Depolymerization method of liquid crystalline resin

A depolymerization method using methanol under pressure and temperature recovers structural units from aromatic polyesters and polyesteramides, addressing the inefficiencies in existing recycling methods and enhancing the recovery of aromatic hydroxycarboxylic acid units in liquid crystal resins.

JP2024142138APending Publication Date: 2024-10-10POLYPLASTICS CO LTD +1

Patent Information

Application Number
JP2023054163
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for recycling wholly aromatic polyesters and polyesteramides do not effectively recover structural units derived from aromatic hydroxycarboxylic acids, limiting the efficient recycling of liquid crystal resins.

Method used

A depolymerization method involving the reaction of liquid crystal resins, which are aromatic polyesters or polyesteramides, with methanol under pressure and specific temperature conditions to recover structural units as methyl esters of aromatic hydroxycarboxylic acids.

Benefits of technology

The method achieves a sufficient recovery rate of structural units derived from aromatic hydroxycarboxylic acids, facilitating effective recycling of liquid crystal resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142138000001
    Figure 2024142138000001
  • Figure 2024142138000002
    Figure 2024142138000002
  • Figure 2024142138000003
    Figure 2024142138000003
Patent Text Reader

Abstract

To provide a depolymerization method of a liquid crystalline resin, in which a monomer derived from a structural unit of a liquid crystalline resin having the structural unit, as a constituent, derived from an aromatic hydroxycarboxylic acid, can be collected at a sufficient collection rate.SOLUTION: A depolymerization method of a liquid crystalline resin includes: a step A of mixing a liquid crystalline resin with a methanol; and a step B of pressuring the methanol, reacting the liquid crystalline resin with the methanol at a reaction temperature of 240-285°C, and depolymerizing the liquid crystalline resin. The liquid crystalline resin is an aromatic polyester or aromatic polyesteramide having a structural unit, as a constituent, derived from an aromatic hydroxycarboxylic acid.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for depolymerizing a liquid crystalline resin. [Background technology]

[0002] Liquid crystal resins have a good balance of excellent fluidity, mechanical strength, heat resistance, chemical resistance, electrical properties, etc., and are therefore widely used as high-performance engineering plastics. On the other hand, from the viewpoint of effective use of resources for protecting the global environment, effective recycling of engineering plastics is required. Known recycling methods include, for example, chemical recycling, material recycling, and thermal recycling (see Patent Document 1).

[0003] Patent Document 1 proposes a method for recycling wholly aromatic polyesters, in which wholly aromatic polyesters are depolymerized under pressure in an aliphatic monohydric alcohol at a temperature of 150°C or higher to recover aromatic dicarboxylic acid diesters and aromatic dihydroxy compounds, comprising: (1) a first step of depolymerizing a wholly aromatic polyester resin in an aliphatic monohydric alcohol under pressure at a temperature of 150°C or higher; (2) a second step of crystallizing and separating an aromatic dicarboxylic acid diester from the reaction mixture obtained in the first step; (3) a third step of distilling off an aliphatic monohydric alcohol from the mother liquor remaining in the second step; and (4) a fourth step of crystallizing the high-boiling point mixture remaining in the third step using a solvent having a solubility parameter (δs) of 10.5 or lower to separate the aromatic dihydroxy compound. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-147121 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the method for recycling wholly aromatic polyesters described in Patent Document 1, the wholly aromatic polyesters to be treated are those derived from aromatic dicarboxylic acids and aromatic dihydroxy compounds as monomers, and there is no description of aromatic polyesters or aromatic polyesteramides having structural units derived from aromatic hydroxycarboxylic acids as constituent components.

[0006] The present invention has been made in consideration of the above-mentioned problems in the conventional art, and an object of the present invention is to provide a method for depolymerizing a liquid crystalline resin, which is capable of recovering the structural unit monomer of a liquid crystalline resin having a structural unit derived from an aromatic hydroxycarboxylic acid as a constituent component at a sufficient recovery rate. [Means for solving the problem]

[0007] As a result of intensive research to solve the above problems, the inventors investigated the reaction conditions of methanol with a liquid crystalline resin and found that it is possible to recover monomers with a good recovery rate within a specified temperature range under pressurized conditions, thereby completing the present invention.

[0008] One aspect of the present invention that solves the above problems is as follows. (1) Step A of mixing a liquid crystal resin and methanol; and step B of reacting the liquid crystalline resin with the methanol under pressure at a reaction temperature of 240 to 285° C. to depolymerize the liquid crystalline resin, The method for depolymerizing a liquid crystalline resin, wherein the liquid crystalline resin is an aromatic polyester or an aromatic polyester amide having, as a constituent, a structural unit derived from an aromatic hydroxycarboxylic acid.

[0009] (2) The method for depolymerizing a liquid crystalline resin according to (1) above, wherein in the step B, a pressurized state of 2.0 to 30.0 MPa is applied.

[0010] (3) The method for depolymerizing a liquid crystalline resin according to (1) or (2) above, wherein in the step B, the reaction temperature is 245 to 265° C.

[0011] (4) The method for depolymerizing a liquid crystalline resin according to any one of (1) to (3) above, wherein the aromatic hydroxycarboxylic acid includes 6-hydroxy-2-naphthoic acid. Effect of the Invention

[0012] According to the present invention, there can be provided a method for depolymerizing a liquid crystalline resin, which is capable of recovering the structural unit monomer of a liquid crystalline resin having a structural unit derived from an aromatic hydroxycarboxylic acid as a constituent component at a sufficient recovery rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The method for depolymerizing a liquid crystalline resin according to the present embodiment includes step A of mixing a liquid crystalline resin with methanol, and step B of depolymerizing the liquid crystalline resin by reacting the liquid crystalline resin with methanol under pressurized conditions and at a reaction temperature of 240 to 285° C. The liquid crystalline resin is an aromatic polyester or aromatic polyesteramide having, as a constituent, a structural unit derived from an aromatic hydroxycarboxylic acid.

[0014] In the method for depolymerizing a liquid crystal resin according to the present embodiment, the liquid crystal resin to be depolymerized is an aromatic polyester or aromatic polyesteramide having a structural unit derived from an aromatic hydroxycarboxylic acid as a constituent. In step A, the liquid crystal resin is mixed with methanol. In step B, the liquid crystal resin is reacted with methanol under pressure at a reaction temperature of 240 to 285° C. to depolymerize the liquid crystal resin. By such steps A and B, the monomer component can be recovered at a sufficient recovery rate. The main component recovered by the depolymerization method of the present embodiment is a methyl ester of an aromatic hydroxycarboxylic acid or a derivative thereof. Therefore, the recovered component cannot strictly be called a monomer constituting a liquid crystal resin. However, since the aromatic hydroxycarboxylic acid is not decomposed into another compound but is recovered while maintaining its structure, the recovered component is called a monomer constituting a liquid crystal resin for convenience. Each step of the method for depolymerizing a liquid crystalline resin according to this embodiment will be described in detail below.

[0015] [Step A] In step A, the liquid crystal resin is mixed with methanol. In this embodiment, the liquid crystal resin to be depolymerized is, as described above, an aromatic polyester or an aromatic polyesteramide having a structural unit derived from an aromatic hydroxycarboxylic acid as a constituent component. The wholly aromatic polyester contains at least a structural unit derived from an aromatic hydroxycarboxylic acid, and examples thereof include the following (1) and (2). (1) Polyesters consisting essentially of one or more aromatic hydroxycarboxylic acids and their derivatives. (2) A polyester mainly composed of (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids and their derivatives, and (c) at least one or more aromatic diols, alicyclic diols, aliphatic diols and their derivatives.

[0016] Examples of aromatic hydroxycarboxylic acids include p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, m-hydroxybenzoic acid, 6-hydroxy-3-naphthoic acid, 6-hydroxy-4-naphthoic acid, 4-hydroxy-4'-carboxydiphenyl ether, 2,6-dichloro-p-hydroxybenzoic acid, 2-chloro-p-hydroxybenzoic acid, 2,6-dimethyl-p-hydroxybenzoic acid, 2,6-difluoro-p-hydroxybenzoic acid, 4-hydroxy-4'-biphenylcarboxylic acid, and vanillic acid. In the present embodiment, the structural unit derived from an aromatic hydroxycarboxylic acid is preferably a structural unit derived from p-hydroxybenzoic acid or 6-hydroxy-2-naphthoic acid. In particular, since 6-hydroxy-2-naphthoic acid is expensive, it would be useful if it could be recovered as methyl 6-hydroxy-2-naphthoate and recycled.

[0017] The aromatic dicarboxylic acid is not particularly limited, and examples thereof include terephthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and compounds represented by the following general formula (I).

[0018] [ka] (Y:-(CH 2 ) n -(n=1 to 4) and -O(CH 2 ) n O-(n=1 to 4).

[0019] The alicyclic dicarboxylic acid is not particularly limited, and examples thereof include 1,4-cyclohexanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.

[0020] The aromatic diol is not particularly limited, and examples thereof include 2,6-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl, hydroquinone, resorcinol, a compound represented by the following general formula (II), and a compound represented by the following general formula (III).

[0021] [ka] (X: alkylene (C 1 ~C 4), alkylidene, -O-, -SO-, -SO 2 is a group selected from -, -S-, and -CO-.

[0022] [ka]

[0023] The alicyclic diol is not particularly limited, and examples thereof include 1,4-cyclohexanedimethanol, 1,4-cyclohexanediol, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.

[0024] On the other hand, the wholly aromatic polyesteramide contains at least a structural unit derived from an aromatic hydroxycarboxylic acid, and examples thereof include the following (1) and (2). (1) A polyesteramide consisting essentially of (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (c1) one or more aromatic hydroxyamines, aromatic diamines, and their derivatives, and (c2) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives. (2) Polyesteramides mainly composed of (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives, (c1) one or more aromatic hydroxyamines, aromatic diamines, and their derivatives, and (c2) one or more aromatic diols, alicyclic diols, and their derivatives.

[0025] The same explanation as given above regarding the wholly aromatic polyester applies to the aromatic dicarboxylic acid, the alicyclic dicarboxylic acid, the aromatic diol, and the alicyclic diol.

[0026] The aromatic hydroxyamine is not particularly limited, and examples thereof include p-aminophenol, m-aminophenol, etc. The alicyclic hydroxyamine is not particularly limited, and examples thereof include 4-hydroxycyclohexanecarboxylic acid, 3-hydroxycyclopentanecarboxylic acid, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.

[0027] Examples of aromatic diamines include p-phenylenediamine, etc. Examples of alicyclic diamines include, but are not limited to, 1,4-cyclohexanediamine, 1,3-cyclopentanediamine, etc. Examples of polymerizable derivatives include, but are not limited to, alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.

[0028] In the method for depolymerizing a liquid crystalline resin according to the present embodiment, the liquid crystalline resin as described above is depolymerized mainly into a methyl ester of an aromatic hydroxycarboxylic acid.

[0029] The liquid crystal resin may also contain various known additives, such as various stabilizers, lubricants, nucleating agents, surfactants, colorants, polymer modifiers, different polymers, and inorganic or organic fibrous, powdery, or plate-like fillers, of which one or more may be blended.

[0030] In step A, examples of the liquid crystalline resin to be depolymerized and mixed with methanol include used liquid crystalline resin products, unused liquid crystalline resin pellets, resin waste generated in the manufacturing process of liquid crystalline resin pellets and liquid crystalline resin products, etc. Such liquid crystalline resin is preferably cut or crushed as necessary when mixed with methanol.

[0031] In step A, when mixing the liquid crystal resin and methanol, it is preferable to mix them so that the mass ratio of methanol to the liquid crystal resin is 0.1 to 100. If the mass ratio is less than 0.1, the recovery rate of the monomer may not be increased, and even if it exceeds 100, no further effect is expected and the amount becomes excessive. The mass ratio is more preferably 0.5 to 50, and further preferably 1 to 25.

[0032] In step A, the liquid crystal resin and methanol are mixed by any method. For example, a method of filling a mixing vessel with the liquid crystal resin and then adding methanol and mixing, a method of filling a mixing vessel with methanol and then adding the liquid crystal resin and mixing, a method of continuously joining the liquid crystal resins in a pipe and then mixing them in a vessel, etc. are included. In addition, in mixing the above components, the mixing temperature and mixing time are not particularly limited.

[0033] After the above step A is completed, that is, after the liquid crystalline resin and methanol are mixed, the process proceeds to step B. Step A and step B may be performed consecutively, or there may be any time between the completion of step A and the start of step B. The mixing vessel used in step A and the reaction vessel used in step B may be the same or different. However, from the viewpoint of being able to proceed to step B in the same state after the completion of step A, it is preferable that the vessels used in steps A and B are the same.

[0034] [Step B] In step B, the methanol is pressurized and the reaction temperature is set to 240 to 285° C., and the liquid crystalline resin is reacted with methanol to depolymerize the liquid crystalline resin.

[0035] Here, in step B, the liquid crystal resin is reacted with methanol at a reaction temperature of 240 to 285°C while keeping the methanol pressurized. If the temperature is less than 240°C or exceeds 285°C, the recovery rate of the monomer becomes insufficient. The reaction temperature in step B is preferably 245 to 265°C, more preferably 250 to 260°C. As long as the methanol is pressurized, the pressure is not particularly limited and can be set appropriately, but is preferably 2.0 to 30.0 MPa, more preferably 5.0 to 30.0 MPa, and even more preferably 5.0 to 25.0 MPa.

[0036] In step B, a reaction vessel having resistance to high temperatures and high pressures is used in order to set the reaction temperature and pressure so that methanol is in a pressurized state, and the shape and volume of the reaction vessel are arbitrary. In addition, the heat source for keeping the temperature within the above range is preferably one capable of controlling the temperature, and examples of the heat medium used in liquid form, a salt bath, a fluidized bed sand bath, a metal bath, a heater, an oven, microwave heating, etc.

[0037] In the method for depolymerizing a liquid crystalline resin of the present embodiment, the reaction time between the liquid crystalline resin and methanol is preferably 5 to 300 minutes, more preferably 10 to 240 minutes, and even more preferably 40 to 180 minutes. Then, the methyl ester of aromatic hydroxycarboxylic acid, which is a liquid crystalline monomer component to be depolymerized, is recovered at a high recovery rate.

[0038] The reaction in step B may be carried out with or without stirring.

[0039] In the method for depolymerizing a liquid crystalline resin according to the present embodiment, the depolymerization of the liquid crystalline resin may be carried out in a batch manner or a continuous manner.

[0040] Furthermore, in the method for depolymerizing a liquid crystal resin according to the present embodiment, the depolymerization can be carried out in the presence of an alkaline additive in order to promote the depolymerization. Examples of the alkaline additive include compounds such as hydroxides, carbonates, hydrogencarbonates, and carboxylates of alkali metals and alkaline earth metals, and amines, and one or more of these can be used. EXAMPLES

[0041] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to the following examples.

[0042] [Examples 1 to 8, Comparative Examples 1 to 6] As the liquid crystalline resin to be depolymerized, 0.2 g of a liquid crystalline resin (aromatic polyester) containing 73 mol % of structural units derived from p-hydroxybenzoic acid and 27 mol % of structural units derived from 6-hydroxy-2-naphthoic acid was prepared, and the following operation was carried out. In each of the Examples and Comparative Examples, a liquid crystalline resin and methanol were mixed in the ratio shown in Table 1, and the mixture was placed in a tubular reaction vessel made of SUS316 (volume: 8.8 cm 3 The tube-type reaction vessel was then placed in a salt bath (KNO 3 , NaNO 2 ) and heated at the temperatures shown in Tables 1 and 2. After the reaction times shown in Tables 1 and 2 had elapsed, the reaction was stopped by quenching. After the reaction was stopped, the decomposition products were recovered with methanol and subjected to suction filtration to separate into a filtrate and a residue. The filtrate of the decomposition products was then analyzed by liquid chromatography to measure the amounts of methyl p-hydroxybenzoate and methyl 6-hydroxy-2-naphthoate, and the recovery rate of each monomer was calculated. In addition, the filtration residue of the decomposition products was dried and then mass measured to calculate the decomposition rate of the liquid crystalline resin. The calculation of each monomer recovery rate and the decomposition rate of the liquid crystalline resin was based on the following formula.

[0043]

number

[0044]

number

[0045]

number

[0046] [Table 1]

[0047] [Table 2]

[0048] From Tables 1 and 2, it can be seen that in all of Examples 1 to 8, the yield of methyl p-hydroxybenzoate and the recovery rate of methyl 6-hydroxy-2-naphthoate are higher than those in Comparative Examples 1 to 6. That is, it can be seen that the method for depolymerizing a liquid crystalline resin according to the present embodiment makes it possible to recover aromatic hydroxycarboxylic acid in the state of methyl ester at a sufficient recovery rate.

Claims

1. Step A of mixing a liquid crystal resin and methanol; and step B of reacting the liquid crystalline resin with the methanol under pressure at a reaction temperature of 240 to 285° C. to depolymerize the liquid crystalline resin, The method for depolymerizing a liquid crystalline resin, wherein the liquid crystalline resin is an aromatic polyester or an aromatic polyester amide having, as a constituent, a structural unit derived from an aromatic hydroxycarboxylic acid.

2. 2. The method for depolymerizing a liquid crystalline resin according to claim 1, wherein in the step B, a pressurized state of 2.0 to 30.0 MPa is applied.

3. 3. The method for depolymerizing a liquid crystalline resin according to claim 1, wherein the reaction temperature in step B is 245 to 265° C.

4. 3. The method for depolymerizing a liquid crystalline resin according to claim 1, wherein the aromatic hydroxycarboxylic acid includes 6-hydroxy-2-naphthoic acid.

Citation Information

Patent Citations

  • Method for chemically recycling all aromatic polyester

    JP2003147121A

Cited By

  • Method for producing liquid crystal polyester depolymerized product, method for producing recycled liquid crystal polyester resin, method for producing recycled liquid crystal polyester molded article, and chemical recycling method

    WO2026058869A1

  • Method for producing liquid crystal polyester depolymerized product, method for producing recycled liquid crystal polyester resin, method for producing recycled liquid crystal polyester molded body, and chemical recycling method

    WO2026058870A1