Composition for vinyl chloride resin film, and vinyl chloride resin film
The use of a carboxylic acid compound in the vinyl chloride resin film composition stabilizes the metal from the heat stabilizer, reducing foreign substance generation and enhancing tensile strength, addressing defects and improving film quality.
Patent Information
- Application Number
- JP2023054220
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional vinyl chloride resin films suffer from the generation of foreign substances during production, leading to defects in appearance and reduced tensile strength, particularly when using compositions containing coarse foreign matter.
A composition for vinyl chloride resin films is formulated with a specific amount of a carboxylic acid compound, a heat stabilizer, and a solvent, which suppresses the generation of foreign substances and enhances tensile strength by forming a stable salt with the metal derived from the heat stabilizer, thereby preventing aggregation and improving film quality.
The composition effectively reduces the formation of defects and enhances the tensile strength of the vinyl chloride resin films, ensuring they have fewer appearance issues and improved mechanical properties.
Smart Images

Figure 2024142174000001 
Figure 2024142174000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition for a vinyl chloride resin film and a vinyl chloride resin film. [Background technology]
[0002] Polyvinyl chloride resin films (hereinafter sometimes referred to as "PVC films") have excellent mechanical properties such as tensile strength and excellent processability, and are used in a variety of applications. Here, polyvinyl chloride resin films are produced, for example, by forming a film from a composition for polyvinyl chloride resin films (hereinafter sometimes referred to as "composition for PVC films"), which is obtained by dissolving and / or dispersing components such as polyvinyl chloride resin in a solvent, by cast molding or the like.
[0003] In order to improve the performance of PVC films, the formulation of compositions for PVC films has been studied. For example, vinyl chloride resin has the property of decomposing under high temperature conditions by a chain reaction of hydrogen chloride elimination. To stop this chain reaction of decomposition, a heat stabilizer has been added to the composition for PVC films (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-263945 Summary of the Invention [Problem to be solved by the invention]
[0005] However, when the conventional PVC film composition is prepared, foreign matter may be generated in the composition. In particular, when a PVC film is produced using a PVC film composition containing coarse foreign matter, there is a problem that defects in appearance may occur. In other words, the conventional PVC film composition has room for improvement in terms of suppressing the generation of foreign matter while ensuring the desired tensile strength of the PVC film obtained from the composition.
[0006] Therefore, an object of the present invention is to provide a composition for a vinyl chloride resin film which is capable of forming a vinyl chloride resin film that is suppressed in the production of foreign matter and has excellent tensile strength. Another object of the present invention is to provide a vinyl chloride resin film which has few defects in appearance and is excellent in tensile strength. [Means for solving the problem]
[0007] The present inventors have conducted extensive research with the aim of solving the above problems, and have found that when a composition for PVC film is prepared by adding a predetermined amount of a carboxylic acid compound having a predetermined structure in addition to a vinyl chloride resin, a heat stabilizer, and a solvent, the generation of foreign matter can be suppressed, and that the use of the composition for PVC film can enable the obtained PVC film to exhibit excellent tensile strength, thereby completing the present invention.
[0008] That is, the present invention aims to advantageously solve the above problems, and provides compositions for vinyl chloride resin films [1] to [5] and a vinyl chloride resin film [6].
[0009] [1] A composition comprising a vinyl chloride resin, a heat stabilizer, a carboxylic acid compound, and a solvent, wherein the carboxylic acid compound is represented by the following formula (I): R 1 -COOH···(I) (In formula (I), R 1is a hydrocarbon group having 1 to 10 carbon atoms.) or a salt thereof, and the amount of the carboxylic acid compound is 0.18 parts by mass or more and 2.00 parts by mass or less per 100 parts by mass of the vinyl chloride resin. A composition for PVC film containing a vinyl chloride resin, a heat stabilizer, a carboxylic acid compound which is the compound of the above formula (I) or a salt thereof, and a solvent, suppresses the generation of foreign matter, and by using this composition for PVC film, a vinyl chloride resin film having excellent tensile strength can be produced.
[0010] [2] The composition for polyvinyl chloride resin films described in [1] above, wherein the heat stabilizer includes a barium-zinc composite heat stabilizer. By using a composition for PVC film containing a barium-zinc composite stabilizer as a heat stabilizer, it is possible to sufficiently suppress the decomposition of the polyvinyl chloride resin while improving the weather resistance of the PVC film.
[0011] [3] The composition for vinyl chloride resin films according to [1] or [2] above, wherein the blending amount of the heat stabilizer is 0.5 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the vinyl chloride resin. By using a composition for PVC film in which the blending amount of the heat stabilizer is within the above-mentioned range, it is possible to sufficiently suppress the decomposition of the vinyl chloride resin and further improve the tensile strength of the PVC film.
[0012] [4] The composition for vinyl chloride resin films according to any one of [1] to [3] above, wherein the carboxylic acid compound includes at least one selected from the group consisting of acetic acid, caprylic acid, capric acid, 4-tert-butylbenzoic acid, acetate, caprylate, caprate, and 4-tert-butylbenzoate. By using a composition for PVC film containing any of the above-mentioned carboxylic acid compounds, it is possible to sufficiently suppress the generation of foreign matter and further improve the tensile strength of the PVC film.
[0013] [5] The composition for vinyl chloride resin films according to any one of [1] to [4] above, wherein the mass ratio of the amount of the carboxylic acid compound to the amount of the heat stabilizer is 0.03 or more and 0.50 or less. By using a composition for PVC film in which the mass ratio of the amount of the carboxylic acid compound to the amount of the heat stabilizer is within the above-mentioned range, the tensile strength of the PVC film can be further improved while sufficiently suppressing the generation of foreign matter.
[0014] [6] A vinyl chloride resin film formed using the composition for vinyl chloride resin film according to any one of [1] to [5] above. A PVC film formed from any of the above-mentioned compositions for a PVC film has few defects in appearance and is excellent in tensile strength. Effect of the Invention
[0015] According to the present invention, it is possible to provide a composition for a vinyl chloride resin film which is capable of forming a vinyl chloride resin film that is suppressed in the production of foreign matter and has excellent tensile strength. Furthermore, according to the present invention, it is possible to provide a vinyl chloride resin film which has few defects in appearance and is excellent in tensile strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present invention will be described in detail.
[0017] (Polyvinyl chloride resin film composition) The composition for PVC film of the present invention contains a vinyl chloride resin, a heat stabilizer, a carboxylic acid compound, and a solvent, and optionally contains other additives. The composition for PVC film of the present invention contains a carboxylic acid compound, which is a compound represented by a predetermined formula (I) or a salt thereof, in a predetermined range of blending amount, and therefore the generation of foreign matter is suppressed. Furthermore, the composition for PVC film of the present invention can be used as a material for producing a vinyl chloride resin film having few defects in appearance and excellent tensile strength. In addition, increasing the tensile strength of the polyvinyl chloride resin film has the advantage of suppressing problems such as the film cracking when used in an outdoor environment or the film breaking when applied to a three-dimensional object.
[0018] <Vinyl chloride resin> Examples of vinyl chloride resins include homopolymers consisting of vinyl chloride monomer units (repeating units derived from vinyl chloride monomers), as well as vinyl chloride copolymers containing preferably 50% by mass or more, more preferably 70% by mass or more, of vinyl chloride monomer units. Specific examples of monomers (comonomers) that can be copolymerized with vinyl chloride monomers and that can constitute vinyl chloride copolymers include those described in International Publication No. 2016 / 098344. Comonomers may be used alone or in combination of two or more types. The vinyl chloride resin may be used alone or in combination of two or more kinds.
[0019] The vinyl chloride resin is preferably dispersed as vinyl chloride resin fine particles in the sol-like PVC film composition, although it is not particularly limited thereto. The average particle size of the vinyl chloride resin fine particles contained in the PVC film composition is preferably 0.01 μm or more and 10 μm or less, although it is not particularly limited thereto. In this specification, the average particle size of the vinyl chloride resin contained in the composition for PVC film can be measured as the volume average particle size by a laser diffraction method in accordance with JIS Z8825.
[0020] The vinyl chloride resin is not particularly limited, but is preferably one produced by emulsion polymerization. The average polymerization degree of the vinyl chloride resin is preferably 500 or more and 4,000 or less, from the viewpoint of further improving the tensile strength of the PVC film. In this specification, the "average degree of polymerization" can be measured in accordance with JIS K6720-2.
[0021] <Heat stabilizer> The heat stabilizer contained in the composition for PVC film of the present invention is not particularly limited, but for example, a heat stabilizer containing at least one metal selected from the group consisting of lead (Pb), barium (Ba), zinc (Zn), calcium (Ca), and tin (Sn) can be used. As the heat stabilizer, from the viewpoint of sufficiently suppressing the decomposition of the vinyl chloride resin, a heat stabilizer containing lead (lead-based heat stabilizer), a heat stabilizer containing barium and zinc (barium-zinc-based composite heat stabilizer), a heat stabilizer containing calcium and zinc (calcium-zinc-based composite heat stabilizer), and a heat stabilizer containing tin (tin-based heat stabilizer) are preferable. And, from the viewpoint of improving the weather resistance of the PVC film, a barium-zinc-based composite heat stabilizer is more preferable. The heat stabilizers may be used alone or in combination of two or more.
[0022] The amount of the heat stabilizer in the composition for PVC film is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 1.5 parts by mass or more, even more preferably 2 parts by mass or more, particularly preferably 3 parts by mass or more, preferably 10 parts by mass or less, more preferably 9 parts by mass or less, even more preferably 7 parts by mass or less, even more preferably 6 parts by mass or less, and particularly preferably 5 parts by mass or less, per 100 parts by mass of vinyl chloride resin. If the amount of the heat stabilizer is 0.5 parts by mass or more, the decomposition of the vinyl chloride resin can be sufficiently suppressed, and if it is 10 parts by mass or less, the tensile strength of the PVC film can be further improved.
[0023] <Carboxylic acid compounds> The carboxylic acid compound contained in the composition for PVC film of the present invention has the following formula (I): R 1 -COOH···(I) In formula (I), R 1is a hydrocarbon group having from 1 to 10 carbon atoms. When the composition for PVC film of the present invention contains the above carboxylic acid compound in an amount of 0.18 part by mass or more per 100 parts by mass of vinyl chloride resin, the generation of foreign matter can be suppressed.
[0024] The reason why the use of the carboxylic acid compound suppresses the generation of foreign matter in the composition for PVC film is not clear, but is presumed to be as follows. First, according to the inventor's research, it has become clear that the heat stabilizer, especially the metal derived from the heat stabilizer, has some effect on the generation of foreign matter. In response to this, if the above-mentioned carboxylic acid compound is blended in a predetermined amount or more in the composition for PVC film, the metal derived from the heat stabilizer and the carboxylic acid compound form a salt and dissolve in the solvent. In this way, by dissolving the metal derived from the heat stabilizer together with the carboxylic acid compound in the solvent, the aggregation of various components caused by the metal derived from the heat stabilizer is suppressed. As a result, it is believed that the generation of coarse foreign matter in the composition for PVC film is suppressed, and the occurrence of defects in the appearance of the PVC film can be prevented.
[0025] In the compound of formula (I) which constitutes a carboxylic acid compound, R 1 As described above, R must be a hydrocarbon group having 1 to 10 carbon atoms. 1 It is presumed that when the number of carbon atoms in the hydrocarbon group constituting the heat stabilizer exceeds 10 and is equal to or greater than 11, the salt formed by the metal derived from the heat stabilizer and the carboxylic acid compound becomes difficult to dissolve in the solvent, and therefore the generation of foreign matter cannot be suppressed. Also, R 1 From the viewpoint of further improving the tensile strength of the PVC film, the number of carbon atoms in the hydrocarbon group constituting the polyvinyl chloride is preferably 2 or more, more preferably 4 or more, even more preferably 6 or more, and still more preferably 7 or more.
[0026] R 1 The hydrocarbon group constituting R may be linear, branched, or cyclic, or may be a combination of two or more of these.1 When the hydrocarbon group constituting the formula (I) has a cyclic structure, the cyclic structure may be an aromatic ring or a non-aromatic ring.
[0027] The carboxylic acid compound may be a compound represented by formula (I) or a salt of the compound (such as a sodium salt, a zinc salt, a barium salt, or a calcium salt).The carboxylic acid compound may be a mixture of the compound represented by formula (I) and a salt thereof.
[0028] As the carboxylic acid compound, from the viewpoint of further improving the tensile strength of the PVC film while sufficiently suppressing the generation of foreign matter, acetic acid, caprylic acid, capric acid, 4-tert-butylbenzoic acid, acetate, caprylate, caprate, and 4-tert-butylbenzoate are preferred, and caprylic acid, 4-tert-butylbenzoic acid, caprylate, and 4-tert-butylbenzoate are more preferred. The carboxylic acid compound may be used alone or in combination of two or more kinds.
[0029] The amount of the above-mentioned predetermined carboxylic acid compound in the composition for PVC film must be 0.18 parts by mass or more, preferably 0.20 parts by mass or more, and 2.00 parts by mass or less per 100 parts by mass of vinyl chloride resin, preferably 1.70 parts by mass or less, more preferably 1.40 parts by mass or less, even more preferably 1.10 parts by mass or less, even more preferably 0.80 parts by mass or less, and particularly preferably 0.50 parts by mass or less. If the amount of the carboxylic acid compound is less than 0.18 parts by mass per 100 parts by mass of vinyl chloride resin, the generation of foreign matter cannot be suppressed. On the other hand, if the amount of the carboxylic acid compound is more than 2.00 parts by mass per 100 parts by mass of vinyl chloride resin, the tensile strength of the PVC film decreases.
[0030] In the composition for PVC film, the mass ratio of the amount of the carboxylic acid compound to the amount of the heat stabilizer is preferably 0.03 or more, more preferably 0.04 or more, and preferably 0.50 or less, more preferably 0.40 or less, even more preferably 0.30 or less, even more preferably 0.25 or less, and particularly preferably 0.20 or less. If the mass ratio of the amount of the carboxylic acid compound to the amount of the heat stabilizer is 0.03 or more, the generation of foreign matter can be sufficiently suppressed, and if it is 0.50 or less, the tensile strength of the PVC film can be further improved.
[0031] <Solvent> As the solvent, a known solvent used in a composition for PVC film can be used. For example, as the solvent, it is preferable to use a dispersion solvent capable of improving the dispersion of vinyl chloride resin in the sol and a dilution solvent capable of adjusting the viscosity of the sol, either individually or in combination. The dispersion solvent is preferably a solvent that slightly swells the vinyl chloride resin at room temperature to promote dispersion and promotes melting and gelling in a high-temperature heating process. Specific examples of suitable dispersion solvents include ketone-based solvents such as diisobutyl ketone and methyl isobutyl ketone, ester-based solvents such as butyl acetate, and glycol ether-based solvents. The dilution solvent is preferably a solvent in which the vinyl chloride resin is insoluble, which reduces the sol viscosity, and which suppresses swelling. Specific examples of suitable dilution solvents include paraffinic hydrocarbon solvents, naphthenic hydrocarbon solvents, aromatic hydrocarbon solvents, and terpene hydrocarbon solvents. Among these, it is preferable to use aromatic hydrocarbon solvents. The solvent may be used alone or in combination of two or more kinds.
[0032] From the viewpoint of efficiently producing a PVC film while sufficiently suppressing the generation of foreign matter, the amount of the solvent in the composition for PVC film is preferably 20 parts by mass or more, and more preferably 30 parts by mass or more, and is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, even more preferably 100 parts by mass or less, and even more preferably 70 parts by mass or less, per 100 parts by mass of vinyl chloride resin.
[0033] <Other additives> The additives other than the vinyl chloride resin, heat stabilizer, carboxylic acid compound and solvent that may be optionally contained in the composition for PVC film of the present invention are not particularly limited, and examples thereof include those described in JP-A-2005-270775. Note that the other additives may be used alone or in combination of two or more. The composition for a PVC film of the present invention preferably contains a plasticizer and / or an ultraviolet absorbing agent as other additives.
[0034] <<Plasticizer>> The plasticizer is not particularly limited as long as it can impart flexibility to the PVC film, and any known plasticizer can be used. From the viewpoint of further improving the tensile strength of the PVC film, however, polyester-based plasticizers are preferred, and adipate polyester-based plasticizers are more preferred. From the viewpoint of further improving the tensile strength of the PVC film, the amount of the plasticizer in the composition for PVC film is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and is preferably 50 parts by mass or less, and more preferably 40 parts by mass or less, per 100 parts by mass of vinyl chloride resin.
[0035] <<Ultraviolet absorbing agent>> The ultraviolet absorbing agent is not particularly limited and any known agent can be used, but preferred examples include salicylic acid-based ultraviolet absorbing agents and benzophenone-based ultraviolet absorbing agents. The amount of plasticizer in the composition for PVC film is, from the viewpoint of imparting excellent ultraviolet absorbing performance to the PVC film while further improving the tensile strength of the PVC film, preferably 0.1 part by mass or more, more preferably 1 part by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, per 100 parts by mass of vinyl chloride resin.
[0036] <Preparation of composition for polyvinyl chloride resin film> The method for preparing the composition for PVC film is not particularly limited, and the composition can be obtained by mixing the above-mentioned components using a known mixer such as a disper. After mixing the components, treatments such as filtration and degassing may be performed as necessary.
[0037] (Vinyl chloride resin film) The PVC film of the present invention is formed using the above-mentioned composition for a PVC film of the present invention. Since the PVC film of the present invention is formed from the above-mentioned composition for a PVC film of the present invention, the PVC film of the present invention has few defects in appearance due to large foreign matter and has excellent tensile strength.
[0038] Here, the PVC film of the present invention is, for example, a dried product of the above-mentioned composition for PVC film of the present invention, and contains a vinyl chloride resin, a heat stabilizer, a carboxylic acid compound, and optionally other additives. Note that, since the components contained in the PVC film of the present invention are derived from the composition for PVC film, the preferred ratio of the components in the PVC film is usually the same as that in the above-mentioned composition for PVC film, except for the solvent.
[0039] The method for producing a PVC film from the composition for PVC film is not particularly limited as long as it is a method capable of removing the solvent and forming a film, but cast molding is preferred. That is, the PVC film of the present invention is preferably a cast film.
[0040] The method for producing a PVC film by cast molding is not particularly limited, and for example, a PVC film can be obtained by applying a composition for a PVC film onto a substrate and drying it. The substrate is not particularly limited, and a known substrate such as a polyethylene terephthalate film (PET film) can be used. The drying conditions are also not particularly limited, and for example, the drying temperature can be 100°C or higher and 200°C or lower, and the drying time can be 10 seconds or higher and 10 minutes or lower.
[0041] The thickness of the PVC film may be appropriately set depending on the application, etc., and may be, for example, 10 μm or more and 300 μm or less. EXAMPLES
[0042] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. The inhibition of the formation of foreign matter in the composition for PVC film and the tensile strength of the PVC film were evaluated by the following methods.
[0043] <Prevention of foreign matter generation> The compositions for PVC films obtained in the examples and comparative examples were left to stand at room temperature for 4 days to prepare evaluation samples. The evaluation samples were subjected to particle size determination in accordance with JIS K5600-2-5 using a grind gauge with a maximum groove depth of 100 μm, and evaluated according to the following criteria. The smaller the particle size, the more the generation of coarse foreign matter is suppressed. A: Particle size is less than 30 μm B: Particle size is 30 μm or more <Tensile strength> Test pieces of 100 mm (MD) × 20 mm (TD) were cut out from the PVC films obtained in the Examples and Comparative Examples. A tensile test was performed on these test pieces using a tensile tester (Minebea Co., Ltd., "NMB TECHNO GRAPH TG-1kN") under the conditions of a chuck distance of 50 mm and a test speed of 200 mm / min. The strength (kgf / mm) at which the test pieces broke was calculated. 2) was measured. This tensile test was performed a total of 6 times, and the average value of the strength in the 6 times was taken as the tensile strength.
[0044] (Example 1) <Preparation of Composition for PVC Film> 100 parts by mass of vinyl chloride resin (manufactured by Mexichem, trade name "GEON178", vinyl chloride resin fine particles, average degree of polymerization: 1800), 28 parts by mass of adipic acid polyester plasticizer (manufactured by Dainichi Seika Kogyo Co., Ltd., trade name "Fine Sizer NS-4070"), 4 parts by mass of barium-zinc composite heat stabilizer (manufactured by Katsuta Kako Co., Ltd., trade name "SB-9301N"), 4 parts by mass of benzophenone-based ultraviolet absorber (manufactured by Cypro Kasei Co., Ltd., trade name "Cisorb 102"), 0.40 part by mass of caprylic acid as a carboxylic acid compound, and 45.3 parts of aromatic hydrocarbon solvent (manufactured by Godo Co., Ltd., trade name "SS-100", aromatic hydrocarbon solvent) were weighed into a container and mixed using a disper at 2000 rpm for 10 minutes. The obtained mixed solution was filtered through a 150-mesh polyester mesh and defoamed while stirring slowly under vacuum until foaming stopped, to obtain a sol-like composition for PVC film. Using this composition for PVC film, evaluation was carried out on the suppression of foreign matter generation. The results are shown in Table 1. <Production of PVC Film> The composition for PVC film obtained as described above was allowed to stand at room temperature for 12 hours or more to obtain a coating liquid. This coating liquid was coated onto a PET film (manufactured by Mitsubishi Chemical Corporation, trade name "T100E38", thickness: 38 μm) as a substrate using a film applicator. Next, the coating liquid on the substrate was dried in a drying oven at 140 °C for 30 seconds, 160 °C for 30 seconds, and 190 °C for 30 seconds for a total of 90 seconds to produce a PVC film (thickness: 30 μm) on the substrate. This PVC was peeled from the substrate film and the tensile strength was measured. The results are shown in Table 1.
[0045] (Example 2) In preparing the composition for PVC film, the amount of caprylic acid as the carboxylic acid compound was changed from 0.40 parts by mass to 1.19 parts by mass, but the composition for PVC film and PVC film were prepared in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 1.
[0046] (Examples 3 to 5) In preparing the compositions for PVC films, 0.49 parts by mass (Example 3), 1.47 parts by mass (Example 4), and 0.20 parts by mass (Example 5) of 4-tert-butylbenzoic acid were used instead of 0.40 parts by mass of caprylic acid as the carboxylic acid compound, but the compositions for PVC films and PVC films were prepared in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 1.
[0047] Example 6 In preparing the composition for PVC film, 0.33 parts by mass of acetic acid was used instead of 0.40 parts by mass of caprylic acid as the carboxylic acid compound, but the composition for PVC film and PVC film were prepared in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 1.
[0048] Comparative Example 1 In preparing the composition for PVC film, except that caprylic acid was not used as the carboxylic acid compound, a composition for PVC film and a PVC film were prepared in the same manner as in Example 1, and various evaluations were carried out. The results are shown in Table 2.
[0049] Comparative Example 2 A composition for PVC film was prepared in the same manner as in Example 1, except that 1.10 parts by mass of lauric acid was used instead of 0.40 parts by mass of caprylic acid as the carboxylic acid compound, and the composition was evaluated for its inhibition of foreign matter generation. The results are shown in Table 2.
[0050] Comparative Example 3 The composition for PVC film was prepared in the same manner as in Example 1, except that the amount of caprylic acid as the carboxylic acid compound was changed from 0.40 parts by mass to 0.16 parts by mass, and the composition for PVC film was evaluated for its inhibition of foreign matter generation. The results are shown in Table 2.
[0051] Comparative Example 4 In preparing the composition for PVC film, the amount of caprylic acid as the carboxylic acid compound was changed from 0.40 parts by mass to 2.50 parts by mass, but the composition for PVC film and the PVC film were prepared in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 2.
[0052] In Tables 1 and 2 shown below, "carboxylic acid compound / thermal stabilizer" means the mass ratio of the amount of carboxylic acid compound to the amount of thermal stabilizer, and the mass ratios in Tables 1 and 2 are values rounded off to two decimal places.
[0053] [Table 1]
[0054] [Table 2]
[0055] From Tables 1 and 2, it can be seen that by using a composition for PVC film that contains a specified amount of a carboxylic acid compound having a specified structure in addition to vinyl chloride resin, a heat stabilizer, and a solvent, it is possible to produce a PVC film that has excellent tensile strength while suppressing the generation of foreign matter. [Industrial Applicability]
[0056] According to the present invention, it is possible to provide a composition for a vinyl chloride resin film which is capable of forming a vinyl chloride resin film that is suppressed in the production of foreign matter and has excellent tensile strength. Furthermore, according to the present invention, it is possible to provide a vinyl chloride resin film which has few defects in appearance and is excellent in tensile strength.
Claims
1. The composition includes a vinyl chloride resin, a heat stabilizer, a carboxylic acid compound, and a solvent, The carboxylic acid compound is represented by the following formula (I): R 1 -COOH・・・(I) (In formula (I), R 1 is a hydrocarbon group having 1 to 10 carbon atoms, The composition for polyvinyl chloride resin films, wherein the amount of the carboxylic acid compound is 0.18 parts by mass or more and 2.00 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
2. The composition for vinyl chloride resin films according to claim 1 , wherein the heat stabilizer comprises a barium-zinc based composite heat stabilizer.
3. The composition for polyvinyl chloride resin films according to claim 1 , wherein the blending amount of the heat stabilizer is 0.5 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
4. 2. The composition for polyvinyl chloride resin films according to claim 1, wherein the carboxylic acid compound comprises at least one selected from the group consisting of acetic acid, caprylic acid, capric acid, 4-tert-butylbenzoic acid, acetate, caprylate, caprate, and 4-tert-butylbenzoate.
5. The composition for vinyl chloride resin films according to claim 1 , wherein a mass ratio of the amount of the carboxylic acid compound to the amount of the heat stabilizer is 0.03 or more and 0.50 or less.
6. A vinyl chloride resin film formed using the composition for vinyl chloride resin films according to any one of claims 1 to 5.
Citation Information
Patent Citations
Paste composition, semi-rigid film made of the composition and its production
JP1994263945A