Liquid ink composition, printed matter, lid material for ptp, and ptp wrapping material

A liquid ink composition with polyvinyl butyral resin as the main binder addresses the challenge of low-temperature adhesion to metal foils in PTP packaging, enhancing efficiency and environmental safety.

JP2024146776APending Publication Date: 2024-10-15DIC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024027816
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-27
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional liquid ink compositions for PTP packaging materials face challenges in achieving good adhesion to metal foils when baked at low temperatures, typically around 150°C, which is desired for improved work efficiency and reduced heat damage, while also requiring environmentally friendly alternatives to nitrified cotton and chlorine-based resins.

Method used

The use of a liquid ink composition with polyvinyl butyral resin as the main binder component, accompanied by specific molecular weight and content ratios, along with other environmentally friendly binder resins, ensures excellent adhesion to metal foils even at low baking temperatures, avoiding nitrified cotton and chlorine-based resins.

Benefits of technology

The solution provides a liquid ink composition with enhanced adhesion to metal foils at low temperatures, improving baking efficiency and reducing heat damage, while being environmentally friendly and recyclable, thus meeting regulatory demands.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146776000003
    Figure 2024146776000003
  • Figure 2024146776000004
    Figure 2024146776000004
  • Figure 2024146776000001
    Figure 2024146776000001
Patent Text Reader

Abstract

To provide a liquid ink composition having good adhesion to a metal foil even when carrying out baking at temperatures as low as 150°C.SOLUTION: A liquid ink composition contains a binder resin. A composition having the highest content in the binder resin is polyvinyl butyral resin. A proportion of the polyvinyl butyral resin in a total amount of the binder resin is preferably larger than 50 mass%. The polyvinyl butyral resin preferably has a weight-average molecular weight of 5,000-150,000.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid ink composition, a printed matter, a PTP lid material, and a PTP packaging material. [Background technology]

[0002] Conventionally, PTP packaging materials (press-through packages) are used to package medicines and the like (see Patent Document 1). The PTP packaging material is composed of a container that contains the contents, such as medicines, and a lid material. The container has a pocket-shaped recess that contains the contents, and a flange portion provided at the end of the recess. The lid material (i.e., PTP lid material) has a metal foil (e.g., hard aluminum foil) as a base material, a printing layer and an OP varnish layer sequentially formed on one side of the metal foil, and a printing layer and a heat seal layer sequentially formed on the other side of the metal foil. Then, after the contents, such as medicines, are placed in the recess of the container, the heat seal layer of the lid material is brought into contact with the flange portion of the container and heat-sealed to perform packaging.

[0003] The printing layer of the PTP lid material is usually formed from a liquid ink composition containing a binder resin, a pigment, a solvent, and additives such as wax, and nitrocellulose resin is mainly used as the binder resin in the liquid ink composition. In addition, in the case of packaging materials used for food, etc., various printing substrates or lamination processes are used, and depending on the type of contents or the purpose of use, front printing, in which printing is done from the front side of the material such as plastic film, or reverse printing, in which the direction of the printed pattern or the printing order of the colors is reversed. Conventionally, inks used in this type of lamination processing have widely used a combination of polyurethane resin and vinyl chloride-vinyl acetate copolymer (PVC) resin as a binder resin that can achieve both excellent dispersibility and high film properties.

[0004] However, as exemplified by the Sustainable Development Goals, the trend of the times is to build a recycling-oriented society that reduces substances that may have adverse effects on the human body or the environment, and the laws and regulations surrounding food packaging are becoming stricter worldwide. In particular, in recent years, there has been a demand for stricter regulations on the ingredients used in packaging and their migration into food. In addition, the movement away from plastic is accelerating, and the demand for recyclable packaging is increasing. Therefore, in the development of gravure ink products, it has become necessary to design ink and packaging components using materials that are guaranteed to be safe for the human body and the environment. In particular, vinyl chloride-vinyl acetate copolymer (PVC) is of concern as a substance that hinders packaging recycling for the following reasons (a) and (b). (a) Chlorine-based resins such as polyvinyl chloride can cause corrosion of equipment or piping by releasing hydrogen chloride and generating hydrochloric acid during the thermal decomposition process of recycling. (b) In thermal recycling, which reuses the energy produced when waste is incinerated, the incineration of chlorine-based resins can result in the emission of environmental hormones such as dioxins. Therefore, there will be a need to develop environmentally friendly inks, such as chlorine-free PVC-free inks. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-2922 A Summary of the Invention [Problem to be solved by the invention]

[0006] In general, in the manufacture of a lid material for PTP packaging materials for packaging medicines and the like, the liquid ink composition is used to print on the original roll of metal foil (e.g., hard aluminum foil original roll) constituting the lid material, and then baking is usually performed at a high temperature of about 200°C. Here, in order to improve the work efficiency and reduce the damage that the original roll of metal foil receives from heat, baking at a lower temperature of about 150°C is desired. However, baking at a low temperature of about 150°C causes a decrease in the adhesion of the printing layer to the metal foil.

[0007] Therefore, an object of the present invention is to solve the above-mentioned problems of the conventional technology and to provide a liquid ink composition which has good adhesion to metal foil even when baked at a low temperature of about 150°C. Another object of the present invention is to provide a printed matter, a PTP lid material, and a PTP packaging material that have good adhesion between the substrate and the printed layer and that use an environmentally friendly liquid ink composition that does not use soluble nitrocellulose or chlorine-based resin. [Means for solving the problem]

[0008] As a result of intensive research into solving the above-mentioned problems, the inventors have discovered that in a liquid ink composition containing a binder resin, by making the main component of the binder resin (i.e., the component with the highest content) a polyvinyl butyral resin, the adhesion of the printed layer to the metal foil is good even when the liquid ink composition is printed on a metal foil and baked at a low temperature of about 150°C to form a printed layer, and have thus completed the present invention. That is, the liquid ink composition, printed matter, PTP lid material, and PTP packaging material of the present invention that solve the above problems are outlined below.

[0009] [1] Contains a binder resin; A liquid ink composition, wherein the binder resin has a largest content of polyvinyl butyral resin. The liquid ink composition of the present invention described in [1] above has good adhesion to metal foil even when baked at a low temperature of about 150°C.

[0010] [2] The liquid ink composition according to [1], wherein the proportion of the polyvinyl butyral resin in the total amount of the binder resin is greater than 50 mass%. The liquid ink composition described in [2] above has improved adhesion to metal foil when baked at a low temperature of about 150°C.

[0011] [3] The liquid ink composition according to [1] or [2], wherein the polyvinyl butyral resin has a weight average molecular weight of 5,000 to 150,000. The polyvinyl butyral resin having a weight average molecular weight of 5,000 to 150,000 used in the liquid ink composition described in [3] above is easily available, and by using such a polyvinyl butyral resin, it is possible to obtain an ink having an excellent balance of fluidity and dispersibility.

[0012] [4] The liquid ink composition according to any one of [1] to [3], further comprising at least one resin selected from the group consisting of ketone resins, rosin resins, polyurethane resins, acrylic resins, and cellulose resins (excluding soluble nitrocellulose resins) in an amount of 0.1 to 49 mass% based on the total amount of the binder resin. The liquid ink composition described in [4] above has improved physical properties as an ink and is excellent in printability.

[0013] [5] The liquid ink composition according to any one of [1] to [4], further comprising a wax. The liquid ink composition described in [5] above can prevent blocking during winding and is easy to process.

[0014] [6] The liquid ink composition according to any one of [1] to [5], further comprising at least one solvent selected from the group consisting of aromatic solvents, ketone solvents, ester solvents, and alcohol solvents. In the liquid ink composition described in [6] above, the solubility of the binder resin is good.

[0015] [7] The liquid ink composition according to any one of [1] to [6], which does not contain either soluble nitrocellulose resin or chlorine-based resin. The liquid ink composition described in [7] above is preferred from the standpoint of the environment and health.

[0016] [8] The liquid ink composition according to any one of [1] to [7], which is for use on a metal foil. The liquid ink composition according to any one of the above items [1] to [7] is particularly useful as a liquid ink composition for metal foil.

[0017] [9] A printed matter, characterized by using the liquid ink composition according to any one of [1] to [8]. The printed matter of the present invention described in [9] above has good adhesion in the printed area.

[0018]

[10] The printed matter according to [9], comprising, in this order, a substrate layer, a removable primer layer, and a layer made of the liquid ink composition according to any one of [1] to [8]. The printed matter described in

[10] above has a removable primer layer, which makes it easier to peel off the layer made of the liquid ink composition (printed layer) or the base layer, and improves the recyclability of the base layer.

[0019]

[11] A PTP lid material comprising the printed matter described in [9] or

[10] . The PTP covering material of the present invention described in

[11] above has good adhesion of the printing layer to the substrate.

[0020]

[12] The PTP covering material according to

[11] , comprising, in this order, an OP varnish layer, a layer made of the liquid ink composition according to any one of [1] to [8], a hard aluminum foil, a layer made of the liquid ink composition according to any one of [1] to [8], and a heat seal layer. In the PTP covering material described in

[12] above, even when baking is performed at a low temperature of about 150°C, the adhesion between the layer of the liquid ink composition and the rigid aluminum foil is good, and by baking at a low temperature of about 150°C, damage to the rigid aluminum foil due to heat can be reduced.

[0021]

[13] A PTP packaging material comprising the PTP lid material described in

[11] or

[12] . The PTP packaging material of the present invention described in

[12] above has excellent adhesion between the printing layer and the metal foil, even when the PTP lid portion is baked at a low temperature of about 150°C during production. In addition, because the baking is performed at a low temperature of about 150°C, the durability of the metal foil is high. Effect of the Invention

[0022] According to the present invention, a liquid ink composition that exhibits good adhesion to metal foil even when baked at a low temperature of about 150°C can be provided. Furthermore, according to the present invention, it is possible to provide a printed matter, a PTP lid material, and a PTP packaging material which use such a liquid ink composition and have good adhesion between the substrate and the printed layer. [Brief description of the drawings]

[0023] [Figure 1] FIG. 2 is a cross-sectional view of an example of a PTP lid material of the present embodiment. [Diagram 2] 1 is a cross-sectional view of an example of a PTP packaging material of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The liquid ink composition, printed matter, PTP lid material, and PTP packaging material of the present invention will be illustrated in detail below based on embodiments.

[0025] <Definition> In this specification, the term "liquid ink composition" refers to a liquid printing ink, such as gravure ink or flexo ink, that is applied to a printing method using a printing plate, and is preferably gravure ink or flexo ink, and may also be simply referred to as an "ink composition". In addition, all "ink" used in the following description refers to "printing ink". In addition, all "parts" refer to "parts by mass," "total amount of ink" refers to the total amount of ink including all volatile components such as solvents, and "total amount of ink solids" refers to the total amount of only non-volatile components, excluding volatile components.

[0026] <Liquid ink composition> The liquid ink composition of the present embodiment contains a binder resin, which has the effect of improving adhesion to an adjacent layer (e.g., a metal foil, etc.). The liquid ink composition of the present embodiment is characterized in that the component with the greatest content (i.e., the main component of the binder resin) of the binder resin is a polyvinyl butyral resin.

[0027] In the liquid ink composition used in the printing layer of the conventional PTP lid material, the main component of the binder resin is nitrocellulose resin, etc., and when baking is performed at a low temperature of about 150 ° C, the adhesion to the metal foil is low. Therefore, with the conventional liquid ink composition, baking must be performed at a high temperature of about 200 ° C, which reduces the work efficiency and damages the metal foil from heat. In contrast, the liquid ink composition of the present embodiment has a binder resin main component of polyvinyl butyral resin, so that the adhesion to the metal foil is good even when baking is performed at a low temperature of about 150 ° C. Therefore, by using the liquid ink composition of the present embodiment, baking at a low temperature of about 150 ° C is possible, the work efficiency of baking is improved, and the damage to the metal foil from heat can be reduced.

[0028] (binder resin) The binder resin in the liquid ink composition of this embodiment has a polyvinyl butyral resin (also called the "main resin") as the component contained most abundantly, and may further contain other binder resins (also called the "auxiliary resins"). In this specification, the term "binder resin" refers to a resin having a binding function, and excludes wax, which will be described later.

[0029] -Polyvinyl butyral resin- The polyvinyl butyral resin is excellent in improving adhesion to metal foil, and is also environmentally friendly since its constituent elements are only carbon atoms, hydrogen atoms, and oxygen atoms.

[0030] The polyvinyl butyral resin is not particularly limited and may be any known resin. In general, the polyvinyl butyral resin may be a reaction product obtained by acetalizing polyvinyl alcohol with butyraldehyde through a known reaction.

[0031] The polyvinyl butyral resin has a weight average molecular weight of preferably 5,000 to 150,000, and more preferably 5,000 to 60,000. Polyvinyl butyral resins having a weight average molecular weight of 5,000 to 150,000 are easy to obtain, and by using such polyvinyl butyral resins, it is possible to obtain inks having an excellent balance between fluidity and dispersibility.

[0032] The glass transition temperature (hereinafter sometimes referred to as Tg) of the polyvinyl butyral resin is preferably in the range of 50° C. to 120° C., more preferably in the range of 55° C. to 115° C., and even more preferably in the range of 60° C. to 110° C. In this specification, the glass transition temperature is obtained by measurement using a differential scanning calorimeter.

[0033] The amount of hydroxyl groups in the polyvinyl butyral resin is preferably in the range of 10% by mass to 40% by mass, and more preferably 15% by mass to 30% by mass. By setting the amount of hydroxyl groups in the polyvinyl butyral resin in the above range, an ink having an excellent balance between fluidity and dispersibility can be obtained.

[0034] The amount of acetyl groups in the polyvinyl butyral resin is preferably 8% by mass or less, and more preferably 5% by mass or less. By setting the amount of acetyl groups in the polyvinyl butyral resin within the above range, an ink having an excellent balance between fluidity and dispersibility can be obtained.

[0035] The proportion of the polyvinyl butyral resin in the total amount of the binder resin is preferably more than 50% by mass. Here, this proportion refers to the proportion in terms of solid content. When the proportion of the polyvinyl butyral resin in the total amount of the binder resin is more than 50% by mass, the adhesion of the liquid ink composition to the metal foil is further improved. Furthermore, the proportion of the polyvinyl butyral resin in the total amount of the binder resin is more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and may be 100% by mass (i.e., the entire binder resin may be a polyvinyl butyral resin).

[0036] -Other binder resins- Examples of binder resins (auxiliary resins) other than the polyvinyl butyral resin (main resin) include ketone resins, rosin resins, polyurethane resins, acrylic resins, cellulose resins, polyester resins, vinyl chloride-vinyl acetate copolymer resins, etc., and further examples include polyamide resins, chlorinated polypropylene resins, ethylene-vinyl acetate copolymer resins, vinyl acetate resins, polyvinyl chloride resins and other vinyl chloride resins, alkyd resins, cyclized rubbers, chlorinated rubbers, butyrals, petroleum resins, etc. Among these, examples of other binder resins (auxiliary resins) include ketone resins, rosin resins, polyurethane resins, acrylic resins, and cellulose resins (excluding nitrocellulose resins).

[0037] The content of the other binder resin (auxiliary resin) is preferably in the range of 0.1 to 49% by mass in the total amount of the binder resin. When the content of the other binder resin (auxiliary resin) is 0.1% by mass or more in the total amount of the binder resin, the physical properties of the ink are improved and the printability is improved. When the content of the other binder resin (auxiliary resin) is 49% by mass or less in the total amount of the binder resin, the proportion of the polyvinyl butyral resin (main resin) can be increased, and even when baking is performed at a low temperature of about 150°C, the adhesion to the metal foil is easily improved. The upper limit of the content of the other binder resin (auxiliary resin) is more preferably 45% by mass or less, even more preferably 40% by mass or less, even more preferably 30% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less in the total amount of the binder resin.

[0038] The liquid ink composition of the present embodiment preferably does not contain either a soluble nitrocellulose resin or a chlorine-based resin as a binder resin. A liquid ink composition that does not contain either a soluble nitrocellulose resin or a chlorine-based resin is preferred from the viewpoints of the environment and health. Carcinogenic NDMA (N-nitrosodimethylamine) has been detected in products that use soluble nitrocellulose resin as ink for pharmaceutical PTP packaging materials, and the soluble nitrocellulose, an ink raw material, is suspected to be the cause of the NDMA. However, this liquid ink composition does not contain soluble nitrocellulose resin as a binder resin, which eliminates such concerns. In addition, overseas (some regions such as the EU), the use of chlorine-based resins (such as vinyl chloride-vinyl acetate copolymer resins) is restricted, and because the liquid ink composition does not contain chlorine-based resins as a binder resin, it can be exported worldwide. Furthermore, by making the liquid ink composition contain less or no vinyl chloride-vinyl acetate copolymer resin, the recyclability of the flexible packaging material using the ink can be improved. When a vinyl chloride resin such as a vinyl chloride-vinyl acetate copolymer resin is contained, it causes the problem of corroding recycling equipment, but by reducing the content of vinyl chloride monomers, corrosion of the recycling equipment can be prevented.

[0039] --Ketone resin-- The ketone resin may be any known one, and for example, a formaldehyde resin, a cyclohexanone-formaldehyde resin, a ketone aldehyde condensation resin, or the like may be suitably used.

[0040] --Rosin-based resin-- The rosin resin is not particularly limited as long as it is a resin having a rosin skeleton, but is preferably a rosin-modified maleic acid resin, a rosin ester, a rosin phenol, a polymerized rosin, etc. The rosin resin preferably has a softening point (by the ring and ball method) of 90 to 200°C.

[0041] --Polyurethane resin-- The polyurethane resin is not particularly limited as long as it is a polyurethane resin obtained by reacting a polyol with a polyisocyanate.

[0042] As the polyol, for example, various known polyols generally used in the production of polyurethane resins can be used, and one or more of them may be used in combination. Specific examples of the polyol include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, pentanediol, 3-methyl-1,5-pentanediol, hexanediol, octanediol, 1,4-butynediol, 1,4-butylenediol, diethylene glycol, triethylene glycol, ... Saturated or unsaturated low molecular weight polyols (1), such as ethylene glycol, dipropylene glycol, glycerin, trimethylolpropane, trimethylolethane, 1,2,6-hexanetriol, 1,2,4-butanetriol, sorbitol, and pentaerythritol; these low molecular weight polyols (1) and sebacic acid, adipic acid, phthalic acid, isophthalic acid, terephthalic acid, maleic acid, fumaric acid, succinic acid, oxalic acid, malonic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, tetrahydrofuran ... polyester polyols (2) obtained by dehydration condensation or polymerization of polycarboxylic acids such as trimellitic acid and pyromellitic acid, or their anhydrides; polyester polyols (3) obtained by ring-opening polymerization of cyclic ester compounds, such as lactones such as polycaprolactone, polyvalerolactone, and poly(β-methyl-γ-valerolactone); polycarbonate polyols (4) obtained by reacting the low molecular weight polyols (1) or the like with, for example, dimethyl carbonate, diphenyl carbonate, ethylene carbonate, phosgene, or the like; polybutadiene glycols (5); glycols (6) obtained by adding ethylene oxide or propylene oxide to bisphenol A; and acrylic polyols (7) obtained by copolymerizing, in one molecule, one or more hydroxyethyl groups, hydroxypropyl acrylate, hydroxybutyl acrylate, or the like, or the corresponding methacrylic acid derivatives, with, for example, acrylic acid, methacrylic acid, or an ester thereof. In addition, various known polyether polyols that are generally used in the production of polyurethane resins can be used, and one or more of them may be used in combination. For example, polyether polyols of polymers or copolymers of methylene oxide, ethylene oxide, propylene oxide, tetrahydrofuran, etc. can be mentioned. Specifically, known general-purpose ones such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol can be used. In the polyurethane resin of the present invention, as the polyol, it is preferable to use a polyester polyol, and it is more preferable to use the polyester polyols (2) and polyether polyols.

[0043] Examples of the polyisocyanate include various known aromatic diisocyanates, aliphatic diisocyanates, and alicyclic diisocyanates that are generally used in the production of polyurethane resins. Specific examples of the polyisocyanate include 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 1-methyl-2,4-phenylene diisocyanate, 1-methyl-2,6-phenylene diisocyanate, 1-methyl-2,5-phenylene diisocyanate, 1-methyl-2,6-phenylene diisocyanate, 1-methyl-3,5-phenylene diisocyanate, 1-ethyl-2,4-phenylene diisocyanate, 1-isopropyl-2,4-phenylene diisocyanate, 1,3-dimethyl-2,4-phenylene diisocyanate, 1,3-dimethyl-4,6-phenylene diisocyanate, 1,4-dimethyl-2,5-phenylene diisocyanate, diethylbenzene diisocyanate, diisopropylbenzene diisocyanate, 1-methyl-3, 5-Diethylbenzene diisocyanate, 3-methyl-1,5-diethylbenzene-2,4-diisocyanate, 1,3,5-triethylbenzene-2,4-diisocyanate, naphthalene-1,4-diisocyanate, naphthalene-1,5-diisocyanate, 1-methyl-naphthalene-1,5-diisocyanate, naphthalene-2,6-diisocyanate, naphthalene-2,7-diisocyanate aromatic polyisocyanates such as 1,1-dinaphthyl-2,2'-diisocyanate, biphenyl-2,4'-diisocyanate, biphenyl-4,4'-diisocyanate, 3,3'-dimethylbiphenyl-4,4'-diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, and diphenylmethane-2,4-diisocyanate;Aliphatic or alicyclic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, dodecamethylene diisocyanate, trimethylhexamethylene diisocyanate, 1,3-cyclopentylene diisocyanate, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, 1,3-di(isocyanatemethyl)cyclohexane, 1,4-di(isocyanatemethyl)cyclohexane, lysine diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 2,4'-dicyclohexylmethane diisocyanate, 2,2'-dicyclohexylmethane diisocyanate, and 3,3'-dimethyl-4,4'-dicyclohexylmethane diisocyanate can be used. These polyisocyanates may be used alone or in combination of two or more.;

[0044] A chain extender can also be used for the polyurethane resin. Examples of the chain extender include ethylenediamine, propylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, and the like, as well as amines having a hydroxyl group in the molecule, such as 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, and di-2-hydroxypropylethylenediamine. These chain extenders can be used alone or in combination of two or more.

[0045] In addition, a monovalent active hydrogen compound can be used as a terminal blocking agent for the purpose of stopping the reaction in the polyurethane resin. Examples of such compounds include dialkylamines such as di-n-butylamine, and alcohols such as ethanol and isopropyl alcohol. Furthermore, when it is particularly desired to introduce a carboxyl group into the polyurethane resin, amino acids such as glycine and L-alanine can be used as a reaction stopper. These terminal blocking agents can be used alone or in combination of two or more.

[0046] The polyurethane resin preferably has a weight average molecular weight of 10,000 to 100,000, and more preferably in the range of 15,000 to 80,000. In the present invention, the number average and weight average molecular weights are values ​​measured by gel permeation chromatography (GPC) under the following conditions.

[0047] Measurement equipment: High-speed GPC equipment (Tosoh Corporation "HLC-8220GPC") Column: The following columns manufactured by Tosoh Corporation were used, connected in series. "TSKgel G5000" (7.8mm I.D. x 30cm) x 1 "TSKgel G4000" (7.8mm I.D. x 30cm) x 1 "TSKgel G3000" (7.8mm I.D. x 30cm) x 1 "TSKgel G2000" (7.8mmI.D. x 30cm) x 1 Detector: RI (differential refractometer) Column temperature: 40℃ Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Injection volume: 100 μL (sample concentration 0.4% by mass in tetrahydrofuran solution) Standard sample: A calibration curve was prepared using the following standard polystyrene.

[0048] [Standard polystyrene] "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation

[0049] --Acrylic resin-- The acrylic resin is not particularly limited as long as it is a copolymer of a polymerizable monomer having a (meth)acrylic acid ester as a main component. Examples of the polymerizable monomer include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, iso-octyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, iso-nonyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, and phenoxyethyl (meth)acrylate. Here, "(meth)acrylate" refers to both acrylate and methacrylate. The polymerization method is not particularly limited, and those obtained by known methods such as bulk polymerization, solution polymerization, emulsion polymerization, and suspension polymerization can be used.

[0050] The acrylic resin preferably has a weight average molecular weight of 5,000 to 200,000, and more preferably has a weight average molecular weight in the range of 10,000 to 100,000.

[0051] --Cellulose resin-- Examples of the cellulose resin (cellulose resin) include cellulose ester resins such as cellulose acetate propionate (CAP) and cellulose acetate butyrate (CAB), soluble cellulose resin (also called "nitrocellulose"), hydroxyalkyl cellulose, and carboxyalkyl cellulose, but from the viewpoint of the environment and health, resins other than soluble cellulose resin are preferred. The cellulose ester resin preferably has an alkyl group, and examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a pentyl group, and a hexyl group, and the alkyl group may further have a substituent. The cellulose resin is preferably cellulose acetate propionate or cellulose acetate butyrate.

[0052] The cellulose resin preferably has a weight average molecular weight of 5,000 to 200,000, and more preferably 10,000 to 50,000. The cellulose resin preferably has a glass transition temperature of 120° C. to 180° C. Use of the cellulose resin is expected to improve the blocking resistance, scratch resistance, and other physical properties of the ink film.

[0053] --Polyester resin-- The polyester resin is not particularly limited as long as it is a polyester resin obtained by reacting an alcohol with a carboxylic acid using a known esterification polymerization reaction.

[0054] Examples of the alcohol include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,2-pentanediol, 3-methyl-1,5-pentanediol, hexanediol, octanediol, 1,4-butynediol, and 1,4-butynediol. Examples of the alcohols include diol, diethylene glycol, triethylene glycol, dipropylene glycol, glycerin, trimethylolpropane, trimethylolethane, 1,2,6-hexanetriol, 1,2,4-butanetriol, sorbitol, pentaerythritol, 1,4-cyclohexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, spiroglycol, and isosorbide. These may be used alone or in combination of two or more. Among these, polyfunctional alcohols are preferred.

[0055] Examples of the carboxylic acid include formic acid, acetic acid, propionic acid, butanoic acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid, oleic acid, linoleic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, phthalic acid, and 1,4-cyclohexanedicarboxylic acid. These can be used alone or in combination of two or more. Among them, polyfunctional carboxylic acids are preferred.

[0056] The polyester resin preferably has a weight average molecular weight of 500 to 6,000, and more preferably 1,400 to 5,500.

[0057] --Vinyl chloride-vinyl acetate copolymer resin-- The vinyl chloride-vinyl acetate copolymer resin is not particularly limited as long as it is a copolymer of vinyl chloride and vinyl acetate. The molecular weight is preferably 5,000 to 100,000 in weight average molecular weight, more preferably 10,000 to 70,000. In 100% by mass of the solid content of the vinyl chloride-vinyl acetate copolymer resin, the structure derived from vinyl acetate monomer is preferably 1 to 30% by mass, and the structure derived from vinyl chloride monomer is preferably 70 to 95% by mass. In this case, the solubility in organic solvents is improved, and further the adhesion to the substrate, the film properties, the scratch resistance, etc. are improved. In addition, from the viewpoint of solubility in organic solvents, it is also preferable to have a hydroxyl group derived from a vinyl alcohol structure. The hydroxyl value is preferably 20 to 200 mgKOH / g. In addition, the glass transition temperature is preferably 50°C to 90°C.

[0058] (Coloring agent) The liquid ink composition of the present embodiment preferably contains a colorant. The colorant may be either a colored pigment or a white pigment. The colorant is preferably a pigment, and examples of the colorant include organic pigments and inorganic pigments that are commonly used in inks, paints, recording materials, and the like.

[0059] Examples of the organic pigment include soluble azo pigments, insoluble azo pigments, azo pigments, phthalocyanine pigments, halogenated phthalocyanine pigments, anthraquinone pigments, anthanthrone pigments, dianthraquinonyl pigments, anthrapyrimidine pigments, perylene pigments, perinone pigments, quinacridone pigments, thioindigo pigments, dioxazine pigments, isoindolinone pigments, quinophthalone pigments, azomethine azo pigments, flavanthrone pigments, diketopyrrolopyrrole pigments, isoindoline pigments, indanthrone pigments, and carbon black pigments. In addition, for example, carmine 6B, lake red C, permanent red 2B, disazo yellow, pyrazolone orange, carmine FB, chromophthal yellow, chromophthal red, phthalocyanine blue, phthalocyanine green, dioxazine violet, quinacridone magenta, quinacridone red, indanthrone blue, pyrimidine yellow, thioindigo bordeaux, thioindigo magenta, perylene red, perinone orange, isoindolinone yellow, aniline black, diketopyrrolopyrrole red, daylight fluorescent pigments, etc. In addition, both non-acid-treated pigments and acid-treated pigments can be used. Specific examples of preferred organic pigments are listed below.

[0060] Examples of black pigments include CI Pigment Black 1, CI Pigment Black 6, CI Pigment Black 7, CI Pigment Black 9, and CI Pigment Black 20.

[0061] Examples of indigo pigments include CI Pigment Blue 15, CI Pigment Blue 15:1, CI Pigment Blue 15:2, CI Pigment Blue 15:3, CI Pigment Blue 15:4, CI Pigment Blue 15:5, CI Pigment Blue 15:6, CI Pigment Blue 16, CI Pigment Blue 17:1, CI Pigment Blue 22, CI Pigment Blue 24:1, CI Pigment Blue 25, CI Pigment Blue 26, CI Pigment Blue 60, CI Pigment Blue 61, CI Pigment Blue 62, CI Pigment Blue 63, CI Pigment Blue 64, CI Pigment Blue 75, CI Pigment Blue 79, and CI Pigment Blue 80.

[0062] Examples of green pigments include CI Pigment Green 1, CI Pigment Green 4, CI Pigment Green 7, CI Pigment Green 8, CI Pigment Green 10, and CI Pigment Green 36.

[0063] Examples of red pigments include CI Pigment Red 1, CI Pigment Red 2, CI Pigment Red 3, CI Pigment Red 4, CI Pigment Red 5, CI Pigment Red 6, CI Pigment Red 7, CI Pigment Red 8, CI Pigment Red 9, CI Pigment Red 10, CI Pigment Red 11, CI Pigment Red 12, CI Pigment Red 15, CI Pigment Red 16, CI Pigment Red 17, CI Pigment Red 18, CI Pigment Red 19, CI Pigment Red 20, CI Pigment Red 21, CI Pigment Red 22, CI Pigment Red 23, CI Pigment Red 24, CI Pigment Red 25, CI Pigment Red 26, CI Pigment Red 27, CI Pigment Red 28, CI Pigment Red 29, CI Pigment Red 30, CI Pigment Red 31, CI Pigment Red 32, CI Pigment Red 33, CI Pigment Red 34, CI Pigment Red 35, CI Pigment Red 36, CI Pigment Red 37, CI Pigment Red 38, CI Pigment Red 39, CI Pigment Red 40, CI Pigment Red 41, CI Pigment Red 42, CI Pigment Red 43, CI Pigment Red 44, CI Pigment Red 45, CI Pigment Red 46, CI Pigment Red 47, CI Pigment Red 48, CI Pigment Red 49, CI Pigment Red 50, CI Pigment Red 51, CI Pigment Red 52, CI Pigment Red 53, CI Pig Tread 19, CI Pigment Red 20, CI Pigment Red 21, CI Pigment Red 22, CI Pigment Red 23, CI Pigment Red 31, CI Pigment Red 32, CI Pigment Red 38, CI Pigment Red 41, CI Pigment Red 43, CI Pigment Red 46, CI Pigment Red 48, CI Pigment Red 48:1, CI Pigment Red 48:2, CI Pigment Red 48:3, CI Pigment Red 48:4, CI Pigment Red CI Pigment Red 48:5, CI Pigment Red 48:6, CI Pigment Red 49, CI Pigment Red 49:1, CI Pigment Red 49:2, CI Pigment Red 49:3, CI Pigment Red 52, CI Pigment Red 52:1, CI Pigment Red 52:2, CI Pigment Red 53, CI Pigment Red 53:1, CI Pigment Red 53:2, CI Pigment Red 53:3, CI Pigment Red 54, CI Pigment Red 57, CI Pigment Red 57: 1, CI Pigment Red 58, CI Pigment Red 58:1, CI Pigment Red 58:2, CI Pigment Red 58:3, CI Pigment Red 58:4, CI Pigment Red 60:1, CI Pigment Red 63, CI Pigment Red 63:1, CI Pigment Red 63:2, CI Pigment Red 63:3, CI Pigment Red 64:1, CI Pigment Red 68, CI Pigment Red 68, CI Pigment Red 81:1, CI Pigment Red 83, C.I. Pigment Red 88, CI Pigment Red 89, CI Pigment Red 95, CI Pigment Red 112, CI Pigment Red 114, CI Pigment Red 119, CI Pigment Red 122, CI Pigment Red 123, CI Pigment Red 136, CI Pigment Red 144, CI Pigment Red 146, CI Pigment Red 147, CI Pigment Red 149, CI Pigment Red 150, CI Pigment Red 164, CI Pigment Red Pigment Red 166, CI Pigment Red 168, CI Pigment Red 169, CI Pigment Red 170, CI Pigment Red 171, CI Pigment Red 172, CI Pigment Red 175, CI Pigment Red 176, CI Pigment Red 177, CI Pigment Red 178, CI Pigment Red 179, CI Pigment Red 180, CI Pigment Red 181, CI Pigment Red 182, CI Pigment Red 183, CI Pigment Red 184, CI Pigment Red 185, CI Pigment Red 187, CI Pigment Red 188, CI Pigment Red 190, CI Pigment Red 192, CI Pigment Red 193, CI Pigment Red 194, CI Pigment Red 200, CI Pigment Red 202, CI Pigment Red 206, CI Pigment Red 207, CI Pigment Red 208, CI Pigment Red 209, CI Pigment Red 210, CI Pigment Red 211, CI Pigment Red Pigment Red 213, CI Pigment Red 214, CI Pigment Red 216, CI Pigment Red 215, CI Pigment Red 216, CI Pigment Red 220, CI Pigment Red 221, CI Pigment Red 223, CI Pigment Red 224, CI Pigment Red 226, CI Pigment Red 237, CI Pigment Red 238, CI Pigment Red 239, CI Pigment Red 240, CI Pigment Red 242, CI Pigment Red 245, CIPigment Red 247, CI Pigment Red 248, CI Pigment Red 251, CI Pigment Red 253, CI Pigment Red 254, CI Pigment Red 255, CI Pigment Red 256, CI Pigment Red 257, CI Pigment Red 258, CI Pigment Red 260, CI Pigment Red 262, CI Pigment Red 263, CI Pigment Red 264, CI Pigment Red 266, CI Pigment Red 268, CI Pigment Red 269, CI Pigment Red 270, CI Pigment Red 271, CI Pigment Red 272, CI Pigment Red 279, etc.

[0064] Examples of purple pigments include CI Pigment Violet 1, CI Pigment Violet 2, CI Pigment Violet 3, CI Pigment Violet 3:1, CI Pigment Violet 3:3, CI Pigment Violet 5:1, CI Pigment Violet 13, CI Pigment Violet 19 (γ type, β type), CI Pigment Violet 23, CI Pigment Violet 25, CI Pigment Violet 27, CI Pigment Violet 29, CI Pigment Violet 31, CI Pigment Violet 32, CI Pigment Violet 36, CI Pigment Violet 37, CI Pigment Violet 38, CI Pigment Violet 42, and CI Pigment Violet 50.

[0065] Examples of yellow pigments include CI Pigment Yellow 1, CI Pigment Yellow 3, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, Pigment Yellow 17, CI Pigment Yellow 24, CI Pigment Yellow 42, CI Pigment Yellow 55, CI Pigment Yellow 62, CI Pigment Yellow 65, CI Pigment Yellow 74, CI Pigment Yellow 83, CI Pigment Yellow 86, CI Pigment Yellow 93, CI Pigment Yellow 94, CI Pigment Yellow 95, CI Pigment Yellow 109, CI Pigment Yellow 110, CI Pigment Yellow 117, CI Pigment Yellow 120, CI Pigment Yellow 122, CI Pigment Yellow 124, CI Pigment Yellow 126, CI Pigment Yellow 128, CI Pigment Yellow 129, CI Pigment Yellow 130, CI Pigment Yellow 131, CI Pigment Yellow 132, CI Pigment Yellow 133, CI Pigment Yellow 134, CI Pigment Yellow 135, CI Pigment Yellow 136, CI Pigment Yellow 137, CI Pigment Yellow 138, CI Pigment Yellow 139, CI Pigment Yellow 140, CI Pigment Yellow 141, CI Pigment Yellow 142, CI Pigment Yellow 143, CI Pigment Yellow 144, CI Pigment Yellow 145, CI Pigment Yellow 146, CI Pigment Yellow 147, CI Pigment Yellow 148, CI Pigment Yellow 149, CI Pigment Yellow 150, CI Pigment Yellow 15 Yellow 120, Pigment Yellow 125, CI Pigment Yellow 128, CI Pigment Yellow 129, CI Pigment Yellow 137, CI Pigment Yellow 138, CI Pigment Yellow 139, CI Pigment Yellow 147, CI Pigment Yellow 148, CI Pigment Yellow 150, CI Pigment Yellow 151, CI Pigment Yellow 153, CI Pigment Yellow 154, CI Pigment Yellow 155, CI Pigment Yellow 166, CI Pigment Yellow 168, CI Pigment Yellow 174, CI Pigment Yellow 180, CI Pigment Yellow 185 and CI Pigment Yellow 213.

[0066] Examples of orange pigments include CI Pigment Orange 5, CI Pigment Orange 13, CI Pigment Orange 16, CI Pigment Orange 34, CI Pigment Orange 36, CI Pigment Orange 37, CI Pigment Orange 38, CI Pigment Orange 43, CI Pigment Orange 51, CI Pigment Range 55, CI Pigment Orange 59, CI Pigment Orange 61, CI Pigment Orange 64, CI Pigment Orange 71, and CI Pigment Orange 74.

[0067] Examples of brown pigments include CI Pigment Brown 23, CI Pigment Brown 25, and CI Pigment Brown 26.

[0068] Among them, preferred pigments include CI Pigment Black 7 as a black pigment, CI Pigment Blue 15, CI Pigment Blue 15:1, CI Pigment Blue 15:2, CI Pigment Blue 15:3, CI Pigment Blue 15:4, CI Pigment Blue 15:6 as indigo pigments, CI Pigment Green 7 as a green pigment, and CI Pigment Red 57:1, CI Pigment Red 48:1, CI Pigment Red 48:2, CI Pigment Red 48:3, CI Pigment Red 146, CI Pigment Red 242, CI Pigment Red 185, CI Pigment Red 1 as red pigments. Examples of pigments that can be used include CI Pigment Red 22, CI Pigment Red 178, CI Pigment Red 149, CI Pigment Red 144, CI Pigment Red 166, purple pigments such as CI Pigment Violet 23 and CI Pigment Violet 37, yellow pigments such as CI Pigment Yellow 83, CI Pigment Yellow 14, CI Pigment Yellow 180, and CI Pigment Yellow 139, and orange pigments such as CI Pigment Orange 38, CI Pigment Orange 13, CI Pigment Orange 34, and CI Pigment Orange 64. It is preferable to use at least one or more pigments selected from these groups.

[0069] Examples of the inorganic pigment include white inorganic pigments such as titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, silica, litbones, antimony white, and gypsum. Among the inorganic pigments, titanium oxide is particularly preferred. Titanium oxide is white and is preferred in terms of coloring power, hiding power, chemical resistance, and weather resistance, and from the viewpoint of printing performance, the titanium oxide is preferably treated with silica and / or alumina.

[0070] Examples of inorganic pigments other than white include carbon black, aluminum particles, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, red iron oxide, yellow iron oxide, zircon, and the like. Aluminum is in powder or paste form, but it is preferable to use it in paste form from the standpoint of handleability and safety. Whether leafing or non-leafing aluminum is used is appropriately selected from the standpoint of brightness and concentration.

[0071] The colorant is preferably contained in an amount sufficient to ensure the concentration and coloring power of the liquid ink composition, i.e., 1 to 60% by mass based on the total mass of the ink, and 10 to 90% by mass based on the total amount of solids in the ink. The colorant may be used alone or in combination of two or more kinds.

[0072] (wax) The liquid ink composition of the present embodiment preferably contains a wax. A liquid ink composition containing a wax can prevent blocking during winding and is easy to process.

[0073] As the wax, it is preferable to use a polyolefin wax or a fatty acid amide wax known in the field of liquid ink. Examples of the polyolefin wax include oxidized polyethylene wax and oxidized polypropylene wax. Examples of the fatty acid amide wax include saturated fatty acid amides such as stearic acid amide and palmitic acid amide, unsaturated fatty acid amides such as erucic acid amide, substituted amides, and aromatic amides.

[0074] The content of the wax is not particularly limited and may be within a known range, but is usually preferably within a range of 0.1 to 20% by mass based on the total solid content of the liquid ink composition.

[0075] (solvent) The liquid ink composition of the present embodiment may contain a solvent (preferably an organic solvent), and preferably contains at least one solvent selected from the group consisting of aromatic solvents, ketone solvents, ester solvents, and alcohol solvents. Aromatic solvents, ketone solvents, ester solvents, and alcohol solvents have good solubility for the above-mentioned polyvinyl butyral resin (main resin) and other binder resins (auxiliary resins). The content of the solvent in the liquid ink composition is preferably in the range of 10 to 90% by mass.

[0076] Examples of the aromatic solvent include toluene, xylene, Solvesso #100, Solvesso #150, etc. Examples of the ketone solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc. Examples of the ester solvent include methyl acetate, ethyl acetate, isopropyl acetate, n-propyl acetate, butyl acetate, amyl acetate, ethyl formate, butyl propionate, propylene glycol monomethyl ether acetate, etc. Examples of the alcohol solvent include methanol, ethanol, n-propanol, isopropanol, n-butanol, propylene glycol monomethyl ether, etc. These can be used alone or in a mixture of two or more. In recent years, from the viewpoint of the working environment, it is more preferable not to use aromatic solvents such as toluene and xylene or ketone solvents.

[0077] The liquid ink composition of the present embodiment may contain water as a volatile component together with the organic solvent. The content of water is preferably less than 10% by mass of the total amount of the ink composition. The addition of water can control the drying property of the ink, and in particular in gravure printing, the gradation part with a small amount of ink transfer, which is a characteristic of gravure printing, can be beautifully reproduced. Furthermore, it is particularly preferable that the content of water is in the range of 1 to 5% by mass of the total amount of the ink composition, since this improves the printability. In addition, the addition of water in this way can also reduce the organic solvent component used. Water may be added to the organic solvent in advance to form a water-containing organic solvent, or a specific amount of water may be added separately.

[0078] (others) The liquid ink composition of the present embodiment may further contain, as necessary, an extender pigment, a pigment dispersant, a leveling agent, an antifoaming agent, a plasticizer, an infrared absorbing agent, an ultraviolet absorbing agent, an aromatic agent, a flame retardant, and the like.

[0079] In order to stably disperse the pigment in the solvent, the binder resin alone can be used, but a dispersant can also be used in combination to further stably disperse the pigment. As the dispersant, anionic, nonionic, cationic, amphoteric, or other surfactants can be used. For example, comb-structured polymer compounds in which polyester is added to polyethyleneimine, or alkylamine derivatives of α-olefin maleic acid polymers, etc. can be mentioned. Specifically, the Solsperse series (ZENECA), AJISPER series (AJINOMOTO), and HOMOGENOL series (KAO) can be mentioned. In addition, the BYK series (BYK-Chemie), EFKA series (EFKA), etc. can also be appropriately used. The dispersant is preferably contained in the ink composition in an amount of 0.05% by mass or more relative to the total mass of the ink composition from the viewpoint of storage stability of the ink composition, and 5% by mass or less from the viewpoint of lamination suitability, and more preferably in the range of 0.1 to 2% by mass.

[0080] In the liquid ink composition of this embodiment, the content of polyvinyl butyral resin (main resin) in the total amount of ink is preferably 5 to 30 mass %, the content of other binder resins (auxiliary resins) is preferably 0 to 10 mass %, the content of colorant is preferably 0 to 45 mass %, the content of solvent is preferably 10 to 90 mass %, and the content of other additives (wax, etc.) is preferably 0 to 10 mass %.

[0081] (Production method) The liquid ink composition of the present embodiment can be produced by dissolving and / or dispersing a binder resin, a colorant, etc. in a solvent. For example, a pigment dispersion is produced by dispersing a pigment (colorant) in an organic solvent with a binder resin, and other compounds, etc. are blended with the resulting pigment dispersion as necessary to produce an ink composition.

[0082] The particle size distribution of the pigment in the pigment dispersion can be adjusted by appropriately adjusting the size of the grinding media of the dispersing machine, the packing rate of the grinding media, the dispersion treatment time, the discharge speed of the pigment dispersion, the viscosity of the pigment dispersion, etc. As the dispersing machine, a commonly used machine, such as a roller mill, a ball mill, a pebble mill, an attritor, a sand mill, etc. can be used. When air bubbles or unexpectedly large particles are contained in the ink composition, they deteriorate the quality of the printed matter, so that it is preferable to remove them by filtration, etc. As the filter, a conventionally known filter can be used.

[0083] The viscosity of the ink composition produced by the above method is preferably in the range of 10 mPa s or more from the viewpoint of preventing sedimentation of the pigment and adequately dispersing it, and 1000 mPa s or less from the viewpoint of workability during ink production and printing. The above viscosity is measured at 25°C using a Tokimec B-type viscometer. The viscosity of the ink composition can be adjusted by appropriately selecting the types and amounts of raw materials used, such as binder resins, colorants, solvents, etc. The viscosity of the ink composition can also be adjusted by adjusting the particle size and particle size distribution of the pigment in the ink composition.

[0084] (hardening agent) A curing agent may be used in the liquid ink composition of this embodiment. The liquid ink composition of the present embodiment, even if it is a one-component composition, can be applied to printing and has excellent workability in printing. That is, the liquid ink composition of the present embodiment has excellent ink dispersibility, flowability, etc., whether it is a one-component type that does not use a curing agent or a two-component type that does use a curing agent.

[0085] The curing agent may be any of the curing agents commonly used in organic solvent-based gravure inks, such as isocyanate-based curing agents.

[0086] It is preferable that the liquid ink composition of this embodiment does not use a melamine resin as a curing agent. By not using a melamine resin as a curing agent in the liquid ink composition, generation of formaldehyde can be suppressed.

[0087] From the viewpoint of curing efficiency, the amount of the curing agent added is preferably in the range of 0.3% by mass to 10.0% by mass, and more preferably in the range of 1.0% by mass to 7.0% by mass, based on the total solid content of the liquid ink composition.

[0088] (Application) The liquid ink composition of the present embodiment can be applied to printing on various objects, but is particularly useful as a liquid ink composition for metal foils. As described above, the liquid ink composition of the present embodiment is particularly useful for metal foils because it has high adhesion to metal foils even when baked at a low temperature of about 150°C.

[0089] <Printed material> The printed matter of the present embodiment is characterized by the use of the liquid ink composition of the present embodiment described above. Since the printed matter of the present embodiment uses the liquid ink composition of the present embodiment, the adhesion of the printed part is good.

[0090] The printed matter may be a substrate having a layer (printed layer) made of the liquid ink composition on the substrate. The substrate may be selected as appropriate depending on the application, and may be a metal foil, a resin film, paper, or the like, with metal foil being preferred. The metal foil may be an aluminum foil. The resin film may be made of PET (polyethylene terephthalate), A-PET (amorphous polyethylene terephthalate), PBT (polybutylene terephthalate), BOPP (biaxially oriented polypropylene), PE (polyethylene), PVC (polyvinyl chloride), PS (polystyrene), Ny (nylon), EVOH (ethylene-vinyl alcohol copolymer), or the like. These films may have a metal deposition layer such as aluminum, or a deposition layer of a metal oxide such as silica or alumina, or a binary deposition layer of these. The paper may be made of natural fibers for papermaking such as wood pulp, using a known papermaking machine. Examples of the natural fibers for papermaking include wood pulps such as softwood pulp and hardwood pulp, non-wood pulps such as Manila hemp pulp, sisal hemp pulp and flax pulp, and pulps obtained by chemically modifying these pulps, etc. Types of pulp that can be used include chemical pulps produced by sulfate cooking, acidic / neutral / alkaline sulfite cooking, soda cooking, etc., ground pulp, chemi-ground pulp, thermomechanical pulp, etc. More specifically, these include uncoated papers such as various types of printing paper, gravure paper, kraft paper, Kent paper, copy paper, bleached paper, and newspaper; lightly coated papers; coated papers such as art paper, one-sided art paper, coated paper, one-sided coated paper, and light-weight coated paper; high-quality paper; double-glazed kraft papers for heavy, general, and special use; unbleached wrapping papers such as veined kraft paper and one-sided glossy kraft paper; pure white roll paper; bleached kraft papers such as double-glazed bleached kraft paper and one-sided glossy bleached kraft paper; other bleached wrapping papers; resin-impregnated papers such as paraffin paper, cardboard and paperboard, vapor-deposited papers in which metals such as aluminum are vapor-deposited onto these papers, and laminated papers in which these papers are laminated with metal foil such as aluminum foil.

[0091] The formation of the printing layer on the substrate can be carried out by a general printing method that has been conventionally used for printing on substrates, using various printing inks such as gravure ink, flexographic ink, offset ink, stencil ink, inkjet ink, etc. The printing layer may be provided on one surface or both surfaces of the substrate.

[0092] The printing layer may be a single layer, or may have multiple printing layers. When there are multiple printing layers, the ink composition used for each printing layer may be the same, may be the same composition but with different pigments, or may have different compositions.

[0093] In the case where there are a plurality of such printed layers, for example, a printed matter having a first printed layer formed with a white ink and a second printed layer formed with a colored ink composition in this order can be used. In addition, the printed matter can be arbitrarily configured to have a first printed layer formed with a colored ink composition, a second white printed layer formed with a white ink, and a third white printed layer in this order. When the second or third printed layer is an overprint varnish, it does not need to contain a colorant such as a pigment.

[0094] The base ink is diluted with a diluting solvent to a viscosity and concentration suitable for gravure printing or flexographic printing, and is supplied to each printing unit either alone or in a mixture, for printing.

[0095] (Laminated body) The present disclosure may be a laminated body having a substrate and a printed layer formed by printing the ink composition for flexible packaging laminate on at least a part of the substrate surface. The printed layer on the substrate surface may be in direct or indirect contact with the substrate surface.

[0096] Preferable configurations of the laminate of this embodiment include, for example, the following (1) to (5). (1) Base material / adhesive layer / printing layer / base material (2) Base material / adhesive layer / base material / printing layer / adhesive layer / base material (3) Substrate / adhesive layer / first printed layer / second printed layer / substrate (4) Substrate / adhesive layer / barrier layer / printing layer / adhesive layer / substrate (5) Base material / printing layer / adhesive layer / base material

[0097] However, the laminate of the present embodiment is not limited to the above (1) to (5), and may further include an additional substrate. When multiple substrates are included, the substrates may be the same or different. The substrate may be a substrate such as a sealable sealant film or a multi-layer film including a sealant layer formed of a heat sealant or the like, and the sealable layer is referred to as a sealant layer.

[0098] The adhesive layers may have the same composition or different compositions. Furthermore, an anchor coat layer may be sandwiched between the adhesive layers to improve the adhesive strength of the adhesive layers.

[0099] In the above configurations (1) to (5), the layers between the substrates are laminated via an adhesive layer. However, in another embodiment of the present disclosure, an extrusion lamination configuration may be used in which a molten resin is extruded without providing an adhesive layer. In the case of extrusion lamination, it is preferable to use polyethylene or polypropylene as the extrusion resin. In that case, an imine-based, butadiene-based, or isocyanate-based anchor coat layer may be provided on the printing layer, and a resin may be melt-extruded on the anchor coat layer.

[0100] The laminate of the present disclosure may also have a removable primer layer as a layer in contact with the printed layer or the adhesive layer. That is, the printed matter of the present embodiment may have a substrate layer, a removable primer layer, and a layer (printed layer) made of the liquid ink composition of the present embodiment in this order. By having a removable primer layer, it is possible to easily peel off the printed layer or peel off multiple films, improve the recyclability of the film, and improve the quality of the recycled plastic.

[0101] The primer layer is preferably a film that can be detached from the base material by treatment with an alkaline solution, for example. As the layer that can be detached from the base material by treatment with an alkaline solution, a known one can be used. For example, it dissolves or swells by hydrolysis or the like in an alkaline solution and detaches from the base material. As long as a film that can be detached from the base material by treatment with an alkaline solution can be formed, there is no particular limitation on the type of the composition for forming the primer layer. For example, a composition containing a urethane resin or polyvinyl alcohol is preferable, or a composition containing a resin having an acidic group is also preferable.

[0102] Here, examples of the resin having an acidic group include resins having an acid value such as a polyurethane resin having an acid value, a rosin-modified maleic acid resin, and a rosin-modified fumaric acid resin; polymerizable monomers having a carboxyl group such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, cinnamic acid, or acid anhydrides thereof; polymerizable monomers having a sulfonic acid group such as sulfonated styrene; polymerizable monomers having a sulfonamide group such as vinylbenzenesulfonamide; (meth)acrylic resins, styrene-(meth)acrylic resins, styrene-(anhydrous)maleic acid resins, terpene-(anhydrous)maleic acid resins, etc., which are radical copolymers obtained by copolymerizing polymerizable monomers having an acidic group; acid-modified polyolefin resins, etc. These can be used alone or in combination of two or more.

[0103] In addition to the above-described resins, the composition for forming the primer layer may contain a solvent such as an organic solvent or an aqueous solvent, and additives. Examples of the additives include the same auxiliaries and acidic additives that can be added to the above-described composition for forming the ink layer.

[0104] <PTP lid material> The PTP lid material of the present embodiment is characterized by including the above-described printed matter of the present embodiment. The PTP lid material of the present embodiment has good adhesion of the printing layer to the base material.

[0105] The PTP covering material of this embodiment preferably comprises, in this order, an OP varnish layer, a layer made of the liquid ink composition, a metal foil, a layer made of the liquid ink composition, and a heat seal layer. Here, the layer made of the liquid ink composition (printed layer) and the metal foil (substrate) correspond to the above-mentioned printed matter. In the PTP covering material having such a configuration, even if baking is performed at a low temperature of about 150°C, the adhesion between the layer made of the liquid ink composition and the metal foil is good, and by baking at a low temperature of about 150°C, damage to the metal foil caused by heat can be reduced.

[0106] In one preferred embodiment, the PTP lid material of this embodiment preferably comprises, in this order, an OP varnish layer, a layer of the liquid ink composition, a hard aluminum foil, a layer of the liquid ink composition, and a heat seal layer. In the PTP lid material of this configuration, even if baking is performed at a low temperature of about 150°C, the adhesion between the layer of the liquid ink composition and the hard aluminum foil is good, and by baking at a low temperature of about 150°C, damage to the hard aluminum foil due to heat can be reduced.

[0107] Next, the PTP lid material of this embodiment will be described in more detail with reference to the drawings. Fig. 1 is a cross-sectional view of an example of a PTP lid material of this embodiment. The PTP lid material 10 shown in Fig. 1 comprises a metal foil 1, layers (printed layers) 2 and 3 made of a liquid ink composition provided on both sides of the metal foil 1, an OP varnish layer 4 provided on the side of the layer (printed layer) 2 made of one liquid ink composition that does not contact the metal foil 1, and a heat seal layer 5 provided on the side of the layer (printed layer) 3 made of the other liquid ink composition that does not contact the metal foil 1. In other words, the PTP lid material 10 shown in Fig. 1 comprises the OP varnish layer 4, the layer 2 made of one liquid ink composition, the metal foil 1, the layer 3 made of the other liquid ink composition, and the heat seal layer 5 in this order.

[0108] (Metal foil) As the metal foil 1, foils made of various metals can be used, and among them, hard aluminum foil is preferable. Here, hard aluminum foil (also called "hard aluminum foil") is a foil obtained by rolling raw aluminum, for example, using a roll or the like to thinly stretch it to about 200 μm to 5 μm, and is distinguished from soft aluminum foil, which is obtained by rolling raw aluminum, thinning it, and then heating it at about 400 ° C to soften it.

[0109] The average thickness of the metal foil 1 is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 5 μm to 100 μm, and more preferably 5 μm to 50 μm.

[0110] (Layer made of liquid ink composition (printed layer)) The liquid ink composition of the present embodiment described above can be applied to the layers (printed layers) 2 and 3 made of the liquid ink composition.

[0111] The PTP lid material preferably has a solid printing layer on the metal foil for printing a barcode, and a character printing layer on top of that. In particular, a PTP lid material for pharmaceuticals may need to have a barcode printed on it to prevent misidentification, and even if the barcode (character printing layer) is directly printed on the metal foil, it may be difficult to read. In response to this, the barcode can be made easier to read by first providing a solid printing layer on the metal foil by solid printing, and then printing and forming a barcode (character printing layer) on top of that. Here, the above-mentioned liquid ink composition can be used for the solid print layer and the character print layer. The solid print layer is a layer formed by performing full-surface printing in one color, and from the viewpoint of making the character print layer clear, a light color such as white is preferable. In addition, the above-mentioned liquid ink composition can be used for the solid print layer, in which a light-colored pigment such as a white pigment is blended as a colorant. The solid print layer can be formed by solid printing the liquid ink composition. In addition, the character printing layer is usually a layer formed by printing characters, but in this specification, layers on which bar codes, patterns, pictures, etc. are printed instead of characters depending on the purpose of the printing are also included in the character printing layer.

[0112] The average thickness of the layers (printed layers) 2, 3 made of the liquid ink composition is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 μm to 5 μm, more preferably 0.1 μm to 3 μm.

[0113] Examples of the method for applying the liquid ink composition to the substrate such as the metal foil include a bar coater, a gravure coater, a roll coater, a knife coater, a kiss coater, and the like. The coating amount of the liquid ink composition on the substrate is 0.5 to 5 g / m. 2 The drying conditions are preferably within a range of 120 to 200° C. for 5 to 100 seconds.

[0114] (OP varnish layer) The OP varnish layer (also called the "overprint varnish layer," "overcoat layer," or "topcoat layer") 4 can be made of polyvinyl butyral resin; a blend of epoxy resin and amino resin; cellulose resin such as nitrocellulose resin, cellulose acetate, cellulose propionate, or cellulose butyrate; polyester resins having a benzene ring such as phthalic acid, naphthalene dicarboxylic acid, or an ethylene oxide (hereinafter sometimes referred to as EO) adduct of bisphenol A, and / or an alicyclic skeleton such as cyclopentanediol or dimethyloltricyclodecane; aromatic isocyanates such as diphenylmethane diisocyanate, toluene diisocyanate, xylene diisocyanate, or naphthalene diisocyanate, alicyclic isocyanates such as isophorone diisocyanate or norbornene diisocyanate, and / or urethane resins in which isocyanuric triisocyanate is combined with a polyol and / or tris(2-hydroxyethyl)isocyanurate; Also, polyisocyanates using the above-mentioned isocyanates may be used as the curing agent. Also, compounds having a benzene ring and an unsaturated double bond, such as styrene and phenoxydiethylene glycol acrylate, and / or compounds having an alicyclic structure and an unsaturated double bond, such as isobornyl acrylate and dicyclopentanyl acrylate, and radical copolymers such as (meth)acrylates can be preferably used.

[0115] The OP varnish layer may be colored or may not be colored. When the OP varnish layer is colored, a colorant may be added to the resin, and the colorant may be any of those described in the liquid ink composition section above.

[0116] The average thickness of the OP varnish layer 4 is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 μm to 10 μm, and more preferably 1 μm to 5 μm.

[0117] (Heat seal layer) The heat seal layer 5 contains, as a main resin component, a known thermoplastic resin that imparts heat sealability, and may further contain other components as necessary.

[0118] The thermoplastic resin is not particularly limited and may be appropriately selected from known thermoplastic resins according to the purpose. Examples of the thermoplastic resin include α-olefin resin, styrene resin, ester resin, acrylic resin, cyclic olefin resin, acrylic / olefin resin, vinyl chloride-vinyl acetate copolymer resin, polyester resin, ethylene-vinyl acetate copolymer resin (EVA), chlorinated ethylene-vinyl acetate copolymer resin, ethylene-vinyl alcohol copolymer resin, shellacs, rosins, rosin-modified maleic acid resin, rosin-modified phenolic resin, nitrocellulose resin, cellulose acetate, cellulose acetyl propionate, cellulose acetyl butyrate, chlorinated rubber, cyclized rubber, vinyl chloride, vinylidene chloride, polyamide resin, ketone resin, butyral resin, chlorinated polypropylene resin, chlorinated polyethylene resin, polyurethane resin, styrene-maleic acid resin, casein, and alkyd resin. These may be used alone or in combination of two or more. Among these, α-olefin resin is preferred because it can provide good heat sealability.

[0119] Examples of the α-olefin resin include homopolymers of α-olefin monomers (polyethylene homopolymer, polypropylene homopolymer, etc.), copolymers mainly composed of α-olefin monomers (propylene-ethylene block copolymer, propylene-ethylene random copolymer, ethylene-butene-1 copolymer, propylene-butene-1 copolymer, etc.), etc. These may be used alone or in combination of two or more kinds.

[0120] The thickness ratio of the heat seal layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 20% to 60%, and more preferably 30% to 60%, of the total thickness of the PTP lid material. The average thickness of the heat seal layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 1 μm to 10 μm, and more preferably from 1 μm to 5 μm.

[0121] The heat seal layer is disposed on the substrate directly or via an optional layer (e.g., a printed layer). The heat seal layer can be formed by applying a heat seal agent in which the resin or the like is dispersed or dissolved in a solvent. As such a heat seal agent, a commercially available hot melt seal agent can also be used. The heat seal agent can be applied entirely or partially to the desired outermost surface of the PTP lid material.

[0122] The heat sealing agent is not particularly limited, and may be in any form, such as a type in which the thermoplastic resin having the above-mentioned heat sealability is dissolved in an organic solvent, a type in which the thermoplastic resin is dissolved in water or an aqueous organic solvent, or an emulsion type in which the thermoplastic resin is dispersed in water or an aqueous organic solvent.

[0123] The organic solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the organic solvent include aromatic hydrocarbons such as toluene, xylene, Solvesso #100, Solvesso #150, etc.; aliphatic hydrocarbons such as hexane, heptane, octane, decane, etc.; and various ester-based organic solvents such as methyl acetate, ethyl acetate, isopropyl acetate, butyl acetate, amyl acetate, ethyl formate, butyl propionate, etc. Examples of aqueous organic solvents include alcohols such as methanol, ethanol, propanol, and butanol; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; and glycol ethers such as ethylene glycol (mono, di)methyl ether, ethylene glycol (mono, di)ethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, monobutyl ether, diethylene glycol (mono, di)methyl ether, diethylene glycol (mono, di)ethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, triethylene glycol (mono, di)methyl ether, propylene glycol (mono, di)methyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, and dipropylene glycol (mono, di)methyl ether.

[0124] The heat sealing agent may further contain other components, such as lubricants such as wax and fillers, defoamers, plasticizers, leveling agents, emulsifiers, dispersion stabilizers, surfactants, tackifiers, preservatives, antibacterial agents, rust inhibitors, antioxidants, crosslinking agents, curing agents, curing catalysts, light stabilizers, ultraviolet absorbers, photocatalytic compounds, dyes, inorganic pigments, organic pigments, extender pigments, and antistatic agents.

[0125] (Anchor coat layer) The PTP covering material may further comprise an anchor coat layer between the layer made of the liquid ink composition and the heat seal layer. In particular, in the case of a lid material for PTP for pharmaceutical products, the heat seal layer is preferably free of colorants since it comes into direct contact with the pharmaceutical product in the content portion. Therefore, when it is desired to provide a colored layer on a layer made of a liquid ink composition (for example, the above-mentioned character printing layer), it is preferable to provide an anchor coat layer between the heat seal layer and the layer, and to color the anchor coat layer. The anchor coat layer can be made of the same resin as the heat seal layer described above, and preferably contains a colorant. The colorant used in the anchor coat layer can be any of the colorants described in the liquid ink composition section above. The anchor coat layer can be formed, for example, by applying a coating liquid of the raw material. The average thickness of the anchor coat layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 μm to 10 μm, and more preferably 1 μm to 5 μm.

[0126] (Preferred embodiment of PTP lid material) The following configurations are suitable for the PTP lid material. In the following description, the layers are listed in the order of lamination. In addition, the OP varnish layer is described as "OP varnish layer (uncolored)" and "OP varnish layer (colored)" to distinguish between colored and uncolored cases.

[0127] First embodiment: OP varnish layer (uncolored) / character printing layer / hard aluminum foil / character printing layer / heat seal layer (uncolored) Second embodiment: OP varnish layer (uncolored) / character printed layer / solid printed layer / hard aluminum foil / character printed layer / heat seal layer (uncolored) Third embodiment: OP varnish layer (uncolored) / character print layer / solid print layer / hard aluminum foil / solid print layer / character print layer / heat seal layer (uncolored) Fourth embodiment: OP varnish layer (uncolored) / character printed layer / hard aluminum foil / solid printed layer / character printed layer / heat seal layer (uncolored)

[0128] In the PTP lid materials of the first to fourth embodiment described above, neither the OP varnish layer nor the heat seal layer is colored, and the character printed layer can be seen as it is. In the second embodiment, in order to make the character printed layer on the OP varnish layer side easier to see, a solid printed layer is provided between the character printed layer on the OP varnish layer side and the hard aluminum foil. In the fourth embodiment, in order to make the character printed layer on the heat seal layer side more easily visible, a solid printed layer is provided between the character printed layer on the heat seal layer side and the hard aluminum foil. In addition, in the third embodiment, solid print layers are provided on both sides of the hard aluminum foil to make the character print layers on both the OP varnish layer side and the heat seal layer side more visible.

[0129] Fifth embodiment: OP varnish layer (colored) / character printed layer / hard aluminum foil / character printed layer / anchor coat layer (colored) / heat seal layer (uncolored) Sixth embodiment: OP varnish layer (colored) / character printed layer / solid printed layer / hard aluminum foil / character printed layer / anchor coat layer (colored) / heat seal layer (uncolored) Seventh embodiment: OP varnish layer (colored) / character printed layer / solid printed layer / hard aluminum foil / solid printed layer / character printed layer / anchor coat layer (colored) / heat seal layer (uncolored) Eighth embodiment: OP varnish layer (colored) / character printed layer / hard aluminum foil / solid printed layer / character printed layer / anchor coat layer (colored) / heat seal layer (uncolored)

[0130] In the PTP lid materials of the fifth to eighth embodiment forms, the OP varnish layer is colored, but the heat seal layer is not colored. Also, in order to provide a colored layer on the character print layer on the content side, a colored anchor coat layer is provided between the character print layer and the heat seal layer. In the sixth embodiment, in order to make the character printed layer on the OP varnish layer side easier to see, a solid printed layer is provided between the character printed layer on the OP varnish layer side and the hard aluminum foil. In the eighth embodiment, in order to make the character printed layer on the heat seal layer side more easily visible, a solid printed layer is provided between the character printed layer on the heat seal layer side and the hard aluminum foil. In addition, in the seventh embodiment, solid print layers are provided on both sides of the hard aluminum foil to make the character print layers on both the OP varnish layer side and the heat seal layer side more visible.

[0131] Ninth embodiment: OP varnish layer (not colored) / character printed layer / hard aluminum foil / character printed layer / anchor coat layer (colored) / heat seal layer (not colored) Tenth embodiment: OP varnish layer (uncolored) / character printed layer / solid printed layer / hard aluminum foil / character printed layer / anchor coat layer (colored) / heat seal layer (uncolored) Eleventh embodiment: OP varnish layer (uncolored) / character printed layer / solid printed layer / hard aluminum foil / solid printed layer / character printed layer / anchor coat layer (colored) / heat seal layer (uncolored) Twelfth embodiment: OP varnish layer (uncolored) / character printed layer / hard aluminum foil / solid printed layer / character printed layer / anchor coat layer (colored) / heat seal layer (uncolored)

[0132] In the PTP lid materials of the ninth to twelfth embodiment, neither the OP varnish layer nor the heat seal layer is colored, but in order to provide a colored layer on the character print layer on the content side, a colored anchor coat layer is provided between the character print layer and the heat seal layer. In the tenth embodiment, in order to make the character printed layer on the OP varnish layer side easier to see, a solid printed layer is provided between the character printed layer on the OP varnish layer side and the hard aluminum foil. In the twelfth embodiment, in order to make the character-printed layer on the heat-sealed layer side more easily visible, a solid print layer is provided between the character-printed layer on the heat-sealed layer side and the hard aluminum foil. In addition, in the eleventh embodiment, solid print layers are provided on both sides of the hard aluminum foil to make the character print layers on both the OP varnish layer side and the heat seal layer side more visible.

[0133] Thirteenth embodiment: OP varnish layer (colored) / character printing layer / hard aluminum foil / character printing layer / heat seal layer (uncolored) 14th embodiment: OP varnish layer (colored) / character printed layer / solid printed layer / hard aluminum foil / character printed layer / heat seal layer (uncolored) Fifteenth embodiment: OP varnish layer (colored) / character printed layer / solid printed layer / hard aluminum foil / solid printed layer / character printed layer / heat seal layer (uncolored) Sixteenth embodiment: OP varnish layer (colored) / character printed layer / hard aluminum foil / solid printed layer / character printed layer / heat seal layer (uncolored)

[0134] In the PTP lid materials of the thirteenth to sixteenth embodiment forms, the OP varnish layer is colored, but the heat seal layer is not colored. However, in order to provide a colored layer on the character print layer on the content side, a colored anchor coat layer is provided between the character print layer and the heat seal layer. In the fourteenth embodiment, in order to make the character printed layer on the OP varnish layer side easier to see, a solid printed layer is provided between the character printed layer on the OP varnish layer side and the hard aluminum foil. In the sixteenth embodiment, in order to make the character printed layer on the heat seal layer side more easily visible, a solid printed layer is provided between the character printed layer on the heat seal layer side and the hard aluminum foil. In addition, in the fifteenth embodiment, solid print layers are provided on both sides of the hard aluminum foil to make the character print layers on both the OP varnish layer side and the heat seal layer side more visible.

[0135] In the first to sixteenth embodiments, the liquid ink composition of the present embodiment can be used as at least one of the character print layer and the solid print layer. As the OP varnish layer, for example, an epoxy / melamine-based resin, an epoxy resin, or a nitrocellulose-based resin can be used. As the heat seal layer and the anchor coat layer, for example, a vinyl chloride-vinyl acetate copolymer resin can be used. It should be noted that these embodiments are only some of the preferred examples of the PTP lid material of the present invention, and various configurations can be adopted for the PTP lid material of the present invention.

[0136] Preferably, none of the components of the PTP lid material of the present embodiment contains nitrocellulose resin and chlorine-based resin. A PTP lid material that contains neither nitrocellulose resin nor chlorine-based resin is preferable from the viewpoints of the environment and health. More specifically, since the PTP lid material does not contain nitrocellulose resin, the concern about the generation of NDMA (N-nitrosodimethylamine) can be eliminated. Further, since the PTP lid material does not contain chlorine-based resin, it can be exported worldwide.

[0137] Also, preferably, none of the components of the PTP lid material of the present embodiment contains melamine resin. By the PTP lid material not containing melamine resin, the generation of formaldehyde can be suppressed.

[0138] <PTP packaging material> The PTP packaging material of the present embodiment is characterized by comprising the above-described PTP lid material of the present embodiment. Even when the PTP packaging material of the present embodiment is baked at a low temperature of about 150°C, the adhesion between the printing layer and the metal foil is excellent. Further, since it is baked at a low temperature of about 150°C, the durability of the metal foil is high.

[0139] Next, the PTP packaging material (press-through package) of the present embodiment will be described in more detail with reference to the drawings. FIG. 2 is a cross-sectional view of an example of the PTP packaging material of the present embodiment. The PTP packaging material 100 shown in FIG. 2 is composed of a container 20 that houses contents such as pharmaceuticals, and a PTP lid material 10 adhered to the container 20. The container 20 includes a pocket-shaped recess 21 that houses the contents 30, and a flange portion 22 provided at an end of the recess 21. The contents 30 such as pharmaceuticals (tablets) are directly housed in the recess 21, and the PTP lid material 10 (more specifically, the heat-sealing layer of the PTP lid material 10) is directly adhered to the flange portion 22.

[0140] The above-described PTP lid material of the present embodiment can be applied to the PTP lid material 10.

[0141] The container 20 can be made of a thermoplastic resin sheet made of polyester resin, polyolefin resin, fluorine resin, polyvinyl chloride, polyvinylidene chloride, or the like. Examples of the polyester resin include polyethylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, and polybutylene terephthalate. Examples of the polyolefin resin include polyethylene resin, polypropylene resin, ethylene-vinyl alcohol copolymer resin, and resin made of cyclic olefin. Examples of the fluorine resin include polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether copolymer (EPA), tetrafluoroethylene-ethylene copolymer (ETFE), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), and chlorotrifluoroethylene-ethylene copolymer (ECTFE).

[0142] The PTP packaging material 100 of this embodiment is used by bonding the above-mentioned PTP lid material 10 and container 20 with a heat seal layer. That is, the PTP packaging material 100 can be manufactured by a method in which contents 30 such as medicines (tablets) are placed in the recess 21 of the container 20, and the PTP lid material 10 is placed on the container 20 with the heat seal layer facing the container 20 and thermally bonded.

[0143] The PTP packaging material of the present embodiment can be used as a packaging material for medicines, tablets, and foods such as candy and chocolate, etc. It can also be used as a packaging material for blister packs of toothbrushes, dry batteries, toys, etc.

[0144] It is preferable that none of the components of the PTP packaging material of the present embodiment described above contain soluble nitrocellulose resin or chlorine-based resin. A PTP packaging material that does not contain either soluble nitrocellulose resin or chlorine-based resin is preferable from the viewpoint of the environment and health. More specifically, the PTP packaging material does not contain soluble nitrocellulose resin, which can eliminate concerns about the generation of NDMA (N-nitrosodimethylamine). Furthermore, the PTP packaging material does not contain chlorine-based resin, which makes it possible to export it to all over the world.

[0145] Moreover, it is preferable that none of the components of the PTP packaging material of this embodiment contain melamine resin, which makes it possible to suppress the generation of formaldehyde. EXAMPLES

[0146] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.

[0147] The weight average molecular weight (polystyrene equivalent) was measured by GPC using an HLC8220 system manufactured by Tosoh Corporation under the following conditions. Separation column: Four TSKgel GMHHR-N columns manufactured by Tosoh Corporation were used. Column temperature: 40℃ Mobile phase: Tetrahydrofuran (Wako Pure Chemical Industries, Ltd.) Flow rate: 1.0mL / min Sample concentration: 1.0% by weight Sample injection volume: 100 microliters Detector: Differential refractometer

[0148] <Preparation and Evaluation of Liquid Ink Composition> Each liquid ink composition of the Examples and Comparative Examples was prepared by mixing the components according to the formulation shown in Table 1. For the liquid ink compositions of Comparative Examples 1 to 4, a melamine resin solution was added before use, and the compositions were then used for printing. The obtained liquid ink composition was evaluated for adhesion to substrate, heat resistance (ink bleeding), and printability by the following methods. The results are shown in Table 2.

[0149] (1) Original fabric adhesion After printing each liquid ink composition on a hard aluminum substrate, baking was performed at a temperature of 150 to 200°C for 5 to 15 seconds, and then cellophane tape was applied and peeled off. The peeling of the ink film was visually judged and classified into a score of 1 to 5. The score is in increments of 0.5, with 1 being poor and 5 being good, and the higher the score, the better the adhesion of the ink film to the hard aluminum substrate. Details of the scores are shown below. 5: No peeling at all 4.5: Approximately 5% peeling 4: Approximately 10% peeling 3.5: Approximately 20% peeling 3: Approximately 30% peeled off 2.5: Approximately 50% peeled off 2: Approximately 70% peeled off 1.5: Approximately 80% peeled off 1: Completely peeled off (about 100% peeled off)

[0150] (2) Heat resistance (ink bleeding) After printing each liquid ink composition on a hard aluminum substrate, pressure was applied with a heat seal bar at 230°C and 0.2 N for 40 seconds, and the bleeding (running) of the letter ink was visually judged and rated on a scale of 1 to 5. The ratings are in increments of 0.5, with 1 being poor and 5 being good, and a higher rating indicates less bleeding of the ink and better heat resistance.

[0151] (3) Printability After each liquid ink composition was printed on a hard aluminum substrate, the state of bleeding of the letter ink was checked. In Example 7, the characters were slightly blurred, but in the other Examples and Comparative Examples, the characters were clear and the printability was excellent.

[0152] [Table 1]

[0153] [Table 2]

[0154] *1 Pigment 1: Yellow pigment, product name "SYMULER FAST YELLOW NIF" manufactured by DIC Corporation *2 Pigment 2: Indigo pigment, product name "FASTOGEN BLUE LDB78" manufactured by DIC Corporation *3 Pigment 3: Ink pigment, Cabot Corporation's product name "Carbon Black Mogul L" *4 Pigment 4: White pigment, Ishihara Sangyo Kaisha, Ltd. product name "Tipaku A-220"

[0155] *5 Nitrocellulose resin: 37.5 parts of industrial nitrocellulose L1 / 4 (nitrocellulose, solid content 70%, viscosity at 25.0% solution concentration 9.0-14.9% according to JIS K-6703, product manufactured by Taihei Chemical Products Co., Ltd.) was added with 62.5 parts of a mixture of isopropyl alcohol / ethyl acetate / toluene (ratio of 20 / 30 / 50 by mass) and mixed thoroughly to prepare a nitrocellulose resin solution. This nitrocellulose resin solution was used to prepare a liquid ink composition. Table 1 shows the content as solid content.

[0156] *6 Polyvinyl butyral resin: Polyvinyl butyral resin (weight average molecular weight 19,000, hydroxyl group amount 26 mass%, glass transition point 70°C, acetyl group amount 4 mass% or less) obtained by reacting polyvinyl alcohol with butyl aldehyde was dissolved in methyl ethyl ketone (MEK) and ethyl acetate at 25% to prepare a polyvinyl butyral resin solution. The polyvinyl butyral resin solution was used to prepare a liquid ink composition. Table 1 shows the content as solids.

[0157] *7 Polyurethane resin: 233.38 parts of neopentyl glycol adipate diol (hydroxyl value: 37.4 mg KOH / g), 2.36 parts of polyethylene glycol (hydroxyl value: 280.5 mg KOH / g), and 31.58 parts of isophorone diisocyanate were charged into a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, and reacted at 90°C for 10 hours under a nitrogen stream to produce a urethane prepolymer with an isocyanate group content of 1.77% by mass, to which 66.8 parts of ethyl acetate were added to obtain a homogeneous solution of the urethane prepolymer. Next, the urethane prepolymer solution was added to a mixture of 10.59 parts of isophorone diamine, 0.28 parts of cyclohexylamine, 387.6 parts of ethyl acetate, and 194.7 parts of isopropyl alcohol, and the mixture was stirred and reacted at 45°C for 5 hours to obtain a polyurethane resin solution. The obtained polyurethane resin solution had a resin solid concentration of 30.3 mass%, and the weight average molecular weight (Mw) of the resin solid was 58,000. The polyurethane resin solution was used to prepare a liquid ink composition. Table 1 shows the content as solid content.

[0158] *8 Ketone resin: "TEGO VARIPLUS SK" manufactured by Evonik Tego Chemie GmbH was added. The solid content is shown in Table 1. *9 PE wax: Gifu Shellac Co., Ltd.'s product name "X-7019" was added. Table 1 shows the solid content. *10 Plasticizer: DIC Corporation's product name "Monocizer ATBC" was added. Table 1 shows the content as solid content. *11 Melamine resin: Resonac's product name "Melan X-81" was added. Table 1 shows the content as solid content. *12 Solvent: The total amount of solvent in the liquid ink composition, including methyl ethyl ketone / normal propyl acetate = 1 / 1 (mass ratio) in addition to the solvent used to dissolve the binder resin etc.

[0159] It can be seen from Table 2 that the liquid ink compositions of the examples according to the present invention have excellent adhesion (bonding) to hard aluminum foil even when baked at a low temperature of about 150°C. [Industrial Applicability]

[0160] The liquid ink composition of the present invention can be applied to printing on various objects, and is particularly useful for printing on metal foil. [Explanation of symbols]

[0161] 10: Lid material for PTP 1: Metal foil 2, 3: Layer made of liquid ink composition (printed layer) 4: OP varnish layer 5: Heat seal layer 100:PTP packaging material 20: Container 21: Recess 22: Flange part 30:Contents

Claims

1. Contains a binder resin, A liquid ink composition characterized in that the binder resin has a largest content of polyvinyl butyral resin.

2. The liquid ink composition according to claim 1 , wherein the proportion of the polyvinyl butyral resin in the total amount of the binder resin is greater than 50% by mass.

3. 2. The liquid ink composition according to claim 1, wherein the polyvinyl butyral resin has a weight average molecular weight of 5,000 to 150,000.

4. 2. The liquid ink composition according to claim 1, further comprising at least one resin selected from the group consisting of ketone resins, rosin resins, polyurethane resins, acrylic resins, and cellulose resins (excluding soluble nitrocellulose resins) in an amount of 0.1 to 49 mass% based on the total amount of the binder resin.

5. The liquid ink composition according to claim 1, further comprising a wax.

6. The liquid ink composition according to claim 1, further comprising at least one solvent selected from the group consisting of aromatic solvents, ketone solvents, ester solvents, and alcohol solvents.

7. 2. The liquid ink composition according to claim 1, which contains neither soluble nitrocellulose resin nor chlorine-based resin.

8. The liquid ink composition according to claim 1, which is for use on metal foil.

9. A printed matter, characterized in that the liquid ink composition according to claim 1 is used.

10. 10. The printed matter according to claim 9, comprising, in this order: a substrate layer; a releasable primer layer; and a layer comprising the liquid ink composition according to claim 1.

11. A lid material for PTP, comprising the printed matter according to claim 9.

12. A PTP lid material as described in claim 11, comprising, in this order: an OP varnish layer, a layer made of the liquid ink composition as described in claim 1, a hard aluminum foil, a layer made of the liquid ink composition as described in claim 1, and a heat seal layer.

13. A PTP packaging material comprising the PTP lid material according to claim 12.

Citation Information

Patent Citations

  • Printing ink composition for PTP packaging, and laminate using printing ink composition for PTP packaging

    JP2018002922A