On-press development type lithographic printing plate precursor, method of preparing lithographic printing plate, lithographic printing method, and compound

The use of specific compounds in the image recording layer of lithographic printing plate precursors addresses the challenge of achieving excellent color development and reduced streak-like unevenness during on-press development, enhancing the performance of lithographic printing plates.

JP2024143724APending Publication Date: 2024-10-11FUJIFILM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023056537
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional lithographic printing plate precursors face challenges in achieving excellent color development with suppressed streak-like unevenness during on-press development, and there is a need for compounds that enhance the performance of on-press development type lithographic printing plates.

Method used

The use of specific compounds, including infrared absorbers, polymerization initiators, and polymerizable compounds represented by certain chemical formulas, in the image recording layer of the lithographic printing plate precursor, which promotes improved color development and reduces streak-like unevenness.

Benefits of technology

The described composition results in lithographic printing plates with enhanced color development and suppressed streak-like unevenness, facilitating effective on-press development without the need for conventional wet processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143724000122
    Figure 2024143724000122
  • Figure 2024143724000123
    Figure 2024143724000123
  • Figure 2024143724000124
    Figure 2024143724000124
Patent Text Reader

Abstract

To provide, e.g., an on-press development type lithographic printing plate precursor with which a lithographic printing plate having excellent color formability and reduced streak-like unevenness can be obtained.SOLUTION: An on-press development type lithographic printing plate precursor includes a support, and an image-recording layer on the support. The image-recording layer contains an infrared absorber, a polymerization initiator, a polymerizable compound, and one or more compounds selected from the group consisting of compounds represented by formulas (1) and (2).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an on-press development type lithographic printing plate precursor, a method for making a lithographic printing plate, a lithographic printing method, and a compound. [Background technology]

[0002] Generally, a lithographic printing plate consists of an oleophilic image area that accepts ink during the printing process, and a hydrophilic non-image area that accepts dampening water. Lithographic printing utilizes the mutual repulsion properties of water and oil-based ink, making the oleophilic image area of ​​the lithographic printing plate the ink-receptive area and the hydrophilic non-image area the dampening water-receptive area (ink-non-receptive area) to create a difference in ink adhesion on the surface of the lithographic printing plate, and after ink is applied only to the image area, the ink is transferred to the printing material such as paper to print. To prepare such a lithographic printing plate, a lithographic printing plate precursor (PS plate) having an oleophilic photosensitive resin layer (image recording layer) on a hydrophilic support has been widely used. Usually, the lithographic printing plate precursor is exposed to light through an original such as a lithographic film, and then the image areas of the image recording layer are left, while the other unnecessary image recording layer is dissolved and removed with an alkaline developer or organic solvent, exposing the hydrophilic support surface to form non-image areas, thereby obtaining a lithographic printing plate.

[0003] Furthermore, due to growing concern about the global environment, environmental issues related to waste liquids accompanying wet processing such as development processing have come into focus. In response to the above environmental issues, efforts are being made to simplify development or plate making, or to eliminate any processing. One of the simple manufacturing methods is a method called "on-press development." In other words, after exposing a lithographic printing plate precursor to light, it is mounted on a printing press as is, without undergoing conventional development, and unnecessary parts of the image recording layer are removed at an early stage of the normal printing process. In the present disclosure, a lithographic printing plate precursor that can be used for such on-press development is referred to as an "on-press development type lithographic printing plate precursor."

[0004] Conventional lithographic printing plate precursors include those described in Patent Documents 1 and 2, for example. Patent Document 1 discloses an on-press development type lithographic printing plate precursor that contains a leuco dye in the image recording layer from the viewpoints of color development and visibility of exposed areas. Patent Document 2 describes a lithographic printing plate precursor containing a leuco dye having a specific structure as a color-forming compound in an image recording layer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2022 / 019217 [Patent Document 2] US Patent Application Publication No. 2021 / 0078350 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of one embodiment of the present disclosure is to provide an on-press development type lithographic printing plate precursor that can provide a lithographic printing plate having excellent color development and suppressed streak-like unevenness. Another problem to be solved by another embodiment of the present disclosure is to provide a method for producing a lithographic printing plate using the on-press development type lithographic printing plate precursor, or a lithographic printing method. A problem to be solved by still another embodiment of the present disclosure is to provide a novel compound useful as a color former precursor. [Means for solving the problem]

[0007] Means for solving the above problems include the following aspects.

[0008] <1> A support and an image recording layer on the support, The image recording layer comprises an infrared absorbing agent, a polymerization initiator, a polymerizable compound, and one or more compounds selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2).

[0009] [ka]

[0010] In formula (1) and formula (2), Ra1 and Ra2 each independently represent a hydrogen atom or a substituted or unsubstituted alkyl group, and Ra1 and Ra2 may be linked to form a ring structure, Rb1 and Rb3 each independently represent a substituted or unsubstituted alkyl group, Rb2 and Rb4 each independently represent a hydrogen atom or a substituted or unsubstituted alkyl group, and EDG each independently represent a hydrogen atom or an electron donating group, provided that at least one of the four EDGs in formula (1) represents an electron donating group.

[0011] <2> The compound represented by the above formula (1) is a compound represented by the following formula (1a): <1> 2. An on-press development type lithographic printing plate precursor according to claim 1.

[0012] [ka]

[0013] In formula (1a), Ra1 and Ra2 each independently represent a hydrogen atom or a substituted or unsubstituted alkyl group, and Ra1 and Ra2 may be linked to form a ring structure, Rb1 represents a substituted or unsubstituted alkyl group, Rb2 represents a hydrogen atom or a substituted or unsubstituted alkyl group, and EDG each independently represents a hydrogen atom or an electron-donating group, provided that at least one of the two EDGs in formula (1a) represents an electron-donating group.

[0014] <3> The electron donating group in the above formula (1) and the above formula (2) is a methoxy group. <1> or <2> 2. An on-press development type lithographic printing plate precursor according to claim 1.

[0015] <4> The compound represented by the above formula (1) is a compound represented by the following formula (1b): <1> ~ <3> 10. The on-press development type lithographic printing plate precursor according to claim 9,

[0016] [ka]

[0017] In formula (1b), Rb1 represents a substituted or unsubstituted alkyl group.

[0018] <5> The compound represented by the above formula (2) is a compound represented by the following formula (2a): <1> ~ <4> 10. The on-press development type lithographic printing plate precursor according to claim 9,

[0019] [ka]

[0020] In formula (2a), Rb1 and Rb3 each independently represent a substituted or unsubstituted alkyl group having 2 or more carbon atoms.

[0021] <6> The polymerization initiator comprises a compound A represented by the following formula (Ia) and one or more compounds B selected from the group consisting of compounds represented by the following formula (Ib) or the following formula (Ic): <1> ~ <5> 10. The on-press development type lithographic printing plate precursor according to claim 9,

[0022] [ka]

[0023] In formulas (Ia) to (Ic), R1, R2, R3, R4, R5, and R6 are each independently a substituted or unsubstituted alkyl group or a substituted or unsubstituted alkoxy group having 2 to 9 carbon atoms, at least one of R3 and R4 is different from R1 or R2, the difference between the total number of carbon atoms in R1 and R2 and the total number of carbon atoms in R3 and R4 is 0 to 4, the difference between the total number of carbon atoms in R1 and R2 and the total number of carbon atoms in R5 and R6 is 0 to 4, and X1, X2, and X3 are each independently a counter anion.

[0024] <7> The infrared absorber contains a compound represented by the following formula (X): <1> ~ <6> 10. The on-press development type lithographic printing plate precursor according to claim 9,

[0025] [ka]

[0026] In formula (X), Ar 11 and Ar 12 each independently represents an atomic group necessary to form a substituted or unsubstituted aromatic ring or a substituted or unsubstituted heteroaromatic ring; R 11 and R 12 are each independently a substituted or unsubstituted alkyl group; R 13 represents a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted heteroaryl group; R 14 represents a hydrogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted heteroaryl group; Y each independently represents an oxygen atom, a sulfur atom, or >C(R 15 R 16 ), R 15 and R 16each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms, A1 and A2 each independently represent a substituted or unsubstituted alkyl group or an atomic group containing 2 or 3 carbon atoms necessary to form a substituted or unsubstituted 5- or 6-membered non-aromatic carbon ring by bonding with each other, and Za represents a counter ion that neutralizes the charge.

[0027] <8> The image recording layer further contains one or more compounds selected from the group consisting of compounds represented by the following formula (Le-10) and compounds represented by the following formula (Z-4): <1> ~ <7> 10. The on-press development type lithographic printing plate precursor according to claim 9,

[0028] [ka]

[0029] In formula (Le-10), each Ar1 independently represents an aryl group or a heteroaryl group, and each Ar2 independently represents an aryl group having a substituent at at least one ortho position, or a heteroaryl group having a substituent at at least one ortho position.

[0030] [ka]

[0031] In formula (Z-4), Rza1 represents a hydrogen atom, an alkyl group, or an alkoxy group; Rzb1 to Rb4 each independently represent a hydrogen atom, an alkyl group, or an aryl group; Rzb1 and Rzb2, and Rzb3 and Rzb4 may be linked to form a ring structure; X represents O or NR; R represents a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group; and Y1 and Y2 each independently represent CH or N.

[0032] <9> The image recording layer further contains a compound represented by the following formula (Ph): <1> ~ <8> 10. The on-press development type lithographic printing plate precursor according to claim 9,

[0033] [ka]

[0034] In formula (Ph), X P represents O, S or NH; Y P represents N or CH; R P1 represents a hydrogen atom or an alkyl group, R P2 and R P3 each independently represents a halogen atom, an alkylthio group, an arylthio group, an alkoxy group, an aryloxy group, an alkyl group, an aryl group, an acylthio group, or an acyl group; mp and np each independently represent an integer of 0 to 4.

[0035] <10> The image recording layer further contains a polymer having a structural unit represented by the following formula (I): <1> ~ <9> 10. The on-press development type lithographic printing plate precursor according to claim 9,

[0036] [ka]

[0037] In formula (I), R 11 and R 12 each independently represents a hydrogen atom or an alkyl group; R 13 represents a hydrogen atom or a monovalent substituent; L 11 and L 12 each independently represents a single bond or a divalent linking group, and Rh represents a substituent containing two or more silicon atoms.

[0038] <11> The polymerizable compound includes a polymerizable compound having 7 or more functional groups. <1> ~ <10> 10. The on-press development type lithographic printing plate precursor according to claim 9, <12> The image recording layer further contains an oil agent. <1> ~ <11> 10. The on-press development type lithographic printing plate precursor according to claim 9,

[0039] <13> the support has an aluminum plate and an anodized aluminum coating disposed on the aluminum plate, the anodized film is located on the image recording layer side of the aluminum plate, the anodized coating has micropores extending in a depth direction from a surface on the image-recording layer side, The average diameter of the micropores on the surface of the anodized film is more than 10 nm and not more than 100 nm. <1> ~ <12> 10. The on-press development type lithographic printing plate precursor according to claim 9, <14> the micropores are composed of large-diameter pores extending from the surface of the anodized coating to a depth of 10 nm to 1,000 nm, and small-diameter pores communicating with the bottoms of the large-diameter pores and extending from the communicating position to a depth of 20 nm to 2,000 nm, the large diameter pores have an average diameter of 15 nm to 100 nm on the surface of the anodized film; The small diameter pores have an average diameter of 13 nm or less at the communicating position. <13> 2. An on-press development type lithographic printing plate precursor according to claim 1.

[0040] <15> <1> ~ <12> imagewise exposing the on-press development type lithographic printing plate precursor according to any one of the above items; and a step of removing the image recording layer in the non-image area by supplying at least one selected from the group consisting of printing ink and dampening water on the printing press. How to make a lithographic printing plate. <16> <1> ~ <12> imagewise exposing the on-press development type lithographic printing plate precursor according to any one of the above items; a step of removing the image recording layer in the non-image area by supplying at least one selected from the group consisting of a printing ink and a dampening water on a printing press to prepare a lithographic printing plate; and printing with the resulting lithographic printing plate. Lithographic printing method.

[0041] <17> A compound represented by the following formula (1b):

[0042] [ka]

[0043] In formula (1b), Rb1 represents a substituted or unsubstituted alkyl group.

[0044] <18> A compound represented by the following formula (2a):

[0045] [ka]

[0046] In formula (2a), Rb1 and Rb3 each independently represent a substituted or unsubstituted alkyl group having 2 or more carbon atoms. Effect of the Invention

[0047] According to one embodiment of the present disclosure, it is possible to provide an on-press development type lithographic printing plate precursor that can yield a lithographic printing plate having excellent color development and suppressed streak-like unevenness. According to another embodiment of the present disclosure, it is possible to provide a method for producing a lithographic printing plate or a method for printing with a lithographic printing plate using the on-press development type lithographic printing plate precursor. Furthermore, according to still another embodiment of the present disclosure, a novel compound useful as a color former precursor can be provided. [Brief description of the drawings]

[0048] [Figure 1] FIG. 2 is a schematic cross-sectional view of one embodiment of a support. [Diagram 2] FIG. 2 is a schematic cross-sectional view of another embodiment of a support. [Diagram 3] FIG. 2 is a schematic view of an anodizing apparatus used in an anodizing treatment in the method for producing a support having an anodized coating. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0049] The contents of the present disclosure will be described in detail below. The following description of the components may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment. In this specification, the use of "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower limit and upper limit. In addition, in the description of groups (atomic groups) in this specification, descriptions that do not indicate whether they are substituted or unsubstituted include those that have no substituents as well as those that have a substituent. For example, an "alkyl group" includes not only an alkyl group that has no substituents (unsubstituted alkyl groups) but also an alkyl group that has a substituent (substituted alkyl groups). In this specification, "(meth)acrylic" is a term used as a concept including both acrylic and methacrylic, and "(meth)acryloyl" is a term used as a concept including both acryloyl and methacryloyl. In addition, the term "step" in this specification includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. In addition, in this disclosure, "mass %" and "weight %" are synonymous, and "parts by mass" and "parts by weight" are synonymous. Unless otherwise specified, each component in a composition or each structural unit in a polymer in the present disclosure may be contained alone or in combination of two or more types. Furthermore, in the present disclosure, the amount of each component in a composition or each structural unit in a polymer means, when a plurality of substances or structural units corresponding to each component or each structural unit in a polymer are present in the composition, the total amount of the corresponding plurality of substances present in the composition or the corresponding plurality of structural units present in the polymer, unless otherwise specified. Furthermore, in the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments. In addition, unless otherwise specified, the weight average molecular weight (Mw) and number average molecular weight (Mn) in the present disclosure are molecular weights detected by a gel permeation chromatography (GPC) analyzer using columns of TSKgel GMHxL, TSKgel G4000HxL, or TSKgel G2000HxL (all product names manufactured by Tosoh Corporation) in a solvent of THF (tetrahydrofuran) and a differential refractometer, and converted using polystyrene as a standard substance. In this disclosure, the term "lithographic printing plate precursor" includes not only lithographic printing plate precursors but also throwaway plate precursors. Furthermore, the term "lithographic printing plate" includes not only lithographic printing plates prepared by subjecting a lithographic printing plate precursor to operations such as exposure and development as necessary, but also throwaway plates. In the case of a throwaway plate precursor, the operations of exposure and development are not necessarily required. Note that a throwaway plate is a lithographic printing plate precursor that is attached to an unused plate cylinder when, for example, a portion of the page is printed in one color or two colors in color newspaper printing. In addition, in the present disclosure, "*" in a chemical structural formula indicates a bonding position with other structures. The present disclosure will be described in detail below.

[0050] (On-press development type lithographic printing plate original plate) The on-press development type lithographic printing plate precursor (also simply referred to as "lithographic printing plate precursor") according to the present disclosure has a support and an image recording layer on the support, and the image recording layer contains one or more compounds selected from the group consisting of an infrared absorber, a polymerization initiator, a polymerizable compound, and a compound represented by formula (1) and a compound represented by formula (2). Hereinafter, the "compound represented by formula (1) and the compound represented by formula (2)" are collectively referred to as the "specific compound". The on-press development type lithographic printing plate precursor according to the present disclosure is a negative-working lithographic printing plate precursor in which exposed areas are polymerized by infrared exposure.

[0051] The present inventors have found that it is difficult to obtain a lithographic printing plate having excellent color development properties and suppressed streak-like unevenness using conventional lithographic printing plate precursors such as those described in Patent Documents 1 and 2. Therefore, the present inventors conducted extensive research and found that, by having an image recording layer with the above-mentioned composition, a lithographic printing plate having excellent color development and suppressed streak-like unevenness can be obtained. Although the detailed mechanism by which the above effects are obtained is unclear, it is speculated as follows. In recent years, in the exposure of a lithographic printing plate precursor, an exposure machine equipped with an exposure head that employs GLV (Grating Light Value) technology has come to be used. When exposed with this type of exposure device, the halftone dot image thickens in the scanning direction, resulting in streaky unevenness that is sometimes called swath unevenness. The compound represented by formula (1) and the compound represented by formula (2) (specific compound) are substitution-type compounds with high electron donating properties, and the difference in the amount of ring-opening isomers generated before and after exposure is large. In addition, the inventors have found that the specific compound has radical termination ability in the closed ring form and does not have radical termination ability in the open ring form, which can further promote the difference in the amount of radicals generated before and after exposure. As a result, it is presumed that the cut-off property of the exposure sensitivity is improved, resulting in a lithographic printing plate with suppressed streak-like unevenness. In addition, it is presumed that the specific compound has excellent color development properties after ring-opening by exposure due to the type of substituent in the ring structure, the number of substituents in the ring structure, and the position at which the substituent is introduced into the ring structure. For these reasons, the on-press development type lithographic printing plate precursor according to the present disclosure can provide a lithographic printing plate that is excellent in color development and in which streak-like unevenness is suppressed.

[0052] Hereinafter, each constituent element of the planographic printing plate precursor according to the present disclosure will be described in detail.

[0053] <Image recording layer> The image recording layer in the lithographic printing plate precursor according to the present disclosure contains an infrared absorbing agent, a polymerization initiator, a polymerizable compound, and one or more compounds selected from the group consisting of a compound represented by formula (1) and a compound represented by formula (2). The image recording layer in the lithographic printing plate precursor according to the present disclosure is preferably a water-soluble or water-dispersible negative-type image recording layer. From the viewpoint of on-press developability, the image recording layer in the lithographic printing plate precursor according to the present disclosure is preferably such that the unexposed areas of the image recording layer are removable with at least one of fountain solution and printing ink.

[0054] Each component contained in the image recording layer will be described in detail below.

[0055] [Compound represented by formula (1) and compound represented by formula (2) (specific compound)] The image recording layer contains one or more compounds selected from the group consisting of compounds represented by the following formula (1) and compounds represented by the following formula (2). These specific compounds are compounds that develop color by ring opening (that is, color formers), and therefore correspond to color former precursors.

[0056] [ka]

[0057] In formula (1) and formula (2), Ra1 and Ra2 each independently represent a hydrogen atom or a substituted or unsubstituted alkyl group, and Ra1 and Ra2 may be linked to form a ring structure, Rb1 and Rb3 each independently represent a substituted or unsubstituted alkyl group, Rb2 and Rb4 each independently represent a hydrogen atom or a substituted or unsubstituted alkyl group, and EDG each independently represent a hydrogen atom or an electron donating group, provided that at least one of the four EDGs in formula (1) represents an electron donating group.

[0058] Here, examples of the substituent in the substituted alkyl group include an aryl group, a heteroaryl group, a halogen atom, an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, a hydroxy group, an alkoxy group, an aryloxy group, a heteroaryloxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, a heteroaryloxycarbonyl group, a cyano group, etc. Furthermore, these substituents may be further substituted with these substituents, alkyl groups, etc.

[0059] The above Ra1 and Ra2 are each independently preferably a substituted or unsubstituted alkyl group, more preferably an unsubstituted alkyl group having 1 to 8 carbon atoms, and further preferably an unsubstituted alkyl group having 1 to 2 carbon atoms. In addition, Ra1 and Ra2 are preferably the same group. Furthermore, Ra1 and Ra2 may be linked to form a ring structure. That is, Ra1 and Ra2 are linked to form a ring structure containing N. The ring structure formed is preferably a 5-membered ring or a 6-membered ring, more preferably a 6-membered ring.

[0060] The above Rb1 and Rb3 are each independently preferably a substituted or unsubstituted alkyl group having 1 to 8 carbon atoms, and more preferably a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms. When Rb1 and Rb3 are substituted alkyl groups, the substituent is preferably an aryl group or an alkoxy group, and among these, an aryl group is more preferable.

[0061] The above Rb2 and Rb4 are each independently preferably a hydrogen atom or an unsubstituted alkyl group having 1 to 8 carbon atoms, and more preferably a hydrogen atom or an unsubstituted alkyl group having 1 to 4 carbon atoms. The above Rb2 is particularly preferably a hydrogen atom or an unsubstituted alkyl group having 1 to 2 carbon atoms. The above Rb4 is particularly preferably a hydrogen atom or an unsubstituted alkyl group having 1 to 2 carbon atoms.

[0062] Examples of the electron-donating group represented by EDG include an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, an alkoxy group, an aryloxy group, a heteroaryloxy group, or an alkyl group. Among these, the electron-donating group represented by EDG is preferably an alkoxy group or an alkyl group, more preferably an alkoxy group, and even more preferably a methoxy group, from the viewpoint of color development.

[0063] At least one of the four EDGs in formula (1) is an electron-donating group, and it is preferable that one or two of the four EDGs are electron-donating groups, and it is more preferable that one of the four EDGs is an electron-donating group. In formula (2), it is preferable that 0 to 2 of the four EDGs are electron-donating groups, and it is more preferable that 0 or 2 of the four EDGs are electron-donating groups.

[0064] From the viewpoint of color development properties, the compound represented by the above formula (1) is preferably a compound represented by the following formula (1a).

[0065] [ka]

[0066] In formula (1a), Ra1 and Ra2 each independently represent a hydrogen atom or a substituted or unsubstituted alkyl group, and Ra1 and Ra2 may be linked to form a ring structure, Rb1 represents a substituted or unsubstituted alkyl group, Rb2 represents a hydrogen atom or a substituted or unsubstituted alkyl group, and EDG each independently represents a hydrogen atom or an electron-donating group, provided that at least one of the two EDGs in formula (1a) represents an electron-donating group. In addition, Ra1, Ra2, Rb1, Rb2, and EDG in formula (1a) have the same meanings as Ra1, Ra2, Rb1, Rb2, and EDG in formula (1) above, and preferred embodiments are also the same.

[0067] From the viewpoint of color development properties, the compound represented by the above formula (1) is more preferably a compound represented by the following formula (1b).

[0068] [ka]

[0069] In formula (1b), Rb1 represents a substituted or unsubstituted alkyl group. In addition, Rb1 in the formula (1b) has the same meaning as Rb1 in the above formula (1), and the preferred embodiments are also the same.

[0070] From the viewpoint of color development, the compound represented by the above formula (2) is preferably a compound represented by the following formula (2a).

[0071] [ka]

[0072] In formula (2a), Rb1 and Rb3 each independently represent a substituted or unsubstituted alkyl group having 2 or more carbon atoms. In addition, Rb1 and Rb3 in the formula (2a) have the same structure as Rb1 and Rb3 in the above formula (1), except that they have 2 or more carbon atoms. 31 The same applies to the preferred embodiments.

[0073] Specific examples of the specific compound are shown below, but the specific compound is not limited to these.

[0074] [ka]

[0075] [ka]

[0076] The compounds represented by formula (1) and formula (2) can be obtained, for example, by adding two equivalents of an indole compound to the corresponding o-alkoxycarbonylbenzaldehyde to synthesize a triarylmethane compound, followed by ester hydrolysis and oxidation.

[0077] The specific compound may be used alone or in combination of two or more. When two or more specific compounds are used in combination, for example, a compound represented by formula (1) and a compound represented by formula (2) may be used in combination. The total content of the specific compounds in the image recording layer is preferably from 0.5% by mass to 10% by mass, and more preferably from 1% by mass to 5% by mass, based on the total mass of the image recording layer. From the viewpoint of suppressing deterioration of the surface condition, the total content of the specific compounds is preferably 10% by mass, more preferably 5% by mass or less, based on the total mass of the image recording layer, and from the viewpoint of color development, the total content of the specific compounds is preferably 0.5% by mass or more, more preferably 1% by mass or more, based on the total mass of the image recording layer.

[0078] [Infrared absorbing agent] The image recording layer contains an infrared absorbing agent. The infrared absorbing agent is not particularly limited, and examples thereof include pigments and dyes. As the dye to be used as the infrared absorber, commercially available dyes and known dyes described in literature such as "Dye Handbook" (edited by the Organic Synthesis Chemistry Association, published in 1970) can be used. Specific examples of the dye include azo dyes, metal complex azo dyes, pyrazolone azo dyes, naphthoquinone dyes, anthraquinone dyes, phthalocyanine dyes, carbonium dyes, quinoneimine dyes, methine dyes, cyanine dyes, squarylium dyes, pyrylium salts, and metal thiolate complex dyes.

[0079] Particularly preferred among these dyes are cyanine dyes, squarylium dyes, pyrylium salts, nickel thiolate complexes, and indolenine cyanine dyes.Furthermore, cyanine dyes and indolenine cyanine dyes are also included.Of these, cyanine dyes are particularly preferred.

[0080] The infrared absorbing agent is preferably a cationic polymethine dye having an oxygen or nitrogen atom at the meso position. Preferred examples of the cationic polymethine dye include cyanine dyes, pyrylium dyes, thiopyrylium dyes, and azulenium dyes, and from the viewpoints of availability, solubility in a solvent during the introduction reaction, and the like, cyanine dyes are preferred.

[0081] Specific examples of cyanine dyes include the compounds described in paragraphs 0017 to 0019 of JP-A-2001-133969, the compounds described in paragraphs 0016 to 0021 of JP-A-2002-023360, and the compounds described in paragraphs 0012 to 0037 of JP-A-2002-040638, preferably the compounds described in paragraphs 0034 to 0041 of JP-A-2002-278057, and the compounds described in paragraphs 0080 to 0086 of JP-A-2008-195018, and particularly preferably the compounds described in paragraphs 0035 to 0043 of JP-A-2007-90850, and the compounds described in paragraphs 0105 to 0113 of JP-A-2012-206495. In addition, the compounds described in paragraphs 0008 to 0009 of JP-A No. 5-5005 and paragraphs 0022 to 0025 of JP-A No. 2001-222101 can also be preferably used. As the pigment, the compounds described in paragraphs 0072 to 0076 of JP-A No. 2008-195018 are preferred.

[0082] The infrared absorbing agent preferably contains an infrared absorbing agent that decomposes upon exposure to infrared rays (decomposable infrared absorbing agent), and more preferably contains a decomposable color-forming infrared absorbing agent. It is presumed that by using a decomposable infrared absorber as the infrared absorber, the infrared absorber or its decomposition products promote polymerization, and further, the decomposition products of the infrared absorber interact with the polymerizable compound, resulting in excellent UV printing resistance. The decomposable infrared absorbent is preferably an infrared absorbent that has the function of absorbing infrared rays, decomposing, and developing color when exposed to infrared rays. Hereinafter, the colored compound formed by the decomposable infrared absorber absorbing infrared light and decomposing when exposed to infrared light is also referred to as a "colored body of the decomposable infrared absorber." The decomposable infrared absorbent preferably has a function of absorbing infrared rays upon exposure to infrared rays and converting the absorbed infrared rays into heat. The decomposable infrared absorbent may be one that absorbs and decomposes at least a portion of light in the infrared wavelength region (wavelength 750 nm to 1 mm), but is preferably an infrared absorbent having a maximum absorption wavelength in the wavelength region of 750 nm to 1,400 nm, and more preferably an infrared absorbent having a maximum absorption wavelength in the wavelength region of 760 nm to 900 nm. More specifically, the decomposable infrared absorbent is preferably a compound that decomposes due to exposure to infrared light to generate a compound having a maximum absorption wavelength in the wavelength range of 500 nm to 600 nm.

[0083] The decomposable infrared absorber is preferably an infrared absorber that decomposes due to heat, electron transfer, or both caused by infrared exposure, and more preferably an infrared absorber that decomposes due to electron transfer caused by infrared exposure. Here, "decomposes due to electron transfer" means that electrons excited from the HOMO (highest occupied molecular orbital) of the decomposable infrared absorber to the LUMO (lowest unoccupied molecular orbital) by infrared exposure transfer intramolecularly to an electron accepting group (a group having an electric potential close to that of the LUMO) in the molecule, resulting in decomposition.

[0084] The infrared absorbing agent preferably contains a compound represented by the following formula 1.

[0085] [ka]

[0086] In formula 1, R1 and R2 each independently represent a hydrogen atom or an alkyl group, R1 and R2 may be bonded to each other to form a ring, R3 to R6 each independently represent a hydrogen atom or an alkyl group, R7 and R8 each independently represent an alkyl group or an aryl group, Y1 and Y2 each independently represent an oxygen atom, a sulfur atom, -NR0- or a dialkylmethylene group, R0 represents a hydrogen atom, an alkyl group or an aryl group, Ar1 and Ar2 each independently represent a group forming a benzene ring or a naphthalene ring which may have a group represented by formula 2 described later, and A1 is -NR9R 10 , -X1-L1 or a group represented by formula 2 described below; R9 and R 10 each independently represents an alkyl group, an aryl group, an alkoxycarbonyl group, or an arylsulfonyl group; X1 represents an oxygen atom or a sulfur atom; L1 represents a hydrocarbon group, a heteroaryl group, or a group whose bond to X1 is cleaved by heat or exposure to infrared light; Za represents a counter ion that neutralizes the charge; and at least one of Ar1 and Ar2 has a group represented by the following formula 2: -X expression 2 In formula 2, X is a halogen atom, -C(=O)-X2-R 11 , -C(=O)-NR 12R 13 , -OC(=O)-R 14 , -CN, -SO2NR 15 R 16 or a perfluoroalkyl group, X2 represents a single bond or an oxygen atom, R 11 and R 14 each independently represents an alkyl group or an aryl group; R 12 , R 13 , R 15 and R 16 each independently represents a hydrogen atom, an alkyl group, or an aryl group.

[0087] Ar1 and Ar2 each independently represent a group forming a benzene ring or a naphthalene ring. The benzene ring and the naphthalene ring may have a substituent other than -X. Examples of the substituent include an alkyl group, an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a carboxy group, a carboxylate group, a sulfo group, a sulfonate group, and a combination of these groups, and the alkyl group is preferable. In addition, in formula 1, at least one of Ar1 and Ar2 has a group represented by formula 2 above, and from the viewpoints of printing durability and visibility, it is preferable that both Ar1 and Ar2 have a group represented by formula 2 above.

[0088] In formula 2, X is a halogen atom, -C(=O)-X2-R 11 , -C(=O)-NR 12 R 13 , -OC(=O)-R 14 , -CN, -SO2NR 15 R 16 or a perfluoroalkyl group, and from the viewpoints of printing durability, visibility, and stability over time, a halogen atom, -C(=O)-X2-R 11 , -C(=O)-NR 12 R 13 , -OC(=O)-R 14 , CN, or -SO2NR 15 R 16 is preferably a halogen atom, -C(=O)-OR 11 , -C(=O)-NR12 R 13 , or -OC(=O)-R 14 is preferably a halogen atom, -C(=O)-OR 11 , or -OC(=O)-R 14 More preferably, it is a fluorine atom, a chlorine atom, a bromine atom, or -C(=O)OR 17 is particularly preferred, and a chlorine atom or a bromine atom is most preferred.

[0089] X2 represents a single bond or an oxygen atom, and is preferably an oxygen atom. R 11 and R 14 each independently represents an alkyl group or an aryl group, preferably an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, and more preferably an alkyl group having 1 to 12 carbon atoms. R 12 , R 13 , R 15 and R 16 each independently represents a hydrogen atom, an alkyl group, or an aryl group, and is preferably a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, and even more preferably an alkyl group having 1 to 12 carbon atoms. R 17 represents an alkyl group or an aryl group, preferably an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, and more preferably an alkyl group having 1 to 12 carbon atoms.

[0090] A1 is -NR9R 10 , -X1-L1 or -X, and from the viewpoints of printing durability, visibility and stability over time, -NR9R 10 or -X1-L1, and -NR 18 R 19 , -SR 20 It is more preferable that: In addition, from the viewpoints of UV plate skip suppression, GLV suitability, and UV printing durability, A1 is preferably -X, more preferably a halogen atom, further preferably a chlorine atom or a bromine atom, and particularly preferably a chlorine atom. R9 and R 10 each independently represents an alkyl group, an aryl group, an alkoxycarbonyl group, or an arylsulfonyl group, preferably an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, and more preferably an alkyl group having 1 to 12 carbon atoms. X1 represents an oxygen atom or a sulfur atom. When L1 is a hydrocarbon group or a heteroaryl group, it is preferably a sulfur atom, and L1 is preferably a group whose bond to X1 is cleaved by exposure to heat or infrared light. L1 represents a hydrocarbon group, a heteroaryl group, or a group whose bond to X1 is cleaved by heat or infrared exposure. From the viewpoint of printing durability, a hydrocarbon group or a heteroaryl group is preferable, an aryl group or a heteroaryl group is more preferable, and a heteroaryl group is even more preferable. From the viewpoints of visibility and prevention of fading over time, L1 is preferably a group in which the bond to X1 is cleaved by exposure to heat or infrared rays. The group whose bond to X1 is cleaved by heat or exposure to infrared rays will be described later. R 18 and R 19 each independently represents an aryl group, preferably an aryl group having 6 to 20 carbon atoms, and more preferably a phenyl group. R 20 represents a hydrocarbon group or a heteroaryl group, preferably an aryl group or a heteroaryl group, and more preferably a heteroaryl group.

[0091] L1 and R 20 Preferred examples of the heteroaryl group in the above formula include the following groups.

[0092] [ka]

[0093] R1~R 10 and the alkyl group in R0 is preferably an alkyl group having 1 to 30 carbon atoms, more preferably an alkyl group having 1 to 15 carbon atoms, and further preferably an alkyl group having 1 to 10 carbon atoms. The alkyl group may be linear, branched, or have a ring structure. Specific examples include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a undecyl group, a dodecyl group, a tridecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, an isopropyl group, an isobutyl group, a s-butyl group, a t-butyl group, an isopentyl group, a neopentyl group, a 1-methylbutyl group, an isohexyl group, a 2-ethylhexyl group, a 2-methylhexyl group, a cyclohexyl group, a cyclopentyl group, and a 2-norbornyl group. Among these alkyl groups, a methyl group, an ethyl group, a propyl group, or a butyl group is particularly preferred.

[0094] The alkyl group may have a substituent, for example, an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a halogen atom, a carboxy group, a carboxylate group, a sulfo group, a sulfonate group, an alkyloxycarbonyl group, an aryloxycarbonyl group, or a combination thereof.

[0095] R9, R 10 , R 18 , R 19 And the aryl group in R0 is preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and even more preferably an aryl group having 6 to 12 carbon atoms. The aryl group may have a substituent, for example, an alkyl group, an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a halogen atom, a carboxy group, a carboxylate group, a sulfo group, a sulfonate group, an alkyloxycarbonyl group, an aryloxycarbonyl group, or a combination thereof. Specific examples of the aryl group include a phenyl group, a naphthyl group, a p-tolyl group, a p-chlorophenyl group, a p-fluorophenyl group, a p-methoxyphenyl group, a p-dimethylaminophenyl group, a p-methylthiophenyl group, and a p-phenylthiophenyl group. Of these aryl groups, a phenyl group, a p-methoxyphenyl group, a p-dimethylaminophenyl group, or a naphthyl group is preferred.

[0096] It is preferred that R1 and R2 are linked to form a ring. When R1 and R2 are linked to form a ring, the number of ring members is preferably 5 or 6, more preferably 6. The ring formed by linking R1 and R2 is preferably a hydrocarbon ring which may have an ethylenically unsaturated bond.

[0097] Y1 and Y2 each independently represent an oxygen atom, a sulfur atom, -NR0-, or a dialkylmethylene group, preferably -NR0- or a dialkylmethylene group, and more preferably a dialkylmethylene group. R0 represents a hydrogen atom, an alkyl group or an aryl group, and is preferably an alkyl group.

[0098] It is preferred that R7 and R8 are the same group. Furthermore, R7 and R8 are each preferably independently a straight-chain alkyl group or an alkyl group having a terminal sulfonate group, and more preferably a methyl group, an ethyl group, or a butyl group having a terminal sulfonate group. The counter cation of the sulfonate group may be the cation on the nitrogen atom in formula 1, or may be an alkali metal cation or an alkaline earth metal cation. Furthermore, from the viewpoint of making the compound represented by formula 1 water-soluble, R7 and R8 are each independently preferably an alkyl group having an anionic structure, more preferably an alkyl group having a carboxylate group or a sulfonate group, and even more preferably an alkyl group having a sulfonate group at the terminal. In addition, in order to lengthen the maximum absorption wavelength of the compound represented by Formula 1 and from the viewpoints of visibility and printing durability of a lithographic printing plate, R7 and R8 are each preferably independently an alkyl group having an aromatic ring, more preferably an alkyl group having an aromatic ring at a terminal, and particularly preferably a 2-phenylethyl group, a 2-naphthalenylethyl group, or a 2-(9-anthracenyl)ethyl group.

[0099] R3 to R6 each independently represent a hydrogen atom or an alkyl group, and are preferably a hydrogen atom.

[0100] In addition, from the viewpoints of stability over time, UV plate skip suppression, GLV suitability and UV printing durability, the compound represented by formula 1 preferably has one or more halogen atoms, more preferably at least one selected from the group consisting of A1, Ar1 and Ar2 has one or more halogen atoms, and particularly preferably A1, Ar1 and Ar2 each have one or more halogen atoms. Furthermore, from the viewpoints of stability over time, UV plate skipping suppression, GLV suitability and UV printing durability, the compound represented by formula 1 more preferably has two or more halogen atoms, even more preferably has three or more halogen atoms, and particularly preferably has three or more and six or less halogen atoms. The halogen atom is preferably a chlorine atom or a bromine atom. Furthermore, in the compound represented by formula 1, from the viewpoints of stability over time, UV plate skipping suppression, GLV suitability, and UV printing durability, it is preferable that at least one of Ar1 and Ar2 has a halogen atom, it is more preferable that at least one of Ar1 and Ar2 has a chlorine atom or a bromine atom, and it is particularly preferable that at least one of Ar1 and Ar2 has a bromine atom.

[0101] Za represents a counter ion that neutralizes the charge, and when it represents an anion species, examples thereof include a sulfonate ion, a carboxylate ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a perchlorate ion, a sulfonamide anion, a sulfonimide anion, etc. When it represents a cationic species, an alkali metal ion, an alkaline earth metal ion, an ammonium ion, a pyridinium ion, or a sulfonium ion is preferred, a sodium ion, a potassium ion, an ammonium ion, a pyridinium ion, or a sulfonium ion is more preferred, a sodium ion, a potassium ion, or an ammonium ion is further preferred, and a sodium ion, a potassium ion, or a trialkylammonium ion is particularly preferred. Among these, from the viewpoints of printing durability and visibility, Za is preferably an organic anion containing a carbon atom, more preferably a sulfonate ion, a carboxylate ion, a sulfonamide anion, or a sulfonimide anion, even more preferably a sulfonamide anion or a sulfonimide anion, and particularly preferably a sulfonimide anion. R1 to R8, R0, A1, Ar1, Ar2, Y1 and Y2 may have an anionic structure or a cationic structure. When all of R1 to R8, R0, A1, Ar1, Ar2, Y1 and Y2 are groups having a neutral charge, Za is a monovalent counter anion. However, when, for example, R1 to R8, R0, A1, Ar1, Ar2, Y1 and Y2 have two or more anionic structures, Za can also be a counter cation. In addition, in formula 1, if the moieties other than Za are electrically neutral, Za may be omitted.

[0102] The sulfonamide anion is preferably an arylsulfonamide anion. The sulfonimide anion is preferably a bisarylsulfonimide anion. Specific examples of sulfonamide anions or sulfonimide anions are shown below, but the present disclosure is not limited thereto. In the following specific examples, Ph represents a phenyl group, Me represents a methyl group, and Et represents an ethyl group.

[0103] [ka]

[0104] From the viewpoint of visibility, the group whose bond to X1 is cleaved by exposure to heat or infrared light is preferably a group represented by any one of the following formulas (1-1) to (1-7), and more preferably a group represented by any one of the following formulas (1-1) to (1-3).

[0105] [ka]

[0106] In formulas (1-1) to (1-7), represents a bonding site with X1 in formula 1, and R 10 each independently represents a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, -OR 14 , -NR 15 R 16 or -SR 17 R 11 each independently represents a hydrogen atom, an alkyl group, or an aryl group; R 12 is an aryl group, -OR 14 , -NR 15 R 16 , -SR 17 , -C(=O)R 18 , -OC(=O)R 18 or a halogen atom, R 13 represents an aryl group, an alkenyl group, an alkoxy group, or an onium group; R 14 ~R 17 each independently represents a hydrogen atom, an alkyl group, or an aryl group; R 18 each independently represents an alkyl group, an aryl group, or -OR 14 , -NR 15 R 16 or -SR 17 and Z 1 represents a counter ion that neutralizes the charge.

[0107] R 10 , R 11and R 14 ~R 18 In a preferred embodiment, when R is an alkyl group, 2 ~R 9 and R 0 The preferred embodiments of the alkyl group in the above formula are the same as those in the above formula. R 10 and R 13 The alkenyl group in preferably has 1 to 30 carbon atoms, more preferably 1 to 15 carbon atoms, and further preferably 1 to 10 carbon atoms. R 10 ~R 18 In a preferred embodiment, when R is an aryl group, 0 The preferred embodiments are the same as those of the aryl group in the above.

[0108] From the viewpoint of visibility, R in formula (1-1) 10 is an alkyl group, an alkenyl group, an aryl group, -OR 14 , -NR 15 R 16 or -SR 17 is preferably an alkyl group, -OR 14 , -NR 15 R 16 or -SR 17 More preferably, it is an alkyl group or -OR 14 More preferably, -OR 14 It is particularly preferred that: In addition, R in formula (1-1) 10 When is an alkyl group, the alkyl group is preferably an alkyl group having an arylthio group or an alkyloxycarbonyl group at the α-position. R in formula (1-1) 10 -OR 14 If R 14 is preferably an alkyl group, more preferably an alkyl group having 1 to 8 carbon atoms, further preferably an isopropyl group or a t-butyl group, and particularly preferably a t-butyl group.

[0109] From the viewpoint of visibility, R in Equation (1-2) 11is preferably a hydrogen atom. From the viewpoint of visibility, R in formula (1-2) 12 is -C(=O)OR 14 , -OC(=O)OR 14 or a halogen atom, preferably -C(=O)OR 14 Or -OC(=O)OR 14 It is more preferable that R in formula (1-2) is 12 -C(=O)OR 14 Or -OC(=O)OR 14 If R 14 is preferably an alkyl group.

[0110] From the viewpoint of visibility, R in Equation (1-3) 11 are each independently preferably a hydrogen atom or an alkyl group, and at least one R 11 However, it is more preferably an alkyl group. Also, R 11 The alkyl group in is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 3 to 10 carbon atoms. Furthermore, R 11 The alkyl group in is preferably a branched alkyl group or a cycloalkyl group, more preferably a secondary or tertiary alkyl group or a cycloalkyl group, and further preferably an isopropyl group, a cyclopentyl group, a cyclohexyl group, or a t-butyl group. From the viewpoint of visibility, R in formula (1-3) 13 is preferably an aryl group, an alkoxy group or an onium group, more preferably a p-dimethylaminophenyl group or a pyridinium group, and further preferably a pyridinium group. R 13In the above formula, examples of the onium group include a pyridinium group, an ammonium group, and a sulfonium group. The onium group may have a substituent. Examples of the substituent include an alkyl group, an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a halogen atom, a carboxy group, a sulfo group, an alkyloxycarbonyl group, an aryloxycarbonyl group, and a combination of these groups. However, an alkyl group, an aryl group, and a combination of these groups are preferred. Among these, pyridinium groups are preferred, and examples thereof include N-alkyl-3-pyridinium groups, N-benzyl-3-pyridinium groups, N-(alkoxypolyalkyleneoxyalkyl)-3-pyridinium groups, N-alkoxycarbonylmethyl-3-pyridinium groups, N-alkyl-4-pyridinium groups, N-benzyl-4-pyridinium groups, N-(alkoxypolyalkyleneoxyalkyl)-4-pyridinium groups, and N-alkoxycarbonylmethyl-4-pyridinium groups. An N-alkyl-3,5-dimethyl-4-pyridinium group or an N-alkyl-3-pyridinium group is more preferred, an N-alkyl-3-pyridinium group or an N-alkyl-4-pyridinium group is even more preferred, an N-methyl-3-pyridinium group, an N-octyl-3-pyridinium group, an N-methyl-4-pyridinium group or an N-octyl-4-pyridinium group is particularly preferred, and an N-octyl-3-pyridinium group or an N-octyl-4-pyridinium group is most preferred. Also, R 13 When is a pyridinium group, examples of the counter anion include a sulfonate ion, a carboxylate ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a p-toluenesulfonate ion, a perchlorate ion, and the like, with the p-toluenesulfonate ion or the hexafluorophosphate ion being preferred.

[0111] From the viewpoint of visibility, R in Equation (1-4) 10 is preferably an alkyl group or an aryl group, and two R 10 It is more preferable that one of them is an alkyl group and the other is an aryl group. From the viewpoint of visibility, R in Equation (1-5)10 is preferably an alkyl group or an aryl group, more preferably an aryl group, and further preferably a p-methylphenyl group. From the viewpoint of visibility, R in Equation (1-6) 10 are each independently preferably an alkyl group or an aryl group, and more preferably a methyl group or a phenyl group. From the viewpoint of visibility, Z in formula (1-7) 1 is a counter ion that neutralizes the charge, and the compound as a whole may be included in the above Za. Z 1 is preferably a sulfonate ion, a carboxylate ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a p-toluenesulfonate ion, or a perchlorate ion, and more preferably a p-toluenesulfonate ion or a hexafluorophosphate ion.

[0112] The group whose bond to X1 is cleaved by exposure to heat or infrared rays is particularly preferably a group represented by formula (1-8).

[0113] [ka]

[0114] In formula (1-8), represents a bonding site with X1 in formula 1, and R 19 and R 20 each independently represents an alkyl group, and Za' represents a counter ion that neutralizes the charge.

[0115] The pyridinium ring and R in formula (1-8) 20 The bonding position to the hydrocarbon group containing the following is preferably the 3- or 4-position of the pyridinium ring, and more preferably the 4-position of the pyridinium ring. R 19 and R 20 The alkyl group in the formula (I) may be linear, branched, or have a ring structure. The alkyl group may have a substituent, and preferred examples of the substituent include an alkoxy group and a terminal alkoxypolyalkyleneoxy group. R 19 is preferably an alkyl group having 1 to 12 carbon atoms, more preferably a linear alkyl group having 1 to 12 carbon atoms, even more preferably a linear alkyl group having 1 to 8 carbon atoms, and particularly preferably a methyl group or an n-octyl group. R 20 is preferably an alkyl group having 1 to 8 carbon atoms, more preferably a branched alkyl group having 3 to 8 carbon atoms, further preferably an isopropyl group or a t-butyl group, and particularly preferably an isopropyl group. Za' may be any counter ion that neutralizes the charge, and the compound as a whole may be included in the above Za. Za' is preferably a sulfonate ion, a carboxylate ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a p-toluenesulfonate ion, or a perchlorate ion, and more preferably a p-toluenesulfonate ion or a hexafluorophosphate ion.

[0116] In addition, from the viewpoint of enhancing the visibility of the exposed area, the decomposable infrared absorber is preferably a group that is decomposed by infrared exposure (specifically, R 1 ) is preferably a cyanine dye. From the viewpoint of improving the visibility of the exposed area, the decomposable infrared absorbing agent is more preferably a compound represented by the following formula 1-1.

[0117] [ka]

[0118] In formula 1-1, R 1 represents a group represented by any one of the following formulas 2-1 to 4-1, and R 11 ~R 18 are each independently a hydrogen atom, a halogen atom, or -Ra , -OR b , -SR c , or -NR d R e R a ~R e each independently represents a hydrocarbon group; A1, A2 and a plurality of R 11 ~R 18 may be linked to form a monocyclic or polycyclic ring, A1 and A2 each independently represent an oxygen atom, a sulfur atom, or a nitrogen atom, n 11 and n 12 Each independently represents an integer of 0 to 5, provided that n 11 and n 12 The sum of is 2 or more, and n 13 and n 14 each independently represents 0 or 1, and L represents an oxygen atom, a sulfur atom, or -NR 10 - represents R 10 represents a hydrogen atom, an alkyl group, or an aryl group, and Za represents a counter ion that neutralizes the charge.

[0119] [ka]

[0120] In formulas 2-1 to 4-1, R 20 , R 30 , R 41 and R 42 each independently represents an alkyl group or an aryl group, Zb represents a counter ion that neutralizes the charge, and the wavy line represents a bonding site with the group represented by L in the above formula 1-1.

[0121] When the compound of formula 1-1 is exposed to infrared light, R 1 The -L bond is cleaved and L is =O, =S, or =NR 10 and discoloration.

[0122] In Formula 1-1, R 1 represents a group represented by any one of the above formulas 2-1 to 4-1. The group represented by formula 2-1, the group represented by formula 3-1, and the group represented by formula 4-1 will each be described below.

[0123] In formula 2-1, R 20 represents an alkyl group or an aryl group, and the wavy line portion represents the bonding site with the group represented by L in formula 1-1. R 20 The alkyl group represented by the formula (I) is preferably an alkyl group having 1 to 30 carbon atoms, more preferably an alkyl group having 1 to 15 carbon atoms, and further preferably an alkyl group having 1 to 10 carbon atoms. The alkyl group may be linear, branched, or have a ring structure. R 20 The aryl group represented by the following formula is preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and even more preferably an aryl group having 6 to 12 carbon atoms. R 20 From the viewpoint of visibility, the group is preferably an alkyl group.

[0124] In addition, from the viewpoint of decomposability and visibility, 20 The alkyl group represented by the formula (I) is preferably a secondary alkyl group or a tertiary alkyl group, and more preferably a tertiary alkyl group. Furthermore, from the viewpoints of decomposability and visibility, 20 The alkyl group represented by the formula (I) is preferably an alkyl group having 1 to 8 carbon atoms, more preferably a branched alkyl group having 3 to 10 carbon atoms, and even more preferably a branched alkyl group having 3 to 6 carbon atoms, particularly preferably an isopropyl group or a tert-butyl group, and most preferably a tert-butyl group.

[0125] Specific examples of the group represented by the above formula 2-1 are given below, but the present disclosure is not limited thereto. In the following structural formula, ● represents a bonding site with the group represented by L in formula 1-1.

[0126] [ka]

[0127] In formula 3-1, R 30 represents an alkyl group or an aryl group, and the wavy line portion represents the bonding site with the group represented by L in formula 1-1. R 30 As the alkyl group and the aryl group represented by the formula 2-1, R 20 The same applies to the alkyl group and the aryl group represented by the following formula (1), and preferred embodiments are also the same.

[0128] From the viewpoint of decomposability and visibility, 30 The alkyl group represented by the formula (I) is preferably a secondary alkyl group or a tertiary alkyl group, and more preferably a tertiary alkyl group. In addition, from the viewpoint of decomposability and visibility, 30 The alkyl group represented by the formula (I) is preferably an alkyl group having 1 to 8 carbon atoms, more preferably a branched alkyl group having 3 to 10 carbon atoms, and even more preferably a branched alkyl group having 3 to 6 carbon atoms, particularly preferably an isopropyl group or a tert-butyl group, and most preferably a tert-butyl group. Furthermore, from the viewpoints of decomposability and visibility, 30 The alkyl group represented by the formula (I) is preferably a substituted alkyl group, more preferably a fluoro-substituted alkyl group, further preferably a perfluoroalkyl group, and particularly preferably a trifluoromethyl group.

[0129] From the viewpoint of decomposability and visibility, 30 The aryl group represented by the following formula (I) is preferably a substituted aryl group, and examples of the substituent include an alkyl group (preferably an alkyl group having 1 to 4 carbon atoms) and an alkoxy group (preferably an alkoxy group having 1 to 4 carbon atoms).

[0130] Specific examples of the group represented by the above formula 3-1 are given below, but the present disclosure is not limited thereto. In the following structural formula, ● represents a bonding site with the group represented by L in formula 1-1.

[0131] [ka]

[0132] In formula 4-1, R 41 and R 42 each independently represents an alkyl group or an aryl group, Zb represents a counter ion that neutralizes the charge, and the wavy line portion represents a bonding site with the group represented by L in formula 1-1. R 41 or R 42 As the alkyl group and the aryl group represented by the formula 2-1, R 20 The same applies to the alkyl group and the aryl group represented by the following formula (1), and preferred embodiments are also the same. R 41 From the viewpoints of decomposability and visibility, the group is preferably an alkyl group. R 42 From the viewpoints of decomposability and visibility, the group is preferably an alkyl group.

[0133] From the viewpoint of decomposability and visibility, 41 The alkyl group represented by the formula (I) is preferably an alkyl group having 1 to 8 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, and particularly preferably a methyl group. From the viewpoint of decomposability and visibility, 42 The alkyl group represented by the formula (I) is preferably a secondary alkyl group or a tertiary alkyl group, and more preferably a tertiary alkyl group. In addition, from the viewpoint of decomposability and visibility, 42 The alkyl group represented by the formula (I) is preferably an alkyl group having 1 to 8 carbon atoms, more preferably a branched alkyl group having 3 to 10 carbon atoms, and even more preferably a branched alkyl group having 3 to 6 carbon atoms, particularly preferably an isopropyl group or a tert-butyl group, and most preferably a tert-butyl group.

[0134] Zb in formula 4-1 may be any counter ion for neutralizing the charge, and the compound as a whole may be included in Za in formula 1-1. Zb is preferably a sulfonate ion, a carboxylate ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a p-toluenesulfonate ion, or a perchlorate ion, and more preferably a tetrafluoroborate ion or a hexafluorophosphate ion.

[0135] Specific examples of the group represented by the above formula 4-1 are given below, but the present disclosure is not limited thereto. In the following structural formula, ● represents a bonding site with the group represented by L in formula 1-1.

[0136] [ka]

[0137] In formula 1-1, L is an oxygen atom or -NR 10 - is preferred, and an oxygen atom is particularly preferred. Also, -NR 10 -R in 10 is preferably an alkyl group. 10 The alkyl group represented by the formula (I) is preferably an alkyl group having 1 to 10 carbon atoms. 10 The alkyl group represented by the formula (I) may be linear, branched, or have a ring structure. Among the alkyl groups, a methyl group or a cyclohexyl group is preferred. -NR 10 -R in 10 When is an aryl group, it is preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and even more preferably an aryl group having 6 to 12 carbon atoms. In addition, these aryl groups may have a substituent.

[0138] In Formula 1-1, R 11 ~R 18 each independently represents a hydrogen atom, -R a , -OR b , -SR c , or -NR d R e It is preferable that: R a ~R e The hydrocarbon group represented by the following formula is preferably a hydrocarbon group having 1 to 30 carbon atoms, more preferably a hydrocarbon group having 1 to 15 carbon atoms, and even more preferably a hydrocarbon group having 1 to 10 carbon atoms. The hydrocarbon group may be linear, branched, or have a ring structure. As the above-mentioned hydrocarbon group, an alkyl group is particularly preferred.

[0139] The alkyl group is preferably an alkyl group having 1 to 30 carbon atoms, more preferably an alkyl group having 1 to 15 carbon atoms, and further preferably an alkyl group having 1 to 10 carbon atoms. The alkyl group may be linear, branched, or have a ring structure. Specific examples include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, an isopropyl group, an isobutyl group, a s-butyl group, a tert-butyl group, an isopentyl group, a neopentyl group, a 1-methylbutyl group, an isohexyl group, a 2-ethylhexyl group, a 2-methylhexyl group, a cyclohexyl group, a cyclopentyl group, and a 2-norbornyl group. Among the alkyl groups, a methyl group, an ethyl group, a propyl group or a butyl group is preferred.

[0140] The alkyl group may have a substituent. Examples of the substituent include an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a halogen atom, a carboxy group, a carboxylate group, a sulfo group, a sulfonate group, an alkyloxycarbonyl group, an aryloxycarbonyl group, and combinations thereof.

[0141] R in Formula 1-1 11 ~R 14 Each independently represents a hydrogen atom or -R a(that is, a hydrocarbon group), more preferably a hydrogen atom or an alkyl group, and further preferably a hydrogen atom, except in the following cases. Among them, R bonded to the carbon atom bonded to L and the carbon atom bonded to 11 and R 13 is preferably an alkyl group, and more preferably the two are linked to form a ring. The ring formed may be a monocyclic ring or a polycyclic ring. Specific examples of the ring formed include monocyclic rings such as a cyclopentene ring, a cyclopentadiene ring, a cyclohexene ring, and a cyclohexadiene ring, and polycyclic rings such as an indene ring and an indole ring. Also, A1 + R attached to the carbon atom to which 12 is R 15 or R 16 (Preferably R 16 ) to form a ring, and R bonded to the carbon atom to which A2 is bonded is preferably 14 is R 17 or R 18 (Preferably R 18 ) to form a ring.

[0142] In formula 1-1, n 13 is 1, and R 16 -R a (i.e., a hydrocarbon group). Also, R 16 is A1 + R attached to the carbon atom to which 12 It is preferable that the ring is formed by linking with the ring. The ring formed is preferably an indolium ring, a pyrylium ring, a thiopyrylium ring, a benzoxazoline ring, or a benzimidazoline ring, and from the viewpoint of improving the visibility of the exposed part, an indolium ring is more preferable. These rings may further have a substituent. In formula 1-1, n 14 is 1, and R 18 -R a (i.e., a hydrocarbon group). Also, R 18 is the R bonded to the carbon atom to which A2 is bonded.14 It is preferable that the ring is formed by linking with the above ring. The ring formed is preferably an indole ring, a pyran ring, a thiopyran ring, a benzoxazole ring, or a benzimidazole ring, and from the viewpoint of improving the visibility of the exposed part, an indole ring is more preferable. These rings may further have a substituent. R in Formula 1-1 16 and R 18 are preferably the same group, and when each of them forms a ring, A1 + and A2, it is preferable that they form a ring having the same structure.

[0143] R in Formula 1-1 15 and R 17 are preferably the same group. 15 and R 17 -R a (that is, a hydrocarbon group), more preferably an alkyl group, and further preferably a substituted alkyl group.

[0144] In the compound represented by formula 1-1, from the viewpoint of improving water solubility, R 15 and R 17 is preferably a substituted alkyl group. R 15 or R 17 Examples of the substituted alkyl group represented by the formula (a1) include groups represented by any of the following formulas (a1) to (a4).

[0145] [ka]

[0146] In formulas (a1) to (a4), R W0 represents an alkylene group having 2 to 6 carbon atoms, W represents a single bond or an oxygen atom, n W1 represents an integer from 1 to 45, and R W1 is an alkyl group having 1 to 12 carbon atoms or -C(=O)-R W5 R W5 represents an alkyl group having 1 to 12 carbon atoms, R W2 ~RW4 each independently represents a single bond or an alkylene group having 1 to 12 carbon atoms, and M represents a hydrogen atom, a sodium atom, a potassium atom, or an onium group.

[0147] In formula (a1), R W0 Specific examples of the alkylene group represented by the formula (I) include an ethylene group, an n-propylene group, an isopropylene group, an n-butylene group, an isobutylene group, an n-pentylene group, an isopentylene group, an n-hexyl group, an isohexyl group, and the like. Of these, an ethylene group, an n-propylene group, an isopropylene group, or an n-butylene group is preferred, and an n-propylene group is particularly preferred. n W1 is preferably 1 to 10, more preferably 1 to 5, and particularly preferably 1 to 3. R W1 Specific examples of the alkyl group represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, an n-hexyl group, an n-octyl group, and an n-dodecyl group. Of these, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, or a tert-butyl group is preferred, a methyl group or an ethyl group is more preferred, and a methyl group is particularly preferred. R W5 The alkyl group represented by R W1 The preferred embodiment is the same as the alkyl group represented by R W1 The preferred embodiments are the same as those of the alkyl group represented by the following formula:

[0148] Specific examples of the group represented by formula (a1) are shown below, but the present disclosure is not limited thereto. In the following structural formula, Me represents a methyl group, Et represents an ethyl group, and * represents a bonding site.

[0149] [ka]

[0150] In formula (a2) to formula (a4), R W2 ~R W4Specific examples of the alkylene group represented by the formula (I) include a methylene group, an ethylene group, an n-propylene group, an isopropylene group, an n-butylene group, an isobutylene group, an n-pentylene group, an isopentylene group, an n-hexyl group, an isohexyl group, an n-octylene group, and an n-dodecylene group. An ethylene group, an n-propylene group, an isopropylene group, or an n-butylene group is preferred, and an ethylene group or an n-propylene group is particularly preferred. In formula (a3), the two M's may be the same or different.

[0151] In the formulae (a2) to (a4), examples of the onium group represented by M include an ammonium group, an iodonium group, a phosphonium group, and a sulfonium group. CO2M in formula (a2), PO3M2 in formula (a2), and SO3M in formula (a4) may each have an anionic structure in which M is dissociated. The counter cation of the anionic structure is A1 + R in formula 1-1 may be 1 -L may be a cation that can be contained therein.

[0152] Among the groups represented by formulae (a1) to (a4), the groups represented by formula (a1), formula (a2) or formula (a4) are preferred.

[0153] n in Formula 1-1 11 and n 12 are preferably the same, and both are preferably an integer of 1 to 5, more preferably an integer of 1 to 3, further preferably 1 or 2, and particularly preferably 2.

[0154] In formula 1-1, A1 and A2 each independently represent an oxygen atom, a sulfur atom, or a nitrogen atom, and preferably a nitrogen atom. In formula 1-1, A1 and A2 are preferably the same atom.

[0155] Za in formula 1-1 represents a counter ion that neutralizes the charge. R 11 ~R 18 and R 1If all of -L are charge-neutral groups, Za is a monovalent counter anion. 11 ~R 18 and R 1 -L may have an anionic or cationic structure, for example, R 11 ~R 18 and R 1 When -L has two or more anion structures, Za can also be a counter cation. If the cyanine dye represented by formula 1-1 has a structure in which the entire compound is charge neutral except for Za, Za is not necessary. When Za is a counter anion, examples of the counter anion include a sulfonate ion, a carboxylate ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a p-toluenesulfonate ion, a perchlorate ion, and the like, with the tetrafluoroborate ion being preferred. When Za is a counter cation, examples of the counter cation include an alkali metal ion, an alkaline earth metal ion, an ammonium ion, a pyridinium ion, and a sulfonium ion. Of these, a sodium ion, a potassium ion, an ammonium ion, a pyridinium ion, or a sulfonium ion is preferred, and a sodium ion, a potassium ion, or an ammonium ion is more preferred.

[0156] From the viewpoint of improving the visibility of the exposed area, the decomposable infrared absorbing agent is more preferably a compound represented by the following formula 1-2 (that is, a cyanine dye).

[0157] [ka]

[0158] In formula 1-2, R 1 represents a group represented by any one of the above formulas 2-1 to 4-1, and R 19 ~R 22 are each independently a hydrogen atom, a halogen atom, or -R a , -OR b , -CN, -SR c , or -NR d R e R23 and R 24 Each independently represents a hydrogen atom or -R a R a ~R e each independently represents a hydrocarbon group; R 19 and R 20 , R 21 and R 22 , or R 23 and R 24 may be linked to form a monocycle or polycycle, and L is an oxygen atom, a sulfur atom, or -NR 10 - represents R 10 represents a hydrogen atom, an alkyl group, or an aryl group; R d1 ~R d4 , W 1 and W 2 each independently represents an alkyl group which may have a substituent, and Za represents a counter ion which neutralizes the charge.

[0159] R in Formula 1-2 1 is R in formula 1-1 1 The same applies to the preferred embodiments.

[0160] In formula 1-2, R 19 ~R 22 are each independently a hydrogen atom, a halogen atom, -R a , -OR b or -CN. More specifically, R 19 and R 21 is a hydrogen atom or -R a It is preferable that: Also, R 20 and R 22 is a hydrogen atom, -R a , -OR b or -CN. R 19 ~R 22 Represented by -R a As the group, an alkyl group or an alkenyl group is preferable. R 19 ~R 22 All of the above are -R aIf R 19 and R 20 and R 21 and R 22 are preferably linked to form a monocyclic or polycyclic ring. R 19 and R 20 or R 21 and R 22 Examples of the ring formed by linking include a benzene ring and a naphthalene ring.

[0161] In formula 1-2, R 23 and R 24 are preferably linked to form a monocycle or polycycle. R 23 and R 24 The ring formed by linking may be a monocycle or a polycycle. Specific examples of the ring formed include monocycles such as a cyclopentene ring, a cyclopentadiene ring, a cyclohexene ring, and a cyclohexadiene ring, and polycycles such as an indene ring.

[0162] In formula 1-2, R d1 ~R d4 is preferably an unsubstituted alkyl group. d1 ~R d4 are preferably the same group. The unsubstituted alkyl group may be an unsubstituted alkyl group having 1 to 4 carbon atoms, and among these, a methyl group is preferable.

[0163] In formula 1-2, W 1 and W 2 are each preferably independently a substituted alkyl group from the viewpoint of increasing the water solubility of the compound represented by formula 1-2. W 1 and W 2 Examples of the substituted alkyl group represented by the formula (a1) include groups represented by any one of formulas (a1) to (a4) in formula 1-1, and preferred embodiments are also the same. Also, W 1 and W 2are each independently, from the viewpoint of on-press developability, an alkyl group having a substituent, and the substituent is preferably at least —OCHCH—, a sulfo group, a salt of a sulfo group, a carboxy group, or a salt of a carboxy group.

[0164] Za represents a counter ion that neutralizes the charge in the molecule. R 19 ~R 22 , R 23 ~R 24 , R d1 ~R d4 , W 1 , W 2 , and R 1 If all of -L are charge-neutral groups, Za is a monovalent counter anion. 19 ~R 22 , R 23 ~R 24 , R d1 ~R d4 , W 1 , W 2 , and R 1 -L may have an anionic or cationic structure, for example, R 19 ~R 22 , R 23 ~R 24 , R d1 ~R d4 , W 1 , W 2 , and R 1 When -L has two or more anion structures, Za can also be a counter cation. In addition, when the compound represented by formula 1-2 has a structure in which the entire compound is charge neutral except for Za, Za is not necessary. Examples of Za when it is a counter anion are the same as Za in formula 1-1, and preferred embodiments are also the same. Examples of Za when it is a counter cation are the same as Za in formula 1-1, and preferred embodiments are also the same.

[0165] From the viewpoints of decomposability and visibility, the cyanine dye as the decomposable infrared absorber is more preferably a compound represented by any one of the following formulas 1-3 to 1-7. In particular, from the viewpoints of decomposability and visibility, a compound represented by any one of formulas 1-3, 1-5, and 1-6 is preferred.

[0166] [ka]

[0167] In formulas 1-3 to 1-7, R 1 represents a group represented by any one of the above formulas 2-1 to 4-1, and R 19 ~R 22 are each independently a hydrogen atom, a halogen atom, or -R a , -OR b , -CN, -SR c , or -NR d R e R 25 and R 26 each independently represents a hydrogen atom, a halogen atom, or -R a R a ~R e each independently represents a hydrocarbon group; R 19 and R 20 , R 21 and R 22 , or R 25 and R 26 may be linked to form a monocycle or polycycle, and L is an oxygen atom, a sulfur atom, or -NR 10 - represents R 10 represents a hydrogen atom, an alkyl group, or an aryl group; R d1 ~R d4 , W 1 and W 2 each independently represents an alkyl group which may have a substituent, and Za represents a counter ion which neutralizes the charge.

[0168] R in Formulas 1-3 to 1-7 1 , R 19 ~R 22 , R d1 ~R d4 , W 1 , W 2 , and L is R in Formula 1-2 1 , R 19~R 22 , R d1 ~R d4 , W 1 , W 2 and L, and the preferred embodiments are also the same. R in Formula 1-7 25 and R 26 are each independently preferably a hydrogen atom or an alkyl group, more preferably an alkyl group, and particularly preferably a methyl group.

[0169] Specific examples of the cyanine dye as the decomposable infrared absorber are given below, but the present disclosure is not limited thereto.

[0170] [ka]

[0171] From the viewpoint of color development, the infrared absorbing agent preferably contains a compound represented by the following formula (X) as a decomposable infrared absorbing agent.

[0172] [ka]

[0173] In formula (X), Ar 11 and Ar 12 each independently represents an atomic group necessary to form a substituted or unsubstituted aromatic ring or a substituted or unsubstituted heteroaromatic ring; R 11 and R 12 are each independently a substituted or unsubstituted alkyl group; R 13 represents a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted heteroaryl group; R 14 represents a hydrogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted heteroaryl group; Y each independently represents an oxygen atom, a sulfur atom, or >C(R 15 R 16), R 15 and R 16 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms, A1 and A2 each independently represent a substituted or unsubstituted alkyl group or a group of atoms including 2 or 3 carbon atoms necessary to form a substituted or unsubstituted 5- or 6-membered non-aromatic carbon ring by linking with each other, and Za represents a counter ion that neutralizes the charge.

[0174] The above Ar 11 and Ar 12 each independently represents an atomic group necessary for forming a substituted or unsubstituted aromatic ring, or a substituted or unsubstituted heteroaromatic ring. Examples of the substituent on the aromatic ring or heteroaromatic ring include an alkyl group, an alkoxy group, a halogen atom, a cyano group, a -COOR group, a -SOR group, or a -SOR group (R represents a substituted or unsubstituted alkyl group), and an alkyl group or a halogen atom is preferred. In addition, the above Ar 11 and Ar 12 is preferably an atomic group necessary for forming a substituted or unsubstituted aromatic ring, and more preferably an atomic group necessary for forming a substituted or unsubstituted benzene ring or naphthalene ring.

[0175] The above Y is independently >C(R 15 R 16 ), and >C(R 15 R 16 ) and R 15 and R 16 are preferably the same dialkylmethylene group. 15 and R 16 are preferably each independently a substituted or unsubstituted alkyl group having 1 or 2 carbon atoms. As the above Y, in particular, >C(R 15 R 16 ) and R 15 and R 16 is preferably a dialkylmethylene group in which R is a methyl group.

[0176] Above R 11 and R 12 is preferably a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms. 11 and R 12 may contain an ether bond or an ester bond in the middle of the carbon chain of the substituted or unsubstituted alkyl group having 1 to 12 carbon atoms.

[0177] Above R 13 is preferably a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms, and more preferably a haloalkyl group in which one or more hydrogen atoms of the alkyl group having 1 to 12 carbon atoms are substituted with a halogen atom. In this case, preferred examples of the halogen atom include a chlorine atom or a bromine atom. Among them, the above R 11 and R 12 are each independently preferably a perfluoroalkyl group.

[0178] Above R 14 is preferably a hydrogen atom or an unsubstituted alkyl group having 1 or 8 carbon atoms.

[0179] It is preferable that A1 and A2 each independently represent a substituted or unsubstituted alkyl group, or an atomic group containing 2 or 3 carbon atoms necessary to form a cyclopentene ring or a cyclohexene ring by bonding with each other.

[0180] When Za is a counter anion, it is preferably an anion containing a halogen atom or an anion containing a boron atom. - , PF6 - , BF4 - , SbF6 - , CH3SO3 - , CF3SO3 - , C6H5SO3 - , CH3C6H5SO3 - , HOC6H5SO3- , ClC6H5SO3 - , CH3C6H5SO3 - , tetraarylborate anion (for example, tetraphenylborate anion), and the like.

[0181] When Za is a counter cation, examples of the counter cation include an alkali metal ion, an alkaline earth metal ion, a tertiary ammonium ion, a quaternary ammonium ion, and an onium ion (such as an iodonium ion, a sulfonium ion, and a phosphonium ion).

[0182] Specific examples of the compound represented by formula (X) are listed below, but the present disclosure is not limited to these.

[0183] [ka]

[0184] In addition, as the infrared absorbent that decomposes upon exposure to infrared rays, those described in JP-T-2008-544322 or WO 2016 / 027886 can be suitably used. In addition, as the cyanine dye, which is a decomposable infrared absorber, the infrared absorbing compounds described in WO 2019 / 219560 can be suitably used.

[0185] The infrared absorbing agent may be used alone or in combination of two or more kinds. Also, a pigment and a dye may be used in combination as the infrared absorbing agent. The total content of the infrared absorbing agent in the image recording layer is preferably from 0.1% by mass to 10.0% by mass, and more preferably from 0.5% by mass to 5.0% by mass, based on the total mass of the image recording layer.

[0186] [Polymerization initiator] The image recording layer in the lithographic printing plate precursor according to the present disclosure preferably contains a polymerization initiator. Moreover, from the viewpoints of sensitivity, printing durability, on-press developability, and ink receptivity, the polymerization initiator preferably contains an electron-accepting polymerization initiator, and more preferably contains an electron-accepting polymerization initiator and an electron-donating polymerization initiator.

[0187] -Electron-accepting polymerization initiator- The image recording layer preferably contains an electron-accepting polymerization initiator as the polymerization initiator. The electron-accepting polymerization initiator is a compound that generates a polymerization initiating species such as a radical by accepting one electron through intermolecular electron transfer when electrons of an infrared absorbing agent are excited by exposure to infrared light. The electron-accepting polymerization initiator used in the present disclosure is a compound that generates a polymerization initiating species such as a radical or a cation by the energy of light, heat, or both, and can be appropriately selected from known thermal polymerization initiators, compounds having a bond with small bond dissociation energy, photopolymerization initiators, and the like. As the electron-accepting polymerization initiator, a radical polymerization initiator is preferable, and an onium salt compound is more preferable. The electron-accepting polymerization initiator is preferably an infrared-sensitive polymerization initiator. Examples of the electron-accepting radical polymerization initiator include (a) organic halides, (b) carbonyl compounds, (c) azo compounds, (d) organic peroxides, (e) metallocene compounds, (f) azide compounds, (g) hexaarylbiimidazole compounds, (i) disulfone compounds, (j) oxime ester compounds, and (k) onium salt compounds.

[0188] As the (a) organic halide, for example, the compounds described in paragraphs 0022 to 0023 of JP-A No. 2008-195018 are preferable. As the (b) carbonyl compound, for example, the compound described in paragraph 0024 of JP-A-2008-195018 is preferable. As the (c) azo compound, for example, the azo compounds described in JP-A-8-108621 can be used. (d) As the organic peroxide, for example, the compound described in paragraph 0025 of JP-A-2008-195018 is preferable. (e) As the metallocene compound, for example, the compound described in paragraph 0026 of JP-A-2008-195018 is preferable. (f) Examples of the azide compounds include 2,6-bis(4-azidobenzylidene)-4-methylcyclohexanone. (g) Preferred examples of the hexaarylbiimidazole compound include the compounds described in paragraph 0027 of JP-A-2008-195018. (i) Examples of the disulfone compound include the compounds described in JP-A-61-166544 and JP-A-2002-328465. As the (j) oxime ester compound, for example, the compounds described in paragraphs 0028 to 0030 of JP-A No. 2008-195018 are preferable.

[0189] Among the electron-accepting polymerization initiators, preferred from the viewpoint of curability are oxime ester compounds and onium salt compounds. Among them, from the viewpoint of printing durability, preferred are iodonium salt compounds, sulfonium salt compounds and azinium salt compounds, more preferred are iodonium salt compounds and sulfonium salt compounds, and particularly preferred are iodonium salt compounds. Specific examples of these compounds are shown below, but the present disclosure is not limited thereto.

[0190] Preferred examples of the iodonium salt compound include diaryliodonium salt compounds, more preferred are diphenyliodonium salt compounds substituted with electron-donating groups such as alkyl groups or alkoxy groups, and more preferred are asymmetric diphenyliodonium salt compounds. Specific examples include diphenyliodonium hexafluorophosphate, 4-methoxyphenyl-4-(2-methylpropyl)phenyliodonium hexafluorophosphate, 4-(2-methylpropyl)phenyl-p-tolyliodonium hexafluorophosphate, 4-hexyloxyphenyl-2,4,6-trimethoxyphenyliodonium hexafluorophosphate, 4-hexyloxyphenyl-2,4-diethoxyphenyliodonium tetrafluoroborate, 4-octyloxyphenyl-2,4,6-trimethoxyphenyliodonium 1-perfluorobutanesulfonate, 4-octyloxyphenyl-2,4,6-trimethoxyphenyliodonium hexafluorophosphate, and bis(4-t-butylphenyl)iodonium hexafluorophosphate.

[0191] As an example of the sulfonium salt compound, a triarylsulfonium salt compound is preferred, particularly a triarylsulfonium salt compound in which at least a part of the electron-withdrawing group, for example, the group on the aromatic ring, is substituted with a halogen atom, and more preferably a triarylsulfonium salt compound in which the total number of halogen atoms substituted on the aromatic ring is 4 or more. Specific examples include triphenylsulfonium hexafluorophosphate, triphenylsulfonium benzoylformate, bis(4-chlorophenyl)phenylsulfonium benzoylformate, bis(4-chlorophenyl)-4-methylphenylsulfonium tetrafluoroborate, tris(4-chlorophenyl)sulfonium 3,5-bis(methoxycarbonyl)benzenesulfonate, tris(4-chlorophenyl)sulfonium hexafluorophosphate, and tris(2,4-dichlorophenyl)sulfonium hexafluorophosphate.

[0192] As the counter anion of the iodonium salt compound and the sulfonium salt compound, a sulfonamide anion or a sulfonimide anion is preferable, and a sulfonimide anion is more preferable. The sulfonamide anion is preferably an arylsulfonamide anion. The sulfonimide anion is preferably a bisarylsulfonimide anion. Specific examples of sulfonamide anions or sulfonimide anions are shown below, but the present disclosure is not limited thereto. In the following specific examples, Ph represents a phenyl group, Me represents a methyl group, and Et represents an ethyl group.

[0193] [ka]

[0194] The polymerization initiator preferably contains, as the electron-accepting polymerization initiator, a compound A represented by the following formula (Ia) and one or more compounds B selected from the group consisting of compounds represented by the following formula (Ib) or (Ic): [ka]

[0195] In formulas (Ia) to (Ic), R1, R2, R3, R4, R5 and R6 are each independently a substituted or unsubstituted alkyl group or a substituted or unsubstituted alkoxy group having 2 to 9 carbon atoms, at least one of R3 and R4 is different from R1 or R2, the difference between the total number of carbon atoms in R1 and R2 and the total number of carbon atoms in R3 and R4 is 0 to 4 (i.e., 0, 1, 2, 3 or 4), the difference between the total number of carbon atoms in R1 and R2 and the total number of carbon atoms in R5 and R6 is 0 to 4, and X1, X2 and X3 are the same or different anions.

[0196] The above R1, R2, R3, R4, R5 and R6 are each preferably a substituted or unsubstituted alkyl group having 2 to 9 carbon atoms or a substituted or unsubstituted alkoxy group having 2 to 9 carbon atoms, more preferably a substituted or unsubstituted alkyl group having 3 to 6 carbon atoms or a substituted or unsubstituted alkoxy group having 3 to 6 carbon atoms, and even more preferably a substituted or unsubstituted alkyl group having 3 to 6 carbon atoms. The alkyl group and alkoxy group may be either linear or branched, but are preferably branched. Examples of the substituted or unsubstituted alkyl group include an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, a t-butyl group, an n-pentyl group, a t-pentyl group, a sec-pentyl group, a neopentyl group, an n-hexyl group, an iso-hexyl group, a sec-hexyl group, a t-hexyl group, an n-heptyl group, an n-octyl group, an iso-octyl group, a 2-ethylhexyl group, and an n-nonyl group. Examples of the substituted or unsubstituted alkoxy group include an ethoxy group, an n-propoxy group, an iso-propoxy group, a t-butoxy group, an n-butoxy group, and an n-octyloxy group.

[0197] The above X1, X2 and X3 are ClO4 - , PF6 - , BF4 - , SbF6 - , CH3SO3 - , CF3SO3 - , C6H5SO3 - , CH3C6H4SO3 - , HOC6H4SO3 - , ClC6H4SO3 - and the borate anion represented by the following structure (Id):

[0198] B - (R 1 )(R 2 )(R 3 )(R 4 ) Formula (Id)

[0199] In formula (Id), R1 , R 2 , R 3 and R 4 R each independently represents a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl group (including a halogen-substituted aryl group), a substituted or unsubstituted alkenyl group, a substituted or unsubstituted alkynyl group, a substituted or unsubstituted cycloalkyl group, or a substituted or unsubstituted heterocyclic group. 1 , R 2 , R 3 and R 4 may be linked together to form a substituted or unsubstituted heterocycle containing a boron atom. The resulting heterocycle has up to seven carbon, nitrogen, oxygen or nitrogen atoms. R 1 , R 2 , R 3 and R 4 The substituent in the formula (I) may be a chlorine atom, a fluorine atom, a nitro group, an alkyl group, an alkoxy group, or an acetoxy group.

[0200] Above R 1 , R 2 , R 3 and R 4 Preferably, all of the groups are substituted or unsubstituted aryl groups, and more preferably all are unsubstituted phenyl groups.

[0201] At least one of X1, X2, and X3 is preferably a tetraarylborate anion containing the same or different aryl groups, more preferably one or more is a tetraphenylborate anion, and further preferably each of X1, X2, and X3 is a tetraphenylborate anion.

[0202] In a preferred embodiment, compound B includes a compound represented by formula (Ic), R1 is the same as R5, and R2 is the same as R6. In particular, R1 is the same as R2, and for example, it is preferred that both R1 and R2 are an iso-propyl group, an iso-butyl group, or a t-butyl group.

[0203] In another preferred embodiment, compound B includes a compound represented by formula (Ib), R1 is the same as R2, and R3 is the same as R4. In this case, both R1 and R2 are preferably iso-propyl, iso-butyl, or t-butyl. In addition, the difference in the number of carbon atoms between R1 and R3 is preferably 1 or 2.

[0204] Compound B may be a mixture of a compound represented by formula (Ib) and a compound represented by formula (Ic).

[0205] The compounds represented by formulae (Ia) to (Ic) may be obtained from companies such as Sigma-Aldrich, or may be synthesized using known synthetic methods and readily available starting materials.

[0206] The molar ratio of compound A to compound B is preferably 10:90 to 90:10, more preferably 20:80 to 80:20, and further preferably 30:70 to 70:30.

[0207] In addition, the electron-accepting polymerization initiator may contain a compound represented by formula (II) described in paragraphs 0186 to 0197 of WO 2022 / 019217 from the viewpoints of developability and UV printing durability of the resulting lithographic printing plate.

[0208] The lowest unoccupied molecular orbital (LUMO) of the electron-accepting polymerization initiator is preferably −3.00 eV or less, and more preferably −3.02 eV or less, from the viewpoints of improving sensitivity and preventing plate skipping. The lower limit is preferably −3.80 eV or more, and more preferably −3.60 eV or more.

[0209] The electron-accepting polymerization initiator may be used alone or in combination of two or more kinds. The content of the electron-accepting polymerization initiator is preferably 0.1% by mass to 50% by mass, more preferably 0.5% by mass to 30% by mass, and particularly preferably 0.8% by mass to 20% by mass, based on the total mass of the image recording layer.

[0210] -Electron-donating polymerization initiator- From the viewpoint of contributing to improvement of the chemical resistance and UV printing durability of the lithographic printing plate, the polymerization initiator preferably contains an electron-donating polymerization initiator, and more preferably contains both the electron-donating polymerization initiator and the above-mentioned electron-donating polymerization initiator. Examples of the electron-donating polymerization initiator include the following five types. (i) Alkyl or aryl ate complexes: It is believed that the carbon-hetero bond is oxidatively cleaved to generate active radicals. Specific examples include borate salt compounds. (ii) Aminoacetic acid compounds: It is believed that the C-X bond on the carbon adjacent to the nitrogen is cleaved by oxidation to generate an active radical. X is preferably a hydrogen atom, a carboxyl group, a trimethylsilyl group, or a benzyl group. Specific examples include N-phenylglycines (which may have a substituent on the phenyl group), N-phenyliminodiacetic acid (which may have a substituent on the phenyl group), etc. (iii) Sulfur-containing compounds: The above-mentioned aminoacetic acid compounds, in which the nitrogen atom is replaced with a sulfur atom, can generate active radicals by the same action. A specific example is phenylthioacetic acid (the phenyl group may have a substituent). (iv) Tin-containing compounds: Compounds in which the nitrogen atom of the above-mentioned aminoacetic acid compounds is replaced with a tin atom can generate active radicals by the same action. (v) Sulfinates: These can generate active radicals by oxidation. Specific examples include sodium arylsulfinate.

[0211] Among these electron-donating polymerization initiators, the image recording layer preferably contains a borate salt compound. As the borate salt compound, a tetraarylborate salt compound or a monoalkyltriarylborate salt compound is preferable, and from the viewpoint of compound stability, a tetraarylborate salt compound is more preferable, and a tetraphenylborate salt compound is particularly preferable. The counter cation of the borate salt compound is not particularly limited, but is preferably an alkali metal ion or a tetraalkylammonium ion, and more preferably a sodium ion, a potassium ion, or a tetrabutylammonium ion.

[0212] A specific example of a preferred borate salt compound is sodium tetraphenylborate.

[0213] In addition, the highest occupied molecular orbital (HOMO) of the electron donating polymerization initiator used in the present disclosure is preferably −6.00 eV or more, more preferably −5.95 eV or more, even more preferably −5.93 eV or more, and particularly preferably greater than −5.90 eV, from the viewpoints of chemical resistance and UV printing durability. The upper limit is preferably −5.00 eV or less, and more preferably −5.40 eV or less.

[0214] As preferred specific examples of the electron-donating polymerization initiator, B-1 to B-8 and other compounds are shown below, but it goes without saying that the present invention is not limited to these. In the following chemical formulas, Bu represents an n-butyl group, and Z represents a counter cation. Z + As the counter cation represented by + , K + , N + (Bu)4, etc. The above Bu represents an n-butyl group. Also, Z + Suitable examples of the counter cation represented by the formula (I) include the onium ions in the above electron-accepting polymerization initiators.

[0215] [ka]

[0216] [ka]

[0217] In addition, from the viewpoints of visibility, UV printing durability, and stability over time, the image recording layer preferably contains at least one compound selected from the group consisting of an onium salt compound as the electron-accepting polymerization initiator and a borate salt compound as the electron-donating polymerization initiator, and more preferably contains an onium salt compound as the electron-accepting polymerization initiator and a borate salt compound as the electron-donating polymerization initiator. In addition, it is preferable that the image recording layer contains a borate salt compound as the electron-donating polymerization initiator, and it is more preferable that the image recording layer contains a borate salt compound as the electron-donating polymerization initiator, and that the value of HOMO of the infrared absorber - HOMO of the borate salt compound is 0.70 eV or less. Each of the HOMOs is calculated by the method described below.

[0218] The electron-donating polymerization initiator may be added either alone or in combination of two or more. The content of the electron-donating polymerization initiator is preferably from 0.01% by mass to 30% by mass, more preferably from 0.05% by mass to 25% by mass, and even more preferably from 0.1% by mass to 20% by mass, based on the total mass of the image recording layer.

[0219] In addition, one of the preferred aspects of the present disclosure is an aspect in which the electron-accepting polymerization initiator and the electron-donating polymerization initiator form a salt. Specifically, for example, the onium salt compound may be a salt of an onium ion and an anion in the electron-donating polymerization initiator (e.g., tetraphenylborate anion).More preferably, the onium salt compound may be an iodonium borate salt compound in which an iodonium cation in the iodonium salt compound (e.g., di-p-tolyliodonium cation) and a borate anion in the electron-donating polymerization initiator form a salt. Specific examples of the embodiment in which the electron-accepting polymerization initiator and the electron-donating polymerization initiator form a salt are shown below, but the present disclosure is not limited thereto.

[0220] [ka]

[0221] In the present disclosure, when the image recording layer contains an onium ion and an anion in the above-mentioned electron-donating polymerization initiator, the image recording layer contains an electron-accepting polymerization initiator and the above-mentioned electron-donating polymerization initiator.

[0222] [Relationship between Electron-Donating Polymerization Initiator, Electron-Accepting Polymerization Initiator, and Infrared Absorber] The image recording layer in the present disclosure contains the electron-donating polymerization initiator, the electron-accepting polymerization initiator, and the infrared absorbing agent, and it is preferable that the HOMO of the electron-donating polymerization initiator is −6.0 eV or more and the LUMO of the electron-accepting polymerization initiator is −3.0 eV or less. More preferred embodiments of the HOMO of the electron-donating polymerization initiator and the LUMO of the electron-accepting polymerization initiator are as described above. In the image recording layer of the present disclosure, it is presumed that the electron-donating polymerization initiator, at least one of the infrared absorbers, and the electron-accepting polymerization initiator transfer energy, for example, as shown in the following chemical formula. Therefore, if the HOMO of the electron-donating polymerization initiator is −6.0 eV or more and the LUMO of the electron-accepting polymerization initiator is −3.0 eV or less, it is believed that the radical generation efficiency is improved, and therefore the chemical resistance and UV printing resistance are more likely to be excellent.

[0223] [ka]

[0224] From the viewpoint of UV printing durability and chemical resistance, the value of at least one HOMO of the infrared absorber-the HOMO of the electron donating polymerization initiator is preferably 1.0 eV or less, more preferably 0.70 eV or less, and particularly preferably 0.60 eV or less. From the same viewpoint, the value of at least one HOMO of the infrared absorber-the HOMO of the electron donating polymerization initiator is preferably -0.200 eV or more, more preferably -0.100 eV or more. Note that a negative value means that the HOMO of the electron donating polymerization initiator is higher than the HOMO of at least one of the infrared absorbers. From the viewpoints of UV printing durability and chemical resistance, the value of the LUMO of the electron-accepting polymerization initiator minus the LUMO of at least one of the infrared absorbing agents is preferably 1.00 eV or less, more preferably 0.700 eV or less. From the same viewpoint, the value of the LUMO of the electron-accepting polymerization initiator minus the LUMO of at least one of the infrared absorbing agents is preferably -0.200 eV or more, more preferably -0.100 eV or more. From the same viewpoint, the value of LUMO of the electron-accepting polymerization initiator minus LUMO of at least one of the infrared absorbers is preferably 1.00 eV to -0.200 eV, more preferably 0.700 eV to -0.100 eV. Note that a negative value means that the LUMO of at least one of the infrared absorbers is higher than the LUMO of the electron-accepting polymerization initiator.

[0225] [Polymerizable compound] The image recording layer in the present disclosure preferably contains a polymerizable compound. In the present disclosure, a polymerizable compound refers to a compound having a polymerizable group. The polymerizable group is not particularly limited and may be any known polymerizable group, but is preferably an ethylenically unsaturated group. The polymerizable group may be either a radically polymerizable group or a cationic polymerizable group, but is preferably a radically polymerizable group. Examples of the radically polymerizable group include a (meth)acryloyl group, an allyl group, a vinylphenyl group, and a vinyl group, and from the viewpoint of reactivity, a (meth)acryloyl group is preferred. The molecular weight of the polymerizable compound (when the polymerizable compound has a molecular weight distribution, the weight average molecular weight) is preferably 50 or more and less than 2,500.

[0226] The polymerizable compound used in the present disclosure may be, for example, a radically polymerizable compound or a cationic polymerizable compound, but is preferably an addition-polymerizable compound having at least one ethylenically unsaturated bond (ethylenically unsaturated compound). The ethylenically unsaturated compound is preferably a compound having at least one terminal ethylenically unsaturated bond, more preferably a compound having two or more terminal ethylenically unsaturated bonds. The polymerizable compound has a chemical form such as a monomer, a prepolymer, i.e., a dimer, a trimer or an oligomer, or a mixture thereof. Among them, from the viewpoint of UV printing durability, the polymerizable compound preferably contains a trifunctional or more polymerizable compound, more preferably contains a heptafunctional or more polymerizable compound, and even more preferably contains a ten-functional or more polymerizable compound. Furthermore, from the viewpoint of UV printing durability of the resulting lithographic printing plate, the polymerizable compound preferably contains a trifunctional or more (preferably heptafunctional or more, more preferably ten-functional or more) ethylenically unsaturated compound, and even more preferably contains a trifunctional or more (preferably heptafunctional or more, more preferably ten-functional or more) (meth)acrylate compound.

[0227] Moreover, from the viewpoints of on-machine developability and stain suppression, the polymerizable compound preferably contains a polymerizable compound having two or fewer functionalities, more preferably contains a bifunctional polymerizable compound, and particularly preferably contains a bifunctional (meth)acrylate compound. From the viewpoints of printing durability, on-press developability, and stain suppression, the content of the difunctional or lower polymerizable compound (preferably a difunctional polymerizable compound) is preferably 5% by mass to 100% by mass, more preferably 10% by mass to 100% by mass, and particularly preferably 15% by mass to 100% by mass, relative to the total mass of the polymerizable compounds in the image recording layer.

[0228] <<Oligomer>> The polymerizable compound contained in the image recording layer preferably contains a polymerizable compound which is an oligomer (hereinafter, also simply referred to as "oligomer"). In the present disclosure, an oligomer refers to a polymerizable compound having a molecular weight (weight average molecular weight when the molecular weight has a molecular weight distribution) of 600 or more and 10,000 or less and containing at least one polymerizable group. From the viewpoint of excellent chemical resistance and UV printing resistance, the molecular weight of the oligomer is preferably 1,000 or more and 5,000 or less.

[0229] In addition, from the viewpoint of improving UV printing durability, the number of polymerizable groups in one oligomer molecule is preferably 2 or more, more preferably 3 or more, even more preferably 6 or more, and particularly preferably 10 or more. The upper limit of the number of polymerizable groups in the oligomer is not particularly limited, but the number of polymerizable groups is preferably 20 or less.

[0230] From the viewpoints of UV printing durability and on-press developability, the oligomer preferably has 7 or more polymerizable groups and a molecular weight of 1,000 or more and 10,000 or less, and more preferably has 7 or more polymerizable groups and a molecular weight of 1,000 or more and 5,000 or less. In addition, the oligomer may contain a polymer component that may be generated during the production process of the oligomer.

[0231] From the viewpoints of UV printing durability, visibility, and on-press developability, the oligomer preferably contains at least one selected from the group consisting of a compound having a urethane bond, a compound having an ester bond, and a compound having an epoxy residue, and more preferably contains a compound having a urethane bond. In the present disclosure, the epoxy residue refers to a structure formed by an epoxy group, and means, for example, a structure similar to the structure obtained by the reaction of an acid group (such as a carboxylic acid group) with an epoxy group.

[0232] The compound having a urethane bond, which is an example of the oligomer, is preferably, for example, a compound having at least a group represented by the following formula (Ac-1) or formula (Ac-2), and more preferably a compound having at least a group represented by the following formula (Ac-1).

[0233] [ka]

[0234] In formula (Ac-1) and formula (Ac-2), L 1 ~L 4 each independently represents a divalent hydrocarbon group having 2 to 20 carbon atoms, and the wavy line portion represents the bonding position to other structures. L 1 ~L 4 are each independently preferably an alkylene group having 2 to 20 carbon atoms, more preferably an alkylene group having 2 to 10 carbon atoms, and further preferably an alkylene group having 4 to 8 carbon atoms. In addition, the alkylene group may have a branched or cyclic structure, but is preferably a linear alkylene group.

[0235] It is preferred that each of the wavy line portions in formula (Ac-1) or formula (Ac-2) independently directly bond to a wavy line portion in a group represented by formula (Ae-1) or formula (Ae-2) below.

[0236] [ka]

[0237] In formula (Ae-1) and formula (Ae-2), R each independently represents an acryloyloxy group or a methacryloyloxy group, and the wavy line portion represents the bonding position to the wavy line portion in formula (Ac-1) and formula (Ac-2).

[0238] Furthermore, as the compound having a urethane bond, a compound in which a polymerizable group is introduced by a polymer reaction into a polyurethane obtained by reacting a polyisocyanate compound with a polyol compound may be used. For example, a compound having a urethane bond may be obtained by reacting a polyurethane oligomer obtained by reacting a polyol compound having an acid group with a polyisocyanate compound, with a compound having an epoxy group and a polymerizable group.

[0239] The number of polymerizable groups in the compound having an ester bond, which is an example of the oligomer, is preferably 3 or more, and more preferably 6 or more.

[0240] As a compound having an epoxy residue, which is an example of an oligomer, a compound containing a hydroxy group within the compound is preferred. The compound having an epoxy residue preferably has 2 to 6 polymerizable groups, and more preferably has 2 to 3 polymerizable groups. The compound having an epoxy residue can be obtained, for example, by reacting a compound having an epoxy group with acrylic acid.

[0241] Specific examples of oligomers are shown in the table below, but the oligomers used in the present disclosure are not limited thereto. As the oligomer, commercially available products may be used, and examples thereof include UA510H, UA-306H, UA-306I, UA-306T (all manufactured by Kyoeisha Chemical Co., Ltd.), UV-1700B, UV-6300B, UV7620EA (all manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), U-15HA (manufactured by Shin-Nakamura Chemical Co., Ltd.), EBECRYL450, EBECRYL657, EBECRYL885, EBECRYL800, EBECRYL3416, EBECRYL860 (all manufactured by Daicel Allnex Corporation), but are not limited thereto.

[0242] From the viewpoint of improving chemical resistance, UV printing durability, and suppression of on-press development residue, the content of the oligomer is preferably 30% by mass to 100% by mass, more preferably 50% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass, relative to the total mass of the polymerizable compounds in the image recording layer.

[0243] <<Low molecular polymerizable compounds>> The polymerizable compound may further contain a polymerizable compound other than the above-mentioned oligomer. From the viewpoint of chemical resistance, the polymerizable compound other than the oligomer is preferably a low molecular weight polymerizable compound. The low molecular weight polymerizable compound may be in a chemical form such as a monomer, a dimer, a trimer, or a mixture thereof. From the viewpoint of chemical resistance, the low molecular weight polymerizable compound is preferably at least one polymerizable compound selected from the group consisting of polymerizable compounds having three or more ethylenically unsaturated groups and polymerizable compounds having an isocyanuric ring structure.

[0244] In the present disclosure, the low molecular weight polymerizable compound refers to a polymerizable compound having a molecular weight of 50 or more and less than 600 (weight average molecular weight when the compound has a molecular weight distribution). The molecular weight of the low molecular weight polymerizable compound is preferably 100 or more and less than 600, more preferably 300 or more and less than 600, and even more preferably 400 or more and less than 600, from the viewpoint of excellent chemical resistance, UV printing durability, and on-press development residue suppression.

[0245] When the polymerizable compound contains a low molecular weight polymerizable compound as a polymerizable compound other than an oligomer (when two or more kinds of low molecular weight polymerizable compounds are contained, the total amount thereof), from the viewpoints of chemical resistance, UV printing durability, and suppression of on-press development residue, the ratio of the oligomer to the low molecular weight polymerizable compound (oligomer / low molecular weight polymerizable compound) is preferably 10 / 1 to 1 / 10, more preferably 10 / 1 to 3 / 7, and even more preferably 10 / 1 to 7 / 3, by mass.

[0246] In addition, as the low molecular weight polymerizable compound, the polymerizable compounds described in paragraphs 0082 to 0086 of WO 2019 / 013268 can also be suitably used.

[0247] Details of the method of use, such as the structure of the polymerizable compound, whether it is used alone or in combination, and the amount added, can be set arbitrarily. In particular, from the viewpoint of UV printing durability, the image recording layer preferably contains two or more types of polymerizable compounds. The content of the polymerizable compounds (when two or more types of polymerizable compounds are contained, the total content of the polymerizable compounds) is preferably 5% by mass to 75% by mass, more preferably 10% by mass to 70% by mass, and even more preferably 15% by mass to 60% by mass, relative to the total mass of the image recording layer.

[0248] [Compound represented by formula (Ph)] From the viewpoint of color development, the image recording layer may further contain a compound represented by the following formula (Ph).

[0249] [ka]

[0250] In formula (Ph), X P represents O, S or NH; Y P represents N or CH; R P1 represents a hydrogen atom or an alkyl group, R P2 and R P3each independently represents a halogen atom, an alkylthio group, an arylthio group, an alkoxy group, an aryloxy group, an alkyl group, an aryl group, an acylthio group, or an acyl group; mp and np each independently represent an integer of 0 to 4.

[0251] Above X P As the group, S or NH is preferable, and S is more preferable. Above Y P As the group, N is preferable. R p1 is preferably a hydrogen atom or a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, and more preferably a hydrogen atom.

[0252] Rp2 and Rp3 are each independently preferably a halogen atom such as a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom, an alkylthio group having 1 to 20 carbon atoms, a phenylthio group, an alkoxy group having 1 to 20 carbon atoms, a phenoxy group, an alkyl group having 1 to 20 carbon atoms, a phenyl, an acetylthio group, or an acetyl group, and more preferably a chlorine atom, an alkylthio group having 1 or 2 carbon atoms, or an acetyl group. These groups may have one or more substituents.

[0253] It is preferable that mp and np are each independently 0, 1, or 2. Both mp and np may be 0, or mp may be 0 and np may be 1 or 2.

[0254] Specific examples of the compound represented by formula (Ph) are shown below.

[0255] [ka]

[0256] The compound represented by formula (Ph) may be added either alone or in combination of two or more. The content of the compound represented by formula (Ph) is preferably from 0.1 to 5% by mass, and more preferably from 0.5 to 3% by mass, based on the total mass of the image recording layer.

[0257] [Polymer having a structural unit represented by formula (I)] The image recording layer may further contain a polymer (I) having a structural unit represented by the following formula (I). Hereinafter, the polymer (I) having a structural unit represented by formula (I) will also be simply referred to as "polymer (I)".

[0258] [ka]

[0259] In formula (I), R 11 and R 12 each independently represents a hydrogen atom or an alkyl group; R 13 represents a hydrogen atom or a monovalent substituent; L 11 and L 12 each independently represents a single bond or a divalent linking group, and Rh represents a substituent containing two or more silicon atoms.

[0260] R 11 and R 12 Examples of the alkyl group represented by the formula (1) include a linear alkyl group having 1 to 18 carbon atoms, and a branched or cyclic alkyl group having 3 to 18 carbon atoms. Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, an isopropyl group, a tert-butyl group, and a cyclohexyl group. R 11 and R 12 Each of them is preferably a hydrogen atom.

[0261] R 13 Examples of the monovalent substituent represented by the formula (I) include an alkyl group, an alkenyl group, and an aryl group. Examples of the alkyl group include linear alkyl groups having 1 to 18 carbon atoms and branched or cyclic alkyl groups having 3 to 18 carbon atoms. Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, an isopropyl group, a tert-butyl group, and a cyclohexyl group. Examples of the alkenyl group include alkenyl groups having a carbon number of 2 to 12. Specific examples of the alkenyl group include a vinyl group, a 1-propenyl group, a 1-butenyl group, a 1-methyl-1-propenyl group, a 1-cyclopentenyl group, and a 1-cyclohexenyl group. The aryl group may, for example, be an aryl group having a carbon number of 6 to 12. Specific examples of the aryl group include a phenyl group, an α-methylphenyl group, and a naphthyl group. R 13 is preferably a hydrogen atom or a methyl group.

[0262] L 11 Examples of the divalent linking group represented by the formula (I) include -C(=O)-O- (a so-called ester bond) and -C(=O)-NH-. In addition, L 11 The divalent linking group represented by the following formula is preferably an ester bond, -C(=O)-O-.

[0263] L 12 The divalent linking group represented by L 11 There are no particular limitations as long as it is a group that can link L to Rh. 12 An example of the divalent linking group represented by the formula: is an alkylene group. The alkylene group is preferably an alkylene group having 2 to 10 carbon atoms, and more preferably an alkylene group having 4 to 8 carbon atoms.

[0264] The substituent containing two or more silicon atoms represented by Rh is not particularly limited as long as the atomic group constituting the substituent contains two or more silicon atoms. From the viewpoint of on-machine developability, the substituent containing two or more silicon atoms preferably contains the silicon atoms as silicon-oxygen bonds (Si-O bonds). The substituent containing two or more silicon atoms preferably has two or more silicon-oxygen bonds, preferably has three or more, and preferably has 3 to 12. The substituent containing two or more silicon atoms preferably contains the silicon-oxygen bonds as a polysiloxane structure. From the viewpoint of on-press developability, the substituent containing two or more silicon atoms preferably has a branched structure, and more preferably has a branched structure branched from the silicon atom at the center.

[0265] Specifically, Rh in formula (I) is preferably a group having two or more structures represented by the following formula (a1).

[0266] JPEG2024143724000047.jpg1933

[0267] In the above formula (a1), * represents a bonding position, and R 1 , R 2 , and R 3 each independently represents an alkyl group, an alkenyl group, an aryl group, or an alkylenearyl group.

[0268] R 1 , R 2 , and R 3 Examples of the alkyl group represented by the formula (1) include linear alkyl groups having 1 to 18 carbon atoms, and branched or cyclic alkyl groups having 3 to 18 carbon atoms. Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, an isopropyl group, a tert-butyl group, and a cyclohexyl group. R 1 , R 2 , and R 3 Examples of the alkenyl group represented by the formula (I) include alkenyl groups having 2 to 12 carbon atoms. Specific examples of the alkenyl group include a vinyl group, a 1-propenyl group, a 1-butenyl group, a 1-methyl-1-propenyl group, a 1-cyclopentenyl group, and a 1-cyclohexenyl group. R 1 , R 2 , and R 3 Examples of the aryl group represented by the formula (I) include aryl groups having a carbon number of 6 to 12. Specific examples of the aryl group include a phenyl group, an α-methylphenyl group, and a naphthyl group. R 1 , R 2 , and R 3Examples of the alkylenearyl group represented by the following formula include alkylenearyl groups having 7 to 30 carbon atoms.

[0269] In formula (a1), R 1 , R 2 , and R 3 is preferably each independently an alkyl group, more preferably all the same alkyl group, further preferably all alkyl groups having 1 to 4 carbon atoms, and particularly preferably all methyl groups.

[0270] The substituent containing two or more silicon atoms is preferably a group containing three or more structures represented by the above formula (a1), and more preferably a group containing 3 to 6 structures.

[0271] The substituent containing two or more silicon atoms is preferably a group represented by the following formula (a2). [ka]

[0272] In the above formula (a2), * represents a bonding position, and R 1 , R 2 , and R 3 each independently represents an alkyl group, an alkenyl group, an aryl group, or an alkylenearyl group. R in formula (a2) 1 , R 2 , and R 3 is R in the above formula (a1). 1 , R 2 , and R 3 The same applies to the preferred embodiments.

[0273] The constitutional unit represented by formula (I) is preferably a constitutional unit represented by the following formula (a3).

[0274] [ka]

[0275] In formula (a3), R 1 , R 2 , and R 3 each independently represents an alkyl group, an alkenyl group, an aryl group, or an alkylenearyl group; R 4 and R 5 each independently represents a hydrogen atom or an alkyl group; R 6 represents a hydrogen atom or a monovalent substituent; L 1 represents a p+1 valent linking group, and p represents an integer of 2 to 12.

[0276] R in formula (a3) 1 , R 2 , and R 3 is R in the above formula (a1). 1 , R 2 , and R 3 The same applies to the preferred embodiments.

[0277] R 4 and R 5 Examples of the alkyl group represented by the formula (1) include linear alkyl groups having 1 to 18 carbon atoms, and branched or cyclic alkyl groups having 3 to 18 carbon atoms. Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, an isopropyl group, a tert-butyl group, and a cyclohexyl group. R 4 and R 5 Each of them is preferably a hydrogen atom.

[0278] R 6 Examples of the monovalent substituent represented by the formula (I) include an alkyl group, an alkenyl group, and an aryl group. The alkyl group, the alkenyl group, and the aryl group are each represented by the formula (I) 1 , R 2 , and R 3 The above-mentioned groups are the same as the alkyl group, alkenyl group, and aryl group represented by the following formula (1), and preferred embodiments are also the same. R 6 is preferably a hydrogen atom or a methyl group.

[0279] L 1Examples of the p+1-valent linking group represented by the formula (1) include p+1-valent hydrocarbon groups having 1 to 10 carbon atoms. As the p+1-valent linking group, a hydrocarbon group in which a part of the carbon atoms constituting the hydrocarbon group is substituted with a heteroatom is also preferably used. As the hydrocarbon group, a saturated hydrocarbon group is preferred. Here, examples of the heteroatom substituting a part of the carbon atom include a silicon atom, an oxygen atom, and a nitrogen atom, and among these, a silicon atom or an oxygen atom is preferred. L 1 The p+1 valent linking group represented by the formula (I) is preferably a branched saturated hydrocarbon group, and also preferably a branched saturated hydrocarbon group in which some of the carbon atoms constituting the branched saturated hydrocarbon group are substituted with heteroatoms (preferably silicon atoms and oxygen atoms). p is an integer of 2 to 12, and an integer of 3 to 12 is preferable.

[0280] Specific examples of the monomer unit for forming the constitutional unit represented by formula (I) include the following monomers represented by K-1 to K-12. Specific examples of the monomer unit for forming the constitutional unit represented by formula (I) are not limited thereto. In the following structures, n is an integer from 2 to 1000.

[0281] [ka]

[0282] The polymer (I) preferably further comprises a structural unit having a hydrophilic group in a side chain. The structural unit having a hydrophilic group in a side chain is preferably a structural unit having a polyalkyleneoxy group in a side chain. In other words, the polymer (I) is preferably a copolymer further comprising a structural unit having a polyalkyleneoxy group in a side chain.

[0283] The structural unit having a hydrophilic group on a side chain in the polymer (I) is preferably a structural unit represented by the following formula (a4).

[0284] [ka]

[0285] In formula (a4), R 7 and R 8 each independently represents a hydrogen atom or an alkyl group; R 9 represents a hydrogen atom or a monovalent substituent; L 2 represents -C(=O)-O- or -C(=O)-NH-; L 3 represents a single bond or a divalent linking group, and X represents a hydrophilic group.

[0286] R 7 and R 8 The alkyl group represented by the formula (a3) ​​is 4 and R 5 The preferred embodiments are also the same as those of the alkyl group represented by the following formula: R 9 is R in the above formula (a3). 6 The same applies to the monovalent substituent represented by the following formula (1), and preferred embodiments are also the same.

[0287] L 3 The divalent linking group represented by L 2 There are no particular limitations as long as it is a group that can link L and X. 3 An example of the divalent linking group represented by the formula: is an alkylene group. The alkylene group is preferably an alkylene group having 2 to 10 carbon atoms, and more preferably an alkylene group having 4 to 8 carbon atoms.

[0288] Examples of the hydrophilic group represented by X include a hydroxyl group, a phosphate group, a polyalkyleneoxy group, or a group combining two or more of these. Here, examples of the polyalkyleneoxy group include a polyethyleneoxy group, a polypropyleneoxy group, a polybutyleneoxy group, or a group combining these.

[0289] Specific examples of monomer units for forming a structural unit having a hydrophilic group on a side chain include monomers represented by H-1 to H-25. Specific examples of monomer units for forming a structural unit having a hydrophilic group on a side chain are not limited thereto. In the following structures, n and m each independently represent an integer of 2 to 100. In the structures below, the term "random" means that multiple types of polyalkyleneoxy groups are arranged randomly.

[0290] [ka]

[0291] The polymer (I) may contain one type of structural unit (b1) represented by the above formula (I) on its own, or may contain two or more types. In the polymer (I), the content of the structural unit (b1) represented by formula (I) may be 100 mass%, preferably 15 mass% to 70 mass%, more preferably 20 mass% to 60 mass%, and further preferably 25 mass% to 50 mass%, relative to the mass of the polymer (I). Furthermore, the polymer (I) may contain one type of structural unit (b2) having a hydrophilic group on the side chain, or may contain two or more types. In the polymer (I), the content of the structural unit (b2) having a hydrophilic group in a side chain is preferably 30% by mass to 85% by mass, more preferably 40% by mass to 80% by mass, and even more preferably 50% by mass to 75% by mass, relative to the mass of the polymer (I).

[0292] The polymer (I) may further contain other structural units. Other structural units include, for example, structural units having a carboxylic acid group in the side chain. For example, structural units having a carboxylic acid group in the side chain include (meth)acrylic acid, itaconic acid, itaconic acid derivatives, etc. It is preferable that the structural unit having a carboxylic acid group in the side chain is included as a structural unit other than the structural unit having the hydrophilic group in the side chain described above. Other structural units include alkyl (meth)acrylates (alkyl groups having 1 to 24 carbon atoms), styrene derivatives, maleic anhydride, maleimide anhydride, (meth)acrylonitrile, vinyl ether derivatives, and alkyl (meth)acrylamide derivatives. In the polymer (I), the content of the other structural units is preferably from 0% by mass to 20% by mass relative to the mass of the polymer (I).

[0293] The weight average molecular weight of the polymer (I) is preferably from 5,000 to 100,000, and more preferably from 8,000 to 60,000, from the viewpoint of obtaining an image recording layer with excellent surface condition.

[0294] Specific examples of the polymer (I) include the following P-1 to P-11: Specific examples of the polymer (I) are not limited to these.

[0295] [ka]

[0296] The content of the polymer (I) is preferably 0.001% by mass to 0.1% by mass, and more preferably 0.002% by mass to 0.01% by mass, based on the total mass of the coating liquid for the image recording layer.

[0297] [Oil agent] The image recording layer may further contain an oil agent. In the present disclosure, the oil agent refers to a hydrophobic compound that is in a liquid state at 80°C and is immiscible and separates when mixed with the same mass of water. When two or more oil agents are used, even if the oil agent contains a compound with a melting point of 80°C or higher, it is sufficient that the two or more oil agents are in a liquid state at 80°C when mixed together. From the viewpoints of on-press developability and suppression of turbidity of the dampening water, the oil agent is preferably a compound having a molecular weight of less than 1,000, more preferably a compound having a molecular weight of 200 to 800, and particularly preferably a compound having a molecular weight of 300 to 500. Furthermore, from the viewpoints of on-press developability and suppression of turbidity of the dampening water, the oil agent is preferably a compound having a boiling point of 200° C. or more at 1 atmospheric pressure, more preferably a compound having a boiling point of 250° C. or more at 1 atmospheric pressure, even more preferably a compound having a boiling point of 300° C. or more at 1 atmospheric pressure, and particularly preferably a compound having a boiling point of 400° C. or more and 500° C. or less at 1 atmospheric pressure. In this disclosure, unless otherwise specified, the term "boiling point" refers to the boiling point at 1 atmospheric pressure. In addition, the melting point of the oil agent at 1 atmosphere is preferably 50°C or lower, more preferably 30°C or lower, and particularly preferably from -200°C to 25°C, from the viewpoints of on-press developability and suppression of turbidity of the dampening water. In this disclosure, unless otherwise specified, the term "melting point" refers to the melting point at 1 atmosphere.

[0298] Examples of the oil agent include a phosphate ester compound, an aromatic hydrocarbon compound, a glyceride compound, a fatty acid compound, and an aromatic ester compound. Among these, from the viewpoints of UV printing durability, ink receptivity, on-press developability, and suppression of turbidity in dampening water, at least one compound selected from the group consisting of phosphate ester compounds, aromatic hydrocarbon compounds, glyceride compounds, and aromatic ester compounds is preferred, at least one compound selected from the group consisting of phosphate ester compounds, aromatic hydrocarbon compounds, and glyceride compounds is more preferred, at least one compound selected from the group consisting of phosphate ester compounds and aromatic hydrocarbon compounds is even more preferred, and a phosphate ester compound is particularly preferred.

[0299] As the phosphate ester compound, from the viewpoints of UV printing durability, ink receptivity, on-press developability, and suppression of turbidity in dampening water, a phosphate triester compound is preferred, a triaryl phosphate ester compound is more preferred, tricresyl phosphate is even more preferred, and a mixture of two or more of the three types of tricresyl phosphate, i.e., the ortho-, meta-, and para-isomers, is particularly preferred. As the aromatic hydrocarbon compound, from the viewpoints of on-press developability and suppression of turbidity of the fountain solution, a compound having two or more aromatic rings is preferred, and a compound having two or more non-condensed benzene rings is more preferred. As the glyceride compound, from the viewpoints of on-press developability and suppression of turbidity of the fountain solution, a triglyceride compound is preferable, a fatty oil is more preferable, and a fatty oil that is liquid at 25° C., such as castor oil, is particularly preferable. As the fatty acid compound, from the viewpoints of on-press developability and suppression of turbidity of the dampening water, unsaturated fatty acids are preferred, unsaturated fatty acids having 8 to 30 carbon atoms are more preferred, and unsaturated fatty acids having 12 to 24 carbon atoms are particularly preferred. As the aromatic ester compound, from the viewpoints of on-press developability and suppression of turbidity of the fountain solution, an aromatic diester compound is preferred, and an aromatic diester compound having an aliphatic ring is more preferred. As the aliphatic ester compound, from the viewpoints of on-press developability and suppression of turbidity of the fountain solution, an aliphatic ester compound having a branched alkyl group is preferable, and an aliphatic ester compound having a branched alkyl group and having 10 to 24 carbon atoms is more preferable.

[0300] From the viewpoints of UV printing durability, ink receptivity, on-press developability, and suppression of turbidity of dampening water, the oil agent preferably contains an oil agent having a phosphorus atom, and is more preferably an oil agent having a phosphorus atom. Moreover, from the viewpoints of on-press developability and suppression of turbidity of dampening water, the oil agent preferably contains an oil agent having an aromatic ring, more preferably contains an oil agent having two or more aromatic rings, and particularly preferably contains an oil agent having two or more non-condensed benzene rings.

[0301] From the viewpoints of UV printing durability, ink receptivity, on-press developability, and suppression of turbidity of dampening water, the clogP value of the oil agent is preferably 5.0 or more, more preferably 5.50 or more, even more preferably 5.50 or more and 10.0 or less, and particularly preferably 5.60 or more and 7.00 or less. The clogP value is a value obtained by calculating the common logarithm logP of the partition coefficient P between 1-octanol and water. Although publicly known methods and software can be used to calculate the clogP value, unless otherwise specified, in this disclosure, the ClogP program incorporated in Cambridge Soft's ChemBioDraw Ultra 12.0 will be used.

[0302] Specific examples of oil agents include tricresyl phosphate, dimethyl(1-phenylethyl)benzene, 2,4-diphenyl-4-methyl-1-pentene, dicyclohexyl phthalate, castor oil, α-linolenic acid, and tri(2-ethylhexyl) phosphate.

[0303] The oil agent may be used alone or in combination of two or more types. However, from the viewpoints of on-press developability and suppression of turbidity of the dampening water, it is preferable that the image recording layer contains two or more types of oil agents having different structures. The content of the oil agent is preferably 0.0001 to 10.0% by mass, more preferably 0.0002 to 1.0% by mass, further preferably 0.0005 to 0.5% by mass, and particularly preferably 0.001 to 0.05% by mass, based on the total mass of the image recording layer.

[0304] 〔particle〕 The image recording layer preferably contains particles. The particles may be organic particles or inorganic particles, but from the viewpoint of UV printing durability, it is preferable that the particles contain organic particles, and it is more preferable that the particles contain polymer particles. As the inorganic particles, known inorganic particles can be used, and metal oxide particles such as silica particles and titania particles can be suitably used.

[0305] The polymer particles are preferably selected from the group consisting of thermoplastic resin particles, thermoreactive resin particles, polymer particles having a polymerizable group, microcapsules containing a hydrophobic compound, and microgels (crosslinked polymer particles). Among them, polymer particles or microgels having a polymerizable group are preferred. In a particularly preferred embodiment, the polymer particles contain at least one ethylenically unsaturated polymerizable group. The presence of such polymer particles provides the effect of increasing the printing durability of the exposed area and the on-press developability of the unexposed area. In addition, the polymer particles are preferably thermoplastic resin particles from the viewpoints of UV printing durability and on-press developability.

[0306] Preferred examples of the thermoplastic resin particles include thermoplastic polymer particles described in Research Disclosure No. 33303 published in January 1992, JP-A Nos. 9-123387, 9-131850, 9-171249, and 9-171250, and European Patent No. 931647. Specific examples of the polymer constituting the thermoplastic resin particles include homopolymers or copolymers of monomers such as ethylene, styrene, vinyl chloride, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, vinylidene chloride, acrylonitrile, vinylcarbazole, acrylates or methacrylates having a polyalkylene structure, or mixtures thereof. Preferred examples include copolymers containing polystyrene, styrene and acrylonitrile, or polymethyl methacrylate. The average particle size of the thermoplastic resin particles is preferably 0.01 μm to 3.0 μm.

[0307] The heat-reactive resin particles include polymer particles having a heat-reactive group, which form a hydrophobic region by crosslinking through a heat reaction and by the change in functional group.

[0308] The thermally reactive group in the polymer particles having a thermally reactive group may be a functional group that undergoes any reaction as long as a chemical bond is formed, but is preferably a polymerizable group, and preferred examples thereof include ethylenically unsaturated groups that undergo radical polymerization reactions (e.g., acryloyl groups, methacryloyl groups, vinyl groups, allyl groups, etc.), cationic polymerizable groups (e.g., vinyl groups, vinyloxy groups, epoxy groups, oxetanyl groups, etc.), isocyanato groups or blocked groups thereof that undergo addition reactions, epoxy groups, vinyloxy groups, and functional groups having active hydrogen atoms that are their reaction partners (e.g., amino groups, hydroxy groups, carboxy groups, etc.), carboxy groups and their reaction partners, hydroxy groups or amino groups that undergo condensation reactions, and acid anhydrides and their reaction partners, amino groups or hydroxy groups, that undergo ring-opening addition reactions.

[0309] As the microcapsules, for example, as described in JP-A-2001-277740 and JP-A-2001-277742, at least a part of the components of the image recording layer is encapsulated in the microcapsules. The components of the image recording layer can also be contained outside the microcapsules. In a preferred embodiment, the image recording layer containing the microcapsules has a hydrophobic component encapsulated in the microcapsules and a hydrophilic component contained outside the microcapsules.

[0310] The microgel (crosslinked polymer particle) can contain a part of the components of the image recording layer on at least one of the surface or the inside thereof. In particular, a reactive microgel having a radical polymerizable group on its surface is preferred from the viewpoints of the sensitivity of the resulting lithographic printing plate precursor and the printing durability of the resulting lithographic printing plate.

[0311] The components of the image recording layer can be microencapsulated or microgelled by known methods.

[0312] From the viewpoint of the printing durability, stain resistance and storage stability of the resulting lithographic printing plate, the polymer particles are preferably those obtained by reacting a polyisocyanate compound, which is an adduct of a polyphenol compound having two or more hydroxy groups in the molecule and isophorone diisocyanate, with a compound having active hydrogen. The polyhydric phenol compound is preferably a compound having a plurality of benzene rings each having a phenolic hydroxy group. The compound having active hydrogen is preferably a polyol compound or a polyamine compound, more preferably a polyol compound, and even more preferably at least one compound selected from the group consisting of propylene glycol, glycerin, and trimethylolpropane. Preferred examples of resin particles obtained by reacting a polyisocyanate compound, which is an adduct of a polyphenol compound having two or more hydroxy groups in the molecule and isophorone diisocyanate, with a compound having active hydrogen include the polymer particles described in paragraphs 0032 to 0095 of JP2012-206495A.

[0313] Furthermore, from the viewpoint of the printing durability and solvent resistance of the resulting lithographic printing plate, it is preferable that the polymer particles have a hydrophobic main chain and contain both i) a constituent unit having a pendant cyano group directly bonded to the hydrophobic main chain, and ii) a constituent unit having a pendant group that includes a hydrophilic polyalkylene oxide segment. A preferred example of the hydrophobic main chain is an acrylic resin chain. Preferred examples of the pendant cyano group include -[CH2CH(C≡N)]- or -[CH2C(CH3)(C≡N)]-. Furthermore, the structural unit having the pendant cyano group can be easily derived from an ethylenically unsaturated monomer, such as acrylonitrile or methacrylonitrile, or a combination thereof. The alkylene oxide in the hydrophilic polyalkylene oxide segment is preferably ethylene oxide or propylene oxide, and more preferably ethylene oxide. The number of repeating alkylene oxide structures in the hydrophilic polyalkylene oxide segment is preferably 10-100, more preferably 25-75, and even more preferably 40-50. Preferred examples of resin particles having a hydrophobic main chain and including both i) a constituent unit having a pendant cyano group directly bonded to the hydrophobic main chain, and ii) a constituent unit having a pendant group containing a hydrophilic polyalkylene oxide segment include those described in paragraphs 0039 to 0068 of JP2008-503365A.

[0314] In addition, from the viewpoints of UV printing durability and on-press developability, the polymer particles preferably have a hydrophilic group. The hydrophilic group is not particularly limited as long as it has a structure having hydrophilicity, and examples of the hydrophilic group include acid groups such as a carboxy group, a hydroxy group, an amino group, a cyano group, and a polyalkylene oxide structure. Among these, from the viewpoints of on-press developability and UV printing durability, a polyalkylene oxide structure is preferred, and a polyethylene oxide structure, a polypropylene oxide structure, or a polyethylene / propylene oxide structure is more preferred. From the viewpoint of on-press developability and suppression of development residue during on-press development, the polyalkylene oxide structure preferably has a polypropylene oxide structure, and more preferably has a polyethylene oxide structure or a polypropylene oxide structure. From the viewpoints of printing durability, ink receptivity, and on-press developability, the hydrophilic group preferably contains a structural unit having a cyano group or a group represented by the following formula Z, more preferably contains a structural unit represented by the following formula (AN) or a group represented by the following formula Z, and particularly preferably contains a group represented by the following formula Z. *-QWY formula Z In formula Z, Q represents a divalent linking group, W represents a divalent group having a hydrophilic structure or a divalent group having a hydrophobic structure, Y represents a monovalent group having a hydrophilic structure or a monovalent group having a hydrophobic structure, either W or Y has a hydrophilic structure, and * represents a bonding site with another structure.

[0315] [ka]

[0316] In formula (AN), R AN represents a hydrogen atom or a methyl group.

[0317] From the viewpoint of UV printing durability, the polymer contained in the polymer particles preferably contains a structural unit formed from a compound having a cyano group. The cyano group is preferably introduced into the resin as a structural unit containing a cyano group by using a compound (monomer) having a cyano group. Examples of the compound having a cyano group include acrylonitrile compounds, and (meth)acrylonitrile is preferred. The structural unit having a cyano group is preferably a structural unit formed from an acrylonitrile compound, and more preferably a structural unit formed from (meth)acrylonitrile, that is, a structural unit represented by the above formula (AN). When the above polymer includes a polymer having a structural unit having a cyano group, the content of the structural unit having a cyano group, preferably the structural unit represented by the above formula (AN), in the polymer having a structural unit having a cyano group is, from the viewpoint of UV printing durability, preferably 5% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, and particularly preferably 30% by mass to 60% by mass, relative to the total mass of the polymer having a structural unit having a cyano group.

[0318] Moreover, from the viewpoints of printing durability, ink receptivity, and on-press developability, the polymer particles preferably contain polymer particles having a group represented by the formula Z above.

[0319] Q in the above formula Z is preferably a divalent linking group having 1 to 20 carbon atoms, and more preferably a divalent linking group having 1 to 10 carbon atoms. Furthermore, Q in the above formula Z is preferably an alkylene group, an arylene group, an ester bond, an amide bond, or a group consisting of a combination of two or more of these, and more preferably a phenylene group, an ester bond, or an amide bond.

[0320] The divalent group having a hydrophilic structure in W of the above formula Z is a polyalkyleneoxy group or a polyalkyleneoxy group having -CH2CH2NR at one end. W It is preferable that R W represents a hydrogen atom or an alkyl group. The divalent group having a hydrophobic structure in W of the above formula Z is -R WA -, -OR WA -O-, -R W NR WA -NR W -, -OC(=O)-R WA -O- or -OC(=O)-R WA It is preferable that R is —O—. WA each independently represents a linear, branched, or cyclic alkylene group having 6 to 120 carbon atoms, a haloalkylene group having 6 to 120 carbon atoms, an arylene group having 6 to 120 carbon atoms, an alkylylene group having 6 to 120 carbon atoms (a divalent group obtained by removing one hydrogen atom from an alkylaryl group), or an aralkylene group having 6 to 120 carbon atoms.

[0321] The monovalent group having a hydrophilic structure in Y of the above formula Z is -OH, -C(=O)OH, a polyalkyleneoxy group having a hydrogen atom or an alkyl group at the end, or a polyalkyleneoxy group having a hydrogen atom or an alkyl group at the other end, and -CH2CH2N(R W It is preferable that the aryl group is a group having a bond with . The monovalent group having a hydrophobic structure for Y in the above formula Z is a linear, branched or cyclic alkyl group having 6 to 120 carbon atoms, a haloalkyl group having 6 to 120 carbon atoms, an aryl group having 6 to 120 carbon atoms, an alkaryl group (alkylaryl group) having 7 to 120 carbon atoms, an aralkyl group having 7 to 120 carbon atoms, -OR WB , -C(=O)OR WB , or -OC(=O)R WB It is preferable that R WB represents an alkyl group having 6 to 20 carbon atoms.

[0322] From the viewpoints of printing durability, ink receptivity, and on-press developability, it is more preferable that in the polymer particles having a group represented by the above formula Z, W is a divalent group having a hydrophilic structure, Q is a phenylene group, an ester bond, or an amide bond, W is a polyalkyleneoxy group, and Y is a polyalkyleneoxy group whose terminal is a hydrogen atom or an alkyl group.

[0323] From the viewpoints of printing durability and on-press developability, the polymer particles preferably contain polymer particles having a polymerizable group, and more preferably contain polymer particles having a polymerizable group on the particle surface. Furthermore, from the viewpoint of printing durability, the polymer particles preferably contain polymer particles having a hydrophilic group and a polymerizable group. The polymerizable group may be a cationically polymerizable group or a radically polymerizable group, but from the viewpoint of reactivity, it is preferably a radically polymerizable group. The polymerizable group is not particularly limited as long as it is a polymerizable group, but from the viewpoint of reactivity, an ethylenically unsaturated group is preferred, a vinylphenyl group (styryl group), a (meth)acryloxy group, or a (meth)acrylamide group is more preferred, and a (meth)acryloxy group is particularly preferred. The polymer in the polymer particles having a polymerizable group preferably has a structural unit having a polymerizable group. Furthermore, polymerizable groups may be introduced onto the surfaces of the polymer particles by a polymer reaction.

[0324] In addition, from the viewpoints of UV printing durability and on-press developability, the image recording layer preferably contains, as the polymer particles, addition polymerization type resin particles having a dispersible group, and it is more preferable that the dispersible group contains a group represented by the above formula Z.

[0325] In addition, from the viewpoints of printing durability, ink receptivity, on-press developability, and suppression of development residue during on-press development, the polymer particles preferably contain a resin having a urea bond, more preferably contain a resin having a structure obtained by at least reacting an isocyanate compound represented by the following formula (Iso) with water, and particularly preferably contain a resin having a structure obtained by at least reacting an isocyanate compound represented by the following formula (Iso) with water, and having a polyethylene oxide structure and a polypropylene oxide structure as the polyoxyalkylene structure. In addition, the particles containing the resin having a urea bond are preferably microgels.

[0326] [ka]

[0327] In formula (Iso), n represents an integer of 0 to 10.

[0328] An example of the reaction between the isocyanate compound represented by the above formula (Iso) and water is the reaction shown below. Note that the following example is an example in which n=0 and the 4,4-isomer is used. As shown below, when the isocyanate compound represented by the above formula (Iso) is reacted with water, a part of the isocyanate group is hydrolyzed by the water to generate an amino group, and the generated amino group reacts with the isocyanate group to generate a urea bond, forming a dimer. The following reaction is repeated to form a resin having a urea bond. In addition, in the reaction described below, by adding a compound (a compound having active hydrogen) that is reactive with an isocyanate group, such as an alcohol compound or an amine compound, it is also possible to introduce the structure of an alcohol compound, an amine compound, or the like into a resin having a urea bond. Preferred examples of the compound having active hydrogen include those described above in relation to the microgel.

[0329] [ka]

[0330] The resin having a urea bond preferably has an ethylenically unsaturated group, and more preferably has a group represented by the following formula (PETA).

[0331] [ka]

[0332] In formula (PETA), the wavy line portion represents the bonding position to other structures.

[0333] From the viewpoints of UV printing durability and on-press developability, the image recording layer preferably contains thermoplastic resin particles. The thermoplastic resin contained in the thermoplastic resin particles is not particularly limited, and examples thereof include polyethylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polymethyl (meth)acrylate, polyethyl (meth)acrylate, polybutyl (meth)acrylate, polyacrylonitrile, polyvinyl acetate, copolymers thereof, etc. The thermoplastic resin may be in a latex state. The thermoplastic resin according to the present disclosure is preferably a resin that forms all or part of the hydrophobic film that forms the recording layer by melting or softening the thermoplastic resin due to the heat generated in the exposure process described below.

[0334] From the viewpoints of ink receptivity and UV printing durability, the thermoplastic resin preferably contains a resin A having a structural unit formed from an aromatic vinyl compound and a structural unit having a cyano group.

[0335] Resin A contained in the thermoplastic resin preferably has a structural unit formed from an aromatic vinyl compound. The aromatic vinyl compound may be any compound having a structure in which a vinyl group is bonded to an aromatic ring, and examples thereof include styrene compounds and vinylnaphthalene compounds, with styrene compounds being preferred, and styrene being more preferred. Examples of the styrene compound include styrene, p-methylstyrene, p-methoxystyrene, β-methylstyrene, p-methyl-β-methylstyrene, α-methylstyrene, and p-methoxy-β-methylstyrene, with styrene being preferred. Examples of the vinylnaphthalene compound include 1-vinylnaphthalene, methyl-1-vinylnaphthalene, β-methyl-1-vinylnaphthalene, 4-methyl-1-vinylnaphthalene, 4-methoxy-1-vinylnaphthalene, and the like, with 1-vinylnaphthalene being preferred.

[0336] Moreover, preferred examples of the structural unit formed from an aromatic vinyl compound include a structural unit represented by the following formula A1.

[0337] [ka]

[0338] In formula A1, R A1 and R A2 each independently represents a hydrogen atom or an alkyl group, Ar represents an aromatic ring group, R A3 represents a substituent, and n represents an integer of 0 or more and not exceeding the maximum number of substituents of Ar. In formula A1, R A1 and R A2 are each independently preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, more preferably a hydrogen atom or a methyl group, and further preferably all are a hydrogen atom. In formula A1, Ar is preferably a benzene ring or a naphthalene ring, and more preferably a benzene ring. In formula A1, R A3is preferably an alkyl group or an alkoxy group, more preferably an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms, and further preferably a methyl group or a methoxy group. In formula A1, R A3 If there are multiple R A3 may be the same or different from each other. In formula A1, n is preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 0.

[0339] In resin A contained in the thermoplastic resin, the content of the structural unit formed by the aromatic vinyl compound is preferably greater than the content of the structural unit having a cyano group, which will be described later, from the viewpoint of ink receptivity, and is more preferably 15% by mass to 85% by mass, and even more preferably 30% by mass to 70% by mass, relative to the total mass of the thermoplastic resin.

[0340] Resin A contained in the thermoplastic resin particles preferably contains a structural unit having a cyano group. The cyano group is preferably introduced into the resin A as a structural unit containing a cyano group by using a compound (monomer) having a cyano group. Examples of the compound having a cyano group include acrylonitrile compounds, and (meth)acrylonitrile is preferred. The structural unit having a cyano group is preferably a structural unit formed from an acrylonitrile compound, and more preferably a structural unit formed from (meth)acrylonitrile.

[0341] Furthermore, preferred examples of the structural unit formed from a compound having a cyano group include a structural unit represented by the following formula B1.

[0342] [ka]

[0343] In formula B1, R B1represents a hydrogen atom or an alkyl group. In formula B1, R B1 is preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, more preferably a hydrogen atom or a methyl group, and even more preferably a hydrogen atom.

[0344] From the viewpoint of ink receptivity, the content of the structural unit having a cyano group in Resin A is preferably less than the content of the structural unit formed by the aromatic vinyl compound, and is more preferably 55% by mass to 90% by mass, and even more preferably 60% by mass to 85% by mass, relative to the total mass of Resin A.

[0345] Furthermore, when resin A contained in the thermoplastic resin contains a structural unit formed by an aromatic vinyl compound and a structural unit having a cyano group, the content ratio of the structural unit formed by the aromatic vinyl compound and the structural unit having a cyano group (structural unit formed by the aromatic vinyl compound:structural unit having a cyano group) is preferably 5:5 to 9:1 on a mass basis, and more preferably 6:4 to 8:2.

[0346] From the viewpoints of UV printing durability and chemical resistance, it is preferable that the resin A contained in the thermoplastic resin particles further contains a structural unit formed from an N-vinyl heterocyclic compound. Examples of the N-vinyl heterocyclic compound include N-vinylpyrrolidone, N-vinylcarbazole, N-vinylpyrrole, N-vinylphenothiazine, N-vinylsuccinimide, N-vinylphthalimide, N-vinylcaprolactam, and N-vinylimidazole, and N-vinylpyrrolidone is preferred.

[0347] Furthermore, preferred examples of the constitutional unit formed by an N-vinyl heterocyclic compound include a constitutional unit represented by the following formula C1.

[0348] [ka]

[0349] In formula C1, Ar N represents a heterocyclic structure containing a nitrogen atom, and Ar N The nitrogen atom in the compound bonds to the carbon atom indicated with an *. In formula C1, Ar N The heterocyclic structure represented by the formula (I) is preferably a pyrrolidone ring, a carbazole ring, a pyrrole ring, a phenothiazine ring, a succinimide ring, a phthalimide ring, a caprolactam ring, or an imidazole ring, and more preferably a pyrrolidone ring. Also, Ar N The heterocyclic structure represented by the formula: may have a known substituent.

[0350] The content of the structural unit formed by the N-vinyl heterocyclic compound in Resin A is preferably 5% by mass to 50% by mass, and more preferably 10% by mass to 40% by mass, based on the total mass of Resin A.

[0351] Resin A contained in the thermoplastic resin particles may contain a structural unit having an acidic group, but from the viewpoint of on-press developability and ink receptivity, it preferably does not contain a structural unit having an acidic group. Specifically, the content of structural units having an acidic group in the thermoplastic resin is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less. The lower limit of the content is not particularly limited, and may be 0% by mass. The acid value of the thermoplastic resin is preferably 160 mgKOH / g or less, more preferably 80 mgKOH / g or less, and even more preferably 40 mgKOH / g or less. The lower limit of the acid value is not particularly limited, and may be 0 mgKOH / g. In the present disclosure, the acid value is determined by a measurement method in accordance with JIS K0070:1992.

[0352] From the viewpoint of ink receptivity, the resin A contained in the thermoplastic resin particles may contain a structural unit containing a hydrophobic group. Examples of the hydrophobic group include an alkyl group, an aryl group, and an aralkyl group. As the structural unit containing a hydrophobic group, a structural unit formed from an alkyl (meth)acrylate compound, an aryl (meth)acrylate compound, or an aralkyl (meth)acrylate compound is preferable, and a structural unit formed from an alkyl (meth)acrylate compound is more preferable. The number of carbon atoms in the alkyl group in the alkyl (meth)acrylate compound is preferably 1 to 10. The alkyl group may be linear or branched, or may have a cyclic structure. Examples of the alkyl (meth)acrylate compound include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and dicyclopentanyl (meth)acrylate. The number of carbon atoms of the aryl group in the aryl (meth)acrylate compound is preferably 6 to 20, and more preferably a phenyl group. The aryl group may have a known substituent. A preferred example of the aryl (meth)acrylate compound is phenyl (meth)acrylate. The number of carbon atoms of the alkyl group in the aralkyl (meth)acrylate compound is preferably 1 to 10. The alkyl group may be linear or branched, or may have a cyclic structure. The number of carbon atoms of the aryl group in the aralkyl (meth)acrylate compound is preferably 6 to 20, and more preferably a phenyl group. A preferred example of the aralkyl (meth)acrylate compound is benzyl (meth)acrylate.

[0353] The content of the structural unit having a hydrophobic group in the resin A contained in the thermoplastic resin particles is preferably 5% by mass to 50% by mass, and more preferably 10% by mass to 30% by mass, relative to the total mass of the resin A.

[0354] The thermoplastic resin contained in the thermoplastic resin particles preferably has a hydrophilic group from the viewpoints of UV printing durability and on-press developability. The hydrophilic group is not particularly limited as long as it has a structure having hydrophilicity, and examples thereof include acid groups such as a carboxy group, a hydroxy group, an amino group, a cyano group, and a polyalkylene oxide structure. From the viewpoints of UV printing durability and on-press developability, the hydrophilic group is preferably a group having a polyalkylene oxide structure, a group having a polyester structure, or a sulfonic acid group, more preferably a group having a polyalkylene oxide structure or a sulfonic acid group, and even more preferably a group having a polyalkylene oxide structure.

[0355] From the viewpoint of on-press developability, the polyalkylene oxide structure is preferably a polyethylene oxide structure, a polypropylene oxide structure, or a poly(ethylene oxide / propylene oxide) structure. From the viewpoint of on-press developability, the hydrophilic group preferably has a polypropylene oxide structure as the polyalkylene oxide structure, and more preferably has a polyethylene oxide structure or a polypropylene oxide structure. The number of alkylene oxide structures in the polyalkylene oxide structure is preferably 2 or more, more preferably 5 or more, further preferably 5 to 200, and particularly preferably 8 to 150, from the viewpoint of on-press developability.

[0356] From the viewpoint of on-press developability, the hydrophilic group is preferably a group represented by the formula Z.

[0357] From the viewpoint of improving UV printing durability, chemical resistance, and on-press developability, it is preferable that resin A contained in the thermoplastic resin particles contains a structural unit having a hydrophilic group. The hydrophilic group may be -OH, -CN, -CONR 1 R 2 , -NR 2 COR 1 (R 1 and R 2 R each independently represents a hydrogen atom, an alkyl group, an alkenyl group, or an aryl group. 1 and R2 may be bonded to form a ring. 3 R 4 , -N + R 3 R 4 R 5 X - (R 3 ~R 5 each independently represents an alkyl group having 1 to 8 carbon atoms; X - represents a counter anion), a group represented by the following formula PO, and a hydrophilic group preferably contained in the thermoplastic resin contained in the above-mentioned thermoplastic resin particles. Among these hydrophilic groups, -CONR 1 R 2 Alternatively, a group represented by the formula PO is preferred, and a group represented by the formula PO is more preferred.

[0358] [ka]

[0359] During the expression PO, L P each independently represents an alkylene group; R P represents a hydrogen atom or an alkyl group, and n represents an integer of 1 to 100. During the expression PO, L P are each independently preferably an ethylene group, a 1-methylethylene group or a 2-methylethylene group, and more preferably an ethylene group. In the formula PO, R P is preferably a hydrogen atom or an alkyl group having 1 to 18 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, even more preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and particularly preferably a hydrogen atom or a methyl group. In the formula PO, n is preferably an integer of 1 to 10, and more preferably an integer of 1 to 4.

[0360] The content of the structural unit having a hydrophilic group in the resin A is preferably from 5% by mass to 60% by mass, and more preferably from 10% by mass to 30% by mass, relative to the total mass of the resin A.

[0361] The resin A contained in the thermoplastic resin particles may further contain other structural units. The other structural units may contain structural units other than the above-mentioned structural units without any particular limitation, and examples thereof include structural units formed by an acrylamide compound, a vinyl ether compound, etc. Examples of the acrylamide compound include (meth)acrylamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-butyl(meth)acrylamide, N,N'-dimethyl(meth)acrylamide, N,N'-diethyl(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, N-hydroxypropyl(meth)acrylamide, and N-hydroxybutyl(meth)acrylamide. Examples of the vinyl ether compound include methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, n-butyl vinyl ether, tert-butyl vinyl ether, 2-ethylhexyl vinyl ether, n-nonyl vinyl ether, lauryl vinyl ether, cyclohexyl vinyl ether, cyclohexylmethyl vinyl ether, 4-methylcyclohexylmethyl vinyl ether, benzyl vinyl ether, dicyclopentenyl vinyl ether, 2-dicyclopentenoxyethyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, butoxyethyl vinyl ether, methoxyethoxyethyl vinyl ether, ethoxyethoxyethyl vinyl ether, methoxypolyethylene glycol vinyl ether, tetrahydrofurfuryl vinyl ether, 2-hydroxyethyl vinyl ether, 2-hydroxypropyl vinyl ether, 4-hydroxybutyl vinyl ether, 4-hydroxymethylcyclohexylmethyl vinyl ether, diethylene glycol monovinyl ether, polyethylene glycol vinyl ether, chloroethyl vinyl ether, chlorobutyl vinyl ether, chloroethoxyethyl vinyl ether, phenylethyl vinyl ether, and phenoxypolyethylene glycol vinyl ether.

[0362] The content of other structural units in the thermoplastic resin is preferably 5% by mass to 50% by mass, and more preferably 10% by mass to 30% by mass, based on the total mass of the thermoplastic resin.

[0363] The glass transition temperature (Tg) of the thermoplastic resin is preferably 60°C to 150°C, more preferably 80°C to 140°C, and even more preferably 90°C to 130°C, from the viewpoints of UV printing durability and ink receptivity. When the thermoplastic resin particles contain two or more types of thermoplastic resins, the value obtained by the FOX equation described below is referred to as the glass transition temperature of the thermoplastic resin.

[0364] In this disclosure, the glass transition temperature of a resin can be measured using differential scanning calorimetry (DSC). The specific measurement method is in accordance with the method described in JIS K 7121 (1987) or JIS K 6240 (2011). The glass transition temperature in this specification is the extrapolated glass transition onset temperature (hereinafter sometimes referred to as Tig). The method for measuring the glass transition temperature will now be described more specifically. When determining the glass transition temperature, the temperature is held at about 50°C lower than the expected Tg of the resin until the apparatus stabilizes, then the material is heated at a heating rate of 20°C / min to a temperature about 30°C higher than the temperature at which the glass transition ends, and a differential thermal analysis (DTA) curve or DSC curve is prepared. The extrapolated glass transition onset temperature (Tig), i.e., the glass transition temperature Tg in this specification, is determined as the temperature at the intersection of a straight line extending from the low-temperature side baseline of a DTA curve or DSC curve to the high-temperature side and a tangent drawn at the point where the gradient of the curve of the stepwise change in the glass transition is maximum.

[0365] When the thermoplastic resin particles contain two or more types of thermoplastic resins, the Tg of the thermoplastic resin contained in the thermoplastic resin particles is determined as follows. When the Tg of the first thermoplastic resin is Tg1(K), the mass fraction of the first thermoplastic resin relative to the total mass of the thermoplastic resin components in the thermoplastic resin particle is W1, the second Tg is Tg2(K), and the mass fraction of the second resin relative to the total mass of the thermoplastic resin components in the thermoplastic resin particle is W2, the Tg0(K) of the thermoplastic resin particle can be estimated according to the following FOX formula. FOX formula: 1 / Tg0=(W1 / Tg1)+(W2 / Tg2) Furthermore, when the thermoplastic resin particles contain three types of resins or when three types of thermoplastic resin particles containing different types of thermoplastic resins are contained in the pretreatment liquid, the Tg of the thermoplastic resin particles can be estimated according to the following formula, as described above, where Tg of the nth resin is Tgn(K) and the mass fraction of the nth resin relative to the total mass of the resin components in the thermoplastic resin particles is Wn. FOX formula: 1 / Tg0=(W1 / Tg1)+(W2 / Tg2)+(W3 / Tg3)...+(Wn / Tgn)

[0366] In this specification, Tg is a value measured by a differential scanning calorimetry (DSC). As the differential scanning calorimetry (DSC), for example, EXSTAR6220 manufactured by SII NanoTechnology Co., Ltd. can be used.

[0367] From the viewpoint of UV printing durability, the arithmetic mean particle size of the thermoplastic resin particles is preferably 1 nm or more and 200 nm or less, more preferably 3 nm or more and less than 80 nm, and even more preferably 10 nm or more and 49 nm or less.

[0368] The arithmetic mean particle size of the thermoplastic resin particles in the present disclosure refers to a value measured by dynamic light scattering (DLS) unless otherwise specified. The arithmetic mean particle size of the thermoplastic resin particles by DLS is measured using Brookhaven BI-90 (manufactured by Brookhaven Instrument Company) according to the manual of the above instrument.

[0369] The weight average molecular weight of the thermoplastic resin contained in the thermoplastic resin particles is preferably 3,000 to 300,000, and more preferably 5,000 to 100,000.

[0370] The method for producing the thermoplastic resin contained in the thermoplastic resin particles is not particularly limited, and the thermoplastic resin can be produced by a known method. For example, it can be obtained by polymerizing a styrene compound, an acrylonitrile compound, and, if necessary, at least one compound selected from the group consisting of the N-vinyl heterocyclic compound, the compound used to form the structural unit having an ethylenically unsaturated group, the compound used to form the structural unit having an acidic group, the compound used to form the structural unit having a hydrophobic group, and the compound used to form the other structural units, by a known method.

[0371] Specific examples of the thermoplastic resin contained in the thermoplastic resin particles are shown in the table below, but the thermoplastic resin used in the present disclosure is not limited to these.

[0372] [ka]

[0373] [ka]

[0374] In the above specific examples, the content ratio of each structural unit can be appropriately changed in accordance with the preferred range of the content of each structural unit described above. The weight average molecular weight of each of the specific compounds can be appropriately changed in accordance with the preferred range of the weight average molecular weight of the thermoplastic resin described above.

[0375] The average particle size of the above particles is preferably 0.01 μm to 3.0 μm, more preferably 0.03 μm to 2.0 μm, and even more preferably 0.10 μm to 1.0 μm. Within this range, good resolution and stability over time can be obtained. The average primary particle size of the above particles in this disclosure is measured by a light scattering method, or by taking an electron microscope photograph of the particles, measuring the particle sizes of 5,000 particles in total on the photograph, and calculating the average value. Note that for non-spherical particles, the particle size is the particle size value of a spherical particle having the same particle area as the particle area on the photograph. In addition, the average particle size in this disclosure is taken to be the volume average particle size unless otherwise specified.

[0376] The image recording layer may contain one type of particles, particularly polymer particles, or may contain two or more types. Furthermore, from the viewpoints of on-press developability and UV printing durability, the content of particles, particularly polymer particles, in the image recording layer is preferably 5% by mass to 90% by mass, more preferably 10% by mass to 90% by mass, even more preferably 20% by mass to 90% by mass, and particularly preferably 50% by mass to 90% by mass, relative to the total mass of the image recording layer. From the viewpoints of on-press developability and UV printing durability, the content of the polymer particles in the image recording layer is preferably 20% by mass to 100% by mass, more preferably 35% by mass to 100% by mass, even more preferably 50% by mass to 100% by mass, and particularly preferably 80% by mass to 100% by mass, relative to the total mass of components of the image recording layer having a molecular weight of 3,000 or more.

[0377] -Binder polymer- The image recording layer may contain a binder polymer. As the binder polymer, a binder polymer used in the image recording layer of the on-machine development type lithographic printing plate precursor can be used. Specifically, as the binder polymer, the binder polymers described in paragraphs 0288 to 0317 of WO 2022 / 019217 can be suitably used.

[0378] In the image recording layer used in the present disclosure, the binder polymer may be used alone or in combination of two or more kinds. The binder polymer can be contained in any amount in the image recording layer, but the content of the binder polymer is preferably 1% by mass to 90% by mass, and more preferably 5% by mass to 80% by mass, relative to the total mass of the image recording layer. Furthermore, when the image recording layer in the present disclosure contains another binder polymer, the content of the other binder polymer relative to the total mass of the thermoplastic resin particles and the other binder polymer is preferably more than 0 mass% and not more than 99 mass%, more preferably 20 mass% to 95 mass%, and even more preferably 40 mass% to 90 mass%.

[0379] [Color former] The image recording layer preferably contains a color former, and more preferably contains an acid color former. The term "color former" as used in the present disclosure means a compound that has the property of developing or decoloring in response to a stimulus such as light or acid, thereby changing the color of the image recording layer, and the term "acid color former" means a compound that has the property of developing or decoloring in response to heating while accepting an electron-accepting compound (e.g., a proton such as an acid), thereby changing the color of the image recording layer. As the acid color former, in particular, a colorless compound having a partial skeleton such as lactone, lactam, sultone, spiropyran, ester, amide, or the like, which quickly opens or cleaves the partial skeleton when it comes into contact with an electron-accepting compound, is preferred.

[0380] Examples of such acid color formers include 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophthalide (also called "crystal violet lactone"), 3,3-bis(4-dimethylaminophenyl)phthalide, 3-(4-dimethylaminophenyl)-3-(4-diethylamino-2-methylphenyl)-6-dimethylaminophthalide, 3-(4-dimethylaminophenyl)-3-(1,2-dimethylindol-3-yl)phthalide, 3-(4-dimethylaminophenyl)-3-(2-methylphenyl)phthalide, and 3-(4-dimethylaminophenyl)-3-(1,2-dimethylindol-3-yl)phthalide. 3,3-bis(1,2-dimethylindol-3-yl)-5-dimethylaminophthalide, 3,3-bis(1,2-dimethylindol-3-yl)-6-dimethylaminophthalide, 3,3-bis(9-ethylcarbazol-3-yl)-6-dimethylaminophthalide, 3,3-bis(2-phenylindol-3-yl)-6-dimethylaminophthalide, 3-(4-dimethylaminophenyl)-3-(1-methylpyrrol-3-yl)-6-dimethylaminophthalide,

[0381] 3,3-bis[1,1-bis(4-dimethylaminophenyl)ethylene-2-yl]-4,5,6,7-tetrachlorophthalide, 3,3-bis[1,1-bis(4-pyrrolidinophenyl)ethylene-2-yl]-4,5,6,7-tetrabromophthalide, 3,3-bis[1-(4-dimethylaminophenyl)-1-(4-methoxyphenyl)ethylene-2-yl]-4,5,6,7-tetrachlorophthalide, 3,3-bis[1-(4-pyrrolidinophenyl)-1-(4-methoxyphenyl)ethylene-2-yl]-4,5,6,7-tetrachlorophthalide, 3-[1,1-di(1-ethyl-2-methylin phthalides such as 3-[1,1-di(1-ethyl-2-methylindol-3-yl)ethylene-2-yl]-3-(4-diethylaminophenyl)phthalide, 3-[1,1-di(1-ethyl-2-methylindol-3-yl)ethylene-2-yl]-3-(4-N-ethyl-N-phenylaminophenyl)phthalide, 3-(2-ethoxy-4-diethylaminophenyl)-3-(1-n-octyl-2-methylindol-3-yl)phthalide, 3,3-bis(1-n-octyl-2-methylindol-3-yl)phthalide, and 3-(2-methyl-4-diethylaminophenyl)-3-(1-n-octyl-2-methylindol-3-yl)phthalide;

[0382] 4,4-Bis-dimethylaminobenzhydrin benzyl ether, N-halophenyl-leucoauramine, N-2,4,5-trichlorophenylleucoauramine, rhodamine-B-anilinolactam, rhodamine-(4-nitroanilino)lactam, rhodamine-B-(4-chloroanilino)lactam, 3,7-bis(diethylamino)-10-benzoylphenoxazine, benzoylleuco methylene blue, 4-nitrobenzoyl methylene blue,

[0383] 3,6-dimethoxyfluoran, 3-dimethylamino-7-methoxyfluoran, 3-diethylamino-6-methoxyfluoran, 3-diethylamino-7-methoxyfluoran, 3-diethylamino-7-chlorofluoran, 3-diethylamino-6-methyl-7-chlorofluoran, 3-diethylamino-6,7-dimethylfluoran, 3-N-cyclohexyl-Nn-butylamino-7-methylfluoran, 3-diethylamino-7-dibenzylaminofluoran, 3-diethylamino-7-octylaminofluoran, 3-diethylamino-7-di-n-hexylaminofluoran, 3-diethylamino-7-anilinofluoran, 3- Diethylamino-7-(2'-fluorophenylamino)fluoran, 3-diethylamino-7-(2'-chlorophenylamino)fluoran, 3-diethylamino-7-(3'-chlorophenylamino)fluoran, 3-diethylamino-7-(2',3'-dichlorophenylamino)fluoran, 3-diethylamino-7-(3'-trifluoromethylphenylamino)fluoran, 3-di-n-butylamino-7-(2'-fluorophenylamino)fluoran, 3-di-n-butylamino-7-(2'-chlorophenylamino)fluoran, 3-N-isopentyl-N-ethylamino-7-(2'-chlorophenylamino)fluoran,

[0384] 3-Nn-hexyl-N-ethylamino-7-(2'-chlorophenylamino)fluoran, 3-diethylamino-6-chloro-7-anilinofluoran, 3-di-n-butylamino-6-chloro-7-anilinofluoran, 3-diethylamino-6-methoxy-7-anilinofluoran, 3-di-n-butylamino-6-ethoxy-7-anilinofluoran, 3-pyrrolidino-6-methyl-7-anilinofluoran, 3-piperidino-6-methyl-7-anilinofluoran, 3-morpholino- 6-Methyl-7-anilinofluoran, 3-dimethylamino-6-methyl-7-anilinofluoran, 3-diethylamino-6-methyl-7-anilinofluoran, 3-di-n-butylamino-6-methyl-7-anilinofluoran, 3-di-n-pentylamino-6-methyl-7-anilinofluoran, 3-N-ethyl-N-methylamino-6-methyl-7-anilinofluoran, 3-Nn-propyl-N-methylamino-6-methyl-7-anilinofluoran, 3-Nn-propyl-N-ethyl N-butyl-N-methylamino-6-methyl-7-anilinofluoran, 3-N-butyl-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-isobutyl-N-methylamino-6-methyl-7-anilinofluoran, 3-N-isobutyl-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-isopentyl-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-hexyl-N-methylamino amino-6-methyl-7-anilinofluoran, 3-N-cyclohexyl-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-cyclohexyl-Nn-propylamino-6-methyl-7-anilinofluoran, 3-N-cyclohexyl-Nn-butylamino-6-methyl-7-anilinofluoran, 3-N-cyclohexyl-Nn-hexylamino-6-methyl-7-anilinofluoran, 3-N-cyclohexyl-Nn-octylamino-6-methyl-7-anilinofluoran,

[0385] 3-N-(2'-methoxyethyl)-N-methylamino-6-methyl-7-anilinofluoran, 3-N-(2'-methoxyethyl)-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-(2'-methoxyethyl)-N-isobutylamino-6-methyl-7-anilinofluoran, 3-N-(2'-ethoxyethyl)-N-methylamino-6-methyl-7-anilinofluoran, 3-N-(2'-ethoxyethyl)-N-ethylamino-6-methyl-7 -Anilinofluoran, 3-N-(3'-methoxypropyl)-N-methylamino-6-methyl-7-anilinofluoran, 3-N-(3'-methoxypropyl)-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-(3'-ethoxypropyl)-N-methylamino-6-methyl-7-anilinofluoran, 3-N-(3'-ethoxypropyl)-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-(3'-ethoxypropyl)-N-ethylamino-6-methyl-7-anilinofluoran, 3-N-(2'-tetrahydrofurfuryl)- N-ethylamino-6-methyl-7-anilinofluoran, 3-N-(4'-methylphenyl)-N-ethylamino-6-methyl-7-anilinofluoran, 3-diethylamino-6-ethyl-7-anilinofluoran, 3-diethylamino-6-methyl-7-(3'-methylphenylamino)fluoran, 3-diethylamino-6-methyl-7-(2',6'-dimethylphenylamino)fluoran, 3-di-n-butylamino-6-methyl-7-(2',6'-dimethylphenylamino)fluoran, fluorans such as 3-di-n-butylamino-7-(2',6'-dimethylphenylamino)fluoran, 3-di-n-butylamino-7-(2',6'-dimethylphenylamino)fluoran, 2,2-bis[4'-(3-N-cyclohexyl-N-methylamino-6-methylfluoran)-7-ylaminophenyl]propane, 3-[4'-(4-phenylaminophenyl)aminophenyl]amino-6-methyl-7-chlorofluoran, and 3-[4'-(dimethylaminophenyl)]amino-5,7-dimethylfluoran;

[0386] 3-(2-methyl-4-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(2-n-propoxycarbonylamino-4-di-n-propylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(2-methylamino-4-di-n-propylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(2-methyl-4-di-n-hexylaminophenyl)-3-(1-n-octyl 3-(2-ethoxy-4-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3,3-bis(2-ethoxy-4-diethylaminophenyl)-4-azaphthalide, 3,3-bis(1-n-octyl-2-methylindol-3-yl)-4-azaphthalide, 3-(2-ethoxy-4-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(2-ethoxy-4-diethylaminophenyl)-3-(1-octyl-2-methylindol-3-yl)-4 or 7-azaphthalide, 3-( 2-ethoxy-4-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4 or 7-azaphthalide, 3-(2-hexyloxy-4-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)-4 or 7-azaphthalide, 3-(2-ethoxy-4-diethylaminophenyl)-3-(1-ethyl-2-phenylindol-3-yl)-4 or 7-azaphthalide, 3-(2-butoxy-4-diethylaminophenyl)-3-(1-ethyl-2-phenylindol-3 -yl)-4 or 7-azaphthalide 3-methyl-spiro-dinaphthopyran, 3-ethyl-spiro-dinaphthopyran, 3-phenyl-spiro-dinaphthopyran, 3-benzyl-spiro-dinaphthopyran, 3-methyl-naphtho-(3-methoxybenzo)spiropyran, 3-propyl-spiro-dibenzopyran-3,6-bis(dimethylamino)fluorene-9-spiro-3'-(6'-dimethylamino)phthalide, 3,6-bis(diethylamino)fluorene-9-spiro-3'-(6'-dimethylamino)phthalide and other phthalides;

[0387] Other examples include 2'-anilino-6'-(N-ethyl-N-isopentyl)amino-3'-methylspiro[isobenzofuran-1(3H),9'-(9H)xanthene-3-one, 2'-anilino-6'-(N-ethyl-N-(4-methylphenyl))amino-3'-methylspiro[isobenzofuran-1(3H),9'-(9H)xanthene]-3-one, 3'-N,N-dibenzylamino-6'-N,N-diethylaminospiro[isobenzofuran-1(3H),9'-(9H)xanthene]-3-one, and 2'-(N-methyl-N-phenyl)amino-6'-(N-ethyl-N-(4-methylphenyl))aminospiro[isobenzofuran-1(3H),9'-(9H)xanthene]-3-one.

[0388] Among these, from the viewpoint of color development, the color former used in the present disclosure is preferably at least one compound selected from the group consisting of spiropyran compounds, spirooxazine compounds, spirolactone compounds, and spirolactam compounds. From the viewpoint of visibility, the hue of the dye after color development is preferably green, blue or black.

[0389] In addition, the acid color former is preferably a leuco dye from the viewpoints of color development and visibility of exposed areas. However, the leuco dye does not include the compounds represented by the above-mentioned formula (1) and formula (2). In other words, the image recording layer in the on-press development type lithographic printing plate precursor according to the present disclosure may use other leuco dyes that do not fall under the compounds represented by the following formula (1) and formula (2). The leuco dye is not particularly limited as long as it has a leuco structure, but it preferably has a spiro structure, and more preferably has a spirolactone ring structure. From the viewpoints of color development and visibility of exposed areas, the leuco dye is preferably a leuco dye having a phthalide structure or a fluoran structure. Furthermore, from the viewpoints of color development and visibility of exposed areas, the leuco dye having the above-mentioned phthalide structure or fluoran structure is preferably a compound represented by any one of the following formulas (Le-1) to (Le-3), and more preferably a compound represented by the following formula (Le-2).

[0390] [ka]

[0391] In formulae (Le-1) to (Le-3), ERG each independently represents an electron donating group, X1 to X4 each independently represent a hydrogen atom, a halogen atom or a dialkylanilino group, X5 to X 10 each independently represents a hydrogen atom, a halogen atom, or a monovalent organic group; Y1 and Y2 each independently represent C or N; when Y1 is N, X1 is not present; and when Y2 is N, X4 is not present; Ra1 represents a hydrogen atom, an alkyl group, or an alkoxy group; and Rb1 to Rb4 each independently represent a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group.

[0392] The electron-donating group in ERG of formulae (Le-1) to (Le-3) is preferably an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, an alkoxy group, an aryloxy group, a heteroaryloxy group, or an alkyl group, more preferably an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, an alkoxy group, or an aryloxy group, further preferably a monoalkylmonoarylamino group, a diarylamino group, a diheteroarylamino group, or a monoarylmonoheteroarylamino group, and particularly preferably a monoalkylmonoarylamino group. In addition, from the viewpoints of color development and visibility of exposed areas, the electron-donating group in the above ERG is preferably a di-substituted amino group having an aryl group having a substituent at at least one ortho position or a heteroaryl group having a substituent at at least one ortho position, more preferably a di-substituted amino group having a phenyl group having a substituent at at least one ortho position and an electron-donating group at the para position, still more preferably an amino group having a phenyl group having a substituent at at least one ortho position and an electron-donating group at the para position, and an aryl group or a heteroaryl group, and particularly preferably an amino group having a phenyl group having a substituent at at least one ortho position and an electron-donating group at the para position, and an aryl group having an electron-donating group or a heteroaryl group having an electron-donating group. In the present disclosure, the ortho position in an aryl group or heteroaryl group other than a phenyl group refers to the bonding position adjacent to the bonding position 1 (e.g., the 2nd position, etc.) when the bonding position of the aryl group or heteroaryl group to another structure is defined as the 1st position.

[0046] Furthermore, from the viewpoints of color development and visibility of exposed areas, the electron-donating group contained in the aryl group or heteroaryl group is preferably an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, an alkoxy group, an aryloxy group, a heteroaryloxy group, or an alkyl group, more preferably an alkoxy group, an aryloxy group, a heteroaryloxy group, or an alkyl group, and particularly preferably an alkoxy group.

[0393] In formulae (Le-1) to (Le-3), X1 to X4 each independently represent preferably a hydrogen atom or a chlorine atom, and more preferably a hydrogen atom, from the viewpoints of color development and visibility of exposed areas. X5 to X in formula (Le-2) or formula (Le-3) 10 are each independently, from the viewpoints of color development and visibility of the exposed area, preferably a hydrogen atom, a halogen atom, an alkyl group, an aryl group, an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, a hydroxy group, an alkoxy group, an aryloxy group, a heteroaryloxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, a heteroaryloxycarbonyl group, or a cyano group, more preferably a hydrogen atom, a halogen atom, an alkyl group, an aryl group, an alkoxy group, or an aryloxy group, further preferably a hydrogen atom, a halogen atom, an alkyl group, or an aryl group, and particularly preferably a hydrogen atom. In the formulae (Le-1) to (Le-3), from the viewpoints of color development and visibility of exposed areas, at least one of Y1 and Y2 is preferably C, and it is more preferable that both Y1 and Y2 are C. From the viewpoints of color development and visibility of exposed areas, Ra1 in formulae (Le-1) to (Le-3) is preferably an alkyl group or an alkoxy group, more preferably an alkoxy group, and particularly preferably a methoxy group. In formulae (Le-1) to (Le-3), Rb1 to Rb4 each independently represent, from the viewpoints of color development and visibility of exposed areas, preferably a hydrogen atom or an alkyl group, more preferably an alkyl group, and particularly preferably a methyl group.

[0394] From the viewpoints of color development and visibility of exposed areas, the leuco dye having a phthalide structure or a fluoran structure is more preferably a compound represented by any one of the following formulas (Le-4) to (Le-6), and even more preferably a compound represented by the following formula (Le-5).

[0395] [ka]

[0396] In formulae (Le-4) to (Le-6), ERG each independently represents an electron donating group, X1 to X4 each independently represent a hydrogen atom, a halogen atom, or a dialkylanilino group, Y1 and Y2 each independently represent C or N, and when Y1 is N, X1 does not exist, and when Y2 is N, X4 does not exist, Ra1 represents a hydrogen atom, an alkyl group, or an alkoxy group, and Rb1 to Rb4 each independently represent a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group.

[0397] In formulae (Le-4) to (Le-6), ERG, X1 to X4, Y1, Y2, Ra1, and Rb1 to Rb4 have the same meanings as ERG, X1 to X4, Y1, Y2, Ra1, and Rb1 to Rb4 in formulae (Le-1) to (Le-3), respectively, and preferred embodiments are also the same.

[0398] Furthermore, from the viewpoints of color development and visibility of exposed areas, the leuco dye having the phthalide structure or the fluoran structure is more preferably a compound represented by any one of the following formulas (Le-7) to (Le-9), and particularly preferably a compound represented by the following formula (Le-8).

[0399] [ka]

[0400] In formulae (Le-7) to (Le-9), X1 to X4 each independently represent a hydrogen atom, a halogen atom, or a dialkylanilino group; Y1 and Y2 each independently represent C or N; when Y1 is N, X1 does not exist; when Y2 is N, X4 does not exist; Ra1 to Ra4 each independently represent a hydrogen atom, an alkyl group, or an alkoxy group; Rb1 to Rb4 each independently represent a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group; and Rc1 and Rc2 each independently represent an aryl group or a heteroaryl group.

[0401] X1 to X4, Y1 and Y2 in formulae (Le-7) to (Le-9) have the same meanings as X1 to X4, Y1 and Y2 in formulae (Le-1) to (Le-3), and preferred embodiments are also the same. In formula (Le-7) or formula (Le-9), Ra1 to Ra4 are each independently preferably an alkyl group or an alkoxy group, more preferably an alkoxy group, and particularly preferably a methoxy group, from the viewpoints of color development and visibility of the exposed area. In formulae (Le-7) to (Le-9), Rb1 to Rb4 each independently represent, from the viewpoints of color development and visibility of the exposed area, preferably a hydrogen atom, an alkyl group, or an aryl group substituted with an alkoxy group, more preferably an alkyl group, and particularly preferably a methyl group. In formula (Le-8), Rc1 and Rc2 each independently represent, from the viewpoints of color development and visibility of exposed areas, preferably a phenyl group or an alkylphenyl group, and more preferably a phenyl group. In addition, in terms of color development and visibility of exposed areas, Rc1 and Rc2 in formula (Le-8) are each preferably an aryl group having a substituent at at least one ortho position, or a heteroaryl group having a substituent at at least one ortho position, more preferably an aryl group having a substituent at at least one ortho position, even more preferably a phenyl group having a substituent at at least one ortho position, and particularly preferably a phenyl group having a substituent at at least one ortho position and an electron-donating group at the para position. Examples of the substituents in Rc1 and Rc2 include the substituents described below. In formula (Le-8), from the viewpoints of color development and visibility of exposed areas, it is preferable that X1 to X4 are hydrogen atoms, and Y1 and Y2 are C. Furthermore, in formula (Le-8), from the viewpoints of color development and visibility of exposed areas, it is preferred that Rb1 and Rb2 each independently represent an aryl group substituted with an alkyl group or an alkoxy group. Furthermore, in formula (Le-8), from the viewpoints of color development and visibility of the exposed area, it is preferable that Rb1 and Rb2 are each independently an aryl group or a heteroaryl group, more preferably an aryl group, still more preferably an aryl group having an electron-donating group, and particularly preferably a phenyl group having an electron-donating group at the para position. In addition, from the viewpoints of color development and visibility of the exposed area, the electron-donating group in Rb1, Rb2, Rc1, and Rc2 is preferably an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, an alkoxy group, an aryloxy group, a heteroaryloxy group, or an alkyl group, more preferably an alkoxy group, an aryloxy group, a heteroaryloxy group, or an alkyl group, and particularly preferably an alkoxy group.

[0402] In addition, from the viewpoints of color development and visibility of exposed areas, it is also preferable that the acid color former contains one or more compounds selected from the group consisting of compounds represented by the following formula (Le-10) and compounds represented by the following formula (Z-4). In other words, it is preferable that the image recording layer in the lithographic printing plate precursor according to the present disclosure further contains one or more compounds selected from the group consisting of compounds represented by the following formula (Le-10) and compounds represented by the following formula (Z-4):

[0403] [ka]

[0404] In formula (Le-10), each Ar1 independently represents an aryl group or a heteroaryl group, and each Ar2 independently represents an aryl group having a substituent at at least one ortho position, or a heteroaryl group having a substituent at at least one ortho position.

[0405] Ar1 in formula (Le-10) has the same meaning as Rb1 and Rb2 in formulae (Le-7) to (Le-9), and preferred embodiments are also the same. Ar2 in formula (Le-10) has the same meaning as Rc1 and Rc2 in formulae (Le-7) to (Le-9), and preferred embodiments are also the same.

[0406] The alkyl group in the formulae (Le-1) to (Le-9) may be linear, branched, or have a ring structure. In addition, the alkyl group in formulae (Le-1) to (Le-9) preferably has 1 to 20 carbon atoms, more preferably 1 to 8 carbon atoms, further preferably 1 to 4 carbon atoms, and particularly preferably 1 or 2 carbon atoms. The aryl group in formulae (Le-1) to (Le-10) preferably has 6 to 20 carbon atoms, more preferably 6 to 10 carbon atoms, and particularly preferably 6 to 8 carbon atoms. Specific examples of the aryl group in the formulae (Le-1) to (Le-10) include a phenyl group, a naphthyl group, an anthracenyl group, and a phenanthrenyl group, each of which may have a substituent. Specific examples of the heteroaryl group in the formulae (Le-1) to (Le-10) include a furyl group, a pyridyl group, a pyrimidyl group, a pyrazoyl group, and a thiophenyl group, each of which may have a substituent.

[0407] In addition, each group such as a monovalent organic group, an alkyl group, an aryl group, a heteroaryl group, a dialkylanilino group, an alkylamino group, and an alkoxy group in the formulae (Le-1) to (Le-10) may have a substituent. Examples of the substituent include an alkyl group, an aryl group, a heteroaryl group, a halogen atom, an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, a hydroxy group, an alkoxy group, an aryloxy group, a heteroaryloxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, a heteroaryloxycarbonyl group, and a cyano group. In addition, these substituents may be further substituted with these substituents.

[0408] [ka]

[0409] In formula (Z-4), Rza1 represents a hydrogen atom, an alkyl group, or an alkoxy group; Rzb1 to Rb4 each independently represent a hydrogen atom, an alkyl group, or an aryl group; Rzb1 and Rzb2, and Rzb3 and Rzb4 may be linked to form a ring structure; X represents O or NR; R represents a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group; and Y1 and Y2 each independently represent CH or N.

[0410] In the formula (Z-4), Rza1 is preferably an alkyl group or an alkoxy group. It is preferable that Rzb1 and Rzb2 in formula (Z-4) each independently represent an alkyl group. In formula (Z-4), Rzb3 and Rzb4 each independently represent a hydrogen atom, an alkyl group, or an aryl group, and it is preferable that one of them is an aryl group. In formula (Z-4), it is preferable that X is O, and Y1 and Y2 are CH.

[0411] The alkyl group in formula (Z-4) may be linear, branched, or have a ring structure. The alkyl group in formula (Z-4) preferably has 1 to 20 carbon atoms, more preferably 1 to 8 carbon atoms, and even more preferably 1 to 5 carbon atoms. The aryl group in formula (Z-4) preferably has 6 to 20 carbon atoms, more preferably 6 to 10 carbon atoms, and particularly preferably 6 to 8 carbon atoms. Each group such as an alkyl group and an aryl group in formula (Z-4) may have a substituent. Examples of the substituent include an alkyl group, an aryl group, a halogen atom, an amino group, an alkylamino group, an arylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a diarylamino group, a hydroxy group, an alkoxy group, an aryloxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, and a cyano group. These substituents may be further substituted with these substituents.

[0412] Suitable leuco dyes having a phthalide structure or a fluoran structure include the following compounds, where Me represents a methyl group.

[0413] [ka]

[0414] [ka]

[0415]

change

[0416]

change

[0417]

change

[0418]

change

[0419]

change

[0420]

change

[0421] As the color developer, commercially available products can be used, such as ETAC, RED500, RED520, CVL, S-205, BLACK305, BLACK400, BLACK100, BLACK500, H-7001, GREEN300, NIRBLACK78, BLUE220, H-3035, BLUE203, ATP, H-1046, H-2114 (all manufactured by Fukui Yamada Chemical Co., Ltd.), ORANGE-DCF, and Vermilio. Examples of such dyes include n-DCF, PINK-DCF, RED-DCF, BLMB, CVL, GREEN-DCF, TH-107 (all manufactured by Hodogaya Chemical Co., Ltd.), ODB, ODB-2, ODB-4, ODB-250, ODB-BlackXV, Blue-63, Blue-502, GN-169, GN-2, Green-118, Red-40, Red-8 (all manufactured by Yamamoto Chemical Industry Co., Ltd.), and crystal violet lactone (manufactured by Tokyo Chemical Industry Co., Ltd.). Among these commercially available products, ETAC, S-205, BLACK305, BLACK400, BLACK100, BLACK500, H-7001, GREEN300, NIRBLACK78, H-3035, ATP, H-1046, H-2114, GREEN-DCF, Blue-63, GN-169, and crystal violet lactone are preferred because the films formed have good visible light absorptance.

[0422] These color formers may be used alone or in combination of two or more kinds. The content of the color former is preferably from 0.5% by mass to 10% by mass, and more preferably from 1% by mass to 5% by mass, based on the total mass of the image recording layer.

[0423] [Chain transfer agent] The image recording layer may contain a chain transfer agent. As the chain transfer agent, a chain transfer agent used in the image recording layer of the on-machine development type lithographic printing plate precursor can be used. Specifically, as the chain transfer agent, the chain transfer agents described in paragraphs 0388 to 0393 of WO2022 / 019217 can be suitably used.

[0424] The chain transfer agent may be added alone or in combination of two or more kinds. The content of the chain transfer agent is preferably from 0.01% by mass to 50% by mass, more preferably from 0.05% by mass to 40% by mass, and even more preferably from 0.1% by mass to 30% by mass, based on the total mass of the image recording layer.

[0425] [Oil Sensitizer] The image recording layer may contain an oil sensitizer to improve ink receptivity. As the oil sensitizer, an oil sensitizer used in the image recording layer of the on-press development type lithographic printing plate precursor can be used. Specifically, as the oil sensitizer, the oil sensitizers described in paragraphs 0395 to 0404 of WO 2022 / 019217 can be suitably used.

[0426] The content of the oil sensitizer is preferably from 1 to 40.0% by mass, more preferably from 2 to 25.0% by mass, and even more preferably from 3 to 20.0% by mass, based on the total mass of the image recording layer.

[0427] The image recording layer may contain one type of oil sensitizer alone, or two or more types may be used in combination. One of the preferred embodiments of the image recording layer used in the present disclosure is an embodiment containing two or more compounds as oil sensitizers. Specifically, from the viewpoint of achieving both on-press developability and ink receptivity, the image recording layer used in the present disclosure preferably uses, as the oil sensitizer, a phosphonium compound, a nitrogen-containing low molecular weight compound, and an ammonium group-containing polymer in combination, and more preferably uses a phosphonium compound, a quaternary ammonium salt, and an ammonium group-containing polymer in combination.

[0428] [Development Accelerator] The image recording layer used in the present disclosure preferably further comprises a development accelerator. The development accelerator preferably has a polarity term SP value of 6.0 to 26.0, more preferably 6.2 to 24.0, further preferably 6.3 to 23.5, and particularly preferably 6.4 to 22.0.

[0429] The SP value in this disclosure (solubility parameter, unit: (cal / cm 3 ) 1 / 2 The value of the polar term in (3) is the value of the polar term δp in the Hansen solubility parameter. The Hansen solubility parameter is a solubility parameter introduced by Hildebrand that is divided into three components, the dispersion term δd, the polar term δp, and the hydrogen bond term δh, and is expressed in a three-dimensional space. In this disclosure, the polar term δp is used. δp[cal / cm 3 ] is the Hansen solubility parameter dipole-dipole term, V[cal / cm 3 ] is the molar volume, μ[D] is the dipole moment. For δp, the following formula simplified by Hansen and Beerbower is generally used:

[0430]

number

[0431] The development accelerator is preferably a hydrophilic high molecular weight compound or a hydrophilic low molecular weight compound. In the present disclosure, "hydrophilic" refers to a value of the polar term of the SP value being 6.0 to 26.0, "hydrophilic polymer compound" refers to a compound having a molecular weight (weight average molecular weight if the molecular weight distribution is present) of 3,000 or more, and "hydrophilic low molecular weight compound" refers to a compound having a molecular weight (weight average molecular weight if the molecular weight distribution is present) of less than 3,000.

[0432] Examples of the hydrophilic polymer compound include cellulose compounds, and the like, with cellulose compounds being preferred. The cellulose compound includes cellulose and a compound in which cellulose is at least partially modified (modified cellulose compound), and the modified cellulose compound is preferred. Preferred examples of modified cellulose compounds include compounds in which at least a portion of the hydroxy groups of cellulose are substituted with at least one group selected from the group consisting of alkyl groups and hydroxyalkyl groups. The degree of substitution of the compound in which at least a portion of the hydroxy groups of the cellulose is substituted with at least one group selected from the group consisting of alkyl groups and hydroxyalkyl groups is preferably 0.1 to 6.0, and more preferably 1 to 4. The modified cellulose compound is preferably an alkyl cellulose compound or a hydroxyalkyl cellulose compound, more preferably a hydroxyalkyl cellulose compound. A preferred example of the alkyl cellulose compound is methyl cellulose. A preferred example of the hydroxyalkyl cellulose compound is hydroxypropyl cellulose.

[0433] The molecular weight of the hydrophilic polymer compound (weight average molecular weight when the compound has a molecular weight distribution) is preferably from 3,000 to 5,000,000, and more preferably from 5,000 to 200,000.

[0434] Examples of the hydrophilic low molecular weight compound include glycol compounds, polyol compounds, organic amine compounds, organic sulfonic acid compounds, organic sulfamine compounds, organic sulfuric acid compounds, organic phosphonic acid compounds, organic carboxylic acid compounds, and betaine compounds, and polyol compounds, organic sulfonic acid compounds, and betaine compounds are preferred.

[0435] Examples of the glycol compound include glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, and tripropylene glycol, and ether or ester derivatives of these compounds. Examples of the polyol compound include glycerin, pentaerythritol, and tris(2-hydroxyethyl)isocyanurate. The organic amine compound includes triethanolamine, diethanolamine, monoethanolamine, and the like, and salts thereof. Examples of the organic sulfonic acid compound include alkylsulfonic acid, toluenesulfonic acid, benzenesulfonic acid, and salts thereof, and preferable examples include alkylsulfonic acids in which the alkyl group has 1 to 10 carbon atoms. The organic sulfamine compounds include alkylsulfamic acids and their salts. The organic sulfate compound includes alkyl sulfates, alkyl ether sulfates, and salts thereof. The organic phosphonic acid compounds include phenylphosphonic acid and salts thereof. The organic carboxylic acid compounds include tartaric acid, oxalic acid, citric acid, malic acid, lactic acid, gluconic acid, and the like, and salts thereof. Examples of the betaine compound include a phosphobetaine compound, a sulfobetaine compound, and a carboxybetaine compound, and a preferred example is trimethylglycine.

[0436] The molecular weight of the hydrophilic low-molecular-weight compound (weight average molecular weight when the compound has a molecular weight distribution) is preferably 100 or more and less than 3,000, and more preferably 300 to 2,500.

[0437] The development accelerator is preferably a compound having a cyclic structure. The cyclic structure is not particularly limited, but examples thereof include a glucose ring in which at least a portion of a hydroxy group may be substituted, an isocyanuric ring, an aromatic ring which may have a heteroatom, and an aliphatic ring which may have a heteroatom, and is preferably a glucose ring or an isocyanuric ring. Examples of the compound having a glucose ring include the above-mentioned cellulose compounds. The compound having an isocyanuric ring includes the above-mentioned tris(2-hydroxyethyl)isocyanurate. Examples of the compound having an aromatic ring include the above-mentioned toluenesulfonic acid and benzenesulfonic acid. Examples of the compound having an aliphatic ring include the above-mentioned alkyl sulfate in which the alkyl group has a ring structure.

[0438] The compound having a cyclic structure preferably has a hydroxy group. Preferred examples of the compound having a hydroxy group and a cyclic structure include the above-mentioned cellulose compound and the above-mentioned tris(2-hydroxyethyl)isocyanurate.

[0439] The development accelerator is preferably an onium salt compound. The onium salt compound includes ammonium compounds and sulfonium compounds, and the ammonium compounds are preferred. The onium salt compound development accelerator includes trimethylglycine. Moreover, the onium salt compound in the electron-accepting polymerization initiator is a compound in which the value of the polarity term of the SP value is not 6.0 to 26.0, and is not included in the development accelerator.

[0440] The image recording layer may contain one type of development accelerator alone, or two or more types may be used in combination. One preferred embodiment of the image recording layer used in the present disclosure is an embodiment containing two or more compounds as development accelerators. Specifically, from the viewpoint of on-machine developability and ink receptivity, the image recording layer used in the present disclosure preferably contains, as a development accelerator, the above-mentioned polyol compound and the above-mentioned betaine compound, the above-mentioned betaine compound and the above-mentioned organic sulfonic acid compound, or the above-mentioned polyol compound and the above-mentioned organic sulfonic acid compound.

[0441] The content of the development accelerator relative to the total mass of the image recording layer is preferably from 0.1 to 20% by mass, more preferably from 0.5 to 15% by mass, and even more preferably from 1 to 10% by mass.

[0442] [Other ingredients] The image recording layer may contain other components such as surfactants, polymerization inhibitors, higher fatty acid derivatives, plasticizers, inorganic particles, inorganic layer compounds, etc. For details, see paragraphs 0114 to 0159 of JP2008-284817A.

[0443] [Formation of Image Recording Layer] The image recording layer in the lithographic printing plate precursor according to the present disclosure can be formed, for example, as described in paragraphs 0142 and 0143 of JP-A No. 2008-195018, by dispersing or dissolving the necessary components described above in a known solvent to prepare a coating liquid, applying the coating liquid onto a support by a known method such as bar coater coating, and drying. The coating amount (solid content) of the image recording layer after coating and drying varies depending on the application, but is generally 0.3 g / m 2 ~3.0g / m 2 In this range, good sensitivity and good film properties of the image recording layer can be obtained. As the solvent, a known solvent can be used.Specific examples of the solvent include water, acetone, methyl ethyl ketone (2-butanone), cyclohexane, ethyl acetate, ethylene dichloride, tetrahydrofuran, toluene, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, acetylacetone, cyclohexanone, diacetone alcohol, ethylene glycol monomethyl ether acetate, ethylene glycol ethyl ether acetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether acetate, 1-methoxy-2-propanol, 3-methoxy-1-propanol, methoxymethoxyethanol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, 3-methoxypropyl acetate, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, methyl lactate, and ethyl lactate. The solvent may be used alone or in combination of two or more kinds. The solid content concentration in the coating liquid is preferably 1% by mass to 50% by mass. The coating amount (solid content) of the image recording layer after coating and drying varies depending on the application, but from the viewpoint of obtaining good sensitivity and good film properties of the image recording layer, it is 0.3 g / m 2 ~3.0g / m 2 is preferred. Furthermore, the thickness of the image recording layer in the planographic printing plate precursor according to the present disclosure is preferably 0.1 μm to 3.0 μm, and more preferably 0.3 μm to 2.0 μm. In the present disclosure, the film thickness of each layer in the lithographic printing plate precursor is confirmed by preparing a slice by cutting the lithographic printing plate precursor in a direction perpendicular to its surface and observing the cross section of the slice with a scanning electron microscope (SEM).

[0444] <Support> The lithographic printing plate precursor according to the present disclosure has a support. The support can be appropriately selected from known supports for lithographic printing plate precursors. The support is preferably a support having a hydrophilic surface (hereinafter, also referred to as a "hydrophilic support").

[0445] The support in the present disclosure is preferably an aluminum plate that has been roughened and anodized by a known method. That is, the support in the present disclosure preferably has an aluminum plate and an anodized aluminum coating disposed on the aluminum plate.

[0446] It is also preferred that the support has an aluminum plate and an anodized aluminum film disposed on the aluminum plate, the anodized film being located closer to the image recording layer than the aluminum plate, the anodized film having micropores extending in the depth direction from the surface on the image recording layer side, and the average diameter of the micropores on the surface of the anodized film being greater than 10 nm and not greater than 100 nm. Furthermore, it is preferable that the micropores are composed of large diameter pores extending from the surface of the anodized film to a depth of 10 nm to 1,000 nm, and small diameter pores that communicate with the bottoms of the large diameter pores and extend from the communicating position to a depth of 20 nm to 2,000 nm, and that the average diameter of the large diameter pores at the surface of the anodized film is 15 nm to 100 nm, and the average diameter of the small diameter pores at the communicating positions is 13 nm or less.

[0447] FIG. 1 is a schematic cross-sectional view of one embodiment of an aluminum support 12a. The aluminum support 12a has a laminated structure in which an aluminum plate 18 and an aluminum anodized film 20a (hereinafter also simply referred to as "anodized film 20a") are laminated in this order. The anodized film 20a in the aluminum support 12a is located closer to the image recording layer than the aluminum plate 18. In other words, the lithographic printing plate precursor according to the present disclosure preferably has at least an anodized film, an image recording layer, and a water-soluble resin layer, in this order, on an aluminum plate.

[0448] -Anodized film- A preferred embodiment of the anodic oxide coating 20a will now be described. The anodized film 20a is a film produced on the surface of the aluminum plate 18 by anodizing, and has extremely fine micropores 22a that are approximately perpendicular to the film surface and are uniformly distributed. The micropores 22a extend from the surface of the anodized film 20a on the image recording layer side (the surface of the anodized film 20a on the side opposite to the aluminum plate 18 side) along the thickness direction (toward the aluminum plate 18).

[0449] The average diameter (average opening diameter) of the micropores 22a in the anodized coating 20a at the surface of the anodized coating is preferably more than 10 nm and not more than 100 nm. In terms of the balance between printing durability, stain resistance, and image visibility, the average opening diameter is more preferably 15 nm to 60 nm, even more preferably 20 nm to 50 nm, and particularly preferably 25 nm to 40 nm. The diameter inside the pores may be wider or narrower than that at the surface layer. When the average diameter exceeds 10 nm, printing durability and image visibility are excellent, and when the average diameter is 100 nm or less, printing durability is excellent. The average diameter of the micropores 22a was determined by observing the surface of the anodized film 20a using a field emission scanning electron microscope (FE-SEM) at a magnification of 150,000 times (N=4), measuring the diameters of the micropores present in an area of ​​400 nm x 600 nm at 50 locations in the four images obtained, and averaging these values. When the shape of the micropores 22a is not circular, the equivalent circle diameter is used. The "equivalent circle diameter" is the diameter of a circle when the shape of the opening is assumed to be a circle having the same projected area as the projected area of ​​the opening.

[0450] 1, the micropores 22a are substantially straight (cylindrical), but may be conical with a diameter decreasing in the depth direction (thickness direction). The shape of the bottom of the micropores 22a is not particularly limited, and may be curved (convex) or flat.

[0451] In the support, the micropores may be composed of a large diameter pore portion extending from the surface of the anodized coating to a certain depth position, and a small diameter pore portion communicating with the bottom of the large diameter pore portion and extending from the communicating position to a certain depth position. For example, as shown in FIG. 2, an aluminum support 12b may include an aluminum plate 18 and an anodized film 20b having micropores 22b each composed of a large diameter portion 24 and a small diameter portion . For example, the micropores 22b in the anodized film 20b are composed of large diameter pores 24 extending from the surface of the anodized film to a depth of 10 nm to 1000 nm (depth D: see FIG. 2) and small diameter pores 26 communicating with the bottoms of the large diameter pores 24 and extending from the communicating position to a depth of 20 nm to 2,000 nm. Specifically, for example, the embodiments described in paragraphs 0107 to 0114 of JP 2019-162855 A can be used.

[0452] -Method of manufacturing the support- As a method for producing a support used in the present disclosure, for example, a production method in which the following steps are carried out in order is preferable. Surface roughening process: A process for roughening the surface of aluminum plates. Anodizing process: A process of anodizing a roughened aluminum plate. Pore ​​widening process: A process in which the aluminum plate having the anodized film obtained in the anodizing process is brought into contact with an acidic or alkaline aqueous solution to expand the diameter of the micropores in the anodized film. The procedure for each step is described in detail below.

[0453] <<Surface roughening process>> The surface roughening process is a process of performing a surface roughening process including electrochemical surface roughening on the surface of the aluminum plate. This process is preferably performed before the anodizing process described later, but may not be performed if the surface of the aluminum plate already has a preferred surface shape. This process can be performed by the method described in paragraphs 0086 to 0101 of JP 2019-162855 A.

[0454] <<Anodizing process>> The procedure for the anodizing treatment step is not particularly limited as long as the above-mentioned micropores can be obtained, and known methods can be used. In the anodizing process, an aqueous solution of sulfuric acid, phosphoric acid, oxalic acid, etc. can be used as an electrolytic bath. For example, the concentration of sulfuric acid can be 100 g / L to 300 g / L. The conditions for the anodizing treatment are appropriately set depending on the electrolyte used. For example, the electrolyte temperature is 5°C to 70°C (preferably 10°C to 60°C), the current density is 0.5 A / dm 2 ~60A / dm 2 (Preferably 1A / dm 2 ~60A / dm 2 ), voltage 1V to 100V (preferably 5V to 50V), electrolysis time 1 second to 100 seconds (preferably 5 seconds to 60 seconds), and coating amount 0.1g / m 2 ~5g / m 2 (Preferably 0.2 g / m 2 ~3g / m 2 ) are mentioned.

[0455] <<Pore-wide processing>> The pore widening treatment is a treatment (pore diameter enlargement treatment) for enlarging the diameter (pore diameter) of the micropores present in the anodized film formed by the above-mentioned anodizing treatment process. The pore widening treatment can be carried out by contacting the aluminum plate obtained by the above-mentioned anodizing treatment step with an acid aqueous solution or an alkaline aqueous solution. The contacting method is not particularly limited, and examples thereof include a dipping method and a spraying method.

[0456] If necessary, the support may have a backcoat layer containing an organic polymer compound described in JP-A-5-45885 or a silicon alkoxy compound described in JP-A-6-35174 on the side opposite the image recording layer.

[0457] <Undercoat layer> The lithographic printing plate precursor according to the present disclosure preferably has an undercoat layer (sometimes called an intermediate layer) between the image recording layer and the support. The undercoat layer strengthens the adhesion between the support and the image recording layer in the exposed area, and facilitates peeling of the image recording layer from the support in the unexposed area, thereby contributing to improving developability while suppressing a decrease in printing durability. In addition, in the case of infrared laser exposure, the undercoat layer functions as a heat insulating layer, thereby preventing the heat generated by exposure from diffusing to the support and decreasing sensitivity.

[0458] The compound used in the undercoat layer may be a polymer having an adsorptive group and a hydrophilic group that can be adsorbed to the support surface. In order to improve adhesion with the image recording layer, a polymer having an adsorptive group and a hydrophilic group and further having a crosslinkable group is preferred. The compound used in the undercoat layer may be a low molecular weight compound or a polymer. The compound used in the undercoat layer may be a mixture of two or more kinds, if necessary.

[0459] When the compound used in the undercoat layer is a polymer, it is preferably a copolymer of a monomer having an adsorptive group, a monomer having a hydrophilic group, and a monomer having a crosslinkable group. The adsorptive group capable of being adsorbed to the surface of the support is preferably a phenolic hydroxy group, a carboxy group, -PO3H2, -OPO3H2, -CONHSO2-, -SO2NHSO2-, or -COCH2COCH3. The hydrophilic group is preferably a sulfo group or a salt thereof, or a salt of a carboxy group. The crosslinkable group is preferably an acryl group, a methacryl group, an acrylamide group, a methacrylamide group, or an allyl group. The polymer may have a crosslinkable group introduced by salt formation between a polar substituent of the polymer and a compound having an ethylenically unsaturated bond and a substituent having an opposite charge to the polar substituent, or may further be copolymerized with a monomer other than the above-mentioned monomers, preferably a hydrophilic monomer.

[0460] Specifically, preferred examples include a silane coupling agent having an addition-polymerizable ethylenic double bond reactive group described in JP-A-10-282679 and a phosphorus compound having an ethylenic double bond reactive group described in JP-A-2-304441. Also preferred are low-molecular or high-molecular compounds having a crosslinkable group (preferably an ethylenic unsaturated bond group), a functional group that interacts with the support surface, and a hydrophilic group described in JP-A-2005-238816, JP-A-2005-125749, JP-A-2006-239867, and JP-A-2006-215263. More preferred examples include polymers having an adsorptive group, a hydrophilic group and a crosslinkable group capable of being adsorbed onto the surface of a support, as described in JP-A Nos. 2005-125749 and 2006-188038.

[0461] The content of the ethylenically unsaturated bond group in the polymer used in the undercoat layer is preferably from 0.1 mmol to 10.0 mmol, and more preferably from 0.2 mmol to 5.5 mmol, per 1 g of the polymer. The weight average molecular weight (Mw) of the polymer used in the undercoat layer is preferably 5,000 or more, and more preferably from 10,000 to 300,000.

[0462] In addition to the above-mentioned compounds for the undercoat layer, the undercoat layer may contain a chelating agent, a secondary or tertiary amine, a polymerization inhibitor, a compound having an amino group or a functional group having polymerization inhibitory ability and a group that interacts with the support surface (e.g., 1,4-diazabicyclo[2.2.2]octane (DABCO), 2,3,5,6-tetrahydroxy-p-quinone, chloranil, sulfophthalic acid, hydroxyethylethylenediaminetriacetic acid, dihydroxyethylethylenediaminediacetic acid, hydroxyethyliminodiacetic acid, etc.) to prevent contamination over time.

[0463] The undercoat layer is applied by a known method. The coating amount (solid content) of the undercoat layer is 0.1 mg / m 2 ~100mg / m 2 is preferred, and 1 mg / m 2 ~30mg / m 2 is more preferred.

[0464] <Outermost layer> The lithographic printing plate precursor according to the present disclosure may have an outermost layer (sometimes called a "protective layer" or "overcoat layer") on the surface of the image recording layer opposite the support. The lithographic printing plate precursor according to the present disclosure preferably has a support, an image recording layer, and an outermost layer in this order. The outermost layer may have a function of preventing the occurrence of scratches in the image recording layer and ablation during exposure to high-intensity laser light, in addition to a function of suppressing image formation inhibiting reactions by blocking oxygen.

[0465] The outermost layer may be a known outermost layer ("protective layer" or "overcoat layer") in an on-press development type lithographic printing plate precursor. Specifically, the outermost layer may be the one described in paragraphs 0444 to 0462 of WO 2022 / 019217.

[0466] The lithographic printing plate precursor according to the present disclosure may have layers other than those described above. The other layers are not particularly limited, and any known layers may be used. For example, a backcoat layer may be provided on the side of the support opposite to the image recording layer, if necessary.

[0467] (Method of making a lithographic printing plate and method of lithographic printing) A lithographic printing plate can be prepared by imagewise exposing the lithographic printing plate precursor according to the present disclosure and then subjecting it to a development treatment. The method for producing a lithographic printing plate according to the present disclosure preferably includes a step of exposing the on-press development-type lithographic printing plate precursor according to the present disclosure in an imagewise manner (hereinafter also referred to as an "exposure step"), and a step of supplying at least one selected from the group consisting of printing ink and fountain solution on the printing press to remove the image recording layer in the non-image areas (hereinafter also referred to as an "on-press development step"). The lithographic printing method according to the present disclosure preferably includes a step of exposing the on-press development-type lithographic printing plate precursor according to the present disclosure in an imagewise manner (exposure step), a step of supplying at least one selected from the group consisting of printing ink and fountain solution to remove the image recording layer in non-image areas on the printing press to prepare a lithographic printing plate (on-press development step), and a step of printing with the obtained lithographic printing plate (printing step).

[0468] Further, a method for producing a lithographic printing plate according to the present disclosure includes a step of imagewise exposing an on-press development type lithographic printing plate precursor to an infrared laser, and a step of removing the image recording layer in a non-image area by supplying at least one selected from the group consisting of printing ink and fountain solution on a printing press, wherein the on-press development type lithographic printing plate precursor has a support and an image recording layer on the support, the image recording layer contains an infrared absorber capable of donating electrons to the initiator, and a color former precursor, and the energy density of the infrared laser exposure having a wavelength of 830 nm is 110 mJ / cm. 2 In the method for producing a lithographic printing plate, when the image recording layer is exposed to light at a rate of 100 nm to 150 nm, a change in lightness ΔL of the image recording layer before and after the exposure is preferably 3.0 or more. Further, the method for producing a lithographic printing plate according to the present disclosure preferably comprises the steps of imagewise exposing an on-press development type lithographic printing plate precursor to an infrared laser, and supplying at least one selected from the group consisting of printing ink and fountain solution on a printing press to remove the image recording layer in non-image areas, wherein the on-press development type lithographic printing plate precursor has a support and an image recording layer on the support, the image recording layer contains an initiator, an infrared absorber, and a color developer precursor, and the image recording layer satisfies the following formula L: 2.0≦L1-L0 Formula L In the formula L, L1 represents the visibility of the image recording layer, and L0 represents the visibility of a layer that is the same as the image recording layer except for the absence of the color former precursor. Furthermore, with regard to the lithographic printing method according to the present disclosure, each of these aspects preferably further includes the printing step described above.

[0469] Hereinafter, preferred aspects of each step of the method for producing a lithographic printing plate according to the present disclosure and the lithographic printing method according to the present disclosure will be described in order. Note that the lithographic printing plate precursor according to the present disclosure can also be developed with a developer. The exposure step and on-press development step in the method for preparing a lithographic printing plate will be described below, but the exposure step in the method for preparing a lithographic printing plate according to the present disclosure is the same as the exposure step in the lithographic printing method according to the present disclosure, and the on-press development step in the method for preparing a lithographic printing plate according to the present disclosure is the same as the on-press development step in the lithographic printing method according to the present disclosure.

[0470] <Exposure process> The method for producing a lithographic printing plate according to the present disclosure preferably includes an exposure step of imagewise exposing the lithographic printing plate precursor according to the present disclosure to form an exposed area and an unexposed area. The lithographic printing plate precursor according to the present disclosure is preferably imagewise exposed by laser exposure through a transparent original having a line image, a halftone dot image, or the like, or by laser light scanning based on digital data. The wavelength of the light source is preferably 750 nm to 1,400 nm. As a light source with a wavelength of 750 nm to 1,400 nm, a solid-state laser or a semiconductor laser that emits infrared rays is suitable. With regard to the infrared laser, the output is preferably 100 mW or more, the exposure time per pixel is preferably 20 microseconds or less, and the amount of irradiation energy is preferably 10 mJ / cm. 2 ~300mJ / cm 2 It is preferable to use a multi-beam laser device in order to shorten the exposure time. The exposure mechanism may be any of an internal drum type, an external drum type, a flatbed type, and the like. Image exposure can be carried out by a conventional method using a plate setter, etc. In the case of on-press development, the lithographic printing plate precursor may be mounted on a printing press and then image exposure may be carried out on the printing press.

[0471] <On-press development process> The method for producing a lithographic printing plate according to the present disclosure preferably includes an on-press development step of supplying at least one selected from the group consisting of printing ink and fountain solution on a printing press to remove the image recording layer in non-image areas. The on-press development method will be described below.

[0472] [On-press development method] In the on-press development method, it is preferable that an oil-based ink and an aqueous component are supplied to the image-exposed lithographic printing plate precursor on a printing press, and the image recording layer in the non-image areas is removed to prepare a lithographic printing plate. That is, after image exposure, the lithographic printing plate precursor is mounted on a printing press as it is without any development treatment, or the lithographic printing plate precursor is mounted on a printing press and then image exposure is performed on the printing press, and then an oil-based ink and an aqueous component are supplied to print. In the early stage of printing, the uncured image recording layer is dissolved or dispersed by either or both of the supplied oil-based ink and aqueous component in the non-image area and removed, exposing a hydrophilic surface in that area. On the other hand, in the exposed area, the image recording layer cured by exposure forms an oil-based ink receptive area having an oleophilic surface. The first thing supplied to the plate surface may be an oil-based ink or an aqueous component, but it is preferable to supply an oil-based ink first in order to prevent the aqueous component from being contaminated by the component of the image recording layer that has been removed. In this way, the lithographic printing plate precursor is developed on the press and used as it is for printing a large number of sheets. As the oil-based ink and aqueous component, printing ink and fountain solution for normal lithographic printing are preferably used.

[0473] As the laser for imagewise exposing the lithographic printing plate precursor according to the present disclosure, the wavelength of the light source is preferably 300 nm to 450 nm or 750 nm to 1,400 nm. In the case of a light source of 300 nm to 450 nm, a lithographic printing plate precursor containing a sensitizing dye having an absorption maximum in this wavelength region in an image recording layer is preferably used, and as a light source of 750 nm to 1,400 nm, the above-mentioned light sources are preferably used. As a light source of 300 nm to 450 nm, a semiconductor laser is suitable.

[0474] <Printing process> The lithographic printing method according to the present disclosure includes a printing step of supplying printing ink to a lithographic printing plate to print a recording medium. The printing ink is not particularly limited, and various known inks can be used as desired. Preferred examples of the printing ink include oil-based inks and ultraviolet-curable inks (UV inks). In the printing process, dampening water may be supplied as necessary. The printing step may also be carried out consecutively to the on-press development step without stopping the printing press. The recording medium is not particularly limited, and any known recording medium can be used as desired.

[0475] In the method for producing a lithographic printing plate from a lithographic printing plate precursor according to the present disclosure and the lithographic printing method according to the present disclosure, the entire surface of the lithographic printing plate precursor may be heated as necessary before exposure, during exposure, or between exposure and development. Such heating promotes the image formation reaction in the image recording layer, and can provide advantages such as improved sensitivity and printing durability and stabilization of sensitivity. Heating before development is preferably performed under mild conditions of 150° C. or less. In the above embodiment, problems such as hardening of non-image areas can be prevented. Heating after development is preferably performed under very strong conditions, preferably in the range of 100° C. to 500° C. In the above range, sufficient image strengthening effect can be obtained and problems such as deterioration of the support and thermal decomposition of the image area can be suppressed.

[0476] <Compound represented by formula (1b) and compound represented by formula (2a)> The compound represented by the above-mentioned formula (1b) and the compound represented by the formula (2a) are both novel compounds and can be suitably used as color former precursors. Details and preferred embodiments of the compound represented by formula (1b) and the compound represented by formula (2a) as the new compound are the same as the details and preferred embodiments of the compound represented by formula (1b) and the compound represented by formula (2a) in the color-forming composition used in the image recording layer in the lithographic printing plate precursor according to the present disclosure described above. EXAMPLES

[0477] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited thereto. In the present examples, "%" and "parts" mean "mass%" and "mass parts", respectively, unless otherwise specified. In the polymer compounds, unless otherwise specified, the molecular weight is the weight average molecular weight (Mw), and the ratio of the constituent repeating units is the molar percentage. The weight average molecular weight (Mw) is a value measured as a polystyrene equivalent value by gel permeation chromatography (GPC).

[0478] <Synthesis of specific compounds> The synthesis examples of the specific compounds are shown below. The structures of the specific compounds and the intermediates leading to the synthesis thereof were identified by NMR.

[0479] [Synthesis of compound C-1] (Synthesis of aldehydes) First, an aldehyde was obtained as follows.

[0480] [ka]

[0481] 12.0 g (88.8 mmol) of N,N-dimethyl-m-toluidine was dissolved in 135 mL of N,N-dimethylformamide, and 24.5 g (160 mmol; 1.8 eq.) of phosphorus oxychloride was slowly added dropwise in an ice bath, and the reaction was allowed to proceed overnight at room temperature. The reaction solution was slowly added to 900 mL of water, stirred at room temperature for 1 hour, neutralized with 2 mol / L aqueous NaOH solution to adjust the pH to 9, and the precipitated solid was collected by filtration and washed with water. Silica gel column chromatography (Hexane-EtOAc; TLC R f = 0.33 (Hexane-EtOAc 4:1)), suspended and washed with hexane, and dried under reduced pressure (70°C) to give 9.1 g of a white solid aldehyde derivative in a 63% yield. 1H NMR (CDCl3) δ2.62(s, 3H), 3.07(s, 6H), 6.43(d, J=2.4Hz, 1H), 6.57(dd, J=2.4 and 8.8Hz, 1H), 7.66(d, J=8.8Hz, 1H), 9.98(s, 1H). 13 C NMR (CDCl3) δ20.37, 39.97, 108.78, 113.36, 123.33, 134.56, 142.80, 153.47, 190.42.

[0482] (Synthesis of phthalide derivatives) Subsequently, the phthalide derivative was obtained as follows.

[0483] [ka]

[0484] The aldehyde: 6.0 g (36.8 mmol), 3-dimethylaminobenzoic acid: 6.07 g (36.8 mmol), acetic anhydride: 6.0 mL, and acetic acid: 2 mL were mixed and reacted at 120° C. for 5 hours. The reaction solution was slowly added to water: 100 mL, extracted with EtOAc (ethyl acetate), washed with brine, dried over MgSO4, concentrated under reduced pressure, and purified by silica gel column chromatography (Hexane-EtOAc; TLC R f = 0.44 (Hexane-EtOAc 2:1)), suspended and washed with hexane, and dried under reduced pressure (70°C) to obtain 5.0 g of a white solid of the phthalide derivative in a yield of 44%. 1 H NMR (CDCl3) δ2.42(s, 3H), 2.94(s, 3H), 3.04(s, 3H), 6.43(dd, J=2.4 and 8.8Hz, 1H), 6.55(s, 1H), 6.57(d, J=2.4Hz, 1H), 6.78(d, J=8.8Hz, 1H), 7.02(dd, J=2.4 and 8.8Hz, 1H), 7.16-7.18(m, 2H). 13C NMR (CDCl3) δ19.81, 40.32, 40.72, 81.13, 106.74, 109.68, 114.36, 118.70, 122.18, 123.45, 127.97, 128.82, 137.02, 138.75, 150.95, 151.23, 171.85.

[0485] (Synthesis of benzoyl benzoic acid derivatives) Subsequently, the benzoyl benzoic acid derivative was obtained as follows.

[0486] [ka]

[0487] 3.0 g (9.7 mmol) of the phthalide body and 12 mL of a 10% by mass NaOH aqueous solution were mixed and stirred at 90°C for 1 hour to completely dissolve. 2.8 g (13 mmol; 1.3 eq.) of sodium 3-nitrobenzenesulfonate was added and reacted at 115°C for 40 hours. After cooling, 6 mL of a 50% by mass acetic acid aqueous solution was added, stirred at room temperature for 45 minutes, and the solid was filtered off. The obtained solid was dissolved in 50 mL of a saturated sodium carbonate aqueous solution, and the insoluble matter was filtered off, and then acetic acid was added to adjust the pH to 5-6. The resulting solid was filtered off and crystallized from MeOH to obtain 1.34 g of a light yellow solid of the benzoylbenzoic acid body. The yield was 42%. 1 H NMR (DMSO-d6) δ2.42(s, 3H), 2.97,(s, 6H), 3.00(s, 6H), 6.45(dd, J=2.4 and 8.8Hz, 1H), 6.56(d, J=2.4Hz, 1H), 6.81(dd, J=2.4 and 8.8Hz, 1H), 6.95(d, J=2.8Hz, 1H), 7.05(d, J=8.8Hz, 1H), 7.16(d, J=8.8Hz, 1H), 12.64(s, 1H). 13C NMR (DMSO-d6) δ22.21, 40.05, 40.26, 108.19, 111.96, 113.13, 114.51, 126.11, 129.62, 130.79, 133.77, 134.61, 140.94, 151.19, 152.24, 169.66, 196.12.

[0488] (Synthesis of 1-butyl-2-methylindole) Subsequently, 1-butyl-2-methylindole was obtained as follows.

[0489] [ka]

[0490] 10.0 g (76.2 mmol) of 2-methylindole was dissolved in 191 mL of N,N-dimethylformamide, and 3.66 g (91.5 mmol; 1.2 eq.) of sodium hydride (60% in oil) was added little by little in an ice bath, and the mixture was stirred at room temperature for 30 minutes. 12.5 g (91.5 mmol; 1.2 eq.) of 1-bromobutane was slowly added dropwise in an ice bath, and the mixture was reacted at room temperature for 2 hours. 190 mL of water was added little by little, and 190 mL of EtOAc was added to separate the layers. The aqueous layer was extracted with 190 mL of EtOAc, and the combined organic layer was washed three times with 200 mL of water and 200 mL of brine, dried over MgSO4, concentrated under reduced pressure, and purified by silica gel column chromatography (Hexane-EtOAc; TLC R f = 0.79 (Hexane-EtOAc 4:1) to give 14.1 g of clear oil of 1-butyl-2-methylindole in 99% yield. 1H NMR (CDCl3) δ0.95(t, J=7.6Hz, 3H), 1.38(sextet, J=7.6Hz, 2H), 1.69-1.76(m, 2H), 2.42(d, J=0.8Hz, 1H), 4.05(t, J=7.6Hz, 2H), 6.23(s, 1H), 7.04(dt, J=1.2 and 6.8Hz, 1H), 7.12(dt, J=1.2 and 6.8Hz, 1H), 7.25-7.27(m, 1H), 7.51(dd, J=0.8 and 8.0Hz, 1H). 13 C NMR (CDCl3) δ12.79, 13.87, 20.30, 32.33, 42.96, 99.73, 108.98, 119.06, 119.61, 120.25, 128.00, 136.34, 136.58.

[0491] (Synthesis of compound C-1) Subsequently, compound C-1, which is a compound represented by formula (1), was obtained as follows.

[0492] [ka]

[0493] 0.50 g (2.7 mmol) of 1-butyl-2-methylindole, 0.96 g (2.9 mmol; 1.1 eq.) of benzoylbenzoic acid derivative and 5.0 mL of toluene were mixed and heated to 90°C. 0.38 mL (4.0 mmol; 1.5 eq.) of acetic anhydride was added and reacted at 90°C for 5 hours. The mixture was cooled to 80°C, 1.35 mL of water was added, and the mixture was stirred while cooling to room temperature. 1 mol / L aqueous NaOH solution was added to adjust the pH to 12, and the organic layer was washed with water, washed with brine, dried over MgSO4, concentrated under reduced pressure, and purified by silica gel column chromatography (Hexane-EtOAc; TLC R f = 0.31 (Hexane-EtOAc 2:1)), suspended and washed with hexane, and dried under reduced pressure (70°C) to obtain 0.975 g of a white solid compound C-1. The yield was 74%. The HPLC purity was 99.705 area% (254 nm). 1 H NMR (DMSO-d6) δ0.86(t, J=7.2Hz, 3H), 1.24(sextet, J=7.6Hz, 2H), 1.51-1.58(m, 2H), 2.03(s, 6H), 2.88(s, 6H), 2.96(s, 6H), 4.07(t, J=7.2Hz, 2H), 6.45(dd, J=2.8 and 8.8Hz, 1H), 6.58(d, J=2.4Hz, 1H), 6.80(t, J=7.2Hz, 1H), 6.92-7.02(m, 4H), 7.10(dd, J=2.4 and 8.8Hz, 1H), 7.28(d, J=8.8Hz, 1H), 7.36(d, J=8.0Hz, 1H). 13 C NMR (DMSO-d6) δ10.16, 13.11, 18.82, 20.43, 31.16, 39.18, (39.55), 90.72, 104.71, 107.76, 108.91, 110.85, 115.16, 118.33, 118.35, 118.43, 119.77, 124.09, 124.36, 125.18, 126.37, 127.12, 131.79, 135.05, 138.30, 140.12, 149.64, 150.25, 169.80.

[0494] [Synthesis of compound C-2] (Synthesis of 1-butyl-5-methoxy-2-methylindole) First, 1-butyl-5-methoxy-2-methylindole was obtained as follows.

[0495] [ka]

[0496] 2.0 g (12.4 mmol) of 5-methoxy-2-methylindole and 31.0 mL of N,N-dimethylformamide were added, and 0.60 g (14.9 mmol; 1.2 eq.) of sodium hydride (60% in oil) was added little by little under ice bath, and the mixture was stirred at room temperature for 30 minutes. 2.04 g (14.9 mmol; 1.2 eq.) of 1-bromobutane was slowly added dropwise under ice bath, and the mixture was reacted at room temperature for 2 hours. 31 mL of water was added little by little, and 31 mL of EtOAc was added to separate the mixture. The aqueous layer was extracted with 31 mL of EtOAc, and the combined organic layer was washed three times with 31 mL of water and 31 mL of brine, dried over MgSO4, concentrated under reduced pressure, and purified by silica gel column chromatography (Hexane-EtOAc; TLC R f = 0.77 (Hexane-EtOAc 4:1) to give 2.23 g of clear oil of 1-butyl-5-methoxy-2-methylindole in a yield of 83%. 1 H NMR (CDCl3) δ0.94(t, J=7.6Hz, 3H), 1.36(sextet, J=7.6Hz, 2H), 1.67-1.74(m, 2H), 2.39(d, J=0.4Hz, 3H), 3.84(s, 3H), 4.01(t, J=7.6Hz, 2H), 6.15(s, 1H), 6.78(dd, J=2.4 and 8.8Hz, 1H), 7.00(d, J=2.4Hz, 1H), 7.14(d, J=8.8Hz, 1H). 13 C NMR (CDCl3) δ12.83, 13.87, 20.29, 32.39, 43.08, 55.92, 99.42, 101.85, 109.60, 110.09, 128.31, 131.91, 136.96, 153.83.

[0497] (Synthesis of compound C-2) Subsequently, compound C-2, which is a compound represented by formula (1), was obtained as follows.

[0498] [ka]

[0499] 0.65 g (3.0 mmol) of 1-butyl-5-methoxy-2-methylindole, 1.0 g (3.3 mmol; 1.1 eq.) of 2-[p-(dimethylamino)benzoyl]-5-(dimethylamino)benzoic acid (MH-BCA) were mixed with 6.5 mL of toluene, heated to 90°C, 0.42 mL (4.5 mmol; 1.5 eq.) of acetic anhydride was added, and the mixture was reacted at 90°C for 100 minutes. The mixture was cooled to 80°C, 1.39 mL of water was added, and the mixture was stirred while being cooled to room temperature. A 1 mol / L aqueous solution of NaOH was added to adjust the pH to 12, and the organic layer was washed with water, washed with brine, dried over MgSO4, concentrated under reduced pressure, and purified by silica gel column chromatography (Hexane-EtOAc; TLC R f = 0.22 (Hexane-EtOAc 2:1)), suspended and washed with hexane, and dried under reduced pressure (70°C) to obtain 1.20 g of a white solid of compound C-2. The yield was 78%. The HPLC purity was 99.508 area% (254 nm). 1 H NMR (DMSO-d6) δ0.87(t, J=7.2Hz, 3H), 1.27(sextet, J=7.2Hz, 2H), 1.52-1.59(m, 2H), 1.91(s, 3H), 2.88(s, 6H), 2.97(s, 6H), 3.40(s, 3H), 4.02(t, J=7.2Hz, 2H), 5.82(d, J=2.4Hz, 1H), 6.65(dd, J=2.4 and 8.8Hz, 1H), 6.71(d, J=8.8Hz, 2H), 7.01(d, J=2.4Hz, 1H), 7.13(dd, J=2.4 and 8.8Hz, 1H), 7.21(d, J=8.8Hz, 2H), 7.28(d, J=9.2Hz, 1H), 7.39(d, J=8.4Hz, 1H). 13C NMR (DMSO-d6) δ11.04, 13.10, 18.93, 31.16, 39.40, 39.65, 89.49, 101.47, 104.92, 108.98, 109.05, 109.47, 111.48, 118.49, 123.92, 125.07, 125.81, 126.02, 129.27, 130.17, 135.69, 140.59, 149.35, 150.52, 152.27, 169.74.

[0500] [Synthesis of compound C-3] (Synthesis of 1-butyl-2-methylindole) First, 1-butyl-2-methylindole was obtained as follows. [ka]

[0501] 10.0 g (76.2 mmol) of 2-methylindole was dissolved in 191 mL of N,N-dimethylformamide, and 3.66 g (91.5 mmol; 1.2 eq.) of sodium hydride (60% in oil) was added little by little in an ice bath, and the mixture was stirred at room temperature for 30 minutes. 12.5 g (91.5 mmol; 1.2 eq.) of 1-bromobutane was slowly added dropwise in an ice bath, and the mixture was reacted at room temperature for 2 hours. 190 mL of water was added little by little, and 190 mL of EtOAc (ethyl acetate) was added to separate the layers. The aqueous layer was extracted with 190 mL of EtOAc, and the combined organic layer was washed three times with 200 mL of water and 200 mL of brine, dried over MgSO4, concentrated under reduced pressure, and purified by silica gel column chromatography (Hexane-EtOAc; TLC R f = 0.79 (Hexane-EtOAc 4:1) to give 14.1 g of clear oil of 1-butyl-2-methylindole in 99% yield. 1H NMR (CDCl3) δ0.95(t, J=7.6Hz, 3H), 1.38(sextet, J=7.6Hz, 2H), 1.69-1.76(m, 2H), 2.42(d, J=0.8Hz, 1H), 4.05(t, J=7.6Hz, 2H), 6.23(s, 1H), 7.04(dt, J=1.2 and 6.8Hz, 1H), 7.12(dt, J=1.2 and 6.8Hz, 1H), 7.25-7.27(m, 1H), 7.51(dd, J=0.8 and 8.0Hz, 1H). 13 C NMR (CDCl3) δ12.79, 13.87, 20.30, 32.33, 42.96, 99.73, 108.98, 119.06, 119.61, 120.25, 128.00, 136.34, 136.58.

[0502] (Synthesis of methyl 5-dimethylamino-2-formylbenzoate) Subsequently, methyl 5-dimethylamino-2-formylbenzoate was obtained as follows.

[0503] [ka]

[0504] In an ice bath, 9.44 g (91.5 mmol; 1.1 eq.) of phosphorus oxychloride was gradually added to 8.53 mL of N,N-dimethylformamide at an internal temperature of 12°C or less, and 10.0 g (55.8 mmol) of methyl 3-dimethylaminobenzoate was added over 15 minutes at an internal temperature of 4°C or less, and the mixture was allowed to react at room temperature for 21 hours. The reaction solution was gradually added to 50 mL of water, adjusted to pH 7 with aqueous ammonia, added with EtOAc, separated, washed with brine, dried over Na2SO4, concentrated under reduced pressure, and purified by silica gel column chromatography (Hexane-EtOAc; TLC R f = 0.33 (Hexane-EtOAc 2:1) to give 5.0 g of a cream-colored solid of methyl 5-dimethylamino-2-formylbenzoate in a 43% yield. 1 H NMR (CDCl3) δ3.11(s, 6H), 3.96(s, 3H), 6.79(dd, J=2.8 and 8.8Hz, 1H), 7.03(d, J=2.8Hz, 1H), 7.90(d, J=8.8Hz, 1H), 10.27(s, 1H).

[0505] (Synthesis of triarylmethane ester (A)) Subsequently, triarylmethane ester (A) was obtained as follows.

[0506] [ka]

[0507] 1.0 g (4.83 mmol) of methyl 5-dimethylamino-2-formylbenzoate and 1.81 g (9.65 mmol; 2.0 eq.) of 1-butyl-2-methylindole were suspended in 9.65 mL of propylene glycol and stirred for 3 hours in an oil bath at 100°C. 2 mg of p-toluenesulfonic acid monohydrate was added and reacted for 10 minutes. The mixture was allowed to cool, water was added, and EtOAc was added. The organic layer was washed with brine, dried over Na2SO4, concentrated under reduced pressure, and purified by silica gel column chromatography (Hexane-EtOAc; TLC R f = 0.73 (Hexane-EtOAc 2:1) to give 2.17 g of a light pink cream solid of triarylmethane ester (A). The yield was 80%. 1H NMR (CDCl3) δ0.92(t, J=7.2Hz, 6H), 1.34(sextet, J=7.6Hz, 4H), 1.63-1.71(m, 4H), 2.11(s, 6H), 2.93(s, 6H), 3.31(s, 3H), 4.03(t, J=7.6Hz, 4H), 6.65(dd, J=2.8 and 8.4Hz, 1H), 6.76-6.82(m, 3H), 6.95(d, J=7.6Hz, 2H), 6.99-7.03(m, 3H), 7.08(d, J=2.8Hz, 1H), 7.20(d, J=8.0Hz, 2H). 13 C NMR (CDCl3) δ10.55, 13.91, 20.22, 32.33, 35.58, 40.63, 42.73, 51.52, 108.42, 113.45, 114.23, 114.92, 118.33, 119.33, 119.69, 128.41, 130.52, 132.04, 132.37, 133.19, 135.86, 148.57, 169.80.

[0508] (Synthesis of triarylmethane ester (B)) Subsequently, triarylmethane ester (A) was obtained as follows.

[0509] [ka]

[0510] Triarylmethane ester (A): 2.0 g (3.55 mmol) was dissolved in methanol: 60 mL, sodium hydroxide: 0.3 g (7.4 mmol; 2.1 eq) and water: 0.2 mL were added, and the mixture was stirred at room temperature and in a water bath at 50°C for 3 hours. The solvent was distilled off, and the mixture was suspended in THF (tetrahydrofuran) and stirred in a water bath at 60°C for 2 hours. The mixture was concentrated under reduced pressure and purified by silica gel column chromatography (Hexane-EtOAc; TLC R f= 0.78 (CHCl3-MeOH 4:1)) to give 1.80 g of triarylmethanecarboxylic acid (B) as a red solid in 92% yield. 1 H NMR (CDCl3) δ0.89(t, J=7.2Hz, 6H), 1.28(sextet, J=7.2Hz, 4H), 1.61-1.69(m, 4H), 2.07(s, 6H), 2.94(s, 6H), 4.01(t, J=7.2Hz, 4H), 6.71(dd, J=2.8 and 8.4Hz, 1H), 6.75-6.84(m, 5H), 6.95(m, 2H), 7.11(d, J=8.8Hz, 1H), 7.19-7.21(m, 3H). 13 C NMR (CDCl3) δ10.42, 13.89, 20.17, 32.28, 35.77, 40.64, 42.73, 108.48, 113.42, 115.00, 115.96, 118.38, 119.50, 119.62, 128.39, 130.17, 131.19, 133.44, 133.86, 135.84, 148.56, 172.94. 13 C NMR (DMSO-d6) δ10.04, 13.68, 19.36, 21.43, 31.83, 34.19, 40.13, 41.80, 108.70, 113.24, 113.74, 117.70, 118.66, 118.84, 119.24, 127.94, 130.01, 130.95, 132.65, 135.40, 148.05, 172.13.

[0511] (Synthesis of compound C-3) Subsequently, compound C-3, which is a compound represented by formula (2), was obtained as follows.

[0512] [ka]

[0513] Triarylmethane carboxylic acid (B): 1.50 g (2.7 mmol), sodium hydroxide: 0.405 g (10.1 mmol; 3.75 eq.) were mixed with water: 20 mL and methanol: 5 mL, heated to 80 ° C., potassium peroxodisulfate: 0.89 g (3.3 mmol; 1.2 eq.) was dissolved in water: 20 mL and added, and reacted at 80 ° C. for 5 hours. It was cooled in a water bath, neutralized to pH 7 with dilute hydrochloric acid, filtered off the solid, washed with water, dried under reduced pressure, and purified by silica gel column chromatography (Hexane-EtOAc; TLC R f = 0.53 (EtOAc), suspended and washed in hexane, and dried under reduced pressure (60°C) to obtain 0.70 g of a pale pink powder of compound C-3. The yield was 47%. The HPLC purity was 95.649 area% (254 nm) and the λmax was 524 nm. 1 H NMR (DMSO-d6) δ0.87(t, J=7.2Hz, 6H), 1.23-1.28(m, 4H), 1.56-1.59(m, 4H), 1.99-2.09(m, 6H), 2.99(s, 6H), 4.11(t, J=6.8Hz, 4H), 6.65-6.86(m, 4H), 7.00-7.04(m, 3H), 7.09-7.12(m, 1H), 7.37-7.43(m, 3H). 13 C NMR (DMSO-d6) δ11.13, 13.63, 19.33, 31.66, 40.08, 88.42, 105.15, 109.53, 111.69, 118.81, 118.85, 120.29, 124.33, 125.13, 125.61, 134.64, 135.47, 141.22, 151.01, 170.51.

[0514] [Synthesis of compounds C-4 to C-10] Compounds C-4 to C-10 were synthesized with reference to the synthesis methods of compounds C-1 to C-3.

[0515] (Examples A1 to A11 and Comparative Examples A1 to A4) <Preparation of the support> An aluminum plate was prepared by electrolytically roughening the surface in a hydrochloric acid solution to obtain an average roughness (Ra) of 0.4 μm. The aluminum plate was then anodized in an aqueous phosphoric acid solution to obtain an average roughness (Ra) of 1.1 g / m 2 of oxide film was formed, followed by a post-treatment aqueous solution of poly(acrylic acid) at 0.03 g / m 2 A coating film having a dry thickness of In this way, a support was obtained.

[0516] <Formation of image recording layer> Next, the image recording layer coating solution (1) having the following composition was applied to the surface of the support using a bar coater, and then dried at 250° C. for 60 seconds to obtain a dry film thickness of 0.9 g / m 2 Thus, an image recording layer having the following properties was obtained. In this way, on-press development type lithographic printing plate precursors of Examples A1 to A11 and Comparative Examples A1 to A4 were obtained.

[0517] -Image recording layer coating liquid (1)- Specific compound or comparative compound (compounds listed in Table 1 below): Amount listed in Table 1 below Polymer dispersion: 0.675 parts Hydroxypropyl methylcellulose 5% by weight aqueous solution (hydroxypropyl methylcellulose: 30% methoxylated, 10% hydroxypropoxylated, viscosity 5 mPa·s (2% by weight aqueous solution at 20°C)): 0.400 parts Monomer 1: 0.333 parts Monomer 2: 0.167 parts Infrared absorbent 1: 0.020 parts Surfactant 1: 0.045 parts Polymerization initiator (iodonium salt compound 1): 0.06 parts 1-Propanol: 2.6 parts 2-Butanone: 3.5 parts 1-Methoxy-2-propanol: 0.92 parts δ-Butyrolactone: 0.10 parts ·Wednesday: 1.16 parts

[0518] Details of each component used in the image recording layer coating solution (1) are as follows. Polymer dispersion: Prepared according to Example 10 of EP 1,765,593 (23.5% by weight of polymer in 80:20 n-propanol / water by weight ratio) Monomer 1: DESMODUR (registered trademark) N100 manufactured by Bayer (40% by mass solution of urethane acrylate: hydroxyethyl acrylate: pentaerythritol triacrylate = 1: 1.5: 1.5 (molar ratio) in 2-butanone) Monomer 2: 40% by mass solution of acrylate of bisphenol A ethylene oxide 10 mole adduct in 2-butanone Infrared absorber 1: Structure shown below Surfactant 1: (BYK 302 manufactured by Byk Chemie (25% by weight solution in 1-methoxy-2-propanol) Iodonium salt compound 1: Structure shown below

[0519] [ka]

[0520] Details of the specific compounds and comparative compounds listed in Table 1 are as follows.

[0521] [ka]

[0522] [ka]

[0523] (Example A12) An on-press development type lithographic printing plate precursor was obtained in the same manner as in Example A2, except that in the image recording layer coating solution (1), the amount of iodonium salt compound 1 was changed to 0.025 parts, and 0.025 parts of iodonium salt compound 2 having the following structure was further added.

[0524] [ka]

[0525] (Example A13) An on-press development type lithographic printing plate precursor was obtained in the same manner as in Example A2, except that in the image recording layer coating solution (1), infrared absorbent 1 was changed to infrared absorbent 2 having the following structure.

[0526] [ka]

[0527] (Example A14) An on-press development type lithographic printing plate precursor was obtained in the same manner as in Example A2, except that in the image recording layer coating solution (1), infrared absorber 1 was changed to infrared absorber 3 having the following structure.

[0528] [ka]

[0529] (Example A15) An on-press development type lithographic printing plate precursor was obtained in the same manner as in Example A2, except that 0.010 parts of a color developer (leuco dye 1) having the following structure, which is a compound represented by formula (Le-10), was further added to the image recording layer coating solution (1).

[0530] [ka]

[0531] (Example A16) An on-press development type lithographic printing plate precursor was obtained in the same manner as in Example A2, except that 0.025 parts of phenothiazine having the following structure, which is a compound represented by formula (Ph), was further added to the image recording layer coating solution (1).

[0532] [ka]

[0533] [evaluation] 1. Evaluation of color development (visibility) The obtained on-press development type lithographic printing plate precursor was exposed to light using a Creo Trendsetter 3244VX equipped with a water-cooled 40 W infrared semiconductor laser under the conditions of an output of 11.5 W, an outer drum rotation speed of 220 rpm, and a resolution of 2,400 dpi (dots per inch, 1 inch = 25.4 mm). The exposure was performed in an environment of 25°C and 50% RH. The color development of the lithographic printing plate precursor immediately after exposure was measured. The measurement was performed using a spectrophotometer CM2600d manufactured by Konica Minolta, Inc. and operation software CM-S100W, using the SCE (specular reflection excluded) method. The visibility (color development) was measured using the L * a * b * Color space L * Using the value (brightness), L * value and L of the unexposed area * The evaluation was based on the difference ΔL' between the values. The larger the ΔL' value, the better the color development. The evaluation results are shown in Table 1.

[0534] 2. Evaluation of streaky unevenness The obtained on-press development type lithographic printing plate precursor was exposed to light at an exposure energy of 110 mJ / cm using an exposure machine (PlateRite HD 8900N series, manufactured by SCREEN Graphic Solutions Co., Ltd.) equipped with an exposure head that uses GLV (Grating Light Value) technology. 2 The exposed image contained an AM screen of 200 lines and an FM (Frequency Modulation Screen) of 20 μm flat screen chart. The exposed lithographic printing plate precursor thus obtained was mounted on a SOR-M monochrome printing press (Heidelberg) without being developed, and 1,000 sheets were printed using ink: Fusion-G MK Red N (DIC Corporation), dampening water: S-S2 2% diluted (FUJIFILM Corporation), blanket: DAY Blanket D 3000 (T&K TOKA Corporation), and paper: Tokubishi Art 127.9gsm (Mitsubishi Paper Mills, Ltd.). Then, the degree of streaky unevenness was visually evaluated on the 1,000th printed sheet. It is said that the less streaky unevenness is observed, the better the GLV suitability. The evaluation results are shown in Table 1. -Evaluation criteria- A: No streaky unevenness is observed on either the FM screen or the AM screen. B: Only on the FM screen, slight streaky unevenness is visible. C: Slight streaky irregularities are visible on both the FM screen and the AM screen. D: Streaky unevenness is observed on both the FM screen and the AM screen.

[0535] [Table 1]

[0536] (Examples B1 to B13 and Comparative Examples B1 to B4) <Preparation of the support> (a) Alkaline etching treatment An aluminum plate was etched by spraying an aqueous solution of caustic soda with a caustic soda concentration of 26% by mass and an aluminum ion concentration of 6.5% by mass at a temperature of 70°C. The plate was then rinsed with water by spraying. The amount of dissolved aluminum on the surface to be subsequently subjected to electrochemical graining treatment was 5 g / m 2 It was.

[0537] (b) Desmutting treatment using an acidic aqueous solution (first desmutting treatment) Next, a desmutting treatment was carried out using an acidic aqueous solution. The acidic aqueous solution used in the desmutting treatment was an aqueous solution of 150 g / L sulfuric acid. The liquid temperature was 30°C. The acidic aqueous solution was sprayed onto the aluminum plate to carry out the desmutting treatment for 3 seconds. After that, a water rinsing treatment was carried out.

[0538] (c) Electrochemical roughening treatment Next, electrochemical graining treatment was performed using an electrolytic solution with a hydrochloric acid concentration of 14 g / L, an aluminum ion concentration of 13 g / L, and a sulfuric acid concentration of 3 g / L, using an alternating current. The temperature of the electrolytic solution was 30° C. The aluminum ion concentration was adjusted by adding aluminum chloride. The AC waveform is a sine wave with symmetrical positive and negative waveforms, the frequency is 50Hz, the anode reaction time and cathode reaction time in one AC cycle are 1:1, and the current density is 75A / dm at the peak current value of the AC waveform. 2 The total amount of electricity that the aluminum plate receives in the anode reaction is 450 C / dm 2 and electrolytic treatment is 112.5C / dm 2 The test was carried out four times with a four second interval between each test. A carbon electrode was used as the counter electrode for the aluminum plate. After that, the plate was washed with water.

[0539] (d) Alkaline etching treatment After electrochemical graining, the aluminum plate was etched by spraying an aqueous solution of caustic soda with a caustic soda concentration of 5% by mass and an aluminum ion concentration of 0.5% by mass at 45°C. The amount of aluminum dissolved from the electrochemically grained surface was 0.2 g / m 2 Then, a water washing treatment was carried out.

[0540] (e) Desmutting using an acidic aqueous solution Next, a desmutting treatment was carried out using an acidic aqueous solution. Specifically, the acidic aqueous solution was sprayed onto the aluminum plate and the desmutting treatment was carried out for 3 seconds. The acidic aqueous solution used for the desmutting treatment was an aqueous solution with a sulfuric acid concentration of 170 g / L and an aluminum ion concentration of 5 g / L. The liquid temperature was 30°C.

[0541] (f) First stage anodizing A first-stage anodizing treatment (also referred to as a first anodizing treatment) was performed using an anodizing treatment device 610 using direct current electrolysis having a structure shown in Fig. 3. Specifically, the first anodizing treatment was performed under the conditions in the "first anodizing treatment" column shown in Table 2 below, and an anodized film of a predetermined film thickness was formed. The anodizing apparatus 610 shown in FIG. 3 will now be described. In an anodizing treatment device 610 shown in Fig. 3, an aluminum sheet 616 is transported as indicated by an arrow in Fig. 3. In a power supply tank 612 in which an electrolytic solution 618 is stored, the aluminum sheet 616 is charged (+) by a power supply electrode 620. Then, in the power supply tank 612, the aluminum sheet 616 is transported upward by a roller 622, and its direction is changed downward by a nip roller 624, and then the aluminum sheet 616 is transported toward an electrolytic treatment tank 614 in which an electrolytic solution 626 is stored, and its direction is changed horizontally by a roller 628. Next, the aluminum sheet 616 is charged (-) by an electrolytic electrode 630, so that an anodized film is formed on the surface of the aluminum sheet 616, and the aluminum sheet 616 that leaves the electrolytic treatment tank 614 is transported to a subsequent process. In the anodizing device 610, a roller 622, a nip roller 624, and a roller 628 constitute a direction changing means, and the aluminum sheet 616 is transported in a mountain shape and an inverted U shape by the rollers 622, 624, and 628 in the space between the power supply tank 612 and the electrolytic treatment tank 614. The power supply electrode 620 and the electrolytic electrode 630 are connected to a DC power source 634.

[0542] (g) Pore-wide treatment The anodized aluminum plate was immersed in an aqueous solution of caustic soda with a temperature of 40° C., a caustic soda concentration of 5 mass %, and an aluminum ion concentration of 0.5 mass % under the conditions shown in Table 2 below to carry out a pore widening treatment. Then, the aluminum plate was washed with water by spraying.

[0543] (h) Second anodizing treatment A second-stage anodizing treatment (also referred to as a second anodizing treatment) was performed using an anodizing treatment apparatus 610 using direct current electrolysis having a structure shown in Fig. 3. Specifically, the second anodizing treatment was performed under the conditions in the "second anodizing treatment" column shown in Table 2 below, and an anodized film of a predetermined film thickness was formed.

[0544] In this manner, a support was prepared. The L of the micropore anodized film surface of the obtained support * a * b * Lightness L in color system * Table 3 shows the average diameter and depth of the larger pores in the micropores on the surface of the oxide film, the average diameter (nm) and depth of the small pores in the micropores at the communicating positions, the depth (nm) of the larger pores and the small pores, the micropore density, and the thickness of the anodized film from the bottom of the small pores to the surface of the aluminum plate (also referred to as the film thickness). In Table 1, the amount of film (AD) in the first anodizing treatment column and the amount of film (AD) in the second anodizing treatment column represent the amount of film obtained by each treatment. The electrolyte used is an aqueous solution containing the components in Table 2.

[0545] [Table 2]

[0546] [Table 3]

[0547] <Formation of undercoat layer> On the obtained support, a coating solution for an undercoat layer having the following composition was applied in a dry amount of 0.1 g / m2 The undercoat layer was formed by coating so as to become

[0548] - Coating solution for undercoat layer - Undercoat layer compound (U-1 below, 11% aqueous solution): 0.10502 parts Sodium gluconate: 0.0700 parts Surfactant (Emalex (registered trademark) 710, Nippon Emulsion Co., Ltd.): 0.00159 parts Preservative (BioHope L, K.I. Kasei Co., Ltd.): 0.00149 parts ·Wed: 3.29000 copies

[0549] [ka]

[0550] <Formation of image recording layer> The image recording layer coating solution (2) described below was applied onto the undercoat layer with a bar and dried in an oven at 120°C for 40 seconds to obtain a dry coating amount of 1.0 g / m 2 Thus, an image recording layer of

[0551] -Image recording layer coating liquid (2)- Specific compound or comparative compound (compounds listed in Table 4 below): Amount listed in Table 4 below Infrared absorber 4: 0.0175 parts Color former (S-22): 0.0120 parts Electron-accepting polymerization initiator (IA-1): 0.0981 parts Electron donor polymerization initiator (TPB): 0.0270 parts ·Polymerizable compound (M-1): 0.3536 parts Tricresyl phosphate: 0.0450 parts Anionic surfactant (A-1): 0.0162 parts Fluorosurfactant (W-1): 0.0042 parts 2-Butanone: 5.3155 parts 1-Methoxy-2-propanol: 2.8825 parts Methanol: 2.3391 parts Microgel liquid 1: 2.8779 parts

[0552] Details of the components used in the image recording layer coating solution (2) are as follows. Infrared absorber 4: non-decomposing infrared absorber, compound having the following structure, λmax=794 nm Infrared absorber 5: non-decomposing infrared absorber, compound having the following structure, λmax=819 nm

[0553] [ka]

[0554] Color former (S-22): Color former (S-22) Color former (S-16): Color former (S-16) Electron-accepting polymerization initiator (IA-1): The following compound, LUMO = -3.02 eV Electron-donating polymerization initiator (TPB): sodium tetraphenylborate, HOMO = -5.90 eV

[0555] [ka]

[0556] [Method of synthesizing polymerizable compound (M-1)] A mixed solution of Takenate D-160N (polyisocyanate trimethylolpropane adduct, Mitsui Chemicals, Inc., 4.7 parts), Aronix M-403 (Toagosei Co., Ltd., an amount such that the NCO value of Takenate D-160N and the hydroxyl value of Aronix M-403 are 1:1), t-butylbenzoquinone (0.02 parts), and methyl ethyl ketone (11.5 parts) was heated to 65°C. Neostan U-600 (bismuth-based polycondensation catalyst, Nitto Kasei Co., Ltd., 0.11 parts) was added to the reaction solution, and the mixture was heated at 65°C for 4 hours. The reaction solution was cooled to room temperature (25°C) and methyl ethyl ketone was added to synthesize a urethane acrylate (M-1) solution with a solid content of 50% by mass. Using a recycle type GPC (instrument: LC908-C60, columns: JAIGEL-1H-40 and 2H-40 (manufactured by Japan Analytical Industry Co., Ltd.)), molecular weight fractionation of the urethane acrylate solution was carried out with an eluent of tetrahydrofuran (THF). The weight average molecular weight was 20,000.

[0557] Anionic surfactant (A-1): The following compound Fluorosurfactant (W-1): The following compound

[0558] [ka]

[0559] [ka]

[0560] [Method for synthesizing microgel liquid 1] -Preparation of oil phase components- 6.66 g of a polyfunctional isocyanate compound (PM-200: manufactured by Wanka Chemical Co., Ltd.), 5.46 g of a 50% by mass ethyl acetate solution of "Takenate (registered trademark) D-116N (an adduct of trimethylolpropane (TMP), m-xylylene diisocyanate (XDI) and polyethylene glycol monomethyl ether (EO90) (structure shown below)" manufactured by Mitsui Chemicals, Inc., 11.24 g of a 65% by mass ethyl acetate solution of dipentaerythritol pentaacrylate (SR-399, manufactured by Sartomer Co., Ltd.), 14.47 g of ethyl acetate, and 0.45 g of Paionin (registered trademark) A-41-C manufactured by Takemoto Oil Co., Ltd. were mixed and stirred at room temperature (25 ° C.) for 15 minutes to obtain an oil phase component.

[0561] [ka]

[0562] -Preparation of aqueous phase components- As the aqueous phase component, 47.2 g of distilled water was prepared.

[0563] -Microcapsule formation process- The aqueous phase components were added to and mixed with the oil phase components, and the resulting mixture was emulsified using a homogenizer at 12,000 rpm for 16 minutes to obtain an emulsion. To the resulting emulsion was added 16.8 g of distilled water, and the resulting liquid was stirred at room temperature for 10 minutes. Next, the liquid after stirring was heated to 45°C, and stirred for 4 hours while maintaining the liquid temperature at 45°C, thereby distilling off ethyl acetate from the liquid. Next, 5.12 g of a 10% by mass aqueous solution of 1,8-diazabicyclo[5.4.0]undec-7-ene-octylate (U-CAT SA102, manufactured by San-Apro Co., Ltd.) was added, stirred at room temperature for 30 minutes, and allowed to stand at 45°C for 24 hours. The solid content was adjusted to 20% by mass with distilled water, and an aqueous dispersion of microgel 1 was obtained. The volume average particle size of microgel 1 was measured using a laser diffraction / scattering particle size distribution measuring device LA-920 (manufactured by Horiba, Ltd.) and was 165 nm.

[0564] <Formation of the outermost layer> The outermost layer coating solution described below was applied onto the image recording layer with a bar and dried in an oven at 120°C for 60 seconds to obtain a dry coating weight of 0.41 g / m 2 The outermost layer was formed. Through the above steps, an on-press development type lithographic printing plate precursor was obtained.

[0565] -Outermost layer coating liquid- The components shown below were dissolved or dispersed in ion-exchanged water so that the solid content was adjusted to 20% by mass, thereby preparing an outermost layer coating solution. Water-soluble polymer (polyvinyl alcohol, Mowiol 4-88 manufactured by Kuraray Co., Ltd.): 250 parts by weight Hydrophobic polymer (polyvinylidene chloride aqueous dispersion, Diofan (registered trademark) A50 manufactured by Solvin): 250 parts by weight Surfactant (nonionic surfactant, Lutensol (registered trademark) A8 manufactured by BASF): 10 parts by mass

[0566] (Examples B14 to B16) An on-press development type lithographic printing plate precursor was obtained in the same manner as in Examples B1 to B3, except that in the image recording layer coating solution (2) of Examples B1 to B3, the fluorosurfactant (W-1) was changed to a polymer (W-2) having the following structure, which is a polymer having a structural unit represented by formula (I).

[0567] [ka]

[0568] (Example B17) An on-press development type lithographic printing plate precursor was obtained in the same manner as in Example B1, except that 0.0013 parts of infrared absorber 5 having the above structure was further added to the image recording layer coating solution (2).

[0569] [evaluation] The evaluation of 1. color development (visibility) and 2. streak-like unevenness were performed in the same manner as in Example A1. The evaluation results are shown in Table 4.

[0570] 3.Evaluation of surface condition The obtained on-press development type lithographic printing plate precursor was processed to 40 cm x 62 cm. The surface of the outermost layer side of the obtained sample was visually observed under white light irradiation of 750 to 1500 Lux, and the surface condition was evaluated according to the following criteria. The evaluation results are shown in Table 4. -Evaluation criteria- A: No visible unevenness is observed across the entire surface. B: Surface unevenness is partially visible. C: Surface unevenness is partially visible in a wider area than in B.

[0571] [Table 4]

[0572] As is clear from Tables 1 and 4, the planographic printing plate precursors according to the examples provide planographic printing plates with excellent color development and suppressed streak-like unevenness. As is clear from Table 4, the planographic printing plate precursors according to the examples provide planographic printing plates with excellent surface condition. [Explanation of symbols]

[0573] 12a, 12b: aluminum support, 14: undercoat layer, 16: image recording layer, 18: aluminum plate, 20a, 20b: anodized film, 22a, 22b: micropores, 24: large diameter pores, 26: small diameter pores, D: depth of large diameter pores, 610: anodizing treatment device, 612: power supply tank, 614: electrolytic treatment tank, 616: aluminum plate, 618, 26: electrolyte, 620: power supply electrode, 622, 628: roller, 624: nip roller, 630: electrolytic electrode, 632: tank wall, 634: DC power source

Claims

1. A support and an image recording layer on the support, the image recording layer contains an infrared absorbing agent, a polymerization initiator, a polymerizable compound, and one or more compounds selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2): 【Chemistry 1】 In formula (1) and formula (2), Ra 1 and Ra 2 each independently represents a hydrogen atom or a substituted or unsubstituted alkyl group; 1 and Ra 2 may be linked to form a ring structure, Rb 1 and Rb 3 each independently represents a substituted or unsubstituted alkyl group; Rb 2 and Rb 4 each independently represents a hydrogen atom or a substituted or unsubstituted alkyl group, and each EDG independently represents a hydrogen atom or an electron-donating group, provided that at least one of the four EDGs in formula (1) represents an electron-donating group.

2. The on-press development type lithographic printing plate precursor according to claim 1 , wherein the compound represented by formula (1) is a compound represented by the following formula (1a): 【Chemistry 2】 In formula (1a), Ra 1 and Ra 2 each independently represents a hydrogen atom or a substituted or unsubstituted alkyl group; 1 and Ra 2 may be linked to form a ring structure, Rb 1 represents a substituted or unsubstituted alkyl group; Rb 2 represents a hydrogen atom or a substituted or unsubstituted alkyl group, and EDG each independently represents a hydrogen atom or an electron-donating group, provided that at least one of the two EDGs in formula (1a) represents an electron-donating group.

3. The on-press development type lithographic printing plate precursor according to claim 1 or 2, wherein the electron donating group in the formula (1) and the formula (2) is a methoxy group.

4. The on-press development type lithographic printing plate precursor according to claim 1 or 2, wherein the compound represented by formula (1) is a compound represented by the following formula (1b): 【Chemistry 3】 In formula (1b), Rb 1 represents a substituted or unsubstituted alkyl group.

5. The on-press development type lithographic printing plate precursor according to claim 1 or 2, wherein the compound represented by formula (2) is a compound represented by the following formula (2a): 【Chemistry 4】 In formula (2a), Rb 1 and Rb 3 each independently represents a substituted or unsubstituted alkyl group having 2 or more carbon atoms.

6. 3. The on-press development type lithographic printing plate precursor according to claim 1 or 2, wherein the polymerization initiator comprises a compound A represented by the following formula (Ia) and one or more compounds B selected from the group consisting of compounds represented by the following formula (Ib) or (Ic): 【Chemistry 5】 In formulas (Ia) to (Ic), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 are each independently a substituted or unsubstituted alkyl group having 2 to 9 carbon atoms, or a substituted or unsubstituted alkoxy group; R 3 and R 4 At least one of 1 Or R 2 Unlike, R 1 and R 2 The total number of carbon atoms in 3 and R 4 The difference between the total number of carbon atoms in R is 0 to 4. 1 and R 2 The total number of carbon atoms in 5 and R 6 The difference between the total number of carbon atoms in X is 0 to 4. 1 , X 2 and X 3 are each independently a counter anion.

7. The on-press development type lithographic printing plate precursor according to claim 1 or 2, wherein the infrared absorber comprises a compound represented by the following formula (X): 【Chemistry 6】 In formula (X), Ar 11 and Ar 12 each independently represents an atomic group necessary to form a substituted or unsubstituted aromatic ring or a substituted or unsubstituted heteroaromatic ring; R 11 and R 12 are each independently a substituted or unsubstituted alkyl group; R 13 represents a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted heteroaryl group; R 14 represents a hydrogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted heteroaryl group; Y each independently represents an oxygen atom, a sulfur atom, or >C(R 15 R 16 ) represents a dialkylmethylene group represented by R 15 and R 16 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; A 1 and A 2 each independently represents a substituted or unsubstituted alkyl group, or represents a group of atoms including 2 or 3 carbon atoms necessary to form a substituted or unsubstituted 5- or 6-membered non-aromatic carbon ring when linked together, and Za represents a counter ion that neutralizes the charge.

8. The on-press development type lithographic printing plate precursor according to claim 1 or 2, wherein the image recording layer further contains one or more compounds selected from the group consisting of compounds represented by the following formula (Le-10) and compounds represented by the following formula (Z-4): 【Chemistry 7】 In formula (Le-10), Ar 1 each independently represents an aryl group or a heteroaryl group; Ar 2 each independently represents an aryl group having a substituent at at least one ortho-position, or a heteroaryl group having a substituent at at least one ortho-position. 【Chemistry 8】 In formula (Z-4), Rza 1 represents a hydrogen atom, an alkyl group or an alkoxy group; 1 ~Rb 4 each independently represents a hydrogen atom, an alkyl group, or an aryl group; 1 and Rzb 2 , Rzb 3 and Rzb 4 may be linked to form a ring structure, X represents O or NR, R represents a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group, Y 1 and Y 2 each independently represents CH or N.

9. The on-press development type lithographic printing plate precursor according to claim 1 or 2, wherein the image recording layer further comprises a compound represented by the following formula (Ph): 【Chemistry 9】 In the formula (Ph), X P represents O, S or NH; Y P represents N or CH; R P1 represents a hydrogen atom or an alkyl group; R P2 and R P3 each independently represents a halogen atom, an alkylthio group, an arylthio group, an alkoxy group, an aryloxy group, an alkyl group, an aryl group, an acylthio group, or an acyl group; mp and np each independently represent an integer of 0 to 4.

10. The on-press development type lithographic printing plate precursor according to claim 1 or 2, wherein the image recording layer further comprises a polymer having a structural unit represented by the following formula (I): 【Chemistry 10】 In formula (I), R 11 and R 12 each independently represents a hydrogen atom or an alkyl group; R 13 represents a hydrogen atom or a monovalent substituent; L 11 and L 12 each independently represents a single bond or a divalent linking group, and Rh represents a substituent containing two or more silicon atoms.

11. The on-press development type lithographic printing plate precursor according to claim 1 or 2, wherein the polymerizable compound comprises a polymerizable compound having seven or more functionalities.

12. The on-press development type lithographic printing plate precursor according to claim 1 or 2, wherein the image recording layer further contains an oil agent.

13. the support has an aluminum plate and an anodized aluminum coating disposed on the aluminum plate, the anodized film is located closer to the image recording layer than the aluminum plate, the anodized coating has micropores extending in a depth direction from a surface on the image recording layer side, The on-press development type lithographic printing plate precursor according to claim 1 or 2, wherein the micropores have an average diameter in the surface of the anodized film of more than 10 nm and not more than 100 nm.

14. the micropores are composed of large-diameter pores extending from the surface of the anodized coating to a depth of 10 nm to 1,000 nm, and small-diameter pores communicating with the bottoms of the large-diameter pores and extending from the communicating positions to a depth of 20 nm to 2,000 nm, the average diameter of the large diameter pores on the surface of the anodized film is 15 nm to 100 nm; The on-press development type lithographic printing plate precursor according to claim 13, wherein the small diameter pores have an average diameter of 13 nm or less at the communicating position.

15. a step of imagewise exposing the on-press development type lithographic printing plate precursor according to claim 1 or 2; and a step of removing the image recording layer in the non-image area by supplying at least one selected from the group consisting of printing ink and dampening water on the printing press. How to make a lithographic printing plate.

16. a step of imagewise exposing the on-press development type lithographic printing plate precursor according to claim 1 or 2; a step of removing the image recording layer in the non-image area by supplying at least one selected from the group consisting of a printing ink and a dampening water on a printing press to prepare a lithographic printing plate; and printing with the resulting lithographic printing plate. Lithographic printing method.

17. A compound represented by the following formula (1b): 【Chemistry 11】 In formula (1b), Rb 1 represents a substituted or unsubstituted alkyl group.

18. A compound represented by the following formula (2a): 【Chemistry 12】 In formula (2a), Rb 1 and Rb 3 each independently represents a substituted or unsubstituted alkyl group having 2 or more carbon atoms.

Citation Information

Patent Citations

  • Lithographic printing plate precursor and method of use

    US20210078350A1

  • On-machine-developing-type planographic printing plate original plate, method for manufacturing planographic printing plate, and planographic printing method

    WO2022019217A1