Electrolyte and electrochemical device

The electrolytic solution, composed of non-flammable fluorine and high-flash point solvents, addresses the challenge of maintaining conductivity and safety in electrochemical devices by using specific solvent blends, ensuring high ionic conductivity and reduced fire risk.

JP2024145463APending Publication Date: 2024-10-15ZEON CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023057825
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing electrochemical devices face challenges in maintaining high ionic conductivity at low temperatures while being highly safe due to the use of flammable organic solvents with low flash points, which pose a fire risk.

Method used

An electrolytic solution comprising a non-flammable fluorine solvent component and specific high-flash point solvent components, blended in specific proportions, along with a salt, to achieve high ionic conductivity and safety.

Benefits of technology

The solution provides an electrolytic solution with high ionic conductivity at low temperatures and enhanced safety by reducing the risk of fire, suitable for electrochemical devices like lithium ion batteries and capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145463000001
    Figure 2024145463000001
  • Figure 2024145463000002
    Figure 2024145463000002
  • Figure 2024145463000003
    Figure 2024145463000003
Patent Text Reader

Abstract

To provide: electrolyte for an electrochemical device, having such an advantage that it indicates a high ion conductance even under low temperature and it has high safety; and the electrochemical device which gains such an advantage.SOLUTION: Electrolyte for an electrochemical device including salt and solvent is provided, the solvent is comprised of a nonflammable fluorine solvent component (SF) and the balance consisting of a solvent component (SR). A ratio of the solvent component (SF) in a 100 wt% of an electrolyte is 15 wt% or more, and the solvent component (SR) includes a solvent component (SR80) having a flash point exceeding 80°C. The solvent component (SR80) includes a solvent component (SR80A), and the solvent component (SR80A) is one or more kinds of a specific chemical compound group. A ratio of the solvent component (SR80) in the 100 wt% of the solvent component (SR) and a ratio of the solvent component (SR80) in 100 wt% of the solvent component (SR) are within a specific range.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolyte solution that can be used in electrochemical devices such as lithium ion primary batteries, lithium ion secondary batteries, and capacitors, and to an electrochemical device containing the electrolyte solution. [Background technology]

[0002] 2. Description of the Related Art In general, electrochemical devices such as primary batteries, secondary batteries, and capacitors include an exterior body and contents sealed therein, such as an electrolyte, electrodes, and separators, for realizing the functions of the device. Generally, an electrolytic solution contains a salt component that functions as an electrolyte, and a solvent component. Various types of solvent components have been conventionally known (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-348762 A [Patent Document 2] JP 2000-223151 A Summary of the Invention [Problem to be solved by the invention]

[0004] An organic solvent with a low flash point is often used in the electrolyte of an electrochemical device. Examples of organic solvents with a low flash point include chain carbonates such as dimethyl carbonate and diethyl carbonate, and chain esters such as methyl acetate and ethyl propionate. Such organic solvents are useful for helping the electrolyte to remain liquid, improving the performance of the electrolyte at low temperatures, and improving the permeability of the electrolyte to other components of the device.

[0005] However, solvents with low flash points are highly flammable and therefore prone to fires, so it is believed that devices will be safer if electrolytes that do not contain such flammable organic solvents are used.

[0006] However, it is difficult to reduce the proportion of low-flammability solvents and maintain other performances as an electrolyte (maintaining a liquid state, exhibiting sufficient ionic conductivity at low temperatures, improving permeability, improving charge / discharge efficiency, etc.). Specifically, examples of known high-flash point solvents include propylene carbonate, γ-butyrolactone, ethylene carbonate, and fluoroethylene carbonate. Propylene carbonate and γ-butyrolactone are liquid at room temperature, so it is easy to obtain a liquid electrolyte, and have relatively high ionic conductivity at low temperatures, but they are incompatible with carbonaceous materials, particularly graphite material negative electrodes, and tend to have low charge / discharge efficiency. Ethylene carbonate and fluoroethylene carbonate are compatible with carbonaceous material negative electrodes containing graphite, and have high charge / discharge efficiency, but are solid at room temperature, so it is difficult to obtain a liquid electrolyte. In particular, solvents mainly composed of ethylene carbonate tend to solidify at room temperature, and have particularly low low-temperature performance.

[0007] It is therefore an object of the present invention to provide an electrolyte for electrochemical devices which exhibits high ionic conductivity even at low temperatures and is highly safe, as well as an electrochemical device which enjoys such advantages. [Means for solving the problem]

[0008] The present inventors have conducted research to solve the above problems, and as a result, have found that the above problems can be solved by adopting specific solvent components constituting an electrolyte solution and mixing them in a specific ratio, thereby completing the present invention. That is, the present invention is as follows.

[0009] (1) An electrolyte for an electrochemical device, comprising a salt and a solvent, The solvent is composed of a non-flammable fluorine solvent component (SF) and a remaining solvent component (SR), The proportion of the solvent component (SF) in 100% by weight of the electrolytic solution is 15% by weight or more, The solvent component (SR) includes a solvent component (SR80) having a flash point of more than 80° C., The solvent component (SR80) includes a solvent component (SR80A), The solvent component (SR80A) is one or more compounds that do not have a carbon-carbon unsaturated bond and is selected from the group consisting of cyclic carbonates having 4 or more carbon atoms, fluoroethylene carbonate, cyclic compounds having 4 or more carbon atoms and having one or more ester bonds in the molecule, dinitriles having 3 or more carbon atoms, sulfones having 2 or more carbon atoms, oxazolidone derivatives having 4 or more carbon atoms, imidazolidinone derivatives having 5 or more carbon atoms, carbonates having 9 or more carbon atoms, lactam derivatives having 5 or more carbon atoms, and mixtures thereof; The ratio of the solvent component (SR80) in 100% by weight of the solvent component (SR) is 90% by weight or more, The electrolyte solution has a ratio of the solvent component (SR80A) of 20% by weight or more in 100% by weight of the solvent component (SR). (2) The electrolyte solution according to (1), wherein the solvent component (SR80) contains ethylene carbonate. (3) The solvent contains an additive (B) as the solvent component (SF) or the solvent component (SR80), The electrolyte solution according to (1) or (2), wherein the additive (B) is at least one selected from the group consisting of a cyclic sulfate ester compound, a vinyl ethylene carbonate compound, and a fluorine compound having an unsaturated bond. (4) The electrolyte according to (3), further comprising sultone. (5) ClO4 as the salt in 100% by weight of the electrolyte - , ClO3 - , and NO3 - The electrolyte solution according to any one of (1) to (4), wherein the total proportion of is 3% by weight or less. (6) The electrolyte according to any one of (1) to (5), having a flash point of more than 80° C. (7) An electrochemical device comprising a positive electrode, a negative electrode, and an electrolyte, The electrolytic solution is the electrolytic solution according to any one of (1) to (6), The electrochemical device, wherein the negative electrode comprises a carbon material. (8) The electrochemical device according to (7), wherein the electrode is a negative electrode containing graphite as the carbon material. (9) The electrochemical device according to (7) or (8), which is an ion battery. (10) The electrochemical device according to (9), which is a lithium ion battery. (11) The electrochemical device according to any one of (7) to (10), which has a storage capacity of 3 Ah or more. Effect of the Invention

[0010] According to the present invention, there are provided an electrolyte for electrochemical devices which exhibits high ionic conductivity even at low temperatures and is highly safe, as well as an electrochemical device which enjoys such advantages. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the present invention will be described in detail with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples described below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto.

[0012] In the following description, the term "solvent" is interpreted in a broad sense and includes the meaning of a dispersion medium. That is, the term "solvent" includes not only a medium in a solution (i.e., a mixture of a liquid medium substance and a solute substance dissolved therein), but also a medium in a dispersion (i.e., a mixture of a liquid medium substance and a dispersion substance dispersed therein as solid particles or emulsion particles), and a medium in a mixture containing both a solute and a dispersion substance.

[0013] (electrolyte) The electrolyte of the present invention comprises a salt and a solvent.

[0014] (salt) A salt is a component that functions as an electrolyte in an electrolytic solution. A salt is generally expressed as a combination of an anion and a cation. Examples of anions and cations include various anions and cations known to constitute electrolytes.

[0015] Specific examples of anions include F - , Cl - , Br - , I - , PF6 - , AsF6 - , BF4 - , B(C2O4)F2 - , B(C2O4)2 - , SbF6 - , AlCl4 - , ClO4 - , CF3SO3 - , C4F9SO3 - , CF3COO - , (CF3CO)2N - , (CF3SO2)3C - , CF2(CF2SO2)2N - (Cyclohexafluoropropane-1,3-bis(sulfonyl)imide), (FSO2)2N - (FSI, bisfluorosulfonylimide), (CF3SO2)2N - (TFSI, bistrifluoromethanesulfonylimide), and (C2F5SO2)2N - Examples include: The salt preferably contains an imide anion as an anion, from the viewpoint of obtaining effects such as a wider temperature range in which the salt is liquid. Furthermore, as the imide anion, fluorine-containing sulfonylimides such as bisfluorosulfonylimides and bistrifluoromethanesulfonylimides are particularly preferred from the above viewpoints. In particular, bisfluorosulfonylimides are preferred. On the other hand, from the viewpoint of safety, it is preferable that the salt does not contain an oxidizing anion or contains a small proportion of an oxidizing anion. Specifically, the oxidizing anion ClO4 - , ClO3 - , and NO3 -It is preferable that the electrolyte does not contain these or contains only a small amount of these. More specifically, the electrolyte contains ClO4 - , ClO3 - , and NO3 - The total proportion of is preferably 3% by weight or less, more preferably 2% by weight or less, and even more preferably 1% by weight or less.

[0016] As the cation, known cations such as alkali metal cations, alkaline earth metal cations, and organic cations can be used. Specific examples thereof include Li + , Na + , Mg 2+ , TEA (triethylammonium cation), TBA (tributylammonium cation), and EMI (ethylmethylimidazolium cation). The salt preferably contains an alkali metal cation, an alkaline earth metal cation, or a combination thereof as a cation, since flammability is suppressed. From the viewpoint of expressing the preferable characteristics, when the salt contains a plurality of kinds of cations, the proportion of the amount of alkali metal cations and alkaline earth metal cations in the cations constituting the salt is preferably 50 mol % or more.

[0017] The ratio of salt in the electrolyte of the present invention is not particularly limited, but can be appropriately adjusted within a range that allows the electrolyte to exhibit its performance. Specifically, the ratio of salt in the electrolyte is preferably 0.1 mol / kg or more, more preferably 0.3 mol / kg or more, and is preferably 10 mol / kg or less, more preferably 6 mol / kg or less. In the present application, the unit of "mol / kg" for the ratio of salt in the electrolyte indicates the number of moles of salt per kg of components other than salt in the electrolyte. On the other hand, when the ratio of salt is expressed in the unit "mol / L", it indicates the number of moles of salt contained in 1 liter of the entire electrolyte. In addition, the amount of salt in the electrolytic solution of the present invention is preferably a value somewhat larger than the solvent component (SR80) in terms of reducing the volatility of the solvent and suppressing flammability. Specifically, the molar ratio of the solvent component (SR80) / cation of the salt is preferably 5 or less, more preferably 4 or less, and even more preferably 3 or less.

[0018] (solvent) The solvent consists of a non-flammable fluorine solvent component (SF) and the remaining solvent component (SR).

[0019] (Solvent composition (SF)) A non-flammable fluorinated solvent component (SF) is a solvent component that has a molecular structure containing fluorine and is a non-flammable substance. Here, a non-flammable solvent component refers to a solvent component that does not have a flash point at a temperature lower than its own boiling point.

[0020] If the electrolyte contains the solvent component (SF), the electrolyte as a whole can easily have a high flash point or no flash point, which reduces the risk of fire when the electrochemical device overheats for some reason and the electrolyte is released outside the device.

[0021] In this application, the flash points of liquids such as solvents, their components, and electrolytes are values ​​evaluated by flash point measurements as specified in the tag closed cup test (JIS K 2265-1) and the Cleveland open cup test (JIS K 2265-4). Flash points up to 79°C are evaluated by the tag closed cup test, and if no flash point of 79°C or less is observed, they are further evaluated by the Cleveland open cup test. Substances that do not ignite and no flash point is observed in the Cleveland open cup test fall into the category of substances with a flash point of 80°C or higher.

[0022] The electrolyte of the present invention may contain only one type of substance as the solvent component (SF), or may contain two or more types of substances. When two or more types of substances are contained, the types and ratios of the substances can be appropriately adjusted to obtain desired physical properties such as boiling point and viscosity.

[0023] The solvent component (SF) preferably has a fluorine atom ratio of 50% by weight or more in its molecule. By having a fluorine atom ratio of 50% by weight or more, the oxidation stability of the electrolyte is increased and the flammability is reduced.

[0024] The solvent component (SF) preferably has one or more structures selected from the group consisting of -CFH-, -CF2H, -CH2-CF2-, -CH2CF3, and a ring structure in one molecule, and more preferably has two or more structures. By having these structures, the polarity of the solvent component (SF) molecule is increased, and as a result, the ability to dissolve salts can be further improved. As the ring structure, a five-membered carbon ring is particularly preferable.

[0025] Specific examples of the solvent component (SF) include a compound having a structure in which one or more hydrogen atoms in a cyclic or chain-like hydrocarbon molecule are replaced with a fluorine atom, a compound having a structure in which one or more hydrogen atoms in a cyclic or chain-like molecule consisting of carbon atoms, hydrogen atoms, and oxygen atoms are replaced with a fluorine atom, and a substituent-containing compound having a structure in which a substituent is further added to the above-mentioned compound. However, in the present application, the solvent component and other substances constituting the electrolyte are not limited by the manufacturing process.

[0026] Preferred examples of cyclic hydrocarbon molecules include cyclopentane, cyclohexane, and cyclopentene. Preferred examples of cyclic molecules consisting of carbon, hydrogen, and oxygen atoms include tetrahydrofuran and tetrahydropyran. Chain hydrocarbon molecules can be linear or branched. Preferred examples of chain molecules consisting of carbon, hydrogen, and oxygen atoms include ethers such as diethyl ether and ethyl propyl ether. Examples of the substituent in the substituent-containing compound include halogen atoms other than fluorine atoms, alkyl groups, fluorinated alkyl groups, ether groups, ester groups, alkoxy groups, and hydroxyl groups.

[0027] More specific preferred examples of the solvent component (SF) include 1,1,2,2,3,3,4-heptafluorocyclopentane (HFCP), 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether (trade name "ASAHIKLIN AE-3000", manufactured by AGC Corporation) (HFE1), 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether (HFE2), bis(2,2,2-trifluoroethyl)ether (HFE3), and 3,3,4,4,5,5-hexafluorocyclopentene (P-C1).

[0028] From the viewpoint of heat generation of the electrochemical device and storage and use in a high-temperature environment, it is preferable that the lower limit of the boiling point of the solvent component (SF) is set to a certain degree or higher. Specifically, the boiling point of the solvent component (SF) is preferably 60° C. or higher, more preferably 70° C. or higher, and even more preferably 80° C. or higher.

[0029] The solvent component (SF) can be a mixture of a substance with a high boiling point and a substance with a low boiling point. In that case, from the above viewpoint, it is preferable that the proportion of the substance with a low boiling point is small. Specifically, it is preferable that the proportion of the solvent component (SF) with a boiling point of 50° C. or less is 50% by weight or less in 100% by weight of the entire solvent component (SF), more preferably the proportion of the solvent component (SF) with a boiling point of 60° C. or less is 50% by weight or less, and even more preferably the proportion of the solvent component (SF) with a boiling point of 70° C. or less is 50% by weight or less.

[0030] On the other hand, from the viewpoint of enabling the configuration of a mechanism for opening the sealing by the exterior and stopping the operation when an abnormality occurs during the operation of the electrochemical device and the pressure inside the exterior rises to or exceeds a specific threshold, and from the viewpoint of suppressing the occurrence of melting and large deformation of device components such as the separator and sealant when the operation is stopped in this way, it is preferable that the upper limit of the boiling point of the solvent component (SF) is a temperature that is lower than a certain level. Specifically, the boiling point of the solvent component (SF) is preferably 170°C or lower, more preferably 160°C or lower, and even more preferably 150°C or lower.

[0031] In addition, from the viewpoint of reducing the proportion of flammable vapor and increasing the proportion of non-flammable vapor in the vapor that is released when the seal is opened, the boiling point of the solvent component (SF) is preferably lower than that of the solvent component (SR80A). From this viewpoint, the boiling point of the solvent component (SF) is preferably 150°C or lower, more preferably 120°C or lower, and even more preferably 90°C or lower.

[0032] The dielectric constant of the solvent component (SF) is preferably a large value. The dielectric constant (measurement frequency 1 kHz) is preferably 6 or more, more preferably 8 or more, and even more preferably 10 or more. A solvent component (SF) having a high dielectric constant has excellent miscibility with other solvent components and can be compatible under a wide range of conditions. The upper limit of the dielectric constant is not particularly limited, but can be, for example, 50 or less.

[0033] The electrolyte of the present invention contains a solvent component (SF) at a large ratio equal to or greater than a specific value. In the present application, the weight percentage of the solvent component (SF) in 100% by weight of the electrolyte may be abbreviated as "(SF)%". (SF)% is 15% by weight or more, preferably 17% by weight or more, and more preferably 30% by weight or more. The upper limit of the ratio of the solvent component is not particularly limited, but may be, for example, 50% by weight or less. By making (SF)% 15% by weight or more, the flash point of the electrolyte can be increased and flammability can be reduced. Furthermore, by making the ratio of the solvent component (SF) a large value, such as 30% by weight or more, the electrolyte as a whole can be made non-hazardous.

[0034] In addition, the ratio of the solvent component (SF) in the entire solvent is preferably 15% by weight or more, more preferably 20% by weight or more, and on the other hand, preferably 90% by weight or less, more preferably 60% by weight or less. By having the ratio of the solvent component (SF) in the solvent be equal to or more than the lower limit, the flammability of the electrolyte can be weakened, and the safety of the electrolyte can be increased. On the other hand, by having the ratio of the solvent component (SF) in the solvent be equal to or less than the upper limit, it is possible to achieve both weak flammability, good compatibility, and high ionic conductivity at low temperatures.

[0035] (Remaining Solvent Component (SR)) The solvent component (SR) is a component of the solvent other than the non-flammable fluorine solvent component (SF). The solvent component (SR) includes a solvent component (SR80) with a flash point of over 80°C. The solvent component (SR80) includes a solvent component (SR80A).

[0036] In this application, for convenience of explanation, the solvent components (SR) other than the solvent component (SR80) are referred to as the solvent component (SRL). Also, the solvent components (SR80) other than the solvent component (SR80A) are referred to as the solvent component (SR80R).

[0037] (Solvent component (SR80A)) The solvent component (SR80A) is one or more compounds that do not have a carbon-carbon unsaturated bond and are selected from the group consisting of the following compounds (i) to (ix) and mixtures thereof. The "number of carbon atoms" in the description of the structure of a molecule or group means the number of carbon atoms per molecule or per group. The same applies to the expression of the numbers of atoms other than carbon and substituents, etc. Compound (i): Cyclic carbonate ester having 4 or more carbon atoms Compound (ii): Fluoroethylene carbonate Compound (iii): A cyclic compound having 4 or more carbon atoms and having one or more ester bonds in the molecule. Compound (iv): Dinitrile having 3 or more carbon atoms Compound (v): Sulfone having 2 or more carbon atoms Compound (vi): Oxazolidone derivative having 4 or more carbon atoms Compound (vii): Imidazolidinone derivative having 5 or more carbon atoms Compound (viii): Carbonic acid ester having 9 or more carbon atoms Compound (ix): Lactam derivative having 5 or more carbon atoms

[0038] Compound (i) (cyclic carbonate having 4 or more carbon atoms) is a compound having 4 or more carbon atoms and having a structure represented by the following formula (i): The upper limit of the carbon number of compound (i) is preferably 15 or less, more preferably 10 or less, and even more preferably 6 or less.

[0039] [ka] In formula (i), R 1 is a group having 3 or more carbon atoms. 1 is preferably a hydrocarbon group having 3 to 5 carbon atoms, more preferably -(CH2)n1- (n1 is an integer of 3 to 5). Specific examples of compound (i) include propylene carbonate (n1 = 3) and butylene carbonate (n1 = 4).

[0040] Compound (ii) (fluoroethylene carbonate) has a structure in which one of the hydrogen atoms of ethylene carbonate is substituted with fluorine.

[0041] Examples of compound (iii) (a cyclic compound having 4 or more carbon atoms and one or more ester bonds in the molecule) include lactones having 4 or more carbon atoms and cyclic compounds having two ester bonds in the molecule having 4 or more carbon atoms. The upper limit of the carbon number of compound (iii) is preferably 15 or less, more preferably 10 or less, and even more preferably 6 or less. Lactones having 4 or more carbon atoms are compounds having 4 or more carbon atoms and having a structure represented by the following formula (iii).

[0042] [ka]

[0043] In formula (iii), R 2 is a group having 3 or more carbon atoms. 2 is preferably a hydrocarbon group having 3 to 5 carbon atoms, more preferably -(CH2)n2- (n2 is an integer of 3 to 5). Specific examples of compound (iii) include γ-butyrolactone (n2=3) and δ-valerolactone (n2=4). On the other hand, examples of compound (iii) having two ester bonds in the molecule include glycolide and lactide.

[0044] Examples of compound (iv) (dinitrile having 3 or more carbon atoms) include compounds represented by the formula NC-R3 The upper limit of the number of carbon atoms in compound (iv) is preferably 10 or less, more preferably 8 or less. 3 is a group having 1 or more carbon atoms, more preferably a hydrocarbon group having 1 to 6 carbon atoms, or a group having an ether structure in which an oxygen atom is present in the chain of a hydrocarbon group having 1 to 6 carbon atoms. Specific examples of compound (iv) include malononitrile, succinonitrile, glutaronitrile, adiponitrile, and 3,3'-oxydipropionitrile.

[0045] The upper limit of the carbon number of the compound (v) (sulfone having 2 or more carbon atoms) can be preferably 10 or less, more preferably 7 or less. Examples of the compound (v) include those represented by the formula: 4 -SO2-R 5 Examples of compounds having a structure represented by R 4 and R 5 is a hydrogen atom or a group having 1 or more carbon atoms, preferably a group having 1 or more carbon atoms, R 4 The number of carbon atoms and R 5 The total number of carbon atoms in R is 2 or more. 4 and R 5 may be bonded to form a ring. 4 The number of carbon atoms and R 5 The total number of carbon atoms (R 4 and R 5 When they are bonded to form a ring, R 4 and R 5 The number of carbon atoms in the portion formed by bonding is preferably 7 or less, and more preferably 5 or less. Specific examples of compound (v) include dimethyl sulfone, ethyl methyl sulfone, diethyl sulfone, and sulfolane.

[0046] Compound (vi) (oxazolidone derivative having 4 or more carbon atoms) is a compound having 4 or more carbon atoms, which has a structure in which hydrogen atoms bonded to carbon atoms or nitrogen atoms of 2-oxazolidone are substituted with one or more substituents. The upper limit of the carbon number of compound (vi) can be 15 or less. Such a substituent can be a hydrocarbon group having 1 to 6 carbon atoms. A specific example of compound (vi) is N-methyl-2-oxazolidone.

[0047] Compound (vii) (imidazolidinone derivative having 5 or more carbon atoms) is a compound having 5 or more carbon atoms, which has a structure in which hydrogen atoms bonded to carbon atoms or nitrogen atoms of 2-imidazolidinone are substituted with one or more substituents. The upper limit of the carbon number of compound (vii) can be preferably 15 or less, more preferably 10 or less, and even more preferably 6 or less. Such a substituent can be a hydrocarbon group having 1 to 6 carbon atoms, preferably 1 to 3 carbon atoms. A specific example of compound (vii) is N,N-dimethyl-2-imidazolidinone.

[0048] The upper limit of the carbon number of the compound (viii) (carbonic acid ester having 9 or more carbon atoms) can be preferably 20 or less, more preferably 16 or less. Examples of the compound (viii) include those represented by the formula: 6 -OC(=O)OR 7 Examples of compounds having a structure represented by R 6 and R 7 is a hydrogen atom or a group having 1 or more carbon atoms, preferably a group having 1 or more carbon atoms, R 6 The number of carbon atoms and R 7 The total number of carbon atoms in R is 8 or more. 6 and R 7 may be bonded to form a ring. 6 The number of carbon atoms and R 7 The total number of carbon atoms (R 6 and R 7 When they are bonded to form a ring, R 6 and R 7 The number of carbon atoms in the portion formed by bonding is preferably 20 or less, and more preferably 15 or less. A specific example of compound (viii) is dibutyl carbonate.

[0049] Compound (ix) (lactam derivative having 5 or more carbon atoms) is a compound having 5 or more carbon atoms, which has a structure in which hydrogen atoms bonded to carbon atoms or nitrogen atoms of lactam are substituted with one or more substituents. The upper limit of the carbon number of compound (ix) is preferably 15 or less, more preferably 10 or less. Such a substituent may be a hydrocarbon group having 1 to 6 carbon atoms. A specific example of compound (ix) is N-methyl-2-pyrrolidone.

[0050] By including the solvent component (SR80A) in the electrolyte, the ionic conductivity of the electrolyte is increased, and the performance of driving an electrochemical device is improved. In addition, by including the solvent component (SR80A) in the electrolyte, the temperature range in which the electrolyte is in a liquid state is expanded. In addition, by including the solvent component (SR80A) in the electrolyte, the solvent component (SR80A) and other components of the electrolyte are well compatible with each other.

[0051] The solvent component (SR80A) is preferably one that can dissolve the salt, which is a component of the electrolyte, well by itself. Specifically, the solvent component (SR80A) is preferably one that can dissolve 1M or more of the salt.

[0052] In the present application, for convenience of description, the weight percentage of the solvent component (SR80) in 100% by weight of the solvent component (SR) may be abbreviated as "(SR80) / (SR)%", and the weight percentage of the solvent component (SR80A) in 100% by weight of the solvent component (SR) may be abbreviated as "(SR80A) / (SR)%". (SR80) / (SR)% is 90% by weight or more, preferably 95% by weight or more, and the upper limit may be 100% by weight. (SR80A) / (SR)% is 20% by weight or more, preferably 30% by weight or more, and the upper limit may be 100% by weight. By making (SR80) / (SR)% and (SR80A) / (SR)% equal to or more than the lower limit, the flammability of the electrolyte can be reduced, the safety of the electrolyte can be increased, and high ionic conductivity can be exhibited even at low temperatures.

[0053] The ratio of the solvent component (SR) in the entire solvent is preferably 10% by weight or more, more preferably 40% by weight or more, and is preferably 85% by weight or less, more preferably 80% by weight or less. By making the ratio of the solvent component (SR) in the solvent equal to or less than the upper limit, the flammability of the electrolyte can be reduced, and the safety of the electrolyte can be improved. On the other hand, by making the ratio of the solvent component (SR) in the solvent equal to or more than the lower limit, it is possible to achieve both low flammability, good compatibility, and high ionic conductivity at low temperatures.

[0054] (Solvent composition (SR80R)) The solvent of the electrolytic solution of the present invention may contain only the solvent component (SR80A) as the solvent component (SR80), but may also contain the other component, the solvent component (SR80R). That is, the solvent component (SR80R) is a solvent component (SR80) that has a flash point of over 80°C and is other than the solvent component (SR80A) among the solvent components (SR) that are components other than the non-flammable fluorine solvent component (SF).

[0055] As the solvent component (SR80R), a substance known to be usable as a solvent component of an electrolyte other than the non-flammable fluorine solvent component (SF) can be appropriately selected and used. Examples of the solvent component (SR80R) include ethylene carbonate, vinylene carbonate (VC), and 1,3-propane sultone (PS).

[0056] Other examples of the solvent component (SR80R) include the following flame-retardant solvent component (R): That is, the flame-retardant solvent component (R) is one or more selected from the group consisting of a phosphate ester or phosphite ester compound (R1) having 1 to 6 carbon atoms per molecule, a compound (R2) in which hydrogen of the compound (R1) is partially fluorinated, and a compound (R3) having a phosphazene ring.

[0057] Specific examples of the compound (R1) include trimethyl phosphate, triethyl phosphate, tributyl phosphate, and trisbutoxyethyl phosphate, as well as the corresponding phosphites. Examples of the compound (R3) include products manufactured by Nippon Chemical Industry under the trade names "Hishicolin-E", "Hishicolin-O", and "Hishicolin-D". The proportion of the flame-retardant solvent component (R) in 100% by weight of the solvent is preferably 1% by weight or more, more preferably 5% by weight or more, and is preferably 25% by weight or less, more preferably 20% by weight or less. By setting the proportion of the flame-retardant solvent component (R) to the lower limit or more, the flame retardancy of the non-aqueous electrolyte can be increased, and the safety of the electrochemical device can be improved. On the other hand, by setting the proportion of the flame-retardant solvent component (R) to the upper limit or less, an increase in the resistance of the device can be avoided.

[0058] Further, examples of the solvent component (SR80R) other than those mentioned above include those substances which correspond to the solvent component (SR80R) among the substances given as specific examples of the additive (B) (described later).

[0059] Among the substances used as the solvent component (SR80R), ethylene carbonate has a high flash point, good compatibility with the carbonaceous material negative electrode, and high charge / discharge efficiency, but low-temperature performance is poor. However, when used in combination with the solvent components (SF) and (SR80A) in the electrolyte of the present invention, it is particularly preferable because it is possible to enjoy the advantages of ethylene carbonate while improving low-temperature performance.

[0060] (Solvent composition (SRL)) The solvent may contain only the solvent component (SR80), but may also contain other solvent components (SRL). That is, the solvent components (SRL) are those solvent components (SR) other than the non-flammable fluorine solvent component (SF) that have a flash point of 80°C or less. However, from the viewpoint of reducing the flammability of the electrolyte, it is preferable that the ratio of the solvent component (SRL) in the solvent is small, and it is more preferable that the solvent does not contain the solvent component (SRL). An example of the solvent component (SRL) is ethyl methyl carbonate (EMC).

[0061] (Additive (B)) In an embodiment, the solvent may contain additive (B) as solvent component (SF), solvent component (SR) (solvent component (SR80A), solvent component (SR80R) or solvent component (SRL)). Additive (B) may be one or more selected from the group consisting of cyclic sulfate ester compounds (B1), vinyl ethylene carbonate compounds (B2), and fluorine compounds having an unsaturated bond (B3).

[0062] Examples of the cyclic sulfate compound (B1) include 1,3,2-dioxathiolane 2,2-dioxide (ethylene sulfate), 4-methyl-1,3,2-dioxathiolane 2,2-dioxide, and 1,3,2-dioxathiane 2,2-dioxide.

[0063] Examples of the vinyl ethylene carbonate compound (B2) include 3-vinyl ethylene carbonate, and compounds having a vinyl ethylene carbonate skeleton, such as 3,4-divinyl ethylene carbonate and 3-ethynyl ethylene carbonate.

[0064] Examples of the fluorine compound (B3) having an unsaturated bond include cyclic fluorine compounds such as 3,3,4,4,5,5-hexafluorocyclopentene and 1-methoxy-2,3,3,4,4,5,5-heptafluorocyclopentene.

[0065] The additive (B) can be used as a so-called negative electrode protectant. The solvent contains the additive (B), which improves the charge / discharge efficiency and suppresses deterioration due to charge / discharge cycles. Vinylene carbonate is well known as a negative electrode protectant, but the inventors have found that vinylene carbonate is less effective in electrolytes that are not mainly made of chain carbonate. On the other hand, the additive (B) described above can be used in combination with a non-flammable fluorine solvent component (SF) to obtain a high effect as a negative electrode protectant. When the solvent contains additive (B), it is preferable to use vinylene carbonates, sultones, acetylene group-containing compounds, vinyl group-containing compounds, fluorinated carbonates, fluorinated anisoles, acid anhydrides, benzenesulfonic acid group-containing compounds, fluorinated cyclic carbonates, amines, fluorinated benzene, phenylcyclohexane, spirodilactone, or combinations thereof as the solvent components used in combination with it. In particular, it is preferable to use sultones such as 1,3-propane sultone. From the viewpoint of suppressing excessive resistance, the ratio of these to 100% by weight of the solvent is preferably 10% by weight or less, more preferably 8% by weight or less, and even more preferably 7% by weight or less. In addition, the lower limit of the amount added is preferably 0.1% by weight or more.

[0066] The additive (B) may be a part of the solvent component (SF) or may be a part of the solvent component (SR) (solvent component (SR80A), solvent component (SR80R) or solvent component (SRL)). For example, the cyclic sulfate ester compound (B1) and the vinyl ethylene carbonate compound (B2) are solvent components (SR80R), and among the cyclic fluorine compounds (B3) having an unsaturated bond, 3,3,4,4,5,5-hexafluorocyclopentene is non-flammable and is solvent component (SF), and 1-methoxy-2,3,3,4,4,5,5-heptafluorocyclopentene has a flash point of over 80°C and is solvent component SR80R.

[0067] In order to effectively obtain the above-mentioned effects, the amount of additive (B) added is preferably 0.01% by weight or more, more preferably 0.5% by weight or more, based on 100% by weight of the electrolytic solution, and is preferably 10% by weight or less, more preferably 7% by weight or less.

[0068] (Properties of the electrolyte) The electrolyte of the present invention preferably exhibits a property in which the salt is uniformly dissolved without phase separation as a whole at 25°C. By having such a property, the electrolyte can exhibit good performance as an electrolyte, such as a high ability to maintain a liquid state, sufficient ionic conductivity at low temperatures, good permeability, and high charge / discharge efficiency. The presence or absence of phase separation refers to the fact that the electrolyte is visually observed at 25°C and neither the presence of solid substances nor separation of liquid phases is observed. Such an electrolyte can be obtained by appropriately adjusting the types and ratios of salt and solvent within the above-mentioned ranges.

[0069] The electrolyte of the present invention preferably has a flash point of more than 80° C. Such a high flash point can enhance the safety of an electrochemical device containing the electrolyte. An electrolyte having a flash point of more than 80° C. can be obtained by appropriately selecting a non-flammable or low-flammable solvent component from the components exemplified above.

[0070] (Electrolyte Solution Manufacturing Method) The method for producing the electrolyte solution of the present invention is not particularly limited, and the electrolyte solution can be produced by mixing the above-mentioned components in an appropriate environment suitable for producing the electrolyte solution.

[0071] (Electrolyte application: electrochemical devices) The electrochemical device of the present invention is an electrochemical device comprising a positive electrode, a negative electrode and an electrolyte, the electrolyte containing the electrolyte of the present invention described above, and the negative electrode containing a carbon material. The electrochemical device of the present invention contains the electrolyte of the present invention as the electrolyte, and uses the electrolyte in combination with an electrode containing a carbon material, in particular, and can enjoy advantages such as a high capacity retention rate, high operating performance at low temperatures, and high safety.

[0072] The electrochemical device of the present invention may include a device exterior and contents, such as a carbon material-containing electrode and the electrolyte solution of the present invention, enclosed in a sealed space inside the device exterior. The device may further include optional components, such as an electrode other than the carbon material-containing electrode and a separator, as necessary. The carbon material-containing electrode may be a negative electrode containing graphite as the carbon material. Such a negative electrode generally has poor compatibility with electrolytes having a high flash point and easy-to-handle properties, and tends to have low charge / discharge efficiency. However, in combination with the electrolyte of the present invention, the decrease in charge / discharge efficiency is suppressed, and the negative electrode can be used particularly well. In addition, silicon, silicon oxide, aluminum, lithium titanate, titanium niobium composite oxide, etc. can be suitably used as a negative electrode material that has a relatively high charge / discharge potential compared to carbon materials and is therefore less likely to reduce and decompose the electrolyte. The electrodes other than the carbon material-containing electrode and the separator are not particularly limited, and known electrodes suited to the application of the device can be appropriately used.

[0073] The material constituting the device exterior is not particularly limited, and may be appropriately selected from known materials used as exteriors for devices such as batteries. In particular, among the materials constituting the device exterior, the innermost layer portion that comes into contact with the electrolyte is preferably a resin material selected from the group consisting of polyolefins, fluororesins, and rubbers. By using such a material as the innermost layer, it is possible to suppress the vaporized solvent component from penetrating the exterior and volatilizing.

[0074] Since the electrolyte of the present invention can be made to have a low risk of leaking out of the device for some reason, the electrochemical device of the present invention can have a mechanism for opening the sealing by the exterior when an abnormality occurs during operation, the temperature inside the exterior rises, and the pressure rises to a specific threshold value or more due to evaporation of the electrolyte, thereby making it possible to detect the occurrence of an abnormality from outside the device and to stop operation when an abnormality occurs. Such a threshold value can be 2 atm to 10 atm. Examples of the mechanism for opening the seal include a pressure vent that opens the seal at a predetermined pressure, and a heat seal portion.

[0075] Specific examples of the electrochemical device of the present invention include various non-aqueous primary batteries, secondary batteries, electric double layer capacitors, electric double layer transistors, electrochromic display materials, electrochemical light emitting devices, electrochemical actuators, and dye-sensitized solar cells. Examples of batteries include lithium primary batteries, lithium ion secondary batteries, lithium metal secondary batteries, sodium ion batteries, potassium ion batteries, magnesium ion batteries, aluminum ion batteries, fluoride ion batteries, and air batteries. The battery is particularly preferably a lithium ion primary battery or a lithium ion secondary battery. In a preferred example, the electrochemical device of the present invention is a battery, and even if it is a large-capacity lithium ion secondary battery, it can smoothly generate an electrochemical reaction and can achieve both safety and large capacity. Specifically, the electrochemical device of the present invention is preferably a battery having a storage capacity of 3 Ah or more.

[0076] The electrochemical device of the present invention may be manufactured by any manufacturing method. In general, the electrochemical device may be manufactured by arranging components such as electrodes and separators inside the exterior, injecting an electrolyte into the interior of the exterior, and sealing the exterior. The method for manufacturing the electrochemical device of the present invention may be such a general method, but is not limited to this. For example, the components are sealed in a state in which electrolytes of different compositions are separately present inside the device, such as by making each component of the electrolyte partly solid, and then dissolving and mixing the solid inside the device, etc., to mix electrolytes of different compositions inside the electrochemical device to form an electrolyte, thereby completing the device. EXAMPLES

[0077] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be modified and carried out as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto.

[0078] In the following description, the units "%" and "parts" that represent amounts are by weight unless otherwise specified. Furthermore, the operations described below were carried out under room temperature and normal pressure conditions unless otherwise specified.

[0079] In the following Examples and Comparative Examples, in the test of the permeability of the electrolyte solution to the separator, when comparing the Examples and Comparative Examples, a PTFE (polytetrafluoroethylene) membrane filter (Omnipore JMWP04700, manufactured by Merck) or paper (TF4535, manufactured by Nippon Kodo Paper Industries) was used. This is because, when a preliminary experiment was performed using a polyolefin separator with lower permeability, it was found that the electrolyte solution of the present invention could permeate while the electrolyte solution of the Comparative Example could not permeate, and therefore, when comparing the two, it was found that it was necessary to use a separator that exhibited a degree of permeability that allowed comparison.

[0080] The meanings of the abbreviations used below are as follows: HFCP: 1,1,2,2,3,3,4-heptafluorocyclopentane P-C1: 3,3,4,4,5,5-hexafluorocyclopentene P-C2: 1-Methoxy-2,3,3,4,4,5,5-heptafluorocyclopentene HFE1: 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether (product name "ASAHIKLIN AE-3000", manufactured by AGC Corporation) HFE2: 1,1,2,2-Tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether HFE3: Bis(2,2,2-trifluoroethyl) ether DMC: Dimethyl carbonate DEC: Diethyl carbonate PC: Propylene carbonate EC: Ethylene carbonate LiFSI: Lithium bisfluorosulfonyl imide (Li + (FSO2)2N - ) LiTFSI: Lithium bistrifluoromethanesulfonylimide (Li + (CF3SO2)2N - ) LiBF4: Lithium tetrafluoroborate TEABF4: Tetraethylammonium tetrafluoroborate LiPF6: Lithium hexafluorophosphate DMS: dimethyl sulfone FEC: Fluoroethylene carbonate SN: Succinonitrile SL: Sulfolane GBL: gamma-butyrolactone VEC: Vinyl ethylene carbonate DTD: 1,3,2-dioxathiolane 2,2-dioxide (ethylene sulfate) MDTD: 4-Methyl-1,3,2-dioxathiolane 2,2-dioxide PCS: 1,3,2-dioxathiane 2,2-dioxide VC: Vinylene carbonate PS: 1,3-propane sultone EMC: Ethyl methyl carbonate

[0081] (Reference example) Using aluminum laminate packaging, which is commonly used as the exterior packaging for electrochemical devices, the degree to which each of the solvent substances escapes to the outside of the packaging was evaluated.

[0082] A 10cm x 20cm rectangular aluminum laminate packaging material was folded in half and two of the three open sides were heat sealed to form a 10cm x 10cm container. 500mg of each of the solvent substances shown in Table 1 was weighed and poured into the container, and the remaining side was heat sealed to completely seal the container, forming a test specimen. The test specimen was weighed and left in an atmosphere-circulating oven set at 60°C, and after 60 days it was weighed again to determine the change in weight.

[0083] Relatively large weight losses were observed for dimethyl carbonate (DMC) and diethyl carbonate (DEC), which are common electrolyte solvents, and it became clear that these solvent substances are likely to dissipate outside the packaging during device use. Such dissipation can lead to undesirable phenomena, such as changes in the electrolyte composition and exposure of device users to the electrolyte. No correlation was found between the amount of dissipation and the boiling point. From this, it is believed that the amount of dissipation increases or decreases depending on the degree of affinity between the polyethylene, which is the material of the heat-sealed part of the packaging material, and the solvent substance.

[0084] [Table 1]

[0085] *1: Because the test environment exceeded the boiling point of the solvent substance, the test specimen expanded, but no leakage of the solvent substance was observed.

[0086] (Example 1 and Comparative Example 1) The components were mixed according to the compositions shown in Tables 2 and 3 below to prepare electrolyte solutions (1-01) to (1-14) of the examples and electrolyte solutions (C1-01) to (C1-02) of the comparative examples. The ionic conductivity of each electrolyte solution at 0°C was measured. The ionic conductivity was measured by an AC impedance method. Furthermore, the properties of each electrolyte solution at 25°C were visually observed with the naked eye. The results are shown in Tables 2 and 3.

[0087] [Table 2]

[0088] [Table 3]

[0089] In Table 2 and subsequent tables, the unit of salt concentration (mol / kg) is the ratio (mol) of salt to the total amount of electrolyte (kg). "(SF) %" is the weight % of the solvent component (SF) in 100 weight % of the electrolyte. "(SR80) / (SR)%" is the weight percentage of the solvent component (SR80) in a remaining solvent component (SR) of 100% by weight. "(SR80A) / (SR)%" is the weight percentage of the Group A solvent component (SR80A) in 100% by weight of the remaining solvent component (SR).

[0090] (Example 2 and Comparative Example 2) (2-1. Preparation of electrolyte) The components were mixed according to the compositions shown in Table 4 below to prepare electrolytic solutions (2-01) to (2-04) of the examples and electrolytic solutions (C2-01) to (C2-04) of the comparative examples.

[0091] (2-2. Flash point measurement) The flash point of the electrolyte prepared in (2-1) was measured by the flash point measurement method according to the tag closed method (JIS K2265-1 (2007)) and the Cleveland open method (JIS K2265-4 (2007)). The results are shown in Table 4.

[0092] When the proportion of fluorine solvent component (SF) in the electrolyte was 15% by weight or more, a flash point higher than the flash point of PC (132°C) was obtained, and when it exceeded 25% by weight, the flash point disappeared. However, when 7.13% by weight was added, the flash point tended to decrease. From this, it was found that in order to keep flammability low, it is essential that the proportion of fluorine solvent component (SF) be 15% by weight or more. It was also found that the addition of EMC, a low-flash point solvent, lowers the flash point. It was also found that the proportion of the solvent component (SR80) with a flash point of over 80°C in the remaining solvent component (SR) must be 90% by weight or more, and preferably 92% by weight or more.

[0093] [Table 4]

[0094] (Example 3, Comparative Example 3 and Reference Example 1) An electrolyte solution containing the additive (B) as a solvent component and an electrolyte solution containing other components were prepared, and the effect of improving the charge / discharge efficiency of the negative electrode by these electrolyte solutions was evaluated.

[0095] A copper foil with a thickness of 10 μm was prepared as the substrate. A layer containing graphite, CMC (carboxymethyl cellulose) and SBR (styrene-butadiene rubber) binder in weight ratios of 97, 1 and 2%, respectively, was provided on the substrate, and the layer was pressed to form a negative electrode mixture layer, thereby preparing a negative electrode for a lithium ion battery consisting of the substrate and the negative electrode mixture layer. The weight of the negative electrode mixture layer was 12 mg / cm. 2 , density is 1.5g / cm 3 This negative electrode was cut into a piece measuring 3 x 4 cm to prepare a test electrode.

[0096] A 200 μm thick lithium metal layer was laminated on a 10 μm thick copper foil to prepare a counter electrode. Nickel tabs were attached to the ends of the test electrode and the counter electrode by ultrasonic welding. A 100 μm thick PTFE membrane filter (Merck, Omnipore JMWP04700) was placed as a separator between the pair of tabbed test electrode and counter electrode to obtain a laminate having a layer structure of (substrate) / (negative electrode composite layer) / (separator) / (lithium metal) / (substrate). The laminate was placed inside an aluminum laminate exterior.

[0097] 0.8 mol / kg LiBF4 as an ionic substance was mixed with the components shown in Tables 5 and 6 to prepare electrolyte solutions (3-01) to (3-11) of the examples, electrolyte solution (C3-01) of the comparative example, and electrolyte solutions (R1-01) to (R1-11) of the reference examples. All of the obtained electrolyte solutions were in a uniform liquid state at 25°C. 600 μl of each of the electrolyte solutions was injected into the aluminum laminate exterior with a micropipette and sealed by heat sealing. This resulted in a test cell for evaluating the compatibility with lithium ion negative electrodes.

[0098] The obtained test cell was charged and discharged at 25° C. at a current value of 0.1 C to determine the initial charge-discharge efficiency (initial coulombic efficiency). The current value was calculated assuming that the discharge capacity of graphite was 360 mAh / g. The negative electrode worked with all of the electrolytes of the present invention. The one with the addition of VC, the most well-known additive for negative electrodes, had a low effect, resulting in the lowest efficiency of the ones tested. The next most effective was the one with the addition of general PS. In contrast, it was found that high efficiency could be obtained with electrolytes with the addition of any of VEC, DTD, MDTD, PCS, and unsaturated cyclic fluorine compounds. In particular, high efficiency was obtained when the electrolyte contained 15% by weight or more of the fluorine solvent component (SF).

[0099] [Table 5]

[0100] [Table 6]

[0101] The numerical values ​​for each component (HFCP, EC, DMS, PC, DTD, MDTD, PCS, VEC, P-C1, P-C2, VC, and PS) in the tables indicate the amount added (unit: parts by weight). In the examples in Tables 5 and 6, (SR80) / (SR)% is always 100%.

[0102] Example 4 0.8 mol / kg of LiPF6 as an ionic substance was mixed with the components shown in Table 7 to prepare the electrolyte solutions (4-01) to (4-03) of the examples. Test cells were obtained in the same manner as in Example 3, except that the electrolyte solutions (4-01) to (4-03) were used instead of those used in Example 3. The test cells were charged and discharged at a current value of 0.1 C at 25° C., and the initial charge / discharge capacity was determined. The results are shown in Table 7. Example 4-02, in which VEC, which is the additive (B), and PS were used in combination, showed a result in which the initial discharge capacity was increased compared to the examples in which only one of them was used.

[0103] [Table 7]

[0104] The numerical values ​​for each component in the table indicate the amount added (unit: parts by weight).

[0105] (Example 5 and Comparative Example 5) An aluminum foil with a thickness of 20 μm was prepared as a substrate. A layer containing lithium cobalt oxide, acetylene black, and a PVDF (polyvinylidene fluoride) binder in weight ratios of 94%, 3%, and 3%, respectively, was provided on the aluminum foil substrate, and the layer was pressed to form a composite layer, thereby preparing a lithium ion positive electrode consisting of the substrate layer and the composite layer. The weight of the composite layer was 22 mg / cm. 2 , density is 3.0g / cm 3 It was.

[0106] On the other hand, a copper foil having a thickness of 10 μm was prepared as a substrate. A layer containing graphite (manufactured by Hitachi Chemical Co., Ltd., product name "MAG-E"), acetylene black, SBR binder and CMC in weight ratios of 97%, 0.5%, 1% and 1.5%, respectively, was provided on the copper foil substrate, and the layer was pressed to form a composite layer, thereby preparing a lithium ion negative electrode consisting of the substrate layer and the composite layer. The weight of the composite layer was 11 mg / cm. 2 , density is 1.4g / cm 3 It was.

[0107] A 100 μm thick PTFE (polytetrafluoroethylene) membrane filter (manufactured by Merck, product name "Omnipore JMWP04700") was prepared as a separator. Tabs were attached to the ends of the lithium ion positive electrode and negative electrode by ultrasonic welding. The tab for the positive electrode was made of aluminum, and the tab for the negative electrode was made of nickel. One separator was placed between the lithium ion positive electrode and negative electrode to obtain a laminate having a layer structure of (positive electrode current collector) / (positive electrode composite layer) / (separator) / (negative electrode composite layer) / (negative electrode current collector). The laminate was placed inside an aluminum laminate exterior.

[0108] 1.0 mol / kg of LiFSI as a salt was mixed with the components shown in Table 8 to prepare the electrolyte solutions (5-01) to (5-03) of the examples and the electrolyte solutions (C5-01) to (C5-02) of the comparative examples. When the properties of the obtained electrolyte solutions at 25°C were observed with the naked eye, all of them were homogeneous solutions. Each of the electrolyte solutions was injected into an aluminum laminate exterior and the exterior was sealed. This resulted in the construction of a fairly standard lithium ion battery.

[0109] The obtained lithium ion battery was charged and discharged. Charge and discharge were repeatedly performed between 4.2 V and 3.0 V at a current value of 0.6 C at 25°C. The current value was calculated assuming the discharge capacity of lithium cobalt oxide to be 145 mAh / g. The percentage of the ratio of the discharge capacity at the 200th cycle to the discharge capacity at the 1st cycle was calculated as the capacity retention rate.

[0110] It was found that the lithium ion battery using the electrolyte solution of the examples was capable of charging and discharging regardless of the content of the fluorine solvent, and showed a better cycle capacity retention rate than the electrolyte solution not containing a fluorine solvent.

[0111] [Table 8]

[0112] The numerical values ​​for each component in the table indicate the amount added (unit: parts by weight). NA: The initial charge was not completed and measurement was discontinued.

[0113] Example 6 An electrolyte solution (6-01) of the example was prepared by mixing 1.1 mol / kg of LiFSI as a salt with the components shown in Table 9. When the properties of the obtained electrolyte solution at 25° C. were observed with the naked eye, it was found to be a homogeneous solution. A test cell was obtained in the same manner as in Example 3, except that this electrolyte (6-01) was used instead of the electrolyte used in Example 3, and the initial charge-discharge efficiency (initial coulombic efficiency) was determined.

[0114] Furthermore, the capacity retention rate was measured in the same manner as in Example 5, except that this electrolyte (6-01) was used instead of that used in Example 5 and the cycle was changed to 100 cycles. The results are shown in Table 9.

[0115] [Table 9]

[0116] The numerical values ​​for each component in the table indicate the amount added (unit: parts by weight). It can be seen that when FEC is used as the main component of the electrolyte, high charge / discharge efficiency can be obtained even without using the additive (B).

[0117] (Example 7 and Comparative Example 7) (7-1. Manufacturing of large capacity batteries) A 20 μm thick aluminum foil was prepared as a positive electrode current collector. On both sides of the positive electrode current collector, layers containing lithium nickel manganese cobalt oxide (Ni:Mn:Co=8:1:1, molar ratio), acetylene black, and PVDF (polyvinylidene fluoride) binder were provided at weight ratios of 94%, 3%, and 3%, respectively, and the layers were pressed to form a positive electrode composite layer, thereby preparing a lithium ion positive electrode consisting of the positive electrode current collector and the positive electrode composite layer. The basis weight of one side of the positive electrode composite layer was 22 mg / cm. 2 , density is 3.0g / cm 3 It was.

[0118] A copper foil with a thickness of 10 μm was prepared as a negative electrode current collector. Layers containing graphite (Hitachi Chemical Co., Ltd. MAG-E), acetylene black, SBR binder, and CMC in weight ratios of 97%, 0.5%, 1%, and 1.5%, respectively, were provided on both sides of the negative electrode current collector, and the layers were pressed to form a negative electrode composite layer, thereby preparing a lithium ion negative electrode consisting of the negative electrode current collector and the negative electrode composite layer. The weight per unit area of ​​one side of the negative electrode composite layer was 11 mg / cm. 2 , density is 1.4g / cm 3 It was.

[0119] The positive and negative electrodes were cut out, and a large number of rectangular positive electrodes measuring 5.2 cm x 5.2 cm and rectangular negative electrodes measuring 5.4 cm x 5.4 cm were prepared. A PET nonwoven fabric (having a ceramic coating layer on the surface, 25 μm thick, product name "NanoBaseX OZ-S25", manufactured by Mitsubishi Paper Mills) was cut out, and a large number of rectangular separators measuring 5.6 cm x 5.6 cm were prepared. 15 rectangular positive electrodes, 30 rectangular separators, and 16 rectangular negative electrodes were stacked in a layer structure of (negative electrode) / (separator) / (positive electrode) / (separator) / (negative electrode) / (separator) / (positive electrode) / (separator) / ··· / (negative electrode). This resulted in a laminate including 15 pairs of positive and negative electrodes facing each other through the separator. Tabs were attached to the ends of each of the positive and negative electrodes by ultrasonic welding. The positive tab was made of aluminum and the negative tab was made of nickel. The stack was placed in an aluminum laminate exterior.

[0120] 0.8 mol / kg of LiPF6 as a salt was mixed with the components shown in Table 10 to prepare the electrolyte solutions (7-01) to (7-02) of the examples and the electrolyte solutions (C7-01) to (C7-02) of the comparative examples. When the properties of the obtained electrolyte solutions at 25°C were observed with the naked eye, all of them were homogeneous solutions. 10 ml of each of the electrolyte solutions was poured into an aluminum laminate exterior, and the opening was heat sealed while reducing the pressure inside to seal the exterior. This resulted in the production of stacked lithium ion batteries (7-01), (7-02), (C7-01) and (C7-02) (charge / discharge capacity 3100mAh).

[0121] (7-2. Overcharge test) An overcharge test was carried out on each of the obtained lithium ion batteries. First, as a preliminary charge and discharge, the battery was charged to 4.2 V at a current of 310 mA (0.1 C) at an ambient temperature of 25°C, and then discharged to 3 V at a current of 310 mA (0.1 C). In the battery (C7-02) whose solvent did not contain fluorine solvent components, swelling of the cell was confirmed during charging. When charging was continued further, the cell of the battery (C7-02) could not withstand the internal pressure and burst. The batteries (7-01) and (7-02) whose solvent contained 15% by weight or more of fluorine solvent components, and the battery (C7-01), were able to perform preliminary charge and discharge without any problems.

[0122] After preliminary charging and discharging, the batteries were charged again at a current of 310 mA (0.1 C) up to 4.2 V in a 25°C environment, and then the current was increased to 3100 mA (1.0 C) and constant current charging was performed with an upper voltage limit of 30 V. For all batteries (7-01), (7-02), and (C7-01), swelling of the batteries was confirmed after they reached 5 V. This is believed to be due to gas generation inside the batteries.

[0123] After reaching the upper limit voltage of 30V, the battery was charged at a constant voltage of 30V. The swelling in all the batteries increased, and eventually they exploded. In the batteries (7-01) and (7-02) whose solvent contained a fluorine solvent component, no flame was observed at the moment of explosion, but white smoke was emitted. Ignition was observed after 2 seconds in both cases. On the other hand, the explosion of the battery (C7-01) was accompanied by a flame. This difference is considered to be due to the composition of the gas that was ejected outside the exterior when the battery exploded. That is, in the case of the embodiment, the gas that was ejected was mainly composed of a non-flammable fluorine solvent component, while in the case of the comparative example, the gas that was ejected was mainly composed of a solvent component with a low flash point.

[0124] In all of the batteries (7-01), (7-02), and (C7-01), solid matter was released into the surrounding area when they exploded. In only the battery (C7-01), the released solid matter was observed to be burning outside the cell even after the release. In the batteries (7-01) and (7-02), the amount of released solid matter was less than that of the battery (C7-01), and no signs of burning were observed. In all of the batteries, the fire was extinguished in about one minute after ignition.

[0125] [Table 10]

[0126] The numerical values ​​for each component in the table indicate the amount added (unit: parts by weight).

[0127] (7-3. Coin cell battery) A coin cell battery was fabricated using an electrolyte of the same composition as that used in the battery (C7-02) that exploded during pre-charging. The positive and negative electrodes were prepared by the same procedure as in (7-1), except that the composite layer was formed on only one side of the current collector and cut into a circle, and one sheet each was used. The diameter of the circular positive electrode was 12 mm, and the diameter of the circular negative electrode was 13 mm. The separator was the same material as that used in (7-1), cut to a diameter of 16 mm, and this was used. For the exterior, a 2032 coin cell was used, and the amount of electrolyte was 120 μl, and these were combined to form a coin cell-shaped lithium-ion battery. This was charged and discharged under the same conditions as the preliminary charge and discharge in (7-1) (ambient temperature 25°C, charged to 4.2 V at a constant current of 0.1 C, and then discharged to 3 V at a constant current of 0.1 C). As a result, charging and discharging were possible without any problems. The reason for the difference with the large-capacity battery is unknown, but it is thought that in large-capacity devices, the electrochemical reaction is smoother when the electrolyte contains a fluorine solvent component.

Claims

1. An electrolyte for an electrochemical device comprising a salt and a solvent, The solvent is composed of a non-flammable fluorine solvent component (SF) and a remaining solvent component (SR), The ratio of the solvent component (SF) in 100% by weight of the electrolyte solution is 15% by weight or more, The solvent component (SR) includes a solvent component (SR80) having a flash point of more than 80° C., The solvent component (SR80) includes a solvent component (SR80A), The solvent component (SR80A) is one or more compounds that do not have a carbon-carbon unsaturated bond and are selected from the group consisting of cyclic carbonates having 4 or more carbon atoms, fluoroethylene carbonate, cyclic compounds having 4 or more carbon atoms and having one or more ester bonds in the molecule, dinitriles having 3 or more carbon atoms, sulfones having 2 or more carbon atoms, oxazolidone derivatives having 4 or more carbon atoms, imidazolidinone derivatives having 5 or more carbon atoms, carbonates having 9 or more carbon atoms, lactam derivatives having 5 or more carbon atoms, and mixtures thereof; The ratio of the solvent component (SR80) in 100% by weight of the solvent component (SR) is 90% by weight or more, The electrolyte solution has a ratio of the solvent component (SR80A) of 20% by weight or more relative to 100% by weight of the solvent component (SR).

2. 2. The electrolyte of claim 1, wherein the solvent component (SR80) comprises ethylene carbonate.

3. The solvent contains an additive (B) as the solvent component (SF) or the solvent component (SR80), 2. The electrolyte solution according to claim 1, wherein the additive (B) is at least one selected from the group consisting of a cyclic sulfate compound, a vinyl ethylene carbonate compound, and a fluorine compound having an unsaturated bond.

4. The electrolyte of claim 3 further comprising a sultone.

5. ClO as the salt in 100% by weight of the electrolyte 4 - , ClO 3 - , and NO 3 - The electrolyte according to claim 1, wherein the total proportion of

6. 2. The electrolyte of claim 1 having a flash point greater than 80°C.

7. An electrochemical device comprising a positive electrode, a negative electrode, and an electrolyte, The electrolytic solution is the electrolytic solution according to any one of claims 1 to 6, The electrochemical device, wherein the negative electrode comprises a carbon material.

8. 8. The electrochemical device according to claim 7, wherein the negative electrode contains graphite as the carbon material.

9. The electrochemical device according to claim 7 , which is an ion battery.

10. 10. The electrochemical device of claim 9 which is a lithium ion battery.

11. The electrochemical device according to claim 7 , having a storage capacity of 3 Ah or more.

Citation Information

Patent Citations

  • Nonaqueous electrolytic secondary battery

    JP1996037024A

  • Nonaqueous electrolyte and nonaqueous electrolyte secondary battery using the same

    JP2001052737A

  • Nonaqueous electrolytic solution for secondary battery, and nonaqueous electrolyte secondary battery using it

    JP2007180016A

  • Nonaqueous electrolyte cell

    JP2013218963A

  • Nonaqueous electrolyte, and nonaqueous electrolyte secondary battery

    JP2000223151A