Light-emitting device

JP2024144706AInactive Publication Date: 2024-10-11SEMICON ENERGY LAB CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024128711
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2009-07-02
Filing Date
2024-08-05
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Flexible light-emitting devices face challenges in longevity due to moisture intrusion from substrates like plastic and metal, which can lead to rapid degradation, and existing sealing methods are inadequate to prevent this issue.

Method used

A light-emitting device structure is developed with a flexible, transparent substrate and multiple insulating layers that sandwich a light-emitting element, sealed by a metal substrate, ensuring minimal water and oxygen permeability, and optionally incorporating a desiccant to further protect the element.

Benefits of technology

The solution provides a highly reliable and flexible light-emitting device with extended lifespan by effectively preventing moisture and oxygen ingress, allowing for curved surface applications and reduced thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144706000001_ABST
    Figure 2024144706000001_ABST
Patent Text Reader

Abstract

To easily provide a high-reliability and flexible light-emitting device and to provide an electronic apparatus or a lighting apparatus in which the light-emitting device is mounted.SOLUTION: A light-emitting device has a structure in which an element part including a light-emitting element is held between a substrate having flexibility and light transmissivity with respect to visible light and a metal substrate and further, insulation layers provided at upper and lower sides of the element part in an outer peripheral part of the element part contact each other, thereby sealing the element part. Thus, a high-reliability light-emitting device is provided. Further, a light-emitting device of such a configuration is mounted in an electronic apparatus or a lighting apparatus, thereby providing a high-reliability electronic apparatus or lighting apparatus.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to electroluminescence (EL) The present invention also relates to a light-emitting device having a light-emitting element using the light-emitting device. The present invention relates to a lighting device or an electronic device having the light-emitting device mounted on a display unit. [Background technology]

[0002] In recent years, the light-emitting devices mounted on displays of televisions, mobile phones, digital cameras, etc., and lighting devices have become There is a demand for flat and thin light-emitting devices, and As a light-emitting device, a light-emitting device using a self-luminous light-emitting element has been attracting attention. One type of optical element is a light-emitting element that uses electroluminescence. The device sandwiches a light-emitting material between a pair of electrodes, and emits light from the light-emitting material by applying a voltage. Such a self-luminous light-emitting element can be thin-filmed. One of its features is its fast response speed.

[0003] The next phase in this field will be the commercialization of flexible light-emitting devices that can reproduce curved surfaces. Commercialization of such a device has been attracting attention, and various proposals have been made (see, for example, Patent Document 1). A light-emitting device using a flexible support substrate is a device that uses a glass substrate or the like as a support substrate. It can be made extremely light in weight compared to

[0004] However, the biggest hurdle in putting such flexible light-emitting devices to practical use is their lifespan. This is because in a flexible light-emitting device, the light-emitting element is supported and the device is also exposed to the outside world. As a supporting substrate to protect the element from moisture and oxygen, a flexible but water-permeable substrate is required. This is due to the need to use plastic substrates, which are expensive and have poor heat resistance. Since the heat resistance of the stick substrate is low, it is not possible to create a high-quality protective film by applying high temperatures. First of all, the intrusion of moisture from the side using the plastic substrate can shorten the life of the light emitting element and ultimately the light emitting device. It will have a huge negative impact.

[0005] For example, in Non-Patent Document 1, a light-emitting device was fabricated on a polyethersulfone (PES)-based substrate. A flexible light-emitting device was created by producing an element and sealing it with an aluminum film. However, its life span is only about 230 hours, which is far from practical use. Patent Document 2 and Non-Patent Document 3 describe flexible LEDs with light-emitting elements fabricated on stainless steel substrates. An example of a light-emitting device is introduced, but the intrusion of moisture from the stainless steel substrate side is suppressed. However, it is not possible to effectively prevent moisture from entering from the light emitting element side. By applying a sealing film made of multiple layers of materials repeatedly laminated on the element, the lifespan is extended. Trying to improve.

[0006] In addition, a thin metal film such as aluminum or a stainless steel substrate has low flexibility and water permeability. However, it does not transmit visible light at normal thickness, so it is not suitable for use in light-emitting devices. In this case, the use of the light-emitting element is limited to only one of the pair of substrates that sandwich the light-emitting element. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2003-204049 A [Non-patent literature]

[0008] [Non-Patent Document 1] Gi Heon Kim et al., IDW'03, 2003, p.387-p.390 [Non-Patent Document 2] Dong Un Jin et al., SID 06 DIGEST, 2006, p.1855-p.1857 [Non-Patent Document 3] Anna Chwang et al., SID 06 DIGEST, 2006, p.1858-p.1861 Summary of the Invention [Problem to be solved by the invention]

[0009] In view of the above problems, one embodiment of the present invention provides a method for easily providing a highly reliable flexible light-emitting device. It is also an object of the present invention to provide an electronic device or a lighting device equipped with the light emitting device. One of the objectives is to provide. [Means for solving the problem]

[0010] The above problem is solved by forming an element portion including a light-emitting element on a substrate having flexibility and transparency to visible light. The element is sandwiched between the metal substrate and an insulating layer provided above and below the element at the outer periphery of the element. This can be achieved by a light emitting device having a structure in which the light emitting elements are sealed by contacting each other. .

[0011] That is, one embodiment of the present invention is a substrate having flexibility and a property of transmitting visible light, a first insulating layer provided on the first insulating layer; a light emitting element provided on the first insulating layer; An element portion having at least a switching element for applying a voltage to the side and upper surfaces of the element portion. a second insulating layer covering the substrate; and a metal substrate provided on the second insulating layer and facing the substrate. At least a part of the first insulating layer and the second insulating layer contact each other on the outer periphery of the element portion. It is a light emitting device.

[0012] Another embodiment of the present invention is a substrate having flexibility and a visible light-transmitting property, a first insulating layer provided on the first insulating layer, a light emitting element provided on the first insulating layer, and a light emitting element for applying a potential to the light emitting element. and a switching element for switching the light emitted from the light emitting element. A second insulating layer, a resin film provided on the second insulating layer, and a substrate and a resin film provided on the resin film. and a metal substrate facing each other, and a first insulating layer and a second insulating layer are formed at the outer periphery of the element portion. In the present invention, the light emitting devices are at least partially in contact with each other.

[0013] In the above configuration, a third insulating layer is provided on the surface of the substrate opposite to the surface facing the light emitting element. A layer may be provided.

[0014] Another embodiment of the present invention is a substrate having flexibility and a visible light-transmitting property, a first insulating layer provided on the first insulating layer, a light emitting element provided on the first insulating layer, and a light emitting element for applying a potential to the light emitting element. and a switching element for switching the light emitted from the light emitting element. a second insulating layer, a sealing material provided on the second insulating layer and surrounding the outer periphery of the element portion, and a substrate. and a metal substrate facing the element portion, and in a region surrounded by a sealing material on the outer periphery of the element portion, In the light emitting device, at least a portion of the first insulating layer and the second insulating layer are in contact with each other.

[0015] Another embodiment of the present invention is an electronic device or a lighting device equipped with a light-emitting device having the above structure. It is located.

[0016] In this specification, a light-emitting element is an element whose luminance is controlled by a current or a voltage. This category includes organic EL (Electro Luminescence) e) Elements, inorganic EL elements, etc.

[0017] The light emitting device disclosed in this specification may be of either a passive matrix type or an active matrix type. It may be of the trix type.

[0018] In this specification, the term "light-emitting device" refers to an image display device, a light-emitting device, or a light The panel also includes a connector, such as FPC (Flexible Printed Circuit). e printed circuit) or TAB (Tape Automated Bonding tape or TCP (Tape Carrier Package) ) is attached to the module, and a printed wiring board is attached to the end of the TAB tape or TCP. The module is mounted with the IC by COG (Chip On Glass) method. Modules in which an integrated circuit is directly mounted are also included in the light emitting device.

[0019] In addition, in this specification, ordinal numbers such as first and second are used for convenience. It does not indicate the order of steps or the order of layers. It does not indicate a specific name for the purpose of reference. Effect of the Invention

[0020] According to one embodiment of the present invention, a thin and highly reliable light-emitting device can be provided. Further, one embodiment of the present invention is a lighting device or a light-emitting device having high reliability, which is provided using the light-emitting device having high reliability. or electronic equipment. [Brief description of the drawings]

[0021] [Figure 1] 1A to 1C illustrate a light-emitting device according to one embodiment of the present invention. [Diagram 2] 1A to 1C illustrate a light-emitting device according to one embodiment of the present invention. [Diagram 3] 1A to 1C illustrate a manufacturing method of a light-emitting device according to one embodiment of the present invention. [Figure 4] 1A to 1C illustrate a manufacturing method of a light-emitting device according to one embodiment of the present invention. [Diagram 5] 1A to 1C illustrate a manufacturing method of a light-emitting device according to one embodiment of the present invention. [Figure 6] 1A to 1C are diagrams showing examples of the structure of a light-emitting element. [Figure 7] 1A to 1C illustrate examples of a structure of a light-emitting device according to one embodiment of the present invention. [Figure 8] 1A to 1C illustrate application examples of a light-emitting device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, the embodiment of the present invention will be described with reference to the drawings. It is to be understood that the invention can be practiced in various different ways without departing from the spirit and scope of the invention. It will be readily understood by those skilled in the art that various modifications may be made to the form and details of the present invention. However, it should not be construed as being limited to the description of this embodiment mode.

[0023] (Embodiment 1) In this embodiment, an example of a light emitting device will be described with reference to FIG. 1 shows the display section of the device.

[0024] The light emitting device of this embodiment shown in FIG. 1A includes a first insulating layer formed on a substrate 100. The element section 150 includes a second insulating layer 140 and an element section 150. The top and sides of the first insulating layer 104 and the second insulating layer 140 are covered with At the end of the light emitting device where the element portion 150 is not present, at least a part of the light emitting device is in contact with the element portion 150. The first insulating layer 104 and the second insulating layer 105 are disposed so as to surround the outer periphery of the element section 150. Preferably, the first insulating layer 104 and the second insulating layer 140 are in contact with each other. It is more preferable that the contact area contacts the outer periphery of the element section 150 twice. A metal substrate 144 is provided facing the substrate 100, and the metal substrate 144 and a second insulating A resin film 142 is provided between the edge layers 140 .

[0025] The substrate 100 may be a flexible substrate that is transparent to visible light. , such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN) Polyester resins, polyacrylonitrile resins, polyimide resins, polymethylmethacrylate resins, etc. Relate resin, polycarbonate resin (PC), polyethersulfone resin (PES) , polyamide resin, cycloolefin resin, polystyrene resin, polyamide-imide resin, Polyvinyl chloride resin or the like can be suitably used. A structure in which a fiber is impregnated with an organic resin can be used. However, it must be flexible and resistant to visible light. As long as the substrate is light-transmitting, it can be used as the substrate 100 without any particular limitation. do.

[0026] A first insulating layer 104 is formed on the substrate 100. The first insulating layer 104 serves as a protective layer. This function prevents moisture and gases such as oxygen from entering the element section 150. In addition, in the manufacturing process of the light emitting device, the semiconductor When separating the element part containing the element, it is necessary to prevent damage such as cracks in the semiconductor element and wiring. The first insulating layer 104 is formed of a material that has low water permeability and is light-transmitting. For example, materials containing nitrogen and silicon, such as silicon nitride, silicon nitride oxide, and silicon oxynitride, are preferred. The first insulating layer 104 may be a single layer or a multilayer. The thickness of the insulating layer 104 is preferably 10 nm or more and 1000 nm or less, more preferably 100 nm or more and 70 0 nm or less is preferable.

[0027] An element section 150 is formed on the first insulating layer 104. The element section 150 is a light-emitting element. 138 and a switching element for applying a potential to the light emitting element 138. The switching element is a transistor (e.g., a bipolar transistor, M OS transistors, etc.), diodes (e.g., PN diodes, PIN diodes, Schottky diode, MIM (Metal Insulator Metal) diode , MIS (Metal Insulator Semiconductor) diode A diode, a diode-connected transistor, a thyristor, etc. can be used. Alternatively, a logic circuit that combines these elements can be used as a switching element. In this embodiment, a thin film transistor 106 is used as the switching element. In addition, the light emitting device may be an integrated driver type, and the element section 150 may include a drive circuit section. Alternatively, a driving circuit can be formed outside the sealed substrate.

[0028] The light-emitting element 138 includes a first electrode 130 that functions as a pixel electrode, and a light-emitting element 138 that covers the edge of the first electrode. The first electrode 130 and the second electrode 136 are disposed on the first electrode 130. One of the second electrodes 136 is used as an anode, and the other is used as a cathode.

[0029] The EL layer 134 constituting the light-emitting element has at least a light-emitting layer. In addition to the light-emitting layer, the device has functional layers such as a hole injection layer, a hole transport layer, an electron transport layer, and an electron injection layer. The EL layer 134 may have a laminated structure including a low molecular weight material and a high molecular weight material. The EL layer 134 may be made of an organic compound material. This includes not only those consisting only of inorganic compounds, but also those containing inorganic compounds.

[0030] The upper surface and side surfaces of the element section 150 including the light emitting element 138 are covered with a second insulating layer 140. The first insulating layer and the second insulating layer are formed in the same manner as in the case of a light-emitting device without the element section 150. At the end portions, at least a portion of the electrodes contact each other to seal the element portion 150 .

[0031] The second insulating layer 140 functions as a protective layer to prevent moisture and gases such as oxygen from entering the element section 150. The second insulating layer 140 is made of a material that has low water permeability and is light-transmitting. For example, materials containing nitrogen and silicon, such as silicon nitride, silicon oxynitride, and silicon oxynitride, are used. The second insulating layer 14 is preferably made of a material such as aluminum oxide. The second insulating layer 140 may be a single layer or a multilayer. m or less, and more preferably 100 nm or more and 700 nm or less.

[0032] 1A, a resin film 142 is formed on a second insulating layer 140. Examples of the material 142 include acrylic resin, polyimide resin, melamine resin, and polyester resin. Grease, polycarbonate resin, phenolic resin, epoxy resin, polyacetal, polyether Polyurethane, polyamide (nylon), furan resin, diallyl phthalate resin, etc. The starting materials are organic compounds such as silica glass and siloxane polymer materials. Inorganic siloxanes that contain Si-O-Si bonds are compounds made of silicon, oxygen, and hydrogen. silane polymer, alkylsiloxane polymer, alkylsilsesquioxane polymer, Representative examples include hydrogenated silsesquioxane polymers and hydrogenated alkylsilsesquioxane polymers. In organic compounds, the hydrogen bonded to the silicon atom is replaced by an organic group such as methyl or phenyl. A siloxane polymer or the like can be used. Alternatively, an organic Resin-impregnated structures may also be used.

[0033] A metal substrate 144 is provided on the resin film 142 so as to face the substrate 100. In order to obtain flexibility, the thickness of the film 144 is 10 μm or more and 200 μm or less. The material for the metal substrate 144 is not particularly limited, but may be aluminum, copper, nickel, etc. Alternatively, an alloy of a metal such as an aluminum alloy or stainless steel is preferably used. The metal substrate 144 has a sufficiently low water permeability and a sufficient flexibility. Since the light-emitting device in this embodiment does not have a light-transmitting property with a thickness of 100 nm, The light emitted from the substrate 100 side on which the film transistor layer is provided is called bottom emission. This results in a light-emitting device of the ion type.

[0034] A desiccant may be provided between the resin film 142 and the metal substrate 144. This can better prevent the light-emitting element from being deteriorated due to moisture. Moisture is absorbed by chemical adsorption, such as by alkaline earth metal oxides, such as calcium and barium oxide. Other drying agents include zeolite and silica. A substance that adsorbs moisture by physical adsorption, such as gel, may also be used.

[0035] The light emitting device of the present embodiment shown in FIG. 1 can be curved. The light-emitting device of various shapes can be attached to various substrates, and when attached to a substrate having a curved surface, This makes it possible to realize electronic devices such as displays having curved surfaces, or lighting devices having curved surfaces.

[0036] In the light emitting device of this embodiment, the upper and side surfaces of the element section 150 are formed of a film with low water permeability. The second insulating layer 140 is formed on the element portion 15. Since the first insulating layer 104 contacts the end of the element portion 150 and seals the element portion 150, It is possible to prevent moisture and gases such as oxygen from entering the insulating film 150. A highly reliable light emitting device in which deterioration caused by gas is suppressed can be obtained.

[0037] In addition, a light-emitting device according to the present embodiment having a different structure from that shown in FIG. 1(A) is shown in FIG. The light-emitting device of this embodiment shown in FIG. 1B has the same structure as the light-emitting device shown in FIG. In the structure, the third insulating layer 152 is provided on the outer side of the substrate 100 (the side opposite to the light emitting element 138). It is.

[0038] In the light-emitting device shown in FIG. 1B, the third insulating layer 152 is provided, so that the light-emitting device can be It is possible to more effectively prevent the intrusion of moisture and gases such as oxygen. This makes it possible to protect the surface of the substrate 100, which is a soft substrate, from scratches, pressure, and the like.

[0039] The third insulating layer 152 is formed by bonding the metal substrate 144 and then depositing the metal substrate 144 by sputtering or plasma. It is formed in a single layer or multiple layers using inorganic compounds by a method such as CVD, coating, or printing. The third insulating layer 152 is preferably a film having transparency to visible light and high hardness. For example, a film containing nitrogen and silicon, such as a silicon nitride film or a silicon oxynitride film, is preferred. The thickness of the third insulating layer 152 is 10 nm or more and 1000 nm or less, and In addition, the thickness of the metal substrate 144 is preferably 100 nm or more and 700 nm or less. By subsequently forming the third insulating layer 152, the light emitting element is not exposed to the atmosphere, and deterioration of the light emitting element is prevented. This can be prevented.

[0040] In addition, the light emitting device of this embodiment having a configuration different from that shown in FIG. 1(A) or (B) may be The location is shown in Figure 1(C).

[0041] The light emitting device of this embodiment shown in FIG. 1C is a light emitting device having an element portion in the light emitting device shown in FIG. Instead of the resin film 142 covering the element 150, a sealant is provided on the second insulating layer 140 to surround the outer periphery of the element portion. In FIG. 1C, the sealing material 156 is provided to bond the metal substrate 144. 56 includes thermosetting epoxy resin, UV-curing acrylic resin, and thermoplastic nylon. It can be formed by using a dispenser method, a printing method, a thermocompression method, etc. A desiccant may be provided in the area surrounded by the sealing material.

[0042] The light emitting device shown in FIG. 1C has an insulating film 1 on the surface of the metal substrate 144 facing the element section 150. The insulating film 154 is formed by a method such as a CVD method, a sputtering method, a SOG method, or a droplet discharge method. , inorganic materials such as silicon oxide and silicon nitride, polyimide, Polyamide, benzocyclobutene, acrylic, epoxy and other organic materials, siloxane materials, etc. It is possible to form the insulating film as a single layer or a multilayer film.

[0043] By providing the insulating film 154, the adhesion with the sealant 156 is improved, so that the light emitting device It is possible to more effectively prevent the intrusion of moisture and gases such as oxygen. When the insulating film 154 is provided, the surface of the metal substrate 144 is etched, and then the insulating film 1 It is preferable to form 54.

[0044] In FIG. 1C, two pairs of grooves (a first groove 160a and a second groove 160b) are provided at the end of the element section 150. A groove portion 160b) is provided, and in each groove portion, the first insulating layer 104 and the second insulating layer The layer 140 is in contact with the first groove portion 160a and the second groove portion 160b, and seals the element portion 150. The grooves 160b are preferably formed so as to surround the outer periphery of each element portion 150. As shown in FIG. 1(C), two pairs of grooves are provided at the end of the element section 150, so that the light emitting device can be bent. Since it is possible to reduce the stress applied to the element section 150 when the element section 150 is bent, the element section 150 is more resistant to bending. It is possible to provide a light emitting device having a high light emitting property.

[0045] The configurations shown in FIGS. 1(A) to 1(C) can be used in combination. be.

[0046] 1A to 1C, the element portion 150 may include a driver circuit portion. Although only one light emitting element 138 is shown in FIGS. 1A to 1C, When the light emitting device of the present embodiment is used for a display purpose, a plurality of light emitting devices are used. A pixel portion having the element 138 is formed. In addition, when a full-color image is displayed, It is necessary to obtain at least three colors of light: red, green, and blue. A method of painting the necessary parts of the L layer 134, a method of making all light-emitting elements emit white light, A method of obtaining each color by transmitting light through a filter layer, making all light-emitting elements blue or There is also a method of emitting light with a shorter wavelength and obtaining each color through a color conversion layer.

[0047] FIG. 2(A) to (D) show an example of a method for installing a color filter layer or a color conversion layer. In FIG. 2(A) to (D), 200 is a color filter layer (if The color filter layer 200 (or color conversion layer) is a light emitting element 138. The color filter layers of adjacent colors are provided for the light emitting element 13. In the area other than the opening area 8 (the area where the first electrode, the EL layer, and the second electrode are directly overlapped), The color filter layer 200 may be formed only in the pixel portion 250. Alternatively, the driving circuit section 252 may be formed. It may be formed outside the light emitting device.

[0048] FIG. 2A shows a state where a wiring 204 for a thin film transistor is formed on a first interlayer insulating film 206. A color filter layer 200 is formed on the color filter layer 200, and a second interlayer insulating film is formed on the color filter layer 200. This is an example of what has been achieved.

[0049] The second interlayer insulating film is made of, for example, polyimide, polyamide, benzocyclobutene, or acrylic. The insulating material may be an organic material such as epoxy, or an inorganic material such as silicon oxide or silicon nitride. For example, as shown in FIG. 2(A), A planarization film 208 was formed using an organic insulating material to flatten the steps caused by the color filters. Then, a barrier film 210 made of an inorganic insulating material is laminated on the planarizing film 208 to form a second By providing the barrier film 210, the color filter Preventing gas generated from layer 200 (or the color conversion layer) from affecting the light emitting element The second interlayer insulating film is preferably made of an organic insulating material and an inorganic insulating material. Multiple layers may be laminated one on top of the other.

[0050] In FIG. 2A, after the second interlayer insulating film is formed, a contact hole is formed in the flattening film 208. Then, an electrode 212 is formed to connect the first electrode 130 of the light-emitting element to the wiring 204. A first electrode 130 of the optical element is provided.

[0051] Note that only one color filter (or color conversion layer) is shown in FIGS. 2(A) to 2(D). However, in the light-emitting device, red, blue and green color filters (or color conversion layers) are used. The color filters (or color conversion layers) are arranged in a predetermined arrangement and shape. There are various patterns, such as stripe arrangement, diagonal mosaic arrangement, and triangular mosaic arrangement. In addition, when using white light emitting elements and color filters, RGB The RGBW4 pixel array is a three-color filter consisting of red, blue, and green. The pixel arrangement has pixels with color filters and pixels without color filters, This is effective in reducing power consumption. In addition, the white light emitting element contains red, blue and green light, for example. NTSC (National Television Standards Com It is preferable that the configuration includes red, blue and green lights as defined by the MITTEE.

[0052] The color filter can be formed using known materials. In the case of using a photosensitive resin, the color filter itself may be exposed to light and developed to form the color filter. However, because the pattern is very fine, it is possible to form the pattern by dry etching. preferable.

[0053] FIG. 2B shows a color filter layer 200 formed after forming a thin film transistor. This is an example in which a first interlayer insulating film 206 is formed on the filter layer 200. After the first interlayer insulating film 206 is formed, a contact hole is formed in the first interlayer insulating film 206. Then, a wiring 204 is formed, and then a first electrode 130 of the light-emitting element is formed to be connected to the wiring 204. Establish a system.

[0054] FIG. 2C shows a state in which a color filter substrate 214 on which a color filter layer 200 is provided is placed. The color filter layer 200 of the color filter substrate 214 is formed. When the surface of the color filter substrate 214 that is not covered by the color filter is attached to the substrate 100 using an adhesive, A coating film 216 may be provided to protect the color filter layer 200 from scratches. Although not shown, the color filter layer 200 of the color filter substrate 214 is formed. The color filter substrate 214 may be attached to the substrate 100 with the coated side facing the substrate 100. The substrate 100 may be made of any of a variety of substrates that are flexible and transparent to visible light, such as a material similar to that of the substrate 100. A color filter layer 200 is formed on the substrate.

[0055] FIG. 2D shows a color filter having a color filter layer 200 previously provided on a substrate 100. This is an example of a configuration in which the substrate 218 is directly bonded to the layer to be peeled off, which has been separated from the fabrication substrate. The color filter substrate 218, which is the substrate 100 on which the color filter layer 200 is provided, is By directly attaching it to the peeled layer having the electrodes, the number of parts is reduced and the manufacturing cost is reduced. Above, we have briefly explained how to install the color filter layer (or color conversion layer). However, in addition to this, a black matrix may be provided between each light-emitting element, or other public The structure of knowledge may be applied.

[0056] In addition, in FIG. 2(A) to FIG. 2(D), a color filter is added to the configuration of the light emitting device shown in FIG. The above description is based on the example of a configuration in which a filter layer is provided, but these configurations are similar to those shown in FIG. 1(B) or FIG. 1(C). The same can be applied to the light emitting device shown in FIG.

[0057] Note that the configuration of this embodiment mode can be used in appropriate combination with the configurations of other embodiments. It is possible.

[0058] (Embodiment 2) An example of a method for manufacturing the light-emitting device according to one embodiment of the present invention will be described with reference to FIGS. In this embodiment, a case of manufacturing a light emitting device shown in FIG. Reveal.

[0059] First, a peeling layer 302 is formed on a substrate 300 having an insulating surface, which is a substrate to be fabricated. The release layer 302 and the first insulating layer 104 are formed continuously. By forming the layers successively, the surface of the peeling layer 302 is not exposed to the air. In this way, impurities can be prevented from being mixed into the separation layer 302 and the first insulating layer 104 .

[0060] The substrate 300 to be fabricated may be a glass substrate, a quartz substrate, a sapphire substrate, a ceramic substrate, or the like. A metal substrate having an insulating layer formed on its surface can be used. A plastic substrate having heat resistance capable of withstanding the processing temperature of the semiconductor device may be used. In the manufacturing process, a manufacturing substrate can be appropriately selected depending on the process to be performed.

[0061] In this step, the peeling layer 302 is provided on the entire surface of the substrate 300. After providing a release layer 302 on the entire surface of the substrate 300 in accordance with the above, the release layer 302 is selectively removed. Alternatively, the release layer may be provided only in a desired area. A layer 302 is formed, but if necessary, a silicon oxide film or an oxide film may be formed in contact with the substrate 300. An insulating layer such as a silicon nitride film, a silicon nitride film, or a silicon oxynitride film is formed, and a A release layer 302 may be formed on the insulating film 302 .

[0062] The peeling layer 302 is formed by sputtering, plasma CVD, coating, printing, or the like. W, Molybdenum (Mo), Titanium (Ti), Tantalum (Ta), Niobium (N b), Nickel (Ni), Cobalt (Co), Zirconium (Zr), Zinc (Zn), Ru Ruthenium (Ru), Rhodium (Rh), Palladium (Pd), Osmium (Os), Iridium (Ir) an element selected from the group consisting of iridium (Ir) and silicon (Si), or an alloy material mainly composed of such an element; Alternatively, a layer made of a compound material containing the above element as a main component is formed as a single layer or a laminated layer. The crystal structure of the layer containing may be any of amorphous, microcrystalline, and polycrystalline. The coating method includes a spin coating method, a dispensing method, and the like.

[0063] When the release layer 302 has a single-layer structure, it is preferably a tungsten layer, a molybdenum layer, or a tungsten layer. A layer containing a mixture of tungsten and molybdenum is formed. Alternatively, a layer containing tungsten oxide or a layer containing an oxynitride, a layer containing an oxide or oxynitride of molybdenum, or a layer containing tungsten A layer containing an oxide or oxynitride of a mixture of tungsten and molybdenum is formed. A mixture of tungsten and molybdenum corresponds, for example, to an alloy of tungsten and molybdenum. do.

[0064] When the peeling layer 302 has a laminated structure, it is preferable that the first layer is a tungsten layer, the second layer is a molybdenum layer, and the third layer is a tungsten layer. A layer containing tungsten or a layer containing a mixture of tungsten and molybdenum is formed, and a second layer containing tungsten Oxides, nitrides, and oxynitrides of tungsten, molybdenum, or mixtures of tungsten and molybdenum Or, a nitride oxide is formed.

[0065] The peeling layer 302 is a stacked structure of a layer containing tungsten and a layer containing an oxide of tungsten. In the case of forming a tungsten-containing layer, an insulating layer made of oxide is formed on the tungsten-containing layer. By forming a layer containing tungsten oxide at the interface between the tungsten layer and the insulating layer, Furthermore, the surface of the tungsten-containing layer may be thermally oxidized. Treatment with oxygen plasma, ozone water or other highly oxidizing solutions to remove tungsten. In addition, the plasma treatment or the heat treatment may be performed by using oxygen, nitrogen, or other organic compounds. The treatment may be carried out in an atmosphere of nitrous oxide alone or a mixture of the above gas with other gases. This can also be used to form layers containing tungsten nitride, oxynitride, and oxynitride. Similarly, after forming a layer containing tungsten, a silicon nitride layer, a silicon oxynitride layer, A silicon nitride oxide layer may be formed.

[0066] The first insulating layer 104 is an insulating material containing nitrogen and silicon, such as silicon nitride, silicon oxynitride, or silicon nitride oxide. It is preferable that the insulating film is formed as a single layer or multiple layers. The first insulating layer 104 is formed by sputtering. It can be formed by using methods such as ring method, plasma CVD method, coating method, printing method, etc. For example, by forming the film at a temperature of 250°C to 400°C using the plasma CVD method, The first insulating layer 104 can be made dense and has very low water permeability. The thickness is preferably 0 nm or more and 1000 nm or less, and more preferably 100 nm or more and 700 nm or less. By providing the insulating layer 104, peeling at the interface with the peeling layer 302 in the subsequent peeling step can be prevented. Furthermore, it is possible to prevent cracks and damage to the semiconductor elements and wiring during the subsequent peeling process. In addition, the first insulating layer 104 functions as a protective layer for the light emitting device to be manufactured. It works.

[0067] Next, a thin film transistor 106 is formed over the first insulating layer 104 (FIG. 3(A)). The thin film transistor 106 includes at least a source region, a drain region, and a channel forming region. The semiconductor layer 106a has a gate insulating layer 106b, and a gate electrode 106c. In order to stabilize the characteristics of the thin film transistor, the first insulating layer 104 and the semiconductor layer 10 An insulating base film may be formed between the first and second insulating layers 6a and 6b. The insulating base film may be made of silicon oxide, silicon nitride, or oxide. It is made of a single layer or multiple layers using inorganic insulating films such as silicon nitride and silicon oxynitride. It is possible.

[0068] The semiconductor layer 106a has a thickness of 10 nm or more and 100 nm or less, and further has a thickness of 20 nm or more and 70 nm or less. The non-single crystal semiconductor layer is a layer formed of a non-single crystal semiconductor. , amorphous semiconductor layers, microcrystalline semiconductor layers, etc. In particular, laser light irradiation and instantaneous thermal annealing are Heat treatment using RTA or furnace annealing, or a combination of these methods It is preferable to use a crystalline semiconductor crystallized by a method. We have developed a crystallization method using metallic elements such as nickel, which have the effect of promoting the crystallization of silicon semiconductors. can be applied.

[0069] The gate insulating layer 106b has a thickness of 5 nm to 200 nm, preferably 10 nm to 100 nm. It is formed of an inorganic insulator such as silicon oxide or silicon oxynitride having a thickness of less than 1 nm.

[0070] The gate electrode 106c is formed of a polycrystalline semiconductor doped with a metal or an impurity of one conductivity type. When metals are used, tungsten (W), molybdenum (Mo), titanium ( Examples of usable materials include Ti, tantalum (Ta), and aluminum (Al). Alternatively, the first metal nitride may be a metal nitride. The first layer may be a layer of metal nitride and the second layer of the metal may be laminated. By making the second layer metal into a gallium oxide, it can be used as a barrier metal. This prevents the semiconductor layer from diffusing into the insulating layer and the semiconductor layer below it. In this case, the end of the first layer may protrude outward beyond the end of the second layer.

[0071] The semiconductor layer 106a, the gate insulating layer 106b, the gate electrode 106c, etc. are combined. The thin film transistor 106 has a single drain structure and an LDD (lightly doped drain) structure. Various structures such as a gate overlap drain structure can be applied. The equivalent is that transistors with the same gate voltage are connected in series. a multi-gate structure in which the semiconductor layer is sandwiched between gate electrodes on the top and bottom; A thin film transistor formed with a Tom-gate structure or the like can be applied.

[0072] In addition, the thin film transistor 106 is a thin film transistor using a metal oxide or an organic semiconductor material for the semiconductor layer. A typical metal oxide is zinc oxide or zinc gallium. Examples include oxide of nium indium.

[0073] Next, the wiring 20 electrically connected to the source region and the drain region of the thin film transistor 106 is 4, and a first light-emitting element that functions as a pixel electrode electrically connected to the wiring 204 is formed. For example, a single layer or a multilayer may be formed to cover the thin film transistor 106. A first interlayer insulating film is formed, and a source electrode and a drain electrode are formed on the first interlayer insulating film. A functional wiring 204 is formed. In FIG. 3(A), the insulating layers 206a and 206b are A first interlayer insulating film 206 made of two layers is formed. Then, the wiring 204 is connected. A first electrode 130 is formed. Note that a second interlayer insulating film is formed on the wiring 204, and the first electrode 130 is formed on the wiring 204. A first electrode may be formed on the second interlayer insulating film.

[0074] The first interlayer insulating film 206 is formed by a method such as a CVD method, a sputtering method, a SOG method, a droplet discharge method, a screen method, or the like. By printing method, inorganic materials such as silicon oxide and silicon nitride, polyimide, polyamide, Single layer made of organic materials such as benzocyclobutene, acrylic, epoxy, etc. and siloxane materials. Alternatively, the insulating layer 206a may be formed of a laminated layer. For example, the insulating layer 206a may be formed of silicon nitride oxide. The second insulating layer 206b can be formed of a silicon oxynitride film.

[0075] The wiring 204 is a laminated structure of titanium (Ti) and aluminum (Al), molybdenum (Mo) A low-resistance material such as aluminum and titanium (Al) are used. Alternatively, it may be formed in combination with a barrier metal made of a high melting point metal material such as molybdenum. is preferred.

[0076] The first electrode 130 is an electrode used as an anode or a cathode of the light-emitting element. When using it as a semiconductor, it is desirable to use a material with a large work function. For example, indium Tin oxide film, indium tin oxide film containing silicon, indium oxide with 2 to 20 wt% A transparent film formed by sputtering using a target containing zinc oxide (ZnO) Conductive films that contain zinc oxide (ZnO), conductive oxynitride films that contain zinc and aluminum, and nitride In addition to single-layer films such as titanium oxide film, chromium film, tungsten film, Zn film, and Pt film, titanium nitride film a laminate of a titanium nitride film and a film mainly made of aluminum; A three-layer structure of a titanium nitride film and a titanium oxide film can be used. The wiring resistance is low and good ohmic contact can be achieved.

[0077] When used as a cathode, materials with a small work function (Al, Ag, Li, Ca, or These alloys (MgAg, MgIn, AlLi, CaF2, or calcium nitride) are used In addition, when the electrode used as the cathode is made to be light-transmitting, it is preferable that the thickness of the electrode is A thin metal film and a light-transmitting conductive film (indium tin oxide film, silicon-containing Indium tin oxide film, indium oxide mixed with 2-20wt% zinc oxide (ZnO) A transparent conductive film formed by sputtering using a target made of zinc oxide (Zn It is preferable to use a laminate with

[0078] Next, a partition wall 13 is formed using an organic material or an inorganic material so as to cover the edge of the first electrode 130. 7 is formed (FIG. 3(B)). For example, by using a positive type photosensitive polyimide, The partition wall 137 can be formed. The film formed on the partition wall 137 has good coverage. In order to achieve this, the upper end or the lower end is provided so as to form a curved surface having a curvature. The partition wall 137 is a negative type that is photosensitive and becomes insoluble in an etchant when exposed to light, or Any positive type that becomes soluble in the etchant when exposed to light can be used. , Epoxy, polyimide, polyamide, polyvinylphenol, benzo as partition wall 137 Single layer or multilayer made of organic materials such as cyclobutene or siloxane materials such as siloxane resin It can be provided in the structure.

[0079] In addition, the partition wall 137 is subjected to a plasma treatment to oxidize or nitride the partition wall 137. Therefore, it is possible to modify the surface of the partition wall 137 to obtain a dense film. By modifying the partition wall 137, the strength of the partition wall 137 is improved, and the cracks during the formation of the openings, etc. This makes it possible to reduce physical damage such as the generation of cracks and film loss during etching.

[0080] Through the above steps, the element formation layer 304, which is the layer to be peeled, can be formed.

[0081] Next, the insulating layer provided on the edge of the substrate 300 is removed by etching or the like, and the pixel section 250 is left. A groove 160 is formed so as to surround the outer periphery of the driving circuit section 252 (the region that becomes the element section of the light emitting device). In FIG. 3C, the partition wall 137, the first interlayer insulating film 206, the gate The first insulating layer 106b is etched to expose the first insulating layer 104. The first interlayer insulating film 20 may be formed so as to expose a film containing nitrogen and silicon. When the gate insulating layer 106 or the gate insulating layer 106b are made of these materials, this is not necessarily the case. There is no need to etch these films. Two or more surrounding grooves 160 may be formed.

[0082] Next, as shown in FIG. 4(A), an adhesive sheet 305 is attached to the element formation layer 304 to set it up. The adhesive sheet 305 is a sheet that can be peeled off by light or heat. By bonding 305, peeling can be easily performed and the element shape before and after peeling can be easily changed. It is possible to reduce the stress applied to the layer 304 and suppress damage to the thin film transistor 106. It becomes.

[0083] Next, the element formation layer 304 including the thin film transistor 106 and the like is peeled off from the substrate 300 (see FIG. 4(B)). Various methods can be used for the peeling method. For example, In the case where a metal oxide layer is formed on the side in contact with the first insulating layer 104, the metal oxide layer is bonded. The crystallization weakens the device formation layer 304, and the device formation layer 304 can be peeled off from the substrate 300. A light-transmitting substrate is used as the substrate 300, and nitrogen, oxygen, hydrogen, or the like is used as the peeling layer 302. (e.g., hydrogen-containing amorphous silicon film, hydrogen-containing alloy film, oxygen-containing alloy film, etc.) In this case, the peeling layer 302 is irradiated with laser light from the substrate 300 to remove the fluorine-containing compound contained in the peeling layer. The nitrogen, oxygen, or hydrogen contained in the gas can be vaporized, so that the element formation layer 304 can be peeled off from the substrate 300. Alternatively, the peeling layer 302 can be removed by etching to form the element formation layer 304 as a substrate. It may be peeled off from the plate 300 .

[0084] Alternatively, the substrate 300 may be mechanically polished and removed, or the substrate 300 may be treated with NF3, BrF3, Use a method of removing the material by etching with halogen fluoride gas such as ClF3 or HF. In this case, the peeling layer 302 may not be used. A metal oxide layer is formed on the side in contact with the first insulating layer 104, and the metal oxide layer is crystallized to reduce brittleness. The peeling layer 302 is then partially decomposed by immersing it in a solution or a fluorinated halide such as NF3, BrF3, or ClF3. After etching with nitrous oxide gas, the weakened metal oxide layer is peeled off. can be done.

[0085] In addition, laser irradiation, etching with gas or solution, or sharp knives or scalpels may be used. A groove is formed to expose the release layer 302, and the release layer 3 At the interface between the insulating layer 302 and the first insulating layer 104 which functions as a protective layer, the element formation layer 304 is formed as a substrate. It can also be peeled off from the plate 300. As a peeling method, for example, a mechanical force is applied. (Processing by peeling off with human hands or a gripping tool, or separation by rotating a roller, etc.) In addition, a liquid is dropped into the groove to form the peeling layer 302 and the first insulating layer 104. The element formation layer 304 may be peeled off from the peeling layer 302 by infiltrating a liquid into the interface. Fluoride gas such as NF3, BrF3, or ClF3 is introduced into the chamber, and the peeling layer is etched with the fluoride gas. The element formation layer 304 is peeled off from the substrate 300 having an insulating surface by removing the insulating film. Furthermore, the peeling may be performed while pouring a liquid such as water on the film.

[0086] As another peeling method, when the peeling layer 302 is formed of tungsten, ammonia The peeling can be performed while etching the peeling layer with a mixed solution of water and hydrogen peroxide. .

[0087] Then, the substrate 300 is peeled off, and a part of the peeling layer 302 or the first insulating layer 104 is removed. The exposed element formation layer 304 is then coated with an adhesive to provide flexibility and transparency to visible light. The substrate 100 is attached (see FIG. 4(C)).

[0088] Adhesives include light-curing adhesives such as ultraviolet-curing adhesives, reaction-curing adhesives, and heat-curing adhesives. Various curing adhesives such as viscoelastic adhesives, anaerobic adhesives, etc. can be used. Adhesive materials include epoxy resin, acrylic resin, silicone resin, and phenolic resin. The substrate 100 may be a structure in which a fibrous body is impregnated with an organic resin ( In the case where a prepreg is used as the substrate 100, The element formation layer 304 and the substrate 100 can be directly bonded together by pressure without using any adhesive. The organic resin of the structure may be a reactive curing type, a heat curing type, or an ultraviolet curing type that requires additional processing. It is advisable to use a material that hardens as it is applied.

[0089] The substrate 100 is previously coated with a film containing nitrogen and silicon, such as silicon nitride or silicon oxynitride, or aluminum nitride. Even if a protective film with low water permeability such as a film containing nitrogen and aluminum such as nium is formed, good.

[0090] After the substrate 100 is provided, the adhesive sheet 305 is removed to expose the first electrode 130 ( See Figure 4(D).

[0091] Through the above steps, an element configuration in which the thin film transistor and the first electrode 130 of the light emitting element are formed is obtained. A layer 304 may be fabricated on the substrate 100 .

[0092] Next, the EL layer 134 is formed on the first electrode 130. The EL layer 134 is made of a low molecular weight material. The EL layer 134 can be formed from either a polyimide or a polymer material. The materials include not only those made of organic compound materials but also those containing inorganic compounds in part. The EL layer 134 has at least a light-emitting layer and has a single-layer structure consisting of one light-emitting layer. For example, a light emitting layer may be formed by stacking layers each having a different function. In addition to the layer, there are hole injection layer, hole transport layer, carrier blocking layer, electron transport layer, electron injection layer The functional layers each having a different function can be appropriately combined. It may contain a layer having two or more functions simultaneously possessed by each layer.

[0093] The EL layer 134 can be formed by a deposition method, an inkjet method, a spin coating method, a dip coating method, or the like. A coating method, a nozzle printing method, or the like can be used regardless of whether it is a wet method or a dry method.

[0094] Next, a second electrode 136 is formed on the EL layer 134, and the first electrode 130 and the EL layer 13 4. A light emitting element 138 is fabricated by laminating a second electrode 136. An element section 150 including the transistor 106 and the light emitting element 138 can be formed. One of the first electrode 130 and the second electrode 136 is used as an anode and the other is used as a cathode. There are.

[0095] When used as an anode, it is desirable to use a material with a large work function. Indium tin oxide film, indium tin oxide film containing silicon, indium oxide 2 to 20 A transparent thin film was formed by sputtering using a target containing wt% zinc oxide (ZnO). Conductive film with optical properties, zinc oxide (ZnO), conductive oxynitride containing zinc and aluminum In addition to single-layer films such as titanium nitride film, chromium film, tungsten film, Zn film, and Pt film, Lamination of titanium and aluminum-based films, titanium nitride film and aluminum-based film For example, a three-layer structure consisting of a film made of titanium and a titanium nitride film can be used.

[0096] In addition, when used as a cathode, materials with a small work function (Al, Ag, Li, Ca, etc.) are used. or their alloys (MgAg, MgIn, AlLi, CaF2, or calcium nitride) In addition, when the electrode used as the cathode is made to be transparent, The metal thin film with a thin thickness and the conductive film with light transmission (indium tin oxide film, silicon Indium tin oxide film containing 2 to 20 wt% zinc oxide (ZnO) in indium oxide A light-transmitting conductive film formed by sputtering using a target containing a mixture of nitric oxide and It is recommended to use a laminate with lead (ZnO, etc.).

[0097] In this embodiment, the first electrode 130 is used as an anode, and the EL layer 134 is A structure in which a hole injection layer, a hole transport layer, a light emitting layer, and an electron injection layer are laminated in this order from the electrode 130 side. Various materials can be used for the light-emitting layer. A compound that emits phosphorescence or a phosphorescent compound that emits phosphorescence can be used.

[0098] Next, a second insulating layer is formed on the second electrode 136 so as to cover the upper and side surfaces of the element section 150. The second insulating layer 140 functions as a protective layer and protects the EL layer. The second insulating layer 140 is formed up to the groove portion 160 to prevent moisture and damage to the insulating layer 134. As a result, the first insulating layer 104 exposed in the groove portion 160 comes into contact with the second insulating layer 140. do. The first insulating layer 104 and the second insulating layer 140 are each formed of a film containing nitrogen and silicon. Therefore, it is possible to bond the element portion 150 firmly in the groove. By forming a groove so as to surround the periphery, it becomes possible to firmly seal the element portion.

[0099] For example, the second insulating layer 140 may be formed by sputtering, plasma CVD, coating, printing, or the like. Materials containing nitrogen and silicon, such as silicon nitride, silicon oxynitride, and silicon oxynitride, can be produced by a printing method or the like. It is formed in a single layer or multiple layers using inorganic insulating materials, aluminum oxide, etc. The second insulating layer 140 may be formed by laminating an insulating film and an organic insulating film such as a resin film. By providing this insulating layer, it is possible to prevent moisture and gases such as oxygen from entering the element. The thickness of the second insulating layer 140 functioning as a protective layer is 10 nm or more and 1000 nm or less. and more preferably from 100 nm to 700 nm.

[0100] Next, a resin film 142 is formed on the second insulating layer 140. The resin film 142 is, for example, The resin film 142 can be formed by applying a composition using a coating method, and then drying and heating the composition. It is preferable to use a material that has good adhesion to the insulating layer 140 of the second insulating layer 140. When the resin film 142 is formed using a resin such as acrylic resin, polyimide resin, or melamine resin, Epoxy resin, polyester resin, polycarbonate resin, phenol resin, polya Cetal, polyether, polyurethane, polyamide (nylon), furan resin, diaryl Organic compounds such as phthalate resins, and siloxane polymer materials such as silica glass The compound consisting of silicon, oxygen, and hydrogen formed from the starting material is the Si-O-Si bond. Inorganic siloxane polymers, alkyl siloxane polymers, alkyl silsesquioxane polymers, Oxane polymer, hydrogenated silsesquioxane polymer, hydrogenated alkyl silsesquioxane Hydrogen bonded to silicon, as typified by selenium polymers, is replaced by organic groups such as methyl and phenyl. Alternatively, the resin film 142 may be an organic siloxane polymer substituted with . Alternatively, a structure in which a fibrous body is impregnated with an organic resin can be used as the insulating layer.

[0101] Next, a metal substrate 144 is bonded onto the resin film 142 (FIG. 5(B)). The adhesive may be used for bonding the substrate 141, or the resin film 142 may be used instead of the adhesive. The material constituting the metal substrate is not particularly limited, but may be aluminum, copper, nickel, etc. Preferably, alloys of metals such as galvanized steel, aluminum alloys, or stainless steel are used. Before bonding the metal substrate 144, baking in a vacuum or plasma treatment is performed. It is preferable to remove water adhering to the surface of the metal substrate by washing the surface with water.

[0102] The metal substrate 144 can also be attached using a laminator. For example, first, The adhesive is attached to a metal substrate using a laminator, and the metal substrate is laminated. The method is to use a magnet to further attach it to the light-emitting element, or to attach it to a metal substrate by screen printing, etc. A method of printing a coating onto a metal substrate and then attaching the coating to a light-emitting element using a laminator is also available. This step is preferably carried out under reduced pressure to reduce the introduction of air bubbles.

[0103] Through the above steps, a light-emitting device of one embodiment of the present invention can be manufactured.

[0104] In this embodiment, a light-emitting device having a thin film transistor is The method of forming the first and second layers on a substrate and then peeling them off has been described above. However, the method is not limited to this, and may be performed after the light emitting element 138 is formed (i.e., after the second electrode 1 of the light emitting element is formed). After forming the first insulating layer 104, the substrate may be peeled off and transposed. After the film is peeled off and transferred to the substrate 100, a thin film transistor or a light emitting element may be manufactured. In addition, in the case where a thin film transistor is not provided, the first insulating layer 104 is provided with a first insulating layer 104. The electrode 130 may be formed on the metal substrate 1 in the same manner. A resin film may also be provided on the surface of 44 to protect the metal substrate.

[0105] In addition, the substrate 100 and the resin film 142 may contain fibrous materials. The fibrous body is made of high-strength fibers of organic or inorganic compounds. It refers to fibers with high tensile modulus or Young's modulus. A typical example is polyvinyl acetate. Alcohol-based fibers, polyester-based fibers, polyamide-based fibers, polyethylene-based fibers, arami Fibers such as polyparaphenylene benzobisoxazole fibers, glass fibers, or carbon fibers. Examples of glass fibers include E glass, S glass, D glass, and Q glass. These are used in the form of woven or nonwoven fabric, and the fiber body is A structure impregnated with an organic resin and cured may be used as the substrate 100. When a structure made of fiber and organic resin is used as 100, damage due to bending or localized pressure is prevented. This is a preferred configuration since it improves reliability.

[0106] In addition, when the substrate 100 contains the above-mentioned fibrous body, the light from the light emitting element is not emitted to the outside. In order to reduce the interference with the fiber, the fiber is made of nanofibers having a diameter of 100 nm or less. It is also preferable to match the refractive index of the fiber body with that of the organic resin or adhesive. .

[0107] The light emitting device of this embodiment uses a metal substrate with low water permeability as a support for the light emitting device. This makes it possible to prevent moisture from entering the light emitting element 138, resulting in a light emitting device with a long life. In addition, the first insulating layer 104 and the second insulating layer 140 functioning as protective layers are The ends of the light emitting element 138 are sealed by sealing the element portion with each other. Therefore, it is possible to prevent the intrusion of gases such as oxygen, thereby making it possible to provide a highly reliable light-emitting device. do.

[0108] In addition, the light-emitting device of this embodiment mode is manufactured by forming a thin film transistor on a highly heat-resistant substrate. Therefore, thin film transistors using crystalline semiconductor layers such as crystalline silicon with high mobility are suitable. Therefore, a driving circuit using such a thin film transistor can be used. The path section and pixel section can be fabricated on the same substrate, making it possible to fabricate light-emitting devices at lower cost. can be done.

[0109] Note that the configuration of this embodiment mode can be used in appropriate combination with the configurations of other embodiments. It is possible.

[0110] (Embodiment 3) In this embodiment, a structure of a light-emitting element included in a light-emitting device will be specifically described with reference to FIG. do.

[0111] An example of the structure of a light-emitting element is shown in FIG. and a second electrode 136. The EL layer 134 is at least The laminate structure is not particularly limited as long as it has a layer, and may include a layer containing a substance having high electron transport properties. or a layer containing a substance with high hole transporting properties, a layer containing a substance with high electron injecting properties, A layer containing a material having a bipolar property (a material having high electron and hole transport properties) is preferably used. For example, a hole injection layer, a hole transport layer, a light emitting layer, and an electron transport layer may be used. In the present embodiment, the EL layer 1 34 describes a structure having a hole injection layer, a hole transport layer, a light emitting layer, and an electron transport layer. The materials constituting each layer are specifically shown below.

[0112] The hole injection layer is provided in contact with the anode and is a layer containing a material with high hole injection properties. Vanadium oxide, ruthenium oxide, tungsten oxide, manganese oxide In addition, phthalocyanine (abbreviation: H2Pc) and copper phthalocyanine can be used. Phthalocyanine compounds such as CuPC, 4,4'-bis[N-(4-diphenyl Aminophenyl)-N-phenylamino]biphenyl (abbreviation: DPAB), N,N'-biphenyl S[4-[bis(3-methylphenyl)amino]phenyl]-N,N'-diphenyl-[ Aromatic amination of 1,1'-biphenyl]-4,4'-diamine (abbreviation: DNTPD) etc. or poly(ethylenedioxythiophene) / poly(styrenesulfonic acid) (PE The hole injection layer can also be formed from a polymer such as DOT / PSS.

[0113] In addition, a composite material containing an acceptor material in a material with high hole transport properties is used as the hole injection layer. In addition, a material having a high hole transporting property may be used. By using a material that has been developed, it is possible to select a material for forming the electrode regardless of the work function of the electrode. In other words, the first electrode 130 can be made of not only a material with a large work function, but also a material with a low work function. Small materials can be used. Acceptor materials include 7,7,8,8-tetramethylphenyl. 2,3,5,6-tetrafluoroquinodimethane (abbreviation: F4-TCNQ), Examples of the oxides include transition metal oxides. Examples of the oxides include those of metals belonging to groups 4 to 8 of the periodic table. Vanadium oxide, niobium oxide, tantalum oxide, chromium oxide, molybdenum oxide, Tungsten, manganese oxide, and rhenium oxide are preferred because of their high electron-accepting properties. In particular, molybdenum oxide is preferred because it is stable in the air, has low hygroscopicity, and is easy to handle.

[0114] As a substance with high hole transport properties used in the composite material, aromatic amine compounds and carbazole derivatives are used. Conductors, aromatic hydrocarbons, polymer compounds (oligomers, dendrimers, polymers, etc.), etc. Various compounds can be used. The organic compound used in the composite material is a hole It is preferable that the organic compound has high transportability. -6 cm 2 / Vs or more However, it is preferable that the material has a hole mobility of 1000 to 15000 m / s. Other materials may be used as long as they are of the same quality. The following lists specific organic compounds that can be used.

[0115] For example, the aromatic amine compound is N,N'-di(p-tolyl)-N,N'-diphenyl Nyl-p-phenylenediamine (DTDPPA), 4,4'-bis[N-(4-diphenyl phenylaminophenyl)-N-phenylamino]biphenyl (abbreviation: DPAB), N, N'-Bis[4-[bis(3-methylphenyl)amino]phenyl]-N,N'-diphenyl Nyl-[1,1'-biphenyl]-4,4'-diamine (abbreviation: DNTPD), 1,3, 5-Tris[N-(4-diphenylaminophenyl)-N-phenylamino]benzene( Abbreviated as DPA3B).

[0116] Specific examples of carbazole derivatives that can be used in composite materials include 3-[N-( 9-Phenylcarbazol-3-yl)-N-phenylamino]-9-phenylcarbazo (abbreviation: PCzPCA1), 3,6-bis[N-(9-phenylcarbazole-3- yl)-N-phenylamino]-9-phenylcarbazole (abbreviation: PCzPCA2), 3-[N-(1-naphthyl)-N-(9-phenylcarbazol-3-yl)amino]- 9-phenylcarbazole (abbreviation: PCzPCN1) and the like.

[0117] Another carbazole derivative that can be used in composite materials is 4,4'-dicarbazole. (N-carbazolyl)biphenyl (abbreviation: CBP), 1,3,5-tris[4-(N-carbazolyl) 9-[4-(10-phenyl-9 -anthryl)phenyl]-9H-carbazole (abbreviation: CzPA), 1,4-bis[4 -(N-carbazolyl)phenyl]-2,3,5,6-tetraphenylbenzene, etc. It is possible.

[0118] In addition, examples of aromatic hydrocarbons that can be used in the composite material include 2-tert- Butyl-9,10-di(2-naphthyl)anthracene (abbreviation: t-BuDNA), 2-t ert-Butyl-9,10-di(1-naphthyl)anthracene, 9,10-bis(3,5 -diphenylphenyl)anthracene (abbreviation: DPPA), 2-tert-butyl-9, 10-Bis(4-phenylphenyl)anthracene (abbreviation: t-BuDBA), 9,10 -Di(2-naphthyl)anthracene (abbreviation: DNA), 9,10-diphenylanthracene DPAnth, 2-tert-butylanthracene (t-BuAnth) h), 9,10-bis(4-methyl-1-naphthyl)anthracene (abbreviation: DMNA), 2-tert-Butyl-9,10-bis[2-(1-naphthyl)phenyl]anthracene , 9,10-bis[2-(1-naphthyl)phenyl]anthracene, 2,3,6,7-tetraphenyl tetramethyl-9,10-di(1-naphthyl)anthracene, 2,3,6,7-tetramethyl 10,10-di(2-naphthyl)anthracene, 9,9'-bianthryl, '-Diphenyl-9,9'-bianthryl, 10,10'-bis(2-phenylphenyl )-9,9'-bianthryl, 10,10'-bis[(2,3,4,5,6-pentaphenyl nyl)phenyl]-9,9'-bianthryl, anthracene, tetracene, rubrene, pentacene perylene, 2,5,8,11-tetra(tert-butyl)perylene, etc. In addition, pentacene, coronene, etc. can also be used. -6 c m 2 The aromatic hydrocarbon having a hole mobility of 14 to 42 carbon atoms is used. is more preferable.

[0119] The aromatic hydrocarbon that can be used in the composite material may have a vinyl skeleton. Examples of aromatic hydrocarbons having a vinyl group include 4,4'-bis(2,2-diphenyl ether). 9,10-bis[4-(2,2-diphenylvinyl)biphenyl (abbreviation: DPVBi) phenylvinyl)phenyl]anthracene (abbreviation: DPVPA), and the like.

[0120] In addition, poly(N-vinylcarbazole) (abbreviation: PVK) and poly(4-vinyltriphenyl PVTPA), poly[N-(4-{N'-[4-(4-diphenylamine N'-phenylamino)phenyl]phenyl-N'-phenylamino}phenyl)methacrylamide Name: PTPDMA), poly[N,N'-bis(4-butylphenyl)-N,N'-bis( It is also possible to use polymer compounds such as poly(phenyl)benzidine (abbreviation: Poly-TPD). Cut.

[0121] The hole transport layer is a layer containing a substance having a high hole transporting property. For example, 4,4'-bis[N-(1-naphthyl)-N-phenylamino]biphenyl (abbreviation N,N'-bis(3-methylphenyl)-N,N'-diphenyl-[1, 1'-biphenyl]-4,4'-diamine (abbreviation: TPD), 4,4',4''-tris (N,N-diphenylamino)triphenylamine (abbreviation: TDATA), 4,4',4 ''-Tris[N-(3-methylphenyl)-N-phenylamino]triphenylamine (abbreviation: MTDATA), 4,4'-bis[N-(spiro-9,9'-bifluorene-2 -yl)-N-phenylamino]biphenyl (abbreviation: BSPB) and other aromatic amine compounds The substances mentioned here are mainly 10 -6 cm 2 / Vs or more holes However, if the material has a higher hole transporting property than the electron transporting property, Note that the layer containing a substance having a high hole transporting property is not limited to a single layer. Alternatively, two or more layers made of the above-mentioned materials may be laminated.

[0122] In addition, poly(N-vinylcarbazole) (abbreviation: PVK) and poly(4 It is also possible to use polymer compounds such as 1-vinyltriphenylamine (PVTPA). Cut.

[0123] The light-emitting layer is a layer containing a light-emitting substance. There are several types of light-emitting layers, including those containing a light-emitting center substance as the main component. Even in the case of a so-called single-film light-emitting layer, a light-emitting center material is dispersed in a host material. The light-emitting layer may be of a host-guest type.

[0124] There is no limitation on the luminescent center material to be used, and any known fluorescent or phosphorescent material may be used. Examples of the fluorescent material include N,N'-bis[4-(9H-carbazole- 9-yl)phenyl]-N,N'-diphenylstilbene-4,4'-diamine (abbreviation: YGA2S), 4-(9H-carbazol-9-yl)-4'-(10-phenyl-9- Anthryl)triphenylamine (abbreviation: YGAPA), etc., with an emission wavelength of 450 nm The above 4-(9H-carbazol-9-yl)-4'-(9,10-diphenyl-2-phenyl) N,9-diphenyl-N-[ 4-(10-phenyl-9-anthryl)phenyl]-9H-carbazol-3-amine (Abbreviation: PCAPA), Perylene, 2,5,8,11-tetra-tert-butylperylene TBP, 4-(10-phenyl-9-anthryl)-4'-(9-phenyl -9H-carbazol-3-yl)triphenylamine (abbreviation: PCBAPA), N,N ''-(2-tert-butylanthracene-9,10-diyldi-4,1-phenylene ) Bis[N,N',N'-triphenyl-1,4-phenylenediamine] (abbreviation: DPA BPA), N,9-diphenyl-N-[4-(9,10-diphenyl-2-anthryl phenyl]-9H-carbazol-3-amine (abbreviation: 2PCAPPA), N-[4-( 9,10-diphenyl-2-anthryl)phenyl]-N,N',N'-triphenyl- 1,4-Phenylenediamine (abbreviation: 2DPAPPA), N,N,N',N',N'', N'',N''',N'''-Octaphenyldibenzo[g,p]chrysene-2,7,1 0,15-Tetraamine (abbreviation: DBC1), Coumarin 30, N-(9,10-diphenyl (2-anthryl)-N,9-diphenyl-9H-carbazol-3-amine (abbreviation: 2PCAPA), N-[9,10-bis(1,1'-biphenyl-2-yl)-2-an Tolyl]-N,9-diphenyl-9H-carbazol-3-amine (abbreviation: 2PCABP hA), N-(9,10-diphenyl-2-anthryl)-N,N',N'-triphenyl N-[9,10-bis(1, 1'-biphenyl-2-yl)-2-anthryl]-N,N',N'-triphenyl-1 ,4-Phenylenediamine (abbreviation: 2DPABPhA), 9,10-bis(1,1'-biphenyl) Phenyl-2-yl)-N-[4-(9H-carbazol-9-yl)phenyl]-N- Phenylanthracene-2-amine (abbreviation: 2YGABPhA), N,N,9-triphenyl N,N'-anthracene-9-amine (abbreviation: DPhAPhA) Coumarin 545T Diphenylquinacridone, (abbreviation: DPQd), rubrene, 5,12-bis(1,1'- Biphenyl-4-yl)-6,11-diphenyltetracene (abbreviation: BPT), 2-(2 -{2-[4-(dimethylamino)phenyl]ethenyl}-6-methyl-4H-pyran- 4-ylidene)propanedinitrile (abbreviation: DCM1), 2-{2-methyl-6-[2- (2,3,6,7-Tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl) ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCM2), N ,N,N',N'-Tetrakis(4-methylphenyl)tetracene-5,11-diamine (abbreviation: p-mPhTD), 7,14-diphenyl-N,N,N',N'-tetrakis( 4-Methylphenyl)acenaphtho[1,2-a]fluoranthene-3,10-diamine( Abbreviation: p-mPhAFD), 2-{2-isopropyl-6-[2-(1,1,7,7-tetramethylphenyl) tetramethyl-2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizine 9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DC JTI), 2-{2-tert-butyl-6-[2-(1,1,7,7-tetramethyl- 2,3,6,7-Tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl) Thenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCJTB), 2 -(2,6-bis{2-[4-(dimethylamino)phenyl]ethenyl}-4H-pyran -4-ylidene)propanedinitrile (abbreviation: BisDCM), 2-{2,6-bis[2 -(8-Methoxy-1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1 H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-yl Bis(2-phenylenedinitrile) (abbreviation: BisDCJTM) and other phosphorescent materials. Examples of the materials include bis[2-(4',6'-difluorophenyl)pyridinato-N, C 2’ ]Iridium(III) tetrakis(1-pyrazolyl)borate (abbreviation: FIr6 ), and bis[2-(4',6'- Difluorophenyl)pyridinato-N,C 2’ ]Iridium(III) picolinate (abbreviation Name: FIrpic), bis[2-(3',5'-bistrifluoromethylphenyl)pyridine Ginat-N,C 2’ ]Iridium(III) picolinate (abbreviation: Ir(CF3ppy) 2(pic)), bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2 ’ ]Iridium(III) acetylacetonate (abbreviation: FIracac), emission wavelength is Tris(2-phenylpyridinato)iridium(III) above 500 nm (green emission) (abbreviation: Ir(ppy)3), bis(2-phenylpyridinato)iridium(III) Cetylacetonate (abbreviation: Ir(ppy)2(acac)), tris(acetylacetonate) Nat)(monophenanthroline)terbium(III) (abbreviation: Tb(acac)3(P hen), bis(benzo[h]quinolinato)iridium(III) acetylacetoner Ir(bzq)2(acac)), bis(2,4-diphenyl-1,3-oxo Sazorath-N,C 2’ ) Iridium(III) acetylacetonate (abbreviation: Ir(dp o) 2(acac)), bis[2-(4'-perfluorophenylphenyl)pyridinato ]Iridium(III) acetylacetonate (abbreviation: Ir(p-PF-ph)2(ac ac)), bis(2-phenylbenzothiazolato-N,C 2’ ) Iridium(III) A Cetylacetonate (abbreviation: Ir(bt)2(acac)), bis[2-(2'-benzo [4,5-α]thienyl)pyridinato-N,C 3’ ]Iridium(III) acetylacetone Tonanate (abbreviation: Ir(btp)2(acac)), bis(1-phenylisoquinolinate -N,C 2’ ) Iridium(III) acetylacetonate (abbreviation: Ir(piq)2( acac)), (acetylacetonato)bis[2,3-bis(4-fluorophenyl) Iridium(III) (abbreviation: Ir(Fdpq)2(acac)), (A Cetylacetonato)bis(2,3,5-triphenylpyrazinate)iridium(III) (Abbreviation: Ir(tppr)2(acac)), 2,3,7,8,12,13,17,18 -Octaethyl-21H,23H-porphyrin platinum(II) (abbreviation: PtOEP), Tris(1,3-diphenyl-1,3-propanedionato)(monophenanthroline)eutectic Eu(DBM)3(Phen) [yl)-3,3,3-trifluoroacetonato](monophenanthroline)europium (III) (abbreviation: Eu(TTA)3(Phen)) and the like. Alternatively, the material may be selected from other known materials, taking into consideration the emission color of each light-emitting element.

[0125] When a host material is used, for example, tris(8-quinolinolato)aluminum(III) (abbreviation: Alq), tris(4-methyl-8-quinolinolato)aluminum(III) ( Abbreviation: Almq3), bis(10-hydroxybenzo[h]quinolinato)beryllium (I I) (abbreviation: BeBq2), bis(2-methyl-8-quinolinolato)(4-phenylphenyl) Bis(8-quinolinolato)aluminum(III) (abbreviation: BAlq), bis(8-quinolinolato)zinc ( II) (abbreviation: Znq), bis[2-(2-benzoxazolyl)phenolato]zinc (I I) (abbreviation: ZnPBO), bis[2-(2-benzothiazolyl)phenolato]zinc (I I) (abbreviation: ZnBTZ) and other metal complexes, 2-(4-biphenylyl)-5-(4-te rt-Butylphenyl)-1,3,4-oxadiazole (abbreviation: PBD), 1,3-Bis(phenyl) S[5-(p-tert-butylphenyl)-1,3,4-oxadiazol-2-yl ]benzene (abbreviation: OXD-7), 3-(4-biphenylyl)-4-phenyl-5-(4 -tert-butylphenyl)-1,2,4-triazole (abbreviation: TAZ), 2,2' ,2''-(1,3,5-benzenetriyl)tris(1-phenyl-1H-benzoimide dazole (abbreviation: TPBI), Bathophenanthroline (abbreviation: BPhen), Vasocutan Proine (abbreviation: BCP), 9-[4-(5-phenyl-1,3,4-oxadiazole -2-yl)phenyl]-9H-carbazole (abbreviation: CO11) and other heterocyclic compounds; Examples of aromatic amine compounds include NPB (or α-NPD), TPD, and BSPB. In addition, anthracene derivatives, phenanthrene derivatives, pyrene derivatives, chrysene derivatives, Dibenzo[g,p]chrysene derivatives and other condensed polycyclic aromatic compounds are exemplified. 9,10-Diphenylanthracene (abbreviation: DPAnth), N,N-diphenyl-9- [4-(10-phenyl-9-anthryl)phenyl]-9H-carbazole-3-amine CzA1PA, 4-(10-phenyl-9-anthryl)triphenylamine DPhPA, 4-(9H-carbazol-9-yl)-4'-(10-phenyl) N,9-diphenyl-9-anthryl)triphenylamine (abbreviation: YGAPA) -N-[4-(10-phenyl-9-anthryl)phenyl]-9H-carbazole-3 -amine (abbreviation: PCAPA), N,9-diphenyl-N-{4-[4-(10-phenyl {9-(anthryl)phenyl}phenyl}-9H-carbazol-3-amine (abbreviation: PCAPBA), N,9-diphenyl-N-(9,10-diphenyl-2-anthryl) -9H-Carbazole-3-amine (abbreviation: 2PCAPA), 6,12-dimethoxy-5 ,11-Diphenylchrysene,N,N,N',N',N'',N'',N''',N'' '-Octaphenyldibenzo[g,p]chrysene-2,7,10,15-tetraamine ( Abbreviation: DBC1), 9-[4-(10-phenyl-9-anthryl)phenyl]-9H- Carbazole (abbreviation: CzPA), 3,6-diphenyl-9-[4-(10-phenyl- 9-Anthryl)phenyl]-9H-carbazole (abbreviation: DPCzPA), 9,10- Bis(3,5-diphenylphenyl)anthracene (abbreviation: DPPA), 9,10-di( 2-naphthyl)anthracene (abbreviation: DNA), 2-tert-butyl-9,10-di( 2-Naphthyl)anthracene (abbreviation: t-BuDNA), 9,9'-Bianthryl (abbreviation: :BANT), 9,9'-(stilbene-3,3'-diyl)diphenanthrene (abbreviation: DPNS), 9,9'-(stilbene-4,4'-diyl)diphenanthrene (abbreviation: D PNS2), 3,3',3''-(benzene-1,3,5-triyl)tripylene (abbreviation Among these and other known substances, the most suitable one is The energy gap of the luminescent center is larger than the triplet energy in the case of phosphorescence. The material has an energy gap (triplet energy), and each layer should have A substance that exhibits transport properties that match the transport properties may be selected.

[0126] The electron transport layer is a layer containing a substance with high electron transport properties. For example, tris(8-quinolinola Tris(4-methyl-8-quinolinolato)aluminum (Alq), Almq3, bis(10-hydroxybenzo[h]quinolinato)beryllium BeBq2, bis(2-methyl-8-quinolinolato)(4-phenylphenanthroline) (BAlq) and other compounds with quinoline or benzoquinoline skeletons. The layer is made of a metal complex having the above structure. )benzoxazolato]zinc (abbreviation: Zn(BOX)2), bis[2-(2-hydroxy oxazoles such as phenyl)benzothiazolato]zinc (abbreviation: Zn(BTZ)2); Metal complexes having thiazole-based ligands can also be used. Also, 2-(4-biphenylyl)-5-(4-tert-butylphenyl)-1,3,4 -oxadiazole (abbreviation: PBD) and 1,3-bis[5-(p-tert-butyl ether) (phenyl)-1,3,4-oxadiazol-2-yl]benzene (abbreviation: OXD-7), 3-(4-biphenylyl)-4-phenyl-5-(4-tert-butylphenyl)-1 , 2,4-triazole (abbreviation: TAZ), bathophenanthroline (abbreviation: BPhen) , Bathocuproine (abbreviation: BCP), etc. can also be used. Mainly 10 -6 cm 2 / Vs or higher. Note that electrons are more likely to be charged than holes. Any substance other than the above may be used for the electron-transporting layer as long as it has a high transporting property.

[0127] The electron transport layer may be a single layer or a laminate of two or more layers of the above-mentioned materials. It may also be possible to use the following.

[0128] In addition, a layer for controlling the movement of electron carriers may be provided between the electron transport layer and the light emitting layer. This is a material with high electron transport properties, as described above, to which a small amount of a substance with high electron trapping properties has been added. A layer that adjusts the carrier balance by suppressing the movement of electron carriers. This type of structure is caused by electrons penetrating the light-emitting layer. This is highly effective in suppressing problems that arise from the use of such a material (such as a reduction in the element life span).

[0129] In addition, an electron injection layer may be provided in contact with the cathode. Lithium fluoride (LiF), cesium fluoride (CsF), calcium fluoride (CaF2), etc. Such alkali metals or alkaline earth metals or compounds thereof can be used. For example, an alkali metal or alkaline earth metal or the like is added to a layer made of a substance having an electron transporting property. These compounds are included, for example, magnesium (Mg) in Alq As the electron injection layer, a layer made of a substance having an electron transporting property can be used. By using a material containing an alkali metal or an alkaline earth metal in the second electrode, This is more preferable since electron injection from the electrode 136 is performed efficiently.

[0130] The material for forming the second electrode 136 of the light-emitting element is a material used for the second electrode 136 as a cathode. In this case, metals, alloys, and electrical conductors with small work functions (specifically, 3.8 eV or less) are used. Compounds and mixtures thereof can be used. Specific examples of such cathode materials include The elements that belong to the first or second group of the periodic table are lithium (Li) and Alkali metals such as cesium (Cs), magnesium (Mg), and calcium (Ca) Alkaline earth metals such as strontium (Sr), and alloys containing these metals (MgAg, Rare earth metals such as AlLi), europium (Eu), ytterbium (Yb) and the like However, when an electron injection layer is provided between the cathode and the electron transport layer, By providing this, regardless of the magnitude of the work function, Al, Ag, ITO, silicon or oxide can be used. Various conductive materials such as indium oxide-tin oxide containing silicon dioxide can be used as the cathode. These conductive materials can be applied by sputtering, inkjet printing, spin coating, etc. The film can be formed by using a method such as a method for forming a thin film.

[0131] In addition, when the second electrode 136 is used as an anode, a material having a large work function (specifically, 4 It is preferable to use metals, alloys, conductive compounds, and mixtures thereof. Specifically, for example, indium oxide-tin oxide (ITO) n Oxide), indium oxide-tin oxide containing silicon or silicon oxide, acid Indium Zinc Oxide (IZO), Tungsten Oxide Examples of these include indium oxide containing tin and zinc oxide (IWZO). Conductive metal oxide films are usually formed by sputtering, but they can also be made by applying the sol-gel method. For example, indium oxide-zinc oxide (IZO) is a compound in which indium oxide is Formed by sputtering using a target containing 1 to 20 wt% zinc oxide. In addition, indium oxide (I) containing tungsten oxide and zinc oxide can be used. WZO) is a material that contains 0.5 to 5 wt% tungsten oxide and 0.0% zinc oxide relative to indium oxide. It can be formed by sputtering using a target containing 1 to 1 wt% of Other metals include gold (Au), platinum (Pt), nickel (Ni), tungsten (W), and chromium (Cr). Aluminum (Cr), Molybdenum (Mo), Iron (Fe), Cobalt (Co), Copper (Cu), Palladium (Pb) Examples of the nitride include palladium (Pd), and nitrides of metal materials (for example, titanium nitride). By placing the above composite material in contact with the anode, the electrode can be made to have a high or low work function. The material can be selected.

[0132] The EL layer 134 is connected to the first electrode 130 and the second electrode 136 as shown in FIG. 6(B). In this case, the EL layer 134 and the EL layer 134 may be stacked. It is preferable to provide a charge generating layer 600 between the above-mentioned layers. The charge generating layer 600 is made of the above-mentioned composite material. The charge generating layer 600 can be formed of a layer of a composite material and a layer of another material. In this case, the layer made of the other material may be a layer of an electric A layer containing a substance having electron donating properties and a substance having high electron transport properties, a layer made of a transparent conductive film, or the like is used. A light-emitting device having such a structure can avoid problems such as energy transfer and quenching. This makes it difficult for this phenomenon to occur, and the range of materials that can be selected is expanded, allowing for the development of light emission that combines high luminous efficiency with a long lifespan. It is easy to fabricate a device. In addition, it is possible to obtain phosphorescence from one EL layer and fluorescence from the other. This structure can be used in combination with the above-mentioned EL layer structure.

[0133] Next, in the case where the EL layer is laminated with three or more layers between the first electrode and the second electrode, As shown in FIG. 6C, the EL layer 134 has a thickness of, for example, n (n is a natural number of 3 or more). In the case of a laminated structure of layers, the mth (m is a natural number, 1≦m≦n-1) EL layer and A charge generating layer 600 is sandwiched between each of the (m+1)th EL layers.

[0134] The charge generating layer 600 is a layer that is generated when a voltage is applied between the first electrode 130 and the second electrode 136. At this time, holes are injected into one of the EL layers 134 formed in contact with the charge generating layer 600. The EL layer 134 has a function of injecting electrons into the other EL layer 134 .

[0135] The charge generating layer 600 may be a composite material of an organic compound and a metal oxide, a metal oxide, an organic compound and an alumina. Alkaline metals, alkaline earth metals, or composite materials with these compounds, as well as the use of these appropriately The composite material of an organic compound and a metal oxide can be formed by combining, for example, Examples include organic compounds and metal oxides such as V2O5, MoO3, and WO3. Aromatic amine compounds, carbazole derivatives, aromatic hydrocarbons, polymer compounds (oligomers) Various compounds such as mers, dendrimers, polymers, etc. can be used. As an organic compound, a hole-transporting organic compound with a hole mobility of 10 -6 cm 2 / Vs or more However, it is preferable to use a material that has a higher hole transporting property than an electron transporting property. In addition, the charge generating layer 600 may be made of any of the following materials. Since it has excellent carrier injection and carrier transport properties, it is suitable for low current driving of light emitting devices and low Voltage driving can be realized.

[0136] In particular, as shown in FIG. 6B or C, a plurality of EL layers are disposed between a pair of electrodes as a charge generating layer. By separating the layers, it is possible to emit light in a high brightness range while keeping the current density low. Since the current density can be kept low, a long-life element can be realized. By making the colors different, it is possible to obtain light emission of a desired color from the entire light-emitting element. For example, in a light-emitting device having two EL layers, the emission color of the first EL layer and the emission color of the second EL layer may be different. By making the luminescent colors of the layers complementary to each other, the luminescent device as a whole emits white light. It is also possible to obtain a device. Complementary colors are colors that become achromatic when mixed together. In other words, when light from materials that emit complementary colors is mixed, white light is emitted. The same can be said for a light-emitting element having three EL layers. For example, the emission color of the first EL layer is red, the emission color of the second EL layer is green, and the emission color of the third EL layer is red. When the EL layer emits blue light, the light emitting device as a whole can emit white light. .

[0137] Note that the configuration of this embodiment mode can be used in appropriate combination with the configurations of other embodiments. It is possible.

[0138] (Embodiment 4) In this embodiment, a modular light emitting device to which an FPC is connected will be described with reference to FIG. FIG. 7A shows a light-emitting device manufactured by the manufacturing method shown in the embodiment 2. FIG. 7(B) is a cross-sectional view taken along line A-A' in FIG. 7(A). do.

[0139] In FIG. 7A, a first An insulating layer is provided, and a pixel section 502, a source side driver circuit 504, and a gate side driver circuit 506 are provided on the insulating layer. The pixel portion and the driver circuit are formed according to the above-mentioned embodiment mode 2. Also, 144 is a metal substrate, which is bonded onto the pixel section and the driving circuit section. It is being done.

[0140] In addition, 508 indicates a signal input to the source side driver circuit 504 and the gate side driver circuit 503. The flexible printed circuit board (FPC) is the wiring for transmitting the signal. Video signal, clock signal from FPC402 The wiring 508 is connected to the pixel section and the driving circuit. The gate electrode of the thin film transistor provided in the portion is formed in the same process. It is possible to further add a printed wiring board (PWB) to the FPC 402 shown in FIG. The light emitting device in this specification may be configured to include a light emitting device main body. This also includes the state in which an FPC or PWB is attached to it.

[0141] Next, the cross-sectional structure will be described with reference to FIG. 4 is provided, and a pixel section 502 and a gate side driving circuit 503 are provided above the first insulating layer 104. The pixel portion 502 is electrically connected to a current control TFT 511 and its drain. The pixel electrode 512 is formed of a plurality of pixels including the first pixel electrode 512. The circuit 503 is a CMM that combines an n-channel TFT 513 and a p-channel TFT 514. It is formed using OS circuits.

[0142] The method of connecting the FPC is not limited to the configuration shown in FIG. 7. For example, from the substrate 100 side, A through-wire is provided at the position where it is to be connected to the wiring 508, and the through-wire is used to connect to the FPC. The through-hole wiring may be, for example, A through hole is formed by a laser, a drill, a punch, or the like, reaching the wiring 508. The holes are filled with conductive resin by screen printing or inkjet printing. Conductive resin is an organic material that contains conductive particles with a particle size of several tens of micrometers or less. This refers to something that has been dissolved or decomposed into resin.

[0143] Conductive particles include, for example, copper (Cu), silver (Ag), nickel (Ni), and gold (Au). , Platinum (Pt), Palladium (Pd), Tantalum (Ta), Molybdenum (Mo), Titanium A conductive paste containing any one of the metal elements, Ti, and Cr, can be used. The organic resin contained in the oil functions as a binder, solvent, dispersant, and coating material for the metal particles. One or more organic resins selected from the following can be used. Representative examples include epoxy. Examples of the resin include organic resins such as resins, phenol resins, and silicone resins.

[0144] In addition, when a structure in which a fibrous body is impregnated with an organic resin is used as the substrate 100, the structure Conductive resin is placed at a specified position on the surface, and the organic resin in the structure and the organic The resin reaction dissolves part of the organic resin in the structure, releasing the metal particles contained in the conductive resin. By penetrating the structure with the dye, a through-wire can be formed.

[0145] In this manner, a modular light emitting device to which the FPC 402 is connected can be obtained.

[0146] Note that the configuration of this embodiment mode can be used in appropriate combination with the configurations of other embodiments. It is possible.

[0147] (Embodiment 5) In this embodiment mode, electronic devices and lighting devices each including the light-emitting device described in the above embodiment mode are The location will be explained.

[0148] Examples of electronic devices having the light-emitting devices according to the first to fourth embodiments include video cameras, digital cameras, and the like. cameras, goggle-type displays, navigation systems, audio playback devices (car Audio, audio components, computers, game devices, mobile information terminals (mobile computers, mobile phones, portable game consoles, electronic books, etc.), image playback devices equipped with recording media Recording devices (specifically, recording devices for Digital Versatile Discs (DVDs) etc.) Examples of such devices include a display device that can play the media and display the images.

[0149] For example, FIG. 8A shows a flexible display, which includes a main body 9601 and a display unit 960. 2, an external memory insertion section 9603, a speaker section 9604, operation keys 9605, etc. The 9601 body also includes a TV antenna, external input terminal, external output terminal, battery, etc. The display unit 9602 of this display may be the same as that shown in the first to fourth embodiments. The flexible display portion 9602 is made of a light-emitting device. It can be stored by rolling it up inside the 01, making it convenient to carry. A display equipped with the light-emitting device according to any one of the first to fourth embodiments, which has a long life and can be easily produced. The display unit 9602 is lightweight and portable, has a long life, and is reasonably priced. This makes it possible to produce a product that is comparatively inexpensive.

[0150] The light-emitting device according to one embodiment of the present invention can also be a passive matrix type light-emitting device. The light-emitting device can also be used as a lighting device. For example, FIG. 8B shows a tabletop lighting device. The lighting unit 9501 includes a lighting section 9501, a support 9503, a support stand 9505, etc. The light emitting device shown in the embodiment mode is used. In order to use a lighting device, the lighting device shown in this embodiment mode is a lighting device having a curved surface or a flexible It is possible to provide a lighting device having a lighting part that can be bent flexibly. By using a light-emitting device that can be used as a lighting device, the degree of freedom in designing the lighting device is improved. In addition, it is possible to install lighting devices on curved surfaces, such as the ceiling of a car. In addition, by using a flexible light-emitting device, it is possible to realize a roll screen-type lighting, for example. It is possible to manufacture a lighting device that can be stored by rolling up the lighting unit when not in use, such as a lighting device. The lighting device may be a ceiling-mounted lighting device or a wall-mounted lighting device. etc. are also included.

[0151] The lighting device of the present embodiment manufactured by applying the above-described embodiment has high reliability. It is possible to make the device brighter.

[0152] In the above manner, electronic devices and lighting devices can be obtained by using the light-emitting device described in the above embodiment modes. The light emitting device can be applied in a wide range of applications. The present invention can be applied to electronic devices and lighting devices in any field, not limited to the above configuration. .

[0153] Note that the configuration of this embodiment mode can be used in appropriate combination with the configurations of other embodiments. It is possible. [Explanation of symbols]

[0154] 100 Substrates 102 Peeling layer 104 First insulating layer 106 Thin Film Transistor 106a Semiconductor layer 106b Gate insulating layer 106c Gate electrode 130 electrodes 134 EL layer 136 Electrode 137 Bulkhead 138 Light-emitting element 140 Second insulating layer 142 Resin Film 144 Metal Substrate 150 Element section 152 Insulating layer 154 Insulating film 156 Sealing material 160 Groove 200 Color Filter Layer 204 Wiring 206 Interlayer insulating film 208 Planarization film 210 Barrier Film 212 Electrode 214 Color filter substrate 216 Coating film 218 Color filter substrate 250 pixels 252 Drive circuit section 300 Substrates 302 Peeling layer 304 Device formation layer 305 Adhesive Sheet 402 FPC 502 Pixel section 503 Gate side drive circuit 504 Source side drive circuit 508 Wiring 511 Current Control TFT 512 Pixel electrode 513 n-channel TFT 514 p-channel TFT 600 Charge generating layer 9501 Lighting Department 9503 Post 9505 Support stand 9601 Main unit 9602 Display section 9603 External memory slot 9604 Speaker section 9605 Operation key

Claims

[Claim 1] A substrate having flexibility and transparency to visible light; a first insulating layer provided on the substrate; an element portion on the first insulating layer; a second insulating layer covering a side surface and an upper surface of the element portion; a metal substrate on the second insulating layer; the element section includes a light emitting element and a switching element, The light emitting device, wherein at least a portion of the first insulating layer and the second insulating layer are in contact with each other along the outer periphery of the element portion.

Citation Information

Patent Citations

  • Organic EL display device and its manufacture method

    CN101336022A

  • Electronic device

    JP2001242827A

  • Luminescent device

    JP2002184569A

  • Organic semiconductor device, optical head using this, and image forming device

    JP2007287557A

  • Display device and its manufacturing method

    JP2007335403A