Ethylene / α-olefin / non-conjugated polyene copolymer, method for producing the same, and composition comprising the same
A novel ethylene/α-olefin/non-conjugated polyene copolymer with optimized composition and structure addresses the moldability and crosslinking limitations of EPDM, offering improved mechanical properties and heat resistance in molded products.
Patent Information
- Application Number
- JP2023054075
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing ethylene-α-olefin rubbers, such as ethylene-propylene-nonconjugated diene copolymers (EPDM), lack sufficient moldability and fast crosslinking properties, limiting their application in areas requiring improved mechanical properties and processing efficiency.
Development of an ethylene/α-olefin/non-conjugated polyene copolymer containing specific non-conjugated polyenes like 5-vinyl-2-norbornene (VNB), with a molar ratio of ethylene to α-olefin between 50/50 and 80/20, intrinsic viscosity between 5.1 and 7.0 dL/g, and a weight fraction of non-conjugated polyene between 0.07% and 10%, optimized for fast crosslinking and enhanced moldability.
The copolymer exhibits excellent moldability, crosslinking properties, and curing properties, resulting in molded products with superior mechanical properties and heat aging resistance.
Abstract
Description
[Technical field]
[0001] The present invention relates to an ethylene-α-olefin-non-conjugated polyene copolymer. More specifically, the present invention relates to a novel ethylene-α-olefin-non-conjugated polyene copolymer having structural units derived from a specific non-conjugated polyene such as 5-vinyl-2-norbornene (VNB) and exhibiting a high crosslinking rate and excellent moldability, as well as a production method thereof and a composition thereof. [Background technology]
[0002] Ethylene-α-olefin rubbers, such as ethylene-propylene-non-conjugated diene copolymer rubber (EPDM), do not have unsaturated bonds in the main chain of their molecular structure, and therefore have superior heat resistance and weather resistance compared to the commonly used conjugated diene rubbers. As a result, they are widely used in a variety of applications, including automotive parts, electric wire materials, construction and civil engineering materials, industrial parts, and as modifiers for various resins.
[0003] It is known that when ethylene-α-olefin rubber is crosslinked using peroxide, especially when it contains non-conjugated polyene such as 5-vinyl-2-norbornene (hereinafter, also referred to as VNB) as a copolymerization component, the crosslinking rate is fast. Furthermore, improvement of moldability is desired. Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention provides a novel ethylene-α-olefin-non-conjugated polyene copolymer having improved processability, a method for producing the ethylene-α-olefin-non-conjugated polyene copolymer, and a composition containing the same. [Means for solving the problem]
[0005] The present invention relates to the following: [1] An ethylene-α-olefin-non-conjugated polyene copolymer (1) that satisfies the following requirements 1 and 2. Requirement 1 It has structural units derived from ethylene (XA), an α-olefin (XB) having 3 to 20 carbon atoms, and a non-conjugated polyene (XC) containing, in the molecule, two or more partial structures selected from the group consisting of the following general formulas (I) and (II): Requirement 2 The following requirements (i) to (iv) are met. (i) The molar ratio of ethylene (XA) / α-olefin (XB) is 50 / 50 to 80 / 20. (ii) The weight fraction of the constitutional unit derived from the non-conjugated polyene (XC) is 0.07% by weight to 10% by weight in 100% by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1). (iii) The intrinsic viscosity [η] is 5.1 to 7.0 dL / g. (iv) The ratio P(η*(ω=0.1) / η*(ω=100)) of the complex viscosity η*(ω=0.1) (Pa sec) at a frequency ω=0.1 rad / s to the complex viscosity η*(ω=100) (Pa sec) at a frequency ω=100 rad / s, obtained by linear viscoelastic measurement (190°C) using a rheometer, the intrinsic viscosity [η], and the weight fraction of the constitutional unit derived from non-conjugated polyene (XC) (weight fraction of (XC)) satisfy the following formula (Z). 2.5≦P / ([η] 2.9 )≦(XC) weight fraction × 4 (Z)
[0006] [ka] [2] The ethylene-α-olefin-non-conjugated polyene copolymer (1) according to [1], wherein the non-conjugated polyene (XC) is 5-vinyl-2-norbornene (VNB). [3] A composition comprising the ethylene-α-olefin-non-conjugated polyene copolymer (1) described in [1] above. [4] The composition according to [2] or [3], further comprising an ethylene-α-olefin-non-conjugated polyene copolymer (2) that satisfies the following requirements 3 and 4: Requirement 3 It has structural units derived from ethylene (X-A'), an α-olefin (X-B') having 3 to 20 carbon atoms, and a non-conjugated polyene (X-C') containing, in the molecule, a total of two or more partial structures selected from the group consisting of the following general formulas (I) and (II): Requirement 4 The intrinsic viscosity [η] is in the range of 1.0 to 2.2 dL / g.
[0007] [ka] [5] Weight average molecular weight (Mw) is 1.0×10 5 ~4.0×10 5 The composition according to [4], characterized in that the molecular weight distribution (Mw / Mn) (as measured by GPC) is in the range of 2.8 to 5.0. [6] A molded article formed from the composition according to any one of [3] to [5]. [7] A method for producing the ethylene-α-olefin-non-conjugated polyene copolymer (1) according to [1], characterized in that monomers consisting of the ethylene (XA) according to claim 1, an α-olefin (XB) having 3 to 20 carbon atoms, and a non-conjugated polyene (XC) are copolymerized in the presence of at least one metallocene compound represented by the following general formula [A-2]:
[0008] [ka] In the formula [A-2], M is a titanium atom, a zirconium atom, or a hafnium atom, n is an integer of 1 to 3, each X is independently a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group, and R 1 ~R 5 and R 6each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 1 ~R 5 Adjacent groups among these may be bonded to each other to form a ring. [8] The method for producing the ethylene-α-olefin-non-conjugated polyene copolymer (1) according to [7], wherein the non-conjugated polyene (XC) is 5-vinyl-2-norbornene (VNB). Effect of the Invention
[0009] According to the present invention, it is possible to provide a novel ethylene-α-olefin-non-conjugated polyene copolymer which contains a specific non-conjugated polyene such as VNB as a copolymerization component and has excellent moldability, and also to provide a production method and uses of the ethylene-α-olefin-non-conjugated polyene copolymer.
[0010] The ethylene-α-olefin-non-conjugated polyene copolymer (1) according to the present invention is excellent in moldability, crosslinking properties, and curing properties, and the obtained molded article has an excellent balance of physical properties such as mechanical properties and is particularly excellent in heat aging resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be specifically described below. <Ethylene-α-olefin-non-conjugated polyene copolymer (1)> The ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention has structural units derived from ethylene (XA), an α-olefin (XB) having 3 to 20 carbon atoms, and a non-conjugated polyene (XC) containing, in the molecule, two or more partial structures selected from the group consisting of the following general formulae (I) and (II):
[0012] [ka]
[0013] The ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention may have, in addition to the structural units derived from the above-mentioned ethylene (XA), α-olefin (XB) and non-conjugated polyene (XC), a structural unit derived from a non-conjugated polyene (XD) containing only one partial structure selected from the group consisting of the above-mentioned general formulae (I) and (II) in the molecule.
[0014] Examples of the α-olefin (XB) having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-eicosene, etc. Among these, α-olefins having 3 to 8 carbon atoms such as propylene, 1-butene, 1-hexene, 1-octene, etc. are preferred, and propylene is particularly preferred.
[0015] Such α-olefins are preferable because the raw material costs are relatively low, the resulting ethylene-α-olefin-non-conjugated polyene copolymers exhibit excellent mechanical properties, and molded articles having rubber elasticity can be obtained. These α-olefins may be used alone or in combination of two or more.
[0016] That is, the ethylene-α-olefin-non-conjugated polyene copolymer of the present invention contains structural units derived from at least one type of α-olefin (XB) having 3 to 20 carbon atoms, and may contain structural units derived from two or more types of α-olefins (XB) having 3 to 20 carbon atoms.
[0017] Examples of the non-conjugated polyene (XC) containing two or more partial structures selected from the group consisting of the above general formulas (I) and (II) in the molecule in total include 5-vinyl-2-norbornene (VNB), norbornadiene, 1,4-hexadiene, dicyclopentadiene, etc. Among these, it is preferable that the non-conjugated polyene (XC) contains VNB, since it is highly available, has good reactivity with peroxide during the crosslinking reaction after polymerization, and tends to improve the heat resistance of the composition containing this copolymer. The non-conjugated polyenes (XC) may be used alone or in combination of two or more.
[0018] The ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention may further contain, in addition to the structural units derived from ethylene (XA), the α-olefin having 3 to 20 carbon atoms (XB) and the non-conjugated polyene (XC), a structural unit derived from a non-conjugated polyene (XD) containing only one partial structure selected from the group consisting of the general formulae (I) and (II) in the molecule. Examples of such non-conjugated polyenes (XD) include 5-ethylidene-2-norbornene (ENB), 5-methylene-2-norbornene, 5-(2-propenyl)-2-norbornene, 5-(3-butenyl)-2-norbornene, 5-(1-methyl-2-propenyl)-2-norbornene, 5-(4-pentenyl)-2-norbornene, 5-(1-methyl-3-butenyl)-2-norbornene, 5-(5-hexenyl)-2-norbornene, 5-(1-methyl-4-pentenyl)-2-norbornene, 5-(2,3-dimethyl-3-butenyl)-2-norbornene, 5-(2-ethyl ... 5-(1,2-dimethyl-5-hexenyl)-2-norbornene, 5-(5-ethyl-5-hexenyl)-2-norbornene, 5-(1,2,3-trimethyl-4-pentenyl)-2-norbornene, 5-(6-heptenyl)-2-norbornene, 5-(3-methyl-5-hexenyl)-2-norbornene, 5-(3,4-dimethyl-4-pentenyl)-2-norbornene, 5-(3-ethyl-4-pentenyl)-2-norbornene, 5-(7-octenyl)-2-norbornene, 5-(2-methyl-6-heptenyl)-2-norbornene, 5-(1,2-dimethyl-5-hexenyl)-2-norbornene, 5-(5-ethyl-5-hexenyl)-2-norbornene, 5-(1,2,3-trimethyl-4-pentenyl)-2-norbornene, and the like. Among these, ENB is preferred because it is easily available, has high reactivity with sulfur and vulcanization accelerators during the crosslinking reaction after polymerization, is easy to control the crosslinking rate, and is likely to provide good mechanical properties.
[0019] The non-conjugated polyene (XD) may be used alone or in combination of two or more. When the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention contains a structural unit derived from a non-conjugated polyene (XD) containing only one partial structure selected from the group consisting of the general formulae (I) and (II) in the molecule, the proportion of the structural unit is not particularly limited within a range that does not impair the object of the present invention, but is usually contained in a weight fraction of about 0 to 20% by weight, preferably 0 to 8% by weight, and more preferably about 0.01 to 8% by weight (wherein the total weight fractions of ethylene (XA), α-olefin (XB), non-conjugated polyene (XC), and non-conjugated polyene (XD) is taken as 100% by weight).
[0020] As described above, the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention is a copolymer having structural units derived from ethylene (XA), an α-olefin (XB) having 3 to 20 carbon atoms, the non-conjugated polyene (XC), and, as necessary, the non-conjugated polyene (XD), and satisfies the following requirements (i) to (iv): (i) The molar ratio of ethylene (XA) / α-olefin (XB) is 50 / 50 to 80 / 20. (ii) The weight fraction of the constitutional unit derived from the non-conjugated polyene (XC) is 0.07% by weight to 10% by weight in 100% by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1). (iii) The intrinsic viscosity [η] is 5.1 to 7.0 dL / g. (iv) The ratio P(η*(ω=0.1) / η*(ω=100)) of the complex viscosity η*(ω=0.1) (Pa sec) at a frequency ω=0.1 rad / s to the complex viscosity η*(ω=100) (Pa sec) at a frequency ω=100 rad / s, obtained by linear viscoelastic measurement (190°C) using a rheometer, the intrinsic viscosity [η], and the weight fraction of the constitutional unit derived from non-conjugated polyene (XC) (weight fraction of (XC)) satisfy the following formula (Z). 2.5≦P / ([η] 2.9 )≦(XC) weight fraction × 4 (Z)
[0021] (i) The requirement (i) specifies that the molar ratio of ethylene (XA) / α-olefin (XB) in the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention satisfies 50 / 50 to 80 / 20, and this molar ratio preferably satisfies 50 / 50 to 90 / 10, more preferably 55 / 45 to 85 / 15, and further preferably 55 / 45 to 78 / 22. When such an ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention is used as a raw material for a crosslinked molded article, the resulting crosslinked molded article exhibits excellent rubber elasticity and is excellent in mechanical strength and flexibility, which is preferable.
[0022] The amount of ethylene (weight fraction of the constitutional unit derived from ethylene (XA)) and the amount of α-olefin (weight fraction of the constitutional unit derived from α-olefin (XB)) in the ethylene-α-olefin-non-conjugated polyene copolymer (1) are 13 It can be determined by C-NMR.
[0023] (ii) Requirement (ii) specifies that the weight fraction of the constituent units derived from the non-conjugated polyene (XC) is in the range of 0.07 to 10% by weight, assuming that the weight fraction of all constituent units of the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention is 100% by weight. The weight fraction of the constituent units derived from this non-conjugated polyene (XC) is preferably 0.1 to 8.0% by weight, more preferably 0.5 to 5.0% by weight.
[0024] When the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention satisfies the requirement (ii), the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention has sufficient hardness and excellent mechanical properties, which is preferable, and when crosslinked using a peroxide, the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention exhibits a fast crosslinking rate and is suitable for producing a crosslinked molded article, which is preferable.
[0025] The amount of non-conjugated polyene (XC) in the ethylene-α-olefin-non-conjugated polyene copolymer (1) (weight fraction of the constitutional unit derived from non-conjugated polyene (XC)) is 13 It can be determined by C-NMR.
[0026] (iii) The requirement (iii) specifies that the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention has an intrinsic viscosity [η] of 5.1 to 7.0 dL / g. The ethylene-α-olefin-non-conjugated polyene copolymer (1) which satisfies the other requirements of the present invention and has an intrinsic viscosity in this range is particularly excellent in processability, improves the efficiency of molding processing, and can be used for molded products for many applications.
[0027] The ethylene / α-olefin / non-conjugated polyene copolymer (1) of the present invention preferably has an intrinsic viscosity [η] of 5.5 to 6.5 dL / g, more preferably 5.5 to 6.0 dL / g.
[0028] The ethylene / α-olefin / non-conjugated polyene copolymer (1) of the present invention preferably has a weight average molecular weight (Mw) of 300,000 to 2,500,000, and more preferably 500,000 to 2,000,000. The ethylene / α-olefin / non-conjugated polyene copolymer of the present invention preferably satisfies both of the above-mentioned intrinsic viscosity [η] and weight average molecular weight (Mw).
[0029] (iv) The requirement (iv) is that the complex viscosity η of the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention is measured by linear viscoelasticity at 190°C using a rheometer at a frequency of ω = 0.1 rad / s. * (ω=0.1)(Pa·sec) and complex viscosity η at frequency ω=100rad / s * (ω=100)(Pa·sec) P(η * (ω=0.1) / η *(ω=100), the intrinsic viscosity [η], and the weight fraction of the constitutional unit derived from the non-conjugated polyene (XC) (weight fraction of (XC): weight %) satisfy the following formula (Z). 2.5≦P / ([η] 2.9 )≦(XC) weight fraction × 4 (Z)
[0030] Here, the complex viscosity η at frequency ω=0.1rad / s * (ω=0.1) and the complex viscosity η at frequency ω=100rad / s * (ω=100) P(η * (ω=0.1) / η * (ω=100)) represents the frequency dependence of viscosity, and is the left side of equation (Z) P / ([η] 2.9 ) tends to show a high value when there is a large amount of long chain branching, although it is influenced by factors such as short chain branching and molecular weight. Generally, in an ethylene-α-olefin-non-conjugated polyene copolymer, the more structural units derived from non-conjugated polyenes it contains, the more long chain branching it tends to have. However, the ethylene-α-olefin-non-conjugated polyene copolymer of the present invention has fewer long chain branches than the conventionally known ethylene-α-olefin-non-conjugated polyene copolymers, and is therefore considered to be able to satisfy the above formula (Z). In the present invention, the P value is calculated by calculating the ratio (η) of the complex viscosity at 0.1 rad / s and the complex viscosity at 100 rad / s, which are determined by performing measurements at 190°C, strain 1.0%, and various frequencies using a viscoelasticity measuring device Ares (manufactured by Rheometric Scientific Co., Ltd.). * The ratio of
[0031] The ethylene / α-olefin / non-conjugated polyene copolymer (1) of the present invention preferably satisfies the following formula (Z′): P / ([η] 2.9 )≦(XC) weight fraction × 5.7 … formula (Z') The intrinsic viscosity [η] means a value measured in decalin at 135°C.
[0032] As described above, the ethylene-α-olefin-non-conjugated polyene copolymer of the present invention preferably contains, in addition to the structural units derived from the above ethylene (XA), α-olefin (XB) and non-conjugated polyene (XC), a structural unit derived from a non-conjugated polyene (XD) containing only one partial structure selected from the group consisting of the general formulae (I) and (II) in the molecule, in a weight fraction of 0 to 20% by weight (wherein the total weight fractions of ethylene (XA), α-olefin (XB), non-conjugated polyene (XC) and non-conjugated polyene (XD) is taken as 100% by weight). The ethylene (XA), the α-olefin (XB), the non-conjugated polyene (XC) and the non-copolyene (XD) may each be derived from biomass.
[0033] The apparent iodine value derived from non-conjugated polyene (XC) is calculated by the following formula: Such an ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention is preferable because the content of structural units derived from a non-conjugated polyene (XD) such as ENB is controlled within a range that does not impair the object of the present invention, it is less likely to cause post-crosslinking, and has sufficient heat aging resistance.
[0034] Here, the number of constitutional units derived from the non-conjugated polyene (XC) per weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer (1) (n c ) or the number of constitutional units derived from non-conjugated polyenes (XC) (n D ) can be calculated from the molecular weight of the non-conjugated polyene (XC) or (XD), the weight fraction of the structural unit derived from the non-conjugated polyene (XC) or (XD) in the copolymer (weight fraction (weight %) of (XC) or (XD)), and the weight average molecular weight (Mw) of the copolymer, according to the following formula. (n c )=(Mw)×{weight fraction of (XC) / 100} / molecular weight of non-conjugated polyene (XC) (n D )=(Mw)×{weight fraction of (XD) / 100} / molecular weight of non-conjugated polyene (XD)
[0035] The ethylene-α-olefin-non-conjugated polyene copolymer of the present invention has a weight average molecular weight (Mw) of 100% or more and a number (n c ) and (n D ) satisfy the above ranges, the ethylene-α-olefin-non-conjugated polyene copolymer (1) is preferable because it has a low content of long chain branches, is excellent in hardening characteristics when crosslinking is performed using a peroxide, has good moldability, and is excellent in balance of physical properties such as mechanical properties, is less likely to cause post-crosslinking, and is particularly excellent in heat aging resistance.
[0036] <Production of ethylene-α-olefin-non-conjugated polyene copolymer (1)> The ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention is a copolymer obtained by copolymerizing monomers consisting of ethylene (XA), an α-olefin (XB) having 3 to 20 carbon atoms, a non-conjugated polyene (XC) containing in the molecule a total of two or more partial structures selected from the group consisting of the general formulae (I) and (II), and, if necessary, a non-conjugated polyene (XD) containing in the molecule only one partial structure selected from the group consisting of the general formulae (I) and (II).
[0037] The ethylene / α-olefin / non-conjugated polyene copolymer (1) of the present invention may be prepared by any method as long as it satisfies the above-mentioned requirements (i) to (iv). However, it is preferable that the copolymer is obtained by copolymerizing monomers in the presence of a metallocene compound, and it is more preferable that the copolymer is obtained by copolymerizing monomers in the presence of a catalyst system containing a metallocene compound.
[0038] Metallocene Compounds The ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention is preferably one obtained by copolymerizing monomers in the presence of at least one metallocene compound selected from the compounds represented by the following general formula [A-2]. When the copolymerization of monomers is carried out using a catalyst system containing such a metallocene compound, the long chain branching contained in the obtained copolymer is suppressed, and the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention that satisfies the above-mentioned requirements can be easily prepared.
[0039] [ka]
[0040] In the formula [A-2], M is a titanium atom, a zirconium atom, or a hafnium atom, n is an integer of 1 to 3, each X is independently a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group, and R 1 ~R 5 and R 6 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 1 ~R 5 Adjacent groups among these may be bonded to each other to form a ring.
[0041] Examples of the hydrocarbon group having 1 to 20 carbon atoms include an alkyl group having 1 to 20 carbon atoms, a cyclic saturated hydrocarbon group having 3 to 20 carbon atoms, a linear unsaturated hydrocarbon group having 2 to 20 carbon atoms, and a cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms.
[0042] Examples of the alkyl group having 1 to 20 carbon atoms include linear saturated hydrocarbon groups such as methyl, ethyl, n-propyl, allyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decanyl, and branched saturated hydrocarbon groups such as isopropyl, isobutyl, s-butyl, t-butyl, t-amyl, neopentyl, 3-methylpentyl, 1,1-diethylpropyl, 1,1-dimethylbutyl, 1-methyl-1-propylbutyl, 1,1-dipropylbutyl, 1,1-dimethyl-2-methylpropyl, 1-methyl-1-isopropyl-2-methylpropyl, and cyclopropylmethyl. The alkyl group preferably has 1 to 6 carbon atoms.
[0043] Examples of cyclic saturated hydrocarbon groups having 3 to 20 carbon atoms include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, norbornenyl, 1-adamantyl, and 2-adamantyl groups, as well as groups in which the hydrogen atoms of these cyclic saturated hydrocarbon groups are replaced with hydrocarbon groups having 1 to 17 carbon atoms, such as 3-methylcyclopentyl, 3-methylcyclohexyl, 4-methylcyclohexyl, 4-cyclohexylcyclohexyl, and 4-phenylcyclohexyl groups. The number of carbon atoms in the cyclic saturated hydrocarbon group is preferably 5 to 11.
[0044] Examples of the linear unsaturated hydrocarbon group having 2 to 20 carbon atoms include alkenyl groups such as ethenyl group (vinyl group), 1-propenyl group, 2-propenyl group (allyl group), 1-methylethenyl group (isopropenyl group), etc., and alkynyl groups such as ethynyl group, 1-propynyl group, 2-propynyl group (propargyl group), etc. The number of carbon atoms in the linear unsaturated hydrocarbon group is preferably 2 to 4.
[0045] Examples of cyclic unsaturated hydrocarbon groups having 3 to 20 carbon atoms include cyclopentadienyl, norbornyl, phenyl, naphthyl, indenyl, azulenyl, phenanthryl, and anthracenyl groups, and groups in which hydrogen atoms of these cyclic unsaturated hydrocarbon groups are replaced with hydrocarbon groups having 1 to 15 carbon atoms, such as 3-methylphenyl (m-tolyl), 4-methylphenyl (p-tolyl), 4-ethylphenyl, 4-t-butylphenyl, 4-cyclohexylphenyl, biphenylyl, 3,4-dimethylphenyl, 3,5-dimethylphenyl, and 2,4,6-trimethylphenyl (mesityl), and groups in which hydrogen atoms of linear or branched saturated hydrocarbon groups are replaced with cyclic saturated or unsaturated hydrocarbon groups having 3 to 19 carbon atoms, such as benzyl and cumyl groups. The number of carbon atoms of the cyclic unsaturated hydrocarbon group is preferably 6 to 10.
[0046] Examples of the alkylene group having 1 to 20 carbon atoms include a methylene group, an ethylene group, a dimethylmethylene group (isopropylidene group), an ethylmethylene group, a 1-methylethylene group, a 2-methylethylene group, a 1,1-dimethylethylene group, a 1,2-dimethylethylene group, an n-propylene group, etc. The number of carbon atoms in the alkylene group is preferably 1 to 6.
[0047] Examples of the arylene group having 6 to 20 carbon atoms include an o-phenylene group, an m-phenylene group, a p-phenylene group, a 4,4'-biphenylylene group, etc. The number of carbon atoms in the arylene group is preferably 6 to 12.
[0048] Examples of the aryl group include, but are not limited to, the above-mentioned examples of the cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms, and are exemplified by substituents derived from aromatic compounds, such as phenyl, 1-naphthyl, 2-naphthyl, anthracenyl, phenanthrenyl, tetracenyl, chrysenyl, pyrenyl, indenyl, azulenyl, pyrrolyl, pyridyl, furanyl, and thiophenyl groups. The aryl group is preferably a phenyl group or a 2-naphthyl group.
[0049] Examples of the aromatic compounds include aromatic hydrocarbons and heterocyclic aromatic compounds such as benzene, naphthalene, anthracene, phenanthrene, tetracene, chrysene, pyrene, indene, azulene, pyrrole, pyridine, furan, and thiophene.
[0050] The substituted aryl group partially overlaps with the examples of the cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms described above, but examples include groups in which one or more hydrogen atoms of the aryl group are substituted with a substituent selected from a hydrocarbon group having 1 to 20 carbon atoms, an aryl group, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a halogen atom, and a halogen-containing group. Specific examples include a 3-methylphenyl group (m-tolyl group), a 4-methylphenyl group (p-tolyl group), a 3-ethylphenyl group, a 4-ethylphenyl group, a 3,4-dimethylphenyl group, a 3,5-dimethylphenyl group, a biphenylyl group, a 4-(trimethylsilyl)phenyl group, a 4-aminophenyl group, a Examples of the aryl group include a 4-(dimethylamino)phenyl group, a 4-(diethylamino)phenyl group, a 4-morpholinylphenyl group, a 4-methoxyphenyl group, a 4-ethoxyphenyl group, a 4-phenoxyphenyl group, a 3,4-dimethoxyphenyl group, a 3,5-dimethoxyphenyl group, a 3-methyl-4-methoxyphenyl group, a 3,5-dimethyl-4-methoxyphenyl group, a 3-(trifluoromethyl)phenyl group, a 4-(trifluoromethyl)phenyl group, a 3-chlorophenyl group, a 4-chlorophenyl group, a 3-fluorophenyl group, a 4-fluorophenyl group, a 5-methylnaphthyl group, and a 2-(6-methyl)pyridyl group. Examples of the substituted aryl group include an "electron-donating group-containing substituted aryl group" described later.
[0051] Examples of the silicon-containing group include alkylsilyl groups such as trimethylsilyl group, triethylsilyl group, t-butyldimethylsilyl group, and triisopropylsilyl group, which are groups in which carbon atoms in a hydrocarbon group having 1 to 20 carbon atoms are replaced with silicon atoms, arylsilyl groups such as dimethylphenylsilyl group, methyldiphenylsilyl group, and t-butyldiphenylsilyl group, pentamethyldisilanyl group, and trimethylsilylmethyl group, etc. The number of carbon atoms in the alkylsilyl group is preferably 1 to 10, and the number of carbon atoms in the arylsilyl group is preferably 6 to 18. Examples of the nitrogen-containing group include an amino group, a nitro group, an N-morpholinyl group, and a dimethylamino group, which is a group in which the =CH- structural unit in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms or silicon-containing group is replaced with a nitrogen atom, a group in which the -CH2- structural unit is replaced with a nitrogen atom to which a hydrocarbon group having 1 to 20 carbon atoms is bonded, or a group in which the -CH3 structural unit is replaced with a nitrogen atom or a nitrile group to which a hydrocarbon group having 1 to 20 carbon atoms is bonded, such as a dimethylamino group, a diethylamino group, a dimethylaminomethyl group, a cyano group, a pyrrolidinyl group, a piperidinyl group, a pyridinyl group, etc. As the nitrogen-containing group, a dimethylamino group or an N-morpholinyl group is preferable.
[0052] Examples of the oxygen-containing group include a hydroxyl group, a group in which the -CH2- structural unit in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms, silicon-containing group or nitrogen-containing group is replaced with an oxygen atom or a carbonyl group, or a group in which the -CH3 structural unit is replaced with an oxygen atom bonded to a hydrocarbon group having 1 to 20 carbon atoms, such as a methoxy group, ethoxy group, t-butoxy group, phenoxy group, trimethylsiloxy group, methoxyethoxy group, hydroxymethyl group, methoxymethyl group, ethoxymethyl group, t-butoxymethyl group, 1-hydroxyethyl group, Examples of the oxygen-containing group include 1-methoxyethyl group, 1-ethoxyethyl group, 2-hydroxyethyl group, 2-methoxyethyl group, 2-ethoxyethyl group, n-2-oxabutylene group, n-2-oxapentylene group, n-3-oxapentylene group, aldehyde group, acetyl group, propionyl group, benzoyl group, trimethylsilylcarbonyl group, carbamoyl group, methylaminocarbonyl group, carboxy group, methoxycarbonyl group, carboxymethyl group, ethoxycarboxymethyl group, carbamoylmethyl group, furanyl group, pyranyl group, etc. As the oxygen-containing group, a methoxy group is preferable.
[0053] Examples of halogen atoms include Group 17 elements such as fluorine, chlorine, bromine, and iodine. Examples of the halogen-containing group include a trifluoromethyl group, a tribromomethyl group, a pentafluoroethyl group, a pentafluorophenyl group, and the like, which are groups in which a hydrogen atom in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms, silicon-containing group, nitrogen-containing group, or oxygen-containing group is substituted with a halogen atom.
[0054] R 6 As the alkyl group, a cyclic saturated hydrocarbon group is preferable, and an adamantyl group is particularly preferable. Each symbol in formula [A-2] is as defined in formula [A-1]. Specific examples of the phosphinimine moiety in the above formula [A-2] are shown below.
[0055] [ka]
[0056] When polymerizing the ethylene·α-olefin·non-conjugated polyene copolymer (1) using the transition metal compound (A), at least one compound selected from the group consisting of (B-1) an organometallic compound, (B-2) an organoaluminum oxy compound, and (B-3) a compound that reacts with the transition metal compound (A) to form an ion pair can be used in combination with the transition metal compound (A). Hereinafter, each of these components will be described.
[0057] ((B-1) Organometallic compound) Specific examples of the organometallic compound (B-1) used in the present invention include compounds containing at least one element of Groups 1, 2, 12, and 13 of the periodic table represented by the following general formulas (B-1a) to (B-1c):
[0058] R a p Al(ОR b ) q H r Y s ···(B-1a) (In the general formula (B-1a), R a and R b may be the same or different from each other and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, Y represents a halogen atom, p is a number where 0 < p ≤ 3, q is a number where 0 ≤ q < 3, r is a number where 0 ≤ r < 3, s is a number where 0 ≤ s < 3, and m + n + p + q = 3.) An organoaluminum compound represented by;
[0059] M 3 AlR c 4···(B-1b) (In the general formula (B-1b), M 3 represents Li, Na or K, and R c represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms.) A complex alkyl compound of an alkali metal of Group 1 of the periodic table and aluminum represented by;
[0060] R d R e M 4···(B-1c) (In general formula (B-1c), R d and R e may be the same as or different from each other and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, and M 4 is Mg, Zn or Cd.) A dialkyl compound with an alkaline earth metal of Group 2 or a metal of Group 12 of the periodic table represented by
[0061] Examples of the organoaluminum compound belonging to the general formula (B-1a) include the following compounds. R a p Al(ОR b ) 3-p ···(B-1a-1) (In formula (B-1a-1), R a and R b may be the same as or different from each other and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, and p is preferably a number such that 1.5 ≦ p ≦ 3.) An organoaluminum compound represented by R a p AlY 3-p ···(B-1a-2) (In formula (B-1a-2), R a represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, Y represents a halogen atom, and p is preferably a number such that 0 < p < 3.) An organoaluminum compound represented by R a p AlH 3-p ···(B-1a-3) (In formula (B-1a-3), R a represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, and p is preferably a number such that 2 ≦ p < 3.) An organoaluminum compound represented by R a p Al(ОR b ) q Y s ···(B-1a-4) (In formula (B-1a-4), R a and R bmay be the same as or different from each other, and represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms. Y represents a halogen atom, p is a number such that 0 < p ≦ 3, q is a number such that 0 ≦ q < 3, s is a number such that 0 ≦ s < 3, and p + q + s = 3.) An organoaluminum compound represented by.
[0062] More specifically, as the organoaluminum compound belonging to the general formula (B-1a), tri-n-alkylaluminums such as trimethylaluminum, triethylaluminum, tri-n-butylaluminum, tripropylaluminum, tripentylaluminum, trihexylaluminum, trioctylaluminum, tridecylaluminum; Tri-branched chain alkylaluminums such as triisopropylaluminum, triisobutylaluminum, tri-sec-butylaluminum, tri-tert-butylaluminum, tri-2-methylbutylaluminum, tri-3-methylbutylaluminum, tri-2-methylpentylaluminum, tri-3-methylpentylaluminum, tri-4-methylpentylaluminum, tri-2-methylhexylaluminum, tri-3-methylhexylaluminum, tri-2-ethylhexylaluminum; Tricycloalkylaluminums such as tricyclohexylaluminum, tricyclooctylaluminum; Triarylaluminums such as triphenylaluminum, tritolylaluminum; Dialkylaluminum hydrides such as diisobutylaluminum hydride;
[0063] (i-C4H9) x Al y (C5H 10 ) z (In the formula, x, y, and z are positive numbers, and z ≧ 2x.) Trialkenylaluminums such as triisoprenylaluminum represented by etc.; Alkylaluminum alkoxides such as isobutylaluminum methoxide, isobutylaluminum ethoxide, isobutylaluminum isopropoxide; Dialkylaluminum alkoxides such as dimethylaluminum methoxide, diethylaluminum ethoxide, and dibutylaluminum butoxide; Alkyl aluminum sesquialkoxides such as ethyl aluminum sesquiethoxide, butyl aluminum sesquibutoxide;
[0064] R a 2.5 Al(OR b ) 0.5 Partially alkoxylated alkylaluminum having an average composition represented by the formula: a and R b may be the same or different and represent a hydrocarbon group having 1 to 15, preferably 1 to 4, carbon atoms; dialkylaluminum aryloxides such as diethylaluminum phenoxide, diethylaluminum (2,6-di-t-butyl-4-methylphenoxide), ethylaluminum bis(2,6-di-t-butyl-4-methylphenoxide), diisobutylaluminum (2,6-di-t-butyl-4-methylphenoxide), and isobutylaluminum bis(2,6-di-t-butyl-4-methylphenoxide); Dialkylaluminum halides such as dimethylaluminum chloride, diethylaluminum chloride, dibutylaluminum chloride, diethylaluminum bromide, and diisobutylaluminum chloride; Alkyl aluminum sesquihalides such as ethyl aluminum sesquichloride, butyl aluminum sesquichloride, and ethyl aluminum sesquibromide; partially halogenated alkylaluminums, such as alkylaluminum dihalides, such as ethylaluminum dichloride, propylaluminum dichloride, butylaluminum dibromide, and the like; Dialkylaluminum hydrides such as diethylaluminum hydride and dibutylaluminum hydride; Other partially hydrogenated alkylaluminums, such as alkylaluminum dihydrides, such as ethylaluminum dihydride, propylaluminum dihydride, etc.; Examples of the aluminum compounds include partially alkoxylated and halogenated alkylaluminum compounds such as ethylaluminum ethoxy chloride, butylaluminum butoxy chloride, and ethylaluminum ethoxy bromide.
[0065] Compounds similar to (B-1a) can also be used in the present invention, such as organoaluminum compounds in which two or more aluminum compounds are bonded via nitrogen atoms, such as (C2H5)2AlN(C2H5)Al(C2H5)2.
[0066] The compounds belonging to the general formula (B-1b) include LiAl(C2H5)4, LiAl(C7H 15 )4 can be mentioned as examples.
[0067] Examples of the compound belonging to the general formula (B-1c) include dimethylmagnesium, diethylmagnesium, dibutylmagnesium, butylethylmagnesium, dimethylzinc, diethylzinc, diphenylzinc, di-n-propylzinc, diisopropylzinc, di-n-butylzinc, diisobutylzinc, bis(pentafluorophenyl)zinc, dimethylcadmium, and diethylcadmium.
[0068] In addition, as the organometallic compound (B-1), methyllithium, ethyllithium, propyllithium, butyllithium, methylmagnesium bromide, methylmagnesium chloride, ethylmagnesium bromide, ethylmagnesium chloride, propylmagnesium bromide, propylmagnesium chloride, butylmagnesium bromide, butylmagnesium chloride, etc. can also be used.
[0069] Furthermore, a compound which forms the above-mentioned organoaluminum compound in the polymerization system, such as a combination of an aluminum halide and an alkyllithium, or a combination of an aluminum halide and an alkylmagnesium, can also be used as the organometallic compound (B-1).
[0070] Among the organometallic compounds (B-1), organoaluminum compounds are preferred from the standpoint of catalytic activity. The organometallic compounds (B-1) as described above may be used singly or in combination of two or more kinds.
[0071] ((B-2) Organoaluminum oxy compound) The organoaluminum oxy compound (B-2) used in the present invention may be a conventionally known aluminoxane, or may be a benzene-insoluble organoaluminum oxy compound such as those exemplified in JP-A-2-78687. Conventionally known aluminoxanes can be produced, for example, by the following method, and are usually obtained as a solution in a hydrocarbon solvent.
[0072] (a) A method in which an organoaluminum compound such as trialkylaluminum is added to a hydrocarbon medium suspension of a compound containing adsorbed water or a salt containing water of crystallization, such as magnesium chloride hydrate, copper sulfate hydrate, aluminum sulfate hydrate, nickel sulfate hydrate, or cerous chloride hydrate, to react the adsorbed water or the water of crystallization with the organoaluminum compound. (b) A method in which water, ice or water vapor is directly reacted with an organoaluminum compound such as trialkylaluminum in a medium such as benzene, toluene, ethyl ether or tetrahydrofuran. (c) A method in which an organoaluminum compound such as trialkylaluminum is reacted with an organotin oxide such as dimethyltin oxide or dibutyltin oxide in a medium such as decane, benzene, or toluene.
[0073] The aluminoxane may contain a small amount of an organometallic component. After the solvent or unreacted organoaluminum compound is removed by distillation from the recovered aluminoxane solution, the resulting aluminoxane may be redissolved in a solvent or suspended in a poor solvent for the aluminoxane.
[0074] Specific examples of the organoaluminum compound used in preparing the aluminoxane include the same organoaluminum compounds as those exemplified as the organoaluminum compounds belonging to the general formula (B-1a) above.
[0075] Of these, trialkylaluminum and tricycloalkylaluminum are preferred, with trimethylaluminum being particularly preferred. The above organoaluminum compounds may be used singly or in combination of two or more.
[0076] Examples of the solvent used in the preparation of aluminoxane include aromatic hydrocarbons such as benzene, toluene, xylene, cumene, and cymene; aliphatic hydrocarbons such as pentane, hexane, heptane, octane, decane, dodecane, hexadecane, and octadecane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, cyclooctane, and methylcyclopentane; petroleum fractions such as gasoline, kerosene, and diesel; and halides of the above aromatic hydrocarbons, aliphatic hydrocarbons, and alicyclic hydrocarbons, especially chlorinated and brominated hydrocarbons. Furthermore, ethers such as ethyl ether and tetrahydrofuran can also be used. Among these solvents, aromatic hydrocarbons or aliphatic hydrocarbons are particularly preferred. These solvents can be used alone or in combination.
[0077] The organoaluminum oxy compound (B-2) according to the present invention includes at least one selected from aluminoxanes having a structure represented by the following general formula (B-2a) or (B-2b), and aluminoxanes having a structure comprising a repeating unit represented by the following general formula (B-2c) and a repeating unit represented by the following general formula (B-2d).
[0078] [ka] (In the general formula, R and R c are each independently a hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms, and specific examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, an isopropenyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, an octyl group, a decyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, a cyclohexyl group, a cyclooctyl group, a phenyl group, a tolyl group, and an ethylphenyl group. Among these examples, a methyl group, an ethyl group, and an isobutyl group are preferred, and a methyl group is particularly preferred, and in the general formulae (B-2a), (B-2b), and (B-2c), R c may be partially substituted with halogen atoms such as chlorine and bromine atoms, and the halogen content may be 40% by weight or less.
[0079] In the general formulae (B-2a) and (B-2b), r represents an integer of 2 to 500, preferably 6 to 300, and particularly preferably 10 to 100. In the general formulae (B-2c) and (B-2d), s and t each represent an integer of 1 or more.
[0080] The aluminoxane having a repeating unit represented by the general formula (B-2c) and a repeating unit represented by the general formula (B-2d) preferably has a molecular weight in the range of 200 to 2000 as measured by cryoscopic method in benzene.
[0081] The benzene-insoluble organoaluminum oxy-compound used in the present invention is preferably one in which the Al component dissolved in benzene at 60°C is usually 10% or less, preferably 5% or less, and particularly preferably 2% or less, calculated as Al atom, i.e., it is preferably insoluble or poorly soluble in benzene.
[0082] The organoaluminum oxy compound (B-2) used in the present invention may also include boron-containing organoaluminum oxy compounds represented by the following general formula (B-2e).
[0083] [ka] (In general formula (B-2e), R 15 represents a hydrocarbon group having 1 to 10 carbon atoms, and four R 16 may be the same or different, and each independently represents a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms.)
[0084] The boron-containing organoaluminum oxy compound represented by the general formula (B-2e) can be produced by reacting an alkylboronic acid represented by the following general formula (B-2f) with an organoaluminum compound in an inert solvent under an inert gas atmosphere at a temperature of −80° C. to room temperature for 1 minute to 24 hours. R 15 -B(OH)2···(B-2f) (In general formula (B-2f), R 15 is R in the general formula (B-2e) 15 It shows the same group as
[0085] Specific examples of the alkylboronic acid represented by the general formula (B-2f) include methylboronic acid, ethylboronic acid, isopropylboronic acid, n-propylboronic acid, n-butylboronic acid, isobutylboronic acid, n-hexylboronic acid, cyclohexylboronic acid, phenylboronic acid, 3,5-difluoroboronic acid, pentafluorophenylboronic acid, and 3,5-bis(trifluoromethyl)phenylboronic acid. Among these, methylboronic acid, n-butylboronic acid, isobutylboronic acid, 3,5-difluorophenylboronic acid, and pentafluorophenylboronic acid are preferred. These are used alone or in combination of two or more.
[0086] Specific examples of the organoaluminum compound to be reacted with such an alkylboronic acid include the same organoaluminum compounds as those exemplified as the organoaluminum compounds belonging to the above general formula (B-1a).
[0087] The organoaluminum compound is preferably a trialkylaluminum or a tricycloalkylaluminum, more preferably a trimethylaluminum, a triethylaluminum or a triisobutylaluminum, which may be used alone or in combination of two or more.
[0088] When an organoaluminum oxy compound (B-2) such as methylaluminoxane is used as a cocatalyst component in addition to the transition metal compound (A), extremely high polymerization activity for olefin compounds is exhibited. The above organoaluminum oxy compounds (B-2) may be used singly or in combination of two or more.
[0089] ((B-3) A compound that reacts with a transition metal compound (A) to form an ion pair) Examples of the compound (B-3) (hereinafter referred to as "ionized ionic compound") used in the present invention that reacts with the transition metal compound (A) to form an ion pair include Lewis acids, ionic compounds, borane compounds, and carborane compounds described in JP-T-1-501950, JP-T-1-502036, JP-A-3-179005, JP-A-3-179006, JP-A-3-207703, JP-A-3-207704, and US-5321106. Furthermore, heteropoly compounds and isopoly compounds can also be mentioned.
[0090] Specifically, the Lewis acid includes a compound represented by BR3 (R is fluorine or a phenyl group which may have a substituent such as fluorine, a methyl group, or a trifluoromethyl group), such as trifluoroboron, triphenylboron, tris(4-fluorophenyl)boron, tris(3,5-difluorophenyl)boron, tris(4-fluoromethylphenyl)boron, tris(pentafluorophenyl)boron, tris(p-tolyl)boron, tris(o-tolyl)boron, and tris(3,5-dimethylphenyl)boron.
[0091] The ionic compound may, for example, be a compound represented by the following general formula (B-3a).
[0092] [ka] (In general formula (B-3a), R 17 H + , a carbonium cation, an oxonium cation, an ammonium cation, a phosphonium cation, a cycloheptyltrienyl cation or a ferrocenium cation having a transition metal, and R 18 ~R 21 may be the same or different and are organic groups, preferably aryl groups or substituted aryl groups.
[0093] Specific examples of the carbonium cation include tri-substituted carbonium cations such as triphenylcarbonium cation, tri(methylphenyl)carbonium cation, and tri(dimethylphenyl)carbonium cation.
[0094] Specific examples of the ammonium cation include trialkylammonium cations such as trimethylammonium cation, triethylammonium cation, tripropylammonium cation, tributylammonium cation, and tri(n-butyl)ammonium cation; N,N-dialkylanilinium cations such as N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N-2,4,6-pentamethylanilinium cation; and dialkylammonium cations such as di(isopropyl)ammonium cation and dicyclohexylammonium cation.
[0095] Specific examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tri(methylphenyl)phosphonium cation, and tri(dimethylphenyl)phosphonium cation.
[0096] R 17 As the cation, a carbonium cation and an ammonium cation are preferred, and in particular, a triphenylcarbonium cation, an N,N-dimethylanilinium cation, and an N,N-diethylanilinium cation are preferred.
[0097] Further, examples of the ionic compound include trialkyl-substituted ammonium salts, N,N-dialkylanilinium salts, dialkylammonium salts, and triarylphosphonium salts.
[0098] Specific examples of the trialkyl-substituted ammonium salt include triethylammonium tetra(phenyl)boron, tripropylammonium tetra(phenyl)boron, tri(n-butyl)ammonium tetra(phenyl)boron, trimethylammonium tetra(p-tolyl)boron, trimethylammonium tetra(o-tolyl)boron, tri(n-butyl)ammonium tetra(pentafluorophenyl)boron, tripropylammonium tetra(o,p-dimethylphenyl)boron, tri(n-butyl)ammonium tetra(m,m-dimethylphenyl)boron, tri(n-butyl)ammonium tetra(p-trifluoromethylphenyl)boron, tri(n-butyl)ammonium tetra(3,5-ditrifluoromethylphenyl)boron, and tri(n-butyl)ammonium tetra(o-tolyl)boron.
[0099] Specific examples of the N,N-dialkylanilinium salt include N,N-dimethylanilinium tetra(phenyl)boron, N,N-diethylanilinium tetra(phenyl)boron, and N,N,2,4,6-pentamethylanilinium tetra(phenyl)boron.
[0100] Specific examples of the dialkylammonium salt include di(1-propyl)ammonium tetra(pentafluorophenyl)boron, dicyclohexylammonium tetra(phenyl)boron, and the like.
[0101] Further examples of the ionic compound include triphenylcarbenium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, ferrocenium tetra(pentafluorophenyl)borate, triphenylcarbenium pentaphenylcyclopentadienyl complex, N,N-diethylanilinium pentaphenylcyclopentadienyl complex, and boron compounds represented by the following formula (B-3b) or (B-3c).
[0102] [ka] (In formula (B-3b), Et represents an ethyl group.)
[0103] [ka] (In formula (B-3c), Et represents an ethyl group.)
[0104] Specific examples of the borane compound, which is an example of the ionizable ionic compound (compound (B-3)), include decaborane; Salts of anions such as bis[tri(n-butyl)ammonium]nonaborate, bis[tri(n-butyl)ammonium]decaborate, bis[tri(n-butyl)ammonium]undecaborate, bis[tri(n-butyl)ammonium]dodecaborate, bis[tri(n-butyl)ammonium]decachlorodecaborate, and bis[tri(n-butyl)ammonium]dodecachlorododecaborate; Examples of the salt include salts of metal borane anions such as tri(n-butyl)ammonium bis(dodecahydride dodecaborate) cobaltate(III) and bis[tri(n-butyl)ammonium]bis(dodecahydride dodecaborate) nickelate(III).
[0105] Specific examples of carborane compounds, which are examples of ionizable ionic compounds, include 4-carbanonaborane, 1,3-dicarbanonaborane, 6,9-dicarbadecaborane, dodecahydride-1-phenyl-1,3-dicarbanonaborane, dodecahydride-1-methyl-1,3-dicarbanonaborane, undecahydride-1,3-dimethyl-1,3-dicarbanonaborane, 7,8-dicarbaundecaborane, 2,7-dicarbaundecaborane, and undecahydride-7,8-dimethyl-1,3-dicarbanonaborane. 1-methyl-7,8-dicarboxylic acid borane, dodecahydride-11-methyl-2,7-dicarboxylic acid borane, tri(n-butyl)ammonium 1-carbadecaborate, tri(n-butyl)ammonium 1-carbaundecaborate, tri(n-butyl)ammonium 1-carbadodecaborate, tri(n-butyl)ammonium 1-trimethylsilyl-1-carbadecaborate, tri(n-butyl)ammonium bromo-1-carbadodecaborate, tri(n-butyl)ammonium ammonium 6-carbadecaborate, tri(n-butyl)ammonium 6-carbadecaborate, tri(n-butyl)ammonium 7-carbaundecaborate, tri(n-butyl)ammonium 7,8-dicaundecaborate, tri(n-butyl)ammonium 2,9-dicaundecaborate, tri(n-butyl)ammonium dodecahydride-8-methyl-7,9-dicaundecaborate, tri(n-butyl)ammonium undecahydride-8-ethyl-7,9-dicaundecaborate Salts of anions such as undecahydride, tri(n-butyl)ammonium undecahydride-8-butyl-7,9-dicarboxaborate, tri(n-butyl)ammonium undecahydride-8-allyl-7,9-dicarboxaborate, tri(n-butyl)ammonium undecahydride-9-trimethylsilyl-7,8-dicarboxaborate, tri(n-butyl)ammonium undecahydride-4,6-dibromo-7-carbaundecaborate; Tri(n-butyl)ammonium bis(nonahydride-1,3-dicarbanonaborate)cobaltate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)ferrate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)cobaltate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)nickelate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)cuprate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)aurate(III), tri(n-butyl)ammonium bis(nonahydride-7,8-dimethyl-7,8-dicarbandecaborate)ferrate salt (III), tri(n-butyl)ammonium bis(nonahydride-7,8-dimethyl-7,8-dicarboxaborate)chromate (III), tri(n-butyl)ammonium bis(tribromooctahydride-7,8-dicarboxaborate)cobaltate (III), tris[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)chromate (III), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)manganate (IV), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)cobaltate (III), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)nickelate (IV), and the like.
[0106] Heteropoly compounds, which are examples of ionized ionic compounds, are compounds that contain an atom selected from silicon, phosphorus, titanium, germanium, arsenic and tin, and one or more atoms selected from vanadium, niobium, molybdenum and tungsten.Specific examples include, but are not limited to, phosphovanadic acid, germanovanadic acid, arsenic vanadic acid, phosphoniobic acid, germanoniobic acid, siliconomybdic acid, phosphomolybdic acid, titanomolybdic acid, germanomolybdic acid, arsenic molybdic acid, tinmolybdic acid, phosphotungstic acid, germanotungstic acid, tintungstic acid, phosphomolybdovanadic acid, phosphotungstovanadic acid, germanotungstovanadic acid, phosphomolybdotungstovanadic acid, germanomolybdotungstovanadic acid, phosphomolybdotungstic acid, phosphomolybdoniobic acid, and the salts of these acids. Examples of the salts include salts of the acids with, for example, alkali metals of Group 1 or alkaline earth metals of Group 2 of the periodic table, specifically, lithium, sodium, potassium, rubidium, cesium, beryllium, magnesium, calcium, strontium, barium, etc., and organic salts such as triphenylethyl salts.
[0107] Isopoly compounds, which are examples of ionized ionic compounds, are compounds composed of metal ions of one type of atom selected from vanadium, niobium, molybdenum, and tungsten, and can be considered to be molecular ion species of metal oxides.Specific examples include, but are not limited to, vanadic acid, niobic acid, molybdic acid, tungstic acid, and salts of these acids.Furthermore, examples of the salts include salts of the acids with metals of Group 1 or 2 of the periodic table, specifically, lithium, sodium, potassium, rubidium, cesium, beryllium, magnesium, calcium, strontium, barium, etc., and organic salts such as triphenylethyl salts.
[0108] The above-mentioned ionizing ionic compound (compound (B-3) which reacts with the transition metal compound (A) to form an ion pair) may be used alone or in combination of two or more kinds. The olefin polymerization catalyst according to the present invention may contain the above-mentioned transition metal compound (A) (hereinafter may be abbreviated as "component (A)"), and at least one compound (B) (hereinafter may be abbreviated as "component (B)") selected from the group consisting of organometallic compounds (B-1), organoaluminum oxy compounds (B-2), and ionizing ionic compounds (B-3), and may also contain the following support (C) as necessary.
[0109] [(C) Carrier] The carrier (C) used in the present invention is an inorganic or organic compound, and is a granular or fine particle solid. By supporting the transition metal compound (A) and the compound (B) on the carrier (C), a polymer with good morphology can be obtained.
[0110] The inorganic compound is preferably a porous oxide, a solid aluminoxane compound, an inorganic halide, clay, a clay mineral, or an ion-exchangeable layered compound. Specifically, the porous oxide may be SiO2, Al2O3, MgO, ZrO, TiO2, B2O3, CaO, ZnO, BaO, ThO2, etc., or a composite or mixture containing these, and further may be, for example, natural or synthetic zeolite, SiO2-MgO, SiO2-Al2O3, SiO2-TiO2, SiO2-V2O5, SiO2-Cr2O3, SiO2-TiO2-MgO, etc. Among these, the porous oxide is preferably one containing SiO2 and / or Al2O3 as the main component.
[0111] The porous oxide may contain small amounts of carbonates, sulfates, nitrates, and oxides such as Na2CO3, K2CO3, CaCO3, MgCO3, Na2SO4, Al2(SO4)3, BaSO4, KNO3, Mg(NO3)2, Al(NO3)3, Na2O, K2O, and Li2O.
[0112] The properties of such porous oxides vary depending on the type and manufacturing method, but the porous oxides preferably used in the present invention have a particle size of 10 to 300 μm, preferably 20 to 200 μm, and a specific surface area of 50 to 1000 m. 2 / g, preferably 100 to 700m 2 / g and the pore volume is 0.3-3.0 cm 3 / g range. Such a porous oxide is calcined at 100 to 1000°C, preferably 150 to 700°C, as required, before use.
[0113] The solid aluminoxane compound may be at least one selected from the aluminoxanes shown in (B-2a) to (B-2d) above. The solid aluminoxane used in the present invention is different from conventionally known olefin polymerization catalyst supports, and does not contain inorganic solid components such as silica or alumina or organic polymer components such as polyethylene or polystyrene, but is solidified with an alkylaluminum compound as the main component. The term "solid" used in the present invention means that the aluminoxane component (B-2) is substantially maintained in a solid state under the reaction environment in which it is used. More specifically, it means that the component (B) is in a solid state under a specific temperature and pressure environment in an inert hydrocarbon solvent such as hexane or toluene used in the reaction when preparing a solid catalyst component for olefin polymerization by contacting the component (A) with the component (B) as described later. In addition, it is also necessary that the component (B) contained in the catalyst component is in a solid state under a specific temperature and pressure environment in a hydrocarbon solvent such as hexane, heptane, or toluene when suspension polymerization is performed using the solid catalyst component for olefin polymerization prepared using the component (B) as described later. The same applies to bulk polymerization in which polymerization is performed in a liquefied monomer instead of a solvent, and gas-phase polymerization in which polymerization is performed in a monomer gas.
[0114] The easiest method to check whether component (B) is in a solid state under the above environment is to check visually, but it is often difficult to check visually, for example, during polymerization. In that case, it can be judged, for example, from the properties of the polymer powder obtained after polymerization and the state of adhesion to the reactor. Conversely, if the properties of the polymer powder are good and there is little adhesion to the reactor, even if a part of component (B) is eluted to some extent under the polymerization environment, it does not deviate from the gist of the present invention. Examples of indices for judging the properties of the polymer powder include bulk density, particle shape, surface shape, and the degree of presence of amorphous polymers, but from the viewpoint of quantitativeness, polymer bulk density is preferred. The bulk density in the present invention is usually 0.01 to 0.9, preferably 0.05 to 0.6, and more preferably 0.1 to 0.5.
[0115] The solid aluminoxane used in the present invention has a solubility in n-hexane maintained at a temperature of 25° C. of usually 0 to 40 mol %, preferably 0 to 20 mol %, and particularly preferably 0 to 10 mol %.
[0116] The solubility of the solid aluminoxane used in the present invention in n-hexane was determined by adding 2 g of the solid aluminoxane carrier to 50 ml of n-hexane kept at 25°C, stirring for 2 hours, separating the solution using a G-4 glass filter, and measuring the aluminum concentration in the filtrate. Therefore, the solubility is determined as the ratio of aluminum atoms present in the filtrate to the amount of aluminum atoms equivalent to 2 g of the aluminoxane used.
[0117] As the solid aluminoxane according to the present invention, known solid aluminoxanes can be used without limit. Known production methods include, for example, those described in JP-B-7-42301, JP-A-6-220126, JP-A-6-220128, JP-A-11-140113, JP-A-11-310607, JP-A-2000-38410, JP-A-2000-95810, and WO2010 / 55652.
[0118] The average particle size of the solid aluminoxane according to the present invention is generally in the range of 0.01 to 50,000 μm, preferably 1 to 1,000 μm, and particularly preferably 1 to 200 μm. The average particle size of solid aluminoxane is determined by observing the particles with a scanning electron microscope, measuring the particle size of 100 or more particles, and averaging the weights. The particle size of solid aluminoxane was determined by measuring the maximum length of the Pythagorean method from the particle image. That is, the length of the particle image sandwiched between two parallel lines in both the horizontal and vertical directions was measured, and the particle size was calculated using the following formula. Particle size = ((horizontal length) 2 +(Vertical length) 2 ) 0.5
[0119] The weight average particle diameter of the solid aluminoxane is calculated from the particle diameter calculated above according to the following formula. Average particle size=Σnd 4 / Σnd 3 (where n is the number of particles and d is the particle size)
[0120] The solid aluminoxane preferably used in the present invention has a specific surface area of 50 to 1000 m 2 / g, preferably 100 to 800m 2 / g and the pore volume is 0.1-2.5 cm 3 / g is preferable.
[0121] As the inorganic halide, MgCl2, MgBr2, MnCl2, MnBr2, etc. can be used. The inorganic halide can be used as it is, or can be used after being pulverized by a ball mill or a vibration mill. In addition, the inorganic halide can be dissolved in a solvent such as alcohol, and then precipitated into fine particles by a precipitating agent.
[0122] The clay is usually composed mainly of clay minerals. The ion-exchangeable layered compound is a compound having a crystal structure in which the planes formed by ionic bonds are stacked in parallel with each other with weak bonding force, and the ions contained therein are exchangeable. Most clay minerals are ion-exchangeable layered compounds. These clays, clay minerals, and ion-exchangeable layered compounds are not limited to natural products, and artificial synthetic products can also be used.
[0123] Examples of the clay, clay mineral, or ion-exchangeable layered compound include ionic crystalline compounds having layered crystal structures such as hexagonal close packing type, antimony type, CdCl2 type, and CdI2 type.
[0124] Furthermore, examples of clay and clay minerals include kaolin, bentonite, kibushi clay, gairome clay, allophane, hisingerite, pyrophyllite, ummo group, montmorillonite group, vermiculite, ryokudeite group, palygorskite, kaolinite, nacrite, dickite, halloysite, etc. Ion-exchangeable layered compounds include crystalline acid salts of polyvalent metals, such as α-Zr(HAsO4)2·H2O, α-Zr(HPO4)2, α-Zr(KPO4)2·3H2O, α-Ti(HPO4)2, α-Ti(HAsO4)2·H2O, α-Sn(HPO4)2·H2O, γ-Zr(HPO4)2, γ-Ti(HPO4)2, and γ-Ti(NH4PO4)2·H2O.
[0125] Such clay, clay mineral, or ion-exchangeable layered compound preferably has a pore volume of 0.1 cc / g or more, particularly preferably 0.3 to 5 cc / g, having a radius of 20 Å or more, as measured by mercury intrusion porosimetry, where the pore volume is measured for a pore radius range of 20 to 30,000 Å by mercury intrusion porosimetry using a mercury porosimeter. When a support having a pore volume of less than 0.1 cc / g and a radius of 20 Å or more is used, it tends to be difficult to obtain high polymerization activity.
[0126] It is also preferable to subject the clay and clay minerals used in the present invention to chemical treatment. As the chemical treatment, any of surface treatments that remove impurities attached to the surface and treatments that affect the crystalline structure of the clay can be used. Specific examples of chemical treatments include acid treatment, alkali treatment, salt treatment, and organic treatment. In addition to removing impurities from the surface, acid treatment increases the surface area by eluting cations such as Al, Fe, and Mg in the crystalline structure. In alkali treatment, the crystalline structure of the clay is destroyed, resulting in a change in the structure of the clay. In addition, salt treatment and organic treatment form ion complexes, molecular complexes, organic derivatives, etc., which can change the surface area and interlayer distance.
[0127] The ion-exchangeable layered compound used in the present invention may be a layered compound in which the space between layers is expanded by utilizing the ion exchangeability and exchanging the exchangeable ions between layers with other large bulky ions. Such bulky ions play a role of supporting the layered structure and are usually called pillars. The introduction of another substance between layers of a layered compound in this way is called intercalation. Examples of guest compounds to be intercalated include cationic inorganic compounds such as TiCl4 and ZrCl4, metal alkoxides such as Ti(OR)4, Zr(OR)4, PO(OR)3, and B(OR)3 (R is a hydrocarbon group, etc.), [Al 13 O4(OH) 24 ] 7+ , [Zr4(OH) 14 ] 2+ , [Fe3O(OCOCH3)6] + Metal hydroxide ions such as these can be used. These compounds can be used alone or in combination of two or more. When intercalating these compounds, polymers obtained by hydrolysis of metal alkoxides (R indicates a hydrocarbon group, etc.) such as Si(OR)4, Al(OR)3, Ge(OR)4, and colloidal inorganic compounds such as SiO2 can also be used. Examples of pillars include oxides produced by intercalating the above metal hydroxide ions between layers and then dehydrating them with heat.
[0128] The clay, clay mineral, and ion-exchangeable layered compound used in the present invention may be used as is, or may be used after treatment such as ball milling or sieving. They may also be used after newly adding and adsorbing water or after heat dehydration treatment. Furthermore, they may be used alone or in combination of two or more kinds.
[0129] Of these, clay or clay minerals are preferred, and montmorillonite, vermiculite, pectolite, taeniolite and synthetic mica are particularly preferred. As described above, the carrier (C) is an inorganic or organic compound, and examples of the organic compound include granular or fine particle solids having a particle size in the range of 10 to 300 μm.Specific examples include (co)polymers produced mainly from α-olefins having 2 to 14 carbon atoms, such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene, or (co)polymers produced mainly from vinylcyclohexane and styrene, and their modified products.
[0130] The olefin polymerization catalyst according to the present invention may further contain, in addition to the above-mentioned transition metal compound (A), the above-mentioned compound (B), and, if necessary, the support (C), the following specific organic compound component (D) may also be contained, if necessary.
[0131] [(D) Organic compound component] In the present invention, the organic compound component (D) is used, if necessary, for the purpose of improving the polymerization performance of the olefin polymerization catalyst of the present invention and the physical properties of the produced polymer (for example, the molecular weight of the produced polymer) (increasing the molecular weight, for example). Examples of such organic compounds include, but are not limited to, alcohols, phenolic compounds, carboxylic acids, phosphorus compounds, and sulfonates.
[0132] The alcohols and phenolic compounds are generally selected from the group consisting of R 22 The formula represented by -OH is used, where R 22represents a hydrocarbon group having 1 to 50 carbon atoms (6 to 50 carbon atoms in the case of phenols) or a halogenated hydrocarbon group having 1 to 50 carbon atoms (6 to 50 carbon atoms in the case of phenols).
[0133] Alcohols include R 22 The phenolic compound is preferably one in which the α,α'-positions of the hydroxyl group are substituted with a hydrocarbon having 1 to 20 carbon atoms.
[0134] The carboxylic acid is usually R 23 The one represented by -COOH is used. 23 represents a hydrocarbon group having 1 to 50 carbon atoms or a halogenated hydrocarbon group having 1 to 50 carbon atoms, and is particularly preferably a halogenated hydrocarbon group having 1 to 50 carbon atoms.
[0135] As the phosphorus compound, phosphoric acids having a P-O-H bond, phosphates having a P-OR or P=O bond, and phosphine oxide compounds are preferably used. The sulfonate salt includes those represented by the following general formula (Da).
[0136] [ka] (In the general formula (Da), M 5 is an atom in groups 1 to 14 of the periodic table, and R 24 is hydrogen, a hydrocarbon group having 1 to 20 carbon atoms, or a halogenated hydrocarbon group having 1 to 20 carbon atoms; Z is a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or a halogenated hydrocarbon group having 1 to 20 carbon atoms; t is an integer of 1 to 7; u is an integer of 1 to 7; and tu is 1 or greater.
[0137] The production of the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention includes a step of copolymerizing monomers consisting of ethylene (XA), an α-olefin (XB) having 3 to 20 carbon atoms, a non-conjugated polyene (XC) containing, in the molecule, two or more partial structures selected from the group consisting of the general formulae (I) and (II), and, if necessary, a non-conjugated polyene (XD) containing, in the molecule, only one partial structure selected from the group consisting of the general formulae (I) and (II).
[0138] In the polymerization, the components constituting the catalyst of the present invention may be used in any manner and added in any order to a polymerization vessel. Examples of the manner include the following. <1> A method in which the transition metal compound (A) is added alone to a polymerization reactor. <2> 2) A method in which the transition metal compound (A) and the compound (B) are added to a polymerization reactor in any order. <3> A method in which a catalyst component in which a transition metal compound (A) is supported on a carrier (C) and a compound (B) are added to a polymerization reactor in any order. <4> A method in which a catalyst component in which a compound (B) is supported on a carrier (C) and a transition metal compound (A) are added to a polymerization vessel in any order. <5> A catalyst component in which a transition metal compound (A) and a compound (B) are supported on a carrier (C) is added to a polymerization vessel. <6> A method in which a catalyst component in which a transition metal compound (A) and a compound (B) are supported on a carrier (C), and the compound (B) are added to a polymerization vessel in any order. In this case, the compound (B) supported on the carrier (C) and the compound (B) added alone may be the same or different. <7> A method in which a catalyst component in which a compound (B) is supported on a carrier (C), and a transition metal compound (A) are added to a polymerization vessel in any order. <8> A method in which a catalyst component in which compound (B) is supported on a carrier (C), a transition metal compound (A), and compound (B) are added to a polymerization vessel in any order. In this case, compound (B) supported on a carrier (C) and compound (B) added alone may be the same or different. <9> A method in which a component in which a transition metal compound (A) is supported on a carrier (C) and a component in which a compound (B) is supported on a carrier (C) are added to a polymerization vessel in any order. <10> ) A method in which a component in which a transition metal compound (A) is supported on a carrier (C), a component in which a compound (B) is supported on a carrier (C), and a compound (B) are added to a polymerization vessel in any order. In this case, the compound (B) supported on the carrier (C) and the compound (B) added alone may be the same or different. <11> 2) A method in which the transition metal compound (A), the compound (B), and the organic compound component (D) are added to a polymerization reactor in any order. <12> A method in which the compound (B) and the organic compound component (D) which have been contacted in advance, and the transition metal compound (A) are added to a polymerization vessel in any order. <13> A method in which the compound (B), the organic compound component (D) supported on the carrier (C), and the transition metal compound (A) are added to a polymerization vessel in any order. <14> A method in which a catalyst component in which a transition metal compound (A) and a compound (B) have been contacted in advance, and an organic compound component (D) are added to a polymerization vessel in any order. <15> A method in which a catalyst component in which a transition metal compound (A) and a compound (B) have been contacted in advance, compound (B), and an organic compound component (D) are added to a polymerization vessel in any order. <16> A method in which a catalyst component in which a transition metal compound (A) and a compound (B) have been contacted in advance, and a component in which a compound (B) and an organic compound component (D) have been contacted in advance are added to a polymerization vessel in any order. In this case, the compound (B) contacted with the transition metal compound (A) and the compound (B) contacted with the organic compound component (D) may be the same or different. <17> A method in which a transition metal compound (A) supported on a carrier (C), a compound (B), and an organic compound component (D) are added to a polymerization reactor in any order. <18> A method in which a component in which a transition metal compound (A) is supported on a carrier (C), and a component in which a compound (B) and an organic compound component (D) are previously contacted are added to a polymerization reactor in any order. <19> A method in which a catalyst component in which a transition metal compound (A), a compound (B) and an organic compound component (D) have been contacted in advance in any order is added to a polymerization vessel. <20> A method in which a catalyst component in which a transition metal compound (A), a compound (B) and an organic compound component (D) have been contacted in advance, and compound (B) are added to a polymerization vessel in any order. In this case, compound (B) that is contacted with transition metal compound (A) and organic compound component (D) and compound (B) that is added alone may be the same or different. <21> A catalyst in which a transition metal compound (A), a compound (B) and an organic compound component (D) are supported on a carrier (C) is added to a polymerization vessel. <22> A method in which a catalyst component in which a transition metal compound (A), a compound (B) and an organic compound component (D) are supported on a carrier (C), and component (B) are added to a polymerization vessel in any order. In this case, the compound (B) supported on the carrier (C) and the compound (B) added alone may be the same or different.
[0139] In the above-mentioned solid catalyst component having the transition metal compound (A) supported on the support (C) and the solid catalyst component having the transition metal compound (A) and the compound (B) supported on the support (C), an olefin may be prepolymerized, or a catalyst component may be further supported on the prepolymerized solid catalyst component.
[0140] In the present invention, the copolymerization can be carried out by either a liquid phase polymerization method such as solution polymerization or suspension polymerization, or a gas phase polymerization method. Specific examples of the inert hydrocarbon medium used in the liquid phase polymerization method include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane, and mixtures thereof, and the olefin itself to be subjected to (co)polymerization can also be used as a solvent.
[0141] When olefin polymerization is carried out using the above-mentioned olefin polymerization catalyst, the transition metal compound (A) is usually used in an amount of 10 -12 ~10 -2 Molar, preferably 10 -10 ~10 -3 It is used in molar amounts.
[0142] The organometallic compound (B-1) is used in an amount such that the molar ratio [(B-1) / M] of the organometallic compound (B-1) to the total transition metal atoms (M) in the transition metal compound (A) is usually 0.01-100,000, preferably 0.05-50,000. The organoaluminum oxy compound (B-2) is used in an amount such that the molar ratio [(B-2) / M] of the aluminum atoms in the organoaluminum oxy compound (B-2) to the total transition metals (M) in the transition metal compound (A) is usually 10-500,000, preferably 20-100,000. The compound (ionized ionic compound) (B-3) that reacts with the transition metal compound (A) to form an ion pair is used in an amount such that the molar ratio [(B-3) / M] of the ionized ionic compound (B-3) to the transition metal atoms (M) in the transition metal compound (A) is usually 1-10, preferably 1-5.
[0143] The organic compound component (D) is used in an amount such that the molar ratio [(D) / (B-1)] to the organometallic compound (B-1) is usually 0.01 to 10, preferably 0.1 to 5. The organic compound component (D) is used in an amount such that the molar ratio [(D) / (B-2)] to the organoaluminum oxy compound (B-2) is usually 0.001 to 2, preferably 0.005 to 1. The organic compound component (D) is used in an amount such that the molar ratio [(D) / (B-3)] to the ionizing ionic compound (B-3) is usually 0.01 to 10, preferably 0.1 to 5.
[0144] The polymerization temperature of the olefin using such an olefin polymerization catalyst is usually in the range of −50 to +200° C., preferably 0 to 170° C. The polymerization pressure is usually normal pressure to 100 kg / cm. 2 -G, preferably normal pressure to 50 kg / cm 2Under the conditions of -G, the polymerization reaction can be carried out in any of batch, semi-continuous and continuous modes. Furthermore, the polymerization can be carried out in two or more stages with different reaction conditions.
[0145] The reaction time (average residence time when copolymerization is carried out by a continuous method) varies depending on conditions such as catalyst concentration and polymerization temperature, but is usually 0.5 minutes to 5 hours, preferably 5 minutes to 3 hours.
[0146] The molecular weight of the resulting ethylene-α-olefin-non-conjugated polyene copolymer (1) can be adjusted by making hydrogen present in the polymerization system or by changing the polymerization temperature. It can also be adjusted by the amount of compound (b) used. Specific examples include triisobutylaluminum, methylaluminoxane, and diethylzinc. When hydrogen is added, the appropriate amount is about 0.001 to 100 NL per kg of olefin.
[0147] The molar ratio of ethylene (XA) to α-olefin (XB) (ethylene (XA) / α-olefin (XB)) is preferably 40 / 60 to 99.9 / 0.1, more preferably 50 / 50 to 90 / 10, further preferably 55 / 45 to 85 / 15, and most preferably 55 / 45 to 78 / 22.
[0148] The amount of the non-conjugated polyene (XC) charged is usually 0.07 to 10% by weight, preferably 0.1 to 8.0% by weight, and more preferably 0.5 to 5.0% by weight, relative to 100% by weight of the total of ethylene (XA), α-olefin (XB), and non-conjugated polyene (XC) (total monomer charge amount).
[0149] <Composition containing ethylene-α-olefin-non-conjugated polyene copolymer (1)> Due to its usefulness, the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention is used together with other components, such as various rubbers, elastomers, resins, plasticizers, fillers, crosslinking agents, crosslinking assistants, vulcanization accelerators, vulcanization assistants, fillers, softeners, antioxidants, processing assistants, activators, heat stabilizers, weather stabilizers, antistatic agents, colorants, lubricants and thickeners, foaming agents, foaming assistants, colorants, dispersants, flame retardants, etc.
[0150] In a preferred embodiment of the composition of the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention and other components, the other components are at least one selected from the group consisting of resins and styrene-based elastomers. In this case, the moldability of the composition is improved, the molding efficiency is improved, and the composition can be used for molded articles for many purposes.
[0151] Examples of such resins include polyamide resins such as nylon 11 and nylon 12; polyester resins such as polyethylene terephthalate and polybutylene terephthalate; ethylene-based resins such as high-pressure low-density polyethylene, linear low-density polyethylene, and high-density polyethylene; propylene-based resins such as random PP and block PP; polyolefin resins such as polybutene and poly-4-methylene-pentene resin; polyvinylidene chloride resins, saponified ethylene-vinyl acetate copolymers, polycarbonate resins, polystyrene resins, and acrylic resins.
[0152] Among these resins, engineering plastics include polyamide, polyacetal, polycarbonate, polyester, polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyarylate, polyamideimide, polyetherimide, polyetheretherketone, polyimide, fluororesin, polyaminobismaleimide, and polybisamidotriazole. The styrene-based elastomer may be, for example, a block copolymer composed of a polystyrene block and a polyolefin block composed of a monomer unit derived from an alkadiene having 4 to 10 carbon atoms, or a hydrogenated product thereof.
[0153] The styrene-based elastomer may be a diblock type copolymer consisting of a polystyrene block and a polyolefin block bonded thereto, or a triblock type copolymer consisting of polystyrene blocks arranged at both ends and a polyolefin block arranged therebetween. The triblock type copolymer can further contribute to improving the impact resistance of the molded article. The content of the polyolefin block in the block copolymer as the styrene-based elastomer may be, for example, 95% by mass or less, or 90% by mass or less, or may be, for example, 5% by mass or more, 10% by mass or more, or 20% by mass or more, when the entire block copolymer is taken as 100% by mass. When the styrene-based elastomer contains an appropriate proportion of polyolefin blocks, a molded article having good properties in terms of transparency, impact resistance, rigidity, and stickiness is easily obtained.
[0154] Examples of styrene-based elastomers include block copolymers (SBC) of polystyrene blocks that form the hard portion (crystalline portion) and conjugated diene monomer blocks such as isoprene or butadiene that form the soft portion, hydrogenated styrene-butadiene-styrene block copolymers (HSBR), styrene-ethylene-propylene-styrene block copolymers (SEPS), styrene-ethylene-butene-styrene block copolymers (SEBS), styrene-isoprene-styrene block copolymers (SIS), styrene-butadiene-styrene copolymers (SBS), styrene-isobutylene-styrene copolymers (SIBS), styrene-isobutylene copolymers (SIB), styrene-isoprene-butadiene-styrene block copolymers, styrene block copolymers (SIS), and hydrogenated copolymers of styrene / styrene-butadiene random copolymer / styrene block (SESS).
[0155] The styrene elastomer may be used alone or in combination of two or more. Of these, the styrene elastomer is preferably at least one selected from styrene-ethylene-butene-styrene block copolymer (SEBS) and hydrogenated styrene / styrene-butadiene random copolymer / styrene block copolymer (SESS). An example of a commercially available hydrogenated styrene-butadiene-styrene block copolymer (HSBR) is Dynaron (registered trademark) by JSR Corporation.
[0156] Styrene-ethylene-propylene-styrene block copolymer (SEPS) is obtained by hydrogenating styrene-isoprene-styrene block copolymer (SIS). Examples of commercially available SIS products include JSR SIS (registered trademark) from JSR Corporation, Hybler (registered trademark) from Kuraray Co., Ltd., and Clayton D (registered trademark) from Shell Co., Ltd. Examples of commercially available SEPS products include Septon (registered trademark) from Kuraray Co., Ltd., and Clayton (registered trademark) from Shell Co., Ltd.
[0157] Examples of commercially available styrene-ethylene-butene-styrene block copolymers (SEBS) include Tuftec (registered trademark) from Asahi Kasei Corporation and Kraton (registered trademark) from Shell Corporation.
[0158] Examples of commercially available styrene-isobutylene-styrene copolymers (SIBS) or styrene-isobutylene copolymers (SIB) include SIBSTAR (registered trademark) from Kaneka Corporation.
[0159] Examples of the SESS include SOE (registered trademark) S1606 manufactured by Asahi Kasei Corporation, or a mixture of SOE (registered trademark) S1606 and S1605. The blending ratio of the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention in a composition consisting of a resin and / or a styrene-based elastomer is preferably 1 to 100 parts by weight, more preferably 5 to 70 parts by weight, of the ethylene-α-olefin-non-conjugated polyene copolymer (1) per 100 parts by weight of the resin and / or the styrene-based elastomer.
[0160] <Compositions consisting of ethylene-α-olefin-non-conjugated polyene copolymers (1) and ethylene-α-olefin-non-conjugated polyene copolymers (2)> Among these, a composition containing the ethylene-α-olefin-polyene copolymer (1) of the present invention and the ethylene-α-olefin-non-conjugated polyene copolymer (2) satisfying the following requirements 3 and 4 has excellent moldability. Requirement 3 It has structural units derived from ethylene (X-A'), an α-olefin (X-B') having 3 to 20 carbon atoms, and a non-conjugated polyene (X-C') containing, in the molecule, a total of two or more partial structures selected from the group consisting of the following general formulas (I) and (II): Requirement 4 The intrinsic viscosity [η] is in the range of 1.0 to 2.2 dL / g. Here, the α-olefin (X-B') having 3 to 20 carbon atoms in requirement 3 is the same as the above-mentioned α-olefin (XB), and the non-conjugated polyene (X-C') is the same as the above-mentioned non-conjugated polyene (XC). Moreover, requirement 4 specifies that the intrinsic viscosity [η] must be in the range of 1.0 to 2.2 dL / g, which is smaller than the intrinsic viscosity [η] of the above-mentioned ethylene-α-olefin-polyene copolymer (1), which is 5.1 to 7.0 dL / g.
[0161] Such copolymers can be produced using vanadium catalysts or various metallocene catalysts, or using the above-mentioned metallocene compounds suitable for producing the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention.
[0162] The weight ratio of the ethylene-α-olefin-non-conjugated polyene copolymer (1) (sometimes abbreviated as polyene copolymer (1)) and the ethylene-α-olefin-non-conjugated polyene copolymer (2) (sometimes abbreviated as polyene copolymer (2)) of the present invention is preferably a polyene copolymer (1) / polyene copolymer (2) weight ratio of 99 / 1 to 1 / 99, more preferably 90 / 10 to 5 / 95, and even more preferably 80 / 20 to 10 / 90. Of these, a polyene copolymer (1) / polyene copolymer (2) weight ratio of 40 / 60 to 20 / 80 is particularly preferred.
[0163] The weight average molecular weight (Mw) of the composition consisting of the polyene copolymer (1) and the polyene copolymer (2) is preferably in the range of 1.0×10 5 ~4.0×10 5 (Measured by GPC). Among them, 1.5×10 5 ~3.5×10 5 (measured by GPC) is the preferred range.
[0164] The molecular weight distribution (Mw / Mn) of the composition consisting of the polyene copolymer (1) and the polyene copolymer (2) (measured by GPC) is preferably in the range of 2.8 to 5.0, and more preferably in the range of 3.0 to 4.5 (measured by GPC).
[0165] It is desirable to use this "composition consisting of polyene copolymer (1) and polyene copolymer (2)" instead of "polyene copolymer (1)" in various compositions using polyene copolymer (1) shown below.
[0166] In addition, when "a composition consisting of polyene copolymer (1) and polyene copolymer (2)" is used instead of "polyene copolymer (1)", the range of the blend ratio per 100 parts by weight of polyene copolymer (1) below shall be read as the range of the blend ratio per 100 parts by weight of "the composition consisting of polyene copolymer (1) and polyene copolymer (2)". As suitable examples of compositions using the ethylene-α-olefin-polyene copolymer (1), a "thermoplastic resin composition" and a "rubber composition" will be described below.
[0167] <Thermoplastic resin composition> The thermoplastic resin composition of the present invention is a resin composition containing the above-mentioned ethylene / α-olefin / non-conjugated polyene copolymer (1) of the present invention and a thermoplastic resin.
[0168] The thermoplastic resin composition of the present invention may appropriately contain various additives that can be blended into resin compositions, fillers, and the ethylene-α-olefin-non-conjugated polyene copolymer of the present invention other than the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention.
[0169] The thermoplastic resin composition of the present invention can be crosslinked and used suitably for various applications, and it is preferable that the thermoplastic resin composition contains a crosslinking agent. As the crosslinking agent, any known crosslinking agent can be used without particular limitation, and among them, organic peroxides are preferable.
[0170] When the thermoplastic resin composition of the present invention contains an organic peroxide, the content (mol) of the organic peroxide preferably satisfies the following formula (Q). Organic peroxide content (mol) x number of oxygen-oxygen bonds in one molecule of organic peroxide ≦ Weight fraction of (XC) / Molecular weight of (XC)×100 … Equation (Q) (In formula (Q), the weight fraction of (XC) represents the weight fraction (wt%) of the constitutional unit derived from the non-conjugated polyene (XC) in the ethylene-α-olefin-non-conjugated polyene copolymer (1), and the molecular weight of (XC) represents the molecular weight of the non-conjugated polyene (XC).) The thermoplastic resin composition of the present invention is preferably a rubber composition described below.
[0171] <Rubber composition> The ethylene-α-olefin-non-conjugated polyene copolymer (1) according to the present invention exhibits good rubber properties and is suitably used as a raw material for rubber compositions.
[0172] The rubber composition according to the present invention may contain, in addition to the ethylene / α-olefin / non-conjugated polyene copolymer (1) according to the present invention, a softener, a filler, other resin components, a crosslinking agent, and the like, as appropriate.
[0173] Softener The softener is not particularly limited, but typically mineral oils or synthetic oils are used.
[0174] Examples of mineral oils include paraffin oil, naphthene oil, aromatic oil, etc. Examples of synthetic oils include butene oligomer, ethylene-α-olefin co-oligomer, etc.
[0175] The ethylene-α-olefin co-oligomer is a polymer obtained by copolymerizing ethylene and an α-olefin, and having a number average molecular weight of less than 10,000 in terms of standard polystyrene measured by GPC. As the ethylene-α-olefin co-oligomer, ethylene-α-olefin co-oligomer having 3 to 8 carbon atoms is preferred, liquid ethylene-propylene rubber (EPR) is more preferred, and liquid ethylene-propylene rubber (EPR) having a number average molecular weight of 2,500 to 5,000 in terms of standard polystyrene measured by GPC is particularly preferred.
[0176] The softeners may be used alone or in combination of two or more. The content of the softener in the rubber composition of the present invention is 0.1 to 300 parts by weight, preferably 1 to 250 parts by weight, and more preferably 5 to 200 parts by weight, based on 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1). Within the above range, the rubber composition is excellent in moldability such as extrusion moldability, press moldability, injection moldability, and roll processability, which is preferable.
[0177] Filler The rubber composition of the present invention preferably contains a filler. The filler is not particularly limited, but inorganic fillers are preferred because they improve the mechanical strength of the rubber composition, such as tensile strength, tear strength, and abrasion resistance.
[0178] As the inorganic filler, for example, carbon black, clay, heavy calcium carbonate, light calcium carbonate, talc, etc. are usually used. As the inorganic filler, carbon black and heavy calcium carbonate are preferred. The fillers may be used alone or in combination of two or more.
[0179] The content of the filler in the rubber composition of the present invention is 1 to 300 parts by weight, preferably 5 to 250 parts by weight, and more preferably 10 to 200 parts by weight, based on 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1) of the present invention. A content within the above range is preferable because the kneadability and processability of the rubber composition are excellent, and the mechanical properties and compression set of the rubber molded product are excellent.
[0180] Other resin components The rubber composition of the present invention may contain, as necessary, a resin component other than the ethylene-α-olefin-non-conjugated polyene copolymer (1). Such other resin components are not particularly limited, but are preferably polyolefin resins.
[0181] When the rubber composition of the present invention contains a polyolefin resin, the hardness of the product can be adjusted and the compound viscosity at the processing temperature can be reduced, thereby improving processability. In addition, the rubber composition of the present invention can be handled as a thermoplastic elastomer, which is preferable because it has a wider range of handling properties and kneading techniques.
[0182] As the polyolefin resin, a polyolefin resin having a number average molecular weight of 10,000 or more in terms of standard polystyrene measured by GPC is preferably used. Examples of polyolefin resins include α-olefin homopolymers and α-olefin copolymers. Examples of α-olefin homopolymers include polyethylene and polypropylene, and examples of α-olefin copolymers include ethylene / α-olefin copolymers having 3 to 20 carbon atoms and ethylene / α-olefin / non-conjugated polyene copolymers having 3 to 20 carbon atoms (however, different from the ethylene / α-olefin / non-conjugated polyene copolymer of the present invention). Examples of ethylene / α-olefin copolymers having 3 to 20 carbon atoms include ethylene / propylene rubber (EPR), propylene / ethylene rubber (PER), ethylene / butene rubber (EBR), ethylene / octene rubber (EOR), etc.
[0183] Furthermore, examples of the ethylene-C3-C20 α-olefin-non-conjugated polyene copolymer (however, different from the ethylene-α-olefin-non-conjugated polyene copolymer (1) according to the present invention) include ethylene-propylene terpolymer (EPT) and ethylene-butene terpolymer (EBT).
[0184] Of these, preferred polyolefin resins are polyethylene, ethylene-α-olefin copolymer, and polypropylene. The polyolefin resins may be used alone or in combination of two or more.
[0185] When the rubber composition of the present invention contains a polyolefin resin, the content of the polyolefin resin is 1 to 100 parts by weight, preferably 5 to 80 parts by weight, and more preferably 10 to 50 parts by weight, per 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1) described above. Within the above range, the hardness of the molded article formed from the rubber composition can be adjusted, and the compound viscosity at the processing temperature can be reduced, so that the processability can be further improved. In addition, it is preferable because it can be handled as a thermoplastic elastomer, and the range of handling and kneading methods can be expanded.
[0186] Crosslinking Agent The rubber composition of the present invention may contain a crosslinking agent. By using a rubber composition containing a crosslinking agent, the rubber composition can be crosslinked to obtain a crosslinked product.
[0187] Examples of the crosslinking agent include crosslinking agents that are generally used when crosslinking rubber, such as sulfur-based compounds, organic peroxides, phenolic resins, hydrosilicone-based compounds, amino resins, quinone or a derivative thereof, amine-based compounds, azo-based compounds, epoxy-based compounds, isocyanates, etc. Among these crosslinking agents, sulfur-based compounds, organic peroxides, and phenolic resins are preferred.
[0188] Since the ethylene-α-olefin-non-conjugated polyene copolymer according to the present invention can achieve particularly excellent crosslinking properties when crosslinked using an organic peroxide, it is particularly preferred that the rubber composition of the present invention contains an organic peroxide as a crosslinking agent.
[0189] When the crosslinking agent is an organic peroxide, specific examples thereof include dicumyl peroxide, di-tert-butyl peroxide, 2,5-di-(tert-butylperoxy)hexane, 2,5-di-methyl-2,5-di-(tert-butylperoxy)hexane, 2,5-di-methyl-2,5-di-(tert-butylperoxy)hexyne-3,1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1,-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butylperoxybenzoate, tert-butylperoxyisopropylcarbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.
[0190] Among these, from the viewpoints of reactivity, odor and scorch stability, bifunctional organic peroxides having two peroxide bonds (-OO-) in one molecule, such as 2,5-di-(tert-butylperoxy)hexane, 2,5-di-methyl-2,5-di-(tert-butylperoxy)hexane, 2,5-di-methyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane and n-butyl-4,4-bis(tert-butylperoxy)valerate, are preferred, and among these, 2,5-di-(tert-butylperoxy)hexane and 2,5-di-methyl-2,5-di-(tert-butylperoxy)hexane are most preferred.
[0191] When the crosslinking agent is an organic peroxide, the amount of the organic peroxide is 0.1 to 20 parts by weight, preferably 0.2 to 15 parts by weight, and more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1). When the amount of the organic peroxide is within the above range, the rubber molding obtained does not bloom on its surface, and the rubber molding exhibits excellent crosslinking properties, which is preferable.
[0192] When an organic peroxide is used as the crosslinking agent, the rubber composition of the present invention preferably contains the following crosslinking aid. When an organic peroxide is used as a crosslinking agent, examples of the crosslinking aid that the rubber composition preferably contains include sulfur, p-quinone dioxime-based crosslinking aids, such as p-quinone dioxime; ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, and other acrylic crosslinking aids; diallyl phthalate, triallyl isocyanurate, and other allyl crosslinking aids; other maleimide crosslinking aids; and divinylbenzene. The amount of the crosslinking aid is usually 0.5 to 10 mol, preferably 0.5 to 7 mol, and more preferably 1 to 5 mol, per mol of the organic peroxide. The amount of the crosslinking aid is also desirably 0.5 to 2 mol, preferably 0.5 to 1.5 mol, and more preferably approximately equimolar, per mol of the organic peroxide.
[0193] In the rubber composition of the present invention, it is also preferable that the amount of organic peroxide contained in the above-mentioned thermoplastic resin composition of the present invention, i.e., the content (mol) of the organic peroxide is an amount that satisfies the following formula (Q). Organic peroxide content (mol) x number of oxygen-oxygen bonds in one molecule of organic peroxide ≦ Weight fraction of (XC) / Molecular weight of (XC)×100 … Equation (Q) (In formula (Q), the weight fraction of (XC) represents the weight fraction (wt%) of the structural unit derived from the non-conjugated polyene (XC) in the ethylene-α-olefin-non-conjugated polyene copolymer, and the molecular weight of (XC) represents the molecular weight of the non-conjugated polyene (XC).) The crosslinking agents may be used alone or in combination of two or more kinds.
[0194] When the crosslinking agent is a sulfur-based compound, specific examples thereof include sulfur, sulfur chloride, sulfur dichloride, morpholine disulfide, alkylphenol disulfide, tetramethylthiuram disulfide, and selenium dithiocarbamate.
[0195] When the crosslinking agent is a sulfur-based compound, the amount of the sulfur-based compound is usually 0.3 to 10 parts by weight, preferably 0.5 to 7.0 parts by weight, and more preferably 0.7 to 5.0 parts by weight, based on 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1). When the amount of the sulfur-based compound is within the above range, the rubber composition exhibits excellent crosslinking properties without blooming on the surface of the obtained rubber molded article, which is preferable. When a sulfur-based compound is used as the crosslinking agent, the rubber composition of the present invention preferably contains the following crosslinking aid.
[0196] When a sulfur-based compound is used as the crosslinking agent, examples of the crosslinking aid that the rubber composition preferably contains include zinc oxide, zinc white, etc. The amount of the crosslinking aid is usually 1 to 20 parts by weight based on 100 parts by weight of the ethylene-olefin-non-conjugated polyene copolymer (1). When a sulfur-based compound is used as the crosslinking agent, it is desirable to use sulfur in combination with a vulcanization accelerator.
[0197] Specific examples of the vulcanization accelerator include thiazole-based compounds such as N-cyclohexyl-2-benzothiazole sulfenamide (CBS) (e.g., "Noccela NS" (trade name; manufactured by Ouchi Shinko Co., Ltd.)), N-oxydiethylene-2-benzothiazole sulfenamide, N,N'-diisopropyl-2-benzothiazole sulfenamide, 2-mercaptobenzothiazole (e.g., "Suncerer M" (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), 2-(4-morpholinodithio)benzothiazole (e.g., "Noccela MDB-P" (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-diethyl-4-morpholinothio)benzothiazole, and dibenzothiazyl disulfide; di guanidine-based compounds such as phenylguanidine, triphenylguanidine, and diorthotolylguanidine; acetaldehyde-aniline condensates, butylaldehyde-aniline condensates, and aldehyde amine-based compounds; imidazoline-based compounds such as 2-mercaptoimidazoline; thiourea-based compounds such as diethylthiourea and dibutylthiourea; thiuram-based compounds such as tetramethylthiuram monosulfide and tetramethylthiuram disulfide (TMTD) (e.g., Noccela TT (trade name; manufactured by Ouchi Shinko Co., Ltd.)); dithioacid salt-based compounds such as zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate (ZnBDC) (e.g., Suncera Bz (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), and tellurium diethyldithiocarbamate; and ethylenethiourea. Examples of the thioureas include N,N'-diethylthiourea, N,N'-dibutylthiourea, and the like; xanthates such as zinc dibutylxatogenate; and zinc oxide (for example, zinc oxide such as "META-Z102" (trade name; manufactured by Inoue Lime Industry Co., Ltd.)).
[0198] The amount of the vulcanization accelerator is usually 0.1 to 20 parts by weight, preferably 0.2 to 15 parts by weight, and more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1). When the amount of the vulcanization accelerator is within the above range, it is preferable because the resulting rubber molded article shows excellent crosslinking properties without blooming on the surface.
[0199] The vulcanization aid can be appropriately selected depending on the application, and can be used alone or in combination of two or more. Specific examples of the vulcanization aid include magnesium oxide, zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name; manufactured by Inoue Lime Industry Co., Ltd.)). The amount of the binder is usually 1 to 20 parts by weight based on 100 parts by weight of the ethylene / α-olefin / non-conjugated polyene copolymer (1).
[0200] Foaming Agent The rubber composition of the present invention may contain a foaming agent. When the rubber composition of the present invention contains a foaming agent, it usually contains the crosslinking agent as well. By using a rubber composition containing a crosslinking agent and a foaming agent, the rubber composition can be crosslinked and foamed to obtain a foam. do.
[0201] Examples of the foaming agent include inorganic foaming agents such as sodium bicarbonate and sodium carbonate; nitroso compounds such as N,N'-dinitrosopentamethylenetetramine and N,N'-dinitrosoterephthalamide; azo compounds such as azodicarbonamide (ADCA) and azobisisobutyronitrile; hydrazide compounds such as benzenesulfonylhydrazide and p,p'-oxybis(benzenesulfonylhydrazide) (OBSH); and organic foaming agents such as azide compounds such as calcium azide and 4,4'-diphenyldisulfonyl azide. ADCA and OBSH are preferred as the foaming agent. The foaming agents may be used alone or in combination.
[0202] When the rubber composition of the present invention contains a foaming agent, the amount of the foaming agent is usually 0.2 to 30 parts by weight, preferably 0.5 to 25 parts by weight, and more preferably 0.5 to 20 parts by weight, based on 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1).
[0203] Foaming Aid When the rubber composition of the present invention contains a foaming agent, it may further contain a foaming assistant, if necessary. The foaming assistant has the effects of lowering the decomposition temperature of the foaming agent, accelerating the decomposition, and homogenizing the bubbles. Examples of such foaming assistants include organic acids such as salicylic acid, phthalic acid, stearic acid, oxalic acid, and citric acid, and salts thereof, and urea and its derivatives.
[0204] When the rubber composition of the present invention contains a foaming aid, the amount of the foaming aid is usually 0.2 to 30 parts by weight, preferably 0.5 to 25 parts by weight, and more preferably 0.5 to 20 parts by weight, based on 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1).
[0205] Processing Aids The rubber composition of the present invention may contain a processing aid. As the processing aid, a wide variety of processing aids that are generally compounded in rubber as processing aids can be used. Specific examples include ricinoleic acid, stearic acid, palmitic acid, lauric acid, barium stearate, zinc stearate, calcium stearate, and esters. Among these, stearic acid is preferred.
[0206] When the rubber composition of the present invention contains a processing aid, the amount of the processing aid is usually 0.1 to 10 parts by weight, preferably 0.5 to 8 parts by weight, and more preferably 1 to 6 parts by weight, based on 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1). Within the above range, there is no bloom on the surface of the obtained rubber composition, and furthermore, crosslinking inhibition does not occur when the rubber composition is crosslinked, which is preferable. In addition, a rubber composition containing a processing aid is preferable because it has excellent moldability such as extrusion moldability, press moldability, and injection moldability, and roll processability.
[0207] Surfactants The rubber composition of the present invention may contain a surfactant. Examples of the surfactant include amines such as di-n-butylamine, dicyclohexylamine, monoethanolamine, triethanolamine, Acting B (manufactured by Yoshitomi Pharmaceutical Co., Ltd.), Acting SL (manufactured by Yoshitomi Pharmaceutical Co., Ltd.), polyethylene glycol, diethylene glycol, polyethylene glycol, lecithin, triaryl methyl ester, zinc compounds of aliphatic and aromatic carboxylic acids (e.g., Struktol activator73, Struktol IB 531, and Struktol FA541, manufactured by Schill & Seilacher), ZEONET ZP (manufactured by Zeon Corporation), octadecyltrimethylammonium bromide, synthetic hydrotalcite, and special quaternary ammonium compounds (e.g., Arcard 2HF (manufactured by Lion Akzo Co., Ltd.)).
[0208] When the rubber composition of the present invention contains a surfactant, the amount of the surfactant is usually 0.2 to 10 parts by weight, preferably 0.3 to 5 parts by weight, and more preferably 0.5 to 4 parts by weight, based on 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1). The surfactant can be appropriately selected depending on the application, and can be used alone or in combination of two or more kinds.
[0209] Anti-aging agents The rubber composition of the present invention may contain an antioxidant. When the rubber composition of the present invention contains an antioxidant, it is possible to extend the life of the product obtained from the composition. As the antioxidant, a conventionally known antioxidant, such as an amine-based antioxidant, a phenol-based antioxidant, or a sulfur-based antioxidant, can be used.
[0210] Specific examples of the anti-aging agent include aromatic secondary amine-based anti-aging agents such as phenylbutylamine and N,N-di-2-naphthyl-p-phenylenediamine; phenol-based anti-aging agents such as dibutylhydroxytoluene and tetrakis[methylene(3,5-di-t-butyl-4-hydroxy)hydrocinnamate]methane; thioether-based anti-aging agents such as bis[2-methyl-4-(3-n-alkylthiopropionyloxy)-5-t-butylphenyl]sulfide; dithiocarbamate-based anti-aging agents such as nickel dibutyldithiocarbamate; and sulfur-based anti-aging agents such as 2-mercaptobenzoylimidazole, zinc salt of 2-mercaptobenzimidazole, dilaurylthiodipropionate, and distearylthiodipropionate.
[0211] When the rubber composition of the present invention contains an antioxidant, the amount of the antioxidant is usually 0.01 to 10 parts by weight, preferably 0.02 to 7 parts by weight, and more preferably 0.03 to 5 parts by weight, based on 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1). If the amount is within the above range, the molded article obtained from the rubber composition of the present invention is excellent in heat aging resistance, which is preferable.
[0212] Anti-gelling agent The rubber composition of the present invention may contain a pseudo-gelling inhibitor, such as "NHM-007" (manufactured by Mitsui Chemicals, Inc.).
[0213] When the rubber composition of the present invention contains a pseudo-gelling inhibitor, the amount of the pseudo-gelling inhibitor is usually 0.1 to 15 parts by weight, preferably 0.5 to 12 parts by weight, and more preferably 1.0 to 10 parts by weight, based on 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1).
[0214] Other Additives The rubber composition of the present invention may further contain other additives, such as a heat stabilizer, a weather stabilizer, an antistatic agent, a colorant, a lubricant, and a thickener.
[0215] <Method of preparing rubber composition> The rubber composition of the present invention is a rubber composition containing the above-mentioned ethylene-α-olefin-non-conjugated polyene copolymer, and preferably contains components such as a softener, a filler, a crosslinking agent, etc. For example, a rubber composition containing 0.1 to 300 parts by weight of a softener and 1 to 300 parts by weight of a filler per 100 parts by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (1) can be mentioned, but the preparation method thereof is not particularly limited.
[0216] Examples of methods for preparing the rubber composition include a method of mixing each component contained in the rubber composition using a conventionally known kneading machine such as a mixer, kneader, or roll, or further a continuous kneading machine such as a twin-screw extruder, and a method of preparing a solution in which each component contained in the rubber composition is dissolved or dispersed, and then removing the solvent.
[0217] The molding and vulcanization may be carried out using a mold or without a mold. When a mold is not used, the rubber composition is usually molded and vulcanized continuously.
[0218] <Crosslinked rubber molded body> The crosslinked rubber molded article of the present invention is obtained by crosslinking a rubber composition containing the above-mentioned ethylene-α-olefin-non-conjugated polyene copolymer and a crosslinking agent, and optionally additives such as a softener and a filler. The crosslinking may or may not involve the use of a mold. When a mold is not used, the rubber composition is usually molded and crosslinked continuously.
[0219] Examples of methods for crosslinking the rubber composition include a method in which (m) a rubber composition containing a crosslinking agent is preformed into a desired shape, usually by a molding method such as extrusion molding, press molding, or injection molding, or by roll processing, and then heated while molding or by introducing the molded product into a crosslinking tank; and a method in which (n) a rubber composition containing a crosslinking agent is preformed in the same manner as in method (m), and then irradiated with an electron beam.
[0220] In the method (m), a crosslinking reaction occurs due to the crosslinking agent in the rubber composition by heating, and a crosslinked product is obtained. In the method (n), a crosslinking reaction occurs due to an electron beam, and a crosslinked product is obtained. In the method (n), the preformed rubber composition is usually irradiated with an electron beam having an energy of 0.1 to 10 MeV so that the absorbed dose of the rubber composition is usually 0.5 to 36 Mrad, preferably 0.5 to 20 Mrad, and more preferably 1 to 10 Mrad.
[0221] <Foam> The foam of the present invention can be obtained by crosslinking and foaming a rubber composition containing the above-mentioned ethylene-α-olefin-non-conjugated polyene copolymer having 3 to 20 carbon atoms, and, if necessary, additives such as a softener, a filler, a crosslinking agent, and a foaming agent.
[0222] Since the rubber composition contains a foaming agent, when the rubber composition is heated, a crosslinking reaction occurs due to the crosslinking agent, and the foaming agent decomposes to generate carbon dioxide gas and nitrogen gas, thereby obtaining a foam having a cell structure.
[0223] <Application> The rubber composition of the present invention is extremely excellent in low-temperature properties, mechanical properties, moldability such as extrusion moldability, press moldability, and injection moldability, and roll processability, and from the rubber composition of the present invention, molded articles excellent in low-temperature properties (flexibility at low temperatures, rubber elasticity, etc.) and mechanical properties can be suitably obtained.
[0224] In addition, by using the above-mentioned ethylene-α-olefin-non-conjugated polyene copolymer, the rubber composition of the present invention can produce a crosslinked product having excellent moldability and crosslinking characteristics and excellent heat resistance stability. Therefore, the crosslinked product obtained from the rubber composition of the present invention can be suitably used in applications where long-term use at high temperatures is expected.
[0225] The rubber composition of the present invention and the molded article obtained from the composition, for example, a crosslinked body or a foamed body, can be used in various applications. Specifically, the rubber composition can be suitably used for tire rubber, O-rings, industrial rolls, packings (e.g., condenser packings), gaskets, belts (e.g., heat insulating belts, copier belts, conveyor belts), hoses such as automobile hoses (e.g., turbocharger hoses, water hoses, brake reservoir hoses, radiator hoses, air hoses), vibration-proof rubber, vibration-proofing or vibration-damping materials (e.g., engine mounts, motor mounts), muffler hangers, sponges (e.g., weather strip sponges, heat insulating sponges, protective sponges, microfoam sponges), cables (ignition cables, cab tire cables, high tension cables), electric wire coating materials (high voltage electric wire coating materials, low voltage electric wire coating materials, marine electric wire coating materials), glass run channels, colored skin materials, paper feed rolls, roofing sheets, etc. Among these, the composition is preferably used for automobile interior and exterior parts and applications requiring heat resistance, and is particularly suitable for hose applications such as brake reservoir hoses and radiator hoses used as automobile interior parts.
[0226] In the present invention, an ethylene-α-olefin-non-conjugated polyene copolymer having properties appropriate for the application can be selected and used within a range that satisfies the above-mentioned requirements. For example, for muffler hanger applications, an ethylene-α-olefin-non-conjugated polyene copolymer having a relatively high molecular weight can be preferably used, and specifically, an ethylene-α-olefin-non-conjugated polyene copolymer having a weight average molecular weight (Mw) of 200,000 to 600,000 can be preferably used.
[0227] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these.
[0228] [Example] [Production of ethylene-α-olefin-non-conjugated polyene copolymer (copolymer-1)] Polymerization Example 1 (Copolymer-1) 1,030 mL of hexane and 1.5 mL of 5-vinyl-2-norbornene (VNB) were charged into a 2 L stainless steel autoclave that had been thoroughly purged with nitrogen, and the temperature inside the system was raised to 70°C. Then, propylene was charged in an amount of 1.10 MPa in partial pressure, and ethylene was supplied to adjust the total pressure to 1.6 MPa-G. Next, 0.3 mmol of triisobutylaluminum, 0.00005 mmol of the transition metal compound A below, and 0.00025 mmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were injected with nitrogen, and the stirring speed was set to 250 rpm to initiate polymerization. Thereafter, the total pressure was maintained at 1.6 MPa-G by continuously supplying only ethylene, and polymerization was carried out at 70°C for 15 minutes. A small amount of ethanol was added to the system to terminate the polymerization, and then unreacted ethylene was purged. The polymer solution was poured into a large excess of a mixed solution of methanol and acetone to precipitate the polymer. The polymer was collected by filtration and dried overnight under reduced pressure at 120°C to obtain 6.34 g of ethylene-propylene-vinyl alcohol copolymer. The physical properties of the polymer are shown in Table 1. Transition metal compound A [pn-Butyl-p,p-bis(tricyclo[3.3.1.1 3,7 ]dec-1-yl)phosphineiminato-κN]dicyclo[(1,2,3,4,5-η)-1-[(2,3,4,5,6,-pentafluorophenyl)methyl]-2,4-cyclopentadien-1-yl]titanium
[0229] The physical properties of the ethylene-propylene-VNB copolymer were measured by the following methods. [Weight fraction of ethylene and VNB (% by weight)] The weight fractions of ethylene and VNB in the ethylene-propylene-VNB copolymer were calculated by preparing the calibration curves for ethylene and VNB, respectively, as shown below. That is, for ethylene, 13Using samples whose ethylene weight fraction was known by C-NMR measurement, the intensity of specific infrared absorption of ethylene was measured for each sample, and a calibration curve between the intensity of specific infrared absorption and the weight fraction of ethylene was created. Similarly, a calibration curve was prepared for VNB between the intensity of a specific infrared absorption and the weight fraction of VNB. For the above copolymer-1, the specific infrared absorption intensity of ethylene and the specific absorption intensity of VNB were measured, and the weight fractions of ethylene and VNB were calculated using the calibration curves.
[0230] (FT-IR measurement method) First, the polymer obtained in the above Polymerization Example 1 was heated to 135°C, melt-stretched by a hot press, and then cooled under pressure at room temperature to obtain a film, and the specific infrared absorption intensity of ethylene and the specific absorption intensity of VNB were measured using the film. FT-IR (FT-IR410 infrared spectrophotometer manufactured by JASCO) was used.
[0231] ( 13 C-NMR measurement method) The weight fraction of ethylene and the weight fraction of VNB of each sample for the calibration curve were determined by the following method. The measurement solvent was o-dichlorobenzene / benzene-d6 (4 / 1 {vol / vol%}) and the measurement conditions were 120°C, 250 ppm spectral width, 5.5 s pulse repetition time, and 4.7 μs pulse width (45° pulse) (100 MHz, JEOL ECX400P), or 120°C, 250 ppm spectral width, 5.5 s pulse repetition time, and 5.0 μs pulse width (45° pulse) (125 MHz, Bruker Biospin AVANCEIIIcryo-500). 13 The C-NMR spectrum was measured, various signals were assigned in a conventional manner, and the weight fractions of ethylene and VNB in each sample were calculated based on the integral values of the signal intensities. These were used to create the above calibration curve. The structural units derived from ethylene (weight fraction of ethylene) of the obtained ethylene-propylene-VNB copolymer (copolymer-1) are shown in Table 1.
[0232] [Limiting viscosity] The intrinsic viscosity [η] is a value measured in decalin at 135°C.
[0233] [Molecular weight (Mw), molecular weight distribution (Mw / Mn)] The Mw and molecular weight distribution (Mw / Mn) were determined using a gel permeation chromatograph HLC-8321 GPC / HT type (manufactured by Tosoh Corporation). The main measurement conditions were as follows: Detector: Differential refractometer Column: 2 TSKgel GMH6-HT + 1 TSKgel GMH6-HTL (each with inner diameter of 7.8 mm and length of 300 mm) Temperature: 140℃ Mobile phase: o-dichlorobenzene (containing 0.025% BHT) Injection volume: 400μL Sample concentration: ca0.15% (w / v) Sample filtration: Filtration through a sintered filter with a pore size of 1.0 μm Column calibration: Monodisperse polystyrene (Tosoh Corporation) Molecular weight conversion: EPR conversion / calibration method taking viscosity into account A universal calibration curve of a third-order polynomial was created by measuring 16 monodisperse standard polystyrenes (molecular weights: 20.6 million to 580) manufactured by Tosoh Corporation. EPR conversion parameters K: 0.000403, α: 0.700
[0234] [P value] The P value was calculated by measuring the complex viscosity at 0.1 rad / s and the complex viscosity at 100 rad / s at 190°C, strain 1.0%, and frequency using a viscoelasticity measuring device, Ares (manufactured by Rheometric Scientific). The ratio (η * The ratio was calculated.
[0235] [Mitsui EPT 3110M] The measurement results for the Mitsui EPT 3110M are shown in Table 1.
[0236] [Table 1]
[0237] [Production of ethylene-α-olefin-non-conjugated polyene copolymer (copolymer-2)] Polymerization Example 2 (Copolymer-2) Polymerization was carried out in the same manner as in Polymerization Example 1, except that 100 mL of H2 was added, the propylene partial pressure was 1.00 MPa, the transition metal compound A described below was 0.0001 mmol, and triphenylcarbenium tetrakis(pentafluorophenyl)borate was 0.0005 mmol, to obtain 6.51 g of an ethylene / propylene / VNB copolymer. The physical properties of the polymer are shown in Table 2. Transition metal compound A [pn-Butyl-p,p-bis(tricyclo[3.3.1.1 3,7 ]dec-1-yl)phosphineiminato-κN]dicyclo[(1,2,3,4,5-η)-1-[(2,3,4,5,6,-pentafluorophenyl)methyl]-2,4-cyclopentadien-1-yl]titanium
[0238] [Composition] Using a 6-inch roll (manufactured by Nitto Koki Co., Ltd.) (roll temperature: F / B=50 / 50°C, roll gap 0.5 mm), copolymer-1 and copolymer-2 were blended in the composition blend ratio shown in Table 2 to obtain a composition. The measurement results of the molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the obtained composition are shown in Table 2.
[0239] [Table 2]
[0240] The roll processability of the resulting composition was evaluated by the method described below, and the results are shown in Table 3. [Roll processability] Roll processability: The roll processability was evaluated under the conditions of a 6-inch roll (manufactured by Nitto Koki Co., Ltd.), roll temperature: F / B=50 / 50° C., and roll gap of 0.5 mm. The evaluation was carried out in three stages: Poor → Fair → Good Good: Excellent roll workability Fair: Good roll workability Poor: Poor roll workability
[0241] [Table 3]
Claims
1. An ethylene / α-olefin / non-conjugated polyene copolymer (1) that satisfies the following requirements 1 and 2: Requirement 1 The copolymer has structural units derived from ethylene (X-A), an α-olefin (X-B) having 3 to 20 carbon atoms, and a non-conjugated polyene (X-C) containing, in the molecule, two or more partial structures selected from the group consisting of the following general formulas (I) and (II): Requirement 2 The following requirements (i) to (iv) are satisfied. (i) The molar ratio of ethylene (XA) / α-olefin (XB) is 50 / 50 to 80 / 20. (ii) The weight fraction of the constitutional units derived from the non-conjugated polyene (XC) is 0.07% by weight to 10% by weight in 100% by weight of the ethylene / α-olefin / non-conjugated polyene copolymer (1). (iii) The intrinsic viscosity [η] is 5.1 to 7.0 dL / g. (iv) The ratio P(η*(ω=0.1) / η*(ω=100)) of the complex viscosity η*(ω=0.1) (Pa sec) at a frequency ω=0.1 rad / s to the complex viscosity η*(ω=100) (Pa sec) at a frequency ω=100 rad / s, which are obtained by linear viscoelastic measurement (190°C) using a rheometer, the intrinsic viscosity [η], and the weight fraction of the constituent unit derived from non-conjugated polyene (X-C) (weight fraction of (X-C)) satisfy the following formula (Z): 2.5≦P / ([η] 2.9 ) ≦ (X−C) weight fraction × 4 Formula (Z) 【Chemistry 1】
2. The ethylene / α-olefin / non-conjugated polyene copolymer (1) according to claim 1, characterized in that the non-conjugated polyene (XC) is 5-vinyl-2-norbornene (VNB).
3. A composition comprising the ethylene-α-olefin-non-conjugated polyene copolymer (1) according to claim 1.
4. The composition according to claim 3, further comprising an ethylene / α-olefin / non-conjugated polyene copolymer (2) that satisfies the following requirements 3 and 4: Requirement 3 The copolymer has structural units derived from ethylene (X-A'), an α-olefin (X-B') having 3 to 20 carbon atoms, and a non-conjugated polyene (X-C') containing, in the molecule, two or more partial structures selected from the group consisting of the following general formulae (I) and (II): Requirement 4 The intrinsic viscosity [η] is in the range of 1.0 to 2.2 dL / g. 【Chemistry 2】
5. Weight average molecular weight (Mw) is 1.0×10 5 ~4.0 x 10 5 (as measured by GPC) and the molecular weight distribution (Mw / Mn) (as measured by GPC) is in the range of 2.8 to 5.
0.
6. A molded article formed from the composition of claim 3.
7. A method for producing the ethylene-α-olefin-non-conjugated polyene copolymer (1) according to claim 1, characterized in that monomers consisting of the ethylene (X-A) according to claim 1, an α-olefin (X-B) having 3 to 20 carbon atoms, and a non-conjugated polyene (X-C) are copolymerized in the presence of at least one metallocene compound represented by the following general formula [A-2]: 【Chemistry 3】 In the formula [A-2], M is a titanium atom, a zirconium atom, or a hafnium atom, n is an integer of 1 to 3, each X is independently a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group, and R 1 ~R 5 and R 6 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 1 ~R 5 Adjacent groups among these may be bonded to each other to form a ring.
8. The method for producing an ethylene / α-olefin / non-conjugated polyene copolymer (1) according to claim 7, characterized in that the non-conjugated polyene (X-C) is 5-vinyl-2-norbornene (VNB).