Capacitor and electrode active material
A nitrogen-containing carbon material with specific structural features and pore distribution addresses the trade-off between initial capacity and reliability in organic electrolyte capacitors, enhancing performance through improved ion movement and stability.
Patent Information
- Application Number
- JP2023055414
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing electrode materials containing nitrogen face a trade-off between initial capacity and reliability in organic electrolyte electric double layer capacitors due to the deterioration of active species at high voltages.
Incorporating a nitrogen-containing carbon material with specific structural features, including 6-membered rings with carbonyl carbons and/or nitrogen atoms, and a tailored pore volume distribution, enhances both initial capacity and reliability by improving ion movement and structural stability.
The capacitor achieves both high initial capacity and reliability by utilizing a nitrogen-containing carbon material with optimized pore distribution and structural stability, suitable for organic electrolyte electric double layer capacitors.
Smart Images

Figure 2024142981000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to capacitors and electrode active materials. [Background technology]
[0002] Patent Document 1 proposes "an electrode material made of a nitrogen-containing carbon foam having a nitrogen content of 2.5 to 30 wt % obtained by carbonizing a melamine resin foam at a temperature of 600 to 1200° C. in an inert atmosphere."
[0003] Patent Document 2 describes a method for producing a polyester fiber having a nitrogen content of 0.5 to 30 mass % and a specific surface area of 200 to 3000 m 2 The paper proposes a nitrogen-containing porous carbon material with a carbon content of 1.0 to 1.5 carbon atoms / g. The paper describes the nitrogen-containing porous carbon material as being obtained by mixing melamine and magnesium citrate, heating the mixture to 700°C or higher in an inert atmosphere, cooling the mixture, and washing the mixture with acid.
[0004] Patent Document 3 proposes "a method for producing a carbon material, comprising the steps of: encapsulating a guest substance in pores of an organic covalent bond structure; and heating the organic covalent bond structure encapsulating the guest substance to carbonize it." [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-269505 A [Patent Document 2] International Publication No. 2011 / 065484 Brochure [Patent Document 3] International Publication No. 2020 / 175616 Brochure Summary of the Invention [Problem to be solved by the invention]
[0006] Patent Documents 1 to 3 propose electrode materials containing nitrogen. Electrode materials containing nitrogen can exhibit high capacitance. However, part of such capacitance is usually pseudocapacitance accompanied by Faraday reaction. Even if a material has good reliability in an electric double layer capacitor using an aqueous electrolyte, a trade-off relationship between initial capacitance and reliability is recognized in an organic electrolyte electric double layer capacitor. This is thought to be because an organic electrolyte electric double layer capacitor is charged to a high voltage of, for example, 3V or more, and therefore the active species of the pseudocapacitance is easily deteriorated. [Means for solving the problem]
[0007] One aspect of the present invention relates to a capacitor comprising a first electrode, a second electrode, and an electrolyte solution, wherein at least one of the first electrode and the second electrode is an electrode containing a nitrogen-containing carbon material, and the nitrogen-containing carbon material contains a six-membered ring, and the six-membered ring contains one or more carbonyl carbons and / or two or more nitrogen atoms.
[0008] Another aspect of the present invention relates to a capacitor including a first electrode, a second electrode, and an electrolyte solution, wherein at least one of the first electrode and the second electrode is an electrode containing a nitrogen-containing carbon material, and a differential pore volume distribution A of the nitrogen-containing carbon material has a first peak in the range of 1.0 nm or more and less than 2.0 nm.
[0009] Yet another aspect of the present invention relates to an electrode active material comprising a nitrogen-containing carbon material, the nitrogen-containing carbon material comprising a six-membered ring, the six-membered ring comprising one or more carbonyl carbons and / or two or more nitrogen atoms.
[0010] Yet another aspect of the present invention relates to an electrode active material comprising a nitrogen-containing carbon material, wherein a differential pore volume distribution A of the nitrogen-containing carbon material has a first peak in the range of 1.0 nm or more and less than 2.0 nm. Effect of the Invention
[0011] According to the present disclosure, a capacitor capable of achieving both initial capacitance and reliability can be obtained. [Brief description of the drawings]
[0012] [Figure 1] 1 is a partially cutaway perspective view of an organic electrolyte electric double layer capacitor according to the present invention. [Diagram 2] FIG. 2 is a diagram showing a differential pore volume distribution of a nitrogen-containing carbon material. [Diagram 3] FIG. 1 is a graph showing the Log differential pore volume distribution of a capacitor electrode containing a nitrogen-containing carbon material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] In the following, the embodiment of the present disclosure will be described by way of example, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials may be exemplified, but other numerical values and materials may be applied as long as the effects of the present disclosure are obtained. In this specification, the description "numerical value A to numerical value B" includes numerical value A and numerical value B, and can be read as "numerical value A or more and numerical value B or less." In the following description, when a lower limit and an upper limit of a numerical value related to a specific physical property or condition are exemplified, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined as long as the lower limit is not equal to or greater than the upper limit. When multiple materials are exemplified, one of them may be selected and used alone, or two or more of them may be used in combination.
[0014] The capacitor according to the present disclosure (hereinafter also referred to as "capacitor (NC)") includes a first electrode, a second electrode, and an electrolyte. The "capacitor" may be read as "condenser." The capacitor refers to an electricity storage device such as an electric double layer capacitor or a lithium ion capacitor.
[0015] At least one of the first electrode and the second electrode is an electrode containing a nitrogen-containing carbon material according to the present disclosure (hereinafter also referred to as "carbon material (NC)") as an electrode active material (hereinafter also referred to as "active material"). The carbon material (NC) contains a six-membered ring (hereinafter also referred to as "six-membered ring (NC)") having the characteristics described above or below, or has a differential pore volume distribution having the characteristics described above or below.
[0016] The six-membered ring (NC) contains one or more carbonyl carbons and / or two or more nitrogen atoms. The six-membered ring (NC) may contain a carbon atom bonded to two nitrogen atoms. The six-membered ring (NC) may form a conjugated system involving all six atoms constituting the six-membered ring. The six-membered ring (NC) may contain both one or more carbonyl carbons and two or more nitrogen atoms. The six-membered ring containing both a carbonyl carbon and a nitrogen atom may be a six-membered ring containing two or three carbonyl carbons and two or three nitrogen atoms. The six-membered ring may have a 1,3,5-trione ring, may have a triazine ring, or may have both a 1,3,5-trione ring and a triazine ring structure (e.g., an isocyanuric ring). The six-membered ring may contain at least one selected from the group consisting of an isocyanuric ring, a triazine ring, and a 1,3,5-trione ring.
[0017] The six-membered ring (NC) is a structure derived from the raw material of the carbon material (NC). On the other hand, the carbon material (NC) is produced by carbonizing the raw material at high temperature. Therefore, the six-membered ring (NC) structure may not be clearly detected. Even in such cases, the carbon material (NC) or its raw material can be identified by measuring the differential pore volume distribution of the carbon material (NC) or an electrode made using the carbon material (NC).
[0018] The electrode containing the carbon material (NC) is hereinafter also referred to as the electrode (E). The electrode (E) may include an active layer and a current collector supporting the active layer. There is no particular limitation on the current collector, and a known current collector used in electrodes of electrochemical devices may be used.
[0019] <Carbon material (NC)> Carbon materials (NC) function as active materials that express capacitance by doping and dedoping ions. The concept of doping ions into carbon materials (NC) includes the adsorption of ions into the carbon material (NC), the occlusion of ions by the carbon material (NC), and the chemical interaction between the carbon material (NC) and ions. The concept of dedoping ions from the carbon material (NC) includes the desorption of ions from the carbon material (NC), the release of ions from the carbon material (NC), and the release of chemical interactions between the carbon material (NC) and ions.
[0020] Here, doping of ions into the carbon material (NC) mainly refers to the adsorption of ions into the carbon material (NC), and dedoping of ions from the carbon material (NC) mainly refers to the desorption of ions from the carbon material (NC). When ions are adsorbed into the carbon material (NC), an electric double layer is formed, and capacitance is expressed. In other words, the electrode (E) is a polarizable electrode. However, the electrode (E) may be an electrode in which the Faraday reaction contributes to the capacitance.
[0021] The carbon material (NC) is suitable as an active material for an electric double layer capacitor containing an organic electrolyte. An electric double layer capacitor (hereinafter also referred to as "EDLC(NC)") containing the carbon material (NC) and an organic electrolyte can exhibit excellent initial capacity. The EDLC(NC) can have low low-temperature resistance. The EDLC(NC) has excellent reliability.
[0022] The six-membered ring (NC) has excellent structural stability. It is believed that the excellent structural stability contributes to the improvement of the reliability of EDLC (NC). The nitrogen atom contained in the six-membered ring (NC) is believed to contribute to the expression of excellent initial capacity or the reduction of low-temperature resistance of EDLC (NC). It is presumed that such a contribution is related to the presence of a carbon atom bonded to the two nitrogen atoms that compose the six-membered ring (NC). Carbon materials (NC) are not only likely to express pseudocapacitance accompanied by a Faraday reaction, but are also believed to have high reversibility of such pseudocapacitance.
[0023] The six-membered ring (NC) preferably contains, for example, an isocyanuric ring. The isocyanuric ring has excellent structural stability. The isocyanuric ring contains three carbonyl carbon atoms bonded to two nitrogen atoms. The isocyanuric ring is particularly stable in an environment with little moisture or protic solvent.
[0024] The six-membered ring (NC) preferably contains, for example, a triazine ring. The triazine ring has excellent structural stability. The triazine ring contains three carbon atoms bonded to two nitrogen atoms. The triazine ring is particularly stable in an environment with little moisture or protic solvent.
[0025] The six-membered ring (NC) may have an aromatic ring directly bonded thereto as a substituent. The aromatic ring of the substituent may be bonded to the 1-, 3-, and 5-positions of the six-membered ring (NC). The aromatic ring of the substituent may be a phenyl group. Such a phenyl group may further have a substituent. The substituent bonded to the phenyl group may be a C1-C6 alkyl group such as a methyl group, an ethyl group, or a propyl group, or a C1-C6 alkenyl group.
[0026] The carbon material (NC) may further include a 1,3,5-trione ring (hereinafter also referred to as a "trione ring"). The double bond oxygen of the trione ring is considered to contribute to the excellent initial capacity or reduced low-temperature resistance of the EDLC (NC). The trione ring has excellent structural stability, and is particularly stable in an environment with little moisture or protic solvent.
[0027] Since an isocyanuric ring contains three carbon atoms bonded to two nitrogen atoms and is also a trione ring, carbon materials containing isocyanuric rings (NCs) are promising active materials.
[0028] Nitrogen content in carbon material (NC) N is preferably 2% by mass or more, more preferably 4% by mass or more and 20% by mass or less. In this case, the content of six-membered rings containing two or more nitrogen atoms is sufficiently high, so that a high capacity can be expected. The structural stability of the carbon material (NC) is also sufficiently improved.
[0029] Oxygen content in carbon material (NC) C OX is preferably 6% by mass or more, more preferably 8% by mass or more and 18% by mass or less. In this case, the content of trione rings is sufficiently high, so that a high capacity can be expected. The structural stability of the carbon material (NC) is also sufficiently improved.
[0030] Nitrogen content C N Oxygen content C OX Ratio of: C OX / C N is preferably 0.25 or more and 3.5 or less. In this case, the carbon material (NC) contains nitrogen atoms and oxygen atoms in a well-balanced manner.
[0031] The differential pore volume distribution of the carbon material (NC) may have a first peak in the range of 1.0 nm or more and less than 2.0 nm. The differential pore volume distribution of the carbon material (NC) may have a second peak in the range of 0.5 nm or more and less than 1.0 nm. The presence of such small pores is advantageous for the movement of ions inside the electrode.
[0032] The differential pore volume distribution of the carbon material (NC) may have a third peak in the range of 2.0 nm or more and less than 3.0 nm. Furthermore, the differential pore volume distribution of the carbon material (NC) may have a fourth peak in the range of 3.0 nm or more and less than 6.0 nm. Furthermore, the differential pore volume distribution of the carbon material (NC) may have a broad fifth peak in the range of 6.0 nm or more and less than 20 nm. The presence of the third peak, fourth peak, and fifth peak in addition to the first and second peaks makes the pore volume distribution hierarchical, and creates an environment more favorable for the movement of ions.
[0033] However, the frequency of the first peak is desirably greater than the frequency of the second peak, and is desirably at least two or three times the frequency of the second peak. Similarly, the frequency of the first peak is desirably greater than the frequency of the third peak, and is desirably at least two or three times the frequency of the third peak.
[0034] In the differential pore volume distribution of carbon material (NC), the total pore volume in the range of 20 nm or less is 0.6 cm 3 / g~1.4cm 3 / g, in which case an environment more favorable for ion migration is formed.
[0035] The reliability of a capacitor (NC) can be evaluated by a float charge test in which a certain voltage is steadily applied to the capacitor at a high temperature of, for example, about 60°C. The reliability of a capacitor can be determined by the capacity retention rate and the resistance increase rate of the capacitor compared to the initial state when float charging is continuously performed for a certain period of time. The higher the capacity retention rate and the smaller the resistance increase rate, the higher the reliability.
[0036] The pore volume distribution of the carbon material (NC) is thought to be related to the improvement of the reliability of the capacitor (NC). For example, the presence of mesopores with a pore size of 20 nm or less in the differential pore volume distribution of the carbon material (NC) is thought to contribute to the improvement of ion diffusivity. When the carbon material (NC) has a hierarchical arrangement of micropores, mesopores, and macropores in a well-balanced manner, the ion diffusivity is significantly improved.
[0037] The reliability of the capacitor (NC) is also affected by the volume distribution of macropores in the differential pore volume distribution of the electrode containing the carbon material (NC). For example, it is believed that macropores in the range of 0.1 μm to 3 μm have a large effect on ion diffusivity. The Log differential pore volume distribution of the electrode containing the carbon material (NC) may have a broad peak in the range of 0.1 μm to 3 μm. This, together with the micropores and mesopores in the differential pore volume distribution of the carbon material (NC), results in a hierarchical distribution of pores, creating an environment more favorable for ion movement.
[0038] The differential pore volume distribution of the carbon material (NC) can be obtained by, for example, analyzing the adsorption isotherm measured by a gas adsorption method using nitrogen gas by the BJH (Barrett Joyner Hallenda) method or the DFT (Density Functional Theory) method. The total pore volume is the integrated value of the pore volume in the pore volume distribution obtained by analysis by the BJH method.
[0039] In the case of a sample in which an electrode containing a carbon material (NC) is removed from a capacitor, the sample is immersed in a highly volatile solvent (e.g., dimethyl carbonate), washed under a reduced pressure of less than 0.1 MPa, and dried under a reduced pressure of less than 0.1 MPa for 2 hours or more. Drying can be performed, for example, at room temperature.
[0040] The pore volume distribution of the carbon material (NC) can be measured, for example, using a BELSORP 28SA device available from BEL Japan Co., Ltd. The Dollimore Heal method (DH method), which is calculated based on the capillary condensation theory (Kelvin's formula), can be used as an analytical theory for mesopores. The pore volume distribution of micropores can be analyzed using the MP method (R. SH. MICHAIL et al., J. Coll. Inter. Sci., 26 (1968) 45). In the MP method, the pores are assumed to have a slit shape, and the sum of the pore volumes with the slit width can be obtained as a function of the slit width. The pore volume distribution may also be calculated using the DFT method. The DFT method is one of the methods also known as the molecular dynamics simulation method, and is a method of analyzing the adsorption phenomenon from the statistical and thermodynamic theory at the molecular level. The autosorb-iQ device manufactured by Anton Paar can be used as the device.
[0041] The Log differential pore volume distribution of the electrode may be measured using a mercury porosimeter in accordance with, for example, "Method for testing pore size distribution of molded bodies by mercury intrusion method for fine ceramics" in accordance with JIS R1655:2003. In the mercury porosimeter, mercury is injected into pores in the electrode sample under low pressure to measure large diameter pores, and then mercury is made to penetrate deeper into the pores under high pressure. The low pressure state is reduced to about 50 μmHg by a vacuum pump. As an example of a method for injecting mercury into the sample, a cell that contains the sample and has an inlet for mercury is used. As an example of a sample, a portion of an electrode having a current collector and an active layer (electrode layer) formed in the same manner as in this embodiment, with a size of 20 mm x 50 mm, is prepared by cutting out the active layer (electrode layer) of the electrode. Under high pressure, mercury is injected into the sample by pressurizing it to about 230 MPa.
[0042] The carbon material (NC) can be prepared or produced, for example, by using polyisocyanate as a raw material. The polyisocyanate preferably has an aromatic ring. Among them, toluene diisocyanate can be easily reacted with toluene diisocyanate through the trimerization reaction shown below:
[0043] [ka]
[0044] A crosslinked product having an isocyanuric ring is formed by the above-mentioned method. The isocyanuric ring of the crosslinked product of the polyisocyanate having an aromatic ring has an aromatic ring bonded to a nitrogen atom as a substituent. Such a crosslinked product is suitable as a raw material for a carbon material (NC) having excellent structural stability.
[0045] By adding a polyhydric alcohol to polyisocyanate or toluene diisocyanate, a crosslinked material with excellent thermal decomposition properties (easily carbonized) can be produced. When the easily carbonized crosslinked material is heated under an inert atmosphere, the desired carbon material (NC) can be obtained at low cost.
[0046] The polyhydric alcohol is preferably one having a structure that easily forms a space between the isocyanuric rings. For example, glycerin, triglycerin, polyalkylene glycol, alkanediol (HO-(CH 2 ) n -OH) is preferred. Alkanediol (HO-(CH 2 ) n The carbon number (n) of -(CH) may be, for example, 2 to 10. An isocyanate group and an alcoholic hydroxyl group react to form a urethane bond. A flexible linking group can be formed inside the crosslinked material via the urethane bond. For example, when an alkanediol is used, the linking group is -(CH 2 ) n -Has a structure.
[0047] The amount of polyhydric alcohol added to polyisocyanate may be appropriately selected, but the amount of polyhydric alcohol is, for example, 100 to 1000 parts by mass, 200 to 700 parts by mass, or 250 to 500 parts by mass per 100 parts by mass of polyisocyanate. Since polyisocyanate is expensive, it is desirable to increase the proportion of polyhydric alcohol in terms of cost.
[0048] The inert atmosphere for carbonizing the crosslinked body may be a non-oxidizing atmosphere, and may be a reduced pressure atmosphere (for example, 0.1 MPa or less (preferably 10 Pa or less)), a reducing atmosphere (for example, a hydrogen atmosphere of 0.01 MPa or less), an inert gas atmosphere (for example, N 2 , Ar, Ne, He, etc.) may be used.
[0049] The heating temperature of the crosslinked body in an inert atmosphere may be 800° C. or less, or 750° C. or less. When the heating temperature exceeds 800° C., the nitrogen content C of the carbon material (NC) N and a decrease in six-membered rings containing a carbonyl carbon and / or two or more nitrogen atoms.
[0050] The heating time is appropriately selected depending on the heating conditions, but may be, for example, about 0.5 to 5 hours.
[0051] <Organic electrolyte> The organic electrolyte solution contains a non-aqueous solvent and an organic salt that dissolves in the non-aqueous solvent. The non-aqueous solvent means a solvent other than water, and includes organic solvents. The organic salt is a salt in which at least one of the anion and the cation contains an organic substance. The concentration of the organic salt in the organic electrolyte solution may be, for example, 0.5 to 2.0 mol / L. Compared with aqueous electrolyte solutions, organic electrolyte solutions have a wider potential window (voltage resistance) and can withstand high voltages, which greatly contributes to improving the energy density and power density of the capacitor.
[0052] As the non-aqueous solvent, a high boiling point solvent is preferable. For example, lactones such as γ-butyrolactone, carbonates such as propylene carbonate, polyhydric alcohols such as ethylene glycol and propylene glycol, cyclic sulfones such as sulfolane, amides such as N-methylacetamide, N,N-dimethylformamide, and N-methyl-2-pyrrolidone, esters such as methyl acetate, ethers such as 1,4-dioxane, ketones such as methyl ethyl ketone, and formaldehyde can be used. Among them, aprotic solvents are preferable from the viewpoint of increasing the structural stability of the carbon material (NC), and 80 mass % or more of the non-aqueous solvent may be an aprotic solvent.
[0053] An example of an organic salt in which the cation contains an organic substance is an onium salt such as a quaternary ammonium salt. An example of an organic salt in which the anion (or both ions) contains an organic substance is a salt of a carboxylic acid and an onium salt (a carboxylic acid onium salt). Specific examples of the carboxylic acid onium salt include trimethylamine maleate, triethylamine borodisalicylate, ethyldimethylamine phthalate, mono 1,2,3,4-tetramethylimidazolinium phthalate, and mono 1,3-dimethyl-2-ethylimidazolinium phthalate. Such an organic salt is considered to have the effect of increasing the polarity of the organic electrolyte, contributing to the improvement of wettability to the carbon material (NC), and increasing the pseudocapacity through a redox reaction derived from the nitrogen atom contained in the organic salt. In addition, it may have the effect of increasing the carrier concentration at the interface between the carbon material (NC) and the organic electrolyte, improving the space charge capacity, and inducing bias of the charge in the carbon hexagonal network plane.
[0054] From the viewpoint of improving the voltage resistance characteristic, the anion preferably contains a fluorine atom, for example, BF 4 - and / or P.F. 6 - Specific examples of preferred organic salts include tetraalkylammonium salts such as ethyltrimethylammonium tetrafluoroborate and triethylmethylammonium tetrafluoroborate.
[0055] The organic electrolyte may contain a small amount of water, however, from the viewpoint of enhancing the structural stability of the carbon material (NC), the water content in the organic electrolyte is preferably 50 ppm by mass or less.
[0056] <Electrode (E)> The electrode (E) may contain optional components such as a binder, a conductive assistant, etc. The binder has the role of assisting the bonding between the particles of the carbon material (NC) and between the particles of the carbon material (NC) and the current collector.
[0057] Examples of binders that can be used include fluororesins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), and vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP); and water-soluble resins such as carboxymethyl cellulose (CMC), polyethylene oxide (PEO), polyethylene glycol (PEG), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyacrylic acid (PAA), and polyvinyl acetate.
[0058] As a method for producing the electrode (E), for example, a carbon material (NC) is dispersed in a dispersion medium such as water together with optional components (such as a binder and a conductive assistant) to prepare a slurry. The obtained slurry is applied to a current collector, and the coating is dried to form an active layer (electrode layer) supported on the current collector, thereby obtaining an electrode (E). The active layer may then be rolled.
[0059] The current collector may be a metal foil, a metal porous body, or the like. The current collector may be made of aluminum, copper, nickel, iron, stainless steel, platinum, or the like. An alloy containing these metals as a main component may also be used. The metal foil may be a plain foil, or may be a foil that has been roughened by etching or the like, or a foil that has been subjected to plasma treatment. The metal porous body may have, for example, a three-dimensional mesh structure.
[0060] <Capacitor> Next, an example of a capacitor equipped with an electrode (E) will be described. Fig. 1 is a partially cutaway perspective view of an electric double layer capacitor (EDLC (NC)) equipped with an organic electrolyte solution.
[0061] The illustrated EDLC (NC) 10 includes a wound type capacitor element 1. The capacitor element 1 is configured by winding a first electrode 2 and a second electrode 3, each of which is a sheet-like electrode (E), with a separator 4 interposed therebetween. The first electrode 2 and the second electrode 3 each have a first current collector and a second current collector made of metal, and a first active layer and a second active layer containing a carbon material (NC) supported on the surface thereof, respectively, and exhibit capacitance by adsorbing and desorbing ions. For example, aluminum foil is used for the first and second current collectors. The surface of the current collector may be roughened by a method such as etching. For example, a nonwoven fabric mainly composed of cellulose is used for the separator 4. Lead wires 5a and 5b are connected to the first electrode 2 and the second electrode 3, respectively, as lead members. The capacitor element 1 is housed in a cylindrical exterior case 6 together with an organic electrolyte (not shown). The material of the exterior case 6 may be, for example, a metal such as aluminum, stainless steel, copper, iron, or brass. The opening of the exterior case 6 is sealed with a sealing member 7. The lead wires 5a and 5b are led out to the outside so as to pass through the sealing member 7. The sealing member 7 is made of, for example, a rubber material such as butyl rubber.
[0062] In the above embodiment, a wound type capacitor has been described, but the scope of application of the present invention is not limited to the above, and the present invention may also be applied to capacitors of other structures, such as stacked type or coin type capacitors.
[0063] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0064] Example 1 A wound type electric double layer capacitor was produced with a rated voltage of 2.8 V. A specific method for producing the electric double layer capacitor will be described below.
[0065] (1) Synthesis of carbon materials (NC) 50 parts by mass of propanediol as an alkanediol was added to 50 parts by mass of 2,4-toluene diisocyanate, and the mixture was left at room temperature for 24 hours to cure, obtaining a crosslinked product. The crosslinked product was heated at 700°C for 0.5 hours in a nitrogen atmosphere to synthesize a carbon material (NC1).
[0066] A structural analysis of the carbon material (NC1) using a combination of FT-IR and XPS confirmed the presence of CO bonds, COC bonds, C=O bonds, C=N bonds, CN bonds, etc., and it was inferred that it contains an isocyanuric ring as the main component.
[0067] When the carbon material (NC1) was analyzed by XPS, the nitrogen content C N is 12.1 mass%, oxygen content C OX is 4.3 mass%, nitrogen content C N Oxygen content C OX Ratio of: C OX / C N The nitrogen content C was calculated according to JIS M8813:2004. N is 15.9 mass%, oxygen content C OX is 6.3 mass%, C OX / C N The analytical equipment used was an oxygen, nitrogen, and hydrogen analyzer (EGMA-830, manufactured by Horiba, Ltd.).
[0068] The differential pore volume distribution of the carbon material (NC1) was measured by the method described above and is shown in Figure 2. In Figure 2, a first peak is observed in the range of 1.0 nm or more and less than 2 nm, a second peak is observed in the range of 0.5 nm or more and less than 1.0 nm, a third peak is observed in the range of 2.0 nm or more and less than 3.0 nm, a fourth peak is observed in the range of 3.0 nm or more and less than 6.0 nm, and a broad fifth peak is observed in the range of 6.0 nm or more and less than 20 nm. The total pore volume in the range of 20 nm or less described above is 0.95 cm 3 / g.
[0069] (2) Preparation of electrode (E) A slurry was prepared by dispersing 100 parts by mass of a carbon material (NC1) as an active material and 10 parts by mass of CMC as a binder in an appropriate amount of water. The obtained slurry was applied to a current collector made of an Al foil with a thickness of 30 μm, and the coating was vacuum dried at 110° C. and rolled to form an active layer, thereby obtaining an electrode (E).
[0070] The Log differential pore volume distribution of electrode (E) was measured by the method described above and the results are shown in Figure 3. In Figure 3, a broad peak is seen in the range of 0.1 μm to 3 μm.
[0071] (3) Preparation of organic electrolyte An organic electrolyte solution was prepared by dissolving an organic salt, triethylmethylammonium tetrafluoroborate, in a non-aqueous solvent, propylene carbonate, at a concentration of 1.0 mol / L.
[0072] (4) Preparation of EDLC(NC) A pair of electrodes (E) was prepared, each was connected to a lead wire, and the electrodes were wound with a cellulose nonwoven separator to form a capacitor element, which was then housed in a specified exterior case together with an organic electrolyte solution and sealed with a sealing member to complete the capacitor A1 of Example 1. Thereafter, an aging treatment was performed at 60° C. for 6 hours while applying a rated voltage of 2.5 V.
[0073] Comparative Example 1 A pair of electrodes was prepared in the same manner as in Example 1, except that general-purpose alkali-activated carbon ("activated carbon (CE1)") was used as the active material, to prepare a capacitor B1 of Comparative Example 1.
[0074] When the activated carbon (CE1) was analyzed by FT-IR and XPS, no nitrogen peak was detected.
[0075] Nitrogen content of activated carbon (CE1) C N is 0.07 mass%, oxygen content C OX is 4.08 mass%, nitrogen content C N Oxygen content C OX Ratio of: C OX / C Nwas 58.
[0076] As a result of measuring the differential pore volume distribution of activated carbon (CE1) using the method described above, only a sharp peak was observed in the range of 0.5 nm to less than 1.0 nm. In addition, the Log differential pore volume distribution of the electrode made using activated carbon (CE1) did not show the broad peak seen in the Log differential pore volume distribution of electrode (E), and the frequency dropped sharply above 0.5 μm.
[0077] [evaluation] <Initial capacity> In an environment of -30°C, the battery was charged at a constant current of 100 mA / g until the voltage reached 2.8 V, and then the battery was held at a voltage of 2.8 V for 7 minutes. Thereafter, in an environment of -30°C, the battery was discharged at a constant current of 100 mA / g until the voltage reached 0 V.
[0078] In the above discharge, the time t (sec) required for the voltage to drop from 2.24 V to 1.12 V was measured. Note that 2.24 V is a voltage equivalent to 80% of 2.8 V (the voltage at full charge), and 1.12 V is a voltage equivalent to 40% of 2.8 V. Using the measured time t, the initial capacity C1 (F) of the capacitor before the float charge test was calculated according to the following formula (A). Capacity C1=Id×t / ΔV1 (A) In addition, in the formula (A), Id is a current value calculated from 100 mA / g and the amount (g) of active material, and ΔV1 is a value obtained by subtracting 1.12 V from 2.24 V.
[0079] <Initial resistance> Using the discharge curve (vertical axis: discharge voltage, horizontal axis: discharge time) obtained by the above discharge, a linear approximation line was obtained in the range of 0.5 to 2 seconds after the start of discharge of the discharge curve, and the voltage VS at the intercept of the approximation line was obtained. The value (V0-VS) obtained by subtracting the voltage VS from the voltage V0 at the start of discharge (0 seconds after the start of discharge) was obtained as ΔV2. Using ΔV2 (V) and the current value Id during discharge (current value calculated from 100 mA / g and the amount of active material (g)), the internal resistance (DCR) R1 (Ω) of the capacitor before the float charge test was calculated from the following formula (B). Internal resistance R1=ΔV / Id (B)
[0080] <Float charge test> In an environment of 60°C, constant current charging was performed at a current of 100 mA / g until the voltage reached 2.8 V, and then the voltage of 2.8 V was maintained for 1000 hours. In this manner, the capacitor was stored with a voltage of 2.8 V applied. Thereafter, in an environment of 60°C, constant current discharging was performed at a current of 100 mA / g until the voltage reached 0 V.
[0081] Thereafter, charging and discharging were performed in an environment of -30°C using the same method as in the measurement of the capacity and internal resistance before the float charge test, and the capacity C2 (F) and internal resistance R2 (Ω) of the capacitor after the float charge test were determined.
[0082] The capacitance retention rate and resistance increase rate of the capacitor were measured relative to the initial value. The capacitance retention rate is the relative value of the capacitance after the float charge test when the initial capacitance is taken as 100%. The resistance increase rate is the relative value of the low-temperature resistance after the float charge test when the initial low-temperature resistance is taken as 100%.
[0083] [Table 1]
[0084] The results in Table 1 show that by using a carbon material (NC) as the active material, a capacitor that can achieve both initial capacity and reliability can be obtained. [Industrial Applicability]
[0085] According to the present invention, a capacitor (eg, an electric double layer capacitor) that can achieve both initial capacitance and reliability can be obtained. [Explanation of symbols]
[0086] 1: capacitor element, 2: first electrode, 3: second electrode, 4: separator, 5a: first lead wire, 5b: second lead wire, 6: exterior case, 7: sealing member, 10: capacitor
Claims
1. A first electrode, a second electrode, and an electrolyte solution, At least one of the first electrode and the second electrode is an electrode containing a nitrogen-containing carbon material, the nitrogen-containing carbon material contains a six-membered ring, The six-membered ring contains one or more carbonyl carbons and / or two or more nitrogen atoms.
2. 2. The capacitor according to claim 1, wherein the six-membered ring includes at least one selected from the group consisting of an isocyanuric ring, a triazine ring, and a 1,3,5-trione ring.
3. A first electrode, a second electrode, and an electrolyte solution, At least one of the first electrode and the second electrode is an electrode containing a nitrogen-containing carbon material, A capacitor, wherein a differential pore volume distribution A of the nitrogen-containing carbon material has a first peak in the range of 1.0 nm or more and less than 2.0 nm.
4. 4. The capacitor according to claim 3, wherein a differential pore volume distribution A of the nitrogen-containing carbon material has a second peak in a range of 0.5 nm or more and less than 1.0 nm.
5. 4. The capacitor according to claim 3, wherein a differential pore volume distribution A of the nitrogen-containing carbon material has a third peak in a range of 2.0 nm or more and less than 3.0 nm.
6. 4. The capacitor according to claim 3, wherein a differential pore volume distribution A of the nitrogen-containing carbon material has a fourth peak in a range of 3.0 nm or more and less than 6.0 nm.
7. 4. The capacitor according to claim 3, wherein a differential pore volume distribution A of the nitrogen-containing carbon material has a broad fifth peak in the range of 6.0 nm or more and less than 20 nm.
8. the nitrogen-containing carbon material contains a six-membered ring, The capacitor of claim 3 , wherein the six-membered ring contains one or more carbonyl carbons and / or two or more nitrogen atoms.
9. 4. The capacitor according to claim 1, wherein a differential pore volume distribution B of the electrode containing the nitrogen-containing carbon material has a broad peak in the range of 0.1 μm or more and 3 μm or less.
10. The nitrogen content C in the nitrogen-containing carbon material N The capacitor according to claim 1 or 3, wherein the content of the metal oxide is 2 mass % or more.
11. The oxygen content C in the nitrogen-containing carbon material OX The capacitor according to claim 10, wherein the content of the Cr is 6 mass % or more.
12. The nitrogen content C N The oxygen content C OX Ratio of: C OX / C N The capacitor of claim 11 , wherein is greater than or equal to 0.25 and less than or equal to 3.
5.
13. The capacitor according to claim 1 , wherein the electrolytic solution contains a non-aqueous solvent and an organic salt that dissolves in the non-aqueous solvent.
14. The capacitor according to claim 1 , wherein the electrolytic solution has a water content of 50 ppm by mass or less.
15. 4. The capacitor according to claim 1, wherein 80% by mass or more of the non-aqueous solvent is an aprotic solvent.
16. A nitrogen-containing carbon material is included, the nitrogen-containing carbon material contains a six-membered ring, The six-membered ring comprises one or more carbonyl carbons and / or two or more nitrogen atoms.
17. The electrode active material according to claim 16, wherein the six-membered ring includes at least one selected from the group consisting of an isocyanuric ring, a triazine ring, and a 1,3,5-trione ring.
18. A nitrogen-containing carbon material is included, The nitrogen-containing carbon material has a differential pore volume distribution A having a first peak in the range of 1.0 nm or more and less than 2.0 nm.
19. the nitrogen-containing carbon material contains a six-membered ring, 20. The electrode active material of claim 18, wherein the six-membered ring contains one or more carbonyl carbons and / or two or more nitrogen atoms.
20. The nitrogen content C in the nitrogen-containing carbon material N The electrode active material according to claim 16 or 18, wherein the content of the metal oxide in the electrolyte is 2 mass% or more.
21. The oxygen content C in the nitrogen-containing carbon material OX The electrode active material according to claim 20, wherein the content of the metal oxide in the electrolyte is 6 mass% or more.
22. The nitrogen content C N The oxygen content C OX Ratio of: C OX / C N The electrode active material according to claim 21 , wherein the σ is 0.25 or more and 3.5 or less.
Citation Information
Patent Citations
Material for electrode and method of manufacturing the same
JP2007269505A
Nitrogen-containing porous carbon material, method for producing same, and electric double layer capacitor using the nitrogen-containing porous carbon material
WO2011065484A1
Carbon material manufacturing method, electrode manufacturing method, electrode, electrochemical device, and carbon material
WO2020175616A1
Cited By
Porous carbon material and capacitor
WO2026163783A1