Polyfunctional vinyl aromatic copolymer
A polyfunctional vinyl aromatic copolymer with a high m-isomer ratio and controlled molecular weight distribution, combined with alkylstyrene and curable resins, addresses the poor processability of conventional copolymers, enhancing the workability and dielectric properties of laminates.
Patent Information
- Application Number
- JP2023053884
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional polyfunctional vinyl aromatic copolymers exhibit poor processability during the production of prepregs, which are raw materials for laminates, necessitating improvements in workability and dielectric properties.
A polyfunctional vinyl aromatic copolymer with a high m-isomer ratio of divinyl aromatic compounds and a specific molecular weight distribution, combined with alkylstyrene and curable resin components, is developed to enhance processability and dielectric properties.
The copolymer provides laminates with improved workability, reduced dielectric loss tangent, enhanced heat resistance, and better solder heat resistance, resulting in superior processability and electrical properties.
Abstract
Description
[Technical field]
[0001] The present disclosure relates to multifunctional vinyl aromatic copolymers, and the like. [Background technology]
[0002] In recent years, with the remarkable progress of information network technology or the expansion of services utilizing information networks, electronic devices are required to have a larger capacity of information and a faster processing speed. In order to meet these demands, printed wiring boards mounted on electronic devices are strongly required to have high processability in addition to the conventionally required properties such as insulation reliability, rigidity, and flame retardancy. Therefore, further improvements have been considered for the resin composition, which is the main insulating material constituting the printed wiring board, and cured resins using vinyl compounds with various chemical structures have been proposed.
[0003] As such a cured resin, for example, Patent Document 1 discloses a soluble polyfunctional vinyl aromatic copolymer obtained by polymerizing a divinyl aromatic compound and a monovinyl aromatic compound in the presence of a Lewis acid catalyst.
[0004] Patent Document 2 proposes a polyfunctional vinyl aromatic copolymer obtained by polymerizing not only a divinyl aromatic compound and a vinyl aromatic compound but also a cycloolefin compound. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2017 / 115813 [Patent Document 2] International Publication No. 2018 / 181842 [Non-patent literature]
[0006] [Non-Patent Document 1] Akifumi Noujima, et al., "Gold Nanoparticle-Catalyzed Environmentally Benign Deoxygenation of Epoxides to Alkenes", Molecules, (2011), 16(10), pp.8209-8227 [Non-Patent Document 2] Gerrit Wienhoefer, et al., "Selective Iron-catalyzed Transfer Hydrogenation of Terminal Alkynes", Chemical Communications (Cambridge, United Kingdom), (2012), 48(40), pp.4827-4829 Summary of the Invention [Problem to be solved by the invention]
[0007] However, there is room for improvement in the processability during production of prepregs in conventional polyfunctional vinyl aromatic copolymers such as those described in Patent Documents 1 and 2. Thus, one of the objects of the present disclosure is to provide a polyfunctional vinyl aromatic copolymer and a curable resin composition containing the same, which can provide a laminate or the like having excellent processability during production of a prepreg, which is a raw material for the laminate. [Means for solving the problem]
[0008] Examples of embodiments of the present disclosure are listed in the following items [1] to
[16] . [1] A polyfunctional vinyl aromatic copolymer having a structural unit derived from a divinyl aromatic compound and a structural unit derived from a monovinyl aromatic compound, wherein the m-form ratio of the divinyl aromatic compound is 60 mol% or more, and the polydispersity (Mw / Mn) of the molecular weight distribution, which is expressed as the ratio of the weight average molecular weight to the number average molecular weight of the polyfunctional vinyl aromatic copolymer, is more than 2.5 and 100 or less. [2] 2. The multifunctional vinyl aromatic copolymer according to item 1, wherein the molecular weight distribution is multimodal. [3] 3. The polyfunctional vinyl aromatic copolymer according to item 1 or 2, further comprising 1 to 99 mol % of structural units derived from alkylstyrene having an alkylstyrene having a carbon chain length of 3 to 20, relative to 100 mol % in total of all structural units. [4] 4. The polyfunctional vinyl aromatic copolymer according to item 3, wherein the alkylstyrene is an alkylstyrene having a carbon chain length of 6 to 10. [5] 5. The multifunctional vinyl aromatic copolymer according to item 4, wherein the alkylstyrene is 4-n-octylstyrene. [6] The polyfunctional vinyl aromatic copolymer according to any one of items 1 to 5, one or more selected from the group consisting of a curable reactive compound, a curable reactive resin, a thermoplastic resin, and a radical polymerization initiator; A curable resin composition comprising: [7] 7. The curable resin composition according to item 6, comprising a curable reactive compound, wherein the curable reactive compound is a trialkenyl isocyanurate and / or a trialkenyl cyanurate. [8] 8. The curable resin composition according to item 6 or 7, comprising a curable reactive resin, the curable reactive resin being polyphenylene ether. [9] 9. The curable resin composition according to any one of items 6 to 8, further comprising a flame retardant and / or a filler.
[10] A cured product obtained by curing the curable resin composition according to any one of items 6 to 9.
[11] A curable composite material comprising the curable resin composition according to any one of items 6 to 9 and a substrate, wherein the substrate constitutes 1% by mass to 99% by mass based on the total mass of the curable composite material.
[12] Item 12. A cured composite material obtained by curing the curable composite material according to item 11.
[13] 13. A laminate comprising a plurality of layers of the cured composite material of claim 12.
[14] 12. A metal-clad laminate having a layer of the curable composite material according to item 11 and a metal foil layer.
[15] A resin-coated metal foil comprising a metal foil and a film formed on one side of the metal foil by curing the curable resin composition according to any one of items 6 to 9.
[16] A resin composition varnish comprising an organic solvent and the curable resin composition according to any one of items 6 to 9 dissolved in the organic solvent. Effect of the Invention
[0009] According to the present disclosure, it is possible to provide a polyfunctional vinyl aromatic copolymer that can provide a laminate or the like having excellent processability, and a curable resin composition containing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present disclosure will be described. The following embodiment is one aspect of the present disclosure, and therefore the present disclosure is not limited to the following embodiment. Therefore, the following embodiment can be appropriately modified and implemented within the scope of the gist of the present disclosure. In addition, in this disclosure, "to" in a numerical range means that the numerical values at both ends are included as the upper limit and lower limit unless otherwise specified. In this disclosure, the upper limit and lower limit of a numerical range can be arbitrarily combined.
[0011] [Multifunctional vinyl aromatic copolymer] The polyfunctional vinyl aromatic copolymer of the present disclosure has a structural unit (a) derived from a divinylaromatic compound and a structural unit (b) derived from a monovinyl aromatic compound. Of the structural units (a) derived from the divinylaromatic compound, 60 mol% or more are m-configuration. The "m-configuration" refers to a structural unit derived from a divinylaromatic compound in which two vinyl groups are coordinated to each other at the m-position (meta position). The polyfunctional vinyl aromatic copolymer has a molecular weight distribution dispersity (Mw / Mn) of more than 2.5 and 100 or less, which is expressed as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn).
[0012] Without being limited by theory, the soluble polyfunctional vinyl aromatic copolymer of the present disclosure has an m-body ratio of the structural unit (a) derived from the above-mentioned divinyl aromatic compound of 60 mol% or more, thereby suppressing a side reaction in which the growing end reacts with the vinyl group of the structural unit (a) derived from the divinyl aromatic compound during polymerization to form a local crosslinked structure, and a polyfunctional vinyl aromatic copolymer that does not have a microgel structure and is soluble in an organic solvent is obtained. During polymerization, the growing end tends to gradually react with the vinyl group of the structural unit (a) to obtain a multi-peaked polyfunctional vinyl aromatic copolymer, but the resulting polyfunctional vinyl copolymer has a branched structure that does not become a microgel, and Mw / Mn is adjusted to be more than 2.5 and 100 or less. By adjusting Mw / Mn to be more than 2.5 and 100 or less, microscopic sparseness and denseness occur in the degree of crosslinking during curing, and multiple microcracks can occur from the sparse parts when cutting or drilling. Therefore, minute cracks are connected according to the shape of the cutting blade or the punching circular blade, so that burrs are less generated and the processability during drilling is good. In addition, when curing, the m-body ratio in the structural unit (a) derived from the divinyl aromatic compound is 60 mol% or more, so that one vinyl group of the divinyl aromatic compound can be suppressed from being used for crosslinking during polymerization and can remain until curing. As a result, in a preferred embodiment, when the amount of radical polymerization initiator added is the same, three-dimensional crosslinking progresses during curing, so that the glass transition temperature tends to improve and the solder heat resistance tends to improve. Furthermore, since many vinyl groups remain until curing, the amount of radical polymerization initiator added can be reduced, and as a result, in a preferred embodiment, the dielectric loss tangent tends to be reduced. Therefore, the polyfunctional vinyl aromatic copolymer in the preferred embodiment can provide a laminate, etc., which is excellent in processability when producing a prepreg, which is the raw material of the laminate, and has excellent dielectric properties and heat resistance.
[0013] The structure of the structural unit (a) is not particularly limited as long as it is derived from a divinyl aromatic compound, but it preferably contains a structure represented by the following chemical formula (1). [ka] (In the formula, R 1 represents an aromatic hydrocarbon group having 6 to 30 carbon atoms, and n represents an integer of 1 or more.
[0014] The structure of the structural unit (a) may include, for example, a structure represented by the following chemical formula (1') in which two vinyl groups derived from a divinyl aromatic compound are both reacted. [ka] (In the formula, R 1 represents an aromatic hydrocarbon group having 6 to 30 carbon atoms, and n represents an integer of 1 or more.
[0015] In the general formulas (1) and (1′), R 1 are each independently a divalent aromatic hydrocarbon group having preferably 6 to 30 carbon atoms, such as a phenylene group, a naphthylene group, a divalent biphenyl group, structural isomers thereof, and combinations thereof, and from the viewpoint of solubility, a phenylene group is preferable. Each n is independently an integer of 1 or more, and the upper limit of n is not limited, but may be, for example, 100 or less.
[0016] The structure of the structural unit (b) is not particularly limited as long as it is derived from a monovinyl aromatic compound (excluding those corresponding to the "alkylstyrene having an alkyl group having 3 to 20 carbon atoms" of the structural unit (c)). However, it is preferable that the structure of the structural unit (b) includes a structure represented by the following chemical formula (2). [ka] (In the formula, R 2 represents an aromatic hydrocarbon group having 6 to 30 carbon atoms, and n represents an integer of 1 or more.
[0017] In general formula (2), R 2is preferably a monovalent aromatic hydrocarbon group having 6 to 30 carbon atoms, such as a phenyl group, a naphthyl group, a monovalent biphenyl group, structural isomers thereof, and combinations thereof, and from the viewpoint of solubility, a phenyl group is preferred. n is an integer of 1 or more, and the upper limit of n is not limited, but may be, for example, 100 or less. In the polyfunctional vinyl aromatic copolymer, the structural unit (a) and the structural unit (b) may be arranged alternately, randomly, in a block or graft form, or in a combination thereof.
[0018] The polyfunctional vinyl aromatic copolymer of the present disclosure may further contain 1 mol% to 99 mol% of structural units (c) derived from an alkylstyrene having an alkyl group having 3 to 20 carbon atoms, relative to the total of all structural units being 100 mol%. The alkyl group having 3 to 20 carbon atoms may be a linear or branched alkyl group, and is preferably a linear alkyl group. From the viewpoint of both improving heat resistance and strength and ease of handling, the number of carbon atoms is preferably 6 to 10, and more preferably 6 to 8. More specifically, examples of the alkyl group include a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, and structural isomers thereof. From the viewpoint of availability, 4-n-octylstyrene having 8 carbon atoms is particularly preferred. The polyfunctional vinyl aromatic copolymer can provide a laminate having higher heat resistance and strength by having structural units derived from these alkylstyrenes. When the carbon number of the alkyl group is 3 or more, the dielectric tangent can be further reduced, and when the carbon number is 20 or less, the compatibility with the main material, crosslinking agent, etc. is excellent, so that the solder heat resistance is improved and burrs are not generated when cutting, and there is a tendency for the processability when drilling to be excellent.
[0019] The content of the structural units derived from alkylstyrene is preferably 1 mol% to 99 mol%, more preferably 5 mol% to 99 mol%, and further preferably 10 mol% to 99 mol%, based on the total of all structural units (100 mol%). By having the structural units derived from alkylstyrene in this content range, the polyfunctional vinyl aromatic copolymer can provide a laminate or the like having higher heat resistance and strength.
[0020] The vinyl group of the structural unit (a) derived from the divinyl aromatic compound acts as a cross-linking component and contributes to improving the heat resistance of the polyfunctional vinyl aromatic copolymer. On the other hand, the structural unit derived from the monovinyl aromatic compound (b) does not act as a cross-linking component because it does not have a vinyl group, but contributes to improving the compatibility with curable resins such as modified PPE, improving the solubility in varnish solvents, and improving the moldability of prepregs, laminates, etc.
[0021] In the structural unit (a) derived from a divinylaromatic compound, the term "m-form" refers to a structural unit derived from a divinylaromatic compound in which two vinyl groups are in the m-position (meta position) relative to each other. That is, in the general formula (1), R 1 This refers to a structural isomer in which the bond to the main chain of the R group and the vinyl group are in the m-position (meta position) relative to each other. In general formula (1'), R 1 It refers to a structural isomer in which the bond to the main chain of the vinyl group and the ethylene group derived from the vinyl group are in the m-position. The ratio of the m-structural isomer in the structural unit (a) (hereinafter referred to as the m-form ratio) is 60 mol% or more, that is, 60 mol% to 100 mol%, preferably 65 mol% to 100 mol%, and more preferably 70 mol% to 100 mol%. This further improves the dielectric properties, heat resistance, appearance, and interlayer peel strength. The m-form ratio in the structural unit (a) derived from a divinylaromatic compound is due to the ratio of the m-form contained in the divinylaromatic compound used as a monomer during polymerization. In other words, in order to synthesize a multifunctional vinyl copolymer having the structural unit (a) derived from a divinylaromatic compound with the above m-form ratio, a divinylaromatic compound monomer with an m-form ratio of preferably 60 mol% to 100 mol%, more preferably 65 mol% to 100 mol%, and even more preferably 70 mol% to 100 mol% is used.
[0022] The structural unit (a) derived from a divinyl aromatic compound can be a plurality of structures, such as a structure in which only one vinyl group represented by general formula (1) has reacted, or a structure in which two vinyl groups represented by general formula (1') have reacted. Of these, the amount of the repeating unit in which only one vinyl group represented by general formula (1) has reacted is preferably 1 mol% to 95 mol%, more preferably 5 mol% to 50 mol%, even more preferably 5 mol% to 40 mol%, and even more preferably 5 mol% to 35 mol% based on the total of the structural units (a), (b), and (c) if included. By being in this range, a side reaction in which the growing end reacts with the vinyl group of the structural unit (a) derived from the divinyl aromatic compound during polymerization to form a crosslinked structure is suppressed, and a polyfunctional vinyl copolymer with a sharp molecular weight distribution and few crosslinked structures can be obtained. In addition, the amount of vinyl groups remaining without being used for crosslinking during curing can be reduced, so that the dielectric loss tangent can be further reduced.
[0023] The amount of the structural unit (b) derived from the monovinyl aromatic compound is preferably 5 mol% to 99 mol%, more preferably 50 mol% to 95 mol%, even more preferably 60 mol% to 95 mol%, and even more preferably 65 mol% to 95 mol% based on the total amount of the structural units (a), (b), and (c) if contained. By being in this range, a polyfunctional vinyl aromatic copolymer having excellent compatibility with curable resins such as modified PPE, solubility in varnish solvents, and moldability of prepregs and laminates is obtained.
[0024] The structural unit (a) derived from a divinyl aromatic compound and the structural unit (b) derived from a monovinyl aromatic compound may each contain one type or a combination of multiple types. Examples of divinyl aromatic compounds are not limited as long as they are aromatic compounds having two vinyl groups, but preferably, divinylbenzene, divinylnaphthalene, divinylbiphenyl, structural isomers thereof, and mixtures thereof are used, and divinylbenzene is more preferable from the viewpoint of solubility. Examples of monovinyl aromatic compounds are not limited as long as they are aromatic compounds having one vinyl group, but for example, vinyl aromatic compounds such as styrene, vinylnaphthalene, and vinylbiphenyl; alkyl-substituted vinyl aromatic compounds such as o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, o-ethylvinylbenzene, m-ethylvinylbenzene, and p-ethylvinylbenzene; and the like. Styrene and ethylvinylbenzene (including each positional isomer or a mixture thereof) are preferable because they prevent gelation of the polyfunctional vinyl aromatic copolymer, have a high effect of improving solvent solubility and processability, are low in cost, and are easily available. The monovinyl aromatic compound does not have to contain styrene.
[0025] As long as the effects of the present disclosure are not impaired, the polyfunctional vinyl aromatic copolymer may have structural units derived from other monomer components, such as a trivinyl aromatic compound, a trivinyl aliphatic compound, a divinyl aliphatic compound, or a monovinyl aliphatic compound, in addition to the divinyl aromatic compound and the monovinyl aromatic compound.
[0026] The number average molecular weight of the polyfunctional vinyl aromatic copolymer (Mn: number average molecular weight in terms of standard polystyrene measured using gel permeation chromatography) is preferably 500 to 1000,000, more preferably 1000 to 500,000, and even more preferably 1000 to 30,000. When Mn is 500 or more, the molecular weight is sufficiently high and the strength of the cured product tends to be increased, and when Mn is 1000,000 or less, the moldability tends to be good. In addition, the value of the dispersity of the molecular weight distribution (Mw / Mn) represented by the ratio of the weight average molecular weight (Mw: weight average molecular weight in terms of standard polystyrene measured using gel permeation chromatography) to Mn is more than 2.5 and not more than 100, preferably more than 3.0 and not more than 80.0, more preferably more than 3.0 and not more than 50.0, and particularly preferably more than 3.0 and not more than 25.0. When Mw / Mn exceeds 2.5, the molecular weight distribution tends to show a multi-modality of two or more peaks, resulting in a broad molecular weight distribution on the high molecular weight side. This suggests the formation of a branched structure during polymerization, which means that polyfunctional vinyl aromatic copolymers with various molecular sizes are being produced, which contributes to the occurrence of microscopic variations in the degree of crosslinking during curing. As a result, multiple microcracks can occur from the sparse areas when cutting or drilling. For this reason, the microcracks connect to fit the shape of the cutting blade or the circular punching blade, resulting in less burrs and better processability when drilling holes.
[0027] [Method of producing polyfunctional vinyl aromatic copolymer] The method for producing the soluble polyfunctional vinyl aromatic copolymer of the present disclosure includes a method for producing a polyfunctional vinyl aromatic copolymer by polymerizing monomers such as a divinyl aromatic compound and a monovinyl aromatic compound in the presence of a catalyst and a cocatalyst. More specifically, a method is preferred in which the divinyl aromatic compound is used in an amount of 1 mol% or more and less than 95 mol%, and the monovinyl aromatic compound is used in an amount of 5 mol% or more and less than 99 mol%, relative to the total amount of the monomers, and polymerization is carried out at a temperature of -78°C to 120°C. Here, a Lewis acid catalyst can be preferably used as the catalyst, and a Lewis base compound can be preferably used as the additive base of the cocatalyst. In addition, it is preferable to use equipment used for polymerization that is dried at 130°C for 2 hours or more immediately before use, and cooled under a nitrogen atmosphere immediately after being taken out of a dryer or the like to remove moisture from the surface appropriately.
[0028] As the catalyst, an initiator generally used in cationic polymerization or living cationic polymerization is selected, and a Lewis acid catalyst is preferably selected from the viewpoint of ease of polymerization control. The Lewis acid catalyst is a compound consisting of a metal ion (acid) and a ligand (base), and can be used without any particular limitation as long as it can accept an electron pair. Among them, from the viewpoint of thermal decomposition resistance of the obtained polyfunctional vinyl aromatic copolymer, a metal fluoride or a complex thereof is preferred, and in particular, a divalent to hexavalent metal fluoride or a complex thereof such as B, Al, Ga, In, Si, Ge, Sn, Pb, Sb, Bi, Ti, W, Zn, Fe, and V is preferred. These catalysts can be used alone or in combination of two or more kinds. From the viewpoint of control of the molecular weight and molecular weight distribution of the obtained polyfunctional vinyl aromatic copolymer and polymerization activity, an ether complex of boron trifluoride is most preferably used. Here, examples of the ether complex include diethyl ether, dimethyl ether, and dibutyl ether. Boron trifluoride diethyl ether complex is particularly preferred because it is easily available and inexpensive.
[0029] The catalyst is preferably used in a molar ratio of 0.0001 to 10 relative to the total amount of monomers, more preferably 0.001 to 1, and even more preferably 0.001 to 0.1. If the molar ratio is 10 or less, the polymerization rate does not become too high, and polymerization control such as molecular weight distribution becomes easy. On the other hand, if it is 0.0001 or more, a sufficient polymerization rate is ensured, the time required for polymerization is reduced, which leads to cost reduction and is preferable for industrial implementation.
[0030] In the method for producing a polyfunctional vinyl aromatic copolymer of the present disclosure, various reagents can be added as co-catalysts. For example, one or more Lewis base compounds are used as the added base. Examples of Lewis base compounds include monoester compounds, diester compounds, thioester compounds, thioether compounds, ketone compounds, ether compounds, and phosphine compounds. An appropriate Lewis base compound is selected depending on the initiator (catalyst) used in the polymerization, and when a boron trifluoride diethyl ether complex is used as the catalyst, for example, a monoester compound or a diester compound is preferably used. Specific examples include acetates such as butyl acetate, and diesters such as dimethyl adipate and diethyl malonate. The Lewis base compounds can be used alone or in combination of two or more.
[0031] During polymerization, Lewis base compounds coordinate with the Lewis acid catalyst, which is a counter anion, to control the interaction between the carbocation, which is an active species, and the counter anion, thereby adjusting the relative reaction frequency between the monomer, which also acts as a chain transfer agent. In general, by adding a Lewis base compound, the carbocation end, which is an active species, interacts with the Lewis base compound, so that side reactions such as the carbocation end acting on other molecular chains can be controlled, and the molecular weight distribution can be controlled.
[0032] The Lewis base compound is added in a molar ratio relative to the amount of the catalyst of preferably 0.1 to 100, more preferably 1 to 100, and particularly preferably 5 to 50. Within the above range, the polymerization rate can be appropriately maintained, while the above-mentioned side reactions can be controlled, and a polyfunctional vinyl aromatic copolymer having a desired Mw / Mn can be obtained.
[0033] A solvent can be added to the polymerization as desired. The solvent is a compound that does not inhibit the polymerization and dissolves the catalyst, cocatalyst, and monomer components to form a homogeneous solution. Specifically, from the viewpoint of the balance between polymerization activity and solubility, toluene, xylene, n-hexane, cyclohexane, methylcyclohexane or ethylcyclohexane, and acetonitrile are particularly preferred. In addition, the amount of the solvent used is preferably determined so that the monomer components in the polymerization solution are 1 vol% to 90 vol%, preferably 1 vol% to 80 vol%, and particularly preferably 1 vol% to 60 vol%, taking into consideration the viscosity of the resulting polymerization solution and the ease of heat removal. If this concentration is 1 vol% or more, sufficient polymerization efficiency is ensured, leading to cost reduction, and if it is 90 vol% or less, the heat generated by polymerization is efficiently removed, leading to stabilization of the quality of the polyfunctional vinyl aromatic copolymer.
[0034] When producing a polyfunctional vinyl aromatic copolymer, it is necessary to polymerize the polymerization solution at a temperature of -78°C to 120°C. The polymerization temperature is selected depending on the catalyst and solvent used, but from the viewpoint of industrial feasibility, it is preferably -20°C to 120°C, more preferably 30°C to 120°C, and particularly preferably 40°C to 120°C. If the polymerization temperature is 120°C or less, the selectivity of the reaction is improved, making it possible to control the molecular weight distribution more, and stable production can be achieved. If it is -78°C or more, sufficient catalytic activity can be ensured and polymerization efficiency can be improved.
[0035] In order to obtain a polymer having a Mw / Mn ratio of more than 2.5 and not more than 100, it is preferable to stir gently, for example at 1000 rpm or less. Stirring is more preferably at 500 rpm or less, more preferably at 300 rpm or less. Stirring at 1000 rpm or less tends to cause non-uniformity in the system, resulting in a polymer with a high Mw / Mn. There is no particular lower limit, but it is sufficient to stir at 1 rpm or more from the viewpoint of removing heat from the polymerization reaction.
[0036] The polymerization terminator used in the polymerization termination reaction is not particularly limited as long as it is a substance that deactivates the acid catalyst or the growing carbocation. For example, aqueous solutions such as sodium bicarbonate aqueous solution, sodium carbonate aqueous solution, sodium hydroxide aqueous solution, and ammonia aqueous solution, and ammoniacal alcohols such as ammoniacal methanol and ammoniacal ethanol, etc. It is preferable to degas the polymerization terminator with an inert gas in order to suppress side reactions with dissolved oxygen and dissolved carbon dioxide.
[0037] After the polymerization reaction is stopped, the method for recovering the polyfunctional vinyl aromatic copolymer is not particularly limited, and may be, for example, a commonly used method such as a heating concentration method, a steam stripping method, or precipitation in a poor solvent. From the viewpoint of removing the compounds used in polymerization and recovery from the copolymer, such as catalysts, cocatalysts, and solvents, and reducing the remaining amount, a method of repeating precipitation in a poor solvent multiple times is preferable. In addition, in the case of a polymer with a large Mw / Mn, it may become a lump, so it is preferable to use it in the form of powder by pulverizing it by a mechanical pulverization method from the viewpoint of solubility when preparing a varnish.
[0038] [Curable resin composition] The curable resin composition of the present disclosure contains a polyfunctional vinyl aromatic copolymer and at least one selected from the group consisting of a curable reactive compound, a curable reactive resin, a thermoplastic resin, and a radical polymerization initiator. If desired, it may further contain an initiator such as a radical polymerization initiator, a flame retardant, a silica filler, and a solvent. Hereinafter, the elements that can constitute the curable resin composition will be described.
[0039] In the present disclosure, the term "curable reactive compound" refers to a low molecular weight compound that functions as a crosslinking agent when curing a curable resin composition, specifically a compound with a molecular weight of less than 300. As the curable reactive compound, trialkenyl isocyanurate and / or trialkenyl cyanurate (hereinafter abbreviated as "trialkenyl isocyanurate / cyanurate") is preferred from the viewpoint of ease of handling since it is liquid at room temperature. As the trialkenyl isocyanurate compound, triallyl isocyanurate (TAIC) and the like, and as the trialkenyl cyanurate compound, triallyl cyanurate (TAC) and the like are more preferred because they further improve the compatibility of the polyfunctional vinyl aromatic copolymer with either the curable reactive resin or the thermoplastic resin, and further improve the heat resistance and interlayer peel strength of the laminate.
[0040] The amount of trialkenyl isocyanurate / cyanurate in the curable resin composition is preferably 2% by mass to 20% by mass based on the total weight of components other than the solvent. From the viewpoint of compatibility with other components, or from the viewpoint of reducing the dielectric loss tangent, improving the heat resistance, and providing a good appearance of a molded product of the resin composition, a prepreg containing the resin composition, a laminate of multiple prepregs, a laminate of a prepreg and a substrate, etc., the amount of trialkenyl isocyanurate / cyanurate is more preferably 2% by mass to 15% by mass, and even more preferably 3% by mass to 10% by mass.
[0041] In addition to trialkenyl isocyanurate / cyanurate, a general crosslinking agent may be added to the curable reactive compound within a range that does not impair the properties. Examples of such a crosslinking agent include a polyfunctional methacrylate compound having two or more methacrylic groups in the molecule, a polyfunctional acrylate compound having two or more acrylic groups in the molecule, a polyfunctional vinyl compound having two or more vinyl groups in the molecule, such as polybutadiene, a vinylbenzyl compound such as divinylbenzene having a vinylbenzyl group in the molecule (excluding the addition as a copolymerizable monomer in the above component (b)), and a polyfunctional maleimide compound having two or more maleimide groups in the molecule, such as 4,4'-bismaleimide diphenylmethane.
[0042] In the present disclosure, the term "curable reactive resin" refers to a polymeric material other than a polyfunctional vinyl aromatic copolymer that can function as a crosslinking agent when curing a curable resin composition, specifically a compound having a molecular weight of 300 or more. As the curable reactive resin, polyphenylene ether (hereinafter abbreviated as "PPE") is preferable in terms of low dielectric properties and heat resistance. PPE contains phenylene ether units as repeating structural units. The phenylene group in the phenylene ether unit may or may not have a substituent. In the present disclosure, the PPE as the curable reactive resin includes dimers, trimers, oligomers, and polymers. The curable reactive resin may be blended as a main material of the curable resin composition, thereby making it possible to obtain a cured product having excellent strength. "Blended as a main material" means that it occupies the largest mass % of the components contained in the curable resin composition.
[0043] The PPE may also contain other structural units other than the phenylene ether unit. The amount of the other structural units is typically 30 mol% or less, 25 mol% or less, 20 mol% or less, 15 mol% or less, 10 mol% or less, or 5 mol% or less based on the number of all unit structures. However, within a range that does not impair the effects of the present disclosure, the amount of the other structural units may exceed 30 mol% based on the number of all unit structures.
[0044] Specific examples of PPE include poly(2,6-dimethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), poly(2,6-dichloro-1,4-phenylene ether), copolymers of 2,6-dimethylphenol and other phenols (e.g., 2,3,6-trimethylphenol, 2-methyl-6-butylphenol, etc.), PPE copolymers obtained by coupling 2,6-dimethylphenol with biphenols or bisphenols, and PPEs having a linear or branched structure obtained by heating poly(2,6-dimethyl-1,4-phenylene ether) or the like with a phenolic compound such as bisphenols or trisphenols in a toluene solvent in the presence of a radical polymerization initiator and redistribution reaction.Furthermore, PPEs in which the terminal hydroxyl groups of these PPEs have been chemically converted to functional groups containing carbon-carbon double bonds can also be mentioned. Specific examples of functional groups having a carbon-carbon double bond include vinyl groups, allyl groups, isopropenyl groups, 1-butenyl groups, 1-pentenyl groups, p-vinylphenyl groups, p-isopropenylphenyl groups, m-vinylphenyl groups, m-isopropenylphenyl groups, o-vinylphenyl groups, o-isopropenylphenyl groups, p-vinylbenzyl groups, p-isopropenylbenzyl groups, m-vinylbenzyl groups, m-isopropenylbenzyl groups, o-vinylbenzyl groups, o-isopropenylbenzyl groups, p-vinylphenylethenyl groups, p-vinylphenylpropenyl groups, p-vinylphenylbutenyl groups, m-vinylphenylethenyl groups, m-vinylphenylpropenyl groups, m-vinylphenylbutenyl groups, o-vinylphenylethenyl groups, o-vinylphenylpropenyl groups, o-vinylphenylbutenyl groups, methacryl groups, acrylic groups, 2-ethylacrylic groups, and 2-hydroxymethylacrylic groups.
[0045] The number average molecular weight of the PPE is preferably 1,000 to 5,000. When the resin composition contains such a low molecular weight PPE, the viscosity increase of the resin composition varnish can be suppressed, and the coatability of the resin composition varnish to a substrate can be improved. By improving the coatability, various properties required for the resin composition or its cured product can also be improved. The number average molecular weight of the low molecular weight PPE is preferably 1,000 to 4,000, or 1,500 to 3,000.
[0046] The curable reactive resin may contain one type of PPE or a combination of two or more types of PPE having a number average molecular weight of 1,000 to 5,000.
[0047] The amount of PPE in the curable resin composition is 50% by mass to 90% by mass based on the total weight of the components other than the solvent. From the viewpoint of compatibility with other components, or from the viewpoint of reducing the dielectric tangent, improving the heat resistance, and improving the appearance of the cured product of the curable resin composition, the prepreg, the laminate of multiple prepregs, the laminate of the prepreg and the substrate, etc., the amount of PPE is preferably 50% by mass to 80% by mass, and more preferably 50% by mass to 70% by mass.
[0048] Examples of the radical polymerization initiator include peroxides such as benzoyl peroxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, di-t-butyl peroxide, t-butylcumyl peroxide, di(2-t-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, dicumyl peroxide, di-t-butylperoxyisophthalate, t-butylperoxybenzoate, 2,2-bis(t-butylperoxy)butane, 2,2-bis(t-butylperoxy)octane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, di(trimethylsilyl)peroxide, and trimethylsilyltriphenylsilyl peroxide. In addition, radical generators such as 2,3-dimethyl-2,3-diphenylbutane can also be used as reaction initiators for the resin composition. Among them, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, di(2-t-butylperoxyisopropyl)benzene, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane are preferred from the viewpoint of providing a cured product having excellent heat resistance and mechanical properties, as well as a low dielectric constant and a low dielectric loss tangent.
[0049] The one-minute half-life temperature of the radical polymerization initiator is preferably 155°C to 185°C, or 160°C to 180°C, or 165°C to 175°C. In the present disclosure, the one-minute half-life temperature is the temperature at which the radical polymerization initiator decomposes and the amount of active oxygen is reduced to half in one minute. The one-minute half-life temperature is a value confirmed by a method in which the radical polymerization initiator is dissolved in a solvent inactive to radicals, such as benzene, to a concentration of 0.05 mol / L to 0.1 mol / L, and the radical polymerization initiator solution is thermally decomposed under a nitrogen atmosphere.
[0050] By having a 1-minute half-life temperature of the radical polymerization initiator of 155°C or higher, when the resin composition is subjected to heat and pressure molding, the reaction with the crosslinking agent can be initiated after the PPE has been sufficiently melted, which tends to result in excellent moldability. On the other hand, by having a 1-minute half-life temperature of the radical polymerization initiator of 185°C or lower, the decomposition speed of the radical polymerization initiator is sufficient under normal heat and pressure molding conditions (for example, a maximum temperature of 200°C), so that the crosslinking reaction with the crosslinking agent can proceed efficiently and slowly, making it possible to form a cured product with good electrical properties (especially dielectric tangent).
[0051] Examples of radical polymerization initiators having a one-minute half-life temperature in the range of 155°C to 185°C include t-hexylperoxyisopropyl monocarbonate (155.0°C) (the one-minute half-life temperature is in parentheses, the same applies below), t-butylperoxy-3,5,5-trimethylhexanoate (166.0°C), t-butylperoxylaurate (159.4°C), t-butylperoxyisopropyl monocarbonate (158.8°C), t-butylperoxy2-ethylhexyl monocarbonate (161.4°C), t-hexylperoxybenzoate (160.3°C), 2,5-dimethyl-2,5-di(benzoylperoxy) )hexane (158.2°C), t-butyl peroxyacetate (159.9°C), 2,2-di-(t-butylperoxy)butane (159.9°C), t-butyl peroxybenzoate (166.8°C), n-butyl 4,4-di-(t-butylperoxy)valerate (172.5°C), di(2-t-butylperoxyisopropyl)benzene (175.4°C), dicumyl peroxide (175.2°C), di-t-hexyl peroxide (176.7°C), 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (179.8°C), and t-butylcumyl peroxide (173.3°C).
[0052] The content of the radical polymerization initiator, based on the total mass of the curable resin composition (100 mass%), is preferably 0.05 mass% or more, more preferably 0.1 mass% or more, even more preferably 0.3 mass% or more, and still more preferably 0.5 mass% or more, from the viewpoint of being able to increase the reaction rate, and is preferably 3 mass% or less, more preferably 2 mass% or less, and still more preferably 1 mass% or less, from the viewpoint of being able to keep the dielectric constant and dielectric tangent of the obtained cured product low.
[0053] The curable resin composition preferably contains a flame retardant. Examples of the flame retardant include inorganic flame retardants such as antimony trioxide, aluminum hydroxide, magnesium hydroxide, and zinc borate; aromatic bromine compounds such as hexabromobenzene, decabromodiphenylethane, 4,4-dibromobiphenyl, and ethylene bistetrabromophthalimide; and phosphorus-based flame retardants such as resorcinol bis-diphenyl phosphate and resorcinol bis-dixylenyl phosphate. These flame retardants are used alone or in combination of two or more. Among these, the flame retardant is preferably decabromodiphenylethane from the viewpoint of providing a low dielectric constant and a low dielectric loss tangent when the curable resin composition is cured.
[0054] The content of the flame retardant is not particularly limited, but from the viewpoint of maintaining flame retardancy at the UL standard 94V-0 level, it is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, relative to 100 parts by mass of the total curable resin composition. Also, from the viewpoint of maintaining low dielectric constant and dielectric loss tangent of the obtained cured product, the content of the flame retardant is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 40 parts by mass or less.
[0055] The curable resin composition may contain a filler. The filler may contain a silica filler. As the silica filler, either natural silica or synthetic silica may be used, and examples thereof include fused silica, amorphous silica, aerosil, and hollow silica. The content of the silica filler may be 10 to 100 parts by mass relative to a total of 100 parts by mass of the PPE and all components usable as a crosslinking agent. In addition, the silica filler may be surface-treated using a silane coupling agent or the like.
[0056] In addition to the above components, the curable resin composition may further contain additives such as a heat stabilizer, an antioxidant, a UV absorber, a surfactant, and a lubricant.
[0057] [Resin composition varnish] The resin composition varnish of the present disclosure contains an organic solvent and the curable resin composition of the present disclosure dissolved in the organic solvent. The resin composition varnish can have a suitable fluidity when impregnated into a glass cloth. In the manufacturing process of the prepreg, it is preferable to dry and remove the solvent using a hot air dryer or the like after impregnating the glass cloth with the resin composition varnish. The solid components in the resin composition varnish may be dissolved or dispersed in the varnish. The amount of the solvent may be appropriately adjusted so that the fluidity of the resin composition varnish is in a suitable range, and for example, the amount of the solvent in the resin composition varnish may be 20% by mass to 80% by mass, or 30% by mass to 70% by mass, or 40% by mass to 60% by mass.
[0058] From the viewpoint of the solubility of the components in the resin composition, the solvent is preferably an aromatic compound such as toluene or xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, or chloroform. These solvents may be used alone or in combination of two or more.
[0059] From the viewpoint of easily ensuring suitable fluidity of the resin composition varnish even at about room temperature, the solvent is preferably an aromatic compound such as toluene, for example, a toluene-methyl ethyl ketone mixed solvent, a toluene-cyclohexanone mixed solvent, a toluene-cyclopentanone mixed solvent, etc. Furthermore, since the resin composition of the present disclosure dissolves suitably in even a solvent containing toluene alone, and thus has excellent impregnation properties into the substrate, a solvent containing toluene alone is also preferred.
[0060] [Uncured product] (Curable composite material) The curable composite material (also referred to as "prepreg") of the present disclosure includes a curable resin composition and a substrate, and the substrate constitutes 1 mass % to 99 mass % based on the total mass of the curable composite material. Examples of the substrate include glass cloth formed from E-glass fiber, L-glass fiber, S-glass fiber, etc., and organic fiber cloth formed from aramid resin fiber, etc. Examples of methods for producing the curable composite material include a method in which a substrate is impregnated with the above-mentioned resin composition varnish of the present disclosure, and the solvent is dried and removed.
[0061] (Metal-clad laminate) The metal-clad laminate of the present disclosure has a layer of the curable composite material of the present disclosure (uncured) and a metal foil layer. The metal-clad laminate of the present disclosure can be manufactured by laminating the layer of the curable composite material of the present disclosure and the metal foil layer. The curable composite material to be combined with the metal foil may be one or more sheets, and the metal foil may be laminated on one or both sides of the curable composite material depending on the application to process it into a metal-clad laminate.
[0062] [Cured product] According to the present disclosure, there is also provided a cured product obtained by curing the curable resin composition of the present disclosure. The cured product of the present disclosure has excellent processability, and in a preferred embodiment, has excellent dielectric properties and heat resistance.
[0063] (cured composite material) The cured product may be a cured composite material obtained by curing the curable composite material (prepreg) of the present disclosure described above. Curing can be carried out by heating at the curing temperature of the resin composition for a predetermined period of time.
[0064] (Laminate) A laminate (laminate) can be provided by stacking a plurality of curable composite materials (prepregs) and curing the laminate. More specifically, a laminate having a plurality of layers of the cured composite material of the present disclosure can be provided by stacking a plurality of curable composite materials (prepregs) and curing the laminate.
[0065] (hardened metal clad laminate) The curable composite material (prepreg) may be laminated with other layers as desired and cured. More specifically, a cured metal-clad laminate having a layer of the curable composite material of the present disclosure and a metal foil layer and a metal-clad laminate is cured to provide a cured metal-clad laminate having a layer of the curable composite material of the present disclosure and a metal foil layer. The dielectric tangent of the cured metal-clad laminate is preferably less than 0.0027, more preferably 0.0026 or less, when measured at 10 GHz by the method described in the Examples. The cured metal-clad laminate preferably has a form in which a layer of the cured product (cured composite material) of the curable composite material (prepreg) and a metal foil layer are laminated and adhered to each other, and is preferably used as a material for electronic circuit boards. Examples of metal foils include aluminum foil and copper foil, and among these, copper foil is preferred because it has low electrical resistance. One particularly preferred application of the cured metal-clad laminate is a printed wiring board. It is preferable that at least a part of the metal foil is removed from the cured metal-clad laminate in the printed wiring board.
[0066] (Printed Wiring Board) The printed wiring board is a metal-clad laminate from which a portion of the metal foil has been removed. The printed wiring board can typically be formed by a method of pressurizing and heating the curable composite material (prepreg) of the present disclosure. The printed wiring board is excellent in processability by being manufactured from the curable composite material (prepreg) of the present disclosure, and in a preferred embodiment, has excellent heat resistance and electrical properties (low dielectric constant and low dielectric loss tangent).
[0067] (Metal foil with resin) Another example of the cured product is a metal foil with a resin. The metal foil with a resin has a metal foil and a film obtained by curing the curable resin composition of the present disclosure on at least one side or both sides of the metal foil. Examples of the metal foil include aluminum foil and copper foil, and among these, copper foil is preferred because it has low electrical resistance. It can be produced by vacuum pressing the film before curing and the metal foil together. EXAMPLES
[0068] Examples of the present disclosure are given below. However, the present disclosure is not limited to the examples.
[0069] [Method of synthesizing divinylbenzene] m-Divinylbenzene was synthesized with reference to Non-Patent Document 1, and p-Divinylbenzene was synthesized with reference to Non-Patent Document 2, respectively.
[0070] [Synthesis of multifunctional vinyl aromatic copolymers] Example 1 3 moles (390 g) of divinylbenzene with a structural isomer ratio of m-isomer of 60%, 7 moles of styrene (Tokyo Chemical Industry Co., Ltd., 728 g), and 18.5 moles of n-propyl acetate (Tokyo Chemical Industry Co., Ltd., 1887 g) were placed in a 3 L flask, and 0.74 moles of boron trifluoride diethyl ether complex (Tokyo Chemical Industry Co., Ltd.) was added at 70 ° C., and the mixture was reacted for 3 hours at a rotation speed of 300 rpm with a stirrer. After the polymerization solution was stopped with an aqueous sodium hydrogen carbonate solution, the oil layer was washed five times with pure water, and reprecipitation treatment was performed twice with methanol (Kanto Chemical Co., Ltd.) and propyl acetate, and the solid was collected by vacuum filtration, air-dried overnight in a draft, and vacuum-dried at 80 ° C. for 3 hours in a vacuum dryer. The obtained solid was weighed, and it was confirmed that 510 g of copolymer A was obtained.
[0071] GPC analysis of the resulting copolymer A showed that Mn was 3,200, Mw was 8,000, and Mw / Mn was 2.6. 13 C-NMR and 1 By carrying out H-NMR analysis, the constitutional units of copolymer A were calculated as follows. Structural unit (a) derived from a divinyl aromatic compound: 43 mol% Structural unit (b) derived from monovinyl aromatic compound: 57 mol% Ratio of m-units in structural units (a) derived from divinyl aromatic compounds: 61 mol%
[0072] (Examples 2 to 25) Copolymers were synthesized in the same manner as in Example 1, except that the m-form ratio in divinylbenzene and the polymerization time were changed and various alkylstyrenes were added so as to satisfy the conditions described in the synthesis conditions column in Tables 1, 2, and 3.
[0073] Tables 1 to 3 show the synthesis results of the examples and the evaluation results obtained by the following evaluation methods. [Table 1]
[0074] [Table 2]
[0075] [Table 3]
[0076] (Comparative Examples 1 and 2, and Examples 26 to 27) A copolymer was synthesized in the same manner as in Example 1, except that the conditions shown in the synthesis conditions column in Table 4 were used.
[0077] Table 4 shows the synthesis results of the comparative examples and the evaluation results by the following evaluation methods. [Table 4]
[0078] [Production of Curable Resin Composition] The following materials were mixed to prepare a curable resin composition.
[0079] (curable reactive compound) TAIC (Mitsubishi Chemical Corporation, molecular weight: 249.7, number of unsaturated double bonds per molecule: 3)
[0080] (hardening reactive resin) - Methacrylic end-modified PPE (product name: SA9000, manufactured by Sabic Innovative Plastics, Mn: 2756, number of terminal functional groups per molecule: 2)
[0081] (Radical polymerization initiator) Bis(1-tert-butylperoxy-1-methylethyl)benzene (product name: Perbutyl P, NOF Corporation)
[0082] [Preparation of Resin Composition Varnish] The curable reactive resin, the polyfunctional vinyl aromatic copolymer, and the curable reactive compound were weighed out in a weight ratio of 50:40:10, and 1% by mass of the radical polymerization initiator was weighed out relative to the solid content and placed in a container. A 50:50 ratio of toluene / methyl ethyl ketone mixed solvent was added to the mixture so that the solid content was 50% by mass, and the mixture was stirred for 5 hours or more to prepare a resin composition varnish.
[0083] [Preparation of prepreg] Low dielectric constant glass cloth L2116 (weight 94g / m 2 A sheet of board (91 μm thick, 50 mm wide) was impregnated with the resin composition varnish at a constant tension of about 100 N / m, scraped off with a slit, and dried at 120° C. for 60 minutes to prepare a prepreg.
[0084] [Create laminate] Eight prepregs were stacked and heated from room temperature at a rate of 3°C / min while applying a pressure of 5kg / cm 2 After reaching 130°C, the material was heated at a rate of 3°C / min while applying a pressure of 40kg / cm. 2 Then, when the temperature reached 200°C, the pressure was increased to 40 kg / cm while maintaining the temperature at 200°C. 2 A laminate was produced by vacuum pressing under the conditions of 100° C. for 60 minutes.
[0085] [Evaluation method] (Method for analyzing the m-unit ratio in the structural units derived from divinyl aromatic compounds in multifunctional vinyl aromatic copolymers) Using a nuclear magnetic resonance spectrometer manufactured by JEOL (model: JNM-ECZ500R / S1 type), 13 It was measured by C-NMR analysis. Chloroform-d1 was used as the solvent, and the resonance line of tetramethylsilane was used as the internal standard. The ratio of the area value of the peak at 125 ppm to the area values of the peaks at 113 ppm, 135 ppm, and 137 ppm was taken as the ratio of m-isomer in the structural unit derived from the divinyl aromatic compound.
[0086] (Method of analyzing the ratio of each structural unit of a polyfunctional vinyl aromatic copolymer) Using a nuclear magnetic resonance spectrometer manufactured by JEOL (model: JNM-ECZ500R / S1 type), 13 C-NMR and 1 It was measured by H-NMR analysis. Chloroform-d1 was used as the solvent, and the resonance line of tetramethylsilane was used as the internal standard. The ratio of the area value of the peaks at 5.2 ppm and 5.7 ppm to the area value of the peaks at 5.8 ppm to 7.7 ppm was taken as the ratio of the structural unit (a) derived from the divinyl aromatic compound, and the value obtained by subtracting the ratio of the structural unit (a) derived from the divinyl aromatic compound from 1 was taken as the ratio of the structural unit (b) derived from the monovinyl aromatic compound.
[0087] (Method of measuring molecular weight distribution) The number average molecular weight (Mn) of the styrene elastomer was determined by comparing with the elution time of a standard polystyrene with a known molecular weight using gel permeation chromatography (GPC). Specifically, after preparing a measurement sample with a sample concentration of 1.0 mass% (solvent: chloroform), the measurement was performed using a measuring device HLC-8320GPC (manufactured by Tosoh Corporation) under the following conditions. Column: Shodex K-806L, 3 columns connected in series Eluent: Chloroform Injection volume: 100μL Flow rate: 1.0mL / min Column temperature: 40℃ Detector: RI
[0088] (Method of evaluating the presence or absence of burrs when cutting prepreg) Five sample pieces measuring 10 mm in length x 10 mm in width were cut from the prepreg using a push cutter (blade: 0.25 mm thick razor blade) at a cutting speed of 1 cm / sec. After cutting, the appearance of the sample pieces near the cut points was visually observed from above and evaluated as follows. A: No cracks or burrs in the resin were found on any of the four sides. B: Resin cracks or burrs are observed on one side. C: Resin cracks or burrs are observed on 2 to 3 sides. D: Resin cracks or burrs are observed on all four sides.
[0089] (Evaluation of drilling workability) Punching was performed using a press-type punching machine equipped with a φ5 mm punch die, and the cross section was then polished. Peeling of the resin from the glass cloth near the outer periphery of the punched test piece was observed using a magnifying glass with a magnification of 40 times, and evaluation was performed as follows. A: No peeling on the entire outer periphery B: Partial peeling over 0% to less than 10% of the outer periphery C: Partial peeling of 10% to less than 20% of the outer periphery D: Peeled-off outer periphery is 20% or more
[0090] (Method of measuring dielectric tangent) The dielectric loss tangent of the laminate at 10 GHz was measured by the cavity resonance method using a network analyzer (N5230A, manufactured by Agilent Technologies) and a cavity resonator (Cavity Resonator CP series, manufactured by Kanto Electronics Application Development Co., Ltd.) as measuring equipment.
[0091] (Method of evaluating solder heat resistance) The laminate was cut to 50 mm x 50 mm and placed in a pressure cooker at 121°C saturated vapor pressure for 10 hours. The laminate was taken out, the moisture on the surface was wiped off, and then immersed in a solder bath at 288°C for 20 seconds. The swelling degree of the laminate after immersion was evaluated according to the following evaluation criteria. A: No bulges of 3 mm or more in diameter occurred. B: 1 to 3 blisters with a diameter of 3 mm or more, and no blisters with a diameter of 5 mm or more C: Four or more blisters with a diameter of 3 mm or more, or one or more blisters with a diameter of 5 mm or more
Claims
1. A polyfunctional vinyl aromatic copolymer having a structural unit derived from a divinyl aromatic compound and a structural unit derived from a monovinyl aromatic compound, wherein the m-form ratio of the divinyl aromatic compound is 60 mol% or more, and the polydispersity (Mw / Mn) of the molecular weight distribution, which is expressed as the ratio of the weight average molecular weight to the number average molecular weight of the polyfunctional vinyl aromatic copolymer, is more than 2.5 and 100 or less.
2. 2. The multifunctional vinyl aromatic copolymer of claim 1, having a multimodal molecular weight distribution.
3. The polyfunctional vinyl aromatic copolymer according to claim 1, further comprising 1 to 99 mol% of structural units derived from alkylstyrene having an alkylstyrene chain length of 3 to 20, based on 100 mol% of the total of all structural units.
4. The polyfunctional vinyl aromatic copolymer according to claim 3, wherein the alkylstyrene is an alkylstyrene having a carbon chain length of 6 to 10.
5. The multifunctional vinyl aromatic copolymer of claim 4, wherein said alkylstyrene is 4-n-octylstyrene.
6. The polyfunctional vinyl aromatic copolymer according to any one of claims 1 to 5, one or more selected from the group consisting of a curable reactive compound, a curable reactive resin, a thermoplastic resin, and a radical polymerization initiator; A curable resin composition comprising:
7. The curable resin composition according to claim 6, comprising a curable reactive compound, the curable reactive compound being a trialkenyl isocyanurate and / or a trialkenyl cyanurate.
8. The curable resin composition according to claim 6 , comprising a curable reactive resin, the curable reactive resin being a polyphenylene ether.
9. The curable resin composition according to claim 6 , further comprising a flame retardant and / or a filler.
10. A cured product obtained by curing the curable resin composition according to claim 6.
11. A curable composite material comprising the curable resin composition according to claim 6 and a substrate, wherein the substrate constitutes 1% by mass to 99% by mass based on the total mass of the curable composite material.
12. A cured composite material obtained by curing the curable composite material of claim 11.
13. A laminate comprising a plurality of layers of the cured composite material of claim 12.
14. A metal clad laminate comprising a layer of the curable composite material of claim 11 and a layer of metal foil.
15. A resin-coated metal foil comprising a metal foil and a film formed on one side of the metal foil by curing the curable resin composition according to claim 6.
16. A resin composition varnish comprising an organic solvent and the curable resin composition according to claim 6 dissolved in the organic solvent.
Citation Information
Patent Citations
Soluble polyfunctional vinyl aromatic copolymer, method for producing same and curable composition
WO2017115813A1
Soluble polyfunctional vinyl aromatic copolymer, method for producing same, curable resin composition and cured product thereof
WO2018181842A1