Multilayer ceramic electronic component, circuit board, and packaging body
The multilayer ceramic component addresses reliability issues by using distinct subcomponents in alternately stacked internal electrode layers with differentiated external electrodes, enhancing interfacial resistance and preventing incorrect potential connections.
Patent Information
- Application Number
- JP2023056081
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
As multilayer ceramic electronic components become thinner to achieve smaller size and larger capacity, the electric field strength increases, leading to potential reliability issues due to high interfacial resistance at the dielectric/internal electrode layer interfaces, especially when the components in the anode and cathode internal electrode layers are the same, risking incorrect potential connections.
The multilayer ceramic component design includes alternately stacked first and second internal electrode layers with different subcomponents, distinct external electrodes, and a visual structure for differentiation, ensuring high interfacial resistance and preventing incorrect potential connections by using materials like nickel and gold as main components with varying subcomponents in each electrode layer.
This design enhances reliability by maintaining high interfacial resistance and preventing incorrect connections, ensuring stable operation of the multilayer ceramic components.
Smart Images

Figure 2024143416000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer ceramic electronic component, a circuit board, and a package. [Background technology]
[0002] Multilayer ceramic electronic components such as multilayer ceramic capacitors (MLCCs) have been developed for incorporation into a variety of electronic devices such as smartphones and personal computers (see, for example, Patent Documents 1 to 6). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2022 / 210642 [Patent Document 2] International Publication No. 2022 / 210629 [Patent Document 3] International Publication No. 2022 / 210628 [Patent Document 4] International Publication No. 2022 / 210627 [Patent Document 5] International Publication No. 2022 / 210625 [Patent Document 6] International Publication No. 2022 / 210624 Summary of the Invention [Problem to be solved by the invention]
[0004] In order to make multilayer ceramic electronic components smaller and with higher capacity, the dielectric layers are becoming thinner. However, when the dielectric layers are made thinner, the electric field strength applied to each dielectric layer becomes relatively higher. Therefore, there is a demand for improved reliability when a voltage is applied.
[0005] One way to improve reliability is to include a secondary component in the internal electrode. The secondary component of the internal electrode can increase the interface resistance of the dielectric / electrode. However, if the components contained in the internal electrode layer used as the anode and the components contained in the internal electrode layer used as the cathode are the same, high interface resistance cannot be obtained at the dielectric / internal electrode layer interface on both sides of the anode and cathode, and high reliability may not be obtained. Furthermore, by distinguishing the anode and cathode, it is possible to prevent mistakes such as connecting the anode to a negative potential and the cathode to a positive potential during use, improving reliability.
[0006] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a multilayer ceramic electronic component, a circuit board, and a package that are highly reliable. [Means for solving the problem]
[0007] The multilayer ceramic electronic component of the present invention comprises an element body having a generally rectangular parallelepiped shape in which first internal electrode layers and second internal electrode layers are alternately stacked with dielectric layers sandwiched therebetween, the first internal electrode layers being extended to a first side surface of the generally rectangular parallelepiped shape and the second internal electrode layers being extended to a second side surface of the generally rectangular parallelepiped shape, a first external electrode provided on the first side surface and a second external electrode provided on the second side surface, wherein at least a portion of the first internal electrode layer and at least a portion of the second internal electrode layer contain a minor component in addition to a main component, the minor component differing between the first internal electrode layer and the second internal electrode layer, and a visual configuration is provided for distinguishing between the first external electrode and the second external electrode.
[0008] In the above-described multilayer ceramic electronic component, the main component of the first internal electrode layers may be the same as the main component of the second internal electrode layers.
[0009] In the above-mentioned monolithic ceramic electronic component, the first internal electrode layers may contain nickel as a main component and iron as a secondary component, and the second internal electrode layers may contain nickel as a main component and gold as a secondary component.
[0010] In the above-described monolithic ceramic electronic component, the visual configuration may be an identification mark provided on a surface of the element body.
[0011] In the above-described multilayer ceramic electronic component, the visual configuration may have asymmetrically different shapes between the first external electrode and the second external electrode.
[0012] A circuit board according to the present invention includes the above-mentioned multilayer ceramic electronic component, and a mounting substrate including a plurality of lands to which the first external electrodes and the second external electrodes of the multilayer ceramic electronic component are respectively connected.
[0013] The packaging body according to the present invention comprises the above-mentioned multilayer ceramic electronic component, a carrier tape having a sealing surface and a recess recessed from the sealing surface for accommodating the multilayer ceramic electronic component, and a top tape attached to the sealing surface and covering the recess.
[0014] Another multilayer ceramic electronic component of the present invention comprises an element body having a generally rectangular parallelepiped shape in which first internal electrode layers and second internal electrode layers are alternately stacked with dielectric layers sandwiched therebetween, the first internal electrode layers being extended to a first side surface of the generally rectangular parallelepiped shape, and the second internal electrode layers being extended to a second side surface of the generally rectangular parallelepiped shape, wherein at least a portion of the first internal electrode layers and at least a portion of the second internal electrode layers contain a minor component in addition to a major component, the minor component differs between the first internal electrode layers and the second internal electrode layers, and the shape of the first internal electrode layer at the first side surface is different from the shape of the second internal electrode layer at the second side surface.
[0015] In the above-mentioned multilayer ceramic electronic component, a width of the first internal electrode layer at the first side surface and a width of the second internal electrode layer at the second side surface may be different in a direction perpendicular to a stacking direction of the first internal electrode layer and the second internal electrode layer. Effect of the Invention
[0016] According to the present invention, it is possible to provide a multilayer ceramic electronic component, a circuit board, and a package that can achieve high reliability. [Brief description of the drawings]
[0017] [Figure 1] FIG. 2 is a partial cross-sectional perspective view of a multilayer ceramic capacitor. [Diagram 2] 2 is a cross-sectional view taken along line AA in FIG. 1. [Diagram 3] FIG. 2 is a cross-sectional view taken along line BB in FIG. [Figure 4] 1A is an enlarged cross-sectional view of the vicinity of a first external electrode, and FIG. 1B is an enlarged cross-sectional view of the vicinity of a second external electrode. [Diagram 5] FIG. 13 is a diagram illustrating a continuity rate. [Figure 6] FIG. 13 is a diagram illustrating the concentration gradient of a subcomponent. [Figure 7] 1 is a diagram illustrating a circuit board on which a multilayer ceramic capacitor is mounted; [Figure 8] 11(a) to 11(c) are diagrams illustrating examples of visual configurations for distinguishing between a first external electrode and a second external electrode. [Figure 9] FIG. 2 is a diagram illustrating a packaging body. [Figure 10] FIG. 2 is a diagram illustrating a packaging body. [Figure 11] 1A is a diagram illustrating a first side surface of the element body from which a first internal electrode layer is led out, and FIG. 1B is a diagram illustrating a second side surface of the element body from which a second internal electrode layer is led out. [Figure 12] FIG. 4 is a plan view of a first internal electrode layer. [Figure 13] 1A to 1C are diagrams illustrating a flow of a method for manufacturing a multilayer ceramic capacitor. [Figure 14] 1A and 1B are diagrams illustrating stacking. [Figure 15] 1A to 1C are diagrams illustrating a pressure bonding process. [Figure 16] FIG. [Figure 17] 13A and 13B are diagrams illustrating an example of attaching a side margin portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment will be described with reference to the drawings.
[0019] (Embodiment) FIG. 1 is a partial cross-sectional perspective view of a multilayer ceramic capacitor 100 according to an embodiment. FIG. 2 is a cross-sectional view taken along line AA in FIG. 1. FIG. 3 is a cross-sectional view taken along line BB in FIG. 1. As illustrated in FIGS. 1 to 3, the multilayer ceramic capacitor 100 includes an element body 10 having a substantially rectangular parallelepiped shape. In the element body 10, four faces other than the upper and lower faces in the stacking direction are referred to as side faces. In the element body 10, a first external electrode 20a and a second external electrode 20b are provided on two opposing side faces (a first side face and a second side face). The first external electrode 20a extends from the first side face to the four adjacent faces. The second external electrode 20b extends from the second side face to the four adjacent faces. However, the first external electrode 20a and the second external electrode 20b are spaced apart from each other.
[0020] In this embodiment, as an example, the first external electrode 20a is used as an anode, and the second external electrode 20b is used as a cathode. It is preferable to provide an external distinction such as a marker so that the first external electrode 20a and the second external electrode 20b can be distinguished from each other.
[0021] 1 to 3, the Z-axis direction (first direction) is the stacking direction, and is the direction in which the internal electrode layers face each other. The X-axis direction (second direction) is the length direction of the element body 10, and is the direction in which the first side surface and the second side surface of the element body 10 face each other, and the direction in which the first external electrode 20a and the second external electrode 20b face each other. The Y-axis direction (third direction) is the width direction of the internal electrode layers, and is the direction in which two side surfaces other than the first side surface and the second side surface (the third side surface and the fourth side surface) of the four side surfaces of the element body 10 face each other. The X-axis direction, the Y-axis direction, and the Z-axis direction are mutually perpendicular.
[0022] The element body 10 has a configuration in which dielectric layers 11 containing a ceramic material that functions as a dielectric and internal electrode layers are alternately laminated. The internal electrode layers include a plurality of first internal electrode layers 12a and a plurality of second internal electrode layers 12b. The first internal electrode layers 12a and the second internal electrode layers 12b are alternately laminated. The edge of the first internal electrode layer 12a is drawn to a first side surface on which the first external electrode 20a of the element body 10 is provided. The edge of the second internal electrode layer 12b is drawn to a second side surface on which the second external electrode 20b of the element body 10 is provided. Thereby, the first internal electrode layer 12a and the second internal electrode layer 12b are alternately conductive to the first external electrode 20a and the second external electrode 20b. As a result, the multilayer ceramic capacitor 100 has a configuration in which capacitor units are laminated. In addition, in the laminate of the dielectric layer 11 and the internal electrode layer, the internal electrode layer is disposed on the outermost layer in the lamination direction, and the upper and lower surfaces of the laminate are covered with the cover layer 13. The cover layer 13 is mainly composed of a ceramic material. For example, the composition of the cover layer 13 may be the same as or different from that of the dielectric layer 11. Note that, as long as the first internal electrode layer 12a and the second internal electrode layer 12b are exposed in different regions on the surface of the laminate and are conductive to different external electrodes, the configuration is not limited to that of FIGS. 1 to 3. The different regions on the surface of the laminate may be the respective surface regions of the opposing faces of the laminate, the respective surface regions of the adjacent faces of the laminate, or different surface regions of the same face of the laminate. As long as the different external electrodes are spaced apart from each other, the first internal electrode layer 12a and the second internal electrode layer 12b may extend from the faces exposed on the surface region of the laminate to other faces.
[0023] The size of the multilayer ceramic capacitor 100 is, for example, 0.25 mm long, 0.125 mm wide, and 0.125 mm high, or 0.4 mm long, 0.2 mm wide, and 0.2 mm high, or 0.6 mm long, 0.3 mm wide, and 0.3 mm high, or 1.0 mm long, 0.5 mm wide, and 0.5 mm high, or 3.2 mm long, 1.6 mm wide, and 1.6 mm high, or 4.5 mm long, 3.2 mm wide, and 2.5 mm high, but is not limited to these sizes. The size of the multilayer ceramic capacitor 100 may be, for example, length>width≧height, width>length≧height, height>length≧width, or height>width≧length.
[0024] The dielectric layer 11 has a main phase made of a ceramic material having a perovskite structure represented by the general formula ABO3. 3-α (0≦α≦1: α represents the amount that deviates from the stoichiometric composition; hereinafter, α will be omitted.) For example, the ceramic material in question is barium titanate (BaTiO3), calcium zirconate (CaZrO3), calcium titanate (CaTiO3), strontium titanate (SrTiO3), magnesium titanate (MgTiO3), BaTiO3, which forms a perovskite structure, 1-x-y Ca x Sr y Ti 1-z Zr z O3 (0≦x≦1, 0≦y≦1, 0≦z≦1), etc. 1-x-y Ca x Sr y Ti 1-z Zr zO3 is barium strontium titanate, barium calcium titanate, barium zirconate, barium titanate zirconate, calcium titanate zirconate, barium calcium titanate zirconate, etc. For example, in the dielectric layer 11, the main component ceramic is contained at 50 at% or more, for example, 90 at% or more. The thickness of the dielectric layer 11 is, for example, 5.0 μm or less, 3.0 μm or less, 1.0 μm or less, 0.5 μm or less, 0.4 μm or less, 0.3 μm or less, or 0.2 μm or less. The thickness of the dielectric layer 11 can be measured by observing the cross section of the multilayer ceramic capacitor 100 with a SEM (scanning electron microscope), measuring the thickness at 10 points for each of 10 different dielectric layers 11, and deriving the average value of all the measurement points.
[0025] An additive may be added to the dielectric layer 11. Examples of additives to the dielectric layer 11 include oxides of zirconium (Zr), magnesium (Mg), manganese (Mn), molybdenum (Mo), vanadium (V), chromium (Cr), rare earth elements (scandium (Sc), cerium (Ce), neodymium (Nd), yttrium (Y), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), and ytterbium (Yb)), oxides containing cobalt (Co), nickel (Ni), lithium (Li), boron (B), sodium (Na), potassium (K), or silicon (Si), or glasses containing cobalt, nickel, lithium, boron, sodium, potassium, or silicon.
[0026] 2, a region where the first internal electrode layer 12a connected to the first external electrode 20a and the second internal electrode layer 12b connected to the second external electrode 20b face each other is a region that generates capacitance in the multilayer ceramic capacitor 100. Therefore, the region that generates capacitance is referred to as a capacitance portion 14. In other words, the capacitance portion 14 is a region where adjacent internal electrode layers connected to different external electrodes face each other.
[0027] The region where the first internal electrode layers 12a connected to the first external electrode 20a face each other in the stacking direction without the second internal electrode layer 12b connected to the second external electrode 20b being interposed therebetween is called the first end margin 15a. The region where the second internal electrode layers 12b connected to the second external electrode 20b face each other in the stacking direction without the first internal electrode layer 12a connected to the first external electrode 20a being interposed therebetween is called the second end margin 15b. Each end margin is a region where the internal electrode layers connected to the same external electrode face each other in the stacking direction without the internal electrode layer connected to a different external electrode being interposed therebetween. The first end margin 15a and the second end margin 15b are regions that do not generate capacitance. The region of the first internal electrode layer 12a located at the end on the first external electrode 20a side and including the first end margin 15a is called the first region 30a. The region of the second internal electrode layer 12b that is located at the end on the second external electrode 20b side and includes the second end margin 15b is referred to as a second region 30b.
[0028] As illustrated in Fig. 3, in the element body 10, the side margin 16 is a region provided so as to cover the ends (ends in the Y-axis direction) of the dielectric layer 11, the first internal electrode layer 12a, and the second internal electrode layer 12b on the third side surface side and the fourth side surface side. That is, in Fig. 3, the side margin 16 is a region provided outside the capacitive section 14 in the Y-axis direction. That is, the side margin 16 is an outer region adjacent to the capacitive section 14 as seen from the stacking direction, and is an outer region adjacent to the capacitive section 14 on the side where the internal electrode layers are not drawn out. The side margin 16 is also a region that does not generate electrical capacitance.
[0029] FIG. 4(a) is an enlarged cross-sectional view of the vicinity of the first external electrode 20a. Hatching is omitted in FIG. 4(a). As illustrated in FIG. 4(a), the first external electrode 20a has a structure in which a plating layer 22a is provided on an underlayer 21a. The underlayer 21a is mainly composed of nickel, copper, etc. The underlayer 21a may contain ceramic particles as a common material, or may contain a glass component. The plating layer 22a is mainly composed of a metal such as nickel, copper, aluminum, zinc, tin, etc., or an alloy of two or more of these metals. The plating layer 22a may be a plating layer of a single metal component, or may be a plurality of plating layers of different metal components. For example, in FIG. 4, the plating layer 22a has a structure in which a first plating layer 23a, a second plating layer 24a, and a third plating layer 25a are formed in this order from the underlayer 21a side. The first plating layer 23a is, for example, a copper plating layer. The second plating layer 24a is, for example, a nickel plating layer, and the third plating layer 25a is, for example, a tin plating layer.
[0030] FIG. 4(b) is an enlarged cross-sectional view of the vicinity of the second external electrode 20b. Hatching is omitted in FIG. 4(b). As illustrated in FIG. 4(b), the second external electrode 20b has a structure in which a plating layer 22b is provided on an underlayer 21b. The underlayer 21b is mainly composed of nickel, copper, etc. The underlayer 21b may contain ceramic particles as a common material, or may contain a glass component. The plating layer 22b is mainly composed of a metal such as nickel, copper, aluminum, zinc, tin, etc., or an alloy of two or more of these metals. The plating layer 22b may be a plating layer of a single metal component, or may be a plurality of plating layers of different metal components. For example, the plating layer 22b has a structure in which a first plating layer 23b, a second plating layer 24b, and a third plating layer 25b are formed in this order from the underlayer 21b side. The first plating layer 23b is, for example, a copper plating layer. The second plating layer 24b is, for example, a nickel plating layer. The third plating layer 25b is, for example, a tin plating layer.
[0031] The underlayer 21a and the underlayer 21b may have the same composition, or may have different compositions. The plating layer 22a and the plating layer 22b may have the same layered structure, or may have different layered structures. For example, the number of layers of the plating layers may be different. The first plating layer 23a and the first plating layer 23b may have the same composition, or may have different compositions. The second plating layer 24a and the second plating layer 24b may have the same composition, or may have different compositions. The third plating layer 25a and the third plating layer 25b may have the same composition, or may have different compositions.
[0032] In order to realize a smaller size and a larger capacity in such a multilayer ceramic capacitor 100, it is necessary to make the dielectric layers thinner. However, when the dielectric layers are made thinner, the electric field strength applied to each dielectric layer becomes relatively high. Therefore, it is necessary to improve the reliability when a voltage is applied. However, if the components contained in the internal electrode layer used as the anode and the components contained in the internal electrode layer used as the cathode are the same, high interfacial resistance cannot be obtained at the dielectric / internal electrode layer interfaces on both sides of the anode and cathode, and high reliability may not be obtained.
[0033] Therefore, the multilayer ceramic capacitor 100 according to this embodiment has a configuration that allows it to obtain high reliability, which will be described in detail below.
[0034] The first internal electrode layer 12a and the second internal electrode layer 12b contain an auxiliary component in addition to a main component. The main component is contained in each internal electrode layer at 50 at % or more. The auxiliary component contained in the first internal electrode layer 12a is different from the auxiliary component contained in the second internal electrode layer 12b. This configuration makes it possible to obtain high interface resistance at both the interface between the first internal electrode layer 12a and the dielectric layer 11 and the interface between the second internal electrode layer 12b and the dielectric layer 11. This makes it possible to obtain high reliability when using each of the first internal electrode layer 12a and the second internal electrode layer 12b as either an anode or a cathode.
[0035] The first internal electrode layer 12a and the second internal electrode layer 12b are mainly composed of base metals such as nickel (Ni), copper (Cu), and tin (Sn), or alloys containing these metals. The main components of the first internal electrode layer 12a and the second internal electrode layer 12b may be precious metals such as platinum (Pt), palladium (Pd), silver (Ag), and gold (Au), or alloys containing these metals. The main components of the first internal electrode layer 12a and the second internal electrode layer 12b may be the same or different. As an example, the main components of the first internal electrode layer 12a and the second internal electrode layer 12b may be the same, that is, nickel, or the same, that is, copper.
[0036] The secondary components in the first internal electrode layer 12a and the second internal electrode layer 12b are, for example, one or more selected from iron (Fe), chromium (Cr), tin (Sn), vanadium (V), hafnium (Hf), osmium (Os), ruthenium (Ru), silicon (Si), boron (B), rhenium (Re), copper (Cu), cobalt (Co), tungsten (W), germanium (Ge), manganese (Mn), tantalum (Ta), silver (Ag), niobium (Nb), molybdenum (Mo), gallium (Ga), aluminum (Al), zinc (Zn), indium (In), zirconium (Zr), magnesium (Mg), titanium (Ti), thallium (Tl), scandium (Sc), yttrium (Y), and lanthanoid elements, which do not overlap with the primary component.
[0037] Here, the effect of the difference between the sub-component contained in the first internal electrode layer 12a and the sub-component contained in the second internal electrode layer 12b will be described in detail.
[0038] It is believed that as deterioration of the multilayer ceramic capacitor 100 progresses, donor defects (mainly oxygen vacancies) accumulate in the second internal electrode layer 12b connected to the second external electrode 20b used as the cathode, causing electron conduction to become dominant, while hole conduction associated with acceptor defects becomes dominant in the first internal electrode layer 12a connected to the first external electrode 20a used as the anode. In other words, since the mechanisms of electrical conduction are different on both electrodes, there is a risk that high reliability cannot be obtained even if both electrodes contain the same element as a minor component.
[0039] When the second internal electrode layer 12b contains an element with a high work function as a subcomponent, the interface resistance to electrons increases, and the above-mentioned desirable results are obtained. On the other hand, when the first internal electrode layer 12a contains an element with a high work function as a subcomponent, the interface resistance to holes decreases, which is the opposite of the desirable work function, and there is a risk that high reliability cannot be obtained.
[0040] Similarly, if the first internal electrode layer 12a contains an element with a low work function as a secondary component, the interface resistance to holes will be high, and the desired results will be obtained as described above. On the other hand, if the second internal electrode layer 12b contains an element with a low work function as a secondary component, the interface resistance to electrons will be low, which is the opposite of the desired work function, and there is a risk that high reliability will not be obtained.
[0041] In contrast to this, in this embodiment, the subcomponent contained in the first internal electrode layer 12a is made different from the subcomponent contained in the second internal electrode layer 12b.
[0042] In order to realize such an embodiment, it is preferable that the main component metal element of the first internal electrode layer 12a constituting the anode side and the main component metal element of the second internal electrode layer 12b constituting the cathode satisfy the following conditions. 1) The main metallic element constituting the first internal electrode layer 12a and the main metallic element constituting the second internal electrode layer 12b are the same, or are different but have the same work function. In this case, as described above, high reliability can be obtained by including an element with a high work function as a secondary component in the second internal electrode layer 12b to increase the interface resistance to electrons, and including an element with a low work function as a secondary component in the first internal electrode layer 12a to increase the interface resistance to holes. 2) The case where the main metallic element constituting the first internal electrode layer 12a and the main metallic element constituting the second internal electrode layer 12b are different metallic elements but have similar values that can be regarded as being substantially equal in work function. The work functions here are close enough to be considered to be almost equal to each other, and the difference is, for example, within 0.05 eV, and preferably within 0.02 eV. When the difference in the work functions of the main component metal elements is small, the change due to the work function of the metal elements contained as the subcomponents is larger, and the main component metal element constituting the first internal electrode layer 12a and the main component metal element constituting the second internal electrode layer 12b are the same. 3) Even if the main component metal element constituting the first internal electrode layer 12a and the main component metal element constituting the second internal electrode layer 12b are different metal elements, the work function of the main component constituting the second internal electrode layer 12b is higher than the work function of the main component constituting the first internal electrode layer 12a. Even if the main component metal element is used, the second internal electrode layer 12b has a high work function and contains an element with a high work function as a subcomponent, thereby making it possible to further increase the interface resistance to electrons, and the first internal electrode layer 12a has a low work function and contains an element with a low work function as a subcomponent, thereby making it possible to further increase the interface resistance to holes. This is a preferred embodiment that can obtain even higher reliability than when the main component metal element is the same between the first internal electrode layer 12a and the second internal electrode layer 12b.
[0043] When the main component metal element constituting the first internal electrode layer 12a is different from the main component metal element constituting the second internal electrode layer 12b, and the work function of the main component metal element constituting the first internal electrode layer 12a is greater than the work function of the main component metal element constituting the second internal electrode layer 12b by more than 0.05 eV, and the difference between the two work functions is so large that it cannot be considered to be approximately equal, even if an element with a slightly higher work function is contained as a secondary component, the low work function of the main component in the second internal electrode layer 12b cannot be compensated for, and the interface resistance to electrons cannot be increased, so that the desirable result of improving reliability may not be obtained. Similarly, even if the first internal electrode layer 12a contains an element with a slightly lower work function as a secondary component, the high work function of the main component in the first internal electrode layer 12a cannot be compensated for, and the interface resistance to holes cannot be increased, so that the desirable result of improving reliability may not be obtained.
[0044] For this reason, it is preferable that (work function of the main component metal element constituting the first internal electrode layer 12a)−(work function of the main component metal element constituting the second internal electrode layer 12b)≦0.05 eV.
[0045] For example, it is preferable that the first internal electrode layer 12a contains nickel as a main component and at least one element selected from iron, chromium, tin, vanadium, hafnium, osmium, ruthenium, silicon, boron, rhenium, copper, cobalt, tungsten, germanium, manganese, tantalum, silver, niobium, molybdenum, gallium, aluminum, zinc, indium, zirconium, magnesium, titanium, thallium, scandium, yttrium, and lanthanoid elements as a subcomponent, and that the second internal electrode layer 12b contains nickel as a main component and at least one element selected from gold, platinum, iridium, palladium, and selenium as a subcomponent. For example, it is preferable that the first internal electrode layer 12a contains copper as a main component and at least one element selected from iron, chromium, tin, vanadium, hafnium, tungsten, germanium, manganese, tantalum, silver, niobium, molybdenum, gallium, aluminum, zinc, indium, zirconium, magnesium, titanium, thallium, scandium, yttrium, and lanthanoid elements as a subcomponent, and the second internal electrode layer 12b contains copper as a main component and at least one element selected from gold, platinum, iridium, palladium, selenium, osmium, ruthenium, rhodium, silicon, and boron as a subcomponent. For example, the main components of the first internal electrode layer 12a and the second internal electrode layer 12b may be the same metal element or a combination of different metal elements. In this case, a subcomponent element is selected for each main component of each internal electrode layer. The condition is that the second internal conductor electrode layer has a higher work function as a secondary component element than the first internal electrode layer, and for example, the main component of the first internal electrode layer 12a may be nickel and the main component of the second internal electrode layer 12b may be copper, or for example, the main component of the first internal electrode layer 12a may be copper and the main component of the second internal electrode layer 12b may be nickel.
[0046] In the first internal electrode layer 12a, the subcomponent is contained, for example, from 0.01 at% to 10.0 at% or from 0.05 at% to 5.0 at% or from 0.1 at% to 3.0 at%. In the second internal electrode layer 12b, the subcomponent is contained, for example, from 0.01 at% to 10.0 at% or from 0.05 at% to 5.0 at% or from 0.1 at% to 3.0 at%.
[0047] The minor component may be segregated in each internal electrode layer. For example, the minor component may be segregated on the surface of each internal electrode layer.
[0048] The average thickness per layer of the first internal electrode layer 12a and the second internal electrode layer 12b in the Z-axis direction is, for example, 1.5 μm or less, 1.0 μm or less, 0.7 μm or less, 0.5 μm or less, 0.3 μm or less, or 0.1 μm or less. The thicknesses of the first internal electrode layer 12a and the second internal electrode layer 12b can be measured by observing a cross section of the multilayer ceramic capacitor 100 with a SEM (scanning electron microscope), measuring the thickness at 10 points for each of 10 different internal electrode layers, and deriving the average value of all the measurement points.
[0049] The continuity rate of the first internal electrode layer 12a and the continuity rate of the second internal electrode layer 12b may be different, but since an internal electrode layer with extremely poor continuity deteriorates reliability, it is preferable that the continuity rates of both internal electrode layers are 50% or more, preferably 60% or more, and more preferably 80% or more. As illustrated in Fig. 5, in an observation area of length L0 in a certain internal electrode layer, the lengths L1, L2,...,Ln of the metal parts are measured and summed up, and the ratio of the metal parts, ΣLn / L0, can be defined as the continuity rate of that layer.
[0050] The first internal electrode layer 12a may include a minor component in a part thereof, and the second internal electrode layer 12b may include a minor component in a part thereof. For example, the end of the first internal electrode layer 12a on the first external electrode 20a side and the end of the second internal electrode layer 12b on the second external electrode 20b side may include a minor component in addition to the main component. Even in this case, high interface resistance can be obtained at both the interface between the first internal electrode layer 12a and the dielectric layer 11 and the interface between the second internal electrode layer 12b and the dielectric layer 11. This makes it possible to obtain high reliability when using each of the first internal electrode layer 12a and the second internal electrode layer 12b as either an anode or a cathode. In particular, the resistance value between the internal electrode layers near the first external electrode 20a and near the second external electrode 20b, where electric field concentration is likely to occur, becomes high. This makes it possible to obtain high reliability.
[0051] The end of the first internal electrode layer 12a on the first external electrode 20a side may refer to the entire first region 30a including the first internal electrode layer 12a within the first end margin 15a and the region of the first internal electrode layer 12a on the first end margin 15a side of the capacitive section 14. The end of the second internal electrode layer 12b on the second external electrode 20b side may refer to the entire second region 30b including the second internal electrode layer 12b within the second end margin 15b and the region of the second internal electrode layer 12b on the second end margin 15b side of the capacitive section 14.
[0052] The subcomponent may have a concentration gradient. For example, as illustrated in FIG. 6, at the end of the first internal electrode layer 12a on the first external electrode 20a side, the concentration of the subcomponent may be higher closer to the first external electrode 20a and lower closer to the second external electrode 20b. In FIG. 6, "0" on the horizontal axis is the boundary between the first external electrode 20a and the element body 10. The further to the right on the horizontal axis, the closer to the second external electrode 20b. That is, the first region 30a, which is the end of the first internal electrode layer 12a on the first external electrode 20a side, may reach the second external electrode 20b while decreasing the concentration of the subcomponent.
[0053] As illustrated in Fig. 6, the second internal electrode layer 12b may have an end portion on the second external electrode 20b side with a higher concentration of the minor component closer to the second external electrode 20b and a lower concentration closer to the first external electrode 20a. In this case, "0" on the horizontal axis of Fig. 6 is the boundary between the second external electrode 20b and the element body 10. The further to the right on the horizontal axis, the closer to the first external electrode 20a. That is, the second region 30b, which is the end portion on the second external electrode 20b side of the second internal electrode layer 12b, may reach the first external electrode 20a while decreasing the minor component concentration.
[0054] The first external electrode 20a preferably contains a subcomponent contained in the end of the first internal electrode layer 12a on the first external electrode 20a side. This is because the bonding strength between the first external electrode 20a and the first internal electrode layer 12a is increased. The second external electrode 20b preferably contains a subcomponent contained in the end of the second internal electrode layer 12b on the second external electrode 20b side. This is because the bonding strength between the second external electrode 20b and the second internal electrode layer 12b is increased.
[0055] 7 is a diagram illustrating a circuit board in which the multilayer ceramic capacitor 100 is mounted on a mounting board 201. As illustrated in FIG. 7, the lower surface in the lamination direction is disposed so as to face a land on the mounting board 201. The first external electrode 20a and the second external electrode 20b are each independently electrically connected to the mounting board 201 via solder 202 with respect to the land on the mounting board 201. For example, each land is determined to be either a positive or negative terminal. For example, the first external electrode 20a is connected to a land used as a positive terminal, and the second external electrode 20b is connected to a land used as a negative terminal.
[0056] The multilayer ceramic capacitor 100 according to the present embodiment is provided with a visual configuration for distinguishing the first external electrode 20a and the second external electrode 20b. For example, as illustrated in FIG. 8(a), an identification mark 60 having an asymmetric shape in the X-axis direction when the Y-axis is the axis of symmetry is attached. The identification mark 60 may have an asymmetric shape in the X-axis direction when the Z-axis is the axis of symmetry. In the example of FIG. 8(a), the identification mark 60 has a triangular shape, but may be an arrow or the like. The position of the identification mark 60 is not particularly limited as long as it is attached to the surface of the multilayer ceramic capacitor 100, but is, for example, between the first external electrode 20a and the second external electrode 20b. This configuration makes it possible to visually recognize the polarity of the multilayer ceramic capacitor 100. This makes it possible to connect the first external electrode 20a and the second external electrode 20b to the mounting substrate 201 with appropriate polarity, thereby improving reliability.
[0057] Alternatively, a difference may be provided between the surface shape of the first external electrode 20a and the surface shape of the second external electrode 20b. For example, as illustrated in Fig. 8(b), one external electrode may be protruded toward the other external electrode and the other external electrode may be recessed at the center in the Y-axis direction or the Z-axis direction on a specific surface of the element body 10. Alternatively, as illustrated in Fig. 8(c), the extension length in the X-axis direction of the first external electrode 20a may be different from the extension length in the X-axis direction of the second external electrode 20b.
[0058] The multilayer ceramic capacitor 100 is prepared in a packaged state as a package 300 when mounted on a mounting substrate 201. Figures 9 and 10 are diagrams illustrating the package 300. Figure 9 is a partial plan view of the package 300. Figure 10 is a cross-sectional view of the package 300 taken along line CC in Figure 9.
[0059] The package 300 includes the multilayer ceramic capacitor 100, a carrier tape 310, and a top tape 320. The carrier tape 310 is configured as a long tape extending in the Y-axis direction. The carrier tape 310 has a plurality of recesses 311 arranged at intervals in the Y-axis direction, each recess 311 housing one of the multilayer ceramic capacitors 100 therein.
[0060] The carrier tape 310 has a seal surface P which is an upward surface perpendicular to the Z-axis direction, and the multiple recesses 311 are recessed downward in the Z-axis direction from the seal surface P. In other words, the carrier tape 310 is configured so that the multilayer ceramic capacitors 100 in the multiple recesses 311 can be taken out from the seal surface P side.
[0061] In the carrier tape 310, a plurality of feed holes 312 are provided which are arranged at intervals in the Y-axis direction and penetrate the carrier tape 310 in the Z-axis direction at positions shifted in the X-axis direction from the row of the plurality of recesses 311. The feed holes 312 are configured as engagement holes used by the tape transport mechanism to transport the carrier tape 310 in the Y-axis direction.
[0062] In the package 300, the top tape 320 is attached to the seal surface P of the carrier tape 310 along the row of the recesses 311, and the recesses 311 accommodating the multilayer ceramic capacitors 100 are collectively covered by the top tape 320. In this way, the multilayer ceramic capacitors 100 are held in the recesses 311.
[0063] 10, in the multilayer ceramic capacitor 10 in the recess 311 of the carrier tape 310, the principal surface of the element body 10 facing upward in the Z-axis direction faces the top tape 320. The principal surface of the element body 10 facing downward in the Z-axis direction faces the bottom surface of the recess 311. In the recess 311, one side in the X-axis direction is defined as the first external electrode 20a, and the other side is defined as the second external electrode 20b. By distinguishing between the first external electrode 20a and the second external electrode 20b, i.e., the anode and the cathode, it is possible to prevent mistakes such as connecting the anode to a negative potential and the cathode to a positive potential during use, thereby improving reliability.
[0064] The element body 10 before the first external electrode 20a and the second external electrode 20b are provided may have a configuration that allows the surface from which the first internal electrode layer 12a is drawn and the surface from which the second internal electrode layer 12b is drawn to be distinguished. For example, FIG. 11(a) is a diagram illustrating a first side surface from which the first internal electrode layer 12a is drawn in the element body 10. FIG. 11(b) is a diagram illustrating a second side surface from which the second internal electrode layer 12b is drawn in the element body 10. As illustrated in FIG. 11(a) and FIG. 11(b), the width in the Y-axis direction of the first internal electrode layer 12a in the portion drawn to the first side surface may be different from the width in the Y-axis direction of the second internal electrode layer 12b in the portion drawn to the second side surface. In this case, the polarity of the element body 10 can be visually recognized.
[0065] For example, the configuration of Fig. 11(a) can be realized by varying the width of the first internal electrode layer 12a. For example, as illustrated in Fig. 12, the first internal electrode layer 12a has a 1a region 121 including a connection portion connected to the first external electrode 20a and having a width W1, and a 1b region 122 having a width W2 in a region corresponding to the vicinity of the end face side of the capacitance section 14. The first region of the first internal electrode layer 12a is composed of the 1a region 121 and the 1b region 122. The width W1 is smaller than the width W2. The widths W1 and W2 refer to the widths in the Y-axis direction. With this configuration, the configuration of Fig. 11(a) is obtained.
[0066] Next, a description will be given of a method for manufacturing the multilayer ceramic capacitor 100. FIG 13 is a diagram illustrating a flow of the method for manufacturing the multilayer ceramic capacitor 100.
[0067] (Raw powder production process) First, a dielectric material for forming the dielectric layer 11 is prepared. The A-site elements and B-site elements contained in the dielectric layer 11 are usually contained in the dielectric layer 11 in the form of a sintered body of ABO3 particles. For example, barium titanate is a tetragonal compound having a perovskite structure and exhibits a high relative dielectric constant. This barium titanate can generally be obtained by synthesizing barium titanate by reacting a titanium raw material such as titanium dioxide with a barium raw material such as barium carbonate. Various methods have been known so far as a method for synthesizing the main component ceramic of the dielectric layer 11, such as a solid-phase method, a sol-gel method, a hydrothermal method, and the like. In this embodiment, any of these methods can be adopted.
[0068] A predetermined additive compound is added to the obtained ceramic raw material powder according to the purpose. The additive compound may be an oxide of zirconium (Zr), magnesium (Mg), manganese (Mn), molybdenum (Mo), vanadium (V), chromium (Cr), rare earth elements (scandium (Sc), cerium (Ce), neodymium (Nd), yttrium (Y), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), or ytterbium (Yb)), or an oxide containing cobalt (Co), nickel (Ni), lithium (Li), boron (B), sodium (Na), potassium (K), or silicon (Si), or a glass containing cobalt, nickel, lithium, boron, sodium, potassium, or silicon.
[0069] For example, a compound containing an additive compound is wet-mixed with a ceramic raw material powder, and then dried and pulverized to prepare a ceramic material. For example, the ceramic material obtained as described above may be pulverized as necessary to adjust the particle size, or may be combined with a classification process to adjust the particle size. Through the above steps, a dielectric material is obtained.
[0070] Next, a dielectric pattern material for forming the side margin 16 is prepared. The dielectric pattern material contains powder of the main component ceramic of the side margin 16. As the powder of the main component ceramic, for example, powder of the main component ceramic of the dielectric material can be used. A predetermined additive compound is added depending on the purpose.
[0071] (Coating process) Next, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the obtained raw material powder and wet mixed. The obtained slurry is used to coat a ceramic green sheet 51 on a substrate by, for example, a die coater method or a doctor blade method, and then dried. The substrate is, for example, a polyethylene terephthalate (PET) film. Figures illustrating the coating process are omitted.
[0072] (Internal electrode formation process) Next, as illustrated in FIG. 13(a), a metal conductive paste for forming an internal electrode containing an organic binder is printed on the surface of a ceramic green sheet 51 by screen printing, gravure printing, or the like to arrange a first internal electrode pattern 52a for the first internal electrode layer 12a or a second internal electrode pattern 52b for the second internal electrode layer 12b. Ceramic particles are added to the metal conductive paste as a common material. The main component of the ceramic particles is not particularly limited, but is preferably the same as the main component ceramic of the dielectric layer 11. The metal conductive paste for forming the first internal electrode layer 12a and the metal conductive paste for forming the second internal electrode layer 12b may contain different subcomponent elements. The metal conductive paste for forming the internal electrodes may not contain subcomponent elements. In this case, the subcomponent elements may be included in the external electrodes.
[0073] Next, a binder such as an ethyl cellulose-based binder and an organic solvent such as a terpineol-based binder are added to the dielectric pattern material obtained in the raw powder preparation process, and the mixture is kneaded in a roll mill to obtain a dielectric pattern paste for the reverse pattern layer. As illustrated in Fig. 14(a), a dielectric pattern paste is printed on a ceramic green sheet 51 in the peripheral area where the internal electrode pattern is not printed, thereby arranging a dielectric pattern 53 and filling in the step with the internal electrode pattern. The ceramic green sheet 51 on which the internal electrode pattern and the dielectric pattern 53 are printed is called a lamination unit.
[0074] 14(b), the lamination units are laminated so that the internal electrode layers and the dielectric layers are alternately arranged and the edges of the internal electrode layers are alternately exposed at both end faces in the length direction of the dielectric layers and alternately drawn out to a pair of external electrodes having different polarities. Specifically, a ceramic green sheet 51 on which a first internal electrode pattern 52a and a dielectric pattern 53 are printed and a ceramic green sheet 51 on which a second internal electrode pattern 52b and a dielectric pattern 53 are printed are laminated in order. For example, the number of layers in the lamination unit is set to 100 to 500.
[0075] (Crimping process) As shown in FIG. 15, a predetermined number of cover sheets 54 (for example, 2 to 10 layers) are laminated on the top and bottom of a laminate in which the lamination units are laminated, and then thermally compressed.
[0076] (coating process) The ceramic laminate thus obtained is subjected to a binder removal process in an N2 atmosphere, and then a metal paste that will become the underlayers 21a and 21b is applied thereto by a dipping method.
[0077] (Firing process) Then, the oxygen partial pressure is 10 -5 ~10 -8 The mixture is fired in a reducing atmosphere at 1,100°C to 1,300°C for 5 minutes to 10 hours.
[0078] (Reoxidation treatment process) In order to return oxygen to the partially reduced main phase of the dielectric layer 11 fired in a reducing atmosphere, a heat treatment is performed in a mixed gas of N2 and water vapor at about 1000°C or in the air at 500°C to 700°C so as not to oxidize the first internal electrode layer 12a and the second internal electrode layer 12b. This process is called a reoxidation treatment process.
[0079] (Identification mark creation process) The identification mark 60 may be formed by applying a paste for the identification mark 60 and baking it after firing the ceramic laminate, or by using a plating or sputtering technique. This provides a visual configuration for distinguishing between the first external electrode 20a and the second external electrode 20b.
[0080] (Plating process) Thereafter, the underlayer 21a is plated with a metal coating of copper, nickel, tin, or the like. The underlayer 21b is plated with a metal coating of copper, nickel, tin, or the like. Through the above steps, the multilayer ceramic capacitor 100 is completed. Different plating processes can be performed on the underlayer 21a and the underlayer 21b. By changing the material, color, and gloss of the plating, a visual configuration can be obtained for distinguishing the first external electrode 20a from the second external electrode 20b. The configurations of Figs. 8(a) to 8(c) can be obtained by adjusting the coating thickness, paste viscosity, application position, and the like when applying the external electrode paste by the dipping method, and can be used to visually distinguish the first external electrode 20a from the second external electrode 20b.
[0081] In order to obtain a concentration gradient of the minor components as shown in FIG. 6, that is, the concentration of the minor components is higher in the first internal electrode layer 12a closer to the first external electrode 20a and lower in the second external electrode 20b, and the concentration of the minor components is higher in the second internal electrode layer 12b closer to the second external electrode 20b and lower in the first external electrode 20a, it is sufficient to use internal electrode patterns that do not contain minor components instead of the first internal electrode pattern 52a and the second internal electrode pattern 52b, and apply a metal paste 40a that will become the base layer 21a to one end surface of the ceramic laminate by a dip method, and apply a metal paste 40b that will become the base layer 21b to the other end surface by a dip method, as illustrated in FIG. 16, and then perform firing. For example, the metal paste 40a contains a metal of the main component and a metal of the minor component. The metal paste 40b contains a metal of the main component and a metal of the minor component. The subcomponents of the metal paste 40a and the metal paste 40b are made different. In this case, metal elements of different subcomponents are diffused to the end of the first internal electrode layer 12a on the first external electrode 20a side and the end of the second internal electrode layer 12b on the second external electrode 20b side. With this configuration, the internal electrodes can be made of a common material, eliminating the trouble of alternately handling and laminating dielectric sheets on which patterns that become different internal electrodes are formed, and the sintering behavior of the internal electrodes can be made uniform, making it possible to uniformize stress and prevent the occurrence of fine structural defects.
[0082] The side margin portion may be attached or applied to the side surface of the laminated portion. Specifically, as illustrated in Fig. 17, a ceramic green sheet 51 and a first internal electrode pattern 52a and a second internal electrode pattern 52b having the same width as the ceramic green sheet 51 are laminated to obtain a laminated portion. Next, a sheet formed of a dielectric pattern paste may be attached as a side margin portion 55 to the side surface of the laminated portion.
[0083] In the above, the base layer for the external electrodes and the ceramic laminate are fired simultaneously, but the present invention is not limited to this. For example, after firing the ceramic laminate, a paste of Ni, Cu, and Ag may be applied and baked, or the terminal electrodes may be formed by plating or sputtering techniques.
[0084] Although the above embodiment is applied to a multilayer ceramic capacitor with two terminal electrodes, it may be applied to a multilayer ceramic capacitor with three or more terminals. In particular, since a three-terminal capacitor that is generally used at high frequencies with low ESL is required to have a sufficiently low ESR, the dielectric layer described in the above embodiment is also suitable for a three-terminal capacitor.
[0085] In the above embodiments, a multilayer ceramic capacitor has been described as an example of a multilayer ceramic electronic component, but the present invention is not limited to this. For example, other multilayer ceramic electronic components such as a varistor or a thermistor may be used.
[0086] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0087] 10 Base 11 Dielectric layer 12a 1st internal electrode layer 12b Second internal electrode layer 13 Cover Layer 14 Capacity part 15 End Margin 16 Side Margin 20a 1st external electrode 20b 2nd external electrode 51 Ceramic green sheet 52a First internal electrode pattern 52b Second internal electrode pattern 53 Dielectric Pattern 54 Cover Sheet 55 Side margin 60 Identification Mark 100 Multilayer ceramic capacitors
Claims
1. an element body in which first internal electrode layers and second internal electrode layers are alternately stacked with dielectric layers sandwiched therebetween, the element body having a substantially rectangular parallelepiped shape, the first internal electrode layers being drawn out to a first side surface of the substantially rectangular parallelepiped shape, and the second internal electrode layers being drawn out to a second side surface of the substantially rectangular parallelepiped shape; a first external electrode provided on the first side surface; a second external electrode provided on the second side surface, At least a portion of the first internal electrode layer and at least a portion of the second internal electrode layer contain a subcomponent in addition to a main component, The subcomponent is different between the first internal electrode layer and the second internal electrode layer, A multilayer ceramic electronic component, comprising: a first external electrode and a second external electrode, the first external electrode and the second external electrode being provided with a visual configuration for distinguishing the first external electrode and the second external electrode from each other.
2. 2. The multilayer ceramic electronic component according to claim 1, wherein the main component of the first internal electrode layers is the same as the main component of the second internal electrode layers.
3. The first internal electrode layer contains nickel as a main component and iron as a secondary component, 2. The multilayer ceramic electronic component according to claim 1, wherein the second internal electrode layers contain nickel as a main component and gold as a secondary component.
4. 3. The multilayer ceramic electronic component according to claim 1, wherein the visual configuration is an identification mark provided on a surface of the element body.
5. 3 . The multilayer ceramic electronic component according to claim 1 , wherein the visual configuration has an asymmetrically different shape between the first external electrode and the second external electrode.
6. The multilayer ceramic electronic component according to claim 1 or 2, a mounting substrate having a plurality of lands to which the first external electrodes and the second external electrodes of the multilayer ceramic electronic component are respectively connected.
7. The multilayer ceramic electronic component according to claim 1 or 2, a carrier tape having a sealing surface and a recess recessed from the sealing surface for accommodating the multilayer ceramic electronic component; a top tape attached to the sealing surface and covering the recess; A packaging body comprising:
8. an element body having a substantially rectangular parallelepiped shape in which first internal electrode layers and second internal electrode layers are alternately stacked with dielectric layers sandwiched therebetween, the first internal electrode layers being drawn out to a first side surface of the substantially rectangular parallelepiped shape, and the second internal electrode layers being drawn out to a second side surface of the substantially rectangular parallelepiped shape; At least a portion of the first internal electrode layer and at least a portion of the second internal electrode layer contain a subcomponent in addition to a main component, The subcomponent is different between the first internal electrode layer and the second internal electrode layer, a shape of the first internal electrode layer on the first side surface and a shape of the second internal electrode layer on the second side surface are different from each other.
9. 9. The multilayer ceramic electronic component according to claim 8, wherein in a direction perpendicular to a stacking direction of the first internal electrode layer and the second internal electrode layer, a width of the first internal electrode layer at the first side surface and a width of the second internal electrode layer at the second side surface are different.
Citation Information
Patent Citations
Multilayer ceramic capacitor
WO2022210624A1
Laminated ceramic capacitor
WO2022210625A1
Multilayered ceramic capacitor
WO2022210627A1
Layered ceramic capacitor
WO2022210628A1
Multilayered ceramic capacitor
WO2022210629A1