Method for producing carbon fiber precursor fiber bundle, method for producing carbon fiber bundle, and carbon fiber bundle

The method addresses the issue of low strength in lignin-based carbon fibers by using acidic water washing and filtration to remove impurities, resulting in high-strength carbon fibers with controlled impurity levels.

JP2024141922AInactive Publication Date: 2024-10-10MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023053802
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Carbon fibers produced using lignin as a precursor material face challenges in achieving high strength due to the presence of impurities such as sodium, potassium, and iron elements, which are not effectively removed by existing methods.

Method used

A method involving the use of acidic water washing and filtration steps to remove impurities, followed by mixing with an acrylonitrile copolymer and heating, utilizing solvents like N,N-dimethylacetamide, to produce a carbon fiber precursor fiber bundle with controlled lignin content and impurity levels.

Benefits of technology

The method results in a carbon fiber bundle with enhanced tensile strength and modulus, achieving 1.75 GPa or more tensile strength and 175 GPa or more tensile modulus, while reducing impurity contents like sulfur, sodium, potassium, and iron to specific low levels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141922000001
    Figure 2024141922000001
Patent Text Reader

Abstract

To provide a method for producing a carbon fiber precursor fiber bundle, which is a carbon fiber precursor fiber bundle containing lignin, and which can produce a carbon fiber bundle having a high tensile strength when made into a carbon fiber bundle.SOLUTION: There is provided a method for producing a carbon fiber precursor fiber bundle, which comprises discharging a spinning solution in which an acrylonitrile copolymer and lignin are dissolved in a solvent from a discharge hole, and which further comprises a removal step for removing impurities contained in the lignin. The method is preferably configured in that: the removal step is at least one of a washing step of washing the lignin with acidic water and a filtration step of filtering a solution in which the lignin is dissolved in a solvent through a filter; the filtering step is provided after the washing step; and a value of pH of the acidic water is 3 to 6.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a lignin-containing carbon fiber precursor fiber bundle, a method for producing a carbon fiber bundle, and a carbon fiber bundle. [Background technology]

[0002] Carbon fiber has excellent specific strength and specific elasticity, and its use as a reinforcing fiber in carbon fiber reinforced composite materials enables significant weight reductions in components. As such, it is used in a wide range of fields as one of the essential materials for realizing a society with high energy efficiency.

[0003] In recent years, its use has expanded in fields such as automobiles and electronic device housings, where there is a strong demand for cost reduction, and there is a strong demand for reduction in the cost of final components, including molding costs. There is also a strong demand for environmental considerations, such as recycling carbon fibers. Lignin is a material that converts petroleum-based raw materials into bio-based materials, contributing to carbon neutrality and is also low cost, so its use is desirable. Patent Document 1 describes a method in which lignin and polyacrylonitrile or polyacrylonitrile copolymer are dissolved in a solvent and used as a spinning raw material to obtain precursor fibers by a solution spinning method, which are then oxidized and carbonized to obtain carbon fibers. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2012 / 013070 Summary of the Invention [Problem to be solved by the invention]

[0005] However, there is a problem that the carbon fiber obtained by heating the carbon fiber precursor fiber containing lignin does not have high strength. An object of the present invention is to provide a method for producing a carbon fiber precursor fiber bundle, which can provide a carbon fiber bundle with high tensile strength even if the carbon fiber precursor fiber bundle contains lignin, a method for producing a carbon fiber bundle, and a carbon fiber bundle. [Means for solving the problem]

[0006] [1] A method for producing a carbon fiber precursor fiber bundle, comprising discharging a spinning dope in which an acrylonitrile copolymer and lignin are dissolved in a solvent from a discharge hole, and including a removal step for removing impurities contained in the lignin. [2] The method for producing a carbon fiber precursor fiber bundle according to [1], wherein the removal step is at least one of a washing step of washing the lignin with acidic water and a filtration step of filtering a solution in which the lignin is dissolved in a solvent through a filter. [3] The method for producing a carbon fiber precursor fiber bundle according to [2], further comprising the filtration step after the washing step. [4] The method for producing a carbon fiber precursor fiber bundle according to [2] or [3], wherein the acidic water has a pH of 3 to 6. [5] The method for producing a carbon fiber precursor fiber bundle according to any one of [2] to [4], wherein the solution in which the lignin has been dissolved in the solvent after the washing step is mixed with an acrylonitrile copolymer in a solvent to obtain a mixed solution, and the mixed solution is heated to obtain a spinning solution in which the acrylonitrile copolymer and the lignin have been dissolved in the solvent. [6] The method for producing a carbon fiber precursor fiber bundle according to any one of [2] to [5], wherein the solution obtained after the filtration step and an acrylonitrile copolymer are mixed in a solvent to obtain a mixed solution, and the mixed solution is heated to obtain a spinning solution in which the acrylonitrile copolymer and lignin are dissolved in the solvent. [7] The method for producing a carbon fiber precursor fiber bundle according to any one of [2] to [6], wherein the filtration precision of the filter is 0.08 to 2.0 μm. [8] The method for producing a carbon fiber precursor fiber bundle according to any one of [1] to [7], wherein the solvent is one or more selected from the group consisting of N,N-dimethylacetamide, N,N-dimethylformamide, and dimethylsulfoxide. [9] The method for producing a carbon fiber precursor fiber bundle according to any one of [2] to [8], wherein the acidic water has a temperature of 10 to 60°C.

[10] The method for producing a carbon fiber precursor fiber bundle according to any one of [2] to [9], wherein the amount of the acidic water is 300 to 900 parts by mass per 100 parts by mass of lignin.

[11] The method for producing a carbon fiber precursor fiber bundle according to any one of [2] to

[10] , wherein the lignin is washed with acidic water, and then washed with 200 to 500 parts by mass of water per 100 parts by mass of the lignin, and then dried.

[12] The method for producing a carbon fiber precursor fiber bundle according to

[11] , wherein the drying temperature is 70 to 95°C.

[13] The method for producing a carbon fiber precursor fiber bundle according to

[11] or

[12] , wherein the dried lignin is dried in a vacuum dryer.

[14] The method for producing a carbon fiber precursor fiber bundle according to any one of [1] to

[13] , wherein the lignin content is 5 to 45 mass% based on the total amount of the lignin and the acrylonitrile copolymer.

[15] The method for producing a carbon fiber precursor fiber bundle according to any one of [2] to

[14] , wherein the lignin content in the solution is 5 to 45 mass %.

[16] The method for producing a carbon fiber precursor fiber bundle according to [5], further comprising adding a solvent to the solution and then adding an acrylonitrile copolymer thereto.

[17] A method for producing a carbon fiber bundle, comprising heating a carbon fiber precursor fiber bundle obtained by the production method described in any one of [1] to

[16] in an oxidizing atmosphere at a temperature in the range of 200°C to 300°C, and then heating it in an inert atmosphere at a temperature in the range of 300°C to 2000°C.

[18] A carbon fiber bundle having a sulfur content of 0.090 mass% or more, a tensile strength of 1.75 GPa or more, and a tensile modulus of elasticity of 175 GPa or more in a strand test.

[19] The carbon fiber bundle according to

[18] , having a sodium element content of 70 ppm or less (by mass).

[20] The carbon fiber bundle according to

[18] or

[19] , wherein the potassium element content is 15 ppm (by mass) or less.

[21] The carbon fiber bundle according to any one of

[18] to

[20] , having an iron element content of 40 ppm (by mass) or less. Effect of the Invention

[0007] The present invention provides a method for producing a carbon fiber precursor fiber bundle, which is a carbon fiber precursor fiber bundle containing lignin, and which gives a carbon fiber bundle with high tensile strength when made into a carbon fiber bundle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The method for producing a carbon fiber precursor fiber bundle of the present invention is a method for producing a carbon fiber precursor fiber bundle by discharging a spinning dope in which an acrylonitrile copolymer and lignin are dissolved in a solvent from a discharge hole, and includes a removal step for removing impurities contained in the lignin. In this study, it was found that the reason why carbon fiber bundles obtained by heating carbon fiber precursor bundles containing lignin do not have high strength is due to impurities of sodium, potassium, and iron contained in the lignin raw material, and another reason is due to impurities that are insoluble in acidic water. It is therefore necessary to remove these impurities.

[0009] In the present invention, isolated lignin isolated by a chemical method is used as the lignin. Among the isolated lignins, lignin obtained from pulp waste liquid generated during chemical pulping in the paper pulp manufacturing process is preferred because it is inexpensive. Among lignins obtained from pulp waste liquor, it is preferable to use kraft lignin, which is lignin obtained from pulp waste liquor generated by the kraft process, which is a chemical pulping method using a high-temperature, high-pressure reaction with sodium hydroxide and sodium sulfide, etc. Since kraft lignin is unnecessary for water and soluble in the solvent used in the spinning dope, it is preferable because it is suitable for use as a fiber raw material by the wet spinning method. The kraft lignin may be made from either broadleaf trees or coniferous trees, with the latter being preferred because it is inexpensive and readily available.

[0010] In the method for producing a carbon fiber precursor fiber bundle of the present invention, the removal step is preferably one or more of a washing step of washing the lignin with acidic water and a filtration step of filtering a solution in which the lignin is dissolved in a solvent through a filter. By washing lignin with acidic water, the impurities such as sodium, potassium, and iron elements dissolve in the acidic water, making it possible to remove the impurities. As an example of a washing method, sodium, potassium, and iron elements are contained in the filtrate by filtering with filter paper, while lignin remains on the filter paper as a residue, making it easy to remove.

[0011] By filtering the solution through a filter, it is possible to remove minute impurities contained in the lignin that do not dissolve in acidic water. This filtration step may be performed using a solution in which lignin is dissolved in a solvent, or using a spinning dope in which the solution and an acrylonitrile copolymer are dissolved in a solvent. From the viewpoint of removing impurities in the lignin, filtration with a dissolving liquid is more preferable because filtration with a dissolving liquid can increase the accuracy of the filter.

[0012] The method for producing a carbon fiber precursor fiber bundle of the present invention preferably includes the filtration step after the washing step. This order makes it easier to remove impurities from the lignin.

[0013] In the method for producing a carbon fiber precursor fiber bundle of the present invention, the acidic water preferably has a pH of 3-6. When the pH of the acidic water is 3 to 6, the impurities such as sodium, potassium, and iron elements are more easily dissolved, and can be removed by filtration with filter paper. From this viewpoint, it is more preferable that the pH of the acidic water is 3.5 to 5.

[0014] In the method for producing a carbon fiber precursor fiber bundle of the present invention, it is preferable to mix a solution in which the lignin after the washing step is dissolved in a solvent with an acrylonitrile copolymer in a solvent to obtain a mixed solution, and then heat the mixed solution to obtain a spinning solution in which the acrylonitrile copolymer and the lignin are dissolved in the solvent. This makes it easier for the lignin and the acrylonitrile copolymer to mix.

[0015] In the method for producing a carbon fiber precursor fiber bundle of the present invention, it is preferable that the solution obtained after the filtration step and an acrylonitrile copolymer are mixed in a solvent to obtain a mixed solution, and then the mixed solution is heated to obtain a spinning solution in which the acrylonitrile copolymer and lignin are dissolved in the solvent. This makes it easier for the lignin and the acrylonitrile copolymer to mix.

[0016] In the method for producing a carbon fiber precursor fiber bundle of the present invention, the filtration accuracy of the filter is preferably 0.08 to 2.0 μm. By filtering through a filter with a filtration accuracy of 0.08 to 2.0 μm, it is possible to remove minute impurities and trace metals contained in the lignin that do not dissolve in acidic water. From this viewpoint, the filtration accuracy is more preferably from 0.1 to 1.0 μm, and further preferably from 0.1 to 0.5 μm. The filtration accuracy refers to the smallest particle size that can capture 95% or more of the particles.

[0017] In the method for producing a carbon fiber precursor fiber bundle of the present invention, the solvent is preferably at least one selected from the group consisting of N,N-dimethylacetamide, N,N-dimethylformamide, and dimethylsulfoxide. By using these solvents, the amount of undissolved lignin-acrylonitrile copolymer can be reduced.

[0018] In the method for producing a carbon fiber precursor fiber bundle of the present invention, the acidic water preferably has a temperature of 10 to 60°C. If the temperature of the acidic water is 10° C. or higher, the impurities such as sodium, potassium, and iron elements can be easily eluted, and if the temperature is 60° C. or lower, it is easy to prevent lignin from dissolving in the water. From these viewpoints, the temperature of the acidic water is more preferably 15 to 50°C, and further preferably 16 to 40°C.

[0019] In the method for producing a carbon fiber precursor fiber bundle of the present invention, the amount of acidic water used to wash the lignin is preferably 300 to 900 parts by mass per 100 parts by mass of lignin. When the amount of acidic water is 300 parts by mass or more per 100 parts by mass of lignin, impurities such as sodium, potassium, and iron elements can be easily washed away, whereas when the amount is 900 parts by mass or less, sufficient washing can be achieved, thereby saving costs and time. From these viewpoints, the amount of the acidic water is more preferably 400 to 700 parts by mass relative to 100 parts by mass of lignin.

[0020] In the method for producing a carbon fiber precursor fiber bundle of the present invention, it is preferable that the lignin is washed with acidic water, and then washed with 200 to 500 parts by mass of water per 100 parts by mass of the lignin, and then dried. When the amount of water is 200 parts by mass or more relative to 100 parts by mass of lignin, it is possible to sufficiently remove the acid, and when the amount of water is 500 parts by mass or less, it is preferable because the time required for washing can be shortened. By washing with water, impurities from the lignin can be reduced, thereby increasing the strength of the carbon fiber bundle.

[0021] In the method for producing a carbon fiber precursor fiber bundle of the present invention, the drying temperature is preferably 70 to 95°C. If the drying temperature is 70°C or higher, the moisture content of the lignin can be sufficiently reduced, and if the drying temperature is 95°C or lower, it is possible to prevent the lignin from deteriorating during drying and becoming less soluble in the solvent, which is preferable. From these viewpoints, the drying temperature is more preferably 75 to 90°C.

[0022] In the method for producing a carbon fiber precursor fiber bundle of the present invention, the dried lignin is preferably dried in a vacuum dryer. Vacuum drying has the effect of further reducing the moisture content in the lignin.

[0023] In the method for producing a carbon fiber precursor fiber bundle of the present invention, the lignin content is preferably 5 to 45 mass % based on the total amount of lignin and the acrylonitrile copolymer. If the lignin content is 5% by mass or more, the resulting carbon fiber bundle will be less dependent on petroleum-derived raw materials, which will lead to cost reduction, and if the lignin content is 45% by mass or less, the resulting carbon fiber bundle will have high tensile strength and tensile modulus, which is preferable. From these viewpoints, the content is more preferably from 5 to 45% by mass, further preferably from 8 to 35% by mass, and particularly preferably from 10 to 35% by mass.

[0024] In the method for producing a carbon fiber precursor fiber bundle of the present invention, it is preferable that a solvent is further added to the solution and then the acrylonitrile copolymer is added. This makes it easier for lignin to dissolve in the spinning dope, which has the effect of preventing the generation of undissolved lignin, and further improves the tensile strength and tensile modulus of the resulting carbon fiber bundle.

[0025] The method for producing a carbon fiber bundle of the present invention includes heating the carbon fiber precursor fiber bundle obtained by the method for producing a carbon fiber precursor fiber bundle in an oxidizing atmosphere at a temperature in the range of 200 to 300°C, and then heating it in an inert atmosphere at a temperature in the range of 300 to 2000°C. By using the carbon fiber precursor fiber bundle, even if the carbon fiber precursor fiber bundle contains lignin, the tensile strength and tensile modulus of the carbon fiber bundle can be increased.

[0026] The carbon fiber bundle of the present invention has a sulfur element content of 0.090% by mass or more, a tensile strength of 1.75 GPa or more and a tensile modulus of 175 GPa or more in a strand test. If the sulfur content is 0.090 mass% or more, there is sufficient lignin contained, which can contribute to carbon neutrality. From this viewpoint, the content of the sulfur element is more preferably equal to or greater than 0.093 mass %, and further preferably equal to or greater than 0.095 mass %. Furthermore, if the tensile strength in the strand test is 1.75 GPa or more and the tensile modulus is 175 GPa or more, it can be used industrially. From this viewpoint, the tensile strength is more preferably 2.4 GPa or more, and even more preferably 2.6 GPa or more, and the tensile modulus is more preferably 227 GPa or more, and even more preferably 230 GPa or more.

[0027] The carbon fiber bundle of the present invention preferably has a sodium element content of 70 ppm (mass basis) or less, more preferably 50 ppm (mass basis) or less, and even more preferably 30 ppm (mass basis) or less. If the content of sodium element is 70 ppm (mass basis) or less, the amount of sodium element contained as an impurity in the lignin is small, and the tensile strength of the carbon fiber bundle can be easily increased.

[0028] The carbon fiber bundle of the present invention preferably has a potassium element content of 15 ppm (mass basis) or less, more preferably 13 ppm (mass basis) or less, and even more preferably 12 ppm (mass basis) or less. If the content of potassium element is 15 ppm (mass basis) or less, the amount of potassium element contained as an impurity in the lignin is small, and the tensile strength of the carbon fiber bundle can be easily increased.

[0029] The carbon fiber bundle of the present invention preferably has an iron element content of 40 ppm (mass basis) or less, more preferably 35 ppm (mass basis) or less, and even more preferably 33 ppm (mass basis) or less. If the iron content is 40 ppm (mass basis) or less, the amount of iron element contained as an impurity in the lignin is small, and the tensile strength of the carbon fiber bundle can be easily increased.

[0030] A more specific explanation will now be given. <Lignin cleaning method> 2 kg of water adjusted to pH=4 (hereinafter referred to as acidic water) is placed in a stainless steel container, and 400 g of kraft lignin is added while stirring 2 L of acidic water. A dispersion of kraft lignin in acidic water is created. After adding 400 g of kraft lignin, continue stirring for 30 minutes to wash. The Büchner funnel with the filter paper placed in it is placed in the suction bottle, and the suction bottle is put into a suction state. The above dispersion liquid in which the washed kraft lignin is dispersed is placed on the Büchner funnel, and the liquid on the Büchner funnel is dropped into the suction bottle. The wet kraft lignin remains on the filter paper. Add pure water to the Büchner funnel containing the wet kraft lignin, and allow the liquid on the Büchner funnel to drip into a suction bottle. The wet kraft lignin remains on the filter paper. Pour pure water into the Büchner funnel containing the wet kraft lignin again, and allow the liquid on the Büchner funnel to drip into the suction bottle. The wet kraft lignin remains on the filter paper. The pure water is added to wash away the acidic water.

[0031] <Drying lignin> In order to dry the wet kraft lignin obtained by the above washing operation, the wet kraft lignin is placed in a hot air dryer set at a temperature of 90°C and dried for 6 hours while stirring once every 30 minutes. In order to further remove moisture from the kraft lignin dried in the hot air dryer as described above, it is dried in a vacuum dryer set at a temperature of 90°C for about 4 hours.

[0032] <Lignin filtration> Put 20 kg of N,N-dimethylacetamide (DMAc) into a stainless steel container and add 4 kg of the above-mentioned washed and dried kraft lignin. Stir for 4 hours to dissolve the kraft lignin in the DMAc.

[0033] [Normal filtration] The obtained solution was filtered through a cartridge filter with a precision of 1.0 μm (product name: Aztool pleated cartridge filter (made of PP) GDT1P10250E0).

[0034] [In the case of precision filtration] The obtained solution was filtered by passing it through (1) a cartridge filter with a precision of 0.5 μm (product name: Aztool pleated cartridge filter (made of PP) GDT05P10250E0), (2) a cartridge filter with a precision of 0.2 μm (product name: Aztool pleated cartridge filter (made of PP) GDT02P10250E0), and (3) a cartridge filter with a precision of 0.1 μm (product name: 3M polypropylene nonwoven depth filter cartridge 0.1 μm, CTJ0010P09NG), in that order.

[0035] <Preparation of spinning dope> The filtered lignin was dissolved in DMAc to produce a solution with a solids concentration of 16.67%. 24 kg of this solution and 37.21 kg of DMAc were mixed, and 9.33 kg of an acrylonitrile copolymer consisting of acrylonitrile units / acrylamide units / methacrylic acid units=97 / 2 / 1 (mass ratio) was further added and stirred to prepare a slurry. This slurry was heated to 120° C. to dissolve the acrylonitrile polymer, thereby preparing a dope (solid content was a blend of acrylonitrile polymer / craft lignin=7 / 3 (mass ratio), solid content concentration was 23.2 wt %).

[0036] <Spinning> The dope obtained above was extruded from a spinning nozzle with a hole diameter of 50 μm and 6,000 holes into a coagulation liquid consisting of an aqueous DMAc solution with a concentration of 40 mass% and a temperature of 28° C. to obtain a coagulated thread, which was simultaneously pulled up while applying tension to the coagulated thread. The coagulated yarn thus taken was stretched 1.15 times in the air, and then passed through three stages of stretching and washing tanks using water in the range of 28°C to 32°C, water in the range of 58°C to 62°C, and water in the range of 78°C to 82°C, where it was simultaneously stretched 1.66 times and washed. After that, it was stretched (relaxed) 0.98 times in a hot water bath using water at 98°C to obtain a drawn yarn. The obtained drawn yarn was immersed in a silicone-based oil dispersion containing 2 wt% silicone-based oil, and densified with a heated roller at 140° C. to obtain a dry fiber bundle. The obtained dry fiber bundle was then drawn 1.5 times while being heated with two pairs of rolls heated to 180° C. to obtain a carbon fiber precursor fiber bundle.

[0037] <Analysis of trace metal amounts> The contents of sodium, potassium and iron contained in the obtained carbon fiber precursor fiber bundle were analyzed by elemental analysis. 1 g of sample was sampled and precisely weighed in a platinum crucible. The platinum crucible containing the sample was placed on a hot plate heated to 540°C and heated for 3 hours. Next, the platinum crucible containing the sample was placed in an electric furnace set at 700°C and heated for 6 hours for incineration. The platinum crucible was removed from the electric furnace and allowed to cool. 0.2 mL of hydrofluoric acid and 1 mL of nitric acid were added to the platinum crucible containing the sample, and the sample was heated on a hot plate at 150°C for 15 minutes. Hydrofluoric acid and nitric acid are added to the platinum crucible in order to dissolve silicon in the hydrofluoric acid and nitric acid, and then remove the silicon by volatilizing it as silicon fluoride. The sample in the platinum crucible was transferred to a 50 mL measuring flask, and ultrapure water was added to the 50 mL measuring flask to make it 50 mL. The sodium, potassium, and iron elements were quantified using an ICP spectroscopic analyzer, PerkinElmer ICOptima 8300.

[0038] <Sulfur content analysis> When analyzing samples containing 0.1 wt% or more of sulfur, the sulfur content was analyzed using a CHNS analyzer. 5 mg of the sample, which had been previously chopped, was sampled and weighed on a tin board. The tin board containing the sample was molded into a tablet, which was then placed in a combustion furnace (UNICUBE, manufactured by Elemental) with the temperature set to 1150°C using helium carrier gas, and oxygen was sprayed on the sample to combust it, and the amount of sulfur was quantified. When analyzing samples containing 0.1 wt% or less of sulfur, the analysis was performed using a LECO CS844. 1 g of sample was sampled in a magnetic crucible and precisely weighed. The sample was placed in a high-frequency furnace at 2000°C using oxygen as carrier gas in a CS meter (LECO CS844) to determine the amount of sulfur.

[0039] <Flame resistance> The carbon fiber precursor fiber bundle was heated in an air atmosphere at a temperature range of 220° C. to 270° C. to obtain a flame-resistant fiber bundle. The flame-resistant time was set to 70 minutes, and the total elongation rate was set to 4%.

[0040] <Carbonization> The flame-resistant fiber bundle was carbonized by heating from 440° C. to 1300° C. in a nitrogen atmosphere to obtain a carbon fiber bundle. The obtained carbon fiber bundle was subjected to a surface treatment and then a sizing agent was applied thereto. EXAMPLES

[0041] <Quantification of lignin content in precursors (carbon fiber precursor fiber bundles) by infrared spectroscopy> The carbon fiber precursor fiber bundles were cut to about 10 mm, and then chopped into pieces of about 0.5 mm. These were then ground in a mortar to prepare a sample. 1 mg of the sample was weighed out, mixed with 200 mg of dried KBr in a mortar, and crushed. This was compressed in a press to form a disk-shaped tablet with a diameter of 13 mm and a thickness of 0.5 mm, and transmission measurements were performed using an FT-IR device (product name: iS50, manufactured by Nicolet). The spectrum was recorded using image processing software OMNIC Version 9.2.41, with the horizontal axis representing wave numbers (units: cm -1) and the vertical axis was the absorbance. Then, the auto baseline function was used to perform baseline correction. The spectrum after correction was used to obtain the 1510-1525 cm -1 The molar absorbance at the maximum molar absorbance and the molar absorbance at 2230-2260 cm -1 The molar absorbance ratio at the point where the molar absorbance is maximum (1510-1525 cm -1 The molar absorbance at the point where the molar absorbance is maximum is calculated by dividing the molar absorbance by the molar absorbance at 2230-2260 cm -1 The molar absorbance at the point where the molar absorbance was maximum was quantitatively evaluated. 1510~1525cm -1 The point where the molar absorbance is maximum is the absorption peak due to the cyano group, which correlates with the amount of acrylonitrile copolymer, and is in the range of 2230 to 2260 cm -1 The molar absorbance at the point where the molar absorbance is maximum is correlated with the amount of kraft lignin. -1 The molar absorbance at the point where the molar absorbance is maximum is calculated by dividing the molar absorbance by the molar absorbance at 2230-2260 cm -1 The amount of lignin in the carbon fiber precursor fiber is quantified by calculating the molar absorbance at the point where the molar absorbance is maximum (1510-1525 cm) and comparing it with a calibration curve prepared in advance. Five blends with known mixing ratios of acrylonitrile copolymer and kraft lignin were prepared for the calibration curve, and the ratio of each blend ratio to the molar absorbance ((1510-1525 cm)) was calculated. -1 The molar absorbance at the point where the molar absorbance is maximum is calculated by dividing the molar absorbance by the molar absorbance at 2230-2260 cm -1 The molar absorbance was calculated from the molar absorbance at the point where the molar absorbance was maximum.

[0042] <Mechanical property evaluation> A resin-impregnated strand was prepared from the obtained carbon fiber bundle, and the tensile modulus and tensile strength were measured.

[0043] Example 1 2 L of water adjusted to pH=4 and temperature of 25°C (hereinafter referred to as acidic water) was placed in a stainless steel container. 400 g of kraft lignin was added to the acidic water while stirring it, and the mixture was stirred for 30 minutes to obtain a dispersion in which the kraft lignin was dispersed in the acidic water. The dispersion was filtered through filter paper, and the kraft lignin remaining on the filter paper was washed with water and dried. The trace metal contents in the lignin washed with acidic water are shown in Table 1. The obtained kraft lignin was dissolved in DMAc to obtain a solution with a solid concentration of 16.7% by mass. The solution was then passed through (1) a cartridge filter with a precision of 0.5 μm (product name: Aztool pleated cartridge filter (made of PP) GDT05P10250E0), (2) a cartridge filter with a precision of 0.2 μm (product name: Aztool pleated cartridge filter (made of PP) GDT02P10250E0), and (3) a cartridge filter with a precision of 0.1 μm (product name: 3M polypropylene nonwoven depth filter cartridge 0.1 μm, CTJ0010P09NG) in that order to obtain a kraft lignin solution. Furthermore, the kraft lignin solution and the acrylonitrile copolymer were mixed with DMAc and heated to obtain a spinning solution in which the acrylonitrile copolymer and the kraft lignin were dissolved in DMAc. The solid content of the acrylonitrile copolymer in the spinning solution was 16.24% by mass, and the solid content of the kraft lignin in the spinning solution was 6.96% by mass. The spinning dope was used to perform spinning according to the procedure in <Spinning> to obtain a carbon fiber precursor fiber bundle. When spinning was performed, even after 6 hours had passed since the start of discharge from the spinning nozzle, the pressure in the spinning nozzle was 2.0 MPa, and spinning could be performed without any increase in pressure in the nozzle. The carbon fiber precursor fiber bundle was flame-retarded according to the procedure in <Flame-retarding>, and further carbonized according to the procedure in <Carbonization> to obtain a carbon fiber bundle. The contents of sodium, potassium and iron contained in the obtained carbon fiber bundle were analyzed using a CHNS analyzer, and the amount of sulfur was analyzed using a CS844 (manufactured by LECO Co., Ltd.). The results are shown in Table 1. The obtained carbon fiber bundle was used to prepare a strand, and the tensile modulus and tensile strength were measured as mechanical property evaluations. The results are shown in Table 1.

[0044] Example 2 A carbon fiber bundle was obtained in the same manner as in Example 1, except that the lignin was not washed with acidic water and the lignin was filtered according to [normal filtration]. The trace metal contents in lignin that was not washed with acidic water are shown in Table 1. When spinning was performed, even after 6 hours had passed since the start of discharge from the spinning nozzle, the pressure in the spinning nozzle was 2.0 MPa, and spinning could be performed without any increase in pressure in the nozzle. The obtained carbon fiber precursor fiber bundle was subjected to flame retardation and carbonization to obtain a carbon fiber bundle. The contents of sodium, potassium and iron contained in the obtained carbon fiber bundle were analyzed using a CHNS analyzer, and the amount of sulfur was analyzed using a CS844 (manufactured by LECO Co., Ltd.). The results are shown in Table 1. The obtained carbon fiber bundle was used to prepare a strand, and the tensile modulus and tensile strength were measured as mechanical property evaluations. The results are shown in Table 1. Since the lignin was not washed with acidic water, a large amount of metal components remained in the carbon fiber bundle, resulting in low strength.

[0045] Comparative Example 1 When spinning was performed according to the procedure in <Spinning> without washing or filtering the lignin, the pressure in the spinning nozzle reached 4.0 MPa or more 10 minutes after the dope started to be discharged from the spinning nozzle, and after another 10 minutes the pressure in the spinning nozzle reached 7.0 MPa, so spinning was stopped.

[0046] [Table 1]

Claims

1. A method for producing a carbon fiber precursor fiber bundle, comprising discharging a spinning dope in which an acrylonitrile copolymer and lignin are dissolved in a solvent from a discharge hole, A method for producing a carbon fiber precursor fiber bundle, comprising a removal step of removing impurities contained in lignin.

2. 2. The method for producing a carbon fiber precursor fiber bundle according to claim 1, wherein the removing step is at least one of a washing step of washing the lignin with acidic water and a filtration step of filtering a solution in which the lignin is dissolved in a solvent through a filter.

3. The method for producing a carbon fiber precursor fiber bundle according to claim 2 , further comprising the filtering step after the washing step.

4. 3. The method for producing a carbon fiber precursor fiber bundle according to claim 2, wherein the acidic water has a pH of 3 to 6.

5. 3. The method for producing a carbon fiber precursor fiber bundle according to claim 2, wherein the solution in which the lignin has been dissolved in the solvent after the washing step and an acrylonitrile copolymer are mixed in a solvent to obtain a mixed solution, and the mixed solution is heated to obtain a spinning solution in which the acrylonitrile copolymer and the lignin have been dissolved in the solvent.

6. 3. The method for producing a carbon fiber precursor fiber bundle according to claim 2, wherein the solution obtained after the filtration step and an acrylonitrile copolymer are mixed with a solvent to obtain a mixed solution, and the mixed solution is heated to obtain a spinning solution in which the acrylonitrile copolymer and lignin are dissolved in the solvent.

7. 3. The method for producing a carbon fiber precursor fiber bundle according to claim 2, wherein the filtration accuracy of the filter is 0.08 to 2.0 μm.

8. 2. The method for producing a carbon fiber precursor fiber bundle according to claim 1, wherein the solvent is at least one selected from the group consisting of N,N-dimethylacetamide, N,N-dimethylformamide, and dimethylsulfoxide.

9. The method for producing a carbon fiber precursor fiber bundle according to claim 2, wherein the temperature of the acidic water is 10 to 60°C.

10. The method for producing a carbon fiber precursor fiber bundle according to claim 2, wherein the amount of the acidic water is 300 to 900 parts by mass per 100 parts by mass of lignin.

11. The method for producing a carbon fiber precursor fiber bundle according to claim 2, wherein the lignin is washed with acidic water, and then washed with 200 to 500 parts by mass of water per 100 parts by mass of the lignin, and dried.

12. The method for producing a carbon fiber precursor fiber bundle according to claim 11, wherein the drying temperature is 70 to 95°C.

13. The method for producing a carbon fiber precursor fiber bundle according to claim 11, wherein the dried lignin is dried in a vacuum dryer.

14. 2. The method for producing a carbon fiber precursor fiber bundle according to claim 1, wherein the lignin content is 5 to 45 mass% based on the total amount of the lignin and the acrylonitrile copolymer.

15. The method for producing a carbon fiber precursor fiber bundle according to claim 2, wherein the content of lignin in the solution is 5 to 45 mass%.

16. The method for producing a carbon fiber precursor fiber bundle according to claim 5, wherein a solvent is further added to the solution before the acrylonitrile copolymer is added.

17. A method for producing a carbon fiber bundle, comprising heating a carbon fiber precursor fiber bundle obtained by the production method according to any one of claims 1 to 16 in an oxidizing atmosphere at a temperature in the range of 200 to 300°C, and then heating it in an inert atmosphere at a temperature in the range of 300 to 2000°C.

18. A carbon fiber bundle having a sulfur content of 0.090 mass % or more, a tensile strength of 1.75 GPa or more, and a tensile modulus of elasticity of 175 GPa or more in a strand test.

19. The carbon fiber bundle according to claim 18, wherein the sodium element content is 70 ppm or less (by mass).

20. The carbon fiber bundle according to claim 18, wherein the content of potassium element is 15 ppm (by mass) or less.

21. The carbon fiber bundle according to claim 18, wherein the iron content is 40 ppm or less (by mass).