Rubber composition and winter tire
The rubber composition for winter tires addresses the balance of elongation, wet grip, and on-ice performance by incorporating an olefin/maleic anhydride copolymer, creating surface irregularities for improved traction and durability.
Patent Information
- Application Number
- JP2023054003
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing rubber compositions for winter tires fail to adequately balance elongation at break, wet grip performance, and on-ice performance, particularly on icy and snowy roads, despite efforts to improve surface roughness and water absorption.
A rubber composition comprising 100 parts by mass of diene rubber, 30 to 100 parts by mass of carbon black and/or white filler, and 0.5 to 30 parts by mass of an olefin/maleic anhydride copolymer with a molar ratio of olefin to maleic anhydride between 0 and 2.0, where the copolymer has a glass transition temperature of 140°C to 170°C and a weight average molecular weight of 3,000 to 100,000, enhancing hydrophilicity and hydrophobicity for improved surface irregularities.
The composition achieves excellent elongation at break, wet grip performance, and on-ice performance by creating surface irregularities through the olefin/maleic anhydride copolymer's interaction with water, resulting in enhanced traction and durability.
Smart Images

Figure 2024142043000007 
Figure 2024142043000001 
Figure 2024142043000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition and a winter tire. [Background technology]
[0002] In recent years, from the standpoint of safety and durability during vehicle travel, there has been a demand for improvements in the wet performance (wet grip performance: braking performance on wet road surfaces) and breaking elongation of tires. Furthermore, winter tires (e.g., studless tires) that are sometimes used on icy and snowy roads are required to have excellent performance on ice (braking performance on icy and snowy roads) in addition to the above-mentioned performance. On snowy and icy roads, the coefficient of friction is lower than on normal roads, making tires more slippery. For this reason, various compounding methods have been developed for improving performance on ice in the rubber compositions used in the treads of winter tires. Methods for improving performance on ice include compounding water-absorbing materials and materials that improve surface roughness.
[0003] For example, Patent Document 1 describes a rubber composition that contains a rubber component and fibers (excluding pulp fibers derived from waste paper) made of a hydrophilic resin, and has a coating layer made of a resin having affinity for the rubber component formed on the surface of the fibers, the hydrophilic resin being an ethylene-vinyl alcohol copolymer, a vinyl alcohol homopolymer, poly(meth)acrylic acid, a poly(meth)acrylic acid ester, polyethylene glycol, a carboxyvinyl copolymer, a styrene-maleic acid copolymer, polyvinylpyrrolidone, or a vinylpyrrolidone-vinyl acetate copolymer, and the resin having affinity for the rubber component is a polyolefin resin, for the purpose of providing a rubber composition that can improve the fracture resistance of the resulting tire while maintaining good drainage properties, and a tire using the same. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5823721 Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors have studied the rubber composition disclosed in Patent Document 1 and have found that when the rubber composition contains a diene rubber and an olefin / maleic anhydride copolymer, such as a styrene-maleic acid copolymer, whose main chain structure is formed from an olefin and maleic anhydride, at least one of the breaking elongation, wet grip performance, and performance on ice may be poor.
[0006] Therefore, an object of the present invention is to provide a rubber composition that is excellent in breaking elongation, wet grip performance, and performance on ice. Another object of the present invention is to provide a winter tire. [Means for solving the problem]
[0007] As a result of extensive research into solving the above problems, the present inventors have found that the problems can be solved by the following configuration.
[0008] [1] Per 100 parts by mass of diene rubber, 30 to 100 parts by mass of carbon black and / or white filler; and 0.5 to 30 parts by mass of an olefin / maleic anhydride copolymer whose main chain structure is formed by an olefin and maleic anhydride, The olefin comprises at least one selected from the group consisting of styrene, α-methylstyrene, and vinyltoluene; A rubber composition, wherein a molar ratio of the olefin to the maleic anhydride is more than 0 and not more than 2.0. [2] The rubber composition according to [1], wherein the glass transition temperature of the olefin / maleic anhydride copolymer is higher than 140°C and not higher than 170°C. [3] The rubber composition according to [1] or [2], wherein the olefin / maleic anhydride copolymer has a weight average molecular weight of 3,000 to 100,000. [4] The rubber composition according to any one of [1] to [3], wherein the olefin / maleic anhydride copolymer includes an unmodified olefin / maleic anhydride copolymer. [5] The rubber composition according to any one of [1] to [4], wherein the diene rubber contains a natural rubber, and the content of the natural rubber is 40 mass % or more of the total amount of the diene rubber. [6] The rubber composition according to any one of [1] to [5], wherein the diene rubber comprises a natural rubber and a polybutadiene rubber. [7] A winter tire manufactured using the rubber composition according to any one of [1] to [6]. Effect of the Invention
[0009] According to the present invention, it is possible to provide a rubber composition which is excellent in elongation at break, wet grip performance, and performance on ice. The present invention also provides a winter tire. [Brief description of the drawings]
[0010] [Figure 1] 1 is a partial cross-sectional schematic view of an example of an embodiment of a winter tire of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below. The following description of the configuration may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, a numerical range expressed using "~" means a range including the numerical values written before and after "~". In this specification, each component contained in the rubber composition of the present invention can be used alone or in combination of two or more kinds. In this specification, when the rubber composition of the present invention uses two or more kinds of a certain component in combination, the "content" of the component means the total content of those two or more kinds, unless otherwise specified. In the present specification, the method for producing each component is not particularly limited unless otherwise specified. For example, a conventionally known method may be used.
[0012] [Rubber composition] The rubber composition of the present invention comprises: Per 100 parts by mass of diene rubber, 30 to 100 parts by mass of carbon black and / or white filler; and 0.5 to 30 parts by mass of an olefin / maleic anhydride copolymer whose main chain structure is formed by an olefin and maleic anhydride, The olefin comprises at least one selected from the group consisting of styrene, α-methylstyrene, and vinyltoluene; The rubber composition has a molar ratio of the olefin to the maleic anhydride of more than 0 and not more than 2.0. In this specification, the above-mentioned "olefin / maleic anhydride copolymer whose main chain structure is formed by an olefin and maleic anhydride" is also referred to as a "specific copolymer".
[0013] The reason why the rubber composition having the above-mentioned structure can solve the problems of the present invention is not necessarily clear, but the present inventors speculate as follows. Note that the following speculation does not limit the mechanism by which the effect is obtained. In other words, even if the effect is obtained by a mechanism other than the following, it is included in the scope of the present invention. The rubber composition of the present invention exhibits excellent hydrophilicity due to the specific copolymer having a repeating unit derived from maleic anhydride. As a result, when a cured product obtained from the rubber composition of the present invention comes into contact with water, the specific copolymer present on the surface of the cured product dissolves, causing unevenness on the surface and improving surface roughness, and it is presumed that the cured product obtained from the rubber composition of the present invention has excellent wet grip performance and performance on ice. In addition, the rubber composition of the present invention exhibits excellent hydrophobicity because the specific copolymer has a repeating unit of at least one olefin selected from the group consisting of styrene, α-methylstyrene, and vinyltoluene, which results in high affinity with diene rubber in the hydrophobic portion of the specific copolymer and high affinity with carbon black and / or white filler in the hydrophilic portion of the specific copolymer, and therefore it is presumed that the cured product obtained from the rubber composition of the present invention has excellent elongation at break. Hereinafter, being superior in at least one of the breaking elongation, wet grip performance, and performance on ice will also be referred to as "being superior in the effect of the present invention."
[0014] [Diene rubber] The rubber composition of the present invention contains a diene-based rubber. The diene rubber is not particularly limited as long as it is a polymer formed from a monomer containing a conjugated diene. Examples of diene rubbers include natural rubber (NR), isoprene rubber (IR), copolymers of aromatic vinyl and conjugated dienes such as polybutadiene rubber (BR) and styrene-butadiene rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR), butyl rubber (IIR), halogenated butyl rubber (Br-IIR, Cl-IIR), and chloroprene rubber (CR).
[0015] The diene rubber preferably contains natural rubber and / or polybutadiene rubber, and more preferably contains natural rubber and polybutadiene rubber, because this provides better effects for the present invention.
[0016] When the diene rubber contains a natural rubber, the content of the natural rubber is preferably 40 mass% or more of the total amount of the diene rubber because the effects of the present invention are more excellent. When the diene rubber contains a polybutadiene rubber, the content of the polybutadiene rubber can be the same as above.
[0017] When the diene rubber contains natural rubber and a diene rubber other than natural rubber (e.g., polybutadiene rubber), the content of the natural rubber is preferably 40 to 60 mass% of the total amount of the diene rubber, because the effect of the present invention is more excellent. When the diene rubber contains natural rubber and a diene rubber other than natural rubber (e.g., polybutadiene rubber), the content of the diene rubber other than natural rubber (e.g., polybutadiene rubber) can be the same as above.
[0018] The glass transition temperature of the diene rubber is preferably -50°C or lower, and more preferably -100 to -60°C, in order to obtain a superior effect of the present invention and ensure flexibility on ice. The glass transition temperature of the diene rubber can be measured at a temperature rise rate of 20° C. / min using a differential scanning calorimeter (DSC) and calculated by the midpoint method. In the present invention, when the diene rubber contains two or more kinds of diene rubbers, the average glass transition temperature of the diene rubber is calculated by multiplying the glass transition temperature (Tg) of each diene rubber by the mass % of each diene rubber relative to the total of the diene rubbers (the mass % is divided by 100), and adding them together. When the diene rubber contains two or more kinds of diene rubbers, the average glass transition temperature of the diene rubber is preferably -50°C or lower, and more preferably -100 to -60°C, in order to achieve a better effect of the present invention and ensure flexibility on ice.
[0019] [Carbon black and / or white filler] The rubber composition of the present invention contains carbon black and / or a white filler. The rubber composition of the present invention preferably contains a white filler, and more preferably contains carbon black and a white filler, because the effects of the present invention are more excellent.
[0020] (Carbon Black) When the rubber composition of the present invention contains carbon black, the carbon black is not particularly limited, and examples of the carbon black include various grades of carbon black such as SAF-HS, SAF, ISAF-HS, ISAF, ISAF-LS, IISAF-HS, HAF-HS, HAF, HAF-LS, FEF, GPF, and SRF. The nitrogen adsorption specific surface area (N2SA) of the carbon black is not particularly limited. When the rubber composition of the present invention contains carbon black, the effect of the present invention is more excellent, so the carbon black has an N2SA of 50 to 200 m 2 It is preferable that the carbon black has an N2SA of 70 to 150 m 2 It is more preferred that the carbon black comprises 0.1 wt. / g. Here, the nitrogen adsorption specific surface area (N2SA) is the amount of nitrogen adsorbed on the surface of carbon black measured according to JIS K6217-2:2001 "Part 2: Determination of specific surface area - Nitrogen adsorption method - Single point method."
[0021] (white filler) When the rubber composition of the present invention contains a white filler, examples of the white filler include silica, calcium carbonate, magnesium carbonate, talc, clay, alumina, aluminum hydroxide, titanium oxide, and calcium sulfate. When the rubber composition of the present invention contains a white filler, the white filler preferably contains silica, because the effects of the present invention are more excellent.
[0022] ((silica)) The silica is not particularly limited, and any conventionally known silica can be used. Examples of the silica include wet silica (hydrated silicic acid) and dry silica (anhydrous silicic acid).
[0023] The cetyltrimethylammonium bromide (CTAB) adsorption specific surface area of the silica is not particularly limited. For the reason that the effect of the present invention is more excellent, the silica is preferably one having a CTAB adsorption specific surface area (hereinafter abbreviated as CTAB) of 100 to 400 m 2It is preferable that the silica has a CTAB of 150 to 300 m 2 It is more preferable that the silica has a CTAB of 160 to 250 m 2 It is even more preferred that the silica content is 0.01 to 0.1 g / g. Here, the CTAB adsorption specific surface area is a value obtained by measuring the amount of CTAB adsorbed on the silica surface in accordance with JIS K6217-3:2001 "Part 3: Determination of specific surface area - CTAB adsorption method."
[0024] [Carbon black and / or white filler content] In the present invention, the content of carbon black and / or white filler (when carbon black and white filler are used in combination, the total amount of these; the same applies below) is 30 to 100 parts by mass based on 100 parts by mass of diene rubber.
[0025] When the rubber composition of the present invention contains carbon black and a white filler, the content of the white filler is preferably 20 to 60 parts by mass based on 100 parts by mass of the diene rubber, because the effects of the present invention are more excellent. When the rubber composition of the present invention contains carbon black and a white filler, the content of carbon black is preferably 10 to 40 parts by mass based on 100 parts by mass of the diene rubber, because the effects of the present invention are more excellent.
[0026] [Olefin / Maleic Anhydride Copolymer] The rubber composition of the present invention contains an olefin / maleic anhydride copolymer (specific copolymer) whose main chain structure is formed by an olefin and maleic anhydride. In the specific copolymer, the olefin contains at least one selected from the group consisting of styrene, α-methylstyrene, and vinyltoluene. The specific copolymer is a copolymer that has both the hydrophobicity derived from the olefin and the hydrophilicity derived from maleic anhydride. In the present invention, the main chain skeleton of the specific copolymer is formed by the above-mentioned olefin and maleic anhydride as monomers, and has a repeating unit X of the above-mentioned olefin and a repeating unit Y of maleic anhydride.
[0027] The specific copolymer can be represented, for example, by the following formula (1). [ka] In formula (1), X represents a repeating unit of an olefin containing at least one selected from the group consisting of styrene, α-methylstyrene, and vinyltoluene. In formula (1), m represents the number of repeating units of the repeating unit X. m is more than 0 and not more than 2.0. m corresponds to the below-described [molar ratio of olefin to maleic anhydride] in the specific copolymer. In addition, when the specific copolymer has repeating units of olefins containing at least two selected from the group consisting of styrene, α-methylstyrene, and vinyltoluene, m in formula (1) represents the total number of repeating units of the olefins containing at least two of the above. In formula (1), n represents the number of repeating units in the repeating units in [ ]. n can be 2 or more. There is no particular upper limit to n. In addition, n can be in a range corresponding to the weight average molecular weight of the specific copolymer described below. X (repeating unit X) in formula (1) includes at least one selected from the group consisting of the following formulae (X1) to (X3). [ka] JPEG2024142043000003.jpg3163 JPEG2024142043000004.jpg2863
[0028] In the specific copolymer, the olefin preferably contains styrene because the effects of the present invention are more excellent. Specific examples of the specific copolymer include a styrene / maleic anhydride copolymer, an α-methylstyrene / maleic anhydride copolymer, and a vinyltoluene / maleic anhydride copolymer. The specific copolymer preferably contains a styrene / maleic anhydride copolymer because the effects of the present invention are more excellent.
[0029] [Molar ratio of olefin to maleic anhydride] In the present invention, the molar ratio of the olefin to the maleic anhydride in the specific copolymer (the molar ratio value expressed as olefin / maleic anhydride) is more than 0 and 2.0 or less. When the molar ratio is within the above range, the specific copolymer has excellent hydrophilicity. The above molar ratio is preferably 0.5 to 1.5 because the effects of the present invention are more excellent.
[0030] (Glass transition temperature of olefin / maleic anhydride copolymer) The glass transition temperature (Tg) of the olefin / maleic anhydride copolymer is preferably 100°C or higher, and more preferably higher than 140°C and 170°C or lower, because the specific copolymer is likely to form domains in the cured product obtained from the rubber composition of the present invention, and appropriate unevenness is likely to be formed on the surface of the cured product, thereby making the effects of the present invention more excellent. The glass transition temperature of the olefin / maleic anhydride copolymer can be measured at a temperature rise rate of 20° C. / min using a differential scanning calorimeter (DSC) and calculated by the midpoint method. When the olefin / maleic anhydride copolymer is a commercially available product, the glass transition temperature listed in a catalog of the commercially available product can be referred to as the glass transition temperature of the olefin / maleic anhydride copolymer.
[0031] (Weight average molecular weight of olefin / maleic anhydride copolymer) The weight average molecular weight (Mw) of the olefin / maleic anhydride copolymer is preferably from 3,000 to 100,000, and more preferably from 4,000 to 8,000, because the effects of the present invention are more excellent. The weight average molecular weight of the olefin / maleic anhydride copolymer can be determined in terms of polystyrene by gel permeation chromatography (GPC). When the olefin / maleic anhydride copolymer is a commercially available product, the weight average molecular weight listed in a catalog of the commercially available product can be referred to as the weight average molecular weight of the olefin / maleic anhydride copolymer.
[0032] The specific copolymer is preferably a copolymer formed only from an olefin and maleic anhydride.
[0033] In one preferred embodiment, the specific copolymer does not have a modified group represented by the following formula (2) derived from maleic anhydride (for example, does not have it at the terminal or side chain). Note that since the modified group represented by the following formula (2) has only one bonding point, the modified group does not form the main chain skeleton of the specific polymer. [ka] In formula (2), * indicates a bonding point.
[0034] (denatured / undenatured) The olefin / maleic anhydride copolymer may be modified or unmodified, but it is preferable that the olefin / maleic anhydride copolymer comprises an unmodified (i.e., unmodified) olefin / maleic anhydride copolymer, because the olefin / maleic anhydride copolymer is likely to form domains in the cured product obtained from the rubber composition of the present invention, and appropriate unevenness is likely to be formed on the surface of the cured product, thereby making the effects of the present invention more excellent.
[0035] When the olefin / maleic anhydride copolymer is modified, the modified olefin / maleic anhydride copolymer may be, for example, an olefin / maleic anhydride copolymer modified with a sodium salt, a potassium salt, an ammonia salt, or a cationic solution.
[0036] [Olefin / Maleic Anhydride Copolymer Content] In the present invention, the content of the olefin / maleic anhydride copolymer (specific copolymer) is 0.5 to 30 parts by mass based on 100 parts by mass of the diene rubber. The content of the specific copolymer is preferably 5 to 25 parts by mass, and more preferably 8 to 20 parts by mass, per 100 parts by mass of the diene rubber, because this provides better effects of the present invention (particularly performance on ice).
[0037] (optional ingredient) The rubber composition of the present invention may contain components (optional components) other than the above-mentioned components, if necessary. Examples of such components include various additives commonly used in rubber compositions, such as silane coupling agents, terpene resins (preferably aromatic modified terpene resins), thermally expandable microcapsules, zinc oxide (zinc white), stearic acid, antioxidants, waxes, plasticizers (e.g., oils), processing aids, thermosetting resins, vulcanizing agents (e.g., sulfur), and vulcanization accelerators.
[0038] (Silane coupling agent) The silane coupling agent that can be further contained in the composition of the present invention is not particularly limited as long as it is a silane compound having a hydrolyzable group and an organic functional group. The hydrolyzable group is not particularly limited, and examples thereof include an alkoxy group, a phenoxy group, a carboxyl group, and an alkenyloxy group. Among them, an alkoxy group is preferable because the effects of the present invention are more excellent. When the hydrolyzable group is an alkoxy group, the number of carbon atoms of the alkoxy group is preferably 1 to 16, and more preferably 1 to 4, because the effects of the present invention are more excellent. Examples of the alkoxy group having 1 to 4 carbon atoms include a methoxy group, an ethoxy group, and a propoxy group.
[0039] The organic functional group is not particularly limited, but is preferably a group capable of forming a chemical bond with an organic compound, and examples thereof include an epoxy group, a vinyl group, an acryloyl group, a methacryloyl group, an amino group, a sulfide group, a mercapto group, a blocked mercapto group (protected mercapto group) (e.g., an octanoylthio group), and the like. Among these, a sulfide group (particularly a disulfide group or a tetrasulfide group), a mercapto group, and a blocked mercapto group are preferred because they provide better effects of the present invention.
[0040] Specific examples of the silane coupling agent include bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, mercaptopropyltrimethoxysilane, mercaptopropyltriethoxysilane, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl-tetrasulfide, trimethoxysilylpropyl-mercaptobenzothiazole tetrasulfide, triethoxysilylpropyl-methacrylate-monosulfide, dimethoxymethylsilylpropyl-N,N-dimethylthiocarbamoyl-tetrasulfide, 3-octanoylthio-1-propyltriethoxysilane, and the like. One of these may be used alone, or two or more may be used in combination.
[0041] When the rubber composition of the present invention contains silica and further contains a silane coupling agent, the content of the silane coupling agent is preferably 3 to 30 mass % relative to the above-mentioned silica content, and more preferably 5 to 20 mass %, because the effects of the present invention are better.
[0042] In addition, when the rubber composition of the present invention further contains a silane coupling agent, the content of the silane coupling agent is preferably 1 to 50 parts by mass, more preferably 2 to 45 parts by mass, and even more preferably 4 to 40 parts by mass, per 100 parts by mass of the above-mentioned diene-based rubber, because the effects of the present invention are more excellent.
[0043] (Method of manufacturing rubber composition) The method for producing the rubber composition of the present invention is not particularly limited, and specific examples thereof include a method of mixing the above-mentioned components using a known method or device (e.g., a Banbury mixer, a kneader, a roll, etc.) When the rubber composition of the present invention contains sulfur or a vulcanization accelerator, it is preferable to first mix the components other than the sulfur and the vulcanization accelerator at a high temperature (preferably 140°C or higher and 150°C or lower), cool the mixture, and then mix the sulfur or the vulcanization accelerator. The rubber composition of the present invention can be vulcanized or crosslinked under conventionally known vulcanization or crosslinking conditions. The temperature during vulcanization or crosslinking is preferably 150 to 170°C.
[0044] (Cured product of the rubber composition of the present invention) The cured product obtainable by vulcanizing or crosslinking the rubber composition of the present invention preferably has domains of the specific copolymer in a diene rubber matrix. The domains of the specific copolymer in the diene rubber matrix preferably form an island-sea structure. In the cured product, the domains may be present inside and on the surface of the cured product. The domains preferably have a granular shape (rounded particle shape). The average particle size of the domains is preferably from 20 to 100 μm, and more preferably from 30 to 80 μm, because this allows appropriate unevenness to be formed on the surface of the resulting cured product, thereby providing better effects for the present invention. In the present invention, the average particle size of the domains due to the specific copolymer is the average value of the diameters obtained by observing the diameters of the domains due to the specific copolymer in the cured product obtained by vulcanizing or crosslinking the rubber composition of the present invention with a scanning electron microscope (SEM) (i.e., the number average particle size obtained by observation with a scanning electron microscope).
[0045] When the cured material comes into contact with water from the outside, for example, rain, snow, puddles, snowy roads, icy and snowy road surfaces, the specific copolymer on the surface of the cured material dissolves in the water, causing unevenness on the surface and improving surface roughness. Incidentally, since the amount of water that may be originally present in the cured product (the cured product immediately after vulcanization or crosslinking) is small, the specific copolymer in the cured product is unlikely to dissolve on contact with the water.
[0046] (Application) The rubber composition of the present invention can be used, for example, in tires, and more specifically, for winter tires.
[0047] [Winter tires] The winter tire of the present invention is a winter tire manufactured using the above-mentioned rubber composition of the present invention. A specific example of the winter tire is a studless tire. The winter tire of the present invention is not particularly limited, except that it is produced using the rubber composition of the present invention. The rubber composition used for the winter tire of the present invention is not particularly limited as long as it is the rubber composition of the present invention. There is no particular limitation as to which part of the winter tire of the present invention the rubber composition of the present invention is used in. Among them, from the viewpoint of excellent breaking elongation, wet grip performance, and performance on ice, the rubber composition of the present invention is preferably used (placed) in the tire tread (cap tread).
[0048] Hereinafter, a winter tire according to the present invention will be described with reference to the accompanying drawings. However, the winter tire according to the present invention is not limited to the accompanying drawings. FIG. 1 is a partial cross-sectional schematic view of an example of an embodiment of a winter tire of the present invention. In FIG. 1, a winter tire has a bead portion 1 , a sidewall portion 2 , and a tire tread portion 3 . A carcass layer 4 with fiber cords embedded therein is installed between the pair of left and right bead portions 1, and the ends of the carcass layer 4 are folded back and wrapped around the bead cores 5 and bead fillers 6 from the inside to the outside of the tire. In the bead portion 1, a rim cushion 8 is disposed in the portion that comes into contact with the rim. In the tire tread portion 3, a belt layer 7 is disposed around one circumference of the tire on the outer side of the carcass layer 4. The tire tread portion 3 is preferably formed using the rubber composition of the present invention.
[0049] The winter tire of the present invention can be produced, for example, according to a conventionally known method. When the winter tire of the present invention is a pneumatic tire, examples of the gas filled in the winter tire include normal air or air with an adjusted oxygen partial pressure; and inert gases such as nitrogen, argon, and helium. EXAMPLES
[0050] The present invention will be described in further detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the following examples.
[0051] [Production of rubber composition] The components shown in Table 1 below were mixed in the ratios (parts by mass) shown in the same table. Specifically, the components shown in Table 1 below, except for sulfur and vulcanization accelerator, were first heated to about 140 to 150°C using a 1.7-liter closed Banbury mixer, mixed for 5 minutes, then discharged and cooled to room temperature to obtain a master batch. Furthermore, sulfur and a vulcanization accelerator were mixed into the obtained master batch using the Banbury mixer to obtain each rubber composition. In Table 1, the amount (parts by mass) of each rubber component is the net amount of rubber.
[0052] 〔evaluation〕 The rubber compositions thus obtained were evaluated as follows, and the results are shown in Table 1.
[0053] <Preparation of vulcanized rubber sheet> The resulting rubber composition (unvulcanized) was press-vulcanized in a mold (15 cm×15 cm×0.2 cm) at 170° C. for 10 minutes to prepare a vulcanized rubber sheet. - Average particle size of the domain Using each of the vulcanized rubber sheets (cured products) prepared as described above, the average particle size (μm) of the domains of the specific copolymer or SMA resins 2 to 4 in each of the cured products was obtained by the method using a scanning electron microscope (SEM) as described above.
[0054] <Elongation at break> From the obtained vulcanized rubber sheet, a JIS No. 3 dumbbell-shaped test piece (thickness 2 mm) was punched out in accordance with JIS K6251:2010, and the breaking elongation was measured under conditions of 20°C and a tensile speed of 500 mm / min. The measurement results were expressed as an index, with the value of Control Example 1 being 100. In the present invention, the breaking elongation was evaluated as excellent when the index exceeded 100. The greater the index is from 100, the more excellent the breaking elongation is. On the other hand, when the index was 100 or less, the elongation at break was evaluated as being poor.
[0055] <Ice performance> The obtained vulcanized rubber sheet was attached to a flat cylindrical rubber base, and the coefficient of friction on ice was measured using an inside drum type ice friction tester. The measurement temperature was -1.5°C and the load was 5.5g / cm. 3 The drum rotation speed was 25km / h. The measurement results were expressed as an index, with the measured value for Control Example 1 being set at 100. The index was calculated by applying the coefficient of friction on ice for each Example to the following formula. Index = (measured value / coefficient of friction on ice of test piece of standard example 1) x 100 In the present invention, a tire is evaluated as having high frictional force on ice and excellent performance on ice when the index exceeds 100. The higher the index is from 100, the better the performance on ice is. On the other hand, when the index was 100 or less, the performance on ice was evaluated as poor.
[0056] <Wet grip performance> The vulcanized rubber sheet thus obtained was subjected to measurement of tan δ(0°C) in accordance with JIS K6394:2007 using a viscoelasticity spectrometer (manufactured by Toyo Seiki Seisakusho) under conditions of an elongation deformation strain rate of 10%±2%, a vibration frequency of 20 Hz, and a temperature of 0°C. The measurement results were expressed as an index, with the measurement value for Control Example 1 being 100. In the present invention, the wet grip performance was evaluated as excellent when the index exceeded 100. The greater the index is from 100, the more excellent the wet grip performance is. On the other hand, when the index was 100 or less, the wet grip performance was evaluated as poor.
[0057] [Table 1]
[0058] Details of each component shown in Table 1 are as follows. (Diene rubber) NR: Natural rubber (STR20, glass transition temperature: -65°C, manufactured by Bonbandit) BR: Polybutadiene rubber (Nipol BR1220, glass transition temperature: -110°C, manufactured by Zeon Corporation) (white filler) Silica: ULTRASIL VN3 (manufactured by Evonik Degussa) (Carbon Black) CB: Show Black N339 (Cabot Japan)
[0059] Silane coupling agent: Silane coupling agent (Si69, manufactured by Evonik Degussa) Zinc oxide: Three types of zinc oxide (manufactured by Seido Chemical Co., Ltd.) Stearic acid: Beads Stearic Acid YR (manufactured by NOF Corporation) Antioxidant: Amine-based antioxidant (Santoflex 6PPD, manufactured by Flexis) Wax: Paraffin wax (manufactured by Ouchi Shinko Chemical Co., Ltd.) Oil: Aroma oil (Extract No. 4S, Showa Shell Sekiyu Co., Ltd.) Sulfur: Oil-treated sulfur (Hosoi Chemicals) Vulcanization accelerator: Sulfenamide vulcanization accelerator (Suncerer CM-G, Sanshin Chemical Co., Ltd.)
[0060] (Olefin / Maleic Anhydride Copolymer) SMA resin 1: A copolymer of styrene and maleic anhydride, with a molar ratio of styrene / maleic anhydride of 1 (styrene:maleic anhydride = 1:1). Polyscope's "XIRAN (registered trademark) 1000", weight average molecular weight 5,000 g / mol, Tg 150°C SMA resin 1 corresponds to a specific copolymer because the molar ratio of styrene / maleic anhydride is 1. On the other hand, SMA resins 2 to 4 described below do not correspond to specific copolymers because the molar ratio of styrene / maleic anhydride exceeds 2.0.
[0061] SMA resin 2 (for comparison): A copolymer of styrene and maleic anhydride with a molar ratio of styrene / maleic anhydride of 3 (styrene:maleic anhydride = 3:1). "SMA3000" manufactured by Sartomer Japan Co., Ltd., weight average molecular weight 9,500, Tg 125℃ SMA resin 3 (comparison): A copolymer of styrene and maleic anhydride, with a molar ratio of styrene / maleic anhydride of 3 (styrene:maleic anhydride = 3:1). Polyscope's "XIRAN (registered trademark) 3600", weight average molecular weight 120,000 g / mol, Tg 160°C SMA resin 4 (comparison): A copolymer of styrene and maleic anhydride, with a molar ratio of styrene / maleic anhydride of 8 (styrene:maleic anhydride = 8:1). "XIRAN (registered trademark) 9000" manufactured by Polyscope, weight average molecular weight 10,000 g / mol, Tg 104°C
[0062] From the results in Table 1, it was confirmed that the rubber composition of the present invention exhibits the desired effects. On the other hand, Comparative Examples 1 to 3, in which the molar ratio of styrene to maleic anhydride in the copolymer of styrene and maleic anhydride exceeds 2.0, were poor in at least any of the elongation at break, wet grip performance, and performance on ice. Comparative Example 4, in which the content of the specific copolymer did not satisfy the prescribed range, had poor elongation at break and poor performance on ice. [Explanation of symbols]
[0063] 1 Bead section 2 Sidewall 3 Tire tread 4 Carcass layer 5 Bead Core 6 Bead Filler 7 Belt layer 8 Rim cushion
Claims
1. Relative to 100 parts by mass of diene rubber, 30 to 100 parts by weight of carbon black and / or white filler; 0.5 to 30 parts by mass of an olefin / maleic anhydride copolymer whose main chain structure is formed by an olefin and maleic anhydride; The olefin comprises at least one selected from the group consisting of styrene, α-methylstyrene, and vinyltoluene; A rubber composition, wherein a molar ratio of the olefin to the maleic anhydride is more than 0 and not more than 2.
0.
2. The rubber composition according to claim 1, wherein the glass transition temperature of the olefin / maleic anhydride copolymer is higher than 140°C and not higher than 170°C.
3. 2. The rubber composition according to claim 1, wherein the olefin / maleic anhydride copolymer has a weight average molecular weight of 3,000 to 100,000.
4. 2. The rubber composition according to claim 1, wherein the olefin / maleic anhydride copolymer comprises an unmodified olefin / maleic anhydride copolymer.
5. The rubber composition according to claim 1 , wherein the diene rubber comprises a natural rubber, and the content of the natural rubber is 40 mass % or more of the total amount of the diene rubber.
6. The rubber composition of claim 1 , wherein the diene-based rubber comprises natural rubber and polybutadiene rubber.
7. A winter tire manufactured using the rubber composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Rubber composition and pneumatic tire
JP2012201742A
Rubber composition for inner liner layer and pneumatic tire prepared using the same
JP2015110700A
Rubber composition for tire tread
KR100879462B1
Rubber tire compound containing IPN-promoting resin
US20230044878A1
Pet / SPS polymer alloy
WO2015037238A1