Organopolysiloxane

A novel organopolysiloxane with specific structural formulas addresses the issue of maintaining fluidity and solubility in phenyl-modified silicones, enhancing filler dispersibility and reducing viscosity in heat dissipation materials.

JP2024142155AActive Publication Date: 2024-10-10SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
JP2023054188
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Existing heat dissipation materials face challenges in maintaining fluidity and solubility when highly filled with thermally conductive fillers, particularly in phenyl-modified silicones, leading to increased viscosity and poor workability.

Method used

Development of a novel organopolysiloxane with specific structural formulas that act as a wetter, enhancing the dispersibility of thermally conductive fillers in phenyl-modified silicones, thereby maintaining fluidity and suppressing viscosity increases.

Benefits of technology

The organopolysiloxane ensures high filler dispersibility and low viscosity in phenyl-modified silicone compositions, enabling efficient heat dissipation with improved workability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142155000027
    Figure 2024142155000027
  • Figure 2024142155000001
    Figure 2024142155000001
  • Figure 2024142155000002
    Figure 2024142155000002
Patent Text Reader

Abstract

To provide novel organopolysiloxane acting as a wetter to allow phenyl modified silicone to be highly filled with a high thermal conductive filler.SOLUTION: The present invention provides organopolysiloxane represented by a general formula (1). (In the formula, each R1 independently represents a C6-10 monovalent aromatic hydrocarbon group, each R2 independently represents a C1-10 alkyl group, R3 represents a C1-4 alkyl group, a is 2 or 3, m is an integer satisfying 1≤m≤30, and n is an integer satisfying 0≤n≤60, provided that the range 3≤m+n≤90 is satisfied. Boding of each siloxane unit in brackets in the general formula (1) may be a block or random.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to organopolysiloxanes. [Background technology]

[0002] The performance of electronic components such as highly integrated circuits, such as CPUs, is significantly reduced due to heat generation during use. To solve this problem, heat dissipation materials are used that improve heat transfer efficiency when introduced into the air space between the heat generating part and the cooling part. Among them, silicone heat dissipation materials are used in a wide range of fields because of their high heat resistance, weather resistance, and electrical insulation properties derived from silicone. Moreover, in recent years, electronic devices have become smaller and more highly integrated, making it important to more efficiently cool the heat they generate, and so there is a demand for heat dissipation materials with high thermal conductivity.

[0003] The thermal conductivity of materials containing silicone oil and thermally conductive filler is affected by the thermal conductivity of the thermally conductive filler itself when the volume fraction of the thermally conductive filler exceeds 0.6. Therefore, in order to increase the thermal conductivity of heat dissipation materials, it is important to increase the loading of the thermally conductive filler. However, simply increasing the loading significantly reduces the fluidity of the conductive grease, making it difficult to process. To solve this problem, a method has been proposed in which the thermally conductive filler is surface-treated with a silane coupling agent (wetter) to disperse it in the silicone base oil and maintain the fluidity of the thermally conductive grease.

[0004] Phenyl-modified silicone, which has a structure in which a portion of methyl silicone has been replaced with a phenyl group, has better heat resistance, cold resistance, and oxidation resistance than methyl silicone. Furthermore, because it has high gas barrier properties and a high refractive index, phenyl-modified silicone is used in cosmetics and sealing materials for light-emitting diodes (Patent Documents 1 and 2). Therefore, it is believed that by using phenyl-modified silicone as a base oil and applying it to heat dissipation materials, properties that cannot be achieved with methyl silicone can be realized. On the other hand, the introduction of phenyl groups makes the silicone skeleton rigid, so there is a problem that the viscosity increases significantly, especially in high-phenyl-modified silicone (Patent Document 3).

[0005] Therefore, when phenyl-modified silicone is used as a base oil and a thermally conductive filler is added to make a grease, the fluidity of the thermally conductive grease is significantly deteriorated. In addition, organopolysiloxanes having trialkoxysilyl groups, which are often used as wetters, have poor solubility in phenyl-modified silicones (Patent Documents 4 and 5). Therefore, there has been a demand for the development of a wetter that is highly soluble in phenyl-modified silicones and suppresses viscosity increases when filled with a thermally conductive filler. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2004-162039 A [Patent Document 2] JP 2007-039621 A [Patent Document 3] JP 2004-262919 A [Patent Document 4] JP 2004-262972 A [Patent Document 5] JP 2005-162975 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a novel organopolysiloxane that acts as a wetter that allows resin materials, particularly phenyl-modified silicones, to be highly loaded with a highly thermally conductive filler. [Means for solving the problem]

[0008] In order to achieve the above object, the present invention provides the following novel organopolysiloxane.

[0009] That is, the present invention relates to a compound represented by the following general formula (1): [ka] (In the formula, R 1 are independently a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms, and R 2 are independently an alkyl group having 1 to 10 carbon atoms; R 3 is an alkyl group having 1 to 4 carbon atoms; a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The bonds of the siloxane units enclosed in parentheses in the general formula (1) may be block or random. The present invention provides an organopolysiloxane characterized by being represented by the following formula:

[0010] Such organopolysiloxanes are suitable as wetters, and for example, phenyl-modified silicones can be highly loaded with highly thermally conductive fillers.

[0011] The organopolysiloxane is preferably represented by the following general formula (2). [ka] (In the formula, R 1 , R 2 , R 3and a are the same as above, x is an integer of 1≦x≦30, m' is an integer of 1≦m'≦3, and n' is an integer of 0≦n'≦2, provided that m'+n' is 3. The bond of the siloxane units enclosed in parentheses with m' and n' may be block or random, and the bond of two types of siloxane units enclosed in parentheses with x is a block polymer.

[0012] Such organopolysiloxanes have high solubility in phenyl-modified silicones.

[0013] R shown in the above general formula (1) and general formula (2) 1 is a phenyl group, and R 2 is preferably a methyl group. From the viewpoint of the synthesis of organopolysiloxane, these groups are preferred.

[0014] The present invention provides a wetter comprising the organopolysiloxane described above. By using the above-described organopolysiloxane as a wetter, the thermally conductive filler can be more effectively dispersed in the phenyl-modified silicone. Effect of the Invention

[0015] The organopolysiloxane of the present invention is useful as a silane coupling agent (wetter) that improves the dispersibility of thermally conductive filler in phenyl-modified silicone.Therefore, the phenyl-modified silicone composition containing the organopolysiloxane of the present invention has a suppressed viscosity and maintains fluidity even when it contains a large amount of thermally conductive filler.Therefore, when the organopolysiloxane of the present invention is introduced into a silicone composition, it is possible to obtain a thermally conductive silicone composition that suppresses viscosity increase even when the thermally conductive filler is highly filled. [Brief description of the drawings]

[0016] [Figure 1]2 is a 29Si-NMR chart of the organopolysiloxane synthesized in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present inventors have searched for organopolysiloxanes suitable for wetters that enable resin materials, particularly phenyl-modified silicones, to be highly loaded with highly thermally conductive fillers, and have found that the one represented by the following general formula (1) is useful for this purpose, thus completing the present invention. That is, the present invention relates to a compound represented by the following general formula (1): [ka] (In the formula, R 1 are independently a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms, and R 2 are independently an alkyl group having 1 to 10 carbon atoms; R 3 is an alkyl group having 1 to 4 carbon atoms; a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The bonds of the siloxane units enclosed in parentheses in the general formula (1) may be block or random. The organopolysiloxane is characterized by being represented by the following formula: In particular, the organopolysiloxane is represented by the following general formula (2): [ka] (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer of 1≦x≦30, m' is an integer of 1≦m'≦3, and n' is an integer of 0≦n'≦2, provided that m'+n' is 3. The bond of the siloxane units enclosed in parentheses with m' and n' may be block or random, and the bond of two types of siloxane units enclosed in parentheses with x is a block polymer. It is preferable that the organopolysiloxane is an organopolysiloxane represented by the following formula:

[0018] The present invention will be described in detail below.

[0019] In the above general formula (1), R 1 R is independently a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms. 1 Specific examples of include aryl groups such as a phenyl group, a tolyl group, a xylyl group, and a mesityl group, and among these, a phenyl group is preferred from the viewpoint of ease of synthesis.

[0020] In the above general formula (1), R 2 R is independently an alkyl group having 1 to 10 carbon atoms, preferably 1 to 5 carbon atoms, and more preferably 1 to 3 carbon atoms. 2 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a tert-butyl group, a pentyl group, a hexyl group, an octyl group, a nonyl group, and a decyl group. Among these, a methyl group or an ethyl group is preferred from the viewpoint of ease of synthesis.

[0021] In the above general formula (1), R 3 R is independently an alkyl group having 1 to 4 carbon atoms, and is preferably a methyl group or an ethyl group. 3 Examples of a include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, and a tert-butyl group. Among them, from the viewpoint of the hydrolysis property of the organopolysiloxane compound of the present invention, a methyl group and an ethyl group are particularly preferable. In addition, in the above general formula (1), a is 2 or 3, but from the viewpoint of ease of synthesis and economic efficiency, a is preferably 3.

[0022] In the above general formula (1), m is usually an integer of 1≦m≦30, preferably 3≦m≦20, and more preferably 5≦m≦18. If m exceeds 30, the viscosity of the organopolysiloxane increases significantly, which is not preferred. In addition, in the above general formula (1), n ​​is usually an integer of 0≦n≦60, preferably 5≦n≦50, and more preferably 10≦n≦40. If it is outside the above range, the compatibility with the phenyl-modified silicone decreases, which is not preferred. Also, m+n is 3≦m+n≦90, and preferably 6≦m+n≦60. If it is outside the above range, the product becomes difficult to handle during synthesis of the compound, which is not preferred. Furthermore, the bonds of the siloxane units enclosed in parentheses in the general formula (1) may be in blocks or random.

[0023] Specific examples of organopolysiloxanes represented by the above general formula (1) include, but are not limited to, the following compounds: In the formulas shown below, "Me" represents a methyl group and "Ph" represents a phenyl group. [ka]

[0024] The organopolysiloxane represented by the above general formula (1) is synthesized, for example, according to the following reaction formula.

[0025] Reaction scheme: [ka]

[0026] In the formula, m and n are 29 Identified by Si-NMR.

[0027] Silanol and 1,1-diphenyl-3,3,5,5-tetramethyltrisiloxane (hereinafter sometimes referred to as phenyl-modified cyclic siloxane) are heated and stirred in acetonitrile solvent in the presence of bis(1,2-benzenedioleate)phenylsilicate sodium salt (NAS, above formula) catalyst, and 2-(trimethoxysilyl)ethyl propionate (ECMS, above formula) is allowed to act as a reaction terminator to synthesize an organopolysiloxane compound as shown in the above general formula (1). The solvent for this reaction is preferably a polar solvent such as acetonitrile (MeCN) or N,N-dimethylformamide (DMF). The reaction temperature is usually 60 to 65°C, and the reaction time is about 2 hours for each step.

[0028] By varying the equivalent weight of the phenyl-modified cyclic siloxane relative to the silanol, the length of the main chain (m+n) of the organopolysiloxane compound, that is, the degree of polymerization, can be adjusted.

[0029] The resulting organopolysiloxane exhibits high solubility in phenyl-modified silicone.

[0030] The phenyl-modified silicone composition of the present invention that contains the organopolysiloxane can be highly loaded with thermally conductive fillers while maintaining their dispersibility, and therefore can be suitably used as a wetter. EXAMPLES

[0031] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the following examples, the kinematic viscosity is a value measured at 25°C using a Canon-Fenske viscometer according to JIS Z8803::2011. The refractive index is a value measured at 25°C using an Abbe refractometer according to JIS K0062:1992. D In the following formula, Me represents a methyl group and Ph represents a phenyl group.

[0032] [Example 1] A 300 mL round separable flask was fitted with a stirrer, thermometer and coiled cooling tube through a four-neck separable cover. Trimethylsilanol (9.0 g, 0.1 mol), phenyl-modified cyclic siloxane (103.8 g, 0.3 mol) and acetonitrile (60.8 g) were added to this separable flask and heated with stirring at 65°C to dissolve the phenyl-modified cyclic siloxane. After the phenyl-modified cyclic siloxane was completely dissolved, NAS (61 mg, 0.0178 mmol) was added and the reaction solution was heated and stirred at 65°C for 2 hours. The progress of the reaction was 1 After tracking with H-NMR spectrum and confirming that the signal of phenyl-modified cyclic siloxane disappeared, the reaction terminator ECMS (29.1 g, 0.13 mol) was added and the mixture was heated and stirred at 65°C for another 2 hours. After confirming by infrared spectroscopy that the peak corresponding to silanol had disappeared, methanol was added to the reaction solution and the mixture was heated and stirred at 65°C for another 1 hour. The reaction solution was returned to room temperature, washed with methanol, and the oil layer was extracted. The solvent and low molecular weight siloxane contained in the obtained oil layer were removed under reduced pressure to obtain an organopolysiloxane compound. This compound was a colorless, transparent liquid with a kinetic viscosity of 314 mm 2 ·s ―1 The refractive index was 1.505. 29 Si-NMR spectrum analysis revealed that it had the following structure (the NMR chart is shown in FIG. 1). 29 Si-NMR spectrum (99.37MHz, CDCl3, 25℃): δ = 7.9 (SiMe3), -17.8 to -21.1 (SiMe2), -46.7 to -47.8 (SiPh2), -84.7 to -85.0 (Si(OMe)3) [ka]

[0033] [Example 2] An organopolysiloxane compound was obtained in the same manner as above, except that 5 equivalents of phenyl-modified cyclic siloxane were used relative to trimethylsilanol. This compound was a colorless, transparent liquid with a kinetic viscosity of 552 mmHg. 2 ·s-1 The refractive index was 1.509. 29 Si-NMR spectroscopic analysis showed that it had the following structure: [ka] 29 Si-NMR spectrum (99.37 MHz, CDCl3, 25°C): δ = 7.9 (SiMe3), -17.8 to -21.3 (SiMe2), -46.7 to -47.7 (SiPh2), -84.7 to -85.0 (Si(OMe)3).

[0034] [Example 3] An organopolysiloxane compound was obtained in the same manner as above, except that 10 equivalents of phenyl-modified cyclic siloxane were used relative to trimethylsilanol. This compound was a colorless, transparent liquid with a kinetic viscosity of 1255 mm. 2 ·s -1 The refractive index was 1.512. 29 Si-NMR spectroscopic analysis showed that it had the following structure: [ka] 29 Si-NMR spectrum (99.37 MHz, CDCl3, 25°C): δ = 7.9 (SiMe3), -17.8 to -21.3 (SiMe2), -46.7 to -47.7 (SiPh2), -84.7 to -85.0 (Si(OMe)3).

[0035] [Example 4] An organopolysiloxane compound was obtained in the same manner as above, except that 15 equivalents of phenyl-modified cyclic siloxane were used relative to trimethylsilanol. This compound was a colorless, transparent liquid with a kinetic viscosity of 2158 mm. 2 ·s -1 The refractive index was 1.515. 29 Si-NMR spectroscopic analysis showed that it had the following structure: [ka] 29 Si-NMR spectrum (99.37MHz, CDCl3, 25℃): δ = 7.9 (SiMe3), -17.6 to -21.3 (SiMe2), -47.0 to -48.0 (SiPh2), -84.7~-85.0(Si(OMe)3).

[0036] [Compatibility test] When the following organosiloxane (B-6) is dispersed in phenyl-modified silicone at 25%, clouding and layer separation occurs. On the other hand, when the above novel organosiloxane is dispersed under the same conditions, clouding and layer separation do not occur, so it can be said that the above novel organosiloxane shows high compatibility with phenyl-modified silicone.

[0037] The compositions of Examples 5-11 and Comparative Examples 1-4 were obtained by mixing components (A) to (C) in the composition ratios shown in Tables 1 and 2, which will be described later.

[0038] [Example 5] A thermally conductive phenyl-modified silicone composition was obtained by mixing A-1 as component (A), B-1 as component (B), and component (C). The components (A) to (C) were weighed out and placed in a plastic container placed in a rotation-revolution mixer (product name: Awatori Rentaro, manufactured by THINKY Corporation), and mixed at room temperature at 2,000 rpm for 1 minute twice. The mixture was then cooled to room temperature and the viscosity was measured.

[0039] [Example 6] A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 5, except that component (B) was changed from B-1 to B-2, and the viscosity was measured.

[0040] [Example 7] A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 5, except that component (B) was changed from B-1 to B-3, and the viscosity was measured.

[0041] [Example 8] A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 5, except that component (B) was changed from B-1 to B-4, and the viscosity was measured.

[0042] [Comparative Example 1] A composition of Comparative Example 1 was prepared in the same manner as in Example 5, except that the component (B) was changed from B-1 to B-5, and the viscosity was measured.

[0043] [Comparative Example 2] A composition of Comparative Example 2 was prepared in the same manner as in Example 5, except that the component (B) was changed from B-1 to B-6, and the viscosity was measured.

[0044] [Example 9] A thermally conductive phenyl-modified silicone composition was prepared in the same manner as in Example 5, except that the component (A) was changed from A-1 to A-2 and the component (B) was changed from B-1 to B-2, and the viscosity was measured.

[0045] [Example 10] Thermally conductive phenyl-modified silicone compositions were prepared in the same manner as in Example 5, except that the component (A) was changed from A-1 to A-3 and the component (B) was changed from B-1 to B-2, and the viscosity was measured.

[0046] [Example 11] Thermally conductive phenyl-modified silicone compositions were prepared in the same manner as in Example 5, except that the (B) component was changed from B-1 to B-2 and the composition and content of the (C) component (C-1 was changed to C-4), and the viscosity was measured.

[0047] [Comparative Example 3] A composition of Comparative Example 3 was prepared in the same manner as in Example 5, except that A-2 was added as the component (A) in addition to A-1, and no component (B) was added, and the viscosity was measured.

[0048] [Comparative Example 4] A composition of Comparative Example 4 was prepared in the same manner as in Example 5, except that the component (B) was not added and the content of the component (C) was changed, and the viscosity was measured.

[0049] (A) Organosiloxane A-1: Represented by the following formula, kinematic viscosity is 700mm2 ·s -1 Organosiloxane [ka]

[0050] A-2: Represented by the following formula, kinematic viscosity is 380mm 2 ·s -1 Phenyl-modified organosiloxane [ka]

[0051] A-3: The following formula is used, and the kinetic viscosity is 2,000 mm 2 ·s -1 Phenyl-modified organosiloxane [ka]

[0052] (B) Wetter B-1: Organosiloxane synthesized in Example 1, represented by the following formula: [ka]

[0053] B-2: Organosiloxane synthesized in Example 2, represented by the following formula: [ka]

[0054] B-3: Organosiloxane synthesized in Example 3, represented by the following formula: [ka]

[0055] B-4: Organosiloxane synthesized in Example 4, represented by the following formula: [ka]

[0056] B-5: Organosiloxane of Comparative Example 1 represented by the following formula [ka]

[0057] B-6: Organosiloxane represented by the following formula: [ka]

[0058] (C) Thermally conductive filler C-1: Spherical alumina powder (average particle size 45 μm) C-2: Spherical alumina powder (average particle size 10 μm) C-3: Irregular alumina powder (average particle size 2 μm) C-4: Irregular aluminum nitride powder (average particle size 30 μm)

[0059] [Manufacturing method] Components (A) to (C) were mixed as follows to obtain compositions of composition examples and comparative examples. The components (A) to (C) were weighed out and placed in a plastic container and placed in a rotation-revolution mixer (product name: Awatori Rentaro, manufactured by THINKY Corporation) in the composition ratios (parts by volume) shown in Table 1. The components were mixed at room temperature at 2,000 rpm for 1 minute twice, and the mixture was then cooled to room temperature.

[0060] [Test Method] The properties of the resulting composition were measured by the following test methods, and the results are shown in the following table.

[0061] [Viscosity measurement] The obtained composition was measured using a viscosity / viscoelasticity measuring device (product name: MARS40 (Thermo Fisher Scientific Co., Ltd.)) at a rotation speed of 10 s -1 The viscosity at 23° C. was measured using parallel plates with a gap of 0.5 mm.

[0062] [Table 1]

[0063] [Table 2]

[0064] The results in Tables 1 and 2 show that the phenyl-modified silicone composition containing the organopolysiloxane of the present invention has a reduced viscosity, allowing for a high loading of thermally conductive filler. In particular, in Example 10, despite the use of high-viscosity A-3 as component A, the viscosity of the composition was reduced compared to Comparative Example 1. On the other hand, when B-5, which does not fall within the range of the general formula (2), was used (Comparative Example 1), and when the composition did not contain the (B) component (Comparative Examples 3 and 4), the viscosity increased. When B-6, which does not contain a phenyl group, was used (Comparative Example 2), the viscosity of the composition did not increase.

[0065] The present specification includes the following aspects. [1]: An organopolysiloxane characterized by being represented by the following general formula (1): [ka] (In the formula, R 1 are independently a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms, and R 2 are independently an alkyl group having 1 to 10 carbon atoms; R 3 is an alkyl group having 1 to 4 carbon atoms; a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The bonds of the siloxane units enclosed in parentheses in the general formula (1) may be block or random. [2]: The organopolysiloxane according to [1], characterized in that the organopolysiloxane is represented by the following general formula (2): [ka] (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer of 1≦x≦30, m' is an integer of 1≦m'≦3, and n' is an integer of 0≦n'≦2, provided that m'+n' is 3. The bonds of the siloxane units enclosed in parentheses in the general formula (2) may be block or random, and the bonds of two types of siloxane units enclosed in parentheses with x are block polymers. [3]: In the general formula (1) and the general formula (2), R 1 is a phenyl group, R 2 is a methyl group. [4]: A wetter comprising the organopolysiloxane according to any one of [1] to [3] above.

[0066] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. The following general formula (1) 【Chemistry 1】 (In the formula, R 1 are each independently a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms; R 2 are independently an alkyl group having 1 to 10 carbon atoms; R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The bonds of the siloxane units enclosed in parentheses in the general formula (1) may be block or random. Organopolysiloxane, characterized by being represented by the following formula:

2. The organopolysiloxane is represented by the following general formula (2): 【Chemistry 2】 (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer of 1≦x≦30, m' is an integer of 1≦m'≦3, and n' is an integer of 0≦n'≦2, provided that m'+n' is 3. The bond of the siloxane units enclosed in parentheses with m' and n' may be block or random, and the bond of two types of siloxane units enclosed in parentheses with x is a block polymer.

2. The organopolysiloxane according to claim 1, which is represented by the formula:

3. The R 1 is a phenyl group, and the R 2 3. The organopolysiloxane according to claim 1, wherein is a methyl group.

4. A wetter comprising the organopolysiloxane according to claim 1 or 2.

5. A wetter comprising the organopolysiloxane according to claim 3.

Citation Information

Patent Citations

  • Organopentasiloxane and its production

    JP1994009657A

  • Heat conductive silicone composition

    JP2004262972A

  • Organosilicon compound, method of producing the same, and curable silicone composition comprising the organosilicon compound as adhesiveness-imparting agent

    JP2011136962A

  • Organopolysiloxane having single terminal functional group and method for manufacturing the same

    JP2013136662A

  • Polysiloxane compound and moisture-curable resin composition

    JP2013221135A

Cited By

  • Heat-softenable heat-conductive silicone composition and heat-softenable heat-conductive silicone cured product

    JP2026083847A