Cast iron pipe

A synthetic resin paint with multiple acrylic resin emulsions of varying glass transition temperatures, combined with a zinc coating, addresses the peeling and scratching issues of water-based paints on cast iron pipes, providing enhanced scratch resistance and quick drying without high-temperature film formation.

JP2024145044APending Publication Date: 2024-10-15KURIMOTO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023057274
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing cast iron pipes coated with water-based paints suffer from soft coating films that peel off when pipes come into contact at high temperatures, leading to scratching and blocking issues.

Method used

A coating layer made of synthetic resin paint containing multiple types of acrylic resin emulsions with different glass transition temperatures, combined with a zinc sprayed coating layer, provides enhanced scratch resistance over a wide temperature range.

Benefits of technology

The coating layer prevents scratching and blocking during transportation and joining of pipes, maintaining film integrity across varying temperatures, while also ensuring quick drying and reduced environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145044000001
    Figure 2024145044000001
Patent Text Reader

Abstract

To provide a cast iron pipe which is less likely to cause scratches in a coating film at the time of conveyance and joint of a pipe, and is excellent in scratch resistance, in a wider temperature range.SOLUTION: A cast iron pipe has a coating layer composed of a synthetic resin coating material containing a plurality of kinds of acrylic resin emulsions having different glass transition temperatures (Tg) on a pipe outer surface.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cast iron pipe having a coating layer of synthetic resin paint on its outer surface, and in particular to a cast iron pipe having excellent scratch resistance over a wide temperature range. [Background technology]

[0002] Traditionally, the outer surface of cast iron pipes used for water supply and sewerage pipes etc. has been prescribed in the Japan Ductile Iron Pipe Association standard JDPA Z 2010 "Synthetic resin coating for ductile cast iron pipes" to be coated with a zinc-based primer (zinc-based thermal spray or zinc-rich paint) to prevent corrosion of water pipes buried underground. It also prescribes that a coating layer be formed by coating the zinc-based primer layer with a paint that meets the criteria of the Japan Water Works Association standard JWWA K 139 "Synthetic resin coating for ductile cast iron pipes for water supply".

[0003] In order to provide sufficient corrosion protection to the outer surface of the cast iron pipe as a top coat of this zinc-based primer layer, the conventional method requires a primary coating of water-based paint and then a secondary coating of solvent-based paint, and therefore at least two steps are required for the corrosion protection treatment of the outer surface of the cast iron pipe.To simplify this process and reduce costs, a water-based paint that uses an acrylic resin emulsion with a specified glass transition temperature (Tg) and has improved drying properties and whitening resistance has been developed (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-002330 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the coating layer made of the water-based paint disclosed in Patent Document 1 has a problem in that the coating film is soft and, for example, when the pipes are placed side by side in a high-temperature storage area, the pipes come into contact with each other, causing blocking in which the coating film peels off, and there is room for improvement in scratch resistance.

[0006] Therefore, an object of the present invention is to provide a cast iron pipe having an outer surface coating layer that has excellent scratch resistance and is less likely to be scratched during transportation or joining of the pipe over a wider temperature range. [Means for solving the problem]

[0007] The inventors have discovered that the above-mentioned problems can be solved by providing a coating layer made of a synthetic resin paint containing multiple types of acrylic resin emulsions having different glass transition temperatures, and that a cast iron pipe can be obtained having a coating layer with excellent scratch resistance that makes it difficult for the coating to be scratched during transportation or joining of the pipe over a wider temperature range, and have completed the present invention.

[0008] That is, the present invention provides [1] A cast iron pipe having a coating layer on its outer surface made of synthetic resin paint containing multiple types of acrylic resin emulsions with different glass transition temperatures (Tg); [2] The cast iron pipe according to the above [1], wherein the synthetic resin coating further contains an acrylic resin dispersion; and [3] The cast iron pipe according to the above [1] or [2] further has a zinc-based sprayed coating layer under the synthetic resin coating layer. Regarding. Effect of the Invention

[0009] According to the present invention, by providing a coating layer on the outer surface of the pipe made of a synthetic resin paint containing multiple types of acrylic resin emulsions having different glass transition temperatures, it is possible to obtain a cast iron pipe having excellent scratch resistance over a wider temperature range, in which the coating film is less likely to be scratched during transportation or joining of the pipe. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The cast iron pipe of the present invention is characterized in that the outer surface of the pipe has a coating layer made of a synthetic resin paint containing multiple types of acrylic resin emulsions having different glass transition temperatures (Tg), and has excellent scratch resistance in a wide temperature range, in which the coating film is less likely to be scratched during pipe transportation or joining. This makes it possible to prevent blocking, in which the coating film peels off, even when the cast iron pipes are stored in a cast iron pipe storage area in summer, in a state where they come into contact with each other. By using an acrylic resin emulsion with a higher glass transition temperature in combination with an acrylic resin emulsion with a lower glass transition temperature, not only is the scratch resistance excellent over a wide temperature range, but the drying is quick and the minimum film formation temperature can be sufficiently reduced, and a cast iron pipe with stable quality can be obtained without requiring a high coating temperature that would cause poor film formation.

[0011] In this specification, the terms "(meth)acrylic", "(meth)acrylic acid", and the like are general terms for "methacrylic", "acrylic", "methacrylic acid", and "acrylic acid", respectively.

[0012] <Synthetic resin paint> The synthetic resin coating material used in the present invention uses a combination of two or more acrylic resin emulsions having different glass transition temperatures. The acrylic resin emulsions having different glass transition temperatures may include three types, or four or more types. In the synthetic resin coating material, the temperature difference in glass transition temperature between the acrylic resin emulsion having the highest glass transition temperature and the acrylic resin emulsion having the lowest glass transition temperature is preferably within the range of 30°C to 85°C, more preferably within the range of 40°C to 80°C. The combination of acrylic resin emulsions having different glass transition temperatures can be determined in consideration of the above-mentioned temperature difference and the theoretical glass transition temperature of the entire resin. The theoretical glass transition temperature of such an entire resin is preferably 35 to 45°C, more preferably 40 to 45°C. By making the theoretical glass transition temperature of the entire resin 35°C or higher, it becomes easier to obtain the desired coating hardness and to ensure scratch resistance, and by making it 45°C or lower, for example, the temperature during painting is set to 70°C or lower, so that a film can be formed even on a pipe preheated to a temperature at which the water-based paint does not bump, and water resistance and corrosion resistance tend to be easily ensured. The glass transition temperature was measured by a differential scanning calorimeter (DSC).

[0013] The synthetic resin paint used in the present invention is a water-based paint. The term "water-based" is used to distinguish it from a solvent-based paint, and means that an aqueous medium, preferably water, is used as the medium, and does not exclude the use of a component containing a certain amount of organic solvent. Therefore, an aqueous solvent, preferably water, is used as the solvent for the synthetic resin paint used in the present invention. In addition, a small amount of organic solvent may be added to adjust the interfacial tension and improve wettability to the zinc-based sprayed coating.

[0014] (Acrylic resin emulsion) The acrylic resin emulsion in the present invention is an emulsion of an acrylic resin stabilized in water by using an emulsifier, and may contain additives such as a surfactant as necessary. The acrylic resin constituting the acrylic resin emulsion is usually a polymer obtained by polymerizing one or more acrylic monomers selected from the group consisting of acrylic acid, methacrylic acid and their esters, but also includes a copolymer obtained by copolymerizing one or more acrylic monomers with one or more monomers other than the acrylic monomers. Of the above acrylic monomers, specific examples of the acrylic acid esters and methacrylic acid esters include, for example, alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, and stearyl (meth)acrylate, benzyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and glycidyl (meth)acrylate. Also, a specific example of a monomer other than the acrylic monomers is styrene.

[0015] The Tg of the acrylic resin in the acrylic resin emulsion used in the present invention is not particularly limited, but a higher Tg of about 90°C or lower Tg of about 1°C can be used.

[0016] The synthesis method of the acrylic resin is not particularly limited, and a known polymerization method such as emulsion polymerization can be used. For example, the acrylic resin emulsion can be prepared by charging a mixture of monomers, emulsifiers, polymerization initiators, etc. (monomer premix) all at once into a reaction vessel containing a predetermined amount of water, emulsion-polymerizing the monomer mixture, and cooling and neutralizing the reactants after the reaction is completed to obtain the desired aqueous acrylic resin emulsion.

[0017] The emulsifier used in the above reaction is an essential component for forcibly emulsifying the obtained acrylic resin in water to obtain an acrylic resin emulsion. Specific examples thereof include anionic polymeric emulsifiers such as fatty acid soap, rosin acid soap, alkyl sulfonate, alkyl benzene sulfonate, dialkyl aryl sulfonate, alkyl sulfosuccinate, and polyoxyethylene alkyl sulfate; and nonionic polymeric emulsifiers such as polyoxyethylene alkyl ether, polyoxyethylene alkyl aryl ether, polyoxyethylene sorbitan fatty acid ester, and oxyethylene oxypropylene block copolymer. These emulsifiers can be used alone or in combination of two or more. It is also possible to use a combination of nonionic and anionic emulsifiers, and cationic surfactants, amphoteric surfactants, and the like. The amount of emulsifier used is preferably 0.3 to 3 parts by weight based on 100 parts by weight of the total amount of polymerizable monomers to be subjected to emulsion polymerization.

[0018] Examples of the polymerization initiator used in the emulsion polymerization reaction include aqueous catalysts such as potassium persulfate, sodium persulfate, ammonium persulfate, and hydrogen peroxide; and oil-based catalysts such as tert-butyl hydroperoxide and cumene hydroperoxide. The amount of the polymerization initiator used is preferably 0.1 to 0.7 parts by weight based on 100 parts by weight of the polymerizable monomer to be subjected to the emulsion polymerization.

[0019] In addition, in the emulsion polymerization reaction, molecular weight regulators such as chain transfer agents and polymerization terminators, and polymerization rate regulators can be appropriately used during polymerization to adjust the molecular weight. Furthermore, the molecular weight may be controlled by interrupting the reaction by cooling. Examples of chain transfer agents include mercaptans such as t-dodecyl mercaptan, n-todecyl mercaptan, octyl mercaptan, n-tetradecyl mercaptan, and n-hexyl mercaptan, terpinolene, t-terpinene, α-methylstyrene dimer, ethyl xanthogen disulfide, diisopropyl xanthogen sulfide, aminophenyl sulfide, and tetraethyl thiuram disulfide, which can be used alone or in combination of two or more. The amount of the chain transfer agent used is preferably 1.0 part by weight or less based on 100 parts by weight of the total amount of polymerizable monomers to be subjected to emulsion polymerization.

[0020] Examples of polymerization terminators include hydroquinone (phenol), amine-based sulfur, hydroxylamine sulfate, ammonia, caustic soda, caustic potassium, and other agents that have a polymerization terminator effect. These agents can be used alone or in combination of two or more. The amount of the agent used varies depending on the type of polymerization inhibitor and its reactivity with the monomer. In the emulsion polymerization reaction, in addition to the emulsifier, chain transfer agent, and polymerization initiator, various additives such as electrolytes and pH adjusters may be used in combination as necessary.

[0021] Specific examples of the acrylic resin emulsions as described above include Boncoat CM-8430, Boncoat CP-6450 (manufactured by DIC Corporation), NeoCryl A655 (manufactured by DSM), Boncoat EC-5400EF (manufactured by DIC Corporation), JE-1056 (manufactured by Seiko PMC Corporation), AE872D (manufactured by E-Tech Co., Ltd.), ES-90 (manufactured by Japan Coating Resins Co., Ltd.), 727 (manufactured by Japan Coating Resins Co., Ltd.), and Joncryl 583-A (manufactured by BASF).

[0022] The total content of the acrylic resin emulsion in the synthetic resin paint of the present invention is preferably 20% by mass or more, more preferably 25% by mass or more, as solid content. By making the total content of the acrylic resin emulsion 20% by mass or more, as solid content, there is a tendency for better improvement in corrosion resistance. The total content of the acrylic resin emulsion in the synthetic resin paint is preferably 40% by mass or less, as solid content, more preferably 35% by mass or less. By making the content of the acrylic resin emulsion 40% by mass or less, as solid content, there is a tendency for more suppression of deterioration of workability.

[0023] (Acrylic resin dispersion) The synthetic resin coating material of the present invention can further contain an acrylic resin dispersion. By containing an acrylic resin dispersion, a coating film with better corrosion resistance can be formed. An acrylic resin dispersion is a self-emulsifying dispersion in which some hydrophilic group is chemically introduced into an acrylic resin skeleton, and the resin itself has emulsifying ability, and additives such as a neutralizer and an antifoaming agent are included as necessary. The acrylic resin skeleton constituting the acrylic resin dispersion can usually be the same as the acrylic resin constituting the above-mentioned acrylic resin emulsion. Representative examples of components having a hydrophilic group to be introduced into the acrylic resin skeleton include, but are not limited to, acids such as (meth)acrylic acid, crotonic acid, citraconic acid, maleic acid, fumaric acid, itaconic acid, and maleic anhydride; and (meth)acrylic acid alkyl esters having an alkyl group of 1 to 24 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, and dodecyl (meth)acrylate. The acrylic resin dispersions may be used alone or in combination of two or more.

[0024] Specific examples of the above-mentioned acrylic resin dispersion include Watersol S-720 (manufactured by DIC Corporation), Acronal YJ-1100D (manufactured by BASF Dispersions), Bayhydrol XP2470 (manufactured by Bayer AG), and the like.

[0025] When an acrylic resin dispersion is used, the content of the acrylic resin dispersion in the synthetic resin paint is preferably 0.5% by mass or more, more preferably 1% by mass or more, as solid content. By making the content of the acrylic resin dispersion 0.5% by mass or more, as solid content, better corrosion prevention tends to be obtained. The content of the acrylic resin dispersion in the synthetic resin paint is preferably 5% by mass or less, as solid content, in consideration of workability, more preferably 2.5% by mass or less. By making the content of the acrylic resin dispersion 5% by mass or less, or even 2.5% by mass or less, as solid content, it tends to suppress the aggregation of particles, suppress adhesion in the pipe during application work, and further improve workability.

[0026] (Film-forming aid) It is preferable that the synthetic resin coating material of the present invention contains a film-forming auxiliary. The film-forming auxiliary is generally used for the purpose of lowering the minimum film-forming temperature of the synthetic resin coating material. Examples of the film-forming auxiliary used in the present invention include propylene glycol, propylene glycol monomethyl ether (PGMME), propylene glycol monoethyl ether, propylene glycol monopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono n-butyl ether, ethylene glycol monoiso-butyl ether, ethylene glycol monotert-butyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono n-butyl ether, ethylene glycol monoiso-butyl ether, diethylene glycol monotert-butyl ether, and 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, and those used in the present technical field for the purpose of lowering the minimum film-forming temperature, such as high boiling point solvents, can be used without particular restriction. In addition, these can be used alone or in combination of two or more.

[0027] When using a film-forming aid, the content of the film-forming aid in the synthetic resin paint is not particularly limited as long as it is an amount that can lower the minimum film-forming temperature to the desired range, that is, 15 to 35 ° C, preferably 18 to 30 ° C, more preferably 18 to 25 ° C, and can be appropriately set according to the type of acrylic resin used. The content of the film-forming aid in the synthetic resin paint is preferably 2 mass % or more, more preferably 3 mass % or more. By using the film-forming aid, the acrylic resin emulsion with a high glass transition temperature tends to become more compatible, and the minimum film-forming temperature tends to be easier to lower. Furthermore, by setting the content of the film-forming aid to 2 mass % or more, it tends to be easier to adjust the Tg and the minimum film-forming temperature to the desired range. In addition, the content of the film-forming aid in the synthetic resin paint is preferably 5 mass % or less, more preferably 4 mass % or less. By setting the content of the film-forming aid to 5 mass % or less, a good coating drying speed tends to be achieved.

[0028] The minimum film-forming temperature of the synthetic resin paint of the present invention is preferably 15° C. or higher, and more preferably 18° C. or higher. The minimum film-forming temperature of the synthetic resin paint of the present invention is preferably 35° C. or lower, more preferably 30° C. or lower, and even more preferably 25° C. or lower. The minimum film-forming temperature is a value measured in accordance with JIS K 6828-2 Synthetic resin emulsions Part 2: Determination of whitening temperature and minimum film-forming temperature.

[0029] (Pigments) In order to impart sufficient coloring and rust prevention to the synthetic resin coating material, pigments can be blended. Specific examples include color pigments such as titanium dioxide, iron oxide, carbon black (for example, trade name MA100, manufactured by Mitsubishi Chemical Corporation), cyanine blue, and cyanine green; extender pigments such as calcium carbonate, talc, barium sulfate, and clay; and rust prevention pigments such as zinc phosphate, calcium phosphate, and aluminum phosphomolybdate. These may be used alone, or two or more of them may be mixed together as necessary.

[0030] Among the pigments, the content of the rust-preventive pigment in the synthetic resin paint is not particularly limited, but is preferably 0.1% by mass or more, and more preferably 1% by mass or more. By making the content of the rust-preventive pigment 0.1% by mass or more, the corrosion resistance of the coating film tends to be improved. The content of the rust-preventive pigment in the synthetic resin paint is preferably 5% by mass or less, and more preferably 4% by mass or less. By making the content of the rust-preventive pigment 5% by mass or less, the water resistance of the coating film tends to be good.

[0031] (Other Ingredients) In addition to the above components, known additives can be added to the synthetic resin paint as needed. Other additives include known additives such as antifoaming agents made of silicone or organic polymers; surface conditioners made of silicone or organic polymers; viscosity adjusters (anti-sagging agents) made of amide wax, organic bentonite, etc.; matting agents made of silica, alumina, etc.; dispersants made of polycarboxylates, etc.; ultraviolet absorbers made of benzophenone, etc.; hindered amine light stabilizers; phenolic antioxidants; waxes, etc. These can be used alone or in combination as needed.

[0032] The synthetic resin paint is produced using equipment commonly used for paint production. The production method is not particularly limited, but for example, a desired paint can be obtained by adding a pigment, additives (pigment dispersant, viscosity modifier, etc.), solvent, etc. to a commercially available resin component, and then dispersing the mixture using a roll mill, SG mill, disperser, etc.

[0033] The formation of the coating layer using the synthetic resin paint is not particularly limited, but is usually performed after heating the cast iron pipe. The surface temperature of the cast iron pipe before coating with the synthetic resin paint is preferably 50 to 80°C. If the temperature is less than 50°C, the coating film is difficult to dry and scratch resistance tends to deteriorate, and if the temperature exceeds 80°C, the water in the paint tends to boil. The coating method is not particularly limited, but it can be applied by a method such as brush coating, roller coating, air spray coating, airless spray coating, immersion coating, or shower coat coating.

[0034] The thickness of the coating layer of the synthetic resin paint is appropriately set depending on the application of the cast iron pipe to be coated, and is not particularly limited. For example, in the case of a cast iron pipe used for water supply and sewerage, the thickness can be appropriately set in the range of approximately 30 to 120 μm.

[0035] The cast iron pipe of the present invention preferably further has a zinc-based sprayed coating layer on the outer surface of the cast iron pipe and underneath the synthetic resin paint coating layer, and more preferably, this zinc-based sprayed coating has been subjected to a sealing treatment.

[0036] <Zinc-based spray coating layer> The zinc-based spray coating is not particularly limited, but examples thereof include zinc spray coating, zinc-aluminum alloy spray coating, zinc-aluminum pseudoalloy spray coating, zinc-silicon-containing aluminum pseudoalloy spray coating, zinc-silicon-manganese-containing aluminum pseudoalloy spray coating, and zinc-tin alloy spray coating. Prior to this step, it is preferable to carry out surface preparation such as blasting and cleaning on the outer surface of the pipe as necessary. The zinc-aluminum pseudoalloy refers to a zinc-aluminum alloy in which sprayed zinc and aluminum overlap irregularly to form a zinc-aluminum alloy in appearance.

[0037] The thickness of the zinc-based sprayed coating can be appropriately set depending on the type of spray material and the application of the resulting cast iron pipe, but for water pipes it is preferably about 20 μm to 250 μm, more preferably 50 to 150 μm.

[0038] The thermal spraying method is not particularly limited, but examples thereof include gas thermal spraying, arc thermal spraying, and plasma thermal spraying. More specifically, examples include a method in which zinc, a zinc-aluminum pseudoalloy or a zinc-aluminum alloy, or a zinc-silicon manganese-containing aluminum pseudoalloy is sprayed onto a cast iron pipe that is rotated and moved in the axial direction by a fixed thermal spray gun, and a method in which zinc is sprayed onto a rotating cast iron pipe while a thermal spray gun is moved.

[0039] The thickness of the sprayed coating layer is 130g / m2 for zinc spraying in the Japan Ductile Iron Pipe Association standard JDPA Z 2010-2009 "Ductile Cast Iron Pipe Synthetic Resin Coating" from the viewpoint of corrosion prevention. 2 It is stipulated that the thickness should be 300 g / m or more, which corresponds to a thickness of 20 μm. 2 Less than 260 g / m 2 The following is more preferable: When a zinc-aluminum pseudoalloy, a zinc-aluminum alloy, a zinc-silicon-containing aluminum pseudoalloy, or a zinc-silicon-manganese-containing aluminum pseudoalloy is sprayed, the coating weight is 130 to 600 g / m from the viewpoint of corrosion resistance. 2 The range is 180 to 500 g / m 2 The range is preferably 200 to 400 g / m 2 The range is more preferable.

[0040] <Sealing treatment> In the cast iron pipe of the present invention, it is preferable to perform a conventional sealing treatment on the surface of the above-mentioned zinc-based sprayed coating layer to provide a sealing treatment layer, which seals the pores in the zinc-based sprayed coating layer and further enhances the corrosion prevention effect.

[0041] The sealing treatment is not particularly limited, and any treatment generally used in the present technical field can be used. For example, treatment with an aqueous treatment liquid containing a resin component such as an acrylic resin, an epoxy resin, or an acrylic silicone resin used in metal coating, an inorganic compound such as colloidal silica, and additives such as a surface conditioner can be used.

[0042] The method for applying the sealing treatment agent to the zinc-based thermal spray coating formed on the outer surface of the cast iron pipe is not particularly limited, but examples include brush coating, roller coating, air spray coating, airless spray coating, dip coating, shower coat coating, and the like.

[0043] The thickness of the applied sealing agent can be appropriately set depending on the type of spray material and the use of the resulting cast iron pipe, but is preferably, for example, about 5 to 30 μm. In particular, in the case of cast iron for water pipes, the thickness is preferably 30 μm or less, more preferably 20 μm or less, and preferably 5 μm or more, more preferably 10 μm. If the thickness is thinner than 5 μm, the sealing effect may not be sufficient over a long period of time, and if the thickness is thicker than 30 μm, drying may be insufficient.

[0044] <Cast iron pipes> The cast iron pipe of the present invention has excellent scratch resistance in a wider temperature range, in which the coating film is less likely to be scratched during transportation or joining of the pipes, by using a combination of two or more acrylic resin emulsions having different glass transition temperatures. This makes it possible to suppress the occurrence of blocking, in which the coating film peels off, even when the cast iron pipes are stored in a cast iron pipe storage area in the summer, in a state where they come into contact with each other. In addition, since the cast iron pipe of the present invention does not use a solvent-based paint, it has almost no solvent odor and is environmentally friendly. In addition, by using an acrylic resin emulsion having a higher glass transition temperature in combination with an acrylic resin emulsion having a lower glass transition temperature, not only is the scratch resistance excellent in a wider temperature range, but the drying is quick and the minimum film formation temperature can be sufficiently reduced, and a cast iron pipe of stable quality can be obtained without requiring a high coating temperature that causes film formation failure. EXAMPLES

[0045] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0046] First, the components used in the examples and comparative examples are shown below. <Zinc thermal spraying> Zinc-silicon-manganese-containing aluminum pseudoalloy thermal spray coating <Synthetic resin paint> Acrylic resin emulsion A: Boncoat CM-8430 (DIC Corporation, Tg 33°C, solid content 40%) Acrylic resin emulsion B: Boncoat CP-6450 (DIC Corporation, Tg 42°C, solids concentration 40%) Acrylic resin emulsion C: Boncoat EC-5400EF (DIC Corporation, Tg 6°C, solids concentration 40%) Acrylic resin emulsion D: JE-1056 (Seiko PMC Co., Ltd., Tg 82°C, solid content 42.5%) Acrylic resin emulsion E: AE872D (manufactured by E-Tech Co., Ltd., Tg 15°C, solid content 51.5%) Acrylic resin emulsion F: ES-90 (Japan Coating Resin Co., Ltd., Tg 80°C, solid content 51%) Acrylic resin emulsion G: 727 (Japan Coating Resin Co., Ltd., Tg 25°C, solid content 50%) Acrylic resin emulsion H: Joncryl 583-A (BASF, Tg 64°C, solids concentration 50%) Acrylic resin dispersion: Watersol S-720 (DIC Corporation, Tg 45°C, solid content 47.5%) Extender pigment: Precipitated barium sulfate 100 manufactured by Sakai Chemical Industry Co., Ltd. Anti-rust pigment: Ca650 manufactured by Teika Co., Ltd. Color pigment: MA100 manufactured by Mitsubishi Chemical Corporation Dispersant: BYK-180 manufactured by BYK-Chemie Japan Co., Ltd. Film-forming aid: Butyl cellosolve (ethylene glycol monobutyl ether) manufactured by Taisho Kasei Co., Ltd.

[0047] Examples 1 to 4 and Comparative Examples 1 and 2 The outer surface of a ductile cast iron pipe with a nominal diameter of 100 is coated with 130g / m2 of zinc-silicon-manganese-containing aluminum. 2A zinc-silicon-manganese-containing aluminum pseudoalloy coating was formed on the cast iron pipe by thermal spraying with a 50°C coating. The cast iron pipe was then heated in a gas furnace until the surface temperature of the cast iron pipe reached 50°C (measured with a contact thermometer), and a synthetic resin paint prepared with the composition shown in Table 1 was sprayed on the pipe to a film thickness of 80μm, followed by drying. The resulting cast iron pipe was evaluated as follows. The results are shown in Table 1. The minimum film-forming temperature of the synthetic resin paint was measured using a thermal gradient tester (film-forming temperature measuring device) under conditions of a set temperature range of 4 to 55°C and a film thickness of 100μm, in accordance with JIS K 6828-2 Synthetic resin emulsion Part 2: Method for determining whitening temperature and minimum film-forming temperature.

[0048] <Drying> For Examples 1 to 4 and Comparative Examples 1 and 2, the painted surface was touched with a finger every 30 seconds after application of the synthetic resin paint, and the time until the paint no longer adhered to the finger was measured. The results are shown in Table 1 according to the following criteria. The performance target is within 1 minute. (Judgment criteria) ◎:30 seconds ○:1 minute △:2 minutes ×:3 minutes

[0049] <Whitening resistance> Each cast iron pipe obtained in Examples 1 to 4 and Comparative Examples 1 and 2 was sprayed with water for 4 hours starting 15 minutes after coating, and the coating film condition was visually checked 20 hours later. The results were evaluated according to the following criteria and are shown in Table 1. (Judgment criteria) ○: No abnormalities △: No whitening of the coating film, white rust present ×: Whitening of coating film

[0050] <Corrosion resistance after water whitening test> After the above-mentioned whitening resistance test, the cast iron pipe was cut into a 150 x 90 mm tile-shaped test piece, and a cutter was used to make a 0.3 x 50 mm X-shaped scratch on the surface of the center of the test piece, reaching the iron base. A 30-day combined cycle test was conducted in accordance with JIS K 5600-7-9 (2006) cyclic corrosion test method, cycle A. The appearance of the coating was visually judged according to the following criteria. The results were evaluated according to the following criteria and are shown in Table 1. (Judgment criteria) ○: White rust on cut area, no rust on normal area △: White rust on both cut and normal parts ×: Red rust on cut parts, white rust on general parts

[0051] <Scratch resistance (23℃)> For each of the cast iron pipes obtained in Examples 1 to 4 and Comparative Examples 1 and 2, the coating hardness of each cast iron pipe after storage at 23° C. for 1 hour after coating was measured in accordance with JIS K 5600-5-4 (1999) hardness (pencil method). The results were evaluated according to the following criteria and are shown in Table 1. (Judgment criteria) ◎:H ○:HB △:B ×:2B

[0052] <Scratch resistance (60℃)> This test was conducted assuming that iron pipes come into contact with each other and become crimped during transportation in summer. Specifically, for each of the cast iron pipes obtained in Examples 1 to 4 and Comparative Examples 1 and 2, the cast iron pipes were fixed together with a clamp (torque was controlled based on the pressure value of the load fastening during pipe transportation), and held at 60°C for 7 hours, assuming the temperature of the cast iron pipes in summer. After that, the appearance of the cast iron pipes was confirmed when they were separated, and they were evaluated according to the following criteria. The results are shown in Table 1. (Judgment criteria) ○: No peeling of coating △: Slight peeling of the coating ×: Paint peeling

[0053] [Table 1]

[0054] As is clear from the test results in Table 1, the coating films of Examples 1 to 4 using synthetic resin coatings containing a combination of multiple acrylic resin emulsions with different glass transition temperatures (Tg) all dried quickly, within 30 seconds, and were excellent in water whitening resistance and scratch resistance 30 minutes after application. The hardness of the coating film after application was quickly developed, and the balance between touch dryness and hardened dryness was good. In addition, it was found that the coating films had excellent scratch resistance (60°C) compared to Comparative Examples 1 and 2, which were overcoated with conventional solvent-based coatings. The overall evaluation was given as × if there was at least one evaluation of × or △ in the test results, and as ○ if all test results were rated as ○ or higher.

[0055] In addition, the mass% of the acrylic resin emulsion and acrylic resin dispersion in Table 1 represents only the solid content, and the water includes the medium in the acrylic resin emulsion and acrylic resin dispersion. The mass% of the film-forming auxiliary in Table 1 represents the total amount contained in the synthetic resin paint, not just the amount added as butyl cellosolve alone.

Claims

1. A cast iron pipe having a coating layer on its outer surface made of synthetic resin paint containing multiple types of acrylic resin emulsions with different glass transition temperatures (Tg).

2. 2. The cast iron pipe according to claim 1, wherein the synthetic resin coating further contains an acrylic resin dispersion.

3. 3. The cast iron pipe according to claim 1, further comprising a zinc-based sprayed coating layer below the synthetic resin coating layer.

Citation Information

Patent Citations

  • Water-based coating composition

    JP1998176122A

  • Corrosion resistant layer for metal pipe

    JP2020002330A