Positive electrode active material
A stabilized lithium-cobalt-based positive electrode active material with calculated substitution energies enhances the energy density and cycle stability of lithium-ion batteries, addressing the instability issues in existing technologies.
Patent Information
- Application Number
- JP2024118441
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-11-16
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-11-05
AI Technical Summary
Existing lithium-ion secondary batteries face challenges in achieving high energy density, improved cycle characteristics, and long-term reliability, particularly due to the instability of positive electrode active materials under repeated charging and discharging cycles.
A positive electrode active material composed of lithium, cobalt, and elements such as magnesium or zirconium, with a layered rock-salt structure, is developed, where the substitution energy differences are calculated using first-principles methods to stabilize the crystal structure and enhance stability during charge-discharge cycles.
The proposed active material maintains high capacity and suppresses capacity degradation, providing excellent charge-discharge cycle characteristics and improved safety in lithium-ion secondary batteries.
Smart Images

Figure 2024144557000001_ABST
Abstract
Description
[Technical field]
[0001] One embodiment of the present invention relates to an object, a method, or a manufacturing method. Alternatively, the present invention relates to a process, a machine, a manufacture, or a composition of matter. One embodiment of the present invention relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, or an electronic device, or a manufacturing method thereof. In particular, the present invention relates to a positive electrode active material that can be used in a secondary battery, a secondary battery, and an electronic device having a secondary battery.
[0002] In this specification, the term "power storage device" refers to elements and devices in general that have a power storage function, including, for example, storage batteries (also called secondary batteries) such as lithium ion secondary batteries, lithium ion capacitors, and electric double layer capacitors.
[0003] In addition, in this specification, electronic devices refer to devices in general that have a power storage device, and electro-optical devices that have a power storage device, information terminal devices that have a power storage device, and the like are all electronic devices. [Background technology]
[0004] In recent years, various types of power storage devices, such as lithium-ion secondary batteries, lithium-ion capacitors, and air batteries, have been actively developed. In particular, the demand for high-output, high-energy-density lithium-ion secondary batteries has rapidly expanded in conjunction with the development of the semiconductor industry, and they are now indispensable in the modern information society as a rechargeable energy source, as they are used in portable information terminals such as mobile phones, smartphones, tablets, and notebook computers, portable music players, digital cameras, medical equipment, and next-generation clean energy vehicles (hybrid electric vehicles (HEVs), electric vehicles (EVs), plug-in hybrid electric vehicles (PHEVs), etc.).
[0005] The characteristics required for lithium ion secondary batteries include higher energy density, improved cycle characteristics, safety in various operating environments, and improved long-term reliability.
[0006] Therefore, improvements in the positive electrode active material have been studied with the aim of improving the cycle characteristics and increasing the capacity of lithium ion secondary batteries (Patent Documents 1 and 2). Research on the crystal structure of the positive electrode active material has also been conducted (Non-Patent Documents 1 to 3).
[0007] X-ray diffraction (XRD) is one of the techniques used to analyze the crystal structure of positive electrode active materials. XRD data can be analyzed by using the Inorganic Crystal Structure Database (ICSD) introduced in Non-Patent Document 5.
[0008] Furthermore, as shown in Non-Patent Documents 6 and 7, the use of first-principles calculations makes it possible to calculate the energy according to the crystal structure, composition, and the like of a compound.
[0009] Patent Document 3 describes LiNi 1-x M x An example of using first-principles calculations for O2 is shown. Patent Document 4 also describes the formation energy of silicon oxide compounds obtained by first-principles calculations. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2002-216760 A [Patent Document 2] JP 2006-261132 A [Patent Document 3] JP 2016-091633 A [Patent Document 4] International Publication No. 2011 / 077654 [Non-patent literature]
[0011] [Non-Patent Document 1] Toyoki Okumura et al, “Correlation of lithium ion distribution and X-ray absorption near-edge structure in O3-and O2-lithium cobalt oxides from first-principle calculation”, Journal of Materials Chemistry, 2012, 22, pp.17340-17348 [Non-Patent Document 2] Motohashi, T. et al, “Electronic phase diagram of the layered cobalt oxide system LixCoO2(0.0≦x≦1.0)”, Physical Review B, 80(16) ,2009, 165114 [Non-Patent Document 3] Zhaohui Chen et al, “Staging Phase Transitions in LixCoO2”, Journal of The Electrochemical Society, 2002, 149(12) A1604-A1609 [Non-Patent Document 4] WE Counts et al, Journal of the American Ceramic Society, 1953, 36[1] 12-17. Fig.01471 [Non-Patent Document 5] Belsky, A. et al., “New developments in the Inorganic Crystal Structure Database (ICSD): accessibility in support of materials research and design”, Acta Cryst., 2002, B58 364-369. [Non-Patent Document 6] Dudarev, SL et al, “Electron-energy-loss spectra and the structural stability of nickel oxide: An LSDA1U study”, Physical Review B, 1998, 57(3) 1505. [Non-Patent Document 7] Zhou, F. et al, “First-principles prediction of redox potentials in transition-metal compounds with LDA+U”, Physical Review B, 2004, 70 235121. Summary of the Invention [Problem to be solved by the invention]
[0012] An object of one embodiment of the present invention is to provide a positive electrode active material for a secondary battery having high capacity and excellent charge / discharge cycle characteristics. Another object of one embodiment of the present invention is to provide a method for manufacturing a positive electrode active material with high productivity. Another object of one embodiment of the present invention is to provide a positive electrode active material that is used in a secondary battery and suppresses a decrease in capacity during charge / discharge cycles. Another object of one embodiment of the present invention is to provide a high-capacity secondary battery. Another object of one embodiment of the present invention is to provide a secondary battery with excellent charge / discharge characteristics. Another object of one embodiment of the present invention is to provide a secondary battery with high safety or reliability.
[0013] Another object of one embodiment of the present invention is to provide a novel substance, active material particles, a power storage device, or a manufacturing method thereof.
[0014] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that it is possible to extract problems other than these from the description of the specification, drawings, and claims. [Means for solving the problem]
[0015] One aspect of the present invention is a positive electrode active material having lithium, cobalt, and element X, having a region represented by a layered rock salt structure, the region having a space group represented by R-3m, and element X having a property that ΔE3, which is the value obtained by subtracting the stabilization energy before substitution from the stabilization energy when substituted at the lithium position of LiCoO2, is smaller than ΔE4, which is the value obtained by subtracting the stabilization energy before substitution from the stabilization energy when substituted at the cobalt position of LiCoO2. ΔE3 and ΔE4 are calculated by first-principles calculation, and it is a positive electrode active material.
[0016] Further, in the above configuration, in the first-principles calculation, it is preferable that LiCoO2 has a layered rock salt structure and is represented by the space group R-3m, and ΔE3 is 1 eV or less.
[0017] Further, in the above configuration, it is preferable that element X has one or more selected from calcium, magnesium, and zirconium.
[0018] Alternatively, one aspect of the present invention is a positive electrode active material having lithium, cobalt, nickel, manganese, and element X, having a region represented by a layered rock salt structure, the region having a space group represented by R-3m, and element X having a property that ΔE5, which is the value obtained by subtracting the stabilization energy before substitution from the stabilization energy when substituted at the lithium position of LiCo x Ni y Mn z O2, is smaller than ΔE6, which is the smallest value among the values obtained by subtracting the stabilization energy before substitution from the respective stabilization energies when substituted at the cobalt position, nickel position, and manganese position of LiCo x Ni y Mn z O2. 0.8 < x + y + z < 1.2 is satisfied, y and z are greater than 0.1 times x and less than 8 times x, and ΔE5 and ΔE6 are calculated by first-principles calculation, and it is a positive electrode active material.
[0019] In the above configuration, it is preferable that the atomic ratio of cobalt, nickel, and manganese in the positive electrode active material is X1:Y1:Z1, where X1 is greater than 0.8 and less than 1.2 times x, Y1 is greater than 0.8 and less than 1.2 times y, and Z1 is greater than 0.8 and less than 1.2 times z.
[0020] In the above configuration, the first-principles calculations showed that LiCo x Ni y Mn z It is preferable that O2 has a layered rock-salt structure and is represented by the space group R-3m, and the absolute value of ΔE5 is 1 eV or less.
[0021] Alternatively, one embodiment of the present invention is a positive electrode active material having lithium, nickel, and an element X, which has a region represented by a layered rock salt structure, the region being represented by a space group of R-3m, and the element X being substituted at the lithium position of LiNiO2, the stabilization energy ΔE7, which is a value obtained by subtracting the stabilization energy before the substitution from the stabilization energy before the substitution, is LiCo x Ni y Mn z The element is one or more elements selected from among elements having properties smaller than ΔE8, which is the stabilization energy when substituted at the nickel position of O2 minus the stabilization energy before substitution, and ΔE7 and ΔE8 are positive electrode active materials calculated by first-principles calculations.
[0022] In the above configuration, it is preferable that LiNiO2 has a layered rock-salt structure and is represented by the space group R-3m in the first-principles calculation, and that ΔE7 is 1 eV or less.
[0023] In the above structure, it is preferable that the element X is substituted at the lithium site or the cobalt site with oxygen at a ratio of 1 to 54 in the first-principles calculation.
[0024] In the above configuration, the concentration of element X in the positive electrode active material detected by X-ray photoelectron spectroscopy is preferably 0.4 to 1.5, where the sum of the concentrations of cobalt, nickel, and manganese detected by X-ray photoelectron spectroscopy is 1.
[0025] In the above structure, the positive electrode active material preferably contains fluorine.
[0026] In the above-described structure, the positive electrode active material preferably contains phosphorus, and the number of phosphorus atoms in the positive electrode active material is preferably 0.01 to 0.12 times the sum of the number of cobalt, nickel, and manganese atoms.
[0027] In the above configuration, a secondary battery using the positive electrode active material in a positive electrode and lithium metal in a negative electrode is charged at a constant current until the battery voltage reaches 4.6 V in a 25° C. environment, and then charged at a constant voltage until the current value reaches 0.01 C. When the positive electrode is analyzed by powder X-ray diffraction using CuKα1 radiation, it is preferable that the battery has diffraction peaks at 2θ=19.30±0.20° and 2θ=45.55±0.10°.
[0028] Another embodiment of the present invention is a secondary battery including a positive electrode in which a positive electrode active material layer including any of the above positive electrode active materials is supported on a current collector, and a negative electrode.
[0029] Another embodiment of the present invention is an electronic device including the above secondary battery and a display portion.
[0030] Another aspect of the present invention is a vehicle having the secondary battery described above and an electric motor. Effect of the Invention
[0031] According to one embodiment of the present invention, a positive electrode active material for a secondary battery having high capacity and excellent charge / discharge cycle characteristics, and a manufacturing method thereof can be provided. In addition, a manufacturing method of the positive electrode active material with good productivity can be provided. In addition, a positive electrode active material that is used in a secondary battery and suppresses a decrease in capacity during charge / discharge cycles can be provided. In addition, a high-capacity secondary battery can be provided. In addition, a secondary battery with excellent charge / discharge characteristics can be provided. In addition, a secondary battery with high safety or reliability can be provided. In addition, a novel material, active material particles, power storage device, or a manufacturing method thereof can be provided. [Brief description of the drawings]
[0032] [Figure 1] FIG. 1 is a diagram illustrating the charge depth and the crystal structure of a positive electrode active material according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram illustrating the charge depth and crystal structure of a conventional positive electrode active material. [Diagram 3] FIG. 3 is an XRD pattern calculated from the crystal structure. [Figure 4] 4A and 4B are diagrams illustrating a crystal structure and magnetism of a positive electrode active material according to one embodiment of the present invention. [Diagram 5] Fig. 5A is a diagram illustrating the crystal structure of a conventional positive electrode active material, and Fig. 5B is a diagram illustrating the magnetism of the conventional positive electrode active material. [Figure 6] FIG. 6 illustrates an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention. [Figure 7] Fig. 7A is a cross-sectional view of an active material layer in which a graphene compound is used as a conductive assistant, and Fig. 7B is a cross-sectional view of an active material layer in which a graphene compound is used as a conductive assistant. [Figure 8] Fig. 8A is a diagram for explaining a method for charging a secondary battery, Fig. 8B is a diagram for explaining a method for charging a secondary battery, and Fig. 8C is a diagram showing an example of a secondary battery voltage and a charging current. [Figure 9]Fig. 9A is a diagram for explaining a method for charging a secondary battery. Fig. 9B is a diagram for explaining a method for charging a secondary battery. Fig. 9C is a diagram for explaining a method for charging a secondary battery. Fig. 9D is a diagram showing an example of a secondary battery voltage and a charging current. [Figure 10] FIG. 10 is a diagram showing an example of the secondary battery voltage and discharge current. [Figure 11] Fig. 11A is a diagram illustrating a coin-type secondary battery, Fig. 11B is a diagram illustrating a coin-type secondary battery, and Fig. 11C is a diagram illustrating charging of the secondary battery. [Figure 12] Fig. 12A is a diagram for explaining a cylindrical secondary battery, Fig. 12B is a diagram for explaining a cylindrical secondary battery, Fig. 12C is a diagram for explaining a plurality of secondary batteries, and Fig. 12D is a diagram for explaining a plurality of secondary batteries. [Figure 13] Fig. 13A is a diagram illustrating an example of a battery pack, and Fig. 13B is a diagram illustrating an example of a battery pack. [Figure 14] Fig. 14A is a diagram for explaining an example of a battery pack. Fig. 14B is a diagram for explaining an example of a battery pack. Fig. 14C is a diagram for explaining an example of a battery pack. Fig. 14D is a diagram for explaining an example of a battery pack. [Figure 15] Fig. 15A is a diagram illustrating an example of a secondary battery, and Fig. 15B is a diagram illustrating an example of a secondary battery. [Figure 16] FIG. 16 is a diagram for explaining an example of a wound body. [Figure 17] Fig. 17A is a diagram for explaining the configuration of a laminated secondary battery, Fig. 17B is a diagram for explaining a laminated secondary battery, and Fig. 17C is a diagram for explaining a laminated secondary battery. [Figure 18] Fig. 18A is a diagram illustrating a laminated secondary battery, and Fig. 18B is a diagram illustrating a laminated secondary battery. [Figure 19] FIG. 19 is a diagram showing the external appearance of a secondary battery. [Figure 20] FIG. 20 is a diagram showing the external appearance of a secondary battery. [Figure 21]Fig. 21A is a diagram showing an example of a positive electrode and an example of a negative electrode, Fig. 21B is a diagram explaining a method for producing a secondary battery, and Fig. 21C is a diagram explaining a method for producing a secondary battery. [Figure 22] Fig. 22A is a diagram explaining a bendable secondary battery. Fig. 22B is a diagram explaining a bendable secondary battery. Fig. 22C is a diagram explaining a bendable secondary battery. Fig. 22D is a diagram explaining a bendable secondary battery. Fig. 22E is a diagram explaining a bendable secondary battery. [Figure 23] Fig. 23A is a diagram illustrating a bendable secondary battery, and Fig. 23B is a diagram illustrating a bendable secondary battery. [Figure 24] FIG. 24A is a diagram for explaining an example of an electronic device. FIG. 24B is a diagram for explaining an example of an electronic device. FIG. 24C is a diagram for explaining an example of an electronic device. FIG. 24D is a diagram for explaining an example of an electronic device. FIG. 24E is a diagram for explaining an example of a secondary battery. FIG. 24F is a diagram for explaining an example of an electronic device. FIG. 24G is a diagram for explaining an example of an electronic device. FIG. 24H is a diagram for explaining an example of an electronic device. [Diagram 25] Fig. 25A is a diagram illustrating an example of an electronic device, Fig. 25B is a diagram illustrating an example of an electronic device, and Fig. 25C is a diagram illustrating a charge control circuit. [Figure 26] FIG. 26 is a diagram illustrating an example of an electronic device. [Figure 27] Fig. 27A is a diagram illustrating an example of a vehicle, Fig. 27B is a diagram illustrating an example of a vehicle, and Fig. 27C is a diagram illustrating an example of a vehicle. [Figure 28] Fig. 28A is a diagram showing the calculation results of energy, Fig. 28B is a diagram showing the calculation results of energy, and Fig. 28C is a diagram showing the calculation results of energy. [Figure 29] Fig. 29A is a diagram showing the calculation results of energy, Fig. 29B is a diagram showing the calculation results of energy, and Fig. 29C is a diagram showing the calculation results of energy. [Diagram 30]Fig. 30A is a diagram showing the calculation results of energy, Fig. 30B is a diagram showing the calculation results of energy, and Fig. 30C is a diagram showing the calculation results of energy. [Diagram 31] Fig. 31A is a diagram showing the calculation results of energy, Fig. 31B is a diagram showing the calculation results of energy, and Fig. 31C is a diagram showing the calculation results of energy. [Diagram 32] Fig. 32A is a diagram showing the calculation results of energy, Fig. 32B is a diagram showing the calculation results of energy, and Fig. 32C is a diagram showing the calculation results of energy. [Diagram 33] Fig. 33A is a diagram showing the calculation results of energy, Fig. 33B is a diagram showing the calculation results of energy, and Fig. 33C is a diagram showing the calculation results of energy. [Diagram 34] Fig. 34A is a diagram showing the calculation results of energy, and Fig. 34B is a diagram showing the calculation results of energy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be easily understood by those skilled in the art that the form and details of the present invention can be modified in various ways. Furthermore, the present invention is not to be interpreted as being limited to the description of the embodiments shown below.
[0034] In addition, in this specification and the like, crystal planes and directions are indicated using Miller indices. In crystallography, crystal planes and directions are indicated by placing a superscript bar on the numbers, but in this specification and the like, due to restrictions on notation in applications, numbers may be indicated by placing a - (minus sign) before them instead of placing a bar above them. Also, individual directions indicating directions within a crystal are expressed with [ ], collective directions indicating all equivalent directions with < >, individual faces indicating crystal faces with ( ), and collective faces with equivalent symmetry with {}.
[0035] In this specification and the like, segregation refers to a phenomenon in which a certain element (eg, B) is spatially non-uniformly distributed in a solid composed of a plurality of elements (eg, A, B, C).
[0036] In this specification, the surface layer of a particle of an active material or the like refers to a region from the surface to a depth of about 10 nm. Surfaces caused by cracks or chips may also be called the surface. The region deeper than the surface layer is called the interior.
[0037] In this specification, the layered rock-salt type crystal structure of a composite oxide containing lithium and a transition metal refers to a crystal structure having a rock-salt type ion arrangement in which cations and anions are alternately arranged, and in which the transition metal and lithium are regularly arranged to form a two-dimensional plane, allowing two-dimensional diffusion of lithium. Defects such as deficiencies of cations or anions may be present. Strictly speaking, the layered rock-salt type crystal structure may have a structure in which the lattice of the rock-salt type crystal is distorted.
[0038] In this specification and the like, the rock salt type crystal structure refers to a structure in which cations and anions are arranged alternately, and it is acceptable for there to be a deficiency of cations or anions.
[0039] In the present specification and the like, the pseudo-spinel crystal structure of a composite oxide containing lithium and a transition metal refers to a crystal structure that is in the space group R-3m and is not a spinel crystal structure, but has ions of cobalt, magnesium, etc. occupying 6-coordination oxygen positions and has a symmetry similar to that of the spinel type in the arrangement of cations. In the pseudo-spinel crystal structure, a light element such as lithium may occupy 4-coordination oxygen positions, and in this case, the arrangement of ions also has a symmetry similar to that of the spinel type.
[0040] It can also be said that the pseudo-spinel type crystal structure is a crystal structure similar to the CdCl2 type crystal structure, although it has random Li between the layers. This CdCl2 type-like crystal structure was observed when lithium nickel oxide was charged to a charge depth of 0.94 (Li 0.06The crystal structure is close to that of lithium cobalt oxide (NiO2), but it is known that pure lithium cobalt oxide or layered rock salt type positive electrode active materials that contain a large amount of cobalt do not usually have this crystal structure.
[0041] The layered rock salt crystal and the anions of the rock salt crystal have a cubic close-packed structure (face-centered cubic lattice structure). It is presumed that the anions of the pseudo-spinel crystal also have a cubic close-packed structure. When they contact, there is a crystal plane where the orientation of the cubic close-packed structure formed by the anions is aligned. However, the space group of the layered rock salt crystal and the pseudo-spinel crystal is R-3m, which is different from the space group Fm-3m (the space group of a general rock salt crystal) and Fd-3m (the space group of a rock salt crystal with the simplest symmetry) of the rock salt crystal, so the Miller indices of the crystal planes that satisfy the above conditions are different between the layered rock salt crystal and the pseudo-spinel crystal and the rock salt crystal. In this specification, when the orientation of the cubic close-packed structure formed by the anions is aligned in the layered rock salt crystal, the pseudo-spinel crystal, and the rock salt crystal, it may be said that the crystal orientation is approximately the same.
[0042] The crystal orientation of the two regions roughly coincides with each other, which can be determined from TEM (transmission electron microscope) images, STEM (scanning transmission electron microscope) images, HAADF-STEM (high-angle annular dark-field scanning transmission electron microscope) images, ABF-STEM (annular bright-field scanning transmission electron microscope) images, etc. X-ray diffraction (XRD), electron beam diffraction, neutron beam diffraction, etc. can also be used for the determination. In TEM images, etc., the arrangement of cations and anions can be observed as repeated bright and dark lines. When the orientation of the cubic close-packed structure in the layered rock salt type crystal and the rock salt type crystal is aligned, it can be observed that the angle between the repeated bright and dark lines between the crystals is 5 degrees or less, more preferably 2.5 degrees or less. In TEM images, etc., light elements such as oxygen and fluorine may not be clearly observed, but in such cases, the agreement of the orientation can be determined from the arrangement of metal elements.
[0043] In this specification, the theoretical capacity of a positive electrode active material refers to the amount of electricity when all of the lithium that can be inserted and removed from the positive electrode active material is removed. For example, the theoretical capacity of LiCoO2 is 274 mAh / g, the theoretical capacity of LiNiO2 is 274 mAh / g, and the theoretical capacity of LiMn2O4 is 148 mAh / g.
[0044] In this specification and the like, the depth of charge when all intercalable and deintercalable lithium is intercalated is defined as 0, and the depth of charge when all intercalable and deintercalable lithium contained in the positive electrode active material is deintercalated is defined as 1.
[0045] In this specification, charging refers to moving lithium ions from the positive electrode to the negative electrode in the battery and moving electrons from the negative electrode to the positive electrode in the external circuit. For a positive electrode active material, charging refers to removing lithium ions. A positive electrode active material with a charge depth of 0.74 to 0.9, more specifically, a charge depth of 0.8 to 0.83, is referred to as a positive electrode active material charged at a high voltage. For example, if LiCoO2 is charged at 219.2 mAh / g, it is a positive electrode active material charged at a high voltage. In addition, a positive electrode active material after constant current charging with a charge voltage of 4.525 V to 4.65 V (in the case of lithium counter electrode) in a 25°C environment and then constant voltage charging until the current value becomes 0.01 C or about 1 / 5 to 1 / 100 of the current value during constant current charging is also referred to as a positive electrode active material charged at a high voltage.
[0046] Similarly, discharging refers to moving lithium ions from the negative electrode to the positive electrode in the battery and moving electrons from the positive electrode to the negative electrode in the external circuit. For positive electrode active materials, discharging refers to inserting lithium ions. A positive electrode active material with a charge depth of 0.06 or less, or a positive electrode active material that has been discharged from a state charged at a high voltage to 90% or more of its charge capacity, is considered to be a fully discharged positive electrode active material. For example, in LiCoO2, if the charge capacity is 219.2mAh / g, it is in a state charged at a high voltage, and a positive electrode active material after discharging 197.3mAh / g or more, which is 90% of the charge capacity, from this state is considered to be a fully discharged positive electrode active material. In addition, in LiCoO2, a positive electrode active material after constant current discharge until the battery voltage becomes 3V or less (in the case of lithium counter electrode) in a 25°C environment is also considered to be a fully discharged positive electrode active material.
[0047] In this specification, a non-equilibrium phase change refers to a phenomenon that causes a non-linear change in a physical quantity. For example, a non-equilibrium phase change occurs around the peak in a dQ / dV curve obtained by differentiating capacitance (Q) with respect to voltage (V), and it is believed that the crystal structure changes significantly.
[0048] (Embodiment 1) In this embodiment, a positive electrode active material and the like according to one embodiment of the present invention will be described.
[0049] [Positive electrode active material structure] In a positive electrode material having a metal (hereinafter, element A) that acts as a carrier ion, the ions of the metal are released from the positive electrode material during charging. If a large amount of element A is released, more ions contribute to the capacity of the secondary battery, and the capacity increases. On the other hand, if a large amount of element A is released, the crystal structure of the compound in the positive electrode material is likely to collapse. The collapse of the crystal structure of the positive electrode material may lead to a decrease in the discharge capacity with charge-discharge cycles. For example, alkali metals such as lithium, sodium, and potassium, and Group 2 elements such as calcium, beryllium, and magnesium can be used as element A.
[0050] A positive electrode material according to one embodiment of the present invention contains an element (hereinafter, referred to as element X) that is easily substituted at the position of element A, and thus the collapse of the crystal structure of the compound of the positive electrode material due to the elimination of element A is suppressed. Details of element X will be described later, and elements such as magnesium, calcium, zirconium, lanthanum, and barium can be used as element X. Elements such as copper, potassium, sodium, and zinc can also be used as element X. Two or more of the above elements may be used in combination as element X.
[0051] Here, substitution at the position of a certain atom in the crystal of the positive electrode material may be expressed as being substituted at the site of the atom.
[0052] In addition, the positive electrode material of one embodiment of the present invention preferably has a metal (hereinafter, element M) whose valence changes with charging and discharging of the secondary battery. The element M is, for example, a transition metal. The positive electrode material of one embodiment of the present invention preferably has, for example, one or more of cobalt, nickel, and manganese as the element M, and particularly preferably has cobalt. In addition, the position of the element M may have an element such as aluminum that does not change its valence and can have the same valence as the element M, more specifically, for example, a typical trivalent element.
[0053] In the case where the element M contains cobalt, nickel, and manganese, for example, the number of nickel atoms is preferably greater than 0.1 times and less than 8 times the sum of the numbers of cobalt, nickel, and manganese atoms, and the number of manganese atoms is preferably greater than 0.1 times and less than 8 times the sum of the numbers of cobalt, nickel, and manganese atoms.
[0054] Alternatively, in the case where the element M contains cobalt, nickel, and manganese, for example, the number of nickel atoms is preferably greater than 0.1 times and less than 8 times the number of cobalt atoms, and the number of manganese atoms is preferably greater than 0.1 times and less than 8 times the number of cobalt atoms.
[0055] Alternatively, in the case where the element M contains cobalt, nickel, and manganese, for example, the number of nickel atoms is less than 0.25 times the sum of the numbers of cobalt, nickel, and manganese atoms, or is greater than 0.5 times and less than 0.6 times the sum of the numbers of cobalt, nickel, and manganese atoms, or is greater than 0.73 times the sum of the numbers of cobalt, nickel, and manganese atoms.
[0056] Alternatively, in the case where element M includes cobalt, nickel, and manganese, the number of nickel atoms is, for example, greater than 0.1 times and less than 0.43 times the number of cobalt atoms, or in the case where element M includes cobalt, nickel, and manganese, the number of nickel atoms is, for example, greater than 6.5 times the number of cobalt atoms.
[0057] Alternatively, in the case of having cobalt, nickel and manganese as the element M, for example, the number of manganese atoms is less than 0.25 times the number of cobalt atoms.
[0058] The positive electrode material of one embodiment of the present invention includes, for example, an oxide having an element A and an element M. The positive electrode material of one embodiment of the present invention includes, for example, an oxide having a chemical formula AM y O Z It has an oxide that can be expressed as (y>0, z>0).
[0059] More preferably, in the compound included in the positive electrode material of one embodiment of the present invention, the compound is represented by the chemical formula AM y O Z (y>0, z>0) and has a layered rock salt type crystal structure. The compound is preferably represented by the space group R-3m.
[0060] In the compound included in the positive electrode material of one embodiment of the present invention, the element X is preferably more likely to be substituted at the position of the element A than at the position of the element M.
[0061] The stability of the compound after element X is substituted at the position of element A and at the position of element M can be estimated, for example, by calculating the total energy of each system before and after substitution in a first-principles calculation and estimating the difference between them. Here, the value obtained by subtracting the energy before substitution from the energy after element X is substituted at the position of element A is defined as ΔE1. Also, the value obtained by subtracting the energy before substitution from the energy after element X is substituted at the position of element M is defined as ΔE2. If ΔE1 is smaller than ΔE2, it is suggested that element X is more easily substituted at the position of element A than at the position of element M.
[0062] It is suggested that the larger the value of ΔE1, the larger the energy required for substitution. When the energy required for substitution is large, for example, a high temperature may be required for the reaction. In the first-principles calculation exemplified in this specification, 1 eV corresponds to approximately 10,000 K. Using this value as a guideline, ΔE1 is preferably, for example, 2.5 eV or less, and more preferably 1 eV or less. Note that the above 10,000 K is a guideline value, and in cases where the crystal has defects, or where a melting point drop occurs due to the effect of halogens, etc., as described below, the energy required for the actual substitution is considered to be lower than the temperature calculated by the first-principles calculation.
[0063] When ΔE1 is a positive value, element X is AM y O Z In some cases, the compound represented by the formula: y O Z It is suggested that the compound is easily substituted by the compound represented by the formula: y O Z At least a part of the outside of the compound represented by the formula (I) may be covered with a compound having element X. This covering may suppress the decrease in capacity due to charging and discharging of the secondary battery. In addition, the element X may be, for example, AM y O Z Alternatively, in the positive electrode active material, a compound containing a large amount of element X and a compound containing a large amount of element AM yO Z In some cases, a phase separation may occur between a compound represented by the formula: and a compound in which a small amount of element X is dissolved.
[0064] When ΔE1 is a negative value, the crystal structure of the compound of the positive electrode material after substitution is stable, and the larger the absolute value, the more stable the structure is. In addition, when ΔE1 is a negative value, substitution occurs more easily than when ΔE1 is a positive value, even when the reaction is performed at a low temperature.
[0065] The ionic radius of the element X is preferably equal to or larger than the ionic radius of the element M or element A, for example.
[0066] By using the positive electrode material of one embodiment of the present invention, the capacity of a secondary battery can be increased and a decrease in the discharge capacity due to charge-discharge cycles can be suppressed.
[0067] <Cathode active material> A secondary battery has, for example, a positive electrode and a negative electrode. A material constituting the positive electrode is a positive electrode active material. The positive electrode active material is, for example, a material that undergoes a reaction that contributes to the charge / discharge capacity. Note that the positive electrode active material may contain a material that does not contribute to the charge / discharge capacity.
[0068] In this specification, etc., the positive electrode active material of one embodiment of the present invention may be expressed as a positive electrode material, a positive electrode material for a secondary battery, or the like. In this specification, etc., the positive electrode active material of one embodiment of the present invention preferably includes a compound. In this specification, etc., the positive electrode active material of one embodiment of the present invention preferably includes a composition. In this specification, etc., the positive electrode active material of one embodiment of the present invention preferably includes a composite.
[0069] The positive electrode active material of one embodiment of the present invention is, for example, an oxide having lithium and cobalt. The positive electrode active material of one embodiment of the present invention is, for example, represented by the space group R-3m. As will be described in detail below, the positive electrode active material of one embodiment of the present invention contains the element X, so that, for example, even if the charge depth becomes deep, the shift of the layer having cobalt and oxygen can be suppressed.
[0070] The positive electrode active material of one embodiment of the present invention preferably has a pseudospinel structure, which will be described later, particularly when the depth of charge is deep.
[0071] The positive electrode active material of one embodiment of the present invention preferably contains a halogen such as fluorine or chlorine in addition to the element X. When the positive electrode active material of one embodiment of the present invention contains the halogen, substitution of the element X at the position of the element A may be promoted.
[0072] <First principles calculation> An example of a method for calculating the above ΔE1 and ΔE2 using first-principles calculations will be shown below.
[0073] ΔE1 is a value obtained by subtracting the energy before the substitution from the energy after the element X is substituted at the position of the element A, and can be expressed, for example, as shown below (Equation 1).
[0074]
number
[0075] Furthermore, ΔE2 is a value obtained by subtracting the energy before substitution from the energy after the element X is substituted at the position of the element M, and can be expressed, for example, as in the following formula (2).
[0076]
number
[0077] Here, E(t_all) is the total energy of the crystal model to be calculated, E(t_X-A) is the total energy of the crystal model when one atom of element A in E(t_all) is replaced with one atom of element X, and E(t_X-M) is the total energy of the crystal model when one atom of element M in E(t_all) is replaced with one atom of element X. E(atom_A) is the energy of one atom of element A, E(atom_X) is the energy of one atom of element X, and E(atom_M) is the energy of one atom of element M.
[0078] The crystal structure is a layered rock-salt structure, the space group is R-3m, the lattice and atomic positions are optimized using first-principles calculations, and each energy is calculated.
[0079] An example of the results of a first-principles calculation is shown below.
[0080] The Vienna Ab initio simulation package (VASP) was used as the software. Generalized-Gradient-Approximation (GGA)+U was used as the functional. The U potential of each element is shown in Table 1. For elements without numerical values, calculations were performed without using the U potential. A potential generated by the PAW (Projector Augmented Wave) method was used as the pseudopotential. The cutoff energy was set to 520 eV. For the U potential, Non-Patent Documents 6 and 7 can be referred to.
[0081] In this specification, the energy obtained in this manner is called stabilization energy.
[0082] Compound AM y O ZIn the above formula, A is lithium, M is cobalt, nickel and manganese, and y=1 and z=2. The number of atoms used in the calculations was 27 atoms of element A, 27 atoms of element M and 54 atoms of oxygen in the crystal structure before the substitution of element X. First-principles calculations were performed for a total of nine compounds with the ratios of nickel, cobalt and manganese in element M shown in Table 2. Condition 1 in Table 2 is LiCoO2 and condition 8 is LiNiO2.
[0083] [Table 1]
[0084] [Table 2]
[0085] Among ΔE1 and ΔE2 obtained by first-principles calculation, the results of condition 1, condition 3, condition 7, and condition 8 are shown in Fig. 28 to Fig. 34. The horizontal axis of each figure is the condition number, and the vertical axis is the energy. Fig. 28A shows the results for aluminum, Fig. 28B shows the results for barium, Fig. 28C shows the results for potassium, Fig. 29A shows the results for lanthanum, Fig. 29B shows the results for magnesium, Fig. 29C shows the results for calcium, Fig. 30A shows the results for copper, Fig. 30B shows the results for iron, Fig. 30C shows the results for gallium, Fig. 31A shows the results for germanium, Fig. 31B shows the results for molybdenum, Fig. 31C shows the results for sodium, Fig. 32A shows the results for phosphorus, Fig. 32B shows the results for sulfur, Fig. 32C shows the results for silicon, Fig. 33A shows the results for tantalum, Fig. 33B shows the results for titanium, Fig. 33C shows the results for vanadium, Fig. 34A shows the results for zinc, and Fig. 34B shows the results for zirconium. Regarding ΔE2, the energy corresponding to the substitution at the cobalt position is expressed as ΔE2c, the value corresponding to the nickel position as ΔE2n, and the value corresponding to the manganese position as ΔE2m.
[0086] Table 3 shows elements X for which ΔE1 was lower than ΔE2 under each of the conditions shown in Table 2.
[0087] [Table 3]
[0088] Among the elements X shown in Table 3, elements X having an absolute value of ΔE1 of 2.5 eV or less are shown in Table 4, and elements X having an absolute value of ΔE1 of 1 eV or less are shown in Table 5. Among the elements X shown in Table 3, elements X having a positive value of ΔE1 are shown in Table 6.
[0089] [Table 4]
[0090] [Table 5]
[0091] [Table 6]
[0092] For example, AM having element X shown in Tables 4 to 6 y O Z When (y>0, z>0), the compound has a layered rock-salt crystal structure, and is represented by the space group R-3m, the shift of the layer having the element M in the charged state may be suppressed, which is preferable.
[0093] As a specific example, the displacement of the CoO2 layer will be described in detail below for the case where y=1, z=2, the element M is cobalt, and the element X is magnesium.
[0094] <An example of positive electrode active material> Fig. 1 shows, as an example of a positive electrode active material according to one embodiment of the present invention, a positive electrode active material 100 having lithium as element A, magnesium as element X, and cobalt as element M. Fig. 2 also shows LiCoO2 as a representative example of a positive electrode active material not having element X.
[0095] In the following, an example in which the element M is cobalt is shown, but nickel may be contained in addition to cobalt. In this case, the ratio Ni / (Co+Ni) of the number of nickel atoms (Ni) to the sum of the numbers of cobalt and nickel atoms (Co+Ni) is preferably less than 0.1, and more preferably 0.075 or less.
[0096] If the battery is charged at a high voltage for a long period of time, the transition metal may leach out of the positive electrode active material into the electrolyte, causing the crystal structure to collapse. However, by containing nickel in the above ratio, it may be possible to suppress the leaching of the transition metal from the positive electrode active material 100.
[0097] The addition of nickel reduces the charge / discharge voltage, so that for the same capacity, the voltage can be lowered to charge / discharge, which may result in suppression of the elution of transition metals and the decomposition of the electrolyte. Here, the charge / discharge voltage refers to the voltage in the range from zero charge depth to a specified charge depth.
[0098] The crystal structure of lithium cobalt oxide LiCoO2, one of the conventional positive electrode active materials, changes depending on the charge depth, as described in Non-Patent Documents 1 and 2. A typical crystal structure of lithium cobalt oxide is shown in FIG.
[0099] As shown in Figure 2, lithium cobalt oxide at a charge depth of 0 (discharged state) has a region with a crystal structure of space group R-3m, and there are three CoO2 layers in the unit cell. Therefore, this crystal structure is sometimes called an O3 type crystal structure. Note that a CoO2 layer is an octahedral structure in which cobalt is coordinated with six oxygen atoms, and the octahedral structure is continuous on a plane with edge sharing.
[0100] Lithium cobalt oxide at a charge depth of 1 has a crystal structure of the space group P-3m1, with one CoO2 layer in the unit cell. Therefore, this crystal structure is sometimes called the O1 type crystal structure.
[0101] Lithium cobalt oxide at a charge depth of about 0.88 has a crystal structure of space group R-3m. This structure can be said to be a structure in which a CoO2 structure such as P-3m1(O1) and a LiCoO2 structure such as R-3m(O3) are alternately stacked. Therefore, this crystal structure is sometimes called an H1-3 type crystal structure. In reality, the number of cobalt atoms per unit cell in the H1-3 type crystal structure is twice that of other structures. However, in Figure 2 and other parts of this specification, the c-axis of the H1-3 type crystal structure is shown as half the unit cell in order to make it easier to compare with other structures.
[0102] When lithium cobalt oxide is repeatedly charged and discharged at a high voltage to a charge depth of about 0.88 or more, its crystal structure repeatedly changes (i.e., undergoes a non-equilibrium phase change) between the H1-3 crystal structure and the R-3m(O3) structure in the discharged state.
[0103] However, these two crystal structures have a large deviation in the CoO2 layer. As shown by the dotted line and arrow in Figure 2, in the H1-3 type crystal structure, the CoO2 layer is significantly deviated from R-3m(O3). Such a dynamic structural change can have a negative effect on the stability of the crystal structure.
[0104] The difference in volume is also large: when compared per the same number of cobalt atoms, the difference in volume between the H1-3 crystal structure and the O3 crystal structure in the discharged state is more than 3.5%.
[0105] In addition, the H1-3 crystal structure, which has continuous CoO2 layers such as P-3m1(O1), is likely to be unstable.
[0106] As a result, the crystal structure of lithium cobalt oxide breaks down when it is repeatedly charged and discharged at high voltages. This break in the crystal structure causes a deterioration in cycle characteristics. This is thought to be because the break in the crystal structure reduces the number of sites where lithium can exist stably and makes it difficult to insert and remove lithium.
[0107] In contrast, in the positive electrode active material 100 of one embodiment of the present invention, the change in crystal structure and the difference in volume per the same number of transition metal atoms between a fully discharged state and a high-voltage charged state are small.
[0108] The crystal structure of the positive electrode active material 100 before and after charging and discharging is shown in FIG. 1. The positive electrode active material 100 is a composite oxide containing lithium, cobalt, and oxygen. In addition to the above, it preferably contains magnesium. It also preferably contains a halogen such as fluorine or chlorine.
[0109] The crystal structure at a charge depth of 0 (discharged state) in FIG. 1 is the same as that in FIG. 2, R-3m(O3). On the other hand, the positive electrode active material 100 according to one embodiment of the present invention has a crystal structure different from that in FIG. 2 when fully charged to a charge depth of about 0.88. In FIG. 1, lithium is omitted in order to explain the symmetry of the cobalt atoms and the symmetry of the oxygen atoms, but in reality, about 12 atomic % of lithium is present relative to cobalt between the CoO2 layers. In addition, it is preferable that magnesium is present dilutely between the CoO2 layers, that is, at the lithium sites. In addition, it is preferable that halogen such as fluorine is present randomly and dilutely at the oxygen sites.
[0110] Magnesium, which is randomly and dilutely present between the CoO2 layers, i.e., at the lithium sites, has the effect of suppressing the displacement of the CoO2 layers. Therefore, in the positive electrode active material 100, the change in the crystal structure when a large amount of lithium is released by charging at a high voltage is suppressed more than in conventional LiCoO2. For example, as shown by the dotted line in Figure 1, there is almost no displacement of the CoO2 layers in these crystal structures.
[0111] In the positive electrode active material 100, the difference in volume per unit cell between the O3 crystal structure at a charge depth of 0 and the pseudo-spinel crystal structure at a charge depth of 0.88 is 2.5% or less, more specifically 2.2% or less.
[0112] Therefore, the crystal structure is not easily destroyed even when repeatedly charged and discharged at high voltage.
[0113] Magnesium, which is present randomly and dilutely between the CoO2 layers, i.e., at the lithium sites, has the effect of suppressing the displacement of the CoO2 layers. Therefore, it is preferable that magnesium is distributed throughout the particles of the positive electrode active material 100. In order to distribute magnesium throughout the particles, it is preferable to perform a heat treatment in the manufacturing process of the positive electrode active material 100.
[0114] However, if the heat treatment temperature is too high, cation mixing occurs, increasing the possibility that magnesium will enter the cobalt site. If magnesium is present at the cobalt site, it will no longer be effective in maintaining the R-3m structure. Furthermore, if the heat treatment temperature is too high, there are concerns that it may have adverse effects such as reducing cobalt to a divalent state and evaporating lithium.
[0115] Therefore, it is preferable to add a halogen compound such as a fluorine compound to the lithium cobalt oxide before the heat treatment for distributing magnesium throughout the particles. The addition of the halogen compound lowers the melting point of the lithium cobalt oxide. Lowering the melting point makes it easier to distribute magnesium throughout the particles at a temperature where cation mixing is unlikely to occur. Furthermore, the presence of a fluorine compound is expected to improve corrosion resistance against hydrofluoric acid produced by decomposition of the electrolyte.
[0116] As described above, when the positive electrode active material of one embodiment of the present invention contains the element X, displacement of the layer containing the element M in a charged state is suppressed.
[0117] <Element X> The element X in the particles of the positive electrode active material will be described below.
[0118] ≪Surface layer≫ The positive electrode active material 100 has particles. The particles of the positive electrode active material have, for example, a region having a crystalline structure. The region having a crystalline structure is preferably a material that functions as a positive electrode in a secondary battery.
[0119] The crystal structure is, for example, a rock salt layered structure. The crystal structure can be represented by, for example, the space group R-3m.
[0120] It is preferable that the element X is distributed throughout the particles of the positive electrode active material 100, but in addition to this, it is more preferable that the concentration of element X in the particle surface layer is higher than the average of the entire particle. In other words, it is more preferable that the concentration of element X in the particle surface layer measured by XPS or the like is higher than the average concentration of element X in the entire particle measured by ICP-MS or the like. The particle surface is, so to speak, all crystal defects, and since element A, which becomes a carrier ion, is removed from the surface during charging, it is a part where the concentration of element A is likely to be lower than that of the inside. Therefore, it is a part that is likely to become unstable and the crystal structure is likely to collapse. If the concentration of element X in the surface layer is high, the change in the crystal structure can be more effectively suppressed. In addition, if the concentration of element X in the surface layer is high, it can be expected that the corrosion resistance to hydrofluoric acid generated by decomposition of the electrolyte is improved.
[0121] It is also preferable that the concentration of halogens such as fluorine is higher in the surface layer of the positive electrode active material 100 than the average of the entire particle. The presence of halogens in the surface layer, which is the region in contact with the electrolyte, can effectively improve corrosion resistance to hydrofluoric acid.
[0122] In this way, the surface layer of the positive electrode active material 100 preferably has a composition different from that of the inside, with a higher concentration of element X and fluorine than the inside. In addition, the composition preferably has a stable crystal structure at room temperature. Therefore, the surface layer may have a crystal structure different from that of the inside. For example, at least a part of the surface layer of the positive electrode active material 100 may have a rock salt crystal structure. In addition, when the surface layer and the inside have different crystal structures, it is preferable that the crystal orientations of the surface layer and the inside are roughly the same.
[0123] However, if the surface layer portion is composed only of a compound having element X, or only of a structure in which a compound having element X and a compound having element M are solid-dissolved, for example, only of a structure in which MgO and CoO(II) are solid-dissolved, it becomes difficult to insert and remove element A. Therefore, the surface layer portion must contain at least element M, and in a discharged state, must also contain element A, and must have a path for insertion and removal of element A. In addition, it is preferable that the concentration of element M is higher than that of element X.
[0124] ≪Grain boundary≫ The element X or halogen contained in the positive electrode active material 100 may be present randomly and dilutely inside, but more preferably, a portion of it is segregated at the grain boundaries.
[0125] In other words, the concentration of element X at and near the grain boundaries of the positive electrode active material 100 is preferably higher than that in other internal regions. Also, the halogen concentration at and near the grain boundaries is preferably higher than that in other internal regions.
[0126] Like the particle surface, the grain boundary is also a planar defect. Therefore, it is easily unstable and the crystal structure is easily changed. Therefore, if the concentration of element X at and near the grain boundary is high, the change in the crystal structure can be more effectively suppressed.
[0127] Furthermore, when the concentrations of element X and halogen are high at and near the grain boundaries, even if cracks occur along the grain boundaries of the particles of the positive electrode active material 100, the concentrations of element X and halogen become high near the surface caused by the cracks. Therefore, the corrosion resistance to hydrofluoric acid can be improved even in the positive electrode active material after cracks occur.
[0128] In this specification and the like, the vicinity of a crystal grain boundary refers to a region within about 10 nm from the grain boundary.
[0129] ≪Particle size≫ If the particle size of the positive electrode active material 100 is too large, there are problems such as the element A being difficult to diffuse, and the surface of the active material layer being too rough when applied to a current collector. On the other hand, if the particle size is too small, there are problems such as the active material layer being difficult to support when applied to a current collector, and excessive reaction with the electrolyte. Therefore, D50 is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 40 μm or less, and even more preferably 5 μm or more and 30 μm or less.
[0130] ≪Charging method≫ High-voltage charging for determining whether a certain composite oxide is the positive electrode active material 100 of one embodiment of the present invention can be performed, for example, by preparing a coin cell (CR2032 type, diameter 20 mm, height 3.2 mm) with a lithium counter electrode and charging it.
[0131] More specifically, for the positive electrode, a slurry in which a positive electrode active material, a conductive additive, and a binder are mixed is applied to a positive electrode current collector made of aluminum foil and used.
[0132] When lithium is used as element A, lithium metal can be used for the counter electrode. When a material other than lithium metal is used for the counter electrode, the potential of the secondary battery is different from the potential of the positive electrode. Unless otherwise specified, the voltage and potential in this specification are the potential of the positive electrode.
[0133] The electrolyte used in the electrolytic solution is 1 mol / L lithium hexafluorophosphate (LiPF6), and the electrolytic solution can be a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) at a volume ratio of EC:DEC = 3:7, with 2 wt% vinylene carbonate (VC).
[0134] The separator can be made of polypropylene having a thickness of 25 μm.
[0135] The positive electrode can and the negative electrode can may be made of stainless steel (SUS).
[0136] The coin cell prepared under the above conditions is charged at a constant current of 4.6 V and 0.5 C, and then charged at a constant voltage until the current value reaches 0.01 C. Here, 1 C is 137 mA / g. The temperature is 25°C. After charging in this manner, the coin cell is disassembled in a glove box in an argon atmosphere and the positive electrode is taken out to obtain a positive electrode active material charged at a high voltage. When various analyses are performed after this, it is preferable to seal the cell in an argon atmosphere to suppress reactions with external components. For example, XRD can be performed by sealing the cell in an airtight container in an argon atmosphere.
[0137] <XPS> X-ray photoelectron spectroscopy (XPS) can analyze the area from the surface to a depth of about 2 to 8 nm (usually about 5 nm), so it can quantitatively analyze the concentration of each element in about half of the surface layer. In addition, narrow scan analysis can analyze the bonding state of elements. The quantitative accuracy of XPS is often about ±1 atomic %, and the lower detection limit is about 1 atomic %, depending on the element.
[0138] When the positive electrode active material 100 is subjected to XPS analysis, the relative value of the concentration of element X is preferably 0.4 to 1.5, and more preferably 0.45 to less than 1.00, when the concentration of element M is set to 1. The relative value of the concentration of halogen such as fluorine is preferably 0.05 to 1.5, and more preferably 0.3 to 1.00.
[0139] In addition, when the positive electrode active material 100 is analyzed by XPS, the peak showing the bond energy between fluorine and other elements is preferably 682 eV or more and less than 685 eV, more preferably about 684.3 eV. This is a value different from both the bond energy of lithium fluoride, 685 eV, and the bond energy of magnesium fluoride, 686 eV. In other words, when the positive electrode active material 100 has fluorine, it is preferable that the bond is other than that of lithium fluoride and magnesium fluoride.
[0140] Furthermore, when the element X is magnesium, when the positive electrode active material 100 is subjected to XPS analysis, the peak showing the bond energy between magnesium and other elements is preferably 1302 eV or more and less than 1304 eV, more preferably about 1303 eV. This is a value different from the bond energy of magnesium fluoride, 1305 eV, and is a value close to the bond energy of magnesium oxide. In other words, when the positive electrode active material 100 contains magnesium, it is preferable that the bond is other than that of magnesium fluoride.
[0141] <EDX> In EDX measurements, the measurement performed while scanning an area and evaluating the area in two dimensions is sometimes called EDX area analysis. In addition, the extraction of data from a linear area from EDX area analysis and the evaluation of the distribution of atomic concentrations within the positive electrode active material particle is sometimes called line analysis.
[0142] EDX surface analysis (e.g., element mapping) can quantitatively analyze the concentration of element X and the concentration of fluorine in the interior, the surface layer, and near the grain boundaries. In addition, EDX line analysis can analyze the peaks of the concentration of element X and the concentration of fluorine.
[0143] When EDX line analysis is performed on the positive electrode active material 100, the peak of the concentration of element X in the surface layer portion is preferably present at a depth of up to 3 nm from the surface toward the center of the positive electrode active material 100, more preferably at a depth of up to 1 nm, and even more preferably at a depth of up to 0.5 nm.
[0144] Furthermore, the distribution of fluorine in the positive electrode active material 100 preferably overlaps with the distribution of element X. Therefore, when EDX line analysis is performed, the peak of the fluorine concentration in the surface layer portion preferably exists within a depth of 3 nm from the surface of the positive electrode active material 100 toward the center, more preferably exists within a depth of 1 nm, and further preferably exists within a depth of 0.5 nm.
[0145] When the positive electrode active material 100 is subjected to a line analysis or an area analysis, the ratio of the number of atoms of element X to cobalt in the vicinity of the grain boundary (X / Co) is preferably 0.020 or more and 0.50 or less, more preferably 0.025 or more and 0.30 or less, and even more preferably 0.030 or more and 0.20 or less.
[0146] ≪dQ / dVvsV curve≫ Furthermore, when the positive electrode active material of one embodiment of the present invention is charged at a high voltage and then discharged at a low rate of, for example, 0.2 C or less, a characteristic voltage change may appear near the end of discharge. This change can be clearly confirmed by the presence of at least one peak in the range of 3.5 V to 3.9 V in the dQ / dV vs. V curve obtained from the discharge curve.
[0147] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0148] (Embodiment 2) In this embodiment, an example of a crystal structure of a positive electrode active material of one embodiment of the present invention will be described.
[0149] The positive electrode active material shown in the first embodiment may have the pseudo-spinel structure shown below. The following describes the pseudo-spinel structure, AM having an element X shown in Tables 4 to 6, etc. y O Z An example will be described in which (y>0, z>0), y=1, z=2, the element M is cobalt, and the element X is magnesium.
[0150] <Pseudospinel> The crystal structure at a charge depth of 0 (discharged state) in FIG. 1 is the same as that in FIG. 2, R-3m (O3). On the other hand, the positive electrode active material 100 according to one embodiment of the present invention has a crystal structure different from that in FIG. 2 when the charge depth is about 0.88, which is a sufficient charge. This crystal structure of space group R-3m is referred to as a pseudo-spinel crystal structure in this specification. In the drawing of the pseudo-spinel crystal structure shown in FIG. 1, lithium is omitted in order to explain the symmetry of the cobalt atom and the symmetry of the oxygen atom, but in reality, about 12 atomic % of lithium is present between the CoO2 layers with respect to cobalt. In both the O3 crystal structure and the pseudo-spinel crystal structure, magnesium is preferably present dilutely between the CoO2 layers, that is, at the lithium site. In addition, it is preferable that halogen such as fluorine is present randomly and dilutely at the oxygen site.
[0151] In the positive electrode active material 100, when a large amount of lithium is released during charging at a high voltage, the change in the crystal structure is suppressed more than in conventional LiCoO2. For example, as shown by the dotted line in Figure 1, there is almost no displacement of the CoO2 layers in these crystal structures.
[0152] In the positive electrode active material 100, the difference in volume per unit cell between the O3 crystal structure at a charge depth of 0 and the pseudo-spinel crystal structure at a charge depth of 0.88 is 2.5% or less, more specifically 2.2% or less.
[0153] Therefore, the crystal structure is not easily destroyed even when repeatedly charged and discharged at high voltage.
[0154] In addition, the pseudospinel crystal structure can be expressed by the coordinates of cobalt and oxygen in the unit cell being Co(0,0,0.5), O(0,0,x), with 0.20≦x≦0.25.
[0155] <XRD> Figure 3 shows ideal powder XRD patterns calculated from the pseudo-spinel crystal structure and H1-3 crystal structure models using CuKα1 radiation. For comparison, ideal XRD patterns calculated from the crystal structures of LiCoO2(O3) at charge depth 0 and CoO2(O1) at charge depth 1 are also shown. The patterns of LiCoO2(O3) and CoO2(O1) were created using Reflex Powder Diffraction, one of the modules of Materials Studio (BIOVIA), from crystal structure information obtained from ICSD (Inorganic Crystal Structure Database) (see Non-Patent Document 5). The 2θ range was 15° to 75°, Step size = 0.01, and wavelength λ1 = 1.540562 × 10 -10 m and λ2 were not set, and Monochromator was set to single. The pattern of the H1-3 type crystal structure was similarly created from the crystal structure information described in Non-Patent Document 3. The pseudospinel pattern was created by estimating the crystal structure from the XRD pattern of the positive electrode active material of one embodiment of the present invention, fitting it using TOPAS ver.3 (crystal structure analysis software manufactured by Bruker), and creating an XRD pattern in the same manner as the others.
[0156] As shown in FIG. 3, in the pseudo-spinel crystal structure, diffraction peaks appear at 2θ=19.30±0.20° (19.10° to 19.50°) and 2θ=45.55±0.10° (45.45° to 45.65°). More specifically, sharp diffraction peaks appear at 2θ=19.30±0.10° (19.20° to 19.40°) and 2θ=45.55±0.05° (45.50° to 45.60°). However, in the H1-3 crystal structure and CoO2(P-3m1, O1), no peaks appear at these positions. Therefore, it can be said that the appearance of peaks at 2θ=19.30±0.20° and 2θ=45.55±0.10° in a state charged at a high voltage is a characteristic of the positive electrode active material 100 of one embodiment of the present invention.
[0157] This can also be said to be because the positions at which the XRD diffraction peaks appear are close between the crystal structure at a charge depth of 0 and the crystal structure when charged at a high voltage. More specifically, the difference in the positions at which the peaks appear for two or more, more preferably three or more, of the main diffraction peaks of both structures is 2θ=0.7 or less, more preferably 2θ=0.5 or less.
[0158] Note that the positive electrode active material 100 of one embodiment of the present invention has a pseudo-spinel crystal structure when charged at a high voltage, but not all of the particles may have a pseudo-spinel crystal structure. Other crystal structures may be included, or a part may be amorphous. However, when Rietveld analysis is performed on the XRD pattern, the pseudo-spinel crystal structure is preferably 50 wt% or more, more preferably 60 wt% or more, and even more preferably 66 wt% or more. When the pseudo-spinel crystal structure is 50 wt% or more, more preferably 60 wt% or more, and even more preferably 66 wt% or more, the positive electrode active material can have sufficiently excellent cycle characteristics.
[0159] Furthermore, even after 100 or more charge / discharge cycles from the start of measurement, when Rietveld analysis is performed, the pseudo-spinel crystal structure preferably accounts for 35 wt% or more, more preferably 40 wt% or more, and even more preferably 43 wt% or more.
[0160] In addition, the crystallite size of the pseudo-spinel structure of the positive electrode active material particles only decreases to about 1 / 10 of that of LiCoO2(O3) in the discharged state. Therefore, even under the same XRD measurement conditions as the positive electrode before charging and discharging, a clear pseudo-spinel crystal structure peak can be confirmed after high-voltage charging. On the other hand, in the case of simple LiCoO2, even if some of the structure resembles a pseudo-spinel crystal structure, the crystallite size becomes smaller and the peak becomes broad and small. The crystallite size can be calculated from the half-width of the XRD peak.
[0161] In addition, it is preferable that the c-axis lattice constant is small in the layered rock-salt crystal structure of the particles of the positive electrode active material in the discharged state, which can be estimated from the XRD pattern. The c-axis lattice constant becomes large when a foreign element is substituted at the lithium site, or when cobalt enters the oxygen tetracoordination site (A site). Therefore, it is believed that a composite oxide with a layered rock-salt crystal structure with few foreign element substitutions and spinel-type crystal structure Co3O4, that is, with few defects, can be first produced, and then a magnesium source and a fluorine source are mixed to insert magnesium into the lithium site, thereby producing a positive electrode active material with good cycle characteristics.
[0162] The c-axis lattice constant of the crystal structure of the positive electrode active material in the discharged state is 14.060 × 10 -10 m or less is preferable, and 14.055×10 -10 m or less is preferable, and 14.051×10 -10 m or less. The lattice constant of the c-axis after annealing is 14.060×10 -10 m or less is preferable.
[0163] In order to keep the c-axis lattice constant in the above range, it is preferable to have a small amount of impurities, and in particular, it is preferable to add transition metals other than cobalt, manganese, and nickel in small amounts, specifically, it is preferable to have an amount of 3000 ppm wt or less, and more preferably 1500 ppm wt or less. Also, it is preferable to have a small amount of cation mixing between lithium and cobalt, manganese, or nickel.
[0164] The characteristics revealed from the XRD pattern are characteristics of the internal structure of the positive electrode active material. In a positive electrode active material having an average particle size (D50) of about 1 μm to 100 μm, the volume of the surface layer is very small compared to the inside, so even if the surface layer of the positive electrode active material 100 has a crystal structure different from that of the inside, it is highly likely that it will not appear in the XRD pattern.
[0165] <ESR> Here, with reference to Figures 4 and 5, we will explain how to determine the difference between a pseudo-spinel crystal structure and other crystal structures using ESR. In a pseudo-spinel crystal structure, as shown in Figures 1 and 4A, cobalt exists in a site with 6 oxygen coordination. As shown in Figure 4B, in cobalt with 6 oxygen coordination, the 3d orbital is e g Orbit and t 2g The orbit is split into two, and the orbit that avoids the direction where oxygen exists is t 2g The orbital energy is low. Some of the cobalt present in the oxygen 6-coordinated sites is t 2g Diamagnetic Co with all orbitals filled 3+ However, the other part of the cobalt present in the oxygen 6-coordinated site is paramagnetic Co 2+ Or Co 4+ The paramagnetic cobalt may be Co 2+ and Co 4+ In either case, there is one unpaired electron, so ESR cannot distinguish between them, but either valence can be used depending on the valence of the surrounding elements.
[0166] On the other hand, it has been said that some conventional positive electrode active materials may have a spinel-type crystal structure that does not contain lithium in the surface layer when charged. In this case, the material has the spinel-type crystal structure Co3O4 shown in Figure 5A.
[0167] When spinel is described by the general formula A[B2]O4, element A is 4-coordinated with oxygen, and element B is 6-coordinated with oxygen. Therefore, in this specification, the site with 4-coordinated oxygen is sometimes called the A site, and the site with 6-coordinated oxygen is sometimes called the B site.
[0168] In the spinel-type crystal structure Co3O4, cobalt is present not only in the B site with 6 oxygen coordination but also in the A site with 4 oxygen coordination. As shown in Figure 5B, in the cobalt with 4 oxygen coordination, the split e g Orbit and t 2g Of the orbitals, e g The orbital energy is low. Therefore, the Co 2+ , Co 3+ and Co 4+All of these have unpaired electrons and are paramagnetic. Therefore, if a particle containing a sufficient amount of spinel-type Co3O4 is analyzed by ESR or other methods, it is possible to find Co with four oxygen coordinations. 2+ , Co 3+ Or Co 4+ A peak due to paramagnetic cobalt should be detected.
[0169] However, in the positive electrode active material 100 of one embodiment of the present invention, the peaks derived from paramagnetic cobalt with 4-coordinated oxygen are so small that they cannot be confirmed. Therefore, unlike positive spinel, the pseudo spinel referred to in this specification does not contain an amount of cobalt with 4-coordinated oxygen that can be detected by ESR. Therefore, compared with the conventional example, the positive electrode active material of one embodiment of the present invention may have a small peak derived from spinel-type Co3O4 that can be detected by ESR or the like, or may be so small that it cannot be confirmed. Since spinel-type Co3O4 does not contribute to the charge / discharge reaction, the less spinel-type Co3O4, the better. In this way, it can be determined from the ESR analysis that the positive electrode active material 100 is different from the conventional example.
[0170] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0171] (Embodiment 3) In this embodiment, an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described.
[0172] [Method of producing positive electrode active material] First, an example of a method for manufacturing a positive electrode active material 100 according to one embodiment of the present invention will be described with reference to FIG.
[0173] <Step S11> 6, first, a halogen source such as a fluorine source or a chlorine source and a source of element X are prepared as materials for the first mixture. It is also preferable to prepare a source of element A.
[0174] If the subsequent mixing and grinding steps are carried out in a wet manner, a solvent is prepared. Examples of the solvent that can be used include ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, and N-methyl-2-pyrrolidone (NMP). It is more preferable to use an aprotic solvent that does not react easily with lithium.
[0175] <Step S12> Next, as shown in step S12, the materials of the first mixture are mixed and pulverized. Mixing can be performed in a dry or wet manner, but the wet method is preferred because it allows for finer pulverization. For example, a ball mill, a bead mill, etc. can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media. It is preferable to thoroughly perform this mixing and pulverization process to finely pulverize the first mixture.
[0176] <Step S13, Step S14> The mixed and pulverized materials are collected (step S13), and a first mixture is obtained (step S14).
[0177] The first mixture preferably has an average particle size (D50: also called the median size) of 600 nm to 20 μm, more preferably 1 μm to 10 μm. If the first mixture is finely pulverized in this way, when it is mixed with a compound having element A and element M in a later process, the first mixture can be easily attached uniformly to the surface of the compound particles. If the first mixture is attached uniformly to the surface of the compound particles, it is preferable because it is easy to distribute the halogen and element X thoroughly to the surface layer of the compound particles after heating.
[0178] <Step S21> Next, as shown in step S21 of FIG. 6, as materials for a compound having the element A and the element M, a source of the element A and a source of the element M are prepared.
[0179] As the source of element M, an oxide, hydroxide, or the like of element M can be used.
[0180] <Step S22> Next, the element A source and the element M source are mixed (step S22). Mixing can be performed in a dry or wet manner. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media.
[0181] <Step S23> Next, the mixed material is heated. This step is sometimes called firing or first heating to distinguish it from the subsequent heating step. Heating is preferably performed at 800°C or higher and lower than 1100°C, more preferably at 900°C or higher and 1000°C or lower, and even more preferably at about 950°C. If the temperature is too low, the decomposition and melting of the starting materials may be insufficient. On the other hand, if the temperature is too high, defects may occur due to excessive reduction of element M, for example, a transition metal, or evaporation of element A.
[0182] The heating time is preferably 2 hours or more and 20 hours or less. The firing is preferably carried out in an atmosphere with little water such as dry air (for example, a dew point of -50°C or less, more preferably -100°C or less). For example, it is preferable to heat at 1000°C for 10 hours, with a temperature increase of 200°C / h and a flow rate of the dry atmosphere of 10 L / min. The heated material can then be cooled to room temperature. For example, it is preferable to set the temperature drop time from a specified temperature to room temperature to 10 hours or more and 50 hours or less.
[0183] However, cooling to room temperature in step S23 is not essential, and cooling may be performed to a temperature higher than room temperature if there is no problem in performing the subsequent steps S24, S25, and S31 to S34.
[0184] <Step S24, Step S25> The calcined material is collected (step S24) to obtain a compound having element A and element M (step S25).y O Z We obtain an oxide represented by (y>0, z>0).
[0185] Alternatively, in step S25, a compound having element A and element M that has been synthesized in advance may be used. In this case, steps S21 to S24 may be omitted.
[0186] <Step S31> Next, the first mixture is mixed with a compound having element A and element M (step S31). The number of atoms TM of element M in the compound having element A and element M and the number of atoms X of element X in the first mixture Mix1 are calculated by Mix1 The ratio of the number of atoms is, for example, TM:X Mix1 = 1:y (0.0005≦y≦0.03), and TM:X Mix1 = 1:y (0.001 ≦ y ≦ 0.01), and TM:X Mix1 =1:0.005.
[0187] <Step S32, Step S33> The mixed materials are collected (step S32) to obtain a second mixture (step S33).
[0188] <Step S34> The second mixture is then heated. This step is sometimes called annealing or second heating to distinguish it from the previous heating step.
[0189] When the second mixture is annealed, it is believed that the material with a low melting point in the first mixture (e.g., the compound used as the halogen source) melts first and distributes in the surface layer of the composite compound particles. It is then assumed that the presence of this molten material lowers the melting points of the other materials, causing them to melt.
[0190] It is believed that the elements contained in the first mixture distributed in the surface layer portion are dissolved in the compound containing lithium, element A and element X to form a solid solution.
[0191] The diffusion of the elements contained in this first mixture is faster in the surface layer and in the vicinity of the grain boundaries than in the interior of the compound particles containing element A and element X. Therefore, the element X and the halogen are present in higher concentrations in the surface layer and in the vicinity of the grain boundaries than in the interior.
[0192] <Step S35> The annealed material described above is recovered to obtain the positive electrode active material 100 according to one embodiment of the present invention.
[0193] The positive electrode active material 100 produced in the above steps may be further coated with another material, and may be further heated.
[0194] For example, the positive electrode active material 100 and a compound having phosphoric acid can be mixed. In addition, the mixture can be heated after mixing. By mixing the compound having phosphoric acid, the positive electrode active material 100 can be obtained in which the elution of transition metals such as cobalt is suppressed even when the charged state at a high voltage is maintained for a long period of time. In addition, by heating the mixture, the phosphoric acid can be coated more uniformly.
[0195] Examples of compounds having phosphoric acid include lithium phosphate and ammonium dihydrogen phosphate. The mixing can be performed by a solid phase method. The heating can be performed at 800° C. or higher for 2 hours.
[0196] [Specific example of a method for producing a positive electrode active material] A specific example of the preparation method is described below. Magnesium is used as the element X, lithium is used as the element A, and a transition metal is used as the element M.
[0197] <Step S11> In step S11, a fluorine source, a lithium source, and a magnesium source are prepared.
[0198] As the fluorine source, for example, lithium fluoride, magnesium fluoride, etc. can be used. Among them, lithium fluoride is preferable because it has a relatively low melting point of 848°C and is easily melted in the annealing step described later. As the chlorine source, for example, lithium chloride, magnesium chloride, etc. can be used. As the magnesium source, for example, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, etc. can be used. As the lithium source, for example, lithium fluoride, lithium carbonate can be used. That is, lithium fluoride can be used as both a lithium source and a fluorine source. Moreover, magnesium fluoride can be used as both a fluorine source and a magnesium source.
[0199] In this embodiment, lithium fluoride LiF is prepared as the fluorine source and lithium source, and magnesium fluoride MgF2 is prepared as the fluorine source and magnesium source. When lithium fluoride LiF and magnesium fluoride MgF2 are mixed at a molar ratio of about LiF:MgF2=65:35, the effect of lowering the melting point is maximized (Non-Patent Document 4). On the other hand, if the amount of lithium fluoride increases, there is a concern that the lithium becomes excessive and the cycle characteristics deteriorate. Therefore, the molar ratio of lithium fluoride LiF and magnesium fluoride MgF2 is preferably LiF:MgF2=x:1 (0≦x≦1.9), more preferably LiF:MgF2=x:1 (0.1≦x≦0.5), and even more preferably LiF:MgF2=x:1 (near x=0.33). In this specification, etc., "near" refers to a value that is greater than 0.9 times and less than 1.1 times the value.
[0200] <Step S12> Next, in step S12, the materials of the first mixture are mixed and pulverized.
[0201] <Step S13, Step S14> The mixed and pulverized materials are collected (step S13), and a first mixture is obtained (step S14).
[0202] The first mixture preferably has an average particle diameter (D50: also called median diameter) of 600 nm to 20 μm, more preferably 1 μm to 10 μm. If the first mixture is finely pulverized in this way, when it is mixed with a composite oxide having lithium, transition metal, and oxygen in a later process, the first mixture can be easily attached uniformly to the surface of the composite oxide particles. If the first mixture is attached uniformly to the surface of the composite oxide particles, it is preferable because it is easy to distribute halogen and magnesium thoroughly in the surface layer of the composite oxide particles after heating. If there is a region in the surface layer that does not contain halogen and magnesium, it may be difficult to form a pseudo-spinel crystal structure described later in the charged state.
[0203] <Step S21> Next, in step S21, a lithium source and a transition metal source are prepared as materials for a composite oxide containing lithium, a transition metal, and oxygen.
[0204] As the lithium source, for example, lithium carbonate, lithium fluoride, etc. can be used.
[0205] As the transition metal, at least one of cobalt, manganese, and nickel can be used. Since it is preferable that the composite oxide containing lithium, a transition metal, and oxygen has a layered rock-salt type crystal structure, it is preferable that the mixture ratio of cobalt, manganese, and nickel is such that the layered rock-salt type crystal structure can be obtained. Furthermore, aluminum may be added to these transition metals within a range that allows the layered rock-salt type crystal structure to be obtained.
[0206] The transition metal source may be an oxide or hydroxide of the above transition metals. The cobalt source may be, for example, cobalt oxide or cobalt hydroxide. The manganese source may be, for example, manganese oxide or manganese hydroxide. The nickel source may be, for example, nickel oxide or nickel hydroxide. The aluminum source may be, for example, aluminum oxide or aluminum hydroxide.
[0207] <Step S22> Next, in step S22, the lithium source and the transition metal source are mixed together.
[0208] <Step S23> Next, the mixed material is heated.
[0209] <Step S24, Step S25> The fired material is recovered (step S24) to obtain a composite oxide containing lithium, a transition metal, and oxygen (step S25). Specifically, lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium cobalt oxide in which a portion of the cobalt is replaced by manganese, or lithium nickel-manganese-cobalt oxide is obtained.
[0210] Alternatively, a composite oxide containing lithium, a transition metal, and oxygen that has been synthesized in advance in step S25 may be used.
[0211] When using a composite oxide having lithium, transition metals, and oxygen that has been synthesized in advance, it is preferable to use one with few impurities. In this specification, the main components of the composite oxide having lithium, transition metals, and oxygen, and the positive electrode active material are lithium, cobalt, nickel, manganese, aluminum, and oxygen, and elements other than the main components are impurities. For example, when analyzed by glow discharge mass spectrometry, the total impurity concentration is preferably 10,000 ppm wt or less, more preferably 5000 ppm wt or less. In particular, the total impurity concentration of transition metals such as titanium and arsenic is preferably 3000 ppm wt or less, more preferably 1500 ppm wt or less.
[0212] For example, lithium cobalt oxide particles (product name: Cellseed C-10N) manufactured by Nippon Chemical Industry Co., Ltd. can be used as the pre-synthesized lithium cobalt oxide. This is lithium cobalt oxide with an average particle diameter (D50) of about 12 μm, and in impurity analysis by glow discharge mass spectrometry (GD-MS), the magnesium concentration and fluorine concentration are 50 ppm wt or less, the calcium concentration, aluminum concentration and silicon concentration are 100 ppm wt or less, the nickel concentration is 150 ppm wt or less, the sulfur concentration is 500 ppm wt or less, the arsenic concentration is 1100 ppm wt or less, and the concentration of other elements other than lithium, cobalt and oxygen is 150 ppm wt or less.
[0213] Alternatively, lithium cobalt oxide particles (product name: Cellseed C-5H) manufactured by Nippon Chemical Industry Co., Ltd. can also be used. This is lithium cobalt oxide with an average particle size (D50) of approximately 6.5 μm, and in impurity analysis by GD-MS, the concentration of elements other than lithium, cobalt, and oxygen is approximately the same as or lower than that of C-10N.
[0214] The composite oxide having lithium, a transition metal, and oxygen in step S25 preferably has a layered rock-salt type crystal structure with few defects and distortion. Therefore, it is preferable that the composite oxide has few impurities. If the composite oxide having lithium, a transition metal, and oxygen contains a large amount of impurities, it is highly likely that the composite oxide will have a crystal structure with many defects or distortion.
[0215] <Step S31> Next, the first mixture is mixed with a composite oxide containing lithium, a transition metal, and oxygen (step S31).
[0216] The mixing in step S31 is preferably performed under milder conditions than those in step S12 in order not to destroy the composite oxide particles. For example, the mixing is preferably performed under conditions of a lower rotation speed or shorter time than those in step S12. It can also be said that the dry method is a milder condition than the wet method. For example, a ball mill, a bead mill, etc. can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media, for example.
[0217] <Step S32, Step S33> The mixed materials are collected (step S32) to obtain a second mixture (step S33).
[0218] In this embodiment, a method of adding a mixture of lithium fluoride and magnesium fluoride to lithium cobalt oxide with few impurities is described, but one embodiment of the present invention is not limited thereto. Instead of the second mixture in step S33, a starting material of lithium cobalt oxide to which a magnesium source and a fluorine source are added and baked may be used. In this case, there is no need to separate the steps S11 to S14 from the steps S21 to S25, and therefore the process is simple and has high productivity.
[0219] Alternatively, lithium cobalt oxide to which magnesium and fluorine have been added in advance may be used. If lithium cobalt oxide to which magnesium and fluorine have been added is used, the steps up to step S32 can be omitted, which is simpler.
[0220] Furthermore, a magnesium source and a fluorine source may be further added to lithium cobalt oxide to which magnesium and fluorine have already been added.
[0221] <Step S34> The second mixture is then heated. This step is sometimes called annealing or second heating to distinguish it from the previous heating step.
[0222] The annealing is preferably performed at an appropriate temperature and time. The appropriate temperature and time vary depending on conditions such as the size and composition of the particles of the composite oxide having lithium, transition metal, and oxygen in step S25. If the particles are small, a lower temperature or a shorter time may be more preferable than if the particles are large.
[0223] For example, when the average particle size (D50) of the particles in step S25 is about 12 μm, the annealing temperature is preferably, for example, 600° C. or more and 950° C. or less. The annealing time is, for example, preferably 3 hours or more, more preferably 10 hours or more, and even more preferably 60 hours or more.
[0224] On the other hand, when the average particle size (D50) of the particles in step S25 is about 5 μm, the annealing temperature is preferably, for example, from 600° C. to 950° C. The annealing time is preferably, for example, from 1 hour to 10 hours, and more preferably about 2 hours.
[0225] The temperature drop time after annealing is preferably, for example, 10 hours or more and 50 hours or less.
[0226] When the second mixture is annealed, it is believed that the material with a low melting point in the first mixture (e.g., lithium fluoride, melting point 848°C) melts first and distributes in the surface layer of the composite oxide particles. It is then assumed that the presence of this molten material lowers the melting points of other materials, causing them to melt. For example, it is believed that magnesium fluoride (melting point 1263°C) melts and distributes in the surface layer of the composite oxide particles.
[0227] It is believed that the elements contained in the first mixture distributed in the surface layer portion are dissolved in the composite oxide containing lithium, a transition metal, and oxygen.
[0228] The diffusion of elements contained in this first mixture is faster in the surface layer and near the grain boundaries than in the interior of the composite oxide particles. Therefore, magnesium and halogen are more concentrated in the surface layer and near the grain boundaries than in the interior. As will be described later, if the magnesium concentration is high in the surface layer and near the grain boundaries, changes in the crystal structure can be more effectively suppressed.
[0229] <Step S35> The annealed material described above is recovered to obtain the positive electrode active material 100 according to one embodiment of the present invention.
[0230] By using the above method, it is possible to produce a positive electrode active material that has a pseudo-spinel crystal structure with few defects when charged at a high voltage. A positive electrode active material in which the pseudo-spinel crystal structure is 50% or more when subjected to Rietveld analysis is a positive electrode active material with excellent cycle characteristics and rate characteristics.
[0231] In order to prepare a positive electrode active material having a pseudo-spinel type crystal structure after high-voltage charging, it is effective that the positive electrode active material has magnesium and fluorine, and is prepared by annealing at an appropriate temperature and time. The magnesium source and the fluorine source may be added to the starting material of the composite oxide. However, when added to the starting material of the composite oxide, if the melting points of the magnesium source and the fluorine source are higher than the firing temperature, the magnesium source and the fluorine source may not melt and may not diffuse sufficiently. Then, there is a high possibility that many defects or distortions will occur in the layered rock salt type crystal structure. Therefore, there is a possibility that defects or distortions will occur in the pseudo-spinel type crystal structure after high-voltage charging.
[0232] Therefore, it is preferable to first obtain a composite oxide having a layered rock-salt crystal structure with few impurities and few defects or distortion. Then, in the subsequent step, it is preferable to mix the composite oxide with a magnesium source and a fluorine source, anneal the mixture, and dissolve magnesium and fluorine in the surface layer of the composite oxide. By preparing the composite oxide in this manner, it is possible to prepare a positive electrode active material having a pseudo-spinel structure with few defects or distortion after high-voltage charging.
[0233] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0234] (Embodiment 4) In this embodiment, an example of a material that can be used in a secondary battery having the positive electrode active material 100 described in the previous embodiment will be described. In this embodiment, a secondary battery in which a positive electrode, a negative electrode, and an electrolyte are enclosed in an exterior body will be described as an example.
[0235] [Positive electrode] The positive electrode has a positive electrode active material layer and a positive electrode current collector.
[0236] <Cathode active material layer> The positive electrode active material layer contains at least a positive electrode active material. In addition to the positive electrode active material, the positive electrode active material layer may contain other substances such as a coating on the surface of the active material, a conductive assistant, or a binder.
[0237] The positive electrode active material may be the positive electrode active material 100 described in the previous embodiment. By using the positive electrode active material 100 described in the previous embodiment, a secondary battery having a high capacity and excellent cycle characteristics can be obtained.
[0238] The conductive assistant may be a carbon material, a metal material, a conductive ceramic material, or the like. A fibrous material may also be used as the conductive assistant. The content of the conductive assistant relative to the total amount of the active material layer is preferably 1 wt% to 10 wt%, more preferably 1 wt% to 5 wt%.
[0239] The conductive assistant can form an electrical conductive network in the active material layer. The conductive assistant can maintain an electrical conductive path between the positive electrode active materials. By adding the conductive assistant to the active material layer, an active material layer having high electrical conductivity can be realized.
[0240] As the conductive assistant, for example, natural graphite, artificial graphite such as mesocarbon microbeads, carbon fiber, etc. can be used. As the carbon fiber, for example, mesophase pitch carbon fiber, isotropic pitch carbon fiber, etc. can be used. As the carbon fiber, carbon nanofiber, carbon nanotube, etc. can be used. Carbon nanotube can be produced by, for example, vapor phase growth method, etc. As the conductive assistant, for example, carbon material such as carbon black (acetylene black (AB) etc.), graphite (graphite) particles, graphene, fullerene, etc. can be used. As the conductive assistant, for example, metal powder or metal fiber such as copper, nickel, aluminum, silver, gold, etc., conductive ceramic material, etc. can be used.
[0241] In addition, a graphene compound may be used as the conductive assistant.
[0242] Graphene compounds may have excellent electrical properties, such as high electrical conductivity, and excellent physical properties, such as high flexibility and high mechanical strength. In addition, graphene compounds have a planar shape. Graphene compounds enable surface contact with low contact resistance. In addition, even if they are thin, they may have very high electrical conductivity, and a conductive path can be efficiently formed in the active material layer with a small amount. Therefore, it is preferable to use a graphene compound as a conductive assistant, since it is possible to increase the contact area between the active material and the conductive assistant. It is preferable to use a spray dryer to form a coating of the graphene compound, which is a conductive assistant, by covering the entire surface of the active material. It is also preferable because it may be possible to reduce electrical resistance. Here, it is particularly preferable to use graphene, multi-graphene, or RGO as the graphene compound. Here, RGO refers to a compound obtained by reducing graphene oxide (GO), for example.
[0243] When using an active material with a small particle size, for example, an active material with a particle size of 1 μm or less, the specific surface area of the active material is large, and more conductive paths connecting the active materials are required. Therefore, the amount of conductive assistant tends to be large, and the amount of active material supported tends to decrease relatively. If the amount of active material supported decreases, the capacity of the secondary battery decreases. In such a case, it is particularly preferable to use a graphene compound as a conductive assistant, since even a small amount of the graphene compound can efficiently form a conductive path, and therefore the amount of active material supported does not decrease.
[0244] As an example, a cross-sectional configuration example in which a graphene compound is used as a conductive assistant in the active material layer 200 will be described below.
[0245] 7A shows a vertical cross-sectional view of an active material layer 200. The active material layer 200 includes a granular positive electrode active material 100, a graphene compound 201 as a conductive assistant, and a binder (not shown). Here, for example, graphene or multi-graphene may be used as the graphene compound 201. Here, the graphene compound 201 preferably has a sheet-like shape. The graphene compound 201 may be a sheet-like shape formed by partially overlapping a plurality of multi-graphenes or (and) a plurality of graphenes.
[0246] In the vertical cross section of the active material layer 200, as shown in Fig. 7B, sheet-like graphene compounds 201 are dispersed approximately uniformly inside the active material layer 200. In Fig. 7B, the graphene compounds 201 are typically represented by thick lines, but are actually thin films having a thickness corresponding to a single layer or multiple layers of carbon molecules. The multiple graphene compounds 201 are formed so as to partially cover the multiple granular positive electrode active materials 100 or to be attached to the surfaces of the multiple granular positive electrode active materials 100, and are therefore in surface contact with each other.
[0247] Here, a mesh-like graphene compound sheet (hereinafter referred to as a graphene compound net or graphene net) can be formed by bonding multiple graphene compounds together. When an active material is covered with a graphene net, the graphene net can also function as a binder that bonds the active materials together. Therefore, the amount of binder can be reduced or no binder can be used, and the ratio of the active material to the electrode volume or weight can be improved. In other words, the capacity of the secondary battery can be increased.
[0248] Here, it is preferable to use graphene oxide as the graphene compound 201, mix it with an active material to form a layer that becomes the active material layer 200, and then reduce it. By using graphene oxide, which has extremely high dispersibility in a polar solvent, to form the graphene compound 201, it is possible to disperse the graphene compound 201 approximately uniformly inside the active material layer 200. Since the solvent is volatilized and removed from the dispersion medium containing the uniformly dispersed graphene oxide and the graphene oxide is reduced, the graphene compound 201 remaining in the active material layer 200 is dispersed to such an extent that it partially overlaps with each other and is in surface contact with each other, thereby forming a three-dimensional conductive path. Note that the reduction of the graphene oxide may be performed by, for example, heat treatment or using a reducing agent.
[0249] Therefore, unlike a granular conductive assistant such as acetylene black that makes point contact with the active material, the graphene compound 201 enables surface contact with low contact resistance, and therefore the electrical conductivity between the granular positive electrode active material 100 and the graphene compound 201 can be improved with a smaller amount than that of a normal conductive assistant. Therefore, the ratio of the positive electrode active material 100 in the active material layer 200 can be increased. This can increase the discharge capacity of the secondary battery.
[0250] Furthermore, by using a spray dryer in advance, the graphene compound, which is a conductive additive, can be formed as a coating to cover the entire surface of the active material, and further a conductive path can be formed between adjacent particles of the active material by the graphene compound.
[0251] As the binder, it is preferable to use a rubber material such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. Also, as the binder, fluororubber can be used.
[0252] Moreover, it is preferable to use, for example, a water-soluble polymer as the binder. For example, polysaccharides can be used as the water-soluble polymer. For example, cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, and regenerated cellulose, and starch can be used as the polysaccharide. It is even more preferable to use these water-soluble polymers in combination with the above-mentioned rubber material.
[0253] Alternatively, it is preferable to use materials such as polystyrene, polymethyl acrylate, polymethyl methacrylate (polymethyl methacrylate, PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, and nitrocellulose as the binder.
[0254] The binder may be used in combination of two or more of the above.
[0255] For example, a material having a particularly excellent viscosity adjusting effect may be used in combination with another material. For example, while rubber materials and the like have excellent adhesive strength and elasticity, it may be difficult to adjust the viscosity when mixed with a solvent. In such a case, it is preferable to mix the material with a material having a particularly excellent viscosity adjusting effect. For example, a water-soluble polymer may be used as a material having a particularly excellent viscosity adjusting effect. In addition, as a water-soluble polymer having a particularly excellent viscosity adjusting effect, the above-mentioned polysaccharides, for example, carboxymethylcellulose (CMC), methylcellulose, ethylcellulose, hydroxypropylcellulose, diacetylcellulose, cellulose derivatives such as regenerated cellulose, and starch may be used.
[0256] In addition, the solubility of cellulose derivatives such as carboxymethylcellulose is increased by converting them into salts such as sodium salts and ammonium salts of carboxymethylcellulose, and they are more likely to exhibit their effect as viscosity adjusters. The increased solubility can also increase the dispersibility of the active material and other components when preparing an electrode slurry. In this specification, the cellulose and cellulose derivatives used as electrode binders include their salts.
[0257] Fluorine-based resins have the advantages of excellent mechanical strength, high chemical resistance, high heat resistance, etc. PVDF, which is one of the fluororesins, has extremely excellent properties among fluororesins, including mechanical strength, excellent processability, and high heat resistance.
[0258] On the other hand, when the slurry prepared when applying the active material layer becomes alkaline, PVDF may gel. Or may become insoluble. The gelation or insolubilization of the binder may reduce the adhesion between the current collector and the active material layer. When the positive electrode active material of one embodiment of the present invention contains phosphorus, for example, a phosphoric acid compound, it is preferable because the pH of the slurry may be lowered to suppress gelation or insolubilization.
[0259] The thickness of the positive electrode active material layer is, for example, 10 μm to 200 μm, or 50 μm to 150 μm. For example, when the positive electrode active material has a material having a layered rock salt crystal structure containing cobalt, the amount of the positive electrode active material layer is 1 mg / cm. 2 More than 50mg / cm 2 or less than 5 mg / cm 2 More than 30mg / cm 2 The density of the positive electrode active material layer is, for example, 2.2 g / cm when the positive electrode active material has a material having a layered rock salt crystal structure containing cobalt. 3 More than 4.9g / cm 3 or less. Or 3.8 g / cm 3 More than 4.5g / cm 3 The following is the result.
[0260] <Positive electrode current collector> The positive electrode current collector may be made of a material having high electrical conductivity, such as metals such as stainless steel, gold, platinum, aluminum, and titanium, and alloys thereof. The material used for the positive electrode current collector is preferably one that does not dissolve at the potential of the positive electrode. Aluminum alloys to which elements that improve heat resistance, such as silicon, titanium, neodymium, scandium, and molybdenum, are added may be used. The positive electrode current collector may be made of a metal element that reacts with silicon to form silicide. Examples of metal elements that react with silicon to form silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, and nickel. The current collector may be in the form of a foil, plate (sheet), net, punched metal, or expanded metal. The current collector may be made of a material having a thickness of 5 μm to 30 μm.
[0261] [Negative electrode] The negative electrode includes a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer may include a conductive assistant and a binder.
[0262] <Negative electrode active material> As the negative electrode active material, for example, an alloy-based material or a carbon-based material can be used.
[0263] As the negative electrode active material, an element capable of carrying out a charge / discharge reaction by alloying / dealloying reaction with lithium can be used. For example, a material containing at least one of silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, indium, etc. can be used. Such elements have a larger capacity than carbon, and silicon in particular has a high theoretical capacity of 4200mAh / g. For this reason, it is preferable to use silicon as the negative electrode active material. Compounds containing these elements may also be used. For example, there are SiO, Mg2Si, Mg2Ge, SnO, SnO2, Mg2Sn, SnS2, V2Sn3, FeSn2, CoSn2, Ni3Sn2, Cu6Sn5, Ag3Sn, Ag3Sb, Ni2MnSb, CeSb3, LaSn3, La3Co2Sn7, CoSb3, InSb, SbSn, etc. Here, elements capable of carrying out charge / discharge reactions through alloying / dealloying reactions with lithium, and compounds containing such elements, are sometimes referred to as alloying materials.
[0264] In this specification, SiO refers to, for example, silicon monoxide. Alternatively, SiO x Here, x preferably has a value close to 1. For example, x is preferably 0.2 or more and 1.5 or less, and more preferably 0.3 or more and 1.2 or less.
[0265] As the carbon-based material, graphite, easily graphitizable carbon (soft carbon), non-graphitizable carbon (hard carbon), carbon nanotubes, graphene, carbon black, and the like may be used.
[0266] Examples of graphite include artificial graphite and natural graphite. Examples of artificial graphite include mesocarbon microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. Here, as the artificial graphite, spherical graphite having a spherical shape can be used. For example, MCMB may have a spherical shape, which is preferable. In addition, it is relatively easy to reduce the surface area of MCMB, which may be preferable. Examples of natural graphite include flake graphite and spheroidized natural graphite.
[0267] When lithium ions are inserted into graphite (when lithium-graphite intercalation compounds are formed), graphite exhibits a low potential similar to that of lithium metal (0.05 V to 0.3 V vs. Li / Li + ) This allows lithium-ion secondary batteries to exhibit high operating voltages. Furthermore, graphite is preferred because it has the advantages of relatively high capacity per unit volume, relatively small volume expansion, low cost, and high safety compared to lithium metal.
[0268] In addition, titanium dioxide (TiO2), lithium titanium oxide (Li4Ti5O 12 ), lithium-graphite intercalation compound (Li x C6), niobium pentoxide (Nb2O5), tungsten oxide (WO2), molybdenum oxide (MoO2), and other oxides can be used.
[0269] In addition, the negative electrode active material is Li3N-type Li, a complex nitride of lithium and transition metals. 3-x M x N (M=Co, Ni, Cu) can be used. For example, Li 2.6 Co 0.4 N3 has a large charge / discharge capacity (900mAh / g, 1890mAh / cm 3 ) and is preferred.
[0270] When a composite nitride of lithium and a transition metal is used, lithium ions are contained in the negative electrode active material, and therefore it is preferable to combine it with a material that does not contain lithium ions, such as V2O5 or Cr3O8, as the positive electrode active material. Even when a material that contains lithium ions is used as the positive electrode active material, the composite nitride of lithium and a transition metal can be used as the negative electrode active material by first removing the lithium ions contained in the positive electrode active material.
[0271] In addition, materials that undergo a conversion reaction can also be used as the negative electrode active material. For example, transition metal oxides that do not form an alloy with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), and iron oxide (FeO), can be used as the negative electrode active material. Further examples of materials that undergo a conversion reaction include oxides such as Fe2O3, CuO, Cu2O, RuO2, and Cr2O3, and CoS 0.89 It also occurs in sulfides such as NiS and CuS, nitrides such as Zn3N2, Cu3N and Ge3N4, phosphides such as NiP2, FeP2 and CoP3, and fluorides such as FeF3 and BiF3.
[0272] As the conductive assistant and binder that the negative electrode active material layer can have, the same materials as the conductive assistant and binder that the positive electrode active material layer can have can be used.
[0273] <Negative electrode current collector> The negative electrode current collector may be made of the same material as the positive electrode current collector, but it is preferable that the negative electrode current collector is made of a material that does not form an alloy with carrier ions such as lithium.
[0274] [Electrolyte] The electrolytic solution has a solvent and an electrolyte. The solvent of the electrolytic solution is preferably an aprotic organic solvent, and for example, one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chloroethylene carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethyl sulfoxide, diethyl ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran, sulfolane, sultone, etc., or two or more of these can be used in any combination and ratio.
[0275] In addition, by using one or more ionic liquids (room-temperature molten salts) that are flame-retardant and non-volatile as a solvent for the electrolyte, even if the internal temperature of the secondary battery rises due to an internal short circuit or overcharging, the secondary battery can be prevented from bursting or catching fire. The ionic liquid is composed of a cation and an anion, and includes an organic cation and an anion. Examples of the organic cation used in the electrolyte include aliphatic onium cations such as quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations, and aromatic cations such as imidazolium cations and pyridinium cations. Examples of the anion used in the electrolyte include monovalent amide anions, monovalent methide anions, fluorosulfonic acid anions, perfluoroalkylsulfonic acid anions, tetrafluoroborate anions, perfluoroalkylborate anions, hexafluorophosphate anions, and perfluoroalkylphosphate anions.
[0276] Examples of the electrolyte to be dissolved in the above-mentioned solvent include LiPF6, LiClO4, LiAsF6, LiBF4, LiAlCl4, LiSCN, LiBr, LiI, Li2SO4, and Li2B 10 Cl 10 , Li2B12 Cl 12 Lithium salts such as LiCF3SO3, LiC4F9SO3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiN(CF3SO2)2, LiN(C4F9SO2)(CF3SO2), LiN(C2F5SO2)2, etc. can be used alone or in any combination and ratio of two or more of these.
[0277] The electrolyte used in the secondary battery is preferably a highly purified electrolyte with a low content of granular dust and elements other than the constituent elements of the electrolyte (hereinafter, simply referred to as "impurities"). Specifically, the weight ratio of impurities to the electrolyte is preferably 1% or less, more preferably 0.1% or less, and even more preferably 0.01% or less.
[0278] In addition, additives such as vinylene carbonate, propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate)borate (LiBOB), and dinitrile compounds such as succinonitrile and adiponitrile may be added to the electrolyte. The concentration of the additive may be, for example, 0.1 wt% to 5 wt% of the total solvent.
[0279] Alternatively, a polymer gel electrolyte may be used in which a polymer is swollen with an electrolytic solution.
[0280] The use of a polymer gel electrolyte improves safety against leakage, etc. Also, it is possible to make the secondary battery thinner and lighter.
[0281] Examples of the polymer that can be gelled include silicone gel, acrylic gel, acrylonitrile gel, polyethylene oxide gel, polypropylene oxide gel, and fluorine-based polymer gel.
[0282] As the polymer, for example, a polymer having a polyalkylene oxide structure such as polyethylene oxide (PEO), PVDF, polyacrylonitrile, etc., and copolymers containing these can be used. For example, PVDF-HFP, which is a copolymer of PVDF and hexafluoropropylene (HFP), can be used. The formed polymer may have a porous shape.
[0283] In addition, instead of the electrolyte, a solid electrolyte containing inorganic materials such as sulfides or oxides, or a solid electrolyte containing polymeric materials such as PEO (polyethylene oxide) can be used. When using a solid electrolyte, the installation of a separator or spacer becomes unnecessary. In addition, since the entire battery can be solidified, there is no risk of leakage, and safety is dramatically improved.
[0284] [Separator] The secondary battery preferably has a separator. The separator may be made of, for example, paper, nonwoven fabric, glass fiber, ceramics, or synthetic fibers such as nylon (polyamide), vinylon (polyvinyl alcohol fiber), polyester, acrylic, polyolefin, or polyurethane. The separator is preferably processed into an envelope shape and disposed so as to encase either the positive electrode or the negative electrode.
[0285] The separator may have a multi-layer structure. For example, an organic material film such as polypropylene or polyethylene may be coated with a ceramic material, a fluorine material, a polyamide material, or a mixture of these. As the ceramic material, for example, aluminum oxide particles or silicon oxide particles may be used. As the fluorine material, for example, PVDF or polytetrafluoroethylene may be used. As the polyamide material, for example, nylon or aramid (meta-aramid or para-aramid) may be used.
[0286] Coating with ceramic materials improves oxidation resistance, suppressing the deterioration of the separator during high-voltage charging and discharging, and improving the reliability of the secondary battery. Coating with fluorine-based materials also improves adhesion between the separator and electrodes, improving output characteristics. Coating with polyamide-based materials, especially aramid, improves heat resistance, improving the safety of the secondary battery.
[0287] For example, both sides of a polypropylene film may be coated with a mixture of aluminum oxide and aramid.Alternatively, the surface of the polypropylene film that contacts the positive electrode may be coated with a mixture of aluminum oxide and aramid, and the surface that contacts the negative electrode may be coated with a fluorine-based material.
[0288] By using a separator with a multi-layer structure, the safety of the secondary battery can be maintained even if the overall thickness of the separator is thin, and therefore the capacity per volume of the secondary battery can be increased.
[0289] [Exterior body] The exterior body of the secondary battery can be made of, for example, a metal material such as aluminum or a resin material. Also, a film-shaped exterior body can be used. As the film, for example, a three-layer structure film can be used in which a thin metal film having excellent flexibility such as aluminum, stainless steel, copper, nickel, etc. is provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, polyamide, etc., and an insulating synthetic resin film such as a polyamide-based resin or polyester-based resin is further provided on the thin metal film as the outer surface of the exterior body.
[0290] [Charge / discharge method] The secondary battery can be charged and discharged, for example, as follows.
[0291] ≪CC charging≫ First, CC charging will be explained as one of the charging methods. CC charging is a charging method in which a constant current flows through the secondary battery throughout the entire charging period, and charging is stopped when a specified voltage is reached. The secondary battery is assumed to be an equivalent circuit with an internal resistance R and a secondary battery capacity C, as shown in Figure 8A. In this case, the secondary battery voltage V B is the voltage V across the internal resistance R R and the voltage V applied to the secondary battery capacity C C It is the sum of.
[0292] During CC charging, as shown in FIG. 8A, the switch is turned on and a constant current I flows through the secondary battery. During this time, the current I is constant, so V R According to Ohm's law, the voltage V across the internal resistance R is R On the other hand, the voltage V applied to the secondary battery capacity C is constant. C increases over time. Therefore, the secondary battery voltage V B increases over time.
[0293] and the secondary battery voltage V B When the voltage V reaches a certain voltage, for example 4.3 V, charging is stopped. When CC charging is stopped, the switch is turned off and the current I becomes 0, as shown in Figure 8B. Therefore, the voltage V across the internal resistance R R Therefore, the secondary battery voltage V B decreases.
[0294] The secondary battery voltage V during CC charging and after CC charging is stopped B An example of the charge current is shown in Fig. 8C. The secondary battery voltage V B However, it is shown that the value decreases slightly after CC charging is stopped.
[0295] ≪CCCV charging≫ Next, we will explain CCCV charging, which is a charging method different from the above. CCCV charging is a charging method in which charging is first performed up to a specified voltage using CC charging, and then charging is performed using CV (constant voltage) charging until the current flow decreases, specifically until the current reaches a cut-off current value.
[0296] During CC charging, as shown in FIG. 9A, the constant current power supply switch is on and the constant voltage power supply switch is off, and a constant current I flows through the secondary battery. During this time, the current I is constant, so V R According to Ohm's law, the voltage V across the internal resistance R is R On the other hand, the voltage V applied to the secondary battery capacity C is constant. C increases over time. Therefore, the secondary battery voltage V B increases over time.
[0297] and the secondary battery voltage V B When the secondary battery voltage V reaches a certain voltage, for example, 4.3 V, the charging mode is switched from CC charging to CV charging. During CV charging, as shown in FIG. 9B, the constant voltage power supply switch is turned on and the constant current power supply switch is turned off, and the secondary battery voltage V B On the other hand, the voltage V applied to the secondary battery capacity C is constant. C V increases over time. B =V R +V C Therefore, the voltage V across the internal resistance R R The voltage V across the internal resistance R decreases over time. R As becomes smaller, V R According to Ohm's law, the current I flowing through the secondary battery also becomes smaller.
[0298] When the current I flowing through the secondary battery becomes a predetermined current, for example, a current equivalent to 0.01 C, charging is stopped. When CCCV charging is stopped, as shown in FIG. 9C, all switches are turned off and the current I becomes 0. Therefore, the voltage V across the internal resistance R R becomes 0V. However, the voltage V applied to the internal resistance R due to CV charging Ris small enough that even if there is no voltage drop across the internal resistance R, the secondary battery voltage V B hardly descends at all.
[0299] The secondary battery voltage V during CCCV charging and after CCCV charging is stopped B An example of the charging current is shown in Figure 9D. Even if CCCV charging is stopped, the secondary battery voltage V B It is shown that the aircraft barely descends at all.
[0300] ≪CC discharge≫ Next, we will explain CC discharge, which is one of the discharging methods. CC discharge is a method in which a constant current flows from the secondary battery throughout the entire discharging period, and the secondary battery voltage V B This is a discharge method in which discharging is stopped when the voltage reaches a predetermined voltage, for example 2.5V.
[0301] The secondary battery voltage V during CC discharge B An example of the secondary battery voltage V B The figure shows how the light descends.
[0302] Next, we will explain the discharge rate and charge rate. The discharge rate is the relative ratio of the current during discharge to the battery capacity, and is expressed in units of C. For a battery with a rated capacity of X (Ah), the current equivalent to 1C is X (A). When a battery is discharged at a current of 2X (A), it is said to have been discharged at 2C, and when a battery is discharged at a current of X / 5 (A), it is said to have been discharged at 0.2C. The same is true for the charge rate; when a battery is charged at a current of 2X (A), it is said to have been charged at 2C, and when a battery is charged at a current of X / 5 (A), it is said to have been charged at 0.2C.
[0303] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0304] (Embodiment 5) In this embodiment, an example of the shape of a secondary battery including the positive electrode active material 100 described in the previous embodiment will be described. The description in the previous embodiment can be referred to for the material used in the secondary battery described in this embodiment.
[0305] [Coin-type secondary battery] First, an example of a coin-type secondary battery will be described. Fig. 11A is an external view of a coin-type (single-layer flat) secondary battery, and Fig. 11B is a cross-sectional view thereof.
[0306] In the coin-type secondary battery 300, a positive electrode can 301, which also serves as a positive electrode terminal, and a negative electrode can 302, which also serves as a negative electrode terminal, are insulated and sealed with a gasket 303 made of polypropylene or the like. The positive electrode 304 is formed of a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector. The negative electrode 307 is formed of a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector.
[0307] In addition, the positive electrode 304 and the negative electrode 307 used in the coin-type secondary battery 300 each need only have an active material layer formed on one side.
[0308] Metals such as nickel, aluminum, and titanium that are corrosion-resistant to the electrolyte, or alloys of these metals and other metals (e.g., stainless steel, etc.) can be used for the positive electrode can 301 and the negative electrode can 302. In order to prevent corrosion by the electrolyte, it is preferable to coat them with nickel, aluminum, etc. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.
[0309] These negative electrode 307, positive electrode 304, and separator 310 are impregnated with an electrolyte, and as shown in FIG. 11B, positive electrode can 301 is placed at the bottom, and positive electrode can 301 and negative electrode can 302 are laminated in this order, and positive electrode can 301 and negative electrode can 302 are crimped together via gasket 303, to produce coin-type secondary battery 300.
[0310] By using the positive electrode active material described in the above embodiment for the positive electrode 304, the coin-type secondary battery 300 can have a high capacity and excellent cycle characteristics.
[0311] Here, the flow of current during charging of a secondary battery will be explained using FIG. 11C. When a secondary battery using lithium is regarded as a closed circuit, the movement of lithium ions and the flow of current are in the same direction. In a secondary battery using lithium, the anode (positive electrode) and the cathode (negative electrode) are interchanged during charging and discharging, and the oxidation reaction and the reduction reaction are interchanged, so the electrode with a high reaction potential is called the positive electrode, and the electrode with a low reaction potential is called the negative electrode. Therefore, in this specification, the positive electrode will be called the "positive electrode" or "+ electrode (plus electrode)" and the negative electrode will be called the "negative electrode" or "- electrode (minus electrode)" whether during charging or discharging, whether a pulse current in the reverse direction is applied during charging or discharging, or whether a charging current is applied. If the terms anode (positive electrode) and cathode (negative electrode) related to oxidation and reduction reactions are used, they may be reversed during charging and discharging, which may cause confusion. Therefore, the terms anode (positive electrode) and cathode (negative electrode) will not be used in this specification. If the terms anode (positive electrode) and cathode (negative electrode) are used, it will be specified whether they are used during charging or discharging, and also whether they correspond to a positive electrode (positive pole) or a negative electrode (negative pole).
[0312] 11C are connected to a charger to charge the secondary battery 300. As the charging of the secondary battery 300 progresses, the potential difference between the electrodes increases.
[0313] [Cylindrical secondary battery] Next, an example of a cylindrical secondary battery will be described with reference to Fig. 12. Fig. 12A shows an external view of a cylindrical secondary battery 600. Fig. 12B is a schematic diagram showing a cross section of the cylindrical secondary battery 600. As shown in Fig. 12B, the cylindrical secondary battery 600 has a positive electrode cap (battery lid) 601 on the top surface, and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap and the battery can (external can) 602 are insulated by a gasket (insulating packing) 610.
[0314] Inside a hollow cylindrical battery can 602, a battery element is provided in which a strip-shaped positive electrode 604 and a negative electrode 606 are wound with a separator 605 sandwiched therebetween. Although not shown, the battery element is wound around a center pin. One end of the battery can 602 is closed and the other end is open. For the battery can 602, metals such as nickel, aluminum, and titanium that are resistant to corrosion by the electrolyte, or alloys of these metals and other metals (e.g., stainless steel, etc.) can be used. In addition, in order to prevent corrosion by the electrolyte, it is preferable to coat the battery can 602 with nickel, aluminum, or the like. Inside the battery can 602, the battery element in which the positive electrode, the negative electrode, and the separator are wound is sandwiched between a pair of opposing insulating plates 608 and 609. In addition, a nonaqueous electrolyte (not shown) is injected inside the battery can 602 in which the battery element is provided. The nonaqueous electrolyte can be the same as that of a coin-type secondary battery.
[0315] Since the positive and negative electrodes used in a cylindrical storage battery are wound, it is preferable to form an active material on both sides of the current collector. A positive electrode terminal (positive electrode current collector lead) 603 is connected to the positive electrode 604, and a negative electrode terminal (negative electrode current collector lead) 607 is connected to the negative electrode 606. Both the positive electrode terminal 603 and the negative electrode terminal 607 can be made of a metal material such as aluminum. The positive electrode terminal 603 is resistance-welded to a safety valve mechanism 612, and the negative electrode terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 612 is electrically connected to the positive electrode cap 601 via a PTC element (Positive Temperature Coefficient) 611. The safety valve mechanism 612 cuts off the electrical connection between the positive electrode cap 601 and the positive electrode 604 when the rise in the internal pressure of the battery exceeds a predetermined threshold value. The PTC element 611 is a thermosensitive resistor whose resistance increases when the temperature rises, and the increase in resistance limits the amount of current to prevent abnormal heat generation. Barium titanate (BaTiO3)-based semiconductor ceramics can be used for the PTC element.
[0316] 12C, a plurality of secondary batteries 600 may be sandwiched between conductive plates 613 and 614 to form a module 615. The plurality of secondary batteries 600 may be connected in parallel, in series, or in parallel and then further in series. By forming a module 615 having a plurality of secondary batteries 600, a large amount of power can be extracted.
[0317] FIG. 12D is a top view of the module 615. To clarify the drawing, the conductive plate 613 is shown by a dotted line. As shown in FIG. 12D, the module 615 may have a conductor 616 that electrically connects the multiple secondary batteries 600. A conductive plate can be provided by overlapping the conductor 616. Also, a temperature control device 617 may be provided between the multiple secondary batteries 600. When the secondary battery 600 is overheated, it can be cooled by the temperature control device 617, and when the secondary battery 600 is too cold, it can be heated by the temperature control device 617. Therefore, the performance of the module 615 is less susceptible to the influence of the outside air temperature. It is preferable that the heat medium of the temperature control device 617 is insulating and non-flammable.
[0318] By using the positive electrode active material described in the above embodiment for the positive electrode 604, the cylindrical secondary battery 600 can have a high capacity and excellent cycle characteristics.
[0319] [Example of secondary battery structure] Another structural example of the secondary battery will be described with reference to FIGS.
[0320] 13A and 13B are diagrams showing the external appearance of a secondary battery. A secondary battery 913 is connected to an antenna 914 and an antenna 915 via a circuit board 900. A label 910 is attached to the secondary battery 913. Furthermore, as shown in FIG. 13B, the secondary battery 913 is connected to a terminal 951 and a terminal 952.
[0321] The circuit board 900 has a terminal 911 and a circuit 912. The terminal 911 is connected to a terminal 951, a terminal 952, an antenna 914, an antenna 915, and the circuit 912. Note that a plurality of terminals 911 may be provided, and each of the plurality of terminals 911 may be a control signal input terminal, a power supply terminal, or the like.
[0322] The circuit 912 may be provided on the back surface of the circuit board 900. The antennas 914 and 915 are not limited to being coil-shaped, and may be, for example, wire-shaped or plate-shaped. In addition, antennas such as planar antennas, aperture antennas, traveling wave antennas, EH antennas, magnetic field antennas, and dielectric antennas may be used. Alternatively, the antennas 914 and 915 may be flat conductors. This flat conductor can function as one of the conductors for electric field coupling. In other words, the antennas 914 and 915 may function as one of the two conductors of the capacitor. This allows power to be exchanged not only by electromagnetic fields and magnetic fields, but also by electric fields.
[0323] The line width of the antenna 914 is preferably larger than the line width of the antenna 915. This allows the amount of power received by the antenna 914 to be increased.
[0324] The secondary battery has a layer 916 between the antenna 914 and the antenna 915 and the secondary battery 913. The layer 916 has a function of, for example, shielding an electromagnetic field caused by the secondary battery 913. The layer 916 can be made of, for example, a magnetic material.
[0325] The structure of the secondary battery is not limited to that shown in FIG.
[0326] For example, as shown in Figures 14A and 14B, an antenna may be provided on each of a pair of opposing surfaces of the secondary battery 913 shown in Figures 13A and 13B. Figure 14A is an external view showing one of the pair of surfaces, and Figure 14B is an external view showing the other of the pair of surfaces. Note that the description of the secondary battery shown in Figures 13A and 13B can be used as appropriate for the same parts as those of the secondary battery shown in Figures 13A and 13B.
[0327] 14A, an antenna 914 is provided on one of a pair of surfaces of a secondary battery 913 with a layer 916 sandwiched therebetween, and as shown in Fig. 14B, an antenna 918 is provided on the other of the pair of surfaces of the secondary battery 913 with a layer 917 sandwiched therebetween. The layer 917 has a function of, for example, being able to shield an electromagnetic field caused by the secondary battery 913. The layer 917 can be made of, for example, a magnetic material.
[0328] The above structure allows the sizes of both the antenna 914 and the antenna 918 to be increased. The antenna 918 has a function of performing data communication with, for example, an external device. For example, an antenna having a shape applicable to the antenna 914 can be applied to the antenna 918. As a communication method between the secondary battery and other devices via the antenna 918, a response method that can be used between the secondary battery and other devices, such as NFC (near field wireless communication), can be applied.
[0329] Alternatively, as shown in Fig. 14C, a display device 920 may be provided on the secondary battery 913 shown in Fig. 13A and Fig. 13B. The display device 920 is electrically connected to the terminal 911. Note that the label 910 does not need to be provided on the portion where the display device 920 is provided. Note that the description of the secondary battery shown in Fig. 13A and Fig. 13B can be appropriately applied to the same portions as those of the secondary battery shown in Fig. 13A and Fig. 13B.
[0330] For example, an image indicating whether charging is in progress, an image indicating the amount of stored power, etc. may be displayed on the display device 920. For example, electronic paper, a liquid crystal display device, an electroluminescence (EL) display device, etc. can be used as the display device 920. For example, the use of electronic paper can reduce the power consumption of the display device 920.
[0331] Alternatively, as shown in Fig. 14D, a sensor 921 may be provided in the secondary battery 913 shown in Fig. 13A and Fig. 13B. The sensor 921 is electrically connected to the terminal 911 via a terminal 922. Note that the description of the secondary battery shown in Fig. 13A and Fig. 13B can be appropriately applied to the same parts as those of the secondary battery shown in Fig. 13A and Fig. 13B.
[0332] The sensor 921 may have a function of measuring, for example, displacement, position, speed, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substance, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor, or infrared ray. By providing the sensor 921, for example, data indicating the environment in which the secondary battery is placed (such as temperature) can be detected and stored in the memory in the circuit 912.
[0333] Further, a structural example of the secondary battery 913 will be described with reference to FIGS.
[0334] A secondary battery 913 shown in FIG. 15A has a wound body 950 in which terminals 951 and 952 are provided inside a housing 930. The wound body 950 is impregnated with an electrolyte inside the housing 930. The terminal 952 contacts the housing 930, and the terminal 951 does not contact the housing 930 by using an insulating material or the like. Note that in FIG. 15A, the housing 930 is illustrated separately for convenience, but in reality, the wound body 950 is covered by the housing 930, and the terminals 951 and 952 extend outside the housing 930. The housing 930 can be made of a metal material (e.g., aluminum) or a resin material.
[0335] As shown in Fig. 15B, the housing 930 shown in Fig. 15A may be formed from a plurality of materials. For example, the secondary battery 913 shown in Fig. 15B has a housing 930a and a housing 930b bonded together, and a wound body 950 is provided in the area surrounded by the housings 930a and 930b.
[0336] The housing 930a can be made of an insulating material such as organic resin. In particular, by using a material such as organic resin on the surface on which the antenna is formed, it is possible to suppress shielding of the electric field by the secondary battery 913. Note that if the shielding of the electric field by the housing 930a is small, antennas such as antenna 914 and antenna 915 may be provided inside the housing 930a. The housing 930b can be made of, for example, a metal material.
[0337] 16 shows the structure of the wound body 950. The wound body 950 has a negative electrode 931, a positive electrode 932, and a separator 933. The wound body 950 is a wound body in which the negative electrode 931 and the positive electrode 932 are stacked on top of each other with the separator 933 in between, and the laminated sheet is wound. Note that the stack of the negative electrode 931, the positive electrode 932, and the separator 933 may be stacked a plurality of times.
[0338] 13 via one of the terminal 951 and the terminal 952. The positive electrode 932 is connected to the terminal 911 shown in FIG 13 via the other of the terminal 951 and the terminal 952.
[0339] By using the positive electrode active material described in the above embodiment for the positive electrode 932, the secondary battery 913 can have high capacity and excellent cycle characteristics.
[0340] [Laminated secondary battery] Next, examples of laminated secondary batteries will be described with reference to Fig. 17 to Fig. 23. If the laminated secondary battery has a flexible configuration, and is mounted in an electronic device having at least a flexible portion, the secondary battery can be bent in accordance with the deformation of the electronic device.
[0341] A laminated secondary battery 980 will be described with reference to Fig. 17. The laminated secondary battery 980 has a wound body 993 shown in Fig. 17A. The wound body 993 has a negative electrode 994, a positive electrode 995, and a separator 996. The wound body 993 is formed by stacking the negative electrode 994 and the positive electrode 995 with the separator 996 sandwiched therebetween, in the same manner as the wound body 950 described in Fig. 16, and winding the laminated sheet.
[0342] The number of layers of the negative electrode 994, the positive electrode 995, and the separator 996 may be appropriately designed according to the required capacity and element volume. The negative electrode 994 is connected to a negative electrode current collector (not shown) via one of the lead electrodes 997 and 998, and the positive electrode 995 is connected to a positive electrode current collector (not shown) via the other of the lead electrodes 997 and 998.
[0343] As shown in Fig. 17B, a film 981 serving as an exterior body and a film 982 having a recess are bonded together by thermocompression or the like to form a space, and the above-mentioned wound body 993 is stored in the space, thereby producing a secondary battery 980 as shown in Fig. 17C. The wound body 993 has lead electrodes 997 and 998, and is impregnated with an electrolyte solution between the film 981 and the film 982 having a recess.
[0344] For example, a metal material such as aluminum or a resin material can be used for the film 981 and the film 982 having the recesses. If a resin material is used as the material for the film 981 and the film 982 having the recesses, the film 981 and the film 982 having the recesses can be deformed when an external force is applied, and a flexible storage battery can be produced.
[0345] Although an example in which two films are used is shown in FIG. 17B and FIG. 17C, a space may be formed by folding one film, and the above-mentioned wound body 993 may be housed in the space.
[0346] By using the positive electrode active material described in the above embodiment for the positive electrode 995, the secondary battery 980 can have a high capacity and excellent cycle characteristics.
[0347] In addition, in FIG. 17, an example of a secondary battery 980 having a wound body in a space formed by a film that serves as an outer casing is described. However, as shown in FIG. 18, for example, a secondary battery may also be used that has a plurality of rectangular positive electrodes, separators, and negative electrodes in a space formed by a film that serves as an outer casing.
[0348] 18A includes a positive electrode 503 having a positive electrode current collector 501 and a positive electrode active material layer 502, a negative electrode 506 having a negative electrode current collector 504 and a negative electrode active material layer 505, a separator 507, an electrolyte 508, and an exterior body 509. The separator 507 is disposed between the positive electrode 503 and the negative electrode 506 provided in the exterior body 509. The interior of the exterior body 509 is filled with the electrolyte 508. The electrolyte solution described in Embodiment 2 can be used as the electrolyte solution 508.
[0349] 18A, the positive electrode current collector 501 and the negative electrode current collector 504 also serve as terminals for obtaining electrical contact with the outside. Therefore, the positive electrode current collector 501 and the negative electrode current collector 504 may be arranged so as to be partially exposed to the outside from the exterior body 509. Alternatively, the positive electrode current collector 501 and the negative electrode current collector 504 may not be exposed to the outside from the exterior body 509, but may be exposed to the outside by using a lead electrode and ultrasonically bonding the lead electrode to the positive electrode current collector 501 or the negative electrode current collector 504.
[0350] In the laminated secondary battery 500, the exterior body 509 may be a three-layer laminate film having a highly flexible thin metal film such as aluminum, stainless steel, copper, nickel, etc., provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, polyamide, etc., and further having an insulating synthetic resin film such as a polyamide-based resin, polyester-based resin, etc., provided on the thin metal film as the outer surface of the exterior body.
[0351] 18B shows an example of a cross-sectional structure of a laminated secondary battery 500. For simplicity, Fig. 18A shows an example of a battery made up of two current collectors, but in reality, the battery is made up of multiple electrode layers as shown in Fig. 18B.
[0352] In FIG. 18B, the number of electrode layers is 16 as an example. Even if the number of electrode layers is 16, the secondary battery 500 has flexibility. FIG. 18B shows a structure of 16 layers in total, including 8 layers of negative electrode collector 504 and 8 layers of positive electrode collector 501. FIG. 18B shows a cross section of the negative electrode lead-out portion, in which 8 layers of negative electrode collector 504 are ultrasonically bonded. Of course, the number of electrode layers is not limited to 16, and may be more or less. When the number of electrode layers is large, a secondary battery having a larger capacity can be obtained. Also, when the number of electrode layers is small, a secondary battery that can be made thin and has excellent flexibility can be obtained.
[0353] 19 and 20 show an example of an external view of a laminated secondary battery 500. In FIG. 19 and FIG. 20, a positive electrode 503, a negative electrode 506, a separator 507, an exterior body 509, a positive electrode lead electrode 510, and a negative electrode lead electrode 511 are provided.
[0354] FIG. 21A shows an external view of a positive electrode 503 and a negative electrode 506. The positive electrode 503 has a positive electrode current collector 501, and a positive electrode active material layer 502 is formed on the surface of the positive electrode current collector 501. The positive electrode 503 has a region where the positive electrode current collector 501 is partially exposed (hereinafter referred to as a tab region). The negative electrode 506 has a negative electrode current collector 504, and a negative electrode active material layer 505 is formed on the surface of the negative electrode current collector 504. The negative electrode 506 has a region where the negative electrode current collector 504 is partially exposed, that is, a tab region. The areas and shapes of the tab regions of the positive electrode and negative electrode are not limited to the example shown in FIG. 21A.
[0355] [Method of manufacturing laminated secondary battery] Here, an example of a method for producing the laminate type secondary battery whose external view is shown in FIG. 19 will be described with reference to FIGS. 21B and 21C.
[0356] First, the negative electrode 506, the separator 507, and the positive electrode 503 are laminated. FIG. 21B shows the laminated negative electrode 506, the separator 507, and the positive electrode 503. Here, an example is shown in which five pairs of negative electrodes and four pairs of positive electrodes are used. Next, the tab regions of the positive electrodes 503 are bonded to each other, and the positive electrode lead electrode 510 is bonded to the tab region of the outermost positive electrode. For example, ultrasonic welding or the like may be used for the bonding. Similarly, the tab regions of the negative electrodes 506 are bonded to each other, and the negative electrode lead electrode 511 is bonded to the tab region of the outermost negative electrode.
[0357] Next, the negative electrode 506 , the separator 507 and the positive electrode 503 are placed on the exterior body 509 .
[0358] Next, as shown in Fig. 21C, exterior body 509 is folded at the portion indicated by the dashed line. After that, the outer periphery of exterior body 509 is joined. For the joining, for example, thermocompression bonding or the like may be used. At this time, a region (hereinafter referred to as an inlet) that is not joined is provided in a part (or one side) of exterior body 509 so that electrolyte 508 can be introduced later.
[0359] Next, electrolytic solution 508 (not shown) is introduced into the inside of exterior body 509 through an inlet provided in exterior body 509. The introduction of electrolytic solution 508 is preferably performed under a reduced pressure atmosphere or an inert atmosphere. Finally, the inlet is joined. In this manner, laminated secondary battery 500 can be produced.
[0360] By using the positive electrode active material described in the above embodiment for the positive electrode 503, the secondary battery 500 can have a high capacity and excellent cycle characteristics.
[0361] [Bendable secondary battery] Next, an example of a bendable secondary battery will be described with reference to FIGS. 22 and 23. FIG.
[0362] FIG. 22A shows a schematic top view of a bendable secondary battery 250. FIG. 22B, FIG. 22C, and FIG. 22D are schematic cross-sectional views taken along the lines C1-C2, C3-C4, and A1-A2 in FIG. 22A, respectively. The secondary battery 250 has an exterior body 251, and a positive electrode 211a and a negative electrode 211b housed inside the exterior body 251. A lead 212a electrically connected to the positive electrode 211a and a lead 212b electrically connected to the negative electrode 211b extend outside the exterior body 251. In addition to the positive electrode 211a and the negative electrode 211b, an electrolyte (not shown) is enclosed in the area surrounded by the exterior body 251.
[0363] The positive electrode 211a and the negative electrode 211b of the secondary battery 250 will be described with reference to Fig. 23. Fig. 23A is a perspective view illustrating the stacking order of the positive electrode 211a, the negative electrode 211b, and the separator 214. Fig. 23B is a perspective view showing the lead 212a and the lead 212b in addition to the positive electrode 211a and the negative electrode 211b.
[0364] 23A, secondary battery 250 has a plurality of rectangular positive electrodes 211a, a plurality of rectangular negative electrodes 211b, and a plurality of separators 214. Positive electrode 211a and negative electrode 211b each have a protruding tab portion and a portion other than the tab. A positive electrode active material layer is formed on one surface of positive electrode 211a in the portion other than the tab, and a negative electrode active material layer is formed on one surface of negative electrode 211b in the portion other than the tab.
[0365] The positive electrode 211a and the negative electrode 211b are stacked so that the surfaces of the positive electrode 211a on which the positive electrode active material layer is not formed and the surfaces of the negative electrode 211b on which the negative electrode active material layer is not formed are in contact with each other.
[0366] Furthermore, a separator 214 is provided between the surface of the positive electrode 211a on which the positive electrode active material is formed and the surface of the negative electrode 211b on which the negative electrode active material is formed. In Fig. 23, the separator 214 is indicated by a dotted line for ease of viewing.
[0367] 23B, the multiple positive electrodes 211a and the lead 212a are electrically connected at a joint 215a, and the multiple negative electrodes 211b and the lead 212b are electrically connected at a joint 215b.
[0368] Next, exterior body 251 will be described with reference to FIGS. 22B, 22C, 22D, and 22E.
[0369] The exterior body 251 has a film-like shape and is folded in two to sandwich the positive electrode 211a and the negative electrode 211b. The exterior body 251 has a folded portion 261, a pair of sealing portions 262, and a sealing portion 263. The pair of sealing portions 262 are provided to sandwich the positive electrode 211a and the negative electrode 211b, and can also be called side seals. The sealing portion 263 has a portion overlapping the lead 212a and the lead 212b, and can also be called a top seal.
[0370] It is preferable that exterior body 251 has a corrugated shape in which ridge lines 271 and valley lines 272 are alternately arranged in the portions overlapping with positive electrode 211a and negative electrode 211b. In addition, it is preferable that seal portion 262 and seal portion 263 of exterior body 251 are flat.
[0371] Fig. 22B is a cross section taken at a portion overlapping with ridge line 271, and Fig. 22C is a cross section taken at a portion overlapping with valley line 272. Fig. 22B and Fig. 22C both correspond to cross sections in the width direction of secondary battery 250 and positive electrode 211a and negative electrode 211b.
[0372] Here, the distance between the ends of the positive electrode 211a and the negative electrode 211b in the width direction, i.e., the ends of the positive electrode 211a and the negative electrode 211b, and the seal portion 262 is defined as the distance La. When the secondary battery 250 is deformed, such as by bending, the positive electrode 211a and the negative electrode 211b are deformed so as to be displaced from each other in the length direction, as described below. At that time, if the distance La is too short, the exterior body 251 and the positive electrode 211a and the negative electrode 211b may rub strongly against each other, and the exterior body 251 may be damaged. In particular, if the metal film of the exterior body 251 is exposed, the metal film may be corroded by the electrolyte. Therefore, it is preferable to set the distance La as long as possible. On the other hand, if the distance La is made too large, the volume of the secondary battery 250 increases.
[0373] Moreover, it is preferable that the distance La between the positive electrode 211a and the negative electrode 211b and the seal portion 262 is increased as the total thickness of the stacked positive electrode 211a and negative electrode 211b is increased.
[0374] More specifically, when the total thickness of the laminated positive electrode 211a, negative electrode 211b, and separator 214 (not shown) is t, the distance La is preferably 0.8 to 3.0 times, more preferably 0.9 to 2.5 times, and even more preferably 1.0 to 2.0 times, of the thickness t. By setting the distance La in this range, a compact battery with high reliability against bending can be realized.
[0375] Furthermore, when the distance between the pair of seal portions 262 is distance Lb, it is preferable to set distance Lb sufficiently larger than the width of positive electrode 211a and negative electrode 211b (here, width Wb of negative electrode 211b). As a result, even if positive electrode 211a and negative electrode 211b come into contact with exterior body 251 when secondary battery 250 is repeatedly deformed, such as by bending, parts of positive electrode 211a and negative electrode 211b can be displaced in the width direction, so that rubbing between positive electrode 211a and negative electrode 211b and exterior body 251 can be effectively prevented.
[0376] For example, it is preferable that the difference between the distance Lb between the pair of seal portions 262 and the width Wb of the negative electrode 211b is 1.6 to 6.0 times, preferably 1.8 to 5.0 times, and more preferably 2.0 to 4.0 times the thickness t of the positive electrode 211a and the negative electrode 211b.
[0377] In other words, it is preferable that the distance Lb, the width Wb, and the thickness t satisfy the relationship of the following formula.
[0378]
number
[0379] Here, a satisfies the range of 0.8 to 3.0, preferably 0.9 to 2.5, and more preferably 1.0 to 2.0.
[0380] 22D is a cross section including lead 212a, and corresponds to a cross section in the longitudinal direction of secondary battery 250, positive electrode 211a, and negative electrode 211b. As shown in FIG. 22D, it is preferable to have a space 273 between exterior body 251 and the ends of positive electrode 211a and negative electrode 211b in the longitudinal direction at bent portion 261.
[0381] Fig. 22E shows a schematic cross-sectional view of the bent secondary battery 250. Fig. 22E corresponds to the cross section taken along the cutting line B1-B2 in Fig. 22A.
[0382] When the secondary battery 250 is bent, a part of the exterior body 251 located on the outside of the bend is stretched, and another part located on the inside is deformed so as to contract. More specifically, the part located on the outside of the exterior body 251 is deformed so that the wave amplitude becomes smaller and the wave period becomes larger. On the other hand, the part located on the inside of the exterior body 251 is deformed so that the wave amplitude becomes larger and the wave period becomes smaller. In this way, the deformation of the exterior body 251 relieves the stress applied to the exterior body 251 due to bending, so that the material constituting the exterior body 251 itself does not need to expand or contract. As a result, the exterior body 251 is not damaged, and the secondary battery 250 can be bent with a small force.
[0383] 22E, when the secondary battery 250 is bent, the positive electrode 211a and the negative electrode 211b are displaced relative to each other. At this time, since one end of the multiple stacked positive electrodes 211a and negative electrodes 211b on the seal portion 263 side is fixed by the fixing member 217, the multiple stacked positive electrodes 211a and negative electrodes 211b are displaced such that the amount of displacement increases toward the bent portion 261. This reduces the stress applied to the positive electrodes 211a and negative electrodes 211b, and the positive electrodes 211a and negative electrodes 211b themselves do not need to expand or contract. As a result, the secondary battery 250 can be bent without damaging the positive electrodes 211a and negative electrodes 211b.
[0384] Furthermore, by providing space 273 between positive electrode 211a and negative electrode 211b and exterior body 251, positive electrode 211a and negative electrode 211b located on the inside when bent can be relatively displaced without coming into contact with exterior body 251.
[0385] 22 and 23 is a battery that is unlikely to suffer damage to the exterior body, the positive electrode 211a and the negative electrode 211b, etc., even if repeatedly bent and stretched, and the battery characteristics are also unlikely to deteriorate. By using the positive electrode active material described in the previous embodiment for the positive electrode 211a of the secondary battery 250, it is possible to obtain a battery with further excellent cycle characteristics.
[0386] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0387] (Embodiment 6) In this embodiment, an example in which a secondary battery which is one embodiment of the present invention is mounted on an electronic device will be described.
[0388] 24A to 24G show examples of electronic devices incorporating the bendable secondary battery described in part of embodiment 3. Examples of electronic devices to which the bendable secondary battery is applied include television devices (also called televisions or television receivers), computer monitors, digital cameras, digital video cameras, digital photo frames, mobile phones (also called mobile phones or mobile phone devices), portable game machines, personal digital assistants, audio playback devices, and large game machines such as pachinko machines.
[0389] Furthermore, a secondary battery having a flexible shape can be incorporated into the inner or outer wall of a house or building, or along the curved surface of the interior or exterior of an automobile.
[0390] 24A illustrates an example of a mobile phone. A mobile phone 7400 includes a display portion 7402 built into a housing 7401, operation buttons 7403, an external connection port 7404, a speaker 7405, a microphone 7406, and the like. Note that the mobile phone 7400 includes a secondary battery 7407. By using the secondary battery of one embodiment of the present invention as the secondary battery 7407, a lightweight mobile phone with a long life can be provided.
[0391] FIG. 24B shows a state in which the mobile phone 7400 is bent. When the mobile phone 7400 is deformed by an external force and bent as a whole, the secondary battery 7407 provided inside is also bent. FIG. 24C shows the state of the bent secondary battery 7407 at that time. The secondary battery 7407 is a thin storage battery. The secondary battery 7407 is fixed in a bent state. The secondary battery 7407 has a lead electrode electrically connected to the current collector. For example, the current collector is a copper foil, and a part of the current collector is alloyed with gallium to improve adhesion with the active material layer in contact with the current collector, so that the secondary battery 7407 has a high reliability when bent.
[0392] FIG. 24D illustrates an example of a bangle-type display device. The portable display device 7100 includes a housing 7101, a display unit 7102, an operation button 7103, and a secondary battery 7104. FIG. 24E illustrates a bent state of the secondary battery 7104. When the secondary battery 7104 is worn on a user's arm in a bent state, the housing is deformed, and the curvature of the secondary battery 7104 changes in part or in whole. Note that the degree of bending at any point of the curve expressed by the value of the radius of the corresponding circle is called the radius of curvature, and the reciprocal of the radius of curvature is called the curvature. Specifically, the housing or the main surface of the secondary battery 7104 changes in part or in whole when the radius of curvature is in the range of 40 mm to 150 mm. High reliability can be maintained if the radius of curvature of the main surface of the secondary battery 7104 is in the range of 40 mm to 150 mm. By using the secondary battery of one embodiment of the present invention as the secondary battery 7104, a lightweight portable display device with a long life can be provided.
[0393] 24F shows an example of a wristwatch-type portable information terminal. A portable information terminal 7200 includes a housing 7201, a display portion 7202, a band 7203, a buckle 7204, operation buttons 7205, an input / output terminal 7206, and the like.
[0394] The portable information terminal 7200 can execute various applications such as mobile telephone, e-mail, document browsing and creation, music playback, Internet communication, and computer games.
[0395] The display surface of the display portion 7202 is curved, and display can be performed along the curved display surface. The display portion 7202 is also provided with a touch sensor, and can be operated by touching the screen with a finger, a stylus, or the like. For example, an application can be started by touching an icon 7207 displayed on the display portion 7202.
[0396] The operation button 7205 can have various functions, such as time setting, power on / off operation, wireless communication on / off operation, silent mode activation / cancellation, power saving mode activation / cancellation, etc. For example, the function of the operation button 7205 can be freely set by an operating system built into the mobile information terminal 7200.
[0397] The mobile information terminal 7200 can also perform short-distance wireless communication according to a communication standard. For example, the mobile information terminal 7200 can communicate with a wireless headset to enable hands-free calling.
[0398] The portable information terminal 7200 also includes an input / output terminal 7206, and can directly exchange data with other information terminals via a connector. Charging can also be performed via the input / output terminal 7206. Note that charging may be performed by wireless power supply without using the input / output terminal 7206.
[0399] The display portion 7202 of the mobile information terminal 7200 includes the secondary battery of one embodiment of the present invention. By using the secondary battery of one embodiment of the present invention, a lightweight mobile information terminal with a long life can be provided. For example, the secondary battery 7104 shown in FIG. 24E can be incorporated in a curved state inside the housing 7201 or in a bendable state inside the band 7203.
[0400] The portable information terminal 7200 preferably has a sensor. For example, it is preferable to mount a human body sensor such as a fingerprint sensor, a pulse sensor, or a body temperature sensor, a touch sensor, a pressure sensor, an acceleration sensor, or the like, as the sensor.
[0401] 24G illustrates an example of an armband-type display device. The display device 7300 includes a display portion 7304 and a secondary battery of one embodiment of the present invention. The display device 7300 can also include a touch sensor in the display portion 7304 and can function as a portable information terminal.
[0402] The display surface of the display portion 7304 is curved, and display can be performed along the curved display surface. In addition, the display device 7300 can change the display state by short-range wireless communication according to a communication standard.
[0403] The display device 7300 also includes an input / output terminal, and can directly exchange data with other information terminals via a connector. Charging can also be performed via the input / output terminal. Note that charging may be performed by wireless power supply without using the input / output terminal.
[0404] By using the secondary battery of one embodiment of the present invention as a secondary battery included in the display device 7300, a lightweight display device with a long lifetime can be provided.
[0405] Moreover, an example in which the secondary battery having good cycle characteristics shown in the above embodiment is mounted on an electronic device will be described with reference to FIGS. 24H, 25, and 26. FIG.
[0406] By using the secondary battery of one embodiment of the present invention as a secondary battery in daily electronic devices, products that are lightweight and have a long life can be provided. For example, daily electronic devices include electric toothbrushes, electric shavers, and electric beauty devices. For the secondary battery of these products, a stick-shaped, small, lightweight, and large-capacity secondary battery is desired in consideration of ease of holding by users.
[0407] FIG. 24H is a perspective view of a device also called a tobacco-receiving smoking device (electronic cigarette). In FIG. 24H, the electronic cigarette 7500 is composed of an atomizer 7501 including a heating element, a secondary battery 7504 that supplies power to the atomizer, and a cartridge 7502 including a liquid supply bottle, a sensor, and the like. To enhance safety, a protection circuit that prevents overcharging and overdischarging of the secondary battery 7504 may be electrically connected to the secondary battery 7504. The secondary battery 7504 shown in FIG. 24H has an external terminal so that it can be connected to a charging device. Since the secondary battery 7504 is the tip part when held, it is desirable that the total length is short and the weight is light. Since the secondary battery of one embodiment of the present invention has a high capacity and good cycle characteristics, a small and lightweight electronic cigarette 7500 that can be used for a long period of time can be provided.
[0408] Next, an example of a tablet terminal that can be folded in two is shown in Fig. 25A and Fig. 25B. The tablet terminal 9600 shown in Fig. 25A and Fig. 25B has a housing 9630a, a housing 9630b, a movable part 9640 that connects the housings 9630a and 9630b, a display part 9631 having a display part 9631a and a display part 9631b, switches 9625 to 9627, a fastener 9629, and an operation switch 9628. By using a flexible panel for the display part 9631, a tablet terminal having a wider display part can be obtained. Fig. 25A shows the tablet terminal 9600 in an open state, and Fig. 25B shows the tablet terminal 9600 in a closed state.
[0409] The tablet terminal 9600 also includes a power storage unit 9635 inside the housing 9630a and the housing 9630b. The power storage unit 9635 passes through the movable portion 9640 and is provided across the housings 9630a and 9630b.
[0410] The entire or part of the display portion 9631 can be a touch panel area, and data can be input by touching an image including an icon, text, an input form, etc. displayed in the area. For example, keyboard buttons may be displayed on the entire surface of the display portion 9631a on the housing 9630a side, and information such as text and images may be displayed on the display portion 9631b on the housing 9630b side.
[0411] A keyboard may be displayed on the display portion 9631b of the housing 9630b, and information such as text and images may be displayed on the display portion 9631a of the housing 9630a. A keyboard display switching button of a touch panel may be displayed on the display portion 9631, and a keyboard may be displayed on the display portion 9631 by touching the button with a finger, a stylus, or the like.
[0412] In addition, a touch input can be simultaneously made to the touch panel area of the display portion 9631a on the housing 9630a side and the touch panel area of the display portion 9631b on the housing 9630b side.
[0413] The switches 9625 to 9627 may be interfaces capable of switching various functions in addition to interfaces for operating the tablet terminal 9600. For example, at least one of the switches 9625 to 9627 may function as a switch for switching on and off the power of the tablet terminal 9600. For example, at least one of the switches 9625 to 9627 may have a function for switching the display orientation, such as portrait or landscape, or a function for switching between black and white or color display. For example, at least one of the switches 9625 to 9627 may have a function for adjusting the brightness of the display unit 9631. The brightness of the display unit 9631 can be optimized according to the amount of external light during use detected by an optical sensor built into the tablet terminal 9600. Note that the tablet terminal may have built-in not only an optical sensor but also other detection devices such as a gyro, an acceleration sensor, or the like for detecting tilt.
[0414] 25A shows an example in which the display area of the display portion 9631a on the housing 9630a side and the display portion 9631b on the housing 9630b side are substantially the same, but the display areas of the display portions 9631a and 9631b are not particularly limited, and one may have a different size from the other, and the display quality may also be different. For example, one may be a display panel that can display with higher resolution than the other.
[0415] 25B shows a tablet terminal 9600 folded in half, and the tablet terminal 9600 includes a housing 9630, a solar cell 9633, and a charge / discharge control circuit 9634 including a DC-DC converter 9636. In addition, a power storage unit according to one embodiment of the present invention is used as a power storage unit 9635.
[0416] As described above, the tablet terminal 9600 can be folded in two, and therefore the housing 9630a and the housing 9630b can be folded so as to overlap each other when not in use. By folding, the display portion 9631 can be protected, and therefore durability of the tablet terminal 9600 can be improved. Furthermore, the power storage unit 9635 using the secondary battery of one embodiment of the present invention has a high capacity and favorable cycle characteristics, and therefore the tablet terminal 9600 that can be used for a long period of time can be provided.
[0417] In addition, the tablet terminal 9600 shown in Figures 25A and 25B can have a function to display various information (still images, videos, text images, etc.), a function to display a calendar, date or time on the display unit, a touch input function to perform touch input operations or edit information displayed on the display unit, and a function to control processing using various software (programs), etc.
[0418] A solar cell 9633 attached to the surface of the tablet terminal 9600 can supply power to a touch panel, a display unit, a video signal processor, or the like. The solar cell 9633 can be provided on one or both sides of the housing 9630, and can be configured to efficiently charge the power storage unit 9635. The use of a lithium ion battery as the power storage unit 9635 has the advantage of enabling miniaturization.
[0419] The configuration and operation of the charge / discharge control circuit 9634 shown in Fig. 25B are described with reference to a block diagram in Fig. 25C. Fig. 25C shows a solar cell 9633, a power storage unit 9635, a DCDC converter 9636, a converter 9637, switches SW1 to SW3, and a display unit 9631. The power storage unit 9635, the DCDC converter 9636, the converter 9637, and the switches SW1 to SW3 correspond to the charge / discharge control circuit 9634 shown in Fig. 25B.
[0420] First, an example of operation in the case where power is generated by the solar cell 9633 using external light will be described. The power generated by the solar cell is stepped up or stepped down by a DC-DC converter 9636 to a voltage for charging a power storage unit 9635. When power from the solar cell 9633 is used for the operation of the display unit 9631, a switch SW1 is turned on, and the converter 9637 steps up or steps down the voltage to a voltage required for the display unit 9631. When no display is to be performed on the display unit 9631, SW1 is turned off and SW2 is turned on to charge the power storage unit 9635.
[0421] Note that the solar cell 9633 is shown as an example of a power generating means, but is not particularly limited thereto, and may be configured to charge the power storage unit 9635 using other power generating means such as a piezoelectric element (piezo element) or a thermoelectric conversion element (Peltier element). For example, a non-contact power transmission module that transmits and receives power wirelessly (non-contact) for charging, or a combination with other charging means may be used.
[0422] FIG. 26 illustrates an example of another electronic device. In FIG. 26, a display device 8000 is an example of an electronic device using a secondary battery 8004 according to one embodiment of the present invention. Specifically, the display device 8000 corresponds to a display device for receiving a TV broadcast and includes a housing 8001, a display unit 8002, a speaker unit 8003, a secondary battery 8004, and the like. The secondary battery 8004 according to one embodiment of the present invention is provided inside the housing 8001. The display device 8000 can receive power from a commercial power source, and can also use power stored in the secondary battery 8004. Thus, even when power cannot be supplied from a commercial power source due to a power outage or the like, the display device 8000 can be used by using the secondary battery 8004 according to one embodiment of the present invention as an uninterruptible power source.
[0423] The display unit 8002 can be a liquid crystal display device, a light-emitting device having a light-emitting element such as an organic EL element in each pixel, an electrophoretic display device, a semiconductor display device such as a DMD (Digital Micromirror Device), a PDP (Plasma Display Panel), or an FED (Field Emission Display).
[0424] The display device includes all display devices for displaying information, such as display devices for receiving TV broadcasts, display devices for personal computers, display devices for advertisements, and the like.
[0425] 26, a stationary lighting device 8100 is an example of an electronic device using a secondary battery 8103 according to one embodiment of the present invention. Specifically, the lighting device 8100 includes a housing 8101, a light source 8102, a secondary battery 8103, and the like. FIG. 26 illustrates an example in which the secondary battery 8103 is provided inside a ceiling 8104 on which the housing 8101 and the light source 8102 are provided, but the secondary battery 8103 may be provided inside the housing 8101. The lighting device 8100 can receive power from a commercial power source or can use power stored in the secondary battery 8103. Thus, even when power cannot be supplied from a commercial power source due to a power outage or the like, the lighting device 8100 can be used by using the secondary battery 8103 according to one embodiment of the present invention as an uninterruptible power source.
[0426] Note that although Figure 26 shows an example of a stationary lighting device 8100 provided on a ceiling 8104, the secondary battery of one embodiment of the present invention can also be used in a stationary lighting device provided on a surface other than the ceiling 8104, such as a side wall 8105, a floor 8106, or a window 8107, or can also be used in a tabletop lighting device.
[0427] An artificial light source that artificially obtains light using electric power can be used as the light source 8102. Specifically, examples of the artificial light source include discharge lamps such as incandescent lamps and fluorescent lamps, and light-emitting elements such as LEDs and organic EL elements.
[0428] 26, an air conditioner including an indoor unit 8200 and an outdoor unit 8204 is an example of an electronic device using a secondary battery 8203 according to one embodiment of the present invention. Specifically, the indoor unit 8200 includes a housing 8201, an air outlet 8202, a secondary battery 8203, and the like. FIG. 26 illustrates an example in which the secondary battery 8203 is provided in the indoor unit 8200, but the secondary battery 8203 may be provided in the outdoor unit 8204. Alternatively, the secondary battery 8203 may be provided in both the indoor unit 8200 and the outdoor unit 8204. The air conditioner can receive power from a commercial power source or can use power stored in the secondary battery 8203. In particular, when a secondary battery 8203 is provided in both the indoor unit 8200 and the outdoor unit 8204, even when power cannot be supplied from a commercial power source due to a power outage or the like, the air conditioner can be used by using the secondary battery 8203 of one embodiment of the present invention as an uninterruptible power source.
[0429] Note that although FIG. 26 illustrates an example of a separate-type air conditioner including an indoor unit and an outdoor unit, a secondary battery according to one embodiment of the present invention can also be used in an integrated air conditioner that has the functions of an indoor unit and an outdoor unit in a single housing.
[0430] 26 , an electric refrigerator-freezer 8300 is an example of an electronic device using a secondary battery 8304 according to one embodiment of the present invention. Specifically, the electric refrigerator-freezer 8300 includes a housing 8301, a refrigerator door 8302, a freezer door 8303, a secondary battery 8304, and the like. In FIG. 26 , the secondary battery 8304 is provided inside the housing 8301. The electric refrigerator-freezer 8300 can receive power from a commercial power source or can use power stored in the secondary battery 8304. Thus, even when power cannot be supplied from the commercial power source due to a power outage or the like, the electric refrigerator-freezer 8300 can be used by using the secondary battery 8304 according to one embodiment of the present invention as an uninterruptible power source.
[0431] Among the electronic devices described above, electronic devices such as high-frequency heating devices such as microwave ovens and electric rice cookers require a large amount of power for a short period of time. Therefore, by using a secondary battery according to one embodiment of the present invention as an auxiliary power source for supplementing the power that cannot be supplied by the commercial power source, it is possible to prevent the breaker of the commercial power source from tripping when the electronic device is in use.
[0432] Also, by storing power in the secondary battery during time periods when electronic devices are not used, particularly during time periods when the ratio of the amount of power actually used to the total amount of power that can be supplied by the commercial power source (called the power usage rate) is low, it is possible to prevent the power usage rate from increasing outside of the above time periods. For example, in the case of an electric refrigerator-freezer 8300, power is stored in the secondary battery 8304 during the night when the temperature is low and the refrigerator door 8302 and the freezer door 8303 are not opened or closed. Then, during the daytime when the temperature is high and the refrigerator door 8302 and the freezer door 8303 are opened and closed, the secondary battery 8304 is used as an auxiliary power source, thereby making it possible to keep the daytime power usage rate low.
[0433] According to one embodiment of the present invention, the cycle characteristics of the secondary battery are improved, and the reliability can be improved. According to one embodiment of the present invention, a high-capacity secondary battery can be obtained, and therefore the characteristics of the secondary battery can be improved, and therefore the secondary battery itself can be made smaller and lighter. Therefore, by mounting the secondary battery according to one embodiment of the present invention in the electronic device described in this embodiment, the electronic device can have a longer life and be lighter.
[0434] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0435] (Embodiment 7) In this embodiment, an example in which a secondary battery according to one embodiment of the present invention is mounted on a vehicle will be described.
[0436] By installing a secondary battery in a vehicle, next-generation clean energy vehicles such as hybrid electric vehicles (HEV), electric vehicles (EV), and plug-in hybrid electric vehicles (PHEV) can be realized.
[0437] FIG. 27 illustrates a vehicle using a secondary battery according to one embodiment of the present invention. An automobile 8400 illustrated in FIG. 27A is an electric automobile using an electric motor as a power source for running. Alternatively, it is a hybrid automobile that can appropriately select and use an electric motor and an engine as a power source for running. By using one embodiment of the present invention, a vehicle with a long cruising distance can be realized. The automobile 8400 also includes a secondary battery. The secondary battery may be used by arranging modules of the secondary battery illustrated in FIG. 12C and FIG. 12D on the floor of the vehicle. Alternatively, a battery pack in which a plurality of secondary batteries illustrated in FIG. 15 are combined may be installed on the floor of the vehicle. The secondary battery not only drives the electric motor 8406 but also supplies power to a light-emitting device such as a headlight 8401 or a room light (not shown).
[0438] The secondary battery can also supply power to display devices such as a speedometer and a tachometer included in the automobile 8400. The secondary battery can also supply power to semiconductor devices such as a navigation system included in the automobile 8400.
[0439] The automobile 8500 shown in FIG. 27B can charge the secondary battery of the automobile 8500 by receiving power supply from an external charging facility by a plug-in method, a non-contact power supply method, or the like. FIG. 27B shows a state in which a secondary battery 8024 mounted on the automobile 8500 is being charged from a ground-mounted charging device 8021 via a cable 8022. When charging, the charging method and connector standards may be appropriately performed by a predetermined method such as CHAdeMO (registered trademark) or Combo. The charging device 8021 may be a charging station installed in a commercial facility, or may be a home power source. For example, the secondary battery 8024 mounted on the automobile 8500 can be charged by an external power supply using plug-in technology. Charging can be performed by converting AC power to DC power via a conversion device such as an ACDC converter.
[0440] Although not shown, a power receiving device may be mounted on a vehicle, and charging may be performed by supplying power contactlessly from a ground power transmitting device. In the case of this contactless power supply method, by incorporating a power transmitting device in a road or an exterior wall, charging may be performed not only while the vehicle is stopped but also while the vehicle is moving. This contactless power supply method may also be used to transmit and receive power between vehicles. Furthermore, a solar cell may be provided on the exterior of the vehicle, and a secondary battery may be charged while the vehicle is stopped or moving. For such contactless power supply, an electromagnetic induction method or a magnetic field resonance method may be used.
[0441] 27C is an example of a two-wheeled vehicle using the secondary battery of one embodiment of the present invention. A scooter 8600 shown in FIG. 27C includes a secondary battery 8602, a side mirror 8601, and a turn signal light 8603. The secondary battery 8602 can supply electricity to the turn signal light 8603.
[0442] 27C, the secondary battery 8602 can be stored in the under-seat storage 8604. Even if the under-seat storage 8604 is small, the secondary battery 8602 can be stored in the under-seat storage 8604. The secondary battery 8602 is removable, and when charging, the secondary battery 8602 can be carried indoors, charged, and stored before riding.
[0443] According to one aspect of the present invention, the cycle characteristics of the secondary battery are improved, and the capacity of the secondary battery can be increased. Therefore, the secondary battery itself can be made small and lightweight. If the secondary battery itself can be made small and lightweight, it contributes to reducing the weight of the vehicle, and the cruising distance can be improved. In addition, the secondary battery mounted on the vehicle can be used as a power supply source other than the vehicle. In this case, for example, it is possible to avoid using a commercial power source during peak power demand. If it is possible to avoid using a commercial power source during peak power demand, it is possible to contribute to energy conservation and reduction of carbon dioxide emissions. In addition, if the cycle characteristics are good, the secondary battery can be used for a long period of time, and the amount of rare metals used, including cobalt, can be reduced.
[0444] This embodiment mode can be implemented in appropriate combination with other embodiment modes. [Explanation of symbols]
[0445] 100: Positive electrode active material
Claims
1. a positive electrode active material having lithium, cobalt, and an element X; It has a region represented by a layered rock salt structure, The region is represented by the space group R-3m; The element X is LiCoO 2 The stabilization energy when the lithium site is substituted is subtracted from the stabilization energy before substitution, and ΔE3 is 2 is one or more elements selected from the group consisting of elements having properties smaller than ΔE4, which is the value obtained by subtracting the stabilization energy before substitution from the stabilization energy when substituted at the cobalt position of The ΔE3 and ΔE4 are calculated by first-principles calculation, In the first-principles calculation, the LiCoO 2 A positive electrode active material having a layered rock salt structure, a space group represented by R-3m, and ΔE3 of 2.5 eV or less.
2. In claim 1, The positive electrode active material contains at least one element X selected from calcium, copper, magnesium, and zirconium.
3. In claim 1 or 2, A secondary battery using the positive electrode active material in a positive electrode and lithium metal in a negative electrode is charged at a constant current until the battery voltage reaches 4.6 V in an environment of 25° C., and then charged at a constant voltage until the current value reaches 0.01 C. When the positive electrode is analyzed by powder X-ray diffraction using CuKα1 radiation, the positive electrode active material has diffraction peaks at 2θ = 19.30 ± 0.20° and 2θ = 45.55 ± 0.10°.
Citation Information
Patent Citations
Positive active material, manufacture of same and nonaqueous solvent secondary battery using same
JP1997017430A
Layered oxide electrode material and its manufacturing method and battery using the same
JP2003151549A
Positive electrode active material particle and manufacturing method of positive electrode active material particle
JP2018088407A
Method for manufacturing positive electrode active material
JP2019179758A
Positive electrode active material for lithium secondary battery and method for manufacturing the same