Printed object having antibacterial property
A printed material with an absorbent base and non-isothiazoline antibacterial agent overprint layer addresses the inadequate evaluation of antibacterial properties on absorbent substrates, ensuring high safety and effective antibacterial performance without discoloration.
Patent Information
- Application Number
- JP2023057016
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for evaluating the antibacterial properties of printed matter with an antibacterial overprint layer on absorbent substrates, such as paper, are inadequate as they either underestimate the antibacterial properties of the surface or fail to account for safety concerns related to certain antibacterial agents, leading to potential health risks and discoloration issues.
A printed material comprising an absorbent base material with an overprint layer containing a non-isothiazoline organic antibacterial agent, a specific resin, and a solvent, applied via offset printing, which ensures high antibacterial properties and safety without discoloration, using a novel antibacterial test method that evaluates the surface antibacterial activity.
The solution provides printed materials with excellent coating properties, high safety, and effective antibacterial performance on the surface, while avoiding health risks and discoloration, and allows accurate evaluation of antibacterial properties.
Smart Images

Figure 2024144865000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a printed matter having antibacterial properties. [Background technology]
[0002] In recent years, the demand for products with antibacterial treatment (antibacterial products) has increased due to the growing awareness of public health, and various antibacterial products are available on the market. General antibacterial products (e.g., plastics or paper) are imparted with antibacterial properties by kneading an antibacterial agent into the base material, but due to restrictions such as the high price of antibacterial agents and environmental hazards depending on the type, the products in which antibacterial agents are used are limited. Since the antibacterial properties of an antibacterial agent are mainly expressed by the antibacterial agent exposed on the surface, one effective solution is to apply a coating only to the surface of the product in order to make the most of the antibacterial properties while minimizing the amount of antibacterial agent added. In recent years, there have been an increasing number of cases in which antibacterial varnish is overprinted on the surface of printed matter, etc.
[0003] In the case of printed matter, it is common to provide an overprint layer for the purpose of protecting the surface after printing with colored inks. It is a logical method to effectively impart antibacterial properties to the surface of a printed matter by imparting antibacterial properties to this overprint layer, and the market for printed matter with antibacterial overprint layers is also expanding. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2023-006814 A [Patent Document 2] Japanese Patent Application Publication No. 9-39369 Summary of the Invention [Problem to be solved by the invention]
[0005] Incidentally, the antibacterial properties of printed matter having an antibacterial overprint layer have been evaluated in accordance with JIS Z2801 (see Patent Documents 1 and 2). JIS Z2801 is an evaluation method for evaluating the antibacterial properties of product surfaces that do not absorb liquids, such as plastic products. However, according to the inventor's research, it was found that when antibacterial tests are performed in accordance with JIS Z2801 on printed matter having an antibacterial overprint layer applied to a liquid-absorbent substrate such as paper, the bacterial liquid seeps into the substrate, resulting in an evaluation of antibacterial properties despite the low antibacterial properties.
[0006] On the other hand, it is considered desirable to evaluate the antibacterial properties of products that absorb liquids, such as textile products, using the bacterial liquid absorption method described in JIS L1902. However, this method evaluates the overall antibacterial properties of the printed matter, including the inside of the printed matter, and there is a problem in that the antibacterial properties of the most important printed matter surface cannot be evaluated correctly. In other words, in the conventional technology, the antibacterial properties of the surface of the printed matter were not evaluated properly.
[0007] Furthermore, the silver-based antibacterial agent used in Patent Document 1 can have a problem in that the coating film discolors over time.
[0008] Furthermore, the antibacterial agent used in Patent Document 2 is an isothiazolinone organic antibacterial agent, but there have been cases of allergic contact dermatitis in products using isothiazolinone compounds (Ministry of Health, Labour and Welfare, "Regarding serious product accidents associated with the use of cooling pads") and it is known to have safety problems such as strong skin sensitization.
[0009] Therefore, an object of the present invention is to provide a printed matter using an absorbent substrate, which has excellent coatability and coating film physical properties of an overprint layer, can impart high safety and good antibacterial properties to the surface of the printed matter, and does not cause discoloration of the coating film over time. [Means for solving the problem]
[0010] The present inventors discovered a method capable of properly evaluating the antibacterial properties of a printed material having an antibacterial overprint layer applied to an absorbent substrate, and investigated antibacterial compositions to be used in antibacterial overprint layers that have high antibacterial properties even when using this evaluation method, leading to the completion of the present invention.
[0011] That is, the present invention provides a printed matter comprising an absorbent substrate and an overprint layer, the overprint layer is an offset printing layer containing a non-isothiazoline organic antibacterial agent, the content of the organic antibacterial agent in the total amount of the overprint layer is 0.1 to 15% by mass, The printed matter including the overprint layer is a printed matter that exhibits an antibacterial activity value of 0.5 or more in the following antibacterial test. <Antibacterial test> Antibacterial test in which Staphylococcus aureus liquid is applied to a standard agar plate containing 2.5g of yeast extract, 5g of casein pancreatic hydrolysate, 1g of glucose, and 15g of agar powder in 1L of water, then transferred to an absorbent printout and the test bacteria is cultured.
[0012] The present invention also relates to the above printed matter, wherein the organic antibacterial agent is an antibacterial agent that does not fall under Category 1, Category 1A, or Category 1B in terms of skin sensitization in Section 2, Summary of Hazards and Toxicities, of the Safety Data Sheet (SDS).
[0013] The present invention also relates to the above printed matter, wherein the organic antibacterial agent comprises one or more selected from the group consisting of organic halogen-based antibacterial agents, pyridine-based antibacterial agents, haloalkylthio-based antibacterial agents, benzimidazole-based antibacterial agents, isophthalonitrile-based antibacterial agents, phenol-based antibacterial agents, triazine-based antibacterial agents, bromine-based antibacterial agents, quaternary ammonium salt-based antibacterial agents, cationic polymer-based antibacterial agents, and organometallic antibacterial agents.
[0014] The present invention also relates to the above printed matter, wherein the overprint layer contains a resin.
[0015] The present invention also relates to the above printed matter, wherein the resin contains a rosin-modified resin.
[0016] The present invention also relates to the above printed matter, which further comprises an ink layer between the absorbent substrate and the overprint layer. Effect of the Invention
[0017] According to the present invention, it is possible to provide a printed item using an absorbent substrate, which has excellent coatability and coating film physical properties of an overprint layer, and which can impart high safety and good antibacterial properties to the surface of the printed item, and which does not discolor the coating film over time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, the embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the present invention.
[0019] In this specification, a numerical range indicated using "~" includes the numerical values before and after "~" as the minimum and maximum values, respectively. In a plurality of numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range in a certain stage can be arbitrarily combined with the upper limit or lower limit of a numerical range in another stage. In addition, unless otherwise specified, the materials and compounds exemplified in this specification may be used alone or in combination of two or more types.
[0020] The printed article of the present invention comprises an absorbent substrate and an overprint layer.
[0021] The overprint layer in the present invention is a layer obtained by offset printing of the antibacterial composition.
[0022] <Antibacterial composition> The form of the antibacterial composition is not important as long as it can be offset printed, but a preferred form is a composition containing an organic antibacterial agent, a resin, and a solvent.Specific examples of the composition include an oxidative polymerization type composition and a heat set type composition.The oxidative polymerization type composition is a composition containing a component that undergoes oxidative polymerization, such as vegetable oil, as a solvent, and the heat set type composition is a composition containing a component that evaporates due to heat, such as a non-aromatic petroleum solvent, as a solvent.
[0023] <Organic antibacterial agent> To ensure antimicrobial properties of the overprint layer, the antimicrobial composition includes a non-isothiazoline organic antimicrobial agent.
[0024] In the printed matter of the present invention, at least a part of the organic antibacterial agent is present on the surface of the printed matter, and it is considered that the surface of the printed matter may come into contact with the skin when the printed matter is used. From the viewpoint of safety, it is preferable to use an antibacterial agent that does not fall under Category 1, Category 1A, or Category 1B in terms of skin sensitization in the "Summary of Hazards" in Section 2 of the Safety Data Sheet (SDS).
[0025] The organic antibacterial agent preferably contains at least one selected from the group consisting of organic halogen-based antibacterial agents, pyridine-based antibacterial agents, haloalkylthio-based antibacterial agents, benzimidazole-based antibacterial agents, isophthalonitrile-based antibacterial agents, phenol-based antibacterial agents, triazine-based antibacterial agents, bromine-based antibacterial agents, quaternary ammonium salt-based antibacterial agents, cationic polymer-based antibacterial agents, and organometallic antibacterial agents.Moreover, it is more preferable that the antibacterial agent contains a nitrogen atom, and specific examples thereof include pyridine-based antibacterial agents, triazine-based antibacterial agents, quaternary ammonium salt-based antibacterial agents, cationic polymer-based antibacterial agents, etc.
[0026] The content of the organic antibacterial agent is 0.1 to 15% by mass based on the total amount of the composition. If it is less than 0.1% by mass, the antibacterial effect is not stable, while if it exceeds 15% by mass, the necessary and sufficient antibacterial effect is saturated, and the antibacterial agent becomes excessive, which is disadvantageous in terms of both cost and printability, and further, the storage stability of the composition is reduced, and the fastness of the coating film may also be reduced. The content of the antibacterial agent is preferably 0.1 to 10% by mass based on the total amount of the composition, more preferably 0.5 to 7% by mass based on the total amount of the composition, and particularly preferably 0.5 to 5% by mass.
[0027] <Resin> The antibacterial composition of the present invention preferably contains a resin, which improves the coatability of the overprint layer. From the viewpoint of coatability, the resin content is preferably from 5 to 60% by mass, and more preferably from 10 to 50% by mass, of the total amount of the composition.
[0028] The resin in the present invention preferably contains a rosin-modified resin. The rosin-modified resin is not particularly limited as long as it is a resin in which a rosin skeleton is introduced. By containing the rosin-modified resin, it is possible to impart excellent viscoelasticity to the antibacterial composition and obtain stable coating properties. The weight-average molecular weight of the rosin-modified resin is preferably 4,000 to 200,000.
[0029] As the rosin-modified resin, a rosin-modified phenolic resin is preferred since it can suppress the scattering of ink (misting) between the ink mixing rollers of a printing press during offset printing.
[0030] In the present invention, Mw (weight average molecular weight) was measured by gel permeation chromatography (hereinafter referred to as "GPC"). The specific measurement method of GPC is as follows. HLC-8320 manufactured by Tosoh Corporation was used, and a calibration curve was prepared using a standard polystyrene sample. Tetrahydrofuran was used as the eluent, and three TSKgel SuperHM-M columns (manufactured by Tosoh Corporation) were used. The measurement was performed at a flow rate of 0.6 mL / min, an injection volume of 10 μL, and a column temperature of 40° C.
[0031] <Solvent> As the solvent used in the antibacterial composition of the present invention, any conventionally known solvent can be used. From the viewpoint of compatibility with the above-mentioned resin and favorable viscoelasticity and drying property of the antibacterial composition, it is preferable to include at least one selected from vegetable oil, polymerized vegetable oil, fatty acid ester, and non-aromatic petroleum solvent. These solvents may be used alone or in combination of two or more.
[0032] <Vegetable oil> The vegetable oil in the present invention refers to triglycerides, which are esterification products of glycerin and fatty acids, and monoglycerides and diglycerides produced by transesterification. The fatty acids may be saturated or unsaturated fatty acids.
[0033] Representative examples of vegetable oils include hemp seed oil, linseed oil, perilla oil, oiticica oil, olive oil, cacao oil, kapok oil, kaya oil, mustard oil, apricot kernel oil, tung oil, kukui oil, walnut oil, poppy seed oil, sesame oil, rice oil, safflower oil, radish seed oil, soybean oil, radish seed oil, camellia oil, corn oil, rapeseed oil, niger oil, rice bran oil, palm oil, castor oil, sunflower oil, grape seed oil, almond oil, pine seed oil, cottonseed oil, coconut oil, peanut oil, dehydrated castor oil, etc. Particularly preferred are soybean oil, coconut oil, linseed oil, rapeseed oil, and tung oil.
[0034] <Polymerized vegetable oil> The polymerized vegetable oil of the present invention can be obtained, for example, by heating and stirring one or more of the vegetable oils listed above to polymerize them. The vegetable oil may be heated and stirred while blowing oxygen into it. The polymerization reaction may be thermal polymerization, and oxidative polymerization is not essential. As the vegetable oil used to produce the polymerized vegetable oil, soybean oil, palm oil, linseed oil, rapeseed oil, and tung oil are particularly preferred.
[0035] <Fatty acid ester> The fatty acid ester in the present invention may be a vegetable oil ester produced from one or more of the vegetable oils listed above, such as soybean oil, cottonseed oil, linseed oil, rice oil, sunflower oil, tall oil, dehydrated castor oil, canola oil, rapeseed oil, etc.
[0036] Other examples of fatty acid esters include fatty acid monoalkyl ester compounds. The fatty acid constituting the monoester is preferably a saturated or unsaturated fatty acid having 16 to 20 carbon atoms, such as stearic acid, isostearic acid, hydroxystearic acid, oleic acid, linoleic acid, linolenic acid, and eleostearic acid. The alkyl group derived from the alcohol constituting the fatty acid monoalkyl ester compound is preferably a carbon atom having 1 to 10, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, and a 2-ethylhexyl group. These alcohols having an alkyl group can be used alone or in combination of two or more kinds.
[0037] The alcohol constituting the fatty acid ester is preferably a monohydric alcohol.
[0038] <Non-aromatic petroleum solvents> The non-aromatic petroleum solvent in the present invention includes paraffinic, naphthenic, and mixed solvents thereof. Examples of commercially available non-aromatic petroleum solvents include "AF Solvent No. 4", "AF Solvent No. 5", "AF Solvent No. 6", and "AF Solvent No. 7" manufactured by ENEOS Corporation. The content of aromatic hydrocarbons mixed in is preferably 1% by weight or less of the total amount of the non-aromatic petroleum solvent.
[0039] In addition, when a non-aromatic petroleum solvent is used, the aniline point is preferably 60 to 130° C. If the aniline point is 130° C. or lower, the binder resin in the varnish composition has excellent solubility and the fluidity of the varnish composition can be sufficiently ensured, resulting in improved leveling and a printed matter with excellent gloss. If the aniline point is 60° C. or higher, the solvent is easily removed from the printed layer during drying, resulting in a varnish composition with excellent drying properties.
[0040] <Additives> Furthermore, various additives can be used in the antibacterial composition of the present invention, if necessary. Examples of the additives include a dryer and wax.
[0041] <Hair dryer> In the case of an oxidative polymerization type composition, it is preferable to contain a drier as an additive. Examples of the drier include a manganese complex, a cobalt complex, a nickel complex, and a zinc complex.
[0042] <Wax> Waxes are classified into natural waxes and synthetic waxes, and the natural waxes are classified into vegetable waxes, animal waxes, mineral waxes, and petroleum waxes.
[0043] Synthetic waxes are further divided into synthetic hydrocarbons, modified waxes, and hydrogenated waxes. The wax preferably used in the present invention is polyethylene wax, which is classified as a synthetic hydrocarbon.
[0044] <Other ingredients> Furthermore, to the antibacterial composition of the present invention, a leveling agent, an antistatic agent, a surfactant, an antifoaming agent, an antioxidant, etc. may be added as necessary within a range that does not impair the effects of the present invention.
[0045] <Printed material> The printed matter of the present invention is a printed matter including an absorbent substrate and an overprint layer (hereinafter also referred to as an absorbent printed matter), and exhibits antibacterial properties in an antibacterial test using the printed matter as a test specimen. An ink layer may also be included between the absorbent substrate and the overprint layer.
[0046] <Absorbent base material> The substrate of the printed matter is an absorbent substrate (liquid-absorbent substrate). An absorbent substrate is a substrate that absorbs moisture when the substrate is cut into a square piece with four sides of 38 mm and left in a sealed state for 24 hours under conditions of a temperature of 37°C and a humidity of 90% or more. Specific examples of absorbent substrates include paper products such as art paper, coated paper, matte coated paper, wood-free paper, craft paper, sawdust paper, synthetic paper, and cardboard; and textile products such as woven fabrics, nonwoven fabrics, gauze, and filters. Even if the material is metal or plastic, if it has fine gaps on the surface and has the property of absorbing liquid, it becomes an absorbent substrate.
[0047] <Overprint layer> The overprint layer is obtained by offset printing the antimicrobial composition onto the surface of the absorbent substrate or ink layer.
[0048] For offset printing, either a normal lithographic plate that uses dampening water or a waterless lithographic plate that does not use dampening water can be used.
[0049] <Ink layer> When the ink layer is provided, the ink can be formed on the absorbent substrate by using a known printing method such as offset printing, gravure printing, flexographic printing, inkjet printing, silk screen printing, etc. Any ink suitable for each printing method can be used, and is not particularly limited.
[0050] <Absorbent printed matter> The absorbent printed matter is a printed matter in which, when Staphylococcus aureus liquid is applied onto the above-mentioned standard agar plate, transferred onto the printed matter, and left for 24 hours in a sealed state under conditions of a temperature of 37°C and a humidity of 90% or more, the weight increase is preferably 1% or more, and more preferably 3% or more, compared to the weight of the printed matter before transfer. As a transfer method, a method can be used in which the printed matter cut into a square piece with sides of 38 mm is placed in contact with the standard agar plate, a cylindrical weight with a mass of 200 g and a diameter of 35 mm is placed on top of it, and the printed matter is collected after 1 minute.
[0051] The absorbent printed matter of the present invention exhibits antibacterial properties in the following antibacterial test using the printed matter as a test specimen. Exhibiting antibacterial properties means that the antibacterial activity value in the test is greater than 0, and this antibacterial activity value is preferably 1.0 or more, and more preferably 2.0 or more. Antibacterial properties according to the following test can be evaluated using the evaluation method in the examples described below. Note that Escherichia coli can also be evaluated in the same manner. <Antibacterial Test> Antibacterial test in which Staphylococcus aureus liquid is applied to a standard agar plate containing 2.5g of yeast extract, 5g of casein pancreatic hydrolysate, 1g of glucose, and 15g of agar powder in 1L of water, then transferred to an absorbent printout and the test bacteria is cultured.
[0052] The antibacterial test in the present invention will be described in detail below. This antibacterial test is a method for evaluating the antibacterial properties of a printed matter (absorbent printed matter) that includes an absorbent substrate and an overprint layer, and unlike JIS Z2801, this test can properly evaluate the antibacterial properties of the absorbent printed matter in the state of the printed matter.
[0053] This antibacterial test involves applying the test bacteria onto a standard agar medium and then removing excess water, which allows the bacteria to be transferred to an absorbent printed material along with a very small amount of water.The test is conducted under high humidity conditions of 90% or more, which does not affect the cultivation of the bacteria, but there is no abundant moisture that would generate metal ions from inorganic antibacterial agents or promote contact between the bacteria embedded inside the fibers and the antibacterial agent, making this a suitable method for evaluating the antibacterial properties of absorbent printed materials.
[0054] <Test piece> A test piece having the size described below is cut out from a printed matter including an absorbent substrate and an overprint layer containing an antibacterial agent, and the surface on the overprint layer side is used as the evaluation surface.
[0055] OK Topcoat+ (Oji Paper Co., Ltd.) was cut into the sizes listed below to serve as control test pieces.
[0056] <Test strain> Staphylococcus aureus
[0057] <Preparation of test bacteria solution> The test bacteria were cultured on TSA medium at 37°C for 23 hours using the slant culture method, and then suspended in peptone saline to obtain 1.2 x 10 6 A test bacterial solution was prepared to give cfu / mL.
[0058] Here, the TSA medium is an agar medium prepared by dissolving 15 g of tryptone, 5 g of soybean-derived peptone, 5 g of sodium chloride, and 15 g of agar powder in 1 L of ultrapure water, sterilizing the mixture by high-pressure steam at 121°C and 2 atm for 20 minutes, and solidifying the mixture in a sterilized petri dish having a diameter of 90 mm. An example of a commercially available product is tryptone soy agar medium manufactured by Solabia Biokar Diagnostics.
[0059] The peptone saline solution was prepared by dissolving 1 g of casein peptone (Kyokuto Peptone, manufactured by Kyokuto Pharmaceutical Industries Co., Ltd.) and 8.5 g of sodium chloride in 1 L of ultrapure water, and sterilizing the solution with high-pressure steam at 121° C. and 2 atm for 20 minutes.
[0060] <Contact between test specimen and bacteria> 1 mL of the test bacteria liquid was dropped onto the standard agar medium, and the dropped test bacteria liquid was allowed to spread over the entire surface of the standard agar medium, and the excess test bacteria liquid was collected. After 5 minutes, a test piece cut into a square piece with sides of 38 mm was placed in contact with the surface of the standard agar medium, and a cylindrical weight with a mass of 200 g and a diameter of 35 mm was placed on top of it.
[0061] <Recovery of live bacteria immediately after contact with bacteria> One minute after the test piece was brought into contact with the bacteria, the test piece was removed and the viable cell count was immediately measured.
[0062] <Recovery of live bacteria after 24 hours of culture> One minute after the test piece was brought into contact with the bacteria, the test piece was removed and cultured for 24 hours under conditions of a temperature of 37°C and a humidity of 90% or higher, after which the viable bacteria count was measured.
[0063] Here, the standard agar medium is an agar medium prepared by dissolving 2.5 g of yeast extract, 5 g of casein pancreatic hydrolysate, 1 g of glucose, and 15 g of agar powder in 1 L of ultrapure water, sterilizing the mixture by high-pressure steam at 121°C and 2 atm for 20 minutes, and solidifying the mixture in a sterilized petri dish having a diameter of 90 mm. An example of a commercially available product is Standard Plate Count Agar Medium manufactured by Kanto Chemical Co., Ltd.
[0064] The control test piece was also contacted with the bacteria in the same manner as above, and viable bacteria were collected immediately after contact with the bacteria and after 24 hours of incubation.
[0065] <Measurement of viable bacteria count> The test pieces immediately after contact with the bacteria and after 24 hours of culture were washed with 10 mL of SCDLP medium for 30 seconds, and the attached bacteria were washed into the SCDLP medium. The dilution factor of the washout solution was set to 1, and 1 mL of the solution was diluted with 9 mL of SCDLP medium to prepare a 10-fold dilution solution. Furthermore, 1 mL of the 10-fold dilution solution was diluted with 9 mL of SCDLP medium to prepare a 100-fold dilution solution, and a 10-fold dilution series was prepared in the same manner. Using 1 mL of the washout solution or the 10-fold dilution series, the viable bacteria count was measured by the pour plate culture method (cultured at 37°C for 48 hours) using standard agar medium. Each test was performed three times, and the average was taken.
[0066] Here, the SCDLP medium is a liquid medium prepared by dissolving 17 g of casein peptone, 3 g of soybean peptone, 5 g of sodium chloride, 2.5 g of potassium monohydrogen phosphate, 2.5 g of glucose, 1 g of lecithin, and 7 g of polysorbate 80 in 1 L of ultrapure water, and autoclaving at 121 °C and 2 atm for 20 minutes. As a commercially available product, the SCDLP medium "Dai-go" for general bacterial examination manufactured by Shiotani MS Co., Ltd. can be mentioned.
[0067] <Establishment conditions for antibacterial test> The number of viable bacteria after 24-hour culture in the control test piece is 10 times or more the number of viable bacteria immediately after contact with the bacterial cells.
[0068] <Calculation of the number of viable bacteria (M)> M = C × D × V C: Number of colony-forming units in the petri dish in the pour plate culture method D: Dilution factor (dilution factor of the bacterial cell dilution solution dispensed into the petri dish) V: Volume of the SCDLP medium used for elution (mL) Also, when the number of colony-forming units C is 0 when the dilution factor D = 1, substitute <1 into C and set M < V.
[0069] <Calculation of antibacterial activity value (R)> The antibacterial activity value (R) was calculated by the following method. R=(U 24 -U0)-(A 24 -A0) U0: Logarithmic value of the number of viable bacteria immediately after inoculation of the control test piece U 24 : Logarithmic value of the number of viable bacteria after 24 hours of the control test piece A0: Logarithmic value of the number of viable bacteria immediately after contact with the test piece A 24 : Logarithmic value of the number of viable bacteria after 24 hours of the test piece However, when A 0- <U0, replace A0 with U o and calculate. Note that the result of the antibacterial activity value (R) is rounded off at the second digit after the decimal point and expressed with one digit after the decimal point.
Example
[0070] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these. In the examples and comparative examples, "parts" means "parts by mass" and "%" means "% by mass".
[0071] <Resin varnish 1 manufacturing example> 40 parts of rosin-modified phenolic resin with a weight average molecular weight of 36500 and an acid value of 22, synthesized by the method described in JP 2022-54006 A, 15 parts of soybean oil, and 44 parts of AF Solvent No. 7 (manufactured by ENEOS Corporation), a non-aromatic petroleum solvent, were added to a container and heated to 190 ° C. After stirring at the same temperature for 30 minutes, the mixture was allowed to cool, and 1 part of ethyl acetoacetate aluminum diisopropoxide (ALCH manufactured by Kawaken Fine Chemical Co., Ltd.) was added as a gelling agent, and the mixture was stirred at 190 ° C. for 30 minutes to obtain resin varnish 1.
[0072] <Resin varnish 2 manufacturing example> 40 parts of rosin-modified phenolic resin with a weight average molecular weight of 36,500 and an acid value of 22, synthesized by the method described in JP 2022-54006 A, and 59 parts of soybean oil were added to a container and heated to 190° C. After stirring at the same temperature for 30 minutes, the mixture was allowed to cool, and 1 part of ethyl acetoacetate aluminum diisopropoxide (ALCH manufactured by Kawaken Fine Chemical Co., Ltd.) was added as a gelling agent, followed by stirring at 190° C. for 30 minutes to obtain resin varnish 2.
[0073] <Resin varnish 3 manufacturing example> 39.5 parts of rosin-modified phenolic resin with a weight average molecular weight of 131200 and an acid value of 13, synthesized by the method described in JP 2022-54006 A, 15 parts of soybean oil, and 44.5 parts of AF Solvent No. 7 (manufactured by ENEOS Corporation), a non-aromatic petroleum solvent, were added to a container and heated to 190 ° C. After stirring at the same temperature for 30 minutes, the mixture was allowed to cool, and 1 part of ethyl acetoacetate aluminum diisopropoxide (ALCH manufactured by Kawaken Fine Chemical Co., Ltd.) was added as a gelling agent, and the mixture was stirred at 190 ° C. for 30 minutes to obtain resin varnish 3.
[0074] <Resin varnish 4 manufacturing example> 41.5 parts of rosin-modified phenolic resin with a weight average molecular weight of 4700 and an acid value of 10, synthesized by the method described in JP 2022-54006 A, 15 parts of soybean oil, and 42.5 parts of AF Solvent No. 7 (manufactured by ENEOS Corporation), a non-aromatic petroleum solvent, were added to a container and heated to 190 ° C. After stirring at the same temperature for 30 minutes, the mixture was allowed to cool, and 1 part of ethyl acetoacetate aluminum diisopropoxide (ALCH manufactured by Kawaken Fine Chemical Co., Ltd.) was added as a gelling agent, and the mixture was stirred at 190 ° C. for 30 minutes to obtain resin varnish 4.
[0075] <Resin varnish 5 manufacturing example> 34.5 parts of rosin-modified phenolic resin with a weight average molecular weight of 131200 and an acid value of 13 synthesized by the method described in JP 2022-54006 A, 15 parts of soybean oil, and 49.5 parts of AF Solvent No. 7 (manufactured by ENEOS Corporation), a non-aromatic petroleum solvent, were added to a container and heated to 190 ° C. After stirring at the same temperature for 30 minutes, the mixture was allowed to cool, and 1 part of ethyl acetoacetate aluminum diisopropoxide (ALCH manufactured by Kawaken Fine Chemical Co., Ltd.) was added as a gelling agent, and the mixture was stirred at 190 ° C. for 30 minutes to obtain resin varnish 5.
[0076] <Resin varnish 6 manufacturing example> 49.5 parts of petroleum resin, Nippon Oil Neopolymer 160 (manufactured by ENEOS Corporation, weight average molecular weight 3500, acid value 30), 15 parts of soybean oil, and 34.5 parts of non-aromatic petroleum solvent, AF Solvent No. 7 (manufactured by ENEOS Corporation), were added to a container and heated to 190°C. After stirring at the same temperature for 30 minutes, the mixture was allowed to cool, and 1 part of ethyl acetoacetate aluminum diisopropoxide (ALCH, manufactured by Kawaken Fine Chemicals Co., Ltd.) was added as a gelling agent, and the mixture was stirred at 190°C for 30 minutes to obtain resin varnish 6.
[0077] <Production Example of Antibacterial Composition> Example 1 78 parts of resin varnish 1, 5 parts of tung oil, 10 parts of AF Solvent No. 7 (manufactured by ENEOS Corporation), a non-aromatic petroleum solvent, 0.5 parts of manganese octylate as a dryer, 0.5 parts of cobalt octylate, 3 parts of polyethylene wax, and 3 parts of antibacterial agent A (PBM-OJ) were charged and antibacterial composition 1 was obtained using a three-roll mill according to a conventional method.
[0078] Examples 2 to 11 The antibacterial compositions of Examples 2 to 11 were obtained in the same manner as Example 1, except that the types and amounts of raw materials shown in Table 1 were used. Note that the numerical values showing the blending amounts in the table represent "parts by mass", and blank spaces indicate that no blend was used.
[0079] Comparative Examples 1 to 5 According to the compositions shown in Table 1, antibacterial compositions of Comparative Examples 1 to 5 were obtained in the same manner as in the above Examples.
[0080] Details of the raw materials listed in Table 1 are as follows. Soybean oil: Regenerated soybean oil (iodine value 117) Tung oil: Tung oil (iodine value 170) AF Solvent No. 7: ENEOS Corporation AF Solvent No. 4: ENEOS Corporation Polyethylene wax: Morimura Chemical Co., Ltd. Manganese octylate: manufactured by Nippon Chemical Industries Co., Ltd. Cobalt octylate: manufactured by Nippon Chemical Industries Co., Ltd. Antibacterial agent A: Triazine antibacterial agent ("PBM-OJ" manufactured by MIC Corporation) Antibacterial agent B: Quaternary ammonium antibacterial agent ("Amorden JM" manufactured by Daiwa Chemical Industry Co., Ltd.) Antibacterial agent C: Cationic polymer antibacterial agent ("FC-V20S" manufactured by Fuji Chemical Co., Ltd.) Antibacterial agent D: Silver-based antibacterial agent ("AG-300" manufactured by Toagosei Co., Ltd.) Antibacterial agent E: Silver-zinc-based antibacterial agent ("Biocide TB-B100" manufactured by Taisho Technos Co., Ltd.)
[0081] <Skin sensitization> This was judged based on the description of skin sensitization in Section 2, Hazardous Hazards Summary, of the Safety Data Sheet (SDS). ○ Not applicable to Category 1, Category 1A, or Category 1B ×...Corresponds to Category 1, Category 1A, or Category 1B
[0082] <Method of preparing test samples for antibacterial testing in the present invention> The obtained antibacterial composition was printed on one side of coated cardboard on which a solid image had been printed using an oil-based offset ink ("TK NEX NV Sumi MZ" manufactured by Toyo Ink Co., Ltd.) to a density of 1.8, using an RI tester (manufactured by Tester Sangyo Co., Ltd.) to apply 0.25 mL of the composition to create a test sample.
[0083] <Antibacterial evaluation (antibacterial test in the present invention)> The evaluation was carried out by the antibacterial activity test of the present invention described above. From the obtained antibacterial activity value (R), the antibacterial properties were evaluated as follows: If the antibacterial activity value is 1.0 or more, the antibacterial effect in this embodiment can be evaluated as being good. ○: 2.0 or higher △: Less than 2.0, 1.0 or more ×: Less than 1.0
[0084] <How to prepare test samples for antibacterial evaluation (JIS Z2801)> A solid image of the obtained antibacterial composition was printed on a polyethylene film in an amount of 0.25 mL using an RI Tester (manufactured by Tester Sangyo Co., Ltd.) to prepare a test sample.
[0085] <Antibacterial evaluation (JIS Z2801)> The antibacterial properties of the antibacterial composition printed on the polyethylene film were evaluated according to the method of JIS Z2801. The obtained antibacterial activity value (R 2801 ) and the antibacterial properties were evaluated as follows: If the antibacterial activity value is 1.0 or more, the antibacterial effect in this embodiment can be evaluated as being good. ○: 2.0 or higher △: Less than 2.0, 1.0 or more ×: Less than 1.0
[0086] <Misting evaluation> 1.5 mL of the antibacterial composition was placed on an Incometer-type misting tester and rotated at 1800 rpm for 2 minutes. The antibacterial composition scattered as it rotated, and the misting quality was compared based on the weight increase of a piece of paper (15 cm wide, 30 cm long) placed directly under the rotating body. When the misting was poor, the amount of antibacterial composition scattered increased and the weight of the paper increased. The evaluation criteria were as follows: ○ The weight increase of the paper is less than 0.1g △: Paper weight increase is 0.1g or more but less than 0.2g × The weight of the paper increases by 0.2g or more
[0087] <How to create a test sample for gloss evaluation> A solid image was printed on OK Topcoat+ (Oji Paper Co., Ltd.) using an RI Tester (Tester Sangyo Co., Ltd.) in an amount of 0.25 mL of the obtained antibacterial composition to prepare a test sample.
[0088] <Gloss evaluation> The gloss of the obtained test sample was measured using a gloss meter (GLOSS METER GM-26D, manufactured by Murakami Color Science Laboratory, incident angle 60°). ◎ Gloss value is 60 or more ○ Gloss value is 50 or more and less than 60 △: Gloss value is 40 or more and less than 50 × Gloss value is less than 40
[0089] <How to prepare test samples for evaluating abrasion resistance> A solid image was printed on OK Topcoat+ (Oji Paper Co., Ltd.) using an RI Tester (Tester Sangyo Co., Ltd.) in an amount of 0.25 mL of the obtained antibacterial varnish composition to prepare a test sample.
[0090] <Abrasion resistance evaluation> The abrasion resistance of the obtained test sample was measured using a Gakushin type abrasion fastness tester (manufactured by Tester Sangyo Co., Ltd.) (measurement conditions: 500 g x 50 times, paper: OK Topcoat+ (Oji Paper Co., Ltd.)). ○ The number of times the print surface was chipped was 50 times. △: The number of times the print surface is damaged is between 10 and 50 times. × The number of times the print surface is damaged is less than 10
[0091] <How to prepare test samples for evaluating discoloration of coating film> A solid image was printed on OK Topcoat+ (Oji Paper Co., Ltd.) using an RI Tester (Tester Sangyo Co., Ltd.) in an amount of 0.25 mL of the obtained antibacterial composition to prepare a test sample.
[0092] <Evaluation of discoloration of coating film> The obtained test samples were stored at 25° C. for 180 days, and the degree of discoloration of the coating film was visually evaluated. ○ No change in hue of the overprint layer over time ×: The hue of the overprint layer changes over time.
[0093] The above results are shown in Table 1.
[0094] [Table 1]
[0095] As described above, the printed matter of the examples had excellent coatability and coating film physical properties of the overprint layer, and was able to provide a printed matter with a high level of safety and good antibacterial properties on the surface of the printed matter, with no discoloration of the coating film over time. On the other hand, Comparative Examples 1 and 2, which used a silver-based antibacterial agent, showed low antibacterial properties in the antibacterial test of the present invention, and the coating film also showed significant discoloration. Comparative Example 3, in which the content of the antibacterial agent was lower than the range of the present invention, had poor antibacterial properties, while Comparative Example 4, in which the content of the antibacterial agent was higher than the range of the present invention, showed antibacterial properties but had poor gloss and abrasion resistance. In Comparative Example 5, in which the substrate was a non-absorbent substrate, the antibacterial test (test for absorbent printed matter) in the present invention was not possible to measure since the bacterial solution was not absorbed by the printed matter.
Claims
1. A printed matter comprising an absorbent substrate and an overprint layer, the overprint layer is an offset printing layer containing a non-isothiazoline organic antibacterial agent, the content of the organic antibacterial agent in the total amount of the overprint layer is 0.1 to 15% by mass, A printed matter including the overprint layer exhibits an antibacterial activity value of 0.5 or more in the following antibacterial test. <Antibacterial Test> Antibacterial test in which the Staphylococcus aureus liquid is applied to a standard agar plate containing 2.5 g of yeast extract, 5 g of casein pancreatic hydrolysate, 1 g of glucose, and 15 g of agar powder in 1 L of water, then transferred to an absorbent printout and the test bacteria is cultured.
2. The printed matter according to claim 1, wherein the organic antibacterial agent is an antibacterial agent that does not fall under Category 1, Category 1A, or Category 1B in skin sensitization in Section 2 of the Safety Data Sheet (SDS) Summary of Hazards and Toxicities.
3. 2. The printed matter according to claim 1, wherein the organic antibacterial agent comprises at least one selected from the group consisting of organic halogen-based antibacterial agents, pyridine-based antibacterial agents, haloalkylthio-based antibacterial agents, benzimidazole-based antibacterial agents, isophthalonitrile-based antibacterial agents, phenol-based antibacterial agents, triazine-based antibacterial agents, bromine-based antibacterial agents, quaternary ammonium salt-based antibacterial agents, cationic polymer-based antibacterial agents, and organometallic antibacterial agents.
4. The printed matter of claim 1 , wherein the overprint layer comprises a resin.
5. The printed matter of claim 4 , wherein the resin comprises a rosin-modified resin.
6. The printed matter according to any one of claims 1 to 5, further comprising an ink layer between the absorbent substrate and the overprint layer.
Citation Information
Patent Citations
Antibacterial offset printed matter and production thereof
JP1997039369A
Antibacterial overprint varnish, antibacterial printed matter, and method for producing antibacterial printed matter