Europium-activated beta-sialon phosphor and light-emitting device
By adding yttrium, titanium, gadolinium and alkaline earth metal elements to the europium activated β-type Theron phosphor to adjust their composition, the problems of low internal quantum efficiency and high crystal defect density in the prior art are solved, and higher luminescence is achieved Efficiency and stability.
Patent Information
- Application Number
- CN202410957562.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-10
- Filing Date
- 2021-09-06
- Publication Date
- 2024-11-22
AI Technical Summary
The existing β-type Theron phosphor has low internal quantum efficiency and high crystal defect density, resulting in a decrease in luminescence characteristics.
By adding yttrium, titanium, gadolinium and alkaline earth metal elements such as yttrium, titanium, gadolinium, magnesium or strontium to the europium activated β-Sylon phosphor, its composition is adjusted at a specific content, crystal defects are reduced and internal quantum efficiency is improved. The specific method includes adding compounds of these elements to the calcination and annealing process and optimizing particle size and purity through an acid treatment and grading process.
The internal quantum efficiency of the europium-activated β-type Theron phosphor is significantly improved, the absorption rate of excitation light of wavelength 600nm is reduced, and the luminescence efficiency and stability are enhanced.
Smart Images

Figure BDA0004949310860000191 
Figure BDA0004949310860000241 
Figure BDA0004949310860000301
Abstract
Description
[0001] This application is a divisional application of the invention patent application with Chinese application number 202180055101.7 (the invention name of the original application is "Europium-activated β-type sialon phosphor and light-emitting device", and the application date of the original application is September 6, 2021). Technical Field
[0002] The present disclosure relates to a europium-activated β-sialon phosphor and a light-emitting device. Background Art
[0003] Oxynitride phosphors are known as phosphors that have little decrease in brightness with temperature rise and are excellent in durability. Among oxynitride phosphors, β-sialon activated with europium is known as a green phosphor that can be excited by ultraviolet light, visible light, or the like.
[0004] β-sialon phosphors can be obtained, for example, by heating a raw material mixture containing silicon nitride powder, aluminum nitride powder, and europium oxide powder in a nitrogen atmosphere. In the research on the practical application of β-sialon phosphors, research has also been conducted to further improve the luminous efficiency (for example, Patent Document 1).
[0005] In addition, research has also been conducted to improve the luminous brightness. For example, Patent Document 2 describes a method for producing a β-sialon phosphor, comprising: a first heat treatment step, heat treating a mixture containing an aluminum compound, a first europium compound and silicon nitride to obtain a first heat-treated product; and a second heat treatment step, heat treating the first heat-treated product and the second europium compound in a rare gas atmosphere to obtain a second heat-treated product. In addition, Patent Document 3 proposes a method for producing a β-sialon phosphor, comprising: a calcination step, calcining a raw material mixture of the β-sialon phosphor at a temperature of 1820°C to 2200°C in a nitrogen atmosphere to obtain a calcined product; and an annealing step, annealing the calcined product at a temperature of 1100°C or above in a reducing atmosphere.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application No. 2013-519750
[0009] Patent Document 2: Japanese Patent Application Publication No. 2017-002278
[0010] Patent Document 3: International Publication No. 2010 / 143590 Summary of the invention
[0011] An object of the present disclosure is to provide a europium-activated β-sialon phosphor having excellent internal quantum efficiency.
[0012] One aspect of the present disclosure provides a europium-activated β-sialon phosphor comprising at least one element selected from yttrium, titanium and gadolinium, wherein the total content of the at least one element is greater than 0 ppm and less than 1000 ppm.
[0013] The europium-activated β-Sialon contains the above-mentioned elements in predetermined amounts and therefore has excellent internal quantum efficiency.
[0014] The at least one element may be yttrium, the at least one element may be titanium, or the at least one element may be yttrium and titanium. The europium-activated β-sialon phosphor contains a predetermined amount of yttrium or titanium, thereby achieving a more excellent internal quantum efficiency.
[0015] The at least one element contains at least one of yttrium and titanium, and the total content of the yttrium and titanium can be 0.1 to 500 ppm. When the total content of yttrium and titanium is within the above range, the crystal defects of the phosphor can be further reduced, so the internal quantum efficiency is more excellent.
[0016] The at least one element may include at least one of yttrium and titanium, and the absorption rate of the excitation light having a wavelength of 600 nm may be 5% or less.
[0017] The at least one element may be gadolinium. The europium-activated β-sialon phosphor contains a predetermined amount of gadolinium, and therefore has a more excellent internal quantum efficiency.
[0018] The content of gadolinium may be 0.1 to 300 ppm. When the content of gadolinium is within the above range, crystal defects of the phosphor can be further reduced, thereby achieving better internal quantum efficiency.
[0019] The europium-activated β-sialon phosphor whose at least one element is gadolinium may have an absorptivity of 6% or less to excitation light having a wavelength of 600 nm.
[0020] One aspect of the present disclosure provides a europium-activated β-sialon phosphor containing alkaline earth metal elements, wherein the total content of the alkaline earth metal elements is greater than 0 ppm and less than 1000 ppm.
[0021] The europium-activated β-sialon phosphor contains a predetermined amount of an alkaline earth metal element and therefore has excellent internal quantum efficiency.
[0022] The alkaline earth metal element may be magnesium or strontium. By including magnesium or strontium, crystal defects of the phosphor can be further reduced, thereby achieving better internal quantum efficiency.
[0023] The total content of the alkaline earth metal elements may be 0.1 to 500 ppm. When the content of the alkaline earth metal elements is within the above range, crystal defects of the phosphor can be further reduced, thereby achieving better internal quantum efficiency.
[0024] The absorption rate of the europium-activated β-sialon phosphor containing the alkaline earth metal element to the excitation light with a wavelength of 600 nm can be 7% or less.
[0025] One aspect of the present disclosure provides a light-emitting device comprising: a light-emitting element that emits primary light, and a wavelength converter that absorbs a portion of the primary light and emits secondary light having a wavelength longer than that of the primary light; the wavelength converter includes the europium-activated β-sialon phosphor.
[0026] The light-emitting device includes the europium-activated β-sialon phosphor as a wavelength converter and therefore has excellent light-emitting efficiency.
[0027] According to the present disclosure, a europium-activated β-sialon phosphor having excellent internal quantum efficiency can be provided. DETAILED DESCRIPTION
[0028] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are examples for describing the present disclosure and are not intended to limit the present disclosure to the following contents.
[0029] The materials exemplified in this specification may be used alone or in combination of two or more unless otherwise specified. In the case where there are multiple substances equivalent to each component in the composition, the content of each component in the composition refers to the total amount of the multiple substances present in the composition unless otherwise specified. The "process" in this specification may be a process independent of each other or a process performed simultaneously.
[0030] One embodiment of the europium-activated β-sialon phosphor contains at least one element selected from yttrium, titanium and gadolinium. The europium-activated β-sialon phosphor may contain one or two elements selected from yttrium, titanium and gadolinium, for example, or one element selected from yttrium, titanium and gadolinium. The at least one element may be, for example, yttrium, titanium, or gadolinium. In the case where the europium-activated β-sialon phosphor contains two of the above elements, the at least one element may be yttrium and titanium. For example, the europium-activated β-sialon phosphor may be a phosphor containing yttrium, a phosphor containing titanium, or a phosphor containing yttrium and titanium. That is, the europium-activated β-sialon phosphor may contain at least one of yttrium and titanium. In addition, the europium-activated β-sialon phosphor may also be a phosphor containing gadolinium.
[0031] The europium-activated β-sialon phosphor may include β-sialon as a main crystal, or may be composed of β-sialon. The europium-activated β-sialon phosphor may include a heterophase within a range that does not impair the gist of the present disclosure. The europium-activated β-sialon phosphor may have Si6-ZAl Z OZ N 8-Z : The composition shown by the compositional formula of Eu. In the above compositional formula, z can be 0.0 < z ≤ 4.2, or can be 0.0 < z ≤ 0.5. The composition of the Eu-activated β-sialon phosphor can be adjusted by changing the components and composition ratios of the raw material composition when manufacturing this phosphor.
[0032] In the composition of the Eu-activated β-sialon phosphor of the present embodiment, the contents of nitrogen atoms (N) and oxygen atoms (O) can be quantified by an oxygen-nitrogen analyzer, and the contents of Eu, Si, Al, Y, Ti, and Gd can be confirmed by performing elemental quantitative analysis using an ICP emission spectroscopic analyzer.
[0033] In the Eu-activated β-sialon phosphor, the total content of the above at least one element is greater than 0 ppm and less than 1000 ppm. The total content of the above at least one element can be adjusted according to the types of the elements contained in the Eu-activated β-sialon phosphor.
[0034] Based on the total amount of the Eu-activated β-sialon phosphor, the total content of Y and Ti is greater than 0 ppm and less than 1000 ppm. The internal quantum efficiency of the Eu-activated β-sialon phosphor of the present embodiment is more excellent. As the reason for obtaining such an effect, the present inventors speculate as follows. That is, it is speculated that in the Eu-activated β-sialon phosphor of the present embodiment, the vacancies that become defects in the phosphor generated during the manufacture of the phosphor are filled by ions of Y or Ti, reducing the defects and making the phosphor with excellent internal quantum efficiency.
[0035] Based on the total amount of the Eu-activated β-sialon phosphor, the lower limit value of the content of the above Y can be, for example, 0.1 ppm or more or 0.2 ppm or more. By the lower limit value of the content of Y being within the above range, the internal quantum efficiency of the Eu-activated β-sialon phosphor can be further improved. Based on the total amount of the Eu-activated β-sialon phosphor, the upper limit value of the content of the above Y can be, for example, 800 ppm or less, 600 ppm or less, or 500 ppm or less. By the upper limit value of the content of Y being within the above range, the occurrence of heterogeneous phases from excessive addition of Y can be suppressed, and the generation of non-luminescent components can be suppressed. Therefore, the reduction of the luminescence characteristics of the Eu-activated β-sialon phosphor can be suppressed. The content of the above Y can be adjusted within the above range. Based on the total amount of the Eu-activated β-sialon phosphor, for example, it can be 0.1 - 900 ppm or 0.1 - 500 ppm.
[0036] Based on the total amount of europium-activated β-sialon phosphor, the lower limit of the titanium content may be, for example, 0.1 ppm or more or 0.2 ppm or more. By setting the lower limit of the titanium content within the above range, the internal quantum efficiency of the europium-activated β-sialon phosphor can be further improved. Based on the total amount of europium-activated β-sialon phosphor, the upper limit of the titanium content may be, for example, 800 ppm or less, 600 ppm or less, or 500 ppm or less. By setting the upper limit of the titanium content within the above range, the occurrence of heterogeneous phases from excessively added titanium can be suppressed, and the generation of non-luminescent components can be suppressed, thereby suppressing the reduction of the luminescent characteristics of the europium-activated β-sialon phosphor. The titanium content may be adjusted within the above range, and may be, for example, 0.1 to 900 ppm or 0.1 to 500 ppm based on the total amount of europium-activated β-sialon phosphor.
[0037] Based on the total amount of the europium-activated β-sialon phosphor, the lower limit of the total content of yttrium and titanium can be, for example, 0.1 ppm or more or 0.2 ppm or more. By setting the lower limit of the total content of yttrium and titanium within the above range, the internal quantum efficiency of the europium-activated β-sialon phosphor can be further improved. Based on the total amount of the europium-activated β-sialon phosphor, the upper limit of the total content of yttrium and titanium can be, for example, 800 ppm or less, 600 ppm or less, or 500 ppm or less. By setting the upper limit of the total content of yttrium and titanium within the above range, the occurrence of heterogeneous phases from excessively added yttrium and titanium elements can be suppressed, and the generation of non-luminescent components can be suppressed, thereby suppressing the reduction of the luminescent characteristics of the europium-activated β-sialon phosphor. The total content of yttrium and titanium can be adjusted within the above range, and can be, for example, 0.1 to 900 ppm or 0.1 to 500 ppm based on the total amount of the europium-activated β-sialon phosphor.
[0038] The content of gadolinium is greater than 0 ppm and less than 1000 ppm based on the total amount of the europium-activated β-sialon phosphor. The europium-activated β-sialon phosphor of this embodiment has a better internal quantum efficiency. The present inventors speculate as follows as to why such an effect can be obtained. That is, it is speculated that in the europium-activated β-sialon phosphor of this embodiment, the defects in the phosphor generated during the manufacture of the phosphor are filled with gadolinium ions to reduce defects, thereby becoming a phosphor with excellent internal quantum efficiency.
[0039] Based on the total amount of the europium-activated β-sialon phosphor, the lower limit value of the gadolinium content can be, for example, 0.1 ppm or more, or 0.2 ppm or more. By setting the lower limit value of the gadolinium content within the above range, the internal quantum efficiency of the europium-activated β-sialon phosphor can be further improved. Based on the total amount of the europium-activated β-sialon phosphor, the upper limit value of the gadolinium content can be, for example, 800 ppm or less, 600 ppm or less, 500 ppm or less, or 300 ppm or less. By setting the upper limit value of the gadolinium content within the above range, the occurrence of heterogeneous phases from the excessively added gadolinium can be suppressed, and the generation of non-luminescent components can be suppressed. Therefore, the reduction in the luminescence characteristics of the europium-activated β-sialon phosphor can be suppressed. The gadolinium content can be adjusted within the above range. Based on the total amount of the europium-activated β-sialon phosphor, it can be, for example, 0.1 to 900 ppm, 0.1 to 500 ppm, or 0.1 to 300 ppm.
[0040] Other embodiments of the europium-activated β-sialon phosphor contain alkaline earth metal elements. The above europium-activated β-sialon phosphor may contain β-sialon as the main crystal or may be composed of β-sialon. The europium-activated β-sialon phosphor may contain heterogeneous phases within the scope that does not impair the gist of the present disclosure. The europium-activated β-sialon phosphor may have Si 6-Z Al Z O Z N 8-Z : Eu composition represented by the composition formula. In the above composition formula, z can be 0.0 < z ≤ 4.2, or can be 0.0 < z ≤ 0.5. The composition of the europium-activated β-sialon phosphor can be adjusted by changing the components and composition ratios of the raw material composition when manufacturing this phosphor.
[0041] In the composition of the europium-activated β-sialon phosphor of the present embodiment, the contents of alkaline earth metal elements such as magnesium (Mg) and strontium (Sr) can be confirmed by performing elemental quantitative analysis using an ICP emission spectroscopic analysis device.
[0042] The alkaline earth metal can be a metal known as a Group II element in the periodic table published by IUPAC. As the above alkaline earth metal elements, for example, at least one selected from magnesium, calcium, strontium, and barium is included, and magnesium or strontium is preferably included.
[0043] The total content of the alkaline earth metal elements is greater than 0 ppm and less than 1000 ppm based on the total amount of the europium-activated β-sialon phosphor. The europium-activated β-sialon phosphor of this embodiment has excellent internal quantum efficiency. The present inventors speculate as follows as to why such an effect can be obtained. That is, it is speculated that in the europium-activated β-sialon phosphor of this embodiment, the defects in the phosphor generated during the manufacture of the phosphor are filled with ions of elements belonging to alkaline earth metals to reduce defects, thereby becoming a phosphor with excellent internal quantum efficiency.
[0044] Based on the total amount of the europium-activated β-sialon phosphor, the lower limit of the total content of the alkaline earth metal elements can be, for example, 0.1 ppm or more or 0.2 ppm or more. By setting the lower limit of the total content of the alkaline earth metal elements to be within the above range, the internal quantum efficiency of the europium-activated β-sialon phosphor can be further improved. Based on the total amount of the europium-activated β-sialon phosphor, the upper limit of the total content of the alkaline earth metal elements can be, for example, 800 ppm or less, 600 ppm or less, 500 ppm or less or 300 ppm or less. By setting the upper limit of the total content of the alkaline earth metal elements to be within the above range, the occurrence of heterogeneous phases from excessively added alkaline earth metal elements can be suppressed, and the generation of non-luminescent components can be suppressed, thereby suppressing the reduction of the luminescent characteristics of the europium-activated β-sialon phosphor. The total content of the alkaline earth metal elements can be adjusted within the above range, and may be, for example, 0.1 to 900 ppm, 0.1 to 500 ppm, or 0.1 to 300 ppm based on the total amount of the europium-activated β-sialon phosphor.
[0045] The 50% cumulative diameter (D50) in the volume-based cumulative particle size distribution of the europium-activated β-sialon phosphor disclosed herein can be adjusted according to the use of the phosphor, etc. The 50% cumulative diameter (D50) in the volume-based cumulative particle size distribution of the europium-activated β-sialon phosphor can be, for example, 0.1 to 50 μm, 3 to 40 μm, or 6 to 30 μm. D50 can be controlled by, for example, adjusting the heating temperature and heating time during the manufacture of the phosphor, and by classification, etc.
[0046] D50 in this specification refers to the particle size when the cumulative value from the small particle size reaches 50% of the total in the distribution curve of the volume-based particle size measured by the laser diffraction and scattering method. The distribution curve related to the particle size of the phosphor is carried out according to the particle size distribution measurement method by laser diffraction and scattering method described in JIS R 1629:1997 "Particle size distribution measurement method for precision ceramic raw materials by laser diffraction and scattering method". The measurement can be carried out using a particle size distribution measuring device. Specifically, first, 0.1g of the phosphor as the measurement object is put into 100mL of ion exchange water, a small amount of sodium hexametaphosphate is added, and an ultrasonic homogenizer is used for 3 minutes of dispersion treatment. The obtained substance is used as a measurement sample, and the particle size is measured using a particle size distribution measuring device. The particle size distribution is determined by the obtained particle size distribution. D50. D50 is also called the median particle size, which refers to the average particle size of the particles as the object. It should be noted that as a particle size distribution measuring device, for example, "Microtrac MT3300EX II" (product name) manufactured by MicrotracBEL Co., Ltd. can be used. As an ultrasonic homogenizer, for example, "Ultrasonic Homogenizer US-150E" (product name, chip size: Amplitude: 100%, oscillation frequency: 19.5KHz, amplitude: about 31μm).
[0047] The europium-activated β-sialon phosphor disclosed in the present invention has a suppressed absorptivity of light having a wavelength of 600 nm. The europium in the above-mentioned phosphor has a small absorption of light having a wavelength of 600 nm, and the influence of the fluorescence generated by the above-mentioned phosphor is also small. Therefore, it is believed that when the absorptivity of light having a wavelength of 600 nm is high, it is due to the absorption caused by the heterophase as a defect or a non-luminescent component. In the europium-activated β-sialon phosphor disclosed in the present invention, for example, the absorptivity of the excitation light having a wavelength of 600 nm can be 7% or less, 6.8% or less, 6.0% or less, 5.0% or less, 4.8% or less, 4.5% or less, or 4.0% or less. The europium-activated β-sialon phosphor has a suppressed absorption of the excitation light having a wavelength of 600 nm, and has little influence of the heterophase as a defect or a non-luminescent component, and therefore can become a phosphor with better internal quantum efficiency.
[0048] When the europium-activated β-sialon phosphor contains at least one of yttrium and titanium, the absorptivity of light having a wavelength of 600 nm may be, for example, 5.0% or less, 4.8% or less, 4.5% or less, or 4.0% or less. When the europium-activated β-sialon phosphor contains gadolinium, the absorptivity of light having a wavelength of 600 nm may be, for example, 6.0% or less, 5.5% or less, or 5% or less.
[0049] When the europium-activated β-sialon phosphor contains an alkaline earth metal element, the absorptivity of light having a wavelength of 600 nm may be, for example, 7% or less, 6% or less, or 5% or less.
[0050] The europium-activated β-sialon phosphor disclosed herein has an excellent internal quantum efficiency, which may be, for example, greater than 80%, 81% or more, 82% or more, 83% or more, or 84% or more.
[0051] Unless otherwise specified, the light absorption rate and internal quantum efficiency in this specification refer to the quantum efficiency obtained when the phosphor is excited by near-ultraviolet light with a wavelength of 455 nm. Specifically, the internal quantum efficiency is measured and obtained by the method described in the Examples of this specification.
[0052] The europium-activated β-sialon phosphor disclosed in the present invention can be manufactured, for example, by the following method. As an example of a method for manufacturing a europium-activated β-sialon phosphor, it can be a method having the following steps: a calcination step, in which a raw material composition containing a silicon source, an aluminum source, and a europium source and containing at least one of them as a nitride is subjected to one or more heat treatments to obtain a calcined body containing β-sialon; and an annealing step, in an atmosphere containing at least one selected from a rare gas, a reducing gas, and an inactive gas, by one or more annealing treatments to obtain an annealed body from a mixture, the mixture containing the above-mentioned calcined body and a supply source of at least one element selected from yttrium, titanium, and gadolinium or at least one of an alkaline earth metal simple substance and a compound having an alkaline earth metal element as a constituent element. As a supply source of at least one element selected from yttrium, titanium and gadolinium, for example, at least one selected from yttrium simple substance, titanium simple substance, a compound having yttrium as a constituent element and a compound having titanium as a constituent element, and at least one selected from gadolinium simple substance or a compound having gadolinium as a constituent element, etc. This example is described below.
[0053] The raw material composition contains a compound having an element that is a constituent element of europium-activated β-Sialon, and contains at least a silicon source, an aluminum source, and a europium source. In the raw material composition, at least one of the silicon source, the aluminum source, and the europium source is a nitride. The nitride contains nitrogen that is a constituent element of europium-activated β-Sialon, and therefore, can also be a nitrogen source.
[0054] A silicon source refers to a compound or a single substance containing silicon as a constituent element, an aluminum source refers to a compound or a single substance containing aluminum as a constituent element, and a europium source refers to a compound or a single substance containing europium as a constituent element. In this specification, a compound containing silicon as a constituent element is also referred to as a silicon compound, a compound containing aluminum as a constituent element is also referred to as an aluminum compound, and a compound containing europium as a constituent element is also referred to as a europium compound.
[0055] The silicon compound, aluminum compound and europium compound may be any one of nitride, oxide, oxynitride and hydroxide, respectively. In addition, the raw material composition may further contain β-Sialon or europium-activated β-Sialon. Here, β-Sialon or europium-activated β-Sialon is a material that serves as a skeleton or a core.
[0056] Silicon compounds include, for example, silicon nitride (Si3N4) and silicon oxide (SiO2). As silicon nitride, it is preferred to use silicon nitride with a high α fraction. The α fraction of silicon nitride can be, for example, 80% by mass or more, 90% by mass or more, or 95% by mass or more. If the α fraction of silicon nitride is within the above range, primary particle growth can be promoted. As silicon nitride, it is preferred to use silicon nitride with a small oxygen content. The oxygen content of silicon nitride can be, for example, less than 3.0% by mass or less than 1.3% by mass. If the oxygen content of silicon nitride is within the above range, the occurrence of defects in the crystal of β-sialon can be suppressed.
[0057] Examples of the aluminum compound include aluminum nitride (AlN), aluminum oxide (Al 2 O 3 ), and aluminum hydroxide (Al(OH) 3 ).
[0058] Examples of europium compounds include europium oxides (europium oxide), europium nitrides (europium nitrides), and europium halides. Examples of europium halides include europium fluoride, europium chloride, europium bromide, and europium iodide. The europium compound preferably includes europium oxide. The valence of europium in the europium compound may be divalent or trivalent, preferably divalent.
[0059] The raw material mixture can be prepared by weighing and mixing the compounds. Mixing can be performed by dry mixing or wet mixing. For example, the dry mixing method can be a method of mixing the components using a V-type mixer. For example, the wet mixing method can be a method of adding a solvent such as water or a dispersion medium to prepare a solution or slurry and mixing the components, and then removing the solvent or dispersion medium.
[0060] The heating temperature in the calcining step may be, for example, 1800 to 2500° C., 1800 to 2400° C., 1850 to 2100° C., 1900 to 2100° C., 1900 to 2050° C., or 1920 to 2050° C. By setting the heating temperature in the calcining step to 1800° C. or higher, the particle growth of β-Sialon can be promoted, and the solid solution amount of europium can be made more sufficient. By setting the heating temperature in the calcining step to 2500° C. or lower, the decomposition of β-Sialon crystals can be sufficiently suppressed.
[0061] From the viewpoint of promoting the primary particle growth of β-Sialon, the heating time in the calcination step may be longer. However, if the heating time is too long, crystal defects may increase. Therefore, the heating time may be, for example, 1 to 30 hours, 3 to 25 hours, or 5 to 20 hours.
[0062] The heating of the raw material mixture in the calcination process can be carried out, for example, under a nitrogen atmosphere. By heating under conditions of high nitrogen partial pressure, the decomposition of silicon nitride at high temperatures can be suppressed. In addition, by treating at high temperatures, particle growth can be promoted. The heating of the raw material mixture in the calcination process can be carried out, for example, under pressure. The pressure at this time can be, for example, 0.01 to 200 MPaG, 0.02 to 200 MPaG, 0.1 to 200 MPaG, 0.1 to 100 MPaG, 0.1 to 50 MPaG, 0.1 to 15 MPaG or 0.1 to 5 MPaG.
[0063] The number of times of heat treatment in the calcination step may be once, but may be, for example, twice or more, 2 to 5 times, or 2 to 4 times. By performing heat treatment multiple times, a europium-activated β-sialon phosphor having a higher emission intensity can be obtained.
[0064] In the calcination process, more than one heat treatment is performed. When multiple heat treatments are performed, they can be sequentially referred to as the first heat treatment, the second heat treatment, etc., and the processes for performing each heat treatment can be sequentially referred to as the first calcination process, the second calcination process, etc. For example, in the case where the above-mentioned manufacturing method performs two heat treatments in the calcination process, the calcination process is also referred to as a first calcination process including a first heat treatment body obtained by subjecting the raw material composition containing nitrides to a first heat treatment, and a second calcination process including a second heat treatment body obtained by subjecting the first heat treatment body to a second heat treatment. Moreover, in this case, the second heat treatment body is equivalent to a calcined body containing β-sialon. Before performing multiple heat treatments, the silicon source, the aluminum source, and the europium source can also be further mixed and heat treated.
[0065] In the case where the calcining process is subjected to heat treatment more than twice, the heating temperature, heating time, heating atmosphere and heating pressure of the first calcining process can be respectively applied to the heating temperature, heating time, heating atmosphere and heating pressure in the above-mentioned heating process. Moreover, the heating temperature, heating time, heating atmosphere and heating pressure after the second calcining process can be the same as the first calcining process, and cannot be different. However, even if the heating temperature, heating time, heating atmosphere and heating pressure after the second calcining process are different from those of the first calcining process, they are within the range of the conditions shown in the above-mentioned heating process.
[0066] The calcined body obtained in the calcining step is a solid solution having a crystal of β-sialon and an element serving as a luminescence center dissolved in a part thereof, and can emit fluorescence itself. The calcined body obtained by the calcining step is sometimes in a block shape, and the particle size can be adjusted by crushing or the like before the annealing step.
[0067] Then, an annealing step is performed. The annealing step in the manufacturing method of this example refers to a step of obtaining an annealed body from a mixture, the mixture comprising the calcined body obtained in the above-mentioned calcining step, and a supply source of at least one element selected from yttrium, titanium and gadolinium, or at least one of an alkaline earth metal element and a compound having an alkaline earth metal element as a constituent element. The above-mentioned step may be, for example, a step of annealing a mixture comprising the calcined body obtained in the above-mentioned calcining step, and at least one selected from yttrium element, titanium element, a compound having yttrium as a constituent element, and a compound having titanium as a constituent element, or a step of annealing a mixture comprising the calcined body obtained in the above-mentioned calcining step, and at least one of gadolinium element or a compound having gadolinium as a constituent element, or a step of annealing a mixture comprising the calcined body obtained in the above-mentioned calcining step, and at least one of an alkaline earth metal element and a compound having an alkaline earth metal element as a constituent element. In the annealing step, the annealed body may be obtained from the mixture by annealing one or more times.
[0068] The compound having yttrium as a constituent element and the compound having titanium as a constituent element may be, for example, an oxide, a nitride, and a hydroxide, but is preferably an oxide. The compound having yttrium as a constituent element and the compound having titanium as a constituent element may be, for example, yttrium oxide (Y2O3) and titanium oxide (Ti2O3).
[0069] The total amount of yttrium, titanium, a compound having yttrium as a constituent element, and a compound having titanium as a constituent element may be, for example, 0.01 to 4 mass %, 0.05 to 3 mass %, or 0.1 to 3 mass % relative to the total amount of the above-mentioned mixture. By making the above-mentioned amount of yttrium or titanium more than 0.01 mass %, it is easier to introduce at least one of yttrium and titanium into the phosphor, and the internal quantum efficiency of the obtained europium-activated β-sialon phosphor can be further improved. By making the above-mentioned amount of 4 mass % or less, the reduction of the luminescence characteristics of the obtained europium-activated β-sialon phosphor can be suppressed.
[0070] The compound having gadolinium as a constituent element may be, for example, an oxide, a nitride, a hydroxide, etc., but is preferably an oxide. The compound having gadolinium as a constituent element may be, for example, gadolinium oxide (Gd2O3), etc.
[0071] The total amount of the gadolinium simple substance and the compound having gadolinium as a constituent element may be, for example, 0.01 to 4 mass%, 0.05 to 3 mass%, or 0.1 to 3 mass% relative to the total amount of the above-mentioned mixture. By making the total amount of the gadolinium simple substance and the compound having gadolinium as a constituent element more than 0.01 mass%, it becomes easy to introduce gadolinium into the phosphor, and the internal quantum efficiency of the obtained europium-activated β-sialon phosphor can be further improved. By making the total amount of the gadolinium simple substance and the compound having gadolinium as a constituent element less than 4 mass%, the heterogeneity from the excessively added gadolinium can be suppressed, and the reduction of the luminescence characteristics of the obtained europium-activated β-sialon phosphor can be suppressed.
[0072] The compound having alkaline earth metal elements as constituent elements may be, for example, oxides, carbonates, nitrides and hydroxides, etc., but is preferably oxides or carbonates. The alkaline earth metal elements may be the alkaline earth metal elements exemplified as constituent components of europium-activated β-sialon phosphors. The compound having alkaline earth metal elements as constituent elements may be, for example, magnesium oxide (MgO) and strontium carbonate (SrCO3), strontium nitride (Sr2N3) and strontium oxide (SrO), etc.
[0073] The total amount of the alkaline earth metal element and the compound having the alkaline earth metal element as a constituent element can be, for example, 0.01 to 4 mass%, 0.05 to 3 mass%, 0.1 to 3 mass% or 0.1 to 1.5 mass% relative to the total amount of the above-mentioned mixture. By making the total amount of the alkaline earth metal element and the compound having the alkaline earth metal element as a constituent element more than 0.01 mass%, it becomes easy to introduce the alkaline earth metal element into the phosphor, and the internal quantum efficiency of the obtained europium-activated β-sialon phosphor can be further improved. By making the total amount of the alkaline earth metal element and the compound having the alkaline earth metal element as a constituent element less than 4 mass%, the heterogeneity from the excessively added alkaline earth metal element can be suppressed, and the reduction of the luminescence characteristics of the obtained europium-activated β-sialon phosphor can be suppressed.
[0074] The annealing step is performed in an atmosphere containing at least one selected from a rare gas, a reducing gas, and an inert gas. By performing the annealing in an atmosphere containing a rare gas, a reducing gas, or an inert gas, the ratio of divalent europium in europium in the solid solution can be increased.
[0075] The above-mentioned rare gas may contain, for example, argon and helium, or may contain argon or may be composed of argon. The above-mentioned reducing gas may contain, for example, ammonia, hydrocarbons, carbon monoxide and hydrogen, or may contain hydrogen or may be composed of hydrogen. The inert gas may contain, for example, nitrogen or may be composed of nitrogen. The atmosphere of the annealing process may also be a mixed gas of two or more of the above-mentioned rare gas, the above-mentioned reducing gas and the inert gas. When the atmosphere of the annealing process is the above-mentioned mixed gas, the content of the above-mentioned reducing gas is based on the total volume of the mixed gas, for example, 1 to 50 volume % or 4 to 20 volume %. The content of the above-mentioned inert gas is based on the total volume of the mixed gas, for example, 1 to 50 volume % or 4 to 20 volume %.
[0076] The pressure during the annealing treatment may be the same as the pressure during the calcining step, but is preferably lower than the pressure conditions during the calcining step, and more preferably atmospheric pressure.
[0077] The temperature of the annealing treatment needs to be set lower than the heating temperature in the calcining process. The upper limit of the temperature of the annealing treatment may be, for example, below 1700°C or below 1680°C. By setting the upper limit of the temperature of the annealing treatment within the above range, it is possible to suppress further particle growth in the calcined body and to coagulate between the solid solution, form secondary particles, etc., thereby coarsening the particles. The lower limit of the temperature of the annealing treatment may be, for example, above 1000°C, above 1100°C, above 1200°C, above 1300°C or above 1400°C. By setting the lower limit of the temperature of the annealing treatment within the above range, the crystal defect density of the β-sialon contained in the annealed body can be reduced, and the internal quantum efficiency can be further improved. The temperature of the annealing treatment can be adjusted within the above range, for example, it may be 1000-1700°C or 1100-1680°C.
[0078] From the viewpoint of further reducing crystal defects in the phosphor included in the annealed body, the heating time in the annealing treatment may be, for example, 1 to 30 hours, 2 to 25 hours, or 3 to 20 hours.
[0079] In the annealing process, more than one annealing treatment is performed. When multiple annealing treatments are performed, they can be sequentially referred to as the first annealing treatment, the second annealing treatment, etc., and the processes for performing the annealing treatments can be sequentially referred to as the first annealing process, the second annealing process, etc. For example, in the case where two annealing treatments are performed in the annealing process in the above-mentioned manufacturing method, the annealing process is also referred to as a first annealing process including performing a first annealing treatment on the calcined body to obtain a first annealed body, and a second annealing process including performing a second annealing treatment on the first annealed body to obtain a second annealed body. Moreover, in this case, the second annealed body is equivalent to the above-mentioned annealed body.
[0080] In the case where the annealing process is performed more than twice, the temperature, heating time and pressure of the annealing process in the first annealing process can be respectively applied to the temperature, heating time and pressure of the annealing process in the above-mentioned annealing process. Moreover, the temperature, heating time and pressure of the annealing process after the second annealing process can be the same as or different from the first annealing process. However, even if the temperature, heating time and pressure of the annealing process after the second annealing process are different from those in the first annealing process, they are within the range of the conditions shown in the above-mentioned annealing process.
[0081] The number of annealing treatments in the annealing step may be 1, but may also be 2 or more, 2 to 5 or 2 to 4. By performing multiple annealing treatments, the crystal defect density of β-sialon contained in the annealed body can be reduced, and a europium-activated β-sialon phosphor with better internal quantum efficiency can be obtained.
[0082] When the annealing process is performed multiple times, the above-mentioned supply source of at least one element selected from yttrium, titanium and gadolinium (for example, the above-mentioned yttrium single substance, titanium single substance, compound having yttrium as a constituent element and compound having titanium as a constituent element or gadolinium single substance and compound having gadolinium as a constituent element, etc.) or at least one of alkaline earth metal single substance and compound having alkaline earth metal element as a constituent element may be blended at once in the first annealing process, or may be blended in multiple annealing processes, but it is preferably blended at once in the first annealing process. It should be noted that when these compounds are blended in equal parts, the description of the total blending amount of the above-mentioned supply source of at least one element selected from yttrium, titanium and gadolinium or at least one of alkaline earth metal single substance and compound having alkaline earth metal element as a constituent element is interpreted as the total amount of the above-mentioned supply source of at least one element selected from yttrium, titanium and gadolinium or at least one of alkaline earth metal single substance and compound having alkaline earth metal element as a constituent element blended in multiple annealing processes.
[0083] The method for producing a europium-activated β-sialon phosphor may include other steps in addition to the calcining step and the annealing step. Other steps include, for example, a step of treating the annealed body obtained in the annealing step with at least one of an acid and an alkali, a classification step of adjusting the particle size of the annealed body or the annealed body obtained by acid treatment, etc. The step of treating the annealed body with an acid is referred to as an acid treatment step, and the step of treating the annealed body with an alkali is referred to as an alkali treatment step.
[0084] By the acid treatment process or the alkali treatment process, for example, the crystal defect density in the phosphor contained in the annealed body can be further reduced, silicon existing on the surface of the solid solution generated by thermal decomposition of β-sialon can be removed, and the pseudo-polymorph of aluminum nitride (AlN) produced as a by-product during the preparation of the first calcined body, i.e., AlN-type polytype (polytypoid), can be removed. The acid can include, for example, hydrofluoric acid and nitric acid. The acid can be a mixed acid of hydrofluoric acid and nitric acid. The alkali can include, for example, sodium hydroxide, etc.
[0085] The classification process can be performed, for example, by any of a wet classification method and a dry classification method. As wet classification, for example, an elutriation classification method can be cited in which particles with small particle sizes are removed by adding the annealed body to a mixed solvent containing ion exchange water and a dispersant (for example, sodium hexametaphosphate, etc.) or a mixed solvent containing ion exchange water and ammonia water and stirring and then leaving it to stand.
[0086] The europium-activated β-sialon phosphor disclosed herein can be used alone or in combination with other phosphors. The europium-activated β-sialon phosphor disclosed herein can be appropriately used in light-emitting devices such as LEDs due to its excellent internal quantum efficiency. The phosphor can also be dispersed in a curing resin for use. The curing resin is not particularly limited, and for example, a resin used as a sealing resin for a light-emitting device can be used.
[0087] One embodiment of the light-emitting device is a light-emitting device having a light-emitting element that emits primary light, and a wavelength converter that absorbs a portion of the primary light and emits secondary light having a wavelength longer than the wavelength of the primary light. The wavelength converter includes the europium-activated β-sialon phosphor. The light-emitting element that emits primary light may be, for example, an InGaN blue LED. The light-emitting element and the wavelength converter may also be dispersed in a sealing resin or the like.
[0088] Although several embodiments have been described above, the present disclosure is not limited to the above embodiments. In addition, the descriptions of the above embodiments can be applied to each other.
[0089] Example
[0090] Hereinafter, the present disclosure will be described in more detail with reference to Examples and Comparative Examples. However, the present disclosure is not limited to the following Examples.
[0091] (Comparative Example I-1)
[0092] [Preparation of Europium-activated β-sialon phosphor]
[0093] In a container, each raw material is weighed so that silicon nitride (Si3N4) becomes 96.0 mass%, aluminum nitride (AlN) becomes 2.8 mass%, aluminum oxide (Al2O3) becomes 0.5 mass% and europium oxide (Eu2O3) becomes 0.7 mass%, and mixed by a V-type mixer (manufactured by Tsutsui Rikagaku Kikai Co., Ltd.) to obtain a mixture. The obtained mixture is completely passed through a sieve with a mesh of 250 μm and agglomerates are removed to obtain a raw material composition. Agglomerates that do not pass through the sieve are crushed and the particle size is adjusted so as to pass through the sieve.
[0094] 200 g of the raw material composition prepared as above was weighed into a cylindrical boron nitride container with a lid (manufactured by Denka Co., Ltd., a molded product with boron nitride (trade name: Denka boron nitride N-1) as the main component, inner diameter: 10 cm, height: 10 cm). Thereafter, the container was placed in an electric furnace equipped with a carbon heater, heated to 2020°C in a nitrogen atmosphere (pressure: 0.90 MPaG), and heated at a heating temperature of 2020°C for 8 hours (calcination process). After heating, the sample that slowly condensed into a block in the above container was collected in a mortar for crushing. After crushing, the first calcined body in powder form was obtained by passing through a sieve with a mesh of 250 μm.
[0095] Next, the first calcined body is filled into a cylindrical boron nitride container, and the container is placed in an electric furnace equipped with a carbon heater. The temperature is raised to 1450°C in an argon atmosphere (pressure: 0.025 MPaG), and heating is performed at a heating temperature of 1450°C for 3 hours (annealing process). After heating, the agglomerates formed by the particles slowly agglomerating in the container are crushed in a mortar and passed through a 250 μm sieve to obtain a powder.
[0096] Next, the obtained powder is added to a mixed acid of hydrofluoric acid (concentration: 50% by mass) and nitric acid (concentration: 70% by mass) (hydrofluoric acid and nitric acid are mixed in a volume ratio of 1:1), and the acid treatment is performed for 30 minutes while stirring at a temperature of 75°C. After the acid treatment, the stirring is terminated and the powder is allowed to settle, and the supernatant and the fine powder obtained by the acid treatment purification are removed. Thereafter, distilled water is further added and stirred again. The stirring is terminated and the powder is allowed to settle, and the supernatant and the fine powder are removed. By repeating this operation at a pH of 8 or less in the aqueous solution until the supernatant becomes transparent, the obtained precipitate is filtered and dried to obtain a europium-activated β-sialon phosphor.
[0097] (Comparative Example I-2)
[0098] A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example I-1 except that the atmosphere in the annealing step was changed from an argon atmosphere to a hydrogen atmosphere and the treatment temperature in the annealing step in an electric furnace equipped with a metal heater was changed to 1650°C.
[0099] (Example I-1)
[0100] In the annealing step, the mixture was adjusted so that the amount of yttrium oxide was 0.1 mass % relative to the total amount of the first calcined body and yttrium oxide was 100 mass %, and then heated in a hydrogen atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example I-2.
[0101] (Example I-2)
[0102] A europium-activated β-sialon phosphor was obtained in the same manner as in Example I-1 except that the blending amount of yttrium oxide was changed to 0.5 mass %.
[0103] (Example I-3)
[0104] A europium-activated β-sialon phosphor was obtained in the same manner as in Example I-1 except that the blending amount of yttrium oxide was changed to 1 mass %.
[0105] (Comparative Example I-3)
[0106] A europium-activated β-sialon phosphor was obtained in the same manner as in Example I-1 except that the blending amount of yttrium oxide was changed to 5 mass %.
[0107] (Example I-4)
[0108] In the annealing step, the mixture was adjusted so that the amount of yttrium oxide was 0.5 mass % relative to the total amount of the first calcined body and yttrium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example I-1.
[0109] (Example I-5)
[0110] In the annealing step, the mixture was adjusted so that the amount of titanium oxide was 0.1 mass % relative to the total amount of the first calcined body and titanium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example I-1.
[0111] (Example I-6)
[0112] A europium-activated β-sialon phosphor was obtained in the same manner as in Example I-5 except that the blending amount of titanium oxide was changed to 0.5 mass %.
[0113] (Example I-7)
[0114] A europium-activated β-sialon phosphor was obtained in the same manner as in Example I-5 except that the blending amount of titanium oxide was changed to 1 mass %.
[0115] (Comparative Example I-4)
[0116] A europium-activated β-sialon phosphor was obtained in the same manner as in Example I-5 except that the blending amount of titanium oxide was changed to 5 mass %.
[0117] (Comparative Example I-5)
[0118] In the annealing step, the mixture was adjusted so that the amount of zirconium oxide was 0.1 mass % relative to the total amount of the first calcined body and zirconium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example I-1.
[0119] (Comparative Example I-6)
[0120] A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example I-5 except that the blending amount of zirconium oxide was changed to 0.5 mass %.
[0121] (Comparative Example I-7)
[0122] In the annealing step, the mixture was adjusted so that the amount of zinc oxide was 0.1 mass % relative to the total amount of the first calcined body and zinc oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example I-1.
[0123] (Comparative Example I-8)
[0124] A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example I-7 except that the blending amount of zinc oxide was changed to 0.5 mass %.
[0125] (Comparative Example I-9)
[0126] A standard sample of β-sialon phosphor (manufactured by SIALON CORPORATION, NIMS Standard Green lot No. NSG1301) was used as the phosphor of Comparative Example I-9.
[0127] <Determination of the Contents of Yttrium, Titanium, Zirconium and Zinc>
[0128] The contents of yttrium, titanium, zirconium and zinc in the europium-activated β-sialon phosphors prepared in Examples I-1 to I-7 and Comparative Examples I-1 to I-8 were measured as shown below.
[0129] <Contents of yttrium, titanium, zirconium and zinc>
[0130] The contents of yttrium, titanium, zirconium and zinc in the europium-activated β-sialon phosphor are measured by the following steps. The phosphor is dissolved by a pressurized acid decomposition method to prepare a sample solution. The obtained sample solution is measured by quantitative analysis of the elements using an ICP emission spectrophotometer (manufactured by Rigaku Co., Ltd., trade name: CIROS-120). It should be noted that the detection limits of yttrium (Y), titanium (Ti), zirconium (Zr) and zinc (Zn) are 100 ppb, respectively.
[0131] [Evaluation of Europium-activated β-sialon phosphor]
[0132] For each of the europium-activated β-sialon phosphors prepared in Examples I-1 to I-7 and Comparative Examples I-1 to I-9, the absorbance when irradiated with excitation light of a wavelength of 455 nm, the internal quantum efficiency and the external quantum efficiency, the chromaticity X, and the absorbance when irradiated with excitation light of a wavelength of 600 nm were evaluated by the methods described below. The results are shown in Table 1.
[0133] <Absorption rate, internal quantum efficiency and external quantum efficiency>
[0134] The absorptivity (excitation light absorptivity), internal quantum efficiency and external quantum efficiency of the fluorescent body when irradiated with an excitation light of a wavelength of 455nm, are calculated by the following steps. First, the fluorescent body to be measured is filled in a concave groove in a manner that the surface becomes smooth, and is installed in the opening of an integrating sphere. Using an optical fiber, monochromatic light with a wavelength of 455nm split from a Xe lamp as a light source is introduced into the above-mentioned integrating sphere as the excitation light of the fluorescent body. The monochromatic light as the excitation light is irradiated on the fluorescent body as the object of measurement, and the fluorescence spectrum is measured. During the measurement, a spectrophotometer (manufactured by Otsuka Electronics Co., Ltd., trade name: MCPD-7000) is used.
[0135] The luminous intensity of the phosphor is determined by the data of the obtained fluorescence spectrum. In addition, the number of excitation reflected light photons (Qref) and the number of fluorescence photons (Qem) are calculated from the data of the obtained fluorescence spectrum. The number of excitation reflected light photons is calculated in the same wavelength range as the number of excitation light photons, and the number of fluorescence photons is calculated in the range of 465 to 800 nm. In addition, using the same device, a standard reflector with a reflectivity of 99% (manufactured by Labsphere, Spectralon (registered trademark)) is installed at the opening of the integrating sphere, and the spectrum of the excitation light with a wavelength of 455 nm is measured. At this time, the number of excitation light photons (Qex) is calculated from the spectrum in the wavelength range of 450 to 465 nm.
[0136] From the above calculation results, the absorptivity of the 455 nm excitation light, the internal quantum efficiency, and the external quantum efficiency of the phosphor to be measured were determined based on the calculation formula shown below.
[0137] Absorption rate of 455nm excitation light = ((Qex-Qref) / Qex)×100
[0138] Internal quantum efficiency = (Qem / (Qex-Qref)) × 100
[0139] External quantum efficiency = (Qem / Qex) × 100
[0140] In addition, based on the above formula, the relationship between the external quantum efficiency, the absorptivity of the excitation light of 455 nm, and the internal quantum efficiency can be expressed as follows.
[0141] External quantum efficiency = 455nm light absorption × internal quantum efficiency
[0142] <Chroma X>
[0143] The chromaticity X is obtained by calculating the CIE chromaticity coordinate x value (chromaticity X) in the XYZ colorimetric system specified in JIS Z8781-3:2016 according to JIS Z8724:2015 from the spectrum data in the wavelength region of 465 to 780 nm of the fluorescence spectrum.
[0144] <600nm light absorption>
[0145] A standard reflector with a reflectivity of 99% (Spectralon (registered trademark) manufactured by Labsphere) was placed at the side opening of the integrating sphere. Monochromatic light with a wavelength of 600 nm was introduced into the integrating sphere through an optical fiber from a light source (Xe lamp), and the reflected light spectrum was measured by a spectrophotometer (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.). At this time, the number of incident light photons (Qex(600)) was calculated from the spectrum in the wavelength range of 590 to 610 nm.
[0146] Next, after the concave groove is filled with β-sialon phosphor in a manner that the surface becomes smooth and is set at the opening of the integrating sphere, monochromatic light with a wavelength of 600nm is irradiated, and the incident reflected light spectrum is measured by a spectrophotometer. The incident reflected light photon number (Qref(600)) is calculated from the obtained spectral data. The incident reflected light photon number (Qref(600)) is calculated in the same wavelength range as the incident light photon number (Qex(600)). The 600nm light absorption rate is calculated based on the following formula from the two obtained photon numbers.
[0147] 600nm light absorption rate = ((Qex(600)-Qref(600)) / Qex(600))×100
[0148] The measured values of the absorptivity, internal quantum efficiency, external quantum efficiency and chromaticity X of the relevant phosphors have the situation that the values change when the manufacturer of the measuring device, the manufacturing batch number, etc. are changed. Therefore, as various measured values, the values measured by the measuring method recorded in this specification are adopted. However, when the manufacturer of the measuring device, the manufacturing batch number, etc. are changed, the measured values obtained by the standard sample of the above-mentioned β-type Sialon phosphor can also be used as the reference value to correct the various measured values. As the standard sample for obtaining the reference value, the standard sample of the β-type Sialon phosphor cited as the above-mentioned comparative example I-9 can be used.
[0149] [Table 1]
[0150]
[0151] (Comparative Example II-1)
[0152] [Preparation of Europium-activated β-sialon phosphor]
[0153] In a container, each raw material is weighed so that silicon nitride (Si3N4) becomes 96.0 mass%, aluminum nitride (AlN) becomes 2.8 mass%, aluminum oxide (Al2O3) becomes 0.5 mass% and europium oxide (Eu2O3) becomes 0.7 mass%, and mixed by a V-type mixer (manufactured by Tsutsui Rikagaku Kikai Co., Ltd.) to obtain a mixture. The obtained mixture is completely passed through a sieve with a mesh of 250 μm and agglomerates are removed to obtain a raw material composition. Agglomerates that do not pass through the sieve are crushed and the particle size is adjusted so as to pass through the sieve.
[0154] 200 g of the raw material composition prepared as above was weighed into a cylindrical boron nitride container with a lid (manufactured by Denka Co., Ltd., a molded product with boron nitride (trade name: Denka boron nitride N-1) as the main component, inner diameter: 10 cm, height: 10 cm). Thereafter, the container was placed in an electric furnace equipped with a carbon heater, heated to 2020°C in a nitrogen atmosphere (pressure: 0.90 MPaG), and heated at a heating temperature of 2020°C for 8 hours (calcination process). After heating, the sample that slowly condensed into a block in the above container was collected in a mortar and crushed. After crushing, the first calcined body in powder form was obtained by passing through a sieve with a mesh of 250 μm.
[0155] Next, the first calcined body is filled into a cylindrical boron nitride container, and the container is placed in an electric furnace equipped with a carbon heater. The temperature is raised to 1450°C in an argon atmosphere (pressure: 0.025 MPaG), and heating is performed at 1450°C for 3 hours (annealing process). After heating, the agglomerates formed by the particles slowly agglomerating in the container are crushed in a mortar and passed through a 250 μm sieve to obtain a powder.
[0156] Next, the obtained powder is added to a mixed acid of hydrofluoric acid (concentration: 50% by mass) and nitric acid (concentration: 70% by mass) (hydrofluoric acid and nitric acid are mixed in a volume ratio of 1:1), and the acid treatment is performed for 30 minutes while stirring at a temperature of 75°C. After the acid treatment, the stirring is terminated and the powder is allowed to settle, and the supernatant and the fine powder obtained by the acid treatment purification are removed. Thereafter, distilled water is further added and stirred again. The stirring is terminated and the powder is allowed to settle, and the supernatant and the fine powder are removed. By repeating this operation at a pH of 8 or less in the aqueous solution until the supernatant becomes transparent, the obtained precipitate is filtered and dried to obtain a europium-activated β-sialon phosphor.
[0157] (Comparative Example II-2)
[0158] In the annealing step, the mixture was adjusted so that the amount of cerium oxide was 0.1 mass % relative to the total amount of the first calcined body and cerium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example II-1.
[0159] (Comparative Example II-3)
[0160] In the annealing step, the mixture was adjusted so that the amount of cerium oxide was 0.5 mass % relative to the total amount of the first calcined body and cerium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example II-1.
[0161] (Comparative Example II-4)
[0162] In the annealing step, the mixture was adjusted so that the amount of lanthanum oxide was 0.1 mass % relative to the total amount of the first calcined body and lanthanum oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example II-1.
[0163] (Comparative Example II-5)
[0164] In the annealing step, the mixture was adjusted so that the amount of lanthanum oxide was 0.5 mass % relative to the total amount of the first calcined body and lanthanum oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example II-1.
[0165] (Example II-1)
[0166] In the annealing step, the mixture was adjusted so that the amount of gadolinium oxide was 0.1 mass % relative to the total amount of the first calcined body and gadolinium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example II-1.
[0167] (Example II-2)
[0168] In the annealing step, the mixture was adjusted so that the amount of gadolinium oxide was 0.5 mass % relative to the total amount of the first calcined body and gadolinium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example II-1.
[0169] (Example II-3)
[0170] In the annealing step, the mixture was adjusted so that the amount of gadolinium oxide was 1 mass % relative to the total amount of the first calcined body and gadolinium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example II-1.
[0171] (Comparative Example II-6)
[0172] In the annealing step, the mixture was adjusted so that the amount of gadolinium oxide was 5 mass % relative to the total amount of the first calcined body and gadolinium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example II-1.
[0173] (Comparative Example II-7)
[0174] A standard sample of β-sialon phosphor (manufactured by SIALON CORPORATION, NIMS Standard Green lot No. NSG1301) was used as the phosphor of Comparative Example II-7.
[0175] <Determination of the Content of Gadolinium, Cerium and Lanthanum>
[0176] The contents of gadolinium, cerium, and lanthanum in each of the europium-activated β-sialon phosphors prepared in Examples II-1 to II-3 and Comparative Examples II-1 to II-7 were measured by the following method.
[0177] <Contents of gadolinium, cerium, and lanthanum>
[0178] The contents of gadolinium, cerium and lanthanum in the europium-activated β-sialon phosphor were determined by the following steps. The phosphor was dissolved by pressurized acid decomposition to prepare a sample solution. The obtained sample solution was measured by quantitative analysis of the elements using an ICP emission spectrophotometer (manufactured by Rigaku Co., Ltd., trade name: CIROS-120). It should be noted that the detection limits of gadolinium (Gd), cerium (Ce) and lanthanum (La) were 100 ppb, respectively.
[0179] [Evaluation of Europium-activated β-sialon phosphor]
[0180] For each of the europium-activated β-sialon phosphors prepared in Examples II-1 to II-3 and Comparative Examples II-1 to II-7, the absorbance when irradiated with excitation light of a wavelength of 455 nm, the internal quantum efficiency and the external quantum efficiency, the chromaticity X, the chromaticity Y, and the absorbance when irradiated with excitation light of a wavelength of 600 nm were evaluated by the methods described below. The results are shown in Table 2.
[0181] <Absorption rate, internal quantum efficiency and external quantum efficiency>
[0182] The absorptivity (excitation light absorptivity), internal quantum efficiency and external quantum efficiency of the fluorescent body when irradiated with an excitation light of a wavelength of 455nm, are calculated by the following steps. First, the fluorescent body to be measured is filled in a concave groove in a manner that the surface becomes smooth, and is installed in the opening of an integrating sphere. Using an optical fiber, monochromatic light with a wavelength of 455nm split from a Xe lamp as a light source is introduced into the above-mentioned integrating sphere as the excitation light of the fluorescent body. The monochromatic light as the excitation light is irradiated on the fluorescent body to be measured, and the fluorescence spectrum is measured. During the measurement, a spectrophotometer (manufactured by Otsuka Electronics Co., Ltd., trade name: MCPD-7000) is used.
[0183] The luminous intensity of the phosphor is determined by the data of the obtained fluorescence spectrum. In addition, the number of excitation reflected light photons (Qref) and the number of fluorescence photons (Qem) are calculated from the data of the obtained fluorescence spectrum. The number of excitation reflected light photons is calculated in the same wavelength range as the number of excitation light photons, and the number of fluorescence photons is calculated in the range of 465 to 800 nm. In addition, using the same device, a standard reflector with a reflectivity of 99% (manufactured by Labsphere, Spectralon (registered trademark)) is installed at the opening of the integrating sphere, and the spectrum of the excitation light with a wavelength of 455 nm is measured. At this time, the number of excitation light photons (Qex) is calculated from the spectrum in the wavelength range of 450 to 465 nm.
[0184] From the above calculation results, the absorptivity of the 455 nm excitation light, the internal quantum efficiency, and the external quantum efficiency of the phosphor to be measured were determined based on the calculation formula shown below.
[0185] Absorption rate of 455nm excitation light = ((Qex-Qref) / Qex)×100
[0186] Internal quantum efficiency = (Qem / (Qex-Qref)) × 100
[0187] External quantum efficiency = (Qem / Qex) × 100
[0188] In addition, based on the above formula, the relationship between the external quantum efficiency, the absorptivity of the excitation light of 455 nm, and the internal quantum efficiency can be expressed as follows.
[0189] External quantum efficiency = 455nm light absorption × internal quantum efficiency
[0190] <Chroma X and Y>
[0191] The chromaticity X and Y are obtained by calculating the x value (chromaticity X) and the y value (chromaticity Y) of the CIE chromaticity coordinate in the XYZ colorimetric system specified in JIS Z8781-3:2016 according to JIS Z8724:2015 from the spectrum data in the wavelength region of 465 to 780 nm of the fluorescence spectrum.
[0192] <600nm light absorption>
[0193] A standard reflector with a reflectivity of 99% (Spectralon (registered trademark) manufactured by Labsphere) was placed at the side opening of the integrating sphere. Monochromatic light with a wavelength of 600 nm was introduced into the integrating sphere through an optical fiber from a light source (Xe lamp), and the reflected light spectrum was measured by a spectrophotometer (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.). At this time, the number of incident light photons (Qex(600)) was calculated from the spectrum in the wavelength range of 590 to 610 nm.
[0194] Next, the concave groove is filled with β-sialon phosphor in a manner that the surface becomes smooth and is set at the opening of the integrating sphere, and then irradiated with monochromatic light of a wavelength of 600nm, and the incident reflected light spectrum is measured by a spectrophotometer. The incident reflected light photon number (Qref(600)) is calculated from the obtained spectral data. The incident reflected light photon number (Qref(600)) is calculated in the same wavelength range as the incident light photon number (Qex(600)). The 600nm light absorption rate is calculated based on the following formula from the two obtained photon numbers.
[0195] 600nm light absorption rate = ((Qex(600)-Qref(600)) / Qex(600))×100
[0196] The measured values of the absorptivity, internal quantum efficiency, external quantum efficiency, chromaticity X and chromaticity Y of the phosphor may change when the manufacturer of the measuring device, the manufacturing batch number, etc. are changed. Therefore, as various measured values, the values measured by the measuring method described in this specification are adopted. However, when the manufacturer of the measuring device, the manufacturing batch number, etc. are changed, the measured values obtained by the standard sample of the above-mentioned β-type Sialon phosphor can also be used as the reference value to correct the various measured values. As the standard sample for obtaining the reference value, the standard sample of the β-type Sialon phosphor cited as the above-mentioned comparative example II-7 can be used.
[0197] [Table 2]
[0198]
[0199] (Comparative Example III-1)
[0200] [Preparation of Europium-activated β-sialon phosphor]
[0201] In a container, each raw material is weighed so that silicon nitride (Si3N4) becomes 96.0 mass%, aluminum nitride (AlN) becomes 2.8 mass%, aluminum oxide (Al2O3) becomes 0.5 mass% and europium oxide (Eu2O3) becomes 0.7 mass%, and mixed by a V-type mixer (manufactured by Tsutsui Rikagaku Kikai Co., Ltd.) to obtain a mixture. The obtained mixture is completely passed through a sieve with a mesh of 250 μm and agglomerates are removed to obtain a raw material composition. Agglomerates that do not pass through the sieve are crushed and the particle size is adjusted so as to pass through the sieve.
[0202] 200 g of the raw material composition prepared as above was weighed into a cylindrical boron nitride container with a lid (manufactured by Denka Co., Ltd., a molded product with boron nitride (trade name: Denka boron nitride N-1) as the main component, inner diameter: 10 cm, height: 10 cm). Thereafter, the container was placed in an electric furnace equipped with a carbon heater, heated to 2020°C under a nitrogen atmosphere (pressure: 0.90 MPaG), and heated at a heating temperature of 2020°C for 8 hours (calcination process). After heating, the sample that slowly condensed into a block in the above container was collected in a mortar and crushed. After crushing, the first calcined body in powder form was obtained by passing through a sieve with a mesh of 250 μm.
[0203] Next, the first calcined body is filled into a cylindrical boron nitride container, and the container is placed in an electric furnace equipped with a carbon heater. The temperature is raised to 1450°C in an argon atmosphere (pressure: 0.025 MPaG), and heating is performed at a heating temperature of 1450°C for 3 hours (annealing process). After heating, the agglomerates formed by the particles slowly agglomerating in the container are crushed in a mortar and passed through a 250 μm sieve to obtain a powder.
[0204] Next, the obtained powder is added to a mixed acid of hydrofluoric acid (concentration: 50% by mass) and nitric acid (concentration: 70% by mass) (hydrofluoric acid and nitric acid are mixed in a volume ratio of 1:1), and the acid treatment is performed for 30 minutes while stirring at a temperature of 75°C. After the acid treatment, the stirring is terminated and the powder is allowed to settle, and the supernatant and the fine powder obtained by the acid treatment purification are removed. Thereafter, distilled water is further added and stirred again. The stirring is terminated and the powder is allowed to settle, and the supernatant and the fine powder are removed. By repeating this operation at a pH of 8 or less in the aqueous solution until the supernatant becomes transparent, the obtained precipitate is filtered and dried to obtain a europium-activated β-sialon phosphor.
[0205] (Example III-1)
[0206] In the annealing step, the mixture was adjusted so that the amount of magnesium oxide was 0.1 mass % relative to the total amount of the first calcined body and magnesium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example III-1.
[0207] (Example III-2)
[0208] In the annealing step, the mixture was adjusted so that the amount of magnesium oxide was 0.5 mass % relative to the total amount of the first calcined body and magnesium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example III-1.
[0209] (Example III-3)
[0210] In the annealing step, the mixture was adjusted so that the amount of magnesium oxide was 1 mass % relative to the total amount of the first calcined body and magnesium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example III-1.
[0211] (Comparative Example III-2)
[0212] In the annealing step, the mixture was adjusted so that the amount of magnesium oxide was 5 mass % relative to the total amount of the first calcined body and magnesium oxide was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example III-1.
[0213] (Example III-4)
[0214] In the annealing step, the mixture was adjusted to have an amount of strontium carbonate of 0.1 mass % relative to 100 mass % of the total amount of the first calcined body and strontium carbonate, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example III-1.
[0215] (Example III-5)
[0216] In the annealing step, the mixture was adjusted to have an amount of strontium carbonate of 0.5 mass % relative to 100 mass % of the total amount of the first calcined body and strontium carbonate, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example III-1.
[0217] (Example III-6)
[0218] In the annealing step, the mixture was adjusted so that the amount of strontium carbonate was 1 mass % relative to the total amount of the first calcined body and strontium carbonate was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example III-1.
[0219] (Example III-7)
[0220] In the annealing step, the mixture was adjusted so that the amount of strontium carbonate was 1.5 mass % relative to the total amount of the first calcined body and strontium carbonate was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example III-1.
[0221] (Comparative Example III-3)
[0222] In the annealing step, the mixture was adjusted so that the amount of strontium carbonate was 5 mass % relative to the total amount of the first calcined body and strontium carbonate was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example III-1.
[0223] (Comparative Example III-4)
[0224] In the annealing step, the mixture was adjusted in such a way that the amount of lithium carbonate was 0.5 mass % relative to the total amount of the first calcined body and lithium carbonate was 100 mass %, and then heated in an argon atmosphere. A europium-activated β-sialon phosphor was obtained in the same manner as in Comparative Example III-1.
[0225] (Comparative Example III-5)
[0226] A standard sample of β-sialon phosphor (manufactured by SIALON CORPORATION, NIMS Standard Green lot No. NSG1301) was used as the phosphor of Comparative Example III-5.
[0227] <Determination of the content of alkaline earth metal elements (magnesium, strontium and lithium)>
[0228] The contents of alkaline earth metal elements (magnesium, strontium, and lithium) in the europium-activated β-sialon phosphors prepared in Examples III-1 to III-7 and Comparative Examples III-1 to III-5 were measured by the following method.
[0229] <Contents of magnesium, strontium and lithium>
[0230] The contents of magnesium, strontium and lithium in the europium-activated β-sialon phosphor were determined by the following steps. The phosphor was dissolved by a pressurized acid decomposition method to prepare a sample solution. The obtained sample solution was measured by quantitative analysis of the elements using an ICP emission spectrophotometer (manufactured by Rigaku Co., Ltd., trade name: CIROS-120). It should be noted that the detection limits of magnesium (Mg), strontium (Sr) and lithium (Li) were 100 ppb, respectively.
[0231] [Evaluation of Europium-activated β-sialon phosphor]
[0232] For each of the europium-activated β-sialon phosphors prepared in Examples III-1 to III-7 and Comparative Examples III-1 to III-5, the absorbance and internal quantum efficiency when irradiated with excitation light of a wavelength of 455 nm, chromaticity X, chromaticity Y, and absorbance when irradiated with excitation light of a wavelength of 600 nm were evaluated by the methods described below. The results are shown in Table 3.
[0233] <Absorption rate and internal quantum efficiency>
[0234] The absorptivity (excitation light absorptivity) and internal quantum efficiency of the fluorescent body when irradiated with an excitation light of a wavelength of 455nm are calculated by the following steps. First, the fluorescent body to be measured is filled in a concave groove in a manner that the surface becomes smooth, and is installed in the opening of an integrating sphere. Using an optical fiber, monochromatic light with a wavelength of 455nm split from a Xe lamp as a light source is introduced into the above-mentioned integrating sphere as the excitation light of the fluorescent body. The monochromatic light as the excitation light is irradiated on the fluorescent body as the object of measurement, and the fluorescence spectrum is measured. During the measurement, a spectrophotometer (manufactured by Otsuka Electronics Co., Ltd., trade name: MCPD-7000) is used.
[0235] The luminous intensity of the phosphor is determined by the data of the obtained fluorescence spectrum. In addition, the number of excitation reflected light photons (Qref) and the number of fluorescence photons (Qem) are calculated from the data of the obtained fluorescence spectrum. The number of excitation reflected light photons is calculated in the same wavelength range as the number of excitation light photons, and the number of fluorescence photons is calculated in the range of 465 to 800 nm. In addition, using the same device, a standard reflector with a reflectivity of 99% (manufactured by Labsphere, Spectralon (registered trademark)) is installed at the opening of the integrating sphere, and the spectrum of the excitation light with a wavelength of 455 nm is measured. At this time, the number of excitation light photons (Qex) is calculated from the spectrum in the wavelength range of 450 to 465 nm.
[0236] From the above calculation results, the absorptivity of the 455 nm excitation light, the internal quantum efficiency, and the external quantum efficiency of the phosphor to be measured were determined based on the calculation formula shown below.
[0237] Absorption rate of 455nm excitation light = ((Qex-Qref) / Qex)×100
[0238] Internal quantum efficiency = (Qem / (Qex-Qref)) × 100
[0239] External quantum efficiency = (Qem / Qex) × 100
[0240] In addition, based on the above formula, the relationship between the external quantum efficiency, the absorptivity of the excitation light of 455 nm, and the internal quantum efficiency can be expressed as follows.
[0241] External quantum efficiency = 455nm light absorption × internal quantum efficiency
[0242] <Chroma X and Y>
[0243] The chromaticity X and Y are obtained by calculating the x value (chromaticity X) and the y value (chromaticity Y) of the CIE chromaticity coordinate in the XYZ colorimetric system specified in JIS Z8781-3:2016 according to JIS Z8724:2015 from the spectrum data in the wavelength region of 465 to 780 nm of the fluorescence spectrum.
[0244] <600nm light absorption>
[0245] A standard reflector with a reflectivity of 99% (Spectralon (registered trademark) manufactured by Labsphere) was placed at the side opening of the integrating sphere. Monochromatic light with a wavelength of 600 nm was introduced into the integrating sphere through an optical fiber from a light source (Xe lamp), and the reflected light spectrum was measured by a spectrophotometer (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.). At this time, the number of incident light photons (Qex(600)) was calculated from the spectrum in the wavelength range of 590 to 610 nm.
[0246] Next, the concave groove is filled with β-sialon phosphor in a manner that the surface becomes smooth and is set at the opening of the integrating sphere, and then irradiated with monochromatic light of a wavelength of 600nm, and the incident reflected light spectrum is measured by a spectrophotometer. The incident reflected light photon number (Qref(600)) is calculated from the obtained spectral data. The incident reflected light photon number (Qref(600)) is calculated in the same wavelength range as the incident light photon number (Qex(600)). The 600nm light absorption rate is calculated based on the following formula from the two obtained photon numbers.
[0247] 600nm light absorption rate = ((Qex(600)-Qref(600)) / Qex(600))×100
[0248] The measured values of the absorptivity, internal quantum efficiency, external quantum efficiency, peak wavelength and half-value width of fluorescence, chromaticity X and chromaticity Y of the phosphor may change when the manufacturer of the measuring device, the manufacturing batch number, etc. are changed. Therefore, as various measured values, the values measured by the measuring method described in this specification are adopted. However, in the case of changing the manufacturer of the measuring device, the manufacturing batch number, etc., the measured values obtained by the standard sample of the above-mentioned β-type Sialon phosphor can also be used as the reference value to correct the various measured values. As the standard sample for obtaining the reference value, the standard sample of the β-type Sialon phosphor cited as the above-mentioned comparative example III-5 can be used.
[0249] [Table 3]
[0250]
[0251] Industrial Applicability
[0252] According to the present disclosure, a europium-activated β-sialon phosphor having excellent internal quantum efficiency can be provided.
Claims
1. A europium-activated β-sialon phosphor having a composition represented by the formula Si 6-Z Al Z O Z N 8-Z :Eu, where in the formula, 0.0 < Z ≤ 4.2 and the valence of europium is 2 or 3. The europium-activated β-sialon phosphor contains magnesium, the content of which is greater than 0 ppm and less than 252.3 ppm, or contains strontium, the content of which is greater than 0 ppm and less than 264.2 ppm, The absorption rate of the europium-activated β-sialon phosphor to excitation light with a wavelength of 600 nm is 7% or less.
2. The europium-activated β-sialon phosphor according to claim 1, wherein The content of magnesium is 0.1 to 1.3 ppm, or the content of strontium is 0.1 to 6.2 ppm.
3. A light emitting device comprising: a light emitting element that emits primary light, and a wavelength converter that absorbs a portion of the primary light and emits secondary light having a wavelength longer than that of the primary light; The wavelength converter comprises the europium-activated β-sialon phosphor according to claim 1 or 2.
Citation Information
Cited By
Eu-activated beta-sialon phosphor particles, beta-sialon phosphor powder, and light-emitting device
CN118786198A