Coating liquid for forming titanic oxide-containing film
A coating liquid with surface-treated titanium oxide particles and a mixed solvent system addresses agglomeration and photocatalytic issues, achieving a transparent, uniform film with high refractive index and light resistance.
Patent Information
- Application Number
- JP2023059611
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing coating compositions using titanium oxide particles suffer from agglomeration due to impurities like sodium from sodium silicate, leading to non-uniform film thickness and reduced transparency, while compositions with high silicon oxide content do not adequately suppress photocatalytic activity, affecting long-term durability.
A coating liquid comprising surface-treated titanium oxide particles with specific organosilicon compounds and a mixed solvent system, along with a binder and photocurable monomers, is used to form a film with high refractive index, uniform thickness, and enhanced light resistance.
The solution results in a transparent, uniform film with suppressed photocatalytic activity, maintaining high refractive index and resistance to degradation, even under prolonged exposure to light.
Smart Images

Figure 2024146607000001 
Figure 2024146607000002 
Figure 2024146607000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating liquid for forming a titanium oxide-containing film. [Background technology]
[0002] Conventionally, films with a high refractive index (high refractive index films) have been used for various applications, such as displays for smartphones and televisions, lenses for glasses, etc. The properties required for such high refractive index films include, of course, a high refractive index, high transparency, a uniform film thickness (no film unevenness), and performance that does not deteriorate even when exposed to light for a long time (high light resistance).
[0003] Generally, methods for obtaining a high refractive index film can be broadly divided into dry methods, such as vacuum deposition and sputtering, in which a metal oxide with a high refractive index, such as titanium oxide, is used to form a film, and wet methods in which a coating liquid containing inorganic oxide particles (filler) with a high refractive index, a binder component, and an organic solvent is applied to a substrate, dried, and then cured to form a film.
[0004] The dry method produces a dense and hard film, but because the process is carried out under vacuum, the area of film that can be produced at one time is limited, raising concerns about costs and productivity.
[0005] On the other hand, the wet method is widely used in recent years because it allows film formation under atmospheric pressure and has excellent continuous productivity.
[0006] Here, a coating composition is disclosed that contains composite oxide fine particles in which the surfaces of rutile-type titanium oxide particles having a refractive index of 1.5 to 2.8 are coated with a metal oxide raw material having excellent light resistance (sodium silicate or potassium silicate), a curable binder, and an organic solvent (see, for example, Patent Document 1).
[0007] A film formed from such a coating composition has a high refractive index derived from titanium oxide, but because the titanium oxide particles are coated with an inorganic oxide having high light resistance, photocatalytic activity is reduced, resulting in a coating film with excellent light resistance.
[0008] Also disclosed is a coating agent that contains core-shell particles in which inorganic oxide particles are coated with a hydrolyzate of a tetrafunctional organosilicon compound (tetraethoxysilane) on the surface of rutile-type titanium oxide particles with excellent ultraviolet absorption ability, and a silicone resin (see, for example, Patent Document 2). The film obtained by applying this coating agent contains a large amount of silicon compounds with excellent light resistance, so the film is less likely to deteriorate even if photocatalysis originating from titanium oxide occurs. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2006-342311 A [Patent Document 2] International Publication No. 2018 / 096914 Summary of the Invention [Problem to be solved by the invention]
[0010] The coating film made of the coating composition described in Patent Document 1 contains sodium derived from sodium silicate. Such impurities cause the inorganic oxide particles and binder components contained in the paint to aggregate, reducing the transparency and uniformity of the film thickness when the film is formed. Furthermore, in order to improve the dispersibility in organic solvents and curable binders, the surface of titanium oxide particles coated with sodium silicate is treated with an organosilicon compound such as methyltrimethoxysilane. However, since the side chain of the organosilicon compound is a treatment agent with a small number of carbon atoms such as a methyl group, it has poor compatibility with organic solvents and binders, causing particle aggregation during film formation. As a result, in addition to reducing transparency, a film with a uniform thickness cannot be obtained.
[0011] The coating agent described in Patent Document 2 has a high proportion of silicon oxide in the film and has excellent light resistance, but since it does not suppress the photocatalytic action of titanium oxide itself, there is a concern that the binder components may deteriorate with long-term use.
[0012] Therefore, an object of the present invention is to provide a coating material which, even if it contains titanium oxide, has high light resistance and is capable of forming a coating film which is highly transparent and has a uniform thickness. [Means for solving the problem]
[0013] The coating liquid of the present invention contains first surface-treated particles in which a first organosilicon compound is bonded to the surface of a particle containing titanium oxide, a second organosilicon compound, a binder component, and an organic solvent. The titanium oxide has a rutile crystal structure, and the first silicon compound "SiX4" is bonded to the surface of the particle containing titanium oxide in an amount of 3 to 10 mass% in terms of SiO2, and the second silicon compound "R-(CH2) n The molar ratio (second organosilicon compound / first organosilicon compound) of "SiX3" or a hydrolyzate thereof to the first organosilicon compound is 0.3 to 2.0, and the solid content contains 2 to 20 mass % of silicon derived from the first organosilicon compound and the second organosilicon compound in terms of SiO2 (X is at least one selected from an alkoxy group, a hydroxyl group, and a halogen; R is an acryl group or a methacryl group; n is an integer of 1 to 8). The organic solvent is a mixed solvent containing a low-boiling organic solvent (S1) with a boiling point of less than 95°C and a high-boiling organic solvent (S2) with a boiling point of 95°C or higher, and the mass ratio (M S1 / M S2 The mass ratio (M) of the inorganic oxide component (F) and the binder component (B) contained in the first surface-treated particles and the second organosilicon compound is 85 / 15 to 50 / 50. F / M B ) is 45 / 55~95 / 5.
[0014] The film formed from such a coating solution has high light resistance because the photocatalytic activity of titanium oxide is reduced by the first organosilicon compound bonded to the surface of the titanium oxide-containing particles. In addition, the side chain "R-(CH2)n The presence of "-" improves the dispersibility of the particles in the coating solution and film, allowing them to be dispersed within the system without agglomeration. In addition, the inclusion of a mixed solvent adjusts the drying speed of the film, allowing it to be formed in a uniform state. Furthermore, because the mixing ratio of the components that form the film (first surface-treated particles, second organosilicon compound, binder component) is appropriate, a highly transparent and uniform film with no unevenness in film thickness can be obtained. In other words, a titanium oxide-containing coating solution that can achieve all of the following properties is obtained: high refractive index, high light resistance, high transparency, and film thickness uniformity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The titanium oxide-containing coating solution according to the present invention contains titanium-containing particles whose surfaces have been modified with two types of organosilicon compounds, a binder, and two types of organic solvents with different boiling points. By using such a coating solution, it is possible to form a film that has high light resistance, high transparency, and uniformity (less unevenness in film thickness) even if it contains titanium oxide.
[0016] [Titanium oxide-containing particles] The crystal structure of titanium oxide is classified into rutile type, anatase type, and brookite type. The titanium oxide in the titanium oxide-containing particles used in the present invention has a rutile type crystal structure from the viewpoint of a high refractive index and high light resistance.
[0017] Particles containing titanium oxide having a rutile crystal structure may contain other elements as long as they contain Ti element, and for example, a particle dispersion liquid containing titanium oxide described in JP 2009-155496 A can be used.
[0018] [First organosilicon compound] A first organosilicon compound is bonded to the surface of the titanium oxide-containing particle. The first organosilicon compound is represented by the general formula "SiX4". X is at least one selected from an alkoxy group, a hydroxyl group, and a halogen. When such a first organosilicon compound is bonded to the surface of the titanium oxide-containing particle, the deterioration of the binder component due to the photocatalytic activity of titanium oxide is suppressed, and the second organosilicon compound described below is easily bonded to the particle surface. The first organosilicon compound coats the particle by hydrolyzing a part or all of X and bonding with the hydroxyl group on the particle surface. In the present invention, the coating does not necessarily mean that the organosilicon compound completely covers the entire particle surface. X is preferably an ethoxy group.
[0019] The first organosilicon compound bonded to the titanium oxide-containing particle surface is 3 to 10 mass % as SiO2 relative to 100 mass parts of the titanium oxide-containing particle. When the particles are coated in the above range, the first organosilicon compound can sufficiently coat the particle surface while maintaining the high refractive index derived from the titanium oxide, and the second organosilicon compound can be easily bonded. In addition, the photocatalytic activity derived from the titanium oxide can be suppressed.
[0020] [Secondary organosilicon compounds] The second organosilicon compound has the general formula "R-(CH2) n The second organosilicon compound is represented by the formula "SiX3" (X is at least one selected from an alkoxy group, a hydroxyl group, and a halogen; R is an acrylic group or a methacrylic group; and n is an integer of 1 to 8). Such a second organosilicon compound is bonded to the particle surface by a hydrolysis polycondensation reaction, improving the dispersibility of the particles (the first surface-treated particles to which the second organosilicon compound is bonded are referred to as second surface-treated particles). In addition, the side chain "R-(CH2) n The presence of "-" improves compatibility (wettability) with the binder component, and as the coating solution dries during film formation, it dries in a uniform state without layer separation, even if the concentrations of particles containing titanium oxide and the binder component become high. As a result, a transparent, uniform film is obtained without the particles agglomerating. In addition, the photocatalytic activity derived from titanium oxide can be suppressed. The preferred number of n is 3.
[0021] The second organosilicon compound is contained in a molar ratio (first / second) of 0.3 to 2.0 with respect to the first organosilicon compound coated on the particle. When contained in the coating liquid in the above range, the second organosilicon compound bonds with the silanol group of the first organosilicon compound coated on the particle surface, and the particles are uniformly dispersed in the dispersion liquid, the coating liquid, and the film. Even if the solid content increases during drying after coating, the particles do not aggregate, and the surface of the film becomes uniform. In addition, the "acrylic group or methacrylic group" contained in the second organosilicon compound reacts with the reactive group of the binder component during curing to form a bond, thereby improving the packing of the particles and contributing to the uniformity of the film surface. In the coating liquid, a free second organosilicon compound that is not bonded to the particle surface may be present. It is preferably 0.4 to 1.9, more preferably 0.4 to 1.5.
[0022] [Binder components] The binder component may be a photocurable monomer that is cured by UV irradiation or a thermosetting monomer that is cured by heat, but in the present invention, taking into consideration application to an organic film with low heat resistance, a photocurable monomer is preferred. The photocurable monomer is not particularly limited as long as it can be cured by UV irradiation, but a monomer having an acrylic group or a methacrylic group is preferably used from the viewpoint of reactivity and compatibility with the surface of the second surface-treated particle.
[0023] The above monomers may be used alone or in combination of two or more. When used alone, it is preferable that the monomer contains three or more polymerizable groups. When used in combination of two or more, it is preferable to use one or more monomers having at least three polymerizable groups.
[0024] [Solid content concentration] The solid content concentration in the coating liquid is preferably 1 to 10% by mass. Here, the solid content in the coating liquid refers to components that do not evaporate even when the coating liquid is heated at 200°C for 3 hours. When the solid content concentration is within the above range, the stability of the coating liquid is improved and the pot life is extended. It is more preferably 1 to 5% by mass.
[0025] [Film forming component] The mass ratio (M F / M B ) is 45 / 55 to 95 / 5. When the mass ratio is within this range, a transparent film with a uniform thickness is obtained without impairing the high refractive index derived from titanium oxide. A mass ratio of 50 / 50 to 80 / 20 is more preferable. The inorganic oxide component contained in the first surface-treated particles and the second organosilicon compound refers to a component that does not volatilize even when heated at 1000°C for 1 hour.
[0026] The amount of silicon derived from the first and second organosilicon compounds in the solid content of the coating solution is 5 to 20 mass% in terms of SiO2. If it is less than 5 mass%, the amount of SiO2 that coats the particles containing titanium oxide is insufficient, so the photocatalytic activity of titanium oxide cannot be suppressed, and as a result, the light resistance of the film decreases. On the other hand, if it exceeds 20 mass%, the content of titanium oxide in the film decreases relatively, and the film refractive index decreases. It is preferably 5.7 to 14.5 mass%, more preferably 5.7 to 10.0%.
[0027] [Organic solvents] The organic solvent is a mixed solvent containing a low-boiling organic solvent (S1) with a boiling point of less than 95°C and a high-boiling organic solvent (S2) with a boiling point of 95°C or more, and the mixing ratio (S1 / S2) is 85 / 15 to 50 / 50. After applying the coating liquid containing the organic solvent, there is a process of evaporating the solvent in the coating liquid regardless of the curing conditions. At that time, if the amount of the low-boiling organic solvent is large, the coating liquid evaporates all at once, and the uniformity of the film decreases due to the influence of convection generated in the film and condensed water due to the latent heat of evaporation of the solvent. On the other hand, if there is a large amount of the high-boiling organic solvent, the solvent tends to remain in the film, and the uniformity of the film decreases. In the case of the above-mentioned mixed solvent, the low-boiling organic solvent evaporates first, concentrating the coating liquid to a certain concentration, and then the high-boiling organic solvent evaporates slowly, thereby obtaining a uniform and transparent film. The boiling point of the high-boiling solvent is preferably 95 to 150°C, more preferably 110 to 150°C.
[0028] The surface tension of the coating material of the present invention is preferably 20 to 25 mN / m. If the surface tension is within this range, the coating material spreads evenly when applied to a substrate, forming a smooth film.
[0029] [Other ingredients] Other components (photopolymerization initiator, leveling agent, etc.) are added to the coating liquid as necessary. The photopolymerization initiator may be a known one. In this case, the photopolymerization initiator is preferably contained in an amount of 1 to 10% by mass relative to the binder component. If the amount is less than 1% by mass, the curing reaction does not proceed easily, and the hardness is likely to decrease. If the amount is more than 10% by mass, the ratio of particles and binder components in the film is reduced, and the hardness and abrasion resistance of the film are likely to decrease. The photopolymerization initiator content is more preferably 4 to 8% by mass.
[0030] A leveling agent may be added to the coating liquid in order to adjust the wettability with the substrate and the leveling property of the surface of the film. The leveling agent is preferably 5 mass % or less in the solid content of the coating liquid, and more preferably is substantially not contained. By substantially not containing a leveling agent, a film can be easily formed on the titanium oxide-containing film made of the coating liquid of the present invention. Examples of the leveling agent include acrylic, acrylic silicone, silicone, and fluorine-based leveling agents.
[0031] [Application method] A film-coated substrate can be manufactured by forming a film on a substrate using the above-mentioned coating liquid. Specifically, the substrate is coated with the coating liquid, and then dried and cured to obtain a film-coated substrate. Examples of the coating method include spin coating, bar coating, gravure coating, and slit coating.
[0032] [Base material] Examples of the substrate to which the coating liquid of the present invention is applied include glass, plastic films, films with hard coat films, etc. The substrate to be used can be selected depending on the application. Examples of plastic films include polyethylene terephthalate (PET), triacetyl cellulose (TAC), acrylic, polycarbonate, cycloolefin polymer, etc. These substrates may have a hard coat (HC) film formed thereon. By forming a titanium oxide-containing film on the HC film, the hardness and scratch resistance of the substrate with the film are increased.
[0033] [Titanium oxide-containing film] The above-mentioned coating liquid is used to directly or indirectly form a titanium oxide-containing film on a substrate. The titanium oxide-containing film is mainly formed of surface-treated particles and a binder component. The titanium oxide-containing coating liquid of the present invention can form a uniform film with high transparency and little film unevenness without adding a leveling agent, and has a low contact angle with water. Therefore, it is useful for an anti-reflection film in which a low refractive index layer is further provided on the coating film of the present invention.
[0034] That is, the contact angle of the titanium oxide-containing film of the present invention with water is preferably 90° or less. If the contact angle of water is 90° or less, when a film is formed on the titanium oxide-containing film, the wettability with the paint applied to the upper layer is good, and a uniform film can be obtained. The contact angle of water is more preferably 70° or less.
[0035] The average surface roughness (Ra) of the titanium oxide-containing film is preferably less than 1 nm. Ra indicates the unevenness of the film surface, and the larger this value, the greater the unevenness of the film surface. In other words, when the value of Ra is large, the film thickness is not uniform, and light is scattered at the uneven parts, resulting in reduced transparency.
[0036] The thickness of the titanium oxide-containing film is appropriately selected depending on the application, but when a low refractive index film is formed on the upper layer and used as an antireflection film, the thickness is preferably 50 to 150 nm. With a thickness in this range, a film with high transparency and excellent antireflection properties can be obtained. EXAMPLES
[0037] [Example 1] Examples of the present invention will now be described in detail.
[0038] <Preparation of first surface-treated particles> First, a titanium oxide-containing particle aqueous dispersion is prepared. The titanium oxide-containing particle aqueous dispersion can be prepared by a known method. In this embodiment, an aqueous dispersion (inorganic oxide concentration 10% by mass) of core-shell particles having a coating layer of a composite oxide of Si and Zr was prepared with reference to Example 6 of JP-A-2009-155496. A cation exchange resin was added to 117.0 g of this aqueous dispersion, and dealkalization was performed. The ion exchange resin was separated and added to a mixed solution of 8.96 g of tetraethoxysilane (manufactured by Tama Chemical Co., Ltd.) and 126.0 g of methanol. After heating and stirring (50°C) for 5 hours, the mixture was cooled to room temperature, and the solvent was replaced from water to methanol using an ultrafiltration membrane. Then, by concentrating, 71.3 g of a first surface-treated particle dispersion (inorganic oxide component concentration 20% by mass) in which a first organic silicon compound was bonded to the surface of particles containing titanium oxide was obtained.
[0039] (Amount of first organosilicon compound bound) The first surface-treated particle dispersion was dried at 100°C for 10 minutes to obtain a first surface-treated particle powder. This powder was heated over a burner to carbonize the organic components, and then sodium peroxide and sodium hydroxide were added. The mixture was dissolved, and sulfuric acid and hydrochloric acid were added to obtain a sample. The sample was subjected to measurement of the Si concentration in the sample using an ICP optical emission spectrometer ICP-OES (Shimadzu Corporation ICPS-8100), and the Si content was calculated and then converted into the SiO2 content.
[0040] The SiO2 content of the titanium oxide-containing particle dispersion was also measured in the same manner, and the difference in the SiO2 content between the titanium oxide-containing particles and the first surface-treated particles was taken as the binding amount of the first organosilicon compound.
[0041] <Preparation of second surface-treated particles> 4.9 g of 3-methacryloxypropyltrimethoxysilane (KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd.) was added to 80.0 g of the first surface-treated particle dispersion, and then the mixture was heated and stirred for 18 hours at 50° C. Then, the solvent was replaced with propylene glycol monomethyl ether (PGME) using a rotary evaporator, and 71.9 g of a second surface-treated particle dispersion with an inorganic oxide component concentration of 20 mass % was obtained.
[0042] (Molar Ratio of First Organosilicon Compound and Second Organosilicon Compound) The molar ratio (second / first) of the second organosilicon compound to the first organosilicon compound was calculated from the number of moles calculated from the combined amount of the above-mentioned first organosilicon compound and the number of moles calculated from the amount of the second organosilicon compound added during the preparation of the second surface-treated particles.
[0043] <Preparation of titanium oxide-containing coating solution> 10.24g of the second surface-treated particle dispersion was mixed with 0.09g of 1,6-hexadiol diacrylate (Tomoe Kogyo Co., Ltd.: SR-238F) and 0.81g of dipentaerythritol hexaacrylate (Kyoeisha Chemical Co., Ltd.: DPE-6A) as binder components, 0.05g of diphenyl (2,4,6 trimethylbenzoyl)-phenylphosphine oxide (IGMResins B.V.: OMNIRAD (registered trademark) TPO-H) as a photopolymerization initiator, and 79.67g of isopropyl alcohol (IPA) and 9.12g of PGME as organic solvents to prepare a titanium oxide-containing coating liquid with a solid content concentration of 3% by mass. The surface tension of this coating liquid was 22mN / m. The surface tension of the coating material was measured by the plate method (Wilhelmy method) using an automatic surface tensiometer (DY-300, manufactured by Kyowa Interface Science Co., Ltd.) at a temperature of 25°C for the titanium oxide-containing coating liquid.
[0044] <Preparation of titanium oxide-containing film-coated substrate> The titanium oxide-containing coating solution was applied to a TAC film (manufactured by Fuji Film Corporation: FT-80UL, thickness: 80 μm, refractive index: 1.49) with a hard coat layer (manufactured by JGC Catalysts and Chemicals Co., Ltd., ELCOM HC-A) by the bar coater method (#4), dried at 80 °C for 120 seconds, and then applied at 400 mJ / cm under a N2 atmosphere. 2 The titanium oxide-containing film was cured by irradiation with ultraviolet light of 1000 nm to obtain a substrate with a titanium oxide-containing film. The film thickness of the substrate with a titanium oxide-containing film was about 70 to 130 nm. Substrates with a titanium oxide-containing film were also prepared in the same manner in the other examples and comparative examples.
[0045] "evaluation" The titanium oxide-containing film-attached substrate was evaluated by the following methods. The results of other examples and comparative examples are also shown in Table 2.
[0046] (exterior) The surface of the substrate with the titanium oxide-containing film was visually observed and evaluated according to the following criteria.
[0047] Evaluation Criteria No defects in appearance such as whitening, streaks, unevenness, or bleeding out are observed on the surface: ◎ Almost no defects in appearance such as whitening, streaks, unevenness, or bleeding out are observed on the surface: ○ Slight appearance defects such as whitening, streaks, unevenness, and bleeding out were observed on the surface: △ Poor appearance such as whitening, streaks, unevenness, and bleeding out were clearly observed on the surface: ×
[0048] (Average roughness R a ) The average roughness (Ra) of the surface of the titanium oxide-containing film-coated substrate and the surface of the antireflective film-coated substrate was measured in a 10 μm square area on the film surface using an atomic force microscope (AFM) (Dimension 3100, manufactured by Bruker Corporation).
[0049] (Refractive Index) A titanium oxide-containing coating solution was spin-coated onto a dummy silicon wafer (Matsuzaki Manufacturing Co., Ltd.: 6-inch dummy wafer (P-type), thickness: 625 μm), and dried at 80 °C for 120 seconds. Then, 400 mJ / cm was applied under a N2 atmosphere.2 The titanium oxide-containing film was then cured by irradiating it with ultraviolet light of 100 nm to form a titanium oxide-containing film, which was used as a sample for measuring the film refractive index. The obtained sample was measured using a spectroscopic ellipsometer (SE-2000, manufactured by Nippon Semilab Co., Ltd.), and the refractive index at a wavelength of 550 nm was taken as the refractive index of the titanium oxide-containing film of the present invention. The thickness of the titanium oxide-containing film was approximately 100 nm.
[0050] (Lightfastness) A sample prepared in the same manner as the refractive index measurement above was irradiated with 100mW ultraviolet light for 6 hours using a metal halide lamp type light resistance tester (Iwasaki Electric Co., Ltd.: Eye Super UV Tester, SUV-F11). The film thickness was then measured using a spectroscopic ellipsometer, and the light resistance was evaluated from the film thickness reduction rate after the test. The film thickness reduction rate was calculated using the formula (1-film thickness after UV irradiation / film thickness before irradiation) x 100 (%). Film thickness reduction rate after light resistance test is less than 5%: ◎ The film thickness reduction rate after light resistance test is 5% or more and less than 10%: 〇 Film thickness reduction rate after light resistance test is 10% or more: ×
[0051] (contact angle) The titanium oxide-containing coating solution was applied to a TAC film (manufactured by Fuji Film Corporation: FT-80UL, thickness: 80 μm, refractive index: 1.49) using a bar coater method (#4), dried at 80 °C for 120 seconds, and then dried at 400 mJ / cm under a N2 atmosphere. 2 The titanium oxide-containing film was cured by irradiating it with ultraviolet light of 1000 nm to form a film, which was used as a sample for contact angle measurement. The thickness of the titanium oxide-containing film was approximately 70 to 130 nm. The contact angle of the obtained sample with a 5 μL droplet of water was measured using a fully automatic contact angle meter (Kyowa Interface Science Co., Ltd.: DM-701).
[0052] [Example 2] A titanium oxide-containing coating liquid was obtained in the same manner as in Example 1, except that 1.6 g of 3-methacryloxypropyltrimethoxysilane (KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd.) was added to 80.0 g of the first surface-treated particle dispersion liquid. The surface tension of this coating liquid was 22 mN / m.
[0053] [Example 3] A titanium oxide-containing coating liquid was obtained in the same manner as in Example 1, except that 6.5 g of 3-methacryloxypropyltrimethoxysilane (KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd.) was added to 80.0 g of the first surface-treated particle dispersion liquid. The surface tension of this coating liquid was 22 mN / m.
[0054] [Example 4] A titanium oxide-containing coating liquid was obtained in the same manner as in Example 1, except that 8.2 g of 3-methacryloxypropyltrimethoxysilane (KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd.) was added to 80.0 g of the first surface-treated particle dispersion liquid. The surface tension of this coating liquid was 22 mN / m.
[0055] [Example 5] A titanium oxide-containing coating liquid was obtained in the same manner as in Example 1, except that 4.9 g of 3-acryloxypropyltrimethoxysilane (KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.) was added to 80.0 g of the first surface-treated particle dispersion liquid. The surface tension of this coating liquid was 15 mN / m.
[0056] [Example 6] A titanium oxide-containing coating liquid was obtained in the same manner as in Example 1, except that 4.9 g of 8-methacryloxyoctyltrimethoxysilane (KBM-5803, manufactured by Shin-Etsu Chemical Co., Ltd.) was added to 80.0 g of the first surface-treated particle dispersion liquid. The surface tension of this coating liquid was 20 mN / m.
[0057] [Example 7] In the preparation of the second surface-treated particles, except that the solvent to be replaced was IPA, 7.32 g of the second surface-treated particle dispersion liquid (inorganic oxide component concentration 20 mass%) obtained in the same manner as in Example 1 was mixed with 0.15 g of 1,6-hexadiol diacrylate (Tomoe Kogyo Co., Ltd.: SR-238F) and 1.35 g of dipentaerythritol hexaacrylate (Kyoeisha Chemical Co., Ltd.: DPE-6A) as binder components, 0.09 g of diphenyl (2,4,6 trimethylbenzoyl)-phenylphosphine oxide (IGMResins B.V.: OMNIRAD (registered trademark) TPO-H) as a photopolymerization initiator, 73.82 g of IPA as an organic solvent, and 17.26 g of PGME to prepare a titanium oxide-containing coating liquid with a solid content concentration of 3 mass%. The surface tension of this coating liquid was 22 mN / m.
[0058] [Example 8] 11.71 g of the second surface-treated particle dispersion obtained in the same manner as in Example 7 was mixed with 0.06 g of 1,6-hexadiol diacrylate (Tomoe Kogyo Co., Ltd.: SR-238F) and 0.54 g of dipentaerythritol hexaacrylate (Kyoeisha Chemical Co., Ltd.: DPE-6A) as binder components, 0.04 g of diphenyl (2,4,6 trimethylbenzoyl)-phenylphosphine oxide (IGMResins B.V.: OMNIRAD (registered trademark) TPO-H) as a photopolymerization initiator, and 70.38 g of IPA and 17.27 g of PGME as organic solvents to prepare a titanium oxide-containing coating liquid with a solid content concentration of 3 mass%. The surface tension of this coating liquid was 22 mN / m.
[0059] [Example 9] 13.17g of the second surface-treated particle dispersion obtained in the same manner as in Example 7 was mixed with 0.03g of 1,6-hexadiol diacrylate (Tomoe Kogyo Co., Ltd.: SR-238F) and 0.27g of dipentaerythritol hexaacrylate (Kyoeisha Chemical Co., Ltd.: DPE-6A) as binder components, 0.02g of diphenyl (2,4,6 trimethylbenzoyl)-phenylphosphine oxide (IGMResins B.V.: OMNIRAD (registered trademark) TPO-H) as a photopolymerization initiator, and 69.23g of IPA and 17.27g of PGME as organic solvents to prepare a titanium oxide-containing coating liquid with a solid content concentration of 3% by mass. The surface tension of this coating liquid was 22mN / m.
[0060] [Example 10] 13.17 g of the second surface-treated particle dispersion obtained in the same manner as in Example 4 was mixed with 0.03 g of 1,6-hexadiol diacrylate (Tomoe Engineering Co., Ltd.: SR-238F) and 0.27 g of dipentaerythritol hexaacrylate (Kyoeisha Chemical Co., Ltd.: DPE-6A) as binder components, 0.02 g of diphenyl (2,4,6 trimethylbenzoyl)-phenylphosphine oxide (IGMResins B.V.: OMNIRAD (registered trademark) TPO-H) as a photopolymerization initiator, and 79.70 g of IPA and 6.80 g of PGME as organic solvents to prepare a titanium oxide-containing coating liquid with a solid content concentration of 3% by mass. The surface tension of this coating liquid was 22 mN / m.
[0061] [Example 11] 3.41 g of the second surface-treated particle dispersion obtained in the same manner as in Example 7 was mixed with 0.03 g of 1,6-hexadiol diacrylate (Tomoe Engineering Co., Ltd.: SR-238F) and 0.27 g of dipentaerythritol hexaacrylate (Kyoeisha Chemical Co., Ltd.: DPE-6A) as binder components, 0.02 g of diphenyl (2,4,6 trimethylbenzoyl)-phenylphosphine oxide (IGMResins B.V.: OMNIRAD (registered trademark) TPO-H) as a photopolymerization initiator, and 78.63 g of IPA and 17.63 g of PGME as organic solvents to prepare a titanium oxide-containing coating liquid with a solid content concentration of 1 mass%. The surface tension of this coating liquid was 22 mN / m.
[0062] [Example 12] 17.07 g of the second surface-treated particle dispersion obtained in the same manner as in Example 7 was mixed with 0.15 g of 1,6-hexadiol diacrylate (Tomoe Engineering Co., Ltd.: SR-238F) and 1.35 g of dipentaerythritol hexaacrylate (Kyoeisha Chemical Co., Ltd.: DPE-6A) as binder components, 0.09 g of diphenyl (2,4,6 trimethylbenzoyl)-phenylphosphine oxide (IGMResins B.V.: OMNIRAD (registered trademark) TPO-H) as a photopolymerization initiator, and 64.42 g of IPA and 16.90 g of PGME as organic solvents to prepare a titanium oxide-containing coating liquid with a solid content concentration of 5% by mass. The surface tension of this coating liquid was 21 mN / m.
[0063] [Example 13] 34.15 g of the second surface-treated particle dispersion obtained in the same manner as in Example 7 was mixed with 0.30 g of 1,6-hexadiol diacrylate (Tomoe Engineering Co., Ltd.: SR-238F) and 2.70 g of dipentaerythritol hexaacrylate (Kyoeisha Chemical Co., Ltd.: DPE-6A) as binder components, 0.18 g of diphenyl (2,4,6 trimethylbenzoyl)-phenylphosphine oxide (IGMResins B.V.: OMNIRAD (registered trademark) TPO-H) as a photopolymerization initiator, and 46.67 g of IPA and 16.00 g of PGME as organic solvents to prepare a titanium oxide-containing coating liquid with a solid content concentration of 10 mass%. The surface tension of this coating liquid was 16 mN / m.
[0064] [Example 14] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 1, except that the amounts of the organic solvents added during preparation of the titanium oxide-containing coating liquid were 48.30 g of IPA and 40.50 g of PGME. The surface tension of this coating liquid was 24 mN / m.
[0065] [Example 15] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 1, except that the organic solvents added during preparation of the titanium oxide-containing coating liquid were 79.67 g of methanol and 9.12 g of PGME. The surface tension of this coating liquid was 23 mN / m.
[0066] [Example 16] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 1, except that the organic solvents added during preparation of the titanium oxide-containing coating liquid were 79.67 g of methyl ethyl ketone (MEK) and 9.12 g of PGME. The surface tension of this coating liquid was 24 mN / m.
[0067] [Example 17] 10.24 g of the second surface-treated particle dispersion obtained in the same manner as in Example 7 was mixed with 0.09 g of 1,6-hexadiol diacrylate (Tomoe Kogyo Co., Ltd.: SR-238F) and 0.81 g of dipentaerythritol hexaacrylate (Kyoeisha Chemical Co., Ltd.: DPE-6A) as binder components, 0.05 g of diphenyl (2,4,6 trimethylbenzoyl)-phenylphosphine oxide (IGMResins B.V.: OMNIRAD (registered trademark) TPO-H) as a photopolymerization initiator, 71.35 g of IPA as an organic solvent, and 17.45 g of normal heptane to prepare a titanium oxide-containing coating liquid with a solid content concentration of 3 mass%. The surface tension of this coating liquid was 19 mN / m.
[0068] [Example 18] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 17, except that the organic solvents added during preparation of the titanium oxide-containing coating liquid were 71.35 g of IPA and 17.45 g of toluene. The surface tension of this coating liquid was 22 mN / m.
[0069] [Example 19] A titanium oxide-containing coating solution was prepared in the same manner as in Example 17, except that the organic solvents added during preparation of the titanium oxide-containing coating solution were 71.35 g of IPA and 17.45 g of isopropyl glycol (I-PG). The surface tension of this coating solution was 24 mN / m.
[0070] [Example 20] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 17, except that the organic solvents added during preparation of the titanium oxide-containing coating liquid were 71.35 g of IPA and 17.45 g of propylene glycol monomethyl ether acetate (PGMEA). The surface tension of this coating liquid was 23 mN / m.
[0071] [Example 21] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 1, except that 6.54 g of tetramethoxysilane (manufactured by Tama Chemical Co., Ltd.) was added instead of tetraethoxysilane when preparing the first surface-treated particles. The surface tension of this coating liquid was 22 mN / m.
[0072] [Example 22] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 1, except that tetrabutoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) was added instead of tetraethoxysilane when preparing the first surface-treated particles. The surface tension of this coating liquid was 22 mN / m.
[0073] [Example 23] 10.24 g of the second surface-treated particle dispersion obtained in the same manner as in Example 1 was mixed with 0.08 g of 1,6-hexadiol diacrylate (SR-238F, manufactured by Tomoe Engineering Co., Ltd.) and 0.68 g of dipentaerythritol hexaacrylate (DPE-6A, manufactured by Kyoeisha Chemical Co., Ltd.) as binder components, 0.05 g of diphenyl(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (OMNIRAD (registered trademark) TPO-H, manufactured by IGM Resins B.V.) as a photopolymerization initiator, 1.50 g of an acrylic silicone copolymer (Disparlon NSH-8430HF, active ingredient concentration 10% by mass, manufactured by Kusumoto Chemical Co., Ltd.) as a leveling agent, and 79.80 g of IPA and 9.15 g of PGME as organic solvents to prepare a titanium oxide-containing coating liquid with a solid content concentration of 3% by mass. The surface tension of this coating liquid was 22 mN / m.
[0074] [Comparative Example 1] A titanium oxide-containing coating liquid was obtained in the same manner as in Example 1, except that the amount of 3-methacryloxypropyltrimethoxysilane (KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd.) used in the preparation of the second surface-treated particles was 0.2 g. The surface tension of this coating liquid was 16 mN / m.
[0075] [Comparative Example 2] A titanium oxide-containing coating liquid was obtained in the same manner as in Example 1, except that the amount of 3-methacryloxypropyltrimethoxysilane (KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd.) used in the preparation of the second surface-treated particles was 9.8 g. The surface tension of this coating liquid was 22 mN / m.
[0076] [Comparative Example 3] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 1, except that the amount of tetraethoxysilane (manufactured by Tama Chemicals) used in preparing the first surface-treated particles was 1.49 g. The surface tension of this coating liquid was 21 mN / m.
[0077] [Comparative Example 4] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 1, except that the amount of tetraethoxysilane (manufactured by Tama Chemicals) used in preparing the first surface-treated particles was 22.40 g. The surface tension of this coating liquid was 21 mN / m.
[0078] [Comparative Example 5] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 1, except that 8.96 g of methyltrimethoxysilane (manufactured by Tama Chemical Co., Ltd.) was added instead of 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: KBM-503) when preparing the first surface-treated particles. The surface tension of this coating liquid was 21 mN / m.
[0079] [Comparative Example 6] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 1, except that the titanium oxide-containing aqueous dispersion liquid used in preparing the first surface-treated particles was an anatase-type titanium oxide-containing particle-type aqueous dispersion liquid prepared with reference to Example 1 of JP-A-2009-155496. The surface tension of this coating liquid was 21 mN / m.
[0080] [Comparative Example 7] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 7, except that the only organic solvent added during preparation of the titanium oxide-containing coating liquid was 88.80 g of IPA. The surface tension of this coating liquid was 22 mN / m.
[0081] [Comparative Example 8] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 1, except that the organic solvent added during preparation of the titanium oxide-containing coating liquid was 88.80 g of PGME alone. The surface tension of this coating liquid was 27 mN / m.
[0082] [Comparative Example 9] A titanium oxide-containing coating liquid was prepared in the same manner as in Example 1, except that the amounts of the organic solvents added during preparation of the titanium oxide-containing coating liquid were 17.30 g of IPA and 71.50 g of PGME. The surface tension of this coating liquid was 25 mN / m.
[0083] [Comparative Example 10] In preparing the titanium oxide-containing coating liquid, 4.39 g of the second surface-treated particle dispersion obtained in the same manner as in Example 7 was mixed with 0.21 g of 1,6-hexadiol diacrylate (Tomoe Engineering Co., Ltd.: SR-238F) and 1.89 g of dipentaerythritol hexaacrylate (Kyoeisha Chemical Co., Ltd.: DPE-6A) as binder components, 0.13 g of diphenyl (2,4,6 trimethylbenzoyl)-phenylphosphine oxide (IGMResins B.V.: OMNIRAD (registered trademark) TPO-H) as a photopolymerization initiator, and 76.12 g of IPA and 17.25 g of PGME as organic solvents to prepare a titanium oxide-containing coating liquid with a solid content concentration of 3% by mass. The surface tension of this coating liquid was 22 mN / m.
[0084] [Comparative Example 11] 114.88 g of the second surface-treated particle dispersion obtained in the same manner as in Example 7 was mixed with 0.03 g of 1,6-hexadiol diacrylate (Tomoe Engineering Co., Ltd.: SR-238F) and 0.27 g of dipentaerythritol hexaacrylate (Kyoeisha Chemical Co., Ltd.: DPE-6A) as binder components, 0.02 g of diphenyl (2,4,6 trimethylbenzoyl)-phenylphosphine oxide (IGMResins B.V.: OMNIRAD (registered trademark) TPO-H) as a photopolymerization initiator, and 681.95 g of IPA and 172.75 g of PGME as organic solvents to prepare a titanium oxide-containing coating liquid with a solid content concentration of 3% by mass. The surface tension of this coating liquid was 22 mN / m.
[0085] [Reference example 1] <Formation of substrate with anti-reflective film> A coating solution for forming a low refractive index film (ELCOM P-5062, manufactured by JGC Catalysts and Chemicals Co., Ltd.) was applied to the substrate with the titanium oxide-containing film obtained in Example 1 by the bar coater method (#4), dried at 80°C for 120 seconds, and then cured by irradiating with 400mJ / cm2 ultraviolet light in a N2 atmosphere to form a low refractive index film, thereby obtaining a substrate with an anti-reflection film. The film thickness of the low refractive index film was about 100nm.
[0086] "evaluation" The properties of the resulting anti-reflective coating were evaluated as follows, and the results are shown in Table 3.
[0087] (exterior) The surface of the anti-reflection film-coated substrate was visually observed and evaluated in the same manner as in the case of the titanium oxide-containing film-coated substrate.
[0088] (reflectance) The reflectance was measured using a microspectrophotometer (OPTM-A1, manufactured by Otsuka Electronics Co., Ltd.) The reflectance of the uncoated TAC substrate at a wavelength of 550 nm was 5.0%.
[0089] [Reference example 2] A substrate with an antireflective film was obtained in the same manner as in Reference Example 1, except that the titanium oxide-containing coating liquid obtained in Example 2 was used.
[0090] [Reference example 3] A substrate with an antireflective film was obtained in the same manner as in Reference Example 1, except that the titanium oxide-containing coating liquid obtained in Example 3 was used.
[0091] [Table 1]
[0092] [Table 2]
[0093] [Table 3]
Claims
1. a first surface-treated particle having a first organosilicon compound represented by formula (1) bonded to the surface of a particle containing titanium oxide; a second organosilicon compound represented by formula (2); A binder component; A coating liquid comprising a mixed solvent containing a low-boiling organic solvent (S1) having a boiling point of less than 95° C. and a high-boiling organic solvent (S2) having a boiling point of 95° C. or higher, The titanium oxide has a rutile crystal structure, the first organosilicon compound is bonded in an amount of 3 to 10 mass % in terms of SiO2 to 10 mass % of 100 mass parts of the particles containing titanium oxide; the molar ratio of the first organosilicon compound to the second organosilicon compound or its hydrolyzed compound (second organosilicon compound / first organosilicon compound) is 0.3 to 2.0; the solid content contains 5 to 20 mass% of silicon derived from the first organosilicon compound and the second organosilicon compound in terms of SiO; The mass ratio of the mixed solvent (M S1 / M S2 ) is between 85 / 15 and 50 / 50; The mass ratio (M F / M B ) is 45 / 55 to 95 / 5. SiX 4 (1) R-(CH 2 ) n SiX 3 (2) (X is at least one selected from an alkoxy group, a hydroxyl group, and a halogen; R is an acryl group or a methacryl group; and n is an integer from 1 to 8.)
2. 2. The coating liquid according to claim 1, having a solids concentration of 1 to 10%.
Citation Information
Patent Citations
Coating and preparation method thereof
CN102304313A
Method for preparing aqueous dispersion sol containing metal oxide fine particle having high refractive index, aqueous dispersion sol obtained by the method, organic solvent dispersion sol and coating composition containing the fine particle
JP2011132484A
Base with hard coated film and coating liquid for forming hard coated film
JP2011136490A
Phosphorus-containing metal oxide fine particle and method for producing the same, coating liquid for forming transparent coating film containing phosphorus-containing metal oxide fine particle, and substrate with transparent coating film
JP2011136871A
Polymer-coated metal oxide microparticle and application thereof
WO2007145285A1