Polyethylene-based sealant film and laminate
A multi-layer polyethylene sealant film with optimized layer densities and thicknesses addresses the challenge of reducing volume while maintaining performance, enhancing elastic modulus and tear resistance, and supporting environmental sustainability.
Patent Information
- Application Number
- JP2023053599
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing polyethylene sealant films face challenges in reducing volume while maintaining elastic modulus, low-temperature sealing performance, and bag tear resistance when using high-density resins.
A polyethylene sealant film composed of three or more layers, with specific layer densities and thickness ratios, including a laminate layer, base layer, and sealant layer, optimized to maintain performance and reduce volume.
The film achieves reduced volume with improved elastic modulus, low-temperature sealing, and bag tear resistance, contributing to environmental sustainability by using high-density resins effectively.
Smart Images

Figure 2024141774000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyethylene sealant film and a laminate using said sealant film. [Background technology]
[0002] In recent years, with the promotion of the Sustainable Development Goals (SDGs), various efforts have been made to reduce the environmental burden, such as by using renewable energy to reduce emissions of greenhouse gases such as carbon dioxide. In the field of resin films, for example, progress has been made in the production of films using plant-derived raw materials (biomass raw materials) instead of petroleum-derived raw materials (see, for example, Patent Document 1).
[0003] Plant-derived raw materials are considered to be carbon-neutral resources because they absorb carbon dioxide from the atmosphere during the plant growth process, and therefore do not increase new carbon dioxide into the atmosphere even if carbon dioxide is released by combustion. Therefore, compared to petroleum-derived raw materials, which increase carbon dioxide in the atmosphere when burned, plant-derived raw materials are effective as resources that can contribute to reducing environmental impact.
[0004] SDGs initiatives in the field of resin films are required to go beyond the use of biomass raw materials and contribute to reducing environmental impact from various angles. One method is to reduce the volume of films. When reducing the volume of a film, for example in the case of polyethylene sealant film, the film's rigidity and elastic modulus decrease as the volume is reduced, so it is possible to prevent the physical properties of the film from decreasing by using a high-density resin.
[0005] However, simply using a high-density resin causes problems such as a high heat-sealing temperature and a low bag-breaking strength when the film is made. Therefore, in a polyethylene sealant film, it is required to reduce the volume of the film while suppressing a decrease in the elastic modulus and also to suppress an increase in the heat-sealing temperature and a decrease in the bag-breaking strength. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2021-171969 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been proposed in consideration of the above-mentioned circumstances, and provides a polyethylene-based sealant film and laminate that can improve the elastic modulus by using a high-density resin material to reduce the volume of the film while avoiding deterioration of low-temperature sealing properties and bag-breakage resistance. [Means for solving the problem]
[0008] That is, the first invention is a film body mainly made of polyethylene resin, which is composed of three or more layers of at least a laminate layer, a base layer, and a sealant layer, and which is laminated in this order, and the layer density (D1) of the laminate layer is 0.919 g / cm 3 The layer density (D2) of the base layer is 0.935 g / cm 3 The layer density (D3) of the sealant layer is 0.924 g / cm 3 The layer density of each layer satisfies the relationship (D3) < (D1) ≦ (D2), and the overall density (D A ) is 0.930~0.935g / cm 3 and the thickness of the sealant layer is 15% or more of the entire layer thickness.
[0009] The second invention relates to a polyethylene sealant film of the first invention, in which the sum of the elastic modulus in the machine direction (MD) and the elastic modulus in the transverse direction (TD) (MD+TD) of the film body is 0.66 GPa or more, as measured based on a test method for plastic tensile properties conforming to JIS K 7127 (1999).
[0010] The third invention relates to a laminate obtained by laminating a biaxially stretched surface substrate having at least one layer structure to the surface layer of the laminate layer of the polyethylene sealant film described in the first or second invention.
[0011] A fourth invention relates to the laminate according to the third invention, wherein the surface substrate is at least one selected from the group consisting of a biaxially oriented polypropylene film, a biaxially oriented polyethylene film, a biaxially oriented polyethylene terephthalate film, and a biaxially oriented polyamide film. Effect of the Invention
[0012] The polyethylene sealant film according to the first aspect of the present invention is a film body mainly made of polyethylene resin, which is composed of three or more layers, namely, at least a laminate layer, a base layer, and a sealant layer, and in which the laminate layer, the base layer, and the sealant layer are laminated in this order. The film body has a layer density (D1) of the laminate layer of 0.919 g / cm. 3 The layer density (D2) of the base layer is 0.935 g / cm 3 The layer density (D3) of the sealant layer is 0.924 g / cm 3 The layer density of each layer satisfies the relationship (D3) < (D1) ≦ (D2), and the overall density (D A ) is 0.930~0.935g / cm 3 Furthermore, since the thickness of the sealant layer is 15% or more of the total layer thickness, the elastic modulus can be improved while appropriately avoiding deterioration of low-temperature sealability and bag rupture resistance, while maintaining the performance as a sealant film, and the volume of the film can be reduced, thereby contributing to reducing the environmental load.
[0013] According to the polyethylene sealant film of the second invention, in the first invention, the sum of the elastic modulus in the machine direction (MD) and the elastic modulus in the transverse direction (TD) (MD+TD) measured based on the test method for plastic tensile properties conforming to JIS K 7127 (1999) of the film body is 0.66 GPa or more, so that the volume of the film can be appropriately reduced.
[0014] According to the laminate of the third invention, a biaxially oriented surface substrate having at least one layer structure is laminated to the surface layer of the laminate layer of the polyethylene sealant film described in the first or second invention, so that a laminate using a sealant film can be provided that can contribute to reducing the environmental load by reducing the volume through improved elastic modulus while appropriately avoiding deterioration of low-temperature sealability and bag-breakage resistance.
[0015] According to the laminate of the fourth invention, in the third invention, the surface substrate is made of one or more of a biaxially oriented polypropylene film, a biaxially oriented polyethylene film, a biaxially oriented polyethylene terephthalate film, and a biaxially oriented polyamide film, and therefore the laminate is inexpensive, has excellent processability and strength, and is suitable for protecting a sealant film. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic cross-sectional view of a laminate using a polyethylene sealant film according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of a bag rupture test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] 1, a polyethylene sealant film 10 according to one embodiment of the present invention is a film body mainly made of polyethylene resin, which is composed of three or more layers, at least a laminate layer 20, a base layer 30, and a sealant layer 40, and which is formed by laminating the laminate layer 20, the base layer 30, and the sealant layer 40 in this order. In the sealant film 10, a surface substrate 60 is laminated on the surface layer of the laminate layer 20 to form a laminate 50.
[0018] The sealant film 10 is manufactured by a known film manufacturing method such as the T-die method. In addition, the sealant film 10 is formed into a laminate 50, and is therefore suitable for use in various packaging materials (packaging bags) for foods, cosmetics, medicines, daily necessities, parts, and other products, as well as in film products for industrial use, etc.
[0019] The polyethylene resin used in the sealant film 10 is selected from linear low density polyethylene resin (LLDPE), high density polyethylene (HDPE), low density polyethylene (LDPE), etc., either alone or in appropriate combination. Each layer of the sealant film may contain other resins. For example, other resins such as masterbatches for additives may be contained within the range that does not impair the properties of the film.
[0020] From the viewpoint of reducing the environmental load, the polyethylene resin may contain polyolefin resin derived from recycled materials such as material recycling and chemical recycling, or biomass. Examples of biomass-derived polyolefin resins include polyethylene-based resins obtained by processing plant materials. Specifically, the polyethylene-based resins are produced by a known resinification process after ethanol is produced from sugar liquid extracted from plant materials such as sugarcane through alcohol fermentation by yeast, and the ethanol is converted into ethylene. The higher the weight ratio of the biomass-derived polyolefin resin, the greater the contribution to reducing the environmental load.
[0021] In each layer, additives such as lubricants, antistatic agents, antiblocking agents, crystal nucleating agents, heat stabilizers, antioxidants, light stabilizers, ultraviolet absorbers, colorants, etc. may be added as needed within the range that does not impair the properties of the film of the present invention. The type of additive is appropriate depending on the application, and for example, low-density polyethylene may be added as a crystal nucleating agent.
[0022] The laminate layer 20 corresponds to one surface layer of the sealant film 10, and is the surface on which the surface substrate 60 described below is laminated. The laminate layer 20 is made of a material appropriately selected from available resin materials, and has a layer density (D1) of 0.919 g / cm 3 The above is satisfied. A resin mainly made of linear low-density polyethylene or a resin mainly made of a combination of linear low-density polyethylene and high-density polyethylene is preferably selected as the resin used for the laminate layer 20. The laminate layer 20 may be subjected to a surface treatment such as a corona treatment, a flame treatment, or a plasma treatment in order to improve the adhesion to the surface substrate 60.
[0023] The base layer 30 corresponds to an intermediate layer of the sealant film 10. The base layer 30 is made of a material appropriately selected from available resin materials and has a layer density (D2) of 0.935 g / cm 3 The resin used for the base layer 30 is preferably selected from resins mainly made of linear low density polyethylene or a combination of linear low density polyethylene and high density polyethylene.
[0024] The sealant layer 40 corresponds to the surface layer on the other side of the sealant film 10, and is the inner side of the bag when used as a packaging material (packaging bag), and is the surface (sealing surface) to be bonded to other films, etc. The sealant layer 40 is made of a material appropriately selected from available resin materials, and has a layer density (D3) of 0.924 g / cm 3 The composition is adjusted so as to satisfy the following: As the resin used for the sealant layer 40, a resin mainly containing linear low density polyethylene is preferably selected.
[0025] In the sealant film 10 of the present invention, in order to reduce the volume, while improving the elastic modulus of the film and avoiding deterioration of low-temperature sealability and bag-breaking resistance, extensive research was conducted focusing on the layer density and layer thickness of the sealant layer, and it was found that the volume of the film can be reduced while maintaining good heat seal temperature and bag-breaking strength performance from the relationship between the layer densities of the sealant layer and other layers and the density and layer thickness of the entire film. That is, the sealant film 10 has layer densities (D1), (D2), and (D3) of the layers 20, 30, and 40 satisfy the relationship (D3)<(D1)≦(D2), and the overall density (D A ) is 0.930~0.935g / cm 3 and the thickness of the sealant layer 40 is adjusted to be 15% or more of the thickness of the entire film.
[0026] The layer density (D1) of the laminate layer 20 and the layer density (D2) of the base layer 30 contribute to the rupture resistance and rigidity of the sealant film 10. 3 The layer density (D2) of the base layer 30 is 0.935 g / cm 3 In order to further increase the rigidity of the film, the layer density (D1) of the laminate layer 20 is preferably 0.924 g / cm. 3 More preferably, 0.931 g / cm 3 The preferred layer density (D2) of the base layer 30 is 0.940 g / cm 3 The layer density (D1) of the laminate layer 20 and the layer density (D2) of the base layer 30 are not particularly limited to upper limits, but from the viewpoint of improving the bag rupture resistance, the upper limits of the layer densities (D1) and (D2) are each 0.955 g / cm 3 is preferred, and 0.950 g / cm 3 is more preferred.
[0027] The layer density (D3) of the sealant layer 40 contributes to the low-temperature sealing property of the sealant film 10. By adjusting the layer density (D3) of the sealant layer 40, which becomes the sealing surface of the film, to a relatively small value, the increase in the heat sealing temperature, etc. is suppressed. The layer density (D3) of the sealant layer 40 is 0.924 g / cm 3 When the viscosity is less than or equal to 0.919 g / cm, good low-temperature sealability can be obtained. From the viewpoint of further improving the low-temperature sealability, 3 The layer density (D3) of the sealant layer is not particularly limited to a lower limit, but from the viewpoint of improving the rigidity of the film, the lower limit of the layer density (D3) is preferably 0.890 g / cm. 3 is preferred, and 0.904 g / cm 3 is more preferred.
[0028] A sealant film having excellent elastic modulus, good low-temperature sealability and bag-breaking resistance can be obtained by having the layer density (D3) of the sealant layer 40 satisfy the relationship (D3)<(D1)≦(D2) between the layer density (D1) of the laminate layer 20 and the layer density (D2) of the base layer 30. If the relationship (D3)<(D1)≦(D2) is not satisfied, there is a risk that any one of the elastic modulus, low-temperature sealability and bag-breaking resistance will be insufficient.
[0029] In the sealant film 10, the relationship between the density of each layer is satisfied while the overall density (D A ) is 0.930~0.935g / cm 3 The overall density of the sealant film 10 (D A ) contributes to the performance of bag rupture resistance, rigidity, elastic modulus, etc. If it is too small, there is a risk that the elastic modulus will decrease and the rigidity of the film will be insufficient, and if it is too large, there is a risk that the bag rupture resistance will decrease. A ) at 0.930~0.935g / cm 3 By adjusting the ratio of the film thickness to the thickness of the film, it is possible to obtain a sealant film that has an excellent elastic modulus, a good balance between the film rigidity and the bag rupture resistance, and allows the volume to be reduced.
[0030] In the sealant film 10, the preferred elastic modulus is the sum of the elastic modulus in the machine direction (MD) and the elastic modulus in the transverse direction (TD) (MD+TD) of 0.66 GPa or more, and more preferably 0.31 (GPa) or more in the machine direction (MD) and 0.34 (GPa) or more in the transverse direction (TD). The elastic modulus is measured based on the test method for tensile properties of plastics in accordance with JIS K 7127 (1999). If the elastic modulus of the sealant film 10 is insufficient, there is a risk that the volume of the film cannot be appropriately reduced.
[0031] The layer thickness (layer ratio) of the sealant layer 40 relative to the total layer thickness of the sealant film 10 contributes to the elastic modulus and bag rupture resistance of the film. If the layer ratio of the sealant layer 40 is too small, the sealant layer 40 will be too thin relative to the entire film, and bag rupture resistance may deteriorate. By setting the layer ratio of the sealant layer 40 to 15% or more, preferably 20% or more, and more preferably 25% or more, it is possible to achieve both the elastic modulus and bag rupture resistance of the film. In addition, although there is no particular upper limit for the layer ratio of the sealant layer 40, if the layer ratio of the sealant layer 40 is large, the density of the entire film will decrease, decreasing the elastic modulus. Therefore, from the viewpoint of increasing the elastic modulus of the film, it is preferably 40% or less, more preferably 35% or less.
[0032] In this way, the sealant film 10 of the present invention can appropriately avoid deterioration of low-temperature sealability and bag-breaking resistance while taking advantage of the improved elastic modulus caused by the use of a high-density resin by adjusting the density of the entire film within an appropriate range where a specific relationship between the layer densities of the layers 20, 30, and 40 is established, and further controlling the layer ratio of the sealant layer 40 corresponding to the sealing surface. Therefore, the sealant film 10 of the present invention can reduce the volume by improving the elastic modulus while maintaining the performance as a sealant film, and can contribute to reducing the environmental load.
[0033] The laminate 50 using the sealant film 10 of the present invention is formed by laminating a surface substrate 60 onto the surface layer of the laminate layer 20 of the sealant film 10. The method for laminating the surface substrate 60 onto the sealant film 10 may be a known method such as a dry lamination method or a melt extrusion lamination method.
[0034] The front substrate 60 is a biaxially stretched film having at least one layer. The front substrate 60 protects the sealant film 10 on the lower layer side, and corresponds to the exterior surface when the laminate 50 is used as a packaging material, for example. In addition to being subjected to printing and the like, the front substrate 60 is given various functions according to the application, such as durability, weather resistance, light resistance, etc., by adding appropriate additives.
[0035] At least one of a biaxially oriented polypropylene film, a biaxially oriented polyethylene film, a biaxially oriented polyethylene terephthalate film, and a biaxially oriented polyamide film is preferably selected for the front substrate 60. These films are inexpensive and have excellent processability and strength, and therefore are suitable for protecting the sealant film 10. EXAMPLES
[0036] [Preparation of sealant film] In producing the sealant films of prototypes 1 to 20, the materials described below were fed to an extrusion device, melted and kneaded, and extruded by the T-die method into three layers: a laminate layer, a base layer, and a sealant layer. At that time, the overall thickness of the film (total thickness) and the layer thickness (layer ratio) relative to the total thickness of each layer were adjusted. After film formation, the laminate layer was subjected to a surface treatment by corona discharge treatment. In prototypes 1 to 20, the resin blending ratio of each layer was 100% by weight. Additives such as antiblocking agents were omitted.
[0037] [Materials used] The following resins were used as the resin materials for the laminate layer, base layer, and sealant layer. For prototypes 1 to 20, the density of each layer of the laminate layer, base layer, and sealant layer and the overall density (g / cm3 The density (ρ blend ) and ρ X is the density of the raw material X, ρ Y is the density of the raw material Y, ρ Z is the density of raw material Z, x is the blending ratio of raw material X, y is the blending ratio of raw material Y, and z is the blending ratio of raw material Z.
[0038]
number
[0039] Resin A1: Linear low-density polyethylene (FX307, manufactured by Sumitomo Chemical Co., Ltd.), density 0.890 g / cm 3 Resin A2: Linear low-density polyethylene (Ube Maruzen Polyethylene Co., Ltd.; 0540F), density 0.904 g / cm 3 Resin A3: Linear low-density polyethylene (Ube Maruzen Polyethylene Co., Ltd.; 1540FC), density 0.913 g / cm 3 Resin A4: Linear low-density polyethylene (2040FC, manufactured by Ube Maruzen Polyethylene Co., Ltd.), density 0.919 g / cm 3 Resin A5: Linear low-density polyethylene (Prime Polymer Co., Ltd.; SP2540), density 0.924 g / cm 3 Resin A6: Linear low-density polyethylene (Ube Maruzen Polyethylene Co., Ltd.; 3570FC), density 0.931 g / cm 3 Resin A7: Linear low-density polyethylene (4040F, manufactured by Ube Maruzen Polyethylene Co., Ltd.), density 0.937 g / cm 3 Resin A8: Linear low-density polyethylene (4540F, manufactured by Ube Maruzen Polyethylene Co., Ltd.), density 0.944 g / cm 3
[0040] Resin B1: High density polyethylene (Japan Polyethylene Corporation; HF562), density 0.963g / cm 3
[0041] Resin C1: Low-density polyethylene (Ube Maruzen Polyethylene Co., Ltd.; R300), density 0.920 g / cm 3 Resin C2: Low-density polyethylene (Ube Maruzen Polyethylene Co., Ltd.; F222NH), density 0.922 g / cm 3
[0042] [Prototype 1] The sealant film of prototype 1 was produced by blending 100.0% by weight of resin A6 in the laminate layer, 69.0% by weight of resin A6 and 31.0% by weight of resin B1 in the base layer, and 100.0% by weight of resin A4 in the sealant layer. In prototype 1, the total thickness was 50 μm, the layer ratio of the laminate layer was 16.0%, the layer ratio of the base layer was 59.0%, and the layer ratio of the sealant layer was 25.0%. The total density was 0.934 g / cm 3 , the layer density of the laminate layer is 0.931g / cm 3 , the layer density of the base layer is 0.941g / cm 3 , the layer density of the sealant layer is 0.919 g / cm 3 It was.
[0043] [Prototype 2] The sealant film of Prototype Example 2 was the same as the sealant film of Prototype Example 1, except that the layer ratio of the base layer was 54.0% and the layer ratio of the sealant layer was 30.0%. In Prototype Example 2, the overall density was 0.933 g / cm 3 It was.
[0044] [Prototype 3] The sealant film of Prototype Example 3 was the same as the sealant film of Prototype Example 1, except that the sealant layer was formed by blending Resin A3 at 100.0% by weight. In Prototype Example 3, the overall density was 0.932 g / cm 3 , the layer density of the sealant layer is 0.913 g / cm 3 It was.
[0045] [Prototype 4] The sealant film of Prototype Example 4 was the same as the sealant film of Prototype Example 1, except that the sealant layer was formed by blending Resin A2 at 100.0 wt %. In Prototype Example 4, the overall density was 0.930 g / cm 3 , the layer density of the sealant layer is 0.904g / cm 3 It was.
[0046] [Prototype 5] The sealant film of prototype 5 was produced by mixing 86.0% by weight of resin A6 and 14.0% by weight of resin B1 in the base layer, and was the same as the sealant film of prototype 1, except that the total thickness was 40 μm, the layer ratio of the base layer was 68.0%, and the layer ratio of the sealant layer was 16.0%. In prototype 5, the total density was 0.932 g / cm 3 , the layer density of the base layer is 0.935g / cm 3 , the layer density of the sealant layer is 0.919 g / cm 3 It was.
[0047] [Prototype 6] The sealant film of Sample 6 was the same as the sealant film of Sample 5, except that the layer ratio of the base layer was 64.0% and the layer ratio of the sealant layer was 20.0%. In Sample 6, the overall density was 0.931 g / cm 3 It was.
[0048] [Prototype 7] The sealant film of prototype 7 was produced by mixing 93.0% by weight of resin A7 and 7.0% by weight of resin C1 in the laminate layer, 93.0% by weight of resin A7 and 7.0% by weight of resin C1 in the base layer, and 100.0% by weight of resin A4 in the sealant layer. In prototype 7, the total thickness was 50 μm, the layer ratio of the laminate layer was 12.5%, the layer ratio of the base layer was 62.5%, and the layer ratio of the sealant layer was 25.0%. The total density was 0.932 g / cm 3 , the layer density of the laminate layer is 0.936g / cm 3 , the layer density of the base layer is 0.936g / cm 3 , the layer density of the sealant layer is 0.919 g / cm 3 It was.
[0049] [Prototype 8] The sealant film of Prototype Example 8 was the same as the sealant film of Prototype Example 1, except that the sealant layer was formed by blending Resin A5 at 100.0 wt%. In Prototype Example 8, the overall density was 0.935 g / cm 3 , the layer density of the sealant layer is 0.924g / cm 3 It was.
[0050] [Prototype 9] The sealant film of prototype 9 was produced by mixing 85.0% by weight of resin A6 and 15.0% by weight of resin B1 in the laminate layer, 85.0% by weight of resin A6 and 15.0% by weight of resin B1 in the base layer, and 100.0% by weight of resin A4 in the sealant layer. In prototype 9, the total thickness was 50 μm, the layer ratio of the laminate layer was 16.0%, the layer ratio of the base layer was 59.0%, and the layer ratio of the sealant layer was 25.0%. The total density was 0.931 g / cm 3 , the layer density of the laminate layer is 0.936g / cm 3 , the layer density of the base layer is 0.936g / cm 3 , the layer density of the sealant layer is 0.919 g / cm 3 It was.
[0051] [Prototype 10] The sealant film of prototype 10 was produced by blending 100.0% by weight of resin A6 in the laminate layer, 100.0% by weight of resin A8 in the base layer, and 100.0% by weight of resin A1 in the sealant layer. In prototype 10, the total thickness was 50 μm, the layer ratio of the laminate layer was 16.0%, the layer ratio of the base layer was 64.0%, and the layer ratio of the sealant layer was 20.0%. The total density was 0.931 g / cm 3 , the layer density of the laminate layer is 0.931g / cm 3 , the layer density of the base layer is 0.944g / cm 3 , the layer density of the sealant layer is 0.890g / cm 3 It was.
[0052] [Prototype example 11] The sealant film of Prototype Example 11 was the same as the sealant film of Prototype Example 1, except that the layer ratio of the base layer was 71.5% and the layer ratio of the sealant layer was 12.5%. In Prototype Example 11, the overall density was 0.936 g / cm 3 It was.
[0053] [Prototype 12] The sealant film of Prototype Example 12 was the same as the sealant film of Prototype Example 1, except that the layer ratio of the base layer was 74.0% and the layer ratio of the sealant layer was 10.0%. In Prototype Example 12, the overall density was 0.937 g / cm 3 It was.
[0054] [Prototype 13] The sealant film of Prototype Example 13 was the same as the sealant film of Prototype Example 1, except that the sealant layer was formed by blending Resin A1 at 100.0 wt %. In Prototype Example 13, the overall density was 0.926 g / cm 3 , the layer density of the sealant layer is 0.890g / cm 3 It was.
[0055] [Prototype 14] The sealant film of prototype 14 was produced by mixing 100.0% by weight of resin A4 in the laminate layer, base layer, and sealant layer. In prototype 14, the total thickness was 50 μm, the layer ratio of the laminate layer was 12.5%, the layer ratio of the base layer was 75.0%, and the layer ratio of the sealant layer was 12.5%. The total density and the layer density of each layer were both 0.919 g / cm. 3 It was.
[0056] [Prototype 15] The sealant film of Prototype Example 15 was the same as the sealant film of Prototype Example 14, except that the laminate layer, the base material layer, and the sealant layer were each formed with 100.0% by weight of Resin A6. In Prototype Example 15, the overall density and the layer density of each layer were both 0.931 g / cm 3 It was.
[0057] [Prototype 16] The sealant film of prototype 16 was produced by blending 100.0% by weight of resin A6 in the laminate layer, 95.6% by weight of resin A6 and 4.4% by weight of resin C2 in the base layer, and 100.0% by weight of resin A4 in the sealant layer. In prototype 16, the total thickness was 50 μm, the layer ratio of the laminate layer was 16.0%, the layer ratio of the base layer was 72.0%, and the layer ratio of the sealant layer was 12.0%. The total density was 0.929 g / cm 3 , the layer density of the laminate layer is 0.931g / cm 3 , the layer density of the base layer is 0.931g / cm 3 , the layer density of the sealant layer is 0.919 g / cm 3 It was.
[0058] [Prototype 17] The sealant film of Prototype Example 17 was the same as that of Prototype Example 14, except that the laminate layer, the base material layer, and the sealant layer were each formed by blending 93.0% by weight of Resin A7 and 7.0% by weight of Resin C1. In Prototype Example 17, the overall density and the layer density of each layer were both 0.936 g / cm 3 It was.
[0059] [Prototype 18] The sealant film of Prototype Example 18 was the same as the sealant film of Prototype Example 17, except that the sealant layer was made by blending Resin A4 at 100.0 wt%. In Prototype Example 18, the overall density was 0.934 g / cm 3 , the layer density of the sealant layer is 0.919 g / cm 3 It was.
[0060] [Prototype Example 19] The sealant film of Prototype Example 19 was the same as the sealant film of Prototype Example 16, except that the base layer was made of 100.0% by weight of Resin A5 and the sealant layer was made of 100.0% by weight of Resin A5. In Prototype Example 19, the overall density was 0.925 g / cm 3 , the layer density of the base layer is 0.924g / cm 3 , the layer density of the sealant layer is 0.924g / cm 3 It was.
[0061] [Prototype Example 20] The sealant film of prototype 20 was produced by blending 100.0% by weight of resin A6 in the laminate layer, 85.0% by weight of resin A6 and 15.0% by weight of resin B1 in the base layer, and 100.0% by weight of resin A6 in the sealant layer. In prototype 20, the total thickness was 50 μm, the layer ratio of the laminate layer was 16.0%, the layer ratio of the base layer was 59.0%, and the layer ratio of the sealant layer was 25.0%. The total density was 0.934 g / cm 3 , the layer density of the laminate layer is 0.931g / cm 3 , the layer density of the base layer is 0.936g / cm 3 , the layer density of the sealant layer is 0.931 g / cm 3 It was.
[0062] For the sealant films of prototypes 1 to 20, the blending ratio of the resin material of each layer is shown in Tables 1 to 4. In addition, the overall density (g / cm 3 ) and total layer thickness (μm), layer density D1 of the laminate layer (g / cm 3 ) and layer ratio (%), layer density D2 of the base layer (g / cm 3 ) and layer ratio (%), layer density D3 of the sealant layer (g / cm 3 ), layer ratio (%), and comparison of the magnitude relationship of the layer density of each layer (layer density comparison) are shown in Tables 5 to 8 described later.
[0063] [Table 1]
[0064] [Table 2]
[0065] [Table 3]
[0066] [Table 4]
[0067] The tensile modulus and heat seal initiation temperature (low-temperature sealability) were measured to evaluate the performance of the sealant films of Prototype Examples 1 to 20. The measurement results are shown in Tables 5 to 8 below.
[0068] [Measurement of tensile modulus] Tensile modulus (GPa) is one of the indicators of processability. For this measurement, a tensile tester (ORIENTEC Co., Ltd., RTF-1310) was used to measure the longitudinal (MD) and transverse (TD) directions based on the test method for plastic tensile properties conforming to JIS K 7127 (1999). In the measurement results, a product was deemed good if the sum of the longitudinal and transverse moduli (MD+TD) was 0.66 or more, and a product was deemed best if the longitudinal (MD) direction was 0.31 (GPa) or more, the transverse (TD) direction was 0.34 (GPa) or more, and the sum of the longitudinal and transverse directions (MD+TD) was 0.66 or more.
[0069] [Measurement of heat seal initiation temperature] The heat seal initiation temperature (℃) is one of the indicators of processing suitability. In this measurement, the heat seal initiation temperature test conforming to JIS Z 1713 (2009) was used as a reference. First, the films of prototypes 1 to 20 were cut into a rectangle of 50 mm in the transverse (TD) direction and 250 mm in the longitudinal (MD) direction to prepare test pieces. The sealant layers of two test pieces were overlapped and heat sealed with a heat seal tester (manufactured by Toyo Seiki Seisakusho Co., Ltd.; "Thermal Gradient Tester") at a heat seal pressure of 0.4 MPa, heat seal time of 1 second, and temperature gradient (temperature rise) of 5℃ each. During heat sealing, a cellophane film for preventing fusion was sandwiched between the hot plate of the heat sealer and the test piece. After heat sealing, the fused test piece was opened to 180°, and the unsealed part of the test piece was clamped in a zipper using a small tabletop tester (manufactured by Shimadzu Corporation; "EZ-SX") to perform T-shaped peeling of the sealed part. The temperature at which the heat seal strength reached 3 (N / 15 mm) was taken as the heat seal initiation temperature, which was calculated by interpolation. From the measurement results, products were judged to be good when they were 120°C or lower.
[0070] Next, laminate films were produced based on the sealant films of prototypes 1 to 20, and the laminate films were subjected to a bag-breaking test to determine whether the laminate films had good or bad bag-breaking resistance. The test results are shown in Tables 5 to 8 below.
[0071] [Preparation of laminate film] A 15 μm-thick biaxially oriented nylon film ("Santonir SNR" manufactured by Mitsubishi Chemical Corporation) was used as the front substrate to be laminated to the sealant films of prototypes 1 to 20. An adhesive prepared for dry lamination (manufactured by Toyo-Morton Co., Ltd., base agent: TM-329, hardener: CAT-8B, solvent: ethyl acetate) was applied at a rate of approximately 3 g / m2 to the film surface of this front substrate. 2 After coating, the adhesive was dried once. Thereafter, the surface substrate was attached to the surface of the laminate layer of the sealant film of each of the prototypes 1 to 20, and the sealant film and the surface substrate were adhered to each other by sequentially passing a roller through the surface substrate to produce a laminate film.
[0072] [Bag Breaking Test] A bag measuring 130 mm x 180 mm was prepared by heat sealing three sides so that the sealant film side (sealant layer) of the laminate film was the inner side of the bag. An impulse sealer (manufactured by Fuji Impulse Co., Ltd.; "OPL-350-MD NP") was used for heat sealing, and the heat sealing conditions were a sealing temperature of 160°C, a heating time of 1.0 seconds, and a cooling temperature of 60°C. After pouring 200 mL of tap water into the prepared bag, the unsealed opening was heat sealed under the same conditions to seal it, and a sample bag was prepared. The prepared sample bag was stored in water at 0°C in a refrigerator for 24 hours. The number of sample bags corresponding to each prototype 1 to 20 was five for each sample bag.
[0073] In the bag-breaking test, a bag-breaking test apparatus 100 shown in Fig. 2 was used, and a sample bag S stored in a refrigerator was placed on the placement section 101 of the bag-breaking test apparatus 100, and an iron plate section 102 weighing 3 kg was tilted from the 90° position shown in the figure toward the sample bag S on the placement section 101 via a rotating section 103 to apply an impact to the sample bag S. This operation was counted as one operation, and the operation was repeated up to 50 times, and the number of sample bags for which breakage was confirmed before the operation reached 50 times (number of broken bags) was calculated. In this bag-breaking test, the operation was repeated 50 times with five sample bags in each of the prototypes 1 to 20, and a product was deemed to be good if no breakage was confirmed even once.
[0074] [Table 5]
[0075] [Table 6]
[0076] [Table 7]
[0077] [Table 8]
[0078] [Results and Discussion] As shown in Tables 5 to 8, prototypes 1 to 10 are pass products judged to be good in terms of elastic modulus, sealing start temperature (low-temperature sealability), and number of broken bags (bag-breakage resistance), while prototypes 11 to 20 are fail products judged to be poor (unacceptable) in terms of at least one of elastic modulus, sealing start temperature (low-temperature sealability), and number of broken bags (bag-breakage resistance).
[0079] First, compared to prototype 1, prototypes 2, 11, and 12 are examples in which the layer ratio of the sealant layer was changed. In prototype 2, the layer ratio of the sealant layer was increased compared to prototype 1, and although the elastic modulus was slightly reduced, all of the elastic modulus, low-temperature sealability, and bag-breaking resistance were good. On the other hand, prototypes 11 and 12 are examples in which the layer ratio of the sealant layer was decreased compared to prototype 1, and a decrease in bag-breaking resistance was observed. In particular, as can be seen from the comparison between prototypes 11 and 12, the smaller the layer ratio, the worse the bag-breaking resistance tended to become. In addition, prototypes 1, 2, 11, and 12 showed a tendency for the elastic modulus to improve as the layer ratio became smaller. This is thought to be because the layer ratio of the relatively low-density sealant layer became smaller, which increased the density of the entire film and improved the elastic modulus.
[0080] In contrast to prototype 1, prototypes 3, 4, 8, and 13 are examples in which the overall density of the film was changed in conjunction with a change in the layer density of the sealant layer. From prototypes 3, 4, 8, and 13, it was observed that the smaller the layer density of the sealant layer, the lower the sealing start temperature (improved low-temperature sealability). In addition, it was observed that the smaller the layer density of the sealant layer, the lower the elastic modulus. This is thought to be because the overall density of the film became smaller as the layer density of the sealant layer was reduced, resulting in a decrease in the elastic modulus.
[0081] Samples 5, 6, and 16 are examples in which the resin composition of the base layer was changed, and the layer ratio of the base layer to the sealant layer was also changed. Comparing Sample 5 with Sample 6, an improvement in the modulus of elasticity was observed as the layer ratio decreased, as described above. Sample 16 has a lower overall density of the film as the density of the base layer is reduced compared to Samples 5 and 6, and the modulus of elasticity was reduced. Furthermore, the layer ratio of the sealant layer was also reduced in Sample 16, and a decrease in bag rupture resistance was observed.
[0082] Sample 7 is a good product in which the resin composition of the laminate layer and the base layer are the same, and Sample 18 is an example in which the layer ratio of the sealant layer is reduced compared to Sample 7. As mentioned above, there was a tendency for the bag rupture resistance to decrease as the layer ratio of the sealant layer decreased.
[0083] Sample 9 is a modified example in which the laminate layer and base layer have different resin compositions and layer ratios than those of Sample 7. Although Sample 9 has a slightly lower overall film density than Sample 7, it exhibits performance comparable to that of Sample 7.
[0084] Prototype 10 is an example in which each layer is made of 100% linear low-density polyethylene with different densities, so that the layer density of each layer is sealant layer (D3) < laminate layer (D1) < base layer (D2). Prototype 10 is excellent in elastic modulus, low-temperature sealability, and bag rupture resistance, and in particular, the layer density of the sealant layer is 0.890 g / cm 3 It is believed that this has enabled the sealing initiation temperature to be significantly reduced.
[0085] Samples 14, 15, and 17 are examples in which each layer is made of the same 100% linear low-density polyethylene. It is believed that Sample 14 was unable to secure sufficient elastic modulus due to the low overall density of the film. It is believed that Samples 15 and 17 had a high heat seal initiation temperature due to the high density of the sealant layer. It is also believed that Samples 15 and 17 had poor bag rupture resistance due to the high density of the sealant layer.
[0086] In prototype 19, the resin composition of the base layer is the same as that of the sealant layer, and the density is 0.924 g / cm 3 This is an example in which the first layer is made of 100% linear low density polyethylene, and the laminate layer is made of 100% linear low density polyethylene. In Prototype 19, the overall density of the film was small, and it is considered that a sufficient elastic modulus could not be secured.
[0087] In prototype 20, the resin composition of the sealant layer is the same as that of the laminate layer, and the density is 0.931 g / cm 3 This is an example in which the base layer is made of 100% linear low density polyethylene of the above, and the base layer is made of 100% linear low density polyethylene of the other. In Prototype 20, the high density of the sealant layer increases the heat seal initiation temperature and deteriorates the bag rupture resistance.
[0088] Considering the prototypes 1 to 20 comprehensively, the layer density (D1) of the laminate layer is 0.931 g / cm 3 Above, the density of the base layer (D2) is 0.935g / cm 3 The layer density of the sealant layer (D3) is 0.890 g / cm 3 The density of each layer satisfies the following: sealant layer (D3) < laminate layer (D1) < base layer (D2), and the overall density (D A ) is 0.930~0.935g / cm 3 At the same time, it is considered preferable that the layer ratio of the sealant layer is 15% or more. [Industrial Applicability]
[0089] As described above, the polyethylene sealant film of the present invention specifies the density of the entire film where the layer densities of the laminate layer, base layer, and sealant layer have a specific relationship, and controls the layer ratio of the sealant layer, thereby appropriately avoiding deterioration of low-temperature sealability and bag-breaking resistance, while maintaining the performance of the sealant film, and achieving volume reduction by improving the elastic modulus. Therefore, the polyethylene sealant film of the present invention and a laminate using this film can contribute to reducing the environmental load, and are promising as a replacement for conventional polyethylene sealant films and laminates. [Explanation of symbols]
[0090] 10 Polyethylene sealant film 20 Laminate Layer 30 base layer 40 Sealant Layer 50 Laminate 60 Table base material 100 Bag Breaking Testing Device 101 Placement part 102 Iron Plate Section 103 Rotating part S sample bag
Claims
1. A film body mainly made of a polyethylene resin, which comprises at least three or more layers, namely, a laminate layer, a base layer, and a sealant layer, and in which the laminate layer, the base layer, and the sealant layer are laminated in this order, The film body has a layer density (D 1 ) is 0.919 g / cm 3 The layer density (D 2 ) is 0.935 g / cm 3 The layer density (D 3 ) is 0.924 g / cm 3 The layer density of each layer is (D 3 ) < (D 1 ) ≦ (D 2 ) relationship, Overall density (D A ) is 0.930 to 0.935 g / cm 3 and the thickness of the sealant layer is 15% or more of the total layer thickness. A polyethylene sealant film characterized by:
2. The polyethylene sealant film according to claim 1, wherein the sum of the elastic modulus in the machine direction (MD) and the elastic modulus in the transverse direction (TD) (MD + TD) of the film body measured based on a test method for plastic tensile properties conforming to JIS K 7127 (1999) is 0.66 GPa or more.
3. A laminate obtained by laminating a biaxially stretched surface substrate having at least one layer structure on the surface layer of the laminate layer of the polyethylene sealant film according to claim 1 or 2.
4. 4. The laminate according to claim 3, wherein the surface substrate comprises at least one of a biaxially oriented polypropylene film, a biaxially oriented polyethylene film, a biaxially oriented polyethylene terephthalate film, and a biaxially oriented polyamide film.
Citation Information
Patent Citations
Polyethylene-based sealant film and laminate film
JP2021171969A