White thermosetting resin composition
A white thermosetting resin composition with a specific silicone resin and pigment addresses the issue of maintaining light reflectance and preventing cracking in optical semiconductor devices, improving their performance and durability under heat stress.
Patent Information
- Application Number
- JP2023054951
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing thermosetting resin compositions for optical semiconductor devices face challenges in maintaining light reflectance and preventing cracking under high temperatures, which affect the optical properties and longevity of LED packages.
A white thermosetting resin composition is developed, containing a specific silicone resin with controlled chemical structure and a white pigment, which maintains light reflectance and prevents cracking even under high heat conditions.
The composition ensures high light reflectance and resistance to cracking, enhancing the performance and durability of optical semiconductor devices under increased heat and light exposure.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a white thermosetting resin composition, an optical semiconductor element using the same, an optical semiconductor element mounting substrate and a method for producing the same, and an optical semiconductor device. [Background technology]
[0002] In recent years, optical semiconductor devices that combine optical semiconductor elements such as LEDs (Light Emitting Diodes) with phosphors have been applied to a variety of applications such as outdoor displays, mobile LCD backlights, and in-vehicle applications due to their advantages such as high energy efficiency and long life, and the demand for such devices is expanding.
[0003] As a result, LED devices have become increasingly bright, raising concerns about rising junction temperatures due to increased heat generation from the element, and deterioration of element materials due to increased direct light energy. In recent years, the development of element materials that are resistant to thermal and light degradation has become a challenge.
[0004] Under these circumstances, as a technology for preventing the problem of brightness reduction caused by heat or light, the following Patent Document 1 proposes a substrate for mounting optical semiconductor elements, in which a reflector with high light reflectance is provided at the portion where the optical semiconductor element is mounted. Patent Document 1 also discloses forming the reflector by transfer molding, and proposes a light-reflecting thermosetting resin composition containing a silicone resin, a curing catalyst, a white pigment, etc. as the material. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-94544 A Summary of the Invention [Problem to be solved by the invention]
[0006] Meanwhile, the manufacture of an LED package involves high-temperature processes such as connecting a substrate for mounting an optical semiconductor element to an optical semiconductor element, sealing the optical semiconductor element with a resin, and solder reflow during mounting on the substrate. In the case of a substrate for mounting an optical semiconductor element produced using a light-reflecting thermosetting resin composition, if the resin material discolors due to heat, it tends to be difficult to ensure the initial optical properties of the LED package. In addition, the substrate for mounting an optical semiconductor element is required to maintain its optical properties even when used for a long time at high temperatures.
[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a white thermosetting resin composition having sufficient light reflectance and moldability and excellent heat resistance and light reflectivity, an optical semiconductor element, an optical semiconductor mounting substrate, an optical semiconductor device, and methods for manufacturing the same, all of which are made using the same. [Means for solving the problem]
[0008] As a result of intensive research conducted to solve the above problems, the present inventors discovered that by blending a specific silicone resin with a highly controlled chemical structure as the silicone resin component in a white thermosetting resin composition containing a silicone resin and a white pigment, it is possible to obtain a resin with high light reflectance, to reduce the decrease in light reflectance of the resin after heat treatment at high temperatures compared to conventional methods, and to suppress the occurrence of cracks, which led to the completion of the present invention.
[0009] The present invention relates to a white thermosetting resin composition containing a specific silicone resin described below and a white pigment.
[0010] In another aspect, the present invention relates to an optical element semiconductor using a white thermosetting resin composition. In the optical element semiconductor, the portion using the cured product of the white thermosetting resin composition may be a side portion or a side portion and a bottom portion. Furthermore, a wavelength conversion portion may be provided between the side portion of the optical element semiconductor and the cured product of the white thermosetting resin composition.
[0011] In another aspect, the white thermosetting resin composition of the present invention can be applied to a substrate to form a substrate for mounting an optical semiconductor element.
[0012] In still another aspect, the present invention relates to an optical semiconductor device including an optical semiconductor element or an optical semiconductor element mounted on a semiconductor mounting substrate.
[0013] In yet another aspect, the present invention relates to a method for manufacturing an optical semiconductor element using a white thermosetting resin composition on a side surface of the optical semiconductor element, the method including a step of applying the white thermosetting resin composition to an optical semiconductor element disposed in an opening in a spacer to form the optical semiconductor element. Effect of the Invention
[0014] The present invention uses a white thermosetting resin composition containing a specific silicone resin and a white pigment, thereby providing a resin whose light reflectivity does not deteriorate when heated and which does not crack, thereby providing a white light reflective layer that is sufficient for high-output LEDs. [Brief description of the drawings]
[0015] [Figure 1] 1 is a schematic cross-sectional view illustrating an embodiment of an optical semiconductor element. [Diagram 2] FIG. 4 is a schematic cross-sectional view showing another embodiment of the optical semiconductor element. [Diagram 3] 1A to 1C are schematic cross-sectional views illustrating an embodiment of a method for producing an optical semiconductor element. [Figure 4] 1 is a schematic cross-sectional view showing one embodiment of an optical semiconductor element mounting board. [Diagram 5] 1 is a schematic cross-sectional view showing one embodiment of an optical semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention relates to items 1 to 13. Item 1. A white thermosetting resin composition containing a silicone resin containing a compound represented by formula (1) and a white pigment. TIFF2024142700000001.tif59168 In formula (1), R 0 are each independently a vinyl group or a hydrogen atom; R 1 are each independently a hydrocarbon group having 1 to 8 carbon atoms; R 2 are each independently a hydrocarbon group having 1 to 8 carbon atoms; m is an average value satisfying 1 to 5; and n is an average value satisfying 2 to 30.
[0017] Item 2. The white thermosetting resin composition according to item 1, wherein the proportion of the compound represented by formula (1) is in the range of 10% by weight to 80% by weight based on the weight of the silicone resin.
[0018] Item 3. The white thermosetting resin composition according to item 1 or 2, wherein the silicone resin contains a compound represented by formula (2). TIFF2024142700000002.tif61125 In formula (2), R 3 each independently represents an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, or a cyclohexyl group; each X independently represents a group represented by formula (X1), formula (X2), or formula (X3); TIFF2024142700000003.tif21145 In formula (X2), R 4 each independently represents an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or a phenyl group; s represents an average value of 2 to 20; In formula (X3), R 5 are each independently an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or a phenyl group; R 6 is an alkenyl group having 2 to 5 carbon atoms; R 7 is an alkylene having 2 to 5 carbon atoms; t is an average value satisfying 2 to 20; In formula (X1), formula (X2), and formula (X3), * indicates a bonding site; When the average number of groups represented by formula (X1) per molecule of the compound represented by formula (2) is x1, the average number of groups represented by formula (X2) is x2, and the average number of groups represented by formula (X3) is x3, x1 + 2x2 + x3 = 4r, 0 < x1 < 4r, 0 ≤ x2 < 2r, and 0 < x3 < 4r are satisfied; r is an average value satisfying 1 to 100.
[0019] Item 4. The white thermosetting resin composition according to item 3, wherein the proportion of the compound represented by formula (2) is in the range of 10% by weight to 90% by weight based on the weight of the silicone resin.
[0020] Item 5. The white thermosetting resin composition according to any one of items 1 to 4, wherein the silicone resin contains a compound represented by formula (3). TIFF2024142700000004.tif3194 In formula (4), R 8 and R 9 are each independently an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or an aromatic hydrocarbon group having 6 to 12 carbon atoms; R 10 are each independently an alkenyl group having 2 to 5 carbon atoms or a hydrogen atom; u is an average value satisfying 1 to 50.
[0021] Item 6. The white thermosetting resin composition according to item 5, wherein the proportion of the compound represented by formula (3) is 30% by weight or less based on the weight of the silicone resin.
[0022] Item 7. The white thermosetting resin composition according to any one of items 1 to 6, wherein the silicone resin contains a compound represented by formula (4). TIFF2024142700000005.tif61125 In formula (4), R 11each independently represents an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, or a cyclohexyl group; each Y independently represents a group represented by formula (Y1), formula (Y2), formula (Y31), formula (Y32), formula (Y33), formula (Y41), or formula (Y42); TIFF2024142700000006.tif92155 In formula (Y2), R 12 each independently represents an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or a phenyl group; w is an average value satisfying a value of 1 to 20; In formula (Y41), R 13 are each independently a methyl group, an ethyl group, a butyl group, or an isopropyl group; In formula (Y42), R 14 are each independently a methyl group, an ethyl group, a butyl group, or an isopropyl group; R 15 each independently represents a methyl group, an ethyl group, a butyl group, an isopropyl group, or an alkenyl having 2 to 5 carbon atoms; x represents an average value of 1 to 20; In formulae (Y1), (Y2), (Y31), (Y32), (Y33), (Y41) and (Y42), * indicates a binding site; When the average number of groups represented by formula (Y1) per molecule of the compound represented by formula (4) is y1, the average number of groups represented by formula (Y2) is y2, the average number of groups represented by formula (Y31), formula (Y32) or formula (Y33) is y3, and the average number of groups represented by formula (Y41) or formula (42) is y4, y1+2y2+y3+y4=4v, satisfying 0.5v≦y1≦3v, 0.5v≦2y2≦2v, 0.1v≦y3≦2v, and 0≦y4≦v; v is an average value that satisfies 1 to 100.
[0023] Item 8. The white thermosetting resin composition according to Item 7, wherein the proportion of the compound represented by formula (4) is in the range of 11% by weight or less based on the weight of the silicone resin.
[0024] Item 9. The white thermosetting resin composition according to any one of Items 1 to 8, wherein the content of the white pigment is 5% by weight to 80% by weight based on the weight of the white thermosetting resin composition.
[0025] Item 10. An optical semiconductor element using the white thermosetting resin composition according to any one of items 1 to 9.
[0026] Item 11. A substrate for mounting an optical semiconductor element, comprising the white thermosetting resin composition according to any one of items 1 to 9.
[0027] Item 12. An optical semiconductor device comprising the optical semiconductor element according to item 10 or the optical semiconductor element mounting substrate according to item 11.
[0028] Item 13. A method for producing an optical semiconductor element, in which the white thermosetting resin composition according to any one of Items 1 to 9 is used for a side surface portion.
[0029] (White thermosetting resin composition) The white thermosetting resin composition of the present embodiment contains a silicone resin and a white pigment. The white thermosetting resin composition may be simply referred to as a thermosetting resin composition.
[0030] A preferred white thermosetting resin composition according to this embodiment contains, as silicone resin components, a compound represented by formula (1), a compound represented by formula (2), a compound represented by formula (3), and a compound represented by formula (4), and a white pigment.
[0031] The white thermosetting resin composition of the present invention contains, as a silicone resin component, a double-decker compound having a silsesquioxane structure represented by formula (1). TIFF2024142700000007.tif59168
[0032] In formula (1), R 0 are each independently a vinyl group or a hydrogen atom; R 1 are each independently a hydrocarbon group having 1 to 8 carbon atoms; R2 are each independently a hydrocarbon group having 1 to 8 carbon atoms; m is an average value satisfying 1 to 5; and n is an average value satisfying 2 to 30.
[0033] Preferred R 0 is a vinyl group.
[0034] R 1 Examples of the hydrocarbon group in include an aliphatic chain hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group. Examples of the aliphatic chain hydrocarbon group include alkyl groups such as a methyl group, an ethyl group, and a propyl group, alkenyl groups such as a vinyl group and a propenyl group, and alkynyl groups such as an ethynyl group and a propynyl group. Examples of the alicyclic hydrocarbon group include a cyclopropyl group, a cyclobutyl group, a cyclohexyl group, and a cyclohexenyl group. Examples of the aromatic hydrocarbon group include a phenyl group, a tolyl group, and the like.
[0035] Preferred R 1 is an aliphatic chain hydrocarbon group or an aromatic hydrocarbon group, and more preferably R 1 is an aliphatic chain hydrocarbon group. Among the aliphatic chain hydrocarbon groups, an alkyl group is preferred, and a methyl group is particularly preferred. Among the aromatic hydrocarbon groups, a phenyl group is preferred.
[0036] R 2 The hydrocarbon group in 1 The hydrocarbon groups are the same as those exemplified in R. 2 The upper limit of the number of carbon atoms in R is preferably 5, more preferably 3. 2 is an aliphatic chain hydrocarbon group. 2 R is an alkyl group, and a methyl group is particularly preferred. 2 When is an alkyl group, the siloxane chain does not contain a crosslinkable group, and the crosslink density upon curing is appropriate. This enhances the stress relaxation ability of the resulting molded article, thereby further improving the crack resistance in high temperature environments.
[0037] It can be said that m represents the degree of polymerization of the silsesquioxane structural unit in formula (1), and n represents the average number of siloxane structural units in the polysiloxane chain (degree of polymerization of the polysiloxane chain).
[0038] The specific structure of the compound represented by formula (1) is as follows, where X is the silsesquioxane structural unit, Y is the siloxane structural unit, m = 2, and n = 5. However, since m and n are each average values, the number of consecutive Y's in a single molecule, i.e., the average number of siloxane structural units in a polysiloxane chain, may vary.
[0039] TIFF2024142700000008.tif25160
[0040] The lower limit of m is 1, and in some cases 1.5 is more preferable, and the upper limit of m is 5, and in some cases 4 is more preferable.
[0041] The lower limit of n may be 2, preferably 3, and more preferably 4. The upper limit of n is 30, preferably 20, and more preferably 10.
[0042] The weight-average molecular weight of the compound represented by formula (1) is preferably in the range of 1000 to 20000. The lower limit is preferably 2000 or more. The upper limit is preferably 10000 or less. When the weight-average molecular weight is in this range, the crosslink density in the obtained molded product becomes appropriate, and the stress relaxation ability is enhanced, thereby improving the crack resistance in a high temperature environment. In addition, by having a weight average molecular weight equal to or less than the above upper limit, the composition becomes a liquid with an appropriate viscosity, and can be suitably used for applications such as sealing materials.
[0043] The viscosity of the compound represented by formula (1) at 25°C is preferably in the range of 1 Pa·s to 100 Pa·s. The lower limit of the viscosity is more preferably 5 Pa·s or more. On the other hand, the upper limit of the viscosity is more preferably 50 Pa·s or less. When the compound represented by formula (1) has such a viscosity, it has a suitable fluidity and is more useful as an encapsulant for semiconductors and the like. The viscosity of the compound represented by formula (1) can be adjusted by the weight average molecular weight, the degree of polymerization of each structural unit, and the like.
[0044] A preferred proportion of the compound represented by formula (1) is in the range of 10% by weight to 80% by weight based on the weight of the silicone resin, and more preferably 20% by weight or more for improving heat resistance.
[0045] The white thermosetting resin composition of the present invention contains a white pigment.
[0046] Examples of the white pigment include titanium oxide, zinc oxide, aluminum oxide, magnesium oxide, antimony oxide, zirconium oxide, silica, inorganic hollow particles, etc. These may be used alone or in combination of two or more kinds.
[0047] The inorganic hollow particles are particles formed from a material other than titanium oxide, zinc oxide, alumina, magnesium oxide, antimony oxide, and zirconium oxide. Examples of the inorganic hollow particles include particles of soda silicate glass, aluminum silicate glass, soda borosilicate glass, and silica.
[0048] The median particle size of the white pigment is preferably in the range of 50 nm to 1000 nm. If the median particle size is 50 nm or more, the particles tend to be prevented from agglomerating and to have good dispersibility, while if it is 1000 nm or less, the light reflectance properties of the cured product tend to be sufficient.
[0049] The preferred proportion of the white pigment is 5 to 80% by weight based on the weight of the white thermosetting resin composition. When the content of the white pigment is 5% by weight or more, the light reflection characteristics of the cured product are easily obtained sufficiently, and when it is 80% by weight or less, the coating property of the thermosetting resin composition is improved, and the production of an optical semiconductor element or the like becomes easy.
[0050] The silicone resin may further contain a compound represented by the formula (2). TIFF2024142700000009.tif61125 In the formula (2), R 3 is each independently an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, or a cyclohexyl group; X is each independently a group represented by the formula (X1), the formula (X2), or the formula (X3); TIFF2024142700000010.tif21145 In the formula (X2), R 4 is each independently an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or a phenyl group; s is an average value satisfying 2 to 20; In the formula (X3), R 5 is each independently an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or a phenyl group; R 6 is an alkenyl group having 2 to 5 carbon atoms; R 7 is an alkylene having 2 to 5 carbon atoms. t is an average value satisfying 2 to 20; In the formula (X1), the formula (X2), and the formula (X3), * indicates the bonding site; When the average number of the groups represented by the formula (X1) per molecule of the compound represented by the formula (2) is x1, the average number of the groups represented by the formula (X2) is x2, and the average number of the groups represented by the formula (X3) is x3, x1 + 2x2 + x3 = 4r, 0 < x1 < 4r, 0 ≦ x2 < 2r, and 0 < x3 < 4r are satisfied; r is an average value satisfying 1 to 100.
[0051] When X contains a group represented by the formula (X2), it may crosslink within the same silsesquioxane structure.
[0052] Preferred R 3 is a methyl group, an ethyl group, or a propyl group, with a methyl group being particularly preferred.
[0053] Preferred R 4 is a methyl group, an ethyl group, or a propyl group, and is particularly preferably a methyl group.
[0054] Preferred R 5 is a methyl group, an ethyl group, or a propyl group, and a methyl group is particularly preferred. 6 and R 7 is an ethyl group. The upper limit of t is preferably 10, more preferably 5, and further preferably 3.
[0055] x1 is preferably greater than r, more preferably greater than 2r. Also, x1 is preferably less than 3r. x2 is preferably equal to or less than r. Also, x3 is preferably greater than r. Also, x3 is preferably less than 3r, more preferably less than 2r. It is also preferable that x1>x3 is satisfied. In one embodiment, x2 may be 0. In this case, r is 1.
[0056] The compound represented by formula (2) can be synthesized, for example, by the method described in WO 2011 / 145638.
[0057] A preferred proportion of the compound represented by formula (2) is in the range of 10% by weight to 90% by weight, based on the weight of the silicone resin, and is more preferably 85% or less for improving heat resistance.
[0058] The silicone resin may further contain a compound represented by formula (3). TIFF2024142700000011.tif3194 In formula (4), R 8 and R 9are each independently an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or an aromatic hydrocarbon group having 6 to 12 carbon atoms; R 10 each independently represents an alkenyl group having 2 to 5 carbon atoms or a hydrogen atom; and u is an average value of 1 to 50.
[0059] Preferred R 8 is an alkyl group, and methyl is particularly preferred. 9 R is an alkyl group or an aromatic hydrocarbon group, and is particularly preferably a methyl group or a phenyl group. 10 In the above formula, the alkenyl having 2 to 5 carbon atoms is preferably a vinyl group.
[0060] The Two R's 10 Compounds in which both R are hydrogen or two R 10 Compounds in which both R are vinyl are preferred. 10 When both R are hydrogen, the upper limit of u is preferably 30, more preferably 15. 10 When both are alkenyl, the upper limit of u is preferably 10, more preferably 5, further preferably 3, and particularly preferably 1.
[0061] A preferred proportion of the compound represented by formula (3) is 30% by weight or less based on the weight of the silicone resin.
[0062] The silicone resin may further contain a compound represented by formula (4). TIFF2024142700000012.tif61125 In formula (4), R 11 each independently represents an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, or a cyclohexyl group; each Y independently represents a group represented by formula (Y1), formula (Y2), formula (Y31), formula (Y32), formula (Y33), formula (Y41), or formula (Y42); TIFF2024142700000013.tif92155 In formula (Y2), R 12each independently represents an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or a phenyl group; w is an average value satisfying a value of 1 to 20; In formula (Y41), R 13 are each independently a methyl group, an ethyl group, a butyl group, or an isopropyl group; In formula (Y42), R 14 are each independently a methyl group, an ethyl group, a butyl group, or an isopropyl group; R 15 are each independently a methyl group, an ethyl group, a butyl group, an isopropyl group, or an alkenyl having from 2 carbon atoms; x is an average value satisfying 1 to 20; In formulae (Y1), (Y2), (Y31), (Y32), (Y33), (Y41) and (Y42), * indicates a binding site; When the average number of groups represented by formula (Y1) per molecule of the compound represented by formula (4) is y1, the average number of groups represented by formula (Y2) is y2, the average number of groups represented by formula (Y31), formula (Y32) or formula (Y33) is y3, and the average number of groups represented by formula (Y41) or formula (42) is y4, y1+2y2+y3+y4=4v, satisfying 0.5v≦y1≦3v, 0.5v≦2y2≦2v, 0.1v≦y3≦2v, and 0≦y4≦v; v is an average value that satisfies 1 to 100.
[0063] Preferred R 11 is an alkyl group, and is particularly preferably a methyl group.
[0064] Preferred R 12 is an alkyl group, and a methyl group is particularly preferred. 13 , R 14 , R 15 is a methyl group.
[0065] It is preferable that y1, y2, y3, and y4 satisfy v≦y1≦2v, 0.3v≦y2≦v, 0.3v≦y3≦v, and 0.3v≦y4≦v, respectively. The lower limit of v may be 3 or 5. The upper limit of v may be 30 or 15.
[0066] A preferred proportion of the compound represented by formula (4) is 11% by weight or less, based on the weight of the silicone resin, and more preferably 5% by weight or less for improving heat resistance.
[0067] For the purpose of curing the white thermosetting resin composition of the present invention, a curing catalyst may be added.
[0068] The curing catalyst is not particularly limited as long as it has catalytic activity to promote the hydrosilylation reaction. Pt catalyst, Rh catalyst, Pd catalyst, Co catalyst, etc. can be used, and Pt catalyst is preferably used. The Pt catalyst is a catalyst containing platinum, and the platinum may be either not oxidized or oxidized. An example of oxidized platinum is platinum oxide. An example of partially oxidized platinum is Adams catalyst.
[0069] Examples of Pt catalysts include Karstedt catalyst, Speier catalyst, and hexachloroplatinic acid. These are generally well-known catalysts. Among these, the non-oxidized Karstedt catalyst is preferably used.
[0070] The proportion of the curing catalyst is preferably an amount sufficient to promote curing of the white thermosetting resin composition of the present embodiment, and specifically, the proportion is preferably in the range of 0.01 ppm to 10 ppm, and more preferably in the range of 0.1 ppm to 3 ppm, based on the weight of the silicone resin.
[0071] The white thermosetting resin composition of the present invention may further contain various additives such as inorganic fillers, antioxidants, release agents, dispersants, and ion scavengers in addition to the above-mentioned components.
[0072] Examples of inorganic fillers include fused spherical silica, crushed silica, silica, antimony oxide, aluminum hydroxide, magnesium hydroxide, barium sulfate, magnesium carbonate, and barium carbonate. The median particle size of the inorganic filler is preferably within the range of 10 to 1000 nm from the viewpoint of improving the packing efficiency with the white pigment. The content of the inorganic filler is preferably 15% by weight or less based on the weight of the white thermosetting resin composition.
[0073] The white thermosetting resin composition of the present invention may contain a coupling agent or the like as necessary. In this case, the interfacial adhesion between the compound represented by (1) or the compound represented by (2) and inorganic components such as white pigments and inorganic fillers can be improved. Examples of the coupling agent include silane coupling agents and titanate coupling agents. As the silane coupling agent, known compounds such as epoxy silanes, amino silanes, cationic silanes, vinyl silanes, acrylic silanes, mercapto silanes, and composites thereof can generally be used. The amount of the coupling agent used is preferably adjusted appropriately in consideration of the surface coverage of the inorganic components, but from the viewpoint of improving the curability, it is preferable to set the amount of the coupling agent to 5% by weight or less based on the weight of the white thermosetting resin composition. The inorganic components such as white pigments and inorganic fillers may be previously treated with the coupling agent.
[0074] A curing retarder may be added to the white thermosetting resin composition of the present invention for the purpose of improving storage stability or adjusting the reactivity of the hydrosilylation reaction during the production process. Examples of the curing retarder include a compound containing an aliphatic unsaturated bond, an organic phosphorus compound, an organic sulfur compound, a nitrogen-containing compound, a tin-based compound, and an organic peroxide.
[0075] Examples of compounds containing an aliphatic unsaturated bond include propargyl alcohols, ene-yne compounds, and maleic acid esters. Examples of organic phosphorus compounds include triorganophosphines, diorganophosphines, organophosphones, and triorganophosphites. Examples of organic sulfur compounds include organomercaptans, diorganosulfides, hydrogen sulfide, benzothiazole, and benzothiazole disulfide. Examples of nitrogen-containing compounds include ammonia, primary to tertiary alkylamines, arylamines, urea, and hydrazine. Examples of tin-based compounds include stannous halide dihydrate and stannous carboxylate. Examples of organic peroxides include di-t-butyl peroxide, dicumyl peroxide, benzoyl peroxide, and t-butyl perbenzoate.
[0076] Among these hardening retarders, those having good retardation activity and being colorless or relatively colorless, for example, pale yellow, are preferred. The hardening retarders may be used alone or in combination of two or more kinds.
[0077] The amount of the curing retarder added is preferably in the range of 0.1 to 10,000 parts by mass, and more preferably in the range of 1 to 50 parts by mass, per part by mass of the curing catalyst used.
[0078] The white thermosetting resin composition of the present invention may contain a thermosetting resin other than the compound represented by formula (1) and the compound represented by formula (2) for the purpose of improving the properties. Examples of the thermosetting resin include, but are not limited to, epoxy resin, acrylic resin, cyanate resin, phenolic resin, polyimide resin, polyamideimide resin, and urethane resin. Among these, epoxy resin is preferred from the viewpoint of high convenience as an electronic component and excellent adhesion to metal components. The thermosetting resin is preferably colorless or relatively uncolored, such as pale yellow.
[0079] The epoxy resin is not particularly limited, but examples thereof include hexafluorobisphenol A diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, bisphenol A diglycidyl ether, 2,2'-bis(4-glycidyloxycyclohexyl)propane, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, vinylcyclohexene dioxide, 2-(3,4-epoxycyclohexyl)-5,5-spiro-(3,4-epoxycyclohexane)-1,3-dioxane, bis(3,4-epoxycyclohexyl)adipate, 1,2-cyclopropanedicarboxylic acid bisglycidyl ester, triglycidyl isocyanurate, monoallyl diglycidyl isocyanurate, and diallyl monoglycidyl isocyanurate. When an epoxy resin is used, it is advisable to further add, as a curing agent, an aliphatic acid or an anhydride thereof, such as hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, tetrahydrophthalic anhydride, hydrogenated methylnadic anhydride, trimellitic anhydride, pyromellitic anhydride, 1,4-cyclohexanedicarboxylic acid, etc. These epoxy resins or curing agents may be used alone or in combination.
[0080] It is preferable to add silica to the white thermosetting resin composition of the present invention for the purpose of controlling viscoelasticity.
[0081] A preferred proportion of silica is 15% by weight or less, based on the weight of the white thermosetting resin composition.
[0082] Silica may be either naturally occurring silica (natural silica) that has been pulverized, or industrially synthesized silica (synthetic silica). Natural silica is a crystal, and therefore has a crystal axis. For this reason, optical characteristics derived from crystals can be expected, but since its specific gravity is somewhat higher than that of synthetic silica, it may affect dispersion in the white thermosetting resin composition. In addition, when natural silica is obtained by pulverizing a natural product, it may be an irregularly shaped particle or a material with a wide particle size distribution.
[0083] Synthetic silica includes wet synthetic silica and dry synthetic silica, but the present invention does not limit the use of either. However, synthetic silica may have water of crystallization regardless of the manufacturing method, and when this water of crystallization may have some effect on the white thermosetting resin composition or its cured product, or LED elements, it is preferable to select the type of silica by taking into consideration the number of water of crystallization.
[0084] Synthetic silica is amorphous rather than crystalline, and as such has the advantage that particle distribution can be controlled and particle size can be made extremely small.
[0085] In particular, fumed silica has a nano-order particle size and is excellent in particle dispersibility. Furthermore, when compared at the same weight, the smaller the particle size, the larger the total surface area, which makes it more preferable to use it because the direction of light reflection becomes more diverse.
[0086] In general, silica has a large surface area and is a hydrophilic material (hydrophilic silica) due to the effect of silanols present on the surface, but it can also be made hydrophobic by chemical modification. The type of silica to be used is selected according to the purpose.
[0087] In view of its intended use, the white thermosetting resin composition of the present invention preferably has an optical reflectance (thickness of 0.1 mm) of 90% or more at wavelengths of 430 to 800 nm after curing. When this optical reflectance is 90% or more, it tends to be able to contribute sufficiently to improving the brightness of an optical semiconductor device. The white thermosetting resin composition of the present embodiment preferably has the optical reflectance of 90% or more. In addition, from the viewpoint of improving the brightness of an optical semiconductor device, the optical reflectance at a wavelength of 450 nm after curing is preferably 90% or more, and more preferably 95% or more.
[0088] From the viewpoint of improving heat-resistant light reflectance, it is preferable that the cured molded product maintains a light reflectance of 90% or more at wavelengths of 430 to 800 nm even after a heat resistance test in which the molded product is exposed to an environment of 200° C. for 1000 hours. It is more preferable that the light reflectance at a wavelength of 450 nm is 90% or more when measured after the above-mentioned heat resistance test. Such light reflectance characteristics of the white thermosetting resin composition can be realized by appropriately adjusting the blending amounts of various components constituting the white thermosetting resin composition, and more specifically, can be achieved by mixing a colorless thermosetting resin component with a white pigment having a high refractive index.
[0089] The method for producing the white thermosetting resin composition of the present invention is not particularly limited. For example, a method of mixing the above-mentioned curing accelerator, silicone resin, white pigment, and, if necessary, the above-mentioned heat curing agent, antioxidant, etc. in predetermined amounts at room temperature or under heating using a mixer such as a homodisper, homomixer, universal mixer, planetarium mixer, kneader, three-roll mill, or bead mill can be mentioned.
[0090] An optical semiconductor element containing the white thermosetting resin composition of the present invention as a reflective layer also constitutes the present invention.
[0091] (Optical semiconductor element having a cured product of a white thermosetting resin composition) The optical semiconductor element including the cured product of the white thermosetting resin composition according to the present embodiment includes the cured product of the white thermosetting resin composition of the present invention on the side surface of the optical semiconductor element, and may or may not include the cured product of the white thermosetting resin composition on the bottom surface. Also, a wavelength conversion layer may or may not be provided between the side surface of the optical semiconductor element and the cured product of the white thermosetting resin composition or on the top of the optical semiconductor element.
[0092] 1 is a schematic cross-sectional view showing one embodiment of an optical semiconductor element. An optical semiconductor element 100 has a light-reflecting layer 101 on its side surface. The light-reflecting layer 101 is made of a cured product of the white thermosetting resin composition according to this embodiment described above.
[0093] 2 is a schematic cross-sectional view showing one embodiment of an optical semiconductor element. Optical semiconductor element 100 has wavelength conversion layers 103 on the top and side surfaces, and a light reflecting layer 101 on the bottom surface. Wavelength conversion layer 103 further has light reflecting layers 101 on the side and bottom surfaces. Light reflecting layer 101 is made of a cured product of the white thermosetting resin composition according to this embodiment described above.
[0094] 3 is a schematic diagram showing one embodiment of a process for producing an optical semiconductor element. The method for producing an optical semiconductor element is not particularly limited, but the element can be produced, for example, by placing a semiconductor element 100 having solder bumps 102 on a spacer 104, applying a white thermosetting resin composition 105 using a dispenser or the like, and removing the spacer after heat curing to expose the solder bumps by buffing the bottom.
[0095] The conditions for heat curing are not particularly limited, but it is preferable to heat the composition in the following order: 80° C. for 40 minutes, 120° C. for 40 minutes, and then 160° C. for 2 hours.
[0096] The optical semiconductor mounting substrate according to this embodiment includes a copper foil and a light reflecting layer formed by using the above-mentioned white thermosetting resin composition laminated on the copper foil.
[0097] Fig. 4 is a schematic cross-sectional view showing a preferred embodiment of an optical semiconductor element mounting substrate. As shown in Fig. 4, an optical semiconductor element mounting substrate 200 comprises a base material 201, a copper foil 202 laminated on the base material 201, and a light reflecting layer 101 laminated on the copper foil 202. The light reflecting layer 101 is formed using the above-mentioned white thermosetting resin composition of the present invention.
[0098] As the base material 201, any base material used for an optical semiconductor mounting substrate can be used without any particular limitation, and examples thereof include a glass epoxy resin laminate plate and a phenol resin laminate plate.
[0099] Optical semiconductor element mounting board 200 can be produced by applying the white thermosetting resin composition according to this embodiment onto base material 201 having copper foil 202 thereon, and then heating and curing it.
[0100] Fig. 5 is a schematic cross-sectional view showing a preferred embodiment of an optical semiconductor device. As shown in Fig. 5, an optical semiconductor device 300 is composed of an optical semiconductor element 100 using a reflective layer 101, and an optical semiconductor element mounting substrate 200. The optical semiconductor element 100 is electrically connected to copper foil 202 via solder bumps 102.
[0101] The optical semiconductor device 300 according to this embodiment is an optical semiconductor device that uses both or either one of the optical semiconductor element 100 and the optical semiconductor element mounting substrate 200 that uses the above-mentioned light reflecting layer 101 .
[0102] The method for forming a reflective layer from the white thermosetting resin composition of the present invention is not particularly limited, and examples include a method in which the optical semiconductor composition of the present invention is injected into a mold form in advance, a lead frame or the like to which a light-emitting element is fixed is immersed in the composition, and then cured; a method in which the optical semiconductor composition of the present invention is injected into a form in which a light-emitting element has been inserted, and then cured; and a method in which the composition is applied to a light-emitting element, then cured and cut into pieces.
[0103] Examples of the method for injecting the white thermosetting resin composition of the present invention include injection using a dispenser, transfer molding, and injection molding. Examples of the method for applying the composition include a method for applying the white thermosetting resin composition of the present invention through a drop, stencil printing, screen printing, or mask onto a light-emitting element and then curing the composition, and a method for injecting the optical semiconductor composition of the present invention into a cup or the like with a light-emitting element at the bottom and then curing the composition.
[0104] The conditions for heat curing are not particularly limited, but it is preferable to heat the composition in the following order: 80° C. for 40 minutes, 120° C. for 40 minutes, and then 160° C. for 2 hours. EXAMPLES
[0105] The present invention will be described in more detail with reference to examples, but the present invention is not limited to the following examples.
[0106] <Measurement of number average molecular weight and weight average molecular weight> The number average molecular weight and weight average molecular weight of the polymer synthesized in the present invention were measured as follows. Using a high-performance liquid chromatography system CO-2065plus manufactured by JASCO Corporation, 20 μL of a THF solution with a sample concentration of 1% by mass was used as the analytical sample, and measurements were performed by the GPC method under the following conditions: column: Shodex KF804L [manufactured by Showa Denko K.K.] (two columns connected in series), column temperature: 40°C, detector: RI, eluent: THF, and eluent flow rate: 1.0 mL per minute, and the values were calculated in terms of polystyrene.
[0107] The reagents used in the examples are as follows. UT771 (titanium oxide coated with zirconium oxide): manufactured by Ishihara Sangyo Kaisha, Ltd. CR-90 (titanium oxide coated with silica): manufactured by Ishihara Sangyo Kaisha, Ltd. FM-2205 (compound (3-1)) (polydimethylsiloxane having vinyl at both ends and a number average molecular weight of 700): manufactured by JNC Corporation FM-1111 (Compound (3-2)): manufactured by JNC Corporation DVTS (1,5-divinyl-1,1,3,3,5,5-hexamethyltrisiloxane) (compound (3-3)): manufactured by GELEST 2BH (1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane) (compound (3-4)): manufactured by Biogen MVS-H (1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane): manufactured by GELEST ECYH-OH (1-ethynylcyclohexanol): manufactured by Tokyo Chemical Industry Co., Ltd. DM-30S (Dry Silica): Tokuyama Corporation Blue flip chip LED (B3838FCP1): Manufactured by Genesis Photonics Inc.
[0108] <Synthesis of compound (1-1)> Compound (1-1) having the following structure was synthesized by the method described in JP 2020-090593 A. (Analysis results) 1 H-NMR (solvent: deuterated chloroform): δ (ppm): -0.15 to 0.42 (m, 187.0H), 5.60 to 6.19 (m, 6.0H), 6.95 to 7.72 (m, 89.9H) 29 Si-NMR (solvent: THF): δ (ppm): -78.1~-76.9(m, 9.0Si), -63.4(s, 2.0Si), -21.3~-17.5(m, 13.2Si), -2.4(s, 1.3Si) Viscosity=11.6Pa·s Number average molecular weight: Mn=3960 Weight average molecular weight: Mw=6760 n=9.5 m=3.2
[0109] TIFF2024142700000014.tif56157
[0110] <Synthesis of compound (1-2)> Compound (1-2) having the following structure was synthesized by the method described in JP 2020-090593 A. (Analysis results) 1 H-NMR (solvent: deuterated chloroform): δ (ppm): -0.15 to 0.42 (m, 74.5H), 5.60 to 6.19 (m, 6.0H), 6.95 to 7.72 (m, 56.4H) 29 Si-NMR (solvent: THF): δ (ppm): -78.1~-76.9(m, 8.6Si), -63.4(s, 2.0Si), -21.3~-17.5(m, 6.9Si), -2.4(s, 1.4Si) Viscosity=21.7Pa·s Number average molecular weight: Mn=1890 Weight average molecular weight: Mw=2650 n=4.3 m=1.5
[0111] TIFF2024142700000015.tif58162
[0112] <Synthesis of compound (2-1)> TIFF2024142700000016.tif41148 Compound (2-1) was synthesized by the method described in WO 2011 / 145638.
[0113] <Synthesis of compound (4-1)> TIFF2024142700000017.tif36168 Compound (4-1) was synthesized by the method described in Japanese Patent No. 5880556.
[0114] <Preparation of Examples 1 to 4 and Comparative Example 1> A white thermosetting resin composition was prepared by uniformly mixing the respective components in the composition ratios (wt%) shown in the following Tables 1 and 2. Each evaluation was carried out using this white thermosetting resin composition.
[0115] <Preparation of slide glass with 0.1 mm thick cured resin film in examples and comparative examples> Each white thermosetting resin composition was applied to a slide glass equipped with a 0.1 mm-thick spacer, and cured by heating at 80°C for 40 minutes, at 120°C for 40 minutes, and then at 160°C for 2 hours, and the spacer was removed to obtain a 30 mm x 55 mm x 0.1 mm-thick cured resin film on the slide glass.
[0116] <Reflectance evaluation> The reflectance of the cured film at a wavelength of 450 nm was measured using a UV-visible spectrophotometer V-650 and an integrating sphere ILV-724 manufactured by JASCO Corporation.
[0117] <Reflectance evaluation after heat resistance test> The cured film after measuring the initial reflectance was placed in an oven set at 200° C. and removed after 1000 hours, and the reflectance of light at a wavelength of 450 nm was measured using a JASCO V-650 UV-Visible Spectrophotometer and an ILV-724 integrating sphere.
[0118] <Reflectivity retention rate> The reflectance retention rate was calculated from the above initial reflectance (wavelength 450 nm) / reflectance after heat resistance test (wavelength 450 nm).
[0119] <Heat crack resistance test> The aforementioned 0.1 mm thick cured resin film was placed in an oven at 250° C., and the time until cracks appeared was measured.
[0120] TIFF2024142700000018.tif8595Among the values shown, the numbers in parentheses indicate the weight percentage based on the weight of the silicone resin.
[0121] As shown in Table 1, compared to Comparative Example 1, the cured film using the white thermosetting resin composition of the present invention retains high reflectance even after the heat resistance test and has significantly excellent heat crack resistance.
[0122] Examples 2 to 4 were prepared in the same manner as in Example 1, and various evaluations were carried out (Table 2).
[0123] TIFF2024142700000019.tif112120Among the values listed, the numbers in parentheses indicate the weight percentage based on the weight of the silicone resin.
[0124] As shown in Table 2, even when a compound represented by formula (1) different from that in Example 1 is used or when the type and content of the filler is changed, it is found that the film has a sufficiently high reflectance and excellent heat crack resistance. [Industrial Applicability]
[0125] The white thermosetting resin composition of the present invention can be used as a light reflector, an insulating film, a sealing material, an adhesive, etc. The white thermosetting resin composition of the present invention is useful as a light reflector for optical semiconductor elements such as LEDs because it suppresses the occurrence of cracks during heat crack resistance tests and heat and light resistance tests. [Explanation of symbols]
[0126] 100...optical semiconductor element, 101...light reflective layer, 102…solder bump, 103...wavelength conversion layer, 104…Spacer, 105...White thermosetting resin composition, 200...Substrate for mounting optical semiconductor elements, 201...Base material, 202...Copper foil, 300...Optical semiconductor device.
Claims
1. A white thermosetting resin composition comprising a silicone resin containing a compound represented by formula (1) and a white pigment. In formula (1), R 0 are each independently a vinyl group or a hydrogen atom; R 1 are each independently a hydrocarbon group having 1 to 8 carbon atoms; R 2 are each independently a hydrocarbon group having 1 to 8 carbon atoms; m is an average value satisfying 1 to 5; and n is an average value satisfying 2 to 30.
2. 2. The white thermosetting resin composition according to claim 1, wherein the proportion of the compound represented by formula (1) is in the range of 10% by weight to 80% by weight based on the weight of the silicone resin.
3. 3. The white thermosetting resin composition according to claim 1, wherein the silicone resin contains a compound represented by formula (2). In formula (2), R 3 each independently represents an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, or a cyclohexyl group; each X independently represents a group represented by formula (X1), formula (X2), or formula (X3); In formula (X2), R 4 each independently represents an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or a phenyl group; s is an average value satisfying 2 to 20; In formula (X3), R 5 are each independently an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or a phenyl group; R 6 is an alkenyl group having 2 to 5 carbon atoms; R 7 is an alkylene group having 2 to 5 carbon atoms; t is an average value of 2 to 20; In formula (X1), formula (X2), and formula (X3), * indicates a binding site; The average number of groups represented by formula (X1) per molecule of the compound represented by formula (2) is x 1 The average number of groups represented by formula (X2) is x 2 The average number of groups represented by formula (X3) is x 3 Then, x 1 +2x 2 +x 3 = 4r, 0 < x 1 < 4r, 0 ≦ x 2 < 2r and 0 < x 3 <4r; r is an average value ranging from 1 to 100.
4. 4. The white thermosetting resin composition according to claim 3, wherein the proportion of the compound represented by formula (2) is in the range of 10% by weight to 90% by weight, based on the weight of the silicone resin.
5. The white thermosetting resin composition according to claim 3 , wherein the silicone resin contains a compound represented by formula (3). In formula (4), R 8 and R 9 are each independently an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or an aromatic hydrocarbon group having 6 to 12 carbon atoms; R 10 each independently represents an alkenyl group having 2 to 5 carbon atoms or a hydrogen atom; and u is an average value of 1 to 50.
6. 6. The white thermosetting resin composition according to claim 5, wherein the proportion of the compound represented by formula (3) is 30% by weight or less based on the weight of the silicone resin.
7. The white thermosetting resin composition according to claim 3 , wherein the silicone resin contains a compound represented by formula (4). In formula (4), R 11 each independently represents an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, or a cyclohexyl group; each Y independently represents a group represented by formula (Y1), formula (Y2), formula (Y31), formula (Y32), formula (Y33), formula (Y41), or formula (Y42); In formula (Y2), R 12 each independently represents an alkyl group having 1 to 4 carbon atoms, a cyclopentyl group, a cyclohexyl group, or a phenyl group; w is an average value satisfying 1 to 20; In formula (Y41), R 13 are each independently a methyl group, an ethyl group, a butyl group, or an isopropyl group; In formula (Y42), R 14 are each independently a methyl group, an ethyl group, a butyl group, or an isopropyl group; R 15 each independently represents a methyl group, an ethyl group, a butyl group, an isopropyl group, or an alkenyl group having 2 to 5 carbon atoms; x represents an average value of 1 to 20; In formulae (Y1), (Y2), (Y31), (Y32), (Y33), (Y41) and (Y42), * indicates a binding site; The average number of groups represented by formula (Y1) per molecule of the compound represented by formula (4) is y 1 The average number of groups represented by formula (Y2) is y 2 y is the average number of groups represented by formula (Y31), formula (Y32) or formula (Y33); 3 The average number of groups represented by formula (Y41) or formula (42) is y 4 Then, y 1 +2y 2 +y 3 +y 4 =4v, 0.5v≦y 1 ≦3v, 0.5v≦2y 2 ≦2v, 0.1v≦y 3 ≦2v and 0≦y 4 ≦v; v is an average value between 1 and 100.
8. 8. The white thermosetting resin composition according to claim 7, wherein the proportion of the compound represented by formula (4) is in the range of 11% by weight or less, based on the weight of the silicone resin.
9. 3. The white thermosetting resin composition according to claim 1, wherein the content of the white pigment is 5% by weight to 80% by weight, based on the weight of the white thermosetting resin composition.
10. An optical semiconductor element comprising the white thermosetting resin composition according to claim 1.
11. A substrate for mounting optical semiconductor elements, comprising the white thermosetting resin composition according to claim 1 .
12. An optical semiconductor device comprising the optical semiconductor element according to claim 10 or the optical semiconductor element mounting substrate according to claim 11.
13. A method for producing an optical semiconductor element, comprising using the white thermosetting resin composition according to claim 1 or 2 for a side surface portion thereof.
Citation Information
Patent Citations
Thermosetting resin composition for light reflection, optical semiconductor element mounting substrate prepared therewith and method for producing the same, and optical semiconductor device