Electrode catalyst, manufacturing method thereof, and fuel cell
By supporting nanowires within the mesopores of a carbon carrier and using ultrasonic arrangement, the electrode catalyst achieves higher catalytic activity and stability, addressing the aggregation issue in existing catalysts.
Patent Information
- Application Number
- JP2023058701
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing electrode catalysts face limitations in catalytic activity due to platinum nanowire aggregation, reducing the effective surface area and hindering high catalytic performance in electrochemical cells.
The electrode catalyst is designed with nanowires supported within the mesopores of a carbon carrier, utilizing ultrasonic waves to arrange the nanowires within these pores, and optionally incorporating an ionic liquid to enhance catalytic activity.
This configuration suppresses nanowire aggregation, increases the surface area, and enhances catalytic activity, particularly for oxygen reduction in fuel cells, with improved performance and stability.
Smart Images

Figure 2024146036000001 
Figure 2024146036000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode catalyst and a method for producing the same.The present invention also relates to a fuel cell. [Background technology]
[0002] In electrochemical cells such as solid polymer fuel cells and water electrolysis devices, a catalyst-supported carrier in which a precious metal catalyst such as platinum is supported on a carrier is used as an electrode catalyst. From the viewpoint of effective use of the catalyst, a carbonaceous material, which is a material with a large specific surface area, is often used as the catalyst carrier.
[0003] For example, Patent Documents 1 and 2 propose using a porous carbon material as a catalyst support and supporting catalyst particles in the pores of the porous carbon material. Patent Document 2 describes that supporting catalyst particles in the pores makes it difficult for the catalyst to come into contact with the ionomer, thereby suppressing poisoning of the catalyst by the ionomer.
[0004] Non-Patent Document 1 describes that platinum nanowires exhibit extremely high catalytic activity in the oxygen reduction reaction. The document also describes that platinum nanowires have relatively high catalytic activity compared to spherical particles with a small aspect ratio.
[0005] Patent Document 3 proposes using a carbon support as a catalyst support, nanowire particles containing platinum as a precious metal catalyst and having their surfaces modified with oleylamine, thereby enabling the nanowire particles to be densely supported on the surface of the carbon support while the oleylamine prevents the nanowire particles from agglomerating. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2014 / 175099 Brochure [Patent Document 2] JP 2018-98198 A [Patent Document 3] Patent Publication No. 2021-190418 [Non-patent literature]
[0007] [Non-Patent Document 1] M. Li, et al., Science, 2016, Vol 354, Issue 6318, pp.1414-1419. Summary of the Invention [Problem to be solved by the invention]
[0008] In order to improve the performance of an electrochemical cell, it is important to improve the performance of the electrode catalyst. However, the electrode catalysts described in Patent Documents 1 and 2 have limitations in terms of how much they can enhance the catalytic activity. The platinum nanowires described in Non-Patent Document 1 have the problem that the platinum nanowires tend to aggregate with each other, reducing the surface area of the nanowires available for catalytic reactions and making it difficult to achieve high catalytic activity. According to the technique described in Patent Document 3, although the aggregation of nanowires can be suppressed to some extent, there is still room for improvement in terms of improving catalytic activity. Therefore, an object of the present invention is to provide an electrode catalyst having a higher catalytic activity than conventional ones, a method for producing the same, and a fuel cell using the same. [Means for solving the problem]
[0009] In order to solve the above problems, the inventors investigated electrode catalysts in which nanowires are supported on a carbon support and found that by having the nanowires reside within the mesopores of the carbon support, the aggregation of the nanowires can be further suppressed, thereby further improving the catalytic activity of the nanowires.
[0010] The present invention has been made based on the above findings, and includes a carbon support having mesopores and linear bodies of a catalytic metal, The above problem is solved by providing an electrode catalyst in which at least a portion of the linear bodies is located within at least a portion of the mesopores.
[0011] The present invention also provides a method for producing an electrode catalyst, which comprises irradiating a mixed solution containing a carbon support having mesopores and linear bodies of a catalytic metal with ultrasonic waves to arrange at least a portion of the linear bodies on the surface of the carbon support. Effect of the Invention
[0012] According to the present invention, an electrode catalyst having higher catalytic activity than conventional ones is provided, and further, according to the present invention, a method for easily producing such an electrode catalyst is provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described below based on its preferred embodiments. The present invention relates to an electrode catalyst. The electrode catalyst of the present invention includes a carbon support having mesopores and linear bodies of a catalytic metal. In the electrode catalyst of the present invention, at least a part of the linear bodies is located in at least a part of the mesopores among the numerous mesopores.
[0014] The carbon support in the present invention has mesopores. The size of the mesopores is mesoscale, that is, the pore diameter is 2.0 nm or more and 50.0 nm or less in diameter. When the carbon support has mesoscale pores, the surface area of the carbon support is increased, and it becomes possible to successfully arrange the linear bodies in the mesopores. From the viewpoint of making this advantage more prominent, the mesopore diameter of the carbon support is preferably 3.0 nm or more, more preferably 3.5 nm or more, and even more preferably 4.0 nm or more. In addition, the mesopore diameter of the carbon support is preferably 30.0 nm or less, more preferably 25.0 nm or less, even more preferably 20.0 nm or less, and even more preferably 15.0 nm or less. The method for measuring the mesopore diameter will be described in the examples described later.
[0015] The mesopores may or may not have a continuous pore structure. From the viewpoint of increasing the catalytic activity of the electrode catalyst of the present invention, it is preferable that the mesopores have a continuous pore structure. That is, it is preferable that the mesopores open on the surface of the carbon support, extend toward the inside of the carbon support, and have the other end open on the surface of the carbon support. The mesopores may be branched inside the carbon support. The mesopores may also intersect with other pores inside the carbon support. When the mesopores have a continuous pore structure, more reactants, such as oxygen, can be supplied to the linear bodies of the catalytic metal located in the mesopores from the multiple openings in the carbon support. As a result, the catalytic activity of the electrode catalyst of the present invention can be increased compared to conventional methods.
[0016] From the viewpoint of successfully arranging the linear bodies in the mesopores of the carbon support, the mesopore volume of the carbon support is preferably 0.05 mL / g to 3.00 mL / g per unit mass of the carbon support, more preferably 0.10 mL / g to 2.50 mL / g, and even more preferably 0.20 mL / g to 2.20 mL / g. "Mesopore volume" refers to the pore volume in the range of 2 nm to 50 nm calculated by analyzing the nitrogen adsorption / desorption isotherm.
[0017] The carbon support in the present invention may have macropores and / or micropores, as long as the effects of the present invention are not impaired. "Macropores" refer to pores with a diameter of more than 50.0 nm. "Micropores" refer to pores with a diameter of less than 2.0 nm.
[0018] The carbon support has a BET specific surface area of 250 m 2 / g or more 2000m 2 / g or less, and 2 / g or more 1800m 2 / g or less is more preferable, and 2 / g or more 1500m 2 / g or less is even more preferable. The BET specific surface area can be measured, for example, as follows. The carbon support is heated in a vacuum at 400°C for 3 hours using a pretreatment device "BELPREP-vacII" manufactured by Microtrack-Bell Corporation. Then, the specific surface area is calculated by the BET (Brunauer-Emmett-Teller) method from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using a specific surface area measuring device "BELSORP-miniII" manufactured by Microtrack-Bell Corporation.
[0019] It is preferable to use a carrier whose main component is carbon as the carbon carrier. "Mainly carbon" means that the ratio of carbon in the carbon carrier is 50 mass% or more. By using a carrier whose main component is carbon, the conductivity of the carrier is improved and the electrical resistance is reduced, which is preferable. Therefore, the carbon contained in the carbon carrier is preferably conductive carbon.
[0020] The carbon support may include, for example, a group of carbonaceous materials called carbon black, activated carbon, graphite, mesoporous carbon, graphene, and other carbon materials. In the present invention, the type of carbon material is not particularly limited, and the desired effect can be achieved regardless of the type of carbon material used. In addition, from the viewpoint of improving electrical conductivity and improving the interaction between the carbon support and the linear body of the catalytic metal, the carbon support may include a carbon material doped with an element such as nitrogen or boron.
[0021] The linear body in the electrode catalyst of the present invention is made of a catalytic metal. The linear body typically extends in one direction. The state in which the linear body extends in one direction varies depending on the state of the linear body when observed. For example, the linear body extends in one direction in a straight line or in a curved, meandering manner. The linear body may have, for example, a shape in which the diameter is almost uniform over its entire length, or a shape in which the diameter is not uniform but is beaded. In this specification, the linear body has a shape in which the ratio of length to diameter is 3.0 or more.
[0022] The diameter of the linear body is preferably smaller than the mesopore size of the carbon support. This allows the linear body to be successfully arranged in the mesopores of the carbon support. From the same viewpoint, the diameter of the linear body is preferably 0.2 nm to 10.0 nm, more preferably 0.5 nm to 7.5 nm, even more preferably 0.7 nm to 6.0 nm, even more preferably 1.0 nm to 5.0 nm, and even more preferably 1.0 nm to 3.0 nm, provided that the diameter is smaller than the mesopore size.
[0023] The difference between the diameter of the linear body and the mesopore diameter of the carbon support is preferably small. Such a relationship between the linear body and the mesopore diameter prevents excessively many linear bodies from being located in the mesopores, and therefore, for example, the linear bodies can be prevented from agglomerating even in the mesopores. As a result, the catalytic activity of the electrode catalyst of the present invention can be made higher than that of the conventional electrode catalyst. For this reason, the ratio of the diameter of the linear body to the mesopore diameter of the carbon support is preferably 0.05 or more, more preferably 0.10 or more, and even more preferably 0.12 or more. Considering only the viewpoint of preventing the aggregation of the linear bodies, the upper limit of the ratio is 1.00. On the other hand, from the viewpoint of easily positioning the linear bodies within the mesopores and from the viewpoint of providing room for the movement of substances within the mesopores, it is preferable that the diameter ratio of the linear bodies to the mesopore diameter of the carbon support is less than 1.00, more preferably 0.90 or less, even more preferably 0.60 or less, even more preferably 0.40 or less, and even more preferably 0.20 or less.
[0024] The diameter of the linear body can be adjusted, for example, when obtaining the linear body in the manufacturing method of the electrode catalyst described below, by adjusting the amount of catalytic metal source used, adjusting the concentration of the reducing agent, adding an additive such as a surfactant, adjusting the heating temperature, or changing the reaction atmosphere.
[0025] In the electrode catalyst of the present invention, the length of the linear body is not particularly limited, but from the viewpoint of ease of handling and the size of the carbon support used, it is preferably 0.6 nm or more and 10,000 nm or less, more preferably 2.0 nm or more and 1,000 nm or less, even more preferably 5.0 nm or more and 500 nm or less, and even more preferably 10.0 nm or more and 100 nm or less. Regardless of the length of the linear body, the effect of the present invention is sufficiently exhibited.
[0026] The length of the linear body can be adjusted, for example, by adjusting the amount of catalytic metal source used, adjusting the reduction time, or adjusting the heating temperature when obtaining the linear body in the manufacturing method of the electrode catalyst described below.
[0027] The aspect ratio of the linear bodies (average length [m] of linear bodies / diameter [m] of linear bodies) is preferably 3 or more and 1000 or less, more preferably 5 or more and 500 or less, even more preferably 5 or more and 100 or less, even more preferably 8 or more and 50 or less, and even more preferably 8 or more and 30 or less. When the aspect ratio of the linear bodies is within this range, the catalytic activity can be increased compared to conventional methods due to the shape of the linear bodies. Furthermore, for example, in the manufacturing method of an electrode catalyst described later, when the linear bodies are arranged in the mesopores, the linear bodies are easily dispersed in the dispersion liquid and the linear bodies are easily arranged in the mesopores.
[0028] The diameter of the filaments is determined by reading the diameters of at least 10 filaments from an electron microscope image and arithmetically averaging them. If the diameter of the linear body is not constant along its entire length, for example if the linear body consists of a portion f1 having a diameter d1 and a portion f2 having a diameter d2, then when portion f1 occupies more than 60% of the entire length of the linear body, diameter d1 is taken as the diameter of the linear body, and when portion f2 occupies more than 60% of the entire length of the linear body, diameter d2 is taken as the diameter of the linear body. When a linear body does not have an area that occupies more than 60% of its total length, the thickest and thinnest values of the linear body are read and the arithmetic average of these is calculated. The length of the filaments was determined by reading the lengths of 20 filaments from an electron microscope image and calculating the arithmetic mean value.
[0029] There is no particular limitation on the type of catalytic metal constituting the linear body, and various metals having catalytic activity for various electrode reactions can be used. The electrode catalyst of the present invention preferably uses a metal having catalytic activity, particularly for the electrode reaction of a fuel cell. Examples of catalytic metals include platinum, ruthenium, iridium, palladium, rhodium, osmium, nickel, cobalt, gold, silver, and alloys containing these metals. These can be used alone or in combination of two or more.
[0030] The linear body preferably contains at least a platinum group element. By containing a platinum group element in the linear body, an electrode catalyst having high catalytic activity and electrochemical stability can be obtained. In particular, when the electrode catalyst of the present invention is used in, for example, an electrode of a fuel cell, high oxygen reduction activity can be obtained. For this reason, the linear body preferably contains at least a platinum group element or an alloy containing these metals, and is preferably made of a platinum group element or an alloy containing these metals. In this specification, "platinum group element" refers to platinum, ruthenium, iridium, palladium, rhodium, and osmium.
[0031] Of the platinum group elements, the linear body preferably contains at least platinum. Platinum is known to have high catalytic activity, particularly with respect to oxygen reduction. Therefore, when the linear body contains platinum, the catalytic activity of the electrode catalyst of the present invention is further increased compared to conventional methods when used in an electrode of a fuel cell having a relatively low operating temperature, such as a polymer electrolyte fuel cell. For this reason, the linear body preferably contains at least platinum or an alloy containing platinum, and is preferably made of platinum or an alloy containing platinum.
[0032] The linear body may be composed of a core portion made of a metal and a shell portion disposed on the surface of the core portion and made of a metal other than the metal. In other words, the linear body may be composed of layers of different kinds of metals. The core portion constitutes the main portion of the linear body. The shell portion may be disposed on the entire surface of the core portion. Alternatively, the shell portion may be present so as to cover only a portion of the surface of the core portion. The boundary between the core portion and the shell portion may be clear, or the boundary may be partially unclear as long as the core portion and the shell portion can be distinguished from each other. As the metal constituting the core or shell, various metals having catalytic activity for various electrode reactions can be used. In particular, it is preferable to use a metal having catalytic activity for the electrode reaction of a fuel cell. Examples of the metal constituting the shell include platinum, ruthenium, iridium, palladium, rhodium, osmium, nickel, cobalt, gold, silver, or alloys containing these metals. The metal constituting the core is not particularly limited as long as it is a metal of a different type from the metal constituting the shell, or an alloy of a different composition from the alloy constituting the shell, and examples of the metal constituting the core include platinum, ruthenium, iridium, palladium, rhodium, osmium, nickel, cobalt, gold, silver, iron, titanium, copper, zinc, or alloys containing these metals. From the viewpoint of further increasing the catalytic activity, it is preferable that the metal constituting the shell contains a platinum group element or an alloy containing these metals, and from the viewpoint of electrochemical stability, it is more preferable that both the metals constituting the core and shell contain a platinum group element or an alloy containing these metals, and it is even more preferable that both the metals constituting the core and shell are made of platinum group elements. When both the metals constituting the core and shell contain a platinum group element, the amount of the platinum group element constituting the core is preferably smaller than the amount of the platinum group element constituting the shell. By adopting such a structure, the amount of the platinum group element used can be reduced while increasing the catalytic activity of the electrode catalyst, resulting in an excellent economy.
[0033] The surface of the linear body may be coated with a substance other than a metal. Here, "coated" includes a case where the catalytic metal constituting the linear body is chemically bonded to the substance other than a metal, and a case where the metal constituting the linear body is physically adsorbed to the substance other than a metal. The linear body may be coated with either one of the substances, or with both substances. Examples of the material that can be used to coat the linear body include oxides, sulfides, organic materials, and carbon materials.
[0034] One of the features of the electrode catalyst of the present invention is that some or all of the linear bodies of the catalytic metal are located in some or all of the mesopores of the carbon support. In order to improve the performance of electrochemical cells, electrode catalysts with high catalytic activity are required. However, when linear bodies, which are considered to have relatively higher catalytic activity than conventionally used particles, are used as electrode catalysts, the linear bodies tend to aggregate and reduce their surface area, which may prevent the linear bodies from fully exerting their inherent high catalytic activity. The inventors of the present invention have conducted extensive research to improve this point, and have unexpectedly found that by using a carbon support having linear bodies and mesopores, and by partitioning the linear bodies by positioning them within the mesopores, it is possible to suppress the aggregation of the linear bodies, thereby bringing out the inherent high catalytic activity of the linear bodies and increasing the catalytic activity of the electrode catalyst compared to conventional methods.
[0035] In the electrode catalyst of the present invention, the presence of linear bodies within the mesopores of the carbon support can be confirmed by observation with a transmission electron microscope.
[0036] In the electrode catalyst of the present invention, the linear bodies may be located not only inside the mesopores of the carbon support but also outside the mesopores. For example, the linear bodies may be located on a part of the surface of the carbon support, or may be located over the entire surface of the carbon support. In addition, when the carbon support has macropores and / or micropores, the linear bodies may be located in either of the pores, or may be located in both of the pores. From the viewpoint of preventing the linear bodies from agglomerating by locating them in the mesopores of the carbon support and increasing the catalytic activity of the electrode catalyst more than before, it is preferable that the linear bodies are located mainly in the mesopores.
[0037] In the electrode catalyst of the present invention, the amount of the linear bodies supported is preferably 1% by mass or more and 70% by mass or less, more preferably 3% by mass or more and 60% by mass or less, even more preferably 5% by mass or more and 50% by mass or less, and even more preferably 10% by mass or more and 40% by mass or less, based on the mass of the electrode catalyst. When the amount of the linear bodies supported in the electrode catalyst is within this range, the catalytic activity of the electrode catalyst can be made higher than before.
[0038] In the electrode catalyst of the present invention, the amount of linear bodies supported can be confirmed by total dissolution inductively coupled plasma optical emission spectrometry or total dissolution inductively coupled plasma mass spectrometry, which will be described below. Specifically, first, a predetermined amount of electrode catalyst powder is completely dissolved using a strong acid or the like to obtain a solution. Next, the amount of elements (mass%) constituting the linear bodies contained in the solution is measured by the above-mentioned analysis method, and the amount of the linear bodies is calculated. The amount of linear bodies supported in the electrode catalyst can be calculated based on the mass of the completely dissolved electrode catalyst powder and the calculated amount of the linear bodies. The type of element of the linear bodies contained in the solution obtained by completely dissolving the electrode catalyst powder can be analyzed by inductively coupled plasma optical emission spectrometry or inductively coupled plasma mass spectrometry.
[0039] In the electrode catalyst of the present invention, it is preferable that an ionic liquid is present on the surface of the carbon support. The "surface of the carbon support" includes both the outer surface and the inner surface of the pores of the carbon support. It is more preferable that the ionic liquid is present in at least a part of the mesopores of the carbon support. The ionic liquid is a salt that is composed of a cation and an anion and is liquid at room temperature and normal pressure. As the ionic liquid, either an aprotic ionic liquid or a protic ionic liquid may be used alone, or a mixture of these may be used.
[0040] Examples of aprotic ionic liquids include 1-butyl-3-methylimidazolium hexafluorophosphate ([BMIM][PF6]), etc. The aprotic ionic liquids may be used alone or in combination of two or more.
[0041] Examples of the protic ionic liquid include 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene bis(trifluoromethylsulfonyl)imide, etc. The protic ionic liquids can be used alone or in combination of two or more.
[0042] In the electrode catalyst of the present invention, the presence of an ionic liquid on the surface of the carbon support allows, for example, when an electrode catalyst layer is formed using the electrode catalyst of the present invention and an ionomer, the ionic liquid can be selectively adsorbed on the surface of a linear body containing a platinum group element or the like. This suppresses the poisoning of the electrode catalyst by the ionomer, and as a result, it is believed that the catalytic activity of the electrode catalyst can be maintained at a high level. In addition, although the detailed cause has not been clarified, the catalytic activity of the electrode catalyst can be effectively maintained at a high level by using an aprotic ionic liquid as the ionic liquid used. Furthermore, the present inventors have found that when the ionic liquid used is an aprotic ionic liquid, the greater the amount of ionomer, the higher the catalytic activity of the electrode catalyst, which is an unexpected effect completely different from that of conventionally known electrode catalysts. From the viewpoint of effectively maintaining the catalytic activity of the electrode catalyst at a high level, it is preferable to use, for example, 1-butyl-3-methylimidazolium hexafluorophosphate as the aprotic ionic liquid.
[0043] In the electrode catalyst of the present invention, the mass ratio of the ionic liquid to the electrode catalyst is preferably 0.005 or more, more preferably 0.01 or more, and even more preferably 0.015 or more. The mass ratio of the ionic liquid to the electrode catalyst is preferably 1.00 or less, more preferably 0.90 or less, and even more preferably 0.80 or less. Since the mass ratio of the ionic liquid to the electrode catalyst is within this range, a sufficient amount of the ionic liquid can be present on the entire surface of the carbon support, and in particular, for example, when the electrode catalyst layer is formed using the electrode catalyst and an ionomer, the poisoning of the electrode catalyst by the ionomer is suppressed, and as a result, the catalytic activity of the electrode catalyst can be maintained at a high level.
[0044] In the electrode catalyst of the present invention, the mass ratio of the ionic liquid to the electrode catalyst can be confirmed, for example, by quantifying the nitrogen component in the cation contained in the ionic liquid. The nitrogen component can be quantified according to a conventional method, for example, by an elemental analyzer (CHN analyzer), X-ray photoelectron spectroscopy (XPS), or energy dispersive X-ray analysis (EDX).
[0045] In the electrode catalyst of the present invention, the mass ratio of the ionic liquid to the linear body is preferably 0.017 to 3.3, more preferably 0.03 to 3.0, and even more preferably 0.05 to 2.7. When the mass ratio of the ionic liquid to the linear body is within this range, a sufficient amount of ionic liquid can be present throughout the linear body, and therefore, in particular, when an electrode catalyst layer is formed using an electrode catalyst and an ionomer, poisoning of the electrode catalyst by the ionomer is suppressed, and as a result, the catalytic activity of the electrode catalyst can be maintained at a high level.
[0046] In the electrode catalyst of the present invention, the mass ratio of the ionic liquid to the linear bodies can be confirmed in the same manner as the mass ratio of the ionic liquid to the electrode catalyst described above.
[0047] The mass ratio of the ionic liquid to the electrode catalyst or the mass ratio of the ionic liquid to the linear bodies can be adjusted, for example, by adjusting the amount of the electrode catalyst or the amount of the ionic liquid used when mixing the obtained electrode catalyst and the ionic liquid.
[0048] In the electrode catalyst of the present invention, it is very difficult to directly confirm that the ionic liquid exists in the mesopores of the carbon support. However, for the following reasons, the inventors speculate that when the electrode catalyst contains an ionic liquid, most of the ionic liquid exists in the mesopores. The surface of the carbon support having mesopores can be divided into the surface inside the pores and the outer surface of the carbon support. Since the pore size of the mesopores is very fine, most of the surface of the carbon support is the surface inside the mesopores. Since the ionic liquid exists in a form adsorbed on the surface of the electrode catalyst, i.e., the surface of the carbon support, it is natural to think that most of the ionic liquid exists inside the mesopores.
[0049] Next, a preferred method for producing the electrode catalyst of the present invention will be described. First, a carbon support, which is one of the raw materials for an electrode catalyst, that is, a carbon support having mesopores, is prepared. A linear body, which is one of the raw materials for the electrode catalyst, is prepared together with a carbon support. There is no particular limitation on the method for producing the linear body, and it can be produced by a wet reduction method (electroless reduction method) or an electrolytic method, but it is preferably produced by a wet reduction method.
[0050] In the wet reduction method, a metal element-containing compound such as bis(acetylacetonato)platinum(II) or bis(acetylacetonato)nickel(II) can be used as the catalytic metal source in the linear body. These catalytic metal sources can be used alone or in combination of two or more. They can also be used in the form of a powder or a solution dissolved in an organic solvent.
[0051] The reducing agent in the wet reduction method can be any reducing agent known in the art, without any particular limitations. Examples of the reducing agent include organic compounds such as reducing sugars, transition metal carbonyl compounds, oleylamine, glucose, etc. These can be used alone or in combination of two or more. These can be used in the form of a powder or an aqueous solution. From the viewpoint of easily reducing the linear body, it is preferable to use an organic compound with a relatively high reducing ability. As the organic compound, it is preferable to use, for example, glucose.
[0052] In addition to the catalyst metal source and the reducing agent, an additive can be used as necessary. For example, a carbonyl compound of a transition metal, a quaternary ammonium salt, etc. can be used as the additive. These can be used alone or in combination of two or more. These can be used in the form of a powder or in the form of a solution dissolved in an organic solvent. From the viewpoint of easily obtaining a linear body having a relatively narrow diameter like the linear body in the present invention, it is preferable to use a carbonyl compound of a transition metal or a quaternary ammonium salt as the additive. For example, molybdenum hexacarbonyl, tungsten hexacarbonyl, etc. can be used as the carbonyl compound of a transition metal. For example, hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, etc. can be used as the quaternary ammonium salt.
[0053] In addition to the above-mentioned catalytic metal source, reducing agent, and additive, a solvent is also prepared to dissolve these substances. Examples of the solvent include various organic solvents such as amines such as alkylamines, ketones, and aromatic hydrocarbons. Specifically, oleylamine, acetone, benzene, toluene, N,N-dimethylformamide, etc. are listed. Among these organic solvents, oleylamine is preferred from the viewpoint of a good balance between ease of handling and high solubility. Furthermore, oleylamine also functions as a reducing agent, so it is also preferred from the viewpoint of efficiently producing the linear body.
[0054] Once the above raw materials are prepared, they are mixed to obtain a solution. The concentration of the catalytic metal source in the solution is 1.0×10 -4 mol / L or more and 0.5 mol / L or less are preferable, and 1.0×10 -3 mol / L or more and 0.1 mol / L or less are more preferable, and 2.0×10 -3 mol / L or more 5.0×10 -2 mol / L or less, and more preferably 5.0×10 -3 mol / L or more 2.5×10 -2 It is more preferable that the total concentration of the catalytic metal sources in the solution is within this range. When two or more catalytic metal sources are used in combination, it is preferable that the total concentration of the catalytic metal sources in the solution is within this range. When the concentration of the catalytic metal sources is within this range, it is relatively easy to obtain a dispersion in which linear bodies having a desired diameter are dispersed in a solvent.
[0055] The concentration of the reducing agent in the solution is 1.0 x 10 -2 mol / L or more and 0.5 mol / L or less are preferable, and 2.0×10 -2 mol / L or more and 0.4 mol / L or less are more preferable, and 3.0×10 -2 More preferably, the concentration is 4.0×10 -2 It is more preferable that the concentration of the reducing agent is 0.2 mol / L or more and 0.5 mol / L or less. When two or more reducing agents are used in combination, it is preferable that the total concentration of the reducing agents contained in the solution is in this range. When the concentration of the reducing agent is in this range, the catalytic metal source can be successfully reduced to obtain a linear body.
[0056] In addition, when an additive is used, the concentration of the additive in the solution is 1.0×10 -3 mol / L or more and 0.2 mol / L or less are preferable, and 2.0×10 -3 mol / L or more and 0.1 mol / L or less are more preferable, and 5.0×10 -3 mol / L or more 5.0×10 -2mol / L or less, and more preferably 1.0×10 -2 mol / L or more 4.0×10 -2 It is more preferable that the total concentration of the additives contained in the solution is within this range. When two or more additives are used in combination, it is preferable that the total concentration of the additives contained in the solution is within this range. When the additive concentration is within this range, a linear body having a desired aspect ratio can be easily obtained.
[0057] The solution is then heated. The heating reduces the catalytic metal source with the reducing agent, and a linear body of catalytic metal is generated from the catalytic metal source. In particular, when an additive is used, when the catalytic metal source is reduced and the metal atoms are aggregated to form an aggregate, the growth of a specific metal crystal face is suppressed due to the action of the additive, and a linear body having a narrow diameter is generated, such as the linear body in the present invention.
[0058] The heating temperature of the solution is not particularly limited as long as it is sufficient to cause reduction of the catalytic metal source, but is preferably 60°C or higher and 300°C or lower, more preferably 80°C or higher and 280°C or lower, and even more preferably 100°C or higher and 260°C or lower. The heating time of the solution is not particularly limited as long as it is long enough to cause reduction of the catalytic metal source, but is preferably from 0.1 to 10 hours, more preferably from 0.5 to 6 hours, and even more preferably from 1 to 4 hours. If necessary, the solution may be heated under reflux.
[0059] After the linear bodies are produced in this manner, the solution is subjected to solid-liquid separation, and the solids are collected, washed, and dried. For washing the solids, for example, a mixture of ethanol and cyclohexane can be used. In this manner, the desired linear bodies are obtained.
[0060] Furthermore, if necessary, after obtaining the linear body, it can be used as an electrode to perform metal plating on the entire surface of the linear body, thereby coating the surface of the linear body with a different type of metal.
[0061] After the carbon support and the linear body are prepared, a dispersion liquid is prepared by mixing the carbon support, the linear body, and a dispersion medium. As the dispersion medium, for example, a mixture of ethanol and cyclohexane can be used.
[0062] The mass ratio of the linear bodies to the carbon support contained in the dispersion is preferably 0.01 to 2.40, more preferably 0.03 to 1.50, and even more preferably 0.05 to 1.00. When the mass ratio of the linear bodies to the carbon support is within this range, the linear bodies can be successfully arranged in the mesopores of the carbon support. The mass of the carbon support relative to the dispersion is preferably 0.01 mg to 0.4 mg, more preferably 0.02 mg to 0.3 mg, and even more preferably 0.03 mg to 0.2 mg per mL of the dispersion. When the mass of the carbon support relative to the dispersion is in this range, the linear bodies can be successfully arranged in the mesopores of the carbon support.
[0063] Then, ultrasonic waves are applied to the dispersion liquid containing the carbon support having mesopores and the linear bodies of the catalytic metal. As a result, at least a part of the linear bodies is arranged in at least a part of the mesopores. The present inventors have found for the first time that the linear bodies can be unexpectedly arranged in the mesopores of the carbon support by applying ultrasonic waves to the dispersion liquid containing the carbon support and the linear bodies. In addition, it is preferable to perform the cooling while cooling the dispersion liquid from the viewpoint of suppressing the temperature rise of the mixed liquid caused by the application of ultrasonic waves. The cooling temperature is preferably 10°C or lower, and more preferably around 0°C. For example, it is preferable to perform the ultrasonic irradiation in an ice bath.
[0064] The dispersion is irradiated with ultrasonic waves at preferably 30 W to 1000 W, more preferably 50 W to 500 W, and even more preferably 100 W to 400 W. When the ultrasonic output is within this range, the linear bodies can be successfully arranged in the mesopores of the carbon support. The ultrasonic irradiation time for the dispersion is preferably 0.5 to 10 hours, more preferably 1 to 8 hours, and even more preferably 2 to 6 hours. By irradiating the dispersion with ultrasonic waves for a time within this range, the linear bodies can be successfully arranged in the mesopores of the carbon support.
[0065] After the linear bodies are arranged in the mesopores of the carbon support in this way, the dispersion is subjected to solid-liquid separation, and the solids are recovered, washed, and dried. For washing the solids, for example, a mixture of ethanol and cyclohexane can be used. In this way, the desired electrode catalyst is obtained.
[0066] In the electrode catalyst of the present invention, when an ionic liquid is present on the surface of a carbon support, i.e., when the ionic liquid is disposed within the mesopores of the carbon support, a carbon support having an ionic liquid previously disposed within the mesopores and a linear body may be used. In detail, first, a mixed dispersion liquid is prepared by mixing a carbon carrier, an ionic liquid, and a dispersion medium. As the dispersion medium, for example, a mixture of ethanol and cyclohexane can be used. Next, ultrasonic waves are irradiated to the mixed dispersion liquid, and the ionic liquid is arranged in the mesopores of the carbon carrier. In order to suppress the temperature rise of the mixed liquid caused by the irradiation of ultrasonic waves, it is preferable to carry out the process while cooling the mixed dispersion liquid. For example, it is preferable to carry out the irradiation of ultrasonic waves in an ice bath. The ultrasonic irradiation of the mixed dispersion is not particularly limited as long as the ionic liquid is placed in the mesopores of the carbon support, but is preferably 30 W or more and 1000 W or less, more preferably 50 W or more and 500 W or less, and even more preferably 100 W or more and 400 W or less. The duration of ultrasonic irradiation of the mixed dispersion is not particularly limited as long as the ionic liquid is disposed within the mesopores of the carbon support, but is preferably from 0.1 hours to 3 hours, more preferably from 0.2 hours to 2.5 hours, and even more preferably from 0.5 hours to 2 hours. Thereafter, the linear bodies are added to the mixed dispersion, and the mixed dispersion is irradiated with ultrasonic waves to place the linear bodies in the mesopores of the carbon support under the above-mentioned various conditions. After the ionic liquid and the linear bodies are arranged on the surface of the carbon support, i.e., in the mesopores of the carbon support, the mixed dispersion is subjected to solid-liquid separation, and the solids are recovered, washed, and dried. For washing the solids, a mixture of ethanol and cyclohexane, for example, can be used.
[0067] The mass ratio of the ionic liquid to the carbon carrier contained in the dispersion is preferably 0.05 or more, more preferably 0.10 or more, and even more preferably 0.15 or more. The mass ratio of the ionic liquid to the carbon carrier is preferably 2.00 or less, more preferably 1.50 or less, and even more preferably 1.00 or less. By having the mass ratio of the ionic liquid to the carbon carrier within this range, the ionic liquid can be successfully present on the surface of the carbon carrier.
[0068] The electrode catalyst thus obtained can be used to form an electrode catalyst layer in a fuel cell. The electrode catalyst layer may contain, in addition to the electrode catalyst, a binder for binding the electrode catalysts together as necessary, an ionomer, or other materials similar to those known in the art.
[0069] The ionomer preferably has proton conductivity. The inclusion of an ionomer in the electrode catalyst layer further improves the performance of the catalyst layer. As the ionomer, for example, a polymer material having a structure in which a perfluoroether pendant side chain having a sulfonic acid group at the end is bonded to a polytetrafluoroethylene main chain can be used. As such an ionomer, for example, Nafion (registered trademark), Flemion (registered trademark), Aciplex (registered trademark), Fumion F (registered trademark), etc. can be mentioned.
[0070] The electrode catalyst layer is preferably formed, for example, by the following method. First, a dispersion liquid containing the electrode catalyst is prepared. To prepare the dispersion liquid, the electrode catalyst and a dispersion medium are mixed. When mixing, an ionomer is also added as necessary.
[0071] As the dispersion medium, for example, organic solvents such as alcohols, aromatic hydrocarbons such as toluene and benzene, aliphatic hydrocarbons such as hexane, other ketones, esters, ethers, and water can be used.
[0072] When an ionomer is used to form the electrode catalyst layer, the mass ratio of the ionomer to the carbon carrier contained in the electrode catalyst is preferably 0.10 to 4.00, more preferably 0.20 to 3.00, and even more preferably 0.30 to 2.30. When the mass ratio of the ionomer to the carbon carrier is within this range, the catalytic activity can be made higher than before.
[0073] Once the dispersion is obtained, an electrode catalyst layer is formed from the dispersion. The electrode catalyst layer is formed, for example, by applying the dispersion to an object to be coated using various coating devices to form a coating film, and then drying the coating film. The object to be coated may be, for example, a film of a fluorine-based resin such as polytetrafluoroethylene. The electrode catalyst layer formed on the object to be coated is superimposed on, for example, a solid electrolyte membrane and heat-pressed to transfer the electrode catalyst layer to the surface of the solid electrolyte membrane. This transfer results in a catalyst-coated membrane (CCM) in which the electrode catalyst layer is disposed on one surface of the solid electrolyte membrane.
[0074] The electrode catalyst layer thus formed is suitable for use as an electrode catalyst layer for the anode and / or cathode of a polymer electrolyte fuel cell. The anode and cathode preferably include an electrode catalyst layer and a gas diffusion layer. The gas diffusion layer functions as a supporting current collector having a current collecting function. Furthermore, the gas diffusion layer has a function of supplying sufficient gas to the electrode catalyst layer. The gas diffusion layer may be, for example, a porous material such as carbon paper or carbon cloth. Specifically, the gas diffusion layer may be formed of carbon cloth woven with a predetermined ratio of carbon fibers whose surfaces are coated with polytetrafluoroethylene and carbon fibers that are not coated.
[0075] Examples of solid electrolyte membranes include perfluorosulfonic acid polymer-based proton conductor membranes, membranes in which inorganic acids such as phosphoric acid are doped into hydrocarbon polymer compounds, organic / inorganic hybrid polymers in which a portion of the polymer is substituted with functional groups of a proton conductor, and proton conductors in which a polymer matrix is impregnated with a phosphoric acid solution or a sulfuric acid solution.
[0076] A membrane electrode assembly (MEA) consisting of an electrode catalyst layer, a solid electrolyte membrane, and a gas diffusion layer is provided with separators on each surface thereof to form a polymer electrolyte fuel cell. As the separator, for example, a separator having a plurality of protrusions (ribs) extending in one direction formed at a predetermined interval on the surface facing the gas diffusion layer can be used. A groove having a rectangular cross section is formed between adjacent protrusions. This groove is used as a flow path for supplying and discharging a fuel gas and an oxidant gas such as air. The fuel gas and the oxidant gas are supplied from a fuel gas supply means and an oxidant gas supply means, respectively. The separators arranged on each surface of the membrane electrode assembly may be arranged so that the grooves formed therein are perpendicular to each other, or may be arranged parallel to each other. The above configuration constitutes the minimum unit of a fuel cell, and a fuel cell can be constructed from a cell stack consisting of tens to hundreds of such configurations arranged in parallel.
[0077] In relation to the above-described embodiment, the following electrode catalyst, a method for producing the same, and a fuel cell are further disclosed. [1] A catalyst comprising a carbon support having mesopores and linear bodies of a catalytic metal, At least a portion of the linear bodies is located within at least a portion of the mesopores.
[0078] [2] The electrode catalyst according to [1], wherein the diameter of the linear body is smaller than the mesopore size of the carbon support. [3] The electrode catalyst according to [1] or [2], wherein the ratio of the diameter of the linear bodies to the mesopore size of the carbon support is 0.05 or more and less than 1.00. [4] The electrode catalyst according to any one of [1] to [3], wherein the linear body contains at least a platinum group element. [5] The electrode catalyst according to [4], wherein the linear body contains at least platinum. [6] The electrode catalyst according to any one of [1] to [5], wherein the mesopore diameter of the carbon support is 2.0 nm or more and 30.0 nm or less.
[0079] [7] The electrode catalyst according to any one of [1] to [6], wherein an ionic liquid is present on a surface of the carbon support. [8] The electrode catalyst according to [7], wherein the ionic liquid is an aprotic ionic liquid. [9] An electrode catalyst for a fuel cell comprising the electrode catalyst according to any one of [1] to [8].
[10] An electrode catalyst layer comprising the electrode catalyst according to any one of [1] to [8] and an ionomer.
[11] A fuel cell comprising the fuel cell electrode catalyst according to [9].
[12] A method for producing an electrode catalyst, comprising irradiating a dispersion containing a carbon support having mesopores and linear bodies of a catalytic metal with ultrasonic waves to arrange at least a portion of the linear bodies on a surface of the carbon support. EXAMPLES
[0080] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass".
[0081] Example 1-1 (1) Preparation of solutions A solution was prepared by mixing 0.025 mmol of bis(acetylacetonato)platinum(II) and 0.025 mmol of bis(acetylacetonato)nickel(II) as the catalytic metal source, 5 mL of oleylamine as the solvent, 0.075 mmol of molybdenum hexacarbonyl and 0.031 mmol of hexadecyltrimethylammonium chloride as the additive, and 0.33 mmol of glucose as the reducing agent.
[0082] (2) Heating, washing and drying of the solution The solution was heated at 160°C for 2 hours in an air atmosphere to reduce bis(acetylacetonato)platinum(II) and bis(acetylacetonato)nickel(II), yielding a solution in which linear bodies were produced. Next, a mixture of ethanol and cyclohexane in a volume ratio of 8:2 (hereinafter also referred to as "mixed solvent") was added to the solution, and the solution was washed by repeated centrifugation. The solid matter obtained was dried to obtain linear bodies. The diameter and aspect ratio of the obtained linear bodies were measured by the above-mentioned method. The composition of the obtained linear body was analyzed by total melting inductively coupled plasma mass spectrometry, and it was found that the linear body contained 95 atm % platinum and 5 atm % nickel. In addition, the platinum and nickel were alloyed in the linear body.
[0083] (3) Supporting linear bodies on carbon supports Carbon support with at least mesopores (mesopore diameter 14 nm, mesopore volume 1.8 mL / g, BET specific surface area 1007 m 2 / g) was prepared. The mesopore diameter of the carbon support was measured by the method described below. In addition, the mesopore volume of the carbon support was measured by the method described above. Next, a mixed solution was prepared by mixing 4.9 mg of the carbon support, 2.1 mg of the linear body, and 50 mL of the mixed solvent so that the amount of the linear body supported in the electrode catalyst was 30%. The mixed solution was placed in an ice bath, and ultrasonic waves were irradiated to the mixed solution at 220 W for 4 hours to obtain a dispersion solution in which the linear body was arranged in the mesopores of the carbon support. For the ultrasonic irradiation, an ultrasonic cleaner AU-80C manufactured by Aiwa Medical Industry Co., Ltd. was used. The mixed solvent was added to the dispersion solution and centrifuged repeatedly to wash it, and the obtained solid was vacuum dried to obtain an electrode catalyst.
[0084] [Example 1-2] (1) Preparation of mixed dispersion A carbon support having mesopores similar to those in Example 1-1 was prepared. In addition, an ionic liquid shown in Table 1 was prepared. A mixed dispersion was prepared by mixing 4.9 mg of the carbon support, 4.9 mg of the ionic liquid, and 50 mL of the mixed solvent so that the value of IL / C, which is the ratio of the mass (IL) of the ionic liquid to the mass (C) of the carbon support, was the value shown in Table 1.
[0085] (2) Supporting ionic liquid on carbon support The mixed dispersion was placed in an ice bath and ultrasonically irradiated to the mixed dispersion at 220 W for 1 hour to place the ionic liquid on the surface of the carbon support. (3) Supporting linear bodies on carbon supports The linear bodies obtained in the same manner as in Example 1 were used. 2.1 mg of linear bodies were added to the mixed dispersion. This mixed dispersion was placed in an ice bath, and ultrasonic waves were irradiated to the mixed dispersion at 220 W for 4 hours to place the linear bodies in the mesopores of the carbon support. A mixed solvent was added to the mixed dispersion, and the mixture was washed by repeated centrifugation, and the obtained solid was dried in vacuum to obtain an electrode catalyst.
[0086] Comparative Example 1-1 An electrode catalyst was obtained in the same manner as in Example 1-1, except that a solid carbon support (diameter 200 nm) was used instead of the carbon support having fine holes. The diameter of the carbon support was obtained by reading the diameters of 10 pieces from a transmission electron microscope image of the carbon support and calculating the arithmetic average.
[0087] Comparative Example 1-2 An electrocatalyst was obtained in the same manner as in Example 1-2, except that a solid carbon support (diameter 200 nm) similar to that in Comparative Example 1-1 was used instead of the carbon support having fine holes.
[0088] Comparative Example 1-3 As the electrode catalyst, a fuel cell catalyst (TEC10V30E manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) in which platinum particles are supported on a carbon support was used.
[0089] 〔evaluation〕 For the electrode catalyst obtained in Example 1-1, the location of the catalytic metal mainly in the carbon support was confirmed by 3D-TEM tomography using a transmission electron microscope. Specifically, based on the slice cross-section of the three-dimensional reconstruction image of the electrode catalyst obtained by 3D-TEM tomography, it was confirmed that the linear bodies containing platinum exist inside the particles of the carbon support. The electrode catalyst obtained in Example 1-2 was obtained by the same manufacturing method as in Example 1-1 except that an ionic liquid was used, so the location of the linear bodies in the carbon support is considered to be the same as in Example 1-1. In Comparative Examples 1-1 and 1-2, a solid carbon support in which mesopores do not exist inside the particles was used, so the linear bodies exist only on the surface of the carbon support. In Comparative Example 1-3, nanoparticles exist on the surface of the carbon support.
[0090] [Pore diameter of carbon support] The nitrogen adsorption and desorption isotherms were analyzed and measured. A gas adsorption amount measuring device "BELSORP-miniII" manufactured by Microtrack-Bell Corporation was used for the nitrogen adsorption and desorption measurement. The carbon carrier was heated in vacuum at 400°C for 3 hours using a pretreatment device "BELPREP-vacII" manufactured by Microtrack-Bell Corporation. Thereafter, the nitrogen adsorption and desorption isotherms were measured at liquid nitrogen temperature (77K) using "BELSORP-miniII". The obtained adsorption isotherms were analyzed using the BJH method, and the mesopore diameter of the carbon carrier in the range of 2 nm to 50 nm was calculated. The carbon carriers used in Comparative Examples 1-1 and 1-2 were solid carbon carriers in which mesopores did not exist inside the particles, so the description in Table 1 was "-".
[0091] [Table 1]
[0092] [Examples 2-1 to 2-6 and Comparative Examples 2-1 to 2-4] The electrode catalysts obtained in Examples 1-1 and 1-2 and Comparative Examples 1-1 to 1-3 were used to evaluate oxygen reduction activity by the following method. (1) Ink manufacturing process The catalyst ink of Example 2-1 was prepared by mixing and stirring 1.4 mg of the electrode catalyst, 1.6 mL of pure water, 0.9 mL of 2-propanol, and 5 μL of an ionomer (Nafion polymer dispersion DE520). The stirring was performed by ultrasonic stirring in an ice bath for 2 hours. The catalyst inks of Examples 2-2 to 2-6 and Comparative Examples 2-1 to 2-4 were prepared so that the mass ratio (I / C) of the ionomer to the carbon carrier was the value shown in Table 2.
[0093] (2) Thin film electrode formation process A rotating disk electrode (RDE) chip incorporating a glassy carbon (GC) electrode was attached to a rotating ring disk electrode (Pine Research, AFMSRCE) and 20 μL of the prepared catalyst ink was dropped onto the GC electrode while rotating at 700 rpm. The amount of metal supported at this time was 17 μg / cm. 2 The catalyst was then evenly fixed on the GC electrode by drying. The GC electrode was then removed from the RDE chip and heated at 145°C for 5 minutes in air, after which the GC electrode was reassembled into the RDE chip.
[0094] 〔evaluation〕 The oxygen reduction activity was evaluated by the rotating disk electrode method. A three-electrode electrochemical cell was used. A glassy carbon disk electrode was used as the working electrode, a platinum mesh was used as the counter electrode, and a reversible hydrogen electrode was used as the working electrode. A 0.1 mol / L aqueous perchloric acid solution was used as the electrolyte, and measurements were performed at room temperature. The electrode surface was cleaned by performing a potential variation cycle by cyclic voltammetry while bubbling argon gas in advance, and the electrochemically active surface area (ECSA) was calculated based on the hydrogen desorption wave. After that, oxygen was bubbled into the electrolyte to saturate it, and the electrode was rotated while oxygen was flowed over the liquid surface, and the oxygen reduction activity at a potential of 0.9 V was evaluated by linear sweep voltammetry. The oxygen reduction activity value was calculated from the Koutecky-Levich plot. The results are shown in Table 2 below.
[0095] [Table 2]
[0096] As is clear from the results shown in Table 2, Examples 2-1 to 2-6 exhibit higher catalytic activity than Comparative Examples 2-1 to 2-4. In addition, among the electrode catalysts in which linear bodies are located in the mesopores of the carbon support, Example 2-4, in which ionic liquid and linear bodies of the catalytic metal are located in the mesopores, shows particularly high catalytic activity compared to Example 2-2, in which linear bodies of the catalytic metal are located in the mesopores but no ionic liquid is present. This is thought to be because the presence of the ionic liquid in the mesopores suppresses the poisoning of the electrode catalyst by the ionomer.
Claims
1. A carbon support having mesopores and linear bodies of a catalytic metal, At least a portion of the linear bodies is located within at least a portion of the mesopores.
2. The electrode catalyst according to claim 1 , wherein the diameter of the filaments is smaller than the mesopore size of the carbon support.
3. 3. The electrode catalyst according to claim 1, wherein a ratio of a diameter of the linear bodies to a diameter of the mesopores of the carbon support is 0.05 or more and less than 1.
00.
4. The electrode catalyst according to claim 1 or 2, wherein the linear bodies contain at least a platinum group element.
5. The electrode catalyst according to claim 4 , wherein the linear bodies contain at least platinum.
6. 3. The electrode catalyst according to claim 1, wherein the mesopore diameter of the carbon support is 2.0 nm or more and 30.0 nm or less.
7. 3. The electrode catalyst according to claim 1, wherein an ionic liquid is present on the surface of the carbon support.
8. The electrocatalyst of claim 7 , wherein the ionic liquid is an aprotic ionic liquid.
9. An electrode catalyst for a fuel cell comprising the electrode catalyst according to claim 1 or 2.
10. An electrode catalyst layer comprising the electrode catalyst according to claim 1 or 2 and an ionomer.
11. A fuel cell comprising the fuel cell electrode catalyst according to claim 9.
12. A method for producing an electrode catalyst, comprising: irradiating a dispersion containing a carbon support having mesopores and linear bodies of a catalytic metal with ultrasonic waves to arrange at least a portion of the linear bodies on a surface of the carbon support.
Citation Information
Patent Citations
Electrode catalyst for fuel cell, and method for manufacturing the same
JP2018098198A
Fuel cell catalyst and manufacturing method thereof
JP2021190418A
Catalyst, electrode catalyst layer using same, membrane electrode assembly and fuel cell
WO2014175099A1