Production method of thermal conductive sheet
By impregnating and firing a sheet with particulate carbon material and resin, the method enhances thermal conductivity and strength, addressing the limitations of conventional sheets in high-temperature applications.
Patent Information
- Application Number
- JP2023054121
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional thermally conductive sheets lack sufficient thermal conductivity and strength at high temperatures, particularly in applications exceeding 300°C, such as solar thermal power generation and semiconductor manufacturing.
A method involving the impregnation of a fired sheet containing particulate carbon material with an organic solvent and resin, followed by firing, to enhance thermal conductivity and strength, including steps like primary sheet forming, laminate forming, slicing, pre-firing, impregnation, and final firing, with specific conditions for orientation and weight loss rates.
The method produces a thermally conductive sheet with excellent strength and thermal conductivity at high temperatures, suitable for use in high-temperature environments.
Smart Images

Figure 2024142109000001 
Figure 2024142109000002 
Figure 2024142109000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a thermally conductive sheet. [Background technology]
[0002] In recent years, the amount of heat generated by electronic components such as power semiconductors (e.g., IGBT modules) and integrated circuit (IC) chips has increased as their performance has improved. As a result, it has become necessary to take measures to prevent malfunctions caused by temperature rises in electronic devices that use these components.
[0003] As a countermeasure against functional failures caused by temperature rises in electronic components, a method is generally adopted in which a heat sink, a heat sink plate, a heat sink fin, or other heat sink made of metal is attached to the heat generating body of the electronic component to promote heat dissipation. When using a heat sink, the heat generating body and the heat sink are closely attached via a sheet-like member with high thermal conductivity, i.e., a thermally conductive sheet, in order to efficiently transfer heat from the heat generating body to the heat sink.
[0004] In recent years, there has been a demand for thermally conductive sheets that can withstand use under high-temperature conditions exceeding 300° C. at sites such as solar thermal power generation, geothermal power generation, and semiconductor manufacturing. As a thermally conductive sheet that can withstand use under high-temperature conditions, thermally conductive sheets with reduced resin content have been considered in order to prevent the thermal conductivity of the thermally conductive sheet from decreasing due to thermal decomposition of the resin.
[0005] For example, Patent Document 1 discloses a composite sheet containing a carbon material, which does not contain resin or contains resin but the resin content is 15 volume % or less, the angle of the long axis direction of the carbon material with respect to the surface of the composite sheet is 60° to 90°, and the thermal conductivity of the composite sheet is 10 W / mK or more. According to Patent Document 1, the composite sheet is difficult to tear under pressure and has excellent compressibility. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2022-130068 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, according to the study by the present inventors, it has become clear that there is still room for improvement in the above-mentioned conventional heat conductive sheets in terms of exhibiting excellent heat conductivity even under high temperature conditions (i.e., excellent heat conductivity at high temperatures).Furthermore, there is a demand for further improving the strength of the above-mentioned conventional heat conductive sheets.
[0008] Therefore, an object of the present invention is to provide a method for producing a thermally conductive sheet that has excellent strength and thermal conductivity at high temperatures. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above problems, and have found that a thermally conductive sheet having excellent strength and thermal conductivity at high temperatures can be produced by impregnating a fired sheet containing particulate carbon material with an impregnation liquid containing an organic solvent and a resin, and then firing the sheet, thereby completing the present invention.
[0010] That is, an object of the present invention is to advantageously solve the above problems, and according to the present invention, there are provided the following methods for producing a thermally conductive sheet [1] to [7]. [1] A method for producing a thermally conductive sheet, comprising: a primary sheet forming step of pressing a composition containing a resin A and a particulate carbon material A into a sheet to obtain a primary sheet; a laminate forming step of stacking a plurality of the primary sheets in the thickness direction or folding or rolling the primary sheet to obtain a laminate; a slicing step of slicing the laminate at an angle of 45° or less to the stacking direction to obtain a secondary sheet; a pre-firing step of firing the secondary sheet to obtain a fired sheet; an impregnation step of impregnating the fired sheet with an impregnation liquid containing an organic solvent and a resin B to obtain an impregnated sheet; and a firing step of firing the impregnated sheet to obtain a thermally conductive sheet. In this way, according to the method for manufacturing a thermally conductive sheet, which includes a predetermined primary sheet molding step, a laminate formation step, a slicing step, a pre-firing step, an impregnation step, and a firing step, it is possible to manufacture a thermally conductive sheet that has excellent strength and thermal conductivity at high temperatures. In the present invention, the term "particulate carbon material" refers to a carbon material having an aspect ratio of 20 or less.
[0011] [2] A method for producing a thermally conductive sheet, comprising: an impregnation step of impregnating a sintered sheet with an impregnation liquid containing an organic solvent and a resin B to obtain an impregnated sheet; and a firing step of firing the impregnated sheet to obtain a thermally conductive sheet, wherein the sintered sheet contains a particulate carbon material A, the angle of the major axis direction of the particulate carbon material A with respect to the surface of the sintered sheet is 60° or more and 90° or less, and the sintered sheet is subjected to the following conditions: Heating rate: 10℃ / min Measurement temperature range: 30℃ to 1000℃ In air In a thermogravimetric curve obtained by performing thermogravimetric analysis on the above-mentioned sheet, the weight loss rate (%) from 150°C to 600°C is 3% or more and 20% or less, with the weight of the fired sheet before the thermogravimetric analysis being 100%. Thus, according to a method for producing a thermally conductive sheet which includes a prescribed impregnation step and a calcination step, in which the angle of the long axis direction of particulate carbon material A relative to the surface of the calcined sheet (hereinafter sometimes simply referred to as "the orientation angle of particulate carbon material A") is within the above-mentioned range, and in a thermogravimetric curve obtained by subjecting the calcined sheet to thermogravimetric analysis under prescribed conditions, the weight loss rate from 150°C to 600°C (hereinafter sometimes simply referred to as "the weight loss rate from 150°C to 600°C") is within the above-mentioned range, a thermally conductive sheet having excellent strength and thermal conductivity at high temperatures can be produced. In the present invention, the "orientation angle of the particulate carbon material A" can be measured according to the method described in the examples of this specification. In the present invention, the "weight loss rate from 150°C to 600°C" of the fired sheet can be calculated using the method described in the examples of this specification.
[0012] [3] The method for producing a thermal conductive sheet according to [1] or [2] above, wherein the impregnation step and the firing step are repeated multiple times. By repeating the impregnation step and the firing step, the strength and thermal conductivity at high temperatures of the obtained thermally conductive sheet can be further improved.
[0013] [4] The method for producing a thermally conductive sheet according to any one of the above [1] to [3], wherein the impregnation liquid further contains a particulate carbon material B. If an impregnation liquid further containing particulate carbon material B is used, the thermal conductivity of the thermally conductive sheet at high temperatures can be further improved.
[0014] [5] The method for producing a thermal conductive sheet according to the above [4], wherein the total content of the resin B and the particulate carbon material B in the impregnation liquid is 15 mass % or less. By using an impregnation liquid in which the total content of resin B and particulate carbon material B falls within the above-mentioned range, the strength of the thermally conductive sheet and the thermal conductivity at high temperatures can be further improved.
[0015] [6] The method for producing a thermal conductive sheet according to any one of the above [1] to [5], wherein the resin B in the impregnation liquid has a cyclic structure. By using an impregnation liquid containing a resin having a cyclic structure, the strength of the thermally conductive sheet and the thermal conductivity at high temperatures can be further improved.
[0016] [7] The method for producing a thermal conductive sheet according to any one of the above [1] to [6], wherein the organic solvent includes at least one selected from the group consisting of hexane, cyclohexane, toluene, methyl ethyl ketone and ethyl acetate. By using an impregnation liquid containing at least one selected from the group consisting of hexane, cyclohexane, toluene, methyl ethyl ketone, and ethyl acetate, the strength of the thermally conductive sheet and its thermal conductivity at high temperatures can be further improved. Effect of the Invention
[0017] According to the present invention, it is possible to provide a method for producing a thermally conductive sheet that can produce a thermally conductive sheet that is excellent in strength and thermal conductivity at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the present invention will be described in detail. The method for producing a thermally conductive sheet of the present invention is used, for example, when producing a thermally conductive sheet containing a particulate carbon material. The thermally conductive sheet produced by the method for producing the present invention can be used, for example, by being sandwiched between a heat generating body and a heat sink when attaching a heat sink to the heat sink. That is, the thermally conductive sheet produced by the method for producing the present invention functions as a heat sink member, and can constitute a heat sink device together with a heat sink such as a heat sink, a heat sink plate, or a heat sink fin.
[0019] The method for producing a thermal conductive sheet of the present invention includes the steps of: (1) A method for producing a thermal conductive sheet, the method including a primary sheet forming step, a laminate forming step, a slicing step, a pre-firing step, an impregnation step, and a firing step; and (2) A method for producing a thermal conductive sheet, comprising an impregnation step and a firing step, the fired sheet comprising a particulate carbon material A, the particulate carbon material A having an orientation angle within a predetermined range, and the fired sheet having a weight loss rate from 150°C to 600°C within a predetermined range. Either of the above two configurations may be used. For ease of explanation, the manufacturing method of a thermal conductive sheet having the above configuration (1) will be referred to as "manufacturing method 1 of a thermal conductive sheet," and the manufacturing method of a thermal conductive sheet having the above configuration (2) will be referred to as "manufacturing method 2 of a thermal conductive sheet."
[0020] (Thermal Conduction Sheet Manufacturing Method 1) The method for producing a thermal conductive sheet according to the present invention includes at least the steps of (A) a primary sheet forming step, (B) a laminate forming step, (C) a slicing step, (D) a pre-firing step, (E) an impregnation step, and (F) a firing step. The method for producing a thermal conductive sheet according to the present invention may further include any step other than the steps (A) to (F).
[0021] Since the thermal conductive sheet manufacturing method 1 of the present invention includes the above steps (A) to (F), it is possible to efficiently manufacture a thermal conductive sheet that is excellent in strength and thermal conductivity at high temperatures. Although the reason why the thermal conductive sheet manufacturing method 1 of the present invention provides the above effects is not clear, it is presumed to be as follows.
[0022] First, the manufacturing method 1 of the thermal conductive sheet of the present invention includes a primary sheet forming step, a laminate forming step, a slicing step, and a preliminary firing step. Here, in the fired sheet obtained through these steps, the particulate carbon material is considered to be well oriented in the thickness direction of the fired sheet. And, in the thermal conductive sheet obtained from such a fired sheet, the particulate carbon material is also well oriented in the thickness direction of the thermal conductive sheet, and therefore, it is considered to have excellent thermal conductivity at high temperatures. The manufacturing method 1 of the thermal conductive sheet of the present invention further includes an impregnation step and a firing step. In the impregnation step, the fired sheet is impregnated with an impregnation liquid containing an organic solvent and resin B to obtain an impregnated sheet. Here, since the impregnation liquid contains an organic solvent and has good impregnation properties for the fired sheet, it is considered that the obtained impregnated sheet contains a sufficient amount of organic solvent and resin B derived from the impregnation liquid. Then, in the firing step, when the impregnated sheet containing such an organic solvent and resin B is fired, it is considered that the organic solvent evaporates and at least a part of resin B is converted into a tar component (resin combustion residue). Such tar components derived from the resin in the thermal conductive sheet improve the strength of the thermal conductive sheet and have excellent thermal conductivity themselves, so they have the function of increasing the thermal conductivity of the thermal conductive sheet at high temperatures. Therefore, according to the thermal conductive sheet manufacturing method 1 of the present invention, a thermal conductive sheet having excellent strength and thermal conductivity at high temperatures can be efficiently manufactured.
[0023] <Primary sheet molding process> In the primary sheet forming step, a composition containing resin A and particulate carbon material A is pressed and formed into a sheet to obtain a primary sheet.
[0024] <<Composition>> The composition used in the primary sheet molding step contains a resin A and a particulate carbon material A. The composition may further contain components other than the resin A and the particulate carbon material A (other components).
[0025] [Resin A] Resin A is not particularly limited, and any resin can be used. For example, either liquid resin or solid resin can be used as resin A. Resin A may be used alone or in combination of two or more types. For example, both liquid resin and solid resin can be used as resin A. When liquid resin and solid resin are used in combination as resin A, the mass ratio of the liquid resin to the solid resin can be adjusted within a range in which the desired effect of the present invention can be obtained.
[0026] The liquid resin is not particularly limited as long as it is liquid at room temperature and normal pressure, and for example, a thermoplastic resin that is liquid at room temperature and normal pressure can be used. In the present invention, "normal temperature" refers to 23° C., and "normal pressure" refers to 1 atm (absolute pressure).
[0027] Examples of liquid resins include fluororesins, silicone resins, acrylic resins, epoxy resins, acrylonitrile-butadiene copolymers (nitrile rubbers), and 1,2-polybutadiene. These may be used alone or in combination of two or more.
[0028] The solid resin is not particularly limited as long as it is not liquid at room temperature and normal pressure. For example, a thermoplastic resin that is solid at room temperature and normal pressure, or a thermosetting resin that is solid at room temperature and normal pressure can be used.
[0029] Examples of thermoplastic resins that are solid at room temperature and pressure include acrylic resins such as poly(2-ethylhexyl acrylate), copolymers of acrylic acid and 2-ethylhexyl acrylate, polymethacrylic acid or its ester, and polyacrylic acid or its ester; silicone resins; fluororesins; polyethylene; polypropylene; ethylene-propylene copolymers; polymethylpentene; polyvinyl chloride; polyvinylidene chloride; polyvinyl acetate; ethylene-vinyl acetate copolymers; polyvinyl alcohol; polyacetal; polyethylene terephthalate; polybutylene terephthalate; polyethylene naphthalate; polystyrene; polyacrylonitrile; styrene-acrylonitrile copolymers. Examples of the polymer include acrylonitrile-butadiene copolymers (nitrile rubbers), acrylonitrile-butadiene-styrene copolymers (ABS resins), styrene-butadiene random copolymers, styrene-butadiene block copolymers or hydrogenated products thereof, and styrene-isoprene block copolymers or hydrogenated products thereof, and other styrene-based resins, polyphenylene ethers, modified polyphenylene ethers, aliphatic polyamides, aromatic polyamides, polyamideimides, polycarbonates, polyphenylene sulfides, polysulfones, polyethersulfones, polyethernitriles, polyetherketones, polyketones, polyurethanes, liquid crystal polymers, and ionomers. These may be used alone or in combination of two or more. In the present invention, rubber is included in the "resin".
[0030] Examples of thermosetting resins that are solid at room temperature and normal pressure include natural rubber, butadiene rubber, isoprene rubber, nitrile rubber, hydrogenated nitrile rubber, chloroprene rubber, ethylene propylene rubber, chlorinated polyethylene, chlorosulfonated polyethylene, butyl rubber, halogenated butyl rubber, polyisobutylene rubber, epoxy resin, polyimide resin, bismaleimide resin, benzocyclobutene resin, phenolic resin, unsaturated polyester, diallyl phthalate resin, polyimide silicone resin, polyurethane, thermosetting polyphenylene ether, thermosetting modified polyphenylene ether, etc. These may be used alone or in combination of two or more.
[0031] Here, it is preferable to use a resin having a cyclic structure as the resin A. It is presumed that using a resin having a cyclic structure as the resin A increases the amount of resin-derived components (tar components) remaining in the thermal conductive sheet, and the strength and thermal conductivity at high temperatures of the obtained thermal conductive sheet can be further improved. The cyclic structure is not particularly limited as long as it is composed of atoms such as carbon, hydrogen, nitrogen, and oxygen, but is preferably a hydrocarbon ring (a ring composed of carbon and hydrogen), and particularly preferably a benzene ring. Examples of resins having a cyclic structure include styrene-based resins such as polystyrene, styrene-acrylonitrile copolymers, acrylonitrile-butadiene-styrene copolymers (ABS resins), styrene-butadiene block copolymers or hydrogenated products thereof, and styrene-isoprene block copolymers or hydrogenated products thereof; imide resins such as polyimide resins and polyamide-imide resins; epoxy resins such as bisphenol-type epoxy resins, novolac-type epoxy resins, cyclic epoxy resins, and alicyclic epoxy resins; etc. Among these, resins having a benzene ring are preferred, styrene-based resins are more preferred, and styrene-butadiene random copolymers are more preferred.
[0032] The content of the styrene unit in the styrene resin is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, when the amount of all repeating units in the styrene resin is 100% by mass. If the content of the styrene monomer unit in the styrene resin is equal to or more than the lower limit, the strength of the obtained heat conductive sheet and the heat conductivity at high temperatures can be further improved. The upper limit of the content of the styrene monomer unit in the styrene resin is not particularly limited, but can be, for example, 50% by mass or less, and can be 40% by mass or less. In the present invention, the term "styrene unit" means "a repeating unit derived from styrene contained in a polymer obtained by using styrene as a monomer".
[0033] [Particulate carbon material A] Here, the particulate carbon material A is not particularly limited as long as it is a carbon material having an aspect ratio of 20 or less, and examples thereof include graphite such as artificial graphite, scaly graphite, exfoliated graphite, natural graphite, acid-treated graphite, expandable graphite, and expanded graphite; carbon black; etc. These may be used alone or in combination of two or more kinds. Among these, it is preferable to use expanded graphite as the particulate carbon material A. If expanded graphite is used as the particulate carbon material A, the thermal conductivity of the thermally conductive sheet at high temperatures can be further improved.
[0034] Expanded graphite that can be suitably used as the particulate carbon material A can be obtained by, for example, chemically treating graphite such as flake graphite with sulfuric acid or the like to obtain expandable graphite, expanding the graphite by heat treatment, and then pulverizing the expanded graphite. Examples of commercially available expanded graphite include EC-1500, EC-1000, EC-500, EC-300, EC-100, EC-50, and EC-10 (all trade names) manufactured by Ito Graphite Industries Co., Ltd.
[0035] --Volume average particle size-- Here, the volume average particle diameter of the particulate carbon material A is preferably 50 μm or more, more preferably 100 μm or more, even more preferably 150 μm or more, particularly preferably 200 μm or more, and is preferably 500 μm or less, more preferably 400 μm or less, and even more preferably 300 μm or less. If the volume average particle diameter of the particulate carbon material A is equal to or greater than the lower limit, the thermal conductivity of the thermal conductive sheet at high temperatures can be further improved. Also, if the volume average particle diameter of the particulate carbon material A is equal to or less than the upper limit, the strength of the thermal conductive sheet can be further improved. In the present invention, the "volume average particle size" of a particulate carbon material refers to the particle size (D50) at which the cumulative volume calculated from the small diameter side in the particle size distribution (volume basis) measured by a laser diffraction method is 50%, and can be measured according to the method described in the examples of this specification.
[0036] Here, in the present invention, the aspect ratio (major axis / minor axis) of the particulate carbon material (particulate carbon material A and B) must be 20 or less, preferably 10 or less, and more preferably 5 or less. The aspect ratio is usually more than 1. In addition, in the present invention, the "aspect ratio" of the particulate carbon material can be determined by observing the particulate carbon material with a SEM (scanning electron microscope), measuring the maximum diameter (major axis) and the particle diameter (minor axis) in the direction perpendicular to the maximum diameter for any 50 particles, and calculating the average value of the ratio of the major axis to the minor axis (major axis / minor axis).
[0037] [Other ingredients] The composition used in the primary sheet molding step may further contain other components in addition to the above-mentioned resin A and particulate carbon material A. Examples of other components that can be used include dispersants and fibrous carbon materials (e.g., carbon nanotubes, vapor-grown carbon fibers, carbon fibers obtained by carbonizing organic fibers, and cut products thereof). The dispersant is not particularly limited, and any known dispersant can be used. The content of the dispersant in the composition can be adjusted within a range in which the desired effects of the present invention can be obtained. In the present invention, the term "fibrous carbon material" refers to a carbon material having an aspect ratio of more than 20.
[0038] [Preparation of Composition] The composition is not particularly limited and can be prepared by mixing the above-mentioned components and then optionally grinding them. The mixing of the above-mentioned components is not particularly limited, and can be performed using a known mixing device such as a kneader; a mixer such as a Henschel mixer, a Hobart mixer, or a high-speed mixer; a twin-screw kneader; or a roll. The mixing may be performed in the presence of a solvent such as ethyl acetate. The resin A may be dissolved or dispersed in advance in a solvent to form a resin solution or resin dispersion, which may then be mixed with the particulate carbon material A and other components that are added as required. The mixing time may be, for example, 5 minutes or more and 60 minutes or less. The mixing temperature may be, for example, 5°C or more and 160°C or less. Furthermore, the crushing that is optionally performed after the mixing of the above-mentioned components is not particularly limited, and can be performed using a known crushing device. The crushing conditions (crushing time, etc.) may be appropriately adjusted within a range in which the desired effects of the present invention can be obtained.
[0039] [Molding of the composition] The composition prepared as described above can be pressed and molded into a sheet. The sheet-like product obtained by pressing the composition in this manner can be used as a primary sheet. If a solvent is used during mixing, it is preferable to remove the solvent before molding into a sheet. For example, if degassing is performed using vacuum degassing, the solvent can be removed at the same time as degassing.
[0040] Here, the composition can be molded into a sheet using a known molding method such as press molding, rolling molding, or extrusion molding, without any particular limitation, as long as the molding method is one in which pressure is applied. Among them, the composition is preferably molded into a sheet by rolling molding (primary processing), and more preferably molded into a sheet by passing the composition between rolls while sandwiched between protective films. The protective film is not particularly limited, and may be a polyethylene terephthalate (PET) film or the like that has been subjected to sandblasting. The roll temperature may be 5°C or higher and 150°C or lower, the roll gap may be 50 μm or higher and 2500 μm or lower, the roll linear pressure may be 1 kg / cm or higher and 3000 kg / cm or lower, and the roll speed may be 0.1 m / min or higher and 20 m / min or lower.
[0041] The content of the particulate carbon material A in the primary sheet is preferably 150 parts by mass or more, more preferably 200 parts by mass or more, even more preferably 250 parts by mass or more, and preferably 600 parts by mass or less, more preferably 550 parts by mass or less, and even more preferably 500 parts by mass or less, relative to 100 parts by mass of the resin A. If the content of the particulate carbon material A in the primary sheet is equal to or more than the lower limit, the strength of the obtained thermal conductive sheet and the thermal conductivity at high temperatures can be further improved. On the other hand, if the content of the particulate carbon material A in the primary sheet is equal to or less than the upper limit, the strength of the obtained thermal conductive sheet can be further improved.
[0042] In addition, the volume fraction of the particulate carbon material A in the primary sheet is preferably 40 volume% or more, more preferably 45 volume% or more, even more preferably 50 volume% or more, particularly preferably 55 volume% or more, and preferably 75 volume% or less, more preferably 70 volume% or less, and even more preferably 65 volume% or less, based on the total volume of the primary sheet being 100 volume%. If the volume fraction of the particulate carbon material A in the primary sheet is equal to or more than the above lower limit, the strength of the obtained heat conductive sheet and the heat conductivity at high temperatures can be further improved. If the volume fraction of the particulate carbon material A is equal to or less than the above upper limit, the strength of the obtained heat conductive sheet can be further improved.
[0043] <Laminate formation process> In the laminate formation step, a laminate is obtained in which a plurality of primary sheets containing resin A and particulate carbon material A are formed in the thickness direction by stacking a plurality of primary sheets obtained in the above-mentioned primary sheet molding step, or by folding or rolling the primary sheets. Here, the formation of the laminate by folding the primary sheets is not particularly limited, and can be performed by folding the primary sheets at a constant width using a folding machine. Furthermore, the formation of the laminate by rolling the primary sheets is not particularly limited, and can be performed by rolling the primary sheets around an axis parallel to the short side direction or long side direction of the primary sheets. Furthermore, the formation of the laminate by stacking the primary sheets is not particularly limited, and can be performed using a lamination device.
[0044] In the laminate formation step, it is preferable to pressurize the obtained laminate in the stacking direction (secondary pressurization) while heating it. By performing secondary pressurization in which the laminate is pressed in the stacking direction while heating it, it is possible to promote fusion between the stacked primary sheets.
[0045] Here, the pressure applied to the laminate in the lamination direction may be 0.05 MPa or more and 0.50 MPa or less. The heating temperature of the laminate is not particularly limited, but is preferably 50° C. or higher and 170° C. or lower. Furthermore, the heating time for the laminate can be, for example, from 10 seconds to 30 minutes.
[0046] In addition, in the laminate obtained by stacking, folding or rolling the primary sheet, it is presumed that the particulate carbon material A is oriented in a direction substantially perpendicular to the stacking direction. For example, when the particulate carbon material A has a scale shape, it is presumed that the direction of the major axis of the main surface of the scale shape is substantially perpendicular to the stacking direction.
[0047] <Slicing process> In the slicing step, the laminate obtained in the laminate forming step described above is sliced at an angle of 45° or less with respect to the lamination direction to obtain secondary sheets consisting of slices of the laminate. Here, the method for slicing the laminate is not particularly limited, and examples thereof include a multi-blade method, a laser processing method, a water jet method, and a knife processing method. Among these, the knife processing method is preferred because it is easy to make the thickness of the secondary sheet uniform. In addition, the cutting tool used when slicing the laminate is not particularly limited, and a slicing member having a smooth plate surface with a slit and a blade portion protruding from the slit portion (for example, a plane or slicer with a sharp blade) can be used.
[0048] The angle at which the laminate is sliced must be 45° or less with respect to the stacking direction, preferably 30° or less with respect to the stacking direction, more preferably 15° or less with respect to the stacking direction, and particularly preferably approximately 0° with respect to the stacking direction (i.e., in the direction along the stacking direction). In the secondary sheet thus obtained, the particulate carbon material A is well oriented in the thickness direction.
[0049] <Pre-firing process> In the pre-firing step, the secondary sheet obtained in the above-mentioned slicing step is fired to burn and remove the resin A contained in the secondary sheet, thereby obtaining a fired sheet. The obtained fired sheet is a sheet obtained by removing a part or all of the resin A from the secondary sheet described above. Therefore, in the fired sheet, the particulate carbon material A is well oriented in the thickness direction. For example, when the particulate carbon material A has a scale shape, the direction of the major axis of the main surface of the scale shape approximately coincides with the thickness direction of the secondary sheet.
[0050] Here, the secondary sheet is preferably fired in a nitrogen atmosphere in the pre-firing step. It is presumed that the amount of resin-derived components (tar components) in the fired sheet increases when the pre-firing step is performed in a nitrogen atmosphere, but the strength of the resulting thermal conductive sheet and the thermal conductivity at high temperatures can be further improved. In addition, the heating temperature (firing temperature) when firing the secondary sheet in the pre-firing step is preferably 200°C or higher, more preferably 250°C or higher, even more preferably 300°C or higher, preferably 1500°C or lower, more preferably 1200°C or lower, even more preferably 1000°C or lower, and particularly preferably 800°C or lower. If the firing temperature is 200°C or higher, the compressibility of the resulting thermal conductive sheet can be well ensured. On the other hand, if the firing temperature is 1500°C or lower, the strength of the resulting thermal conductive sheet can be further improved. In the present invention, the term "nitrogen atmosphere" refers to an atmosphere having a nitrogen concentration of 90% by volume or more.
[0051] The heating time (firing time) for firing the secondary sheet in the pre-firing step can be adjusted depending on the firing temperature, and can be, for example, from 30 minutes to 72 hours.
[0052] <<Baked sheet>> Thickness The thickness of the fired sheet is preferably 100 μm or more, more preferably 150 μm or more, even more preferably 200 μm or more, and preferably 500 μm or less, more preferably 400 μm or less. If the thickness of the fired sheet is equal to or greater than the lower limit, the strength of the resulting thermal conductive sheet and the thermal conductivity at high temperatures can be further improved. On the other hand, if the thickness of the fired sheet is equal to or less than the upper limit, the thermal resistance of the resulting thermal conductive sheet can be appropriately reduced. The "thickness" of the fired sheet can be measured according to the method described in the Examples of this specification.
[0053] [density] The density of the fired sheet is 1.2 g / cm 3 It is preferable that the content is 1.25 g / cm or more. 3 More preferably, it is 1.3 g / cm or more. 3 More preferably, it is 1.35 g / cm or more. 3 If the density of the fired sheet is equal to or higher than the above lower limit, the strength of the resulting thermally conductive sheet and the thermal conductivity at high temperatures can be further improved. The upper limit of the density of the fired sheet is not particularly limited, but is, for example, 1.6 g / cm. 3 It can be less than 1.5 g / cm 3 It can be as follows: The "density" of the fired sheet can be measured according to the method described in the Examples of this specification.
[0054] <Impregnation process> In the impregnation step, the fired sheet obtained in the above-mentioned pre-firing step is impregnated with an impregnation liquid to obtain an impregnated sheet. The obtained impregnated sheet is a sheet in which the above-mentioned fired sheet contains the impregnation liquid.
[0055] <<Impregnation liquid>> The impregnation liquid contains at least a resin B and an organic solvent as a solvent, and optionally further contains a particulate carbon material B and other additive components.
[0056] [Organic solvents] The solvent of the impregnation liquid is not particularly limited as long as it contains an organic solvent. For example, the impregnation liquid may contain only an organic solvent as the solvent, or the solvent may be a mixture of an organic solvent and water. The impregnation liquid may contain one type of organic solvent, or may contain two or more types of organic solvents.
[0057] The organic solvent contained in the impregnation liquid is not particularly limited as long as it has the ability to impregnate the fired sheet. Among them, from the viewpoint of further improving the strength and thermal conductivity at high temperatures of the obtained thermal conductive sheet, organic solvents that dissolve resins having a cyclic structure well, such as hexane, cyclohexane, toluene, methyl ethyl ketone, and ethyl acetate, are preferred, and cyclohexane is more preferred.
[0058] Here, from the viewpoint of increasing the impregnation of the sintered sheet with the impregnation liquid and further improving the strength and thermal conductivity at high temperatures of the obtained thermally conductive sheet, the proportion of the organic solvent in the solvent in the impregnation liquid is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 100 mass% (i.e., the impregnation liquid contains only an organic solvent as the solvent), with the total amount of the solvent being 100 mass%.
[0059] [Resin B] Resin B contained in the impregnation liquid may be, for example, the same as resin A described above in the section "primary sheet molding process". Among them, resins having a cyclic structure are preferred, styrene-based resins are more preferred, and styrene-butadiene random copolymers are even more preferred. It is presumed that the use of a resin having a cyclic structure as resin B increases the amount of resin-derived components (tar components) remaining in the thermal conductive sheet, and the strength and thermal conductivity at high temperatures of the obtained thermal conductive sheet can be further improved. Note that resin B may be used alone or in combination of two or more types in any ratio.
[0060] The content of resin B in the impregnation liquid is preferably 1% by mass or more, more preferably 2.5% by mass or more, even more preferably 5% by mass or more, particularly preferably 7.5% by mass or more, preferably 15% by mass or less, more preferably 14% by mass or less, and even more preferably 13% by mass or less, based on the total amount of the impregnation liquid being 100% by mass. If the content of resin B in the impregnation liquid is 1% by mass or more, the amount of resin B impregnated into the fired sheet increases, and the strength and thermal conductivity at high temperatures of the obtained thermal conductive sheet can be further improved. In addition, if the content of resin B in the impregnation liquid is 15% by mass or less, the viscosity of the impregnation liquid can be prevented from increasing excessively, and the impregnation of the fired sheet with the impregnation liquid can be well secured. Therefore, the strength and thermal conductivity at high temperatures of the obtained thermal conductive sheet can be further improved.
[0061] [Particulate carbon material B] Here, from the viewpoint of further improving the thermal conductivity of the obtained thermally conductive sheet at high temperatures, the impregnation liquid preferably further contains a particulate carbon material B. Examples of the particulate carbon material B contained in the impregnation liquid include the same as the particulate carbon material A described above in the section "Primary sheet molding step". Among them, graphite is preferable, expanded graphite, exfoliated graphite, and graphene are more preferable, and expanded graphite is even more preferable. Note that the particulate carbon material B may be used alone or in combination of two or more kinds at any ratio.
[0062] --Volume average particle size-- Here, the particulate carbon material B preferably has a volume average particle diameter of 0.5 μm or more, more preferably 1 μm or more, even more preferably 2 μm or more, particularly preferably 4 μm or more, and preferably 10 μm or less, more preferably 9 μm or less, and even more preferably 8 μm or less. If the volume average particle diameter of the particulate carbon material B is 0.5 μm or more, it is possible to effectively fill the narrow gaps of the voids present in the fired sheet, and the thermal conductivity of the obtained thermal conductive sheet at high temperatures can be further improved. In addition, if the volume average particle diameter of the particulate carbon material B is 10 μm or less, the particulate carbon material B efficiently enters the narrow gaps of the voids present in the fired sheet, thereby increasing the impregnation of the particulate carbon material B into the fired sheet, and the thermal conductivity of the obtained thermal conductive sheet at high temperatures can be further improved.
[0063] When the impregnation liquid contains particulate carbonaceous material B, the content of particulate carbonaceous material B in the impregnation liquid is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, preferably 15% by mass or less, more preferably 12.5% by mass or less, and even more preferably 10% by mass or less, based on the total amount of the impregnation liquid being 100% by mass. If the content of particulate carbonaceous material B in the impregnation liquid is 1% by mass or more, the amount of particulate carbonaceous material B impregnated into the fired sheet increases, and the thermal conductivity of the obtained thermal conductive sheet at high temperatures can be further improved. If the content of particulate carbonaceous material B in the impregnation liquid is 15% by mass or less, the impregnation of the fired sheet with the impregnation liquid can be well ensured, and the thermal conductivity of the obtained thermal conductive sheet at high temperatures can be further improved.
[0064] In addition, the total content of resin B and particulate carbon material B in the impregnation liquid is preferably 1% by mass or more, more preferably 2.5% by mass or more, even more preferably 5% by mass or more, preferably 15% by mass or less, more preferably 14% by mass or less, even more preferably 13% by mass or less, and particularly preferably 12% by mass or less, based on the total amount of the impregnation liquid being 100% by mass. If the total content of resin B and particulate carbon material B in the impregnation liquid is 1% by mass or more, the amount of resin B and particulate carbon material B impregnated into the fired sheet increases, and the strength and thermal conductivity at high temperatures of the obtained thermal conductive sheet can be further improved. In addition, if the total content of resin B and particulate carbon material B in the impregnation liquid is 15% by mass or less, the viscosity of the impregnation liquid is prevented from increasing excessively, and the impregnation of the fired sheet with the impregnation liquid can be well secured. Therefore, the strength and thermal conductivity at high temperatures of the obtained thermal conductive sheet can be further improved.
[0065] [Additional ingredients] Examples of additive components that the impregnation liquid may optionally contain (components other than the solvent, resin B, and particulate carbon material B) include the other components described above in the section "Primary sheet forming process" and surfactants (dispersants). The content of the additive components in the impregnation liquid is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.1% by mass or less, and particularly preferably 0% by mass (i.e., the impregnation liquid does not contain any additive components), based on the total amount of the impregnation liquid being 100% by mass, from the viewpoint of ensuring good impregnation of the sintered sheet with the impregnation liquid and further improving the strength of the obtained thermal conductive sheet and the thermal conductivity at high temperatures. The additive components may be used alone or in combination of two or more kinds at any ratio.
[0066] [Impregnation method] The method of impregnating the calcined sheet with the impregnating liquid is not particularly limited. For example, the calcined sheet can be impregnated with the impregnating liquid by immersing the calcined sheet in the impregnating liquid in a container and then evacuating the container. The conditions for evacuating the sheet are not particularly limited, and may be appropriately adjusted so that bubbles are generated from the surface of the calcined sheet and the solvent does not boil.
[0067] <<Firing process>> In the firing step, the impregnated sheet obtained in the above-mentioned impregnation step is fired to burn off the solvent and resin contained in the impregnated sheet and remove them, thereby obtaining a thermally conductive sheet. The obtained thermally conductive sheet is a sheet obtained by removing the solvent from the above-mentioned impregnated sheet and removing a part or all of the resin. It is presumed that the unremoved resin remains in the thermally conductive sheet as a component derived from the resin (tar component).
[0068] Here, the impregnated sheet is preferably baked in a nitrogen atmosphere in the baking process. It is presumed that the baking process is performed in a nitrogen atmosphere because the amount of resin-derived components (tar components) in the thermal conductive sheet increases, and the strength of the obtained thermal conductive sheet and the thermal conductivity at high temperatures can be further improved. In addition, the heating temperature (baking temperature) when baking the impregnated sheet in the baking process is preferably 200°C or higher, more preferably 250°C or higher, and even more preferably 300°C or higher, preferably 1500°C or lower, more preferably 1200°C or lower, even more preferably 1000°C or lower, and particularly preferably 800°C or lower. If the baking temperature in the baking process is 200°C or higher, the compressibility of the obtained thermal conductive sheet can be sufficiently ensured. On the other hand, if the baking temperature in the baking process is 1500°C or lower, the strength of the obtained thermal conductive sheet can be further improved.
[0069] The heating time (firing time) for firing the fired sheet in the firing step can be adjusted depending on the firing temperature, and can be, for example, from 30 minutes to 72 hours.
[0070] In addition, the impregnation step and the firing step are preferably repeated multiple times from the viewpoint of further improving the strength of the obtained thermal conductive sheet and the thermal conductivity at high temperatures. That is, it is preferable to perform the impregnation step and the firing step again after the first firing step. In addition, it is preferable to perform the impregnation step and the firing step three or less times from the viewpoint of the production efficiency of the thermal conductive sheet.
[0071] (Thermal Conduction Sheet Manufacturing Method 2) The method for producing a thermally conductive sheet 2 of the present invention includes an impregnation step of impregnating a fired sheet containing particulate carbon material A with an impregnation liquid containing an organic solvent and resin B to obtain an impregnated sheet, and a firing step of firing the impregnated sheet to obtain a thermally conductive sheet. Note that the method for producing a thermally conductive sheet 2 of the present invention may further include any step other than the impregnation step and the firing step.
[0072] Here, the thermal conductive sheet manufacturing method 2 of the present invention is characterized in that the orientation angle of the particulate carbon material A is 60° or more and 90° or less, and the weight loss rate of the fired sheet from 150°C to 600°C is 3% or more and 20% or less.
[0073] The thermal conductive sheet manufacturing method 2 of the present invention uses a fired sheet having predetermined properties and includes a predetermined impregnation step and firing step, so that a thermal conductive sheet having excellent strength and thermal conductivity at high temperatures can be efficiently manufactured. Although the reason why the above-mentioned effects are obtained by the thermal conductive sheet manufacturing method 2 of the present invention is not clear, it is presumed to be as follows.
[0074] First, the thermal conductive sheet manufacturing method 2 of the present invention uses a sintered sheet having a predetermined property, and includes an impregnation step and a sintering step. Here, the sintered sheet contains particulate carbon material A, and the particulate carbon material A is oriented at an angle of 60° to 90° with respect to the surface of the sintered sheet. The thermal conductive sheet obtained from such a sintered sheet also has particulate carbon material A oriented at an angle of 60° to 90° in the thickness direction of the thermal conductive sheet, and is therefore considered to have excellent thermal conductivity at high temperatures. Next, according to the study of the present inventor, it was revealed that the strength and thermal conductivity of the obtained thermal conductive sheet at high temperatures are improved when the weight loss rate from 150°C to 600°C is 3% or more and 20% or less in the thermogravimetric curve obtained by performing thermogravimetric analysis on the fired sheet under predetermined conditions. In the present inventor's deduction, the components in the fired sheet that are thermally decomposed in the range of 150°C to 600°C in the air atmosphere are considered to be tar components (resin combustion residues) generated when the resin (resin A) used to form the primary sheet and secondary sheet, which are precursors of the fired sheet, is fired during firing of the secondary sheet in the preliminary firing step, for example, when the fired sheet is produced through the primary sheet forming step, laminate forming step, slicing step, and pre-firing step in the manufacturing method 1 of the thermal conductive sheet of the present invention. Such tar components derived from the resin in the thermal conductive sheet improve the strength of the thermal conductive sheet and, since they themselves have excellent thermal conductivity, have the function of increasing the thermal conductivity of the thermal conductive sheet at high temperatures. When the fired sheet is subjected to thermogravimetric analysis under specified conditions, it is believed that the tar components derived from the resin disappear (thermal decomposition) due to evaporation, decomposition, etc., between 150°C and 600°C. In other words, in the thermogravimetric curve obtained by performing thermogravimetric analysis under specified conditions on the fired sheet, the weight loss from 150°C to 600°C is believed to be due to the disappearance (thermal decomposition) of the tar components derived from the resin in the fired sheet. Therefore, the above-mentioned "weight loss rate from 150°C to 600°C" can be said to correspond to the proportion (weight %) of the weight of the tar components derived from the resin in 100% of the weight of the fired sheet. Since the weight loss rate of the fired sheet from 150°C to 600°C is 3% or more, it can be said that the fired sheet contains a sufficient amount of tar components, and the thermal conductive sheet obtained from the fired sheet has excellent strength and thermal conductivity at high temperatures. In addition, since the weight loss rate of the fired sheet from 150°C to 600°C is 20% or less, it can be said that the fired sheet does not contain an excessive amount of tar components that would cause the amount of particulate carbon material in the fired sheet to be excessively reduced. Furthermore, the manufacturing method 2 of the thermal conductive sheet of the present invention includes an impregnation step and a firing step. As described above in the section "Manufacturing method 1 of the thermal conductive sheet", the amount of tar components in the obtained thermal conductive sheet can be increased by going through the impregnation step and the firing step. Therefore, according to the thermally conductive sheet manufacturing method 2 of the present invention, a thermally conductive sheet having excellent strength and thermal conductivity at high temperatures can be efficiently manufactured.
[0075] <Impregnation process> In the impregnation step, the fired sheet is impregnated with an impregnation liquid to obtain an impregnated sheet. The obtained impregnated sheet is a sheet comprising the fired sheet described above and the impregnation liquid.
[0076] <<Baked sheet>> The fired sheet used in the impregnation step contains the particulate carbon material A, and optionally further contains components other than the particulate carbon material A (other components).
[0077] [Particulate carbon material A] As the particulate carbon material A, for example, those described above in the section "Method for producing a thermally conductive sheet 1" can be used. The preferred examples and attributes of the particulate carbon material A are also as described above in the section "Method for producing a thermally conductive sheet 1". The particulate carbon material A may be used alone or in combination of two or more types.
[0078] --Orientation angle-- The angle of the major axis direction of the particulate carbon material A relative to the surface of the fired sheet (the orientation angle of the particulate carbon material A) must be 60° or more and 90° or less, and the orientation angle of the particulate carbon material A is preferably 65° or more, and more preferably 70° or more. If the orientation angle of the particulate carbon material A is outside the above-mentioned range, the thermal resistance of the obtained thermal conductive sheet increases and the thermal conductivity decreases. If the orientation angle of the particulate carbon material A is within the above-mentioned range, the thermal conductivity of the obtained thermal conductive sheet at high temperatures can be further improved and the thermal resistance at high pressures can be reduced.
[0079] [Other ingredients] The fired sheet may further contain components (other components) other than the particulate carbon material A. Examples of the other components include those described in the section "Method for producing a thermal conductive sheet 1." The other components may be used alone or in combination of two or more at any ratio.
[0080] [Weight loss rate from 150℃ to 600℃] Here, the calcined sheet must have a weight loss rate of 3% or more and 20% or less from 150 ° C to 600 ° C in a thermogravimetric curve obtained by performing thermogravimetric analysis under predetermined conditions, with the weight of the calcined sheet before the thermogravimetric analysis being 100%, and the weight loss rate from 150 ° C to 600 ° C is preferably 6% or more, more preferably 9% or more, even more preferably 13% or more, and preferably 19% or less. If the weight loss rate of the calcined sheet from 150 ° C to 600 ° C is less than 3%, it is presumed that the amount of tar components in the calcined sheet is reduced, but the strength and thermal conductivity at high temperatures of the resulting thermal conductive sheet are reduced. In addition, if the weight loss rate of the calcined sheet from 150 ° C to 600 ° C is more than 20%, it is presumed that the proportion of particulate carbon material A in the calcined sheet is reduced, but the strength and thermal conductivity at high temperatures of the resulting thermal conductive sheet are reduced. The weight loss rate of the fired sheet from 150°C to 600°C can be adjusted by changing the type and amount of resin used to prepare the fired sheet, the firing conditions when obtaining the fired sheet (e.g., firing temperature and time), etc. Specifically, the weight loss rate of the fired sheet from 150°C to 600°C can be increased by increasing the amount of resin used to prepare the fired sheet and / or using a resin having a cyclic structure as the resin. The weight loss rate of the fired sheet from 150°C to 600°C can also be increased by lowering the firing temperature when obtaining the fired sheet.
[0081] The thickness and density of the fired sheet are as described above in the section "Method 1 for producing a thermally conductive sheet."
[0082] [How to make the fired sheet] The fired sheet is not particularly limited, but can be produced, for example, through the primary sheet forming step, laminate forming step, slicing step, and pre-firing step described above in the section "Method of producing a thermal conductive sheet 1." The various conditions in each step are also as described above in the section "Method of producing a thermal conductive sheet 1."
[0083] <<Impregnation liquid>> As the impregnation liquid, the liquids mentioned above in the section "Method of manufacturing thermal conductive sheet 1" can be used.
[0084] <<Impregnation method>> As the impregnation method, for example, the method described above in "Method of manufacturing thermal conductive sheet 1" can be used.
[0085] <Firing process> In the firing step, the impregnated sheet obtained in the above-mentioned impregnation step is fired to burn off the solvent and resin contained in the impregnated sheet and remove them, thereby obtaining a thermally conductive sheet. The obtained thermally conductive sheet is a sheet obtained by removing the solvent from the above-mentioned impregnated sheet and removing part or all of the resin. It is presumed that the resin that was not removed remains in the thermally conductive sheet as a component derived from the resin (tar component). The firing conditions in the firing step are as described above in the section "Method 1 for manufacturing a thermally conductive sheet." EXAMPLES
[0086] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" expressing amounts are based on mass unless otherwise specified. The volume average particle diameter of the particulate carbon material, the volume fraction of particulate carbon material A in the primary sheet, the weight loss rate, thickness and density of the fired sheet from 150°C to 600°C, the orientation angle of particulate carbon material A in the fired sheet, and the strength and thermal conductivity at high temperatures of the thermal conductive sheet were measured or evaluated by the following methods.
[0087] <Volume average particle size of particulate carbon material> The volume average particle diameter of the particulate carbon material was measured using a laser diffraction / scattering type particle size distribution measuring device (manufactured by Horiba, Ltd., model "LA960"). Specifically, a particle size distribution curve was created with the obtained particle diameter on the horizontal axis and the volume-converted particle frequency on the vertical axis. In the particle size distribution curve, the particle diameter (D50) at which the cumulative volume calculated from the small diameter side was 50% was obtained, and this was taken as the volume average particle diameter value of the particulate carbon material. <Volume fraction of particulate carbon material A in the primary sheet> The volume fraction of particulate carbon material A in the primary sheet was calculated by dividing the mass of particulate carbon material A contained in the primary sheet by the density to determine the volume occupied by particulate carbon material A, and then calculating the proportion (volume %) of the particulate carbon material A in 100 volume % of the primary sheet. <Orientation angle of particulate carbon material A> The orientation angle of the particulate carbon material A in the fired sheet was determined by observing a cross section of the fired sheet cut into a regular octagon with a scanning electron microscope (SEM, Hitachi High-Technologies Corporation's "SU-3500") at a magnification that covered the entire sheet from top to bottom. The magnification was 700x. 50 lines were drawn along the long axis of the particulate carbon material A in this cross section, and the average angle of the long axis with respect to the surface of the fired sheet was calculated. If the angle exceeded 90°, a supplementary angle was used. This was performed for eight faces, and the largest value among the eight faces was taken as the orientation angle of the particulate carbon material A in the fired sheet. <Weight loss rate from 150℃ to 600℃> The weight loss rate of the fired sheet from 150°C to 600°C was measured using a thermogravimetric measuring device (manufactured by Hitachi High-Tech Science Corporation, product name "TA7000"). Specifically, the weight (W(g)) of the fired sheet was measured under the conditions of a temperature rise rate of 10°C / min and a measurement temperature range of 30 to 1000°C in an air atmosphere measurement environment. Based on the obtained data, a graph (thermogravimetric curve) was created in which the elapsed time after the start of measurement was plotted on the horizontal axis (X-coordinate axis) and the weight (W(g)) of the fired sheet was plotted on the vertical axis (Y-coordinate axis). Then, the weight loss rate (TG(%)) of the fired sheet from 150°C to 600°C was calculated from the following formula (1). TG(%)={(W 150 -W 600 ) / W0}×100 (1) [In the formula (1), W0 is the weight (g) of the fired sheet before the thermogravimetric analysis, and W 150 is the weight (g) of the fired sheet at 150 ° C., and W 600 is the weight (g) of the fired sheet at 600°C. <Thickness of fired sheet> Using a film thickness gauge (manufactured by Mitutoyo, product name "Digimatic Indicator ID-C112XBS"), the thickness of the fired sheet produced in the manufacturing example was measured at five points, approximately the center point and each of the four corners (squares), and the average value (μm) of the measured thicknesses was taken as the thickness of the fired sheet. <Density of fired sheet> The mass, area and thickness of the fired sheet produced in the manufacturing example were measured, and the mass was divided by the volume (= area x thickness) to determine the density of the fired sheet (g / cm 3 ) was calculated. <Thermal conductivity at high temperatures> Thermal diffusivity in the thickness direction α(m 2 / s), specific heat at constant pressure C p (J / g K), and specific gravity ρ (g / m 3 ) were measured by the following methods. [Thermal diffusivity in the thickness direction α] Measurements were performed using a thermal diffusivity / thermal conductivity measuring device (manufactured by Bethel Corporation, product name "Thermowave Analyzer TA35") while flowing nitrogen gas, and the thermal diffusivity in the thickness direction at 300°C under a nitrogen atmosphere was measured. [Constant pressure specific heat C p ] The specific heat was measured at 25° C. under a temperature increase rate of 10° C. / min using a differential scanning calorimeter (manufactured by Rigaku, product name "DSC8230"). [Specific gravity ρ (density)] The mass, area and thickness of the thermal conductive sheet were measured, and the mass was divided by the volume (= area x thickness) to determine the density of the thermal conductive sheet (g / cm 3 ) was calculated. Then, each measurement value is calculated using the following formula (2): λ=α×C p ×ρ (2) The thermal conductivity λ (W / m K) of the thermal conductive sheet in the thickness direction at 300°C was calculated by substituting the above formula into the formula. The thermal conductivity λ of the thermal conductive sheet in the thickness direction at 300°C is higher, so the thermal conductive sheet has better thermal conductivity at high temperatures. A: Thermal conductivity λ of the thermal conductive sheet in the thickness direction is 140 W / m K or more. B: Thermal conductivity λ in the thickness direction of the thermal conductive sheet is 130 W / m K or more and less than 140 W / m K C: Thermal conductivity λ in the thickness direction of the thermal conductive sheet is 120 W / m K or more and less than 130 W / m K. D: Thermal conductivity λ in the thickness direction of the thermal conductive sheet is less than 120 W / m K <Strength> The thermally conductive sheets prepared in the examples and comparative examples were cut to a size of 1 cm x 5 cm to prepare test pieces. A 6 cm x 6 cm x 2 cm pedestal was also prepared. The right half of the test piece was placed on the pedestal from the center, and the left half was placed so that it protruded from the pedestal. Furthermore, an aluminum plate of 6 cm x 6 cm x 2 mm was placed on the right half of the test piece. Then, under a temperature condition of 25°C, weights of 100 mg, 200 mg, and 300 mg were placed alternately on the part of the test piece protruding from the pedestal, and the strength of the thermally conductive sheet was evaluated according to the following criteria. A: The test piece did not break under the weight of 300 mg. B: The test specimen did not break with a weight of 200 mg, but broke with a weight of 300 mg. C: The test specimen did not break with a weight of 100 mg, but broke with a weight of 200 mg. D: The test piece broke under the weight of 100 mg.
[0088] Fired sheets 1 to 3 were produced according to the following Production Examples 1 to 3. The properties and production conditions of fired sheets 1 to 3 are shown in Table 1.
[0089] (Production Example 1) <Preparation of fired sheet 1> [Preparation of Composition] Resin A was a styrene-butadiene random copolymer that was solid at room temperature and normal pressure (manufactured by Zeon Corporation, product name "Nipol (registered trademark) 1502", specific gravity: 0.94 g / cm 3 100 parts of the carbon material A and 450 parts of expanded graphite (manufactured by Ito Graphite Industries Co., Ltd., product name "EC-50", volume average particle size: 250 μm, aspect ratio = 1.5) as particulate carbon material A were mixed and stirred for 20 minutes at a temperature of 150° C. using a pressure kneader (manufactured by Nippon Spindle Co., Ltd.). Next, the resulting mixture was placed in a crusher (manufactured by Osaka Chemical Co., Ltd., product name "Wonder Crush Mill D3V-10") and crushed for 10 seconds to obtain a composition. [Primary sheet forming process] Next, 500 g of the obtained composition was rolled (primary pressurization) into a sheet using a first roll and a second roll under the following conditions: a gap between the first roll and the second roll of 2 mm, a roll temperature of 25° C., a sheet discharge speed (circumferential speed of the first roll) of 2 m / min, and a peripheral speed ratio of the second roll to the first roll (second roll / first roll): 1.15 / 1. The rolling was repeated while keeping the sheet conveying direction the same. The rolling was performed 10 times in total to obtain a primary sheet with a thickness of 2 mm. The volume fraction of the particulate carbon material A in the obtained primary sheet was measured. The results are shown in Table 1. [Laminate formation process] Next, the obtained primary sheet was cut to a size of 150 mm length x 150 mm width x 0.8 mm thickness, and 188 sheets were stacked in the thickness direction of the primary sheet. Further, the sheets were pressed (secondary pressurization) in the stacking direction at a temperature of 120°C and a pressure of 0.1 MPa for 3 minutes to obtain a laminate with a height of approximately 150 mm. [Slicing process] The laminated side of the secondarily pressed laminate was then pressed with a pressure of 0.3 MPa and sliced at an angle of 0° to the lamination direction (in other words, in the normal direction to the main surface of the laminated primary sheets) using a wood slicer (manufactured by Marunaka Iron Works Co., Ltd., product name ``Super Finishing Planer Super Mecha S'') to obtain a secondary sheet measuring 150 mm in length x 150 mm in width x 0.30 mm in thickness. [Pre-firing process] Thereafter, the obtained secondary sheet was fired at 400° C. for 4 hours in a nitrogen atmosphere to obtain fired sheet 1 (thickness: 300 μm). The weight loss rate from 150° C. to 600° C., the orientation angle of the particulate carbon material A, the thickness and the density of the obtained fired sheet 1 were measured. The results are shown in Table 1.
[0090] (Production Example 2) <Preparation of fired sheet 2> Except for changing the amount of expanded graphite used from 450 parts to 290 parts, fired sheet 2 (thickness 300 μm) was produced in the same manner as in Production Example 1. Then, fired sheet 2 was subjected to various measurements in the same manner as in Production Example 1. The results are shown in Table 1.
[0091] (Production Example 3) <Preparation of fired sheet 3> Except for changing the amount of expanded graphite used from 450 parts to 170 parts, fired sheet 3 (thickness 300 μm) was produced in the same manner as in Production Example 1. Then, fired sheet 3 was subjected to various measurements in the same manner as in Production Example 1. The results are shown in Table 1.
[0092] Impregnation Solutions 1 to 5 were prepared according to the following Preparation Examples 1 to 5. The compositions of Impregnation Solutions 1 to 5 are shown in Table 2.
[0093] (Preparation Example 1) <Preparation of Impregnation Solution 1> Impregnation solution 1 was prepared by dissolving 10 parts of a styrene-butadiene random copolymer (manufactured by Nippon Zeon Co., Ltd., product name "Nipol 1502") that is solid at room temperature and normal pressure as resin B in 90 parts of cyclohexane as an organic solvent.
[0094] (Preparation Example 2) <Preparation of impregnation solution 2> Impregnation liquid 2 was prepared by dissolving or dispersing 1 part of a styrene-butadiene random copolymer (manufactured by Zeon Corporation, product name "Nipol 1502") that is solid at room temperature and normal pressure as resin B and 9 parts of expanded graphite (manufactured by Ito Graphite Industries Co., Ltd., product name "EC-1500", volume average particle size: 7 μm, aspect ratio = 1.5) as particulate carbon material B in 90 parts of cyclohexane as an organic solvent.
[0095] (Preparation Example 3) <Preparation of impregnation solution 3> Impregnation liquid 3 was prepared by dissolving or dispersing 5 parts of a styrene-butadiene random copolymer (manufactured by Zeon Corporation, product name "Nipol 1502") that is solid at room temperature and normal pressure as resin B and 5 parts of expanded graphite (manufactured by Ito Graphite Industries Co., Ltd., product name "EC-1500", volume average particle size: 7 μm, aspect ratio = 1.5) as particulate carbon material B in 90 parts of cyclohexane as an organic solvent.
[0096] (Preparation Example 4) <Preparation of Impregnation Solution 4> Impregnation solution 4 was prepared by dissolving 15 parts of a styrene-butadiene random copolymer (manufactured by Nippon Zeon Co., Ltd., product name "Nipol 1502") that is solid at room temperature and normal pressure as resin B in 85 parts of cyclohexane as an organic solvent.
[0097] (Preparation Example 5) <Preparation of Impregnation Solution 5> Impregnation liquid 5 was prepared by diluting styrene-butadiene latex (manufactured by Zeon Corporation, product name "Nipol 2507H") as resin B with water to a solids concentration of 10%.
[0098] Example 1 <Manufacture of thermal conductive sheets> [Impregnation process] 1200 ml of impregnation liquid 1 was placed in a beaker, and calcined sheet 1 was immersed therein. Next, the beaker was evacuated to allow calcined sheet 1 to be impregnated with impregnation liquid 1 for 1 minute to obtain an impregnated sheet. The vacuum conditions were appropriately adjusted so that air bubbles were generated on the surface of the calcined sheet, and cyclohexane did not boil. [Firing process] The obtained impregnated sheet was dried in an oven at 100°C, and then sintered at 400°C for 6 hours in a nitrogen atmosphere to obtain a thermally conductive sheet. The strength and thermal conductivity at high temperatures of this thermally conductive sheet were evaluated. The results are shown in Table 3.
[0099] Example 2 A thermally conductive sheet was produced in the same manner as in Example 1, except that the impregnation step and the firing step were carried out again on the thermally conductive sheet produced in Example 1. Then, evaluation was carried out in the same manner as in Example 1. The results are shown in Table 3.
[0100] Example 3 A thermally conductive sheet was produced in the same manner as in Example 1, except that the firing temperature in the firing step was changed from 400° C. to 1000° C. Then, evaluation was performed in the same manner as in Example 1. The results are shown in Table 3.
[0101] Example 4 A thermally conductive sheet was produced in the same manner as in Example 1, except that Impregnating Liquid 2 was used instead of Impregnating Liquid 1. Then, evaluation was performed in the same manner as in Example 1. The results are shown in Table 3.
[0102] Example 5 A thermally conductive sheet was produced in the same manner as in Example 1, except that Impregnating Liquid 3 was used instead of Impregnating Liquid 1. Then, evaluation was performed in the same manner as in Example 1. The results are shown in Table 3.
[0103] Example 6 A thermally conductive sheet was produced in the same manner as in Example 1, except that sintered sheet 2 was used instead of sintered sheet 1. Then, evaluation was performed in the same manner as in Example 1. The results are shown in Table 3.
[0104] Example 7 A thermally conductive sheet was produced in the same manner as in Example 1, except that sintered sheet 2 was used instead of sintered sheet 1 and impregnation liquid 2 was used instead of impregnation liquid 1. Then, evaluation was performed in the same manner as in Example 1. The results are shown in Table 4.
[0105] Example 8 A thermally conductive sheet was produced in the same manner as in Example 1, except that sintered sheet 2 was used instead of sintered sheet 1 and impregnation liquid 3 was used instead of impregnation liquid 1. Then, evaluation was performed in the same manner as in Example 1. The results are shown in Table 4.
[0106] Example 9 A thermally conductive sheet was produced in the same manner as in Example 1, except that Impregnating Liquid 4 was used instead of Impregnating Liquid 1. Then, evaluation was performed in the same manner as in Example 1. The results are shown in Table 4.
[0107] Example 10 A thermally conductive sheet was produced in the same manner as in Example 1, except that sintered sheet 3 was used instead of sintered sheet 1. Then, evaluation was performed in the same manner as in Example 1. The results are shown in Table 4.
[0108] Comparative Example 1 The impregnation step and the firing step were not carried out, and the fired sheet 1 was used as the thermal conductive sheet. Then, evaluation was carried out in the same manner as in Example 1. The results are shown in Table 4.
[0109] Comparative Example 2 A thermally conductive sheet was produced in the same manner as in Example 1, except that Impregnating Liquid 5 was used instead of Impregnating Liquid 1. Then, evaluation was performed in the same manner as in Example 1. The results are shown in Table 4.
[0110] Comparative Example 3 The impregnation step and the firing step were not carried out, and the fired sheet 2 was used as the thermal conductive sheet. Then, evaluation was carried out in the same manner as in Example 1. The results are shown in Table 4.
[0111] In addition, in Tables 1 to 4 shown below, "SBR" stands for styrene-butadiene random copolymer (solid at room temperature and pressure). "SBRL" stands for styrene-butadiene latex; "Orientation angle of particulate carbon material A" refers to the angle of the major axis direction of particulate carbon material A with respect to the surface of the fired sheet, "Weight reduction rate" refers to the weight reduction rate from 150°C to 600°C in a thermogravimetric curve obtained by subjecting a fired sheet to thermogravimetric analysis under specified conditions.
[0112] [Table 1]
[0113] [Table 2]
[0114] [Table 3]
[0115] [Table 4]
[0116] From Tables 1 to 4, it can be seen that in Examples 1 to 10, which used thermal conductive sheet manufacturing method 1 including predetermined steps (primary sheet molding step, laminate formation step, slicing step, pre-firing step, impregnation step and firing step), thermal conductive sheets with excellent strength and thermal conductivity at high temperatures can be manufactured. Furthermore, in Examples 1 to 9, which used the thermal conductive sheet manufacturing method 2 that includes specified steps (impregnation step and calcination step) and in which the orientation angle of the particulate carbon material A and the weight loss rate of the calcined sheet from 150°C to 600°C are each within a specified range, it can be seen that a thermal conductive sheet with excellent strength and thermal conductivity at high temperatures can be manufactured. On the other hand, in Comparative Examples 1 and 3, which used manufacturing methods for thermally conductive sheets that did not include the specified impregnation and firing steps, and in Comparative Example 2, which used an impregnation liquid that did not include an organic solvent in the impregnation step, it was found that a thermally conductive sheet having excellent strength and thermal conductivity at high temperatures could not be manufactured. [Industrial Applicability]
[0117] According to the present invention, it is possible to provide a method for producing a thermally conductive sheet having excellent strength and thermal conductivity at high temperatures.
Claims
1. a primary sheet forming step of pressurizing a composition containing a resin A and a particulate carbon material A into a sheet to obtain a primary sheet; a laminate forming step of laminating a plurality of the primary sheets in the thickness direction or folding or rolling the primary sheets to obtain a laminate; a slicing step of slicing the laminate at an angle of 45° or less with respect to the lamination direction to obtain a secondary sheet; a pre-firing step of firing the secondary sheet to obtain a fired sheet; an impregnation step of impregnating the fired sheet with an impregnation liquid containing an organic solvent and a resin B to obtain an impregnated sheet; a firing step of firing the impregnated sheet to obtain a thermally conductive sheet; A method for manufacturing a thermally conductive sheet, comprising:
2. an impregnation step of impregnating the fired sheet with an impregnation liquid containing an organic solvent and resin B to obtain an impregnated sheet; a firing step of firing the impregnated sheet to obtain a thermally conductive sheet; A method for manufacturing a thermally conductive sheet, comprising: The fired sheet contains particulate carbon material A, the angle of the major axis direction of the particulate carbon material A with respect to the surface of the fired sheet is 60° or more and 90° or less; The fired sheet is subjected to the following conditions: Temperature increase rate: 10°C / min Measurement temperature range: 30°C to 1000°C In the atmosphere In a thermogravimetric curve obtained by performing thermogravimetric analysis, the weight loss rate (%) from 150°C to 600°C is 3% or more and 20% or less, with the weight of the fired sheet before the thermogravimetric analysis measurement being 100%.
3. The method for producing a thermal conductive sheet according to claim 1 or 2, wherein the impregnation step and the firing step are repeated multiple times.
4. The method for producing a thermally conductive sheet according to claim 1 or 2, wherein the impregnation liquid further contains particulate carbon material B.
5. The method for producing a thermal conductive sheet according to claim 4 , wherein the total content of the resin B and the particulate carbon material B in the impregnation liquid is 15 mass % or less.
6. The method for producing a thermal conductive sheet according to claim 1 or 2, wherein the resin B has a cyclic structure.
7. 3. The method for producing a thermal conductive sheet according to claim 1, wherein the organic solvent comprises at least one selected from the group consisting of hexane, cyclohexane, toluene, methyl ethyl ketone, and ethyl acetate.
Citation Information