Polyurethane resin composition

The polyurethane resin composition addresses mechanical and hydrolysis issues by using a diol compound with a polylactone-polytrimethylene ether glycol A-B-A block copolymer and aromatic diisocyanate, enhancing tensile stress, abrasion resistance, and low-temperature flexibility.

JP2024142182APending Publication Date: 2024-10-10DAICEL CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023054228
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional polyurethane resin compositions using polyols like polypropylene glycol and polyester structures face issues with insufficient mechanical properties, abrasion resistance, and hydrolysis resistance, along with loss of flexibility at low temperatures.

Method used

A polyurethane resin composition incorporating a diol compound with an A-B-A block copolymer, where the A component is a polylactone chain and the B component is a polytrimethylene ether glycol chain, in a specific mass ratio, along with an aromatic diisocyanate and a chain extender, to enhance mechanical properties, hydrolysis resistance, and low-temperature flexibility.

Benefits of technology

The composition achieves improved tensile stress, abrasion resistance, and hydrolysis resistance while maintaining flexibility at low temperatures, with optimal ratios of ether and ester structures in the diol compound.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a polyurethane resin composition capable of forming a polyurethane resin that exhibits a combination of mechanical physical properties, hydrolysis resistance, and low-temperature flexibility.SOLUTION: A polyurethane resin composition disclosed herein includes: a urethane prepolymer which has a diol compound and an aromatic diisocyanate as constituent units; and a chain extender, wherein the diol compound contains a block copolymer of A-B-A. In the block copolymer, the component A is a polylactone chain and the component B is a polytrimethylene ether glycol chain. The content of the component A is 33-67 mass% relative to the total amount of the block copolymer of A-B-A.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a polyurethane resin composition. [Background technology]

[0002] Polyurethanes are typically block copolymers consisting of blocks of soft and hard segments, the soft segments being formed primarily from polyols and the hard segments being formed primarily from diisocyanates and chain extenders (it is believed that the hydroxyls at the ends of the polyols form part of the hard segments).

[0003] In particular, in conventional inventions, it is known to use polyether polyols such as polypropylene glycol, polytetramethylene ether glycol, and polytrimethylene ether glycol as the polyol used in the above polyurethane (for example, Patent Document 1).

[0004] Additionally, it is also known to use a compound containing a polyester structure as the polyol in order to improve mechanical properties such as tensile stress and abrasion resistance (for example, Non-Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-535733 A [Non-patent literature]

[0006] [Non-Patent Document 1] Mitsuo Akiba, "Deterioration and Stabilization of Polyurethane", Journal of the Adhesion Society of Japan, Vol. 40, No. 6, 2004, 241-252 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the polyurethane resin composition using the polyol described in Patent Document 1 has a problem that mechanical properties such as tensile stress and abrasion resistance are insufficient. In addition, the polyol described in Patent Document 1 precipitates at low temperatures, which causes a problem that the flexibility of the resin is impaired.

[0008] Furthermore, when the polyester structure described in Non-Patent Document 1 is contained, although the mechanical properties are improved, there is a problem with hydrolysis resistance.

[0009] Therefore, an object of the present disclosure is to provide a polyurethane resin composition capable of forming a polyurethane-based resin having excellent mechanical properties, hydrolysis resistance, and low-temperature flexibility. [Means for solving the problem]

[0010] As a result of earnest efforts made by the present inventors to solve the above problems, they have found that a polyurethane resin composition comprising a urethane prepolymer having a diol compound and an aromatic diisocyanate as structural units, and a chain extender, wherein the diol compound comprises an ABA block copolymer, the A component of the ABA block copolymer is a polylactone chain and the B component is a polytrimethylene ether glycol chain, and the content of the A component relative to the total amount of the ABA block copolymer is a specific ratio, provides mechanical properties, hydrolysis resistance, and low-temperature flexibility. The present disclosure relates to a polyurethane resin composition completed based on these findings.

[0011] That is, the present disclosure provides a polyurethane resin composition comprising a urethane prepolymer having a diol compound and an aromatic diisocyanate as constituent units, and a chain extender, wherein the diol compound comprises an ABA block copolymer, the ABA block copolymer has an A component being a polylactone chain and a B component being a polytrimethylene ether glycol chain, and the content of the A component relative to the total amount of the ABA block copolymer is 33 to 67 mass%.

[0012] The polyurethane resin composition contains a urethane prepolymer having a diol compound and an aromatic diisocyanate as constituent units, and a chain extender, the diol compound contains an ABA block copolymer, the ABA block copolymer having an A component as a polylactone chain and a B component as a polytrimethylene ether glycol chain, and the content of the A component relative to the total amount of the ABA block copolymer is 33 to 67 mass %, so that mechanical properties such as sufficient abrasion resistance and tensile stress can be obtained while exhibiting low-temperature flexibility and hydrolysis resistance.

[0013] The ABA block copolymer preferably has a number average molecular weight of 4,000 or less.

[0014] The polylactone chain is preferably a polycaprolactone chain, which makes it easier to improve mechanical properties.

[0015] The aromatic diisocyanate is preferably diphenylmethane diisocyanate.

[0016] Preferably, the chain extender is 1,4-butanediol.

[0017] The present disclosure also provides a polyurethane resin obtained by polymerizing the urethane prepolymer in the polyurethane resin composition and the chain extender. Effect of the Invention

[0018] The polyurethane resin composition of the present disclosure can form a polyurethane-based resin that combines mechanical properties such as tensile stress and abrasion resistance, hydrolysis resistance, and low-temperature flexibility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] [Polyurethane resin composition] A polyurethane resin composition according to an embodiment of the present disclosure comprises a urethane prepolymer having a diol compound and an aromatic diisocyanate as constituent units, and a chain extender, wherein the diol compound comprises an ABA block copolymer, wherein the A component of the ABA block copolymer is a polylactone chain and the B component is a polytrimethylene ether glycol chain, and the content of the A component with respect to the total amount of the ABA block copolymer is 33 to 67% by mass.

[0020] The diol compound contains an ABA block copolymer, and the A component of the ABA block copolymer is a polylactone chain and the B component is a polytrimethylene ether glycol chain. The content of the A component relative to the total amount of the ABA block copolymer is 33 to 67 mass%, so that the amount of the ether structure and the ester structure in the diol compound is appropriate, and the polyurethane resin composition containing the diol compound has mechanical properties while also having hydrolysis resistance and low-temperature flexibility. In the present disclosure, "mechanical properties" is a general term for physical properties such as abrasion resistance and tensile stress.

[0021] <Urethane prepolymer> The urethane resin composition contains a urethane prepolymer having the diol compound and the aromatic diisocyanate as constituent units. That is, the urethane prepolymer contains a prepolymer obtained by reacting a polyol containing the diol compound, an isocyanate containing the aromatic diisocyanate, and other components as necessary.

[0022] The k value of the urethane prepolymer (i.e., the molar ratio of polyisocyanate to polyol constituting the urethane prepolymer [polyisocyanate / polyol]) is preferably 2.00 or more and less than 5.00, more preferably 3.00 or more and 4.80 or less, and even more preferably 3.50 or more and 4.50 or less. When the k value is less than 5.00, a polyurethane resin composition having high flexibility and fatigue resistance can be obtained. Furthermore, when the k value is 2.00 or more, sufficient strength is easily obtained.

[0023] (Diol Compound) The diol compound contained in the polyol contains an ABA block copolymer, and the A component of the ABA block copolymer is a polylactone chain and the B component is a polytrimethylene ether glycol chain. Although polylactone chains having different structures may be used as the A components in the ABA block copolymer, it is preferable to use the same polylactone chain from the viewpoint of exerting the respective physical properties defined in the present disclosure.

[0024] Examples of lactones that form the polylactone chain include 3- to 16-membered lactone compounds such as α-acetolactone, β-propiolactone, γ-butyrolactone, δ-valerolactone, ε-caprolactone, 8-hydroxyoctanoic acid lactone, 12-hydroxydodecanoic acid lactone, 13-hydroxytridecanoic acid lactone, 14-hydroxytetradecanoic acid lactone, and 15-hydroxypentadecanoic acid lactone; and dioxanes such as 3-ethyl-2-keto-1,4-dioxane, 1,4-dioxane-2-one, and 3-propyl-2-keto-1,4-dioxane.

[0025] The lactone may have a substituent such as an alkyl group or an alkoxy group.

[0026] Examples of the alkyl group include linear or branched alkyl groups having about 1 to 10 carbon atoms, such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, s-butyl, t-butyl, pentyl, hexyl, heptyl, octyl, and decyl groups.

[0027] Examples of the alkoxy group include lower alkoxy groups having about 1 to 10 carbon atoms (preferably 1 to 6 carbon atoms, more preferably 1 to 4 carbon atoms), such as methoxy, ethoxy, propoxy, isopropoxy, butoxy, isobutoxy, t-butoxy, pentyloxy, and hexyloxy.

[0028] In the present disclosure, the polylactone chain can be formed from one of the lactones alone or two or more of them in combination. Among them, the polycaprolactone chain formed from ε-caprolactone is preferred because it is easy to improve the mechanical properties.

[0029] The polylactone chain (component A) preferably has a number average molecular weight (Mn) of 250 to 1500, more preferably 300 to 1250. When the number average molecular weight of the lactone is within the above range, the amount of the ester structure in the diol compound can be made appropriate.

[0030] The number average molecular weight (Mn) of the polytrimethylene ether glycol chain (component B) is preferably 500 to 3000, more preferably 600 to 2000, and further preferably 800 to 1500. By being within the above range, the amount of ether structures in the ABA block copolymer can be made appropriate.

[0031] The number average molecular weight (Mn) of the ABA block copolymer is preferably 1000 to 4000, and more preferably 1500 to 3000. When the number average molecular weight of the ABA block copolymer and the number average molecular weight of the diol compound are 1000 or more, flexibility is easily exhibited, and when it is 4000 or less, sufficient strength is easily exhibited.

[0032] The content of the A component in the ABA block copolymer is 33 to 67% by mass, preferably 40 to 65% by mass, and more preferably 45 to 60% by mass. When the content of the A component is within the above range, the ratio of ester to ether in the ABA block copolymer is appropriate, making it easy to exhibit mechanical properties.

[0033] The diol compound may contain a diol compound other than the ABA block copolymer. However, in order to maintain an appropriate amount of ether and ester structures in the diol compound, it is preferable that the diol compound does not contain a diol compound other than the ABA block copolymer.

[0034] The proportion of the ABA block copolymer in the diol compound is preferably 60 mol % or more, more preferably 80 mol % or more, even more preferably 90 mol % or more, and particularly preferably 95 mol % or more, relative to 100 mol % of the total amount of the diol compound.

[0035] Examples of diol compounds other than the ABA block copolymer include polyether diols other than polytrimethylene ether glycol, glycerin, ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, polybutadiene polyol, polyisoprene polyol, polyester polyol, and copolymers of the above-listed compounds with the above-listed lactones or the above-listed polylactone chains.

[0036] The proportion of the diol compound in the polyol constituting the urethane prepolymer is preferably 60 mol % or more, more preferably 80 mol % or more, even more preferably 90 mol % or more, and particularly preferably 95 mol % or more, relative to 100 mol % of the total amount of the polyol.

[0037] The number average molecular weight (Mn) of the diol compound is preferably 1000 to 4000, more preferably 1500 to 3000, and further preferably 1800 to 2200. When the number average molecular weight of the diol compound is 1000 or more, flexibility is easily exhibited, and when it is 4000 or less, sufficient strength is easily exhibited.

[0038] The hydroxyl value of the diol compound as measured according to JIS K1557 is preferably 28 to 113 KOHmg / g, more preferably 37 to 113 KOHmg / g, and even more preferably 51 to 63 KOHmg / g. By using a diol within this range, a polyurethane having flexibility, high tensile strength, and good abrasion resistance can be obtained.

[0039] The viscosity of the diol compound at 60°C measured according to JIS K 1558 is preferably 330 mPa·s or less, more preferably 300 mPa·s or less, and even more preferably 280 mPa·s or less. By having the viscosity within the above range, the crystallinity can be reduced. The lower limit is not particularly limited, but is preferably 100 mPa·s or more.

[0040] The molecular weight distribution (Mw / Mn) of the diol component is preferably 2.0 or less, more preferably 1.8 or less, and even more preferably 1.5 or less. When the molecular weight distribution is within the above range, the polyurethane has low viscosity and excellent processability, and stable quality can be obtained when used as a polyurethane.

[0041] (Aromatic diisocyanate compounds) The polyurethane resin composition contains an aromatic diisocyanate compound as a constituent unit of the urethane prepolymer. The aromatic diisocyanate compound may be used alone or in combination of two or more.

[0042] Examples of the aromatic diisocyanate compound include tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), 4,4'-diisocyanato-3,3'-dimethylbiphenyl (tolidine diisocyanate (TODI)), 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate (NDI), xylylene diisocyanate, 1,3-phenylene diisocyanate, and 1,4-phenylene diisocyanate (PPDI). Among these, TDI, MDI, TODI, NDI, and PPDI are preferred, and MDI is more preferred. Examples of MDI include 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, and 4,4'-diphenylmethane diisocyanate.

[0043] The urethane prepolymer may contain a diisocyanate compound other than the aromatic diisocyanate compound. Examples of the other diisocyanate compound include an aliphatic diisocyanate compound and an alicyclic diisocyanate compound. Only one type of the other diisocyanate compound may be used, or two or more types may be used.

[0044] Examples of the aliphatic diisocyanate compound include 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,7-heptamethylene diisocyanate, 1,8-octamethylene diisocyanate, 1,9-nonamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, and 1,10-decamethylene diisocyanate.

[0045] Examples of the alicyclic diisocyanate compound include 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, 1,4-bis(isocyanatemethyl)cyclohexane, 4,4'-dicyclohexylmethane diisocyanate, isophorone diisocyanate, and norbornene diisocyanate.

[0046] The proportion of the aromatic diisocyanate compound in the isocyanate constituting the urethane prepolymer is preferably 60 mol % or more, more preferably 80 mol % or more, even more preferably 90 mol % or more, and particularly preferably 95 mol % or more, relative to 100 mol % of the total amount of the isocyanate.

[0047] (Chain extender) The polyurethane resin composition may contain any known or commonly used chain extenders. The chain extenders may be used alone or in combination of two or more.

[0048] The chain extender is not particularly limited, but examples thereof include low molecular weight polyols, polyamines, etc. The molecular weight of the chain extender is, for example, 500 or less, preferably 300 or less.

[0049] Examples of the chain extender include diols such as ethylene glycol, diethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,2-pentanediol, 2,3-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol; and diamines such as hexamethylenediamine, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, and 4,4'-methylenebis-2-chloroaniline. Among these, diols are preferred, and 1,4-butanediol is particularly preferred.

[0050] The proportion of 1,4-butanediol in the chain extender is preferably 60 mol % or more, more preferably 80 mol % or more, even more preferably 90 mol % or more, and particularly preferably 95 mol % or more, relative to 100 mol % of the total amount of the chain extender.

[0051] The polyurethane resin composition is preferably one obtained by reacting the aromatic diisocyanate compound with the diol compound and the chain extender in such a manner that the ratio of the number of moles of the isocyanate group to the number of moles of the isocyanate-reactive group (hydroxyl group, amino group, etc.) [NCO / NCO reactive group] is preferably 0.9 to 1.1, more preferably 0.93 to 1.07, and even more preferably 0.97 to 1.03. That is, the polyurethane resin composition is preferably one obtained by reacting the aromatic diisocyanate compound and the diol compound and the chain extender in such a manner that the ratio of the number of moles of the structural part derived from the isocyanate group to the number of moles of the structural part derived from the isocyanate-reactive group is within the above range.

[0052] (Other Ingredients) The polyurethane resin composition may contain other components in addition to the diol compound, the aromatic diisocyanate, and the chain extender. Examples of the other components include conductive agents, light stabilizers, ultraviolet absorbers, antioxidants, solvents, fillers, flame retardants, pigments, antimicrobial agents, antistatic agents, processing aids, and viscosity improvers. The content of the other compounds is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0% by mass, relative to the total amount (100% by mass) of the polyurethane resin composition.

[0053] [Polyurethane resin] The polyurethane resin composition can be cured by a known or conventional method to produce a polyurethane resin, which is preferably a urethane prepolymer crosslinked with the chain extender.

[0054] The polyurethane resin can be produced, for example, by a prepolymer method.

[0055] The prepolymer method includes, for example, a method in which components A and B contained in a diol compound are mixed, an ABA block copolymer is prepared by a known or conventional method, and then an aromatic diisocyanate compound is reacted in advance at a temperature of 120° C. or less so that the isocyanate groups are in excess relative to the hydroxyl groups in the diol compound to obtain a prepolymer having an isocyanate group terminal, and the resulting prepolymer is reacted with a chain extender.

[0056] The polyurethane resin prepared by the above method preferably has a structural portion containing the urethane prepolymer and a structural portion containing the chain extender.

[0057] In the DMA chart obtained by viscoelasticity measurement, it is preferable that the polyurethane resin has no shoulder peak between −40° C. and 40° C. (preferably −60° C. and 40° C.) In this case, the polyurethane resin composition is less likely to harden in the low temperature range, and low-temperature flexibility is easily exhibited.

[0058] The polyurethane resin preferably has an A hardness of 85 or more and a D hardness of 50 or less, as measured in accordance with JIS K 7312. When the A hardness is 85 or more, it is easy to exhibit high strength, and when the D hardness is 50 or less, it is easy to exhibit flexibility.

[0059] In addition, the polyurethane resin preferably has a tensile stress of 38 MPa or more at 400 to 500% elongation measured at a temperature of 23°C using a No. 3 dumbbell according to JIS K 7312, more preferably 40 MPa or more, and even more preferably 42 MPa or more. If the sample breaks within the above conditions, the value at the time of break is evaluated, and if the sample does not break, the value of the tensile stress at 500% elongation is evaluated. By having the tensile stress of 38 MPa or more, the polyurethane resin composition can exhibit sufficient strength. Although there is no particular upper limit, it is preferably 70 MPa or less.

[0060] In addition, in a Taber abrasion test carried out in accordance with JIS K 7312, the polyurethane resin preferably loses weight (amount of wear) of 12 mg or less, more preferably 11 mg or less, when a test piece of the polyurethane resin molded into a shape of 2 mm thick × 12 mm long × 20 mm wide is rubbed 1000 times at a temperature of 23° C. When the amount of wear is 12 mg or less, it becomes easy to exhibit abrasion resistance.

[0061] The polyurethane resin preferably has a tensile stress retention of 80% or more, more preferably 90% or more, and even more preferably 100% after 7 days under conditions of 70° C. and RH 95%. A tensile stress retention of 80% or more makes it easier for the polyurethane resin composition to exhibit hydrolysis resistance.

[0062] The above polyurethane resins have excellent mechanical properties, hydrolysis resistance, and low-temperature flexibility, and can be used in many fields, including electrical and electronic parts, precision instruments, home appliances, AV equipment, office automation equipment, automobiles, agriculture, forestry, fisheries, food, textiles, clothing, leather, and medicine.

[0063] Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. In addition, each configuration in each embodiment and their combinations are merely examples, and addition, omission, and other modifications of configurations are possible as appropriate within the scope of the present disclosure. The present disclosure is not limited by the embodiments, but is limited only by the claims. EXAMPLES

[0064] Hereinafter, one embodiment of the present disclosure will be described in more detail based on examples.

[0065] Example 1, Comparative Example 1 (Preparation of Diol Compound) Add PO3G (polytrimethylene ether glycol) and CLM to the flask in the following molar ratio: PO3G:CLM=1:(2000-(56100 / hydroxyl value of PO3G×2)) / 114.14 After dehydration under reduced pressure, a catalyst was added and reacted at 160°C to obtain a diol compound of Example 1, which is an ABA block copolymer having polycaprolactone diol as component A and PO3G as component B. The content of component A relative to the total amount of the diol compound was 50 mass%. In addition, the diol compound of Comparative Example 1 was obtained by synthesizing in the same manner, except that PO3G was replaced with PTMG (polytetramethylene ether glycol).

[0066] (Preparation of Prepolymer) The diol compound and aromatic diisocyanate compound were added to a flask according to the k value (molar ratio of isocyanate / polyol) shown in Table 1, mixed, and reacted at 80° C. until the remaining amount of isocyanate groups was 9 NCO%, thereby obtaining prepolymers of Example 1 and Comparative Example 1. In Table 1, "-" indicates that no compound was added, or that the item was not measured or could not be measured.

[0067] (Preparation of polyurethane resin test pieces) The above prepolymer and chain extender were charged into a cup container so that the molar ratio of isocyanate groups to hydroxyl groups was 1.03, and mixed and defoamed using a vacuum degassing mixer (product name "Rotating / Revolving Mixer Awatori Rentaro Vacuum Type ARV-310", manufactured by Thinky Corporation) to produce a polyurethane resin composition. The mixture was then poured into a mold measuring 2 mm thick x 12 mm long x 20 mm wide, and heated in an oven at 120°C for 16 hours to harden. The mixture was then left to cure for 48 hours in a high-temperature, high-quality environment at 23°C and 50% Rh to produce a polyurethane resin test piece.

[0068] Comparative Examples 2 to 4 (Preparation of Prepolymer) Prepolymers of Comparative Examples 2 to 4 were obtained in the same manner as in Example 1, except that each of the diol compounds shown in Table 1 was used as the diol compound.

[0069] (Preparation of polyurethane resin test pieces) Test pieces of the polyurethane resin composition and the polyurethane-based resin were prepared in the same manner as in Example 1, except that the prepolymers of Comparative Examples 2 to 4 were used.

[0070] Details of each component in Table 1 are given below. PO3G1000: Polytrimethylene ether glycol, manufactured by SK Chemicals, number average molecular weight 1000 PO3G2000: Polytrimethylene ether glycol, manufactured by SK Chemicals, number average molecular weight 2000 PTMG1000: Polytetramethylene ether glycol, manufactured by Mitsubishi Chemical Corporation, number average molecular weight 1000 PTMG2000: Polytetramethylene ether glycol, manufactured by Mitsubishi Chemical Corporation, number average molecular weight 2000 PCL2000: Polycaprolactone diol, manufactured by Daicel Corporation, number average molecular weight 2000 MDI: 4,4'-diphenylmethane diisocyanate, trade name "Millionate MT", manufactured by Tosoh Corporation BDO: 1,4-butanediol, manufactured by Mitsubishi Chemical Corporation

[0071] [evaluation] The test pieces of the diol compounds and polyurethane resins obtained in the examples and comparative examples were subjected to the following evaluations, and the results are shown in Table 1.

[0072] (1) Hydroxyl value The hydroxyl values ​​of the diol compounds in the examples and comparative examples were measured in accordance with JIS K 1557.

[0073] (2) Viscosity The viscosity at 60° C. of the diol compounds in the examples and comparative examples was measured in accordance with JIS K 1557.

[0074] (3)Molecular weight distribution Each of the diol compounds of the Examples and Comparative Examples was dissolved in THF, and the molecular weight distribution in the THF solution was measured using GPC (product name "HLC-8420GPC", manufactured by Tosoh Corporation).

[0075] (4)Hardness The D hardness at 23° C. of the test pieces of the polyurethane resins prepared in the examples and comparative examples was measured in accordance with JIS K 7312.

[0076] (5) Cold hardening For the polyurethane resin test pieces prepared in the examples and comparative examples, a viscoelasticity measuring device (product name "DMA7100", manufactured by Hitachi High-Tech Science Corporation) was used to measure E' at each temperature under the following conditions: chuck distance 20 mm, temperature -100 to 200°C, heating rate 2°C / min, frequency 10 Hz, initial strain, dynamic strain 0.05, and tensile mode, and a DMA chart was prepared.

[0077] In the DMA chart obtained by measuring the storage modulus, those in which a shoulder peak was observed between -60°C and 40°C were evaluated as "with cold hardening," and those in which a shoulder peak was not observed were evaluated as "without cold hardening."

[0078] (6) Tensile stress Using the polyurethane resin test pieces prepared in the Examples and Comparative Examples, tensile stresses at 100%, 300%, and 500% elongation at a temperature of 23° C. were measured using a No. 3 dumbbell in accordance with JIS K 7312. The values ​​in parentheses in Table 1 indicate the degree of elongation at break when the polyurethane test piece breaks, and when the polyurethane test piece does not break within the above range, the tensile stress value at 500% elongation was evaluated.

[0079] (7) Abrasion resistance Using the polyurethane resin test pieces prepared in the Examples and Comparative Examples, a Taber abrasion test was carried out in accordance with JIS K 7312, and the abrasion amount (mg) after 1000 cycles was measured at a temperature of 23°C.

[0080] (8) Tensile stress retention rate The polyurethane resin test pieces prepared in the examples and comparative examples were used and left to stand for 7 days under conditions of 70°C and 95% RH using an environmental tester (product name "Small Environmental Tester SH-641", manufactured by ESPEC). The retention of tensile stress before and after the test was evaluated as follows. When the calculated value of the retention of tensile stress was 100% or more, the result was evaluated as 100%. Tensile stress retention rate (%) = (tensile stress before test - tensile stress after test) / (tensile stress before test) x 100

[0081] [Table 1]

[0082] It was confirmed that the polyurethane resin formed from the polyurethane resin composition used in Example 1 has excellent mechanical properties such as tensile stress and abrasion resistance, low-temperature flexibility, and hydrolysis resistance. On the other hand, it was confirmed that when the diol compound does not contain a polylactone chain, there are problems with mechanical properties such as tensile stress and abrasion resistance, and low-temperature flexibility (Comparative Examples 2 and 3). In addition, when a polyether polyol chain other than polytrimethylene ether glycol is used as the B component in the ABA block copolymer, the mechanical properties such as tensile stress and abrasion resistance are insufficient (Comparative Example 1), and when only a polylactone chain is used, the hydrolysis resistance is poor (Comparative Example 4).

[0083] Variations of the present disclosure are described below. [Appendix 1] The composition includes a urethane prepolymer having a diol compound and an aromatic diisocyanate as structural units, and a chain extender, the diol compound includes an ABA block copolymer, the A component of the ABA block copolymer being a polylactone chain and the B component being a polytrimethylene ether glycol chain; A polyurethane resin composition, wherein the content of the A component based on the total amount of the ABA block copolymer is 33 to 67 mass %. [Appendix 2] 2. The polyurethane resin composition according to claim 1, wherein the ABA block copolymer has a number average molecular weight of 4,000 or less. [Appendix 3] 3. The polyurethane resin composition according to claim 1, wherein the polylactone chain is polycaprolactone. [Appendix 4] 4. The polyurethane resin composition according to any one of claims 1 to 3, wherein the aromatic diisocyanate is diphenylmethane diisocyanate. [Appendix 5] 5. The polyurethane resin composition according to any one of claims 1 to 4, wherein the chain extender is 1,4-butanediol. [Appendix 6] A polyurethane resin in which the urethane prepolymer in the polyurethane resin composition according to any one of claims 1 to 5 is crosslinked with the chain extender.

Claims

1. The composition includes a urethane prepolymer having a diol compound and an aromatic diisocyanate as structural units, and a chain extender, the diol compound includes an A-B-A block copolymer, the A component of the A-B-A block copolymer being a polylactone chain and the B component being a polytrimethylene ether glycol chain; A polyurethane resin composition, wherein the content of the A component relative to the total amount of the A-B-A block copolymer is 33 to 67 mass %.

2. 2. The polyurethane resin composition according to claim 1, wherein the A-B-A block copolymer has a number average molecular weight of 4,000 or less.

3. 3. The polyurethane resin composition according to claim 1, wherein the polylactone chain is polycaprolactone.

4. 3. The polyurethane resin composition according to claim 1, wherein the aromatic diisocyanate is diphenylmethane diisocyanate.

5. 3. The polyurethane resin composition according to claim 1, wherein the chain extender is 1,4-butanediol.

6. A polyurethane resin in which the urethane prepolymer in the polyurethane resin composition according to claim 1 or 2 is crosslinked with the chain extender.

Citation Information

Patent Citations

  • EPA and DHA-enriched omega-3 supplement for the treatment of dry eye, meibomian gland inflammation, and xerostomia

    JP2005535733A