Composite semipermeable membrane and water production method

A composite semipermeable membrane with a convex pore size distribution in the porous layer addresses the issue of compaction under high temperature and pressure, maintaining water permeability and salt removal performance in challenging conditions.

JP2024143504APending Publication Date: 2024-10-11TORAY INDUSTRIES INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023056225
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional composite semipermeable membranes experience a decrease in water permeability and salt removal performance due to pore compaction under high temperature and pressure conditions, particularly in applications like seawater desalination and ZLD (Zero Liquid Discharge), where temperature fluctuations and high pressures affect water production.

Method used

The composite semipermeable membrane features a porous layer with a convex pore size distribution, where the maximum average pore diameter is located between cross-sectional images R3 to R18, and the average pore diameter ranges from 0.1 μm to 0.6 μm, ensuring high water permeability and salt removal even under high temperature and pressure.

Benefits of technology

The membrane maintains high water permeability and salt removal performance by preventing pore compaction, thus stabilizing water production and efficiency in high-pressure and temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143504000001_ABST
    Figure 2024143504000001_ABST
Patent Text Reader

Abstract

To provide a composite semipermeable membrane which has an excellent initial water production capacity, and high permeability retention property and salt removal property even after the high-temperature and high-pressure operation.SOLUTION: A composite semipermeable membrane comprises a substrate, a porous layer provided on the substrate, and a separation functional layer provided on the porous layer. When a cross section image of the porous layer captured by a scanning electron microscope is divided equally into 20 pieces in the thickness direction, and the cross section images are the cross section images R1, R2, ... Rn ... R20 (n is an integer from 1 to 20) from the substrate side toward the separation functional layer side, the average hole diameter maximum value of the porous layer is present in one of the cross section images R3-R18, and the average hole diameter of the porous layer in the cross section image R1 and the cross section image R2 is 0.1 μm or more and less than 0.6 μm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite semipermeable membrane and a method for producing water. [Background technology]

[0002] Composite semipermeable membranes, which have a substrate, a porous layer, and a separation functional layer, are used as composite separation membranes for reverse osmosis treatment to remove solutes from raw water, such as in seawater desalination. In reverse osmosis treatment, a pressure equal to or greater than the difference between the osmotic pressure on the feed water side and the osmotic pressure on the permeated water side is applied to the feed water side of the composite separation membrane. In recent years, they are also used in ZLD (Zero Liquid Discharge) to reduce wastewater to zero, and for concentration in valuable resource recovery processes, and there are an increasing number of cases where they are operated at higher pressures than before depending on the solute concentration.

[0003] In such high-pressure operation of reverse osmosis treatment, the permeability of the composite semipermeable membrane may decrease. Patent documents 1 to 4 point out that the cause of the decrease in permeability is the blockage of internal pores due to compaction under high-pressure operation of the porous layer.

[0004] In Patent Document 1, the average film thickness t0 (μm) of the porous layer and the pure water permeability coefficient p0 (g / (cm) after applying a pressure of 5.5 MPa for 3 hours and then releasing the pressure are 2 s MPa), the average thickness t1 (μm) of the porous layer after applying a pressure of 10 MPa in the thickness direction for 3 hours and then releasing it, and the pure water permeability coefficient p1 (g / (cm 2 Patent Document 1 discloses a composite semipermeable membrane in which t1 / t0 and p1 / p0 satisfy specific numerical ranges in the case of a porous layer having a pressure of 1.0 MPa (s·MPa). According to Patent Document 1, t1 / t0 and p1 / p0 are indexes that represent the ability of the porous layer to resist compaction, that is, indexes that represent the strength of the framework of the composite semipermeable membrane, and a membrane that satisfies the above conditions is suppressed from being compacted.

[0005] The composite semipermeable membrane of Patent Document 2 includes a dense layer in which the porous layer is in contact with a separation functional layer, and a macrovoid layer located between the dense layer and the substrate. Patent Document 2 discloses that, in particular, when the number of macrovoids per unit length in the membrane surface direction in the macrovoid layer is within a specific range, the thickness of the porous layer is maintained even during operation at high pressure.

[0006] Patent Document 3 discloses that the composite semipermeable membrane is pre-compacted for 2 hours or more in order to minimize changes in performance during operation.

[0007] Patent document 4 discloses a porous layer design in which the surface of the porous layer is made thinner, the resin density is increased, and the pore size gradually increases from the separation functional layer toward the substrate in order to suppress the separation functional layer from falling onto the surface of the porous layer. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2001-252538 A [Patent Document 2] JP 2018-039003 A [Patent Document 3] JP 2014-014739 A [Patent Document 4] JP 2001-252537 A Summary of the Invention [Problem to be solved by the invention]

[0009] In processes that operate at high pressure, such as ZLD (Zero Liquid Discharge), there is concern about a decrease in the amount of water produced by the composite separation membrane. Furthermore, when using natural water supply, such as seawater desalination, the temperature of the supply water is not constant throughout the year, and it becomes higher in the summer. Not only the high pressure but also the high temperature of the supply water can cause a decrease in the amount of water produced.

[0010] However, conventional methods for suppressing compaction of the porous layer had the problem of poor water production capacity during high-temperature operation. An object of the present invention is to provide a composite semipermeable membrane that has high water permeability retention and salt rejection even after operation at high temperatures and high pressures. [Means for solving the problem]

[0011] Means of the Invention The present inventors have conducted extensive research to solve the above problems and have found that the above objects can be achieved by the composite semipermeable membrane shown below, thereby completing the present invention. In order to solve the above problems, the composite semipermeable membrane of the present invention has the following configuration. A composite semipermeable membrane having a substrate, a porous layer provided on the substrate, and a separation functional layer provided on the porous layer, A cross-sectional image of the porous layer taken by a scanning electron microscope is divided into 20 equal parts in the thickness direction, and cross-sectional images R1, R2, . . . Rn, . . . R20 (n is an integer from 1 to 20) are taken from the substrate side to the separation functional layer side, respectively. the maximum average pore diameter of the porous layer is present in any one of the cross-sectional images R3 to R18, The average pore size of the porous layer in the cross-sectional image R1 and the cross-sectional image R2 is 0.1 μm or more and less than 0.6 μm. Effect of the Invention

[0012] According to the present invention, a composite semipermeable membrane having high water permeability retention and salt rejection properties even after operation at high temperatures and high pressures can be obtained. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic cross-sectional view of a composite semipermeable membrane in one embodiment of the present invention. [Diagram 2] FIG. 2 is an SEM cross-sectional image of the porous membrane in the composite semipermeable membrane of Comparative Example 2. [Diagram 3] FIG. 3 is an SEM cross-sectional image of the porous membrane in the composite semipermeable membrane of Example 2. [Figure 4] FIG. 4 shows SEM cross-sectional images of the porous layers in the composite semipermeable membranes produced in the Examples and Comparative Examples, and a graph showing the distribution of the average pore size. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] 1.Composite semipermeable membrane 1, a composite semipermeable membrane 1 having a substrate 2, a porous layer 3 provided on the substrate 2, and a separation functional layer 4 provided on the porous layer 3 will be described below as one embodiment of the present invention. In addition, the main surface of the porous layer 3 facing the separation functional layer is referred to as a front surface 11, and the main surface facing the substrate is referred to as a back surface 12.

[0015] (base material) Materials constituting the substrate include polyester polymers, polyamide polymers, polyolefin polymers, or mixtures or copolymers thereof. Among them, polyester polymers having high mechanical and thermal stability are particularly preferred. The substrate is preferably in the form of a fabric having high mechanical and thermal stability. As the fabric, a long fiber nonwoven fabric, a short fiber nonwoven fabric, or a woven or knitted fabric can be preferably used. Here, the long fiber nonwoven fabric refers to a nonwoven fabric having an average fiber length of 300 mm or more and an average fiber diameter of 3 to 30 μm.

[0016] (Thickness of substrate) The thickness of the substrate is preferably in the range of 10 to 200 μm, and more preferably in the range of 30 to 150 μm. The thickness of the substrate can be measured by a dial thickness gauge or a digital thickness gauge. Measuring instruments that can be used include products from PEACOCK by Ozaki Manufacturing Co., Ltd. and Techlock Corporation. When using a dial thickness gauge or a digital thickness gauge, the thickness is measured at any 20 points and the arithmetic average is calculated to determine the thickness of the substrate.

[0017] (Base material weight) The weight of the base material is 40 to 120 g / m 2The weight per unit area is preferably 40 g / m 2 More preferably, 50 g / m 2 By setting the thickness to the above, it is possible to obtain a good membrane formability with little excessive penetration during polymer solution casting, and it is possible to obtain a composite semipermeable membrane having high membrane peel strength and mechanical strength and excellent durability. 2 Less than 100 g / m 2 By setting it to the value below, the thickness of the composite semipermeable membrane can be reduced, the semipermeable membrane area per composite semipermeable membrane element can be increased, and sufficient water permeability can be ensured, so that a "solidified fluid flow" (described later) is easily formed in the resin solution when the porous layer is formed.

[0018] (Pure water permeability coefficient of substrate) The pure water permeability coefficient of the substrate at 25°C is 100 to 1400 [×10 -9 m 3 / m 2 ·sec·Pa], and 200 to 1000 [×10 -9 m 3 / m 2 ·sec·Pa] is more preferable. The pure water permeability coefficient of the substrate can be calculated by the following method. First, the substrate is cut into a circle with a diameter of 4.3 cm, and the cut sample is set in a stirring type ultra holder (UHP-43K manufactured by Advantec Toyo Co., Ltd.). Next, pure water at 25°C is poured into the cell, and after attaching the cap, the pressure is increased to a constant level using nitrogen or compressed air. Finally, the amount of pure water permeating at a certain time is measured, and the pure water permeability coefficient [×10 -9 m 3 / m 2 sec Pa]. Pure water permeability coefficient = Pure water permeation amount / (effective filtration area of ​​substrate x water collection time x supply pressure) By setting the pure water permeability coefficient of the substrate within the above range, a "solidifying fluid flow" (described later) is easily formed in the resin solution when the porous layer is formed.

[0019] (Porous layer) The porous layer is preferably made of a thermoplastic resin. Here, the thermoplastic resin refers to a resin made of a chain polymer substance, which exhibits the property of deforming or flowing when heated by an external force.

[0020] Examples of thermoplastic resins include homopolymers such as polysulfone, polyethersulfone, polyamide, polyester, cellulose polymer, vinyl polymer, polyphenylene sulfide, polyphenylene sulfide sulfone, polyphenylene sulfone, and polyphenylene oxide, or copolymers thereof, which may be used alone or in blends. Here, examples of cellulose polymers include cellulose acetate and cellulose nitrate, and examples of vinyl polymers include polyethylene, polypropylene, polyvinyl chloride, chlorinated vinyl chloride, and polyacrylonitrile. Among these, polysulfone, polyacrylonitrile, polyamide, polyester, polyvinyl alcohol, polyphenylene sulfide sulfone, polyphenylene sulfone, polyphenylene sulfide, polyethersulfone, polyvinylidene fluoride, cellulose acetate, polyvinyl chloride, and chlorinated vinyl chloride are preferred.

[0021] More preferred examples of the thermoplastic resin include cellulose acetate, polyvinyl chloride or chlorinated vinyl chloride, polysulfone, polyphenylene sulfide sulfone, and polyphenylene sulfone. Among these materials, polysulfone is generally used because it has high chemical, mechanical, and thermal stability and is easy to mold. The porous layer preferably contains these listed compounds as a main component.

[0022] The polysulfone preferably has a mass average molecular weight (Mw) of 10,000 to 200,000, more preferably 15,000 to 100,000, as measured by gel permeation chromatography (GPC) using N-methylpyrrolidone as a solvent and polystyrene as a standard. When the Mw of the polysulfone is 10,000 or more, the mechanical strength and heat resistance suitable for the porous layer can be obtained. When the Mw is 200,000 or less, the viscosity of the solution falls within an appropriate range, and good moldability can be achieved.

[0023] (Average pore size distribution of porous layer) Generally, when a porous layer is obtained on a substrate by non-solvent induced phase separation, the surface of the resin solution comes into contact with a large amount of solidifying fluid, causing instantaneous phase separation and the formation of fine and dense pores through solidification. On the other hand, since the inside of the resin solution comes into contact with the coagulating fluid that has diffused through the resin solution, the inside of the resin solution comes into contact with the coagulating fluid relatively slowly, which slows down the coagulation process and results in the formation of coarse and sparse pores, resulting in an asymmetric structure of the porous layer.

[0024] Considering the consolidation of the asymmetric structure, the lower the porosity, the higher the compressive strength during high temperature and high pressure operation, so consolidation is suppressed. On the other hand, the higher the porosity, the less favorable it is for consolidation, but the more water permeation paths there are in the porous layer, and the better the water permeability. In response to these conflicting demands for suppressing collapse and ensuring water permeation paths, the inventors have investigated designing the shape of the pore size distribution of the average pore size of the porous layer as a convex structure, rather than the conventional asymmetric structure. Figure 2 shows an SEM cross-sectional image of the porous membrane in the conventional composite semipermeable membrane produced in Comparative Example 2. As shown in Figure 2, in a conventional porous layer, the average pore size is maximum near the main surface (rear surface) on the substrate side and decreases toward the main surface (front surface) on the separation functional layer side, that is, the shape of the pore size distribution is usually asymmetric. Fig. 3 shows an SEM cross-sectional image of the porous membrane in the composite semipermeable membrane of the present invention produced in Example 2. As shown in Fig. 3, in the porous layer in the composite semipermeable membrane according to the embodiment of the present invention, the average pore size is small near the surface or back surface of the porous layer, and is maximum in the range excluding the surface or back surface, preferably in the central portion, that is, the shape of the average pore size distribution has a convex structure. As a result, compared with a conventional composite semipermeable membrane using a porous layer having an asymmetric structure, the composite semipermeable membrane according to the embodiment of the present invention suppresses compaction of the composite semipermeable membrane during high-temperature and high-pressure operation.

[0025] In order to obtain the porous layer according to the embodiment of the present invention, a means for contacting the solidifying fluid from both the main surface (rear surface) of the porous layer on the substrate side and the main surface (front surface) of the porous layer on the separation functional layer side can be mentioned. Therefore, in the case of a hollow porous membrane that does not contact with the solidifying fluid via a substrate or a resin sheet, the resin solution and the solidifying fluid directly contact each other from both sides, so that the pore size distribution of the above-mentioned convex structure can be easily obtained.

[0026] However, in composite semipermeable membranes that require high-pressure operation for seawater desalination, brackish water desalination, and other purposes, and in spiral-type separation membrane elements that use such composite semipermeable membranes, the strength of the composite semipermeable membrane is essential and the presence of a substrate is indispensable. Therefore, with conventional techniques, it has not been possible to obtain a composite semipermeable membrane that is composed of a porous layer having dense pores on the back surface of the porous layer and in which the pore size distribution has a convex structure.

[0027] The composite semipermeable membrane according to an embodiment of the present invention comprises a substrate, a porous layer provided on the substrate, and a separation functional layer provided on the porous layer, and the porous layer has an upwardly convex average pore size distribution from the back surface (the main surface on the substrate side) to the front surface (the main surface on the separation functional layer side), and has dense pores on the back surface.

[0028] Specifically, when a cross-sectional image of the porous layer taken by a scanning electron microscope is divided into 20 equal parts in the thickness direction, and cross-sectional images R1, R2, ... Rn... R20 (n is an integer from 1 to 20) are taken from the substrate side to the separation functional layer side, respectively, the maximum average pore size of the porous layer is present in one of cross-sectional images R3 to R18. This means that the average pore size distribution of the porous layer has an upwardly convex structure. The average pore size of the porous layer in each of cross-sectional images R1 and R2 is 0.1 μm or more and less than 0.6 μm, which means that the porous layer has dense pores on the back surface (the main surface on the substrate side). The average pore size can be measured by observing the cross-sectional structure of the porous layer with a SEM at 10,000 times magnification, as described in detail below.

[0029] Since it is desirable for the porous layer to have dense layers that can withstand compaction on both sides of the porous layer, the maximum average pore size of the porous layer is preferably present in any of the cross-sectional images R3 to R18, and more preferably present in any of the cross-sectional images R6 to R15. In addition, it is effective from the viewpoint of suppressing compaction that the average pore size of the porous layer is larger in the range excluding the vicinity of the surface and the vicinity of the back surface than in the vicinity of the surface and the vicinity of the back surface, and the maximum value of the average pore size of the porous layer may exist in multiple values ​​in the cross-sectional images R3 to R18. In this case, the average pore size distribution has a structure with two or more convex shapes.

[0030] When the average pore size of the porous layer in the cross-sectional images R1 and R2 is less than 0.1 μm, it is advantageous for suppressing compaction, but it is difficult to obtain a porous layer with high water generation. Also, when the average pore size of the porous layer in the cross-sectional images R1 and R2 is 0.6 μm or more, or when the average pore size in the cross-sectional image R1 is 0.1 μm or more and less than 0.6 μm but does not satisfy the requirement of 0.1 μm or more and less than 0.6 μm, it is advantageous for high water generation but disadvantageous for suppressing compaction.

[0031] Furthermore, in order to enhance the effect of suppressing compaction, it is desirable that a dense layer that can withstand compaction, that is, a layer with a small average pore size, is present in large amounts on the back surface side (substrate side). That is, it is preferable that the average pore diameter of the porous layer in the cross-sectional images R1, R2, and R3 is 0.1 μm or more and less than 0.6 μm, it is even more preferable that the average pore diameter of the porous layer in the cross-sectional images R1, R2, R3, and R4 is 0.1 μm or more and less than 0.6 μm, and it is particularly preferable that the average pore diameter of the porous layer in the cross-sectional images R1, R2, R3, R4, and R5 is 0.1 μm or more and less than 0.6 μm.

[0032] By setting the average pore size of the porous layer on the substrate side to 0.1 μm or more and less than 0.6 μm, compaction during high-temperature and high-pressure operation is suppressed, but it becomes difficult to ensure the amount of water produced. In order to solve the conflicting requirements of suppressing collapse and ensuring water permeation paths, the porous layer according to this embodiment needs to have a convex pore size distribution structure from the back surface to the front surface.

[0033] Furthermore, in order to simultaneously suppress compaction and achieve high water production, a larger convex structure is necessary, and when the average pore size of the porous layer in cross-sectional image R1 is X and the maximum average pore size of the porous layer from cross-sectional image R1 to R20 is Y, it is preferable that Y / X is 1.1 or more and 10 or less. If Y / X is 1.1 or more, there are many voids, which is advantageous for high water production, and if it is 10 or less, the voids of the porous layer do not become excessively large, making it possible to simultaneously suppress compaction.

[0034] In order to achieve both suppression of compaction and high water production, the maximum value Y of the average pore size is important, and the maximum value Y is preferably 0.5 μm or more and 2.0 μm or less, and more preferably 0.7 μm or more and 1.4 μm or less. By setting the maximum value Y to 0.5 μm or more, even if the porous layer has high density, high water production can be ensured, and by setting the maximum value Y to 2.0 μm or less, the number of sparse pores is not too large, which is advantageous for suppressing compaction.

[0035] (Main surface (rear surface) of the porous layer on the substrate side) Furthermore, in order to realize high water generation properties, it is preferable that sufficient flow paths are secured on the main surface of the porous layer facing the substrate. Here, in order to verify the presence or absence of the flow paths, for example, a specific dye is used. As an example, when an aqueous solution containing the dye substance methyl violet at a concentration of 0.05% by mass is brought into contact with only the substrate side of a composite semipermeable membrane for 5 minutes and the porous layer is peeled off from the substrate, the area of ​​the peeled surface of the porous layer stained with methyl violet on the substrate peeled surface is preferably 15% to 50% of the total peeled surface area, and more preferably 20% to 50%. The dyed area of ​​the porous layer on the contact surface with the substrate is dyed by contacting the dye from the substrate side, which is thought to visualize the water permeation flow paths. Therefore, the larger the dyed area, the more flow paths there are on the back surface of the porous layer, which can improve water permeability. In addition, since the water permeability is affected by the power of the pore size, the average pore size of the portion stained with methyl violet is preferably 0.5 mm or more, and more preferably 1.0 mm or more.

[0036] In the porous layer, the areas that were in contact with the substrate are not dyed because there are no pores. Therefore, if the dyed area is 15% or more, the porous layer can secure sufficient flow paths on the back side, and can achieve even higher water generation properties. In addition, if the dyed area is 50% or less, the contact area with the substrate is large, and sufficient adhesive strength between the substrate and the porous layer can be secured. The average pore size and the dyed area of ​​the dyed portion can be measured by observing the substrate-side peeled surface of the porous layer with a microscope at a magnification of 50. Details will be described later.

[0037] (Thickness of porous layer) The thickness of the porous layer is preferably 10 μm to 70 μm, more preferably 20 μm to 50 μm. By controlling the thickness of the porous layer within the above range, sufficient strength for pressure resistance can be maintained and the water permeability resistance layer can be designed to be small, so that the change in water permeability due to pressurized operation can be suppressed. The thickness of the composite of the substrate and the porous layer (hereinafter also referred to as "porous support") is preferably 30 μm or more and 300 μm or less, and more preferably 100 μm or more and 200 μm or less.

[0038] (Average surface pore size of porous layer) The average pore size of the surface of the porous layer (the main surface in contact with the separation functional layer) is preferably 3 nm to 10 nm. When the average pore size of the surface is in this range, the sagging of the separation functional layer can be suppressed to a small extent, and as a result, the salt rejection rate after high-pressure operation can be stabilized. The surface average pore size of the porous layer can be measured by surface observation using a scanning electron microscope (SEM). In the case of a composite semipermeable membrane, the surface of the porous layer can be observed by removing the separation functional layer. As a method for removing the separation functional layer from the composite semipermeable membrane, when the separation functional layer is made of polyamide as described later, a method of immersing the composite semipermeable membrane in an aqueous sodium hypochlorite solution for preferably 24 to 100 hours can be mentioned. The porous layer (which may be a porous support) is air-dried at room temperature, and the surface is observed at 200,000 times magnification using an SEM. In the obtained image, the hole part is image-analyzed to calculate the circle equivalent diameter. The same operation is performed for five samples, and the arithmetic mean of the data of the circle equivalent diameter of all the holes is calculated, and the surface average pore size is determined. Note that, before observing with an SEM, it is preferable to coat the sample as thinly as possible with a material selected from, for example, platinum, platinum-palladium, or ruthenium tetroxide. As the SEM, a scanning electron microscope (for example, S-5500 manufactured by Hitachi High-Technologies Corporation) can be used, and observation is performed at an accelerating voltage of 2 to 5 kV. Analysis software (Imagej) can be used for image analysis.

[0039] (Pure water permeability coefficient of pressurized porous layer) The porous layer (or the porous support) has a pure water permeability coefficient of 0.15 (× 10) after pressure application at 7 MPa, 45°C, and 6 hours. -9 m 3 / (m 2 sec Pa) or more, and more preferably 0.20 (× 10 -9 m 3 / (m 2It is more preferable that the water permeability of the porous layer (or the porous support) is 0.15 (×10 sec Pa) or more. -9 m 3 / (m 2 By setting the pressure drop to 0.1 s·sec·Pa or higher, the resistance of the porous layer in the composite separation membrane during high-pressure operation is sufficiently small. As a result, the decrease in the amount of water produced by the composite semipermeable membrane after high-pressure operation can be suppressed.

[0040] The pure water permeability coefficient of the porous layer after pressurization under the above conditions being in the above range means that the water path in the porous layer is maintained even under high temperature and high pressure conditions. In other words, by satisfying this condition, the composite semipermeable membrane can maintain water permeability even under high temperature and high pressure conditions.

[0041] In addition, since the pure water permeability coefficient of the porous support is equivalent to that of the porous layer, the pure water permeability coefficient of the porous support may be within the above range. In other words, the pure water permeability coefficient of the porous layer can also be calculated by removing the separation functional layer and measuring the pure water permeability coefficient of the porous support.

[0042] Pressurization is performed by passing an aqueous solution of 3.5% NaCl by mass, at 45°C and pH 6.5 through the composite semipermeable membrane at 45°C and 7 MPa for 6 hours. If the separation functional layer is removed before pressurization, a water-impermeable film such as a PTFE film is placed on the surface of the porous layer, and pressure is applied to the water-impermeable film side using the aqueous solution under the same conditions.

[0043] The pure water permeability coefficient of the porous layer (or porous support) is measured using the porous layer (or porous support) in a state in which the separation functional layer has been removed and the surface of the porous layer is exposed. Here, the separation functional layer may be removed either before or after pressurization. For example, the separation functional layer may be removed from the composite semipermeable membrane, and then the porous layer (which may be the porous support) may be pressurized, or the separation functional layer may be removed from the pressurized composite semipermeable membrane.

[0044] As a method for removing the separation functional layer from the composite semipermeable membrane, when the separation functional layer is composed of polyamide, a method of immersing the composite semipermeable membrane in a 2% by mass aqueous solution of sodium hypochlorite, preferably for 24 to 100 hours, can be mentioned.

[0045] (separation functional layer) The separation functional layer preferably contains a crosslinked aromatic polyamide, and more preferably contains a crosslinked aromatic polyamide as a main component. The main component refers to a component that occupies 50% by mass or more of the components of the separation functional layer. By containing 50% by mass or more of crosslinked aromatic polyamide, the separation functional layer can exhibit high removal performance. Furthermore, the content of crosslinked aromatic polyamide in the separation functional layer is preferably 80% by mass or more, and more preferably 90% by mass or more.

[0046] Crosslinked aromatic polyamides can be formed by chemically reacting polyfunctional aromatic amines with polyfunctional aromatic acid chlorides. At least one of the polyfunctional aromatic amines and polyfunctional aromatic acid chlorides preferably contains a compound with three or more functional groups. This results in a rigid molecular chain and a good pore structure for removing fine solutes such as hydrated ions and boron.

[0047] The polyfunctional aromatic amine means an aromatic amine having at least two or more amino groups, either primary or secondary, in one molecule, and at least one of the amino groups being a primary amino group. Examples of the polyfunctional aromatic amine include polyfunctional aromatic amines in which two amino groups are bonded to an aromatic ring at the ortho, meta, or para positions, such as o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, o-xylylenediamine, m-xylylenediamine, p-xylylenediamine, o-diaminopyridine, m-diaminopyridine, and p-diaminopyridine, and polyfunctional aromatic amines such as 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, 3-aminobenzylamine, and 4-aminobenzylamine. Other examples include aliphatic amines such as ethylenediamine and propylenediamine, and alicyclic polyfunctional amines such as 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, piperazine, 2,5-dimethylpiperazine, 2-methylpiperazine, 2,6-dimethylpiperazine, 2,3,5-trimethylpiperazine, 2,5-diethylpiperazine, 2,3,5-triethylpiperazine, 2-n-propylpiperazine, 2,5-di-n-butylpiperazine, 1,3-bispiperidylpropane, and 4-aminomethylpiperazine. These polyfunctional amines may be used alone or in combination.

[0048] In particular, m-phenylenediamine, p-phenylenediamine, and 1,3,5-triaminobenzene are preferably used in consideration of the selective separation, permeability, and heat resistance of the membrane. Among them, m-phenylenediamine (hereinafter also referred to as m-PDA) is more preferably used in view of ease of availability and ease of handling. These polyfunctional aromatic amines may be used alone or in combination of two or more kinds.

[0049] The polyfunctional aromatic acid chloride refers to an aromatic acid chloride having at least two chlorocarbonyl groups in one molecule. For example, the trifunctional acid chloride may be trimesic acid chloride, and the bifunctional acid chloride may be biphenyldicarboxylic acid dichloride, azobenzenedicarboxylic acid dichloride, terephthalic acid chloride, isophthalic acid chloride, naphthalenedicarboxylic acid chloride, and the like. In addition, the polyfunctional acid chloride may be aliphatic bifunctional acid halides such as adipoyl chloride and sebacoyl chloride, and alicyclic bifunctional acid halides such as cyclopentanedicarboxylic acid dichloride, cyclohexanedicarboxylic acid dichloride, and tetrahydrofurandicarboxylic acid dichloride. These polyfunctional acid halides may be used alone or in combination. Considering the selective separation property and heat resistance of the membrane, it is preferable to use a polyfunctional aromatic acid chloride having 2 to 4 carbonyl chloride groups in one molecule.

[0050] 2. Manufacturing method of composite semipermeable membrane (Porous layer forming process) The step of forming the porous layer includes the steps of: (a) a step of dissolving a thermoplastic resin (hereinafter referred to as resin) in a good solvent and disposing a resin solution on a substrate surface; (b) At the beginning of phase separation, a step of forming a flow of solidifying fluid in the resin solution from the substrate side to the separation functional layer forming surface side (for example, a step of pressing or sucking a solidifying fluid containing a non-solvent against the back surface of the substrate). (c) solidifying the resin in a resin solidification fluid. In the above step (a), the resin solution is applied onto the substrate. Then, in the above step (b), phase separation is initiated from the back surface of the porous layer (the main surface on the substrate side), and a region having dense pores in the above-mentioned range is obtained on the back surface side. That is, a porous layer is obtained by the competition between the phase separation progress rates from both the separation functional layer forming surface side and the substrate side. Then, in step (c), the resin is completely solidified to obtain a porous support body.

[0051] The step of forming the porous layer may further include a step of preparing a resin solution by dissolving a resin, which is a component of the porous layer, in a good solvent for the resin.

[0052] The "resin" is a material that is the main component of the porous layer, and is specifically as described above. A "good solvent" is one that dissolves resin. By selecting a good solvent, the speed of the good solvent flowing out of the resin solution in the above step (b) can be adjusted. As a result, the pore size on the substrate side and the flow path on the substrate surface of the porous layer can be controlled. As the good solvent, at least one solvent selected from the group consisting of amides such as N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), tetramethylurea (THU), N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), N,N-dimethylisobutyramide (DMIB), N,N-diisopropylisobutyramide, and N,N-bis(2-ethylhexyl)isobutyramide; lower alkyl ketones such as acetone and methyl ethyl ketone (MEK); esters such as trimethyl phosphate; and lactones such as γ-butyrolactone are preferably used. More preferably, the good solvent includes dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N-methyl-2-pyrrolidone (NMP).

[0053] For example, a solution of the above polysulfone can be cast onto a substrate to a certain thickness and then wet-coagulated in water to obtain a porous layer having fine pores with diameters of several 1 to 20 nm over most of the surface.

[0054] Step (a) can be carried out by applying a solution of the resin to the substrate or by immersing the substrate in the solution of the resin. The resin solution can be applied to the substrate by various coating methods, but a pre-metered coating method such as die coating, slide coating, curtain coating, etc., which can supply a precise amount of coating solution, is preferably used. Furthermore, in forming a porous layer, a slit die method for applying the resin solution is more preferably used.

[0055] When the resin solution contains polysulfone, the polysulfone concentration (i.e., solid content concentration) is preferably 15% by mass or more, more preferably 16% by mass or more, and even more preferably 17% by mass or more. The polysulfone concentration of the resin solution is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less.

[0056] The thickness of the back surface dense pore region can be adjusted by setting the polysulfone concentration within the above range and forming a flow of a solidifying fluid as described below.

[0057] In addition, by keeping the polysulfone concentration at 30% by mass or less, the viscosity of the resin solution is in an appropriate range, and a structure in which the pores in the dense pore region are connected can be obtained. Therefore, within this range, a good initial water production capacity of the composite semipermeable membrane and a good water production capacity after high-temperature and high-pressure operation can be obtained.

[0058] When polysulfone is used, the temperature of the resin solution during application is usually within the range of 10 to 60° C. If the temperature is within this range, the resin solution can be applied without precipitating, which is preferable. The preferable temperature range of the resin solution may be appropriately adjusted depending on the viscosity of the resin solution used.

[0059] The polymer contained in the resin solution can be appropriately adjusted taking into consideration various properties such as strength, permeability, and surface properties of the porous layer to be produced.

[0060] The solvent contained in the resin solution may be the same or different as long as it is a good solvent for the resin. The solvent can be appropriately adjusted taking into consideration the strength characteristics of the porous layer to be produced and the impregnation of the base material with the resin solution. Examples of the non-solvent include water, hexane, pentane, benzene, toluene, methanol, ethanol, trichloroethylene, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butylene glycol, pentanediol, hexanediol, low molecular weight polyethylene glycol and other aliphatic hydrocarbons, aromatic hydrocarbons, aliphatic alcohols, and mixed solvents thereof.

[0061] The resin solution may contain additives for adjusting the dense pore region, void region, pore size, porosity, hydrophilicity, elasticity, etc. of the porous layer. Examples of additives for adjusting the pore size and porosity include water, alcohols, polyethylene glycol, polyvinylpyrrolidone, polyvinyl alcohol, polyacrylic acid, and other water-soluble polymers or salts thereof, as well as inorganic salts such as lithium chloride, sodium chloride, calcium chloride, and lithium nitrate, formaldehyde, and formamide, but are not limited thereto. Examples of additives for adjusting the hydrophilicity and elasticity include various surfactants.

[0062] In addition, by containing a non-solvent such as water and a good solvent in the solidification fluid, it is possible to form a dense layer on the membrane surface by non-solvent-induced phase separation. The solidification fluid may be a liquid or a gas.

[0063] The concentration of the good solvent in the coagulation bath is preferably 0.5% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and is preferably 50% by mass or less, more preferably 30% by mass or less. The concentration of the non-solvent in the coagulation bath is preferably 50% by mass or more, more preferably 70% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less.

[0064] In order to form an area on the back surface side having a cross-sectional average pore size of 0.1 μm or more and less than 0.6 μm and to form a porous layer having an upwardly convex cross-sectional pore size distribution, it is preferable to form a flow of solidifying fluid from the back surface (substrate side) to the opposite side in the thickness direction of the layer formed from the resin solution at the early stage of phase separation (before the resin solution forming the porous layer is completely solidified).

[0065] The initial stage of phase separation depends on the type, concentration and temperature of the thermoplastic resin, but for example, when polysulfone resin is used as the thermoplastic resin and DMF is used as the good solvent, it is preferably within 3 seconds, more preferably within 2 seconds, and even more preferably within 1 second after contact with the coagulation liquid. Specific examples of the means for injecting the coagulation liquid include a method of pushing the coagulation liquid from the substrate side toward the resin solution side, and when pushing the coagulation liquid, the pressure is preferably 5 kPa or more, more preferably 7 kPa or more, and even more preferably 9 kPa or more. It is also preferable to push the coagulation liquid in multiple stages of two or more times, and in that case, the pressure per time is preferably 1 kPa or more, more preferably 3 kPa or more, and even more preferably 5 kPa or more.

[0066] By pushing the solidifying fluid in multiple stages, the solidifying fluid penetrates into the porous layer, so that micropores can be formed over a wider range from the substrate side toward the separation functional layer.

[0067] The pushing or suction time is preferably 0.1 to 3 seconds, more preferably 0.5 to 3 seconds per time. By controlling the time within this range, the solidifying fluid can be pushed in sufficiently, and the solidifying fluid can be impregnated into the porous layer, so that micropores can be formed over a wider range from the substrate side toward the separating functional layer.

[0068] By forming a flow of solidifying fluid before solidification, the thickness of the region having dense pores in the above-mentioned range on the substrate side can be controlled. In addition, by controlling the time for forming the flow of solidifying fluid, the degree of convex structure of the cross-sectional pore size distribution can be controlled, and by controlling the strength of the flow of solidifying fluid, the flow path on the substrate side can be secured.

[0069] Specific examples of means for forming a flow include, as in the above-mentioned method, using pressure to push the solidifying fluid from the substrate side toward the resin solution, or sucking the solidifying fluid from the substrate side, and a method in which a hydrophilized substrate is used to induce a flow of the solidifying fluid into the resin solution.

[0070] The liquid temperature of the coagulation bath is preferably within a range of 5 to 30° C., more preferably 5 to 20° C. If it is 30° C. or lower, the vibration of the coagulation bath surface due to thermal motion is not intensified, and the smoothness of the surface of the porous layer is increased. If it is 5° C. or higher, a sufficient coagulation speed is obtained, and film formability is good.

[0071] Next, the obtained porous support is preferably washed with hot water to remove the membrane-forming solvent remaining in the membrane. The temperature of the hot water is preferably 50 to 100°C, more preferably 60 to 95°C. By washing at 100°C or less, the shrinkage of the porous support can be kept small. By washing at 50°C or more, a high washing effect can be obtained.

[0072] (Separation functional layer formation process) Next, a method for forming the separation functional layer will be described. The separation functional layer can be obtained, for example, by chemically reacting a polyfunctional aromatic amine with a polyfunctional aromatic acid chloride to form a crosslinked aromatic polyamide as described above. As a method of chemical reaction, the interfacial polymerization method is the most preferable from the viewpoint of productivity and performance. That is, the separation functional layer is formed by performing interfacial polycondensation on the surface of the porous layer using an aqueous solution containing a polyfunctional amine and an organic solvent containing a polyfunctional acid halide. Through this process, a crosslinked aromatic polyamide is formed.

[0073] More specifically, the interfacial polymerization step includes the steps of (d) contacting the porous layer with an aqueous solution containing a polyfunctional aromatic amine, and (e) after step (d), contacting the porous layer with a solution in which a polyfunctional aromatic acid chloride is dissolved.

[0074] In step (d), the concentration of the polyfunctional aromatic amine in the aqueous polyfunctional aromatic amine solution is preferably in the range of 0.1% by mass to 20% by mass, more preferably in the range of 0.5% by mass to 15% by mass. When the concentration of the polyfunctional aromatic amine is in this range, sufficient solute removal performance and water permeability can be obtained.

[0075] The contact of the polyfunctional aromatic amine aqueous solution is preferably performed uniformly and continuously on the porous layer.Specific examples include a method of coating the polyfunctional aromatic amine aqueous solution on the porous layer, and a method of immersing the porous layer in the polyfunctional aromatic amine aqueous solution.The contact time of the porous layer and the polyfunctional aromatic amine aqueous solution is preferably 1 second or more and 10 minutes or less, and more preferably 10 seconds or more and 3 minutes or less.

[0076] After the polyfunctional aromatic amine aqueous solution is brought into contact with the porous layer, it is preferable to drain the solution so that no droplets remain on the membrane. By draining the solution, the occurrence of defects in the separation functional layer can be suppressed. As a method of draining the solution, a method of vertically holding the porous support after contact with the polyfunctional aromatic amine aqueous solution to allow excess aqueous solution to flow down naturally, or a method of blowing an air flow such as nitrogen from an air nozzle to forcibly drain the solution can be used. In addition, after draining, the membrane surface can be dried to remove some of the water content of the aqueous solution.

[0077] The concentration of the polyfunctional aromatic acid chloride in the organic solvent solution is preferably in the range of 0.01% by mass to 10% by mass, and more preferably in the range of 0.02% by mass to 2.0% by mass, because a sufficient reaction rate can be obtained by making it 0.01% by mass or more, and the occurrence of side reactions can be suppressed by making it 10% by mass or less.

[0078] The organic solvent is preferably one that is immiscible with water, dissolves the polyfunctional aromatic acid chloride, and does not destroy the porous support, and is inactive against the polyfunctional aromatic amine and the polyfunctional aromatic acid chloride. Preferred examples include hydrocarbon compounds and mixed solvents such as n-nonane, n-decane, n-undecane, n-dodecane, isooctane, isodecane, and isododecane.

[0079] The method of contacting the porous layer with the organic solvent solution of the polyfunctional aromatic acid chloride and the aqueous polyfunctional aromatic amine solution may be the same as the method of coating the porous layer with the aqueous polyfunctional aromatic amine solution.

[0080] After the reaction, the organic solvent is removed from the membrane surface by, for example, a method of holding the support membrane vertically and allowing the excess organic solvent to flow down by gravity, a method of blowing air onto the organic solvent with a blower to dry and remove the excess organic solvent, or a method of removing the excess organic solvent with a mixed fluid of water and air.

[0081] In addition, depending on the performance of the intended composite semipermeable membrane, a crosslinked aliphatic polyamide or a crosslinked alicyclic polyamide may be formed by using an aliphatic amine or an alicyclic polyfunctional amine instead of a polyfunctional aromatic amine, and an aliphatic bifunctional acid halide or an alicyclic bifunctional acid halide instead of a polyfunctional aromatic acid chloride.

[0082] (Method of using composite semipermeable membrane) The composite semipermeable membrane according to the embodiment of the present invention is preferably used as a spiral-type composite separation membrane element by being wound around a cylindrical water collection pipe having a large number of holes, together with a feed water flow path material such as a plastic net, a permeate water flow path material such as tricot, and, if necessary, a film for increasing pressure resistance. Furthermore, this element can be connected in series or in parallel and housed in a pressure vessel to form a composite separation membrane module.

[0083] Furthermore, the above-mentioned composite semipermeable membrane, its element, and module can be combined with a pump for supplying feed water thereto, a device for pretreating the feed water, etc. to form a fluid separation device. By using this separation device, the feed water can be separated into permeated water such as drinking water and concentrated water that did not permeate the membrane, thereby obtaining water suitable for the purpose.

[0084] The feed water to be treated by the composite semipermeable membrane according to the embodiment of the present invention includes liquid mixtures containing 500 mg / L to 100 g / L of TDS (Total Dissolved Solids), such as seawater, brackish water, and wastewater. In general, TDS refers to the amount of total dissolved solids, and is expressed as "mass / volume" or "mass ratio." According to the definition, it can be calculated from the weight of the residue obtained by evaporating a solution filtered through a 0.45 micron filter at a temperature of 39.5°C to 40.5°C, but it can be calculated more simply from the practical salinity (S).

[0085] The higher the operating pressure of the fluid separation device, the higher the solute removal rate, but the more energy required for operation will increase. Also, taking into consideration the durability of the composite semipermeable membrane, the operating pressure when the treated water is passed through the composite semipermeable membrane is preferably 0.5 MPa or more and 12 MPa or less. As the supply water temperature increases, the solute removal rate decreases, but as the temperature decreases, the membrane permeation flux also decreases, so it is preferably 5°C or more and 55°C or less. When operating at temperatures above 35°C and with a TSD of 40,000 mg / L or more, a typical composite semipermeable membrane experiences a significant drop in water production due to compaction of the porous layer. This necessitates an increase in the operating pressure to maintain a constant water production rate in the fluid separation unit, which increases the energy required for operation. In the water production method using the composite semipermeable membrane according to the embodiment of the present invention, even when operated at 35° C. or higher and with a TSD of 40,000 mg / L or more, compaction of the porous layer does not progress, so that a decrease in the water production rate of the composite semipermeable membrane is suppressed, the increase in operating pressure for keeping the water production rate of the fluid separation unit constant can be reduced, and the increase in energy required for operation can be reduced. In addition, if the pH of the feed water becomes high, there is a risk of scale formation of magnesium and the like in the case of feed water with a high solute concentration, such as seawater, and there is also concern that membrane deterioration may occur due to operation at a high pH, ​​so operation in the neutral range is preferable.

[0086] Based on the above, this specification discloses the following composite semipermeable membrane and separation membrane element. [1] A composite semipermeable membrane having a substrate, a porous layer provided on the substrate, and a separation functional layer provided on the porous layer, A cross-sectional image of the porous layer taken by a scanning electron microscope is divided into 20 equal parts in the thickness direction, and cross-sectional images R1, R2, . . . Rn, . . . R20 (n is an integer from 1 to 20) are taken from the substrate side to the separation functional layer side, respectively. the maximum average pore diameter of the porous layer is present in any one of the cross-sectional images R3 to R18, The average pore size of the porous layer in the cross-sectional image R1 and the cross-sectional image R2 is 0.1 μm or more and less than 0.6 μm. [2] The composite semipermeable membrane according to [1], wherein, when an average pore size of the porous layer in the cross-sectional image R1 is X and a maximum average pore size of the porous layer in the cross-sectional images R1 to R20 is Y, Y / X is 1.1 or more and 10 or less. [3] The composite semipermeable membrane according to [1] or [2], wherein the average pore size of the porous layer in the cross-sectional image R1, the cross-sectional image R2, and the cross-sectional image R3 is 0.1 μm or more and less than 0.6 μm. [4] The composite semipermeable membrane according to any one of [1] to [3], wherein the average pore size of the porous layer in the cross-sectional image R1, the cross-sectional image R2, the cross-sectional image R3, and the cross-sectional image R4 is 0.1 μm or more and less than 0.6 μm. [5] The composite semipermeable membrane according to any one of [1] to [4], wherein the average pore size of the porous layer in the cross-sectional image R1, the cross-sectional image R2, the cross-sectional image R3, the cross-sectional image R4, and the cross-sectional image R5 is 0.1 μm or more and less than 0.6 μm. [6] The composite semipermeable membrane according to any one of [1] to [5], wherein the maximum average pore size of the porous layer in the cross-sectional images R1 to R20 is 0.5 μm or more and 2.0 μm or less. [7] The composite semipermeable membrane according to any one of [1] to [6], wherein, after contacting only the substrate side of the composite semipermeable membrane with a 0.05% by mass aqueous solution of methyl violet for 5 minutes and peeling the substrate from the porous layer, the area ratio of the dyed peeled surface on the peeled surface of the porous layer is 15% or more and 50% or less of the entire area of ​​the peeled surface. [8] The composite semipermeable membrane according to any one of [1] to [7], wherein the porous layer has a thickness of 20 μm or more and 70 μm or less. [9] A fresh water production method comprising a separation step of separating an aqueous solution having a temperature of 35°C or higher and a TDS (Total Dissolved Solids) of 40,000 mg / L or higher into a concentrated water and a permeated water by using the composite semipermeable membrane according to any one of [1] to [8]. EXAMPLES

[0087] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto.

[0088] 1. Average pore size of the porous layer As a pretreatment for maintaining the porous morphology, the membrane sample was immersed in liquid nitrogen to freeze it, then cut and dried. After that, a thin layer of platinum / palladium or ruthenium tetroxide, preferably ruthenium tetroxide, was vapor-deposited onto the membrane cross section to obtain an observation sample. The average pore diameter calculated from the cross-sectional image of the porous layer was measured by continuously observing the cross-section of the porous layer (or porous support) from the substrate side to the separation functional layer side using a scanning electron microscope (SEM) at a magnification of 10,000 times. First, the obtained cross-sectional images were linked to generate an image of the entire porous layer. The generated image was divided into 20 equal parts with respect to the thickness T of the porous layer, and 20 cross-sectional images R1, R2, ... Rn... R20 (n is an integer between 1 and 20, and the smaller n, the closer it is to the back surface). Each of these images was subjected to the following processing and analysis using image-J, an image analysis software. First, the image was converted to an 8-bit image using the "image" function. Next, the minimum and maximum thresholds were set to 0 and 105, respectively, and binarization was performed using "Threshold," with the range between the minimum and maximum values ​​being black and the rest being white (the holes were black). For each image, the area S of the black area (hole) and the number of holes N are calculated, and the cross-sectional hole diameter Z is the diameter of a circle with the same area (equivalent circle diameter), Z = 2 × (S / π). 1 / 2 By these operations, cross-sectional pore diameters Z at 20 points from the substrate side toward the separation functional layer direction are obtained from the 20 images. The same procedure was repeated 10 times, excluding positions where there were pores with a major axis of 5 μm or more, and the cross-sectional pore diameter Z in each image was calculated. The arithmetic mean value of the 10 cross-sectional pore diameters in the direction parallel to the substrate was taken as the average cross-sectional pore diameter.

[0089] 2. Staining area of ​​methyl violet solution After contacting the substrate side of the wet composite semipermeable membrane with a 0.05% by mass aqueous solution of methyl violet for 5 minutes, the aqueous solution was removed from the substrate and air-dried at room temperature. Next, the substrate was peeled off from the porous layer in a 180° direction at a peeling speed of 50 mm / min, and the contact surface of the porous layer exposed by peeling with the substrate was observed at 50x magnification with a digital microscope to obtain an image. The image of the contact surface of the porous layer with the substrate obtained was analyzed using analysis software (image-j) to calculate the proportion of the stained area relative to the area of ​​the entire analysis range. The same operation was performed on three samples, and the arithmetic mean value of the three points was adopted.

[0090] 3. Thickness of the porous layer The thickness of the composite semipermeable membrane that had been air-dried at room temperature was measured using a dial thickness gauge (constant pressure thickness gauge PG-01A, manufactured by Techlock Corporation). Next, the substrate was peeled off from the porous layer in a 180° direction at a peeling speed of 50 mm / min, and the thickness of the resulting substrate was measured using a dial thickness gauge. Finally, the thickness of the porous layer was calculated by subtracting the thickness of the substrate from the thickness of the composite semipermeable membrane. The thickness was measured at any 20 points, and the arithmetic mean was calculated to determine the thickness of the substrate and the composite semipermeable membrane.

[0091] 4. Pure water permeability coefficient of the porous layer after pressure application Raw water (NaCl concentration 4.0% by mass) adjusted to pH 6.5 at a temperature of 35°C to 45°C was supplied to the composite separation membrane at an operating pressure of 7.0 MPa, and membrane filtration was carried out for 6 hours. Next, the composite separation membrane was immersed in a 2% by mass aqueous solution of sodium hypochlorite at 25°C for 100 hours to remove the polyamide separation function layer, and a porous support was obtained. The obtained porous support was cut into a circle with a diameter of 4.3 cm, and the cut sample was set in a stirring type ultra holder (UHP-43K manufactured by Advantec Toyo Co., Ltd.) (effective filtration area: 10.9 cm 2 Next, pure water at 25°C was poured into the container, the cap was attached, and the pressure in the porous support was increased to 0.2 MPa with nitrogen. Finally, the amount of pure water permeated at a certain time was measured, and the pure water permeability coefficient (× 10 -9 m 3 / m 2 ·s·Pa) was calculated. Pure water permeability coefficient = Pure water permeation amount ÷ (effective filtration area of ​​porous support × water collection time × supply pressure)

[0092] 5. Desalination rate (NaCl removal rate) and water production rate (Flux) of composite semipermeable membrane Raw water (NaCl concentration, 3.2% by mass) adjusted to a temperature of 25°C and pH 6.5 was supplied to the composite semipermeable membrane at an operating pressure of 5.5 MPa and membrane filtration was performed for 2 hours. After that, the electrical conductivity of the supply water and the permeated water was measured with a multi-purpose water quality meter (MM60R) manufactured by DKK-TOA Corporation. Next, the electrical conductivity was converted to calculate the NaCl concentration using a calibration curve prepared in advance. From this NaCl concentration, the salt removal performance, i.e., the NaCl removal rate, was calculated using the following formula. NaCl removal rate (%) = 100 × {1-(NaCl concentration in permeate water / NaCl concentration in feed water)} In the above test, the amount of water passing through the membrane in a certain period of time was measured and converted into the amount of water passing through (cubic meters) per day per square meter of membrane surface, and the amount of water produced (m 3 / m 2 The data are expressed as 100 mg / day.

[0093] 6. Desalination rate (MgSO4 removal rate) and water production rate (Flux) of composite semipermeable membrane Saltwater adjusted to a temperature of 25°C, pH 6.5, and MgSO4 concentration of 2000 mg / L was supplied to the composite semipermeable membrane at an operating pressure of 0.48 MPa to perform membrane filtration. The electrical conductivity of the supply water and permeate was then measured using a multi-purpose water quality meter (MM60R) manufactured by DKK-TOA Corporation. The electrical conductivity was then converted using a calibration curve prepared in advance to calculate the MgSO4 concentration. The salt removal performance, i.e., MgSO4 concentration, was calculated from this MgSO4 concentration using the following formula. MgSO4 removal rate (%) = 100 x {1 - (MgSO4 concentration in permeate water / MgSO4 concentration in feed water)} In the above test, the amount of water passing through the membrane in a certain period of time was measured and converted into the amount of water passing through (cubic meters) per day per square meter of membrane surface, and the amount of water produced (m 3 / m 2 The data are expressed as 100 mg / day.

[0094] 7. Desalination rate after pressurization (NaCl removal rate), amount of water produced after pressurization Raw water adjusted to pH 6.5 (NaCl concentration 4.0% by mass) was supplied to the composite semipermeable membrane whose performance was evaluated in 5 above at a temperature of 35°C or 45°C and an operating pressure of 7.0 MPa to perform membrane filtration for 6 hours, and then the temperature was returned to 25°C and the operating pressure to 5.5 MPa, and the NaCl removal rate and water production rate after pressurization were determined in the same manner as in 5 above, thereby determining the salt rejection rate and water production rate after high-pressure operation.

[0095] 8. Desalination rate after pressurization (MgSO4 removal rate), amount of water produced after pressurization Raw water adjusted to pH 6.5 (MgSO4 concentration 4.0% by mass) was supplied to the composite semipermeable membrane whose performance was evaluated in 6 above at 45°C and an operating pressure of 7.0 MPa to perform membrane filtration for 6 hours, and then the temperature was returned to 25°C and the operating pressure to 0.48 MPa, and the MgSO4 removal rate and water production rate after pressurization were determined in the same manner as in 6 above, thereby determining the salt rejection rate and water production rate after high-pressure operation.

[0096] 9. Pure water permeability coefficient of substrate The substrate was cut into a circle with a diameter of 4.3 cm, and the cut sample was placed in a stirring type ultra holder (UHP-43K manufactured by Advantec Toyo Co., Ltd.) (effective filtration area: 10.9 cm 2 Next, pure water at 25°C was placed in the container, the cap was attached, and the pressure was increased to 10 kPa with nitrogen. Finally, the amount of pure water permeated at a certain time was measured, and the pure water permeability coefficient (×10 -9 m 3 / m 2 ·s·Pa) was calculated. Pure water permeability coefficient = Pure water permeation amount ÷ (effective filtration area of ​​substrate × water collection time × supply pressure)

[0097] Example 1 The base material is a long-fiber polyester nonwoven fabric (thickness 90 μm, pure water permeability coefficient 800 (× 10 -9 m 3 / (m 2 An 18 mass % solution of polysulfone in DMF was applied to a substrate (1.0 sec·Pa)) at 25°C to a coating thickness of 160 μm, and then 1.0 second later, the substrate was immersed in pure water at 20°C. 1.0 second after the start of immersion, pure water at 20°C was pressed against the substrate from the side with a pressure of 5 kPa for 0.5 seconds. Thereafter, the substrate was left in pure water for 1 minute to prepare a porous support. The thickness of the porous layer was 40 μm. The obtained porous support was immersed in a 3% by mass aqueous solution of m-phenylenediamine (m-PDA) for 2 minutes. The porous support was slowly pulled up vertically, and excess aqueous solution was removed from the surface of the porous support by blowing nitrogen onto it with an air nozzle. Then, a decane solution containing 0.165% by mass of trimesoyl chloride (TMC) was applied so that the surface was completely wet, and the surface was left to stand for 1 minute. The membrane was then turned vertically to drain off excess solution, and the membrane was washed with pure water. Through the above operations, a composite semipermeable membrane with a crosslinked aromatic polyamide separation functional layer was obtained. The post-pressurization salt rejection rate (NaCl removal rate) and post-pressurization water production rate were measured by supplying raw water (NaCl concentration, 4.0% by mass) adjusted to pH 6.5 at a temperature of 45°C and an operating pressure of 7.0 MPa and carrying out membrane filtration treatment for 6 hours, and then supplying raw water (NaCl concentration, 3.2% by mass) adjusted to pH 6.5 at a temperature of 25°C and an operating pressure of 5.5 MPa and carrying out membrane filtration treatment for 2 hours.

[0098] Example 2 A composite semipermeable membrane having a crosslinked aromatic polyamide separation functional layer was obtained in the same manner as in Example 1, except that, 1.0 second after the start of immersion in pure water, pure water at 20°C was pressed against the substrate side at a pressure of 7 kPa for 0.3 seconds. The salt rejection rate after pressurization (NaCl removal rate) and the amount of water produced after pressurization were measured in the same manner as in Example 1.

[0099] Example 3 A composite semipermeable membrane having a crosslinked aromatic polyamide separation functional layer was obtained in the same manner as in Example 1, except that, 1.0 second after the start of immersion in pure water, pure water at 20°C was pressed against the substrate side at a pressure of 9 kPa for 0.2 seconds. The salt rejection rate after pressurization (NaCl removal rate) and the amount of water produced after pressurization were measured in the same manner as in Example 1.

[0100] Example 4 Except for the fact that the coating thickness of the polysulfone solution was set to 120 μm when preparing the porous support, a composite semipermeable membrane having a crosslinked aromatic polyamide separation functional layer was obtained in the same manner as in Example 1. In addition, the salt rejection rate after pressurization (NaCl removal rate) and the amount of water produced after pressurization were measured in the same manner as in Example 1.

[0101] Example 5 Except for the fact that the coating thickness of the polysulfone solution was 180 μm when preparing the porous support, a composite semipermeable membrane having a crosslinked aromatic polyamide separation functional layer was obtained in the same manner as in Example 1. Moreover, the salt rejection rate after pressurization (NaCl removal rate) and the amount of water produced after pressurization were measured in the same manner as in Example 1.

[0102] Example 6 In preparing the porous support, 0.5 seconds after the start of immersion in pure water, pure water at 20°C was pressed against the substrate from the substrate side at a pressure of 3 kPa for 0.3 seconds, and 1.0 seconds later, pure water at 20°C was pressed against the substrate from the substrate side at a pressure of 5 kPa for 0.3 seconds, and then the porous support was allowed to stand in the pure water for 1 minute, but other than this, a composite semipermeable membrane having a crosslinked aromatic polyamide separation functional layer was obtained in the same manner as in Example 1. In addition, the salt rejection rate after pressurization (NaCl removal rate) and the amount of water produced after pressurization were measured in the same manner as in Example 1.

[0103] Example 7 In preparing the porous support, 1.0 second after the start of immersion in pure water, pure water at 20°C was pressed against the substrate side at a pressure of 5 kPa for 0.3 seconds, and 0.5 seconds later, pure water at 20°C was pressed against the substrate side at a pressure of 5 kPa for 0.3 seconds, and then the porous support was allowed to stand in the pure water for 1 minute, in the same manner as in Example 1, to obtain a composite semipermeable membrane having a crosslinked aromatic polyamide separation functional layer. In addition, the salt rejection rate after pressurization (NaCl removal rate) and the amount of water produced after pressurization were measured in the same manner as in Example 1.

[0104] Example 8 In the same manner as in Example 1, a composite semipermeable membrane having a crosslinked aromatic polyamide separating functional layer was obtained. The post-pressurization salt rejection rate (NaCl removal rate) and post-pressurization water production rate were measured by supplying raw water (NaCl concentration: 4.0% by mass) adjusted to pH 6.5 at a temperature of 35°C and an operating pressure of 7.0 MPa and carrying out membrane filtration treatment for 6 hours, and then supplying raw water (NaCl concentration: 3.2% by mass) adjusted to pH 6.5 at a temperature of 25°C and an operating pressure of 5.5 MPa and carrying out membrane filtration treatment for 2 hours.

[0105] Example 9 First, a porous support was prepared in the same manner as in Example 1. The obtained porous support was immersed in an aqueous solution containing 1.0% by mass of piperazine and 100 ppm of sodium dodecyl diphenyl ether disulfonate for 30 seconds, and then the porous support was slowly pulled up vertically and nitrogen was blown from an air nozzle to remove excess aqueous solution from the surface of the porous layer. Next, a decane solution containing 0.40% by mass of trimesic acid chloride (TMC) was applied so that the surface of the porous layer was completely wetted and left to stand for 30 seconds, after which the membrane was turned vertically to remove excess solution by draining, and the decane solution was dried by blowing air at 25 ° C. using a blower. Finally, a composite semipermeable membrane having a crosslinked aliphatic polyamide separation functional layer was obtained by washing with pure water at 80 ° C.

[0106] Example 10 A composite semipermeable membrane having a crosslinked aliphatic polyamide separating function layer was obtained in the same manner as in Example 9, except that a porous support was prepared in the same manner as in Example 7.

[0107] Comparative Example 1 The base material is a polyester nonwoven fabric (thickness 90 μm, pure water permeability coefficient 700 (× 10 -9 m 3 / (m 2 A 18% by mass solution of polysulfone in DMF was applied to a substrate (1.0 sq. cm) at 25°C (coating thickness: 150 μm) and 1.0 sec after application, the substrate was immersed in pure water at 20°C. Within 1 sec after immersion in the pure water, pure water was pressed against the substrate side at a pressure of 3 kPa for approximately 10 sec, and the substrate was then left in the pure water for 1 minute to produce a porous support with a porous layer formed on the substrate. Otherwise, a composite semipermeable membrane having a crosslinked aromatic polyamide separating functional layer was obtained in the same manner as in Example 1. Moreover, in the same manner as in Example 1, the salt rejection rate after pressurization (NaCl removal rate) and the amount of water produced after pressurization were measured.

[0108] Comparative Example 2 The base material is a long-fiber polyester nonwoven fabric (thickness 90 μm, pure water permeability coefficient 800 (× 10 -9 m 3 / (m 2A 18% by mass solution of polysulfone in DMF was cast onto the support (1.0 MPa, 1.0 s ... Otherwise, a composite semipermeable membrane having a crosslinked aromatic polyamide separating functional layer was obtained in the same manner as in Example 1. Moreover, in the same manner as in Example 1, the salt rejection rate after pressurization (NaCl removal rate) and the amount of water produced after pressurization were measured.

[0109] Comparative Example 3 Except for changing the polysulfone concentration to 14.5% by mass, a composite semipermeable membrane having a crosslinked aromatic polyamide separation functional layer was obtained in the same manner as in Comparative Example 2. In addition, the salt rejection rate after pressurization (NaCl removal rate) and the amount of water produced after pressurization were measured in the same manner as in Example 1.

[0110] Comparative Example 4 A composite semipermeable membrane having a crosslinked aromatic polyamide separation functional layer was obtained in the same manner as in Example 1, except that a porous support was prepared in the same manner as in Comparative Example 1. The salt rejection rate after pressurization (NaCl removal rate) and the amount of water produced after pressurization were measured in the same manner as in Example 8.

[0111] Comparative Example 5 A composite semipermeable membrane having a crosslinked aliphatic polyamide separating function layer was obtained in the same manner as in Example 6, except that a porous support was prepared in the same manner as in Comparative Example 1.

[0112] The properties of the porous layer obtained as above are shown in Table 1, and the performance of the composite semipermeable membrane is shown in Tables 2 and 3. FIG. 4 shows SEM cross-sectional images of the porous layers in Examples 2, 6, and 7 and Comparative Examples 1 and 2, and the distribution of the average pore size. Furthermore, an SEM cross-sectional image of the porous membrane in the composite semipermeable membrane of Comparative Example 2 is shown in FIG. 2, and an SEM cross-sectional image of the porous membrane in the composite semipermeable membrane of Example 2 is shown in FIG.

[0113] [Table 1]

[0114] [Table 2]

[0115] [Table 3]

[0116] As is clear from the results shown in Tables 1, 2, and 3, the composite semipermeable membranes of Examples 1 to 9, in which the maximum average pore size of the porous layer is present in any of Images R3 to R18 and the average pore size of the porous layer in Images R1 and R2 is 0.1 μm or more and less than 0.6 μm, respectively, have sufficient water production and salt removal properties even after high-temperature and high-pressure operation, and are able to suppress a decrease in the amount of water produced. Furthermore, in the composite semipermeable membranes of Examples 2 and 3, in which the maximum average pore size of the porous layer was observed in Images R10 and R11, the average pore size was maximum near the center of the porous layer, and particularly high water production ability, salt rejection ability, and effect of suppressing a decrease in the amount of water produced were obtained. Furthermore, the composite semipermeable membranes of Examples 6, 7, and 10, in which the average pore size of the porous layer in Images R1 to R5 is 0.1 μm or more and less than 0.6 μm, respectively, also exhibited particularly high water production, salt removal, and suppression of a decrease in the amount of water produced. This is believed to be because the region in which pores with small average pore sizes exist is widely present on the back surface side (substrate side) of the porous layer, so that the pores are less likely to collapse even under high-pressure operation, and the effect of suppressing compaction is easily achieved. In the composite semipermeable membranes of Comparative Examples 1, 4, and 5, in which the average pore size of the porous layer in Image R2 exceeded 0.6 μm, the amount of water produced decreased after high-temperature and high-pressure operation. This is thought to be because the area in which pores with a small average pore size existed was not present on the back side (substrate side) of the porous layer, and therefore the pores were crushed by high-pressure operation, and the effect of suppressing compaction was not obtained. The composite semipermeable membranes of Comparative Example 2 and Comparative Example 3, in which the maximum average pore size of the porous layer is present in Image R1, also showed a decrease in the amount of water produced after high-temperature and high-pressure operation. This is believed to be because the pore size distribution of the porous layer does not have a convex structure from the back surface (substrate side) to the front surface (separation functional layer side), and therefore sufficient water permeation paths were not secured. [Industrial Applicability]

[0117] The composite semipermeable membrane according to the embodiment of the present invention is useful as a composite separation membrane, and is used, for example, in seawater desalination, brackish water desalination, drinking water production, industrial ultrapure water production, wastewater treatment, and valuable resource recovery. [Explanation of symbols]

[0118] 1 Composite semipermeable membrane 2 Base material 3 Porous layer 4 Separation functional layer 11 Surface 12 Back side

Claims

1. A composite semipermeable membrane having a substrate, a porous layer provided on the substrate, and a separation functional layer provided on the porous layer, A cross-sectional image of the porous layer taken by a scanning electron microscope is divided into 20 equal parts in the thickness direction, and cross-sectional images R1, R2, ... Rn ... R20 (n is an integer from 1 to 20) are taken from the substrate side to the separation functional layer side, respectively. the maximum average pore diameter of the porous layer is present in any one of the cross-sectional images R3 to R18, The average pore size of the porous layer in the cross-sectional image R1 and the cross-sectional image R2 is 0.1 μm or more and less than 0.6 μm.

2. 2. The composite semipermeable membrane according to claim 1, wherein, when the average pore diameter of the porous layer in the cross-sectional image R1 is X and the maximum average pore diameter of the porous layer in the cross-sectional images R1 to R20 is Y, Y / X is 1.1 or more and 10 or less.

3. The composite semipermeable membrane according to claim 1 , wherein the average pore size of the porous layer in the cross-sectional image R1 , the cross-sectional image R2 , and the cross-sectional image R3 is 0.1 μm or more and less than 0.6 μm.

4. The composite semipermeable membrane according to claim 1 , wherein the average pore size of the porous layer in each of the cross-sectional images R1, R2, R3, and R4 is 0.1 μm or more and less than 0.6 μm.

5. The composite semipermeable membrane according to claim 1 , wherein the average pore size of the porous layer in each of the cross-sectional images R1, R2, R3, R4, and R5 is 0.1 μm or more and less than 0.6 μm.

6. The composite semipermeable membrane according to claim 1, wherein the maximum average pore size of the porous layer in the cross-sectional images R1 to R20 is 0.5 μm or more and 2.0 μm or less.

7. 2. The composite semipermeable membrane according to claim 1, wherein a 0.05% by mass aqueous solution of methyl violet is contacted with only the substrate side of the composite semipermeable membrane for 5 minutes, and the substrate is peeled off from the porous layer. The composite semipermeable membrane according to claim 1, wherein the area ratio of the dyed peeled off surface of the porous layer after the substrate is peeled off from the porous layer is 15% or more and 50% or less of the entire peeled off surface area.

8. 2. The composite semipermeable membrane according to claim 1, wherein the porous layer has a thickness of 20 μm or more and 70 μm or less.

9. A fresh water production method comprising a separation step of separating an aqueous solution having a temperature of 35° C. or higher and a TDS (Total Dissolved Solids) of 40,000 mg / L or higher into a concentrated water and a permeated water by using the composite semipermeable membrane according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Reverse osmosis composite membrane

    JP2001252537A

  • Reverse osmosis composite membrane

    JP2001252538A

  • Method of manufacturing composite semipermeable membrane element and composite semipermeable membrane element

    JP2014014739A

  • Composite semipermeable membrane and production method of the same

    JP2018039003A