Self-adsorption laminate and composition for self-adsorption foamed sheet
The self-adhesive laminate with controlled peeling forces addresses the challenge of balanced adhesion to PVC and water-repellent wallpapers, ensuring versatile and easy reapplication.
Patent Information
- Application Number
- JP2023054226
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional self-adhesive laminates face difficulties in achieving balanced adhesion to both polyvinyl chloride (PVC) wallpaper and water-repellent wallpaper, often leading to poor reworkability and improper adhesion to either type, making it challenging for consumers to select the appropriate laminate.
A self-adhesive laminate composed of an acrylic resin foam sheet with controlled peeling forces (P1 and P2) within specific ranges and an absolute difference (|P1-P2|) less than 1.00 N/cm, combined with a base material, ensuring balanced adhesion to both PVC and water-repellent wallpapers.
The laminate exhibits well-balanced adhesion to both PVC and water-repellent wallpapers, enhancing versatility and reworkability by maintaining appropriate peeling forces within predetermined limits.
Smart Images

Figure 2024142180000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a self-adhesive laminate and a composition for a self-adhesive foam sheet. [Background technology]
[0002] Conventionally, a sheet-like member made of a foam material having a large number of fine pores and having self-adhesive properties, i.e., a self-adhesive foam sheet (hereinafter, sometimes simply referred to as a "foam sheet"), has been used as an adhesive sheet to be attached to an adherend such as a wall or window glass. The adhesive mode of the self-adhesive foam sheet is not by glue adhesion, but by adhering to the adherend using the fine pores. Therefore, the self-adhesive foam sheet is easier to reattach than the conventional adhesive sheets that use glue adhesion, and is suitable for use in applications such as wallpaper, posters, and stickers.
[0003] When used for these applications, the self-adhesive foam sheet is usually used in the form of a self-adhesive laminate (hereinafter, sometimes simply referred to as a "laminate") laminated with a substrate. By applying a decoration such as printing to the surface of this self-adhesive laminate facing the substrate, it can be advantageously used for the above applications (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-23156 A Summary of the Invention [Problem to be solved by the invention]
[0005] The wallpaper constituting the wall on which the laminate is attached is generally polyvinyl chloride wallpaper (wallpaper with at least the surface layer made of polyvinyl chloride. Hereinafter, this may be abbreviated as "PVC wallpaper.") In recent years, the use of wallpaper with a water-repellent surface treatment to enhance water repellency (hereinafter, this will be referred to as "water-repellent wallpaper") has also expanded. Here, while conventional laminates can be easily attached to PVC wallpaper, they may have difficulty attaching to water-repellent wallpaper, or may peel off over time even if they are attached once. In addition, when the adhesion of conventional laminates to water-repellent wallpaper is increased, the adhesion to PVC wallpaper increases excessively, making it difficult to peel off and reattach (i.e., reworkability is impaired). When general consumers select and purchase laminates, it is not easy to determine whether the wall to which they are to be attached is PVC wallpaper or water-repellent wallpaper. In other words, conventional laminates have had the problem of exhibiting a good balance of appropriate adhesion to both PVC wallpaper and water-repellent wallpaper, thereby increasing versatility.
[0006] SUMMARY OF THE PRESENT EMBODIMENTS The present invention has an object to provide a self-adhesive laminate that exhibits a well-balanced and appropriate adhesion to both polyvinyl chloride wallpaper and water-repellent wallpaper. Another object of the present invention is to provide a composition for a self-adhesive foam sheet that can be used to prepare a self-adhesive laminate that exhibits a well-balanced and appropriate adhesion to both polyvinyl chloride wallpaper and water-repellent wallpaper. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems, and have found that a laminate including a foamed sheet in which two types of peel strengths measured by a specific method are within a specific range and the absolute value of the difference between the two types of peel strengths is less than a specific value exhibits appropriate adhesion to both PVC wallpaper and water-repellent wallpaper and has excellent versatility, thereby completing the present invention.
[0008] That is, according to the present invention, there are provided the following self-adhesive laminates (1) to (3) and compositions for self-adhesive foam sheets (4) to (7).
[0009] [1] A self-adhesive laminate formed by laminating a substrate and a self-adhesive foam sheet made of an acrylic resin foam, wherein the self-adhesive foam sheet has a peel strength P1 against polyvinyl chloride wallpaper and a peel strength P2 against water-repellent wallpaper both of which are 1.00 N / cm or more and 4.00 N / cm or less, and the absolute value of the difference between the peel strength P1 and the peel strength P2 is less than 1.00 N / cm. A laminate including a foam sheet having peel strength P1 and peel strength P2 each within the range of 1.00 to 4.00 N / cm and an absolute value of the difference between peel strength P1 and peel strength P2 (hereinafter sometimes referred to as "|P1-P2|") of less than 1.00 N / cm exhibits a well-balanced and appropriate adhesion to both PVC wallpaper and water-repellent wallpaper and is highly versatile. In this specification, the "peeling strength P1 from polyvinyl chloride wallpaper" and the "peeling strength P2 from water-repellent wallpaper" of the self-adhesive foam sheet can be measured using the method described in the Examples.
[0010] [2] The self-adhesive laminate according to [1] above, wherein the self-adhesive foam sheet has an average thickness of more than 40 μm. By making the average thickness of the foamed sheet exceed 40 μm, there is an advantage that the peel strengths P1 and P2 of the foamed sheet can be increased, and the peel strengths P1 and P2, and |P1-P2| can be easily controlled within a predetermined range. In this specification, the "average thickness" of a self-adhesive foam sheet or the like refers to the arithmetic mean value of thicknesses at any six points on the self-adhesive foam sheet or the like to be measured.
[0011] [3] The tensile modulus of the self-adhesive foam sheet is 0.05 N / mm 2 The self-adhesive foam sheet according to the above item [1] or [2], wherein the breaking elongation of the self-adhesive foam sheet is 300% or more. The tensile modulus of the foam sheet is 0.05 N / mm 2or less and the breaking elongation is 300% or more, there is an advantage in that it becomes easier to control the peel forces P1 and P2, and |P1-P2| within a predetermined range. In this specification, the "tensile modulus" and "breaking elongation" of the self-adhesive foam sheet can be measured by the methods described in the Examples.
[0012] [4] A composition for a self-adhesive foam sheet comprising an acrylic resin and a crosslinking agent, the acrylic resin having a tensile modulus of elasticity of 0.30 N / mm 2 The composition for self-adhesive foam sheet is as follows: Tensile modulus: 0.30N / mm 2 When an acrylic resin foam formed from a foam sheet composition containing an acrylic resin having a modulus of elasticity or less and a breaking elongation of 500% or more and a crosslinking agent is used as a foam sheet, a laminate that exhibits a well-balanced and appropriate adhesion to both PVC wallpaper and water-repellent wallpaper and has excellent versatility can be produced. In this specification, the "tensile modulus" and "elongation at break" of the acrylic resin can be measured by the methods described in the Examples.
[0013] [5] The composition for a self-adhesive foam sheet according to the above [4], wherein the acrylic resin has a glass transition temperature of -40°C or lower. Forming a foamed sheet using a foamed sheet composition containing an acrylic resin having a glass transition temperature of -40°C or lower has the advantage that the peel strengths P1 and P2 and |P1-P2| can be easily controlled within a predetermined range. In addition, a foamed sheet having excellent conformability to irregularities during attachment and excellent adhesion stability over a long period of time can be obtained. In this specification, the "glass transition temperature" of a resin such as an acrylic resin can be measured by the method described in the examples.
[0014] [6] The composition for self-adhesive foam sheet according to the above [4] or [5], wherein the content of the crosslinking agent is 0.5 parts by mass or more and 3 parts by mass or less per 100 parts by mass of the acrylic resin. When a foam sheet is formed using a foam sheet composition having a crosslinking agent content within the above range, it is advantageous in that the peel strengths P1 and P2 and |P1-P2| can be easily controlled within a predetermined range, and a foam sheet having excellent strength and flexibility can be obtained.
[0015] [7] The composition for a self-adhesive foam sheet according to any one of the above [4] to [6], wherein the acrylic resin is a polymer containing 2-ethylhexyl acrylate units in a proportion of 50% by mass or more. Forming a foam sheet using a foam sheet composition containing an acrylic resin containing 50% by mass or more of 2-ethylhexyl acrylate units as repeating units has the advantage that the peel forces P1 and P2, as well as |P1-P2|, can be easily controlled within specified ranges. In this specification, the term "monomer unit" means "a repeating unit derived from a monomer contained in a polymer obtained by using that monomer", for example, the above "2-ethylhexyl acrylate unit" means a repeating unit derived from 2-ethylhexyl acrylate. Effect of the Invention
[0016] According to the present invention, it is possible to provide a self-adhesive laminate that exhibits a well-balanced and appropriate adhesion to both polyvinyl chloride wallpaper and water-repellent wallpaper. Furthermore, according to the present invention, it is possible to provide a composition for a self-adhesive foam sheet that can be used to prepare a self-adhesive laminate that exhibits a well-balanced and appropriate adhesion to both polyvinyl chloride wallpaper and water-repellent wallpaper. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described in detail. The self-adhesive laminate of the present invention is not particularly limited, and the self-adhesive foam sheet of the self-adhesive laminate is used by attaching it to a surface to be adhered, such as a wall surface with wallpaper, and can be easily peeled off from the surface to be adhered after use. The composition for the self-adhesive foam sheet of the present invention can be used to prepare the self-adhesive foam sheet constituting the self-adhesive laminate of the present invention.
[0018] (Self-adhesive laminate) The laminate of the present invention is formed by laminating a foamed sheet made of an acrylic resin foam and a substrate. The laminate of the present invention is characterized in that the foamed sheet has a peel strength P1 against polyvinyl chloride wallpaper and a peel strength P2 against water-repellent wallpaper of 1.00 N / cm or more and 4.00 N / cm or less, and the absolute value of the difference between the peel strength P1 and the peel strength P2 is less than 1.00 N / cm. The laminate of the present invention, which includes a foamed sheet having such properties, exhibits a good balance of appropriate adhesion to both PVC wallpaper and water-repellent wallpaper, and is highly versatile.
[0019] The structure of the laminate of the present invention is not particularly limited as long as the foam sheet is laminated on one side in the thickness direction of the substrate, and one surface (the surface to be bonded to the adherend during use) is composed of the foam sheet. For example, the laminate may have a structure in which an arbitrary layer such as an adhesive layer is interposed between the substrate and the foam sheet. For example, the laminate may have a peelable separator film laminated on the surface on the foam sheet side during transportation or storage before being bonded to the adherend.
[0020] <Self-adhesive foam sheet> The foam sheet is made of an acrylic resin foam and has predetermined properties.
[0021] <<Peeling force P1>> The foam sheet needs to have a peeling force P1 against the PVC wallpaper of 1.00 N / cm or more and 4.00 N / cm or less, as described above, preferably 1.40 N / cm or more, more preferably 1.80 N / cm or more, even more preferably 2.20 N / cm or more, particularly preferably 2.60 N / cm or more, preferably 3.70 N / cm or less, more preferably 3.40 N / cm or less, even more preferably 3.10 N / cm or less, and particularly preferably 2.90 N / cm or less. If the peeling force P1 is less than 1.00 N / cm, the adhesion of the laminate to the PVC wallpaper decreases. On the other hand, if the peeling force P1 exceeds 4.00 N / cm, it becomes difficult to peel from the PVC wallpaper, and the reworkability of the laminate cannot be ensured. In other words, if the peeling force P1 is in the range of 1.00 N / cm or more and 4.00 N / cm or less, it can be said that the laminate has a moderate adhesion to the PVC wallpaper.
[0022] <<Peel force P2>> The foam sheet needs to have a peeling force P2 against the water-repellent wallpaper of 1.00 N / cm or more and 4.00 N / cm or less, as described above, preferably 1.30 N / cm or more, more preferably 1.60 N / cm or more, even more preferably 1.90 N / cm or more, particularly preferably 2.10 N / cm or more, preferably 3.50 N / cm or less, more preferably 3.00 N / cm or less, even more preferably 2.70 N / cm or less, and particularly preferably 2.40 N / cm or less. If the peeling force P2 is less than 1.00 N / cm, the adhesion of the laminate to the water-repellent wallpaper decreases. On the other hand, if the peeling force P2 exceeds 4.00 N / cm, it becomes difficult to peel from the water-repellent wallpaper, and the reworkability of the laminate cannot be ensured. In other words, if the peeling force P2 is within the range of 1.00 N / cm or more and 4.00 N / cm or less, it can be said that the laminate has a moderate adhesion to the water-repellent wallpaper.
[0023] <<Absolute value of the difference between peel force P1 and peel force P2>> As described above, the foam sheet needs to have |P1-P2| less than 1.00 N / cm, preferably less than 0.90 N / cm, more preferably less than 0.80 N / cm, even more preferably less than 0.70 N / cm, and particularly preferably less than 0.65 N / cm. If |P1-P2| is 1.00 N / cm or more, the gap between adhesion to PVC wallpaper and adhesion to water-repellent wallpaper becomes large, and the laminate cannot exhibit a balanced appropriate adhesion to both general wallpaper and water-repellent wallpaper.
[0024] <<Average thickness>> The foam sheet preferably has an average thickness of more than 40 μm, more preferably 60 μm or more, even more preferably 100 μm or more, preferably 1 mm or less, and more preferably 500 μm or less. If the average thickness of the foam sheet is more than 40 μm, the foam sheet can improve the conformability to unevenness when the laminate including the foam sheet is attached to the adherend. Therefore, the peeling force P1 and the peeling force P2 can be increased, and the adhesion to both the PVC wallpaper and the water-repellent wallpaper can be improved. That is, there is an advantage that the peeling forces P1 and P2, and |P1-P2| can be easily controlled within a predetermined range. On the other hand, if the average thickness of the foam sheet is 1 mm or less, the increase in the weight of the laminate including the foam sheet can be suppressed, and the workability can be improved.
[0025] <<Tensile modulus>> The foam sheet has a tensile modulus of 0.05N / mm 2 It is preferable that the resistance is less than 0.04 N / mm 2 More preferably, it is 0.03 N / mm 2 More preferably, it is 0.02 N / mm 2 It is particularly preferable that the tensile modulus of the foam sheet is 0.05 N / mm 2 If the peeling forces P1 and P2 and |P1-P2| are not more than the above range, there is an advantage that they can be easily controlled within a predetermined range. The lower limit of the tensile modulus of elasticity of the foamed sheet is not particularly limited, but may be, for example, 0.001 N / mm 2It can be more than that.
[0026] <<Elongation at break>> The foamed sheet preferably has a breaking elongation of 300% or more, more preferably 350% or more, even more preferably 400% or more, even more preferably 450% or more, and particularly preferably 500% or more. If the breaking elongation of the foamed sheet is 300% or more, there is an advantage that the peeling forces P1 and P2 and |P1-P2| can be easily controlled within a predetermined range. The upper limit of the breaking elongation of the foamed sheet is not particularly limited, but can be, for example, 1000% or less.
[0027] The properties of the foamed sheet described above (peel forces P1 and P2, |P1-P2|, average thickness, tensile modulus, breaking elongation, etc.) can be adjusted, for example, by changing the composition and solids concentration of the composition for the foamed sheet, the ratio of air bubbles mixed in during foaming, the thickness of coating the foam, and the drying and crosslinking conditions.
[0028] <Base material> The substrate is not particularly limited, and may be a known substrate (such as a paper substrate or a plastic substrate) used in a self-adhesive laminate. However, for the laminate of the present invention, it is preferable to use a substrate including at least one layer selected from the group consisting of a nonwoven fabric layer, a resin layer made of a crystalline resin having a melting point of 120° C. or more or a non-crystalline resin having a glass transition temperature of 50° C. or more, and an aluminum layer. If a substrate having at least one of these layers is bonded to a foam sheet via the layer, the dimensional change when the laminate absorbs moisture can be suppressed (i.e., moisture resistance can be improved). In addition to at least one of the above layers, the substrate may optionally include a layer (hereinafter simply referred to as "other layer") made of a material other than the above-mentioned specified material. The other layer is usually formed on the surface of the layer made of the specified material opposite to the side on which the self-adhesive foam sheet is provided. The other layer may be provided on a part of the surface or on the entire surface, but is preferably provided on the entire surface.
[0029] The substrate may be composed of only a layer made of the above-mentioned predetermined material. Among them, the substrate is preferably composed of a nonwoven fabric layer, or a nonwoven fabric layer and a predetermined resin layer. When the substrate includes two or more layers selected from the group consisting of a nonwoven fabric layer, a specific resin layer, and an aluminum layer, the method for integrating these layers is not particularly limited, and these layers can be integrated using known techniques such as the use of an adhesive, fusion bonding, and pressure bonding.
[0030] The average thickness of the layer made of the predetermined material is not particularly limited, but is preferably 50 μm or more, more preferably 100 μm or more, even more preferably 130 μm or more, and is preferably 1000 μm or less. If the average thickness of the layer made of the predetermined material is 50 μm or more, the mechanical strength of the laminate can be improved, and when the base material includes a nonwoven fabric layer, and when a foam formed from a foam sheet composition described later or a resin composition for forming a predetermined resin layer is coated on the nonwoven fabric layer, strike-through can be effectively suppressed. If the thickness of the layer made of the predetermined material is 1000 μm or less, deterioration of heat transmission during heating and drying when preparing a foam sheet can be suppressed, and the foam sheet can be sufficiently dried.
[0031] <<Nonwoven layer>> The nonwoven fabric layer is a layer made of nonwoven fabric. Nonwoven fabric (fleece) is a material in which fibers are entangled three-dimensionally. Specifically, as defined in JIS L 0222, "nonwoven fabric" refers to "a fiber sheet, web, or batt in which the fibers are oriented in one direction or randomly and are bonded to each other by at least one of entanglement, fusion, and adhesion" (excluding paper, woven fabric, knitted fabric, tufts, and crepe felt). Thus, since nonwoven fabric is made of fibers entangled three-dimensionally, it is presumed that the dimensions of the nonwoven fabric are unlikely to change even when it absorbs moisture. The material of the nonwoven fabric is not particularly limited, but it is preferable to use a resin such as polyester such as polyethylene terephthalate, polypropylene, polyethylene, polyamide, vinyl acetate, vinyl chloride, acrylic, polyurethane, polyoxymethylene, polytetrafluorethylene, polyimide, polyvinyl alcohol, etc. These resins can be used alone or in combination of two or more. Among them, it is preferable to use polyester as the resin from the viewpoints of heat resistance, water resistance, chemical resistance, etc. Also, from the viewpoint of suppressing deterioration of the appearance of the substrate due to shrinkage or melting during the heat treatment in producing the foamed sheet, it is preferable to use a resin having excellent heat resistance (for example, in the case of using a crystalline resin, one having a melting point of 100° C. or more).
[0032] From the viewpoint of further improving the moisture resistance of the laminate, it is preferable that the fibers constituting the nonwoven fabric are composed only of the above-mentioned resins, but the nonwoven fabric used in the present invention may contain pulp. Here, pulp refers to a fibrous material in which a plurality of cellulose fibers are aggregated. For example, the nonwoven fabric may contain pulp in an amount of 50% by mass or more and 90% by mass or less when the total amount of the components contained in the nonwoven fabric is taken as 100% by mass.
[0033] The nonwoven fabric layer may contain, within the scope of the invention, a binder (adhesive) that can be used in the manufacture of the nonwoven fabric, a component such as a resin constituting a specific resin layer described below, and / or a component such as an acrylic resin constituting the foamed sheet. Furthermore, the nonwoven fabric layer may contain additives such as flame retardants, inorganic agents, colorants, sizing agents, fixing agents, mildew inhibitors, matting agents, and antibacterial agents, as appropriate, within the scope of the invention. It should be noted that the nonwoven fabric layer does not include a "resin layer made of a crystalline resin having a melting point of 120°C or higher or a non-crystalline resin having a glass transition temperature of 50°C or higher" described below.
[0034] The method for producing the nonwoven fabric is not particularly limited, and may be, for example, any of the wet method, spunbond method, thermal bond method, chemical bond method, needle punch method, stitch bond method, and hydroentanglement (spunlace) method.
[0035] <<Resin layer made of crystalline resin with a melting point of 120°C or higher or amorphous resin with a glass transition temperature of 50°C or higher>> The resin layer made of a crystalline resin having a melting point of 120°C or higher or a non-crystalline resin having a glass transition temperature of 50°C or higher is a film (sheet) made of a crystalline resin having a melting point of 120°C or higher, or a film (sheet) made of a non-crystalline resin having a glass transition temperature of 50°C or higher. These resins are resistant to dimensional changes even when they absorb moisture and have excellent heat resistance, so that they can improve moisture resistance while suppressing deterioration of the substrate due to heat during heating and drying when producing a foamed sheet.
[0036] Examples of the crystalline resin having a melting point of 120° C. or more include, but are not limited to, polyesters such as polyethylene terephthalate; polyolefins such as polypropylene and polyethylene; polyamides; polyvinylidene chloride; etc. These resins may be used alone or in combination of two or more. Among them, polyesters are preferably used as the crystalline resin having a melting point of 120° C. or more from the viewpoints of moisture resistance and heat resistance. In this specification, the "melting point" of a crystalline resin can be determined in accordance with JIS K7121 using a differential scanning calorimeter.
[0037] Examples of the amorphous resin having a glass transition temperature of 50° C. or higher include, but are not limited to, polyvinyl chloride (vinyl chloride resin), polycarbonate, polystyrene, etc. These resins may be used alone or in combination of two or more. Among them, from the viewpoints of processability, printability, flame retardancy, durability, weather resistance, chemical resistance, etc., it is preferable to use polyvinyl chloride as the amorphous resin having a glass transition temperature of 50° C. or higher.
[0038] The resin may be foamed, that is, the predetermined resin layer may be a foamed resin film (sheet). The above-mentioned predetermined resin layer does not usually contain an acrylic resin foam constituting the self-adhesive foam sheet.
[0039] The method for producing the resin film (sheet) is not particularly limited, and a known method can be adopted. For example, the resin layer composition containing the resin or a foam thereof is coated on a release sheet (such as a release-resistant processing paper) and molded into a sheet, then heated and dried to form a resin layer directly on the release sheet, and the release sheet is peeled off from the obtained laminate, thereby obtaining the resin layer alone (as an independent film (sheet)). Alternatively, when the substrate includes the nonwoven fabric layer and / or the aluminum layer, the resin layer (film) may be obtained by coating the resin layer composition containing the resin or a foam thereof on the nonwoven fabric layer or aluminum layer, molding it into a sheet, and then heating and drying it. Here, other components (components other than resin) that the resin layer composition may contain, the preparation method and coating method of the resin layer composition, and the foaming method of the resin and the crosslinking method of the foam, etc. are not particularly limited, and the same ones as those described in the sections "Composition for self-adhesive foam sheet" and "Production of self-adhesive foam sheet and self-adhesive laminate" described below can be used.
[0040] <<Aluminum layer>> The aluminum layer is a film (sheet) made of aluminum. Aluminum is a material that is resistant to dimensional changes due to moisture absorption, is lightweight, and has excellent heat insulating properties. Therefore, the aluminum layer can improve moisture resistance while suppressing weight increase and improving heat insulating properties.
[0041] The method for producing the aluminum film (sheet) is not particularly limited, and the aluminum film (sheet) can be formed by a known method. When the substrate has the above-mentioned predetermined resin layer, the aluminum layer may be formed by forming an aluminum film on the predetermined resin layer by a vapor deposition method.
[0042] <<Other layers>> The other layers that the substrate may contain are not particularly limited, but may include a metal layer other than aluminum, a glass layer, and the like.
[0043] The average thickness of the other layers is not particularly limited, but is preferably 10 μm or more, more preferably 50 μm or more, and more preferably 500 μm or less.
[0044] The other layers are not particularly limited, and can be provided on the layer made of a predetermined material by a known method.
[0045] The method for integrating the layer made of the above-mentioned specific material with the other layer is not particularly limited, and can be carried out using known techniques such as the use of adhesives, fusion bonding, and pressure bonding.
[0046] <<Average thickness of substrate>> The average thickness of the substrate is not particularly limited, but is preferably 50 μm or more, more preferably 100 μm or more, even more preferably 130 μm or more, and is preferably 1000 μm or less. If the average thickness of the substrate is 50 μm or more, the moisture resistance of the laminate can be further improved, and when the substrate includes a nonwoven fabric layer, and a foamed sheet formed from a foamed sheet composition described later or a resin composition for forming the above-mentioned specified resin layer is coated on the nonwoven fabric layer, strike-through can be effectively suppressed. In addition, if the average thickness of the substrate is 1000 μm or less, deterioration of heat transmission during heating and drying when preparing a foamed sheet can be suppressed, and the foamed sheet can be sufficiently dried.
[0047] <<Basis weight of substrate>> The basis weight of the substrate is not particularly limited, but is preferably 10 g / m 2 It is preferable that the thickness is 20 g / m or more. 2 More preferably, it is 500 g / m or more. 2 It is preferable that the thickness is less than 400 g / m 2It is more preferable that the basis weight of the substrate is 10 g / m or less. 2 If the basis weight of the substrate is 500 g / m or more, the strength of the laminate can be increased. 2 If it is below this value, the increase in the weight can be suppressed and workability can be improved.
[0048] The substrate may be manufactured as required, or a commercially available product may be used. Commercially available nonwoven fabric products that can be used as the substrate include, for example, "315TH-140" and "05-TH-20" manufactured by Teijin Frontier Co., Ltd. In addition, a commercially available substrate having a nonwoven fabric layer and a resin layer includes, for example, fleece (nonwoven fabric) wallpaper such as "FW-01" manufactured by Asahipen Co., Ltd.
[0049] (Self-adhesive foam sheet composition) The foam sheet composition of the present invention contains an acrylic resin and a crosslinking agent, and optionally further contains at least one selected from the group consisting of a foam stabilizer, a solvent, and other additives. The foam sheet composition of the present invention can be suitably used for forming an acrylic resin foam as a foam sheet constituting the laminate of the present invention described above.
[0050] <Acrylic resin> Acrylic resin is a polymer containing (meth)acrylate monomer units and has a tensile modulus of 0.30 N / mm 2 The breaking elongation must be 500% or more. In this specification, the term "(meth)acrylate" means acrylate and / or methacrylate.
[0051] <<Composition>> The polymer constituting the acrylic resin contains (meth)acrylate monomer units as described above, and optionally further contains other monomer units.
[0052] Here, the (meth)acrylate monomer unit is a repeating unit derived from a (meth)acrylate monomer. The (meth)acrylate monomer is not particularly limited, but examples thereof include (meth)acrylic acid alkyl ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, n-heptyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-dodecyl (meth)acrylate; (meth)acrylic acid alkoxyalkyl ester monomers such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, and ethoxymethyl (meth)acrylate; and the like. These may be used alone or in combination of two or more. Among these, from the viewpoint of controlling the peeling forces P1 and P2, and |P1-P2| of the foam sheet within a predetermined range and efficiently obtaining a laminate that exhibits a good balance of moderate adhesion to both PVC wallpaper and water-repellent wallpaper, it is preferable to use at least one of 2-ethylhexyl acrylate and methyl methacrylate as the (meth)acrylate monomer, more preferably to use at least 2-ethylhexyl acrylate, and even more preferably to use both 2-ethylhexyl acrylate and methyl methacrylate. In other words, the acrylic resin is preferably a polymer containing at least one of 2-ethylhexyl acrylate units and methyl methacrylate units, more preferably a polymer containing at least 2-ethylhexyl acrylate units, and even more preferably a polymer containing both 2-ethylhexyl acrylate units and methyl methacrylate units. In this specification, "(meth)acrylic" means acrylic and / or methacrylic.
[0053] From the viewpoint of controlling the peel strengths P1 and P2, and |P1-P2| of the foam sheet within specified ranges and efficiently obtaining a laminate that exhibits appropriate adhesion to both PVC wallpaper and water-repellent wallpaper in a well-balanced manner, the proportion of (meth)acrylate monomer units in the polymer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, particularly preferably 90% by mass or more, and is preferably 100% by mass or less, and 99% by mass or less, assuming that all repeating units (total monomer units) contained in the polymer are 100% by mass. Furthermore, when the polymer contains 2-ethylhexyl acrylate units, from the viewpoint of controlling the peel strengths P1 and P2, and |P1-P2| of the foam sheet within predetermined ranges and efficiently obtaining a laminate that exhibits appropriate adhesion to both PVC wallpaper and water-repellent wallpaper in a well-balanced manner, the proportion of 2-ethylhexyl acrylate units in the polymer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, particularly preferably 85% by mass or more, and can be 100% by mass or less, preferably 98% by mass or less, more preferably 95% by mass or less, even more preferably 92% by mass or less, and even more preferably 88% by mass or less, based on 100% by mass of all repeating units (total monomer units) contained in the polymer. When the polymer contains methyl methacrylate units, from the viewpoint of controlling the peel strengths P1 and P2, and |P1-P2| of the foam sheet within predetermined ranges and efficiently obtaining a laminate that exhibits appropriate adhesion to both PVC wallpaper and water-repellent wallpaper in a well-balanced manner, the proportion of methyl methacrylate units in the polymer is preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 5% by mass or more, even more preferably 7% by mass or more, particularly preferably 9% by mass or more, and can be 30% by mass or less, preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on 100% by mass of all repeating units (total monomer units) contained in the polymer.
[0054] The other monomer units are not particularly limited, and examples thereof include the monomer units described in International Publication No. 2018 / 151274. Specifically, the other monomer units are not particularly limited, and examples thereof include unsaturated carboxylic acid monomer units, vinyl cyanide monomer units, and alkenyl aromatic monomer units. Among these, the unsaturated carboxylic acid monomer unit is preferred from the viewpoint of forming a crosslinked structure using a crosslinking agent described below. Here, the unsaturated carboxylic acid monomer unit is a repeating unit derived from an unsaturated carboxylic acid monomer. The unsaturated carboxylic acid monomer is not particularly limited, but examples thereof include acrylic acid, methacrylic acid, itaconic acid, and the like. These can be used alone or in combination of two or more. Among these, acrylic acid is preferred as the unsaturated carboxylic acid monomer from the viewpoint of efficiently obtaining a laminate that exhibits a good balance of appropriate adhesion to both PVC wallpaper and water-repellent wallpaper by controlling the peeling forces P1 and P2 and |P1-P2| of the foamed sheet within a predetermined range. In other words, the acrylic resin is preferably a polymer containing an acrylic acid unit. When the polymer contains unsaturated carboxylic acid monomer units, from the viewpoint of controlling the peel strengths P1 and P2, and |P1-P2| of the foam sheet within predetermined ranges and efficiently obtaining a laminate that exhibits appropriate adhesion to both PVC wallpaper and water-repellent wallpaper in a well-balanced manner, the proportion of unsaturated carboxylic acid monomer units in the polymer is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, preferably 5% by mass or less, more preferably 4% by mass or less, even more preferably 3% by mass or less, and particularly preferably 2% by mass or less, based on 100% by mass of all repeating units (total monomer units) contained in the polymer.
[0055] <<Tensile modulus>> The tensile modulus of the acrylic resin is 0.30 N / mm 2 It must be less than 0.25N / mm 2 It is preferable that the resistance is less than 0.20 N / mm 2 More preferably, it is 0.10 N / mm 2 More preferably, it is 0.05 N / mm 2 It is even more preferable that the tensile modulus of the acrylic resin is 0.30 N / mm 2 If the tensile modulus of the acrylic resin exceeds 0.30 N / mm, the peel strength P2 of the foam sheet decreases and |P1-P2| increases, making it impossible to efficiently obtain a laminate that exhibits a good balance of appropriate adhesion to both the PVC wallpaper and the water-repellent wallpaper. 2 If the peel strength P2 of the foam sheet is increased while |P1-P2| is decreased, a laminate exhibiting a good balance of appropriate adhesion to both PVC wallpaper and water-repellent wallpaper can be efficiently obtained. The lower limit of the tensile modulus of elasticity of the acrylic resin is not particularly limited, but is, for example, 0.001 N / mm 2 It can be more than that. The tensile modulus of the acrylic resin can be controlled by adjusting the composition of the polymer constituting the acrylic resin and the polymerization conditions.
[0056] <<Elongation at break>> The acrylic resin preferably has a breaking elongation of 500% or more, more preferably 550% or more, even more preferably 600% or more, even more preferably 650% or more, and particularly preferably 700% or more. If the breaking elongation of the acrylic resin is less than 500%, the peeling forces P1 and P2 of the foamed sheet are reduced, and a laminate exhibiting a suitable adhesion to both PVC wallpaper and water-repellent wallpaper in a well-balanced manner cannot be efficiently obtained. In other words, if the breaking elongation of the acrylic resin is 500% or more, the peeling forces P1 and P2 of the foamed sheet can be increased to efficiently obtain a laminate exhibiting a suitable adhesion to both PVC wallpaper and water-repellent wallpaper in a well-balanced manner. The upper limit of the breaking elongation of the acrylic resin is not particularly limited, but can be, for example, 1500% or less. The breaking elongation of the acrylic resin can be controlled by adjusting the composition of the polymer constituting the acrylic resin and the polymerization conditions.
[0057] <Crosslinking agent> The crosslinking agent contained in the composition for foaming sheet is not particularly limited as long as it can crosslink the acrylic resin, and examples thereof include epoxy-based crosslinking agents, carbodiimide-based crosslinking agents, oxazoline-based crosslinking agents, polyfunctional isocyanate-based crosslinking agents such as tolylene diisocyanate, trimethylolpropane tolylene diisocyanate, and diphenylmethane triisocyanate, metal salt-based crosslinking agents, metal chelate-based crosslinking agents, and peroxide-based crosslinking agents. These may be used alone or in combination of two or more. Among these, carbodiimide-based crosslinking agents and oxazoline-based crosslinking agents are preferred from the viewpoint of efficiently obtaining a laminate that exhibits a good balance of appropriate adhesion to both PVC wallpaper and water-repellent wallpaper by controlling the peeling forces P1 and P2, and |P1-P2| of the foaming sheet within a predetermined range.
[0058] As the carbodiimide crosslinking agent, a compound having two or more carbodiimide groups in one molecule is preferably used. The carbodiimide crosslinking agent may be synthesized, or a commercially available product may be used. Examples of commercially available carbodiimide crosslinking agents include "DICNAL (registered trademark) HX" manufactured by DIC Corporation and "Carbodilite (registered trademark)" manufactured by Nisshinbo Chemical Co., Ltd. As the oxazoline crosslinking agent, a compound having two or more oxazoline groups in one molecule is preferably used. The oxazoline crosslinking agent may be synthesized, or a commercially available product may be used. Examples of commercially available oxazoline crosslinking agents include "Epocross WS-300", "Epocross WS-500", and "Epocross WS-700" manufactured by Nippon Shokubai Co., Ltd.
[0059] The content of the crosslinking agent in the composition for foamed sheet is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and preferably 3 parts by mass or less, more preferably 2 parts by mass or less, even more preferably 1.5 parts by mass or less, and particularly preferably 1.3 parts by mass or less, per 100 parts by mass of the acrylic resin. If a foamed sheet is formed using a composition for foamed sheet in which the content of the crosslinking agent is within the above-mentioned range, there is an advantage that the peel forces P1 and P2, and |P1-P2| can be easily controlled within a predetermined range. In addition, a foamed sheet having excellent strength and flexibility can be obtained.
[0060] <Foam stabilizer> The foam stabilizer that may be optionally contained in the composition for a foam sheet may be a known foam stabilizer such as a higher fatty acid salt or a surfactant. The foam stabilizer may remain in the acrylic resin foam formed using the composition for a foam sheet. The content of the foam stabilizer in the foam sheet composition is not particularly limited and can be from 0.1 to 20 parts by mass per 100 parts by mass of the acrylic resin. If the amount of the foam stabilizer is within the above range, an acrylic resin foam having a good open-cell structure can be obtained.
[0061] <Solvent> The solvent that the foam sheet composition may optionally contain is not particularly limited, and examples thereof include water and organic solvents, with water being preferred.
[0062] <Other additives> Examples of other additives that may be optionally contained in the foam sheet composition include foaming aids, thickeners, thickening aids, fillers, preservatives, fungicides, gelling agents, flame retardants, antioxidants, antioxidants, pigments, dyes, tackifiers, conductive compounds, water-resistant agents, oil-resistant agents, etc. The above-mentioned other additives are not particularly limited, and known additives, such as those described in International Publication No. 2016 / 147679, can be used.
[0063] (Manufacture of self-adhesive foam sheets and self-adhesive laminates) The method for producing a foamed sheet (acrylic resin foam) provided in the laminate of the present invention using the above-mentioned foamed sheet composition of the present invention is not particularly limited, and can be performed, for example, by foaming a prepared foamed sheet composition to obtain a foam in an uncured (uncrosslinked) state, molding the foam into a sheet, and curing (crosslinking reaction) as necessary.
[0064] Here, the foam sheet composition can be prepared by mixing the above-mentioned components in any method and order. For example, when an acrylic resin latex is used to prepare the foam sheet composition, a crosslinking agent, and if necessary, a foam stabilizer and other additives, etc., can be added to the latex and mixed by a known method. When a solid acrylic resin is used without using a solvent to prepare the foam sheet composition, a solid acrylic resin, a crosslinking agent, and if necessary, a foam stabilizer and other additives, etc. can be mixed by a known method (for example, using a known roll, Henschel mixer, kneader, etc.).
[0065] The viscosity of the foam sheet composition containing a solvent (for example, in the form of an emulsion or dispersion) is preferably 1,000 mPa·s or more, more preferably 2,000 mPa·s or more, even more preferably 3,500 mPa·s or more, and preferably 10,000 mPa·s or less, more preferably 5,500 mPa·s or less. If the viscosity of the foam sheet composition is 1,000 mPa·s or more, it is possible to prevent dripping that makes it difficult to control the thickness when coating a foam formed from the foam sheet composition on a substrate or a release sheet (such as release-resistant processing paper). On the other hand, if the viscosity of the foam sheet composition is 10,000 mPa·s or less, it is also possible to prevent difficulty in controlling the expansion ratio by mechanical foaming when forming a foam sheet. The viscosity of the foam sheet composition can be measured at a temperature of 23° C. using a Brookfield type viscometer.
[0066] In addition, as a method for foaming the composition for foaming sheet, it is preferable to adopt mechanical foaming from the viewpoint of obtaining a foamed sheet having excellent flexibility. The foaming ratio may be appropriately adjusted, but is preferably 1.5 times or more, more preferably 1.6 times or more, and is also preferably 2.2 times or less, more preferably 2.0 times or less. If the foaming ratio is 1.5 times or more, a foamed sheet having excellent unevenness-following ability during attachment and long-term adhesion stability can be obtained. If the foaming ratio is 2.2 times or less, the occurrence of resin residue on the adherend surface during peeling can be suppressed.
[0067] The mechanical foaming can be carried out by, but not limited to, mixing a certain amount of air into the emulsion or dispersion of the foamed sheet composition and stirring continuously or batchwise with an oak mixer, whipper, etc. The foam thus obtained (foamed emulsion or foamed dispersion) is creamy.
[0068] Furthermore, the method of forming the foam into a sheet is not particularly limited. A suitable method is, for example, a method of coating the foam onto the above-mentioned substrate having a nonwoven fabric layer, a specific resin layer, or an aluminum layer, and forming it into a sheet. In this way, by coating the foam onto the substrate and allowing the crosslinking reaction to proceed, a laminate in which the foam sheet is provided directly on the substrate can be obtained.
[0069] The foam coating can also be performed on a release sheet instead of the above-mentioned substrate. If the foam is coated on the release sheet and the crosslinking reaction is allowed to proceed, a laminate in which the foam sheet is provided directly on the release sheet can be obtained. Then, by peeling the release sheet from the foam sheet of this laminate, the foam sheet can be obtained alone (as an independent film).
[0070] As a method for coating the foam onto a substrate or a release sheet (hereinafter, these may be collectively referred to as "substrate, etc."), a commonly known coating device such as an applicator, a bar coater, a roll coater, a reverse roll coater, a screen coater, a doctor knife coater, or a comma knife coater can be used.
[0071] A method for crosslinking a foam molded into a sheet is preferably a method for heating and drying the foam. The method for heating and drying is not particularly limited as long as it is a method capable of drying and crosslinking a foam molded into a sheet, and a known drying oven (for example, a hot air circulation type oven, a hot oil circulation hot air chamber, a far infrared heater chamber) can be used. The drying temperature can be, for example, 60°C or higher and 180°C or lower. It is preferable to perform multi-stage drying such that drying is performed from the inside at a low temperature in the early stage of drying and is sufficiently dried at a higher temperature in the later stage of drying, rather than performing drying at a constant temperature.
[0072] The laminate of the foamed sheet and the substrate or the like obtained as described above is not particularly limited, but for example, after a separator film is attached to the self-adhesive surface, the laminate can be wound up by a winder and cut to an easy-to-use size by a press cutter, a slitter, or the like.
[0073] When the foamed sheet made of the above-mentioned acrylic resin foam is formed on a substrate, the obtained laminate can be used as the laminate of the present invention as it is or after being processed, such as cut, as necessary. In addition, when the foamed sheet made of the above-mentioned acrylic resin foam is molded on a release sheet, the foamed sheet peeled off from the release sheet can be laminated and integrated with a substrate to obtain the laminate of the present invention. Here, the foamed sheet and the substrate can be integrated by a known method such as the use of an adhesive, fusion bonding, or pressure bonding.
[0074] (Applications of self-adhesive laminates) The substrate surface of the laminate of the present invention may be subjected to printing, for example, by offset printing, seal printing, flexographic printing, silk screen printing, gravure printing, a laser printer, a thermal transfer printer, an inkjet printer, etc. In addition, the substrate of the laminate of the present invention may be decorated. The laminate of the present invention can be advantageously used as a sheet to be attached to a surface to be adhered, for example, as wallpaper to be applied over wallpaper, without any particular limitation. EXAMPLES
[0075] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, the units "%" and "parts" expressing amounts are by mass unless otherwise specified. In the examples and comparative examples, the glass transition temperature, tensile modulus and breaking elongation of the acrylic resin, the tensile modulus and breaking elongation of the foamed sheet, the peeling force P1 from PVC wallpaper, the peeling force P2 from water-repellent wallpaper, and |P1-P2| were measured or evaluated by the following methods.
[0076] <Glass transition temperature of acrylic resin> The measurement was performed using a differential scanning calorimeter in accordance with JIS K7121 under conditions of a measurement temperature of -50°C to 160°C and a temperature rise rate of 10°C / min. <Tensile modulus of acrylic resin> The acrylic resin alone was dried at 23°C for 78 hours to obtain a test resin sheet with a thickness of 1 mm. This test resin sheet was cut into a JIS K 7113:1995 No. 2 shape, and a tensile test was carried out using an autograph (Shimadzu Corporation, "AG-IS") at a tensile speed of 200 mm / min and a gripper distance of 40 mm according to the test method of JIS K 7113:1995 to measure stress. The tensile modulus E was calculated using the following formula: m (N / mm 2 ) was calculated. E m =Δσ / Δε=(σ 25% -σ 5% ) / (0.25-0.05) Δδ: Stress difference between two points on a line due to the original average cross-sectional area Δε: Difference in strain between the same two points as above The stress at the two points is the stress at 5% elongation (σ 5% ), stress at 25% elongation (σ 25% ) was used. <Breaking elongation of acrylic resin> A tensile test was carried out in the same manner as in the above "Tensile modulus of acrylic resin" to break the test resin sheet. The breaking elongation l (%) was calculated by the following formula using the sheet length L (=distance between grippers, unit: mm) when the test resin sheet broke and the initial sheet length L0 (=distance between grippers, 40 mm) before the tensile test. l=(L-L0) / L0×100=(L-40) / 40×100 <Tensile modulus of foam sheet> In each of the examples and comparative examples, a foamed sheet composition and a laminate were produced in the same procedure as in the corresponding example or comparative example, except that a release sheet (manufactured by Mitsui Chemicals Toagosei Co., Ltd., "SP-PET-O1-BU", average thickness: 100 μm) was used as the base material. Subsequently, the release sheet was peeled off from the foamed sheet of the laminate, and the foamed sheet was cut into a No. 2 shape according to JIS K 7113:1995 to obtain a test foamed sheet. For the obtained test foamed sheet, using an autograph (manufactured by Shimadzu Corporation, "AG-IS"), with a tensile speed of 200 mm / min and a grip distance of 40 mm, a tensile test was carried out according to the test method of JIS K 7113:1995, and the stress was measured. Then, the tensile modulus of elasticity E m (N / mm 2 ) was calculated. E m =Δσ / Δε=(σ 25% -σ 5% ) / (0.25 - 0.05) Δδ: Stress difference based on the original average cross-sectional area between two points on the straight line Δε: Strain difference between the same two points Note that the stresses at the two points are the stress at 5% elongation (σ 5% ), and the stress at 25% elongation (σ 25% ) were used. <Elongation at break of the foamed sheet> In each of the examples and comparative examples, a foamed sheet composition and a laminate were produced in the same procedure as in the corresponding example or comparative example, except that a release sheet (manufactured by Mitsui Chemicals Toagosei Co., Ltd., "SP-PET-O1-BU", average thickness: 100 μm) was used as the base material. Subsequently, the release sheet was peeled off from the foamed sheet of the laminate, and the foamed sheet was cut into a No. 2 shape according to JIS K 7113:1995 to obtain a test foamed sheet. A tensile test was carried out in the same manner as the above "tensile modulus of elasticity of the foamed sheet", and the test foamed sheet was broken. Using the sheet length L (= grip distance, unit: mm) at the time of breakage of the test foamed sheet and the initial sheet length L0 (= grip distance, 40 mm) before the tensile test, the elongation at break l (%) was calculated by the following formula. l=(L - L0) / L0×100=(L - 40) / 40×100 <Peeling force P1 for PVC wallpaper> The prepared laminate was cut into a size of 125 mm x 25 mm to prepare a test piece. Next, the PVC wallpaper cut into a size of 125 mm x 50 mm was attached to an aluminum plate of the same size with double-sided tape to prepare an adherend. The foam sheet side of the test piece was attached to the PVC wallpaper side of the adherend, and the test piece was pressed with a roller under a load of 2 kgf from above, and left for 1 hour under an environment of 23 ° C and 50% RH. Then, the end of the test piece was fixed to the upper chuck of an autograph (manufactured by Shimadzu Corporation, "AG-IS"), the adherend was fixed to the lower chuck, and a 180-degree peel test was performed at a speed of 300 mm / min under an environment of 23 ° C and 50% RH. The peel force (N / mm) at this time was taken as the peel force P1 for the PVC wallpaper. -PVC wallpaper- The following PVC wallpaper was used to measure the peel strength P1. Product name: LB9233 (manufactured by Lilycolor) Material: Polyvinyl chloride Furthermore, when the shape of the PVC wallpaper was measured with a one-shot 3D shape measuring machine (Keyence, "VR-3100"), the arithmetic mean height Sa was 0.1 mm, the maximum height Sz was 0.8 mm, and when the plane passing through the most protruding part was taken as the reference plane, the proportion of the area contained within a range of -100 μm from the reference plane was 35.8%. <Peeling power against water-repellent wallpaper P2> The prepared laminate was cut into a size of 125 mm x 25 mm to prepare a test piece. Next, the water-repellent wallpaper cut into a size of 125 mm x 50 mm was attached to an aluminum plate of the same size with double-sided tape to prepare an adherend. The foam sheet side of the test piece was attached to the water-repellent wallpaper side of the adherend, and the test piece was pressed with a roller under a load of 2 kgf from above, and left for 1 hour under an environment of 23 ° C and 50% RH. Then, the end of the test piece was fixed to the upper chuck of an autograph (manufactured by Shimadzu Corporation, "AG-IS"), the adherend was fixed to the lower chuck, and a 180-degree peel test was performed at a speed of 300 mm / min under an environment of 23 ° C and 50% RH. The peel force (N / mm) at this time was taken as the peel force P2 for the water-repellent wallpaper. -Water-repellent wallpaper- The following water-repellent wallpaper was used to measure the peel strength P2. Product name: LV3453 (manufactured by Lilycolor) Material: Polyvinyl chloride (water-repellent top coat) In addition, when the shape of the water-repellent wallpaper was measured using a one-shot 3D shape measuring machine (Keyence, "VR-3100"), the arithmetic mean height Sa was 0.1 mm, the maximum height Sz was 0.6 mm, and when the plane passing through the most protruding part was taken as the reference plane, the proportion of the area contained within a range of -100 μm from the reference plane was 66.0%. <Foam sheet |P1-P2|> The peeling forces P1 and P2 obtained in the above measurements were used to calculate the absolute value of the difference therebetween.
[0077] Example 1 <Preparation of Polymer A> 27.0 parts of deionized water were mixed with 100 parts of a monomer mixture consisting of 86.6 parts of 2-ethylhexyl acrylate, 11.8 parts of methyl methacrylate, and 1.6 parts of acrylic acid, and 0.4 parts of sodium polyoxyethylene alkyl sulfate (Kao Corporation: Latemul E-118B) and stirred to obtain a monomer emulsion. Next, a glass reaction vessel equipped with a reflux condenser, a dropping funnel, a thermometer, a nitrogen inlet, and a stirrer was prepared separately from the above, and 43.0 parts of deionized water and 0.2 parts of sodium polyoxyethylene alkyl sulfate were placed in this glass reaction vessel, and the temperature was raised to 80°C while stirring. Then, while maintaining the temperature at 80°C, 0.3 parts of ammonium persulfate dissolved in 5.7 parts of deionized water was added, and then the monomer emulsion obtained above was gradually added over 4 hours. After the addition was completed, stirring was continued for another 4 hours, and then the reaction was terminated by cooling to obtain a reaction mixture. The polymerization conversion rate at this time was almost 100% (98% or more), and the resulting reaction mixture was adjusted to pH 7.5 with 5% ammonia water, and 2.5 parts of polyoxyethylene lauryl ether (Kao Corporation: Emulgen 120) was added, followed by concentration to obtain a polymer latex with a solid content concentration of 60.2%. The polymer A (acrylic resin) contained in the obtained polymer latex contained 86.6% 2-ethylhexyl acrylate units, 11.8% methyl methacrylate units, and 1.6% acrylic acid units. The glass transition temperature, tensile modulus, and breaking elongation of the polymer A were measured. The results are shown in Table 1. <Preparation of foam sheet composition> In a mixing vessel, 100 parts of the polymer latex containing polymer A, 1 part of a carbodiimide-based crosslinking agent (crosslinking agent, manufactured by Nisshinbo Chemical Co., Ltd., "Carbodilite E-02"), and 3.5 parts of titanium oxide water dispersion (pigment, manufactured by DIC Corporation, DISPERSE WHITE HG-701) were added and stirred with a disperser. Next, while continuing to stir, 6 parts of a foam stabilizer [a 1 / 1 mixture of an alkyl betaine amphoteric acid / fatty acid alkanolamide mixture (manufactured by DIC Corporation, DICNAL M-20) / sulfonic acid type anionic surfactant (manufactured by DIC Corporation, DICNAL M-40)] and 0.6 parts of 28% ammonia water as a thickening aid were added in this order, and the mixture was filtered through a 150 mesh. Finally, 1 part of a thickener (carboxylic acid modified acrylic acid ester polymer, manufactured by Toagosei Co., Ltd., Aron B-300K) was added to adjust the viscosity to 4,500 mPa·s, and a composition for foam sheets was obtained. <Preparation of Laminate> The composition for a foamed sheet obtained as described above was stirred with a whisk until the foaming ratio reached 1.8 times, and the stirring speed was further reduced and stirring was continued for 5 minutes. The foamed foam sheet composition (foam) was coated on a nonwoven fabric layer of a substrate (manufactured by Asahipen Co., Ltd., "FW-01"; substrate consisting of a nonwoven fabric layer made of pulp and polyester fibers and a foamed polyvinyl chloride resin layer, average thickness: 468 μm) using an applicator. This was placed in a drying oven and held at 100°C for 1.33 minutes, 120°C for 1.33 minutes, and 130°C for 1.33 minutes to perform drying and crosslinking, thereby obtaining a laminate comprising a foam sheet on the substrate. The average thickness of the foam sheet was 200 μm. The foamed sheet was evaluated for tensile modulus, breaking elongation, peel strength P1 and P2, and |P1-P2| using the obtained laminate. The results are shown in Table 1.
[0078] Example 2 In preparing the composition for a foam sheet, except that the amount of the carbodiimide-based crosslinking agent was changed from 1 part to 1.5 parts in terms of solid content, polymer A, the composition for a foam sheet, and the laminate were prepared in the same manner as in Example 1, and various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.
[0079] Comparative Example 1 Polymer B (acrylic resin), a foam sheet composition and a laminate were prepared as described below, and various evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1. <Preparation of Polymer B> 27.0 parts of deionized water was mixed with 100 parts of a monomer mixture consisting of 36.9 parts of 2-ethylhexyl acrylate, 60.0 parts of n-butyl acrylate, 0.5 parts of acrylonitrile, and 2.6 parts of acrylic acid, and 0.8 parts of sodium dodecylbenzenesulfonate (Kao Corporation: Neopelex G-15) and stirred to obtain a monomer emulsion. Next, a glass reaction vessel equipped with a reflux condenser, a dropping funnel, a thermometer, a nitrogen inlet, and a stirrer was prepared separately from the above, and 43.0 parts of deionized water and 0.4 parts of sodium dodecylbenzenesulfonate were placed in this glass reaction vessel, and the temperature was raised to 80°C while stirring. Then, while maintaining the temperature at 80°C, 0.3 parts of ammonium persulfate dissolved in 5.7 parts of deionized water was added, and then the monomer emulsion obtained above was gradually added over 4 hours. After the addition was completed, stirring was continued for another 4 hours, and then the reaction was terminated by cooling to obtain a reaction mixture. The polymerization conversion rate at this time was almost 100% (98% or more), and the resulting reaction mixture was adjusted to pH 8.9 with 5% ammonia water, and 0.3 parts of sodium lauryl sulfate (Kao Corporation: EMALE 2F paste) was added, followed by concentration to obtain a polymer latex with a solid content concentration of 56%. Polymer B (acrylic resin) contained in the obtained polymer latex contained 36.9% of 2-ethylhexyl acrylate units, 60.0% of n-butyl acrylate units, 0.5% of acrylonitrile units, and 2.6% of acrylic acid units. <Preparation of foam sheet composition> In a mixing vessel, 100 parts of the polymer latex containing polymer B, 1 part of an epoxy-based crosslinking agent (crosslinking agent, manufactured by Japan Coating Resins Co., Ltd., product name "Rikabond EX-8"), and 3.5 parts of titanium oxide water dispersion (pigment, manufactured by DIC Corporation, DISPERSE WHITE HG-701) were added and stirred with a disperser. Next, while continuing to stir, 4 parts of a foam stabilizer [ammonium stearate, manufactured by San Nopco Ltd., product name "Nopco DC-100A)] were added, and the mixture was filtered through a 150 mesh to obtain a foam sheet composition with a viscosity of 4,000 mPa s. <Preparation of Laminate> The composition for a foamed sheet obtained as described above was stirred with a whisk until the foaming ratio reached 1.8 times, and the stirring speed was further reduced and stirring was continued for 5 minutes. The foamed foam sheet composition (foam) was coated on a nonwoven fabric layer of a substrate (manufactured by Asahipen Co., Ltd., "FW-01"; substrate consisting of a nonwoven fabric layer made of pulp and polyester fibers and a foamed polyvinyl chloride resin layer, average thickness: 468 μm) using an applicator. This was placed in a drying oven and held at 80°C for 1.33 minutes, 120°C for 1.33 minutes, and 140°C for 1.33 minutes to perform drying and crosslinking, thereby obtaining a laminate comprising a foam sheet on the substrate. The average thickness of the foam sheet was 200 μm.
[0080] Comparative Example 2 Polymer C (acrylic resin), a foam sheet composition and a laminate were prepared as described below, and various evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1. <Preparation of Polymer C> 27.0 parts of deionized water was mixed with 100 parts of a monomer mixture consisting of 84.4 parts of n-butyl acrylate, 7.1 parts of n-butyl methacrylate, 0.8 parts of acrylonitrile, 2.2 parts of 2-ethylhexyl acrylate, 3.6 parts of methyl methacrylate, and 1.9 parts of acrylic acid, and 0.4 parts of sodium polyoxyethylene alkyl sulfate (Kao Corporation: Latemul E-118B) and stirred to obtain a monomer emulsion. Next, a glass reaction vessel equipped with a reflux condenser, a dropping funnel, a thermometer, a nitrogen inlet, and a stirrer was prepared separately from the above, and 43.0 parts of deionized water and 0.2 parts of sodium polyoxyethylene alkyl sulfate were placed in this glass reaction vessel, and the temperature was raised to 80°C while stirring. Then, while maintaining the temperature at 80°C, 0.3 parts of ammonium persulfate dissolved in 5.7 parts of deionized water was added, and then the monomer emulsion obtained above was gradually added over 4 hours. After the addition was completed, stirring was continued for another 4 hours, and then the reaction was terminated by cooling to obtain a reaction mixture. The polymerization conversion rate at this time was almost 100% (98% or more), and the resulting reaction mixture was adjusted to pH 5.5 with 5% ammonia water, and 1.0 part of polyoxyethylene lauryl ether (Kao Corporation: Emulgen 120) was added, followed by concentration to obtain a polymer latex with a solid content concentration of 53%. Polymer C (acrylic resin) contained in the obtained polymer latex contained 84.4% n-butyl acrylate units, 7.1% n-butyl methacrylate units, 0.8% acrylonitrile units, 2.2% 2-ethylhexyl acrylate units, 3.6% methyl methacrylate units, and 1.9% acrylic acid units. <Preparation of foam sheet composition> In a mixing vessel, 100 parts of the polymer latex containing polymer C, 1 part of a carbodiimide-based crosslinking agent (crosslinking agent, manufactured by Nisshinbo Chemical Co., Ltd., "Carbodilite E-02"), and 3.5 parts of titanium oxide water dispersion (pigment, manufactured by DIC Corporation, DISPERSE WHITE HG-701) were added and stirred with a disperser. Next, while continuing to stir, 6 parts of a foam stabilizer [a 1 / 1 mixture of an alkyl betaine amphoteric acid-fatty acid alkanolamide mixture (manufactured by DIC Corporation, DICNAL M-20) / sulfonic acid type anionic surfactant (manufactured by DIC Corporation, DICNAL M-40)] and 0.6 parts of 28% ammonia water as a thickening aid were added in this order, and the mixture was filtered through a 150 mesh. Finally, 4 parts of a thickener (carboxylic acid-modified acrylic acid ester polymer, manufactured by Toagosei Co., Ltd., Aron B-300K) were added to adjust the viscosity to 4,500 mPa·s, and a composition for foam sheets was obtained. <Preparation of Laminate> The composition for a foamed sheet obtained as described above was stirred with a whisk until the foaming ratio reached 1.8 times, and the stirring speed was further reduced and stirring was continued for 5 minutes. The foamed foam sheet composition (foam) was coated on a nonwoven fabric layer of a substrate (manufactured by Asahipen Co., Ltd., "FW-01"; substrate consisting of a nonwoven fabric layer made of pulp and polyester fibers and a foamed polyvinyl chloride resin layer, average thickness: 468 μm) using an applicator. This was placed in a drying oven and held at 100°C for 1.33 minutes, 120°C for 1.33 minutes, and 130°C for 1.33 minutes to perform drying and crosslinking, thereby obtaining a laminate comprising a foam sheet on the substrate. The average thickness of the foam sheet was 200 μm.
[0081] [Table 1]
[0082] From Table 1, in Examples 1 and 2, the tensile modulus was 0.3 N / mm 2 It can be seen that by using a foam sheet composition containing an acrylic resin having a peel strength P1 or less and a breaking elongation of 500% or more, and a crosslinking agent, it is possible to obtain a foam sheet in which both the peel strength P1 and the peel strength P2 are 1.00 to 4.00 N / cm or less and |P1-P2| is less than 1.00 N / cm, and a laminate that exhibits appropriate adhesion in a good balance to both PVC wallpaper and water-repellent wallpaper can be obtained. [Industrial Applicability]
[0083] According to the present invention, it is possible to provide a self-adhesive laminate that exhibits a well-balanced and appropriate adhesion to both polyvinyl chloride wallpaper and water-repellent wallpaper. Furthermore, according to the present invention, it is possible to provide a composition for a self-adhesive foam sheet that can be used to prepare a self-adhesive laminate that exhibits a well-balanced and appropriate adhesion to both polyvinyl chloride wallpaper and water-repellent wallpaper.
Claims
1. A self-adhesive laminate comprising a substrate and a self-adhesive foam sheet made of an acrylic resin foam, The self-adhesive foam sheet is a self-adhesive laminate, in which both the peel strength P1 against polyvinyl chloride wallpaper and the peel strength P2 against water-repellent wallpaper are 1.00 N / cm or more and 4.00 N / cm or less, and the absolute value of the difference between the peel strength P1 and the peel strength P2 is less than 1.00 N / cm.
2. 2. The self-adhesive laminate of claim 1, wherein the self-adhesive foam sheet has an average thickness of more than 40 μm.
3. The self-adhesive foam sheet has a tensile modulus of 0.05 N / mm 2 3. The self-adhesive laminate according to claim 1, wherein the self-adhesive foam sheet has a breaking elongation of 300% or more.
4. A composition for a self-adhesive foam sheet, comprising an acrylic resin and a crosslinking agent, The acrylic resin has a tensile modulus of 0.30 N / mm 2 and the acrylic resin has a breaking elongation of 500% or more.
5. 5. The composition for a self-adhesive foam sheet according to claim 4, wherein the acrylic resin has a glass transition temperature of -40°C or lower.
6. 5. The composition for a self-adhesive foam sheet according to claim 4, wherein the content of the crosslinking agent is from 0.5 parts by mass to 3 parts by mass per 100 parts by mass of the acrylic resin.
7. 7. The composition for a self-adhesive foam sheet according to claim 4, wherein the acrylic resin is a polymer containing 2-ethylhexyl acrylate units in a proportion of 50% by mass or more.
Citation Information
Patent Citations
Wallpaper sheet
JP2020023156A