Piezoelectric film element and manufacturing method thereof

The aerosol deposition and treatment method for piezoelectric films addresses the limitations of sputtering by producing thicker, lead-free piezoelectric elements with enhanced power generation capacity and reduced environmental impact.

JP2024143238APending Publication Date: 2024-10-11OSAKA GAS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023055807
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional piezoelectric film elements manufactured using sputtering methods are limited to thin films due to slow deposition rates, high costs, and environmental concerns with lead-containing materials, restricting their power generation capacity.

Method used

A method involving aerosol deposition of a piezoelectric film on a metal substrate, followed by annealing and poling treatments, to create a thick film with a high piezoelectric constant, using lead-free potassium sodium niobate, which allows for faster and cost-effective production of piezoelectric elements with enhanced power generation.

Benefits of technology

The method enables the production of piezoelectric film elements with increased power generation capacity by compensating for lower piezoelectric constants with thicker films, while minimizing environmental impact through the use of lead-free materials and avoiding substrate diffusion issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143238000001_ABST
    Figure 2024143238000001_ABST
Patent Text Reader

Abstract

To provide a piezoelectric film element having a thickened piezoelectric film and a manufacturing method thereof.SOLUTION: A piezoelectric film element 10 includes a metallic substrate 11 and a piezoelectric film 12 formed on the substrate 11. The piezoelectric film 12 is an aerosol deposition film formed on the substrate 11 by an aerosol deposition method so as to have a thickness of 10 μm or more. A manufacturing method for the piezoelectric film element 10 includes the steps of forming a piezoelectric film having a thickness of 10 μm or more on the metallic substrate 11 by an aerosol deposition method, and annealing the piezoelectric film 12 formed on the substrate 11.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a piezoelectric film element and a method for manufacturing the same. [Background technology]

[0002] Piezoelectric film elements can generate electricity according to the amount of deformation when force is applied, and are attracting attention for use in applications such as energy harvesting. Conventional piezoelectric film elements are generally manufactured by depositing a piezoelectric film on a substrate using a sputtering method, as described in Patent Document 1, for example.

[0003] The sputtering method has a slow film formation speed (said to be a maximum of 1.0 μm / h), and requires a high vacuum environment, which makes the equipment expensive, so its application to the formation of piezoelectric films of 10 μm or more is impractical in terms of manufacturing costs. Therefore, piezoelectric film elements manufactured using the sputtering method have been limited to those with so-called thin-film type piezoelectric films with a thickness of several μm. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-023483 A Summary of the Invention [Problem to be solved by the invention]

[0005] By the way, it is known that the power generation performance of a piezoelectric film element is positively related to the thickness of the piezoelectric film, and the larger the thickness of the piezoelectric film, the greater the amount of power generated by the piezoelectric film element. For this reason, there is a demand for piezoelectric film elements with thicker piezoelectric films so that they can generate more power.

[0006] The present invention has been made in view of the above problems, and an object of the present invention is to provide a piezoelectric film element having a thickened piezoelectric film and a manufacturing method thereof.

Means for Solving the Problems

[0007] A characteristic configuration of a method for manufacturing a piezoelectric film element according to an aspect of the present invention for achieving the above object includes a step of forming a piezoelectric film having a film thickness of 10 μm or more on a metal substrate by an aerosol deposition method, and a step of annealing the piezoelectric film formed on the substrate.

[0008] Film formation by the aerosol deposition method has a high film formation rate (about 5 to 50 μm / min) and low equipment costs. According to the manufacturing method of the present invention, a piezoelectric film element having a so-called thick film type piezoelectric film with a film thickness of 10 μm or more can be easily manufactured. A piezoelectric film element having such a thickened piezoelectric film can ensure a larger amount of power generation.

[0009] In addition, although crystal defects and strains are introduced into the piezoelectric film formed by the aerosol deposition method during the film formation process, the piezoelectric constant increases by removing these defects and strains by annealing treatment. That is, according to the manufacturing method of the present invention, a piezoelectric film element having a high piezoelectric constant of the piezoelectric film can be manufactured, thereby ensuring an even larger amount of power generation.

[0010] A further characteristic configuration of the method for manufacturing a piezoelectric film element according to the present invention is that the piezoelectric film is composed of potassium sodium niobate.

[0011] Lead zirconate titanate (Pb(Zr,Ti)O3: PZT), which is widely used as a material for piezoelectric films, has a very high piezoelectric constant, which is one of the factors affecting the power generation amount of piezoelectric films, but it is severely regulated because it contains a high concentration of lead, a substance harmful to the environment and the human body. In contrast, potassium sodium niobate (K 1-x Na x NbO3, 0 < x < 1: KNN) is a lead-free piezoelectric material. According to the manufacturing method of the present invention, a piezoelectric film element with a low environmental load can be obtained.

[0012] A further characteristic feature of the method for producing a piezoelectric film element according to the present invention is that it further comprises a step of subjecting the annealed piezoelectric film to a poling treatment.

[0013] The piezoelectric film formed by the aerosol deposition method has a higher piezoelectric constant when the direction of polarization is aligned in one direction by a poling process in which an electric field is applied. In other words, the manufacturing method according to the present invention makes it possible to manufacture a piezoelectric film element having a high piezoelectric constant and thus capable of generating even more electricity.

[0014] A further characteristic feature of the manufacturing method of the piezoelectric film element according to the present invention is that the piezoelectric film is heated to 500°C to 850°C in the annealing treatment.

[0015] By carrying out the annealing treatment under the above conditions, a piezoelectric film exhibiting a high piezoelectric constant can be obtained.

[0016] A further characteristic feature of the manufacturing method of the piezoelectric film element according to the present invention is that in the poling treatment, a voltage of 40 kV / cm to 50 kV / cm is applied to the piezoelectric film at 0° C. to 150° C. for 10 to 30 minutes.

[0017] By carrying out the poling treatment under the above conditions, a piezoelectric film exhibiting a high piezoelectric constant can be obtained.

[0018] A further characteristic feature of the method for producing a piezoelectric film element according to the present invention is that the substrate is made of Ti.

[0019] It is known that heating during annealing may cause the components of the substrate to diffuse to the film side, which may affect the properties of the piezoelectric film. For example, when the substrate is made of stainless steel, if the components of stainless steel, Fe and Cr, diffuse to the film side, it will result in a short circuit due to the manifestation of electron conductivity derived from transition metals. As a result, the piezoelectric constant cannot be evaluated and no electromotive force is generated, so the power generation amount is zero. On the other hand, even if Ti diffuses to the film side, since electron conductivity does not manifest, it does not reduce the power generation amount of the piezoelectric film to zero like Fe and Cr. That is, according to the manufacturing method according to the present invention that employs a Ti substrate, the influence on the power generation amount of the piezoelectric film due to the diffusion phenomenon during annealing can be avoided.

[0020] A characteristic configuration of a piezoelectric film element according to an aspect of the present invention for achieving the above object includes a metal substrate and a piezoelectric film formed on the substrate, and the piezoelectric film is an aerosol deposition film having a film thickness of 10 μm or more.

[0021] Compared with a sputtering film, an aerosol deposition film can be formed at a high speed using relatively low-cost equipment, so it is easy to increase the film thickness. By adopting an aerosol deposition film as the piezoelectric film, a piezoelectric film element having a so-called thick film type piezoelectric film with a film thickness of 10 μm or more can be easily obtained. According to the piezoelectric film element according to the present invention provided with such a thickened piezoelectric film, more power generation amount can be ensured.

[0022] A further characteristic configuration of the piezoelectric film element according to the present invention is that the piezoelectric film is made of potassium sodium niobate.

[0023] Potassium sodium niobate (K 1-x Na x NbO3, 0 < x < 1: KNN) is a lead-free piezoelectric material. According to the above characteristic configuration of the present invention, a piezoelectric film element with a low environmental load can be obtained.

[0024] A further characteristic configuration of the piezoelectric film element according to the present invention is that the piezoelectric constant d of the piezoelectric film 33 is less than 100 pC / N.

[0025] Aerosol-deposited films tend to have lower piezoelectric constants than sputtered films made of the same piezoelectric material. When the piezoelectric material is KNN, the piezoelectric constant d 33 is approximately 110, whereas the piezoelectric constant of the aerosol-deposited film is less than 100.

[0026] When an aerosol deposition film with a low piezoelectric constant is used, the amount of electricity generated by the piezoelectric film element is usually low. However, as mentioned above, the aerosol deposition film can be easily made thick. Therefore, the piezoelectric film element according to the present invention can ensure an amount of electricity generated equal to or higher than that of a sputtering film by increasing the thickness of the aerosol deposition film.

[0027] A further characteristic feature of the piezoelectric film element according to the present invention is that the substrate is made of Ti.

[0028] According to the present invention, which employs a substrate made of Ti, it is possible to obtain a piezoelectric film element in which the effect of the diffusion phenomenon during annealing on the amount of power generated by the piezoelectric film is suppressed. [Brief description of the drawings]

[0029] [Figure 1] 1 is a cross-sectional view showing a piezoelectric film element according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Hereinafter, the piezoelectric film element and the manufacturing method thereof according to the present invention will be specifically described using embodiments.

[0031] <Piezoelectric film element> As shown in FIG. 1, a piezoelectric film element 10 according to one embodiment of the present invention includes a substrate 11 and a piezoelectric film 12 formed on the substrate 11. The piezoelectric film 12 is a piezoelectric material.

[0032] In this embodiment, as the substrate 11, those made of Ti with a thickness of 0.1 mm or more and 2 mm or less are preferably used. However, the present invention is not limited thereto, and those made of metals other than Ti such as stainless steel or those with a thickness outside the above range can also be used.

[0033] The piezoelectric film 12 is an aerosol deposition film with a film thickness of 10 μm or more, which is formed on the substrate 11 by the aerosol deposition (AD) method. The film thickness of the piezoelectric film 12 can be set to any value within the range (~1 mm) that can be formed by the aerosol deposition method. For example, it can be 10 μm, 30 μm, 40 μm, 100 μm.

[0034] In this embodiment, the piezoelectric film 12 is formed using potassium sodium niobate (K 1-x Na x NbO3, 0 < x < 1: KNN). However, the present invention is not limited thereto, and any material that can form a piezoelectric film with a film thickness of 10 μm or more by the aerosol deposition method can be used. For example, oxide materials having piezoelectric properties such as barium titanate (BaTiO3) and lithium niobate (LiNbO3) can be used.

[0035] The piezoelectric film formed by the aerosol deposition method tends to have a lower piezoelectric constant than the piezoelectric film formed by the sputtering method. When the piezoelectric material is KNN, the piezoelectric constant d 33 of the piezoelectric film formed by the sputtering method is about 110 pC / N, while the piezoelectric constant d 33 of the piezoelectric film formed by the aerosol deposition method varies depending on the film formation conditions but is basically less than 100 pC / N. That is, in this embodiment, the piezoelectric film 12 has a piezoelectric constant d 33 less than 100 pC / N.

[0036] 1, the piezoelectric film element 10 may further include a lower electrode formed on the surface of the piezoelectric film 12 facing the substrate 11, and an upper electrode formed on the surface of the piezoelectric film 12 opposite the substrate 11. The material for the lower electrode and the upper electrode may be any conductive material, such as a metal (such as a Pt / Ti laminate) or a metal oxide. In this embodiment in which the substrate 11 is made of Ti, the piezoelectric film element 10 further includes an insulating layer provided between the substrate 11 and the lower electrode.

[0037] <Manufacturing method of piezoelectric film element> Next, a method for manufacturing the piezoelectric film element 10 described above will be described. First, a piezoelectric film 12 having a thickness of 10 μm or more is formed on a Ti substrate 11 by an aerosol deposition method. In film formation by the aerosol deposition method, a powder of KNN having the same composition as the desired piezoelectric film 12 is used as a raw material, and an aerosol in which the powder raw material is dispersed in a carrier gas is sprayed onto the substrate 11. As a result, a piezoelectric film 12 made of KNN is formed on the substrate 11. The thickness of the piezoelectric film 12 can be controlled by, for example, adjusting the film formation time.

[0038] Next, an annealing process is performed on the piezoelectric film 12 formed on the substrate 11. In the annealing process, the piezoelectric film 12 is heated at a predetermined temperature for a predetermined time. This removes crystal defects and distortions introduced during the formation of the piezoelectric film 12, and increases the piezoelectric constant of the piezoelectric film 12. The annealing temperature is preferably 500°C to 850°C, and can be, for example, 600°C, 700°C, or 800°C. The holding time of the annealing process is preferably 10 minutes to 120 minutes, and can be, for example, 30 minutes or 60 minutes.

[0039] Then, although not necessarily required, a poling process may be further performed on the annealed piezoelectric film 12. In the poling process, a predetermined voltage is applied to the piezoelectric film 12 at a predetermined temperature for a predetermined time. This aligns the polarization direction in one direction, and increases the piezoelectric constant of the piezoelectric film 12. The temperature of the poling process is preferably 0°C to 150°C, and can be, for example, 140°C or 150°C. The voltage of the poling process is preferably 40 kV / cm to 50 kV / cm, and can be, for example, 40 kV / cm, 45 kV / cm, or 50 kV / cm. The time of the poling process is preferably 10 minutes to 30 minutes, and can be, for example, 10 minutes or 20 minutes.

[0040] <Effects of the embodiment> The piezoelectric film element 10 according to the present invention employs a piezoelectric film 12 formed by the aerosol deposition method, which has a lower piezoelectric constant than a piezoelectric film formed by the sputtering method, and therefore generates less power. However, the piezoelectric film 12 formed by the aerosol deposition method can be formed at a high speed (approximately 5 to 50 μm / min) and can be easily thickened to a thickness of 10 μm or more. Therefore, the decrease in the amount of power generated due to the low piezoelectric constant can be compensated for by the increase in the amount of power generated by the thickening of the piezoelectric film 12. In other words, according to the piezoelectric film element 10 of the present invention, by increasing the thickness of the piezoelectric film 12, it is possible to ensure an amount of power generated that is equal to or higher than that of a piezoelectric film formed by sputtering.

[0041] For example, the amount of power generated by a piezoelectric film element can be calculated using the following formulas 1 and 2. V∝d×t×X / A (Formula 1) In Equation 1, V is the electromotive force of the piezoelectric film, d is the piezoelectric constant of the piezoelectric film, t is the film thickness of the piezoelectric film, X is the stress applied to the piezoelectric film, and A is the cross-sectional area of ​​the piezoelectric film. P=V 2 / 2R (Formula 2) In Equation 2, P is the amount of power generated, and R is the resistance value of the load resistor connected to the piezoelectric film element.

[0042] As shown in formula 1, both the piezoelectric constant d and film thickness t are proportional to the electromotive force V. Therefore, for example, in the case of a piezoelectric film of the same thickness produced by aerosol deposition, which has a piezoelectric constant 1 / 3 of that of a piezoelectric film produced by sputtering, the power generation amount P calculated based on formula 2 is 1 / 9 of that of a piezoelectric film produced by sputtering. Nevertheless, if the film thickness t of the piezoelectric film produced by aerosol deposition is made three times larger, the power generation amount P will be equal to or greater than that of a piezoelectric film produced by sputtering. EXAMPLES

[0043] The piezoelectric film element and the manufacturing method thereof according to the present invention will be specifically described below with reference to examples.

[0044] (Production Example 1) The substrate was made of Ti and had a thickness of 0.5 mm, and the raw material powder had a composition of KNN and an average particle size of 1 μm. The raw material powder was sprayed onto the surface of the substrate by the aerosol deposition method to form a piezoelectric film with a thickness of 40 μm. The conditions for film formation were as follows. The piezoelectric film element thus produced was designated as Production Example 1. Deposition chamber vacuum degree: 650Pa Carrier gas: Air Gas flow rate: 90L / min Nozzle scan speed: 4mm / sec

[0045] (Production Example 2) The piezoelectric film of the piezoelectric film element of Production Example 1 was further subjected to a poling treatment in which a voltage of 40 kV / cm was applied for 20 minutes at 140° C. The piezoelectric film element thus produced was designated Production Example 2.

[0046] (Production Example 3) The piezoelectric film of the piezoelectric film element of Production Example 1 was further subjected to an annealing treatment in an air atmosphere at a heating temperature of 600° C. for a holding time of 60 minutes.

[0047] (Production Example 4) The piezoelectric film of the piezoelectric film element of Production Example 3 was further subjected to a poling treatment in which a voltage of 40 kV / cm was applied for 20 minutes at 140° C. The piezoelectric film element thus produced was designated Production Example 4.

[0048] (Production Example 5) The piezoelectric film of the piezoelectric film element of Production Example 1 was further subjected to an annealing treatment in an air atmosphere at a heating temperature of 700° C. for a holding time of 60 minutes.

[0049] (Production Example 6) The piezoelectric film of the piezoelectric film element of Production Example 5 was further subjected to a poling treatment in which a voltage of 40 kV / cm was applied for 20 minutes at 140° C. The piezoelectric film element thus produced was designated Production Example 6.

[0050] (Production Example 7) A piezoelectric film element was manufactured under the same conditions as in Manufacturing Example 5, except that a substrate made of SUS445 was used and the film formation time was adjusted so that the thickness of the piezoelectric film was 20 μm. This was Manufacturing Example 7.

[0051] For the piezoelectric film elements of Manufacturing Examples 1 to 7, the piezoelectric constant d 33 was measured and listed in Table 1. For comparison, Table 1 also lists the piezoelectric constant of a KNN piezoelectric film (conventional example 1) formed to a thickness of 3 μm by sputtering, and the piezoelectric constant of a PZT piezoelectric film (conventional example 2) formed to a thickness of 3 μm by sputtering. The piezoelectric constants of these comparative examples are generally known values. [Table 1]

[0052] For the piezoelectric film elements of Production Examples 5 and 7, the elements contained in the piezoelectric film were further analyzed by a known method, and the results are shown in Table 2. [Table 2]

[0053] From Table 1, it was found that the piezoelectric constants of the piezoelectric films of the piezoelectric film elements of Production Examples 3 and 5, which were annealed, were increased compared to the piezoelectric film element of Production Example 1, which was not annealed, and the increase in the piezoelectric constant was greater with annealing at 700° C. than with annealing at 600° C. It was also found that the piezoelectric film elements of Production Examples 4 and 6, which were subjected to poling in addition to annealing, further increased the piezoelectric constant of the piezoelectric film.

[0054] Also, from Table 1, it was found that the aerosol deposition method can form a piezoelectric film that has a lower piezoelectric constant but can be made thicker for practical use, compared to the sputtering method. Therefore, according to the piezoelectric film element of the present invention manufactured by the aerosol deposition method, the decrease in the amount of power generated due to the low piezoelectric constant can be compensated for by the increase in the amount of power generated due to the thickening of the piezoelectric film. For example, in the case of the piezoelectric film element of Manufacturing Example 6, based on the above formulas 1 and 2, the contribution of the piezoelectric constant of the piezoelectric film to the amount of power generated is about 1 / 11 of that of Conventional Example 1, but the contribution of the thickness of the piezoelectric film to the amount of power generated is about 177 times or more than that of Conventional Example 1. Therefore, it is considered that the piezoelectric film element of Manufacturing Example 6 has an amount of power generated that is greater than that of Conventional Example 1. It is noted that the piezoelectric film element of Manufacturing Example 6 has a greater amount of power generated than that of Conventional Example 2. It is considered that the other manufacturing examples with a lower piezoelectric constant than Manufacturing Example 6 can also have an amount of power generated that is greater than that of the conventional example by making the piezoelectric film thicker.

[0055] Furthermore, from Tables 1 and 2, it was found that in both the piezoelectric film elements of Production Example 5 and Production Example 7, which were annealed at 700°C, elements derived from the substrate were diffused into the piezoelectric film, but the piezoelectric constant of the piezoelectric film element of Production Example 7, which used a substrate made of SUS445, could not be evaluated. [Explanation of symbols]

[0056] 10 Piezoelectric film element 11 Substrate 12 Piezoelectric film

Claims

1. forming a piezoelectric film having a thickness of 10 μm or more on a metal substrate by an aerosol deposition method; and a step of annealing the piezoelectric film formed on the substrate.

2. 2. The method for manufacturing a piezoelectric film element according to claim 1, wherein the piezoelectric film is made of potassium sodium niobate.

3. The method for manufacturing a piezoelectric film element according to claim 2 , further comprising a step of subjecting the annealed piezoelectric film to a poling treatment.

4. 2. The method for manufacturing a piezoelectric film element according to claim 1, wherein the piezoelectric film is heated to 500° C. to 850° C. in the annealing process.

5. 4. The method for manufacturing a piezoelectric film element according to claim 3, wherein the poling treatment involves applying a voltage of 40 kV / cm to 50 kV / cm to the piezoelectric film at 0° C. to 150° C. for 10 minutes to 30 minutes.

6. The method for manufacturing a piezoelectric film element according to claim 1 , wherein the substrate is made of Ti.

7. A metal substrate; a piezoelectric film formed on the substrate; The piezoelectric film is an aerosol deposition film having a thickness of 10 μm or more.

8. 8. The piezoelectric film element according to claim 7, wherein the piezoelectric film is made of potassium sodium niobate.

9. The piezoelectric constant d of the piezoelectric film 33 The piezoelectric film element according to claim 8, wherein the resistivity is less than 100 pC / N.

10. The piezoelectric film element according to claim 7 , wherein the substrate is made of Ti.

Citation Information

Patent Citations

  • Piezoelectric film manufacturing method, vibration piece, vibrator, oscillator, electronic equipment, and movable body

    JP2015023483A