Polarizing plate

The polarizing plate with a polyester resin film and adhesive layers addresses rainbow unevenness and light leakage issues by enhancing optical properties, ensuring improved visibility in liquid crystal displays.

JP2024142941APending Publication Date: 2024-10-11SUMITOMO CHEM CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023055362
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing polarizing plates fail to effectively suppress rainbow unevenness visible from an oblique direction and light leakage at the ends due to shrinkage at high temperatures.

Method used

A polarizing plate design comprising a polyester resin film with specific retardation values and thickness, combined with adhesive layers and a (meth)acrylic resin film, to enhance optical properties and reduce shrinkage-induced issues.

Benefits of technology

The design effectively suppresses rainbow unevenness and light leakage at high temperatures, improving visibility and performance of liquid crystal display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142941000001_ABST
    Figure 2024142941000001_ABST
Patent Text Reader

Abstract

To provide a polarizing plate with which rainbow unevenness visually recognized from an oblique direction of the polarizing plate is suppressed and light leakage occurring at polarizing plate edge due to the shrinkage of the polarizing plate under high temperature is suppressed, as well as provide a polarizing plate with an adhesive layer including the polarizing plate, and a liquid crystal display device including the polarizing plate with the adhesive layer.SOLUTION: Provided is a polarizing plate including a polyester resin film, a first adhesive layer, a polarizer, a second adhesive layer, and a (meth)acrylic resin film in this order. The contractive force of the polarizer in the absorption axis direction is 4.0 N / 2 mm or less. As for a phase difference value Re defined by Re=(nx-ny)×d, the phase difference value Re1 of the polyester resin film measured in a first disposition is 6000 nm or greater, the phase difference value Re2 measured in a second disposition is 5000 nm or greater, the phase difference value Re3 measured in a third disposition is 6000 nm or greater, and the phase difference value Re4 measured in a fourth disposition is 7000 nm or greater.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing plate, and further to a polarizing plate with a pressure-sensitive adhesive layer and a liquid crystal display device that include the polarizing plate. [Background technology]

[0002] In recent years, there has been a demand for improved visibility of liquid crystal display devices. In order to improve the visibility of liquid crystal display devices, there is also a demand for suppressing unevenness in polarizing plates, which are one of the components constituting liquid crystal display devices, and suppressing light leakage that occurs at the ends of the polarizing plates due to shrinkage of the polarizing plates in high-temperature environments. In order to suppress unevenness of the polarizing plate and suppress light leakage occurring at the edge of the polarizing plate, the type and combination of the polarizer protective film in the polarizing plate are being studied. For example, Patent Document 1 describes that when a biaxially stretched polyethylene terephthalate film having a thickness of 38 μm is used as one polarizer protective film, an acrylic-containing film having a cellulose ester resin composition is used as the other polarizer protective film, so that unevenness in the polarization degree of the polarizing plate can be suppressed. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2011-123402 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, even the polarizing plate described in Patent Document 1 does not sufficiently suppress rainbow unevenness visible from an oblique direction of the polarizing plate or suppress light leakage from the edge of the polarizing plate under high temperatures.

[0005] The object of the present invention is to provide a polarizing plate in which rainbow unevenness when viewed from an oblique direction of the polarizing plate is suppressed and light leakage at the ends of the polarizing plate due to shrinkage of the polarizing plate at high temperatures is suppressed, as well as a polarizing plate with an adhesive layer including the polarizing plate and a liquid crystal display device including the polarizing plate with an adhesive layer. [Means for solving the problem]

[0006] The present invention includes the following inventions. [1] A polarizing plate comprising, in this order, a polyester resin film, a first adhesive layer, a polarizer, a second adhesive layer, and a (meth)acrylic resin film, The contraction force of the polarizer in the absorption axis direction is less than 4.0 N / 2 mm; The polyester resin film is a polarizing plate in which the retardation value Re defined by the formula (1) satisfies the following [i] to [iv]. Re = (n x -n y )×d (1) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is measured to be 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the phase difference value Re4 measured is 7000 nm or more. [2] The polarizing plate according to [1], wherein the polyester resin film has a thickness of 60 μm or more. [3] The polarizing plate according to [1] or [2], wherein the ratio of a retardation value Re1 to a retardation value Rth in the thickness direction of the polyester resin film defined by the formula (2) is 0.5 or more. Rth = (n x +n y ) / 2-n z 〕×d (2) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and n z represents the refractive index in the thickness direction of the film, and d represents the thickness of the film. [4] A polarizing plate with a pressure-sensitive adhesive layer, comprising the polarizing plate according to any one of [1] to [3] and a pressure-sensitive adhesive layer, A polarizing plate with a pressure-sensitive adhesive layer, in which the pressure-sensitive adhesive layer is laminated on a surface of the (meth)acrylic resin film opposite to the polarizer. [5] A liquid crystal display device comprising the polarizing plate with the pressure-sensitive adhesive layer according to [4]. Effect of the Invention

[0007] According to the present invention, it is possible to provide a polarizing plate in which rainbow unevenness from an oblique direction of the polarizing plate is suppressed and light leakage at the ends of the polarizing plate due to shrinkage of the polarizing plate at high temperatures is suppressed, as well as a polarizing plate with an adhesive layer including the polarizing plate and a liquid crystal display device including the polarizing plate with an adhesive layer. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the polarizing plate of the present invention. [Diagram 2] FIG. 11 is a schematic perspective view for explaining a phase difference value Re1 and a method for measuring the same. [Diagram 3] FIG. 13 is a schematic perspective view illustrating a phase difference value Re2 and a method for measuring the phase difference value Re2. [Figure 4] FIG. 11 is a schematic perspective view illustrating a phase difference value Re3 and a method for measuring the phase difference value Re3. [Diagram 5] FIG. 13 is a schematic perspective view illustrating a phase difference value Re4 and a method for measuring the same. [Figure 6] FIG. 1 is a schematic cross-sectional view showing an example of a pressure-sensitive adhesive layer-attached polarizing plate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The polarizing plate of the present invention comprises, in this order, a polyester resin film, a first adhesive layer, a polarizer, a second adhesive layer, and a (meth)acrylic resin film. An example of the layer structure of the polarizing plate of the present invention is shown in Figure 1. The polarizing plate 1 shown in Figure 1 includes a polyester resin film 10, a first adhesive layer 15, a polarizer 30, a second adhesive layer 25, and a (meth)acrylic resin film 20, in this order. 1, in the polarizing plate of the present invention, the polyester resin film 10 and the first adhesive layer 15 are preferably in direct contact with each other. Also, the (meth)acrylic resin film 20 and the second adhesive layer 25 are preferably in direct contact with each other. The polarizer 30 and the first adhesive layer 15 are preferably in direct contact with each other. The polarizer 30 and the second adhesive layer 25 are preferably in direct contact with each other.

[0010] <Polyester resin film> The polyester resin film used in the present invention satisfies the following [i] to [iv] with respect to the retardation value Re defined by the formula (1). Re = (n x -n y )×d (1) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane (the direction perpendicular to the slow axis direction in the film plane), and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is measured to be 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the phase difference value Re4 measured is 7000 nm or more.

[0011] The slow axis direction in the film plane is the direction in which the refractive index is maximum in the plane. In addition, in this specification, the retardation value Re is the retardation value at a wavelength of 587 nm.

[0012] 2 is a schematic perspective view illustrating the retardation value Re1 and a method for measuring the retardation value Re1. The retardation value Re1 is a retardation value measured in a first arrangement in which the polyester resin film 100 is arranged so that the angle between the surface of the polyester resin film 100 and a measurement direction 210 is 90°. The measurement direction is a direction from a light source 201 of the retardation measurement device to an observation device 202 that detects and observes light transmitted through the polyester resin film, and is the so-called optical path of the retardation measurement device.

[0013] 3 is a schematic perspective view illustrating the retardation value Re2 and a method for measuring the retardation value Re2. The retardation value Re2 is a retardation value measured for a polyester resin film tilted by rotating the polyester resin film 100 in the first arrangement by 30° about its fast axis 400 as a central axis 300, that is, a polyester resin film 110 in the second arrangement. The angle between the surface of the polyester resin film 110 in the second arrangement and the measurement direction 210 is 60°.

[0014] 4 is a schematic perspective view illustrating the retardation value Re3 and its measurement method. The retardation value Re3 is a retardation value measured for a polyester resin film tilted by rotating the polyester resin film 100 in the first arrangement by 30° around an axis 310 that forms an angle of 45° with respect to the fast axis 400 in the polyester resin film plane, that is, a polyester resin film 120 in the third arrangement. The angle between the plane of the polyester resin film 120 in the third arrangement and the measurement direction 210 is 60°.

[0015] 5 is a schematic perspective view illustrating the retardation value Re4 and its measurement method. The retardation value Re4 is a retardation value measured for a polyester resin film tilted by rotating the polyester resin film 100 in the first arrangement by 30° about its slow axis 500 as the central axis 320, that is, a polyester resin film 130 in the fourth arrangement. The angle between the surface of the polyester resin film 130 in the fourth arrangement and the measurement direction 210 is 60°.

[0016] The retardation value Re1 of the polyester resin film is preferably 7000nm or more, more preferably 7500nm or more, and even more preferably 8000nm or more. The retardation value Re1 of the polyester resin film is usually 30000nm or less, preferably 20000nm or less, more preferably 15000nm or less, even more preferably 10000nm or less, and even more preferably 9000nm or less. When the upper limit of the retardation value Re1 exceeds 30000nm, the thickness of the polyester resin film becomes considerably large in order to satisfy the retardation value, and the handleability as an optical film tends to be greatly reduced. When the retardation value Re1 of the polyester resin film is 6000nm or more, it is easy to reduce rainbow unevenness (rainbow-like color spots) when viewed from an oblique direction.

[0017] The retardation value Re2 of the polyester resin film is 5000 nm or more. The retardation value Re2 is preferably 5500 nm or more, more preferably 6000 nm or more, even more preferably 6500 nm or more, and even more preferably 7000 nm or more. The retardation value Re2 is usually 30000 nm or less, preferably 20000 nm or less, more preferably 15000 nm or less, even more preferably 10000 nm or less, and even more preferably 9000 nm or less. When the retardation value Re2 of the polyester resin film is 5000 nm or more, rainbow unevenness when viewed from an oblique direction is easily reduced.

[0018] The phase difference value Re3 of the polyester resin film is 6000 nm or more. The phase difference value Re3 is preferably 7000 nm or more, more preferably 7500 nm or more, and even more preferably 8000 nm or more. The phase difference value Re3 is usually 30000 nm or less, preferably 20000 nm or less, more preferably 15000 nm or less, even more preferably 10000 nm or less, and even more preferably 9000 nm or less. When the phase difference value Re3 of the polyester resin film is 6000 nm or more, rainbow unevenness when viewed from an oblique direction is easily reduced.

[0019] The phase difference value Re4 of the polyester resin film is 7000 nm or more. The phase difference value Re4 is preferably 8000 nm or more, more preferably 8500 nm or more, and even more preferably 9000 nm or more. The phase difference value Re4 is usually 30000 nm or less, preferably 20000 nm or less, more preferably 15000 nm or less, and even more preferably 10000 nm or less. When the phase difference value Re4 of the polyester resin film is 7000 nm or more, rainbow unevenness when viewed from an oblique direction is easily reduced.

[0020] Re1 to Re4 can be measured using a phase difference measuring device (KOBRA-HB-RESPC, manufactured by Oji Scientific Instruments Co., Ltd.).

[0021] By using a polyester resin film in which Re1 to Re4 are each within the above range, rainbow unevenness visible from an oblique direction of the polarizing plate can be suppressed.

[0022] The ratio Re1 / Rth of the retardation value Re1 to the retardation value Rth in the thickness direction of the polyester resin film is usually 0.4 or more, preferably 0.5 or more, more preferably 0.6 or more, even more preferably 0.7 or more, and even more preferably 0.9 or more. If the ratio Re1 / Rth is large, rainbow unevenness due to the observation angle tends to be less likely to occur. Since the ratio Re1 / Rth is 2.0 in a completely uniaxial (uniaxially symmetric) film, the ratio Re1 / Rth is preferably 2.0 or less, and more preferably 1.5 or less.

[0023] The thickness direction retardation value Rth is expressed by the following formula (2): The thickness direction retardation value Rth is the thickness direction retardation value at a wavelength of 587 nm. Rth = (n x +n y ) / 2-n z 〕×d (2) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and n z represents the refractive index in the film thickness direction (direction perpendicular to the film surface), and d represents the film thickness.

[0024] The angle between the fast axis or slow axis of the polyester resin film and the transmission axis of the polarizer is, for example, -20° to +20°, preferably -15° to +15°, more preferably -10° to +10°, even more preferably -5° to +5°, still more preferably -3° to +3°, particularly preferably -2° to +2°, and particularly preferably -1° to +1°. In a preferred embodiment, the fast axis or slow axis of the polyester resin film and the transmission axis of the polarizer are substantially parallel. Here, being substantially parallel means that the transmission axis of the polarizer and the fast axis or slow axis of the polyester resin film are parallel to an extent that allows for a misalignment that inevitably occurs when the polarizer and the polyester resin film are bonded together. The smaller the angle between the fast axis or slow axis of the polyester-based resin film and the transmission axis of the polarizer, the smaller the change in polarization state caused by linearly polarized light passing through the polyester-based resin film, and therefore the more likely it is that rainbow unevenness will be suppressed.

[0025] In order to suppress deterioration of the optically functional dye such as iodine contained in the polarizer, the polyester resin film preferably has a light transmittance of 40% or less at a wavelength of 380 nm. The light transmittance of 380 nm is more preferably 35% or less, even more preferably 30% or less, and particularly preferably 20% or less. If the light transmittance is 40% or less, deterioration of the optically functional dye due to ultraviolet light can be suppressed.

[0026] At least one layer selected from the group consisting of an antireflection layer and a low antireflection layer may be provided on at least one surface of the polyester resin film. The surface reflectance of the antireflection layer is preferably 5.7% or less. If the surface reflectance of the antireflection layer exceeds 5.7%, rainbow unevenness tends to be easily visible. The surface reflectance of the antireflection layer is more preferably 5.3% or less, even more preferably 5.0% or less, and particularly preferably 4.5% or less. The lower limit of the surface reflectance of the antireflection layer is not particularly limited, but is, for example, 2.0%. The surface reflectance can be measured by any method. For example, a polyester resin film is attached to a black acrylic plate via an adhesive on the opposite side of the antireflection layer side of the polyester resin film, and the light reflectance at a wavelength of 550 nm can be measured from the surface on the antireflection layer side using a spectrophotometer (CM-2600d, manufactured by Konica Minolta Japan, Inc.).

[0027] The anti-reflection layer may be a single layer or a multi-layer. Examples of the anti-reflection layer include an anti-glare hard coat layer having a fine uneven surface to prevent reflection of external light. The anti-glare hard coat layer may be formed by dispersing a filler inside the hard coat layer to form an uneven surface, or may be formed by embossing the hard coat layer to form an uneven surface. For example, when forming an anti-glare hard coat layer using an ultraviolet curing resin, a resin composition obtained by dispersing a filler in an ultraviolet curing resin may be applied to a polyester resin film and irradiated with ultraviolet light, or an ultraviolet curing resin may be applied to a polyester resin film and the coating film may be adhered to the uneven surface of a mold and irradiated with ultraviolet light.

[0028] As a material for forming the antiglare hard coat layer, an ultraviolet curable resin, a thermosetting resin, an electron beam curable resin, etc. can be used, but from the viewpoints of productivity, hardness, etc., an ultraviolet curable resin is preferably used.

[0029] The surface reflectance of the low antireflection layer is preferably 4.0% or less. The surface reflectance of the low antireflection layer is more preferably 3.0% or less, even more preferably 2.0% or less, even more preferably 1.5% or less, and particularly preferably 1.0% or less. The lower limit of the surface reflectance of the low antireflection layer is not particularly limited, but may be, for example, 0.01%.

[0030] The low-reflection anti-layer may be a single layer or a multilayer. When the low-reflection anti-layer is a single layer, the anti-reflection effect can be obtained by forming the low-refractive index layer made of a material having a lower refractive index than the polyester resin film so that the thickness of the low-refractive index layer is 1 / 4 the wavelength of the light or an odd multiple of that wavelength. When the anti-reflection anti-layer is a multilayer, the anti-reflection effect can be obtained by laminating low-refractive index layers and high-refractive index layers alternately in two or more layers, with the thickness of each layer being appropriately controlled. If necessary, a hard coat layer can be laminated between the low-reflection anti-layer and the polyester resin film.

[0031] The low-reflection anti-layer may be a known one, and is preferably a layer formed by coating an organic thin film having a lower refractive index than the polyester resin film or the hard coat layer laminated on the polyester resin film.

[0032] The thickness of at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer is usually 0.01 to 20 μm, preferably 0.03 to 1 μm, and more preferably 0.05 to 0.15 μm.

[0033] The surface reflectance of the polyester resin film is preferably 5.7% or less, more preferably 5.3% or less, even more preferably 4.0% or less, even more preferably 3.0% or less, particularly preferably 2.0% or less, and most preferably 1.5% or less. The surface reflectance of the polyester resin film is usually 0.01% or more. When the surface reflectance of the polyester-based resin film is 5.7% or less, rainbow unevenness in a polarizing plate to which the polyester-based resin film is applied tends to be more effectively suppressed. In addition, when at least one layer selected from the group consisting of an antireflection layer and a low reflection layer is laminated as described above, the surface reflectance of the entire laminate of at least one layer selected from the group consisting of an antireflection layer and a low reflection layer may be 5.7% or less. By lowering the surface reflectance, the interface reflectance between the substrate film and air can be lowered, and it is presumed that rainbow unevenness is suppressed.

[0034] In the case where at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer is provided on only one surface of the polyester-based resin film, it is preferable that the at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer is provided on the surface of the polyester-based resin film opposite the polarizer.

[0035] When providing at least one selected from the group consisting of an antireflection layer and a low antireflection layer, it is preferable that the polyester resin film has an easy-adhesion layer on its surface. In this case, from the viewpoint of suppressing interference due to reflected light, it is preferable to adjust the refractive index of the easy-adhesion layer so that it is close to the geometric mean of the refractive index of the antireflection layer or low antireflection layer and the refractive index of the polyester resin film. The refractive index of the easy-adhesion layer can be adjusted by a known method, and can be easily adjusted, for example, by adding titanium, germanium, or other metal species to the binder resin.

[0036] In order to improve the adhesion to the polarizer, the polyester-based resin film preferably has an easy-adhesion layer on at least one side thereof, the easy-adhesion layer being composed mainly of at least one of polyester resin, polyurethane resin, and polyacrylic resin. Here, the "main component" refers to a component that is 50% by mass or more of the solid components constituting the easy-adhesion layer. The coating liquid used to form the easy-adhesion layer is preferably an aqueous coating liquid containing at least one of water-soluble or water-dispersible copolymer polyester resin, acrylic resin, and polyurethane resin. Examples of these coating liquids include water-soluble or water-dispersible copolymer polyester resin solutions, acrylic resin solutions, and polyurethane resin solutions disclosed in Japanese Patent No. 3567927, Japanese Patent No. 3589232, Japanese Patent No. 3589233, Japanese Patent No. 3900191, and Japanese Patent No. 4150982, etc.

[0037] When a polyester resin is used as the easy-adhesion layer, it is preferable to use a water-soluble or water-dispersible resin in terms of compatibility with the polyvinyl alcohol resin. In order to make the polyester resin water-soluble or water-dispersible, it is preferable to copolymerize a compound containing a hydrophilic group such as a sulfonate group or a carboxylate group. Among them, a dicarboxylic acid component having a sulfonate group is suitable from the viewpoint of imparting hydrophilicity while maintaining the acid value of the polyester resin low and controlling the reactivity with the crosslinking agent. Examples of the dicarboxylic acid component having a sulfonate group include sulfoterephthalic acid, 5-sulfoisophthalic acid, 4-sulfonaphthaleneisophthalic acid-2,7-dicarboxylic acid, and 5-(4-sulfophenoxy)isophthalic acid or an alkali metal salt thereof, and among them, 5-sulfoisophthalic acid is preferable. The dicarboxylic acid component having a sulfonate group is preferably 1 to 15 mol %, more preferably 1.5 to 12 mol %, and even more preferably 2 to 10 mol % of the dicarboxylic acid component of the polyester resin. When the amount of the dicarboxylic acid component having a sulfonate group is equal to or more than the lower limit, it is suitable for making the polyester resin water-soluble or water-dispersible, whereas when the amount of the dicarboxylic acid component having a sulfonate group is equal to or less than the upper limit, it is suitable for improving adhesion to the polyester film substrate.

[0038] The easy-adhesion layer can be obtained by applying the coating liquid to one or both sides of a polyester resin film, drying the film at 100 to 150° C., and then stretching the film in the lateral direction. The final coating amount of the easy-adhesion layer is 0.05 to 0.20 g / m 2 The coating amount is preferably 0.05 g / m 2 If the coating amount is less than 0.20 g / m, the adhesion to the polarizer may be insufficient. 2 When the easy-adhesion layer is provided on both sides of the polyester-based resin film, the coating amount of the easy-adhesion layer on both sides may be the same or different, and each can be independently set within the above range.

[0039] It is preferable to add particles to the easy-adhesion layer to give it easy slipperiness. The average particle size of the particles is preferably 2 μm or less. If the average particle size of the particles exceeds 2 μm, the particles are likely to fall off from the easy-adhesion layer. Examples of particles to be contained in the easy-adhesion layer include inorganic particles such as titanium oxide, barium sulfate, calcium carbonate, calcium sulfate, silica, alumina, talc, kaolin, clay, calcium phosphate, mica, hectorite, zirconia, tungsten oxide, lithium fluoride, and calcium fluoride, and organic polymer particles such as styrene-based, acrylic-based, melamine-based, benzoguanamine-based, and silicone-based particles. These may be added to the easy-adhesion layer alone, or two or more types may be added in combination.

[0040] The coating liquid can be applied by any known method, such as reverse roll coating, gravure coating, kiss coating, roll brushing, spray coating, air knife coating, wire bar coating, and pipe doctor coating, which can be used alone or in combination.

[0041] The thickness of the polyester resin film is optional, but is usually 15 μm to 200 μm, preferably 20 μm to 100 μm, more preferably 25 μm to 95 μm, even more preferably 60 μm to 90 μm, and even more preferably 75 μm to 85 μm. If the thickness of the polyester-based resin film is less than 15 μm, the anisotropy of the mechanical properties of the film becomes significant, making it more susceptible to tears, breaks, etc., and the practicality of the film tends to decrease. On the other hand, if the thickness of the polyester-based resin film exceeds 200 μm, the thickness as a polarizing plate becomes too thick. When at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer is provided as described above, the total thickness including the layer may be within the above range.

[0042] The polyester resin film used in the present invention can be produced according to a general polyester film production method, for example, by the method described in JP-A-2021-103319, JP-A-2021-99521, etc. The retardation values ​​of Re1 to Re4 can be controlled within a specific range by appropriately setting the stretching ratio, stretching temperature, and film thickness. For example, a high retardation value can be easily obtained by increasing the stretching ratio, decreasing the stretching temperature, and increasing the film thickness. The retardation values ​​of Re1 to Re4 can be set by selecting the film formation conditions and thickness from the above conditions, taking into account the physical properties required for processing.

[0043] The material for forming the polyester-based resin film is not particularly limited, and polyethylene terephthalate or polyethylene naphthalate can be used, but other copolymer components may be included. From the viewpoint of controlling the retardation value of the polyester-based resin film, the material for forming the polyester-based resin film is preferably a polyethylene terephthalate resin.

[0044] <(Meth)acrylic resin film> The (meth)acrylic resin film is excellent in mechanical properties, solvent resistance, scratch resistance, light resistance, transparency, cost, etc. By using a (meth)acrylic resin film as a polarizer protective film, it is possible to improve the mechanical strength and reduce the thickness of a polarizing plate, a liquid crystal panel including the same, and a liquid crystal display device. In addition, by using the above-mentioned polyester resin film as one polarizer protective film and a (meth)acrylic resin film as the other polarizer protective film, it is possible to effectively suppress rainbow unevenness when viewed from an oblique direction. Furthermore, by using the above-mentioned polyester resin film as one polarizer protective film and a (meth)acrylic resin film having a small photoelastic coefficient as the other polarizer protective film, it is possible to effectively suppress light leakage occurring at the end of the polarizing plate due to shrinkage of the polarizer in a high-temperature environment.

[0045] The (meth)acrylic resin constituting the (meth)acrylic resin film means a material obtained by mixing a (meth)acrylic resin and additives added as necessary, and melt-kneading the mixture. In this specification, the term "(meth)acrylic resin" means either an acrylic resin or a methacrylic resin, and the "(meth)" in (meth)acrylic acid ester, (meth)acrylate, (meth)acryloyl, etc. has the same meaning.

[0046] The (meth)acrylic resin is preferably a polymer mainly composed of a (meth)acrylic acid ester. The (meth)acrylic resin may be a homopolymer of one type of (meth)acrylic ester, or may be a copolymer of a (meth)acrylic acid ester and another (meth)acrylic acid ester. Examples of the (meth)acrylic acid ester include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, and the number of carbon atoms in the alkyl group is usually about 1 to 8. Examples of polymerizable monomers that can be copolymerized with the (meth)acrylic acid ester include styrene-based monomers such as styrene and alkylstyrene; monofunctional monomers such as unsaturated nitriles such as acrylonitrile and methacrylonitrile; and polyfunctional monomers such as alkenyl esters of unsaturated carboxylic acids such as allyl (meth)acrylate and methallyl (meth)acrylate; dialkenyl esters of dibasic acids such as diallyl maleate; and unsaturated carboxylic acid diesters of glycols such as alkylene glycol di(meth)acrylate. The (meth)acrylic resin film may contain two or more kinds of (meth)acrylic resins.

[0047] When the (meth)acrylic resin film contains two or more kinds of (meth)acrylic resins, it is preferable that the syndiotacticity (rr) of at least one of the (meth)acrylic resins is 50% or more. From the viewpoint of increasing the toughness of the film and increasing the heat resistance and adhesion to the polarizer of the film, the syndiotacticity (rr) of the triad is preferably 55% or more, more preferably 60% or more, even more preferably 65% ​​or more, and even more preferably 70% or more. The syndiotacticity (rr) of the triad is usually 90% or less, and may be 85% or less.

[0048] The syndiotacticity (rr) of a triad is the proportion of two diads (diads) in a triad of three consecutive units that are both racemo (denoted as rr). The syndiotacticity (rr) of a triad (%) is calculated by the following formula: 1 The H-NMR spectrum is measured, and the area (X) of the region from 0.6 to 0.95 ppm and the area (Y) of the region from 0.6 to 1.35 ppm are measured from the spectrum when the internal standard TMS is set to 0 ppm, and the area is calculated as (X / Y)×100.

[0049] A (meth)acrylic resin having a triad syndiotacticity (rr) of 50% or more can be prepared, for example, according to the method described in WO 2016 / 080124.

[0050] When a (meth)acrylic resin having a triad syndiotacticity (rr) of 50% or more is contained, the content of the (meth)acrylic resin having a triad syndiotacticity (rr) of 50% or more, relative to the entire (meth)acrylic resin, is preferably 1 mass% or more and 50 mass% or less, more preferably 5 mass% or more and 40 mass% or less, even more preferably 10 mass% or more and 35 mass% or less, and still more preferably 15 mass% or more and 30 mass% or less, from the viewpoints of toughness of the film and adhesion to a polarizer.

[0051] As the (meth)acrylic resin, a (meth)acrylic resin having a ring structure can be used. Examples of the (meth)acrylic resin having a ring structure include a (meth)acrylic resin having a lactone ring structure, and a (meth)acrylic resin having a glutaric anhydride structure or a glutarimide structure. The (meth)acrylic resin having a ring structure is preferred because it has high heat resistance, high moist heat resistance, high transparency, and high mechanical strength when biaxially stretched. Examples of (meth)acrylic resins having a ring structure such as a lactone ring structure include those described in JP-A Nos. 2000-230016, 2001-151814, 2002-120326, 2002-254544, and 2005-146084. Examples of (meth)acrylic resins having a glutaric anhydride structure or a glutarimide structure include those described in JP-A-6-256537, JP-A-6-11615, and JP-A-2009-203348.

[0052] The (meth)acrylic resin having a lactone ring structure is preferably represented by the following general formula: <1> The ring structure is represented by the following formula: [ka] (In the formula, R 1 , R 2 and R 3 each independently represents a hydrogen atom or an organic residue having 1 to 20 carbon atoms. The organic residue may contain an oxygen atom.

[0053] General formula in the structure of (meth)acrylic resin having a lactone ring structure <1> The content of the lactone ring structure represented by the general formula in the structure of the (meth)acrylic resin having a lactone ring structure is preferably 5 to 90 mass %, more preferably 10 to 70 mass %, further preferably 10 to 60 mass %, and particularly preferably 10 to 50 mass %. <1> If the content of the lactone ring structure represented by the general formula in the structure of the (meth)acrylic resin having a lactone ring structure is less than 5 mass %, the heat resistance, solvent resistance, and surface hardness may be insufficient. <1> If the content of the lactone ring structure represented by the formula (I) is more than 90% by mass, the molding processability may be poor. The content of the lactone ring structure in the (meth)acrylic resin having the lactone ring structure can be determined by gas chromatography and dynamic TG measurement, for example, as described in JP-A-2006-171464.

[0054] The (meth)acrylic resin having a lactone ring structure is represented by the general formula: <1> The lactone ring structure may have a structure other than the lactone ring structure represented by the general formula: <1> The structure other than the lactone ring structure represented by the following general formula (I) is not particularly limited, but a method for producing a (meth)acrylic resin having a lactone ring structure includes the steps of: <2> A polymer structural unit (repeating structural unit) formed by polymerizing at least one monomer selected from the monomers represented by the following formula is preferred. [ka] (In the formula, R 4 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group, a -OAc group, a -CN group, or a -CO-R 5 represents an acetyl group; 5 represents a hydrogen atom or an organic residue having 1 to 20 carbon atoms.

[0055] General formula in (meth)acrylic resin structure having lactone ring structure <1> The content ratio of structures other than the lactone ring structure represented by the formula (I) is preferably 10 to 95% by mass, more preferably 10 to 90% by mass, even more preferably 40 to 90% by mass, and particularly preferably 50 to 90% by mass in the case of a polymer structural unit (repeating structural unit) formed by polymerizing a (meth)acrylic acid ester, and is preferably 0 to 30% by mass, more preferably 0 to 20% by mass, even more preferably 0 to 15% by mass, and particularly preferably 0 to 10% by mass in the case of a polymer structural unit (repeating structural unit) formed by polymerizing a hydroxyl group-containing monomer. In the case of a polymer structural unit (repeating structural unit) formed by polymerizing an unsaturated carboxylic acid, it is preferably 0 to 30% by mass, more preferably 0 to 20% by mass, even more preferably 0 to 15% by mass, and particularly preferably 0 to 10% by mass. <2> In the case of a polymer structural unit (repeating structural unit) formed by polymerizing a monomer represented by the following formula:

[0056] The (meth)acrylic resin having a lactone ring structure has a weight average molecular weight of preferably 1000 to 2000000, more preferably 5000 to 1000000, still more preferably 10000 to 500000, and particularly preferably 50000 to 500000. If the weight average molecular weight is outside the above range, it is not preferable from the viewpoint of molding processability.

[0057] Examples of thermoplastic resins to be mixed with the (meth)acrylic resin having a lactone ring structure include olefin polymers such as polyethylene, polypropylene, ethylene-propylene copolymer, and poly(4-methyl-1-pentene); halogen-containing polymers such as vinyl chloride and chlorinated vinyl resin; acrylic polymers such as polymethyl methacrylate; styrene polymers such as polystyrene, styrene-methyl methacrylate copolymer, styrene-acrylonitrile copolymer, and acrylonitrile-butadiene-styrene block copolymer; polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyamides such as nylon 6, nylon 66, and nylon 610; polyacetal; polycarbonate; polyphenylene oxide; polyphenylene sulfide; polyether ether ketone; polysulfone; polyethersulfone; polyoxybenzylene; polyamide imide; rubbery polymers such as ABS resins and ASA resins blended with polybutadiene rubber and acrylic rubber; and the like.

[0058] The (meth)acrylic resin having a glutaric anhydride structure or a glutarimide structure is preferably represented by the above general formula <2> and the following general formula: <3> The ring structure is represented by the following formula: [ka] (In the formula, R 1 and R 2 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; R 3 is hydrogen, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or a substituent containing an aromatic ring having 5 to 15 carbon atoms.

[0059] The content of the glutarimide structure is preferably 20% by mass or more, more preferably 20% by mass to 95% by mass, further preferably 40% by mass to 90% by mass, and particularly preferably 50% by mass to 80% by mass, of the (meth)acrylic resin having a glutarimide structure.

[0060] When the content of the glutarimide unit is within the above range, the heat resistance and transparency of the obtained glutarimide-containing (meth)acrylic resin are not reduced, and the moldability and mechanical strength when processed into a film are not extremely reduced.

[0061] On the other hand, if the content of glutarimide units is less than the above range, the heat resistance of the resulting glutarimide resin tends to be insufficient and the transparency tends to be impaired, whereas if the content is more than the above range, the heat resistance and melt viscosity tend to be unnecessarily high, resulting in poor moldability, extremely low mechanical strength during film processing, and impaired transparency.

[0062] The weight-average molecular weight of the (meth)acrylic resin having the glutarimide structure is not particularly limited, but is preferably 10,000 to 500,000. If it is within the above range, the molding processability will not decrease, and the mechanical strength will not be insufficient when processed into a film. On the other hand, if the weight-average molecular weight is smaller than the above range, the mechanical strength when made into a film tends to be insufficient. Also, if it is larger than the above range, the viscosity during melt extrusion will be high, the molding processability will decrease, and the productivity of the molded product will tend to decrease.

[0063] In addition, the (meth)acrylic resin may be a mixture or copolymer of a (meth)acrylic acid ester and an imide compound, which is a thermoplastic resin. Examples of the imide compound include maleimide, and N-substituted maleimides such as N-methylmaleimide, N-ethylmaleimide, Nn-propylmaleimide, Ni-propylmaleimide, Nn-butylmaleimide, Ni-butylmaleimide, Ns-butylmaleimide, Nt-butylmaleimide, Nn-pentylmaleimide, Nn-hexylmaleimide, Nn-heptylmaleimide, Nn-octylmaleimide, N-laurylmaleimide, N-stearylmaleimide, N-cyclopropylmaleimide, N-cyclobutylmaleimide, N-cyclopentylmaleimide, N-cyclohexylmaleimide, N-cycloheptylmaleimide, and N-cyclooctylmaleimide. These maleimide compounds may be used alone or in combination of two or more.

[0064] The (meth)acrylic resin preferably contains acrylic rubber particles in terms of the impact resistance and film formability of the film. The amount of acrylic rubber particles that can be contained in the (meth)acrylic resin is preferably 5% by mass or more, more preferably 10% by mass or more, based on 100% by mass of the total amount of the (meth)acrylic resin and the acrylic rubber particles. The upper limit of the amount of the acrylic rubber particles is not critical, but if the amount of the acrylic rubber particles is too large, the surface hardness of the film decreases, and when the film is subjected to a surface treatment, the solvent resistance to the organic solvent in the surface treatment agent decreases. Therefore, the amount of the acrylic rubber particles that can be contained in the (meth)acrylic resin is preferably 80% by mass or less, more preferably 60% by mass or less.

[0065] The acrylic rubber particles are particles that contain an acrylic acid ester-based elastic polymer as an essential component, and may be a single-layer structure that is substantially made of this elastic polymer alone, or may be a multi-layer structure that has this elastic polymer as one layer.Specifically, as this elastic polymer, a crosslinked elastic copolymer obtained by polymerization of monomers consisting of 50-99.9 mass% alkyl acrylate, 0-49.9 mass% of at least one other vinyl monomer that can be copolymerized therewith, and 0.1-10 mass% of a copolymerizable crosslinkable monomer is preferably used.

[0066] Examples of alkyl acrylates include methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate, and the number of carbon atoms in the alkyl group is usually about 1 to 8. Examples of other vinyl monomers copolymerizable with the alkyl acrylates include compounds having one polymerizable carbon-carbon double bond in the molecule, more specifically, methacrylic acid esters such as methyl methacrylate, aromatic vinyl compounds such as styrene, and vinyl cyanide compounds such as acrylonitrile. Examples of the copolymerizable crosslinkable monomers include crosslinkable compounds having at least two polymerizable carbon-carbon double bonds in the molecule, more specifically, (meth)acrylates of polyhydric alcohols such as ethylene glycol di(meth)acrylate and butanediol di(meth)acrylate, alkenyl esters of (meth)acrylic acid such as allyl (meth)acrylate and methallyl (meth)acrylate, and divinylbenzene.

[0067] In addition to the acrylic rubber particles, the (meth)acrylic resin may contain ordinary additives such as ultraviolet absorbers, organic dyes, pigments, inorganic dyes, antioxidants, antistatic agents, surfactants, etc. Among these, ultraviolet absorbers are preferably used to improve weather resistance. Examples of ultraviolet absorbers include 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(5-methyl-2-hydroxyphenyl)-2H-benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-amyl-2-hydroxyphenyl)-2H-benzotriazole, Benzotriazole-based ultraviolet absorbers such as 2-(2'-hydroxy-5'-tert-octylphenyl)-2H-benzotriazole; 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxy-4'-chlorobenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone; salicylic acid phenyl ester-based ultraviolet absorbers such as p-tert-butylphenyl salicylic acid ester and p-octylphenyl salicylic acid ester, and the like can be mentioned, and two or more of them may be used as necessary. When the (meth)acrylic resin contains an ultraviolet absorber, the amount thereof is usually 0.1% by mass or more, preferably 0.3% by mass or more, and preferably 2% by mass or less, based on 100% by mass of the total amount of the (meth)acrylic resin and the ultraviolet absorber.

[0068] As a method for obtaining a (meth)acrylic resin film, various generally known methods such as a method using a feed block and a method using a multi-manifold die can be used. Among them, a method of laminating via a feed block, performing multi-layer melt extrusion from a T-die, and contacting at least one side of the obtained laminated film-like material with a roll or belt to form a film is preferable in that a film with good surface properties can be obtained. In particular, from the viewpoint of improving the surface smoothness and surface gloss of the (meth)acrylic resin film, a method of contacting both sides of the laminated film-like material obtained by the above-mentioned multi-layer melt extrusion with a roll or belt surface to form a film is preferable. In the roll or belt used in this case, the roll surface or belt surface that comes into contact with the (meth)acrylic resin is preferably a mirror surface in order to impart smoothness to the (meth)acrylic resin film surface. The obtained film can be stretched to improve the film strength.

[0069] A film formed from a (meth)acrylic resin is unlikely to have a retardation in an unstretched state, but a retardation occurs when stretched, so that a retardation-reducing agent can be added to the (meth)acrylic resin to prevent the retardation from occurring even when stretched. Examples of the retardation-reducing agent include styrene-acrylonitrile copolymers. The retardation value can be controlled by the stretching ratio and the amount of the retardation-reducing agent added.

[0070] The thickness of the (meth)acrylic resin film is usually 1 μm or more and 80 μm or less, preferably 3 μm or more and 65 μm or less, more preferably 5 μm or more and 55 μm or less, even more preferably 7 μm or more and 45 μm or less, and particularly preferably 20 μm or more and 45 μm or less.

[0071] The glass transition temperature of the (meth)acrylic resin film is 100°C or higher, preferably 110°C or higher, more preferably 115°C or higher, and even more preferably 120°C or higher. The glass transition temperature is usually 170°C or lower. When the glass transition temperature of the (meth)acrylic resin film is 110°C or higher, the change in the molecular orientation of the (meth)acrylic resin in the (meth)acrylic resin film in a high-temperature environment is suppressed, and the change in the retardation value Re and the retardation value Rth in the thickness direction is suppressed, and the light leakage due to the shrinkage of the polarizer in a high-temperature environment tends to be more effectively suppressed. The retardation value Re and the retardation value Rth in the thickness direction of the (meth)acrylic resin film are retardation values ​​at a wavelength of 587 nm.

[0072] When the absolute value of the thickness direction retardation value Rth of the (meth)acrylic resin film is 15 nm or less, the (meth)acrylic resin film may serve both as an optical compensation film and a polarizer protective film in an IPS liquid crystal display device. The absolute value of the retardation value Rth in the thickness direction of the (meth)acrylic resin film is preferably 11 nm or less, more preferably 8 nm or less, and even more preferably 5 nm or less.

[0073] <Polarizer> A polarizer is a film that has the function of selectively transmitting linearly polarized light in one direction from natural light. Examples of polarizers include iodine-based polarizers in which iodine as a dichroic pigment is adsorbed and oriented on a polyvinyl alcohol-based resin film, dye-based polarizers in which a dichroic dye as a dichroic pigment is adsorbed and oriented on a polyvinyl alcohol-based resin film, and coated polarizers in which a dichroic dye in a lyotropic liquid crystal state is coated, oriented, and fixed. These polarizers are called absorption-type polarizers because they selectively transmit linearly polarized light in one direction from natural light and absorb linearly polarized light in the other direction.

[0074] The polarizer is not limited to an absorptive polarizer, and may be a reflective polarizer that selectively transmits linearly polarized light in one direction from natural light and reflects linearly polarized light in the other direction, or a scattering polarizer that scatters linearly polarized light in the other direction. However, an absorptive polarizer is preferred because it provides excellent visibility when the polarizing plate is applied to a liquid crystal display device or the like. Among these, the polarizer is more preferably a polyvinyl alcohol-based polarizer made of a polyvinyl alcohol-based resin, even more preferably a polyvinyl alcohol-based polarizer in which a dichroic pigment such as iodine or a dichroic dye is adsorbed and oriented in a polyvinyl alcohol-based resin film, and particularly preferably a polyvinyl alcohol-based polarizer in which iodine is adsorbed and oriented in a polyvinyl alcohol-based resin film.

[0075] A polyvinyl alcohol-based polarizer in which a dichroic dye is adsorbed and oriented in a polyvinyl alcohol-based resin film can usually be produced through a dyeing step of dyeing a polyvinyl alcohol-based resin film (hereinafter, also abbreviated as "PVA-based film" or "film") with a dichroic dye, a crosslinking step of treating the PVA-based film after the dyeing step in a crosslinking bath containing a crosslinking agent, and a stretching step of uniaxially stretching the PVA-based film.

[0076] The method for producing a polarizer may further include other steps in addition to those described above, such as a swelling step for swelling the film before the dyeing step, a water washing step for washing the film surface after the crosslinking step, a drying step for drying the PVA-based film after the crosslinking step, and a complementary color step for adjusting the hue of the film after the crosslinking step.

[0077] The stretching step, i.e. uniaxial stretching of the PVA-based film, may be carried out simultaneously with any of the other process steps listed above.

[0078] The various treatment steps included in the polarizer manufacturing method can be continuously carried out by continuously transporting the PVA-based film, which is the raw film, along the film transport path of the polarizer manufacturing device. The film transport path is equipped with equipment (treatment baths, furnaces, etc.) for carrying out the various treatment steps described above in the order in which they are carried out. The treatment bath refers to a bath that contains a treatment liquid for treating the PVA-based film, such as a swelling bath, dyeing bath, crosslinking bath, or washing bath.

[0079] The film transport path can be constructed by arranging guide rolls, nip rolls, etc. at appropriate positions in addition to the above-mentioned equipment. For example, guide rolls can be arranged before, after, or within each treatment bath, which allows the film to be introduced into and immersed in the treatment bath and drawn out from the treatment bath. More specifically, two or more guide rolls are provided in each treatment bath, and the film can be immersed in each treatment bath by transporting the film along these guide rolls.

[0080] Polyvinyl alcohol resins are obtained by saponifying polyvinyl acetate resins. Polyvinyl acetate resins include polyvinyl acetate, which is a homopolymer of vinyl acetate, as well as copolymers of vinyl acetate and other monomers that can be copolymerized with it. Examples of other monomers that can be copolymerized with vinyl acetate include unsaturated carboxylic acid compounds, olefin compounds, vinyl ether compounds, unsaturated sulfone compounds, and (meth)acrylamide compounds having an ammonium group.

[0081] The saponification degree of the polyvinyl alcohol resin is usually about 85 mol% or more and 100 mol% or less, preferably 99 mol% or more. The polyvinyl alcohol resin may be modified, and polyvinyl formal, polyvinyl acetal, etc. modified with aldehydes can also be used. The average polymerization degree of the polyvinyl alcohol resin is usually 1000 or more and 10000 or less, preferably 1500 or more and 5000 or less. The average polymerization degree of the PVA resin can be determined in accordance with JIS K 6726 (1994). If the average polymerization degree is less than 100, it is difficult to obtain a preferable polarizing performance, and if it exceeds 10000, the film processability may be poor.

[0082] The thickness of the PVA-based film as a raw film is, for example, about 10 μm or more and 100 μm or less, and from the viewpoint of thinning polarizers, polarizing plates, liquid crystal display devices, etc., it is preferably 60 μm or less, more preferably 50 μm or less, even more preferably 30 μm or less, and even more preferably 20 μm or less.

[0083] The PVA-based film, which is the raw film, can be prepared, for example, as a roll (wound product) of a long unstretched PVA-based film. In this case, the polarizer is also obtained as a long product. Each step of the polarizer manufacturing method will be described in detail below.

[0084] (Swelling process) The swelling treatment in the swelling step is a treatment that is carried out as necessary for the purpose of removing foreign matter from the PVA-based film, which is the raw film, removing plasticizers, imparting easy dyeing properties, plasticizing the film, etc. Specifically, it can be a treatment in which the PVA-based film is immersed in a swelling bath containing water. The PVA-based film may be immersed in one swelling bath, or may be immersed in two or more swelling baths sequentially. Before the swelling treatment, during the swelling treatment, or before and during the swelling treatment, the film may or may not be subjected to a uniaxial stretching treatment. The swelling bath may be water (for example, pure water) or an aqueous solution containing a water-soluble organic solvent such as an alcohol. The temperature of the swelling bath when the PVA-based film is immersed is usually about 10 to 70° C., preferably about 15 to 50° C., and the immersion time of the film is usually about 10 to 600 seconds, preferably about 20 to 300 seconds.

[0085] (dying process) The dyeing treatment in the dyeing step is a treatment performed for the purpose of adsorbing and orienting a dichroic dye on a PVA-based film, and specifically, it can be a treatment of immersing a PVA-based film in a dye bath containing a dichroic dye. The PVA-based film may be immersed in one dye bath, or may be immersed in two or more dye baths sequentially. In order to enhance the dyeability of the dichroic dye, the PVA-based film to be subjected to the dyeing step may be subjected to at least some degree of uniaxial stretching treatment. Instead of or in addition to the uniaxial stretching treatment before the dyeing treatment, a uniaxial stretching treatment may be performed during the dyeing treatment.

[0086] The dichroic dye can be iodine or a dichroic organic dye. Examples of the dichroic organic dye include Red BR, Red LR, Red R, Pink LB, Rubin BL, Bordeaux GS, Sky Blue LG, Lemon Yellow, Blue BR, Blue 2R, Navy RY, Green LG, Violet LB, Violet B, Black H, Black B, Black GSP, Yellow 3G, Yellow R, Orange LR, Orange 3R, Scarlet GL, Scarlet KGL, Congo Red, Brilliant Violet BK, Spra Blue G, Spra Blue GL, Spra Orange GL, Direct Sky Blue, Direct Fast Orange S, Fast Black, etc. The dichroic dye may be used alone or in combination of two or more kinds.

[0087] When iodine is used as the dichroic dye, an aqueous solution containing iodine and potassium iodide can be used in the dye bath. Instead of potassium iodide, other iodides such as zinc iodide may be used, or potassium iodide may be used in combination with other iodides. In addition, compounds other than iodides, such as boric acid, zinc chloride, cobalt chloride, etc., may be coexisted. When boric acid is added, it is distinguished from the crosslinking treatment described below in that it contains iodine. The content of iodine in the aqueous solution is usually about 0.003 to 1 part by mass per 100 parts by mass of water. In addition, the content of iodides such as potassium iodide is usually about 0.1 to 20 parts by mass per 100 parts by mass of water.

[0088] The temperature of the dye bath when the PVA-based film is immersed is usually about 10 to 45°C, preferably about 10 to 40°C, and more preferably about 20 to 35°C, and the immersion time of the film is usually about 30 to 600 seconds, and preferably about 60 to 300 seconds.

[0089] When a dichroic organic dye is used as the dichroic pigment, an aqueous solution containing the dichroic organic dye can be used in the dye bath. The content of the dichroic organic dye in the aqueous solution is usually 1×10 per 100 parts by mass of water. -4 ~10 parts by mass, preferably 1 × 10 -3 The dye bath may contain a dyeing assistant, for example, an inorganic salt such as sodium sulfate, a surfactant, etc. The dichroic organic dye may be used alone or in combination of two or more kinds. The temperature of the dye bath when the film is immersed is, for example, about 20 to 80°C, preferably about 30 to 70°C, and the immersion time of the film is usually about 20 to 600 seconds, preferably about 30 to 300 seconds.

[0090] (Crosslinking process) In the crosslinking step, the PVA-based film after the dyeing step is treated with a crosslinking agent. The crosslinking treatment is a treatment performed for the purpose of water resistance or hue adjustment by crosslinking, and specifically, it can be a treatment in which the film after the dyeing step is immersed in a crosslinking bath containing a crosslinking agent. The film may be immersed in one crosslinking bath, or may be immersed in two or more crosslinking baths in sequence. A uniaxial stretching treatment may be performed during the crosslinking treatment.

[0091] The crosslinking agent includes boric acid, and may further include other crosslinking agents such as glyoxal and glutaraldehyde. The content of boric acid in the crosslinking bath is usually about 0.1 to 15 parts by mass, preferably about 1 to 10 parts by mass, per 100 parts by mass of water. When the dichroic dye is iodine, the crosslinking bath preferably contains an iodide in addition to boric acid. The content of iodide in the crosslinking bath is usually about 0.1 to 20 parts by mass, preferably about 3 to 15 parts by mass, per 100 parts by mass of water. Examples of iodides include potassium iodide and zinc iodide. In addition, compounds other than iodides, such as zinc chloride, cobalt chloride, zirconium chloride, sodium thiosulfate, potassium sulfite, and sodium sulfate, may be present in the crosslinking bath. In the crosslinking step, when the PVA-based film is immersed in two or more crosslinking baths in sequence, the compositions and contents of the components contained in the crosslinking baths may be the same as each other, but are preferably different from each other.

[0092] From the viewpoint of obtaining a polarizer having higher optical properties, the temperature of the crosslinking bath when the PVA-based film is immersed is preferably 55.0° C. or higher, more preferably 58° C. or higher, and may be 58.5° C. or higher, and is usually 85.0° C. or lower, preferably 70.0° C. or lower, may be 65.0° C. or lower, may be 63.0° C. or lower, or may be 61.0° C. or lower. The immersion time for immersion in a crosslinking bath at this temperature is usually about 10 to 600 seconds, and preferably about 20 to 300 seconds.

[0093] When the PVA-based film is immersed in two or more crosslinking baths in sequence, the temperature and crosslinking time in at least one of the crosslinking baths may be within the above-mentioned range, and the temperature and crosslinking time in the other crosslinking baths may be within or outside the above-mentioned temperature and crosslinking time ranges. When the PVA-based film is immersed in two or more crosslinking baths in sequence, it is preferable to use a crosslinking bath with a temperature of 58.0°C or higher as the crosslinking bath to be immersed first. The temperature in the other crosslinking baths may be, for example, about 50 to 85°C, or about 50 to 70°C, and the immersion time of the film may be, for example, about 10 to 600 seconds, or about 20 to 300 seconds.

[0094] (Cleaning process) The cleaning treatment in the cleaning step is a treatment carried out as necessary for the purpose of removing excess crosslinking agent and chemicals such as dichroic dye attached to the PVA-based film, and is a treatment of cleaning the PVA-based film after the crosslinking step using a cleaning solution containing water. Specifically, it can be a treatment of immersing the PVA-based film after the crosslinking step in a cleaning bath (cleaning solution). The PVA-based film may be immersed in one cleaning bath, or may be immersed in two or more cleaning baths sequentially. Alternatively, the cleaning treatment may be a treatment of spraying the cleaning solution as a shower onto the PVA-based film after the crosslinking step, or the above-mentioned immersion and spraying may be combined.

[0095] The cleaning liquid may be water (e.g., pure water) or an aqueous solution containing a water-soluble organic solvent such as alcohols. The temperature of the cleaning liquid may be, for example, about 1 to 40° C., and the cleaning time may be, for example, about 1 to 60 seconds.

[0096] (drying process) The drying process is a drying treatment for promoting crosslinking of the PVA-based film while adjusting the moisture content of the PVA-based film. The drying treatment can be performed using a hot air dryer, an infrared heater, or a heated roll conveyor. The temperature of the drying treatment is usually about 30 to 110°C, and preferably 50 to 90°C. The time of the drying treatment is usually about 60 to 600 seconds, and preferably 120 to 600 seconds. The moisture content in the polarizer is adjusted by the drying treatment. The moisture content is usually about 5 to 20 mass% and preferably 8 to 15 mass% with respect to the total mass of the polarizer. When the moisture content is 5 mass% or more, the polarizer has sufficient flexibility, and therefore, damage after drying or breakage during conveyance can be suppressed. Furthermore, when the moisture content is 20 mass% or less, the polarizer has sufficient thermal stability. The drying treatment may be performed as necessary, and may not be performed.

[0097] (Stretching process) The stretching step is a step of stretching a PVA-based film, and the PVA-based film is preferably uniaxially stretched. As described above, the PVA-based film is uniaxially stretched in one or more stages of the processing steps provided in the polarizer manufacturing facility, such as the swelling step, dyeing step, crosslinking step, washing step, and drying step. The uniaxial stretching process may be either dry stretching in air or wet stretching in a bath, or both. The uniaxial stretching process may be inter-roll stretching, which involves longitudinal uniaxial stretching with a difference in peripheral speed between two nip rolls, hot roll stretching, tenter stretching, etc., but preferably includes inter-roll stretching. The total stretching ratio based on the raw film (when stretching is performed in two or more stages, the cumulative stretching ratio) is preferably 5.0 times or more, may be 5.5 times or more, may be 5.6 times or more, may be 5.8 times or more, may be 6.0 times or more, and is usually 8 times or less.

[0098] The contraction force of the polarizer in the absorption axis direction is less than 4.0 N / 2 mm. The contraction force of the polarizer in the absorption axis direction is preferably 3.7 N / 2 mm or less, more preferably 3.5 N / 2 mm or less, even more preferably 3.0 N / 2 mm or less, and even more preferably 2.5 N / 2 mm or less. The contraction force of the polarizer in the absorption axis direction is usually 0.5 N / 2 mm or more. When the contraction force of the polarizer in the absorption axis direction is less than 4.0 N / 2 mm, the contraction of the polarizer can be suppressed, and it is presumed that the stress on the (meth)acrylic resin film applied to the end of the polarizer at high temperatures can be reduced, and the associated change in phase difference of the (meth)acrylic resin film can be suppressed, thereby suppressing light leakage at the end of the polarizer. The contraction force of the polarizer in the absorption axis direction can be obtained as desired by adjusting the amount of boron contained in the crosslinking bath when manufacturing the polarizer, the immersion time in the crosslinking liquid, the temperature of the crosslinking bath, the total stretch ratio based on the original film, and the like. The contraction force in the absorption axis direction of the polarizer can be measured by the method described in the Examples section.

[0099] The thickness of the polarizer can be 30 μm or less, and is preferably 25 μm or less (for example, 20 μm or less, further 15 μm or less, further 10 μm or less, and further 8 μm or less). The thickness of the polarizer is usually 2 μm or more. Reducing the thickness of the polarizer is advantageous for reducing the thickness of the polarizing plate, and further the liquid crystal panel and liquid crystal display device to which the polarizer is applied.

[0100] The visibility-corrected polarization degree of the polarizer may be, for example, 99.00% or more, preferably 99.90% or more, more preferably 99.98% or more, and even more preferably 99.99% or more, and is usually 100% or less, for example, less than 100%. The luminosity-corrected transmittance of the polarizer may be, for example, 40% or more, preferably 41% or more, more preferably 42% or more, and even more preferably 43% or more, and is usually 50.0% or less, and may be, for example, less than 50.0%, or may be 49.0% or less.

[0101] The luminosity-corrected polarization degree and luminosity-corrected transmittance of a polarizer can be calculated by performing luminosity correction using a 2-degree visual field (C light source) of "JIS Z 8701" on the polarization degree and transmittance obtained using a spectrophotometer with an integrating sphere (e.g., "V7100" manufactured by JASCO Corporation).

[0102] <Adhesive layer> The first adhesive layer for bonding the polarizer and the polyester resin film, and the second adhesive layer for bonding the polarizer and the (meth)acrylic resin film may each be formed from a known adhesive composition. The first adhesive layer and the second adhesive layer may be formed from the same adhesive composition, or may be formed from different adhesive compositions. The first adhesive layer and the second adhesive layer may each be formed from an aqueous adhesive composition, or may be formed from a curable adhesive composition that is cured by heating or irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays.

[0103] Examples of the aqueous adhesive composition include those in which a polyvinyl alcohol resin or a urethane resin is dissolved in water as the main component, and those in which a polyvinyl alcohol resin or a urethane resin is dispersed in water as the main component. The aqueous adhesive composition may further contain a curing component or a crosslinking agent such as a polyaldehyde, a melamine compound, a zirconia compound, a zinc compound, a glyoxal compound, or a water-soluble epoxy resin. Examples of the aqueous adhesive composition include the adhesive composition described in JP 2010-191389 A, the adhesive composition described in JP 2011-107686 A, the composition described in JP 2020-172088 A, and the composition described in JP 2005-208456 A.

[0104] The curable adhesive composition is preferably an active energy ray curable adhesive composition that contains a curable (polymerizable) compound as a main component and is cured by irradiation with active energy rays. Examples of the active energy ray curable adhesive composition include a cationic polymerization type adhesive composition that contains a cationic polymerizable compound as a curable compound, a radical polymerization type adhesive composition that contains a radical polymerizable compound as a curable compound, and a hybrid type adhesive composition that contains both a cationic polymerizable compound and a radical polymerizable compound as a curable compound.

[0105] The cationically polymerizable compound is a compound or oligomer that undergoes a cationic polymerization reaction and hardens when exposed to active energy rays such as ultraviolet light, visible light, electron beams, and X-rays, or when heated. Specific examples of the cationically polymerizable compound include epoxy compounds, oxetane compounds, and vinyl compounds. Examples of epoxy compounds include alicyclic epoxy compounds such as 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate (compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule); aromatic epoxy compounds such as diglycidyl ether of bisphenol A (compounds having an aromatic ring and an epoxy group in the molecule); and aliphatic epoxy compounds such as 2-ethylhexyl glycidyl ether and 1,4-butanediol diglycidyl ether (compounds having at least one oxirane ring bonded to an aliphatic carbon atom in the molecule). Examples of the oxetane compound include compounds having one or more oxetane rings in the molecule, such as 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane.

[0106] The cationic polymerization adhesive composition preferably contains a cationic polymerization initiator. The cationic polymerization initiator may be a thermal cationic polymerization initiator or a photo-induced cationic polymerization initiator. Examples of the cationic polymerization initiator include aromatic diazonium salts such as benzenediazonium hexafluoroantimonate; aromatic iodonium salts such as diphenyliodonium tetrakis(pentafluorophenyl)borate; aromatic sulfonium salts such as triphenylsulfonium hexafluorophosphate; and iron-arene complexes such as xylene-cyclopentadienyl iron(II) hexafluoroantimonate. The content of the cationic polymerization initiator is usually 0.1 to 10 parts by mass relative to 100 parts by mass of the cationic polymerizable compound. Two or more kinds of cationic polymerization initiators may be included.

[0107] Examples of cationic polymerization adhesive compositions include the cationic polymerizable compositions described in JP 2016-126345 A and JP 2021-113969 A.

[0108] The radical polymerizable compound is a compound or oligomer that undergoes a radical polymerization reaction and hardens when exposed to active energy rays such as ultraviolet light, visible light, electron beams, and X-rays or when heated, and specifically includes a compound having an ethylenically unsaturated bond. Examples of the compound having an ethylenically unsaturated bond include a (meth)acrylic compound having one or more (meth)acryloyl groups in the molecule, and a vinyl compound having one or more vinyl groups in the molecule.

[0109] Examples of the (meth)acrylic compound include (meth)acrylate monomers having at least one (meth)acryloyloxy group in the molecule, (meth)acrylamide monomers, and (meth)acryl group-containing compounds obtained by reacting two or more functional group-containing compounds and having at least two (meth)acryloyl groups in the molecule, such as (meth)acrylic oligomers. The radical polymerization adhesive composition preferably contains a radical polymerization initiator. The radical polymerization initiator may be a thermal radical polymerization initiator or a photoradical polymerization initiator. Examples of the radical polymerization initiator include acetophenone-based initiators such as acetophenone and 3-methylacetophenone; benzophenone-based initiators such as benzophenone, 4-chlorobenzophenone, and 4,4'-diaminobenzophenone; benzoin ether-based initiators such as benzoin propyl ether and benzoin ethyl ether; thioxanthone-based initiators such as 4-isopropylthioxanthone; xanthone, fluorenone, and the like. The content of the radical polymerization initiator is usually 0.1 to 10 parts by mass relative to 100 parts by mass of the radical polymerizable compound. Two or more types of radical polymerization initiators may be included.

[0110] Examples of radical polymerization adhesive compositions include the radical polymerizable compositions described in JP 2016-126345 A, JP 2016-153474 A, and WO 2017 / 183335 A.

[0111] The active energy ray-curable adhesive composition may contain additives such as an ion trapping agent, an antioxidant, a chain transfer agent, a tackifier, a thermoplastic resin, a filler, a flow adjuster, a plasticizer, an antifoaming agent, an antistatic agent, a leveling agent, and a solvent, as necessary.

[0112] The polarizer and the polyester-based resin film can be bonded to each other by applying an adhesive composition to at least one of the bonding surfaces selected from the bonding surface of the polarizer and the bonding surface of the polyester-based resin film, laminating the two films with the coating layer of the adhesive composition therebetween, pressing the films together from above and below using a laminating roll or the like, and then drying the adhesive layer, curing it by irradiating it with active energy rays, or curing it by heating. To form a coating layer of the adhesive composition, various coating methods can be used, such as a die coater, a comma coater, a gravure coater, a wire bar coater, or a doctor blade coater. Alternatively, the adhesive composition may be allowed to flow while continuously supplying the polarizer and the polyester resin film so that the bonding surfaces of both are on the inner side.

[0113] Before forming the coating layer of the adhesive layer, at least one of the bonding surfaces selected from the bonding surface of the polarizer and the bonding surface of the polyester-based resin film may be subjected to an adhesion-improving treatment such as a saponification treatment, a corona treatment, a plasma treatment, a primer treatment, or an anchor coating treatment.

[0114] The lamination of the polarizer and the acrylic resin film can be carried out in the same manner as the lamination of the polarizer and the polyester resin film.

[0115] The light irradiation intensity when irradiating with active energy rays is determined depending on the composition of the active energy ray-curable adhesive composition and is not particularly limited, but is preferably 10 mW / cm 2 More than 1,000mW / cm 2 The irradiation intensity is preferably an intensity in a wavelength region effective for activating a photocationic polymerization initiator or a photoradical polymerization initiator. Irradiation is performed once or multiple times with such a light irradiation intensity, and the integrated light amount is 10 mJ / cm or less. 2 More preferably, it is 100 mJ / cm or more. 2 More than 1,000mJ / cm 2 It is more preferable to set it as follows:

[0116] The light source used to polymerize and cure the active energy ray-curable adhesive composition is not particularly limited, but examples include low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, xenon lamps, halogen lamps, chemical lamps, black light lamps, microwave excited mercury lamps, and metal halide lamps.

[0117] When the first adhesive layer and the second adhesive layer are formed from an aqueous adhesive composition, the thickness of the first adhesive layer and the second adhesive layer may be, for example, 5 μm or less, preferably 1 μm or less, and more preferably 0.5 μm or less, and may be 0.01 μm or more, and preferably 0.05 μm or more. When the first adhesive layer and the second adhesive layer are formed from a curable adhesive composition (preferably an active energy ray-curable adhesive composition), the thickness of the first adhesive layer and the second adhesive layer may be, for example, 15 μm or less, preferably 10 μm or less, and more preferably 5 μm or less, and may be 0.1 μm or more, preferably 0.3 μm or more, and more preferably 0.5 μm or more.

[0118] The first adhesive layer and the second adhesive layer are each preferably formed from a cationic polymerization adhesive composition. The first adhesive layer and the second adhesive layer may have the same thickness or different thicknesses, but it is preferable that they have the same thickness. Note that "the same thickness" includes an error of about 0.3 μm.

[0119] <Other configuration requirements> The polarizing plate of the present invention may further include an optically functional film to impart a desired optical function, such as a retardation film, a light collecting plate, a brightness enhancing film, a light diffusion layer (light diffusion film), etc. The optically functional film is attached to the polarizing plate via an adhesive layer or a pressure-sensitive adhesive layer. The adhesive layer and pressure-sensitive adhesive layer may be the same as the adhesive layer described above and the pressure-sensitive adhesive layer described below, respectively.

[0120] <Polarizing plate with adhesive layer> The present invention also relates to a polarizing plate with an adhesive layer, comprising the above polarizing plate and an adhesive layer. The polarizing plate with an adhesive layer can be applied to, for example, a liquid crystal display device. In the liquid crystal display device, the polarizing plate with an adhesive layer is disposed on the viewing side and / or the back side of a liquid crystal cell, which is an image display element.

[0121] An example of the layer structure of the polarizing plate with a pressure-sensitive adhesive layer of the present invention is shown in Fig. 6. The polarizing plate with a pressure-sensitive adhesive layer 2 shown in Fig. 6 includes a polarizing plate including a polyester resin film 10, a first adhesive layer 15, a polarizer 30, a second adhesive layer 25, and a (meth)acrylic resin film 20, in this order, and a pressure-sensitive adhesive layer 40. As in the polarizing plate 2 with a pressure-sensitive adhesive layer shown in FIG. 6, the pressure-sensitive adhesive layer 40 is preferably laminated on the surface of the (meth)acrylic resin film 20 opposite to the polarizer 30 .

[0122] The polarizing plate with the pressure-sensitive adhesive layer can be attached to a liquid crystal cell via the pressure-sensitive adhesive layer 40. That is, from the viewpoint of visibility, in a liquid crystal panel and a liquid crystal display device, the polarizing plate of the present invention is preferably disposed such that the (meth)acrylic resin film 20 side faces the liquid crystal cell.

[0123] The pressure-sensitive adhesive layer 40 may be laminated on either the polyester resin film 10 or the (meth)acrylic resin film 20, but is preferably laminated on the (meth)acrylic resin film 20 as described above. When the pressure-sensitive adhesive layer 40 is laminated on the (meth)acrylic resin film, the polyester resin film 10 is disposed on the opposite side (e.g., the viewing side) to the image display element. When an optically functional film is laminated on the (meth)acrylic resin film on the opposite side to the polarizer 30, the pressure-sensitive adhesive layer 40 may be further laminated on the optically functional film on the opposite side to the (meth)acrylic resin film 20.

[0124] Examples of the pressure-sensitive adhesive composition forming the pressure-sensitive adhesive layer include pressure-sensitive adhesive compositions containing, as a base polymer, a (meth)acrylic resin, a silicone resin, a polyester resin, a polyurethane resin, a polyether resin, etc. Among these, from the viewpoints of transparency, adhesive strength, reliability, heat resistance, reworkability, etc., a (meth)acrylic pressure-sensitive adhesive composition containing a (meth)acrylic resin is preferred.

[0125] The thickness of the pressure-sensitive adhesive layer is determined depending on the adhesive strength etc., and is, for example, from 1 μm to 50 μm, preferably from 2 μm to 40 μm, and more preferably from 3 μm to 30 μm. EXAMPLES

[0126] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.

[0127] (Production Example 1: Production of Polarizer) A long polyvinyl alcohol (PVA) raw film having a thickness of 45 μm [average polymerization degree 2400 or more, saponification degree 99.9 mol% or more] was continuously conveyed while being unwound from a roll, and was immersed in a swelling bath of pure water at 30 ° C. for a residence time of 90 seconds (swelling step). After that, the film pulled out from the swelling bath was immersed in a dyeing bath at 30 ° C. containing iodine with potassium iodide / boric acid / water at a ratio of 2 / 0.3 / 100 (mass ratio) for a residence time of 150 seconds (dyeing step). Next, the film pulled out from the dyeing bath was immersed in a first crosslinking bath at 60 ° C. with potassium iodide / boric acid / water at a ratio of 12 / 2 / 100 (mass ratio) for a residence time of 50 seconds, and then in a second crosslinking bath at 40 ° C. with potassium iodide / boric acid / water at a ratio of 12 / 2 / 100 (mass ratio) for a residence time of 10 seconds (crosslinking step). In the dyeing and crosslinking steps, the film was uniaxially stretched longitudinally by inter-roll stretching in the bath. The total stretch ratio based on the original film was 6.1 times. The film pulled out of the second crosslinking bath was immersed in a washing bath of pure water at 5°C for a residence time of 3 seconds (washing step). Thereafter, the film was dried at a temperature of 80°C for a residence time of 100 seconds to obtain polarizer 1. The obtained polarizer had a thickness of 19 μm.

[0128] (Production Example 2: Production of Polarizer) A long polyvinyl alcohol (PVA) raw film having a thickness of 45 μm [average polymerization degree 2400 or more, saponification degree 99.9 mol% or more] was continuously conveyed while being unwound from a roll, and was immersed in a swelling bath of pure water at 30 ° C. for a residence time of 90 seconds (swelling step). After that, the film pulled out from the swelling bath was immersed in a dyeing bath at 30 ° C. containing iodine with potassium iodide / boric acid / water at a ratio of 2 / 0.3 / 100 (mass ratio) for a residence time of 150 seconds (dyeing step). Next, the film pulled out from the dyeing bath was immersed in a first crosslinking bath at 61 ° C. with potassium iodide / boric acid / water at a ratio of 12 / 4 / 100 (mass ratio) for a residence time of 50 seconds, and then in a second crosslinking bath at 40 ° C. with potassium iodide / boric acid / water at a ratio of 12 / 4 / 100 (mass ratio) for a residence time of 10 seconds (crosslinking step). In the dyeing and crosslinking steps, the film was uniaxially stretched longitudinally by inter-roll stretching in the bath. The total stretch ratio based on the original film was 5.7 times. The film pulled out of the second crosslinking bath was immersed in a washing bath of pure water at 5°C for a residence time of 3 seconds (washing step). Thereafter, the film was dried at a temperature of 80°C for a residence time of 100 seconds to obtain polarizer 2. The thickness of the obtained polarizer 2 was 19 μm.

[0129] (Production Example 3: Production of Polarizer) A long polyvinyl alcohol (PVA) raw film having a thickness of 45 μm [average polymerization degree 2400 or more, saponification degree 99.9 mol% or more] was continuously conveyed while being unwound from a roll, and was immersed in a swelling bath of pure water at 30 ° C. for a residence time of 90 seconds (swelling step). After that, the film pulled out from the swelling bath was immersed in a dyeing bath at 30 ° C. containing iodine with potassium iodide / boric acid / water at a ratio of 2 / 0.3 / 100 (mass ratio) for a residence time of 150 seconds (dyeing step). Next, the film pulled out from the dyeing bath was immersed in a first crosslinking bath at 57 ° C. with potassium iodide / boric acid / water at a ratio of 12 / 4 / 100 (mass ratio) for a residence time of 50 seconds, and then in a second crosslinking bath at 40 ° C. with potassium iodide / boric acid / water at a ratio of 12 / 3 / 100 (mass ratio) for a residence time of 10 seconds (crosslinking step). In the dyeing and crosslinking steps, the film was uniaxially stretched longitudinally by inter-roll stretching in the bath. The total stretch ratio based on the original film was 5.7 times. The film pulled out of the second crosslinking bath was immersed in a washing bath of pure water at 5°C for a residence time of 3 seconds (washing step). Thereafter, the film was dried at a temperature of 80°C for a residence time of 100 seconds to obtain polarizer 3. The thickness of the obtained polarizer 3 was 19 μm.

[0130] (Production Example 4: Production of Polarizer) A long polyvinyl alcohol (PVA) raw film having a thickness of 45 μm [average polymerization degree 2400 or more, saponification degree 99.9 mol% or more] was continuously conveyed while being unwound from a roll, and was immersed in a swelling bath of pure water at 30 ° C. for a residence time of 90 seconds (swelling step). After that, the film pulled out from the swelling bath was immersed in a dyeing bath at 30 ° C. containing iodine with potassium iodide / boric acid / water at a ratio of 2 / 0.3 / 100 (mass ratio) for a residence time of 150 seconds (dyeing step). Next, the film pulled out from the dyeing bath was immersed in a first crosslinking bath at 53 ° C. with potassium iodide / boric acid / water at a ratio of 12 / 4 / 100 (mass ratio) for a residence time of 50 seconds, and then in a second crosslinking bath at 40 ° C. with potassium iodide / boric acid / water at a ratio of 12 / 4 / 100 (mass ratio) for a residence time of 10 seconds (crosslinking step). In the dyeing and crosslinking steps, the film was uniaxially stretched longitudinally by inter-roll stretching in the bath. The total stretch ratio based on the original film was 6.0 times. The film pulled out of the second crosslinking bath was immersed in a washing bath of pure water at 5°C for a residence time of 3 seconds (washing step). Thereafter, the film was dried at a temperature of 80°C for a residence time of 100 seconds to obtain polarizer 4. The thickness of polarizer 4 obtained as described above was 19 μm.

[0131] Measurement samples with a width of 2 mm and a length of 10 mm, with the absorption axis direction (MD, stretching direction) as the long side, were cut out from the polarizers obtained in Production Examples 1 to 4. The samples were set in a thermomechanical analyzer (TMA) "EXSTAR-6000" manufactured by SII NanoTechnology, Inc., and the shrinkage force in the long side direction (absorption axis direction) generated when the samples were held at 80°C for 4 hours while keeping the dimensions constant was measured. The results are shown in Table 1.

[0132] (Production Example 5: Production of polyethylene terephthalate resin (1)) While the esterification reactor was heated to 200°C, 86.4 parts of terephthalic acid and 64.6 parts of ethylene glycol were charged into the esterification reactor to obtain a mixture. While stirring the mixture, 0.017 parts of antimony trioxide, 0.064 parts of magnesium acetate tetrahydrate, and 0.16 parts of triethylamine were added as catalysts to the mixture. The gauge pressure in the esterification reactor was set to 0.34 MPa, and a pressurized esterification reaction was carried out under conditions of 240°C. The esterification reactor was then returned to normal pressure, and 0.014 parts of phosphoric acid were added. The temperature was then raised to 260°C over 15 minutes, and 0.012 parts of trimethyl phosphate were added to obtain a mixture. After 15 minutes, the mixture was dispersed using a high-pressure disperser, and after another 15 minutes, the esterification reaction product was transferred to a polycondensation reactor and subjected to a polycondensation reaction under reduced pressure at 280°C. After the polycondensation reaction was completed, the mixture was filtered using a Naslon filter with a 95% cutoff diameter of 5 μm, extruded from a nozzle in the form of a strand, cooled and solidified using cooling water that had been previously filtered (pore diameter: 1 μm or less), and cut into pellets to obtain polyethylene terephthalate resin (hereinafter referred to as PET (1)).

[0133] (Production Example 6: Production of polyethylene terephthalate resin (2)) 10 parts of the dried ultraviolet absorber (2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazin-4-one) and 90 parts of the PET (1) obtained in Production Example 5 were mixed and kneaded using an extruder to obtain a polyethylene terephthalate resin (2) containing an ultraviolet absorber (hereinafter referred to as PET (2)).

[0134] (Production Example 7: Preparation of Coating Solution for Forming Adhesive Layer) A water-dispersible sulfonate metal salt group-containing copolymer polyester resin was prepared by carrying out an ester exchange reaction and a polycondensation reaction in a conventional manner between a dicarboxylic acid component consisting of 46 mol % terephthalic acid, 46 mol % isophthalic acid, and 8 mol % sodium 5-sulfonatoisophthalate, and a glycol component consisting of 50 mol % ethylene glycol and 50 mol % neopentyl glycol. Next, 51.4 parts of water, 38 parts of isopropyl alcohol, 5 parts of n-butyl cellosolve, and 0.06 parts of nonionic surfactant were mixed to obtain a mixture. The mixture obtained was heated to 77°C and stirred, while adding 5 parts of the above-mentioned water-dispersible sulfonate metal salt group-containing copolymer polyester resin, and continued to stir until no resin lumps remained, to obtain a resin water dispersion. The obtained resin water dispersion was cooled to 25°C to obtain a uniform water-dispersible copolymer polyester resin solution with a solid content concentration of 5.0% by mass. 3 parts of aggregated silica particles were dispersed in 50 parts of water to obtain an aqueous dispersion of aggregated silica particles. 0.54 parts of the aqueous dispersion of aggregated silica particles was added to 99.46 parts of the water-dispersible copolymerized polyester resin liquid, and 20 parts of water was further added while stirring to obtain a coating liquid for forming an easy-adhesion layer.

[0135] (Production Example 8: Production of Protective Film 1) PET (3) was prepared by mixing 90 parts of PET (1) produced in Production Example 5 and 10 parts of PET (2) produced in Production Example 6, and was dried under reduced pressure at 135 ° C for 6 hours, and then fed to extruder 2 (for intermediate layer B). PET (1) was also dried and fed to extruder 1 (for outer layer A and outer layer C). PET (1) fed to extruder 1 and PET (3) fed to extruder 2 were each melted at 285 ° C. These two types of polymers were each filtered with a stainless steel sintered filter medium (nominal filtration accuracy 10 μm particles 95% cut) and laminated in a two-type three-layer merging block, extruded from a die in the form of a sheet, and then wrapped around a casting drum with a surface temperature of 30 ° C. using an electrostatic casting method, cooled and solidified, and an unstretched PET film was produced. At this time, the discharge amount of each extruder was adjusted so that the thickness ratio of A layer, B layer, and C layer was 10:80:10. Next, both sides of the obtained unstretched PET film were coated with 0.08 g / m2 of PET using the reverse roll method. 2 After the coating liquid for forming the easy-adhesion layer was applied so as to become The unstretched PET film on which this coating layer was formed was stretched 4.0 times in the width direction in a hot air zone at a temperature of 125°C in a tenter stretching machine while holding the ends of the film with clips. Next, while maintaining the width stretched in the width direction, it was treated at a temperature of 225°C for 10 seconds, and further subjected to a relaxation treatment of 3.0% in the width direction to obtain a uniaxially stretched PET film on which an easy-adhesion layer with a film thickness of about 80 μm was formed. This was named protective film 1.

[0136] (Production Example 9: Production of Protective Film 2) A mixture of 90 parts of a (meth)acrylic resin having a lactone ring structure and 10 parts of an acrylonitrile-styrene (AS) resin (lactone ring content: 28.5%) was extruded and stretched 2.0 times in length and 2.4 times in width to obtain a 40 μm thick acrylic resin film, which was designated as protective film 2.

[0137] <Example 1> One side of each of the protective films 1 and 2 was subjected to a corona treatment, and an epoxy-based ultraviolet-curable adhesive was applied to the corona-treated surface by using an adhesive applicator. The polarizer 1 obtained in the above-mentioned Production Example 1 was then superimposed on the coated layer surface, and then pressed and laminated using a lamination roll to obtain a polarizing plate precursor. At this time, the protective film 1 (polyester-based resin film) was laminated so that the stretching direction (width direction) and the absorption axis direction (stretching direction of the polarizer) were perpendicular to each other. A belt conveyor-equipped ultraviolet irradiation device (the lamp was a metal halide lamp manufactured by Eye Graphics Co., Ltd.) was used to irradiate the polarizing plate precursor with an integrated light amount of 200 mJ / cm from the protective film 2 ((meth)acrylic resin film) side. 2 The adhesive was cured by irradiating it with ultraviolet light so that the wavelength was (UVB) to obtain a polarizing plate. The polarizing plate had a layer structure of protective film 1 (polyester resin film) / adhesive layer / polarizer / adhesive layer / protective film 2 ((meth)acrylic resin film).

[0138] Next, a release film-attached adhesive layer having a (meth)acrylic adhesive layer (thickness 20 μm) on the release-treated surface of a release film was prepared. The release film-attached adhesive layer was laminated on the (meth)acrylic resin film side of the polarizing plate after corona treatment of the surface of protective film 2 ((meth)acrylic resin film), to obtain a polarizing plate with an adhesive layer. The polarizing plate with an adhesive layer has a structure of protective film 1 (polyester resin film) / adhesive layer / polarizer / adhesive layer / protective film 2 ((meth)acrylic resin film) / adhesive layer / release film.

[0139] <Example 2> A polarizing plate and a polarizing plate with a pressure-sensitive adhesive layer were obtained in the same manner as in Example 1, except that Polarizer 2 was used instead of Polarizer 1.

[0140] <Example 3> A polarizing plate and a polarizing plate with a pressure-sensitive adhesive layer were obtained in the same manner as in Example 1, except that Polarizer 3 was used instead of Polarizer 1.

[0141] <Comparative Example 1> A polarizing plate and a polarizing plate with a pressure-sensitive adhesive layer were obtained in the same manner as in Example 1, except that Polarizer 4 was used instead of Polarizer 1.

[0142] <Comparative Example 2> A polarizing plate and a polarizing plate with an adhesive layer were obtained in the same manner as in Comparative Example 1, except that a biaxially stretched polyethylene terephthalate (PET) protective film (manufactured by Mitsubishi Chemical Corporation) made of a polyester resin with a thickness of 38 μm was used instead of the protective film 1. The retardation values ​​Re1 to Re4 of the 38 μm-thick polyester resin film are as shown in Table 1. As in Example 1, this polarizing plate is bonded so that the stretching direction (width direction) of the biaxially stretched polyethylene terephthalate protective film and the absorption axis direction (stretching direction of the polarizer) are perpendicular to each other. The stretching direction (width direction) of the biaxially stretched polyethylene terephthalate protective film refers to the width direction when the film is unwound from the film roll.

[0143] (Measurement of Retardation Value of Polyester Resin Film) The retardation values ​​Re1 to Re4 of the polyester resin films used in the examples and comparative examples were measured at a wavelength of 587 nm using a retardation measuring device (KOBRA-HB-RESPC, manufactured by Oji Scientific Instruments Co., Ltd.). The results are shown in Table 1. Re1: A retardation value measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the surface of the polyester-based resin film and the measurement direction is 90°. Re2: Retardation value measured in a second arrangement in which the polyester-based resin film in the first arrangement is rotated 30° about its fast axis as the central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. Re3: A phase difference value measured in a third arrangement in which the polyester-based resin film in the first arrangement is rotated 30° around an axis that forms an angle of 45° with respect to the fast axis in the plane of the polyester-based resin film as the central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. Re4: Retardation value measured in a fourth arrangement in which the polyester-based resin film in the first arrangement is rotated 30° about its slow axis as the central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°.

[0144] (Measurement of Retardation Value in Thickness Direction of Polyester Resin Film) The thickness direction retardation value Rth of the polyester resin film was measured at a wavelength of 587 nm using a retardation measuring device (KOBRA-HB-RESPC, manufactured by Oji Scientific Instruments Co., Ltd.) with the angle between the surface of the polyester resin film and the measurement direction being 60°. Re1 / Rth was calculated from the thickness direction retardation value Rth and the retardation value Re1. The results are shown in Table 1.

[0145] (Measurement of rainbow unevenness) After peeling off the release film from the polarizing plate with the adhesive layer obtained in Example 1, the adhesive layer side was attached to a non-alkali glass substrate (thickness 0.7 mm, Corning Eagle XG) to obtain a glass-attached polarizing plate laminate. The above-mentioned glass-bonded polarizing plate laminate was placed in a backlight light source so that the glass substrate side was the light source, and the polarizing plate was visually observed in a dark place in an oblique direction from the polyester resin film side of the polarizing plate to check the visibility of rainbow unevenness and evaluate it according to the following criteria. Further, rainbow unevenness was similarly evaluated for the polarizing plates with the pressure-sensitive adhesive layer obtained in Examples 2 and 3 and the polarizing plates with the pressure-sensitive adhesive layer obtained in Comparative Examples 1 and 2. The results are shown in Table 1. ○: Weak rainbow unevenness ×: Strong rainbow unevenness

[0146] (Light leakage measurement) In Example 1, the polarizing plate with the adhesive layer was cut to a size of 150 mm x 90 mm. Either the long side or the short side of the cut polarizing plate with the adhesive layer was parallel to the absorption axis. After peeling off the release film from the cut polarizing plate with the adhesive layer (the long side direction is parallel to the absorption axis), the adhesive side was attached to one side of an alkali glass substrate (thickness 1.1 mm, manufactured by Nippon Sheet Glass Co., Ltd.), and further, the polarizing plate with the adhesive layer produced in Example 1 was cut in the same manner as above and attached to a surface of the glass substrate other than the polarizing plate attachment surface so that the transmission axes of the two polarizing plates were perpendicular to each other, thereby obtaining a glass-attached polarizing plate laminate. The glass-attached polarizing plate laminate has a structure of polyester resin film / adhesive layer / polarizing film / adhesive layer / acrylic resin film / adhesive layer / glass substrate / adhesive layer / acrylic resin film / adhesive layer / polarizing film / adhesive layer / polyester resin film. The obtained glass-bonded polarizing plate laminate was left in an environment at a temperature of 85°C for 100 hours, and then the glass-bonded polarizing plate laminate was placed in a backlight light source, and the in-plane uniformity of light leakage was visually observed and evaluated in a dark place according to the following criteria. The light leakage was also evaluated in the same manner for the polarizing plates with pressure-sensitive adhesive layers of Examples 2 and 3 and Comparative Examples 1 and 2. The results are shown in Table 1. ◎: Light leakage from the edge is very weak ○: Light leakage from the edge is weak ×: Strong light leakage at the edge

[0147] [Table 1] [Explanation of symbols]

[0148] 1 polarizing plate, 2 polarizing plate with adhesive layer, 10 polyester resin film, 15 first adhesive layer, 20 (meth)acrylic resin film, 25 second adhesive layer, 30 polarizer, 40 adhesive layer, 100 polyester resin film (first arrangement), 110 polyester resin film (second arrangement), 120 polyester resin film (third arrangement), 130 polyester resin film (fourth arrangement), 201 light source, 202 observation device, 210 measurement direction, 300, 310, 320 central axis, 400 fast axis of polyester resin film in first arrangement, 500 slow axis of polyester resin film in first arrangement.

Claims

1. A polarizing plate including, in this order, a polyester resin film, a first adhesive layer, a polarizer, a second adhesive layer, and a (meth)acrylic resin film, The contraction force of the polarizer in the absorption axis direction is less than 4.0 N / 2 mm; The polyester resin film is a polarizing plate in which the retardation value Re defined by the formula (1) satisfies the following [i] to [iv]. Re=(n x -n y )×d (1) [In the formula, n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as a central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated by 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the retardation value Re4 is 7000 nm or more.

2. 2. The polarizing plate according to claim 1, wherein the polyester resin film has a thickness of 60 [mu]m or more.

3. 2. The polarizing plate according to claim 1, wherein the ratio of a retardation value Re1 to a retardation value Rth in the thickness direction of the polyester resin film defined by the formula (2) is 0.5 or more. Rth=〔(n x +n y ) / 2-n z 〕×d (2) [In the formula, n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and n z represents the refractive index in the thickness direction of the film, and d represents the thickness of the film.

4. A polarizing plate with a pressure-sensitive adhesive layer, comprising the polarizing plate according to any one of claims 1 to 3 and a pressure-sensitive adhesive layer, A polarizing plate with a pressure-sensitive adhesive layer, wherein the pressure-sensitive adhesive layer is laminated on a surface of the (meth)acrylic resin film opposite to the polarizer.

5. A liquid crystal display comprising the pressure-sensitive adhesive layer-attached polarizing plate according to claim 4.

Citation Information

Patent Citations

  • Resin film, method for producing the same, polarizing plate, and liquid crystal display

    JP2013028755A

  • Polarizing film and manufacturing method thereof and polarizer

    JP2013148806A

  • Polarizing plate and image display device

    JP2014206702A

  • Liquid crystal display device

    JP2014219438A

  • Polarizing film, polarizing plate, and liquid crystal panel

    JP2015222368A