Active material, battery, and manufacturing method thereof

A silicon clathrate type crystal phase active material with Si and Al, and optional voids, addresses the volume change issue in Si-based batteries, enhancing stability and reducing confining pressure requirements.

JP2024144489AInactive Publication Date: 2024-10-11TOYOTA JIDOSHA KK
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024117428
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Silicon (Si) based active materials for batteries experience significant volume changes during charging and discharging, which can lead to structural instability and require high confining pressures to mitigate these changes.

Method used

The use of a silicon clathrate type crystal phase active material containing Si and Al, with a specific ratio of Al to Si, and optionally voids within the primary particles, to minimize volume changes during charging and discharging.

Benefits of technology

The proposed active material reduces volume changes during charging and discharging, allowing for reduced confining pressures and improved stability in batteries, particularly in all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144489000001_ABST
    Figure 2024144489000001_ABST
Patent Text Reader

Abstract

To provide an active material having a small volume change due to charge / discharge.SOLUTION: An active material according to the present disclosure includes at least Si and Al, and has a silicon clathrate type crystal phase, and the ratio of Al to the total of Si and Al is 0.1 atm% or more and 1 atm% or less.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to active materials, batteries, and methods of making the same. [Background technology]

[0002] In recent years, the development of batteries has been actively carried out. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles is underway. In addition, Si is known as an active material used in batteries.

[0003] For example, Patent Document 1 discloses that it is theoretically possible to use silicon clathrate as the negative electrode active material of a lithium ion battery. 46 and Si 34 has been disclosed.

[0004] Patent Document 2 discloses an electrode active material containing a clathrate compound including a crystal lattice and a guest substance contained in the crystal lattice. Specifically, it is disclosed that the guest substance includes at least one selected from the group consisting of Ba, Ca, and Li, and the crystal lattice includes at least one selected from the group consisting of Ga, Al, In, Ag, Au, Cu, Ni, and Co, and at least one selected from the group consisting of Si and Sn.

[0005] Furthermore, Non-Patent Document 1 discloses a ternary silicon clathrate having an I-type crystal phase. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] US Patent Application Publication No. 2012 / 0021283 [Patent Document 2] International Publication No. 2014 / 050100 [Non-patent literature]

[0007] [Non-Patent Document 1] Tiago FT Cerqueira et al., "Prediction and Synthesis of a Non-Zintl Silicon Clathrate", Chem. Mater. 2016, 28, 3711-3717 Summary of the Invention [Problem to be solved by the invention]

[0008] Silicon has a large theoretical capacity and is effective in increasing the energy density of batteries, but its volume changes significantly during charging and discharging.

[0009] The present disclosure has been made in consideration of the above circumstances, and has as its main object to provide an active material that undergoes small volumetric change upon charging and discharging. [Means for solving the problem]

[0010] In order to solve the above problems, the present disclosure provides an active material that contains at least Si and Al, has a silicon clathrate-type crystal phase, and has a ratio of the Al to the total of the Si and the Al of 0.1 atm% or more and 1 atm% or less.

[0011] According to the present disclosure, since the active material has a silicon clathrate crystal phase, the volume change due to charging and discharging can be reduced. Furthermore, since the active material in the present disclosure contains Al in addition to Si, the volume change due to charging and discharging can be reduced.

[0012] In the above disclosure, the active material may have voids inside the primary particles.

[0013] In the above disclosure, the voids may have a porosity of 2% or more and 15% or less.

[0014] In the above disclosure, the active material may have a silicon clathrate II type crystal phase as the silicon clathrate type crystal phase.

[0015] The present disclosure also provides a battery having a positive electrode layer, a negative electrode layer, and an electrolyte layer formed between the positive electrode layer and the negative electrode layer, wherein the negative electrode layer contains the active material described above.

[0016] According to the present disclosure, by using the above-described active material, a battery can be obtained in which the volume change due to charging and discharging is small.

[0017] The present disclosure also provides a method for producing an active material, comprising: a preparation step of preparing a Zintl compound that contains Na, Si and Al, has at least a Zintl phase, and has a ratio of Al to the total of the Si and the Al of less than 10 atm%; a Na removal step of removing the Na from the Zintl compound to form an intermediate having a silicon clathrate type crystal phase; and an Al removal step of removing the Al from the intermediate.

[0018] According to the present disclosure, by using a Zintl compound containing Al in addition to Na and Si, it is possible to obtain an active material that exhibits small volume change upon charging and discharging.

[0019] In the above disclosure, the preparing step may be a step of preparing the Zintl compound by heat treating a raw material mixture containing a Na source, a Si source, and an Al source.

[0020] The present disclosure also provides a method for manufacturing a battery, the method including: an active material manufacturing step of manufacturing an active material by the above-described active material manufacturing method; and an anode layer forming step of forming an anode layer using the active material.

[0021] According to the present disclosure, by using the above-mentioned active material, a battery with small volume change due to charging and discharging can be obtained. Effect of the Invention

[0022] The present disclosure has an effect of providing an active material that undergoes small volumetric change upon charging and discharging. [Brief description of the drawings]

[0023] [Figure 1] FIG. 2 is a schematic perspective view illustrating a crystalline phase of Si. [Diagram 2] FIG. 1 is a schematic cross-sectional view illustrating a battery according to the present disclosure. [Diagram 3] 1 is a flowchart illustrating a method for producing an active material in the present disclosure. [Figure 4] 1 shows the results of XRD measurement of the intermediate and active material obtained in Example 2. [Diagram 5] 1 shows the results of SEM observation of the active material obtained in Example 2. [Figure 6] 1 shows the results of SEM observation (cross section) of the active materials obtained in Examples 1 to 4 and Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The active material, the battery, and the manufacturing method thereof according to the present disclosure will be described in detail below.

[0025] A. Active material The active material according to the present disclosure contains at least Si and Al and has a silicon clathrate type crystal phase, with the ratio of the Al to the total of the Si and Al being 0.1 atm % or more and 1 atm % or less.

[0026] The active material in the present disclosure has a silicon clathrate crystal phase. In the silicon clathrate crystal phase, the skeleton atoms have a cage-shaped structure (cage), in which metal ions such as Li ions can enter. Even if metal ions enter the cage, the amount of expansion is small, so that the volume change due to charging and discharging is small. Examples of silicon clathrate crystal phases include silicon clathrate I and II crystal phases.

[0027] In the crystal phase of silicon clathrate type I and type II, as shown in Figs. 1(a) and (b), a polyhedron including a pentagon or hexagon is formed by a plurality of Si elements. The polyhedron has a space inside that can encapsulate metal ions such as Li ions. By inserting metal ions into this space, the volume change due to charging and discharging can be suppressed. In addition, since the crystal phase of silicon clathrate type I and type II has a space inside that can encapsulate metal ions, it has the advantage that the crystal structure is easily maintained even after repeated charging and discharging. In addition, in particular in all-solid-state batteries, it is generally necessary to apply a high confining pressure in order to suppress the volume change due to charging and discharging, but by using the active material in the present disclosure, the confining pressure can be reduced, and as a result, the size of the confining jig can be suppressed. On the other hand, normal Si particles have a diamond-type crystal phase. In the diamond-type crystal phase, as shown in Fig. 1(c), a tetrahedron is formed by a plurality of Si elements. Since the tetrahedron does not have a space inside that can encapsulate metal ions such as Li ions, the volume change due to charging and discharging is large.

[0028] Thus, according to the present disclosure, since the active material has a silicon clathrate crystal phase, the volume change due to charging and discharging can be reduced. Furthermore, since the active material in the present disclosure contains Al in addition to Si, the volume change due to charging and discharging can be reduced. The reason for this is presumed to be that a part of Si constituting the cage of the silicon clathrate crystal phase is replaced by Al, which is a different element, and the cage becomes larger. In addition, the larger cage reduces the resistance when metal ions are conducted. In addition, as described later, the active material in the present disclosure preferably has voids inside the primary particles, and in this case, in addition to the silicon clathrate crystal phase, the voids also contribute to suppressing the volume change, so that the volume change due to charging and discharging can be further suppressed.

[0029] The active material in the present disclosure contains at least Si and Al. The active material may contain only Si and Al as metal elements, or may contain other metal elements. Examples of other metal elements include Na. The active material may contain only Si, Al, and Na as metal elements. The total ratio of Si and Al to all metal elements contained in the active material is, for example, 60 atm% or more, may be 70 atm% or more, or may be 80 atm% or more.

[0030] In the active material, the ratio of Al to the total of Si and Al is usually 0.1 atm% or more, and may be 0.2 atm% or more, whereas the ratio of Al to the total of Si and Al is usually 1 atm% or less.

[0031] The composition of the active material in the present disclosure is not particularly limited, but may include Na x (Si,Al) 136 It is preferable that the composition is represented by (0≦x≦20). x may be 0 or may be greater than 0. On the other hand, x may be 10 or less, or 5 or less. The composition of the active material can be determined by, for example, EDX, XRD, XRF, ICP, or atomic absorption spectrometry.

[0032] The active material in the present disclosure has a silicon clathrate type crystal phase. The active material preferably has a silicon clathrate type as the main phase. "Having a silicon clathrate type as the main phase" means that the peak belonging to the silicon clathrate type crystal phase is the peak with the highest diffraction intensity among the peaks observed in X-ray diffraction measurement. The definition of "main phase" is the same for other crystal phases. In addition, the silicon clathrate type crystal phase has at least Si, but may further have Al. That is, a part of Si constituting the silicon clathrate type crystal phase may be replaced with Al.

[0033] Examples of silicon clathrate crystal phases include silicon clathrate I crystal phase and silicon clathrate II crystal phase. The active material in the present disclosure may contain silicon clathrate I crystal phase as the main phase, or may contain silicon clathrate II crystal phase as the main phase, but the latter is preferred. This is because it can further reduce the volume change caused by charging and discharging.

[0034] In addition, the active material in the present disclosure may (i) have a silicon clathrate I type crystal phase and may not have a silicon clathrate II type crystal phase, (ii) may not have a silicon clathrate I type crystal phase and may have a silicon clathrate II type crystal phase, or (iii) may have a silicon clathrate I type crystal phase and a silicon clathrate II type crystal phase. "Having no crystal phase" can be confirmed by observing no peak of the crystal phase in X-ray diffraction measurement. The definition of "having no crystal phase" is the same for other crystal phases.

[0035] The silicon clathrate I type crystal phase usually belongs to the space group (Pm-3n). The silicon clathrate I type crystal phase has typical peaks at 2θ=19.44°, 21.32°, 30.33°, 31.60°, 32.82°, 36.29°, 52.39°, and 55.49° in X-ray diffraction measurement using CuKα radiation. These peak positions may vary within a range of ±0.50°, ±0.30°, or ±0.10°, respectively.

[0036] The silicon clathrate II crystal phase usually belongs to the space group (Fd-3m). The silicon clathrate II crystal phase has typical peaks at 2θ=20.09°, 21.00°, 26.51°, 31.72°, 36.26°, and 53.01° in X-ray diffraction measurement using CuKα radiation. These peak positions may vary within a range of ±0.50°, ±0.30°, or ±0.10°, respectively.

[0037] The lattice constant of the crystal phase of silicon clathrate II type is, for example, 14.702 Å or more, and may be 14.706 Å or more. On the other hand, the lattice constant of the crystal phase of silicon clathrate II type is, for example, 14.717 Å or less. The lattice constant can be obtained by performing XRD measurement on the active material and performing Rietveld analysis on the obtained XRD chart.

[0038] In addition, the active material in the present disclosure may or may not have a diamond-type Si crystalline phase. The diamond-type Si crystalline phase has typical peaks at 2θ=28.44°, 47.31°, 56.10°, 69.17°, and 76.37° in X-ray diffraction measurement using CuKα radiation. These peak positions may vary within a range of ±0.50°, ±0.30°, or ±0.10°.

[0039] The peak intensity of peak A located at 2θ=31.72°±0.50° in the silicon clathrate II crystal phase is I A The peak intensity of peak B located at 2θ=28.44°±0.50° in the diamond-type Si crystal phase is I B Let us assume that B / I A is, for example, less than 1, and may be 0.5 or less, or may be 0.3 or less.

[0040] In addition, the active material of the present disclosure preferably does not have a peak due to a by-product, which will be described in detail in "C. Method for producing active material" below.

[0041] The shape of the active material in the present disclosure may be, for example, particulate. The active material may be primary particles, or may be secondary particles formed by agglomeration of primary particles. In either case, it is preferable that the primary particles have voids inside. The porosity of the voids is, for example, 2% or more, 5% or more, or 10% or more. On the other hand, the porosity is, for example, 40% or less, 20% or less, or 15% or less.

[0042] For example, the porosity can be calculated using the following procedure. First, a cross section of the electrode layer containing the active material is prepared by ion milling. The cross section is then observed with a SEM (scanning electron microscope) to obtain a photograph of the particles. From the obtained photograph, image analysis software is used to clearly distinguish between the silicon portion and the void portion, and the image is binarized. The areas of the silicon portion and the void portion are determined, and the porosity (%) is calculated using the following formula: Porosity (%) = 100 × (area of ​​void part) / ((area of ​​silicon part) + (area of ​​void part))

[0043] Specific image analysis and porosity calculation can be performed as follows. For example, Fiji ImageJ bundled with Java 1.8.0_172 (hereinafter, Fiji) is used as image analysis software. A secondary electron image and a backscattered electron image of the same field of view are combined to create an RGB color image. Then, in order to remove noise for each pixel, the obtained RGB image is blurred using the Fiji function "Median (filter size = 2)". Next, using the Fiji function "Weka Machine Learning", a person manually designates multiple arbitrary areas in the image from which the noise has been removed as silicon parts or void parts, respectively, to create training data that distinguishes between silicon parts and void parts. Then, based on the created training data, a machine distinguishes between silicon parts and void parts within Fiji, and the area ratio of the silicon parts and void parts is calculated.

[0044] For RGB color imaging, since both the secondary electron image and the backscattered electron image are expressed in grayscale, for example, the brightness x of each pixel in the secondary electron image is assigned to the Red value, and the brightness y of the backscattered electron image is similarly assigned to the Green value. This results in an RGB image where, for example, each pixel is represented as R=x, G=y, B=(x+y) / 2.

[0045] Detailed conditions for the above "Weka Machine Learning" are shown below. As training features (numerical image features that the machine focuses on when creating training data in machine learning), select Gaussian blur, Hessian, Membrane projections, Mean, Maximum, Anisotropic diffusion, Sobel filter, Difference of Gaussians, Variance, Minimum, and Median. As for other parameters, set Membrane thickness to 3, Membrane patch size to 19, Minimum sigma to 1.0, and Maximum sigma to 16.0.

[0046] The average particle size of the primary particles is, for example, 50 nm or more, may be 100 nm or more, or may be 150 nm or more. On the other hand, the average particle size of the primary particles is, for example, 3000 nm or less, may be 1500 nm or less, or may be 1000 nm or less. Also, the average particle size of the secondary particles is, for example, 1 μm or more, may be 2 μm or more, or may be 5 μm or more. On the other hand, the average particle size of the secondary particles is, for example, 60 μm or less, or may be 40 μm or less. The average particle size can be determined, for example, by observation with a SEM. It is preferable that the number of samples is large, for example, 20 or more, may be 50 or more, or may be 100 or more.

[0047] The active material in the present disclosure is generally used in batteries. The active material in the present disclosure may be either an anode active material or a cathode active material, with the former being preferred. The present disclosure can also provide an electrode layer (anode layer or cathode layer) having the above-mentioned active material, and a battery having the electrode layer. Examples of methods for producing the active material include the methods described in "C. Method for producing active material" below.

[0048] B.Battery Fig. 2 is a schematic cross-sectional view illustrating a battery according to the present disclosure. The battery 10 shown in Fig. 2 has a positive electrode layer 1, a negative electrode layer 2, an electrolyte layer 3 formed between the positive electrode layer 1 and the negative electrode layer 2, a positive electrode current collector 4 that collects current from the positive electrode layer 1, and a negative electrode current collector 5 that collects current from the negative electrode layer 2. In the present disclosure, the negative electrode layer 2 contains the active material described above in "A. Active material".

[0049] According to the present disclosure, by using the above-described active material, a battery can be obtained in which the volume change due to charging and discharging is small.

[0050] 1. Negative electrode layer The negative electrode layer is a layer containing at least a negative electrode active material. The negative electrode active material is the same as that described in "A. Active material" above, so the description here is omitted. The ratio of the negative electrode active material in the negative electrode layer is, for example, 20% by weight or more, may be 30% by weight or more, or may be 40% by weight or more. If the ratio of the negative electrode active material is too small, there is a possibility that sufficient energy density cannot be obtained. On the other hand, the ratio of the negative electrode active material is, for example, 80% by weight or less, may be 70% by weight or less, or may be 60% by weight or less. If the ratio of the negative electrode active material is too high, there is a possibility that the ionic conductivity and electronic conductivity in the negative electrode layer are relatively reduced.

[0051] The negative electrode layer may contain at least one of an electrolyte, a conductive material, and a binder, as necessary. Examples of the electrolyte include the electrolytes described in "C. Battery 3. Electrolyte Layer" below. Examples of the conductive material include carbon materials, metal particles, and conductive polymers. Examples of the carbon material include particulate carbon materials such as acetylene black (AB) and Ketjen black (KB), and fibrous carbon materials such as carbon fibers, carbon nanotubes (CNT), and carbon nanofibers (CNF). Examples of the binder include rubber-based binders and fluoride-based binders.

[0052] The thickness of the negative electrode layer is, for example, 0.1 μm or more and 1000 μm or less. The negative electrode layer in the present disclosure is generally used in batteries.

[0053] 2. Positive electrode layer The positive electrode layer is a layer containing at least a positive electrode active material, and may contain at least one of an electrolyte, a conductive material, and a binder, as necessary.

[0054] Examples of the positive electrode active material include oxide active materials. Examples of the oxide active material include LiCoO2, LiMnO2, LiNiO2, LiVO2, and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, etc., rock salt layered active materials, LiMn2O4, Li4Ti5O 12 , Li(Ni 0.5 Mn 1.5 )O4 and the like; and olivine type active materials such as LiFePO4, LiMnPO4, LiNiPO4, and LiCoPO4.

[0055] A coating layer containing a Li-ion conductive oxide may be formed on the surface of the oxide active material. This is because it can suppress the reaction between the oxide active material and a solid electrolyte (particularly a sulfide solid electrolyte). An example of the Li-ion conductive oxide is LiNbO3. The thickness of the coating layer is, for example, 1 nm or more and 30 nm or less. In addition, for example, Li2S can be used as the positive electrode active material.

[0056] The shape of the positive electrode active material may be, for example, particulate. 50 ) is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle diameter (D 50 ) is, for example, 50 μm or less, and may be 20 μm or less. 50 ) can be calculated, for example, from measurements using a laser diffraction particle size distribution analyzer or a scanning electron microscope (SEM).

[0057] The electrolyte, conductive material, and binder used in the positive electrode layer are the same as those described in "1. Negative electrode layer" above, so the description here is omitted. The thickness of the positive electrode layer is, for example, 0.1 μm or more and 1000 μm or less.

[0058] 3. Electrolyte layer The electrolyte layer is a layer formed between the positive electrode layer and the negative electrode layer, and contains at least an electrolyte. The electrolyte may be a solid electrolyte or a liquid electrolyte (electrolytic solution).

[0059] Examples of the solid electrolyte include inorganic solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and halide solid electrolytes, and organic polymer electrolytes such as polymer electrolytes. Examples of the sulfide solid electrolyte include solid electrolytes containing Li, X (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S. The sulfide solid electrolyte may further contain at least one of O and a halogen. Examples of the halogen include F, Cl, Br, and I. The sulfide solid electrolyte may be glass (amorphous) or glass ceramics. Examples of the sulfide solid electrolyte include Li2S-P2S5, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-SiS2, Li2S-GeS2, and Li2S-P2S5-GeS2.

[0060] The electrolyte preferably contains a supporting salt and a solvent. Examples of the supporting salt (lithium salt) of the electrolyte having lithium ion conductivity include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6, and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3. Examples of the solvent used in the electrolyte include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolyte preferably contains two or more kinds of solvents.

[0061] The thickness of the electrolyte layer is, for example, not less than 0.1 μm and not more than 1000 μm.

[0062] 4.Other configurations The battery in the present disclosure preferably has a positive electrode current collector that collects the positive electrode layer and a negative electrode current collector that collects the negative electrode layer. Examples of the material of the positive electrode current collector include SUS, aluminum, nickel, iron, titanium, and carbon. On the other hand, examples of the material of the negative electrode current collector include SUS, copper, nickel, and carbon.

[0063] The battery of the present disclosure may further include a restraining tool that applies a restraining pressure to the positive electrode layer, the electrolyte layer, and the negative electrode layer along the thickness direction. In particular, when the electrolyte layer is a solid electrolyte layer, it is preferable to apply a restraining pressure in order to form a good ion conduction path and an electron conduction path. The restraining pressure is, for example, 0.1 MPa or more, may be 1 MPa or more, or may be 5 MPa or more. On the other hand, the restraining pressure is, for example, 100 MPa or less, may be 50 MPa or less, or may be 20 MPa or less.

[0064] 5.Battery The type of battery in the present disclosure is not particularly limited, but is typically a lithium ion battery. The battery in the present disclosure may be a liquid battery containing an electrolytic solution as an electrolyte layer, or may be an all-solid-state battery having a solid electrolyte layer as an electrolyte layer. The battery in the present disclosure may be a primary battery or a secondary battery, but is preferably a secondary battery. This is because it can be repeatedly charged and discharged, and is useful, for example, as an in-vehicle battery.

[0065] The battery in the present disclosure may be a single cell or a stacked battery. The stacked battery may be a monopolar stacked battery (a parallel-connected stacked battery) or a bipolar stacked battery (a series-connected stacked battery). The shape of the battery may be, for example, a coin type, a laminate type, a cylindrical type, or a square type.

[0066] C. Method of manufacturing active material Fig. 3 is a flow chart illustrating a method for producing an active material according to the present disclosure. In the production method shown in Fig. 3, first, a Zintl compound containing Na, Si, and Al, having at least a Zintl phase, and having a ratio of Al to the total of Si and Al of less than 10 atm% is prepared (preparation step). Next, Na is removed from the Zintl compound to form an intermediate having a silicon clathrate type crystal phase (Na removal step). Next, Al is removed from the intermediate (Al removal step). This results in an active material having a silicon clathrate type crystal phase and voids inside the primary particles.

[0067] According to the present disclosure, by using a Zintl compound containing Al in addition to Na and Si, it is possible to obtain an active material that exhibits small volume change upon charging and discharging.

[0068] 1. Preparation process The preparation step in the present disclosure is a step of preparing a Zintl compound that contains Na, Si and Al, has at least a Zintl phase, and has a ratio of the Al to the total of the Si and the Al of less than 10 atm %.

[0069] The Zintl compound contains at least Na, Si and Al. The Zintl compound may contain only Na, Si and Al as metal elements, or may contain other metal elements. The total ratio of Na, Si and Al to all metal elements contained in the Zintl compound is, for example, 70 atm% or more, may be 80 atm% or more, or may be 90 atm% or more.

[0070] In the Zintl compound, the ratio of Al to the total of Si and Al is, for example, 0.1 atm% or more, may be 0.5 atm% or more, or may be 1 atm% or more. On the other hand, the ratio of Al to the total of Si and Al is usually less than 10 atm% and may be 8 atm% or less. The composition of the Zintl compound is not particularly limited, but may include Na z (Si,Al) 136It is preferable that the composition is represented by the formula (121≦z≦151). z may be 126 or more, or may be 131 or more. On the other hand, z may be 141 or less.

[0071] The Zintl compound has a Zintl phase. The Zintl phase has typical peaks at 2θ=16.10°, 16.56°, 17.64°, 20.16°, 27.96°, 33.60°, 35.68°, 40.22°, and 41.14° in an X-ray diffraction measurement using CuKα radiation. These peak positions may vary within a range of ±0.50°, or may vary within a range of ±0.30°. The Zintl compound preferably has a Zintl phase as a main phase. The Zintl compound may or may not have a silicon clathrate I type crystal phase. The Zintl compound may or may not have a silicon clathrate II type crystal phase.

[0072] The intermediate may have a Zintl phase containing Na, Si and Al, and a by-product containing at least Al. The Zintl phase preferably contains Na, Si and Al. A typical Zintl phase is composed of Na and Si, but if a portion of the Si is replaced by Al, it is presumed that a desired silicon clathrate type crystal phase (a silicon clathrate type crystal phase in which a portion of Si is replaced by Al) can be easily obtained.

[0073] The by-product contains at least Al. In X-ray diffraction measurement using CuKα radiation, the by-product preferably has peaks at 2θ=34.8° and 36.0°. These peak positions may vary within a range of ±0.3°, or within a range of ±0.1°. The by-product may contain at least one of Na and O in addition to Al.

[0074] The Zintl compound can be obtained by subjecting a raw material mixture containing a Na source, a Si source, and an Al source to heat treatment. Examples of the Na source include Na alone and an alloy mainly composed of Na. Examples of the Si source include Si alone and an alloy mainly composed of Si. Examples of the Al source include Al alone, an alloy mainly composed of Al, and an Al oxide. Examples of the Al oxide include Al2O3.

[0075] In the raw material mixture, the ratio of Na to the sum of Si and Al is not particularly limited, but may be, for example, 0.8 molar parts or more, or 1 molar part or more, per 1 molar part of the sum of Si and Al. On the other hand, for example, 1.5 molar parts or less, or 1.3 molar parts or less, per 1 molar part of the sum of Si and Al. Also, in the raw material mixture, the ratio of Al to the sum of Si and Al is, for example, 0.1 atm% or more, or may be 0.5 atm% or more, or may be 1 atm% or more. On the other hand, in the raw material mixture, the ratio of Al to the sum of Si and Al is, for example, less than 10 atm% or 8 atm% or less.

[0076] The heat treatment temperature is, for example, 500° C. or higher and 1000° C. or lower. The heat treatment time is, for example, 1 hour or higher and 50 hours or lower. In particular, it is preferable to perform the heat treatment under the conditions of about 700° C. (for example, 650° C. or higher and 750° C. or lower) and about 20 hours (for example, 15 hours or higher and 25 hours or lower).

[0077] 2.Na removal process The Na removal step in the present disclosure is a step of removing the Na from the Zintl compound to form an intermediate having a silicon clathrate type crystal phase.

[0078] A method for removing Na from the Zintl compound includes, for example, heat treatment. The heat treatment temperature is, for example, 280° C. or higher, and may be 300° C. or higher. Meanwhile, the heat treatment temperature is, for example, 500° C. or lower. The heat treatment time is, for example, 1 hour or more and 50 hours or less. The heat treatment may be performed in a normal pressure atmosphere or a reduced pressure atmosphere. In the latter case, the pressure during the heat treatment is, for example, 10 Pa or lower, may be 1 Pa or lower, or may be 0.1 Pa or lower. The heat treatment may also be performed in an inert atmosphere such as an Ar atmosphere.

[0079] The intermediate has a silicon clathrate type crystal phase. The intermediate preferably has a silicon clathrate type crystal phase as a main phase. The intermediate may contain a silicon clathrate I type crystal phase as a main phase, or may contain a silicon clathrate II type crystal phase as a main phase, but the latter is preferred. This is because the volume change due to charging and discharging can be further reduced.

[0080] The intermediate may (i) have a silicon clathrate I type crystal phase and may not have a silicon clathrate II type crystal phase, (ii) may not have a silicon clathrate I type crystal phase and may have a silicon clathrate II type crystal phase, or (iii) may have a silicon clathrate I type crystal phase and a silicon clathrate II type crystal phase. The composition of the intermediate is not particularly limited, but may include Na y (Si,Al) 136 It is preferable that the formula is expressed as (0≦y≦24). y may be 0 or may be greater than 0. On the other hand, y may be 20 or less, or may be 10 or less.

[0081] 3.Al removal process The Al removing step in the present disclosure is a step of removing the Al from the intermediate. "Removing Al" also includes removing compounds containing Al (e.g., the above-mentioned by-products). By removing Al, an active material having voids inside the primary particles is obtained.

[0082] An example of a method for removing Al from the intermediate is acid treatment. The acid treatment is, for example, a treatment in which an acid solution is brought into contact with the intermediate. The acid solution has, for example, an acid and a solvent. Examples of acids used in the acid solution include hydrochloric acid, sulfuric acid, acetic acid, formic acid, propionic acid, oxalic acid, and hydrofluoric acid. The solvent used in the acid solution may be water or an organic solvent. The acid concentration (normality) in the acid solution is not particularly limited, but is, for example, 0.5 N or more and 3 N or less. Instead of the acid solution, the acid itself may be used without diluting it with a solvent.

[0083] 4.Active material The active material obtained by each of the above-mentioned steps has a silicon clathrate type crystal phase. The active material preferably contains at least Si and Al, and the ratio of Al to the total of Si and Al is within a predetermined range. Furthermore, the active material preferably has voids inside the primary particles. For preferred embodiments of the active material, the contents described in "A. Active material" above can be cited as appropriate.

[0084] D. Battery manufacturing method The present disclosure provides a method for manufacturing a battery, including an active material manufacturing step of manufacturing an active material by the above-described active material manufacturing method, and a negative electrode layer forming step of forming a negative electrode layer using the active material.

[0085] According to the present disclosure, by using the above-mentioned active material, a battery with small volume change due to charging and discharging can be obtained. Note that the active material manufacturing process is the same as that described in "C. Method for manufacturing active material" above.

[0086] In the negative electrode layer forming step, the negative electrode layer is formed using the active material. The method for forming the negative electrode layer is not particularly limited, and a known method can be adopted. For example, a slurry containing at least the active material is applied to the negative electrode current collector, and then dried to obtain the negative electrode layer formed on the negative electrode current collector. For preferred aspects of the obtained negative electrode layer, the contents described in "B. Battery 1. Negative Electrode Layer" above can be appropriately cited.

[0087] The method for forming the battery is not particularly limited, and a known method can be adopted. The method for manufacturing the battery in the present disclosure may include, in addition to the active material manufacturing step and the anode layer forming step, a cathode layer forming step for forming a cathode layer, an electrolyte layer forming step for forming an electrolyte layer, and an arrangement step for arranging the cathode layer, the electrolyte layer, and the anode layer in this order. For preferred embodiments of the obtained battery, the contents described in "B. Battery" above can be appropriately cited.

[0088] The present disclosure is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present disclosure and that exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES

[0089] [Example 1] (Synthesis of active materials) Si elemental substance (99% purity, with Si oxide coating on the surface), Al elemental substance, and Na elemental substance (99.5% purity) were mixed to a molar ratio (atm ratio) of Si elemental substance:Al elemental substance:Na elemental substance = 0.995:0.005:1.1. In the obtained mixture, the ratio of Al to the total of Si and Al was 0.5 atm%. Next, the obtained mixture was put into a boron nitride crucible, sealed under an Ar atmosphere, and heated under conditions of 700 ° C. and 20 hours to synthesize a Zintle compound (lump) containing Na, Si, and Al. The obtained Zintle compound was crushed and heated under conditions of 340 ° C. under vacuum (about 0.1 Pa) for 20 hours to remove Na, and an intermediate was obtained. The obtained intermediate was treated with dilute hydrochloric acid (1N) for 10 minutes to remove Al (by-product containing Al), and an active material was obtained.

[0090] (Preparation of negative electrode) The dispersion medium (butyl butyrate), binder (butyl butyrate solution in which 5% by weight of polyvinylidene fluoride was dissolved), the above-mentioned active material, solid electrolyte (Li2S-P2S5-based glass ceramic), and conductive material (VGCF (vapor grown carbon fiber)) were placed in a polypropylene container, shaken for 3 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.), and further stirred for 30 seconds with an ultrasonic dispersion device to prepare a slurry for the negative electrode layer. The slurry for the negative electrode layer was applied onto a negative electrode current collector (copper foil) by the blade method using an applicator, and then dried for 30 minutes on a hot plate adjusted to 100°C. As a result, a negative electrode having a negative electrode layer and a negative electrode current collector was obtained.

[0091] (Preparation of positive electrode) Dispersion medium (butyl butyrate), binder (butyl butyrate solution containing 5% by weight of polyvinylidene fluoride), positive electrode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 The positive electrode layer slurry was produced by placing the positive electrode layer slurry in a polypropylene container, shaking the positive electrode layer slurry for 3 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.) and stirring for 30 seconds with an ultrasonic disperser. The positive electrode layer slurry was applied to a positive electrode current collector (aluminum foil) by the blade method using an applicator, and then dried for 30 minutes on a hot plate adjusted to 100°C. This produced a positive electrode having a positive electrode layer and a positive electrode current collector.

[0092] (Preparation of solid electrolyte layer) A dispersion medium (heptane), a binder (a heptane solution containing 5% by weight of butadiene rubber), and a solid electrolyte (Li2S-P2S5-based glass ceramic containing lithium iodide) were placed in a polypropylene container and stirred for 30 seconds with an ultrasonic dispersion device. The polypropylene container was then shaken for 30 minutes with a shaker to produce a slurry for the solid electrolyte layer. The slurry for the solid electrolyte layer was applied to an aluminum foil substrate by a blade method using an applicator, and then dried for 30 minutes on a hot plate heated to 100°C to produce a solid electrolyte layer on the substrate.

[0093] (Preparation of evaluation battery) The negative electrode, the solid electrolyte layer, and the positive electrode were laminated in this order, and the resulting laminate was pressed under conditions of 130° C., 200 MPa, and 3 minutes to obtain a battery for evaluation.

[0094] [Examples 2 to 4] Active materials and evaluation batteries were obtained in the same manner as in Example 1, except that the ratio of Al to the total of Si and Al (Al charging amount) was changed to 1 atm% (Example 2), 3 atm% (Example 3), and 5 atm% (Example 4).

[0095] [Comparative Example 1] An active material and a battery for evaluation were obtained in the same manner as in Example 1, except that elemental Al was not used.

[0096] [Comparative Example 2] An active material and a battery for evaluation were obtained in the same manner as in Example 2, except that the acid treatment was not carried out.

[0097] [Comparative Example 3] An active material and a battery for evaluation were obtained in the same manner as in Example 1, except that the ratio of Al to the total of Si and Al (Al charging amount) was changed to 10 atm %.

[0098] [evaluation] (XRD measurement) X-ray diffraction (XRD) measurement using CuKα radiation was performed on the active materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3. It was confirmed that all of the active materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3 had a silicon clathrate II type crystal phase as the main phase. In addition, the XRD patterns of the silicon clathrate II type crystal phase were subjected to Rietveld analysis to determine the lattice constants. Furthermore, the relative values ​​of the lattice constants of Examples 1 to 4 and Comparative Examples 2 and 3 were determined based on the lattice constant of Comparative Example 1. The results are shown in Table 1.

[0099] As a representative result, the XRD charts of the intermediate (before acid treatment) and active material (after acid treatment) obtained in Example 2 are shown in FIG. 4. As shown in FIG. 4(a), it was confirmed that the intermediate before the acid treatment has a silicon clathrate II type crystal phase as the main phase, and further has peaks derived from by-products at 2θ=34.8° and 36.0°. On the other hand, as shown in FIG. 4(b), it was confirmed that the active material after the acid treatment also has a silicon clathrate II type crystal phase as the main phase, similar to the intermediate. On the other hand, unlike the intermediate, the active material after the acid treatment had no peaks derived from by-products. That is, it was confirmed that the by-products were removed by the acid treatment.

[0100] (SEM-EDX measurement) The active materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were subjected to SEM-EDX (scanning electron microscope-energy dispersive X-ray spectroscopy) measurement. As a representative result, an SEM image of the active material obtained in Example 2 is shown in FIG. 5. As shown in FIG. 5, the active material obtained in Example 2 was confirmed to be porous. Furthermore, the EDX result confirmed that Al and Na were uniformly dispersed. Furthermore, O was detected in a proportion greater than Al and less than Na. Furthermore, the EDX result determined the proportion of Al to the total of Si and Al, which was 0.2 atm%. Furthermore, the SEM-EDX measurement of the intermediate suggested that the by-product contained Na, Al, and O.

[0101] The cross-sections of particles were observed with an SEM for the active materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3. The results of Examples 1 to 4 and Comparative Example 3 (results of adding Al and carrying out an acid treatment) are shown in FIG. 6. As shown in FIG. 6, voids were formed inside the primary particles. In addition, the SEM images were analyzed to determine the porosity. The results are shown in Table 1.

[0102] (Measurement of increase in confining pressure) The evaluation batteries obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were charged, and the increase in the confining pressure was measured. Specifically, the evaluation batteries were confined at 5 MPa using a confining jig capable of measuring the confining pressure with a load cell, placed in a desiccator, and charged at a constant current of 0.1 C to a voltage of 4.55 V, and the confining pressure at 4.55 V was measured, and the increase in the confining pressure from the state before charging was calculated. The results are shown in Table 1. The results of the increase in the confining pressure in Table 1 are relative values ​​when the result of Comparative Example 1 is set to 1.

[0103] [Table 1]

[0104] As shown in Table 1, it was confirmed that the increase in the confining pressure was smaller in Examples 1 to 4 than in Comparative Examples 1 to 3. In addition, the following points were confirmed. First, regarding the lattice constant, it was confirmed that the lattice constant was larger in Examples 1 to 4 than in Comparative Example 1. It is presumed that the reason for the increase in the lattice constant is that a part of Si is replaced by Al, which is a different element. It is presumed that this replacement makes the cage of the silicon clathrate type crystal phase larger (reducing the density as an active material), and as a result, even when Li is inserted, the increase in the confining pressure can be suppressed.

[0105] Next, in Examples 1 to 4, by-products were removed by performing an acid treatment, and voids were formed inside the primary particles. Thus, it is presumed that, in Examples 1 to 4, voids were formed inside the primary particles, and thus, even when Li was inserted, an increase in the confining pressure could be suppressed. On the other hand, in Comparative Example 1, since Al was not added, voids were not formed inside the primary particles.

[0106] In Comparative Example 2, since the acid treatment was not performed, voids were not formed inside the primary particles. It is presumed that since the acid treatment was not performed in Comparative Example 2, by-products remained in the active material, and the effect of suppressing the increase in the confining pressure was not obtained. It is also presumed that the remaining by-products became resistance, inhibiting the Li ion path, causing the resistance increase.

[0107] In addition, the increase in confining pressure in Comparative Example 3 was larger than that in Comparative Example 1. This is presumably because the amount of by-products generated was large due to the large amount of Al charged, making it difficult to maintain the silicon clathrate type crystal phase after the acid treatment. [Explanation of symbols]

[0108] 1 ... Positive electrode layer 2...electrolyte layer 3...Anode layer 4...Positive electrode current collector 5...Negative electrode current collector 10...battery

Claims

1. An active material containing at least Si and Al, In the active material, a ratio of the Al to the total of the Si and the Al is 0.1 atm % or more and 1 atm % or less, The active material has voids inside primary particles.

2. The active material according to claim 1 , wherein the porosity of the pores is 2% or more and 15% or less.

3. The active material according to claim 1 or 2, wherein the active material has a silicon clathrate type crystal phase.

4. The active material according to claim 3 , wherein the active material has a silicon clathrate II type crystal phase as the silicon clathrate type crystal phase.

5. A battery having a positive electrode layer, a negative electrode layer, and an electrolyte layer formed between the positive electrode layer and the negative electrode layer, A battery, wherein the negative electrode layer contains the active material according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Clathrate compound and thermoelectric conversion element using same

    JP2007073640A

  • Clathrate compound, thermoelectric conversion material, and manufacturing method of thermoelectric conversion material

    JP2012033867A

  • Electroactive material for a metal ion battery

    JP2017531276A

  • Active material and battery

    JP2020017513A

  • Active material, battery and method for producing active material

    JP2020087886A