Resin composition, pellet, molded product, method for producing resin composition, kit, laser-welded product, and method for producing laser-welded product

A carbon black masterbatch-blended resin composition addresses the need for laser-absorbing resin members by enhancing laser weldability and marking capabilities, resulting in strong and visibly marked molded products.

JP2024145412APending Publication Date: 2024-10-15MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023057741
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

There is a demand for resin compositions that can be used as laser-absorbing resin members during laser welding and can be laser marked, but existing compositions do not meet these requirements effectively.

Method used

A resin composition is developed by blending a masterbatch of carbon black with polyester resin, specifically containing 0.01 to 0.4 parts by mass of carbon black for every 100 parts by mass of polyester resin and amorphous resin, with a difference in solubility parameter (SP value) between the resins ranging from 0 to 3.0, to enhance laser weldability and marking.

Benefits of technology

The resin composition achieves high laser welding strength and enables effective laser marking, producing molded products with improved mechanical properties and design visibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145412000001_ABST
    Figure 2024145412000001_ABST
Patent Text Reader

Abstract

To provide a novel resin composition for use as a laser-absorbing resin member in laser welding, allowing for laser marking, and a pellet, a molded product, a method for producing a resin composition, a kit, a laser-welded product, and a method for producing a laser-welded product.SOLUTION: A resin composition comprises 0.01 pt.mass or more and 0.4 pts.mass or less of carbon black relative to 100 pts.mass of the total of more than 50 pts.mass and 90 pts.mass or less of polyester resin and 10 pts.mass or more and 50 pts.mass or less of amorphous resin, wherein at least a part of the amorphous resin is derived from masterbatch of the carbon black.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a pellet, a molded article, a method for producing a resin composition, a kit, a laser welded article, and a method for producing a laser welded article. In particular, the present invention relates to a resin composition containing a polyester resin as a main component. [Background technology]

[0002] Polyester resins, including polybutylene terephthalate resin, are excellent in mechanical strength, chemical resistance, electrical insulation, etc., and also have excellent heat resistance, moldability, and recyclability, and are therefore widely used in various types of equipment parts.

[0003] Recently, there has been an increase in the use of welding processes to improve productivity, and laser welding, which has little impact on electronic components, is becoming more and more popular. Laser welding is a technique in which a laser-transmitting resin member (hereinafter sometimes referred to as "transmitting resin member") made of a laser-transmitting material and a laser-absorbing resin member (hereinafter sometimes referred to as "absorbing resin member") made of a laser-absorbent material are overlapped, and laser light is irradiated from the transmitting resin member side to generate heat at the interface with the absorbing resin member to weld them together. Resin compositions used in molded products for such purposes are required to have the ability to be welded by irradiation with laser light (laser weldability).

[0004] On the other hand, in the case of molded products, product information is often printed or drawn on the surface of the molded product for the sake of design when completed, information display, part identification during assembly, etc. When it is required that these maintain their visibility for a long period of time, laser marking is sometimes used from the viewpoint of reliability. Furthermore, in recent years, resin compositions that can be used as laser-absorbing resin members during laser welding and that are laser markable have also been investigated (Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-050822 A Summary of the Invention [Problem to be solved by the invention]

[0006] As described above, resin compositions that can be used as laser-absorbing resin components during laser welding and that are laser-markable have been investigated. However, as demand for resin compositions having such properties increases, new resin compositions are required. The present invention aims to solve these problems, and to provide a resin composition that can be used as a laser-absorbing resin part during laser welding, a novel resin composition that is laser markable, as well as pellets, molded products, methods for producing the resin composition, kits, laser-welded products, and methods for producing laser-welded products. [Means for solving the problem]

[0007] In light of the above problems, the present inventors have conducted research and found that the above problems can be solved by blending a masterbatch of carbon black with a specified resin in addition to a polyester resin. Specifically, the above problems were solved by the following means. <1> A resin composition comprising: more than 50 parts by mass but not exceeding 90 parts by mass; and 10 parts by mass or more and 50 parts by mass or less of an amorphous resin, for a total of 100 parts by mass; and 0.01 part by mass or more and 0.4 part by mass or less of carbon black, wherein at least a portion of the amorphous resin is derived from a master batch of the carbon black. <2> The polyester resin includes a polybutylene terephthalate resin. <1> The resin composition according to claim 1. <3> The SP value of the polyester resin (SP 1 ) and the SP value of the amorphous resin (SP 2) absolute difference (|SP 1 -SP 2 |) is between 0 and 3.0, <1> or <2> The resin composition according to claim 1. <4> The amorphous resin includes a styrene-based resin. <1> ~ <3> 10. The resin composition according to claim 9 . <5> The amorphous resin includes an acrylonitrile-styrene resin. <1> ~ <4> 10. The resin composition according to claim 9 . <6> Further, the elastomer <1> ~ <5> 10. The resin composition according to claim 9 . <7> Used on the laser light absorbing side during laser welding. <1> ~ <6> 10. The resin composition according to claim 9 . <8> Used on the laser light absorbing side during laser welding, and also for laser marking. <1> ~ <7> 10. The resin composition according to claim 9 . <9> The polyester resin contains a polybutylene terephthalate resin, the amorphous resin contains an acrylonitrile-styrene resin, and further contains an elastomer, the laminate is used on the laser light absorbing side during laser welding, and is for laser marking. <1> ~ <8> 10. The resin composition according to claim 9 . <10> The polyester resin contains 0.01 to 0.4 parts by mass of carbon black relative to a total of 100 parts by mass of a polyester resin and a second thermoplastic resin other than the polyester resin, and at least a part of the second thermoplastic resin is derived from a master batch of the carbon black, and the SP value of the polyester resin (SP 1 ) and the SP value of the second thermoplastic resin (SP 22 ) absolute difference (|SP 1 -SP 22 |) is 0 to 3.0. <11> The polyester resin contains polybutylene terephthalate resin, is used on the laser light absorbing side during laser welding, and is for laser marking. <10> The resin composition according to claim 1. <12> <1> ~ <11> 2. A pellet of the resin composition according to claim 1. <13> <1> ~ <11> 2. A molded article formed from the resin composition according to claim 1. <14> A method for producing a resin composition, comprising: adding and melt-kneading 0.01 part by mass or more and 0.4 part by mass or less of carbon black to a total of 100 parts by mass of more than 50 parts by mass and 90 parts by mass or less of polyester resin and 10 parts by mass or more and 50 parts by mass or less of amorphous resin, wherein at least a portion of the amorphous resin is added as a masterbatch of the carbon black. <15> The resin composition comprises: <1> ~ <11> The resin composition according to any one of the above items. <14> The manufacturing method described in <16> A laser-transmittable resin composition; <1> ~ <11> A kit comprising the resin composition according to any one of the above items. <17> a laser-transmittable resin member formed from a laser-transmittable resin composition; <1> ~ <11> 2. A laser-welded product formed from the resin composition according to claim 1 and a laser-absorbing resin member. <18> The method includes irradiating a laser to a laser-absorbing resin workpiece to perform laser marking, and laser welding a laser-transmitting resin workpiece and the laser-absorbing resin workpiece. <17> A method for producing a laser welded product according to claim 1. <19> The laser welding is performed by galvano scanning laser welding. <18> A method for producing a laser welded product according to claim 1. Effect of the Invention

[0008] It is now possible to provide a new resin composition that can be used as a laser-absorbing resin part during laser welding and that can be laser-marked, as well as pellets, molded products, a method for producing the resin composition, a kit, a laser-welded product, and a method for producing a laser-welded product. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a schematic view showing a test piece (transmissive resin member I) for measuring the laser welding strength in the examples. [Diagram 2]FIG. 2 is a schematic diagram showing a test piece (absorbent resin member II) for measuring the laser welding strength in the examples. [Diagram 3] FIG. 2 is a schematic diagram showing a test piece (a combination of a transmissive resin member I and an absorptive resin member II) for measuring the laser welding strength of the examples. [Figure 4] FIG. 2 is a schematic diagram showing a method for measuring laser welding strength in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the present embodiment is an example for explaining the present invention, and the present invention is not limited to the present embodiment. In this specification, the use of "to" means that the numerical values ​​before and after it are included as the lower limit and upper limit. In this specification, various physical properties and characteristic values ​​are those at 23° C. unless otherwise specified. In this specification, unless otherwise specified, the weight average molecular weight is a polystyrene-equivalent value measured by GPC (gel permeation chromatography) using a Tosoh HLC-8320GPC EcoSEC with tetrahydrofuran as a solvent and Shodex KF-G, KF-805L x 3, KF-800D columns at a column temperature of 40°C and a flow rate of 1.2 mL / min, and detected at a detection wavelength of 254 nm. If the measurement methods, etc. described in the standards shown in this specification vary from year to year, they will be based on the standards as of January 1, 2023, unless otherwise stated. The scale of Figures 1 to 4 may not be consistent with reality.

[0011] The resin composition of the present embodiment is characterized in that it contains 0.01 to 0.4 parts by mass of carbon black per 100 parts by mass in total of more than 50 parts by mass and 90 parts by mass or less of polyester resin and 10 to 50 parts by mass of amorphous resin, and at least a part of the amorphous resin is derived from a master batch of the carbon black. By adopting such a configuration, it is possible to provide a resin composition that can be used as a laser-absorbing resin member during laser welding and that can be laser-marked. Here, "at least a portion of the amorphous resin is derived from the carbon black masterbatch" means that at least a portion of the amorphous resin is used as a resin for the carbon black masterbatch and is a component added to the resin composition.

[0012] In this embodiment, in addition to the polyester resin, an amorphous resin is included, and the carbon black is added in a state of being masterbatched with the amorphous resin. It is presumed that such a configuration creates islands of the amorphous resin in the sea of ​​polyester resin in the resin composition, and carbon black tends to aggregate in the islands. As a result, it is presumed that the aggregated carbon black concentrates and generates heat, which increases the laser welding strength.

[0013] In another embodiment, the polyester resin is more than 50 parts by mass and not more than 90 parts by mass, and the second thermoplastic resin other than the polyester resin is 10 parts by mass or more and 50 parts by mass or less, and the total mass of the polyester resin is 100 parts by mass. In addition, at least a part of the second thermoplastic resin is derived from a master batch of the carbon black, and the SP value of the polyester resin (SP 1 ) and the SP value of the second thermoplastic resin (SP 22 ) absolute difference (|SP 1 -SP 22 |) is 0 to 3.0. In this embodiment, the carbon black has an SP value (SP 1 ) and SP value (SP22 ) absolute difference (|SP 1 -SP 22 The carbon black is added in a state of being masterbatched with a second thermoplastic resin having a ratio | of 0 to 3.0. By adopting such a configuration, it is presumed that islands of the second thermoplastic resin are formed in a sea of ​​polyester resin in the resin composition, and that the carbon black tends to aggregate easily in the islands. As a result, it is presumed that the aggregated carbon black is concentrated and generates heat, thereby increasing the laser welding strength. The details of this embodiment will be described below.

[0014] <Polyester resin> The resin composition of the present embodiment contains a polyester resin. The polyester resin is a polyester obtained by polycondensation of a dicarboxylic acid compound and a dihydroxy compound, polycondensation of an oxycarboxylic acid compound, or polycondensation of these compounds, and may be either a homopolyester or a copolyester. The polyester resin used in the present embodiment is preferably a polyalkylene terephthalate resin, more preferably a polyethylene terephthalate resin and / or a polybutylene terephthalate resin, and even more preferably a polybutylene terephthalate resin. The polyester resin used in this embodiment is a crystalline resin.

[0015] As the dicarboxylic acid compound constituting the polyester resin, an aromatic dicarboxylic acid or an ester-forming derivative thereof is preferably used. Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, biphenyl-2,2'-dicarboxylic acid, biphenyl-3,3'-dicarboxylic acid, biphenyl-4,4'-dicarboxylic acid, diphenylether-4,4'-dicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid, diphenylsulfone-4,4'-dicarboxylic acid, diphenylisopropylidene-4,4'-dicarboxylic acid, 1,2-bis(phenoxy)ethane-4,4'-dicarboxylic acid, anthracene-2,5-dicarboxylic acid, anthracene-2,6-dicarboxylic acid, p-tert-phenylene-4,4'-dicarboxylic acid, and pyridine-2,5-dicarboxylic acid. Terephthalic acid is preferably used.

[0016] These aromatic dicarboxylic acids may be used in combination of two or more kinds. As is well known, these can be used in the polycondensation reaction not only as free acids but also as ester-forming derivatives such as dimethyl esters. In addition, small amounts of these aromatic dicarboxylic acids can be used in combination with one or more aliphatic dicarboxylic acids such as adipic acid, azelaic acid, dodecanedioic acid, and sebacic acid, and alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid.

[0017] Examples of dihydroxy compounds constituting the polyester resin include aliphatic diols such as ethylene glycol, propylene glycol, butanediol, hexylene glycol, neopentyl glycol, 2-methylpropane-1,3-diol, diethylene glycol, and triethylene glycol, alicyclic diols such as cyclohexane-1,4-dimethanol, and mixtures thereof. In addition, one or more long-chain diols having a molecular weight of 400 to 6,000, i.e., polyethylene glycol, poly-1,3-propylene glycol, and polytetramethylene glycol, may be copolymerized in small amounts. Additionally, aromatic diols such as hydroquinone, resorcin, naphthalenediol, dihydroxydiphenyl ether, and 2,2-bis(4-hydroxyphenyl)propane can also be used.

[0018] In addition to the above-mentioned bifunctional monomers, a small amount of a trifunctional monomer such as trimellitic acid, trimesic acid, pyromellitic acid, pentaerythritol, or trimethylolpropane may be used in combination to introduce a branched structure, or a monofunctional compound such as a fatty acid may be used in combination to adjust the molecular weight. The polyester resin is usually made of a polycondensation product of a dicarboxylic acid and a diol, i.e., 50% by mass, preferably 70% by mass or more of the total polyester resin is made of this polycondensation product. The dicarboxylic acid is preferably an aromatic carboxylic acid, and the diol is preferably an aliphatic diol.

[0019] Among them, polyalkylene terephthalate resins in which 95 mol % or more of the acid component is terephthalic acid and 95 mass % or more of the alcohol component is an aliphatic diol are preferred. Representative examples thereof are polybutylene terephthalate resins and polyethylene terephthalate resins, with polybutylene terephthalate resins being preferred. These are preferably close to homopolyesters, that is, 95 mass % or more of the entire resin is composed of terephthalic acid components and 1,4-butanediol or ethylene glycol components.

[0020] The polyester resin is also preferably copolymerized with isophthalic acid, dimer acid, polyalkylene glycol such as polytetramethylene glycol (PTMG), etc. Examples of such copolymers include those in which the copolymerization amount is 1 mol % or more and less than 50 mol % of the total segments of polyalkylene terephthalate.

[0021] The polyester resin used in the present embodiment may contain recycled products. Examples of recycled polyester resins include those obtained by material recycling in which scraps or rejected products from molded products, or collected used polyester resin molded bodies are crushed, washed, and reused, and those obtained by chemical recycling (chemical decomposition method).

[0022] An example of the blend form of the polyester resin of this embodiment is that it contains at least polybutylene terephthalate resin. The mass ratio of the polybutylene terephthalate resin in this blend form is preferably 30 mass% or more, more preferably 50 mass% or more, even more preferably 52 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 90 mass% or more, and may be 95 mass% or more in 100 mass% of the polyester resin. By making it equal to or more than the lower limit, the load deflection temperature of the obtained molded product becomes higher, and the moldability of the resin composition tends to become better. The mass ratio of the polybutylene terephthalate resin in the first embodiment may be 100 mass% in 100 mass% of the polyester resin contained in the resin composition, or may be 90 mass% or less, 70 mass% or less, or 60 mass% or less depending on the application. In the above blend form, the resin other than the polybutylene terephthalate resin is preferably a polyethylene terephthalate resin. In the above blend form, it is particularly preferred that the polybutylene terephthalate resin is contained at 30% by mass or more (preferably 50% by mass or more) in 100% by mass of the polyester resin, and the total of the polybutylene terephthalate resin and the polyethylene terephthalate resin (the content of the polyethylene terephthalate resin may be 0% by mass) accounts for 90% by mass or more (preferably 95% by mass or more) in 100% by mass of the polyester resin. By blending the polyethylene terephthalate resin, warping of the obtained molded product tends to be more effectively suppressed.

[0023] In addition, the SP value of the polyester resin used in this embodiment is preferably 18.5 or more, more preferably 19.0 or more, and even more preferably 20.0 or more, and is preferably 23.0 or less, more preferably 22.0 or less, and may be 21.5 or less. The SP value can be calculated by determining the solubility in a solvent with a known SP value and using the Hansen Solubility Parameters in Practice ver.5.0 based on that. When the resin composition of the present embodiment contains two or more polyester resins, the SP value is the sum of the values ​​obtained by multiplying the SP value of each polyester resin by the mass fraction.

[0024] The terminal carboxyl group concentration of the polyester resin is preferably 1 to 23 eq / ton, and more preferably 7 to 22 eq / ton. By setting the concentration within such a range, the flowability of the resin composition tends to be further improved. In the case where the resin composition in the present embodiment contains two or more polyester resins, the terminal carboxyl group concentration of the polyester resin is the terminal carboxyl group concentration of the mixture. The amount of terminal carboxyl groups can be determined by dissolving 0.5 g of the polyester resin in 25 mL of benzyl alcohol and titrating the resultant with a 0.01 mol / L benzyl alcohol solution of sodium hydroxide.

[0025] The polyester resin used in the present embodiment preferably has an intrinsic viscosity of 0.40 to 2.00 dL / g. By making the intrinsic viscosity equal to or less than the upper limit, the moldability of the obtained molded article tends to be improved. Also, by making the intrinsic viscosity equal to or more than the lower limit, the mechanical properties such as tensile strength and bending strength tend to be improved. The intrinsic viscosity of the polyester resin is preferably 0.50 dL / g or more, more preferably 0.65 dL / g or more, and even more preferably 0.70 dL / g or more. The intrinsic viscosity is preferably 1.50 dL / g or less, and more preferably 1.00 dL / g or less.

[0026] The intrinsic viscosity of the polyester resin is measured by the following method. Polybutylene terephthalate resin pellets are dissolved in a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (mass ratio 1 / 1) by stirring at 110°C for 1 hour to a concentration of 1.00 g / dL. The solution is then cooled to 30°C. The time it takes for the sample solution and the solvent alone to fall at 30°C is measured using a fully automatic solution viscometer, and the intrinsic viscosity is calculated using the formula: Intrinsic viscosity=((1+4K H η sp ) 0.5 -1) / (2K H C) Here, η sp = η / η0-1, where η is the time it takes for the sample solution to fall, η0 is the time it takes for the solvent alone to fall, C is the concentration of the sample solution (g / dL), and K H is Huggins' constant. K H was set to 0.33. In the present embodiment, when the resin composition contains two or more polyester resins, the intrinsic viscosity of the polyester resin is the intrinsic viscosity of the mixture.

[0027] The resin composition in this embodiment preferably contains polyester resin in a proportion of 20 mass% or more, more preferably 25 mass% or more, even more preferably 30 mass% or more, and even more preferably 42 mass% or more, and preferably 55 mass% or less, more preferably 50 mass% or less, and even more preferably 45 mass% or less, based on 100 mass% of the resin composition. The resin composition in the present embodiment may contain only one type of polyester resin, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.

[0028] <Amorphous resin and / or second thermoplastic resin> The resin composition of the present embodiment contains an amorphous resin and / or a second thermoplastic resin. It is presumed that the inclusion of these resins causes a sea-island structure to be formed in the resin composition by the amorphous resin and / or the second thermoplastic resin, making it easier for the carbon black to aggregate in the island portions, and the aggregated carbon black generates heat in a concentrated manner, thereby increasing the laser welding strength. The resin composition of the present embodiment usually contains both the amorphous resin and / or the second thermoplastic resin derived from the carbon black masterbatch and the amorphous resin and / or the second thermoplastic resin blended separately from the masterbatch. In the present embodiment, the amount of the amorphous resin and / or the second thermoplastic resin derived from the carbon black masterbatch is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less, based on the total amount of the amorphous resin and / or the second thermoplastic resin contained in the resin composition (100% by mass). The amorphous resin and / or the second thermoplastic resin derived from the carbon black masterbatch and the amorphous resin and / or the second thermoplastic resin blended separately from the masterbatch may be the same resin or different resins. In this embodiment, it is preferable that the amorphous resin and / or the second thermoplastic resin derived from the carbon black masterbatch and the amorphous resin and / or the second thermoplastic resin blended separately from the masterbatch each contain a styrene-based resin. Details of these resins will be described later.

[0029] In one embodiment of the present invention, the SP value of the polyester resin (SP 1 ) and the SP value of amorphous resin (SP 2 ) Absolute value of the difference |SP 1 -SP 2 | is between 0 and 3.0. In another embodiment of the present invention, the SP value of the polyester resin (SP 1 ) and the SP value of the second thermoplastic resin (SP 22 ) Absolute value of the difference |SP 1 -SP 22| is between 0 and 3.0. In this embodiment, the absolute value of the difference between the SP values ​​(|SP 1 -SP 2 |, |SP 1 -SP 22 |) is preferably greater than 0, more preferably 0.1 or greater, even more preferably 0.5 or greater, even more preferably 1.0 or greater, even more preferably 1.5 or greater, even more preferably 2.0 or greater, and preferably 2.8 or less. In this embodiment, the SP value of the polyester resin (SP 1 ) ≧ SP value of amorphous resin (SP 2 ) is preferred. When the resin composition of the present embodiment contains two or more kinds of amorphous resins and / or a second thermoplastic resin, the SP value is the sum of values ​​obtained by multiplying the SP value of each polyester resin by the mass fraction.

[0030] In this embodiment, the SP value of the amorphous resin (SP 2 ) and / or the SP value of the second thermoplastic resin (SP 22 ) are each independently preferably 21.5 or less, more preferably 21.0 or less, even more preferably less than 20.0, more preferably 19.5 or less, even more preferably less than 19.0, may be less than 18.5, and are preferably 17.0 or more, and may be 17.5 or more.

[0031] Examples of the amorphous resin include a styrene resin, a polycarbonate resin, a polyphenylene ether resin, and a polysulfone resin, and the styrene resin and the polycarbonate resin are preferable, and the styrene resin is more preferable. In the resin composition used in the present embodiment, 90% by mass or more of the amorphous resin is preferably a styrene resin.

[0032] <<Styrene-based resin>> Examples of styrene-based resins include resins obtained by polymerizing a styrene-based monomer and, if necessary, one or more other vinyl monomers copolymerizable therewith.

[0033] Examples of the styrene monomer include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, vinylxylene, ethylstyrene, dimethylstyrene, p-tert-butylstyrene, vinylnaphthalene, and other styrene derivatives, with styrene being particularly preferred. These may be used alone or in combination of two or more.

[0034] Examples of other vinyl monomers copolymerizable with styrene-based monomers include α,β-unsaturated carboxylic acids and their anhydrides, such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, phthalic acid, and itaconic acid; methacrylic acid alkyl esters, such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, amyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, octyl methacrylate, cyclohexyl methacrylate, and dodecyl methacrylate; and methyl acrylate, ethyl acrylate, and the like. Examples of the acrylic acid esters include alkyl esters of acrylic acid such as butyl acrylate, amyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate, octyl acrylate, cyclohexyl acrylate, and dodecyl acrylate; aryl esters of acrylic acid such as phenyl acrylate and benzyl acrylate; aryl methacrylic acid esters such as phenyl methacrylate and benzyl methacrylate; maleimide monomers such as maleimide, N-methylmaleimide, and N-phenylmaleimide; and acrylonitrile.

[0035] As the styrene-based resin, a copolymer of a styrene-based monomer and an acrylonitrile monomer (acrylonitrile-styrene resin) is preferable. In the acrylonitrile-styrene resin, the proportion of styrene-based monomers in the total of 100% by mass of monomers constituting the resin is preferably 20% by mass or more, more preferably 30% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less. The acrylonitrile-styrene resin may be a copolymer of a styrene-based monomer, acrylonitrile, and another monomer copolymerizable with either of them. The proportion of the other monomer is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, among which 5% by mass or less, 3% by mass or less, 2% by mass or less, and particularly preferably 1% by mass or less, based on 100% by mass of the total monomers constituting the acrylonitrile-styrene resin. The method for producing the acrylonitrile-styrene resin is not limited, and any known method can be used, such as bulk polymerization, emulsion polymerization, solution polymerization, and suspension polymerization.

[0036] <<Polycarbonate resin>> The polycarbonate resin used in this embodiment may be a known polycarbonate resin. The polycarbonate resin is usually a thermoplastic polymer or copolymer that may be branched, obtained by reacting a dihydroxy compound or a small amount of a polyhydroxy compound with phosgene or a carbonic acid diester. The method for producing the polycarbonate resin is not particularly limited, and polycarbonate resins produced by the conventionally known phosgene method (interfacial polymerization method) or melting method (ester exchange method) may be used, but polycarbonate resins produced by the melting method are preferred from the viewpoints of laser transparency and laser weldability.

[0037] The dihydroxy compound as the raw material is preferably an aromatic dihydroxy compound, and examples thereof include 2,2-bis(4-hydroxyphenyl)propane (i.e., bisphenol A), tetramethylbisphenol A, bis(4-hydroxyphenyl)-p-diisopropylbenzene, hydroquinone, resorcinol, 4,4-dihydroxydiphenyl, and the like, preferably bisphenol A. In addition, a compound in which one or more tetraalkylphosphonium sulfonates are bonded to the above aromatic dihydroxy compound can also be used.

[0038] As the polycarbonate resin, among the above, aromatic polycarbonate resin derived from 2,2-bis(4-hydroxyphenyl)propane, or aromatic polycarbonate copolymer derived from 2,2-bis(4-hydroxyphenyl)propane and other aromatic dihydroxy compounds is preferable. Also, it may be a copolymer such as a copolymer with a polymer or oligomer having a siloxane structure. Furthermore, two or more of the above polycarbonate resins may be mixed and used.

[0039] The viscosity average molecular weight of the polycarbonate resin is preferably 5,000 to 30,000, more preferably 10,000 to 28,000, and even more preferably 14,000 to 24,000. By using a resin having a viscosity average molecular weight of 5,000 or more, the mechanical strength of the resulting molded article tends to be improved. In addition, by using a resin having a viscosity average molecular weight of 30,000 or less, the flowability of the resin composition tends to be improved, and moldability and laser weldability tend to be improved. The viscosity average molecular weight of the polycarbonate resin is the viscosity average molecular weight [Mv] calculated from the solution viscosity measured at 25°C using methylene chloride as a solvent.

[0040] On the other hand, the second thermoplastic resin in this embodiment is a thermoplastic resin other than a polyester resin, and the SP value (SP 1) is appropriately determined in relation to the above. Suitable examples of the second thermoplastic resin are the same as the examples of the amorphous resin described above.

[0041] In this embodiment, when the polyester resin is a polybutylene terephthalate resin, examples of the amorphous resin and / or the second thermoplastic resin include a styrene resin, a polycarbonate resin, a polyphenylene ether resin, and a polysulfone resin (PSF resin). When the polyester resin is a polyethylene terephthalate resin, examples of the amorphous resin and / or the second thermoplastic resin include a styrene resin, a polycarbonate resin, and the like.

[0042] The total content of the amorphous resin and / or the second thermoplastic resin in this embodiment is 10 parts by mass or more, preferably 15 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 23 parts by mass or more, and may be 30 parts by mass or more, relative to 100 parts by mass of the total of the polyester resin, the amorphous resin, and / or the second thermoplastic resin. By making it equal to or more than the lower limit, the warping of the resin composition tends to be reduced. In addition, the total content of the amorphous resin and / or the second thermoplastic resin in this embodiment is 50 parts by mass or less, preferably 45 parts by mass or less, more preferably 40 parts by mass or less, even more preferably 38 parts by mass or less, and may be 32 parts by mass or less, relative to 100 parts by mass of the total of the polyester resin, the amorphous resin, and / or the second thermoplastic resin. By making it equal to or less than the upper limit, the heat resistance, mechanical properties such as tensile strength and bending strength, and laser weldability of the resin composition tend to be further improved.

[0043] <Carbon black> The resin composition of the present embodiment contains carbon black. By including carbon black, laser welding and laser marking become possible. In this embodiment, the carbon black is added in a state of being masterbatched with the amorphous resin. Alternatively, the carbon black is added in a state where the SP value of the polyester resin (SP 1)'s SP value (SP 22 ) Absolute value of the difference |SP 1 -SP 22 The carbon black is added in a state of being masterbatched with a second thermoplastic resin having a | of 0 to 3.0. With such a configuration, a sea-island structure is formed in the resin composition by the polyester resin and the amorphous resin, etc., and it is presumed that the carbon black is likely to aggregate in the island portions, and the aggregated carbon black is concentrated to generate heat, thereby increasing the laser welding strength. In addition, the resin composition of the present embodiment may contain both carbon black masterbatched with an amorphous resin, and carbon black masterbatched with a second thermoplastic resin that satisfies the absolute value of the difference in SP values ​​described above.

[0044] In this embodiment, the proportion of carbon black in the carbon black masterbatch is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, even more preferably 25% by mass or more, even more preferably 30% by mass or more, even more preferably 35% by mass or more, and may even be 40% by mass or more or 45% by mass or more, and is preferably 65% ​​by mass or less, more preferably 60% by mass or less, and even more preferably 55% by mass or less. In the carbon black masterbatch used in this embodiment, the total amount of the carbon black, the amorphous resin and / or the second thermoplastic resin preferably accounts for 99 to 100% by mass of the entire carbon black masterbatch.

[0045] The carbon black is not limited in type, raw material, or production method, and any of furnace black, channel black, acetylene black, ketjen black, etc. can be used. Among these, furnace black is preferred. The number average particle size of carbon black is preferably 5 to 60 nm. The upper limit is preferably 60 nm or less, more preferably 40 nm or less, even more preferably 30 nm or less, and even more preferably 25 nm or less. The lower limit is preferably 10 nm or more, more preferably 13 nm or more, even more preferably 16 nm or more, and even more preferably 19 nm or more. By keeping the upper and lower limits, the appearance, laser weldability, and laser markability of the molded product tend to be improved. The number average particle size can be obtained by obtaining an aggregate enlarged image according to the procedure described in the ASTM D3849 standard (Standard Test Method for Carbon Black-Morphological Characterization by Electron Microscopy), measuring the particle sizes of 3,000 unit constituent particles from this aggregate image, and taking the arithmetic average.

[0046] DBP oil absorption of carbon black (unit: cm 3 / 100g) is 40~300cm 3 / 100g. The upper limit is preferably 300 cm 3 / 100g or less is preferable, and 200cm 3 / 100g or less is more preferable, and 150cm 3 More preferably, the weight is 100g or less. 3 The lower limit may be 40 cm / 100 g or less. 3 / 100g or more is preferable, 50cm 3 / 100g or more is preferable, 60cm 3 By keeping the value within the above upper and lower limits, the appearance, laser welding strength, and laser marking properties of the molded product tend to be improved. 3 / 100g) can be measured in accordance with JIS K6217.

[0047] The content of carbon black in the resin composition of this embodiment is 0.01 parts by mass or more, preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.15 parts by mass or more, and even more preferably 0.20 parts by mass or more, based on 100 parts by mass of the polyester resin, the amorphous resin, and / or the second thermoplastic resin in total. By making it equal to or more than the lower limit, the coloring effect, the laser welding strength, and the laser marking property are more effectively exhibited. In addition, the upper limit of the content of carbon black is 0.4 parts by mass or less, more preferably 0.35 parts by mass or less, based on 100 parts by mass of the polyester resin, the amorphous resin, and / or the second thermoplastic resin in total. By making it equal to or less than the upper limit, the mechanical strength and the laser welding strength of the obtained molded product tend to be further improved.

[0048] The content of the carbon black master batch in the resin composition of the present embodiment is preferably 0.02 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.2 parts by mass or more, and even more preferably 0.25 parts by mass or more, relative to 100 parts by mass of the total of the polyester resin, the amorphous resin, and / or the second thermoplastic resin. By making it equal to or more than the lower limit, the coloring effect is more effectively exhibited and the laser weldability tends to be improved. In addition, the upper limit of the content of the carbon black master batch is preferably 1.0 parts by mass or less, more preferably 0.8 parts by mass or less, and even more preferably 0.7 parts by mass or less, relative to 100 parts by mass of the total of the polyester resin, the amorphous resin, and / or the second thermoplastic resin. By making it equal to or less than the upper limit, the mechanical strength of the obtained molded product tends to be further improved. The resin composition of the present embodiment may contain only one type of carbon black, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.

[0049] <Elastomer> The resin composition of this embodiment may contain an elastomer. By containing an elastomer, the impact resistance of the obtained absorbent resin member can be improved. However, the elastomer has rubber properties at room temperature (e.g., 23°C) and does not fall under the above-mentioned amorphous resin and / or second thermoplastic resin. Specifically, having rubber properties at room temperature means that the flexural modulus at room temperature is 300 MPa or less. As the elastomer, a wide variety of elastomers that are used for improving impact resistance by being blended with polyester resins can be used.

[0050] An example of the elastomer is an elastomer containing an epoxy group. By including an elastomer containing an epoxy group, it is likely that an absorbing resin member having higher impact resistance can be obtained.

[0051] A first embodiment of the elastomer containing an epoxy group is a copolymer obtained by copolymerizing an α-olefin, a glycidyl ester of an α,β-unsaturated acid, and, if necessary, an unsaturated monomer copolymerizable therewith. It is preferable to use 60 mass% or more of the α-olefin and the glycidyl ester of an α,β-unsaturated acid in all the copolymerization components.

[0052] Examples of α-olefins include ethylene, propylene, butene-1, and pentene-1. Two or more of these may be used. Examples of glycidyl esters of α,β-unsaturated acids include glycidyl acrylate, glycidyl methacrylate, glycidyl ethacrylate, and glycidyl itaconate. Two or more of these may be used. Examples of vinyl monomers copolymerizable with the above components include vinyl ethers, vinyl esters such as vinyl acetate and vinyl propionate, acrylic and methacrylic esters such as methyl, ethyl, propyl, and butyl, acrylonitrile, and styrene. Two or more of these may be used.

[0053] Preferred examples of the elastomer containing an epoxy group of the first embodiment include ethylene / glycidyl methacrylate copolymer, ethylene / glycidyl methacrylate / vinyl acetate copolymer, ethylene / glycidyl methacrylate / alkyl acrylate copolymer, ethylene / alkyl acrylate / vinyl acetate copolymer, etc. In particular, from the viewpoint of excellent toughness and further improving the wet heat resistance and impact resistance of the absorbent resin member, ethylene / glycidyl methacrylate / alkyl acrylate (preferably butyl acrylate) copolymer is preferred. Specific examples of the elastomer containing an epoxy group of the first embodiment are available under the trade names "Rotadar" (registered trademark) AX8900 and AX8700 manufactured by Arkema.

[0054] A second embodiment of the elastomer containing epoxy groups is a core-shell type elastomer. By using a core-shell type elastomer, the molecular particle size is small, so that it is easy to disperse in polybutylene terephthalate resin, and the welding strength tends to increase due to the reaction of the reactive groups. An example of a core-shell type elastomer is one in which a monomer component is graft-copolymerized onto a core polymer. The core is preferably a rubber polymer, examples of which include acrylonitrile-acrylic rubber polymer-styrene graft copolymer (ASA resin), methyl methacrylate-acrylic rubber polymer-styrene graft copolymer (MSA resin), methyl methacrylate-acrylonitrile-acrylic rubber polymer-styrene graft copolymer (MASA resin), polyorganosiloxane-containing rubber polymer, and the like, with polyorganosiloxane-containing rubber polymer being preferred. The polyorganosiloxane-containing rubbery polymer generally has a glass transition temperature of 0° C. or lower, preferably −20° C. or lower, and more preferably −30° C. or lower. Specific examples of the rubber component are not particularly limited as long as they contain polyorganosiloxane rubber, and examples thereof include polyorganosiloxane rubber, and composite rubber (IPN type) of polyorganosiloxane rubber and polyalkyl acrylate rubber.

[0055] Specific examples of the monomer component graft copolymerizable with the core include aromatic vinyl compounds, vinyl cyanide compounds, (meth)acrylic acid ester compounds, (meth)acrylic acid compounds, epoxy group-containing (meth)acrylic acid ester compounds such as glycidyl (meth)acrylate, maleimide compounds such as maleimide, N-methylmaleimide, and N-phenylmaleimide, α,β-unsaturated carboxylic acid compounds such as maleic acid, phthalic acid, and itaconic acid, and anhydrides thereof (for example, maleic anhydride, etc.).

[0056] Specific examples of rubber polymers, aromatic vinyl compounds, vinyl cyanide compounds, and (meth)acrylic acid ester compounds are described in paragraphs 0042 to 0046 of JP 2019-059813 A, the contents of which are incorporated herein by reference.

[0057] The epoxy group-containing elastomer of the second embodiment is preferably a compound obtained by graft polymerizing an epoxy group-containing (meth)acrylic acid ester compound onto a polyorganosiloxane-containing rubbery polymer (preferably a composite rubber of a polyorganosiloxane rubber and a polyalkyl acrylate rubber).

[0058] Specific examples of the elastomer containing an epoxy group according to the second embodiment include "Metablen (registered trademark, the same applies below) S-2002" and "Metablen S-2200" manufactured by Mitsubishi Rayon Co., Ltd.

[0059] Another example of the elastomer is a graft copolymer obtained by graft-copolymerizing a rubber component with a monomer component copolymerizable therewith. The method for producing the graft copolymer may be any of bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc., and the copolymerization method may be one-stage grafting or multi-stage grafting.

[0060] The rubber component usually has a glass transition temperature of 0° C. or lower, preferably -20° C. or lower, and more preferably -30° C. or lower. Specific examples of the rubber component include polybutadiene rubber, polyisoprene rubber, polyalkyl acrylate rubber such as polybutyl acrylate, poly(2-ethylhexyl acrylate), and butyl acrylate-2-ethylhexyl acrylate copolymer, silicone rubber such as polyorganosiloxane rubber, butadiene-acrylic composite rubber, IPN (Interpenetrating Polymer Network) type composite rubber consisting of polyorganosiloxane rubber and polyalkyl acrylate rubber, styrene-butadiene rubber, ethylene-α-olefin rubber such as ethylene-propylene rubber, ethylene-butene rubber, and ethylene-octene rubber, ethylene-acrylic rubber, and fluororubber. These may be used alone or in combination of two or more. Among these, polybutadiene rubber, polyalkyl acrylate rubber, polyorganosiloxane rubber, IPN type composite rubber consisting of polyorganosiloxane rubber and polyalkyl acrylate rubber, and styrene-butadiene rubber are preferred from the standpoint of mechanical properties and surface appearance.

[0061] Specific examples of the monomer component capable of graft copolymerization with the rubber component are the same as those of the monomer component capable of graft copolymerization with the rubber component described in the second embodiment of the elastomer containing an epoxy group.

[0062] The graft copolymer obtained by copolymerizing a rubber component is preferably a core / shell type graft copolymer in terms of impact resistance and surface appearance. Among them, a core / shell type graft copolymer is particularly preferred, which is made of at least one rubber component selected from polybutadiene-containing rubber, polybutyl acrylate-containing rubber, polyorganosiloxane rubber, and an IPN type composite rubber consisting of polyorganosiloxane rubber and polyalkyl acrylate rubber, and a shell layer formed by copolymerizing (meth)acrylic acid ester around the core layer. The above-mentioned core / shell type graft copolymer preferably contains 40% by mass or more of the rubber component, more preferably 60% by mass or more. In addition, it is preferable that the (meth)acrylic acid is contained in an amount of 10% by mass or more. In this embodiment, the core / shell type does not necessarily have to be one in which the core layer and the shell layer can be clearly distinguished, and is intended to broadly include a compound obtained by graft polymerizing a rubber component around a core portion.

[0063] Preferable specific examples of these core / shell type graft copolymers include methyl methacrylate-butadiene-styrene copolymer (MBS), methyl methacrylate-acrylonitrile-butadiene-styrene copolymer (MABS), methyl methacrylate-butadiene copolymer (MB), methyl methacrylate-acrylic rubber copolymer (MA), methyl methacrylate-acrylic rubber-styrene copolymer (MAS), methyl methacrylate-acrylic-butadiene rubber copolymer, methyl methacrylate-acrylic-butadiene rubber-styrene copolymer, methyl methacrylate-(acrylic-silicone IPN rubber) copolymer, etc. Such rubbery polymers may be used alone or in combination of two or more.

[0064] Examples of such elastomers include "PARALOID (registered trademark, the same applies below) EXL2602", "PARALOID EXL2603", "PARALOID EXL2655", "PARALOID EXL2311", "PARALOID EXL2313", "PARALOID EXL2315", "PARALOID KM330", "PARALOID KM336P", and "PARALOID KCZ201" manufactured by Rohm and Haas Japan Co., Ltd.; "METABLEN (registered trademark, the same applies below) C-223A", "METABLEN E-901", "METABLEN S-2001", and "METABLEN SRK-200" manufactured by Mitsubishi Rayon Co., Ltd.; "KANE ACE (registered trademark, the same applies below) M-511", "KANE ACE M-600", "KANE ACE M-400", "KANE ACE M-580", "KANE ACE M-711", and "KANE ACE MR-01" manufactured by Kaneka Corporation; and "UBESTA XPA" manufactured by Ube Industries, Ltd.

[0065] The elastomer (particularly, the elastomer containing an epoxy group) preferably has a melt flow rate (MFR) of 0.1 to 50 g / 10 min, more preferably 0.5 to 30 g / 10 min, measured at 190° C. under a load of 2.16 kgf according to JIS K 7210. By setting the MFR within the above range, there is a tendency for impact resistance to be improved while appearance defects are more effectively suppressed.

[0066] When the resin composition of the present embodiment contains an elastomer, the content thereof is preferably 5 parts by mass or more, more preferably 7 parts by mass or more, and even more preferably 9 parts by mass or more, relative to 100 parts by mass of the total of the polyester resin, the amorphous resin, and / or the second thermoplastic resin. By making the content equal to or more than the lower limit, the impact resistance is improved and the laser welding strength tends to be improved. In addition, the content of the elastomer is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, even more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and may be 15 parts by mass or less, relative to 100 parts by mass of the total of the polyester resin, the amorphous resin, and / or the second thermoplastic resin. By making the content equal to or less than the upper limit, the effect of suppressing the decrease in laser welding strength tends to be improved. The resin composition of the present embodiment may contain only one type of elastomer, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.

[0067] <Reactive compounds> The resin composition of the present embodiment may further contain a reactive compound (preferably an epoxy compound). By containing a reactive compound, the weld strength tends to be high. However, when the reactive compound also corresponds to an elastomer, it is classified as an elastomer in this specification. The reactive compound is preferably a compound that can chemically react with a carboxy group or hydroxy group present at the end of the polybutylene terephthalate resin to cause a crosslinking reaction or chain extension. The reactive compound preferably contains at least one selected from the group consisting of an epoxy compound, a carbodiimide compound, a compound having an oxazoline group (ring), a compound having an oxazine group (ring), a compound having a carboxy group, and a compound having an amide group, more preferably contains at least one selected from an epoxy compound and a carbodiimide compound, and further preferably contains an epoxy compound. In particular, the resin composition of this embodiment preferably contains at least 90 mass % of the reactive compound, more preferably at least 95 mass %, and particularly preferably at least 99 mass % of the reactive compound is an epoxy compound. The epoxy compound is not particularly limited as long as it has one or more epoxy groups in one molecule, and a wide variety of known epoxy compounds can be used. By including an epoxy compound, the range of laser irradiation conditions tends to be broadened.

[0068] Examples of the epoxy compound include a glycidyl compound, an epoxy compound having an aromatic ring, and an alicyclic epoxy compound, and it is preferable to contain at least an epoxy compound having an aromatic ring.

[0069] Specific examples of epoxy compounds include bisphenol A type epoxy compounds (including bisphenol A diglycidyl ether), bisphenol F type epoxy compounds (including bisphenol F diglycidyl ether), biphenyl type epoxy compounds (including bis(glycidyloxy)biphenyl), resorcin type epoxy compounds (including resorcinol diglycidyl ether), novolac type epoxy compounds, epoxy compounds having an aromatic ring such as benzoic acid glycidyl ester, terephthalic acid diglycidyl ester, orthophthalic acid diglycidyl ester, methyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, decyl glycidyl ether, sucrose, glycidyl ether ... Examples of such diglycidyl ethers include (di)glycidyl ethers such as tearyl glycidyl ether, phenyl glycidyl ether, butylphenyl glycidyl ether, allyl glycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, glycerin diglycidyl ether, and propylene glycol diglycidyl ether; paraffin-based (e.g., saturated fatty acid-based) or olefin-based (e.g., unsaturated fatty acid-based) (di)glycidyl esters such as sorbic acid glycidyl ester, adipic acid diglycidyl ester, epoxidized linseed oil, and epoxidized soybean oil; and alicyclic epoxy compounds such as vinylcyclohexene dioxide and dicyclopentadiene oxide. Among these, bisphenol A type epoxy compounds, novolac type epoxy compounds, bisphenol F type epoxy compounds, biphenyl type epoxy compounds, etc. are preferred, and in particular, orthocresol / novolac type epoxy resins (polyglycidyl ether compounds of O-cresol-formaldehyde polycondensates) are more preferred. Commercially available products include "Joncryl ADR4368C" (product name: manufactured by BASF), Epicoat 1003 (product name: manufactured by Mitsubishi Chemical Corporation), and Nippon Steel Sumikin Chemical Co., Ltd. (product name: YDCN704).

[0070] The epoxy compound preferably has a weight average molecular weight of 15000 or less, more preferably 10000 or less. There is no particular lower limit, but the weight average molecular weight is preferably 100 or more, more preferably 300 or more. By setting the weight average molecular weight within such a range, the effect of the present embodiment tends to be more effectively exhibited.

[0071] The epoxy compound preferably has an epoxy equivalent of 100 g / eq or more, more preferably 150 g / eq or more, and more preferably 150 g / eq or more. The epoxy compound preferably has an epoxy equivalent of 1500 g / eq or less, more preferably 800 g / eq or less, and even more preferably 200 g / eq or less. By setting the epoxy equivalent to the lower limit or more, the flowability tends to be high and molding tends to be easy, whereas by setting it to the upper limit or less, the weld strength and the hydrolysis resistance of the welded body tend to be higher.

[0072] When the resin composition of the present embodiment contains a reactive compound (preferably an epoxy compound), the content is preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.4 parts by mass or more, relative to 100 parts by mass of the polyester resin, the amorphous resin, and / or the second thermoplastic resin in total. By making it equal to or more than the lower limit, the welding strength increases and the hydrolysis resistance of the resin composition tends to improve. In addition, the upper limit of the content of the reactive compound is preferably 18 parts by mass or less, more preferably 15 parts by mass or less, even more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, even more preferably 3 parts by mass or less, and may be 1 part by mass or less, relative to 100 parts by mass of the polyester resin, the amorphous resin, and / or the second thermoplastic resin in total. By making it equal to or less than the upper limit, the flowability tends to be higher and the moldability improved. The resin composition of the present embodiment may contain only one type of reactive compound, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.

[0073] <Inorganic fillers> The resin composition of the present embodiment may contain an inorganic filler, which can increase the mechanical strength of the resulting absorbing resin member. As the inorganic filler, fibrous inorganic fillers such as glass fiber, carbon fiber, basalt fiber, wollastonite, potassium titanate fiber, etc. can be used. Granular or amorphous fillers such as calcium carbonate, titanium oxide, feldspar minerals, clay, glass beads, etc.; scaly fillers such as glass flakes, graphite, etc. can also be used. Among them, from the viewpoints of mechanical strength, rigidity, and heat resistance, it is preferable to use fibrous fillers, particularly glass fiber. The glass fibers are made of glass compositions such as A glass, C glass, E glass, S glass, D glass, M glass, and R glass, and E glass (alkali-free glass) is particularly preferred since it does not adversely affect the polybutylene terephthalate resin. Examples of fibers include those that have a cross-sectional shape, such as a perfect circle, ellipse, or polygon, cut perpendicular to the length direction, and have a fibrous appearance with a length that is sufficiently long compared to the cross section.

[0074] The glass fiber used in the resin composition of the present embodiment may be a single fiber or a plurality of single fibers twisted together. The form of the glass fiber may be any of "glass roving" in which a single fiber or a plurality of twisted fibers are continuously wound, "chopped strand" cut to a length of 1 to 10 mm, and "milled fiber" pulverized to a length of 10 to 500 μm, but chopped strand is preferred. Such glass fiber is commercially available from Asahi Fiber Glass under the trade names "Glaslon Chopped Strand" and "Glaslon Milled Fiber", and is easily available. Glass fibers of different forms can also be used in combination.

[0075] In the present embodiment, the glass fiber preferably has an irregular cross-sectional shape. The irregular cross-sectional shape has a flattening ratio, expressed as the ratio of the major axis to the minor axis (D2 / D1), where D2 is the major axis and D1 is the minor axis of the cross section perpendicular to the longitudinal direction of the fiber, of, for example, 1.5 to 10, preferably 2.5 to 10, more preferably 2.5 to 8, and even more preferably 2.5 to 5. For such flat glass, refer to the description in paragraphs 0065 to 0072 of JP2011-195820A, the contents of which are incorporated herein by reference.

[0076] When the resin composition of this embodiment contains an inorganic filler (preferably glass fiber), the content is preferably 25 parts by mass or more, more preferably 30 parts by mass or more, even more preferably 35 parts by mass or more, even more preferably 40 parts by mass or more, and even more preferably 45 parts by mass or more, relative to 100 parts by mass of the total of the polyester resin and the amorphous resin and / or the second thermoplastic resin. By making it equal to or more than the lower limit, the mechanical hardness of the obtained absorbent resin member tends to be further improved. The upper limit of the content of the inorganic filler is preferably 100 parts by mass or less, more preferably 80 parts by mass or less, even more preferably 70 parts by mass or less, even more preferably 60 parts by mass or less, and even more preferably 55 parts by mass or less, relative to 100 parts by mass of the total of the polyester resin and the amorphous resin and / or the second thermoplastic resin. By making it equal to or less than the upper limit, the effect of suppressing the decrease in tensile elongation tends to be further improved.

[0077] In addition, when the resin composition of this embodiment contains an inorganic filler (preferably glass fiber), the content thereof in the resin composition is preferably 20% by mass or more, and more preferably 25% by mass or more. By making it equal to or more than the lower limit, the mechanical hardness of the obtained absorbent resin member tends to be further improved. The upper limit of the content of the inorganic filler in the resin composition is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less, and may be 35% by mass or less. By making it equal to or less than the upper limit, the effect of suppressing the decrease in tensile elongation tends to be further improved. The resin composition of the present embodiment may contain only one type of inorganic filler, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.

[0078] <Stabilizer> The resin composition of the present embodiment may contain a stabilizer. Examples of the stabilizer include a phenol-based stabilizer (preferably a hindered phenol-based stabilizer), a hindered amine-based stabilizer, a phosphorus-based stabilizer, and a sulfur-based stabilizer. Among these, the phenol-based stabilizer, the phosphorus-based stabilizer, and the sulfur-based stabilizer are preferred. As the stabilizer, specifically, the description in paragraphs 0046 to 0057 of JP 2018-070722 A, the description in paragraphs 0030 to 0037 of JP 2019-056035 A, the description in paragraphs 0066 to 0078 of WO 2017 / 038949 A, and the description in paragraphs 0051 to 0060 of JP 2020-147662 A can be referred to, the contents of which are incorporated herein by reference.

[0079] The content of the stabilizer in the resin composition of this embodiment is preferably 0.01 parts by mass or more, more preferably 0.10 parts by mass or more, per 100 parts by mass of the polyester resin, the amorphous resin, and / or the second thermoplastic resin in total. The upper limit of the content of the stabilizer is preferably 4 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, per 100 parts by mass of the polyester resin, the amorphous resin, and / or the second thermoplastic resin in total. The resin composition of the present embodiment may contain only one type of stabilizer, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.

[0080] <Release agent> The resin composition of the present embodiment may contain a release agent, such as an aliphatic carboxylic acid, an ester of an aliphatic carboxylic acid and an alcohol, an aliphatic hydrocarbon compound having a number average molecular weight of 200 to 15,000, wax, or polysiloxane-based silicone oil. For details, please refer to paragraphs 0112 to 0121 of International Publication No. 2020 / 013127, the contents of which are incorporated herein by reference.

[0081] The content of the release agent is usually 0.001 parts by mass or more, preferably 0.01 parts by mass or more, and usually 2 parts by mass or less, preferably 1 part by mass or less, based on 100 parts by mass of the total of the polyester resin and the amorphous resin and / or the second thermoplastic resin. By making the content of the release agent equal to or more than the lower limit of the above range, it is easy to obtain a sufficient effect of releasability, and by making the content of the release agent equal to or less than the upper limit of the above range, sufficient hydrolysis resistance is obtained, and mold contamination during injection molding is less likely to occur. The resin composition of the present embodiment may contain only one type of release agent, or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.

[0082] <Other ingredients> The resin composition may contain other components in addition to the above-mentioned components as necessary, as long as the desired physical properties are not significantly impaired. Examples of other components include various resin additives. The other components may be contained in one type, or in any combination and ratio of two or more types. Specific examples of the additives include flame retardants, flame retardant auxiliaries, nucleating agents, ultraviolet absorbers, antistatic agents, antifogging agents, antiblocking agents, flow improvers, plasticizers, dispersants, and antibacterial agents. In the resin composition of the present embodiment, the total of the polyester resin, the amorphous resin and / or the second thermoplastic resin, the carbon black, and any other components blended as necessary is 100% by mass, and the total of the polyester resin, the amorphous resin and / or the second thermoplastic resin, the carbon black, the reactive compound, the elastomer, the inorganic filler, the stabilizer, and the release agent preferably accounts for 90 to 100% by mass, more preferably 95 to 100% by mass, and even more preferably 99 to 100% by mass. The resin composition of the present embodiment is a polyester resin and an amorphous resin and / or a second thermoplastic resin (absolute value of difference in SP value from the polyester resin (|SP 1 -SP 2 The thermoplastic resin may or may not contain a thermoplastic resin other than the thermoplastic resin having a |) of 0 to 3.0. The resin composition of the present embodiment may be configured to be substantially free of other thermoplastic resins than the polyester resin, the amorphous resin, and / or the second thermoplastic resin. Substantially free means that the content of the other thermoplastic resins is 10% by mass or less of the total amount of the polyester resin, the amorphous resin, and / or the second thermoplastic resin contained in the resin composition, preferably less than 5% by mass, more preferably less than 3% by mass, and even more preferably less than 1% by mass.

[0083] <<Physical Properties>> Next, preferred values ​​for the resin composition of this embodiment will be described. The resin composition of the present embodiment preferably has excellent mechanical strength. The resin composition of the present embodiment is molded into an ISO test piece having a thickness of 4 mm, and the bending strength according to ISO 178 is preferably 100 MPa or more, and more preferably 150 MPa or more. The upper limit is not particularly set, but for example, 300 MPa or less is practical, and even 250 MPa or less satisfies the performance requirements.

[0084] The resin composition of this embodiment is molded into an ISO test piece having a thickness of 4 mm, and has a notched Charpy impact strength according to ISO179 of 5 kJ / m 2 It is preferable that the concentration is 7 kJ / m or more. 2 The upper limit is not particularly limited, but is, for example, 50 kJ / m 2 The following is practical: 30 kJ / m 2 The following is sufficient to meet the performance requirements.

[0085] The resin composition of the present embodiment preferably has excellent fluidity. Specifically, the melt volume rate (MVR) per unit time is preferably 13.0 cm under the conditions of a temperature of 250° C. and a load of 5.0 kgf according to JIS K7210. 3 / 10 minutes or more is preferable, 15.0 cm 3 More preferably, the upper limit of the MVR is 20 cm / min or more. 3 / 10 minutes or less is acceptable.

[0086] <Applications of resin composition> The resin composition of the present embodiment can be applied to various storage containers, electric and electronic equipment parts, office automation (OA) equipment parts, home appliance parts, machine mechanism parts, vehicle mechanism parts, etc. In particular, it can be suitably used for food containers, chemical containers, oil and fat product containers, hollow vehicle parts (various tanks, intake manifold parts, camera housings), vehicle electrical parts (various control units, ignition coil parts, etc.), motor parts, various sensor parts, connector parts, switch parts, breaker parts, relay parts, coil parts, transformer parts, lamp parts, etc.

[0087] More specifically, the resin composition of the present embodiment is preferably used on the laser light absorbing side during laser welding. That is, one example of the use of the resin composition of the present embodiment is as an absorbing resin part during laser welding. The shape of the absorbing resin member is not particularly limited, but since the members are used by being joined together by laser welding, the shape usually has at least a surface contact portion (flat surface, curved surface). In laser welding, the laser light transmitted through the transmitting resin member is absorbed by the absorbing resin member, melting it, and the two members are welded together.

[0088] The resin composition of the present embodiment is also used for laser marking, and is particularly suitable as a resin composition used on the laser light absorbing side during laser welding and for laser marking.

[0089] On the other hand, the laser-transmitting resin member (transmitting resin member) used during laser welding is preferably formed from a laser-transmitting resin composition containing a polyester resin and a light-transmitting dye, and the laser-transmitting resin composition is preferably formed from a resin composition having a light transmittance of 5% or more (upper limit is, for example, 50% or less) at a wavelength of 1064 nm when molded to a thickness of 1.5 mm. The details of the polyester resin are the same as those of the polyester resin described in the section on the resin composition above, and the preferred ranges are also the same. The light-transmitting dye will be described in detail later.

[0090] The shape of the transmissive resin member is not particularly limited, but since the members are used by joining them together by laser welding, the shape usually has at least a surface contact area (flat surface, curved surface). In laser welding, the laser light transmitted through the transmissive resin member is absorbed by the absorbing resin member, melts, and the two members are welded together. Here, the thickness of the transmissive resin member through which the laser light transmits (thickness in the laser transmission direction at the portion through which the laser light transmits) can be appropriately determined, but is, for example, 5 mm or less, preferably 4 mm or less. The lower limit is, for example, 100 μm or more.

[0091] The laser-transmittable resin composition may or may not contain a polycarbonate resin. The details of the polycarbonate resin are the same as those of the polycarbonate resin described in the section on the resin composition of the present embodiment, and the preferred ranges are also the same.

[0092] The laser-transmittable resin composition may contain an elastomer. Details of the elastomer are the same as those described in the section on the resin composition of this embodiment, and the preferred ranges are also the same. The laser-transmittable resin composition may contain a reactive compound. Details of the reactive compound are the same as those described in the section on the resin composition of the present embodiment, and the preferred ranges are also the same. The laser-transmittable resin composition may contain an inorganic filler. Details of the inorganic filler are the same as those of the inorganic filler described in the section on the resin composition of the present embodiment above, and the preferred ranges are also the same. The laser-transmittable resin composition may contain a release agent and / or a stabilizer. The details of the release agent and / or stabilizer are the same as those described in the section on the resin composition of the present embodiment, and the preferred ranges are also the same.

[0093] <<Light-transmitting dye>> Next, the light-transmitting dye contained in the laser-transmitting resin composition will be described. The light-transmitting dye is not particularly limited as long as it transmits at least a certain amount of the laser for laser welding, and any known dye can be used. The light-transmitting dye includes, for example, a dye that has a transmittance of 5% or more when a total of 100% by mass of polybutylene terephthalate resin (e.g., Novaduran (registered trademark) 5008), 30% by mass of glass fiber (e.g., Nippon Electric Glass Co., Ltd., product name: T-127), and 0.2% by mass of a dye (a dye considered to be a light-transmitting dye) are mixed. In addition, by mixing the transparent dye in this embodiment, for example, the transmittance at a wavelength of 1064 nm when the laser-transmitting resin composition is molded to a thickness of 1.5 mm can be made 5% or more. The light-transmitting pigment is usually a dye. The light-transmitting dye can be appropriately selected depending on the application, and the color is not particularly limited. The light-transmitting dye used in this embodiment is preferably a black dye and / or a black dye composition containing two or more chromatic dyes. The black dye composition means a composition that exhibits black color by combining two or more chromatic dyes such as red, blue, and green. A first embodiment of the black pigment composition contains a green pigment and a red pigment, and a second embodiment of the black pigment composition contains a red pigment, a blue pigment and a yellow pigment. Specific examples of light-transmitting dyes include nigrosine, naphthalocyanine, aniline black, phthalocyanine, porphyrin, perinone, quaterrylene, azo, azomethine, anthraquinone, pyrazolone, squaric acid derivatives, perylene, chromium complexes, and immonium. Azomethine, anthraquinone, and perinone are preferred, and anthraquinone and perinone are more preferred.

[0094] Examples of commercially available products include colorants e-BIND LTW-8731H and e-BIND LTW-8701H manufactured by Orient Chemical Industry Co., Ltd., colorants Plast Yellow 8000, Plast Red M 8315, Plast Red 8370, and Oil Green 5602 manufactured by Arimoto Chemical Industry Co., Ltd., colorants Macrolex Yellow 3G, Macrolex Red EG, and Macrolex Green 5B manufactured by LANXESS, and KP Plast HK, KP Plast Red HG, KP Plast Red H2G, KP Plast Blue R, KP Plast Blue GR, and KP Plast Green G manufactured by Kiwa Chemical Industry Co., Ltd. Furthermore, dyes described in Japanese Patent No. 4157300 and Japanese Patent No. 4040460 can also be used, the contents of which are incorporated herein by reference.

[0095] The laser-transmittable resin composition used in this embodiment preferably contains 0.001 to 5 parts by mass of the light-transmittable dye relative to 100 parts by mass of the polyester resin. The lower limit of the content is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, and even more preferably 0.2 parts by mass or more. By setting it to the lower limit or more, the transmissible resin member is colored, and the design of the laser-welded product is improved. In addition, the upper limit of the content is preferably 3 parts by mass or less, more preferably 2 parts by mass or less, even more preferably 1 part by mass or less, even more preferably 0.8 parts by mass or less, and even more preferably 0.5 parts by mass or less. By setting it to the upper limit or less, bleeding out of the light-transmittable dye can be effectively suppressed. The laser-transmittable resin composition may contain only one type of light-transmittable dye, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.

[0096] The laser-transmittable resin composition may contain other components in addition to those described above, as necessary, as long as the desired physical properties are not significantly impaired. Examples of other components include various resin additives. The other components may be contained alone or in any combination and ratio of two or more. Specific examples of the additives include flame retardants, flame retardant auxiliaries, nucleating agents, ultraviolet absorbers, antistatic agents, antifogging agents, antiblocking agents, flow improvers, plasticizers, dispersants, and antibacterial agents. The laser transparent resin composition used in the present embodiment is 100% by mass in total of the polyester resin, light transparent dye, and components blended as necessary, and the polyester resin, light transparent dye, and polycarbonate resin, flame retardant, flame retardant assistant, anti-dripping agent, reactive compound, elastomer, inorganic filler, stabilizer, and release agent blended as necessary preferably account for 90 to 100% by mass in total, more preferably 95 to 100% by mass, and even more preferably 99 to 100% by mass.

[0097] <Method of producing resin composition> The resin composition and the laser-transmitting resin composition of the present embodiment can be produced by a conventional method for preparing a resin composition. Usually, each component and various additives added as required are thoroughly mixed together and then melt-kneaded in a single-screw or twin-screw extruder. Alternatively, the resin composition can be prepared by not mixing each component in advance, or by mixing only a part of the components in advance, feeding the mixture to an extruder using a feeder, and melt-kneading the mixture. The resin composition of the present embodiment particularly includes adding and melt-kneading 0.01 part by mass or more and 0.4 part by mass or less of carbon black to a total of 100 parts by mass of the polyester resin and the amorphous resin and / or the second thermoplastic resin, and preferably includes adding at least a portion of the amorphous resin and / or the second thermoplastic resin as a masterbatch of the carbon black. When a fibrous inorganic filler such as glass fiber is used, it is also preferable to feed it from a side feeder midway through the cylinder of the extruder. The heating temperature during melt kneading can usually be appropriately selected from the range of 220 to 300°C. If the temperature is too high, decomposition gas is likely to be generated, which may cause opacity. Therefore, it is desirable to select a screw configuration that takes into consideration shear heat generation, etc. In order to suppress decomposition during kneading and molding in the subsequent process, it is desirable to use an antioxidant or heat stabilizer.

[0098] <Method of manufacturing absorbent resin member and permeable resin member> The manufacturing method of the absorbent resin member and the permeable resin member is not particularly limited, and any molding method generally used for polyester resin compositions can be used. Examples include injection molding, ultra-high speed injection molding, injection compression molding, two-color molding, gas-assisted hollow molding, molding using a heat-insulating mold, molding using a rapid heating mold, foam molding (including supercritical fluid), insert molding, IMC (in-mold coating molding) molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, blow molding, etc., among which injection molding is preferred. For details of injection molding, refer to paragraphs 0113 to 0116 of Japanese Patent No. 6183822, the contents of which are incorporated herein by reference.

[0099] <Method of manufacturing laser welded products> Next, a laser welding method will be described. In this embodiment, the transmissible resin member and the absorptive resin member can be laser-welded to form a laser-welded product. By laser welding, the transmissible resin member and the absorptive resin member can be firmly welded without using an adhesive. The transmissive resin member and the absorptive resin member may be laser welded by any known laser welding method, but are suitable for galvano scanning type laser welding. Galvano scanning type laser welding, also known as quasi-simultaneous welding, is a method in which a laser beam is scanned with a built-in galvanometer mirror. By using galvano scanning type laser welding, the entire welded part is heated almost simultaneously, so the residual stress of the resulting laser welded product tends to be smaller. That is, a preferred example of a method for producing a laser welded product of this embodiment is to use the kit of this embodiment or the resin composition of this embodiment, and a laser-transmittable resin composition having a light transmittance of 5% or more and less than 25% at a wavelength of 1064 nm when molded to a thickness of 1.5 mm, and to perform galvano scanning laser welding.

[0100] The laser light source used in laser welding can be determined according to the absorption wavelength of the light of the light-absorbing dye, and a laser with a wavelength in the range of 800 to 1100 nm is preferable. The type of laser light to be irradiated can include, for example, a solid-state laser, a fiber laser, a semiconductor laser, a gas laser, and a liquid laser. For example, a YAG (yttrium aluminum garnet crystal) laser (wavelengths of 1064 nm and 1070 nm) and an LD (laser diode) laser (wavelengths of 808 nm, 840 nm, 940 nm, and 980 nm) can be preferably used. Among them, laser light with wavelengths of 940 nm, 980 nm, and 1070 nm are preferable.

[0101] The laser focal diameter is preferably 0.1 mm or more, more preferably 0.2 mm or more, and even more preferably 0.5 mm or more. By setting it to the upper limit or less, the welding strength of the laser welded part can be further increased. In addition, the laser irradiation diameter is preferably 30 mm or less, more preferably 10 mm or less, and even more preferably 3.0 mm or less. By setting it to the lower limit or more, the welding width can be more effectively controlled. The focal diameter of the laser light can be selected according to the width and height of the surface to be welded. The laser light may be focused or defocused on the joining surface, and it is preferable to select an appropriate method depending on the desired welded body.

[0102] The laser output is preferably 1 W or more, more preferably 10 W or more, even more preferably 30 W or more, and even more preferably 100 W or more. By setting it to the lower limit or more, more sufficient welding strength can be obtained even if the welding time is short. In addition, the laser output is preferably 1000 W or less, more preferably 500 W or less, even more preferably 400 W or less, and even more preferably 300 W or less. By setting it to the upper limit or less, the cost of laser welding equipment can be effectively reduced. The laser irradiation speed is preferably 10 mm / s or more, more preferably 30 mm / s or more, even more preferably 50 mm / s or more, and even more preferably 500 mm / s or more. By making it equal to or more than the lower limit, the residual stress of the laser welded product can be more effectively reduced. In addition, the laser irradiation speed is preferably 20,000 mm / s or less, more preferably 10,000 mm / s or less, even more preferably 5,000 mm / s or less, and even more preferably 3,000 mm / s or less. By making it equal to or less than the upper limit, a more sufficient welding strength can be obtained for the welded product. In addition, with regard to the laser scanning method, it is preferable to adjust the laser output, the line to be welded, the scanning speed, and / or the scanning method according to the shape of the joining surface from the viewpoints of welding efficiency, welding strength, welding appearance, and equipment load.

[0103] More specifically, for example, when welding a transparent resin member and an absorptive resin member, first, the parts to be welded of both are brought into contact with each other. At this time, the welded parts of both are preferably in surface contact, and may be flat surfaces, curved surfaces, or a combination of flat surfaces and curved surfaces. When maintaining the overlapped state, a transparent plate material such as a glass plate, a quartz plate, or an acrylic plate may be placed on the transparent resin member, that is, on the laser irradiation side, and pressure may be applied. In particular, when a glass plate or a quartz plate is placed, it is suitable for promoting the dissipation of heat generated during laser welding and obtaining a good appearance. In addition, pressure may be applied with a metal plate surrounding the periphery of the part to be welded of the transparent resin member. Next, a laser beam is irradiated from the transparent resin member side. At this time, a lens may be used to focus the laser beam at the interface between the two members, if necessary. The focused beam passes through the transparent resin member and is absorbed near the surface of the absorbing resin member, generating heat and melting it. The heat is then transferred to the transparent resin member by thermal conduction, melting it, forming a molten pool at the interface between the two members, and after cooling, the two members are joined together. In this way, the laser welded product of the transmitting resin member and the absorbing resin member has high weld strength. Note that the laser welded product in this embodiment includes not only finished products and parts, but also members that form part of these products and parts.

[0104] The laser welded product of the transmissive resin member formed from the above-mentioned laser-transmittable resin composition and the absorptive resin member formed from the resin composition can have a laser weld strength of 800 N or more, 1000 N or more, 1100 N or more, or 1200 N or more. The upper limit of the laser weld strength is not particularly specified, but 4000 N or less is practical. The laser weld strength is measured according to the description of the examples described later.

[0105] <Kits and laser welded parts> The kit of the present embodiment includes the resin composition of the present embodiment and a laser-transmitting resin composition. In the kit, the resin composition of the present embodiment serves as a laser-absorbent resin composition. Such a kit has excellent laser weldability and is preferably used as a kit for producing a molded product (laser-welded product) by laser welding. Furthermore, laser marking can also be performed. That is, the resin composition of the present embodiment included in the kit serves as a laser-ray-absorbent resin composition, and a molded article formed from such a laser-ray-absorbent resin composition becomes an absorbing resin member for laser beams during laser welding. The kit of the present embodiment may also be a kit having a laser-absorbing resin member formed from the resin composition of the present embodiment and a laser-transmitting resin composition containing a polyester resin and a light-transmitting dye. The laser welded product of this embodiment can be manufactured by a manufacturing method including irradiating a laser to a laser-absorbing resin member formed from the resin composition of this embodiment to perform laser marking, and laser welding the laser-absorbing resin member and a laser-transmitting resin member formed from a laser-transmitting resin composition containing a polyester resin and a light-transmitting dye. When manufacturing the laser welded product of this embodiment, the laser welding and the laser marking may be performed in any order, or may be performed simultaneously. The absorbing resin member formed from the resin composition of this embodiment can be laser marked.

[0106] The molded product obtained by laser welding in this embodiment has good mechanical strength, high welding strength, and little damage to the resin due to laser irradiation, and can be used in various applications, such as various storage containers, electrical and electronic equipment parts, office automation (OA) equipment parts, home appliance parts, machine mechanism parts, and vehicle mechanism parts. In particular, it can be suitably used in food containers, pharmaceutical containers, oil and fat product containers, hollow vehicle parts (various tanks, intake manifold parts, camera housings), vehicle electrical parts (various control units, ignition coil parts, etc.), in-vehicle electronic parts and sensor parts (housings for millimeter-wave radar, LiDAR, ECU cases, sonar sensors, etc.), electronically controlled throttle bodies, motor parts, various sensor parts, connector parts, switch parts, breaker parts, relay parts, coil parts, transformer parts, lamp parts, etc. In particular, the resin composition and kit of this embodiment are suitable for in-vehicle camera parts and in-vehicle camera modules including in-vehicle camera parts, millimeter-wave radar modules, sensor modules, and electric parking brake (EPB) parts. EXAMPLES

[0107] The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments used in the examples are difficult to obtain due to discontinuation or the like, measurements can be made using other instruments with equivalent performance.

[0108] 1.Raw materials The following raw materials were used: [Table 1]

[0109] [Table 2]

[0110] 2. Examples 1 and 2, Comparative Examples 1 to 6 <Production of Resin Composition (Pellets)> As shown in Table 3 or Table 4, the components other than the glass fiber were placed in a stainless steel tumbler and mixed by stirring for 1 hour. Each component in Table 3 or Table 4 is expressed in parts by mass. The obtained mixture was put into the main hopper of a 30 mm vent-type twin-screw extruder (manufactured by Japan Steel Works, Ltd., "TEX30α"), and the glass fiber (GF) was fed from the seventh side feeder from the hopper. The mixture was kneaded and extruded in a strand shape under the conditions of extruder barrel setting temperatures C1 to C15 of 260°C, die temperature of 250°C, screw rotation speed of 200 rpm, and discharge rate of 40 kg / hour, to obtain pellets of the resin composition.

[0111] <MVR of resin composition> The pellets obtained above were subjected to melt volume rate per unit time (MVR, unit: cm) measurement at a temperature of 250°C and a load of 5.0 kgf in accordance with JIS K7210. 3 / 10min) was measured. For the measurement, a melt indexer manufactured by Takara Industries Co., Ltd. was used. The higher the MVR, the better the liquidity.

[0112] <Bending properties> The pellets obtained above were dried at 110°C for 5 hours, and then injection molded into 4 mm thick ISO test pieces using an injection molding machine (Japan Steel Works, Ltd., "J85AD") under conditions of a cylinder temperature of 250°C and a mold temperature of 80°C. In accordance with ISO178, the flexural strength (unit: MPa) and flexural modulus (unit: MPa) were measured at a temperature of 23°C using the above ISO tensile test pieces (4 mm thick).

[0113] <Notched Charpy impact strength> The pellets obtained above were dried at 110°C for 5 hours, and then injection molded into 4 mm thick ISO test pieces using an injection molding machine (Japan Steel Works, Ltd., "J85AD") under conditions of a cylinder temperature of 250°C and a mold temperature of 80°C. The notched Charpy impact strength was measured according to ISO179.

[0114] <Disc warpage> Using the above resin composition, a disk with a diameter of 100 mm and a thickness of 1.6 mm was molded using a side gate mold with an injection molding machine (Nissei Plastic Industrial Co., Ltd.'s "NEX80-9E") under conditions of a cylinder temperature of 260°C and a mold temperature of 80°C, a filling time of 0.5 seconds, and a holding pressure of 50% of the peak pressure. After molding, the disk was left overnight in an environment of 23°C and 50% RH, and the warpage of the disk (unit: mm) was measured using a Keyence Corporation's three-dimensional measuring machine (VL series). Each sample was measured five times, and the average value was calculated.

[0115] <Laser welding strength> <<Production of laser-transmitting resin composition (pellets)>> The following materials were used as raw materials for the laser-transmittable resin composition. Polybutylene terephthalate resin (Mitsubishi Engineering Plastics 5008-C): 47 parts by weight Polycarbonate resin (Mitsubishi Engineering Plastics H-4000FN): 20 parts by weight Nucleating agent (Hayashi Kasei Micron White 5000S): 0.005 parts by weight Stabilizer (ADEKA Adeka STAB AX-71): 0.1 parts by weight Stabilizer (ADEKA Adekastab AO-60): 0.2 parts by weight Reactive compound (Changchun CNE220): 1.0 parts by mass Release agent (Clariant Licowax E): 0.4 parts by weight Dye 1 (Plast Red 8370, manufactured by Arimoto Chemical Co., Ltd.): 0.42 parts by weight Dye 2 (Kiwa Kagaku Kogyo Co., Ltd. KP Plast Blue R): 0.45 parts by mass Dye 3 (Kiwa Kagaku Kogyo Co., Ltd. KP Plast Yellow HK): 0.38 parts by mass Inorganic pigment (Tokan Material Technology Co., Ltd. 42-920A): 0.1 parts by weight Glass (Nippon Electric Glass Co., Ltd. T-127): 30 parts by weight

[0116] The above ingredients except for the glass fiber were put into a stainless steel tumbler and mixed by stirring for 1 hour. The obtained mixture was put into the main hopper of a 30 mm vent type twin screw extruder (manufactured by Japan Steel Works, Ltd., "TEX30α"), and the glass fiber (GF) was fed from the seventh side feeder from the hopper. The extruder barrel temperature setting C1 to C15 was set at 260°C, the die was set at 250°C, the screw rotation speed was set at 200 rpm, and the discharge rate was set at 40 kg / hour. The mixture was then extruded into a strand shape to produce a laser-transmitting resin composition (pellets).

[0117] <<Transmittance of transparent resin material>> The laser-transmittable resin composition pellets were dried at 120°C for 7 hours, and then a 60 mm x 60 mm x 1.5 mm thick transmittance measurement (transmittance resin member) plate for transmittance measurement was injection molded using an injection molding machine ("NEX80-9E" manufactured by Nissei Plastic Industrial Co., Ltd.) under injection conditions of a cylinder temperature of 260°C, a mold temperature of 60°C, and an injection speed of 90 mm / sec. The transmittance (%) at a wavelength of 1064 nm was measured using an ultraviolet-visible-near infrared spectrophotometer from a point 45 mm from the gate side and at the center of the width of the test plate, and was found to be 41%. The ultraviolet-visible-near infrared spectrophotometer used was a Shimadzu Corporation "UV-3100PC" equipped with an integrating sphere.

[0118] <<Preparation of transparent resin parts>> The laser-transmittable resin composition obtained above was dried at 120°C for 7 hours, and then molded using an injection molding machine ("J55" manufactured by Japan Steel Works, Ltd.) at a cylinder temperature of 260°C and a mold temperature of 60°C to produce a molded product (transmittable resin member I) having a thickness of 1.5 mm as shown in Figure 1.

[0119] <<Production of absorbent resin components>> The light absorbing resin pellets obtained above were dried at 120°C for 7 hours, and then molded using an injection molding machine ("J55" manufactured by Japan Steel Works, Ltd.) at a cylinder temperature of 260°C and a mold temperature of 60°C to produce a molded product (absorbent resin member II) with a rib thickness of 1.0 mm as shown in Figure 2.

[0120] As shown in Figure 3, the transparent resin member and the absorptive resin member were prepared by stacking a lid-shaped transparent resin member I on a box-shaped absorptive resin member II, and a laser light source was positioned vertically above the flange, which is the overlapping part of the transparent resin member I and the absorptive resin member II. A pressing force of 4.92 N / mm (extrusion force during welding) was applied inwardly from both sides in the thickness direction to the overlapping part of the transparent resin member I and the absorptive resin member II using a glass plate, and a laser was irradiated under the following conditions to obtain a laser welded product. The welding equipment is as follows:

[0121] <<Galvano scanning type laser welding>> Laser device: IPG YLR-300-AC-Y14 Wavelength: 1070nm Collimator: 7.5mm Laser Type: Fiber Laser power: 150W Galvanometer scanner: ARGES Fiber Elephants21 Aperture: 21mm Laser irradiation speed: 900mm / s Laser irradiation cycles: 20 or 25 cycles Welded part circumference: 137mm The laser beam was defocused and the position of the laser scanner was adjusted so that the spot diameter irradiated onto the welding surface was 2 mm.

[0122] <<Laser welding strength measurement>> As shown in Figure 4, holes 21, 22 were drilled, and welding strength measuring jigs 23, 24 were placed inside. Measurement jigs 25, 26 were inserted from the top and bottom of the box made of the permeable resin member I and the absorptive resin member II prepared above, respectively, and connected to the jigs 23, 24 stored inside. The boxes were then pulled vertically (pulling speed: 5 mm / min) to measure the strength at which the permeable resin member I and the absorptive resin member II separated (welding strength). The equipment used was a universal 1t Tensilon testing machine (load cell 10 kN) manufactured by ORIENTEC.

[0123] <Laser marking properties> The center of the absorbent resin member obtained above was laser marked in a size of 10 mm x 10 mm square under the following conditions. The marking was evaluated on a four-level scale of A to D as shown below. Laser marking device: Panasonic LP-Z310 Laser type: Yb fiber laser (wavelength 1064 nm) Laser power: 30W Scan speed: 600mm / s Printing pulse period: 50μs <<Evaluation>> After laser marking, the visibility of the marked area against the non-marked area was confirmed by visual observation and evaluated according to the following evaluation criteria. The evaluation was performed by five experts and judged by majority vote. A: Marked and non-marked areas can be visually distinguished from each other with sufficient visibility. B: The visibility of the markings was poor when visually inspected.

[0124] [Table 3]

[0125] [Table 4]

[0126] In Tables 3 and 4 above, "difference in SP value of resin" refers to the difference in absolute value between the SP value of PBT and the SP value of the resin used in the carbon black master batch (|SP 1 -SP 2 |). In Tables 3 and 4, the "amount of CB itself" refers to the amount of carbon black (parts by mass) per 100 parts by mass of the polyester resin and the amorphous resin combined, i.e., the amount of carbon black itself not including the resin used in the master batch. As is clear from the above results, the molded articles made from the resin composition of the present embodiment had high laser welding strength and were capable of being laser marked (Examples 1 and 2). In contrast, when carbon black was not masterbatched with an amorphous resin or a thermoplastic resin satisfying a predetermined SP value (Comparative Example 1 and Comparative Examples 3 to 6), the laser weldability was poor and the visibility of the laser marking was poor. On the other hand, even when carbon black was masterbatched with an amorphous resin or a thermoplastic resin satisfying a predetermined SP value, when the amount of carbon black blended was high (Comparative Example 2), laser marking was possible, but laser weldability was poor. [Explanation of symbols]

[0127] 21, 22 holes 23, 24 Fixture for measuring adhesion 25, 26 Measuring tool

Claims

1. A resin composition comprising: more than 50 parts by mass but not exceeding 90 parts by mass; and 10 parts by mass or more but not exceeding 50 parts by mass of an amorphous resin, and 0.01 part by mass or more but not exceeding 0.4 part by mass of carbon black, per 100 parts by mass in total of more than 50 parts by mass but not exceeding 90 parts by mass of a polyester resin and 10 parts by mass or more but not exceeding 50 parts by mass of an amorphous resin, wherein at least a portion of the amorphous resin is derived from a master batch of the carbon black.

2. The resin composition of claim 1 , wherein the polyester resin comprises a polybutylene terephthalate resin.

3. The SP value of the polyester resin (SP 1 ) and the SP value of the amorphous resin (SP 2 ) absolute value of the difference (|SP 1 -SP 2 The resin composition according to claim 1 or 2, wherein |) is 0 to 3.

0.

4. The resin composition according to claim 1 , wherein the amorphous resin comprises a styrene-based resin.

5. The resin composition according to claim 1 or 2, wherein the amorphous resin comprises an acrylonitrile-styrene resin.

6. The resin composition according to claim 1 or 2, further comprising an elastomer.

7. The resin composition according to claim 1 or 2, which is used on the laser light absorbing side during laser welding.

8. The resin composition according to claim 1 or 2, which is used on the laser light absorbing side during laser welding and is for laser marking.

9. the polyester resin comprises a polybutylene terephthalate resin, the amorphous resin comprises an acrylonitrile-styrene resin, Further comprising an elastomer, The resin composition according to claim 1, which is used on the laser light absorbing side during laser welding and is for laser marking.

10. The polyester resin contains 0.01 parts by mass or more and 0.4 parts by mass or less of carbon black relative to 100 parts by mass of a total of a polyester resin and a second thermoplastic resin other than the polyester resin, and at least a part of the second thermoplastic resin is derived from a master batch of the carbon black, and the SP value of the polyester resin (SP 1 ) and the SP value of the second thermoplastic resin (SP 22 ) absolute value of the difference (|SP 1 -SP 22 |) is 0 to 3.

0.

11. the polyester resin comprises a polybutylene terephthalate resin, The resin composition according to claim 10, which is used on the laser light absorbing side during laser welding and is for laser marking.

12. A pellet of the resin composition according to any one of claims 1, 2, 9, 10 and 11.

13. A molded article formed from the resin composition according to any one of claims 1, 2, 9, 10 and 11.

14. 1. A method for producing a resin composition, comprising: adding and melt-kneading 0.01 part by mass or more and 0.4 part by mass or less of carbon black to a total of 100 parts by mass of more than 50 parts by mass and 90 parts by mass or less of a polyester resin and 10 parts by mass or more and 50 parts by mass or less of an amorphous resin, wherein at least a portion of the amorphous resin is added as a master batch of the carbon black.

15. The method according to claim 14, wherein the resin composition is the resin composition according to any one of claims 1, 2, 9, 10 and 11.

16. A kit comprising a laser-transmittable resin composition and the resin composition according to any one of claims 1, 2, 9, 10 and 11.

17. 12. A laser-welded product comprising a laser-transmittable resin workpiece formed from a laser-transmittable resin composition and a laser-absorbent resin workpiece formed from the resin composition according to claim 1.

18. Irradiating a laser on a laser-absorbing resin member to perform laser marking; and The method for producing a laser welded product according to claim 17, comprising laser welding a laser-transmitting resin workpiece and the laser-absorbing resin workpiece together.

19. The method for producing a laser welded product according to claim 18, wherein the laser welding is performed by galvano scanning type laser welding.

Citation Information

Patent Citations

  • Polyester resin composition for wattmeter outer package

    JP2014133790A

  • Polyester resin composition

    JP2017155147A

  • Polyester-based resin composition

    JP2020152770A

  • Laser welded body