Magnetic substrate, coil component including magnetic substrate, circuit board including coil component, and electronic device including circuit board

A magnetic substrate with a high filling rate of soft magnetic metal particles covered by Al and Si oxides, and optionally Cr oxide, addresses insulation and distortion issues, achieving improved magnetic properties and reduced losses.

JP2024145587APending Publication Date: 2024-10-15TAIYO YUDEN KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023058011
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Increasing the filling rate of soft magnetic metal particles in magnetic substrates leads to insufficient oxide film formation on particle surfaces due to reduced gaps, compromising electrical insulation and causing magnetic substrate distortion and high coercive force.

Method used

A magnetic substrate with a filling rate of 85% or more, featuring soft magnetic metal particles covered by insulating films made of Al and Si oxides, and optionally Cr oxide, to ensure adequate insulation and reduce magnetic losses.

Benefits of technology

The solution provides a magnetic substrate with excellent insulation properties and reduced magnetic losses, maintaining high magnetic permeability and saturation characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145587000001_ABST
    Figure 2024145587000001_ABST
Patent Text Reader

Abstract

To provide a magnetic substrate having excellent insulating and magnetic properties.SOLUTION: A magnetic substrate according to an embodiment includes a plurality of soft magnetic metal particles and a plurality of insulating films covering the surfaces of each of the plurality of soft magnetic metal particles. In the magnetic substrate, the plurality of soft magnetic metal particles are filled with a filling rate of 85% or more. The KAM value of the soft magnetic metal particles is 0.6 or less. The soft magnetic metal particles contain 95 wt% or more of Fe, Si, and Al. The insulating film contains an oxide of Si and an oxide of Al.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The disclosure in this specification mainly relates to a magnetic base, a coil component including a magnetic base, a circuit board including a coil component, and an electronic device including a circuit board. [Background technology]

[0002] A soft magnetic substrate containing a large number of soft magnetic metal particles made of a soft magnetic material is used as a magnetic substrate for coil components. The surface of each of the soft magnetic metal particles contained in the soft magnetic substrate is covered with an insulating film, and adjacent soft magnetic metal particles are bonded to each other via the insulating film. The soft magnetic substrate is characterized by being less susceptible to magnetic saturation than a magnetic substrate made of ferrite, and is therefore particularly suitable for use in coil components used in circuits through which large currents flow.

[0003] International Publication No. 2018 / 180659 (Patent Document 1) describes a method of forming a green body by pressure-molding Fe-Si-based soft magnetic metal particles, the main components of which are Fe and Si, and then performing primary heating at a temperature of 500°C or more and 800°C or less at a first oxygen partial pressure described in paragraph

[0034] of the same publication to relieve distortion in the pressure-molded green body, and then performing secondary heating on the green body at a second oxygen partial pressure higher than the first oxygen partial pressure to form an oxide coating made of an oxide of Si around the soft magnetic metal particles. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2018 / 180659 Summary of the Invention [Problem to be solved by the invention]

[0005] In order to increase the magnetic permeability of the magnetic substrate, it is desirable to increase the proportion of soft magnetic metal particles in the magnetic substrate (filling rate). In the manufacturing process of the magnetic substrate, the filling rate of the soft magnetic metal particles in the magnetic substrate can be increased by producing a compact of soft magnetic metal particles at a high molding pressure.

[0006] However, when the compact is compressed under high pressure, the gaps between the soft magnetic metal particles become smaller, making it difficult to supply sufficient oxygen to form an oxide film on the surface of the soft magnetic metal particles during heating. Therefore, when the filling rate of the soft magnetic metal particles in the magnetic base is increased, an oxide film is not sufficiently formed on the surface of the soft magnetic metal particles, resulting in a problem that electrical insulation between the soft magnetic metal particles cannot be ensured.

[0007] Furthermore, when the compact is molded under high pressure, there is a problem in that the magnetic substrate also becomes distorted after heating. If the magnetic substrate has a large distortion, the coercive force increases, resulting in a large magnetic loss.

[0008] It is an object of the invention disclosed herein to solve or alleviate at least some of the above-mentioned problems, and more specifically to provide a magnetic substrate having excellent insulating and magnetic properties.

[0009] Objects of the present invention other than those mentioned above will become clear throughout the entire description of the specification. The invention disclosed in this specification may solve problems that are understood from other than the description in the "Problems to be Solved by the Invention" column. When the effects of an embodiment are described in this specification, the problems of the invention corresponding to the embodiment can be understood from the effects. [Means for solving the problem]

[0010] The magnetic substrate in one embodiment includes a plurality of soft magnetic metal particles and a plurality of insulating films covering the surfaces of each of the soft magnetic metal particles. In the magnetic substrate, the soft magnetic metal particles are filled with a filling rate of 85% or more. The KAM value of the soft magnetic metal particles is 0.6 or less. The soft magnetic metal particles contain 95 wt% or more Fe, Si, and Al. The insulating film contains an oxide of Si and an oxide of Al. Effect of the Invention

[0011] According to the embodiments of the invention disclosed in this specification, a magnetic substrate having excellent insulating properties and magnetic properties can be obtained. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a perspective view illustrating a coil component including a magnetic composite according to an embodiment. [Diagram 2] FIG. 2 is an exploded perspective view of the coil component of FIG. [Diagram 3] 2 is a cross-sectional view that illustrates a cross section of the coil device of FIG. 1 taken along line II. [Figure 4] FIG. 2 is an enlarged cross-sectional view that shows a schematic enlargement of a partial region of a cross section of a magnetic substrate according to one embodiment. [Diagram 5] FIG. 11 is an enlarged cross-sectional view that shows a schematic enlargement of a partial region of a cross section of a magnetic substrate according to another embodiment. [Figure 6] FIG. 4 is an enlarged cross-sectional view that shows a schematic enlargement of a partial region of a cross section of a magnetic substrate according to another embodiment. [Figure 7] FIG. 4 is a flow chart showing a manufacturing process of the coil component according to the embodiment of the present invention. [Figure 8] FIG. 6 is a flow diagram showing a manufacturing process of a coil component according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Various embodiments of the present invention will be described below with reference to the drawings as appropriate. Components common to multiple drawings are given the same reference numerals. Please note that the drawings are not necessarily drawn to scale for the sake of convenience. The embodiments of the present invention described below do not necessarily limit the invention according to the claims. Elements described in the following embodiments are not necessarily essential to the solution of the invention.

[0014] One embodiment disclosed in the present specification relates to a magnetic substrate of a coil component. The magnetic substrate includes a plurality of soft magnetic metal particles. In the following, first, a coil component 1 including a magnetic substrate according to one embodiment will be described with reference to Figs. 1 to 3, and then a microstructure of the magnetic substrate will be described with reference to Fig. 4.

[0015] Fig. 1 is a perspective view that shows a schematic diagram of the coil component 1, and Fig. 2 is an exploded perspective view of the coil component 1. Fig. 3 is a schematic cross-sectional view of the coil component 1, in which the coil component 1 is cut along line II in Fig. 1. For ease of explanation, external electrodes are omitted from Fig. 2.

[0016] 1 to 3 show a laminated inductor as an example of a coil component 1. The illustrated laminated inductor is one example of a coil component 1 to which the present invention can be applied, and the present invention can be applied to various types of coil components other than laminated inductors. For example, the coil component 1 can also be applied to a wire-wound coil component or a planar coil.

[0017] As shown in the figure, the coil component 1 includes a magnetic base 10, a coil conductor 25 provided inside the magnetic base 10, an external electrode 21 provided on the surface of the magnetic base 10, and an external electrode 22 provided on the surface of the magnetic base 10 at a position spaced apart from the external electrode 21. The magnetic base 10 is a magnetic base made of a magnetic material. The magnetic base 10 is an example of a "magnetic base" described in the claims.

[0018] The magnetic substrate 10 includes a large number of soft magnetic metal particles. The average particle size of the soft magnetic metal particles included in the magnetic substrate 10 is, for example, in the range of 1 μm to 10 μm. The average particle size of the soft magnetic metal particles may be 5 μm or less. The average particle size of the soft magnetic metal particles included in the magnetic substrate 10 can be determined by cutting the magnetic substrate 10 along its thickness direction (T-axis direction) to expose a cross section, photographing the cross section with a scanning electron microscope (SEM) at a magnification of about 10,000 times to 50,000 times, determining the circle equivalent diameter (Heywood diameter) of each soft magnetic metal particle by image analysis, and determining the average value of the circle equivalent diameters of each soft magnetic metal particle as the average particle size of the soft magnetic metal particles. The average particle size of the soft magnetic metal particles included in the magnetic substrate 10 may be 1 μm to 10 μm, or 2 μm to 8 μm. Since the average particle size of the soft magnetic metal particles and the average particle size of the raw material powder do not differ significantly, the particle size distribution of the raw material powder can be measured by a laser diffraction scattering method in accordance with JIS Z 8825, and the D50 value of the volume-based particle size distribution measured by this laser diffraction scattering method can be used as the average particle size of the soft magnetic metal particles contained in the magnetic base 10.

[0019] The external electrode 21 is electrically connected to one end of the coil conductor 25 , and the external electrode 22 is electrically connected to the other end of the coil conductor 25 .

[0020] The coil component 1 can be mounted on a mounting board 2a. In the illustrated embodiment, the mounting board 2a is provided with land portions 3a and 3b. The coil component 1 is mounted on the mounting board 2a by joining an external electrode 21 to the land portion 3a and connecting an external electrode 22 to the land portion 3b. A circuit board 2 according to an embodiment of the present invention includes the coil component 1 and a mounting board 2a on which the coil component 1 is mounted. The circuit board 2 can be mounted on various electronic devices. Electronic devices on which the circuit board 2 can be mounted include smartphones, tablets, game consoles, automotive electrical equipment, servers, and various other electronic devices.

[0021] The coil component 1 may be an inductor, a transformer, a filter, a reactor, an inductor array, or any other of various coil components. The coil component 1 may be a coupled inductor, a choke coil, or any other of various magnetically coupled coil components. Applications of the coil component 1 are not limited to those explicitly described in this specification.

[0022] When the coil component 1 is an inductor array or a magnetically coupled coil component, the coil conductor 25 is composed of two or more conductor parts. The two or more conductor parts constituting the coil conductor 25 are electrically insulated from each other within the magnetic base 10.

[0023] In one embodiment, the magnetic base 10 is configured so that the dimension in the L-axis direction (length dimension) is larger than the dimension in the W-axis direction (width dimension) and the dimension in the T-axis direction (height dimension). For example, the length dimension is in the range of 1.0 mm to 6.0 mm, the width dimension is in the range of 0.5 mm to 4.5 mm, and the height dimension is in the range of 0.5 mm to 4.5 mm. The dimensions of the magnetic base 10 are not limited to the dimensions specifically described in this specification. In this specification, the term "rectangular parallelepiped" or "rectangular parallelepiped shape" does not mean only "rectangular parallelepiped" in the mathematically strict sense. The dimensions and shape of the magnetic base 10 are not limited to those explicitly described in this specification.

[0024] The magnetic base 10 has a first main surface 10a, a second main surface 10b, a first end surface 10c, a second end surface 10d, a first side surface 10e, and a second side surface 10f. The outer surface of the magnetic base 10 is defined by these six surfaces. The first main surface 10a and the second main surface 10b form the surfaces at both ends of the magnetic base 10 in the height direction, the first end surface 10c and the second end surface 10d form the surfaces at both ends of the magnetic base 10 in the length direction, and the first side surface 10e and the second side surface 10f form the surfaces at both ends of the magnetic base 10 in the width direction. As shown in FIG. 1, the first main surface 10a on the upper side of the magnetic base 10 may be referred to as the "upper surface" in this specification. Similarly, the second main surface 10b may be referred to as the "lower surface" or "bottom surface". The coil component 1 is disposed so that the second main surface 10b faces the mounting board 2a, and therefore the second main surface 10b is sometimes called a "mounting surface." The upper surface 10a and the lower surface 10b are spaced apart by the height dimension of the magnetic base 10, the first end surface 10c and the second end surface 10d are spaced apart by the length dimension of the magnetic base 10, and the first side surface 10e and the second side surface 10f are spaced apart by the width dimension of the magnetic base 10.

[0025] 2, the magnetic substrate 10 has a body layer 20, a lower cover layer 19 provided on the lower surface of the body layer 20, and an upper cover layer 18 provided on the upper surface of the body layer 20. The upper cover layer 18, the lower cover layer 19, and the body layer 20 are components of the magnetic substrate 10.

[0026] The main body layer 20 includes magnetic films 11 to 17. In the main body layer 20, the magnetic film 17, the magnetic film 16, the magnetic film 15, the magnetic film 14, the magnetic film 13, the magnetic film 12, and the magnetic film 11 are laminated in this order from the negative side to the positive side in the T-axis direction.

[0027] Conductive patterns C11 to C17 are formed on the upper surfaces of the magnetic films 11 to 17, respectively. Each of the conductive patterns C11 to C17 extends around the coil axis Ax1 (see FIG. 3) in a plane (LW plane) perpendicular to the coil axis Ax1. The conductive patterns C11 to C17 are formed, for example, by printing a conductive paste made of a metal or alloy with excellent conductivity by a screen printing method. The conductive paste may be made of Ag, Pd, Cu, Al, or an alloy thereof. The conductive paste is produced by kneading a conductive powder made of a conductive material with excellent conductivity, such as Ag, Pd, Cu, Al, or an alloy thereof, with a binder resin and a solvent. The binder resin may be a PVB resin, a phenol resin, a resin known as a binder resin other than the above, or a mixture thereof. When Cu powder is used as the conductive powder, a thermally decomposable resin such as an acrylic resin may be used as the binder resin in order to suppress excessive oxidation of the Cu powder during degreasing. The thermally decomposable resin is decomposed without a combustion reaction with oxygen. The thermally decomposable resin is thermally decomposed when heated to a temperature equal to or higher than the thermal decomposition temperature even in a non-oxygen atmosphere (for example, a nitrogen atmosphere), and no residue is left behind. Therefore, by using a thermally decomposable resin as a binder resin, the degreasing process can be performed in a non-oxygen atmosphere. As the acrylic resin for the conductive paste, for example, a (meth)acrylic acid copolymer, a (meth)acrylic acid-(meth)acrylic acid ester copolymer, a styrene-(meth)acrylic acid copolymer, or a styrene-(meth)acrylic acid-(meth)acrylic acid ester copolymer can be used. As the solvent, toluene, ethanol, terpineol, or a mixture thereof can be used. The conductive paste can contain an adjusting agent for adjusting the thixotropy. The conductive patterns C11 to C17 may be formed by other materials and methods. The conductive patterns C11 to C17 may be formed by, for example, a sputtering method, an inkjet method, or other known methods.

[0028] Vias V1 to V6 are formed at predetermined positions of the magnetic films 11 to 16, respectively. The vias V1 to V6 are formed by forming through holes penetrating the magnetic films 11 to 16 in the T-axis direction at predetermined positions of the magnetic films 11 to 16, and filling the through holes with a conductive material. Each of the conductor patterns C11 to C17 is electrically connected to the adjacent conductor patterns via the vias V1 to V6.

[0029] The end of the conductor pattern C11 opposite to the end connected to the via V1 is connected to an external electrode 22. The end of the conductor pattern C17 opposite to the end connected to the via V6 is connected to an external electrode 21.

[0030] The upper cover layer 18 includes magnetic films 18a-18d made of a magnetic material, and the lower cover layer 19 includes magnetic films 19a-19d made of a magnetic material. In this specification, the magnetic films 18a-18d and the magnetic films 19a-19d may be collectively referred to as "cover layer magnetic films." In addition, the components of the magnetic substrate 10 do not necessarily have a laminated structure in which a plurality of magnetic films are laminated. For example, the upper cover layer 18 may be a molded body molded from a magnetic material, instead of a laminate in which a plurality of magnetic films 18a-18d are laminated.

[0031] 3, the coil conductor 25 has a winding portion 25a wound around a coil axis Ax1 extending along the thickness direction (T-axis direction), a lead-out portion 25b1 extending from one end of the winding portion 25a to the first end face 10c of the magnetic base 10, and a lead-out portion 25b2 extending from the other end of the winding portion 25a to the second end face 10d of the magnetic base 10. The conductor patterns C11 to C17 and the vias V1 to V6 form the spiral winding portion 25a. That is, the winding portion 25a has the conductor patterns C11 to C17 and the vias V1 to V6.

[0032] Next, the microstructure of the magnetic base 10 will be described with reference to Fig. 4. Fig. 4 is an enlarged cross-sectional view that shows a schematic enlargement of a partial region of the cross section shown in Fig. 3. Fig. 4 shows a schematic view of two portions of the numerous soft magnetic metal particles contained in the magnetic base 10.

[0033] As shown in FIG. 4, the soft magnetic metal particles contained in the magnetic substrate 10 include a first soft magnetic metal particle 30a and a second soft magnetic metal particle 30b. The first soft magnetic metal particle 30a and the second soft magnetic metal particle 30b are arranged adjacent to each other. In FIG. 4, the cross sections of the first soft magnetic metal particle 30a and the second soft magnetic metal particle 30b are drawn as circles for convenience. The soft magnetic metal particles contained in the magnetic substrate 10 may have various cross-sectional shapes other than circles. The soft magnetic metal particles contained in the magnetic substrate 10 are mainly composed of iron (Fe). The first soft magnetic metal particle 30a and the second soft magnetic metal particle 30b are examples of the soft magnetic metal particles contained in the magnetic substrate 10. The description of the first soft magnetic metal particle 30a and the second soft magnetic metal particle 30b also applies to soft magnetic metal particles other than the first soft magnetic metal particle 30a or the second soft magnetic metal particle 30b contained in the magnetic substrate 10.

[0034] The soft magnetic metal particles contained in the magnetic substrate 10 contain Fe at a content ratio of 95 wt% or more so that the magnetic substrate 10 has high magnetic saturation characteristics. The content ratio of Fe contained in the soft magnetic metal particles contained in the magnetic substrate 10 is measured by exposing a cross section of the magnetic substrate 10 by cutting the magnetic substrate 10 along the coil axis Ax and performing energy dispersive X-ray spectroscopy (EDS) analysis on this cross section. The content ratio of Fe can be measured by a scanning electron microscope (SEM) equipped with an energy dispersive X-ray spectroscopy (EDS) detector. EDS analysis using an SEM equipped with an EDS detector is called SEM-EDS analysis. The content ratio of Fe is measured, for example, using a scanning electron microscope SU7000 manufactured by Hitachi High-Tech Corporation and an energy dispersive X-ray spectroscopy detector Octane Elite manufactured by Ametech Co., Ltd. at an acceleration voltage of 5 kV. The content ratios of elements other than Fe contained in the first soft magnetic metal particles 30a are also measured by SEM-EDS analysis in the same manner as the content ratio of Fe.

[0035] The surface of each of the soft magnetic metal particles included in the magnetic substrate 10 is covered with an insulating film. Therefore, the soft magnetic metal particles included in the magnetic substrate 10 are electrically insulated from each other. For example, the surface of the first soft magnetic metal particle 30a is covered with a first insulating film 40a, and the surface of the second soft magnetic metal particle 30b is covered with a second insulating film 40b. The first insulating film 40a desirably covers the entire surface of the first soft magnetic metal particle 30a, and the second insulating film 40b desirably covers the entire surface of the second soft magnetic metal particle 30b. In the magnetic substrate 10, each soft magnetic metal particle is bonded to an adjacent soft magnetic metal particle via an insulating film provided on each surface. That is, the insulating films provided on the surfaces of adjacent soft magnetic metal particles are bonded to each other, and the soft magnetic metal particles covered with the insulating film are bonded to each other by the bonding of the insulating films. For example, the first soft magnetic metal particle 30a is bonded to the second soft magnetic metal particle 30b adjacent to the first soft magnetic metal particle 30a via a first insulating film 40a provided on the surface of the first soft magnetic metal particle 30a and a second insulating film 40b provided on the surface of the second soft magnetic metal particle 30b. Since the surfaces of the soft magnetic metal particles are covered with an insulating film, the magnetic base 10 is 5 It has a volume resistivity of Ω·cm or more.

[0036] The soft magnetic metal particles contained in the magnetic substrate 10 can be obtained, for example, by heating raw material powder made of a soft magnetic material. As described in detail below, the magnetic substrate 10 can be produced by mixing soft magnetic metal powder made of a soft magnetic material with a resin to produce a mixed resin composition, and then heating this mixed resin composition. By the heat treatment in the manufacturing process of the magnetic substrate 10, the elements contained in the raw material powder diffuse to the surface of the raw material powder and are oxidized on the surface of the raw material powder, so that an insulating film containing an oxide of the elements contained in the raw material powder is formed on the surface of the soft magnetic metal particles.

[0037] The raw material powder of the soft magnetic metal particles contained in the magnetic base 10 is mainly composed of Fe. The raw material powder of the soft magnetic metal particles contained in the magnetic base 10 can contain additive elements in addition to Fe. For example, the raw material powder of the soft magnetic metal particles contained in the magnetic base 10 contains silicon (Si) and aluminum (Al) as additives in addition to Fe. The raw material powder may further contain magnesium (Mg). The raw material powder of the soft magnetic metal particles may contain both Al and Mg. The raw material powder of the soft magnetic metal particles may further contain chromium (Cr). The raw material powder of the soft magnetic metal particles may contain a trace amount of at least one element selected from the group consisting of titanium (Ti), zinc (Zn), and manganese (Mn).

[0038] Since Al is significantly more easily oxidized than Fe, it is oxidized before Fe when the raw material powder is heat-treated in an atmosphere in which oxygen is present. Therefore, by including Al in the raw material powder in addition to Fe, the oxidation of Fe is suppressed. Furthermore, by including Al in the raw material powder, even if the amount of oxygen around the raw material powder is small, the oxide of Al (Al 2 O 3 ) is likely to form an oxide film covering the surface of the raw material powder.

[0039] Like Al, Mg is significantly more easily oxidized than Fe, and is therefore oxidized before Fe when the raw material powder is heat-treated in an atmosphere containing oxygen. Therefore, by containing Al and Mg in addition to Fe in the raw material powder, the oxidation of Fe is suppressed. Furthermore, by containing Al and Mg in the raw material powder, even if the amount of oxygen around the raw material powder is small, an oxide film containing an oxide of Al and an oxide of Mg (MgO) is likely to form to cover the surface of the raw material powder.

[0040] By adding Si to the raw material powder, the hardness of the raw material powder can be increased. By using raw material powder with increased hardness, it becomes easier to produce a generally uniform green body by compression molding.

[0041] By including Cr in the raw material powder, when Fe is oxidized, insulating chromite is more likely to be produced instead of conductive magnetite. Therefore, by including Cr in the raw material powder, the insulating properties of the magnetic base 10 can be improved.

[0042] By heating the raw material powder, Si, Al, Mg, and Cr are thermally diffused to the surface of the raw material powder and oxidized by oxygen in the atmosphere, but a portion of each element remains in the soft magnetic metal particles.

[0043] The insulating film provided on the surface of the soft magnetic metal particles included in the magnetic base 10 contains an oxide of an element included in the raw material powder. The "insulating film provided on the surface of the soft magnetic metal particles included in the magnetic base 10" includes the first insulating film 40a provided on the surface of the first soft magnetic metal particles 30a and the second insulating film 40b provided on the surface of the second soft magnetic metal particles 30b. For convenience of explanation, the insulating film provided on the surface of the soft magnetic metal particles included in the magnetic base 10 may be simply called an "insulating film". Since Al and Si are more easily oxidized than Fe, when the raw material powder contains Al and Si in addition to Fe, the insulating film contains oxides of Al and Si. When the raw material powder contains Mg, the insulating film contains an oxide of Mg. The insulating film may contain a small amount of oxide of at least one element selected from the group consisting of titanium (Ti), zinc (Zn), and manganese (Mn).

[0044] In one embodiment, the thickness of the insulating film is equal to the distance between adjacent soft magnetic metal grains. The average of the distances between adjacent soft magnetic metal grains included in the observation field of the central region of the cross section of the magnetic substrate 10 at a predetermined magnification (for example, 10,000 times) can be the thickness of the insulating film provided on the surface of the soft magnetic metal grain. The thickness of the insulating film is, for example, 5 to 20 nm. The thickness of the insulating film does not have to be uniform along the circumferential direction of the soft magnetic metal grain. In other words, the insulating film may have different thicknesses at different positions in the circumferential direction of the soft magnetic metal grain. When the insulating film has different thicknesses depending on the position in the circumferential direction of the soft magnetic metal grain, the average of the different thicknesses can be the thickness of the insulating film. The thickness of the thinnest part of the insulating film may be thinner than 5 nm. The thickness of the thickest part of the insulating film may be thicker than 20 nm. When the insulating film has different thicknesses depending on the position in the circumferential direction of the soft magnetic metal grain, the maximum thickness is less than 10 times the minimum thickness.

[0045] The magnetic substrate 10 is filled with soft magnetic metal particles at a filling rate of 85% or more. The filling rate of the soft magnetic metal particles in the magnetic substrate 10 can be the ratio of the area occupied by the soft magnetic metal particles to the total area of ​​the observation field in a scanning electron microscope (SEM) image obtained by cutting the magnetic substrate 10 along its thickness direction (T-axis direction) to expose a cross section and photographing the cross section at a magnification of, for example, 10,000 to 50,000 times. The area occupied by the soft magnetic metal particles in the observation region of the SEM image may be the area of ​​the part excluding the area of ​​the voids and the area of ​​the insulating film included in the observation field from the total area of ​​the observation field of the SEM image.

[0046] In one embodiment, the KAM value of the soft magnetic metal particles contained in the magnetic substrate 10 is 0.6 or less. The KAM value of the soft magnetic metal particles contained in the magnetic substrate 10 may be 0.5 or less. The KAM value of the soft magnetic metal particles contained in the magnetic substrate 10 is 0.3 or more. The KAM value of the soft magnetic metal particles contained in the magnetic substrate 10 can be calculated as follows. The magnetic substrate 10 is cut along its thickness direction (T-axis direction) to expose the cross section, and a region near the center of the cross section is polished. EBSD measurement is performed on the polished cross section of the magnetic substrate using a scanning electron microscope (SEM) equipped with an electron backscatter diffraction (EBSD) detector under conditions of an acceleration voltage of 15 kV, a magnification of 10,000 times, and a step size of 0.05 μm, to obtain an IQ map showing the distribution of Image Quality (IQ value) in the observation field, and a region with an IQ value equal to or greater than a predetermined threshold is identified as a region where soft magnetic metal particles exist. This threshold can be set to a value of 15% to 30%. For the region in which the soft magnetic metal particles are present, the average value of the kernel average misorientation (KAM value) is calculated from the EESD pattern. The average value of the KAM value in the region in which the soft magnetic metal particles are present in the observation field of view calculated in this manner can be set as the KAM value of the soft magnetic metal particles in the magnetic substrate 10. For the above measurement, an SEM SU7000 manufactured by Hitachi High-Tech Corporation can be used as the SEM, and an EBSD Velocity manufactured by Ametech Co., Ltd. can be used as the EESD detector.

[0047] The insulating film covering the surface of the soft magnetic metal particle will be further described with reference to Fig. 4. As shown in Fig. 4, the first insulating film 40a covers the first surface region 31a, which is a part of the surface of the first soft magnetic metal particle 30a, and is made of an oxide of Al (Al 2 O 3 The first oxide region 41a mainly contains an oxide of Mg (MgO) or an oxide of Si (SiO 2 and a second oxide region 42a containing .alpha.-(.alpha.) as a main component.

[0048] The first oxide region 41a is made of alumina (Al 2 O 3 ) as a main component. When the EDS analysis shows that the abundance of Al element (atomic ratio (at%) of Al element) is the largest among elements other than oxygen contained in the first oxide region 41a, the first oxide region 41a can be said to have alumina as a main component. The first oxide region 41a has high insulating properties because it has insulating alumina as a main component. When there is a possibility that the first oxide region 41a contains an oxide of aluminum other than alumina (e.g., aluminum(II) oxide), it may be determined by performing Raman spectroscopy analysis that the oxide contained as a main component in the first oxide region 41a is alumina (aluminum(III) oxide) rather than aluminum(II) oxide.

[0049] The second oxide region 42a is made of silica (SiO 2 ) as a main component. When the EDS analysis shows that the abundance of Si element (atomic ratio (at%) of Si element) is the largest among elements other than oxygen contained in the second oxide region 42a, the second oxide region 42a can be said to have silica as a main component. The second oxide region 42a has high insulating properties because it has insulating silica as its main component. When there is a possibility that the second oxide region 42a contains an oxide of silicon other than silica (e.g., silicon monoxide), it may be determined by performing Raman spectroscopy analysis that the oxide contained as a main component in the second oxide region 42a is silica (silicon dioxide) rather than silicon monoxide.

[0050] The insulating film may contain, in addition to the oxide of an element contained in the raw material powder, a nitride of the element. The proportion of oxide in the insulating film (by mass) is greater than the proportion of nitride in the insulating film. The nitride contained in the insulating film may include aluminum nitride and silicon nitride. By including a nitride of an element contained in the raw material powder in the insulating film, excessive oxidation of the element contained in the raw material powder is suppressed. Generally, oxides have a higher hardness than nitrides, so that including more oxides than nitrides in the insulating film can increase the mechanical strength of the magnetic base 10.

[0051] The surface of the first soft magnetic metal particle 30a is divided into a first surface region 31a and a second surface region 32a. Of the surface of the first soft magnetic metal particle 30a, the first surface region 31a is covered with the first oxide region 41a, and the second surface region 32a is covered with the second oxide region 42a, so that the entire surface of the first soft magnetic metal particle 30a is covered with the insulating first oxide region 41a and second oxide region 42a.

[0052] The first oxide region 41a may be formed to cover not only the first surface region 31a of the first soft magnetic metal particle 30a but also at least a part of the outer surface of the second oxide region 42a. By covering the outer surface of the second oxide region 42a with the first oxide region 41a, even if a defect occurs in a part of the second oxide region 42a, the defect can be covered with the first oxide region 41a to prevent dielectric breakdown from occurring starting from the defect in the second oxide region 42a. In the embodiment shown in FIG. 4, the entire outer surface of the second oxide region 42a is covered with the first oxide region 41a. By covering the entire outer surface of the second oxide region 42a with the first oxide region 41a, dielectric breakdown can be further suppressed.

[0053] The first oxide region 41a may be provided so as to cover only a portion of the outer surface of the second oxide region 42a. In this case, the amount of the first oxide region 41a present on the surface of the first soft magnetic metal particle 30a can be reduced. Therefore, by the first oxide region 41a covering only a portion of the outer surface of the second oxide region 42a, the filling rate of the soft magnetic metal particles in the magnetic base 10 can be improved compared to the embodiment in which the first oxide region 41a covers the entire outer surface of the second oxide region 42a.

[0054] In the embodiment shown in FIG. 4, the first insulating film 40a includes a plurality of second oxide regions 42a that are spaced apart from each other. Thus, the second oxide regions 42a that contain an oxide of Si as a main component are not formed in a layer shape so as to cover the entire surface of the first soft magnetic metal particle 30a, but are formed discretely on the surface of the first soft magnetic metal particle 30a. By setting the amount of Si contained in the raw material powder to 4 wt% or less, a plurality of second oxide regions 42a can be formed discretely on the surface of the first soft magnetic metal particle 30a. The content of Si in the raw material powder can be 1 to 4 wt%. In addition, in order to provide a thin insulating film, the content of Al can be, for example, 1 wt% or less. When the raw material powder contains Mg or when the raw material powder is a mixed powder of an Fe-Si-Al alloy and Mg powder, the content of Mg and Al in total can be 1 wt% or less.

[0055] A second insulating film 40b is provided on the surface of the second soft magnetic metal particle 30b arranged adjacent to the first soft magnetic metal particle 30a. The second insulating film 40b includes a first oxide region 41b that covers the first surface region 31b, which is a part of the surface of the second soft magnetic metal particle 30b, and contains an oxide of Al as a main component, and a second oxide region 42b that covers the second surface region 32b, which is a part of the surface of the second soft magnetic metal particle 30b, and contains an oxide of Si as a main component. The first oxide region 41b contains an oxide of Al as a main component, similar to the first oxide region 41a. The above description of the first oxide region 41a also applies to the first oxide region 41b. The second oxide region 42b contains an oxide of Si as a main component, similar to the second oxide region 42a.

[0056] In the magnetic substrate 10, the soft magnetic metal particles are covered with an insulating film containing an oxide of Al and an oxide of Si, so that the insulating properties of the magnetic substrate 10 can be improved. In order to achieve high insulating properties with an insulating film made of a single type of oxide, the entire surface of the soft magnetic metal particles must be covered with a layer of the oxide. In the magnetic substrate 10, even if there is a region on the surface of the soft magnetic metal particles that is not covered with an oxide of Si, the region can be covered with an oxide of Al. Specifically, in the magnetic substrate 10, the second oxide region 42a is formed only on a part of the first soft magnetic metal particles 30a (i.e., only on the second surface region 32a), but the other region on the surface of the first soft magnetic metal particles 30a (i.e., the first surface region 31a) is covered with the first oxide region 41a mainly composed of an oxide of Al. Therefore, it is possible to suppress a decrease in insulating properties caused by a part of the surface of the first soft magnetic metal particles 30a being exposed. The soft magnetic metal particles other than the first soft magnetic metal particles 30a contained in the magnetic base 10 are also covered with an insulating film containing oxides of two elements (that is, Al and Si), so that the insulating properties of the magnetic base 10 can be improved.

[0057] The difference between the insulating film (for example, the first insulating film 40a) provided on the surface of the soft magnetic metal particles contained in the magnetic substrate 10 of the present application and the insulating film provided on the surface of the conventional soft magnetic metal particles will be described. Conventionally, when an insulating film covering the surface of a soft magnetic metal particle contains oxides of two or more elements, the insulating film has a laminated structure in which the oxides of each element are formed in layers and the oxide layers formed in layers are laminated. In other words, the insulating film of the conventional magnetic substrate covers the entire outer surface of the soft magnetic metal particle with a first oxide layer mainly composed of an oxide of a first element, and covers the entire outer surface of the first oxide layer with a second oxide layer mainly composed of an oxide of a second element. A conventional magnetic substrate in which an insulating film has a laminated structure is described, for example, in JP 2021-158261 A.

[0058] In contrast, in the magnetic substrate 10 of the present application, the first surface region 31a of the surface of the first soft magnetic metal particle 30a is covered with the first oxide region 41a, and the second surface region 32a of the first soft magnetic metal particle 30a is covered with the second oxide region. Therefore, in the magnetic substrate 10 to which the present invention is applied, the proportion of the insulating film in the magnetic substrate 10 can be made smaller than that of a conventional magnetic substrate having an insulating film in which two or more oxide layers are stacked. As a result, the filling rate of the soft magnetic metal particles in the magnetic substrate 10 can be increased to 85% or more, and the magnetic properties can be improved compared to that of a conventional magnetic substrate having an insulating film in which two or more oxide layers are stacked.

[0059] As described above, the oxide of Al contained in the insulating film covering the surface of the soft magnetic metal particles contained in the magnetic base 10 may be derived from Al contained in the raw powder of the soft magnetic metal particles, but in another embodiment, the oxide of Al may not be derived from the raw powder of the soft magnetic metal particles. For example, the raw powder of the soft magnetic metal particles and alumina particles may be mixed in a friction mixer to fix the alumina particles to the surface of the soft magnetic metal particles. This allows the oxide of Al that is not derived from the Al element contained in the raw powder to be attached to the surface of the soft magnetic metal particles. The first oxide regions 41a, 41b may be composed of alumina powder attached to the soft magnetic metal particles. When the oxide of Al contained in the insulating film covering the surface of the soft magnetic metal particles is not derived from an element contained in the raw powder, the raw powder may not contain Al. Similarly, the oxide of Mg contained in the insulating film covering the surface of the soft magnetic metal particles contained in the magnetic base 10 may not be derived from the raw powder of the soft magnetic metal particles. For example, the raw powder of the soft magnetic metal particles and the raw powder of the magnesium metal powder may be mixed in a friction mixer to adhere the magnesium powder to the surface of the soft magnetic metal particles. This allows Mg oxides that are not derived from the Mg element contained in the raw powder to adhere to the surface of the soft magnetic metal particles. The raw powder of magnesium may be either a metal powder or an oxide powder.

[0060] As described above, the oxide of Si contained in the insulating film covering the surface of the soft magnetic metal particles contained in the magnetic base 10 may be derived from Si contained in the raw material powder of the soft magnetic metal particles, but in another embodiment, the oxide of Si may not be derived from the raw material powder of the soft magnetic metal particles. For example, the raw material powder is impregnated with a mixed solution of TEOS (tetraethoxysilane), ethanol, and ammonia water, and the mixed solution is stirred and then dried to form an oxide of Si (silica) on the surface of the raw material powder (soft magnetic metal particles). The oxide of Si thus generated may be amorphous. This allows the oxide of Si that is not derived from the Si element contained in the raw material powder to adhere to the surface of the soft magnetic metal particles. The second oxide regions 42a and 42b may be composed of silica formed on the surface of the soft magnetic metal particles. When the oxide of Si contained in the insulating film covering the surface of the soft magnetic metal particles is not derived from an element contained in the raw material powder, the raw material powder does not need to contain Si.

[0061] When the Al oxide or Si oxide contained in the insulating film covering the surface of the soft magnetic metal particles is not derived from the Al or Si contained in the raw material powder, the content ratio of Al or Si in the raw material powder can be reduced. When the Al oxide contained in the insulating film is not derived from the Al contained in the raw material powder, the content ratio of Al in the raw material powder can be 0.1 to 0.8 wt%. When the Si oxide contained in the insulating film is not derived from the Si contained in the raw material powder, the content ratio of Si in the raw material powder can be 0.7 to 2.5 wt%. By reducing the content ratio of Al or Si in the raw material powder, the content ratio of Fe in the raw material powder can be increased, and as a result, the content ratio of Fe in the soft magnetic metal particles can also be increased.

[0062] Next, with reference to FIG. 5, another embodiment of the substrate to which the present invention is applied will be described. FIG. 5 is an enlarged cross-sectional view that typically shows a partial region of a cross section of a magnetic substrate 110 according to another embodiment. The magnetic substrate 110 shown in FIG. 5 is different from the magnetic substrate 10 in that the insulating film includes a third oxide region mainly composed of an oxide of Cr. As shown in FIG. 5, in the magnetic substrate 110, the first insulating film 40a covering the first soft magnetic metal grains 30a has a third oxide region 43a in addition to the first oxide region 41a and the second oxide region 42a, and the second insulating film 40b covering the second soft magnetic metal grains 30b has a third oxide region 43b in addition to the first oxide region 41b and the second oxide region 42b. The first insulating film 40a may include a plurality of third oxide regions 43a that are spaced apart from each other. The second insulating film 40b may include a plurality of third oxide regions 43b that are spaced apart from each other.

[0063] The third oxide region 43a is formed at a position spaced apart from the surface of the first soft magnetic metal particle 30a. In other words, at least one of the first oxide region 41a and the second oxide region 42a is interposed between the third oxide region 43a and the surface of the first soft magnetic metal particle 30a. In the illustrated embodiment, the third oxide region 43a is also disposed at a position spaced apart from the second oxide region 42a. In other words, the first oxide region 41a is interposed between the third oxide region 43a and the second oxide region 42a. The third oxide region 43a may be formed so as to be in contact with the second oxide region 42a.

[0064] The third oxide region 43a is provided radially outward of the first soft magnetic metal particle 30a relative to the first oxide region 41a. In one embodiment, at least one of the multiple third oxide regions 43a may be provided in a position corresponding to the first surface region 31a in the circumferential direction around the first soft magnetic metal particle 30a. In other words, at least one of the multiple third oxide regions 43a may be provided radially outward of the first surface region 31a. The first oxide region 41a is provided in a region corresponding to the first surface region 31a in the circumferential direction of the first soft magnetic metal particle 30a, and the second oxide region 42a is not provided. On the other hand, the second oxide region 42a is provided in a region corresponding to the second surface region 32a in the circumferential direction of the first soft magnetic metal particle 30a, and the first oxide region 41a is provided radially outward. Therefore, the first oxide region 41a is recessed toward the inside at a position corresponding to the first surface region 31a in the circumferential direction of the first soft magnetic metal particle 30a. In one embodiment, the third oxide region 43a is disposed in a recess of the first oxide region 41a at a position corresponding to the first surface region 31a in the circumferential direction of the first soft magnetic metal particle 30a. By disposing the third oxide region 43a in the recess of the first oxide region 41a, the thickness of the first insulating film 40a can be made uniform in the circumferential direction. If a part of the first insulating film 40a is thinner than other parts, there is a possibility that dielectric breakdown will occur from the part with the thinner thickness. By making the thickness of the first insulating film 40a uniform in the circumferential direction, dielectric breakdown can be prevented from occurring from the part with the thinner thickness of the first insulating film 40a.

[0065] Similar to the third oxide region 43a, the third oxide region 43b is formed at a position spaced apart from the surface of the second soft magnetic metal particle 30b. The third oxide region 43b may be disposed at a position spaced apart from the second oxide region 42b. The third oxide region 43b may be formed so as to be in contact with the second oxide region 42b. Furthermore, the third oxide region 43b may be disposed in a recess in the first oxide region 41b at a position corresponding to the first surface region 31b in the circumferential direction of the second soft magnetic metal particle 30b.

[0066] The third oxide regions 43a and 43c are mainly composed of an oxide of Cr. 2 O 4 When an oxide containing Fe is formed on the insulating film covering the Fe-based soft magnetic metal particles, the Fe oxide is hematite (Fe 2 O 3 ) and magnetite (Fe 3 O 4 ) When nonmagnetic hematite and ferromagnetic magnetite are mixed between soft magnetic metal particles, local magnetic saturation is likely to occur in the region where magnetite is present. By making the main component of the third oxide region 43a containing Fe nonmagnetic chromite, the uniformity of the magnetic flux between the soft magnetic metal particles can be improved, and as a result, the occurrence of local magnetic saturation between the soft magnetic metal particles can be suppressed. As a result, the magnetic base 110 has improved magnetic saturation characteristics compared to a magnetic base containing a large amount of magnetite.

[0067] The third oxide regions 43a to 43c contained in the insulating film are made of chromite (FeCr 2 O 4 ), Hematite (Fe 2 O 3 ), and magnetite (Fe 3 O 4) may be included. In one embodiment, in each of the third oxide regions 43a to 43c, the content ratio of chromite in the total of the oxides (the total of chromite, hematite, and magnetite) may be 50% or more. By making the content ratio of nonmagnetic chromite 50% or more, the relative permeability of the insulating film can be reduced compared to when a large amount of ferromagnetic oxides (for example, magnetite) is included, and the magnetic saturation characteristics of the magnetic base 110 can be improved. In another embodiment, the sum of the content ratio of chromite and the content ratio of hematite in the total of the oxides may be 80% or more. By making the sum of the content ratio of nonmagnetic chromite and hematite 80% or more, the relative permeability of the insulating film can be reduced compared to when a large amount of ferromagnetic oxides (for example, magnetite) is included, and the magnetic saturation characteristics of the magnetic base 110 can be improved.

[0068] Next, with reference to FIG. 6, the magnetic substrate 210 to which the present invention is applied will be described. FIG. 6 is an enlarged cross-sectional view that shows a schematic enlargement of a part of the cross-section of the magnetic substrate 210. The cross-section of the magnetic substrate 210 shown in FIG. 6 shows an enlarged view of the vicinity of the boundary between three soft magnetic metal particles. As shown in the figure, the magnetic substrate 210 has a first soft magnetic metal particle 30a, a second soft magnetic metal particle 30b, and a third soft magnetic metal particle 30c. The first soft magnetic metal particle 30a, the second soft magnetic metal particle 30b, and the third soft magnetic metal particle 30c are arranged adjacent to each other. As described above, the first soft magnetic metal particle 30a is covered by the first insulating film 40a, and the second soft magnetic metal particle 30b is covered by the second insulating film 40b. Similarly, the third soft magnetic metal particle 30c is covered by the third insulating film 40c. The third insulating film 40c is configured in the same manner as the first insulating film 40a and the second insulating film 40b. That is, the third insulating film 40c includes a first oxide region 41c that covers the first surface region 31c that is a part of the surface of the third soft magnetic metal particle 30c and contains an oxide of Al as a main component, a second oxide region 42c that covers the second surface region 32c that is a part of the surface of the third soft magnetic metal particle 30c and contains an oxide of Si as a main component, and a third oxide region 43c that is disposed apart from the surface of the third soft magnetic metal particle 30c and contains an oxide of Cr as a main component. The main component of the third oxide region 43c may be chromite, similar to the third oxide regions 43a and 43b.

[0069] In the magnetic base 210, there are gaps between the soft magnetic metal particles that are not filled with an insulating film. For example, as shown in FIG. 6, in the magnetic base 210, there are gaps G1 between the first soft magnetic metal particle 30a, the second soft magnetic metal particle 30b, and the third soft magnetic metal particle 30c. At least a part of the gap G1 is defined by the third oxide region 43d that is mainly composed of an oxide of Cr. In other words, the third oxide region 43d is disposed at a position facing the gap between the soft magnetic metal particles. The main component of the third oxide region 43d may be chromite, similar to the third oxide regions 43a to 43c. In the illustrated example, the gap G1 is defined by the third oxide region 43d and the first oxide regions 41a to 41c.

[0070] In the magnetic base 210, some of the gaps existing between the soft magnetic metal particles are filled with the third oxide region 43d, so that the mechanical strength of the magnetic base 210 can be improved compared to the case where the third oxide region 43d does not exist. When the main component of the third oxide region 43d is chromite, some of the gaps are filled with the third oxide region 43d mainly composed of chromite having high hardness, so that the mechanical strength of the magnetic base 210 can be further improved.

[0071] The first insulating film 40a may further include a fourth oxide region in addition to the first oxide region 41a, the second oxide region 42a, and the third oxide region 43a. The fourth oxide region may include an oxide derived from an element contained in the raw material powder of the soft magnetic metal particles, or may include an oxide other than the above. The fourth oxide region may be insulating.

[0072] Next, an example of a method for manufacturing the coil component 1 will be described with reference to FIG. 7. Since the magnetic base 10 is produced in the process of manufacturing the coil component 1, the method for manufacturing the magnetic base 10 will also be described with reference to FIG. 7. When the raw material powder contains Cr, a magnetic base 110 or a magnetic base 210 containing an oxide of Cr is produced in place of the magnetic base 10 in the process of FIG. 7. FIG. 7 is a flow diagram showing a method for manufacturing the coil component 1 according to an embodiment of the present invention. In the following description, it is assumed that the coil component 1 is manufactured by a sheet lamination method. The coil component 1 may be manufactured by a known method other than the sheet lamination method. For example, the coil component 1 can be manufactured by a lamination method such as a print lamination method, a thin film process method, or a slurry build method.

[0073] First, in step S1, a magnetic sheet is produced. The magnetic sheet is produced from a magnetic material paste obtained by kneading soft magnetic metal powder (raw material powder), which is the raw material of soft magnetic metal particles, with a binder resin and a solvent. This raw material powder is made of a soft magnetic metal material. The raw material powder contains Fe, Al, and Si. The raw material powder may contain Cr. The raw material powder contains 95 wt% or more of Fe. The total content ratio of Al, Si, Cr, and other additive elements is 5 wt% or less. The raw material powder may contain 0.2 to 1 wt% of Al. The raw material powder may contain 1 to 4 wt% of Si. The raw material powder may contain 0.5 to 1 wt% of Cr. The content of Si in the raw material powder may be higher than the content of Al. The grain size of the raw material powder is 10 μm or less. The grain size of the raw material powder is 5 μm or less. By setting the particle size of the raw material powder to 10 μm or less, preferably 5 μm or less, the raw material powder can be densely packed in a compact containing the raw material powder, and the heat treatment can be stably carried out.

[0074] The binder resin for the magnetic material paste is, for example, an acrylic resin. The binder resin for the magnetic material paste may be a PVB resin, a phenol resin, a resin known as a binder resin other than the above, or a mixture thereof. The solvent is, for example, toluene. This magnetic material paste is applied to the surface of a plastic base film by a doctor blade method or other general method. A sheet-shaped molded body is obtained by drying the magnetic material paste applied to the surface of the base film. A plurality of magnetic sheets are produced by pressurizing and molding this sheet-shaped molded body in a mold at a molding pressure of about 10 to 100 MPa.

[0075] Next, in step S2, a conductive paste is applied to some of the magnetic sheets prepared in step S1. The conductive paste is produced by kneading a conductive powder made of a conductive material with excellent conductivity, such as Ag, Pd, Cu, Al, or an alloy thereof, with a binder resin and a solvent. The binder resin for the conductive paste may be the same type of resin as the binder resin for the magnetic material paste. Both the binder resin for the conductive paste and the binder resin for the magnetic material paste may be acrylic resin.

[0076] By applying a conductive paste to the magnetic sheet, an unfired conductive pattern that will become the conductive patterns C11 to C17 after firing is formed on the magnetic sheet. Through holes penetrating in the stacking direction are formed in parts of the magnetic sheet. When the conductive paste is applied to a magnetic sheet having through holes, the conductive paste is also embedded in the through holes. In this way, unfired vias that will become the vias V1 to V5 after firing are formed in the through holes of the magnetic sheet. The conductive paste is applied to the magnetic sheet by, for example, a screen printing method.

[0077] Next, in step S3, the magnetic sheets prepared in step S1 are laminated to prepare an upper laminate which becomes the upper cover layer 18, an intermediate laminate which becomes the main layer 20, and a lower laminate which becomes the lower cover layer 19. The upper laminate and the lower laminate are each formed by laminating four of the magnetic sheets prepared in step S1 on which no unsintered conductor pattern is formed. The four magnetic sheets of the upper laminate become the magnetic films 18a to 18d in the finished coil component 1, and the four magnetic sheets of the lower laminate become the magnetic films 19a to 19d in the finished coil component 1. The intermediate laminate is formed by laminating seven magnetic sheets on which an unsintered conductor pattern is formed in a predetermined order. The seven magnetic sheets of the intermediate laminate become the magnetic films 11 to 17 in the finished coil component 1. The intermediate laminate prepared as described above is sandwiched between the upper laminate and the lower laminate from above and below, and the upper laminate and the lower laminate are thermocompressed to the intermediate laminate to obtain a main laminate. Next, the main body laminate is divided into pieces of a desired size using a cutting machine such as a dicing machine or a laser processing machine to obtain a chip laminate. The chip laminate is an example of a molded body including an element that becomes the magnetic base 10 after heat treatment and an unsintered conductor pattern that becomes the coil conductor 25 after heat treatment. The element that becomes the magnetic base 10 after heat treatment and the molded body including the unsintered conductor pattern that becomes the coil conductor 25 after heat treatment may be produced by a method other than the sheet lamination method.

[0078] In the green body produced in step S3, the filling rate of the raw material powder is 85% or more. The filling rate of the raw material powder in the green body is realized by adjusting the molding pressure when molding the magnetic sheet according to the type of binder resin, the particle size of the raw material, and other parameters. In order to achieve a filling rate of 85% or more in the green body, it is desirable to set the molding pressure when molding the magnetic sheet to about 10 to 100 MPa. The filling rate of the raw material powder in the green body can be expressed as a percentage of the area occupied by the raw material powder to the total area of ​​the observation field in an SEM image of the cross section of the green body.

[0079] Next, in step S4, the molded body produced in step S3 is degreased. When a thermally decomposable resin is used as the binder resin for the magnetic material paste and the conductive paste, the molded body can be degreased in a non-oxygen atmosphere such as a nitrogen atmosphere. By performing the degreasing in a non-oxygen atmosphere, it is possible to prevent Fe contained in the raw material powder from being oxidized in the degreasing. The degreasing is performed at a temperature higher than the thermal decomposition start temperature of the binder resin for the magnetic material paste. When an acrylic resin is used as the binder resin for the magnetic material paste, the degreasing is performed at a temperature higher than the thermal decomposition start temperature of the acrylic resin, for example, 300°C to 500°C. The thermally decomposable resin contained in the molded body is decomposed by the degreasing, so that no thermally decomposable resin remains in the molded body after the degreasing is completed. By using the same thermally decomposable resin as the binder resin for the magnetic material paste for the binder resin for the conductive paste, the thermally decomposable resin contained in the unsintered conductor pattern is also thermally decomposed in the degreasing in step S4. In this manner, in step S4, both the magnetic sheets and the unsintered conductor patterns constituting the compact are degreased.

[0080] Next, in step S5, the degreased compact is subjected to a first heating treatment. The first heating treatment is performed at a first heating temperature of 590°C to 900°C in a low oxygen concentration atmosphere containing oxygen in the range of 5 to 1000 ppm. The first heating treatment may be performed in a low oxygen concentration atmosphere of about 5 to 100 ppm. By heating the raw material powder at 590°C to 900°C, Al and Si in each raw material powder are diffused to the surface vicinity by thermal diffusion and bonded with oxygen in the atmosphere. If the raw material powder contains Cr, Cr also diffuses to the surface vicinity of the raw material powder. In the first heating treatment, oxides of Al and Si, which are easily oxidized among the additive elements that have moved to the surface of each raw material powder, are generated. By the first heating treatment, an oxide region mainly composed of an oxide of Al (for example, the first oxide region 41a) and an oxide region mainly composed of an oxide of Si (for example, the second oxide region 42a) are formed on the surface of the heated raw material powder, as shown in Figs. 4 to 6. The first heating time for the first heat treatment can be between 1 hour and 6 hours. The first heating time can be, for example, 1 hour. In the first heat treatment, Fe, which is less easily oxidized than Al and Si, may also be slightly oxidized. Since the first heat treatment is performed in an atmosphere with a low oxygen concentration, when Fe is oxidized, hematite (Fe 2 O 3 ) compared to magnetite (Fe 3 O 4 In the first heat treatment, oxides of Fe are generated radially outward from the first oxide region 41a and the second oxide region 42a.

[0081] Since the first heat treatment is carried out at a high temperature of 590° C. or more, the first heat treatment can alleviate distortion that occurs in the molded body during pressure molding when producing the magnetic sheet.

[0082] Next, in step S6, the compact after being heated in the first heat treatment is subjected to a second heat treatment in an oxygen concentration higher than that in the first heat treatment. The second heat treatment may be performed in a low oxygen atmosphere of more than 1000 ppm and not more than 10000 ppm. Since the second heat treatment is performed in an oxygen concentration higher than that in the first heat treatment, the oxidation of Si and Al proceeds further. When the raw material powder contains Cr, the magnetite generated in the first heat treatment combines with Cr during the second heat treatment to form chromite (FeCr 2 O 4 As described above, the filling rate of the raw material powder in the compact is high at 85% or more, so that the supply of excess oxygen to the surface of the raw material powder is suppressed. Therefore, in the second heat treatment, in the region where magnetite and Cr element are present near the surface of the raw material powder, hematite (Fe 2 O 3 ) and chromium(III) oxide, 2 O 4 ) is likely to be generated.

[0083] In this way, when the raw material powder contains Cr, an oxide region mainly composed of chromite (e.g., the third oxide region 43a) is generated radially outside the first oxide region 41a or the second oxide region 42a by the second heat treatment. When the raw material powder does not contain Cr, chromite is not generated. In addition, by increasing the filling rate of the raw material powder in the compact (e.g., to 85% or more), the amount of oxygen supplied to the raw material powder surface can be restricted, and the range of oxygen concentration in the atmosphere in which the second heat treatment is performed can be expanded (the upper limit can be increased).

[0084] In the second heat treatment, in addition to the oxidation of the raw material powder, the conductor powder in the unsintered conductor pattern is also sintered. The conductor powder in the unsintered conductor pattern is sintered to obtain the coil conductor 25. When copper powder is used as the conductor powder, the copper crystals are densely sintered to become the coil conductor 25.

[0085] The second heating process is performed at the second heating temperature for the second heating time. The second heating temperature and the second heating time are determined so that an insulating film having a sufficient thickness to ensure insulation is formed on the surface of the raw material powder. The second heating temperature can be, for example, between 550°C and 900°C. The higher the second heating temperature, the faster the oxidation progresses, so the second heating time varies depending on the second heating temperature. When the second heating temperature is 550°C, the second heating time can be between 1 hour and 6 hours. When the second heating temperature is 700°C, the second heating time can be between 30 minutes and 1 hour.

[0086] In this way, the raw material powder contained in the compact is oxidized by the first heat treatment and the second heat treatment, and the raw material powder is used to generate soft magnetic metal particles whose surfaces are covered with an insulating film. When the raw material powder does not contain Cr, the first soft magnetic metal particles 30a covered with the first insulating film 40a and the second soft magnetic metal particles 30b covered with the second insulating film 40b are generated, as shown in FIG. 4, for example. When the raw material powder contains Cr, the first insulating film 40a is generated to include the third oxide region 43a mainly composed of chromite, and the second insulating film 40b is generated to include the third oxide region 43b mainly composed of chromite, as shown in FIG. 5 or FIG. 6. The second heat treatment bonds adjacent soft magnetic metal particles together via the insulating film formed on their surfaces. In this way, the magnetic base 10, 110, or 210 to which the soft magnetic metal particles are bonded is obtained.

[0087] Next, in step S7, the external electrodes 21 and 22 are formed on the surface of the magnetic base 10 obtained in step S6. The external electrode 21 is connected to one end of the coil conductor 25, and the external electrode 22 is connected to the other end of the coil conductor 25. Before forming the external electrodes 21 and 22, the molded body after the second heat treatment may be impregnated with a resin. The molded body is impregnated with a thermosetting resin such as an epoxy resin. This allows the resin to permeate into the gaps between the soft magnetic metal particles in the magnetic base 10. Then, by hardening the resin impregnated in the magnetic base 10, the mechanical strength of the magnetic base 10 can be improved.

[0088] Through the above steps, the coil component 1 is manufactured.

[0089] Next, another embodiment of the method for manufacturing the coil device 1 will be described with reference to Fig. 8. The manufacturing method shown in Fig. 8 differs from the manufacturing method shown in Fig. 7 in that the raw material powder is preheated before the magnetic sheet is produced, and an oxide of Si is generated on the surface of the raw material powder by this preheating.

[0090] As shown in Fig. 8, first, in step S21, raw material powder that is the raw material of soft magnetic metal particles is prepared, and the raw material powder is preheated. The preheating is performed at a temperature lower than 500°C for 1 hour. This preheating causes Si oxide to be discretely generated on the surface of the raw material powder. Using this raw material powder on whose surface the Si oxide is discretely formed, steps S1 to S3 are performed as in Fig. 7, and a compact in which magnetic sheets are laminated is produced. In step S4, this compact is degreased.

[0091] Next, in step S22, the degreased compact is subjected to a heat treatment. The heat treatment in step S22 is performed under the same conditions as the second heat treatment in step S6 in FIG. 7. This second heat treatment oxidizes Al in the raw material powder contained in the compact to generate an oxide of Al, and soft magnetic metal particles having surfaces covered with an insulating film are generated from the raw material powder. The heat treatment in step S22 bonds adjacent soft magnetic metal particles to each other via the insulating film formed on their surfaces. In this manner, a magnetic base 10 in which soft magnetic metal particles are bonded is obtained.

[0092] Next, in step S7, the external electrodes 21 and 22 are formed on the surface of the magnetic base 10 obtained in step S22. Through the above steps, the coil component 1 is manufactured. EXAMPLES

[0093] According to the above steps S1 and S3 to S6, the composition of the raw material powder, the first heating temperature, and the second heating temperature were changed to produce the following 16 types of samples.

[0094] Samples 1 to 10 were prepared as follows. First, soft magnetic metal powder (raw material powder) with an average particle size of 10 μm was prepared. The composition ratio of the soft magnetic metal powder expressed on a mass basis was Fe: 95 wt%, Si: 4 wt%, and Al: 1%. This raw material powder was kneaded with acrylic resin and toluene (solvent) to obtain a magnetic material paste. This magnetic material paste was applied to the surface of a plastic base film, and the applied magnetic material paste was dried to obtain a sheet-shaped molded body. Next, this sheet-shaped molded body was pressurized and molded at a molding pressure of about 50 MPa to produce a magnetic sheet. Next, only 10 layers of this magnetic sheet were stacked to produce a sheet-shaped laminate. This sheet-shaped laminate was diced to produce a chip-shaped element with a length of 1.6 mm, a width of 0.8 mm, and a height of 0.5 mm. Next, a degreasing process was performed on this chip-shaped element. In the degreasing process, the chip-shaped element was heated at 400° C. for 30 minutes in a nitrogen atmosphere. Next, the degreased compact was subjected to a heat treatment (first heat treatment) for 3 hours in a 10 ppm low oxygen atmosphere at the first heating temperature shown in Table 1. Next, the laminate after the first heat treatment was subjected to a heat treatment (second heat treatment) for 1 hour in a 5000 ppm low oxygen atmosphere at the first heating temperature shown in Table 1. In this manner, Samples 1 to 10 were obtained.

[0095] Next, Samples 11 to 13 were prepared as follows. First, soft magnetic metal powder (raw material powder) with an average particle size of 10 μm was prepared. The composition ratio of the soft magnetic metal powder expressed on a mass basis was Fe: 95 wt%, Si: 3.5 wt%, Al: 0.5%, and Cr: 1%. Using this raw material powder, a laminate was prepared in the same manner as Samples 1 to 10, and the laminate was subjected to a degreasing treatment, a first heating treatment, and a second heating treatment in this order to obtain Samples 11 to 13. The first heating treatment was performed at the first heating temperature shown in Table 1, and the second heating treatment was performed at the second heating temperature shown in Table 1.

[0096] Samples 14 to 16 were prepared as follows. First, soft magnetic metal powder and magnesium oxide powder having the same composition as the raw powder used to prepare Samples 1 to 10 were mixed in a friction mixer to adhere the magnesium oxide powder to the surface of the soft magnetic metal powder, thereby obtaining a raw material. Using this raw powder (raw powder having magnesium oxide powder adhered to the surface of the soft magnetic metal powder), a laminate was prepared in the same manner as Samples 1 to 10, and the laminate was subjected to a degreasing treatment, a first heating treatment, and a second heating treatment in this order to obtain Samples 14 to 16. The first heating treatment was performed at the first heating temperature shown in Table 1, and the second heating treatment was performed at the second heating temperature shown in Table 1.

[0097] Next, the filling ratios of Samples 1 to 16 were measured as follows. First, each sample was cut to expose the cross section, and an SEM image of the cross section was taken at a magnification of 10,000 times using a scanning electron microscope (SEM). The area where the soft magnetic metal particles existed was identified from the brightness difference in the SEM image, and the area of ​​the area where the soft magnetic metal particles existed was measured. Then, the ratio of the area of ​​the area where the soft magnetic metal particles existed to the total area of ​​the observation field was calculated, and the value expressed as a percentage of this calculated ratio was taken as the filling ratio. The filling ratio calculated in this way was entered in the "filling ratio" column of Table 1.

[0098] Next, the KAM values ​​of Samples 1 to 16 were measured as follows. First, each sample was cut to expose the cross section, and the cross section was polished. EBSD measurement was performed on the polished cross section of the magnetic substrate using an SEM equipped with an EBSD detector under conditions of an acceleration voltage of 15 kV, a magnification of 10,000 times, and a step size of 0.05 μm, and an IQ map showing the distribution of Image Quality (IQ value) in the observation field was obtained. In this IQ map, the area with an IQ value of 15% or more was identified as the area where soft magnetic metal particles exist. For the area where soft magnetic metal particles exist identified in this way, the average value of the KAM value was calculated from the EESD pattern using data analysis software (OIM Analyasis ver.8.5). The average value of the KAM value calculated in this way is listed in the "KAM value" column of Table 1.

[0099] Next, Samples 1 to 16 were set in a Lake Share 8600 SERIES VSM, and the coercive force of Samples 1 to 16 was measured at a maximum magnetic field of 5 kOe. The coercive forces thus measured are shown in the "Coercive force" column of Table 1.

[0100] [Table 1]

[0101] In Table 1, samples not included in the present invention (i.e., comparative examples) are marked with an asterisk (*) next to the sample number. Specifically, samples 12 to 19 are comparative examples not included in the present invention.

[0102] As shown in Table 1, the filling rate of each sample was 85% or more. As shown in Table 1, the KAM value of Samples 1 to 5, which were subjected to the first heating treatment at a first heating temperature of 570°C or less, was 0.7 or more, while the KAM value of Samples 6 to 16, which were subjected to the first heating treatment at a first heating temperature of 590°C or more, was 0.6 or less. It was confirmed that the distortion during compression molding was alleviated and a KAM value of 0.6 or less was obtained by performing the first heating treatment at 590°C or more. In addition, it was confirmed that the coercive force of Samples 6 to 16, which had a KAM value of 0.6 or less, was 730 or less, which was smaller than that of Samples 1 to 5. Therefore, the magnetic loss (hysteresis loss) can be reduced in Samples 6 to 16.

[0103] The volume resistivity of Samples 6 to 16 was measured in accordance with JIS-K6911. Specifically, an Au film was formed on two opposing surfaces of each sample, and the Au film was used as an electrode. A voltage was applied between the electrodes so that the electric field strength was 60 V / cm, and the resistance value was measured, and the volume resistivity was calculated from the resistance value. 5 The samples 6 to 7 and 9 to 16 had a high volume resistivity of 10 7It was confirmed that the material had a particularly high volume resistivity of more than Ω·cm. For comparison, the volume resistivity of a magnetic substrate prepared in the same manner as sample 6 using raw material powder (Fe: 94 wt%, Si: 6 wt%) that did not contain Al was measured. 2 From this result, it was found that by including Al, which is easily oxidized, in the raw powder, a magnetic base with high insulating properties can be obtained by covering the surfaces of the soft magnetic metal particles with Al oxide, even if the amount of oxygen supplied to the raw powder surface is reduced by increasing the packing rate of the soft magnetic metal particles.

[0104] In the embodiment described herein, the soft magnetic metal particles contained in the magnetic substrate 10 contain 95 wt% or more of Fe, and the high concentration of Fe contained in the soft magnetic metal particles results in a magnetic substrate 10 that exhibits high magnetic permeability and DC bias characteristics. In addition, the filling rate of the soft magnetic metal particles in the magnetic substrate 10 is 85% or more, and therefore the magnetic substrate 10 has high magnetic permeability. Thus, the magnetic substrate 10 has excellent magnetic properties.

[0105] In the magnetic base 10 according to the embodiment described in this specification, the filling rate of the soft magnetic metal particles is 85% or more, so that the amount of oxygen supplied to the surface of the raw material powder is limited when the raw material powder is heated. Therefore, oxidation of Fe contained in the raw material powder is suppressed during the manufacturing process, so that the soft magnetic metal particles contained in the magnetic base 10 can contain Fe at 95 wt% or more.

[0106] In addition, since the raw material powder of the soft magnetic metal particles contains Al, even if the amount of oxygen supplied to the surface of the raw material powder is small, the surface of the soft magnetic metal particles can be covered with an insulating oxide film mainly composed of Al oxide, so that the magnetic base 10 has excellent insulating properties.

[0107] As described above, according to the embodiment described in this specification, a magnetic base 10 having excellent insulating properties and magnetic properties can be obtained. The above explanation also applies to the magnetic base 110 and the magnetic base 210.

[0108] The dimensions, materials, and arrangements of each component described in the various embodiments above are not limited to those explicitly described in each embodiment, and each component can be modified to have any dimensions, materials, and arrangements that may fall within the scope of the present invention.

[0109] Components not explicitly described in this specification may be added to each of the above-described embodiments, and some of the components described in each embodiment may be omitted.

[0110] The designations "first," "second," "third," and the like in this specification are given to identify components, and do not necessarily limit the number, order, or content. Furthermore, numbers for identifying components are used in different contexts, and a number used in one context does not necessarily indicate the same configuration in another context. Furthermore, a component identified by a certain number does not prevent the component from also having the function of a component identified by another number.

[0111] This specification also discloses the following techniques: [Appendix 1] A plurality of soft magnetic metal particles, which are filled at a filling rate of 85% or more, have a KAM value of 0.6 or less, and contain 95 wt% or more of Fe, Si, and Al; a plurality of insulating films covering the surfaces of the soft magnetic metal particles and containing an oxide of Si and an oxide of Al; A magnetic substrate comprising: [Appendix 2] The soft magnetic metal particles contain Mg. The magnetic substrate according to [Appendix 1]. [Appendix 3] The soft magnetic metal particles contain Cr, The insulating film contains chromite. The magnetic substrate according to [Appendix 1] or [Appendix 2]. [Appendix 4] The filling rate of the soft magnetic metal particles is 86% or less. The magnetic substrate according to any one of [Appendix 1] to [Appendix 3]. [Appendix 5] A magnetic substrate according to any one of [Appendix 1] to [Appendix 4], A coil conductor provided on the magnetic base; A coil component comprising: [Appendix 6] A circuit board including the coil component according to [Appendix 5]. [Appendix 7] An electronic component comprising the circuit board described in [Appendix 6]. [Appendix 8] A forming step of obtaining a compact containing a plurality of soft magnetic metal powders containing 95 wt % or more of Fe, Si, and Al at a filling rate of 85% or more; a first heating step of heating the compact at 590 to 900° C. in a first oxygen concentration of 5 to 10 ppm; a second heating step of heating the compact heated in the first heating step at 550 to 900° C. in a first oxygen concentration of 5 to 10 ppm; A method for manufacturing a magnetic substrate comprising the steps of: [Explanation of symbols]

[0112] 1 Coil parts 10, 110, 210 magnetic substrate 21, 22 External electrode 30a First soft magnetic metal particle 30b Second soft magnetic metal particle 30c 3rd soft magnetic metal particle 40a, 40b, 40c insulating film 41a, 41b, 41c first oxide region 42a, 42b, 42c second oxide region 43a, 43b, 43c, 43d 3rd oxide region

Claims

1. A plurality of soft magnetic metal particles, which are filled at a filling rate of 85% or more, have a KAM value of 0.6 or less, and contain 95 wt% or more of Fe, Si, and Al; a plurality of insulating films covering the surfaces of the soft magnetic metal particles, the insulating films containing an oxide of Si and an oxide of Al; A magnetic substrate comprising:

2. The soft magnetic metal particles contain Mg. The magnetic substrate according to claim 1 .

3. The soft magnetic metal particles contain Cr, The insulating film contains chromite.

3. The magnetic substrate according to claim 1 or 2.

4. The filling rate of the soft magnetic metal particles is 87% or less.

3. The magnetic substrate according to claim 1 or 2.

5. The magnetic substrate according to claim 1 or 2, A coil conductor provided on the magnetic base; A coil component comprising:

6. A circuit board comprising the coil component according to claim 5 .

7. An electronic component comprising the circuit board according to claim 6.

8. A forming step of obtaining a compact containing a plurality of raw material powders containing Fe, Si, and Al or Mg at a filling rate of 85% or more; A first heating step of heating the molded body at 590 to 900° C. in a first oxygen concentration of 1000 ppm or less; a second heating step of heating the molded body heated in the first heating step at a second oxygen concentration higher than the first oxygen concentration and not more than 10,000 ppm at a temperature of 550 to 900° C.; A method for manufacturing a magnetic substrate comprising the steps of:

Citation Information

Patent Citations

  • Method for producing composite magnetic body, magnetic powder, composite magnetic body and coil component

    WO2018180659A1