Α-sialon phosphor and light-emitting device

By optimizing the composition and manufacturing process of α-sialon phosphors with specific thermal expansion coefficients, the luminescent properties and thermal stability are enhanced, addressing the need for improved performance in white LEDs.

JP2024146310AActive Publication Date: 2024-10-15DENKA CO LTD

Patent Information

Application Number
JP2023059122
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

The increasing demand for improved luminescent properties in α-sialon phosphors, particularly those activated with rare earth elements, has not been adequately met by existing technologies, necessitating the development of phosphors with enhanced fluorescence efficiency and thermal stability for use in white LEDs.

Method used

The development of an α-type Sialon phosphor with specific compositional and structural parameters, including a general formula (Ca x ,Eu y )(Si 12-(m+n)Al m+n )(O n N 16-n ) and controlled thermal expansion coefficients, optimized through manufacturing processes such as annealing and hydrogen gas annealing, to enhance luminescent properties and thermal stability.

Benefits of technology

The resulting α-sialon phosphor exhibits improved luminescent characteristics and thermal stability, facilitating efficient conversion of blue light into longer wavelengths, thereby enhancing the performance of white LEDs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146310000001_ABST
    Figure 2024146310000001_ABST
Patent Text Reader

Abstract

To provide an α-sialon phosphor with improved luminescence properties.SOLUTION: An α-sialon phosphor is represented by a general formula (Cax,Euy)(Si12-(m+n)Alm+n)(OnN16-n), and has an average coefficient of linear expansion α' at 25-900°C from 4.2 ppm / °C to 4.6 ppm / °C inclusive. In the general formula, 0<x<2.0, 0<y≤0.5, 0.3≤x+y≤2.0, 0<m≤4.0, and 0<n≤3.0 are satisfied.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an α-sialon phosphor and a light emitting device. [Background technology]

[0002] Alpha-SiAlON phosphors activated with rare earth elements such as Eu can efficiently convert blue light into long-wavelength light, and are therefore used as wavelength conversion materials for white LEDs, for example.

[0003] In α-type sialon phosphors, the Si-N bonds of α-type silicon nitride crystals are usually partially replaced with Al-N bonds and Al-O bonds, and in order to maintain electrical neutrality, certain elements (Ca, Li, Mg, Y, or lanthanide metals excluding La and Ce) are intercalated and dissolved between the crystal lattices. Fluorescence properties are expressed by making some of the intercalated and dissolved elements rare earth elements that become the emission center. Among them, α-type sialon phosphors in which Ca is solid-dissolved and part of it is replaced with Eu are excited relatively efficiently in a wide wavelength range from ultraviolet to blue, and emit yellow or orange light.

[0004] In order to further improve the fluorescent properties of α-sialon phosphors, various attempts have been proposed (for example, Patent Documents 1 to 3, etc.). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-96882 A [Patent Document 2] Patent No. 6667025 [Patent Document 3] Patent No. 6785333 Summary of the Invention [Problem to be solved by the invention]

[0006] With the popularization of white LEDs, the performance requirements for α-sialon phosphors are increasing more and more.

[0007] The present inventors have conducted various studies in order to obtain an α-sialon phosphor having improved light emission characteristics this time.

Means for Solving the Problems

[0008] The present inventors have completed the invention provided below through various studies.

[0009] 1. An α-sialon phosphor represented by the following general formula and having an average linear expansion coefficient α´ at 25 to 900 °C of 4.2 ppm / °C or more and 4.6 ppm / °C or less. General formula: (Ca x , Eu y )(Si 12-(m+n) Al m+n )(O n N 16-n ) In the above general formula, x, y, m and n satisfy the following. 0 < x < 2.0 0 < y ≤ 0.5 0.3 ≤ x + y ≤ 2.0 0 < m ≤ 4.0 0 < n ≤ 3.0 2. The α-sialon phosphor according to 1., where 2.5 ≤ m ≤ 4.0 and 0 < n ≤ 0.5. 3. The α-sialon phosphor according to 1. or 2., where when the average linear expansion coefficient at 25 to 300 °C is α1´ and the average linear expansion coefficient at 700 to 900 °C is α2´, α2´ / α1´ is 1.3 to 1.8. 4. The α-sialon phosphor according to any one of 1. to 3., where at 25 °C, the lattice constant a 25 of the unit cell is 7.900 Å or more and 7.960 Å or less, and the lattice constant c 25The α-sialon phosphor has a surface roughness of 5.720 Å or more and 5.780 Å or less. 5. An α-sialon phosphor according to any one of 1. to 4., At 25°C, the lattice volume of the unit cell is V 25 is 308 Å 3 More than 320 Å 3 The α-SiAlON phosphor is shown below. 6. A light-emitting element; A wavelength conversion section that includes the α-sialon phosphor according to any one of 1. to 5. and converts the wavelength of light emitted from the light-emitting element into a longer wavelength light. A light emitting device comprising: Effect of the Invention

[0010] According to the present invention, there is provided an α-sialon phosphor having improved luminescence characteristics. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic cross-sectional view illustrating a structure of a light emitting device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The drawings are for illustrative purposes only. The shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products.

[0013] In this specification, unless otherwise specified, the expression "X to Y" in the explanation of a numerical range means from X to Y. For example, "1 to 5% by mass" means "from 1% by mass to 5% by mass".

[0014] <α-type Sialon phosphor> The α-sialon phosphor of this embodiment is General formula: (Ca x ,EU y )(Si 12-(m+n) Al m+n)(O n N 16-n ) It is expressed as: In the above general formula, x, y, m and n satisfy the following: 0 <x<2.0 0 <y≦0.5 0.3≦x+y≦2.0 0 <m≦4.0 0 <n≦3.0

[0015] Moreover, the average linear expansion coefficient α' of the α-sialon phosphor of this embodiment at 25 to 900°C is 4.2 ppm / °C or more and 4.6 ppm / °C or less.

[0016] The α-sialon phosphor of this embodiment has good light emission characteristics. Although the reason for this is not necessarily clear, it is presumed that the α-sialon phosphor of this embodiment has a crystal structure that easily emits fluorescence efficiently, taking into consideration that m and n in the above general formula are within specific numerical ranges, and that the thermal expansion coefficient is considered to be an index that can correlate with the crystal structure.

[0017] In this embodiment, the average linear expansion coefficient α' can be obtained by measuring and analyzing the relationship between temperature and lattice constant, for example, as shown in the following [One example of a procedure for obtaining the average linear expansion coefficient α']. For details on how to obtain the average linear expansion coefficient α', please refer to the examples described later.

[0018] [An example of a procedure for calculating the average linear expansion coefficient α'] (1) X-ray diffraction measurement of the α-sialon phosphor is performed at several points within the temperature range of 25 to 900°C. (2) From the results of the X-ray diffraction measurement, the lattice constant of the crystal in the phosphor at each temperature T is obtained. In the case of an α-type SiAlON phosphor, the lattice constant a T and c T In the crystal structure of α-SiAlON, the lattice constant b T is a T will be the same value. (3) Temperature T - Lattice constant a T , temperature T - lattice constant c TCreate a graph on which each of the above is plotted. Then, find the approximate straight line equation for each graph. The approximate straight line can be determined using the least squares method. (4) From the approximation line, the lattice constant a at 25°C 25 and c 25 , and the lattice constant a at 900°C 900 and c 900 Read these values ​​and use them in formula 1 below. 25 and V 900 Substituting into the formula, the lattice volume at 25°C V 25 and the lattice volume V at 900°C 900 Then, calculate the volume expansion coefficient β based on the following formula 2.

[0019]

number

[0020]

number

[0021] (5) Calculate the average linear expansion coefficient α' using the formula α' = β / 3. This formula α' = β / 3 is used to calculate the average linear expansion coefficient of a polycrystalline material, assuming that the sample is an isotropic material.

[0022] The α-sialon phosphor of this embodiment can be produced by using appropriate raw materials in appropriate amounts and by adopting appropriate production conditions. "Using appropriate materials in appropriate amounts" includes adjusting the amounts of raw materials so as to satisfy x, y, m, and n in the general formula given above. Regarding "appropriate manufacturing conditions," which will be described in detail later, an "annealing process" in an inert gas atmosphere such as nitrogen gas and a "hydrogen annealing process" in a hydrogen gas atmosphere can be mentioned. By adopting appropriate manufacturing methods and conditions, the α-sialon phosphor of the present embodiment can be manufactured. Conversely, if appropriate manufacturing methods and conditions are not adopted, even if appropriate materials are used in appropriate amounts, the α-sialon phosphor of the present embodiment may not be obtained.

[0023] Continue the description of the α-sialon phosphor of the present embodiment.

[0024] (General formula: (Ca x , Eu y )(Si 12-(m+n) Al m+n )(O n N 16-n )) x only needs to satisfy 0 < x < 2.0, preferably 1.0 ≤ x < 2.0, more preferably 1.3 ≤ x < 2.0, y only needs to satisfy 0 < y < 0.5, preferably 0.01 ≤ y ≤ 0.1, x + y only needs to satisfy 0.3 ≤ x + y ≤ 2.0, preferably 1.0 ≤ x + y ≤ 2.0, more preferably 1.3 ≤ 2.0, m only needs to satisfy 0 < m ≤ 4.0, preferably 2.5 ≤ m ≤ 4.0, more preferably 2.8 ≤ m ≤ 4.0, n only needs to satisfy 0 < n ≤ 3.0, preferably 0 < n ≤ 0.5, more preferably 0.1 ≤ n ≤ 0.4.

[0025] By optimizing x, y, x + y, m, and n, the luminescence characteristics of the α-sialon phosphor may be further enhanced. Also, by optimizing x, y, x + y, m, and n, it may become easier to more appropriately control the average linear expansion coefficient α'.

[0026] (Regarding lattice constant and lattice volume) The lattice constant a of the unit cell of the α-sialon phosphor of the present embodiment at 25°C 25is preferably 7.900 Å or more and 7.960 Å or less, and the lattice constant c 25 is preferably 5.720 Å or more and 5.780 Å or less. Incidentally, in the crystal structure of α-SiAlON, the lattice constant b 25 is a 25 will be the same value. In addition, the lattice volume V of the unit lattice of the α-SiAlON phosphor of this embodiment at 25° C. 25 is preferably 308 Å 3 More than 320 Å 3 The following is the result. As described above, the α-sialon of the present embodiment is presumed to have a crystal structure that is likely to efficiently emit fluorescence. The numerical ranges of these lattice constants are considered to reflect the "crystal structure that is likely to efficiently emit fluorescence." The above values ​​can be determined by the Pawley method.

[0027] (Average linear expansion coefficient at low temperatures and average linear expansion coefficient at high temperatures) In the α-sialon phosphor of this embodiment, the average linear expansion coefficient at low temperatures and the average linear expansion coefficient at high temperatures are within appropriate numerical ranges, so that the light emitting characteristics can be further improved in some cases. Specifically, when the average linear expansion coefficient of the α-sialon phosphor of this embodiment at 25 to 300°C is α1' and the average linear expansion coefficient at 700 to 900°C is α2', α2' / α1' is preferably 1.3 to 1.8, more preferably 1.3 to 1.7, and even more preferably 1.3 to 1.6.

[0028] The method for determining α1' and α2' will now be described in detail.

[0029] How to calculate the average linear expansion coefficient α1´ at 25~300℃ (1) Lattice constant a obtained by the Pawley method 25 ,c 25 (The definitions of these symbols are the same as above) are substituted into the following formula, and the lattice volume at 25°C V 25 Incidentally, since the crystal structure of α-sialon is hexagonal, the lattice volume is expressed by this formula.

[0030]

number

[0031] (2) Similarly, the lattice constant a at 300°C 300 ,c 300 Using the value of , the lattice volume at 300℃ V 300 Calculate.

[0032] (3) Calculate the volume expansion coefficient β1 according to the following formula. ΔT is 300℃-25℃=275℃.

[0033]

number

[0034] (4) Assuming that the sample is an isotropic material, calculate the average linear expansion coefficient α1' as a polycrystalline body using the formula α1' = β1 / 3.

[0035] How to calculate the average linear expansion coefficient α2´ at 700~900℃ (1) The lattice constant a at 700℃ was calculated by the Pawley method. 700 , c 700 Find the value of . Substituting the following equation, the lattice volume at 700℃ V 700 Incidentally, since the crystal structure of α-sialon is hexagonal, the lattice volume is expressed by this formula.

[0036]

number

[0037] (2) Similarly, the lattice constant a at 900°C 900 , c 900 Then, calculate the lattice volume V at 900℃. 900 Calculate.

[0038] (3) Calculate the volume expansion coefficient β2 using the following formula. ΔT is 900℃-700℃=200℃.

[0039]

number

[0040] (4) Assuming that the sample is an isotropic material, calculate the average linear expansion coefficient α2' as a polycrystalline body using the formula α2' = β2 / 3.

[0041] (About the characteristics) The α-sialon phosphor of this embodiment is typically in powder form. The lower limit of the median diameter D50 of the powdered α-SiAlON phosphor particles is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. The upper limit of the median diameter D50 is preferably 30 μm or less, more preferably 20 μm or less. By making the median diameter D50 5 μm or more, the transparency of the composite described below can be further improved. On the other hand, by making the median diameter D50 30 μm or less, chipping can be suppressed when cutting the composite with a dicer or the like. The median diameter D50 can be determined by a laser diffraction scattering method in accordance with JIS R1629: 1997. For more specific measurement methods, see the examples given later.

[0042] <Method of manufacturing α-SiAlON phosphor> As described above, the α-sialon phosphor of this embodiment can be produced by using appropriate raw materials in appropriate amounts and by adopting appropriate production conditions. An example of the production method will be described below.

[0043] Raw material mixing First, raw materials containing elements that constitute Eu-containing α-SiAlON phosphor particles are mixed. In α-SiAlON phosphor particles with a low oxygen content synthesized using calcium nitride as the calcium raw material, calcium is dissolved in a high concentration. In particular, when the Ca solid solution concentration is high, a phosphor is obtained that has an emission peak wavelength on the higher wavelength side (590 nm or more, more specifically 590 nm to 610 nm, and even more specifically 592 nm to 608 nm) than the conventional composition using oxide raw materials.

[0044] Other examples of raw material powders include silicon nitride, aluminum nitride, and Eu compounds. Eu compounds include europium oxide, compounds that become europium oxide after heating, and europium nitride. Europium nitride is preferred because it can reduce the amount of oxygen in the system.

[0045] An appropriate amount of pre-synthesized α-sialon phosphor particles may be added to the raw material powder. These phosphor particles may become the starting point for grain growth, and it may be possible to obtain α-sialon phosphor particles with a relatively large minor axis diameter. In addition, it may be possible to control the grain shape by changing the shape of the α-sialon particles to be added.

[0046] Methods for mixing the raw materials include dry mixing and wet mixing in an inert solvent that does not substantially react with the raw material components, followed by removal of the solvent. Mixing equipment includes V-type mixers, rocking mixers, ball mills, and vibration mills. Mixing calcium nitride, which is unstable in air, is preferably carried out in a glove box with an inert atmosphere, as its hydrolysis and oxidation will affect the properties of the synthesized product.

[0047] Heat treatment (firing) The powder obtained by mixing (hereinafter simply referred to as raw material powder) is filled into a container made of a material that is low in reactivity with the raw materials and the phosphor to be synthesized, such as a boron nitride container. Then, it is heated for a predetermined time in a nitrogen atmosphere. In this way, an α-sialon phosphor can be obtained. The temperature of the heat treatment is preferably 1650°C or higher and 1950°C or lower. By setting the heat treatment temperature at 1650°C or higher, the amount of remaining unreacted products can be suppressed and primary particles can be grown sufficiently. Also, by setting the heat treatment temperature at 1950°C or lower, significant sintering between particles can be suppressed.

[0048] It is preferable to pack the raw material powder in a container so that the raw material powder has a high bulk in order to suppress interparticle sintering during heating. Specifically, the raw material powder is packed in a container so that the bulk density is 0.6 g / cm 3 It is preferable that:

[0049] The heating time in the heat treatment is preferably in the range of 2 hours to 24 hours, which is a time range that does not cause inconveniences such as the presence of a large amount of unreacted matter, insufficient growth of primary particles, or sintering between particles.

[0050] The above-mentioned process produces an α-sialon phosphor having an ingot-shaped external shape. This ingot-shaped α-sialon phosphor is subjected to a crushing process using a crusher, mortar crusher, ball mill, vibration mill, jet mill, or other crushing machine, and a sieve classification process after the crushing process, to obtain a powdered α-sialon phosphor with an adjusted secondary particle size. In addition, the particle size of the secondary particles can be adjusted by performing a process of dispersing the phosphor in an aqueous solution and removing secondary particles that are small in particle size and do not easily settle.

[0051] Annealing process In this embodiment, the powdered α-sialon phosphor obtained through the heat treatment is preferably heated (annealed) in a nitrogen atmosphere. In this specification, the heat treatment in a nitrogen atmosphere is referred to as the "annealing step". The heating temperature in the annealing step is preferably 1300 to 1600°C, more preferably 1400 to 1500°C. A heating temperature of 1600°C or higher is not preferred because it may cause decomposition of the α-sialon and volatilization of Eu, which is the luminescence center. Also, a heating temperature of 1300°C or lower is not preferred because it may not be possible to sufficiently improve the crystallinity. The heating temperature in the annealing step is preferably lower than the heating temperature in the above-mentioned heating step (firing).

[0052] The pressure in the annealing step is preferably atmospheric pressure or near atmospheric pressure, specifically 0.02 to 0.9 MPa (gauge pressure). The time for the annealing step is preferably 5 to 20 hours, more preferably 10 to 18 hours.

[0053] Hydrogen gas annealing process After the annealing step, the treated product obtained in the annealing step is heat-treated in a hydrogen gas atmosphere. In this specification, this step is referred to as a "hydrogen gas annealing step." In the hydrogen gas annealing step, it is preferable to cool the α-SiAlON phosphor after the annealing step to about room temperature and then heat-treat it in a hydrogen gas atmosphere. By performing the annealing step and the hydrogen gas annealing step consecutively, the fluorescent properties are significantly improved.

[0054] According to the knowledge of the present inventors, the hydrogen gas annealing process is a process for reducing defects in the phosphor. It is believed that the heat treatment in a hydrogen gas atmosphere allows hydrogen gas to enter the crystal and stabilize the crystal defects. As a result, it is believed that an α-SiAlON phosphor with an average linear expansion coefficient α' of 4.2 ppm / °C or more and 4.6 ppm / °C or less and with good luminescence characteristics can be obtained.

[0055] The heating temperature in the hydrogen gas annealing step is preferably 1300 to 1600° C., and more preferably 1400 to 1500° C. If the heating temperature is below 1300° C., the hydrogen gas does not penetrate into the crystal lattice and the effect is difficult to obtain, while if it is above 1600° C., the crystal structure of the α-SiAlON phosphor may decompose. In addition, the heating temperature in the hydrogen gas annealing step is preferably set to a temperature lower than the heating temperature in the firing step.

[0056] The pressure in the hydrogen gas annealing step is preferably atmospheric pressure or near atmospheric pressure, specifically 0.02 to 0.9 MPa (gauge pressure). The time for the hydrogen gas annealing step is preferably 3 to 16 hours, and more preferably 5 to 12 hours.

[0057] The purity of the hydrogen gas used in the hydrogen gas annealing step is preferably 99% or more, and more preferably 99.9% or more. However, as long as the α-SiAlON phosphor of this embodiment can be obtained, the hydrogen gas annealing step may use a mixed gas of hydrogen gas and other gases. Examples of the other gases include nitrogen gas and rare gases such as argon gas. The mixed gas preferably contains 30 vol% or more of hydrogen gas, and more preferably contains 40 vol% or more of hydrogen gas.

[0058] Acid treatment process In this embodiment, it is preferable to carry out an acid treatment after carrying out the above-mentioned steps, which may reduce heterogeneous phases that do not contribute to light emission or that cause deterioration of the light emission characteristics, thereby further improving the light emission characteristics.

[0059] In the acid treatment step, for example, the α-sialon phosphor is immersed in an acidic aqueous solution. The acidic aqueous solution may be an acidic aqueous solution containing one acid selected from acids such as hydrofluoric acid, nitric acid, and hydrochloric acid, or a mixed acid aqueous solution obtained by mixing two or more of the above acids. Among these, an aqueous hydrofluoric acid solution containing only hydrofluoric acid and an aqueous mixed acid solution obtained by mixing hydrofluoric acid and nitric acid are more preferable. The concentration of the original solution of the acidic aqueous solution is appropriately set depending on the strength of the acid used, and is preferably, for example, 0.7% to 100%, more preferably 0.7% to 40%. In addition, the temperature when carrying out the acid treatment is preferably 60°C to 90°C, and the reaction time (immersion time) is preferably 15 minutes to 80 minutes.

[0060] Stirring at high speed makes it easier to sufficiently treat the phosphor surface with acid. Here, "high speed" depends on the stirring device used, but when a laboratory-level magnetic stirrer is used, the stirring speed is, for example, 400 rpm or more, and in reality, 400 rpm to 500 rpm. For the normal purpose of stirring, which is to constantly supply new acid to the particle surface, a stirring speed of about 200 rpm is sufficient, but by stirring at high speeds of 400 rpm or more, the particle surface can be sufficiently treated by physical actions in addition to chemical actions.

[0061] <Light emitting device> FIG. 1 is a schematic cross-sectional view illustrating the structure of a light emitting device. As shown in FIG. 1, the light emitting device 100 includes a light emitting element 120, a heat sink 130, a case 140, a first lead frame 150, a second lead frame 160, bonding wires 170 and 172, and a composite body 40. The light emitting device 100 includes a light emitting element 120, a heat sink 130, a case 140, a first lead frame 150, a second lead frame 160, bonding wires 170 and 172, and a composite body 40.

[0062] The light emitting element 120 is mounted in a predetermined region on the upper surface of the heat sink 130. By mounting the light emitting element 120 on the heat sink 130, it is possible to improve the heat dissipation properties of the light emitting element 120. Note that a packaging substrate may be used instead of the heat sink 130.

[0063] The light emitting element 120 is a semiconductor element that emits excitation light. For example, an LED chip that emits light with a wavelength of 300 nm to 500 nm, which corresponds to near ultraviolet to blue light, can be used as the light emitting element 120. One electrode (not shown) disposed on the upper surface side of the light emitting element 120 is connected to the surface of the first lead frame 150 via a bonding wire 170 such as a gold wire. The other electrode (not shown) formed on the upper surface of the light emitting element 120 is connected to the surface of the second lead frame 160 via a bonding wire 172 such as a gold wire.

[0064] A generally funnel-shaped recess whose hole diameter gradually increases from the bottom surface toward the top is formed in the case 140. The light emitting element 120 is provided on the bottom surface of the recess. The wall surface of the recess surrounding the light emitting element 120 serves as a reflector.

[0065] The composite 40 is filled in the recess whose wall surface is formed by the case 140. The composite 40 is a wavelength conversion member that lengthens the wavelength of the excitation light emitted from the light emitting element 120. The composite of this embodiment is used as the composite 40, and the phosphor 1 of this embodiment is dispersed in a sealing material 30 such as a resin. The light emitting device 100 emits a mixed color of the light of the light emitting element 120 and the light generated from the phosphor 1 that is excited by absorbing the light of the light emitting element 120. It is preferable that the light emitting device 100 emits white light by mixing the light of the light emitting element 120 and the light generated from the phosphor 1.

[0066] Incidentally, examples of resins that can be used for the sealing material 30 in the composite 40 include transparent resins such as silicone resin, epoxy resin, and urethane resin. The composite 40 can be produced, for example, by adding the α-sialon phosphor of this embodiment to liquid resin or powdered glass or ceramics, mixing them uniformly, and then curing or sintering them by heat treatment.

[0067] The light emitting device 100 of this embodiment uses the above-mentioned α-sialon phosphor as the phosphor 1, and thus has excellent light emitting characteristics.

[0068] Incidentally, although a surface mount type light emitting device is illustrated in FIG. 1, the light emitting device is not limited to the surface mount type, and may be a bullet type, a COB (chip on board) type, or a CSP (chip scale package) type.

[0069] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0070] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. It should be noted that the present invention is not limited to the Examples.

[0071] <Example 1: Production of α-type Sialon phosphor> In a glove box, 60.14% by mass of Si3N4 powder (manufactured by Ube Industries, Ltd., E10 grade), 23.96% by mass of AlN powder (manufactured by Tokuyama Corporation, E grade), 2.07% by mass of EuN powder (manufactured by Kojundo Chemical Laboratory Co., Ltd.) and 13.83% by mass of Ca3N2 powder (manufactured by Kojundo Chemical Laboratory Co., Ltd.) were dry-blended so that the m value was 3.75, the n value was 0, the x value was 1.795, and the y value was 0.08, and then the mixture was passed through a nylon sieve with an opening of 250 μm. In this way, a raw material mixed powder was obtained. 120 g of this mixed raw material powder was packed into a cylindrical boron nitride container with an internal volume of 0.4 liters and a lid (manufactured by Denka Co., Ltd., N-1 grade).

[0072] The container filled with the raw material mixed powder was heat-treated in an electric furnace equipped with a carbon heater in a nitrogen atmosphere at atmospheric pressure at 1800°C for 16 hours. Since calcium nitride contained in the raw material mixed powder is easily hydrolyzed in air, the boron nitride container filled with the raw material mixed powder was quickly set in the electric furnace after being removed from the glove box and immediately evacuated to prevent the calcium nitride from reacting.

[0073] The synthesized product was lightly crushed in a mortar and passed through a sieve with 150 μm openings to obtain a phosphor powder. When the crystal phase of this phosphor powder was examined by powder X-ray diffraction measurement (hereinafter referred to as XRD measurement) using CuKα radiation, the crystal phase present was found to be α-sialon.

[0074] The boron nitride container filled with the obtained phosphor powder was heat-treated in an electric furnace equipped with a carbon heater in a nitrogen atmosphere at atmospheric pressure at 1400°C for 16 hours (annealing step). The composite was lightly crushed in a mortar and passed through a sieve with 150 μm openings to obtain phosphor powder. The boron nitride container filled with the phosphor powder was then heat-treated in an electric furnace equipped with a metal heater in a hydrogen atmosphere at atmospheric pressure at 1400°C for 16 hours (hydrogen annealing step). The composite was lightly crushed in a mortar and passed through a sieve with 150 μm openings to obtain phosphor powder.

[0075] Next, 50 ml of 50% hydrofluoric acid and 50 ml of 70% nitric acid were mixed to prepare a mixed stock solution. 300 ml of distilled water was added to the mixed stock solution to dilute the concentration of the mixed stock solution to 25%, and 400 ml of mixed acid aqueous solution was prepared. 30 g of the powder consisting of the above-mentioned α-type sialon phosphor particles was added to this mixed acid aqueous solution, and acid treatment was performed by immersing the powder for 60 minutes while keeping the temperature of the mixed acid aqueous solution at 80°C and stirring it at a rotation speed of 450 rpm using a magnetic stirrer. After the acid treatment, the powder was thoroughly washed with distilled water to remove the acid, filtered, dried, and then passed through a sieve with an opening of 45 μm. In this manner, a powdered α-sialon phosphor was obtained.

[0076] The composition of the obtained α-sialon phosphor was analyzed to determine x, y, x+y, m, and n in the general formula. The specific method of the composition analysis is as follows.

[0077] The Eu, Ca, Si, and Al contents in the phosphor were quantitatively analyzed using an ICP emission spectrometer (SPECTRO Corporation, CIROS-120) after dissolving the α-SiAlON phosphor by pressure acid decomposition. The O and N contents in the phosphor were quantitatively analyzed using an oxygen and nitrogen analyzer (EMGA-920, manufactured by Horiba, Ltd.). The composition analysis results were found to be consistent with the general formula (Ca x ,EU y )(Si 12-(m+n) Al m+n )(On N 16-n ), the m value was 3.5, the n value was 0.27, the x value was 1.63, the y value was 0.05, and the x+y value was 1.68.

[0078] <Calculation of lattice constant and average linear expansion coefficient> (X-ray diffraction measurement) The α-SiAlON phosphor was placed on a sample plate, and the sample was spread out with a glass plate so that the sample surface was flush with the sample plate surface. X-ray diffraction measurements were then performed under the following conditions. Si (NIST SRM 640c, hereafter also referred to as "Si_640c") was also measured as an angle standard sample (external standard). Equipment: Rigaku X-ray diffraction equipment Ultima IV Optical system: Parallel beam method X-ray source: Cu sealed tube Applied voltage / current: 40kV / 40mA Detector: Scintillation counter Measurement stage High temperature specimen equipment Measurement atmosphere N2 flow (30mL / min) Setting temperature 25℃, 300℃, 500℃, 700℃, 900℃ (other than Si_640c) 25℃(Si_640c) Heating rate: 20℃ / min Interval 10min Measurement angle range 2θ=24~140° Sampling width 0.04° Scan speed: 2° / min Repeated measurements 4 times (except Si_640c) 3 times (Si_640c) Slit configuration: Incident side solar slit: 5.0°, receiving side solar slit: 5.0° thin film PSA DS: 1mm, DS vertical: 10mm, SS: open, RS: open Sample plate made of Pt

[0079] (Calculation of lattice constant) In the above X-ray diffraction measurement, the results of the measurements at each temperature (25°C, 300°C, 500°C, 700°C, 900°C) were used to perform analysis using the powder X-ray diffraction pattern comprehensive analysis software Jade 9 manufactured by Materials Data. This allowed precise calculation of the lattice constant. The conditions for the analysis are described below. Method Pawley method Analysis temperature 25℃, 300℃, 500℃, 700℃, 900℃ Angle range 2θ=24~140°(Note 1) Background 4th-Order Polynomial Refinement Peak shift zero point correction 2θ 0.005948 (Note 2) Sample displacement cosθ 0 (fixed) Vertical divergence cot(2θ) -0.012557 (Note 2) Peak shape pseudo-Voigt function Peak intensity ratio refinement (Note 1: In the analysis by the Pawley method in the angle range 2θ = 24 to 140°, when diffraction lines other than those of α-SiAlON were observed, these diffraction lines were appropriately excluded before the analysis was performed.) (Note 2: The measurement results of a standard sample (Si_640c) were analyzed and the values ​​obtained were used.)

[0080] (Calculation of volume expansion rate) (1) Lattice constant a for measurement temperature T T and c T A graph was created by plotting the above. An approximate linear equation was then obtained for the range from 25 to 900°C. The approximate linear equation can be obtained by the least squares method. T and b T will have the same value. (2) Using the approximate linear equation, the lattice constant a at 25°C 25 and c 25 was calculated. (3) Using the approximate linear equation, the lattice constant a at 900°C 900 and c 900 was calculated. (4) Lattice constant a 25and c 25 Using the value of , the lattice volume at 25 °C V 25 was calculated (Note 3). (5) Lattice constant a 900 and c 900 Using the value of , the lattice volume at 900℃ V 900 was calculated (Note 3). (6) The volume expansion coefficient β was calculated using the following formula, where ΔT is 900℃-25℃=875℃. (Note 3: The crystal structure of α-SiAlON is hexagonal.)

[0081]

number

[0082] (Calculation of average linear expansion coefficient) The average linear expansion coefficient α' was calculated using the formula α' = β / 3. Incidentally, this formula α' = β / 3 is used to calculate the average linear expansion coefficient of a polycrystalline body, assuming that the sample is an isotropic material.

[0083] (Calculation of average linear expansion coefficient α1' at 25-300°C and average linear expansion coefficient α2' at 700-900°C) According to the series of procedures described above, the average linear expansion coefficient α1' at 25 to 300° C. and the average linear expansion coefficient α2' at 700 to 900° C. were calculated.

[0084] (Measurement of particle size distribution and calculation of median size) Measurements were performed using a Microtrac MT3300EX II (Microtrac Bell Corporation) using the laser diffraction scattering method in accordance with JIS R1629:1997. Specifically, 0.5 g of powdered α-SiAlON phosphor was added to 100 cc of ion-exchanged water, and a dispersion was performed for 3 minutes using an Ultrasonic Homogenizer US-150E (Nihon Seiki Seisakusho Co., Ltd., tip size φ20 mm, Amplitude 100%, oscillation frequency 19.5 KHz, amplitude approximately 31 μm) to obtain a dispersion. This dispersion was set in an MT3300EX II to measure the particle size distribution. The median diameter D50 was calculated from the obtained particle size distribution.

[0085] <Evaluation of luminescence characteristics> The absorptance, internal quantum efficiency, and external quantum efficiency of the obtained powdered α-sialon phosphor were measured using a spectrophotometer (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.), and were calculated according to the following procedure. Powdered α-SiAlON phosphor was filled into the concave cell so that the surface was smooth. This cell was attached to a designated position of an integrating sphere. Monochromatic light with a wavelength of 455 nm was split from a light source (Xe lamp) and introduced into the integrating sphere using an optical fiber. This monochromatic light was irradiated onto a phosphor sample, and the fluorescence spectrum of the sample was measured. A standard reflector with a reflectance of 99% (Spectralon, manufactured by Labsphere) was attached to the sample, and the spectrum of the excitation light with a wavelength of 455 nm was measured. The number of excitation light photons (Qex) was calculated from the spectrum in the wavelength range of 450 nm to 465 nm. A cell filled with powdered α-SiAlON phosphor was attached to the sample section, and the number of reflected excitation photons (Qref) and the number of fluorescent photons (Qem) were calculated from the obtained spectrum data. The number of reflected excitation photons was calculated in the same wavelength range as the number of excitation photons, and the number of fluorescent photons was calculated in the range of 465 nm to 800 nm. Absorption rate (%) = (Qex-Qref) / Qex x 100 Internal quantum efficiency (%) = (Qem / (Qex-Qref)) x 100 External quantum efficiency (%) = (Qem / Qex) x 100 When the standard sample NSG1301 sold by Sialon Co., Ltd. was measured using the above measurement method, the external quantum efficiency was 55.6% and the internal quantum efficiency was 74.8%. The device was calibrated using this sample as the standard.

[0086] <Example 2: Production and evaluation of α-type Sialon phosphor> Except for changing the charged composition, an α-sialon phosphor was produced in the same manner as in Example 1. Then, the light emission characteristics were evaluated. In the produced α-sialon phosphor, the m value was 3.0, the n value was 0.25, the x value was 1.45, the y value was 0.05, and the x+y value was 1.50.

[0087] <Example 3: Production and evaluation of α-type Sialon phosphor> Except for changing the charged composition, an α-sialon phosphor was produced in the same manner as in Example 1. Then, the light emission characteristics were evaluated. In the produced α-sialon phosphor, the m value was 4.0, the n value was 0.21, the x value was 1.94, the y value was 0.06, and the x+y value was 2.01.

[0088] <Comparative Example 1: Production and Evaluation of α-SiAlON Phosphor> Except for changing the composition of the materials used and not carrying out the hydrogen annealing step, an α-sialon phosphor was produced in the same manner as in Example 1. Then, the light emission characteristics were evaluated. In the produced α-sialon phosphor, the m value was 2.0, the n value was 0.32, the x value was 0.94, the y value was 0.06, and the x+y value was 1.00.

[0089] <Comparative Example 2: Production and Evaluation of α-SiAlON Phosphor> Except for changing the composition of the materials used and not carrying out the hydrogen annealing step, an α-sialon phosphor was produced in the same manner as in Example 1. Then, the light emission characteristics were evaluated. In the produced α-sialon phosphor, the m value was 3.5, the n value was 1.47, the x value was 1.70, the y value was 0.05, and the x+y value was 1.75.

[0090] Information on each example and comparative example is summarized in the following table. In the table, the units of each numerical value are as follows. α´, α1´, and α2´: ppm / °C a 25 and c 25 : Å V 25 : Å 3 Absorption rate, internal quantum efficiency, and external quantum efficiency: %

[0091]

Table 1

[0092]

Table 2

[0093] As shown in Tables 1 and 2, the α-sialon phosphor having a composition satisfying 0 < x < 2.0, 0 < y ≤ 0.5, 0.3 ≤ x + y ≤ 2.2, 0 < m ≤ 4.0, and 0 < n ≤ 3.0 in the general formula: (Ca x , Eu y )(Si 12-(m+n) Al m+n )(O n N 16-n ) and having an average linear expansion rate α´ of 4.2 ppm / °C or more and 4.6 ppm / °C or less at 25 to 900°C showed good internal quantum efficiency and external quantum efficiency compared to α-sialon phosphors that do not.

Explanation of symbols

[0094] 1 Phosphor 30 Sealing material 40 Composite 100 Light-emitting device 120 Light-emitting element 130 Heat sink 140 Case 150 First lead frame 160 Second lead frame 170 Bonding Wire 172 Bonding Wire

Claims

1. An α-sialon phosphor represented by the following general formula, having an average linear expansion coefficient α' of 4.2 ppm / °C or more and 4.6 ppm / °C or less at 25 to 900°C: General formula: (Ca x , Eu y ) (Si 12-(m+n) A m+n ) (O n N 16-n ) In the above general formula, x, y, m and n satisfy the following: 0<x<2.0 0<y≦0.5 0.3≦x+y≦2.0 0<m≦4.0 0<n≦3.0

2. 2. The α-sialon phosphor according to claim 1, An α-sialon phosphor having a structure satisfying the formula: 2.5≦m≦4.0 and 0<n≦0.

5.

3. 3. The α-sialon phosphor according to claim 1, The average linear expansion coefficient at 25 to 300°C is α 1 ', and the average linear expansion coefficient at 700 to 900°C is α 2 ´, then α 2 ´ / α 1 An α-sialon phosphor in which ' is 1.3 to 1.

8.

4. 3. The α-sialon phosphor according to claim 1, At 25°C, the lattice constant a 25 is 7.900 Å or more and 7.960 Å or less, and the lattice constant c 25 The α-sialon phosphor has a surface roughness of 5.720 Å or more and 5.780 Å or less.

5. 3. The α-sialon phosphor according to claim 1, At 25°C, the lattice volume V of the unit cell 25 is 308 Å 3 More than 320 Å 3 The α-SiAlON phosphor is shown below.

6. A light-emitting element; A wavelength conversion section including the α-sialon phosphor according to claim 1 or 2, which converts the wavelength of light emitted from the light-emitting element into a longer wavelength light; A light emitting device comprising:

Citation Information

Patent Citations

  • High-lighting-effect and high-stability alpha-SiAlON:Eu&lt;2+&gt; yellow fluorescent powder and preparation method thereof

    CN107057696A

  • Ca-CONTAINING α-SIALON PHOSPHOR AND METHOD FOR PRODUCING THE SAME

    JP2012224757A

  • Method for producing powdered precursor material, powdered precursor material and use thereof

    JP2016506976A

  • Oxynitride fluorescent substance powder, silicon nitride powder for manufacturing same, and method for manufacturing same

    WO2013054901A1

  • Oxynitride phosphor powder