Manufacturing method of active material composite particles, and manufacturing method of secondary battery
The production of active material composite particles with voids formed by removing a second component from a granule containing elemental Si and a polymer enhances the cycle characteristics of Si-based active materials.
Patent Information
- Application Number
- JP2023058139
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Active materials containing Si have room for improvement in cycle characteristics.
A method for producing active material composite particles by obtaining a granule containing elemental Si as a first component, a component other than elemental Si as a second component, and a polymer, followed by acid treatment to remove the second component while leaving the first component and polymer, forming voids in the granule.
The active material composite particles exhibit excellent cycle characteristics due to the formation of voids that absorb the expansion of Si during charging, reducing the overall volume change and improving the cycle performance of the negative electrode.
Smart Images

Figure 2024145684000001_ABST
Abstract
Description
[Technical field]
[0001] The present application discloses a method for producing active material composite particles and a method for producing a secondary battery. [Background technology]
[0002] Patent Document 1 discloses a granulated negative electrode active material that contains a composite of Si and carbon and a binder. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-021571 A Summary of the Invention [Problem to be solved by the invention]
[0004] There is room for improvement in the cycle characteristics of active materials containing Si. [Means for solving the problem]
[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A method for producing active material composite particles, comprising the steps of: Obtaining a granule containing elemental Si as a first component, a component other than elemental Si as a second component, and a polymer; and and subjecting the granules to an acid treatment to remove the second component from the granules while leaving the first component and the polymer in the granules, thereby forming voids in the granules. A method for producing active material composite particles. <Aspect 2> The method for producing aspect 1, The second component is SiO 2 That is, Manufacturing method. <Aspect 3> The method for producing aspect 1 or 2, The acid treatment includes a hydrofluoric acid treatment. Manufacturing method. <Aspect 4> In any one of the production methods of the first to third aspects, The polymer comprises a fluorine-containing polymer. Manufacturing method. <Aspect 5> A method for manufacturing a secondary battery, comprising: Obtaining active material composite particles by a production method according to any one of aspects 1 to 4; and Obtaining a negative electrode active material layer using the active material composite particles. Manufacturing method. Effect of the Invention
[0006] The active material composite particles of the present disclosure have excellent cycle characteristics. [Brief description of the drawings]
[0007] [Figure 1] 1 shows an example of a flow of a method for producing active material composite particles. [Diagram 2] 1A and 1B are schematic diagrams showing the states of granules before and after the acid treatment, respectively. [Diagram 3] 1 illustrates an example of a flow of a method for manufacturing a secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] 1. Manufacturing method of active material composite particles A method for producing an active material composite particle 1 according to an embodiment will be described with reference to Figs. 1 and 2. As shown in Figs. 1 and 2, the method for producing an active material composite particle 1 according to an embodiment includes the following steps: Step S1: Obtaining a granule 1a containing a first component 1ax (simple substance Si), a second component 1ay (a component other than simple substance Si), and a polymer 1az; and Step S2: The granules 1a are subjected to an acid treatment to remove the second component 1ay from the granules 1a while leaving the first component 1ax and the polymer 1az in the granules 1a, thereby forming voids 1b in the granules 1a.
[0009] 1.1 Process S1 In step S1, a granule 1a is obtained, which contains a first component 1ax (simple substance Si), a second component 1ay (a component other than simple substance Si), and a polymer 1az.
[0010] 1.1.1 First component The first component 1ax is an elemental Si. The elemental Si as the first component 1ax is less likely to be removed by the acid treatment described below compared to the second component 1ay, and is likely to remain in the granule 1a even after the acid treatment. The elemental Si as the first component 1ax may be present as particles, for example. That is, in step S1, particles containing elemental Si as the first component 1ax (Si particles) may be used.
[0011] The Si particles may exist as primary particles or secondary particles. The chemical composition of the Si particles is not particularly limited. The ratio of the Si element to all elements contained in the Si particles may be, for example, 50 mol% or more, 70 mol% or more, or 90 mol% or more. The Si particles may contain other elements such as alkali metal elements such as Li element in addition to the Si element. Examples of the other elements include alkali metal elements such as Li element, Sn element, Fe element, Co element, Ni element, Ti element, Cr element, B element, P element, etc. In addition, the Si particles may contain impurities such as oxides. The simple Si contained in the Si particles may be amorphous Si or crystalline Si. The crystal phase contained in the Si particles is not particularly limited.
[0012] The size of the Si particles is not particularly limited. The average primary particle diameter of the Si particles may be, for example, 10 nm or more, 30 nm or more, 50 nm or more, 100 nm or more, or 150 nm or more, and may be 10 μm or less, 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. The average secondary particle diameter of the Si particles may be, for example, 100 nm or more, 1 μm or more, or 2 μm or more, and may be 20 μm or less, 15 μm or less, or 10 μm or less. The average primary particle diameter and the average secondary particle diameter can be obtained by observation with an electron microscope such as SEM, and are obtained, for example, as the number average value of the maximum Feret diameter of each of a plurality of particles. The number of samples depends on the number of Si particles contained in the granule 1a, but is preferably large. The number of samples may be, for example, 1 or more, 2 or more, 5 or more, 20 or more, 50 or more, or 100 or more. The average primary particle size and the average secondary particle size can be appropriately adjusted, for example, by appropriately changing the production conditions of the Si particles or by carrying out a classification process.
[0013] The Si particles may be porous. By the Si particles being porous, the expansion of the Si particles during charging can be alleviated by the voids in the Si particles. There is no particular limitation on the form of the voids in the porous Si particles. The porous Si particles may be particles containing nanoporous silicon. Nanoporous silicon refers to silicon having a plurality of pores with a pore diameter of the nanometer order (less than 1000 nm, preferably 100 nm or less). The porous Si particles may contain pores with a diameter of 55 nm or less. Pores with a diameter of 55 nm or less are difficult to crush even by pressing. That is, porous Si particles containing pores with a diameter of 55 nm or less tend to maintain their porosity even after pressing. For example, the porous Si particles may contain pores with a diameter of 55 nm or less in an amount of 0.21 cc or more, 0.22 cc / g or more, or 0.23 cc / g or more, or 0.30 cc / g or less, 0.28 cc / g or less, or 0.26 cc / g or less per 1 g of the porous Si particles. The amount of pores with a diameter of 55 nm or less contained in the porous Si particles can be determined from the pore size distribution by, for example, a nitrogen gas adsorption method or a DFT method.
[0014] When the Si particles are porous, the porosity is not particularly limited. The porosity of the porous Si particles may be, for example, 1% or more, 5% or more, 10% or more, or 20% or more, and may be 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, or 30% or less. The porosity of the Si particles can be determined, for example, by observation using a scanning electron microscope (SEM). It is preferable to have a large number of samples, for example, 100 or more. The porosity can be an average value determined from these samples.
[0015] When the first component 1ax is contained as Si particles, the number of Si particles contained in one granule 1a is not particularly limited. The number may be 1 or more, 2 or more, 5 or more, 10 or more, or 50 or more, and may be 1000 or less, 500, or 100 or less.
[0016] 1.1.2 Second Component The second component 1ay is a component other than the simple substance Si. The second component 1ay is removed by an acid treatment described later. That is, the second component 1ay may be a component that dissolves in a predetermined acid. For example, the second component 1ay may be SiO 2 The second component 1ay may be SiO 2 In the case of SiO 2 , most of it can be easily removed from the granules 1a by the acid treatment described below. 2 Even if a part of the second component 1ay remains in the granule 1a, it is unlikely to adversely affect the electrochemical reaction (such as the intercalation and deintercalation reaction of carrier ions) as an active material. The second component 1ay may be present as particles, for example. That is, in step S1, particles (second particles) containing the second component 1ay may be used. For example, in step S1, SiO 2 Particles containing (SiO 2 particles) may be used.
[0017] The second particles may be present as primary particles or as secondary particles. The second particles may be, for example, SiO 2 as described above. 2It may be a particle. SiO 2 SiO in particles 2 The content may be, for example, 50% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, or 90% by mass or more and 100% by mass or less. 2 The particles are SiO 2 In addition, other elements, compounds, and impurities may be included.
[0018] The size of the second particles is not particularly limited. The average primary particle diameter of the second particles may be, for example, 10 nm or more, 30 nm or more, 50 nm or more, 100 nm or more, or 150 nm or more, and may be 10 μm or less, 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. The average secondary particle diameter of the second particles may be, for example, 100 nm or more, 1 μm or more, or 2 μm or more, and may be 20 μm or less, 15 μm or less, or 10 μm or less. The average primary particle diameter and the average secondary particle diameter can be obtained by observation with an electron microscope such as SEM, and are obtained, for example, as the number average value of the maximum Feret diameter of each of a plurality of particles. The number of samples depends on the number of second particles contained in the granule 1a, but is preferably large. The number of samples may be, for example, 1 or more, 2 or more, 5 or more, 20 or more, 50 or more, or 100 or more. The average primary particle size and the average secondary particle size can be appropriately adjusted, for example, by appropriately changing the production conditions of the secondary particles or by carrying out a classification process.
[0019] When the second component 1ay is contained as the second particles, the number of the second particles contained in one granule 1a is not particularly limited. The number may be 1 or more, 2 or more, 5 or more, 10 or more, or 50 or more, and may be 1000 or less, 500, or 100 or less.
[0020] 1.1.3 Polymers The polymer 1az may function as a binder for, for example, binding the above-mentioned first components 1ax together or maintaining the shape of the active material composite particles 1. The polymer 1az may also function as a cushioning material. The type of the polymer 1az is not particularly limited. As the polymer 1az, various binders known as constituent materials of secondary batteries may be adopted. For example, the polymer 1az may be at least one selected from butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, carboxymethyl cellulose (CMC)-based binders, polyacrylate-based binders, polyacrylic acid ester-based binders, and the like. In particular, when the polymer 1az contains a fluorine-containing polymer, particularly when it contains one or both of a polyvinylidene fluoride (PVdF)-based binder and a polytetrafluoroethylene (PTFE)-based binder, and further when it contains a PVdF-based binder, higher performance is likely to be ensured. The PVdF-based binder may be a copolymer having a unit derived from a monomer other than VdF. Only one type of polymer 1az may be used alone, or two or more types may be used in combination.
[0021] 1.1.4 Content of each ingredient In the granule 1a, the contents of the first component 1ax, the second component 1ay, and the polymer 1az are not particularly limited. The granule 1a may contain, for example, 50% by mass or more and less than 100% by mass of the first component 1ax, more than 0% by mass and less than 50% by mass of the second component 1ay, and more than 0% by mass and less than 50% by mass of the polymer 1az. Alternatively, the granule 1a may contain 60% by mass or more and 90% by mass or less of the first component 1ax, 5% by mass or more and 30% by mass or less of the second component 1ay, and more than 5% by mass and 30% by mass or less of the polymer 1az.
[0022] 1.1.5 Other ingredients The granule 1a may consist of only the first component 1ax, the second component 1ay, and the polymer 1az, or may contain other components other than these. Examples of other components include various solid components and liquid components.
[0023] 1.1.6 Obtaining granules In step S1, for example, the above-mentioned first component 1ax, second component 1ay, and polymer 1az may be mixed in a dry state to allow each component to adhere to each other, thereby obtaining granules 1a. In this case, there is no particular limitation on the mixing means, and they may be mixed manually using a mortar or the like, or may be mixed mechanically using various mixing devices. Alternatively, in step S1, a slurry or solution containing the above-mentioned first component 1ax, second component 1ay, and polymer 1az may be obtained, and the slurry or solution may be dried to obtain granules 1a. For example, polymer 1az may be dissolved in a solvent to obtain a polymer solution, and Si particles as the first component 1ax and second particles (e.g., SiO ) as the second component 1ay may be added to the polymer solution. 2 The first particle) is dispersed in the second polymer 1az to obtain a slurry, and the slurry is then dried to obtain a granule 1a in which the Si particles and the second particles are bound together via the polymer 1az. In this case, the type of the solvent is not particularly limited. Also, the means for drying the slurry is not particularly limited.
[0024] In step S1, Step S1-1: forming a slurry containing a first component 1ax, a second component 1ay, and a polymer 1az into droplets to obtain slurry droplets; and Step S1-2: The slurry droplets are dried by a gas flow in a heated gas to obtain a granule 1a containing a first component 1ax, a second component 1ay, and a polymer 1az; may also include
[0025] The "slurry" in step S1-1 may be a suspension or a suspension containing the first component 1ax, the second component 1ay, and the polymer 1az, and may have a degree of fluidity that allows it to be made into droplets. The "dropletization" of the slurry means that the slurry containing the first component 1ax, the second component 1ay, and the polymer 1az is made into grains containing the first component 1ax, the second component 1ay, the polymer 1az, and a solvent. The method of making the slurry containing the first component 1ax, the second component 1ay, and the polymer 1az into droplets is not particularly limited. For example, a method of making the slurry into droplets by spraying the slurry can be mentioned. When spraying the slurry, a spray nozzle may be used. Methods of spraying the slurry using a spray nozzle include, but are not limited to, a pressurized nozzle method and a two-fluid nozzle method. Alternatively, the slurry may be made into droplets using a rotary atomizer.
[0026] In step S1-1, the size of the slurry droplets is not particularly limited. The diameter (sphere-equivalent diameter) of the slurry droplets may be, for example, 0.5 μm or more or 5 μm or more, and may be 5000 μm or less or 1000 μm or less. The diameter of the slurry droplets can be measured, for example, using a two-dimensional image obtained by capturing an image of the slurry droplets, or can be measured using a laser diffraction type particle size distribution meter. Alternatively, the droplet diameter can be estimated from the operating conditions of the device that forms the slurry droplets.
[0027] The "airflow drying" in step S1-2 means drying the slurry droplets while suspending them in a high-temperature airflow. The "airflow drying" can include not only drying but also an associated operation using a dynamic airflow. By continuously applying hot air to the slurry droplets by airflow drying, a force is continuously applied to the slurry droplets. By utilizing this, for example, step S1-2 may include disintegrating (crushing) the aggregates of the slurry droplets (or the aggregates of the granules 1a) by airflow drying. In other words, even if the slurry droplets and the like are excessively aggregated in step S1-2, the aggregates can be crushed by airflow drying. Therefore, a slurry with a low solid content concentration can be used, and the processing speed can be easily increased. In this way, by crushing the slurry droplets and the like by airflow drying in step S1-2, the manufacturing time can be easily shortened. In step S1-2, the above-mentioned drying and crushing may be performed simultaneously or separately. In step S1-2, a first air flow drying step in which the drying of the slurry droplets is predominant and a second air flow drying step in which the crushing of the aggregates is predominant may be performed. Also, the second air flow drying step may be performed repeatedly.
[0028] In step S1-2, the temperature of the heated gas, the supply amount (flow rate) of the heated gas, the supply rate (flow rate) of the heated gas, and the treatment time (drying time) by the heated gas can be appropriately set in consideration of the size of the device used and the shape of the slurry droplets. For example, conditions such as those disclosed in JP 2022-047501 A may be adopted. In step S1-2, a heated gas that is substantially inert to each of the above components may be used. For example, an oxygen-containing gas such as air, an inert gas such as nitrogen or argon, or low dew point dry air can be used. As an apparatus for performing airflow drying, for example, a spray dryer can be used, but is not limited thereto.
[0029] 1.2 Process S2 In step S2, the granules 1a are subjected to an acid treatment to remove the second component 1ay from the granules 1a while leaving the first component 1ax and the polymer 1az in the granules 1a, thereby forming voids 1b in the granules 1a. That is, the second component 1ay is etched by subjecting the granules 1a to the acid treatment.
[0030] The acid used in the acid treatment in step S2 may be any acid capable of removing the second component 1ay from the granule 1a while leaving the first component 1ax and the polymer 1az in the granule 1a. The acid treatment in step S2 may include, for example, hydrofluoric acid treatment. That is, the second component 1ay contained in the granule 1a may be dissolved and removed from the granule 1a while leaving the first component 1ax and the polymer 1az in the granule 1a by contacting the granule 1a with hydrofluoric acid (hydrogen fluoride aqueous solution). In step S2, for example, 50 mol% to 100 mol%, 70 mol% to 100 mol%, or 90 mol% to 100 mol% of the second component 1ay contained in the granule 1a may be dissolved in the acid and removed.
[0031] In step S2, the method of contacting the granules 1a with the acid is not particularly limited. The granules 1a may be immersed in the acid, or the acid may be sprayed onto the granules 1a. Alternatively, the granules 1a may be dispersed in a solvent to form a slurry, and the acid may be added to the slurry to contact the granules 1a with the acid in the slurry. In this case, water or various organic solvents may be used as the solvent for dispersing the granules 1a. For example, alcohol such as ethanol may be used as the solvent. In step S2, the time of the acid treatment is not particularly limited. For example, the granules 1a may be dispersed in a solvent to form a slurry, and the slurry may be added with acid and stirred for 1 minute to 10 hours. In step S2, the temperature and atmosphere of the acid treatment are also not particularly limited.
[0032] 1.3 Active material composite particles 1 After step S2, optional filtration, washing and drying are performed to recover the solid content, thereby obtaining active material composite particles 1 that contain the first component 1ax and the polymer 1az and have voids 1b. In the active material composite particles 1, the expansion of Si during charging is absorbed by the voids 1b, and the amount of expansion of the active material composite particles 1 as a whole is reduced. For example, when the active material composite particles 1 are applied to the negative electrode of a secondary battery, the volume change of the negative electrode accompanying charging and discharging is reduced. This makes it possible to suppress an increase in the binding pressure and interfacial peeling, and improves cycle characteristics.
[0033] 1.3.1 Components of active material composite particles The active material composite particle 1 includes at least a first component 1ax and a polymer 1az. The active material composite particle 1 may include, for example, 50% by mass or more and less than 100% by mass of the first component 1ax, 0% by mass or more and 10% by mass or less of the second component 1ay, and more than 0% by mass and 50% by mass or less of the polymer 1az. Alternatively, the active material composite particle 1 may include 60% by mass or more and 90% by mass or less of the first component 1ax, 0% by mass or more and 5% by mass or less of the second component 1ay, and 10% by mass or more and 30% by mass or less of the polymer 1az.
[0034] 1.3.2 Particle size of active material composite particles The active material composite particle 1 can be regarded as a secondary particle including the first component 1ax, the polymer 1az, and the voids 1b. The average particle diameter of the composite particle 1 is not particularly limited. The average particle diameter of the composite particle 1 may be 100 nm or more, 500 nm or more, 1 μm or more, 2 μm or more, or 3 μm or more, and may be 1 mm or less, 500 μm or less, 300 μm or less, 100 μm or less, 50 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. The average particle diameter of the composite particle 1 can be obtained by observation with an electron microscope such as SEM, and is obtained, for example, as the number average value of the maximum Feret diameter of a plurality of composite particles. The number of samples is preferably large, for example, 20 or more, may be 50 or more, or may be 100 or more. Alternatively, the average particle diameter (D50, median diameter) of the composite particle 1 measured using a laser diffraction particle distribution measurement device may be 100 nm or more, 500 nm or more, 1 μm or more, 2 μm or more, or 3 μm or more, or may be 1 mm or less, 500 μm or less, 300 μm or less, 100 μm or less, 50 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less.
[0035] 1.3.3 Structure and shape of active material composite particles In the active material composite particle 1, the arrangement of the first component 1ax, the polymer 1az, and the voids 1b is not particularly limited. The active material composite particle 1 may have a major axis and a minor axis, for example, before being applied to a secondary battery. The ratio of the major axis to the minor axis may be, for example, 1.0 or more or 1.1 or more, or 1.3 or less or 1.2 or less.
[0036] 2. Manufacturing method of secondary batteries The active material composite particle 1 of the present disclosure can be used, for example, as a negative electrode active material of a secondary battery. As shown in Fig. 3, a method for producing a secondary battery 100 according to one embodiment includes obtaining an active material composite particle 1 by the production method of the present disclosure, and obtaining a negative electrode active material layer 20 using the active material composite particle 1. The secondary battery 100 may be, for example, a lithium ion secondary battery.
[0037] The negative electrode active material layer 20 may contain, in addition to the active material composite particles 1, other negative electrode active materials, electrolytes, conductive assistants, binders, and the like. The electrolyte may be, for example, an inorganic solid electrolyte. In this way, when an inorganic solid electrolyte is combined with the active material composite particles 1 in the negative electrode active material layer 20, more excellent effects of the technology of the present disclosure can be obtained. The inorganic solid electrolyte may be a sulfide solid electrolyte or other inorganic solid electrolytes.
[0038] The secondary battery 100 can be manufactured by applying a known method, except that the active material composite particles 1 are used as the negative electrode active material. For example, it can be manufactured as follows. However, the manufacturing method of the secondary battery 100 is not limited to the following method, and each layer may be formed by, for example, dry molding or the like. (1) The active material composite particles 1 constituting the negative electrode active material layer 20 and the like are dispersed in a solvent to obtain a negative electrode slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. Thereafter, the negative electrode slurry is applied to the surface of the negative electrode current collector 10 or the electrolyte layer 30 described below using a doctor blade or the like, and then dried to form the negative electrode active material layer 20 on the surface of the negative electrode current collector 10 or the electrolyte layer 30. Here, the negative electrode active material layer 20 may be press-molded. (2) The positive electrode active material constituting the positive electrode active material layer 40 is dispersed in a solvent to obtain a positive electrode slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. Thereafter, the positive electrode slurry is applied to the surface of the positive electrode current collector 50 or the electrolyte layer 30 described below using a doctor blade or the like, and then dried to form the positive electrode active material layer 40 on the surface of the positive electrode current collector 50 or the electrolyte layer 30. Here, the positive electrode active material layer 40 may be press-molded. (3) The layers are laminated so that the electrolyte layer 30 is sandwiched between the negative electrode active material layer 20 and the positive electrode active material layer 40, to obtain a laminate having the negative electrode current collector 10, the negative electrode active material layer 20, the electrolyte layer 30, the positive electrode active material layer 40, and the positive electrode current collector 50 in this order. The electrolyte layer may be obtained by molding an electrolyte mixture containing a solid electrolyte and a binder, or may be obtained by press molding. Here, the laminate may be further press molded. Other members such as terminals are attached to the laminate as necessary. When an electrolytic solution is used, a separator may be used for the electrolyte layer. (4) The laminate is housed in a battery case and sealed to obtain a secondary battery. EXAMPLES
[0039] As described above, one embodiment of the technology of the present disclosure has been described, but the technology of the present disclosure can be modified in various ways other than the above embodiment without departing from the gist of the technology. The technology of the present disclosure will be described in more detail below while showing examples, but the technology of the present disclosure is not limited to the following examples.
[0040] 1. Preparation of active material composite particles 1.1 Example 1 1.3 g of PVdF-HFP (manufactured by Kureha Corporation) was added to 500 mL of dimethyl carbonate and stirred to dissolve, to prepare a polymer solution. 5.0 g of Si particles and SiO 2 1.0 g of particles (Sigma-Aldrich, average particle size 0.1 μm to 0.2 μm) was added and dispersed using an ultrasonic homogenizer to obtain a slurry. The slurry was sprayed and dried using a spray dryer (ADL311S, Yamato Scientific Co., Ltd.) to obtain elemental Si, SiO 2 Granules consisting of PVdF-HFP were prepared.
[0041] 2 g of the obtained granules were dispersed in 100 mL of ethanol, and then 3 mL of a 47 wt % aqueous hydrogen fluoride solution was added thereto. After the addition, the mixture was stirred for 3 hours, and then filtered under reduced pressure to recover the active material composite particles. In the active material composite particles, the SiO 2 was removed by treatment with an aqueous hydrogen fluoride solution (hydrofluoric acid treatment), and voids were formed. The obtained active material composite particles were vacuum dried at 120° C. for 12 hours, and used as a negative electrode active material described later.
[0042] 1.2 Comparative Example 1: No acid treatment In Example 1, the elemental Si, SiO 2 The granules made of PVdF-HFP were used as they were as the negative electrode active material.
[0043] 1.3 Comparative example 2: SiO 2 none 5.0 g of particles of simple substance Si was added to the polymer solution prepared in the same manner as in Example 1, and dispersed using an ultrasonic homogenizer to obtain a slurry. The slurry was sprayed and dried using a spray dryer (ADL311S manufactured by Yamato Scientific Co., Ltd.) to produce granules consisting of simple substance Si and PVdF-HFP, which were used as the negative electrode active material.
[0044] 2. Fabrication of all-solid-state batteries 2.1 Preparation of the positive electrode active material layer In a PP container, butyl butyrate as a solvent, a 5 wt% butyl butyrate solution of a PVDF-based binder, and LiNi as a positive electrode active material were placed. 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 Particles (average particle size 6 μm) and Li as a sulfide solid electrolyte 2 SP 2 S 5The glass ceramic and VGCF as a conductive assistant were added, and the mixture was stirred for 30 seconds with an ultrasonic dispersion device (UH-50 manufactured by SMT). Next, the container was shaken for 3 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.), and further stirred for 30 seconds with an ultrasonic dispersion device. After that, the mixture was shaken for 3 minutes with a shaker to obtain a positive electrode slurry. Using an applicator, the positive electrode slurry was applied to an Al foil (manufactured by Showa Denko) by the blade method, and dried on a hot plate at 100°C for 30 minutes to form a positive electrode active material layer on the Al foil.
[0045] 2.2 Preparation of negative electrode active material layer In a PP container, dibutyl ether and mesitylene were used as solvents, a 5 wt% mesitylene solution of a PVDF-based binder, VGCF as a conductive additive, and Li as a solid electrolyte. 2 SP 2 S 5 The glass ceramic and the above-mentioned active material composite particles or granules as the negative electrode active material were added to a container and stirred for 30 seconds with an ultrasonic dispersing device (UH-50 manufactured by SMT). Next, the container was shaken for 30 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.) to obtain a negative electrode slurry. Using an applicator, the negative electrode slurry was applied to a Cu foil (manufactured by UACJ) by the blade method, and dried on a hot plate at 100°C for 30 minutes to form a negative electrode active material layer on the Cu foil.
[0046] 2.3 Preparation of solid electrolyte layer In a PP container, heptane as a solvent, a 5 wt% heptane solution of SBR binder, and Li as a solid electrolyte were placed. 2 SP 2 S 5 The electrolyte slurry was then applied to an Al foil substrate by the blade method using an applicator, and the mixture was dried on a hot plate at 100°C for 30 minutes to form a solid electrolyte layer on the Al foil.
[0047] 2.4 Lamination of each layer The above positive electrode active material layer and solid electrolyte layer were laminated to obtain a first laminate having Al foil / positive electrode active material layer / solid electrolyte layer / Al foil. The first laminate was set in a roll press and pressed at a pressure of 100 kN / cm and a temperature of 165° C. Thereafter, the Al foil as a substrate was removed from the first laminate to obtain a positive electrode laminate having Al foil / positive electrode active material layer / solid electrolyte layer.
[0048] The negative electrode active material layer and the solid electrolyte layer were laminated to obtain a second laminate having Cu foil / negative electrode active material layer / solid electrolyte layer / Al foil. The second laminate was set in a roll press and pressed at a pressure of 60 kN / cm and a temperature of 25° C. Thereafter, the Al foil as a substrate was removed from the second laminate to obtain a first negative electrode laminate having Cu foil / negative electrode active material layer / solid electrolyte layer.
[0049] The Al foil and solid electrolyte layer as the substrate and the above-mentioned first negative electrode laminate were laminated in the order of Al foil / solid electrolyte layer / solid electrolyte layer / negative electrode active material layer / Cu foil to obtain a third laminate. The third laminate was set in a flat uniaxial press and temporarily pressed at 100 MPa and 25° C. for 10 seconds. Thereafter, the Al foil was peeled off from the third laminate to obtain a second negative electrode laminate having the solid electrolyte layer / solid electrolyte layer / negative electrode active material layer / Cu foil. The area of the second negative electrode laminate was set to be larger than the area of the above-mentioned positive electrode laminate.
[0050] The positive electrode laminate and the second negative electrode laminate were laminated in the order of Al foil / positive electrode active material layer / solid electrolyte layer / solid electrolyte layer / solid electrolyte layer / negative electrode active material layer / Cu foil to obtain a fourth laminate. The fourth laminate was set in a flat uniaxial press and pressed at 200 MPa and 120° C. for 1 minute. This produced an all-solid-state battery for evaluation.
[0051] 3. Evaluation of all-solid-state batteries The fabricated all-solid-state battery was restrained at a predetermined restraining pressure using a restraining jig, charged at a constant current of 1 / 10C to 4.55V, discharged at 1C to 3.0V, charged at a constant current-constant voltage of 1 / 3C to 4.35V, discharged at a constant current-constant voltage of 1 / 3C to 3.00V, and then repeated a constant current charge-discharge test at 2C 200 times as a cycle test. The ratio of the discharge capacity at the 200th cycle to the initial discharge capacity of the cycle test ([discharge capacity at the 200th cycle / initial discharge capacity] x 100) was calculated as the discharge capacity retention rate.
[0052] 4. Evaluation Results Table 1 below shows the discharge capacity retention rates of the all-solid-state batteries of Example 1 and Comparative Examples 1 and 2. In Table 1 below, the discharge capacity retention rate of Comparative Example 2 is set to 100, and the discharge capacity retention rates of Example 1 and Comparative Example 1 are shown relative to each other.
[0053] [Table 1]
[0054] As shown in Table 1, the all-solid-state battery according to Example 1 has excellent cycle characteristics compared to the all-solid-state batteries according to Comparative Examples 1 and 2. In the all-solid-state battery according to Example 1, SiO 2 It is considered that the removal of the active material composite particles formed voids, which absorbed the expansion of Si during charging, and reduced the amount of expansion of the active material composite particles as a whole. In other words, it is considered that the volume change of the negative electrode accompanying charging and discharging was reduced, and the increase in the restraining pressure and the interface peeling were suppressed, improving the cycle characteristics.
[0055] In the above examples, SiO was used as the second component in producing the active material composite particles. 2Although the above example shows a case where a fluorine-containing polymer is used as the polymer and a hydrofluoric acid treatment is used as the acid treatment, it is considered that similar active material composite particles can be formed by acid treatment even when other materials are used. In addition, in the above example, the case where an all-solid-state battery is produced as the secondary battery for evaluation is shown as an example, but the effect of the active material composite particles can be expected in other secondary batteries as well.
[0056] As described above, according to the following method, it is possible to produce active material composite particles having excellent cycle characteristics. That is, the method for producing active material composite particles according to the present disclosure includes the steps of: Step S1: Obtaining a granule containing elemental Si as a first component, a component other than elemental Si as a second component, and a polymer; and Step S2: The granules are subjected to an acid treatment to remove the second component from the granules while leaving the first component and the polymer in the granules, thereby forming voids in the granules. [Explanation of symbols]
[0057] 1 Active material composite particles 1a Granules 1ax 1st component 1ay 2nd component 1az Polymer 1b void 100 Secondary battery 10 Negative electrode current collector 20 Negative electrode active material layer 30 Electrolyte layer 40 Cathode active material layer 50 Positive electrode current collector
Claims
1. A method for producing active material composite particles, comprising the steps of: Obtaining a granule containing a first component, a component other than the simple substance Si, and a polymer as a second component; and and subjecting the granules to an acid treatment to remove the second component from the granules while leaving the first component and the polymer in the granules, thereby forming voids in the granules. A method for producing active material composite particles.
2. The method according to claim 1, The second component is SiO 2 That is, Manufacturing method.
3. The method according to claim 1, The acid treatment includes a hydrofluoric acid treatment. Manufacturing method.
4. The method according to claim 1, The polymer comprises a fluorine-containing polymer. Manufacturing method.
5. A method for manufacturing a secondary battery, comprising: Obtaining active material composite particles by the production method according to any one of claims 1 to 4; and Obtaining a negative electrode active material layer using the active material composite particles. Manufacturing method.
Citation Information
Patent Citations
Silicon-carbon composite material with nano micropores and preparation method as well as application thereof
CN103311523A
Nano silicon / porous carbon composite anode material of lithium ion batteries as well as preparation method and application of composite anode material
CN106848199A
Porous spherical core-shell structure silicon-carbon composite material and preparation method thereof and lithium ion battery
CN109192957A
Silicon-containing mineral-based porous silicon-carbon composite negative electrode material and preparation method thereof
CN113871604A
Positive electrode used for lithium sulfur secondary battery, and lithium sulfur secondary battery