Raw material powder for depositing film, method for preparing raw material powder for depositing film, and method for depositing film

By using microporous crystalline aluminosilicate particles with controlled moisture content in the AD method, the challenges of forming ceramic films are overcome, resulting in improved film quality and reduced defects.

JP2024143236APending Publication Date: 2024-10-11OSAKA GAS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023055805
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The aerosol deposition method (AD method) faces challenges in forming ceramic films using dry crystalline aluminosilicate particles due to difficulties in achieving adequate impact force and particle aggregation, which hinders effective film formation.

Method used

The use of microporous crystalline aluminosilicate particles with a moisture content of 8.5 wt% to 19 wt% dispersed in a carrier gas, combined with specific heat treatment to adjust moisture content, facilitates the formation of ceramic films by the AD method.

Benefits of technology

This approach enables the formation of high-quality ceramic films by ensuring appropriate impact force and preventing particle aggregation, thereby improving film formation efficiency and reducing defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143236000001_ABST
    Figure 2024143236000001_ABST
Patent Text Reader

Abstract

To provide raw material powder for depositing a film that allows preferable film deposition with an aerosol deposition method using raw material powder including a crystalline aluminosilicate.SOLUTION: Raw material powder for depositing a film includes particulates of a microporous crystalline aluminosilicate and is used for depositing a ceramic film on a processing object surface Ka by jetting an aerosol in which the particulates are dispersed in a carrier gas toward the processing object surface Ka of a substrate K. The raw material powder for depositing a film has a water content of 8.5 wt.% or more and 19 wt.% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powdered raw material for film formation, a method for preparing the powdered raw material for film formation, and a method for film formation. [Background technology]

[0002] A method known as the aerosol deposition method (AD method) is known as a method for forming a ceramic film on a substrate without a high-temperature heat treatment such as sintering. In the AD method, raw material powder consisting of particles that will become the material for the film is sprayed from a nozzle toward the substrate at approximately the speed of sound, and the particles are crushed and deformed by the energy generated when the raw material powder collides with the substrate, forming a dense film on the substrate.

[0003] In the AD method, it is generally recommended to use raw material powder in a dry state. For example, Patent Document 1 discloses that, in order to prevent the raw material powder from agglomerating, the amount of water contained in the raw material powder (moisture content) is set to 0.45 wt% or less, which prevents the raw material powder from agglomerating and makes it easier to form a membrane. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-119574 A Summary of the Invention [Problem to be solved by the invention]

[0005] Meanwhile, the inventors of the present application have investigated the feasibility of forming ceramic films made of various materials on a substrate by the AD method, and have discovered that it is difficult to form a film when dry raw material powder made of crystalline aluminosilicate particles is used.

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a film-forming raw material powder that enables good film formation by an aerosol deposition method using a raw material powder containing a crystalline aluminosilicate, a method for preparing the film-forming raw material powder, and a film-forming method. [Means for solving the problem]

[0007] The characteristic configuration of the powdered film-forming raw material according to the present invention for achieving the above object is as follows: 1. A film-forming raw material powder used for forming a ceramic film on a treatment target surface of a substrate, the raw material powder comprising microporous crystalline aluminosilicate particles, the aerosol of the particles being dispersed in a carrier gas being sprayed toward the treatment target surface of the substrate, the raw material powder comprising: The moisture content is between 8.5wt% and 19wt%.

[0008] As a result of extensive research, the inventors of the present application have found that when using raw material powder containing crystalline aluminosilicate particles and spraying an aerosol in which the particles are dispersed in a carrier gas toward the surface of a substrate to be treated to form a ceramic film on the surface to be treated (when forming a ceramic film by the so-called AD method), it is difficult to form a film if raw material powder in a dry state, as in the conventional method, but good film formation is possible by using raw material powder containing a predetermined amount of moisture, and have completed the present invention.

[0009] That is, according to the above-mentioned characteristic configuration, since the moisture content of the powdered film-forming raw material is 8.5 wt % or more and 19 wt % or less, by using the powdered film-forming raw material, a good film can be formed on the processing target surface by the AD method.

[0010] Further, the film-forming raw material powder according to the present invention has a further characteristic configuration, The framework structure of the crystalline aluminosilicate is any one of an LTA type, an FAU-NA type, and an FAU-K type.

[0011] According to the above characteristic configuration, by using it as a raw material powder for the AD method, it is possible to form a good film made of a crystalline aluminosilicate whose skeletal structure is any one of the LTA type, FAU-NA type, and FAU-K type.

[0012] The characteristic configuration of the method for preparing a powdered raw material for film formation according to the present invention for achieving the above object is as follows: 1. A method for preparing a powdered film-forming raw material used for forming a ceramic film on a surface to be treated, comprising spraying an aerosol containing microporous crystalline aluminosilicate particles dispersed in a carrier gas toward a surface to be treated of a substrate, the method comprising: The method includes a step of adjusting the moisture content of the powdered film-forming raw material to 8.5 wt % or more and 19 wt % or less.

[0013] According to the above-mentioned characteristic configuration, it is possible to prepare a powdered film-forming raw material having a moisture content of 8.5 wt% or more and 19 wt% or less. By using the prepared powdered film-forming raw material, it is possible to form a good film on a processing target surface by the AD method.

[0014] Further, the method for preparing a powdered film-forming raw material according to the present invention has the following characteristic configuration: The framework structure of the crystalline aluminosilicate is any one of an LTA type, an FAU-NA type, and an FAU-K type.

[0015] According to the above-mentioned characteristic configuration, by using the prepared film-forming raw material powder for film formation by the AD method, a good film made of a crystalline aluminosilicate having a skeletal structure of any one of an LTA type, an FAU-NA type, and an FAU-K type can be formed.

[0016] The film forming method according to the present invention for achieving the above object comprises the following features: 1. A method for forming a ceramic film on a surface to be treated, comprising using a powdered film-forming raw material containing microporous crystalline aluminosilicate particles, and spraying an aerosol in which the particles are dispersed in a carrier gas toward a surface to be treated of a substrate, the method comprising the steps of: a raw material powder preparation step of preparing the raw material powder for film formation having a moisture content of 8.5 wt % or more and 19 wt % or less; a film-forming step of dispersing the film-forming raw material powder obtained in the raw material powder preparation step in the carrier gas to form an aerosol, which is then sprayed onto the treatment target surface.

[0017] According to the above-mentioned characteristic configuration, the powdered film-forming raw material is prepared so that the moisture content is 8.5 wt % or more and 19 wt % or less, and the film-forming process is performed using the powdered film-forming raw material, so that a good film can be formed on the surface to be treated.

[0018] Further, a further characteristic configuration of the film forming method according to the present invention is as follows: The framework structure of the crystalline aluminosilicate is any one of an LTA type, an FAU-NA type, and an FAU-K type.

[0019] According to the above characteristic configuration, it is possible to form a good film made of a crystalline aluminosilicate whose skeletal structure is any one of the LTA type, FAU-NA type, and FAU-K type. Effect of the Invention

[0020] As described above, according to the film-forming raw material powder, the method for preparing the film-forming raw material powder, and the film-forming method of the present invention, it is possible to form a good film by the aerosol deposition method using a raw material powder containing a crystalline aluminosilicate. [Brief description of the drawings]

[0021] [Figure 1] 1 is a diagram showing a schematic configuration of a film forming apparatus used in a film forming method according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, a powdered film-forming raw material, a method for preparing the powdered film-forming raw material, and a method for forming a film according to an embodiment will be described with reference to the drawings. In the following description, the terms "upper" and "lower" refer to the upper and lower sides in the drawings.

[0023] [Film forming equipment] First, a film forming apparatus 1 used in the film forming method according to this embodiment will be described.

[0024] Fig. 1 is a diagram showing a schematic configuration of a film forming apparatus 1. As shown in Fig. 1, the film forming apparatus 1 is an apparatus that ejects an aerosol in which a film-forming raw material powder is dispersed in a carrier gas toward a processing target surface Ka of a substrate K to form a film on the processing target surface Ka of the substrate K. In other words, the film forming apparatus 1 is an apparatus that forms a film on the processing target surface Ka of the substrate K by an aerosol deposition method.

[0025] In this embodiment, the film formation apparatus 1 includes a processing chamber 2 in which a substrate K is disposed, a holding unit 4 which holds the substrate K that is the target of the film formation processing, a moving mechanism 3 configured to move the holding unit 4, an aerosol transport pipe 5 which ejects an aerosol from an ejection tip 5a, an aerosol generating unit 15 which generates an aerosol in which film formation raw material powder is dispersed in a gas, a raw material powder supply mechanism 16 which delivers the film formation raw material powder to the aerosol generating unit 15, and a carrier gas delivery mechanism 18 which delivers a carrier gas to the aerosol generating unit 15.

[0026] The processing chamber 2 is made of an airtight casing, and has an opening 2a formed on the upper end surface. A holder 4 and an aerosol transport pipe 5 are disposed inside the processing chamber 2. A mechanical booster pump P1 and a vacuum pump P2 serving as exhaust equipment are connected to the opening 2a of the processing chamber 2 via an exhaust pipe S1. The pressure inside the processing chamber 2 is reduced to a predetermined pressure (for example, about 0.75 kPa) or less by exhausting gas by the mechanical booster pump P1 and the vacuum pump P2.

[0027] The holder 4 is configured to be able to hold the substrate K with the processing target surface Ka facing downward so that the processing target surface Ka is parallel to a horizontal plane. As a method for holding the substrate K, a known method such as a method using vacuum suction or a method using Coulomb force can be used.

[0028] The moving mechanism 3 is composed of a horizontal drive mechanism (not shown) that moves the holder 4 in the horizontal direction, an elevation drive mechanism (not shown) that moves the holder 4 in the vertical direction, etc. Although the moving mechanism 3 is shown to be disposed outside the processing chamber 2 in FIG. 1, the moving mechanism 3 may be disposed inside the processing chamber 2.

[0029] The aerosol transport pipe 5 is a cylindrical straight pipe member, and the cross-sectional shape of the ejection end 5a is circular. The aerosol transport pipe 5 is disposed in the processing chamber 2 so that the ejection end 5a faces the holding part 4. The end of the aerosol transport pipe 5 opposite the ejection end 5a is connected to the aerosol generating part 15. With this aerosol transport pipe 5, the aerosol is ejected from the ejection end 5a toward the processing target surface Ka of the substrate K.

[0030] The aerosol generating unit 15 is configured to generate an aerosol in which the powdered raw material for film formation is dispersed in a gas, as described above. The aerosol generating unit 15 is connected to the aerosol transport pipe 5, as well as a raw material supply pipe S2 and a carrier gas delivery pipe S3, which will be described later. The aerosol generating unit 15 generates an aerosol in which the powdered raw material for film formation, which is supplied at a constant speed by the raw material powder supply mechanism 16, and the carrier gas, which is delivered by the carrier gas delivery mechanism 18, are mixed together. The generated aerosol is delivered to the aerosol transport pipe 5.

[0031] The raw material powder supply mechanism 16 is composed of a raw material powder supply unit 17, a raw material supply pipe S2, etc. The raw material powder for film formation is stored in the raw material powder supply unit 17. The raw material powder for film formation is supplied to the aerosol generating unit 15 through the raw material supply pipe S2. The details of the raw material powder for film formation will be described later.

[0032] The carrier gas delivery mechanism 18 is composed of a gas supply unit 19, a carrier gas pressure control unit 20, a carrier gas flow rate control unit 21, a carrier gas delivery pipe S3, and the like.

[0033] A carrier gas supply pipe S3 is connected to the gas supply unit 19. The gas supply unit 19 is configured to supply a carrier gas such as air, N2, He, or Ar to the carrier gas supply pipe S3 by a compressor or a gas cylinder.

[0034] The carrier gas delivery pipe S3 is for delivering the carrier gas supplied from the gas supply unit 19 to the aerosol generation unit 15. In this embodiment, the carrier gas delivered from the gas supply unit 19 is delivered to the aerosol generation unit 15 via the carrier gas pressure control unit 20 and the carrier gas flow rate control unit 21 in this order. That is, the carrier gas delivery pipe S3 is composed of a plurality of pipes connecting the gas supply unit 19, the carrier gas pressure control unit 20, the carrier gas flow rate control unit 21, and the aerosol generation unit 15. A pressure sensor M1 for detecting the pressure in the carrier gas delivery pipe S3 is provided between the carrier gas flow rate control unit 21 and the aerosol generation unit 15 in the carrier gas delivery pipe S3.

[0035] The carrier gas pressure control unit 20 stabilizes the carrier gas flowing through the carrier gas delivery pipe S3 at an appropriate pressure. The carrier gas flow rate control unit 21 controls the flow rate of the carrier gas flowing through the carrier gas delivery pipe S3. The operations of the carrier gas pressure control unit 20 and the carrier gas flow rate control unit 21 are appropriately controlled by a control device based on the pressure detected by the pressure sensor M1.

[0036] [Raw material powder for film formation] Next, the powdered raw material for film formation according to the present embodiment will be described. The powdered raw material for film formation contains microporous crystalline alumina particles, and is used for forming a ceramic film on a surface to be treated by ejecting an aerosol in which the particles are dispersed in a carrier gas toward the surface to be treated of a substrate.

[0037] Here, according to new findings obtained by the inventors of the present application, when the raw material powder for film formation is composed of particles of crystalline aluminosilicate, the true specific gravity of the particles in a dry state is small (2 g / cm 3Since the moisture content of the powder is about 100% (approximately 100%), the impact force when it collides with the substrate K is weak, making it difficult to form a film. In contrast, when moisture is absorbed into the crystal lattice, the specific gravity of the particles increases, which increases the impact force, making it easier to form a film. On the other hand, when excessive moisture is absorbed, the particles aggregate together, and when they collide with the substrate K, the particles are crushed and deformed, resulting in a deposited green compact, which causes poor film formation. For this reason, it is necessary to adjust the moisture content of the raw material powder for film formation to an appropriate range.

[0038] As a result of extensive research, the inventors of the present application have discovered that when using a film-forming raw material powder composed of crystalline aluminosilicate particles, if the moisture content of the film-forming raw material powder is 8.5 wt% or more and 19 wt% or less, it is possible to form a good film while suppressing film formation defects such as the formation of a compact.

[0039] Therefore, in the present embodiment, the film-forming raw material powder is used with a moisture content adjusted to 8.5 wt% or more and 19 wt% or less. The moisture content of the film-forming raw material powder is more preferably more than 10 wt% and less than 18.5 wt%.

[0040] As the crystalline aluminosilicate constituting the powdered film-forming raw material, those having various skeletal structures can be used, but in this embodiment, an LTA-type crystalline aluminosilicate is used.

[0041] [Method of preparing raw material powder for film formation] Next, a method for preparing the raw material powder for film formation will be described. The method for preparing the raw material powder for film formation includes a step of adjusting the moisture content of the raw material powder for film formation to 8.5 wt% or more and 19 wt% or less. This step corresponds to the raw material powder preparation step in the film formation method.

[0042] The powdered raw material for film formation can be prepared by adding excess moisture to particles of crystalline aluminosilicate, and then adjusting the moisture content of the powdered raw material for film formation by heat treatment. In this embodiment, the particles of crystalline aluminosilicate after the addition of moisture are heated on a hot plate, and the evaporation rate of the moisture is adjusted by adjusting the heating temperature and heating time, thereby preparing a powdered raw material for film formation having a desired moisture content.

[0043] In this embodiment, the heat treatment is performed in a space with a dew point lower than -20° C. More specifically, the heat treatment is performed in a space with a dew point of -10° C. or higher and -50° C. or lower. By performing the heat treatment in a low dew point environment in this way, the amount of moisture in the heating space is small, and the effect of moisture re-adsorption is suppressed, making it easy to adjust the moisture content.

[0044] In this embodiment, the heat treatment is performed at a heating temperature of 100°C or more and 200°C or less. When the heating temperature is high, such as exceeding 200°C, the moisture volatilization rate increases, and the moisture can be removed quickly, but fine adjustment of the moisture content is difficult. On the other hand, when the heating temperature is below 100°C, the moisture taken into the crystal lattice is difficult to remove from the crystal lattice, and adjustment of the moisture content is difficult. From the viewpoint of setting the moisture volatilization rate at an appropriate rate and balancing the ease of adjusting the moisture content with the time required for adjusting the moisture content, it is preferable to perform the heat treatment at a heating temperature of 150°C or more and 200°C or less.

[0045] In this embodiment, the moisture content is measured using a halogen moisture meter. Specifically, the heat-treated crystalline aluminosilicate particles are heated at a predetermined temperature for a predetermined time, the weight change before and after heating is measured, and the weight loss is taken as the moisture content to measure the moisture content.

[0046] [Film formation method] Next, a film formation method according to the present embodiment will be described. The film formation method includes a raw material powder preparation process for preparing a film formation raw material powder having a moisture content of 8.5 wt% or more and 19 wt% or less, and a film formation process for spraying an aerosol obtained by dispersing the film formation raw material powder obtained in the raw material powder preparation process in a carrier gas toward a treatment target surface.

[0047] Specifically, in the film formation method of this embodiment, first, as described above, raw material powder for film formation having a moisture content of 8.5 wt % or more and 19 wt % or less is prepared (raw material powder preparation process), and the prepared raw material powder for film formation is stored in the raw material powder supply section 17.

[0048] Next, the carrier gas is fed from the gas supply unit 19 to the aerosol generation unit 15 while adjusting the flow rate and pressure of the carrier gas flowing through the carrier gas feed pipe S3 by the carrier gas pressure control unit 20 and the carrier gas flow rate control unit 21. In the aerosol generation unit 15, an aerosol is generated in which the fed carrier gas and the film formation raw material powder fed from the raw material powder supply unit 17 are mixed. The generated aerosol is fed to the aerosol transport pipe 5.

[0049] The aerosol supplied to the aerosol transport pipe 5 is ejected from the ejection end 5a toward the treatment surface Ka of the substrate K, and the ejected aerosol collides with the treatment surface Ka of the substrate K to form a film on the treatment surface Ka (film formation process).

[0050] In the film formation method according to the present embodiment, the raw material powder for film formation is made of crystalline aluminosilicate particles, and the moisture content is adjusted to 8.5 wt% or more and 19 wt% or less. This allows an appropriate amount of moisture to be incorporated into the crystal lattice of the crystalline aluminosilicate particles, making it difficult for the particles to aggregate with each other, and the particles with a specific gravity higher than the true specific gravity collide with the substrate K. Therefore, this film formation method makes it possible to form a good film while suppressing the occurrence of film formation defects such as the formation of a green compact.

[0051] [Examples and Comparative Examples] Examples 1 to 3 and Comparative Examples 1 to 5 are described below. In Examples 1 to 3 and Comparative Examples 1 to 5, the conditions other than the moisture content of the powdered film-forming raw material used were kept constant, and the aerosol was sprayed onto the treatment target surface while the substrate was moved back and forth along the horizontal direction to perform the film-forming process for a predetermined time. The aerosol transport pipe had a circular cross-sectional shape at the ejection end and a cross-sectional area of ​​24 mm 2The distance between the nozzle tip and the surface of the substrate to be treated was fixed at 50 mm. 3 The particles used were LTA-type crystalline aluminosilicate with an average particle size of 2.6 μm. The flow rate of the carrier gas was 12 L / min, and the pressure in the treatment chamber was 0.75 kPa.

[0052] The powdered raw material for film formation used in each of the Examples and Comparative Examples was prepared so that the moisture content would be a desired value by adding excess moisture to particles of crystalline aluminosilicate, and then removing the moisture by heat treatment. Specifically, in a space with a dew point of -40°C, the particles of crystalline aluminosilicate to which excess moisture had been added were heated on a hot plate, and the rate of evaporation of the moisture was adjusted by adjusting the heating temperature in the range of 150 to 200°C and the heating time, thereby preparing a powdered raw material for film formation having a desired moisture content.

[0053] The moisture content was measured using a halogen moisture meter. Specifically, the crystalline aluminosilicate particles were heated on a hot plate at 199°C for 5 minutes, the weight change was measured, and the weight loss was used as the moisture content to calculate the moisture content.

[0054] Table 1 shows the moisture content (moisture content) of the powdered raw material for film formation used in Examples 1 to 3 and Comparative Examples 1 to 5, and the film weight of the film formed by the film formation process. Note that the film weight of the film formed refers to the weight of a film with good film quality in appearance, and does not include the weight of a defective film such as a powder compact.

[0055] [Table 1]

[0056] As shown in Table 1, in Comparative Examples 1 to 3, in which the moisture content of the powdered raw material for film formation was less than 8.5 wt%, the film weight of the film-formed body was 0 mg, and no film was formed on the surface to be treated. This is presumably the result of insufficient impact force when colliding with the substrate due to insufficient density of the particles. On the other hand, in Comparative Examples 4 and 5, in which the moisture content was more than 19 wt%, the film weight of the film-formed body was also almost 0 mg, and no film was formed on the surface to be treated. In Comparative Examples 4 and 5, the moisture content was too high, causing severe particle aggregation, making it difficult to supply the powdered raw material for film formation from the raw material supply unit to the aerosol generation unit, and as a result, it was difficult to form a film on the surface to be treated.

[0057] In contrast, in Examples 1 to 3, in which the moisture content of the membrane-forming raw material powder was 8.5 wt% or more and 19 wt% or less, the membrane weight of the membrane-formed body was 3.7 mg, 5.5 mg, and 3.8 mg, respectively, and a sufficient amount of membrane was formed on the treatment target surface. In particular, in Example 2, in which the moisture content was 13.4 wt%, the membrane weight of the membrane-formed body was greater than those of Examples 1 and 3. From this, it can be seen that a larger number of good membranes can be formed by setting the moisture content of the membrane-formed raw material powder to be more than 10 wt% and less than 18.5 wt%.

[0058] [Another embodiment] [1] In the above embodiment, the LTA type crystalline aluminosilicate is used, but the present invention is not limited to this embodiment. As described above, crystalline aluminosilicates having various skeletal structures can be used. Since the raw material powder for film formation needs to have a certain water content, it is preferable that the skeletal structure has a skeletal structure that easily absorbs water into the crystal lattice. Examples of skeletal structures that easily absorb water into the crystal lattice include those with a high silica content, such as the LTA type, FAU-NA type, and FAU-K type. Therefore, it is preferable that the skeletal structure of the crystalline aluminosilicate is any one of the LTA type, FAU-NA type, and FAU-K type.

[0059] [2] In the above embodiment, when adjusting the moisture content of the powdered film-forming raw material, the particles of the crystalline aluminosilicate after adding moisture are heated on a hot plate, but the present invention is not limited to this embodiment. Any embodiment may be used as long as the moisture can be removed by applying energy from the outside, and for example, the particles may be heated using an electric furnace or irradiated with microwaves.

[0060] [3] In the above embodiment, the heat treatment is performed in a space with a dew point lower than -20°C (specifically, a space with a dew point of -10°C or higher and -50°C or lower), but the present invention is not limited to this. Although there is a possibility of being affected by re-adsorption of moisture, the heat treatment may be performed in a general atmospheric environment.

[0061] [4] In the above embodiment, the heat treatment is performed at a temperature between 100° C. and 200° C., but the present invention is not limited to this. As long as the temperature is capable of removing moisture, the heat treatment may be performed at a temperature above 200° C. or below 100° C.

[0062] [5] In the above embodiment, the moisture content is measured using a halogen moisture meter, but the present invention is not limited to this. For example, the moisture content may be measured using an analyzer capable of TG-DTA (thermogravimetry-differential thermal analysis).

[0063] [6] In the above embodiment, a cylindrical straight tube member is used as the aerosol transport tube 5, and the cross-sectional shape of the ejection end 5a is circular, but this is not limited to the above. The cross-sectional shape of the ejection end of the aerosol transport tube may be elliptical, or may be polygonal, such as triangular or rectangular (including slits).

[0064] [7] In the above embodiment, the holder 4 holds the substrate K so that the surface Ka to be treated faces downward, but the present invention is not limited to this. The positions of the holder and the ejection end of the aerosol transport pipe may be switched up and down, and the holder may hold the substrate so that the surface to be treated faces upward.

[0065] In addition, the configurations disclosed in the above embodiments (including other embodiments, the same applies below) can be applied in combination with configurations disclosed in other embodiments, provided no contradiction arises. Furthermore, the embodiments disclosed in this specification are illustrative, and the embodiments of the present invention are not limited thereto, and can be appropriately modified within the scope that does not deviate from the purpose of the present invention. [Explanation of symbols]

[0066] 1: Film deposition equipment 2: Processing room 3: Movement mechanism 5: Aerosol transport pipe 15: Aerosol generating section 16: Raw material powder supply mechanism 18: Carrier gas supply mechanism K: Base material Ka: Processing surface

Claims

1. 1. A film-forming raw material powder used for forming a ceramic film on a treatment target surface of a substrate, the raw material powder comprising microporous crystalline aluminosilicate particles, the aerosol of the particles being dispersed in a carrier gas being sprayed toward the treatment target surface of the substrate, the raw material powder comprising: The film-forming raw material powder has a moisture content of 8.5 wt % or more and 19 wt % or less.

2. 2. The powdered film-forming raw material according to claim 1, wherein the skeletal structure of the crystalline aluminosilicate is any one of an LTA type, an FAU-NA type, and an FAU-K type.

3. 1. A method for preparing a powdered film-forming raw material used for forming a ceramic film on a surface to be treated, comprising spraying an aerosol containing microporous crystalline aluminosilicate particles dispersed in a carrier gas toward a surface to be treated of a substrate, the method comprising: A method for preparing a powdered raw material for a membrane, comprising: adjusting a moisture content of the powdered raw material for a membrane to 8.5 wt % or more and 19 wt % or less.

4. 4. The method for preparing the powdered film-forming raw material according to claim 3, wherein the skeletal structure of the crystalline aluminosilicate is any one of an LTA type, an FAU-NA type, and an FAU-K type.

5. 1. A method for forming a ceramic film on a surface to be treated, comprising using a powdered film-forming raw material containing microporous crystalline aluminosilicate particles, and spraying an aerosol in which the particles are dispersed in a carrier gas toward a surface to be treated of a substrate, the method comprising the steps of: a raw material powder preparation step of preparing the film-forming raw material powder having a moisture content of 8.5 wt % or more and 19 wt % or less; a film formation step of dispersing the film-forming raw material powder obtained in the raw material powder preparation step in the carrier gas to form an aerosol, and spraying the aerosol toward the treatment target surface.

6. 6. The film forming method according to claim 5, wherein the skeletal structure of the crystalline aluminosilicate is any one of an LTA type, an FAU-NA type, and an FAU-K type.

Citation Information

Patent Citations

  • Mineral additive blend composition and combustion device operation method for avoiding problems such as aggregation, deposition, and corrosion, and for reducing emissions.

    JP2015506452A

  • Allophane film complex, sheet using same, and method for producing allophane film complex

    WO2019058912A1

  • Coating film and article with coating film formed on surface

    WO2021246026A1

  • Composite structure, manufacturing method therefor, and brittle-material particle for forming composite structure

    JP2003119574A