Method for producing calcium-containing composition with fixed co2 and apparatus therefor
By mixing calcium-containing compositions with water and CO2 in a fluidized bed reactor, the method achieves low-moisture, high-versatility immobilization of CO2, addressing the limitations of existing carbonation methods and facilitating integration with cement and concrete.
Patent Information
- Application Number
- JP2024032713
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-15
AI Technical Summary
Existing methods for carbonating calcium components to immobilize CO2 in concrete are hindered by the need for water, which complicates the process, requires additional drying steps, and limits the versatility of the final product due to unpredictable moisture content, making it difficult to integrate with cement and concrete mixtures.
A method involving mixing a calcium-containing composition with water and CO2 gas to achieve a fixed calcium-containing composition with a moisture content of 5% by mass or less, utilizing a fluidized bed reactor for simultaneous carbonation and drying, and using ammonia to enhance the carbonation process.
The method effectively immobilizes CO2 in the calcium-containing composition with low moisture content, ensuring compatibility with cement and concrete applications without the need for separate drying processes, thus enhancing the product's versatility and reducing energy consumption.
Smart Images

Figure 2024146787000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and an apparatus for producing a CO2 fixing calcium-containing composition. [Background technology]
[0002] Since CO2 is a greenhouse gas, it is known to have an impact on global warming. In recent years, there has been a demand for reducing CO2 emissions around the world, especially in developed countries, and this requires reducing the amount of CO2 generated and capturing and effectively using CO2 that has already been generated. In the industrial sector, CO2 emissions are relatively large, particularly from thermal power plants and cement manufacturing plants, and many attempts have been made to reduce CO2 emissions from these facilities by reducing the amount of fossil fuel used, to capture CO2 from exhaust gas, and to immobilize the captured CO2.
[0003] As an attempt to capture and fix CO2, for example, Patent Document 1 describes a technology for effectively fixing CO2 in concrete. It is described that this technology fixes CO2 by producing calcium carbonate through a reaction between calcium hydroxide, which is produced during cement hydration, and added CO2.
[0004] Patent Document 2 also describes a manufacturing method for construction materials that can fix CO2 in a short time. Specifically, it describes that by placing alkaline solids such as coal ash in a container such as a portable container and introducing carbon dioxide gas into the container to carbonate the alkaline solids, carbonation proceeds more quickly than in the case of contacting carbon dioxide with conventional concrete. It describes that calcium components such as calcium oxide contained in alkaline solids such as coal ash and incineration ash are carbonated to produce calcium carbonate. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-37493 A [Patent Document 2] Patent Publication No. 2021-155270 [Non-patent literature]
[0006] [Non-Patent Document 1] Environmental Engineering Research Papers Vol. 41 2004 (49) Basic study on the immobilization of heavy metals by carbonation for the effective utilization of incineration ash Summary of the Invention [Problem to be solved by the invention]
[0007] There have been many attempts to fix CO2 as calcium carbonate by carbonating calcium components, and in order to make the carbonation reaction efficient, it is important that water is present in the reaction between calcium and CO2. This is thought to be because the calcium components react with water and change into calcium hydroxide, which is more likely to promote the carbonation reaction. Calcium hydroxide then reacts with CO2 to change into calcium carbonate. The chemical reaction formula when the calcium component is calcium oxide is shown below (1) and (2).
[0008] Formula (1) CaO+H2O→Ca(OH)2 Formula (2) Ca(OH)2+CO2→CaCO3+H2O
[0009] For example, Non-Patent Document 1 describes an example in which carbonation is applied to insolubilize lead contained in incineration ash. The document describes that when the moisture content of the incineration ash is set to 10 to 20 mass%, a large amount of CO2 is fixed. However, when water is required for the CO2 fixation reaction, the problem is that water remains in the final product. For example, when the product is mixed with cement and used, cement reacts when it comes into contact with water, which is not practically preferable. Furthermore, taking the example of mixing during concrete production, since water is mixed with cement and aggregate at the same time in concrete production, the presence of water itself is not a problem, but if the moisture content is not accurately known, the amount of water brought in from the product is not known, making it impossible to design the mix for concrete. In addition, the moisture content changes depending on various conditions such as the storage state of the product and the weather, making it difficult to manage accurately. For this reason, the presence of water in the product imposes restrictions on subsequent use, resulting in low versatility.
[0010] On the other hand, if a separate drying process is provided to dry the product containing water, energy is required, and if fossil fuels are used as a heat source for drying, CO2 is generated, which is even more undesirable. Furthermore, both reaction equipment and drying equipment are required, making the process complicated.
[0011] Therefore, the objective of the present invention is to obtain a product in which CO2 is fixed, with a low moisture content and high versatility, in a process that does not emit large amounts of CO2, even under efficient carbonation conditions in the presence of water. [Means for solving the problem]
[0012] In view of the above problems, the inventors have conducted intensive research and, as a result, have succeeded in solving the above problems by mixing a calcium-containing composition with water, and then effectively utilizing the CO2-containing gas used for reacting the mixture with CO2 for drying, thereby enabling the reaction operation and drying operation to be carried out in a single device, and in obtaining a CO2-fixing calcium-containing composition with a low water content and in which a sufficient amount of CO2 is fixed, thereby completing the present invention.
[0013] That is, the present invention is a method for producing a CO2-fixed calcium-containing composition by mixing a calcium-containing composition with water to obtain a mixture, and then contacting the mixture with a gas containing CO2 to fix CO2 in the calcium-containing composition, wherein the water content of the CO2-fixed calcium-containing composition is 5 mass% or less when the CO2-fixed calcium-containing composition obtained as a product is taken as 100 mass%.
[0014] In the manufacturing method of the present invention, it is preferable that the reaction of fixing CO2 in the calcium-containing composition using a CO2-containing gas and drying to reduce the water content of the CO2-fixed calcium-containing composition to 5 mass% or less are carried out simultaneously.
[0015] In addition, the amount of water mixed per 100 parts by mass of the dry calcium-containing composition is preferably 10 parts by mass or more, and the amount of water mixed per 100 parts by mass of the dry calcium-containing composition is preferably 10 to 30 parts by mass.
[0016] The temperature of the CO2-containing gas is preferably 60°C or higher, and more preferably 100°C or higher.
[0017] Preferably, the moisture content of the CO2-fixing calcium-containing composition is 1% by mass or less when the CO2-fixing calcium-containing composition obtained as a product is taken as 100% by mass. More preferably, the reaction operation for fixing CO2 in the calcium-containing composition and the drying operation for reducing the moisture content of the CO2-fixing calcium-containing composition to 1% by mass or less are carried out in a single apparatus. Particularly preferably, the reaction operation and the drying operation are carried out in a fluidized bed reactor.
[0018] The gas containing CO2 is preferably gas extracted from a cement clinker production facility or gas extracted from a thermal power generation facility.
[0019] It is preferable that the water to be mixed with the calcium-containing composition contains ammonia.
[0020] Preferably, after producing the CO2 fixing calcium-containing composition, the produced CO2 fixing calcium-containing composition is mixed into Portland cement or blended cement so that the composition is contained in an amount of 5 mass% or less to produce Portland cement or blended cement.
[0021] Preferably, after producing the CO2 fixing calcium-containing composition, the produced CO2 fixing calcium-containing composition is used as a concrete admixture.
[0022] The apparatus for producing a CO2 fixing calcium-containing composition of the present invention comprises: a storage facility for storing the calcium-containing composition; a metering device for supplying the calcium-containing composition to the fluidized bed reactor; a water injection device for mixing water with the calcium-containing composition before it is supplied to the fluidized bed reactor; and a fluidized bed reactor for carrying out a carbonation reaction of the calcium-containing composition. A blower for supplying a gas containing CO2 to the fluidized bed reactor; A dust collector for collecting dust contained in the exhaust gas; and a blower for sucking in exhaust gas. Effect of the Invention
[0023] According to the present invention, a CO2-fixing calcium-containing composition having a low water content and in which a sufficient amount of CO2 is fixed can be obtained in a process that does not emit a large amount of CO2, even under efficient carbonation conditions in the presence of water. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is a schematic diagram of an apparatus for producing a CO2-fixing calcium-containing composition using a fluidized bed reactor according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of the apparatus used in the test. [Diagram 3] FIG. 3 is a characteristic diagram showing the main data in Table 3. [Figure 4] FIG. 4 is a characteristic diagram showing the main data in Table 4. [Diagram 5] FIG. 5 is a schematic diagram of the device of the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The present invention is applied to a method for obtaining a CO2-fixing calcium-containing composition having a water content of 5% by mass or less, preferably 1% by mass or less, when the CO2-fixing calcium-containing composition is taken as 100% by mass, by mixing the calcium-containing composition with water and then effectively utilizing the gas used for the reaction of the mixture with CO2 for drying. Note that various operations in all of the following steps, such as the step of mixing the calcium-containing composition with water and the carbonation step of fixing CO2 in the calcium-containing composition, may be carried out continuously or batchwise.
[0026] Here, the calcium-containing composition is not limited in content as long as it contains calcium in the composition. However, in order to fix CO2 sufficiently, the higher the calcium content, the more preferable. Examples of calcium-containing compositions include incineration ash of general waste, coal ash generated when burning coal in a thermal power plant, biomass ash generated when burning biomass fuel or both coal and biomass fuel in a thermal power plant, slag generated in the process of iron and steel making and various metal refining, and other sludge, cement, gypsum, quicklime, slaked lime, etc. However, when the entire amount of calcium contained in the composition exists as calcium carbonate, calcium is already contained only in a carbonated state, and further fixation of CO2 is not possible, so it is excluded from the calcium-containing composition of the present invention. As the calcium-containing composition, it is preferable that the calcium contained exists in a crystalline form from the viewpoint of good reactivity with CO2. When the entire amount of calcium exists as amorphous, calcium existing as amorphous has low reactivity with CO2 and is inferior in efficiency of fixation of CO2. As long as calcium exists in a crystalline form other than calcium carbonate, it can be used as a preferred calcium-containing composition of the present invention without any problems. Examples of crystalline forms other than calcium carbonate include calcium oxide, calcium sulfate, calcium hydroxide, calcium silicate, calcium chloride, calcium aluminate, etc. Whether calcium is crystalline or amorphous can be determined by X-ray diffraction. The presence or absence and amount of crystalline calcium oxide can also be determined by JCAS I-01-1997 Quantitative Method for Free Calcium Oxide.
[0027] The type of water to be mixed with the calcium-containing composition is not particularly limited. Tap water or industrial water can be used, but water containing components other than water, such as rainwater, seawater, wastewater from surrounding equipment or facilities, or cooling water, can also be used. In addition, it is preferable that the water used contains ammonia. The inclusion of ammonia can further promote the progress of carbonation. The concentration of ammonia is not particularly limited, but since a sufficient effect can be expected with a concentration of 10% by mass, the concentration is, for example, 1% by mass or more and 10% by mass or less.
[0028] The amount of water mixed into the calcium-containing composition is preferably 10 parts by mass or more, more preferably 10 to 30 parts by mass, per 100 parts by mass of the calcium-containing composition in a dry state. The higher the water content, the more the CO2 fixation reaction is promoted, but if the water content is too high, the time and energy required for drying will increase. In addition, since there is no significant change in the amount of CO2 fixation at a water content exceeding 30 parts by mass, it is preferable to set the upper limit at 30 parts by mass for practical purposes.
[0029] The calcium-containing composition and water are preferably mixed before the calcium-containing composition and water are supplied to a reactor for a carbonation reaction in which CO2 is fixed in the calcium-containing composition by contacting the calcium-containing mixture with a gas containing CO2. Known techniques and devices can be used for the mixing method, and examples of the mixing method include a method of mixing by spraying water during the transportation process of the calcium-containing composition, and a method of separately supplying the calcium-containing composition and water into a mixer, mixing them in advance, and supplying them to the reactor.
[0030] Next, the mixture of the calcium-containing composition and water is contacted with a gas containing CO2. The CO2 concentration of the gas containing CO2 is not particularly limited, but in order to efficiently carry out the carbonation reaction, it is preferable that the amount of CO2 supplied is greater than the amount of CO2 that the calcium-containing composition can fix. For example, when carrying out the carbonation reaction in a continuous manner, if a calcium-containing composition containing 1 mass% of crystalline calcium oxide is supplied to a reaction apparatus at 100 kg / h, calcium oxide capable of fixing CO2 is supplied at 100 kg / h x 1 mass% = 1 kg / h. It is known that the carbonation reaction of calcium oxide proceeds according to the above formulas (1) and (2), and here, 1 kg of calcium oxide (molar mass: 56.1 kg / kmol) is 0.018 kmol according to the following formula (3). According to the above equations (1) and (2), the amount of CO2 that reacts with 0.018 kmol of CaO is the same, 0.018 kmol. If we assume that CO2 is at standard conditions, the volume of 1 kmol of gas at standard conditions is 22.4 Nm 3 Therefore, according to the following formula (4), CO2 is 0.4 Nm 3 This is the required calculation.
[0031] Formula (3) 1kg / h÷56.1kg / kmol=0.018kmol / h Equation (4) 22.4Nm 3 / kmol×0.018kmol / h=0.4Nm 3 / h
[0032] Therefore, when a calcium-containing composition containing 1% by mass of crystalline calcium oxide is fed into a reactor at a rate of 100 kg / h, the calcium oxide content is 0.4 Nm 3 It is preferable that the CO2 concentration in the gas containing CO2 is 1% by volume, and the CO2 concentration is 100 times that of the gas containing CO2, that is, 40 Nm 3 / h or more, if the CO2 concentration is 10 volume %, the 3 / h or more of gas may be supplied to the reactor.
[0033] In addition, it is preferable that drying is carried out simultaneously with the reaction to fix CO2 in the reactor. In general, a gas with a high temperature is suitable for drying. As a gas containing CO2 and having a temperature higher than room temperature, for example, gas extracted from a thermal power generation plant, a manufacturing process of cement clinker or chemical products, a waste incineration process, etc. can be suitably used. While it is preferable that the temperature of the gas containing CO2 is higher than room temperature, if it is too high, it will be a problem. This is because water needs to be present in the carbonation reaction with the calcium-containing composition, but if the temperature is too high, the calcium-containing composition will dry before the carbonation reaction occurs, and sufficient reaction time cannot be ensured. Therefore, it is preferable to adjust the gas temperature to be preferably 20 to 300°C, more preferably 60 to 300°C, and even more preferably 100 to 200°C and supply it to the reactor. If the temperature of the gas containing CO2 is too low, it can be heated to a suitable temperature, but it is meaningless if the amount of CO2 generated at that time becomes greater than the amount of CO2 that can be fixed. Therefore, if fossil fuels are used, it is necessary to adjust the amount of CO2 generated so that it does not exceed the amount of CO2 that can be fixed. This does not apply when renewable energy or natural energy is used.
[0034] The time required for the reaction can be appropriately set depending on the amount of the mixture of the calcium-containing composition and water supplied to the reaction apparatus, the amount of the gas containing CO2, the temperature, the CO2 concentration, etc.
[0035] The relative humidity of the CO2-containing gas is, for example, 90% or less and greater than 0%, preferably 60% or less and greater than 0%.
[0036] The CO2 concentration in the CO2-containing gas is preferably 1 vol% or more and 100 vol% or less, more preferably 10 vol% or more and 100 vol% or less, and most preferably 20 vol% or more and 100 vol% or less.
[0037] The reactor may be a known device capable of supplying powder and gas and contacting them. Suitable examples include a fluidized bed reactor and a rotary dryer. Fluidized beds are used for drying and incinerating powder, such as fluidized bed dryers and fluidized bed incinerators. The following will explain in detail with reference to FIG. 1, but the embodiments that can be implemented in the present invention are not limited to this.
[0038] (a) shows a storage facility for storing the calcium-containing composition. The calcium-containing composition extracted downward from (a) is transported and supplied to (d) a fluidized bed reactor by (b) a constant volume supply device. During the transportation process, a predetermined amount of water is mixed with the calcium-containing composition by (c) a water injection device. Then, the mixture of the calcium-containing composition and water is supplied to (d) a fluidized bed reactor. Note that the solid arrows indicate the flow of the calcium-containing composition and / or water.
[0039] Gas containing CO2 is supplied from the bottom of the fluidized bed reactor (d) through the blower (e). The gas dispersed by the dispersion plate (f) comes into contact with the calcium-containing composition to carry out the CO2 fixation reaction and drying. The exhaust gas is discharged from above, and after the dust is collected by the dust collector (g), it is exhausted by the blower (h). The powder collected by the dust collector (g) can be returned to the storage facility for storing the calcium-containing composition (a) or can be mixed with the CO2 fixation calcium-containing composition, which is the product, for use.
[0040] The amount of CO2 fixed in the CO2 fixing calcium-containing composition obtained as a product is not particularly limited, since it may vary depending on the type and components of the Ca-containing composition used. However, it is meaningless if the amount of CO2 fixed in the CO2 fixing calcium-containing composition is not greater than the amount of CO2 generated due to factors such as the electricity used in the process of the present invention, the electricity generated in the process of using the CO2 fixing Ca-containing composition after production, and the fuel during transportation. Considering these reasons, it is preferable that at least 1 mass% of CO2 is fixed, and more preferably 2 mass% of CO2 is fixed, when the calcium-containing composition after CO2 fixation is taken as 100 mass%. In addition, if the calcium-containing composition contains calcium carbonate at the time point before fixing CO2 by the method of the present invention, the amount of calcium carbonate must be known in advance and considered separately from the amount of fixation according to the present invention. Specifically, it is necessary to subtract the amount of CO2 originally contained in the calcium-containing composition from the amount of CO2 in the finally obtained CO2 fixing calcium-containing composition. The method for measuring the amount of CO2 fixation in the present invention is basically based on using a method using a TG-DTA device. A predetermined amount of CO2 fixed calcium-containing composition is charged in a TG-DTA apparatus, and the temperature is raised from room temperature to 1000°C at a rate of 10°C / min in a nitrogen atmosphere. The mass loss rate in the range of 550°C to 700°C on the obtained TG curve is the amount of CO2 fixed. Other methods include, for example, a method using a coulometer, a method using a TOC meter, a method using a CHN meter, and a method of quantifying calcium carbonate using the X-ray diffraction / Rietveld method. When using these methods, the amount of CO2 fixed is determined by fully reflecting the correlation with the method using the TG-DTA apparatus.
[0041] The moisture content of the CO2 fixing calcium-containing composition (composition after CO2 fixation) is 5% by mass or less when the total amount is 100% by mass. If it exceeds 5% by mass, it becomes difficult to handle it in the same way as a normal dry powder. Furthermore, the moisture content of the CO2 fixing calcium-containing composition is preferably 1% by mass or less. If it is 1% by mass or less, when it is mixed with Portland cement or mixed cement and used, there is no problem that the cement reacts with water and the cement reacts before use. In addition, when it is used as a concrete admixture, there is no problem that the quality of the concrete is affected or the mix design is difficult. In addition, as a material that can be mixed with cement or concrete, for example, there is fly ash for concrete specified in JIS A 6201. Fly ash for concrete is specified to have a moisture content (moisture) of 1% by mass or less.
[0042] The CO2 fixing calcium-containing composition thus produced can be used as it is or after mixing with other materials. Examples of usage include mixing with cement, mixing with cement-based materials such as cement-based solidification materials and mortar, mixing with concrete, etc. EXAMPLES
[0043] Examples and comparative examples are shown below, but the technical scope of the present invention is not limited to these.
[0044] Ash obtained by co-firing coal and biomass fuel (hereinafter, biomass ash) was used as the calcium-containing composition. Table 1 shows the components of the biomass ash measured by X-ray fluorescence analysis, and Table 2 shows the form of calcium measured by X-ray diffraction / Rietveld method. The biomass ash contains 11.1 mass% calcium as CaO, 4.0 mass% crystalline calcium oxide that contributes to carbonation, and 0.5 mass% calcium sulfate in oxide equivalent. The contents shown in Tables 1 and 2 are values in oxide equivalent. The moisture content of the obtained CO2-fixing calcium-containing composition was calculated from the mass reduction rate when 10 g of the recovered CO2-fixing calcium-containing composition was placed on a stainless steel tray and dried in a dryer at 100 °C for 24 hours.
[0045] The amount of CO2 originally contained in the biomass ash used as the calcium-containing composition and the amount of CO2 fixed in the CO2-fixing calcium-containing composition recovered after a predetermined reaction time were measured by a method using a TG-DTA device. A predetermined amount of sample was charged into the TG-DTA device, and the temperature was raised from room temperature to 1000°C at a heating rate of 10°C / min in a nitrogen atmosphere. The mass reduction rate in the range of 550°C to 700°C on the TG curve obtained at that time was determined to be due to decarbonation of calcium carbonate, and was defined as the amount of CO2 fixed in this example. The amount of CO2 fixed in the CO2-fixing calcium-containing composition was obtained by subtracting the amount of CO2 originally contained in the biomass ash used as the Ca-containing composition. The amount of CO2 originally contained in the biomass ash used as the Ca-containing composition was 1.5% by mass.
[0046] [Table 1]
[0047] [Table 2]
[0048] Then, using the device shown in FIG. 2, CO2 fixation to biomass ash was carried out. This device simulates a fluidized bed reactor. A cylindrical container (i) with an inner diameter of 40 mm was covered with mesh on the top and bottom, and a mixture of biomass ash and water was charged inside. Under all conditions, 50 g of dry biomass ash was fixed, and 10 to 40 parts by mass of water was mixed in advance with respect to 100 parts by mass of the biomass ash. In addition, a case was also carried out in which ammonia water was added to water instead of water to make 10% by mass ammonia water, and the mixture amount of 10% by mass ammonia water was 20 parts by mass. Then, gas containing CO2 was supplied from a hole at the bottom and ventilated into the cylindrical container while contacting it with the biomass ash, and a carbonation reaction operation was performed and a drying operation of the CO2 fixed calcium-containing composition was performed at the same time. The structure is such that exhaust gas is released from a hole at the top. In the figure, (j) is a heater for CO2 gas, and (k) is a thermometer for measuring the gas temperature.
[0049] Commercially available carbon dioxide gas was used as the gas containing CO2. The experiment was carried out under two conditions of CO2 concentration: 100% by volume and 20% by volume. To adjust the CO2 concentration to 20% by volume, it was mixed with commercially available N2 gas to adjust the concentration.
[0050] The gas temperature supplied to the reactor was set at three different conditions: 20° C., 60° C., and 100° C. In order to maintain each temperature, the temperature was adjusted by heating using a gas heater before being supplied to the cylindrical vessel.
[0051] The flow rate of the gas containing CO2 was adjusted to 10 L / min at a given temperature standard, regardless of the CO2 concentration.
[0052] Tables 3, 4, and 5 show the conditions and results. Note that (1) to (7) in the tables correspond to the following items. (1) Amount of water mixed (parts by mass) per 100 parts by mass of calcium-containing composition (2) CO2 concentration (volume percent) of gas containing CO2 (3) Temperature of the gas containing CO2 (℃) (4) Reaction time (min) (5) The amount of CO2 fixed by the recovered CO2-fixing calcium-containing composition (the value obtained by subtracting the amount of CO2 originally contained in the calcium-containing composition) (6) The ratio of the amount of CO2 fixed (mass%) to the maximum amount of CO2 fixed (mass%) when water is not mixed into the calcium-containing composition (hereinafter referred to as the standard ratio). (7) Moisture content (mass%) of the recovered CO2 fixing calcium-containing composition
[0053] [Table 3]
[0054] All the examples shown in Table 3 are examples in which the CO2 concentration of the CO2-containing gas is 100% by volume and the temperature of the CO2-containing gas is 20°C. The main data in Table 3 are shown again in Figure 3. The horizontal axis is the amount of water mixed into the calcium-containing composition, and the vertical axis is the reaction time. The data is a pair of the amount of CO2 fixed and the moisture content of the CO2-fixed calcium-containing composition. It is preferable that the reaction time is short, the amount of CO2 fixed is high, and the moisture content is low. It can be seen from Figure 3 that the amount of water mixed is preferably 10 parts by mass or more and 30 parts by mass or less.
[0055] Comparative Examples 1 to 4 show examples in which water was not mixed into the calcium-containing composition. The amount of CO2 fixed did not change after 20 minutes of reaction time, and was a maximum of 1.2 mass%. The reference ratio shown in (6) in the table below shows the value when the maximum amount of CO2 fixed in the case where water was not mixed into the calcium-containing composition was set to 1.2 mass.
[0056] Comparative Examples 5 to 7 and Examples 1 to 2 show examples in which 10 parts by mass of water was mixed with 100 parts by mass of the calcium-containing composition. It was found that by mixing water to 10 parts by mass, the amount of CO2 fixed increased to a maximum of 1.7% by mass, or 1.4 in terms of the reference ratio. On the other hand, the moisture content of the recovered CO2 fixing calcium-containing composition exceeded 5% by mass under the conditions of a reaction time of up to 30 minutes shown in Comparative Examples 5 to 7, which was not a preferable state. In Example 1, where the reaction time was 60 minutes, the moisture content was 4.2% by mass, which was a preferable state. However, in Example 2, the moisture content was 0.4% by mass, and it was found that a more suitable CO2 fixing calcium-containing composition was obtained.
[0057] Comparative Examples 8 to 11 and Examples 3 to 4 show examples in which 20 parts by mass of water was mixed with 100 parts by mass of the calcium-containing composition. By mixing water to 20 parts by mass, the amount of CO2 fixed further increased to a maximum of 2.1% by mass, or 1.8 in terms of the reference ratio. On the other hand, the moisture content of the recovered CO2 fixing calcium-containing composition exceeded 5% by mass under the conditions of up to 60 minutes of reaction time shown in Comparative Examples 8 to 11, which was not a preferable state. In Example 3, in which the reaction time was 90 minutes, the moisture content was 3.3% by mass, which was a preferable state. In Example 4, the moisture content was 0.8% by mass, and it was found that a more suitable CO2 fixing calcium-containing composition was obtained.
[0058] Comparative Examples 12 to 16 and Examples 5 to 6 show examples in which water was mixed to 30 parts by mass per 100 parts by mass of the calcium-containing composition. By mixing water to 30 parts by mass, the amount of CO2 fixed further increased to a maximum of 3.1% by mass, or 2.6 in terms of the reference ratio. On the other hand, the moisture content of the recovered CO2 fixing calcium-containing composition exceeded 5% by mass under the conditions of up to a reaction time of 90 minutes shown in Comparative Examples 12 to 16, which was not a preferable state. In Example 5, in which the reaction time was 120 minutes, the moisture content was 2.9% by mass, which was a preferable state. However, in Example 6, the moisture content was 0.2% by mass, and it was found that a more suitable CO2 fixing calcium-containing composition was obtained.
[0059] Comparative Examples 17 to 22 and Examples 7 to 8 show examples in which 40 parts by mass of water was mixed with 100 parts by mass of the calcium-containing composition. When 40 parts by mass of water was mixed, there was no significant difference in the amount of CO2 fixed compared to the case of 30 parts by mass. The moisture content of the recovered CO2 fixing calcium-containing composition exceeded 5% by mass under the conditions up to 120 minutes shown in Comparative Examples 17 to 22, which is not in a preferable state. In Example 7, where the reaction time was 180 minutes, the moisture content was 3.0% by mass, which is in a preferable state, and in Example 8, the moisture content was 0.9% by mass, and it was found that a CO2 fixing calcium-containing composition that can be used more preferably was obtained.
[0060] It was found that the conditions of Comparative Examples 17 to 22 and Examples 7 to 8 were almost equivalent in terms of the quality of the moisture content of the recovered CO2 fixing calcium-containing composition, but took a long time to dry, compared with the conditions of Comparative Examples 12 to 16 and Examples 5 to 6. Therefore, taking into consideration the amount of water required in the process and the energy required for drying, it was found that under the conditions of the present examples, it is not preferable to mix water in an amount greater than 30 parts by mass per 100 parts by mass of the calcium-containing composition.
[0061] [Table 4]
[0062] All of the examples shown in Table 4 are examples in which the amount of water mixed per 100 parts by mass of the calcium-containing composition is 20 parts by mass, and the CO2 concentration of the CO2-containing gas is 20% by volume. The main data in Table 4 are shown again in Figure 4. The horizontal axis is the reaction temperature, and the vertical axis is the reaction time. The data are pairs of the amount of CO2 fixed and the moisture content of the CO2-fixed calcium-containing composition. It is preferable that the reaction time is short, the amount of CO2 fixed is high, and the moisture content is low. It can be seen from Figure 4 that the reaction temperature is preferably 60°C or higher, and more preferably 100°C or higher.
[0063] Comparative Examples 23 to 26 and Examples 9 to 10 are examples in which the CO2 concentration of the CO2-containing gas was reduced to 20% by volume under the conditions of Comparative Examples 8 to 11 and Examples 3 to 4. The amount of CO2 fixed was almost the same as in Comparative Examples 8 to 11 and Examples 3 to 4. Also, the time required to reduce the water content of the recovered CO2-fixed calcium-containing composition to 5% by mass or less was the same, 90 minutes. In other words, it was found that the CO2 fixation reaction does not pose a problem even if the CO2 concentration is low, as long as a sufficient amount of CO2 required for the reaction with the calcium-containing composition is supplied.
[0064] In Comparative Example 27 and Examples 11 to 12, the temperature of the CO2-containing gas was 60°C. The amount of CO2 fixed was almost the same as in Comparative Examples 23 to 26 and Examples 9 to 10, in which the temperature was 20°C. The moisture content of the recovered CO2-fixing calcium-containing composition decreased to 4.4% by mass in 20 minutes and to 0.9% by mass in 30 minutes, demonstrating that a CO2-fixing calcium-containing composition that can be suitably used can be obtained in a shorter time.
[0065] In Examples 13 and 14, the temperature of the CO2-containing gas was 100°C. The amount of CO2 fixed was almost the same as that in Comparative Example 27 and Examples 11 and 12, in which the temperature was 60°C. The moisture content of the recovered CO2-fixing calcium-containing composition decreased to 4.0% by mass in 10 minutes and to 1.0% by mass in 20 minutes, indicating that a CO2-fixing calcium-containing composition that can be suitably used can be obtained in an even shorter time.
[0066] [Table 5]
[0067] All of the examples shown in Table 5 are examples in which 10 mass% 10 mass% ammonia water was 20 mass parts per 100 mass parts of the calcium-containing composition, the CO2 concentration of the CO2-containing gas was 20 volume%, and the temperature was 20°C.
[0068] Comparative Examples 28 to 31 and Examples 15 to 16 are examples in which water was replaced with ammonia water compared to the conditions of Comparative Examples 23 to 26 and Examples 9 to 10. The amount of CO2 fixed increased to a maximum of 3.5 mass% and a reference ratio of 1.9 compared to Comparative Examples 23 to 26 and Examples 9 to 10. In addition, the time required for the water content of the recovered CO2 fixing calcium-containing composition to reach 5 mass% or less was the same, 90 minutes. In other words, it was found that the addition of ammonia water promotes the fixation reaction of CO2.
[0069] Example 2 In the fluidized bed reactor (d) in Figure 1, CO2 absorption is fast and a dry CO2-fixed calcium-containing composition can be obtained with a small amount of thermal energy. This is because the calcium-containing composition comes into uniform contact with the CO2-containing gas due to the fluidized bed. However, the fluidized bed reactor (d) is not suitable for small-scale plants. An example of a reactor suitable for small-scale plants is shown in Figure 5.
[0070] Agitator blades (n) are arranged in a closed housing (k) and rotated by a motor (m). A calcium-containing composition such as incineration ash is introduced from an ash inlet (p), and water is introduced from a water inlet (r). A CO2-containing gas is introduced from a gas inlet (s), and CO2 is supplied to the calcium-containing composition from an exhaust gas outlet, and the exhaust gas that has received water vapor is discharged. Then, the product CO2-fixed calcium-containing composition is discharged from an outlet (u). The device of FIG. 5 has a lower CO2 absorption efficiency and a lower thermal efficiency than the device of FIG. 1. However, the device of FIG. 5 is smaller in scale and has lower equipment costs than the device of FIG. 1. The embodiment of FIG. 5 is the same as the embodiments of FIG. 1 to FIG. 4, except for the points specifically noted. [Explanation of symbols]
[0071] (a) Storage facilities for calcium-containing compositions (b) Metering device (c) Water injection device (d) Fluidized Bed Reactor (e) Blower (f) Dispersion plate (g) Dust collector (h) Air blower (k) Housing (m) Motor (n) Stirring blade (p) Ash inlet (r) Water inlet (s) CO2-containing gas inlet (t) Exhaust gas outlet (u) Product outlet
Claims
1. The calcium-containing composition and water are mixed together, and CO 2 By contacting the gas containing CO 2 A method for producing a calcium-containing composition having an immobilized calcium salt, comprising the steps of: A calcium-containing composition, liquid water, and a CO 2 CO with a concentration of 1% by volume or more and 100% by volume or less 2 A gas containing the gas is supplied. Supplied CO 2 The calcium-containing composition and the water are flowed by the contained gas, or the calcium-containing composition and the water are stirred, so that CO is introduced into the calcium-containing composition. 2 and drying the calcium-containing composition at the same time. CO with a moisture content of 5% by mass or less 2 The present invention is characterized in that an immobilized calcium-containing composition is produced, CO 2 A method for producing an immobilized calcium-containing composition.
2. 2. The CO2 extract of claim 1, wherein the calcium-containing composition is at least one member of the group consisting of ash, slag, and sludge. 2 A method for producing an immobilized calcium-containing composition.
3. The CO composition according to claim 1, characterized in that the amount of water mixed is 10 parts by mass or more per 100 parts by mass of the calcium-containing composition in a dry state. 2 A method for producing an immobilized calcium-containing composition.
4. The CO composition according to claim 3, characterized in that the amount of water mixed is 10 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the calcium-containing composition in a dry state. 2 A method for producing an immobilized calcium-containing composition.
5. CO 2 2. The method according to claim 1, wherein the temperature of the gas containing CO is 60° C. or higher. 2 A method for producing an immobilized calcium-containing composition.
6. CO 2 6. The method according to claim 5, wherein the temperature of the gas containing CO is 100° C. or higher. 2 A method for producing an immobilized calcium-containing composition.
7. CO with a moisture content of 1% by mass or less 2 The method for producing an immobilized calcium-containing composition according to any one of claims 1 to 6, 2 A method for producing an immobilized calcium-containing composition.
8. 8. The CO process according to claim 7, wherein the reactor is a fluidized bed reactor. 2 A method for producing an immobilized calcium-containing composition.
9. CO 2 2. The method according to claim 1, wherein the gas containing CO is a gas extracted from a cement clinker production facility. 2 A method for producing an immobilized calcium-containing composition.
10. CO 2 2. The method according to claim 1, wherein the gas containing CO is gas extracted from a thermal power plant. 2 A method for producing an immobilized calcium-containing composition.
11. Produced CO 2 The CO2 extract according to claim 1, characterized in that the immobilized calcium-containing composition is mixed into cement to a concentration of 5 mass% or less. 2 A method for producing an immobilized calcium-containing composition.
12. Produced CO 2 The CO2 composition according to claim 1, characterized in that the fixed calcium-containing composition is used as a concrete admixture. 2 A method for producing an immobilized calcium-containing composition.
13. 2. The CO gas according to claim 1, wherein the liquid water is mixed with ammonia. 2 A method for producing an immobilized calcium-containing composition.
14. The calcium-containing composition and water are mixed together, and CO 2 By contacting the gas containing CO 2 A manufacturing apparatus for manufacturing a calcium-containing composition having an immobilized calcium salt, comprising: a storage facility for storing the calcium-containing composition; a metering device for supplying the calcium-containing composition to the fluidized bed reactor; a water injection device for mixing water with the calcium-containing composition before it is fed to the fluidized bed reactor; a fluidized bed reactor for carrying out a carbonation reaction of the calcium-containing composition; CO 2 a blower for supplying a gas containing the compound to a fluidized bed reactor; A dust collector for collecting dust contained in the exhaust gas; A CO 2 An apparatus for producing an immobilized calcium-containing composition.
Citation Information
Patent Citations
Concrete, and manufacturing method thereof
JP2020037493A
Manufacturing method of construction material