Coating composition and coated body
A coating composition with a specific acrylic resin and crosslinking agent formulation addresses the challenge of low solvent content in aluminum wheel coatings, ensuring excellent scratch resistance, hardness, and chemical resistance, particularly against acidic cleaners.
Patent Information
- Application Number
- JP2023053832
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing coating compositions for aluminum wheels face challenges in achieving low organic solvent content while maintaining excellent scratch resistance, coating hardness, and chemical resistance, particularly when exposed to acidic cleaning solutions.
A coating composition comprising an acrylic resin with specific hydroxyl group content and a crosslinking agent, such as an amino resin, is formulated with a reduced organic solvent content of 600 g/L, optimizing the resin's molecular weight and hydroxyl group ratio to enhance crosslinking and curing efficiency.
The composition achieves a coating film with superior scratch resistance, coating hardness, and chemical resistance, even when subjected to acidic cleaning, while adhering to low VOC regulations.
Smart Images

Figure 2024141944000001 
Figure 2024141944000002 
Figure 2024141944000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating composition and a coated body. [Background technology]
[0002] Wheels for automobiles and motorcycles are mainly made from aluminum alloys. Cast aluminum wheels in particular can be easily processed into complex shapes, allowing for a wide variety of designs and mass production. Cast aluminum wheels are machined and then gloss-treated, after which a clear coat is applied to the surface to protect the base material. The clear coat is generally applied in the following order: a primer clear coat, and then a top clear coat. As a primer paint, for example, Patent Document 1 discloses an acrylic resin paint containing N-butoxymethylacrylamide as a thermosetting resin and transparent fine powdered silica and / or alumina. Patent Document 2 discloses a primer paint composition containing a copolymer resin, fumed silica, and a phosphoric acid compound containing magnesium to improve corrosion resistance. Patent Document 3 discloses a thermosetting liquid paint composition for aluminum wheels, which contains an acrylic resin obtained by copolymerizing a monomer mixture containing 8 to 40% by weight of a secondary hydroxyl group-containing unsaturated monomer, and an amino resin.
[0003] Meanwhile, in recent years, China has been requiring the use of materials that comply with mandatory standards (GB standards) for low-VOC (volatile organic compound) paints, adhesives, etc., and as a result, there is a demand for paints with reduced organic solvent content. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. Hei 1-194979 [Patent Document 2] International Publication No. 2014 / 181593 [Patent Document 3] International Publication No. 2004 / 094545 Summary of the Invention [Problem to be solved by the invention]
[0005] To prepare a paint with a reduced amount of organic solvent, it is necessary to design the viscosity of the resin to be low. However, simply lowering the viscosity of the paint by lowering the molecular weight of the resin tends to deteriorate the physical properties of the resulting coating film. In particular, aluminum wheels tend to have poor resistance to acidic cleaning solutions, which are washed after production. The present invention has been made in consideration of the above circumstances, and has an object to provide a coating composition that is excellent in abrasion resistance, coating film hardness, and chemical resistance, and a coated body coated with the coating composition. [Means for solving the problem]
[0006] The present invention relates to a coating composition comprising an acrylic resin (X) having a hydroxyl group number per number average molecular weight of 2.0 or more and 6.0 or less, a crosslinking agent (Y) that reacts with hydroxyl groups, and an organic solvent (Z), the content of the organic solvent (Z) being 600 g / L or less.
[0007] The crosslinking agent (Y) that reacts with a hydroxyl group preferably contains an amino resin.
[0008] It is preferred that the hydroxyl value calculated from the primary hydroxyl groups of the acrylic resin (X) is 40 mgKOH / g or more and 130 mgKOH / g or less, and the ratio of the primary hydroxyl value to the secondary hydroxyl value is 100:0 or more and 100:60 or less.
[0009] The coated body of the present invention has a coating film made of the coating composition of the present invention on a substrate.
[0010] The glass transition temperature Tg of the coating film is preferably 50°C or higher and 98°C or lower. Effect of the Invention
[0011] According to the present invention, it is possible to obtain a coating composition having excellent scratch resistance, coating film hardness and chemical resistance, and a coated body coated with the coating composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, one embodiment of the present invention will be described.
[0013] [Paint composition] The coating composition of the present invention comprises an acrylic resin (X) having a hydroxyl group number per number average molecular weight of 2.0 or more and 6.0 or less, a crosslinking agent (Y) that reacts with hydroxyl groups (hereinafter, may be simply referred to as crosslinking agent (Y)), and an organic solvent (Z), and the content of the organic solvent (Z) is 600 g / L or less. Each component will be described in detail below.
[0014] <Acrylic resin (X)> Examples of the polymerizable monomer constituting the acrylic resin (X) include one or more acrylic components selected from acrylic acid, methacrylic acid, and their esters, amides, and nitriles; and polymerizable unsaturated monomers such as styrene and vinyl group-containing ester compounds (excluding acrylic components).
[0015] (Acrylic component) Examples of the acrylic component include the following compounds (a1) to (a5).
[0016] -(meth)acrylic acid and alcohol having 1 to 24 carbon atoms (a1)- Examples of the ester (a1) of (meth)acrylic acid and an alcohol having 1 to 24 carbon atoms include methyl (meth)acrylate, 2-isocyanatoethyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, tridecyl (meth)acrylate, and stearyl (meth)acrylate.
[0017] -Carboxyl group-containing monomer (a2)- Examples of the carboxyl group-containing monomer (a2) include acrylic acid, methacrylic acid, maleic acid, and maleic anhydride.
[0018] -Hydroxyl group-containing monomer (a3)- Examples of the hydroxyl group-containing monomer (a3) include monoesters of (meth)acrylic acid and dihydric alcohols, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate, as well as (meth)acrylates having a polyoxyethylene chain with a hydroxyl group at the molecular terminal.
[0019] -Epoxy group-containing polymerizable unsaturated monomer (a4)- Examples of the epoxy group-containing polymerizable unsaturated monomer (a4) include glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and the like.
[0020] -Aminoalkyl(meth)acrylate (a5)- Examples of the aminoalkyl (meth)acrylate (a5) include N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylate.
[0021] (Polymerizable unsaturated monomer (a6)) As the polymerizable monomer other than the acrylic component, the following polymerizable unsaturated monomer (a6) can be mentioned. Examples of the polymerizable unsaturated monomer (a6) include vinyl group-containing aromatic compounds such as styrene, α-methylstyrene, and vinyl toluene, and vinyl group-containing compounds such as vinyl acetate.
[0022] The properties of the acrylic resin (X) will be described below.
[0023] (Number average molecular weight Mn) The number average molecular weight Mn of the acrylic resin (X) is 1500 or more and 7500 or less. By being 1500 or more, a coating film having good scratch resistance and coating film hardness can be obtained when crosslinked. By being 7500 or less, a coating composition having an organic solvent amount of 600 g / L or less can be obtained. The number average molecular weight Mn of the acrylic resin (X) is preferably 2000 or more and 6000 or less. In this specification, the number average molecular weight Mn of the acrylic resin (X) is measured by the measurement method shown in the examples described later. In the coating composition of the present invention, by making the number average molecular weight of the acrylic resin (X) relatively low as described above, it is possible to reduce the content of the organic solvent (Z).
[0024] (Hydroxyl value calculated from primary hydroxyl groups) In the acrylic resin (X), the hydroxyl value calculated from the primary hydroxyl groups is preferably 40 mgKOH / g or more and 130 mgKOH / g or less, more preferably 60 mgKOH / g or more and 120 mgKOH / g or less. By having the hydroxyl value calculated from the primary hydroxyl groups of the acrylic resin (X) of 40 mgKOH / g or more, sufficient curability to exhibit good coating film performance can be ensured, and scratch resistance and coating film hardness can be ensured. In addition, by having the hydroxyl value calculated from the primary hydroxyl groups of the acrylic resin (X) of 130 mgKOH / g or less, unreacted hydroxyl groups can be reduced, resulting in excellent chemical resistance.
[0025] (Hydroxyl value calculated from secondary hydroxyl groups) In the acrylic resin (X), the hydroxyl value calculated from the secondary hydroxyl groups is preferably 40 mgKOH / g or less, more preferably 25 mgKOH / g or less, and even more preferably 10 mgKOH / g or less. By having a hydroxyl value calculated from the secondary hydroxyl groups of 40 mgKOH / g or less, a coating film excellent in chemical resistance, scratch resistance, and coating film hardness can be obtained.
[0026] Here, the total hydroxyl value of the acrylic resin (X) is the number of milligrams of potassium hydroxide required to completely acetylate the hydroxyl groups in 1 g of the resin with acetic anhydride and then neutralize the free acetic acid generated by acetylation.
[0027] (Ratio of primary hydroxyl value to secondary hydroxyl value) Since secondary hydroxyl groups are less reactive than primary hydroxyl groups, the balance between the reaction between the acrylic resin (X) and the crosslinking agent (Y) and between the crosslinking agents (Y) becomes poor, and the resulting coating film tends to be inferior in chemical resistance, scratch resistance, and coating film hardness. For this reason, the ratio of the primary hydroxyl value to the secondary hydroxyl value in the acrylic resin (X) is preferably 100:0 or more and 100:60 or less, and more preferably 100:0 or more and 100:35 or less.
[0028] (Acid value) The acid value of the acrylic resin (X) is preferably 10 mgKOH / g or more and 50 mgKOH / g or less. By having an acid value of 10 mgKOH / g or more, it becomes easier to act as a catalyst in the reaction with the amino resin, and a coating film having good scratch resistance and coating film hardness can be obtained. By having an acid value of 50 mgKOH / g or less, a coating film having few residual acid groups and good chemical resistance can be obtained. In the present invention, the acid value of the acrylic resin (X) is a value determined in accordance with JIS-K-5601-2-1:1999.
[0029] (Total number of hydroxyl groups per number average molecular weight) The total number of hydroxyl groups per number average molecular weight is preferably 2.0 or more and 6.0 or less, more preferably 2.5 or more and 5.5 or less. By having the total number of hydroxyl groups per number average molecular weight of 2.0 or more, the number of crosslinking points with the crosslinking agent (Y) increases, curing proceeds well, and a coating film having excellent coating film hardness and scratch resistance can be obtained. In addition, by having the total number of hydroxyl groups per number average molecular weight of 6.0 or less, a coating film having few residual hydroxyl groups and excellent chemical resistance can be obtained. The total number of hydroxyl groups per number average molecular weight is determined by the method described in the Examples below.
[0030] (Weight average molecular weight Mw) The weight average molecular weight Mw of the acrylic resin (X) is preferably 3000 or more and 18000 or less. By being 3000 or more, a coating film having good scratch resistance and coating film hardness can be obtained when crosslinked. By being 18000 or less, a coating composition having an organic solvent amount of 600 g / L or less can be obtained. The weight average molecular weight Mw of the acrylic resin (X) is more preferably 5000 or more and 14000 or less. In this specification, the weight average molecular weight Mw of the acrylic resin (X) is measured by the measurement method shown in the examples described later.
[0031] (Total number of hydroxyl groups per weight average molecular weight) The total number of hydroxyl groups per weight average molecular weight is preferably 4.0 or more and 11.0 or less. By having the total number of hydroxyl groups per weight average molecular weight of 4.0 or more, the number of crosslinking points with the crosslinking agent (Y) increases, curing proceeds well, and a coating film having good scratch resistance and coating film hardness can be obtained. By having the total number of hydroxyl groups per weight average molecular weight of 11.0 or less, a coating film having few residual hydroxyl groups and good chemical resistance can be obtained. The total number of hydroxyl groups per weight average molecular weight is determined by the method described in the Examples below.
[0032] <Crosslinking agent (Y) that reacts with hydroxyl groups> The crosslinking agent (Y) that reacts with a hydroxyl group preferably contains an amino resin, and examples of the amino resin include urea resin, melamine resin, and benzoguanamine resin.
[0033] (mass ratio of acrylic resin (X) to crosslinking agent (Y) that reacts with hydroxyl groups) The mass ratio of the acrylic resin (X) to the crosslinking agent (Y) reactive with a hydroxyl group, "acrylic resin (X) / crosslinking agent (Y) reactive with a hydroxyl group," is preferably 60 / 40 or more and 75 / 25 or less, and more preferably 60 / 40 or more and 70 / 30 or less. By adjusting the ratio of the acrylic resin (X) and the crosslinking agent (Y) that reacts with hydroxyl groups within the above range, a coating film having good coating hardness, scratch resistance and chemical resistance can be obtained.
[0034] <Organic solvent (Z)> Examples of the organic solvent (Z) include butyl acetate, xylene, ethylene glycol mono-normal propyl ether, toluene, methyl isobutyl ketone, isopropyl alcohol, butanol, acetone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, methyl ethyl ketone, ethyl 3-ethoxypropionate, aromatic solvents (e.g., Solvesso 150, toluene, xylene), etc. Known commercially available products can be used as these solvents.
[0035] The content of the organic solvent (Z) in the coating composition of the present invention is 600 g / L or less. The content of the organic solvent (Z) in the coating composition of the present invention can be further set to 550 g / L or less, or further set to 450 g / L or less. When the content of the organic solvent (Z) is 600 g / L or less, coating is possible without diluting the coating composition. In addition, in the present invention, even if a coating composition having an even lower content of organic solvent (Z) of 430 g / L or less is prepared and then diluted to a viscosity suitable for coating immediately before coating, the content of organic solvent (Z) in the coating composition at the time of coating can be 600 g / L or less. Therefore, the coating composition of the present invention is an environmentally friendly coating composition. Furthermore, even if the coating composition of the present invention has a low content of organic solvent (Z) as described above, it has good curability and is excellent in abrasion resistance, coating film hardness, and chemical resistance.
[0036] The concentration of the organic solvent (Z) in the coating composition of the present invention is preferably from 35% by mass to 55% by mass, from the viewpoints of coatability and environmental considerations.
[0037] <Other ingredients> The coating composition of the present invention can appropriately use additives necessary for a coating composition. For example, various coating additives that are generally known and commonly used in the art, such as pigments, pigment dispersants, defoamers, antisagging agents, UV absorbers, light stabilizers, and antifungal agents, can be used in conventional amounts. Furthermore, the coating composition of the present invention can also be used in combination with other resins, such as acrylic-modified alkyd resins, alkyd resins, silicone resins, fluororesins, or epoxy resins, as appropriate, for the purpose of improving performance within a range that does not affect the effects of the present invention.
[0038] <Total light transmittance> The coating composition of the present invention is preferably a clear coating from the viewpoint of application to highly decorative substrates. In this specification, the clear coating is a coating that forms a transparent coating film, and when the coating film has a thickness of 30 μm, the transmittance is 80% or more, preferably 90% or more, more preferably 95% or more, and even more preferably 97% or more. In this specification, the transmittance means the total light transmittance in the visible region (360 nm to 750 nm), and can be measured in accordance with JIS K 7375:2008.
[0039] [Properties of the coating] The properties of the coating film formed using the coating composition of the present invention will now be described.
[0040] <Water contact angle of coating film> The coating film obtained by coating so as to have a dry thickness of 30 μm preferably has a water contact angle of 80° or more. When the contact angle of water on the coating surface is 80° or more, the penetration of hydrophilic components into the coating is easily inhibited.
[0041] <Cross-link density of coating film> The crosslink density of the coating film is preferably 0.00050 mol / cc or more and 0.00180 mol / cc or less, and more preferably 0.00077 mol / cc or more and 0.00125 mol / cc or less. By adjusting the crosslink density of the coating film within the above range, a coating film having good coating film hardness, scratch resistance, and chemical resistance can be obtained.
[0042] <Molecular weight between crosslinks of coating film (1 / crosslink density)> The molecular weight between crosslinks of the coating film (1 / crosslink density) is preferably 550 cc / mol to 2000 cc / mol, more preferably 800 cc / mol to 1300 cc / mol. By adjusting the molecular weight between crosslinks (1 / crosslink density) of the coating film to the above range, a coating film having good coating film hardness, scratch resistance, and chemical resistance can be obtained.
[0043] <Glass transition temperature Tg of coating film> The glass transition temperature Tg of the coating film obtained by coating to a dry thickness of 30 μm is preferably 50° C. or higher and 98° C. or lower, and more preferably 65° C. or higher and 95° C. or lower. When the glass transition temperature Tg of the coating film is 50° C. or higher, a coating film having excellent scratch resistance and coating film hardness can be obtained. When the glass transition temperature Tg is 98° C. or lower, a coating film having good chemical resistance can be obtained.
[0044] <Coating film hardness> The hardness of the coating film, measured according to JIS K5600 5-3:1999 scratch hardness (pencil method), is preferably 2B or more, more preferably HB or more. If the coating film has such hardness, the design can be maintained for a long period of time even when the coating film is used on a metal substrate (e.g., an aluminum wheel of an automobile, etc.), and therefore high quality can be provided.
[0045] [Painting method] The coating method of the present invention involves coating a substrate with the coating composition of the present invention. Examples of coating methods include dipping, electrostatic coating, spin coating, flow coating, roll coating, spray coating, blade coating, and air knife coating. Among these, spray coating and roll coating are preferred from the viewpoint of easy control of film thickness.
[0046] The reaction of the coating film formed by applying the coating composition is not yet complete when the coating film is formed, and the drying and curing reaction are terminated by baking (heat drying) to cause a curing reaction after the coating film is formed. The baking conditions are preferably 80 to 180°C and 5 to 90 minutes.
[0047] <Base material> The substrate in the present invention is not particularly limited, and its shape may be, for example, a plate, a sheet, or a foil. In addition, if the substrate is a metal substrate, it may be steel, galvanized steel, stainless steel, magnesium alloy, aluminum, or an aluminum alloy, and among these, an aluminum alloy is preferable. The metal substrate may be subjected to various surface treatments, such as oxidation treatment. As an example, a substrate in which aluminum has been subjected to oxidation treatment by a method such as anodizing, phosphate treatment, chromate treatment, or non-chromate treatment may be used. In addition, the metal substrate may be coated with an electrodeposition coating film or a primer, or the coating composition of the present invention may be applied to a metal substrate on which a decorative layer has been formed. The decorative layer may be formed using a paint, ink, vapor deposition method, or the like, and may be a metallic decorative layer. In addition, the paint and ink used to form the decorative layer may be solvent-based, water-based, or solventless, and a paint or ink that is cured using heat or active energy rays may also be used. The coating composition of the present invention is useful as a top clear coating for metal substrates, and the coating film formed has excellent scratch resistance, coating hardness and chemical resistance.
[0048] [Painted body] The coated body of the present invention has a coating film made of the coating composition of the present invention on a substrate. The coating film can be formed by the coating method described above. The coated body of the present invention has a coating film made of the above-mentioned coating composition, and therefore has excellent scratch resistance, coating hardness and chemical resistance. Furthermore, the coated body of the present invention may further have a surface protective layer having stain resistance and the like on the coating film. EXAMPLES
[0049] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below.
[0050] [Preparation of acrylic resin solution] First, a resin solution containing the acrylic resin (X) used in the examples and comparative examples is prepared. [Resin solution T1] A resin solution T1 containing an acrylic resin (X) was prepared according to the following procedure. Table 1 shows the monomers and solvents required for preparing the resin, as well as the properties of the acrylic resin (X). 30.0 parts by mass of xylene, 31.0 parts by mass of styrene, 12.0 parts by mass of 2-ethylhexyl acrylate, 43.0 parts by mass of 2-ethylhexyl methacrylate, 2.0 parts by mass of acrylic acid, 12 parts by mass of 2-hydroxyethyl methacrylate, and 4.0 parts by mass of 2-2'-azobis-2-methylbutyronitrile were reacted under nitrogen gas at 100°C for 8 hours. The mixture was then diluted with 32.7 parts by mass of xylene to obtain an acrylic resin solution T1 with a heating residue of 60% by mass.
[0051] The acrylic resin (X) contained in the acrylic resin solution T1 had a hydroxyl value of 45 mgKOH / g, an acid value of 11 mgKOH / g, a number average molecular weight of 3,500, and a weight average molecular weight of 6,000.
[0052] [Resin solutions T2 to T21] Resin solutions T2 to T21 were prepared in the same manner as resin solution T1, except that the compounds and compositions were changed as shown in Tables 1 to 3.
[0053] (heated residue) 1.0 g of the resin solution was precisely weighed into an aluminum cup and dried for 30 minutes in an oven at 150° C. After drying, the mass of the residue was precisely weighed, and the ratio of the mass of the residue to the original mass was calculated as the heating residue (mass %).
[0054] (Hydroxyl value) The hydroxyl groups in 1 g of acrylic resin (X) were completely acetylated with acetic anhydride, and the amount of potassium hydroxide required to neutralize the free acetic acid generated by the acetylation was then determined in mg, and this value was taken as the hydroxyl value of the acrylic resin (X).
[0055] (Acid value) The acid value of the acrylic resin (X) was determined in accordance with JIS-K-5601-2-1:1999.
[0056] (Number average molecular weight Mn) The number average molecular weight Mn of the acrylic resin (X) was measured by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector using a TSKgel column SuperMultiporeHZ-M (manufactured by Tosoh Corporation). The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.
[0057] (Weight average molecular weight Mw) The weight average molecular weight Mw of the acrylic resin (X) was measured by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector using a TSKgel column SuperMultiporeHZ-M (manufactured by Tosoh Corporation). The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.
[0058] (Glass transition temperature Tg of acrylic resin (X)) The glass transition temperature Tg of the acrylic resin (X) was calculated by the Fox formula.
[0059] (Total number of hydroxyl groups per number average molecular weight Mn of acrylic resin (X)) The total number of hydroxyl groups per number average molecular weight Mn of the acrylic resin (X) was calculated from the measurement results of the number average molecular weight Mn and the hydroxyl value according to the following formula (1). "Total number of hydroxyl groups per number average molecular weight Mn" = Number average molecular weight of acrylic resin × (hydroxyl value of acrylic resin (mgKOH / g) / 56100) (1)
[0060] (Total number of hydroxyl groups per weight average molecular weight Mw of acrylic resin (X)) The total number of hydroxyl groups per weight average molecular weight Mw of the acrylic resin (X) was calculated from the measurement results of the weight average molecular weight Mw and the hydroxyl value according to the following formula (2). "Total number of hydroxyl groups per weight average molecular weight Mw" = Weight average molecular weight of acrylic resin × (hydroxyl value of acrylic resin (mgKOH / g) / 56100) (2)
[0061] (Ratio of primary hydroxyl value to secondary hydroxyl value) The ratio of the primary hydroxyl value to the secondary hydroxyl value of the acrylic resin (X) was calculated by calculating the theoretical primary hydroxyl value and the theoretical secondary hydroxyl value, respectively, and then calculating the ratio thereof.
[0062] [Table 1]
[0063] [Table 2]
[0064] [Table 3]
[0065] Next, the resin solution was used to prepare coating compositions of the examples and comparative examples and coating films formed by applying and curing the coating compositions. The components used in the coating compositions and their formulations are shown in Tables 4 to 6. In Tables 4 to 6, the amount of each component used is expressed in parts by mass.
[0066] [Example 1] (Preparation of Coating Composition) As the acrylic resin (X), 61.7 parts by mass of resin solution T1; as the crosslinking agent (Y) that reacts with hydroxyl groups, 26.5 parts by mass of a melamine resin solution (a mixed solution of n-butylated melamine resin in xylene and n-butanol (heating residue 60% by mass), product name: AMIDIR L-117-60, manufactured by DIC Corporation); as the organic solvent (Z), 3.0 parts by mass of propylene glycol monomethyl ether acetate, 1.0 part by mass of butyl acetate, and 2.8 parts by mass of Solvesso 150 (manufactured by JX Nippon Oil & Energy Corporation); as an ultraviolet absorber, 1.0 part by mass of a hydroxyphenyltriazine-based ultraviolet absorber (product name: TINUVIN400, manufactured by BASF Corporation); The coating composition of Example 1 was prepared by mixing 1.0 part by mass of a coating solution (manufactured by Nippoh Chemical Co., Ltd.) as a dehydrating agent (trade name: MOA, manufactured by Nippoh Chemical Co., Ltd.) and 3.0 parts by mass of methyl orthoacetate (trade name: MOA, manufactured by Nippoh Chemical Co., Ltd.) as a dehydrating agent, followed by stirring with a disperser.
[0067] (Preparation of painted body (base material: aluminum)) The above coating composition was spray-painted onto a substrate made of aluminum, 0.8 mm thick, and 150 mm x 70 mm in size, so that the dry film thickness was 30 μm, and then the coating composition was dried at 140° C. for 20 minutes to form a coating film, producing a coated body (substrate: aluminum). This coated body was used to evaluate chemical resistance, scratch resistance, and coating hardness.
[0068] (Preparation of painted body (base material: polypropylene)) The above coating composition was spray-painted onto a substrate made of polypropylene, 3.0 mm thick, and 100 mm x 100 mm in size, so that the dry film thickness was 30 μm. The coating composition was then dried at 140°C for 20 minutes to form a coating film, producing a coated body (substrate: polypropylene). This coated body was used to measure the glass transition temperature Tg, the molecular weight between crosslinks, and the crosslink density of the coating film.
[0069] [Examples 2 to 14, Comparative Examples 1 to 10] Coating compositions were prepared in the same manner as in Example 1, except that the resin solution containing the acrylic resin (X) was changed as shown in Table 6 instead of Table 4.
[0070] [evaluation] The coated bodies of the above Examples and Comparative Examples were evaluated as follows. The evaluation results are shown in Tables 4 to 6.
[0071] (Fort Cup viscosity in seconds when applied) The outflow time of the coating composition during application was measured at 20°C using a Ford cup #4 in accordance with a method in accordance with JIS K5600-2-2:1999.
[0072] (Glass transition temperature Tg of coating film) The coating films of Examples 1 to 14 and Comparative Examples 1 to 10 were peeled off from the polypropylene resin plate and then cut to a length of 50 mm and a width of 8 mm to prepare a measurement sample. The dynamic viscoelasticity of the sample was measured using a dynamic viscoelasticity measuring device RSA G2 (manufactured by TA Instruments) at a measurement length of 24 mm, a frequency of 1 Hz, and a heating rate of 5°C / min. The dynamic glass transition temperature measured as the temperature showing the maximum value of tan δ (loss modulus / storage modulus) was taken as the glass transition temperature.
[0073] (Molecular weight between crosslinks, crosslink density of coating film) The molecular weight of the resin between crosslinks is called the inter-crosslink molecular weight, and is expressed as the reciprocal of the crosslink density. The higher the crosslink density, the smaller this value becomes. The intercrosslink molecular weight of the cured coating film of the present invention is a theoretically calculated value obtained by applying the minimum value of the storage modulus obtained during measurement of the glass transition temperature of the cured coating film to the following theoretical formula of rubber viscoelasticity. Formula 1:n=E' / 3RT Where: n :Crosslink density (mol / cc) 1 / n: Molecular weight between crosslinks (cc / mol) R: Gas constant (8.314 J / K / mol) T: Absolute temperature (K) at which the storage modulus is E' E': Minimum storage modulus (Pa)
[0074] (Chemical resistance) On the surfaces of the coating films of Examples 1 to 14 and Comparative Examples 1 to 10, 1 ml of hydrofluoric acid solution (10% hydrofluoric acid) was dropped, and then the surfaces were left in a test tank without forced convection at a temperature of 23° C. for 2 hours for chemical treatment. Thereafter, the hydrofluoric acid solution was removed by rinsing with water, and the appearance of the coating film after the chemical treatment was visually evaluated according to the following evaluation criteria. -Evaluation criteria- AA: No change in the appearance of the coating. A: The gloss of the coating film decreases slightly. C: The gloss of the coating film is significantly reduced.
[0075] (Coating film hardness) The coating films of Examples 1 to 14 and Comparative Examples 1 to 10 were measured for scratch hardness (pencil method) according to JIS K5600-5-4:1999, and evaluated according to the following evaluation criteria. -Evaluation criteria- AA: Pencil hardness HB or higher A: Pencil hardness is 2B or more and B or less C: Pencil hardness is 3B or less
[0076] (Scratch resistance) Using a friction fastness tester (manufactured by DAIEI KAGAKU SEIKI), a load of 1 kg was applied to the coating surface of the coated body and the coating was moved back and forth 10 times using a white cloth for dye fastness testing conforming to JIS L 0849. After the 10 cycles, the coating surface was washed with running water and naturally dried, after which the gloss of the coating was visually observed and evaluated according to the following criteria. AA: No change in gloss A: Very slightly dull C: Significant loss of gloss
[0077] [Table 4]
[0078] [Table 5]
[0079] [Table 6]
[0080] As shown in Tables 4 to 6, the coating films of Examples 1 to 14 using the coating composition of the present invention were excellent in scratch resistance, coating hardness and chemical resistance. Comparative Examples 1 and 2, which used resin solutions T13 and T14 in which the total number of hydroxyl groups per number average molecular weight was in the range of 1.1 to 1.4, were inferior in both scratch resistance and coating hardness. Comparative Examples 3 to 8, which used resin solutions T15 to T20 in which the total number of hydroxyl groups per number average molecular weight was in the range of 6.4 to 7.5, were inferior in chemical resistance. Moreover, Comparative Example 9, which used resin solution T21 in which the total number of hydroxyl groups per number average molecule was 0, was inferior in both scratch resistance and coating hardness. Furthermore, Comparative Example 10, which did not contain the melamine resin crosslinking agent, was inferior in chemical resistance, scratch resistance and coating hardness. [Industrial Applicability]
[0081] The coating composition of the present invention can be used as a top coat coating when forming a coating film on a metal substrate in fields such as automobile manufacturing.
Claims
1. An acrylic resin (X) having a hydroxyl group number per number average molecular weight of 2.0 or more and 6.0 or less; A crosslinking agent (Y) that reacts with hydroxyl groups, and Contains an organic solvent (Z), A coating composition having an organic solvent (Z) content of 600 g / L or less.
2. 2. The coating composition according to claim 1, wherein the crosslinking agent (Y) which reacts with hydroxyl groups comprises an amino resin.
3. 2. The coating composition according to claim 1, wherein the hydroxyl value calculated from the primary hydroxyl groups of the acrylic resin (X) is 40 mgKOH / g or more and 130 mgKOH / g or less, and the ratio of the primary hydroxyl value to the secondary hydroxyl value is 100:0 or more and 100:60 or less.
4. A coated body having a coating film made of the coating composition according to any one of claims 1 to 3 on a substrate.
5. 5. The coated body according to claim 4, wherein the glass transition temperature Tg of the coating film is 50° C. or higher and 98° C. or lower.
Citation Information
Patent Citations
High-solid coating composition
JP2002201430A
Top coat formation method, and clear coating composition used for the same
JP2008126140A
Coating composition and coated body using the same
JP2015067764A
Coating method
JP2019084465A
Method of coating aluminum foil
JP1989194979A