Polymerizable cholesteric liquid crystal composition, optically anisotropic film and electromagnetic wave reflection film

A polymerizable cholesteric liquid crystal composition without a fluorene skeleton, combining achiral and chiral compounds, addresses the heat resistance issue in optically anisotropic films, ensuring stable helical pitch in electromagnetic wave reflective films.

JP2024143937AActive Publication Date: 2024-10-11DAI NIPPON PRINTING CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023056896
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-11
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Optically anisotropic films made from polymerizable cholesteric liquid crystal compositions exhibit insufficient heat resistance, with the helical pitch changing due to heat exposure.

Method used

A polymerizable cholesteric liquid crystal composition is formulated without a polymerizable liquid crystal compound having a fluorene skeleton, incorporating an achiral polymerizable liquid crystal compound with a solid-liquid crystal phase transition temperature of 50°C to 120°C and a chiral polymerizable compound with a phase transition temperature of 60°C to 90°C, along with a photopolymerization initiator, and optionally including a solvent and leveling agent, to enhance heat resistance.

Benefits of technology

The composition forms an optically anisotropic film with improved heat resistance, maintaining uniformity of helical pitch even after heat exposure, suitable for electromagnetic wave reflective films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143937000024
    Figure 2024143937000024
  • Figure 2024143937000025
    Figure 2024143937000025
  • Figure 2024143937000026
    Figure 2024143937000026
Patent Text Reader

Abstract

To provide a polymerizable cholesteric liquid crystal composition capable of forming an optically anisotropic film having excellent heat resistance and an optically anisotropic film such as an electromagnetic wave reflection film using the polymerizable cholesteric liquid crystal composition.SOLUTION: There is provided a polymerizable cholesteric liquid crystal composition which comprises an achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50 to 120°C, a chiral polymerizable compound having a phase transition temperature of 60 to 90°C and a photopolymerization initiator and comprises no polymerizable liquid crystal compound having a fluorene skeleton.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a polymerizable cholesteric liquid crystal composition, and an optically anisotropic film and an electromagnetic wave reflective film using the liquid crystal composition. [Background technology]

[0002] In recent years, polymerizable liquid crystal compounds have been used in optically anisotropic films such as polarizing plates, polarizing reflectors, and retardation plates. This is because polymerizable liquid crystal compounds exhibit optical anisotropy in the liquid crystal state, and this anisotropy is fixed by polymerization. Since the optical properties required for optically anisotropic films differ depending on the purpose, various compounds are sometimes combined and used as polymerizable liquid crystal compositions to obtain properties suited to the purpose.

[0003] Patent Documents 1 and 2 disclose polymerizable liquid crystal compositions containing a polymerizable liquid crystal compound having a fluorene skeleton and an optically active compound. The polymerizable liquid crystal compositions containing these optically active compounds can be applied to various uses by controlling the type and amount of the optically active compound to change the helical pitch of the optically anisotropic film having a twisted alignment. The optically anisotropic film having a twisted alignment reflects light that matches the length of the helical pitch and the direction of rotation of the helix. When the length of the helical pitch is in the range of 380 nm to 780 nm, it reflects visible light. When the length of the helical pitch is longer than 780 nm, it reflects near infrared light and infrared light, and when the length of the helical pitch is shorter than 380 nm, it reflects ultraviolet light.

[0004] Known uses of optically anisotropic films include brightness enhancing films for displays (eg, Patent Document 3), near-infrared reflective layers (eg, Patent Document 4), and electromagnetic wave reflective films (eg, Patent Document 5). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-113131 A [Patent Document 2] JP 2015-110728 A [Patent Document 3] JP 2017-194709 A [Patent Document 4] JP 2009-522399 A [Patent Document 5] International Publication No. 2012 / 014552 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the optically anisotropic films, which are cured films of the polymerizable cholesteric liquid crystal compositions specifically described in Patent Documents 1 and 2, still have insufficient heat resistance and have the problem that the helical pitch is easily changed by heat. In view of the above-mentioned circumstances, an embodiment of the present disclosure aims to provide a polymerizable cholesteric liquid crystal composition capable of forming an optically anisotropic film having excellent heat resistance, and an optically anisotropic film, such as an electromagnetic wave reflective film, using the polymerizable cholesteric liquid crystal composition. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted intensive research to achieve the above object, and have found that heat resistance can be improved by forming a polymerizable cholesteric liquid crystal composition containing a chiral polymerizable compound having a specific phase transition temperature, an achiral polymerizable liquid crystal compound having a specific solid-liquid crystal phase transition temperature, and a photopolymerization initiator, but not containing a polymerizable liquid crystal compound having a fluorene skeleton, and have thus completed the present invention. That is, the present disclosure includes the following aspects.

[0008] [1] A polymerizable cholesteric liquid crystal composition comprising an achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50°C to 120°C, a chiral polymerizable compound having a phase transition temperature of 60°C to 90°C, and a photopolymerization initiator, and not containing a polymerizable liquid crystal compound having a fluorene skeleton. [2] The polymerizable cholesteric liquid crystal composition according to the above [1], further comprising a non-fluorinated leveling agent. [3] Further, the composition contains a solvent. The polymerizable cholesteric liquid crystal composition according to [1] or [2] above, wherein the solvent contains 30 mass% or more of a solvent having a boiling point within ±20°C of the phase transition temperature of the chiral polymerizable compound in the total solvent. [4] The polymerizable cholesteric liquid crystal composition according to any one of [1] to [3] above, wherein the achiral polymerizable liquid crystal compound is at least one selected from the group consisting of compounds represented by the following general formula (1):

[0009] [ka] In the general formula (1), Ar represents a 1,4-phenylene group or a naphthalene-2,6-diyl group. L 1 and L 2 each independently represents -O-, -S-, -COO-, -OCO-, -CH-CH-OCO-, -OCO-CH-CH-, -CH-OCO-, -OCO-CH-, or a single bond; A 1 and A 2 each independently represents a 1,4-phenylene group, a 1,4-cyclohexylene group, or a naphthalene-2,6-diyl group; The Ar and A 1 and A 2 Each of the groups may be one or more substituents E 1 may be substituted by the substituent E 1 is a halogen atom, a nitro group, a cyano group, a tetrazole group, an alkyl group having 1 to 7 carbon atoms, or an alkoxy group having 1 to 7 carbon atoms, R 1 and R 2 each independently represents a group selected from the following general formula (R-1): General formula (R-1): -L r1 -R sp1 -Z 1 In general formula (R-1), L r1represents -O-, -S-, -COO-, -OCO-, -OCOO-, or a single bond; R sp1 represents an alkylene group having 1 to 20 carbon atoms in which one -CH2- or two or more non-adjacent -CH2- may each be independently replaced by -O-, -COO-, or -OCO-, or a single bond; Z 1 represents a polymerizable functional group. n1 and n2 each independently represent an integer of 0 to 2, provided that n1+n2 is 1 or more; L 1 , L 2 , A 1 , and A 2 When there are a plurality of each, they may be the same or different.) [5] The polymerizable cholesteric liquid crystal composition according to any one of [1] to [4] above, wherein the chiral polymerizable compound is at least one selected from the group consisting of compounds represented by the following general formula (2):

[0010] [ka] (In the general formula (2), L 3 and L 4 each independently represents -O-, -S-, -COO-, -OCO-, or a single bond; A 3 and A 4 each independently represents a 1,4-phenylene group, a 1,4-cyclohexylene group, or a naphthalene-2,6-diyl group; R 3 and R 4 each independently represents a group selected from the following general formula (R-2): General formula (R-2): -L r2 -R sp2 -Z 2 In general formula (R-2), L r2 represents -O-, -S-, -COO-, -OCO-, -OCOO-, or a single bond; R sp2represents an alkylene group having 1 to 20 carbon atoms in which one -CH2- or two or more non-adjacent -CH2- may each be independently replaced by -O-, -COO-, or -OCO-, or a single bond; Z 2 represents a polymerizable functional group. Substituent E 2 and E 3 each independently represents an alkyl group having 1 to 3 carbon atoms or a halogen; n3 and n4 each independently represent an integer of 1 to 3, and m1 and m2 each independently represent an integer of 0 to 2; L 3 , L 4 , A 3 , and A 4 When there are a plurality of each, they may be the same or different.)

[0011] [6] An optically anisotropic film which is a cured film of the polymerizable cholesteric liquid crystal composition according to any one of the above [1] to [5]. [7] An electromagnetic wave reflective film which is a cured film of a polymerizable cholesteric liquid crystal composition, After heating the electromagnetic wave reflective film at 90°C for 72 hours, An electromagnetic wave reflective film, wherein the helical pitch of the cholesteric liquid crystal in a cured film of the polymerizable cholesteric liquid crystal composition satisfies the following formulae (A-1), (A-2), and (A-3): P1-P1×0.05≦P2≦P1+P1×0.05 (A-1) P1-P1×0.05≦P3≦P1+P1×0.05 (A-2) P2-P2×0.05≦P1≦P2+P2×0.05 (A-3) (Here, P1 represents the length of the helical pitch including the position of the first surface of the cured film, P2 represents the length of the helical pitch including the position of the second surface of the cured film opposite to the first surface, and P3 represents the length of the helical pitch including the position of the center of the cured film in the layer thickness direction.) [8] The electromagnetic wave reflective film according to [7] above, wherein the polymerizable cholesteric liquid crystal composition is the polymerizable cholesteric liquid crystal composition according to any one of [1] to [5] above. Effect of the Invention

[0012] According to an embodiment of the present disclosure, it is possible to provide a polymerizable cholesteric liquid crystal composition capable of forming an optically anisotropic film having excellent heat resistance, and an optically anisotropic film, such as an electromagnetic wave reflective film, using the polymerizable cholesteric liquid crystal composition. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of an electromagnetic wave reflecting film of the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing one embodiment of a laminate including an electromagnetic wave reflecting film of the present disclosure. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing one embodiment of a laminate including an electromagnetic wave reflecting film of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiments and examples of the present disclosure will be described with reference to the drawings. However, the present disclosure can be implemented in many different forms, and is not to be interpreted as being limited to the description of the embodiments and examples exemplified below. In addition, in order to make the explanation clearer, the drawings may be schematic in terms of the width, thickness, shape, etc. of each part compared to the actual form, but these are merely examples and do not limit the interpretation of the present disclosure. In addition, in this specification and each figure, elements similar to those described above with respect to the previous figures may be given the same reference numerals, and detailed explanations may be omitted as appropriate. In addition, for convenience of explanation, the terms "upper" and "lower" may be used in the explanation, but the up-down direction may be reversed. "In this specification, when a certain component or region is described as being "on (or under)" another component or region, unless otherwise specified, this includes not only the case where it is directly on (or directly under) the other component, but also the case where it is above (or below) the other component, i.e., the case where another component is included between the other component and the component above (or below) the other component.

[0015] In the present disclosure, the alignment regulation force refers to the action of aligning liquid crystal compounds in a specific direction. In the present disclosure, (meth)acrylic refers to either acrylic or methacrylic, and (meth)acrylate refers to either acrylate or methacrylate. In addition, in this specification, the terms "plate," "sheet," and "film" are not distinguished from one another solely based on the difference in name, and a "film surface (plate surface, sheet surface)" refers to a surface that coincides with the planar direction of the target film-like (plate-like, sheet-like) member when viewed overall and globally. In addition, in the present disclosure, the use of "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0016] A. Polymerizable cholesteric liquid crystal composition The polymerizable cholesteric liquid crystal composition of the present disclosure contains an achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50°C to 120°C, a chiral polymerizable compound having a phase transition temperature of 60°C to 90°C, and a photopolymerization initiator, but does not contain a polymerizable liquid crystal compound having a fluorene skeleton.

[0017] The polymerizable cholesteric liquid crystal composition of the present disclosure contains an achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50° C. to 120° C. in combination with a chiral polymerizable compound having a phase transition temperature of 60° C. to 90° C., and does not contain a polymerizable liquid crystal compound having a fluorene skeleton, so that the polymerizable cholesteric liquid crystal composition has improved heat resistance and can suppress the variation of the helical pitch before and after a heat resistance test. The mechanism by which the heat resistance is improved is still unknown, but is presumed to be as follows. The solid-liquid crystal phase transition temperature of most achiral polymerizable liquid crystal compounds is about 50°C to 180°C, but when the compound is dissolved in a solution and a coating film is formed to form a liquid crystal phase, the phase transition tends to occur at a temperature lower than the solid-liquid crystal phase transition temperature. On the other hand, resin substrates such as polyethylene terephthalate (PET) substrates and triacetyl cellulose (TAC) substrates are often used as substrates for forming a cured film of the polymerizable liquid crystal composition, but such resin substrates are prone to heat wrinkles when heated at high temperatures. Therefore, the polymerizable liquid crystal composition is applied onto a substrate and heated at a temperature of usually 60°C to 120°C, preferably 110°C or less or 100°C or less, to dry the solvent and align the liquid crystal, thereby forming a coating film of the polymerizable liquid crystal composition. The polymerizable cholesteric liquid crystal composition of the present disclosure contains an achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50°C to 120°C in combination with a chiral polymerizable compound having a phase transition temperature of 60°C to 90°C. Therefore, when a coating film of the polymerizable cholesteric liquid crystal composition is formed and then heated at a normal preferred temperature, the chiral polymerizable compound having a phase transition temperature of 60°C to 90°C undergoes phase transition first, or the chiral polymerizable compound and the achiral polymerizable liquid crystal compound undergo phase transition simultaneously. In such a case, the molecular motion of the chiral polymerizable compound becomes active, and a good mixed state of the chiral polymerizable compound and the polymerizable liquid crystal compound is obtained, and a coating film having a uniform concentration of the chiral polymerizable compound and the polymerizable liquid crystal compound in the film thickness direction is obtained. In such a well-mixed coating film, the polymerizable liquid crystal compound is oriented, and then polymerization between the chiral polymerizable compound and the polymerizable liquid crystal compound proceeds, thereby improving the polymerization rate between the chiral polymerizable compound and the polymerizable liquid crystal compound. As a result, a cured film of the liquid crystal composition can be obtained which has high uniformity of the helical pitch in the film thickness direction and high heat resistance, and which has a high uniformity of the helical pitch in the film thickness direction even after a heat resistance test. In addition, since the phase transition temperature of the chiral polymerizable compound is set to 60°C or higher, the purity of the chiral polymerizable compound can be easily improved, bleeding in the coating film is less likely, and heat resistance can be ensured.

[0018] On the other hand, if the phase transition temperature of the chiral polymerizable compound is higher than 90°C, it becomes difficult to obtain a good mixed state between the chiral polymerizable compound and the polymerizable liquid crystal compound, and the polymerization rate between the chiral polymerizable compound and the polymerizable liquid crystal compound also becomes low, which is considered to result in low heat resistance. In addition, since the polymerizable liquid crystal compound having a fluorene skeleton has a rigid structure and therefore has low solubility in a solvent and low compatibility with a chiral polymerizable compound, it is considered that the polymerization rate between the chiral polymerizable compound and the polymerizable liquid crystal compound is insufficient, resulting in low heat resistance (Comparative Example described later). Therefore, it is considered that the polymerizable cholesteric liquid crystal composition of the present disclosure has improved heat resistance by not containing a polymerizable liquid crystal compound having a fluorene skeleton.

[0019] The polymerizable cholesteric liquid crystal composition of the present disclosure contains at least an achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50°C to 120°C, a chiral polymerizable compound having a phase transition temperature of 60°C to 90°C, and a photopolymerization initiator, and does not contain a polymerizable liquid crystal compound having a fluorene skeleton, but preferably further contains a solvent. It may further contain a leveling agent. Furthermore, it may further contain other components within a range that does not impair the effect. Hereinafter, each component constituting the polymerizable liquid crystal composition of the present disclosure will be described in order.

[0020] 1. Achiral polymerizable liquid crystal compound with a solid-liquid crystal phase transition temperature of 50℃ to 120℃ The achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50° C. to 120° C. can be appropriately selected from conventionally known polymerizable liquid crystal compounds having no asymmetric carbon atom. In the present disclosure, the solid-liquid crystal phase transition temperature means the temperature at which a liquid crystal compound changes from a solid to a liquid crystal. In the present disclosure, the solid-liquid crystal phase transition temperature of a liquid crystal compound is measured using a differential scanning calorimeter (DSC). The measurement method using a differential scanning calorimeter (DSC) can be used to measure even when two or more liquid crystal compounds are mixed or when a chiral polymerizable compound described below is mixed. In the present disclosure, the solid-liquid crystal phase transition temperature of a liquid crystal compound is specifically measured by the following method. The measurement is performed in accordance with JIS K7121-1987, 8. The phase transition temperature is the extrapolated melting onset temperature (Tim) in accordance with JIS K7121-1987, 9.1(2). However, the method of preparing a sample by distilling off the solvent and the heating and cooling program (heating rate, cooling rate, heating start temperature, end temperature) are performed as follows. First, the solvent is removed from the liquid crystal composition using a rotary evaporator to obtain a measurement sample. 5 mg of the measurement sample is sealed in an aluminum sample pan, and then set in a DSC. Under a nitrogen atmosphere, the sample is cooled from 25°C to -10°C at a rate of -25°C / min, and maintained at -10°C for 15 minutes. Thereafter, as a first heating step, the sample is heated from -10°C to 150°C at a rate of 10°C / min, and maintained at 150°C for 1 minute. As a first cooling step, the sample is cooled from 150°C to -10°C at a rate of -10°C / min, and maintained at -10°C for 10 minutes. Thereafter, as a second heating step, the sample is heated from -10°C to 150°C at a rate of 10°C / min, and maintained at 150°C for 1 minute. As a second cooling step, the sample is cooled from 150°C to 25°C at a rate of -10°C / min. The endothermic onset temperature detected during the second heating step, i.e., the extrapolated melting onset temperature (Tim), which is the temperature at the intersection of a straight line extending the low-temperature baseline to the high-temperature side and a tangent line drawn at the point where the slope of the curve on the low-temperature side of the melting peak is maximum, is taken as the phase transition temperature.

[0021] In addition, the DSC measurements in the present examples and comparative examples were both performed with the upper limit temperature set to 150° C. However, in the case of a compound that initiates polymerization by 150° C., the upper limit temperature of the DSC measurement is changed to be lower than the polymerization initiation temperature of the compound. In this case, whether or not the compound is polymerized is observed according to the following steps i) to iii) to determine the upper limit temperature during DSC measurement. i) The temperature reached in the first heating run is set to 150°C, and if no peak is detected in the second heating run or the peak area becomes significantly smaller, a new DSC measurement is performed under conditions in which the temperature reached in the first heating run is 5°C lower. ii) If no peak is detected in the second heating cycle even when the temperature reached in the first heating cycle is lowered by 5°C, or if the peak area becomes significantly smaller, perform DSC measurement again under conditions in which the temperature reached in the first heating cycle is further lowered by 5°C. iii) Repeat step ii) above until a peak is detected in the second heating. The temperature at which a peak can be detected in the second heating is set as the upper limit temperature for DSC measurement (upper limit of heating temperature).

[0022] In the present disclosure, the achiral polymerizable liquid crystal compound may be a polymerizable liquid crystal compound having a polymerizable functional group at at least one end of a mesogenic group, but from the viewpoint of improving heat resistance, it is more preferable that the compound is a polymerizable liquid crystal compound having a polymerizable functional group at both ends of a mesogenic group. A polymerizable liquid crystal compound having two or more polymerizable functional groups in one molecule can improve the hardness and durability of a coating film. Examples of polymerizable liquid crystal compounds having two or more polymerizable functional groups in one molecule include nematic monoacrylate 2 described in Nature vol 378, page 467-469 (1995); (17) to (28) described in paragraph 0013 of JP-A-2002-145830, (a-1) to (a-35) described in paragraph 0018, (a-36) to (a-63) described in paragraph 0022; Chemical 74 described in paragraph 0336 of WO 2022 / 215751 and Chemical 75 described in paragraph 0337; and compounds described in M5, M6, and M7 described in DIC Technical Review 2001 P38. These can be appropriately selected and used. Examples of the achiral polymerizable liquid crystal compound used in the present disclosure include polymerizable liquid crystal compounds selected from the group consisting of compounds represented by the following general formula (1).

[0023] [ka] In the general formula (1), Ar represents a 1,4-phenylene group or a naphthalene-2,6-diyl group. L 1 and L 2each independently represents -O-, -S-, -COO-, -OCO-, -CH-CH-OCO-, -OCO-CH-CH-, -CH-OCO-, -OCO-CH-, or a single bond; A 1 and A 2 each independently represents a 1,4-phenylene group, a 1,4-cyclohexylene group, or a naphthalene-2,6-diyl group; The Ar and A 1 and A 2 Each of the groups may be one or more substituents E 1 and the substituent E 1 is a halogen atom, a nitro group, a cyano group, a tetrazole group, an alkyl group having 1 to 7 carbon atoms, or an alkoxy group having 1 to 7 carbon atoms, R 1 and R 2 each independently represents a group selected from the following general formula (R-1): General formula (R-1): -L r1 -R sp1 -Z 1 In general formula (R-1), L r1 represents -O-, -S-, -COO-, -OCO-, -OCOO-, or a single bond; R sp1 represents an alkylene group having 1 to 20 carbon atoms in which one -CH2- or two or more non-adjacent -CH2- may each be independently replaced by -O-, -COO-, or -OCO-, or a single bond; Z 1 represents a polymerizable functional group. n1 and n2 each independently represent an integer of 0 to 2, provided that n1+n2 is 1 or more; L 1 , L 2 , A 1 , and A 2 When there are a plurality of each, they may be the same or different.)

[0024] L 1 and L 2each independently represents -O-, -S-, -COO-, -OCO-, -CH2-CH2-OCO-, -OCO-CH2-CH2-, -CH2-OCO-, -OCO-CH2-, or a single bond; from the viewpoint of availability of raw materials and ease of synthesis, it is preferable that each independently represents -O-, -COO-, -OCO-, or a single bond, and when a plurality of these are present, they may be the same or different.

[0025] A 1 and A 2 In the formula, 1,4-cyclohexylene is L 1 , L 2 Or L r1 There may be stereoisomers of cis and trans configurations based on the difference in the configuration of the carbon atom bonded to 1,4-cyclohexylene. 1,4-cyclohexylene may be either cis or trans, or may be a mixture of cis and trans isomers, but because of good orientation, it is preferably trans or cis, and more preferably trans.

[0026] n1 and n2 each independently represent an integer of 0 to 2, and n1+n2 is 1 or more, but may be 2 or more and may be 3 or less.

[0027] In general formula (R-1), R sp1 Specifically, from the viewpoint of availability of raw materials and ease of synthesis, it is more preferable that each independently represent an alkylene group having 1 to 12 carbon atoms which may be replaced by one -CH2- or two or more non-adjacent -CH2-, each independently represent an alkylene group having 1 to 12 carbon atoms or a single bond, further more preferably each independently represent an alkylene group having 2 to 10 carbon atoms, and particularly preferably each independently represent an alkylene group having 2 to 6 carbon atoms, and when there are a plurality of -CH2-, they may be the same or different.

[0028] In general formula (R-1), L r1represents -O-, -S-, -COO-, -OCO-, -OCOO-, or a single bond; however, from the viewpoint of availability of raw materials and ease of synthesis, it is preferable that each independently represent -O-, -COO-, -OCO-, -OCOO-, or a single bond, and when a plurality of these are present, they may be the same or different.

[0029] In general formula (R-1), Z 1 represents a polymerizable functional group. The polymerizable functional group used in the present disclosure can be any group used in conventional polymerizable liquid crystal compounds without any restrictions. Examples of the polymerizable functional group include cyclic ether-containing groups such as oxirane rings and oxetane rings, and ethylenic double bond-containing groups. Among them, ethylenic double bond-containing groups are preferred because they exhibit photocurability and are easy to handle. Z 1 The polymerizable functional groups in each of the formulas (Z-1) to (Z-7) are preferably independently selected from the following formulas (Z-1) to (Z-7). In the following formulas (Z-1) to (Z-7), * (asterisk) represents R sp1 The bond position is shown.

[0030] [ka] (In formulas (Z-1) to (Z-7), R z are each independently a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, a methyl group, an ethyl group, or a trifluoromethyl group.

[0031] When using ultraviolet polymerization as the polymerization method, Z 1 is preferably the formula (Z-1), the formula (Z-2), the formula (Z-3), the formula (Z-5), or the formula (Z-7), more preferably the formula (Z-1), the formula (Z-3), or the formula (Z-7), further preferably the formula (Z-1). In the formula (Z-1), R z It is more preferable that is a hydrogen atom, a methyl group or a trifluoromethyl group.

[0032] The Ar and A 1 and A 2Substituent E which may be substituted with 1 Examples of the alkyl group include halogen, a nitro group, a cyano group, a tetrazole group, an alkyl group having 1 to 7 carbon atoms, and an alkoxy group having 1 to 7 carbon atoms. The halogen may be fluorine, chlorine, bromine or iodine, preferably fluorine, chlorine or bromine. The alkyl group having 1 to 7 carbon atoms may be either linear or branched, and examples thereof include linear alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, and an n-heptyl group, and branched alkyl groups such as an i-propyl group, an i-butyl group, a t-butyl group, and a 2-methylbutyl group. The alkyl group may be an alkyl group having 1 to 5 carbon atoms, or an alkyl group having 1 to 3 carbon atoms. The alkoxy group having 1 to 7 carbon atoms is, for example, -OR a (where R a is an alkyl group having 1 to 7 carbon atoms, -OR a R in a Examples of the alkyl group include the same as the alkyl group having 1 to 7 carbon atoms, and may be an alkoxy group having 1 to 5 carbon atoms or an alkoxy group having 1 to 3 carbon atoms. Substituent E 1 The number of Ar, A 1 and A 2 Each of these may be 0 to 3, 0 to 2, or 0 or 1.

[0033] A mesogenic group contained in a polymerizable liquid crystal compound, or -(A 1 -L 1 ) n1 -Ar-(L 2 -A 2 ) n2 As the -, partial structures represented by the following chemical formulae (m-1) to (m-11) are preferably used, and among them, partial structures represented by at least one selected from the group consisting of the following chemical formulae (m-2), (m-3), (m-5), (m-7), (m-8), and (m-10) are preferably used from the viewpoint of solvent solubility. The hydrogen atoms in the phenylene group and naphthylene group in the partial structures represented by the following chemical formulae (m-1) to (m-11) can be substituted with the above-mentioned substituent E1 may be substituted by:

[0034] [ka]

[0035] The achiral polymerizable liquid crystal compound used in the present disclosure is represented by the general formula (1) R 1 -(A 1 -L 1 ) n1 -Ar-(L 2 -A 2 ) n2 -R 2 Specific examples of the polymerizable liquid crystal compounds that have the structures shown in the following table Lc-1 to Lc-120 and have a solid-liquid crystal phase transition temperature of 50°C to 120°C can be used, but are not limited to these.

[0036] [Table 1]

[0037] [Table 2]

[0038] [Table 3]

[0039] In the structures represented by Lc-1 to Lc-120, R sp1 In the formula, n is 1 to 20, among which R sp1 In the formula, n is preferably 2 or more, and more preferably 4 or more, while it is preferably 12 or less, and more preferably 10 or less, and may be 6 or less. Also, Z 1 In the formula (Z-1), R z are each independently preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom. In the structures represented by Lc-1 to Lc-120, R 1 and R 2 may be different, e.g. R sp1 The n in may be different.

[0040] Furthermore, in the structures represented by Lc-1 to Lc-120, Ar is a 1,4-phenylene group or a naphthalene-2,6-diyl group, A 1 and A 2 Each of the 1,4-phenylene group and the naphthalene-2,6-diyl group may be one or more of the substituents E 1 The Ar and A may be substituted. 1 and A 2 Specifically, the 1,4-phenylene group or the naphthalene-2,6-diyl group may each have the following structure, for example:

[0041] [ka]

[0042] In addition, the solid-liquid crystal phase transition temperature of the achiral polymerizable liquid crystal compound used in the present disclosure having a solid-liquid crystal phase transition temperature of 50°C to 120°C is preferably 50°C to 100°C, may be 50°C to 90°C, or may be 50°C to 80°C, from the viewpoint of the load on a production device for aligning the liquid crystal.

[0043] In addition, the achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50° C. to 120° C. used in the present disclosure is preferably soluble in at least one solvent selected from the group consisting of methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone at a concentration of 10% by mass or more, and more preferably soluble at 20% by mass or more, in view of improving the solvent solubility of the polymerizable cholesteric liquid crystal composition. When the solvent solubility of the polymerizable liquid crystal composition is improved, a uniform coating film is easily formed when the polymerizable cholesteric liquid crystal composition is used to form a coating film, and the load on the manufacturing process and manufacturing equipment for drying the solvent is reduced, the options for usable substrates are expanded, and the process margin during alignment is expanded, resulting in more uniform and better alignment.

[0044] In the present disclosure, in order to improve heat resistance, the polymerizable liquid crystal compound having a fluorene skeleton is not contained. Here, the polymerizable liquid crystal compound having a fluorene skeleton refers to a compound having a fluorene skeleton represented by the following structure, among polymerizable liquid crystal compounds having a polymerizable functional group at at least one end of a mesogen group.

[0045] [ka] (In the formula, W 11 each independently represents a hydrogen atom or a substituent.

[0046] The achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50° C. to 120° C. used in the present disclosure can be synthesized by a conventionally known synthesis method, and can be synthesized by appropriately referring to Makromol. Chem., 190, 3201-3215 (1989), Makromol. Chem., 190, 2255-2268 (1989), International Publication No. 97 / 000600, U.S. Patent No. 5770107, JP-A No. 2004-231638, etc. In addition, the achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50° C. to 120° C. may be appropriately selected from commercially available products.

[0047] The achiral polymerizable liquid crystal compounds having a solid-liquid crystal phase transition temperature of 50° C. to 120° C. used in the present disclosure may be used alone or in combination of two or more. The content ratio of the achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50°C to 120°C used in the present disclosure may be appropriately adjusted to adjust the desired optical anisotropy, etc., and is not limited thereto, and may be 75% by mass to 99% by mass, 85% by mass to 96% by mass, or 90% by mass to 96% by mass, based on the total solid content of the polymerizable cholesteric liquid crystal composition.

[0048] In the polymerizable cholesteric liquid crystal composition of the present disclosure, a liquid crystal compound other than the achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50° C. to 120° C. may be used within a range in which the effects of the present invention are not impaired. As the liquid crystal compound other than the achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50° C. to 120° C., a conventionally known liquid crystal compound can be used. In the polymerizable cholesteric liquid crystal composition of the present disclosure, the achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50° C. to 120° C. is preferably 50% by mass or more, may be 70% by mass or more, may be 80% by mass or more, or may be 100% by mass, based on the total amount of the achiral liquid crystal compound, from the viewpoint of improving heat resistance.

[0049] 2. Chiral polymerizable compound with a phase transition temperature of 60℃ to 90℃ The chiral polymerizable compound has a function of inducing a helical structure of a cholesteric liquid crystal phase as a chiral agent. The chiral polymerizable compound (chiral agent) generally contains an asymmetric carbon atom, but may be an axially asymmetric compound or a planarly asymmetric compound that does not contain an asymmetric carbon atom. The chiral polymerizable compound may or may not exhibit liquid crystallinity. When the chiral polymerizable compound exhibits liquid crystallinity, the phase transition temperature is a solid-liquid crystal phase transition temperature, and when the chiral polymerizable compound does not exhibit liquid crystallinity, the phase transition temperature is a solid-liquid phase transition temperature. The solid-liquid phase transition temperature of the chiral polymerizable compound is measured in the same manner as the achiral polymerizable liquid crystal compound. When the chiral polymerizable compound does not exhibit liquid crystallinity, the solid-liquid phase transition temperature is also measured using a differential scanning calorimeter (DSC) in the same manner as the achiral polymerizable liquid crystal compound. A measurement sample is set in the DSC, and heating and cooling are repeated twice, and the endothermic onset temperature (extrapolated melting onset temperature) detected in the second heating is taken as the phase transition temperature of the chiral polymerizable compound. The upper limit of the measurement temperature is determined to be lower than the polymerization onset temperature measured by measuring the polymerization onset temperature of the compound.

[0050] In the present disclosure, since both the chiral polymerizable compound and the polymerizable liquid crystal compound have a polymerizable functional group, a polymer can be formed by a polymerization reaction between the chiral polymerizable compound and the polymerizable liquid crystal compound, and the heat resistance can be improved. Therefore, it is preferable that the polymerizable functional group of the chiral polymerizable compound is the same type of group as the polymerizable functional group of the polymerizable liquid crystal compound. That is, when the polymerizable functional group of the polymerizable liquid crystal compound is a radical polymerizable group such as the unsaturated polymerizable group as in (Z-1) and (Z-2), the polymerizable functional group of the chiral polymerizable compound is also a radical polymerizable group, and when the polymerizable functional group of the polymerizable liquid crystal compound is a cationic polymerizable group as in (Z-3) to (Z-7), the polymerizable functional group of the chiral polymerizable compound may also be a cationic polymerizable group.

[0051] In the present disclosure, examples of the chiral polymerizable compound having a phase transition temperature of 60° C. to 90° C. can be appropriately selected from the compounds described in, for example, the chiral polymerizable compounds having a phase transition temperature of 60° C. to 90° C. described in paragraphs

[0127] to

[0139] of JP-A No. 2015-135474, the chiral polymerizable compounds having a phase transition temperature of 60° C. to 90° C. described in paragraph

[0209] of JP-A No. 2015-127793, and the chiral polymerizable compounds having a phase transition temperature of 60° C. to 90° C. described in paragraph

[0210] of JP-A No. 2015-110728. The chiral polymerizable compound used in the present disclosure may, for example, be a polymerizable compound selected from the group consisting of compounds represented by the following general formula (2).

[0052] [ka] (In the general formula (2), L 3 and L 4 each independently represents -O-, -S-, -COO-, -OCO-, or a single bond; A 3 and A 4 each independently represents a 1,4-phenylene group, a 1,4-cyclohexylene group, or a naphthalene-2,6-diyl group; R 3 and R 4 each independently represents a group selected from the following general formula (R-2): General formula (R-2): -L r2 -R sp2 -Z 2 In general formula (R-2), L r2 represents -O-, -S-, -COO-, -OCO-, or a single bond; R sp2 represents an alkylene group having 1 to 20 carbon atoms in which one -CH2- or two or more non-adjacent -CH2- may each be independently replaced by -O-, -COO-, or -OCO-, or a single bond; Z 2 represents a polymerizable functional group. Substituent E 2 and E 3 each independently represents an alkyl group having 1 to 3 carbon atoms or a halogen; n3 and n4 each independently represent an integer of 1 to 3, and m1 and m2 each independently represent an integer of 0 to 2; L 3 , L 4 , A 3 , and A 4 When there are a plurality of each, they may be the same or different.)

[0053] L 3 and L 4each independently represents -O-, -S-, -COO-, -OCO-, or a single bond; from the viewpoint of availability of raw materials and ease of synthesis, it is preferable that each independently represents -O-, -COO-, -OCO-, or a single bond, and when a plurality of groups are present, they may be the same or different.

[0054] A 3 and A 4 In the formula, 1,4-cyclohexylene is A 1 and A 2 It may be the same as 1,4-cyclohexylene in the above. In addition, in the general formula (R-2), L r2 , R sp2 , Z 2 respectively represent L in the general formula (R-1) of the general formula (1). r1 , R sp1 , Z 1 It may be similar to:

[0055] n3 and n4 each independently represent 1 to 3, and may be appropriately selected depending on the phase transition temperature.

[0056] Substituent E 2 and E 3 In the above, the alkyl group having 1 to 3 carbon atoms or the halogen atom is preferably the above-mentioned substituent E 1 Examples of the above-mentioned examples are as follows. m1 and m2 each independently represent 0 to 2, and may be 0 or 1.

[0057] The chiral polymerizable compound used in the present disclosure is represented by the general formula (2) -(L 3 -A 3 ) n3 -R 3 and -(L 4 -A 4 ) n4 -R 4 Specific examples of the polymerizable compound that can be used include those having the structures shown in Ch-1 to Ch-60 in the following table and having a phase transition temperature of 60° C. to 90° C., but are not limited thereto. In the table, L for n3 and n4=13 / L 4 is the side that is bound to the binaphthalene moiety. For example, in Ch-13, n3 and n4=2, and A 3 / A 4 But R 3 / R 4 It represents that it is bonded to

[0058] [Table 4]

[0059] In the structures represented by Ch-1 to Ch-60, R sp2 In the formula, n is 1 to 20, among which R sp2 In the formula, n is preferably 2 or more, and more preferably 4 or more, while it is preferably 12 or less, and more preferably 10 or less, and may be 6 or less. Also, Z 2 In the formula (Z-1), R z are each independently preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom. In the structures represented by Ch-1 to Ch-60, R 3 and R 4 may be different, e.g. R sp2 The n in may be different.

[0060] In addition, in the compound represented by the general formula (2), each binaphthalene has one or more of the substituents E 1 Specifically, for example, it may have the following structure:

[0061] [ka]

[0062] In addition, examples of the chiral polymerizable compound having a phase transition temperature of 60°C to 90°C used in the present invention are not limited to the polymerizable compound represented by the general formula (2) above, and for example, the following polymerizable compounds can be used.

[0063] [ka]

[0064] The phase transition temperature of the chiral polymerizable liquid crystal compound used in the present disclosure having a phase transition temperature of 60° C. to 90° C. may be 60° C. to 80° C. in view of the load on a production device that causes phase transition of the liquid crystal mixture by heating.

[0065] In addition, the chiral polymerizable liquid crystal compound having a phase transition temperature of 60° C. to 90° C. used in the present disclosure is preferably soluble in at least one solvent selected from the group consisting of methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone at a concentration of 10% by mass or more, and more preferably soluble at 20% by mass or more, in view of improving the solvent solubility of the polymerizable cholesteric liquid crystal composition. When the solvent solubility of the polymerizable liquid crystal composition is improved, a uniform coating film is easily formed when the polymerizable cholesteric liquid crystal composition is used to form a coating film, and the load on the manufacturing process and manufacturing equipment for drying the solvent is reduced, the options for usable substrates are expanded, and the process margin during alignment is expanded, resulting in more uniform and better alignment.

[0066] The chiral polymerizable compound having a phase transition temperature of 60° C. to 90° C. used in the present disclosure can be synthesized by a conventionally known synthesis method, for example, by appropriately referring to JP-A-2005-263778, GB2298202, DE19843724, etc. In addition, the chiral polymerizable compound having a phase transition temperature of 60° C. to 90° C. may be appropriately selected from commercially available products and used.

[0067] The chiral polymerizable compounds having a phase transition temperature of 60° C. to 90° C. used in the present disclosure may be used alone or in combination of two or more. The content ratio of the chiral polymerizable compound having a phase transition temperature of 60°C to 90°C used in the present disclosure may be appropriately adjusted to adjust the desired optical anisotropy, etc., and is not limited thereto, and may be 0.01% by mass to 15% by mass, 1% by mass to 10% by mass, or 1% by mass to 5% by mass relative to the total solid content of the polymerizable cholesteric liquid crystal composition.

[0068] In the polymerizable cholesteric liquid crystal composition of the present disclosure, a chiral compound different from the chiral polymerizable compound having a phase transition temperature of 60° C. to 90° C. may be used within a range in which the effects of the present invention are not impaired. As the chiral compound different from the chiral polymerizable compound having a phase transition temperature of 60° C. to 90° C., a chiral agent of a conventionally known cholesteric liquid crystal composition can be used. However, in the polymerizable cholesteric liquid crystal composition of the present disclosure, the chiral polymerizable compound having a phase transition temperature of 60° C. to 90° C. is preferably 90% by mass or more, and may be 100% by mass, based on the total amount of the chiral compound, from the viewpoint of improving heat resistance.

[0069] 3. Photopolymerization initiator In the present disclosure, the photopolymerization initiator can be appropriately selected from conventionally known ones according to the polymerizable functional groups of the achiral polymerizable liquid crystal compound and the chiral polymerizable compound. When the polymerizable functional group of the achiral polymerizable liquid crystal compound and the chiral polymerizable compound is a radical polymerizable group, a radical polymerization initiator can be used, and when the polymerizable functional group is a cationic polymerizable group, a cationic polymerization initiator can be used.

[0070] Specific examples of such photopolymerization initiators include aromatic ketones including thioxanthone and the like, α-aminoalkylphenones, α-hydroxyketones, acylphosphine oxides, oxime esters, aromatic onium salts, organic peroxides, thio compounds, hexaarylbiimidazole compounds, ketoxime ester compounds, borate compounds, azinium compounds, metallocene compounds, active ester compounds, compounds having a carbon-halogen bond, and alkylamine compounds. Among these, at least one selected from the group consisting of acylphosphine oxide-based polymerization initiators, α-aminoalkylphenone-based polymerization initiators, α-hydroxyketone-based polymerization initiators, and oxime ester-based polymerization initiators is preferred because it hardens to the inside of the coating film and improves durability.

[0071] Examples of the acylphosphine oxide polymerization initiator include bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide (e.g., trade name: Irgacure 819, manufactured by BASF), bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphenylphosphine oxide, and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (trade name: Lucirin TPO, manufactured by BASF, etc.).

[0072] Examples of the α-aminoalkylphenone polymerization initiator include 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one (e.g., Irgacure 907, manufactured by BASF), 2-benzyl-2-(dimethylamino)-1-(4-morpholinophenyl)-1-butanone (e.g., Irgacure 369, manufactured by BASF), and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone (Irgacure 379EG, manufactured by BASF).

[0073] Examples of the α-hydroxyketone polymerization initiator include 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propan-1-one (e.g., trade name: Irgacure 127, manufactured by BASF, etc.), 2-hydroxy-4'-hydroxyethoxy-2-methylpropiophenone (e.g., trade name: Irgacure 2959, manufactured by BASF, etc.), 1-hydroxy-cyclohexyl-phenyl-ketone (e.g., trade name: Irgacure 184, manufactured by BASF, etc.), and oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone} (e.g., trade name: ESACURE ONE, manufactured by Lamberti, etc.).

[0074] Examples of the oxime ester polymerization initiator include 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)] (trade name: Irgacure OXE-01, manufactured by BASF), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyloxime) (trade name: Irgacure OXE-02, manufactured by BASF), methanone, ethanone, 1-[9-ethyl-6-(1,3-dioxolane, 4-(2-methoxyphenoxy)-9H-carbazol-3-yl]-, 1-(o-acetyloxime) (trade name: ADEKA OPT-N-1919, manufactured by ADEKA Corporation).

[0075] In the present disclosure, the photopolymerization initiator may be used alone or in combination of two or more. In the present disclosure, the content of the photopolymerization initiator may be 0.5% by mass to 10% by mass, 0.5% by mass to 8% by mass, or 0.5% by mass to 5% by mass, relative to the total solid content of the polymerizable cholesteric liquid crystal composition, in order to promote curing of the polymerizable compound.

[0076] 4.Leveling agent The polymerizable cholesteric liquid crystal composition of the present disclosure may further contain a leveling agent from the viewpoint of making the surface tension of the coating film uniform and improving the coatability. From the viewpoint of making the surface tension of the coating film uniform and improving the coatability, the leveling agent may be a nonionic surfactant, and examples of the nonionic surfactant include vinyl-based, silicone-based, fluorine-based, and hydrocarbon-based surfactants. In order to make the surface tension of the coating film uniform and improve the coating property, the leveling agent used in the polymerizable cholesteric liquid crystal composition of the present disclosure is preferably a non-fluorine-based leveling agent. Examples of the non-fluorine-based leveling agent include vinyl-based, silicone-based, and hydrocarbon-based surfactants. When a non-fluorine-based leveling agent is used, there is a tendency that the reflectance increases and the haze is reduced.

[0077] Examples of the vinyl surfactant include polyalkyl acrylate, polyalkyl methacrylate, polyalkyl vinyl ether, polybutadiene, polyolefin, and polyvinyl ether. Examples of silicone surfactants include polydimethylsiloxane, polyphenylsiloxane, specially modified siloxane, fluorine-modified siloxane, and surface-treated siloxane. Examples of the hydrocarbon surfactant include polyethylene, polypropylene, polyisobutylene, paraffin, liquid paraffin, chlorinated polypropylene, chlorinated paraffin, and chlorinated liquid paraffin.

[0078] The leveling agents may be used alone or in combination of two or more. Among these, from the viewpoint of making the surface tension of the coating film uniform and improving the coatability, vinyl surfactants which are nonionic surfactants are preferred, and acrylic surfactants such as polyalkyl acrylates (acrylic polymers) or polyalkyl methacrylates are more preferred. Examples of acrylic surfactants that have such acrylic polymers or acrylic (co)polymers as their main components include the Polyflow series (No. 7, No. 50E, No. 50EHF, No. 54N, No. 75, No. 77, No. 85, No. 85HF, No. 90, No. 90D-50, No. 95, No. 99C), the TEGO Flow series (300, 370, ZFS460), and the BYK series (350, 352, 354, 355, 356, 358N, 361N, 381, 392, 394, 3441, 3440).

[0079] In the present disclosure, the leveling agent may be used alone or in combination of two or more kinds. In the present disclosure, when a leveling agent is contained in the polymerizable cholesteric liquid crystal composition, the content ratio thereof may be 0.0001 mass % to 0.5 mass %, 0.0002 mass % to 0.01 mass %, or 0.0003 mass % to 0.05 mass %, relative to the total solid content of the polymerizable cholesteric liquid crystal composition.

[0080] 5. Solvent The polymerizable cholesteric liquid crystal composition of the present disclosure may further contain a solvent from the viewpoint of coatability. The solvent may be appropriately selected from conventionally known solvents capable of dissolving or dispersing each component contained in the polymerizable cholesteric liquid crystal composition. Examples of the solvent include ester-based solvents, amide-based solvents, alcohol-based solvents, ether-based solvents, glycol monoalkyl ether-based solvents, aromatic hydrocarbon-based solvents, halogenated aliphatic hydrocarbon-based solvents, alicyclic hydrocarbon-based solvents, ketone-based solvents, and acetate-based solvents.

[0081] Preferred examples of the ester solvent include ethyl acetate, propyl acetate, isopropyl acetate, methyl propionate, and isobutyl acetate. Preferred examples of the amide solvent include N,N-dimethylacetamide and N,N-dimethylformamide. Preferred examples of the alcohol solvent include ethanol, 1-propanol, 2-propanol, and 1-butanol. Preferred examples of the ether solvent include ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, bis(2-propyl) ether, 1,3-dioxolane, 1,4-dioxane, tetrahydrofuran (THF), methyltetrahydrofuran, and 4-methyltetrahydropyran.

[0082] Preferred examples of glycol monoalkyl ether solvents include ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, and the like. Preferred examples of the aromatic hydrocarbon solvent include toluene, anisole, and xylene. Preferred examples of the halogenated aliphatic hydrocarbon solvent include chloroform and monochlorobenzene. Preferred examples of the alicyclic hydrocarbon solvent include cyclohexane and methylcyclohexane.

[0083] Preferred examples of the ketone solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, 2-heptanone, cyclohexanone, cyclopentanone, and methyl propyl ketone. Preferred examples of acetate solvents include ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, methyl acetoacetate, and 1-methoxy-2-propyl acetate.

[0084] The solvents may be used alone or in combination of two or more. From the viewpoint of viscosity and electrical conductivity related to the suitability for coating, the solvent may be at least one selected from the group consisting of ketone-based solvents and ester-based solvents.

[0085] In order to improve heat resistance, the polymerizable cholesteric liquid crystal composition of the present disclosure preferably contains 30% by mass or more of a solvent having a boiling point within ±20° C. of the phase transition temperature of the chiral polymerizable compound in the total solvent. When 30% by mass or more of a solvent having a boiling point within ±20° C. of the phase transition temperature of the chiral polymerizable compound is contained in the total solvent, evaporation of the solvent and phase transition of the chiral polymerizable compound become competitive in the coating and drying process, so that the chiral polymerizable compound is uniformly distributed in the film, thereby improving heat resistance. The solvent having a boiling point within the range of ±20° C. of the phase transition temperature of the chiral polymerizable compound may be, among others, a solvent having a boiling point within the range of the phase transition temperature of the chiral polymerizable compound or higher and the phase transition temperature of the chiral polymerizable compound +20° C. or lower. In this disclosure, the boiling point of a solvent refers to the boiling point at 1 atmospheric pressure.

[0086] In the polymerizable cholesteric liquid crystal composition of the present disclosure, from the viewpoint of improving heat resistance and making the pitch uniform, the solvent may be a mixed solvent of at least one selected from the group consisting of solvents having a boiling point within the range of ±20°C of the phase transition temperature of the chiral polymerizable compound and at least one selected from the group consisting of solvents having a boiling point exceeding +20°C of the phase transition temperature of the chiral polymerizable compound, and the solvent may be a mixed solvent of at least one selected from the group consisting of solvents having a boiling point within the range of not less than the phase transition temperature of the chiral polymerizable compound and not more than +20°C of the phase transition temperature of the chiral polymerizable compound and at least one selected from the group consisting of solvents having a boiling point exceeding +20°C of the phase transition temperature of the chiral polymerizable compound. The upper limit of the boiling point of at least one selected from the group consisting of solvents having a boiling point exceeding +20°C of the phase transition temperature of the chiral polymerizable compound may be 205°C or less.

[0087] The content ratio of the solvent in the polymerizable cholesteric liquid crystal composition of the present disclosure is not particularly limited, and may be appropriately set in consideration of the optimal viscosity when applied. The content of the solvent may be 70% by mass to 85% by mass, or 80% by mass to 85% by mass, based on the total amount of the polymerizable cholesteric liquid crystal composition including the solvent.

[0088] 6. Other Ingredients The polymerizable liquid crystal composition of the present disclosure may further contain other components within a range that does not impair the effects. Specifically, the polymerizable liquid crystal composition may contain other components such as an antistatic agent, a light stabilizer, an ultraviolet absorber, an antioxidant, a curing assistant, an acrylate resin, etc. These may be appropriately selected from conventionally known materials.

[0089] The polymerizable liquid crystal composition of the present disclosure can be analyzed for each component using a conventionally known analytical method. When determining the phase transition temperatures of an achiral polymerizable liquid crystal compound and a chiral polymerizable compound from a polymerizable liquid crystal composition, the achiral polymerizable liquid crystal compound and the chiral polymerizable compound may be first isolated, and then each phase transition temperature may be determined. Examples of isolation methods that can be used include silica gel chromatography, preparative HPLC, and reprecipitation. From the phase transition temperature and the results of NMR measurement of the isolated compound, it can be confirmed whether it is an achiral polymerizable liquid crystal compound or a chiral polymerizable compound. For each of the isolated compounds (achiral polymerizable liquid crystal compound, chiral polymerizable compound), a DSC measurement is performed as described in the Examples below to determine the endothermic peak (phase transition temperature) of each compound alone. By comparing the endothermic peak (phase transition temperature) of the DSC measurement of the compound alone with the detection temperature of the endothermic peak of the DSC measurement of the polymerizable liquid crystal composition (mixed state), the peaks of the achiral polymerizable liquid crystal compound and the chiral polymerizable compound in the polymerizable liquid crystal composition can be distinguished.

[0090] The polymerizable cholesteric liquid crystal composition of the present embodiment has good heat resistance and is therefore suitable for various applications, such as electromagnetic wave reflection films, brightness-enhancing films for displays, and heat-shielding films, which will be described later.

[0091] B. Optically anisotropic film The optically anisotropic film of the present disclosure is a cured film of the polymerizable cholesteric liquid crystal composition of the present disclosure. The optically anisotropic film of the present disclosure is a polymer composition obtained by forming a film from the polymerizable cholesteric liquid crystal composition of the present disclosure, twisting the polymerizable liquid crystal compound in the formed film of the polymerizable cholesteric liquid crystal composition, and polymerizing the aligned polymerizable liquid crystal compound and the chiral polymerizable compound. The twisted alignment is fixed by polymerizing the aligned polymerizable liquid crystal compound and the chiral polymerizable compound.

[0092] The film formation of the polymerizable cholesteric liquid crystal composition of the present disclosure may be performed by uniformly applying the polymerizable cholesteric liquid crystal composition onto a support that has been subjected to an alignment treatment to form a coating film. By appropriately adjusting the coating amount of the polymerizable cholesteric liquid crystal composition and the concentration of the polymerizable cholesteric liquid crystal composition, the film thickness is adjusted so as to provide a desired optical anisotropy.

[0093] Examples of the support include glass substrates and resin substrates. Examples of the resin substrate include transparent resin substrates formed using acetylcellulose-based resins such as triacetylcellulose, polyester-based resins such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, and polylactic acid, olefin-based resins such as polypropylene, polyethylene, and polymethylpentene, acrylic resins, polyurethane resins, polyethersulfone, polycarbonate, polysulfone, polyether, polyetherketone, acrylonitrile, methacrylonitrile, cycloolefin polymer, and cycloolefin copolymer. These supports may be subjected to a conventionally known surface treatment such as corona treatment or plasma treatment, or may be laminates.

[0094] Examples of the alignment treatment on the support include surface treatments such as conventionally known rubbing treatment and photoalignment treatment, and a conventionally known horizontal alignment film can be appropriately selected and used. The rubbing treatment may be directly applied to the supporting substrate, or a polymer coating may be provided in advance on the supporting substrate, and the rubbing treatment may be applied to the polymer coating.

[0095] When the alignment control force is imparted by the rubbing method, a polymer that exerts an alignment control force by rubbing is used for the horizontal alignment film. Examples of the polymer include polyvinyl alcohol, polyimide, polyamide, and derivatives thereof, and among them, polyvinyl alcohol is preferable. The method for forming the horizontal alignment film by the rubbing method may be appropriately selected from conventionally known methods. For example, a coating film containing the above polymer is formed on the support, and then the coating film is rubbed with a known rubbing roller or the like to obtain a horizontal alignment film.

[0096] When forming a horizontal alignment film by a photo-alignment method, a photo-alignment composition containing a photo-alignment material that exerts an alignment control force by irradiating polarized light is used as the composition for the alignment film. The photo-alignment material may be a photodimerization type material or a photoisomerization type material. Specifically, for example, cinnamate, coumarin, benzylidenephthalimidine, benzylideneacetophenone, diphenylacetylene, stilbazole, uracil, quinolinone, maleimide, or a polymer having a cinnamylidene acetic acid derivative can be mentioned, and among them, a polymer having at least one of cinnamate and coumarin, and their derivatives are preferably used. Specific examples of such photodimerization-type materials include, for example, compounds described in JP-A-9-118717, JP-T-10-506420, JP-T-2003-505561, WO2010 / 150748, JP-A-2015-151548, and JP-A-2021-103225.

[0097] The method for forming the photo-alignment film by the photo-alignment method may be appropriately selected from conventionally known methods. For example, the photo-alignment composition is uniformly applied onto the support, irradiated with polarized light, and then irradiated with light over the entire surface of the coating film to obtain a photo-alignment film.

[0098] The coating method may be appropriately selected as long as it can form a film with a desired thickness with good accuracy, for example, gravure coating, reverse coating, knife coating, dip coating, spray coating, air knife coating, spin coating, roll coating, printing, immersion and pulling up, curtain coating, die coating, casting, bar coating, extrusion coating, E-type coating, etc.

[0099] The polymerizable liquid crystal compound in the polymerizable cholesteric liquid crystal composition thus formed is twistedly aligned by adjusting and heating the polymerizable liquid crystal compound in the polymerizable cholesteric liquid crystal composition thus formed to a temperature at which the polymerizable liquid crystal compound can be aligned. The heating may be carried out simultaneously with drying of the solvent contained in the polymerizable cholesteric liquid crystal composition when the composition is formed into a film. By the heat treatment, the main chain portion having an orientation property of the polymerizable liquid crystal compound can be aligned and dried, and the aligned state can be fixed in a state where it is maintained. The alignment temperature varies depending on each substance in the polymerizable cholesteric liquid crystal composition, and therefore needs to be adjusted appropriately. The polymerizable cholesteric liquid crystal composition of the present disclosure contains an achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50° C. to 120° C. and a chiral polymerizable compound having a phase transition temperature of 60° C. to 90° C., and in order to improve heat resistance, the heat treatment is preferably performed within a range of, for example, 60° C. to 120° C. As the heating means, known heating and drying means can be appropriately selected and used. The heating time may be appropriately selected, for example, within the range of 10 seconds to 2 hours, preferably 20 seconds to 30 minutes.

[0100] After the alignment step, the polymerizable liquid crystal compound and the chiral polymerizable compound are polymerized. The polymerization method for forming the cured film can be appropriately selected according to the polymerizable functional group contained in the polymerizable liquid crystal compound of the present disclosure. In the alignment step, the polymerizable liquid crystal compound can be polymerized by, for example, irradiating the coating film fixed while maintaining the alignment state of at least the polymerizable liquid crystal compound, and an optically anisotropic film that is a cured film of the polymerizable cholesteric liquid crystal composition can be obtained.

[0101] The wavelength of light used for the light irradiation is not particularly limited, but it is preferable to match it as closely as possible to the maximum absorption wavelength of the photopolymerization initiator. Electron beams, ultraviolet rays, visible light, infrared rays (heat rays), etc. can be used. Usually, ultraviolet rays or visible light are used. The wavelength range is 150 to 500 nm. A preferred range is 220 to 450 nm, and a more preferred range is 250 to 400 nm. Examples of the light source are low pressure mercury lamps (germicidal lamps, fluorescent chemical lamps, black lights), high pressure discharge lamps (high pressure mercury lamps, metal halide lamps), and short arc discharge lamps (ultra-high pressure mercury lamps, xenon lamps, mercury xenon lamps). Preferred examples of the light source are metal halide lamps, xenon lamps, ultra-high pressure mercury lamps, and high pressure mercury lamps. The wavelength range of the irradiation light source may be selected by placing a filter or the like between the light source and the polymerizable liquid crystal layer to pass only a specific wavelength range. The amount of light emitted from the light source is usually 2 to 10,000 mJ / cm when it reaches the coating surface. 2 The preferred range of light intensity is 10 to 3000 mJ / cm 2 and a more preferred range is 100 to 2000 mJ / cm 2 The polymerization environment may be any of a nitrogen atmosphere, an inert gas atmosphere, and an air atmosphere, but a nitrogen atmosphere or an inert gas atmosphere is preferred from the viewpoint of improving the curing property.

[0102] The support and the alignment film may be peeled off and removed after the optically anisotropic film is formed.

[0103] The optically anisotropic film thus obtained is suitably used for various optical member applications such as electromagnetic wave reflecting films, brightness enhancing films for displays, and heat ray shielding films, which will be described later.

[0104] C. Electromagnetic wave reflective film The electromagnetic wave reflective film of the present disclosure is an electromagnetic wave reflective film which is a cured film of a polymerizable cholesteric liquid crystal composition, After heating the electromagnetic wave reflective film at 90°C for 72 hours, The helical pitch of the cholesteric liquid crystal in the cured film of the polymerizable cholesteric liquid crystal composition satisfies the following formulae (A-1), (A-2), and (A-3). P1-P1×0.05≦P2≦P1+P1×0.05 (A-1) P1-P1×0.05≦P3≦P1+P1×0.05 (A-2) P2-P2×0.05≦P1≦P2+P2×0.05 (A-3) (Here, P1 represents the length of the helical pitch including the position of the first surface of the cured film, P2 represents the length of the helical pitch including the position of the second surface of the cured film opposite to the first surface, and P3 represents the length of the helical pitch including the position of the center of the cured film in the layer thickness direction.)

[0105] The electromagnetic wave reflective film of the present disclosure is an electromagnetic wave reflective film having high heat resistance and high uniformity of the helical pitch in the film thickness direction, since the helical pitch of the cholesteric liquid crystal in the cured film of the polymerizable cholesteric liquid crystal composition satisfies the formulas (A-1), (A-2), and (A-3) after the electromagnetic wave reflective film is heated at 90°C for 72 hours.

[0106] Cholesteric liquid crystal phases are known to exhibit selective reflectivity at specific wavelengths. In a typical cholesteric liquid crystal phase, the central wavelength of selective reflection (selective reflection central wavelength) λ depends on the helical pitch P in the cholesteric liquid crystal phase, and follows the relationship between the average refractive index n of the cholesteric liquid crystal phase and λ = n × P. Therefore, the selective reflection central wavelength can be adjusted by adjusting this helical pitch. The longer the helical pitch, the longer the selective reflection central wavelength of the cholesteric liquid crystal phase becomes. The helical pitch is one pitch (helical period) of the helical structure of the cholesteric liquid crystal phase, in other words, one turn of the helix, i.e., the length in the helical axis direction in which the director of the liquid crystal compound that constitutes the cholesteric liquid crystal phase (the long axis direction in the case of a rod-shaped liquid crystal compound) rotates 360°.

[0107] The helical pitch of the cholesteric liquid crystal phase depends on the type and concentration of the chiral compound (chiral agent) used together with the achiral liquid crystal compound when forming a cured film of the polymerizable cholesteric liquid crystal composition. Therefore, by adjusting these, the desired helical pitch can be obtained.

[0108] In addition, cholesteric liquid crystal phases exhibit selective reflection for either left-handed or right-handed circularly polarized light at a specific wavelength. Whether the reflected light is right-handed or left-handed circularly polarized light depends on the helical twist direction of the cholesteric liquid crystal phase. When the helical twist direction of the cholesteric liquid crystal layer is right-handed, right-handed circularly polarized light is reflected, and when the helical twist direction is left-handed, left-handed circularly polarized light is reflected. The direction of rotation of the cholesteric liquid crystal phase can be adjusted by the type of achiral liquid crystal compound and / or the type of chiral compound (chiral agent) that forms the cholesteric liquid crystal layer.

[0109] FIG. 1 is a schematic diagram showing an example of a striped pattern of bright areas B and dark areas D seen when a cross section of an electromagnetic wave reflective film of the present disclosure is observed using a scanning transmission electron microscope (STEM). As shown in FIG. 1, in a cross section of the electromagnetic wave reflective film 10 of the present disclosure, which is a cured film of a polymerizable cholesteric liquid crystal composition, a layered structure in which light areas B (continuous lines formed by light areas B) and dark areas D (continuous lines formed by dark areas D) are alternately laminated is usually observed. In a STEM cross section as shown in FIG. 1, light areas B and dark areas D are observed due to the liquid crystal compound being helically oriented in the cured film of the polymerizable cholesteric liquid crystal composition, and the orientation of the liquid crystal compound differs depending on the position in the thickness direction (vertical direction in FIG. 1). Therefore, in a STEM cross section of the cured film of the polymerizable cholesteric liquid crystal composition, the length of one pitch of the helical structure (helical period) is the thickness of four layers, that is, light areas B, dark areas D, light areas B, and dark areas D.

[0110] In the electromagnetic wave reflecting film 10 of the present disclosure, the helical pitch of the cholesteric liquid crystal in the cured film of the polymerizable cholesteric liquid crystal composition satisfies the following formulas (A-1), (A-2), and (A-3) after the electromagnetic wave reflecting film 10 is heated at 90° C. for 72 hours. Therefore, in the electromagnetic wave reflecting film 10 of the present disclosure, the helical pitch of the cholesteric liquid crystal in the cured film of the polymerizable cholesteric liquid crystal composition usually satisfies the following formulas (A-1), (A-2), and (A-3) even before the electromagnetic wave reflecting film 10 is heated at 90° C. for 72 hours. P1-P1×0.05≦P2≦P1+P1×0.05 (A-1) P1-P1×0.05≦P3≦P1+P1×0.05 (A-2) P2-P2×0.05≦P1≦P2+P2×0.05 (A-3) Here, P1 represents the length of the helical pitch including the position of the first surface S1 of the cured film, P2 represents the length of the helical pitch including the position of the second surface S2 opposite to the first surface S1 of the cured film, and P3 represents the length of the helical pitch including the position of the central part C in the layer thickness direction of the cured film.

[0111] The helical pitch in the electromagnetic wave reflective film of the present disclosure is determined by observing a cross section of the electromagnetic wave reflective film using a scanning transmission electron microscope (STEM). Specifically, the center of a sample of an electromagnetic wave reflection film (optically anisotropic film) is cut into a rectangular shape (2 mm x 5 mm), embedded in a thermosetting resin, and then cut with a microtome to produce an ultrathin section (80 nm thick). The obtained ultrathin section is observed by STEM under the following measurement conditions (detector TE, acceleration voltage 30 kV, emission current 10 μA, magnification 5000 times) to obtain a cross-sectional image of the electromagnetic wave reflection film (optically anisotropic film). In the cross-sectional image obtained by STEM, one pitch is dark part D-light part B-dark part D-light part B, or light part B-dark part D-light part B-dark part D, and one pitch is measured using cross-sectional image analysis software (Hitachi High-Tech, Data Manager). For one field of view, the points corresponding to pitch lengths P1, P2, and P3 are each measured three times, and the average values ​​of the three measurements are designated as P1, P2, and P3. The pitch length is found by using analysis software to draw a straight line at the points corresponding to dark area D-light area B-dark area D-light area B, or light area B-dark area D-light area B-dark area D, and then calculating the length of that line on the analysis software.

[0112] Since it is desirable for the electromagnetic wave reflective film of the present disclosure to have a wavelength reflection band that does not change due to heat, it is more preferable that the helical pitch of the cholesteric liquid crystal in the cured film of the polymerizable cholesteric liquid crystal composition before and after heating at 90° C. for 72 hours satisfy the following formulas (A'-1), (A'-2), and (A'-3), and it is even more preferable that the helical pitch of the cholesteric liquid crystal in the cured film of the polymerizable cholesteric liquid crystal composition satisfy the following formulas (A"-1), (A"-2), and (A"-3). P1-P1×0.03≦P2≦P1+P1×0.03 (A'-1) P1-P1×0.03≦P3≦P1+P1×0.03 (A'-2) P2-P2×0.03≦P1≦P2+P2×0.03 (A'-3) P1-P1×0.02≦P2≦P1+P1×0.02 (A”-1) P1-P1×0.02≦P3≦P1+P1×0.02 (A”-2) P2-P2×0.02≦P1≦P2+P2×0.02 (A”-3)

[0113] Moreover, from the viewpoint of heat resistance, the electromagnetic wave reflective film of the present disclosure preferably satisfies the following formula (B). Formula (B) ΔPave={|(P 1b -P 1a )| / P 1b +|(P 2b -P 2a )| / P 2b +|(P 3b -P 3a )| / P 3b} / 3≦0.05 (Here, P 1b is the length of the helical pitch including the position of the first surface S1 of the cured film before heating at 90 ° C. for 72 hours, P1a is the length of the helical pitch including the position of the first surface S1 of the cured film after heating at 90° C. for 72 hours, P 2b is the length of the helical pitch including the position of the second surface S2 opposite to the first surface S1 of the cured film before heating at 90° C. for 72 hours, P 2a is the length of the helical pitch including the position of the second surface S2 opposite to the first surface S1 of the cured film after heating at 90° C. for 72 hours, P 3b is the length of the helical pitch including the position of the center part C in the layer thickness direction of the cured film before heating at 90 ° C for 72 hours, P 3a represents the length of the helical pitch including the position of the center part C in the layer thickness direction of the cured film after heating at 90° C. for 72 hours.)

[0114] The ΔPave may be 0.04 or less, may be 0.03 or less, may be 0.02 or less, or may be 0.01 or less.

[0115] In the electromagnetic wave reflecting film 10 of Fig. 1, the striped pattern (layer structure) of the bright areas B (continuous lines formed by the bright areas B) and the dark areas D (continuous lines formed by the dark areas D) is formed so as to be parallel to the surface (formation surface) of the cured film. In this embodiment, the electromagnetic wave reflecting film 10 exhibits specular reflectivity. That is, when light is incident from the normal direction of the electromagnetic wave reflecting film 10, the light is reflected in the normal direction.

[0116] The electromagnetic wave reflective film of the present disclosure preferably has a reflectance of 42% or more, and more preferably 45% or more, at a reflection wavelength of 315 nm to 1000 nm. In this disclosure, the reflected wavelength and reflectance are measured using a spectrophotometer. More specifically, if the electromagnetic wave reflective film has a resin substrate, it is peeled off and the electromagnetic wave reflective film is transferred to adhesive glass to prepare a measurement sample. The measurement sample transferred to the glass is measured with black tape attached to the glass surface to prevent reflected light from the back side from affecting the measurement value. The reflectance measurement is performed in accordance with JIS R3106-2019, and the reflection spectrum is measured using a spectrophotometer at wavelengths from 380 nm to 780 nm. The specular reflection of the barium sulfate white plate is used as the baseline, and the measurement position of the sample is the center position of the sample. The obtained spectrum is analyzed using the UV-Visible spectrophotometer software, and a line graph is created with the reflection wavelength on the horizontal axis and the reflectance on the vertical axis. The reflection wavelength and reflectance at the peak top position of the created line graph are adopted as the measured values. If the peak shape is a trapezoid, the center position of the upper side of the trapezoid is regarded as the peak top.

[0117] The electromagnetic wave reflective film of the present disclosure preferably has a haze of 1.5% or less, and more preferably 1.0% or less. In the present disclosure, the haze is measured using a haze meter in accordance with JIS K7361-1:2000. The electromagnetic wave reflective film is cut into a size of 50 mm x 50 mm, and the haze value is measured three times for each electromagnetic wave reflective film, and the average value of the values ​​obtained from the three measurements is used. "Measured three times" does not mean measuring the same place three times, but measuring three different places.

[0118] The electromagnetic wave reflective film of the present disclosure is a cured film of a polymerizable cholesteric liquid crystal composition, and may be produced by appropriately selecting a polymerizable cholesteric liquid crystal composition containing a polymerizable liquid crystal compound and a chiral agent, and the electromagnetic wave reflective film of the present disclosure may be a cured film of the polymerizable cholesteric liquid crystal composition of the present disclosure.

[0119] The thickness of the electromagnetic wave reflective film of the present disclosure varies depending on the purpose, but a rough guideline is 1 μm to 15 μm, with a preferred range being 1 μm to 10 μm, and a more preferred range being 2 μm to 6 μm.

[0120] The fact that the electromagnetic wave reflection film of the present disclosure is a cured film of a polymerizable cholesteric liquid crystal composition can be confirmed by collecting and analyzing a material from the electromagnetic wave reflection film. As the analysis method, NMR, IR, GC-MS, XPS, TOF-SIMS, or a combination of these methods can be applied.

[0121] The electromagnetic wave reflective film of the present disclosure can be produced using a polymerizable cholesteric liquid crystal composition in the same manner as in the production of the optically anisotropic film of the present disclosure.

[0122] The electromagnetic wave reflecting film of the present disclosure may be a laminate including an electromagnetic wave reflecting film. Each of Figs. 2 and 3 shows one embodiment of a laminate including an electromagnetic wave reflecting film of the present disclosure. One embodiment of the laminate 100 including an electromagnetic wave reflecting film shown in the example of Fig. 2 is a laminate in which an alignment film 30 and an electromagnetic wave reflecting film 10 are laminated in this order on a support 20. One embodiment of the laminate 100 including an electromagnetic wave reflecting film shown in the example of Fig. 3 is a laminate in which the electromagnetic wave reflecting film 10 is laminated on a support 20'. The laminate 100 including an electromagnetic wave reflecting film shown in the example of Fig. 3 may be subjected to an orientation treatment that exerts an orientation regulating force on the surface of the support 20' on the electromagnetic wave reflecting film 10 side. The support, alignment film, and alignment treatment in the laminate may be the same as those explained for the optically anisotropic film. In the laminate, the electromagnetic wave reflective film may be a single layer, or may be a laminate of two or more layers. EXAMPLES

[0123] The present invention will be specifically described below based on examples. The materials, reagents, amounts of substances and their ratios, operations, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the present invention is not limited to the following examples.

[0124] <Method for measuring solid-liquid crystal phase transition temperature or solid-liquid phase transition temperature> Measurements were performed using a differential scanning calorimeter (DSC) (Shimadzu Science, DSC-60) according to the following method. The measurements were performed in accordance with JIS K7121-1987, 8. The phase transition temperature was the extrapolated melting onset temperature (Tim) according to JIS K7121-1987, 9.1(2). However, the method of preparing the sample by distilling off the solvent and the heating and cooling program (heating rate, cooling rate, heating start temperature, end temperature) were as follows. First, the solvent was removed from the liquid crystal composition using a rotary evaporator to obtain a measurement sample. 5 mg of the measurement sample was sealed in an aluminum sample pan, and then set in a DSC, cooled from 25°C to -10°C at a rate of -25°C / min under a nitrogen atmosphere, and maintained at -10°C for 15 minutes. Thereafter, as a first heating run, the temperature was raised from -10°C to 150°C at a rate of 10°C / min, and maintained at 150°C for 1 minute. As a first cooling run, the temperature was lowered from 150°C to -10°C at a rate of -10°C / min, and maintained at -10°C for 10 minutes. Thereafter, as a second heating run, the temperature was raised from -10°C to 150°C at a rate of 10°C / min, and maintained at 150°C for 1 minute. As a second cooling run, the temperature was lowered from 150°C to 25°C at a rate of -10°C / min. The endothermic onset temperature detected during the second heating step, i.e., the extrapolated melting onset temperature (Tim), which is the temperature at the intersection of a straight line extending the low-temperature baseline to the high-temperature side and a tangent line drawn at the point where the slope of the curve on the low-temperature side of the melting peak is maximum, was determined as the phase transition temperature.

[0125] The compounds used in the examples and comparative examples are shown below. (1-A); Solid-liquid crystal phase transition temperature: 80℃ (1-B); Solid-liquid crystal phase transition temperature: 54℃ (1-C); Solid-liquid crystal phase transition temperature: 120℃ (C1-a): Polymerizable liquid crystal compound having a fluorene skeleton, solid-liquid crystal phase transition temperature: 84°C (2-A); Phase transition temperature: 76℃ (2-B); Phase transition temperature: 60℃ (2-C); Phase transition temperature: 76°C (optical isomer of 2-A above) (2-D); Phase transition temperature: 88℃ (C2-a); Phase transition temperature: 110℃ (C2-b); Phase transition temperature: 138℃

[0126] [ka]

[0127] [ka]

[0128] [ka]

[0129] The compound (1-A) used was a reagent commercially available from Tokyo Chemical Industry Co., Ltd. As the compound (1-B), Paliocolor LC242 commercially available from BASF was used. The compound (1-C) was synthesized by the following method. Compound 1 (5.0 g), triethylamine hydrochloride (TEA·HCl) (7.7 g), and trisodium azide (2.0 g) were added to 20 mL of toluene and stirred at 110 ° C for 5 hours. The reaction solution was cooled to 60 ° C, and 30 mL of water was added. After stirring for 15 minutes, the mixture was left to stand, and the aqueous layer was collected by separation. 35% hydrochloric acid was added to the collected aqueous layer until the pH became 4, and the resulting solid was collected by filtration. The collected solid was dried under reduced pressure at 40 ° C to obtain compound 2 (6.2 g). Compound 1 (1.5 g) and compound 3 (7.7 g) synthesized with reference to Patent Application No. 2019-116420 were added to 15 mL of chloroform, and then dimethylaminopyridine (0.01 g) and N,N'-diisopropylcarbodiimide (3.0 g) were added at 15 ° C, and the mixture was stirred for 4 hours. Next, 500 mL of methanol was added, and the precipitated solid was collected by filtration. The collected solid was dried under reduced pressure at 40° C. to obtain compound (1-C).

[0130] [ka]

[0131] The compound (C1-a) was synthesized according to the method described in JP-A-2003-238491.

[0132] The compounds (2-A), (2-B) and (2-C) were synthesized by combining the methods described in JP 2005-263778 A, U.S. Pat. No. 5,886,242 and UK Patent Application Publication No. 2,298,202. In the compounds (2-A) and (2-B), the R-form was used at the binaphthalene moiety. In the compound (2-C), the S-form was used at the binaphthalene moiety.

[0133] The compound (2-D) was synthesized by the following method. Compound 4 (1.1 g) and 4-hydroxybenzoic acid (1.0 g) were added to 10 mL of methylene chloride, and then dimethylaminopyridine (0.01 g) and N,N'-diisopropylcarbodiimide (1.4 g) were added at 15°C and stirred for 1 hour. The solvent was removed from the reaction solution, and the mixture was purified by silica gel column chromatography to obtain the following compound 5 (2.6 g). Next, compound 5 (2.6 g) and compound 6 (4.8 g) obtained from Merck (Sigma-Aldrich) were added to 20 mL of methylene chloride, and then dimethylaminopyridine (0.01 g) and N,N'-diisopropylcarbodiimide (1.3 g) were added at 15°C and stirred for 4 hours. Next, 200 mL of methanol was added, and the precipitated solid was collected by filtration. The collected solid was purified by silica gel column chromatography to obtain compound (2-D) (5.6 g).

[0134] [ka]

[0135] As the compound (C2-a), Paliocolor LC756 commercially available from BASF was used.

[0136] The compound (C2-b) was synthesized by the following method. The following compound 7 (10.0 g) and the following compound 8 (15.0 g) were added to 100 mL of methylene chloride, and then dimethylaminopyridine (0.1 g) and N,N'-diisopropylcarbodiimide (8.0 g) were added at 15°C, and the mixture was stirred for 17 hours. Next, 500 mL of methanol was added, and the precipitated solid was collected by filtration. The collected solid was purified by silica gel column chromatography to obtain the following compound 9 (0.5 g). The following compound 3 (0.5 g) and the following compound 4 (0.1 g) were added to 10 mL of methylene chloride, and then dimethylaminopyridine (0.01 g) and N,N'-diisopropylcarbodiimide (0.1 g) were added at 15°C, and the mixture was stirred for 5 hours. The reaction mixture was concentrated under reduced pressure, and the concentrated residue was purified by silica gel column chromatography to obtain compound (C2-b) (0.1 g).

[0137] [ka]

[0138] [Example 1] (1) Preparation of polymerizable cholesteric liquid crystal composition 24.5 parts by mass of an achiral polymerizable liquid crystal compound (compound (1-A)), 0.5 parts by mass of a chiral polymerizable compound (compound (2-A)), 1 part by mass of a photopolymerization initiator (Omnirad907, manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.01 part by mass of a leveling agent (acrylic surfactant, Polyflow No. 75, manufactured by Kyoeisha Chemical Co., Ltd.) were dissolved in 24 parts by mass of methyl ethyl ketone (MEK) and 50 parts by mass of methyl isobutyl ketone (MIBK) to produce polymerizable cholesteric liquid crystal composition 1.

[0139] (2) Manufacturing of electromagnetic wave reflective films (optically anisotropic films) (2-1) Formation of photo-alignment film A composition for a photoalignment film was prepared in the same manner as the photoalignment film material of Example 1 of JP 2021-103225 A. The composition for photoalignment film was applied by spin coating onto one side of a PET substrate (Toyobo Co., Ltd., E5100, thickness 38 μm) so that the film thickness after curing would be 0.2 μm, and the composition was dried and thermally cured by heating in an oven at 90° C. for 2 minutes to form a cured coating film. Thereafter, the surface of the cured coating film was exposed to polarized ultraviolet light containing a 313 nm emission line using an Hg-Xe lamp and a Glan-Taylor prism in a direction perpendicular to the substrate normal at an exposure dose of 100 mJ / cm. 2 An alignment film was formed by irradiating the liquid crystal with light at 400 nm.

[0140] (2-2) Preparation of electromagnetic wave reflective film (optically anisotropic film) The polymerizable cholesteric liquid crystal composition 1 was applied onto the formed alignment film to a thickness of 100 μm after curing. The polymerizable liquid crystal composition was applied to a thickness of about 4 μm to form a film. The film was then dried in an oven at 90° C. for 2 minutes, and then irradiated with ultraviolet light (UV) at a dose of 400 mJ / cm using an H bulb manufactured by Fusion Co., Ltd. under a nitrogen atmosphere. 2 An electromagnetic wave reflective film (optically anisotropic film) was formed by irradiating the light with an electric field of 1000 V.

[0141] [Examples 2 to 15, Comparative Examples 1 to 3] (1) Preparation of polymerizable cholesteric liquid crystal composition Polymerizable cholesteric liquid crystal compositions 2 to 15 and comparative polymerizable cholesteric liquid crystal compositions 1 to 3 were obtained in the same manner as in Example 1, except that the type and / or amount of at least one of the achiral polymerizable liquid crystal compound, the chiral polymerizable compound, the solvent, and the leveling agent was changed according to Table 5 below. (2) Manufacturing of electromagnetic wave reflective films (optically anisotropic films) In Example 1, except that polymerizable cholesteric liquid crystal compositions 2 to 15 and comparative polymerizable cholesteric liquid crystal compositions 1 to 3 were used instead of polymerizable cholesteric liquid crystal composition 1, and the drying temperature was set to the temperature shown in Table 5, electromagnetic wave reflective films (optically anisotropic films) 2 to 15 and comparative electromagnetic wave reflective films (optically anisotropic films) 1 to 3 were obtained in the same manner as in Example 1.

[0142] [evaluation] <Sample Creation> The PET substrate of the electromagnetic wave reflection film (optically anisotropic film) obtained in each Example and Comparative Example was peeled off, and the electromagnetic wave reflection film (optically anisotropic film) and the alignment film were transferred to adhesive glass (Corning EagleXG glass (50mm x 50mm) bonded with Lintec adhesive CLEAR-PET50-06-50) to obtain a sample, and the reflectance and haze were measured. The electromagnetic wave reflection film of the sample transferred to the glass was also cut to a size of 50mm x 50mm.

[0143] <Measurement of reflection wavelength and reflectance> For the electromagnetic wave reflective film (optically anisotropic film) obtained in each of the Examples and Comparative Examples, the reflection wavelength and reflectance were measured using a spectrophotometer (UV2700, manufactured by Shimadzu Corporation). For the samples to be measured, black tape (Yamato vinyl tape No. 200-50-21) was attached to the entire glass side of the samples transferred to the glass to prevent reflected light from the back side from affecting the measured values. The reflectance measurement was performed according to JIS R3106-2019, and the reflection spectrum was measured from wavelengths of 380 nm to 780 nm. The specular reflection of the barium sulfate white plate was used as the baseline, and the measurement position of the sample was the center position of the sample. The measurement was performed once. The obtained spectrum was analyzed using UVProbe (Shimadzu Corporation, UV-Visible Spectrophotometer software) and a line graph was created with the reflection wavelength on the horizontal axis and the reflectance on the vertical axis. The reflection wavelength and reflectance at the peak top position of the created line graph were used as the measured values. When the peak shape was a trapezoid, the center position of the upper side of the trapezoid was taken as the peak top. If the reflectance is 5% or more, it is determined that a cholesteric liquid crystal phase is formed.

[0144] <Helical pitch measurement> Ultrathin sections were prepared using a microtome for the cross sections of the electromagnetic wave reflective films (optically anisotropic films) obtained in each Example and Comparative Example, and observed under a scanning transmission electron microscope (STEM, Hitachi High-Technologies Corporation, S-4800) to measure the length of the helical pitch. Specifically, the center of a film sample of an electromagnetic wave reflection film (optically anisotropic film) was cut into a rectangular shape (2 mm × 5 mm), and then embedded in a thermosetting resin (Liquid A (62 mL of Lubeac 812 manufactured by Nacalai Tesque and 100 mL of dodecenyl succinic anhydride (DDSA) manufactured by Fuji Film Wako) and Liquid B (a mixture of methyl nadic anhydride (MNA) manufactured by Merck and DMP30 (trade name, obtained from Nissin EM) in a ratio of 7:3 (volume ratio)) prepared according to the Luft method at 80°C for 6 hours by hardening, and then cut with a microtome to prepare ultrathin sections (80 nm thick) by cutting out a smooth cross section. The obtained ultrathin cross-sectional sections were measured by STEM under the following measurement conditions (detector: Observation was performed using a TE, accelerating voltage of 30 kV, emission current of 10 μA, and magnification of 5000 times to obtain a cross-sectional image of the electromagnetic wave reflective film (optically anisotropic film). In the cross-sectional image obtained using STEM, one pitch is dark area D-light area B-dark area D-light area B, or light area B-dark area D-light area B-dark area D, and the length of one pitch was measured using cross-sectional image analysis software (Hitachi High-Tech, Data Manager). The measurements were made for pitch lengths P1, P2, and P3 in one field of view, with n=3 for each, and the average values ​​were designated as P1, P2, and P3. The pitch length was determined by drawing a straight line using analysis software at the locations corresponding to dark area D-light area B-dark area D-light area B, or light area B-dark area D-light area B-dark area D, and then calculating the length of that line using the analysis software.

[0145] <Heat resistance test> The obtained electromagnetic wave reflective film (optically anisotropic film) was heated in an oven at 90° C. for 72 hours. After heating at 90° C. for 72 hours, the electromagnetic wave reflective film (optically anisotropic film) was subjected to measurement of the helical pitch as described above. (Evaluation criteria for helical pitch variation) A: Satisfies the following formulas (A''-1), (A''-2), and (A''-3). P1-P1×0.02≦P2≦P1+P1×0.02 (A”-1) P1-P1×0.02≦P3≦P1+P1×0.02 (A”-2) P2-P2×0.02≦P1≦P2+P2×0.02 (A”-3) B: does not satisfy the above formula (A''-1), formula (A''-2), and formula (A''-3), but satisfies the following formulas (A-1), (A-2), and (A-3): P1-P1×0.05≦P2≦P1+P1×0.05 (A-1) P1-P1×0.05≦P3≦P1+P1×0.05 (A-2) P2-P2×0.05≦P1≦P2+P2×0.05 (A-3) C: The formulae (A-1), (A-2), and (A-3) are not satisfied.

[0146] <Haze measurement> The electromagnetic wave reflective films (optically anisotropic films) obtained in each Example and Comparative Example were measured using a haze meter (HM-150N, manufactured by MURAKAMI COLORLAB) in accordance with JIS K7361-1:2000. The haze value was measured three times for each electromagnetic wave reflective film using a sample in which an electromagnetic wave reflective film cut to a size of 50 mm x 50 mm was transferred to glass, and the sample was placed so that the glass substrate side was the light source side. The haze value was calculated as the average value of the three measurements. "Measured three times" does not mean that the same place is measured three times, but that three different places are measured.

[0147] [Table 5] The abbreviations for the solvents and leveling agents in the table are as follows. MEK: Methyl ethyl ketone (boiling point 80°C) MIBK: Methyl isobutyl ketone (boiling point 116°C) CPN: Cyclopentanone (boiling point 131℃) EtOAc: Ethyl acetate (boiling point 77°C) Me-THF: 2-methyltetrahydrofuran (boiling point 78°C) 4-Me-THP: 4-methyltetrahydropyran (boiling point 105°C) [Explanation of symbols]

[0148] 10 Electromagnetic wave reflective film 20 Support 20' support 30 Orientation film 100 Laminate

Claims

1. A polymerizable cholesteric liquid crystal composition comprising an achiral polymerizable liquid crystal compound having a solid-liquid crystal phase transition temperature of 50°C to 120°C, a chiral polymerizable compound having a phase transition temperature of 60°C to 90°C, and a photopolymerization initiator, and not comprising a polymerizable liquid crystal compound having a fluorene skeleton.

2. The polymerizable cholesteric liquid crystal composition according to claim 1 , further comprising a non-fluorine-containing leveling agent.

3. Further, it contains a solvent, The polymerizable cholesteric liquid crystal composition according to claim 1 or 2, wherein the solvent contains 30 mass % or more of a solvent having a boiling point within a range of ±20° C. of the phase transition temperature of the chiral polymerizable compound based on the total solvent.

4. 3. The polymerizable cholesteric liquid crystal composition according to claim 1, wherein the achiral polymerizable liquid crystal compound is at least one selected from the group consisting of compounds represented by the following general formula (1): 【Chemistry 1】 In the general formula (1), Ar represents a 1,4-phenylene group or a naphthalene-2,6-diyl group. L 1 and L 2 are each independently -O-, -S-, -COO-, -OCO-, or -CH 2 -CH 2 -OCO-, -OCO-CH 2 -CH 2 --, --CH 2 -OCO-, -OCO-CH 2 represents - or a single bond, A 1 and A 2 each independently represents a 1,4-phenylene group, a 1,4-cyclohexylene group, or a naphthalene-2,6-diyl group; The Ar and A 1 and A 2 Each of the groups E 1 may be substituted by the substituent E 1 is a halogen atom, a nitro group, a cyano group, a tetrazole group, an alkyl group having 1 to 7 carbon atoms, or an alkoxy group having 1 to 7 carbon atoms, R 1 and R 2 each independently represents a group selected from the following general formula (R-1): General formula (R-1): -L r1 -R sp1 -Z 1 In general formula (R-1), L r1 represents -O-, -S-, -COO-, -OCO-, -OCOO-, or a single bond; R sp1 is one -CH 2 - or two or more non-adjacent -CH 2 each independently represents an alkylene group having 1 to 20 carbon atoms which may be replaced by —O—, —COO—, or —OCO—, or a single bond; Z 1 represents a polymerizable functional group. n1 and n2 each independently represent an integer of 0 to 2, provided that n1+n2 is 1 or more; L 1 , L 2 , A 1 , and A 2 When there are a plurality of each, they may be the same or different.)

5. 3. The polymerizable cholesteric liquid crystal composition according to claim 1, wherein the chiral polymerizable compound is at least one selected from the group consisting of compounds represented by the following general formula (2): 【Chemistry 2】 (In the general formula (2), L 3 and L 4 each independently represents -O-, -S-, -COO-, -OCO-, or a single bond; A 3 and A 4 each independently represents a 1,4-phenylene group, a 1,4-cyclohexylene group, or a naphthalene-2,6-diyl group; R 3 and R 4 each independently represents a group selected from the following general formula (R-2): General formula (R-2): -L r2 -R sp2 -Z 2 In general formula (R-2), L r2 represents -O-, -S-, -COO-, -OCO-, -OCOO-, or a single bond; R sp2 is one -CH 2 - or two or more non-adjacent -CH 2 each independently represents an alkylene group having 1 to 20 carbon atoms which may be replaced by —O—, —COO—, or —OCO—, or a single bond; Z 2 represents a polymerizable functional group. Substituent E 2 and E 3 each independently represents an alkyl group having 1 to 3 carbon atoms or a halogen; n3 and n4 each independently represent 1 to 3, m1 and m2 each independently represent 0 to 2, L 3 , L 4 , A 3 , and A 4 When there are a plurality of each, they may be the same or different.)

6. 3. An optically anisotropic film which is a cured film of the polymerizable cholesteric liquid crystal composition according to claim 1.

7. An electromagnetic wave reflective film which is a cured film of a polymerizable cholesteric liquid crystal composition, After heating the electromagnetic wave reflective film at 90° C. for 72 hours, The electromagnetic wave reflective film, wherein the helical pitch of the cholesteric liquid crystal in the cured film of the polymerizable cholesteric liquid crystal composition satisfies the following formulae (A-1), (A-2), and (A-3): P 1 -P 1 ×0.05≦P 2 ≦P 1 +P 1 ×0.05 (A-1) P 1 -P 1 ×0.05≦P 3 ≦P 1 +P 1 ×0.05 (A-2) P 2 -P 2 ×0.05≦P 1 ≦P 2 +P 2 ×0.05 (A-3) (Here, P 1 is the length of the helical pitch including the position of the first surface of the cured film, P 2 is the length of the helical pitch including the position of the second surface of the cured film opposite to the first surface, P 3 represents the length of the helical pitch including the center position in the layer thickness direction of the cured film.)

8. 8. The electromagnetic wave reflective film according to claim 7, wherein the polymerizable cholesteric liquid crystal composition is the polymerizable cholesteric liquid crystal composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Cholesteric liquid crystal elastomer composite film and preparation method thereof

    CN115449112A

  • Polymer liquid crystal brightness enhancement film and OLED display device

    CN115572499A

  • Polymerizable liquid crystal composition

    JP2009286885A

  • Polymerizable chiral compound

    JP2013087109A

  • Ultraviolet ray-curable resin composition, and laminate

    WO2015093093A1