[0090] (Rubber mold) The rubber molded products include anti-vibration rubber, vibration-damping materials, boots, etc. Anti-vibration rubber and vibration-damping materials are rubbers that prevent the transmission and spread of vibrations, and specifically include torsional dampers, engine mounts, muffler hangers, etc. for automobiles and various vehicles that absorb vibrations during engine operation to prevent noise. The rubber composition of the present invention can improve the water resistance and alkali resistance of anti-vibration rubber and vibration-damping materials. This makes it possible to produce anti-vibration rubber and vibration-damping materials with excellent water resistance and alkali resistance, which was difficult to achieve with conventional rubber compositions. A boot is a bellows-shaped member whose outer diameter gradually increases from one end to the other end, and specifically includes constant velocity joint cover boots, ball joint cover boots (dust cover boots), rack and pinion gear boots, etc., for protecting drive parts of automobile drive systems, etc. The rubber composition of the present invention can improve water resistance and alkali resistance. This makes it possible to manufacture boots that can be used in harsher environments than conventional rubber compositions.

[0091] (Gaskets, etc.) Gaskets, oil seals and packings are components that prevent leakage of liquids and gases and intrusion of garbage and foreign objects such as rainwater and dust into machines and equipment. Specifically, there are gaskets used for fixed applications and oil seals and packings used for moving parts. For gaskets where the sealing part is fixed with bolts, various materials are used according to the purpose, as opposed to soft gaskets such as O-rings and rubber sheets. In addition, packings are used for rotating parts such as the shafts of pumps and motors, movable parts of valves, reciprocating parts such as pistons, connecting parts of couplers, water stop parts of water faucets, etc. The rubber composition of the present invention can improve the water resistance and alkali resistance of these members. This makes it possible to manufacture sealing members with excellent water resistance and alkali resistance, which was difficult to achieve with conventional rubber compositions.

[0092] (Rubber roll) A rubber roll is manufactured by adhesively covering a metal core such as an iron core with rubber, and is generally manufactured by winding a rubber sheet around a metal iron core in a spiral shape. Rubber materials such as NBR, EPDM, and CR are used for rubber rolls according to the required characteristics of various applications such as papermaking, various metal manufacturing, film manufacturing, printing, general industrial use, agricultural machinery such as rice hulling, and food processing. CR has good mechanical strength that can withstand the friction of the object being conveyed, so it is used in a wide range of rubber roll applications. Furthermore, there is a problem that rubber rolls that convey heavy objects are deformed by load, and improvements are required. The rubber composition of the present invention can increase the water resistance and alkali resistance of the rubber roll. This makes it possible to manufacture an embossing rubber roll that is excellent in water resistance and alkali resistance, which was difficult to achieve with conventional rubber compositions. The rubber composition according to one embodiment of the present invention can be used as a rubber roll used in at least one of an acid washing line and an alkali washing line.

[0093] A rubber roll according to one embodiment of the present invention comprises a core and a surface layer provided on the peripheral surface of the core, the surface layer including the vulcanized molded article described above, and the rubber roll is used in at least one of an acid washing line and an alkali washing line.

[0094] (Industrial Cables) An industrial cable is a linear member for transmitting electrical or optical signals. It is made by covering a good conductor such as copper or a copper alloy, or an optical fiber, with an insulating covering layer, and a wide variety of industrial cables are manufactured depending on their structure and installation location. The rubber composition of the present invention can improve the water resistance and alkali resistance of industrial cables. This makes it possible to manufacture industrial cables with excellent water resistance and alkali resistance, which was difficult to achieve with conventional rubber compositions.

[0095] (Industrial conveyor belts) Industrial conveyor belts are available in rubber, resin, and metal, and are selected according to a wide variety of usage methods. Among these, rubber conveyor belts are inexpensive and widely used, but when used in an environment where friction and collision with conveyed goods are frequent, they tend to deteriorate and break. The rubber composition of the present invention can improve the water resistance and alkali resistance of industrial conveyor belts. This makes it possible to manufacture industrial conveyor belts with excellent water resistance and alkali resistance that can be used in harsh environments, which was difficult with conventional rubber compositions.

[0096] (sponge) A sponge is a porous material with numerous fine holes inside, and is specifically used in vibration-proofing materials, sponge seal parts, wet suits, shoes, etc. The rubber composition of the present invention can improve the acid resistance and water resistance of the sponge. In addition, since a chloroprene-unsaturated nitrile copolymer rubber is used, it is also possible to improve the flame retardancy of the sponge. This makes it possible to produce a sponge with excellent water resistance and alkali resistance that can be used in harsh environments, which was difficult with conventional rubber compositions, and a sponge with excellent flame retardancy. Furthermore, the hardness of the sponge obtained can be appropriately adjusted by adjusting the content of the foaming agent, etc.

[0097] Examples of methods for molding the rubber composition (unvulcanized state) and vulcanized product according to one embodiment of the present invention include press molding, extrusion molding, and calendar molding. The temperature for vulcanizing the rubber composition may be appropriately set according to the composition of the rubber composition, and may be 140 to 220°C. The vulcanization temperature may be, for example, 140, 150, 160, 170, 180, 190, 200, 210, or 220°C, and may be within a range between any two of the numerical values ​​exemplified here. The vulcanization time for vulcanizing the rubber composition may be appropriately set according to the composition of the rubber composition, the shape of the unvulcanized molded product, and the like, and may be 10 to 300 minutes. For example, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300 minutes, or may be within a range between any two of the values ​​exemplified here. EXAMPLES

[0098] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.

[0099] <Production method of chloroprene rubber (A-2)> In a polymerization vessel having an internal volume of 3 L equipped with a heating / cooling jacket and an agitator, 24 parts by mass of chloroprene (monomer), 24 parts by mass of acrylonitrile (monomer), 0.5 parts by mass of diethyl xanthogen disulfide, 200 parts by mass of pure water, 5.00 parts by mass of potassium rosinate (manufactured by Harima Chemicals Co., Ltd.), 0.40 parts by mass of sodium hydroxide, and 2.0 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (manufactured by Kao Corporation) were added. Next, 0.1 parts by mass of potassium persulfate was added as a polymerization initiator, and emulsion polymerization was carried out under a nitrogen gas flow at a polymerization temperature of 40°C. The above-mentioned chloroprene was added in portions starting 20 seconds after the start of polymerization, and the portion-added flow rate was adjusted with an electromagnetic valve based on the change in the heat quantity of the refrigerant for 10 seconds from the start of polymerization, and the flow rate was readjusted every 10 seconds thereafter, so that the polymerization was carried out continuously. When the polymerization rate relative to the total amount of chloroprene and acrylonitrile reached 50%, 0.02 parts by mass of phenothiazine, a polymerization terminator, was added to terminate the polymerization. Thereafter, unreacted monomers in the reaction solution were removed under reduced pressure to obtain a chloroprene-based latex containing a chloroprene-acrylonitrile copolymer.

[0100] The above-mentioned polymerization rate [%] of the chloroprene-based latex was calculated from the dry mass when the chloroprene-based latex was air-dried. Specifically, it was calculated from the following formula (A). In the formula, the "solid content concentration" is the concentration [mass %] of the solid content obtained by heating 2 g of the sampled chloroprene-based latex at 130°C and excluding volatile components such as the solvent (water), volatile chemicals, and raw materials. The "total charge amount" is the total amount [g] of the raw materials, reagents, and solvent (water) charged in the polymerization vessel from the start of polymerization to a certain time. The "evaporation residue" is the mass [g] of the chemicals and raw materials charged from the start of polymerization to a certain time that do not volatilize under the condition of 130°C and remain as solids together with the polymer. The "charge amount of monomer" is the total amount [g] of the monomer charged in the polymerization vessel at the beginning and the amount of the monomer added in portions from the start of polymerization to a certain time. The "monomer" here is the total amount of chloroprene and acrylonitrile. Conversion rate = {[(total charge amount × solid concentration / 100) - evaporation residue] / charge amount of monomer} × 100 (A)

[0101] The pH of the above-mentioned chloroprene-based latex (R-2) was adjusted to 7.0 using acetic acid or sodium hydroxide, and then the chloroprene-based latex was freeze-coagulated on a metal plate cooled to -20°C to break the emulsion, thereby obtaining a sheet. The sheet was washed with water and then dried at 130°C for 15 minutes to obtain a solid chloroprene-based rubber (A-2).

[0102] The content of acrylonitrile monomer units contained in the chloroprene rubber (A-2) was calculated from the content of nitrogen atoms in the chloroprene-acrylonitrile copolymer rubber. Specifically, the content of nitrogen atoms in 100 mg of the chloroprene rubber (A-2) was measured using an elemental analyzer (Sumigraph 220F: manufactured by Sumika Chemical Analysis Center Co., Ltd.), and the content of acrylonitrile monomer units was calculated. The content of acrylonitrile monomer units was 20.0 mass%.

[0103] The above elemental analysis was carried out as follows. The electric furnace temperatures were set to 900°C for the reactor, 600°C for the reduction furnace, 70°C for the column, and 100°C for the detector. Oxygen gas was flowed at 0.2 mL / min as the combustion gas, and helium gas was flowed at 80 mL / min as the carrier gas. A calibration curve was created using aspartic acid (10.52%) with a known nitrogen content as the standard substance. The chloroprene rubber (A-2) obtained by the above production method had an acrylonitrile monomer unit content of 20.0 mass %.

[0104] <Production method of chloroprene rubber (A-1)> The amount of acrylonitrile monomer added in the polymerization step was changed to obtain a chloroprene-based rubber (A-1) having an acrylonitrile monomer unit content of 25.0 mass % in the chloroprene-based rubber.

[0105] (Examples 1 to 13, Comparative Examples 1 to 13) <Preparation of Rubber Composition> Among the components shown in Tables 1 to 4, the components excluding the organic peroxide, vulcanization accelerator, maleimide compound, and vulcanizing agent were mixed on an 8-inch open roll to obtain a rubber composition precursor not containing a vulcanizing agent, etc. (first mixing step). Subsequently, the obtained rubber composition precursor was allowed to stand at 23°C for 12 hours. Thereafter, the rubber composition precursor, the organic peroxide, the vulcanization accelerator, the maleimide compound, and the vulcanizing agent were kneaded on an 8-inch open roll (second mixing step) to obtain rubber compositions of the examples and comparative examples.

[0106] (Comparative Examples 14 and 15) <Preparation of Rubber Composition> Of the components shown in Table 4, the components excluding the organic peroxide, the acid acceptor, and the vulcanizing agent were mixed on an 8-inch open roll to obtain a rubber composition precursor not containing a vulcanizing agent, etc. (first mixing step). Next, without going through a leaving step, the rubber composition precursor, the vulcanization accelerator, the organic peroxide, the maleimide compound, and the vulcanizing agent were kneaded on an 8-inch open roll (second mixing step) to obtain a rubber composition of the comparative example.

[0107] The components used to obtain the composition are as follows: Rubber composition: Chloroprene rubber A-1: ​​Chloroprene-acrylonitrile copolymer AN (acrylonitrile monomer unit) content 25% by mass Chloroprene rubber A-2: Chloroprene-acrylonitrile copolymer AN (acrylonitrile monomer unit) content 20% by mass, Natural rubber: HB Chemical, SMR-CV60

[0108] Carbon black: Asahi #70, manufactured by Asahi Carbon Co., Ltd., HAF Organic peroxide: 1,4-bis[(t-butylperoxy)isopropyl]benzene, NOF Corporation, Perbutyl P-40 Vulcanization Accelerator: Trimethylthiourea, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., Noccela TMU Sulfur: Sulfur, Hosoi Chemical Industry Co., Ltd., fine sulfur 200 mesh Noccela TT: Tetramethylthiuram disulfide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., Noccela TT Noccela CZ: N-cyclohexyl-2-benzothiazolyl sulfenamide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., Noccela CZ Maleimide compound: m-phenylenedimaleimide, Ouchi Shinko Chemical Industry Co., Ltd., Valnoc PM Plasticizer: Ether ester compound, manufactured by ADEKA Corporation, Adeka Cizer RS-700 Vulcanizing agent: Zinc oxide, Sakai Chemical Industry Co., Ltd., Zinc oxide type 2 Acid acceptor: Magnesium oxide, Kyowa Chemical Industry Co., Ltd., Kyowamag 150 Anti-aging agents: Nocrac CD: 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, Ouchi Shinko Chemical Industry Co., Ltd., Nocrac CD Nocrac 6C: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., Nocrac 6C Processing aid: Stearic acid, New Japan Chemical Co., Ltd., Stearic acid 50S

[0109] <Preparation of Test Vulcanized Molded Body 1> The obtained rubber composition was press-vulcanized at 170°C for 20 minutes according to JIS K 6299:2012 to produce a sheet-like vulcanized molded product having a thickness of 2 mm (test vulcanized molded product 1). Note that the rubber compositions according to Comparative Examples 6 to 8 and 10 to 12 generated a large amount of heat and scorched during processing, so they could not be molded and the vulcanized molded product could not be evaluated.

[0110] (Hardness) The vulcanized molded test bodies 1 were stacked to a thickness of 6.0 mm or more to form a laminate. The hardness of the laminate was measured with a type A durometer according to JIS K 6253-3:2023. The thickness of the laminate was 6.0 to 7.0 mm.

[0111] (Water resistance (volume change rate after immersion in 70°C water for 144 hours)) A test piece measuring 25 mm in length and 20 mm in width was punched out from the above-mentioned vulcanized molded test article 1 to obtain a test piece. The obtained test piece was immersed in water at 70°C for 144 hours. The volume change rate ΔV was calculated based on JIS K 6258. The obtained volume change rate ΔV was evaluated according to the following criteria. A: Less than 3% B: 3% or more, less than 6% C: 6% or more, less than 9% D: 9% or more

[0112] (Alkaline resistance (volume change rate after immersion in 10% sodium hydroxide at 70°C for 144 hours)) A test piece measuring 25 mm in length and 20 mm in width was punched out from the above-mentioned vulcanized molded test article 1 to obtain a test piece. The obtained test piece was immersed in 10% sodium hydroxide at 70°C for 144 hours. The volume change rate ΔV was calculated based on JIS K 6258. The obtained volume change rate ΔV was evaluated according to the following criteria. A: Less than 4% B: 4% or more, less than 7% C: 7% or more, less than 10% D: 10% or more

[0113] (Fever) The rubber composition was press-vulcanized at 170°C for 20 minutes to obtain a cylindrical vulcanized molded body (test vulcanized molded body 2) with a diameter of 15 mm and a height of 25 mm. Based on JIS K 6265:2018, heat generation was evaluated by a constant strain flexometer test using a Goodrich Flexometer. The constant strain flexometer test is a test method for evaluating fatigue characteristics due to heat generation inside a test piece by applying a dynamic repeated load to a test piece such as vulcanized rubber. In detail, a static initial load is applied to the test piece under a constant temperature condition, and a sine vibration of a constant amplitude is further applied to measure the heat generation and creep amount of the test piece that change over time. The test method was based on JIS K 6265:2018 and was performed under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute, and heat generation (°C) was measured.

[0114] [Table 1]

[0115]

Table 2

[0116]

Table 3

[0117]

Table 4

Claims

1. A rubber composition comprising a rubber component, The vulcanized molded test pieces 1 of the rubber composition are stacked to a thickness of 6.0 mm or more to form a laminate, the hardness of which is measured with a type A durometer according to JIS K 6253-3:2023 and designated as X; The test vulcanized molded article 2 of the rubber composition is evaluated in a constant strain flexometer test based on JIS K 6265:2018 under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute, where the heat generation is defined as Y. The hardness X and the heat generation Y satisfy the following formula (1), The test vulcanized molded article 1 is a sheet-like vulcanized molded article having a thickness of 2 mm obtained by press-vulcanizing the rubber composition at 170° C. for 20 minutes in accordance with JIS K 6299:2012. The test vulcanized molded body 2 is a cylindrical vulcanized molded body having a diameter of 15 mm and a height of 25 mm, obtained by press-vulcanizing the rubber composition at 170° C. for 20 minutes. Rubber composition. 1.4X-Y>20.0 (1)

2. The rubber composition according to claim 1 , wherein the hardness X is 40 or more and 98 or less.

3. The rubber composition according to claim 1 or 2, wherein the rubber component contains a chloroprene-based polymer.

4. The rubber composition according to claim 3, wherein the chloroprene polymer contains 70 to 85 mass % of chloroprene monomer units relative to 100 mass % of the chloroprene polymer.

5. A vulcanized molded article of the rubber composition according to claim 1 or 2.

6. A rubber roll, The present invention comprises a core bar and a surface layer provided on a peripheral surface of the core bar, The surface layer comprises the vulcanized molded article according to claim 5, The rubber roll is used in at least one of an acid washing line and an alkali washing line.

7. A vulcanized molded article containing a rubber component, When the vulcanized molded article is a test vulcanized molded article 1' having a thickness of 6.0 mm or more, the hardness measured with a type A durometer based on JIS K 6253-3:2023 is defined as X', When the vulcanized molded body is made into a cylindrical test vulcanized molded body 2' having a diameter of 15 mm and a height of 25 mm, the heat generation determined by evaluation in a constant strain flexometer test based on JIS K 6265:2018 under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute is defined as Y'. A vulcanized molded product, in which hardness X' and heat generation Y' satisfy the following formula (2). 1.4X'-Y'>20.0 (2)

Citation Information

Patent Citations

  • Sulfur modified chloroprene rubber composition

    JP1999209522A

  • Copolymer of chloroprene monomer and unsaturated nitrile compound, composition containing copolymer, vulcanization molded body of composition, and use of vulcanization molded body

    WO2020044899A1