Composition for forming carbon dioxide absorption gel, carbon dioxide absorption gel, carbon dioxide absorber, and carbon dioxide absorption device
A carbon dioxide-absorbing gel is formed using a copolymer and room-temperature molten salt with specific monomers, addressing leakage and stability issues, resulting in a stable and efficient carbon dioxide absorber.
Patent Information
- Application Number
- JP2024043450
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-15
AI Technical Summary
Existing carbon dioxide absorbent gels using ionic liquids face issues such as leakage and poor storage stability due to high ionic liquid concentrations and rapid reaction times, leading to inconsistent film formation and thickness.
A carbon dioxide-absorbing gel-forming composition comprising a copolymer with (meth)acrylic acid esters and (meth)acrylamide monomers, crosslinked with a room-temperature molten salt, where the monomers have specific chemical formula weights and ratios, forming a stable gel structure that retains the molten salt without leakage.
The composition allows for the formation of a carbon dioxide-absorbing gel with excellent storage stability and high carbon dioxide absorption performance, preventing ionic liquid leakage and maintaining effective absorption capabilities over time.
Smart Images

Figure 2024146817000001 
Figure 2024146817000002 
Figure 2024146817000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon dioxide absorbing gel-forming composition, a carbon dioxide absorbing gel, a carbon dioxide absorbent containing the gel, and a carbon dioxide absorbing device containing the carbon dioxide absorbent. [Background technology]
[0002] In recent years, climate change due to global warming has become a problem. Carbon dioxide is said to be the greenhouse gas that has the greatest impact on global warming, and research into technologies for capturing carbon dioxide is being actively conducted.
[0003] As a technology for capturing carbon dioxide, ionic liquids (also known as room temperature molten salts) are attracting attention due to their excellent carbon dioxide absorption capacity.
[0004] For example, Patent Document 1 proposes a gas separation gel membrane obtained by heating and drying a mixture of an ionic liquid and an aqueous solution of polyvinyl alcohol. Although a gel membrane can be obtained from the mixture by a simple operation, there is a problem that the ionic liquid leaks from the formed gel membrane when the concentration of the ionic liquid in the gel membrane is high.
[0005] In addition, Patent Document 2 proposes a gel composition obtained by drying and dehydrating a hydrogel obtained by crosslinking two compounds having different functional groups at the ends with an amide bond, and immersing the dehydrated product obtained in an ionic liquid. However, since the reaction starts immediately when the two compounds are mixed, the reaction proceeds too much before and during coating or molding of the mixture of the two compounds, resulting in thickening and gelling, which may cause problems such as failure to form a film of the desired area, variation in film thickness, and failure to form a desired molded product. In addition, there is a process of drying and dehydrating the hydrogel to form a dehydrated product and a process of immersing the dehydrated product in an ionic liquid, and it is not easy to obtain an ionic liquid gel. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 5877961
[0007] [Patent Document 2] JP 2013-60504 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a composition for forming a carbon dioxide absorbent gel that can form a carbon dioxide absorbent gel without leakage of ionic liquid by a simple procedure and has excellent storage stability. [Means for solving the problem]
[0009] The present inventors conducted extensive research to solve the above problems and arrived at the present invention. That is, the present invention is as follows. [1] A carbon dioxide-absorbing gel-forming composition comprising: a copolymer (A) having, as essential constituent monomers, a (meth)acrylic acid ester (a1) having a glycidyl group and a chemical formula weight of 500 or less; and a (meth)acrylamide-based monomer (a2) having a chemical formula weight of 500 or less; and an room-temperature molten salt (B) composed of an anion and an organic cation, wherein the (meth)acrylamide-based monomer (a2) is at least one amide selected from the group consisting of (meth)acrylamide, N-substituted (meth)acrylamide, and N,N-disubstituted (meth)acrylamide. [2] The carbon dioxide absorbing gel forming composition according to [1], wherein the organic cation is a cation represented by general formula (1).
[0010] [ka]
[0011] [In general formula (1), R 1 and R 3 each independently represents an alkyl group having 1 to 6 carbon atoms; R 2 , R 4 and R 5 represents a hydrogen atom. [3] The carbon dioxide-absorbing gel-forming composition according to [1] or [2], wherein the (meth)acrylic acid ester (a1) is one or more selected from the group consisting of glycidyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate glycidyl ether, and the (meth)acrylamide monomer (a2) is one or more selected from the group consisting of N,N-dimethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and N-benzyl(meth)acrylamide. [4] The carbon dioxide-absorbing gel-forming composition according to any one of [1] to [3], wherein a polymerization ratio of the (meth)acrylic acid ester (a1) is 5 to 30% by weight based on the total weight of the (meth)acrylic acid ester (a1) and the (meth)acrylamide-based monomer (a2). [5] The carbon dioxide-absorbing gel-forming composition according to any one of [1] to [4], wherein the weight of the room-temperature molten salt (B) is 80% by weight or more and 95% by weight or less based on the total weight of the copolymer (A) and the room-temperature molten salt (B). [6] A carbon dioxide absorbing gel obtained by reacting the carbon dioxide absorbing gel-forming composition according to any one of [1] to [5]. [7] A carbon dioxide absorbent comprising the carbon dioxide absorbing gel described in [6]. [8] [7] A carbon dioxide absorbing device comprising the carbon dioxide absorbent described in [7]. Effect of the Invention
[0012] According to the present invention, a carbon dioxide absorbent gel free from leakage of ionic liquid can be formed by a simple procedure, and a carbon dioxide absorbent gel-forming composition having excellent storage stability can be provided. Therefore, a carbon dioxide absorber and a carbon dioxide absorbing device having excellent carbon dioxide absorption performance can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Carbon dioxide absorbing gel-forming composition (hereinafter referred to as "gel-forming composition")] The gel-forming composition of the present invention is a gel-forming composition comprising a copolymer (A) having as essential constituent monomers a (meth)acrylic acid ester (a1) having a glycidyl group and a chemical formula weight of 500 or less, and a (meth)acrylamide-based monomer (a2) having a chemical formula weight of 500 or less, and an anion and an organic cation and a room-temperature molten salt (B), the (meth)acrylamide-based monomer (a2) being at least one amide selected from the group consisting of (meth)acrylamide, N-substituted (meth)acrylamide, and N,N-disubstituted (meth)acrylamide. Here, the (meth)acrylic acid ester means a methacrylic acid ester and / or an acrylic acid ester, and the (meth)acrylamide means a methacrylamide and / or an acrylamide. The room-temperature molten salt means an organic salt formed from an anion and a cation, and has a melting point of 100° C. or less, and is also called an ionic liquid.
[0014] The gel-forming composition of the present invention comprises a copolymer (A) of a (meth)acrylic acid ester (a1) having a glycidyl group and a chemical formula weight of 500 or less and a (meth)acrylamide monomer (a2) having a chemical formula weight of 500 or less, and a room-temperature molten salt (B) composed of an anion and an organic cation. The gel-forming composition of the present invention forms a gel by crosslinking the glycidyl groups of the copolymer (A) with each other when heated, and retaining the room-temperature molten salt (B) inside the three-dimensional network structure generated by the crosslinking reaction between the copolymers (A). In the gel obtained by reacting the gel-forming composition of the present invention, the amide groups of the copolymer (A) and the room-temperature molten salt (B) attract each other due to Coulomb force, so that the room-temperature molten salt (B) can be efficiently supported within the gel, and the room-temperature molten salt (B) does not easily seep out, so that a carbon dioxide absorber that can be used for a long period of time can be obtained.
[0015] <(Meth)acrylic acid ester (a1)> The (meth)acrylic acid ester (a1) is a (meth)acrylic acid ester having a glycidyl group and a chemical formula weight of 500 or less. The (meth)acrylic acid ester having a glycidyl group may be a compound having one or more acryloyl groups and one or more glycidyl groups in one molecule, and may be a compound having one each of an acryloyl group and a glycidyl group, or may be a compound having two or more acryloyl groups and two or more glycidyl groups. For example, it may be a diacrylate having two acryloyl groups or a diglycidyl ether having two glycidyl groups, and is not particularly limited.
[0016] Examples of the (meth)acrylic acid ester (a1) having a glycidyl group include glycidyl (meth)acrylate {chemical formula weight: 128 (142)}, glycidyloxyalkyl (meth)acrylate [2-hydroxyethyl (meth)acrylate glycidyl ether {chemical formula weight: 172 (186)}, 3-hydroxypropyl (meth)acrylate glycidyl ether {chemical formula weight: 186 (200)}, 2-hydroxypropyl (meth)acrylate glycidyl ether {chemical formula weight: 186 (200)}, 4-hydroxybutyl (meth)acrylate glycidyl ether {chemical formula weight: 200 (214)}, and 2-hydroxybutyl (meth)acrylate glycidyl ether {chemical formula weight: 200 (214)}. , 5-hydroxypentyl (meth)acrylate glycidyl ether {chemical formula weight: 214 (228)}, 6-hydroxyhexyl (meth)acrylate glycidyl ether {chemical formula weight: 228 (242)}, 3-hydroxy-3-methylbutyl (meth)acrylate glycidyl ether {chemical formula weight: 214 (228)}, etc.], 2-hydroxy-3-phenoxypropyl (meth)acrylate glycidyl ether {chemical formula weight: 278 (292)}, pentaerythritol tri(meth)acrylate glycidyl ether {chemical formula weight: 354 (398)}, (meth)acrylic acid esters represented by the following general formula (2), and (meth)acrylic acid esters represented by the following general formula (3), etc. are included. The chemical formula weights of the acrylate and methacrylate are listed next to the compound name, and the chemical formula weight of the methacrylate is listed in parentheses.
[0017] CH2=CR 6 -C(O)O-(R 7 O) n -X 1 (2)
[0018] In the general formula (2), R 6 is H or CH3, R 6 As the radical, H is preferable.
[0019] X 1 represents a glycidyl group.
[0020] R 7 is an alkylene group having 2 to 3 carbon atoms, preferably an ethylene group (CHCH) or a 1,2-propylene group [CH(CH)CH or CHCH(CH)], n is an integer of 1 or more, R 7 If there are two or more in a molecule, R 7 may all be the same or different.
[0021] Since the (meth)acrylic acid ester represented by the general formula (2) has a chemical formula weight of 500 or less, R 7 are all ethylene groups, the upper limit of n is 8, and R 7 When all of R are 1,2-propylene groups, the upper limit of n is 6. 7 When the alkyl group contains both an ethylene group and a methylethylene group, the number of ethylene groups is 3 to 7 and the number of 1,2-propylene groups is 1 to 5, and n, which is the sum of the ethylene groups and the 1,2-propylene groups, is 8 or less.
[0022] R 7 is an ethylene group, R 7 The group represented by O is a group obtained by ring-opening addition of ethylene oxide [hereinafter also referred to as an ethyleneoxy group], and R 7 is a 1,2-propylene group, R 7 The group represented by O is a group obtained by ring-opening addition of propylene oxide (hereinafter also referred to as a propyleneoxy group). R 7 When R contains an ethylene group and a 1,2-propylene group, 7 There is no limitation on the mode of bonding between the ethyleneoxy group and the propyleneoxy group represented by O, and they may be bonded regularly (block bonds, alternating bonds, etc.) or randomly, and random bonding is preferred.
[0023] The (meth)acrylic acid ester represented by the general formula (2) is preferably a (meth)acrylic acid ester having one or two ethyleneoxy groups and / or one or two propyleneoxy groups, and (R 7(Meth)acrylic esters having only ethyleneoxy groups as O) and n being 1 or 2 are more preferred.
[0024] CH2=CR 8 -C(O)O-(R 9 O) n -[R 10 O] m -X 2 (3)
[0025] In the general formula (3), R 8 is H or CH3, R 8 As the radical, H is preferable.
[0026] X 2 represents a glycidyl group.
[0027] R 9 is an ethylene group. n is an integer of 1 or more and 3 or less. n is preferably 1 or 2.
[0028] R 10 is a butylene group. m is an integer of 1 or more and 3 or less. m is preferably 1 or 2.
[0029] Examples of the (meth)acrylic acid ester represented by the general formula (2) include glycidyl ether diethylene glycol (meth)acrylate {chemical formula weight: 216, (230)}, glycidyl ether triethylene glycol (meth)acrylate {chemical formula weight: 260, (274)}, glycidyl ether dipropylene glycol (meth)acrylate {chemical formula weight: 244, (258)}, and glycidyl ether tripropylene glycol (meth)acrylate {chemical formula weight: 302, (316)}. The chemical formula weights of the acrylate and methacrylate are listed in succession following the compound name, and the chemical formula weight of the methacrylate is listed in parentheses.
[0030] Examples of the (meth)acrylic acid ester represented by the general formula (3) include glycidyl ether butylene glycol ethylene glycol ether (meth)acrylate {chemical formula weight: 244, (258)}, glycidyl ether dibutylene glycol ethylene glycol ether (meth)acrylate {chemical formula weight: 316, (330)}, and glycidyl ether butylene glycol diethylene glycol ether (meth)acrylate {chemical formula weight: 288, (302)}. The chemical formula weights of the acrylate and methacrylate are listed in succession following the compound name, and the chemical formula weight of the methacrylate is listed in parentheses.
[0031] The chemical formula weight of the (meth)acrylic acid ester (a1) is preferably from 128 to 500, more preferably from 128 to 400, from the viewpoint of suppressing the exudation of the room-temperature molten salt (B) from the gel.
[0032] From the viewpoint of suppressing the exudation of the room temperature molten salt (B) from the gel, the (meth)acrylic acid ester (a1) may be, for example, glycidyl (meth)acrylate, {chemical formula weight: 128 (142)}, 2-hydroxyethyl (meth)acrylate glycidyl ether {chemical formula weight: 172 (186)}, 3-hydroxypropyl (meth)acrylate glycidyl ether {chemical formula weight: 186 (200)}, 2-hydroxypropyl (meth)acrylate glycidyl ether, Preferred are glycidyl (meth)acrylate {chemical formula weight: 186 (200)}, 4-hydroxybutyl (meth)acrylate glycidyl ether {chemical formula weight: 200 (214)}, 2-hydroxybutyl (meth)acrylate glycidyl ether {chemical formula weight: 200 (214)}, and the compounds represented by general formula (2), and more preferred are glycidyl (meth)acrylate {chemical formula weight: 128 (142)} and 4-hydroxybutyl (meth)acrylate glycidyl ether. As the (meth)acrylic acid ester (a1), one type may be used alone, or two or more types may be used in combination.
[0033] <(Meth)acrylamide monomer (a2)> The (meth)acrylamide monomer (a2) is a (meth)acrylamide having a chemical formula weight of 500 or less.
[0034] The (meth)acrylamide monomer (a2) includes at least one (meth)acrylamide selected from the group consisting of (meth)acrylamide, N-substituted (meth)acrylamide, and N,N-disubstituted (meth)acrylamide.
[0035] Examples of N-substituted (meth)acrylamides include compounds represented by the following general formula (4).
[0036] CH2=CR 11 -C(O)-NH(R 12 ) (4)
[0037] In general formula (4), R 11 is H or CH3, R 12 represents an alkyl group having 1 to 28 carbon atoms, an aryl group having 6 to 28 carbon atoms, or an arylalkyl group having 6 to 28 carbon atoms.
[0038] R 12 Examples of the alkyl group having 1 to 28 carbon atoms represented by the formula (1) include a methyl group, an ethyl group, a linear alkyl group having 3 to 28 carbon atoms, and a branched alkyl group having 3 to 28 carbon atoms, and examples of the linear alkyl group include a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the branched alkyl group include an isopropyl group, a sec-butyl group, a isobutyl group, a tert-butyl group, a isopentyl group, a tert-pentyl group, and a 2,2-dimethylpropyl ... a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the branched alkyl group having 3 to 6 carbon atoms are preferred from the viewpoint of suppressing the exudation of the room-temperature molten salt (B) from the gel, and a methyl group, an ethyl group, and an isopropyl group are more preferred.
[0039] R 12Examples of the aryl group having 6 to 28 carbon atoms represented by the formula include a phenyl group, a group in which at least one of the five hydrogen atoms of a phenyl group is replaced with a monovalent atom or monovalent atomic group other than a hydrogen atom (hereinafter referred to as a substituted phenyl group), a hydrocarbon group having two or more phenyl groups (excluding a phenyl group and a substituted phenyl group), and a condensed polycyclic aromatic hydrocarbon group. Examples of the substituted phenyl group include a methylphenyl group and a dimethylphenyl group, and examples of the hydrocarbon group having two or more phenyl groups include a biphenyl group and a triphenylmethyl group. Examples of the condensed polycyclic aromatic hydrocarbon group include a naphthyl group and a phenanthrene group. Among these, a phenyl group and a substituted phenyl group having 6 to 12 carbon atoms are preferred from the viewpoint of suppressing the exudation of the room temperature molten salt (B) from the gel, and a phenyl group and a methylphenyl group are more preferred. R 12 Examples of the arylalkyl group having 6 to 28 carbon atoms represented by the following formula include a benzyl group.
[0040] Examples of compounds that can be represented by general formula (4) include N-methyl(meth)acrylamide {chemical formula weight: 85, (99)}, N-ethyl(meth)acrylamide {chemical formula weight: 99, (113)}, N-isopropyl(meth)acrylamide {chemical formula weight: 113, (127)}, and N-benzyl(meth)acrylamide {chemical formula weight: 161, (175)}. The chemical formula weights of the acrylate and methacrylate are listed in succession following the compound name, with the chemical formula weight of the methacrylate listed in parentheses.
[0041] Examples of N,N-disubstituted (meth)acrylamides include compounds represented by the following general formula (5).
[0042] CH2=CR 13 -C(O)-NR 14 (R 15 ) (5)
[0043] In general formula (5), R 13 is H or CH3, R 14 and R 15is an alkyl group having 1 to 28 carbon atoms, an aryl group having 6 to 28 carbon atoms, or an arylalkyl group having 6 to 28 carbon atoms, R 14 The number of carbon atoms and R 15 The total number of carbon atoms is 2 to 28.
[0044] R 14 and R 15 Examples of the alkyl group having 1 to 28 carbon atoms represented by the formula (1) include a methyl group, an ethyl group, a linear alkyl group having 3 to 28 carbon atoms, and a branched alkyl group having 3 to 28 carbon atoms, etc. Examples of the linear alkyl group include a propyl group, a butyl group, a pentyl group, and a hexyl group, etc. Examples of the branched alkyl group include an isopropyl group, a sec-butyl group, a isobutyl group, a tert-butyl group, a isopentyl group, a tert-pentyl group, and a 2,2-dimethylpropyl group, etc. Among them, from the viewpoint of suppressing the exudation of the room-temperature molten salt (B) from the gel, a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and a branched alkyl group having 3 to 6 carbon atoms, etc. are preferred, and a methyl group, an ethyl group, and an isopropyl group, etc. are more preferred.
[0045] R 14 and R 15 Examples of the aryl group having 6 to 28 carbon atoms represented by the formula (I) include a phenyl group, a substituted phenyl group, a hydrocarbon group having two or more phenyl groups (excluding a phenyl group and a substituted phenyl group), and a condensed polycyclic aromatic hydrocarbon group. Examples of the substituted phenyl group include a methylphenyl group and a dimethylphenyl group. Examples of the hydrocarbon group having two or more phenyl groups include a biphenyl group and a triphenylmethyl group. Examples of the condensed polycyclic aromatic hydrocarbon group include a naphthyl group and a phenanthrene group. Among these, a phenyl group and a substituted phenyl group having 6 to 12 carbon atoms are preferred from the viewpoint of suppressing the exudation of the room-temperature molten salt (B) from the gel, and a phenyl group and a methylphenyl group are more preferred. 14 and R 15 Examples of the arylalkyl group having 6 to 28 carbon atoms represented by the following formula include a benzyl group.
[0046] Examples of compounds that can be represented by general formula (5) include N,N-dimethyl(meth)acrylamide {chemical formula weight: 99, (113)} and N,N-diethyl(meth)acrylamide {chemical formula weight: 127, (141)}. The chemical formula weights of the acrylate and methacrylate are listed in succession following the compound name, with the chemical formula weight of the methacrylate listed in parentheses.
[0047] The chemical formula weight of the (meth)acrylamide monomer (a2) is preferably from 71 to 500, more preferably from 71 to 400, from the viewpoint of suppressing the exudation of the room-temperature molten salt (B) from the gel.
[0048] As the (meth)acrylamide monomer (a2) having a chemical formula weight of 500 or less, from the viewpoint of suppressing the leaching of the room-temperature molten salt (B) from the gel, (meth)acrylamide {chemical formula weight: 71, (85)}, N-isopropyl(meth)acrylamide {chemical formula weight: 113, (127)}, N-benzyl(meth)acrylamide {chemical formula weight: 161, (175)} and N,N-dimethyl(meth)acrylamide {chemical formula weight: 99, (113)} are preferred, and N,N-dimethyl(meth)acrylamide {chemical formula weight: 99, (113)}, N-isopropyl(meth)acrylamide {chemical formula weight: 113, (127)} and N-benzyl(meth)acrylamide {chemical formula weight: 161, (175)} are more preferred. As the (meth)acrylamide monomer (a2), one type may be used alone, or two or more types may be used in combination.
[0049] <Copolymer (A)> Copolymer (A) contains, as essential constituent monomers, a (meth)acrylic acid ester (a1) having a glycidyl group and a chemical formula weight of 500 or less, and a (meth)acrylamide monomer (a2) having a chemical formula weight of 500 or less. There is no limitation on the order of bonding of the monomers constituting copolymer (A), and it may be a block polymer or a random polymer.
[0050] The copolymer (A) may contain at least one type of (meth)acrylic acid ester (a1) and at least one type of (meth)acrylamide-based monomer (a2) as monomers, and two or more types of each of the (meth)acrylic acid ester (a1) and the (meth)acrylamide-based monomer (a2) may be used.
[0051] The copolymer (A) may contain another compound (a3) as a monomer. Preferred examples of the other compound (a3) include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate.
[0052] In the copolymer (A) of the present invention, the polymerization ratio of the (meth)acrylic acid ester (a1) based on the total weight of the (meth)acrylic acid ester (a1) and the (meth)acrylamide monomer (a2) is preferably 5 to 30% by weight, and more preferably 15 to 20% by weight, from the viewpoint of suppressing the exudation of the room-temperature molten salt (B) from the gel.
[0053] The polymerization ratio of the (meth)acrylamide-based monomer (a2) based on the total weight of the (meth)acrylic acid ester (a1) and the (meth)acrylamide-based monomer (a2) is preferably 70 to 95% by weight, and more preferably 80 to 85% by weight, from the viewpoint of suppressing the exudation of the room-temperature molten salt (B) from the gel.
[0054] When the other compound (a3) is contained, the weight proportion of the other compound (a3) is preferably 0.1 to 10% by weight based on the total weight of the (meth)acrylic acid ester (a1), the (meth)acrylamide-based monomer (a2) and the other compound (a3).
[0055] Examples of the copolymer (A) include poly(N,N-dimethyl(meth)acrylamide-co-glycidyl(meth)acrylate), poly(N-isopropyl(meth)acrylamide-co-glycidyl(meth)acrylate), poly((meth)acrylamide-co-glycidyl(meth)acrylate), poly(N,N-dimethyl(meth)acrylamide-co-4-hydroxybutyl(meth)acrylate glycidyl ether), poly(N-isopropyl(meth)acrylamide-co-4-hydroxybutyl(meth)acrylate glycidyl ether), and poly((meth)acrylamide-co-4-hydroxybutyl(meth)acrylate glycidyl ether). From the viewpoint of suppressing the exudation of the room temperature molten salt (B) from the gel, the copolymer (A) is preferably poly(N,N-dimethyl(meth)acrylamide-co-glycidyl(meth)acrylate), poly(N-isopropyl(meth)acrylamide-co-glycidyl(meth)acrylate), poly((meth)acrylamide-co-glycidyl(meth)acrylate), poly(N-benzyl(meth)acrylamide-co-glycidyl(meth)acrylate), poly(N-benzyl(meth)acrylamide-co-4-hydroxybutyl(meth)acrylate), and poly(N,N-dimethylacrylamide-co-glycidyl methacrylate), poly(N-isopropylmethacrylamide-co-glycidyl methacrylate), poly(N-benzylacrylamide-co-glycidyl methacrylate), and poly(N,N-dimethylacrylamide-co-4-hydroxybutyl acrylate glycidyl ether).
[0056] When the copolymer (A) is poly(N,N-dimethylacrylamide-co-glycidyl methacrylate), the weight proportion of glycidyl methacrylate, which is the (meth)acrylic acid ester (a1), is preferably 5 to 30% by weight based on the total weight of N,N-dimethylacrylamide and glycidyl methacrylate.
[0057] The weight average molecular weight of the copolymer (A) of the present invention is preferably 50,000 to 5,000,000, and more preferably 100,000 to 2,000,000, from the viewpoint of suppressing the exudation of the room temperature molten salt (B) from the gel. The weight average molecular weight of the copolymer (A) can be measured by gel permeation chromatography (GPC) under the following conditions, and Mw was determined by GPC under the following measurement conditions in the examples.
[0058] <Measurement conditions for weight average molecular weight (Mw) of copolymer (A)> Equipment: "HLC-8320" [Tosoh Corporation] Column: "TSK GEL α-M" [manufactured by Tosoh Corporation] Measurement temperature: 40℃ Sample solution: 0.25% by weight N,N-dimethylformamide solution (insoluble matter was filtered off using a glass filter) Solution injection volume: 100μl Detector: Refractive index detector Reference material: 12 standard polystyrenes (TSKstandard POLYSTYRENE) (molecular weight: 500, 1,050, 2,800, 5,970, 9,100, 18,100, 37,900, 96,400, 190,000, 355,000, 1,090,000, 2,890,000) [manufactured by Tosoh Corporation]
[0059] The copolymer (A) can be produced by a known method, and a solution polymerization method is preferred.
[0060] An example of the solution polymerization method is a method in which a monomer composition (a monomer composition containing a (meth)acrylic acid ester (a1), a (meth)acrylamide monomer (a2), and other compounds (a3) used as necessary) and a polymerization initiator (azobisisobutyronitrile, 2,2'azobis(2-methylbutyronitrile, etc.) are dropped into a solvent such as ethyl acetate to polymerize. The polymerization temperature is preferably 60 to 230°C, more preferably 70 to 180°C, from the viewpoint of protecting the glycidyl group.
[0061] <Room temperature molten salt (B)> The gel-forming composition of the present invention contains an ambient-temperature molten salt (B). The room-temperature molten salt (B) comprises an anion and an organic cation.
[0062] The organic cation is preferably a cation represented by the general formula (1).
[0063] [ka]
[0064] In general formula (1), R 1 and R 3 each independently represents an alkyl group having 1 to 6 carbon atoms; R 2 , R 4 and R 5 each represents a hydrogen atom.
[0065] R 1 and R 3 Examples of the alkyl group having 1 to 6 carbon atoms represented by the formula (1) include a linear alkyl group having 1 to 6 carbon atoms and a branched alkyl group having 3 to 6 carbon atoms, and examples of the linear alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the branched alkyl group include an isopropyl group, a sec-butyl group, an isobutyl group, a tert-butyl group, an isopentyl group, a tert-pentyl group, and a 2,2-dimethylpropyl group. Among these, a methyl group, an ethyl group, and a branched alkyl group having 3 to 4 carbon atoms are preferred from the viewpoint of the amount of carbon dioxide absorption, and a methyl group and an ethyl group are more preferred.
[0066] Examples of the cation include 1-methyl-3-imidazolium cation, 1-ethylimidazolium cation, 1-propylimidazolium cation, 1-butylimidazolium cation, 1,3-dimethyl-imidazolium cation, 1,3-diethyl-imidazolium cation, 1-ethyl-3-methylimidazolium cation, 1-propyl-3-methylimidazolium cation, 1-butyl-3-methylimidazolium cation, and 1-hexyl-3-methylimidazolium cation. From the viewpoint of the amount of carbon dioxide absorption, the cation is preferably a 1-ethyl-3-methylimidazolium cation, a 1,3-dimethyl-imidazolium cation, a 1,3-diethyl-imidazolium cation, or a 1-butyl-3-methylimidazolium cation, and more preferably a 1-ethyl-3-methylimidazolium cation.
[0067] There are no particular limitations on the anion, so long as it can form a room-temperature molten salt in combination with an organic cation.
[0068] The anion is PF6 - , BF4 - , BF3(CF3) - , F - , Cl - , Br - , I - , AlCl4 - , Al2Cl7 - , NO3 - , (NC)2N - , (FSO2)2N - , (CF3SO2)2N - , (CF3CF2SO2)2N - , (CF3SO2)3C - , CH3COO - , CH3CH2COO - , (CH3)3CCOO - , (CH3O)CH2COO - , CF3COO - , CF3CF2CF2COO - , CF3SO3 - , CF3(CF2)3SO3 -, AsF6 - , and SbF6 - etc.
[0069] The anion is preferably BF4 from the viewpoint of carbon dioxide absorption. - , (NC)2N - , (FSO2)2N - , (CF3SO2)2N - , (CF3CF2SO2)2N - , (CF3SO2)3C - , CH3COO - , CH3CH2COO - , (CH3)3CCOO - , and (CH3O)CH2COO - and more preferably BF4 - [Tetrafluoroborate], (FSO2)2N - [Bis(fluorosulfonyl)imide], (NC)2N - [Dicyanamide] and CH3CH2COO - [Propionate].
[0070] As the room-temperature molten salt (B), from the viewpoint of the amount of carbon dioxide absorption, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium dicyanamide and 1-ethyl-3-methylimidazolium propionate are preferred. The composition for absorbing acidic gas of the present invention may contain two or more kinds of room-temperature molten salts (B).
[0071] The room-temperature molten salt (B) can be produced by a known method, for example, the alkyl halide method, the dialkyl carbonate method, the direct alkylation method, or the like.
[0072] <Other ingredients (C)> The gel-forming composition of the present invention may contain components other than the copolymer (A) and the room-temperature molten salt (B) [hereinafter, other components (C)]. Examples of other components (C) include crosslinking agents, thickeners, crosslinking reaction catalysts, and solvents. The crosslinking agent referred to here is a polyfunctional compound that reacts with two or more glycidyl groups.
[0073] Examples of the crosslinking agent include ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, oxalic acid, succinic acid, adipic acid, azelaic acid, and dodecanedioic acid. From the viewpoint of suppressing the exudation of the room-temperature molten salt (B) from the gel, preferred crosslinking agents are ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, and pentaethylenehexamine, and more preferred is pentaethylenehexamine.
[0074] Thickening agents include polyvinyl alcohol, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, xanthan gum, and the like.
[0075] Crosslinking reaction catalysts include salicylic acid, glycolic acid, and 1,8-diazabicyclo[5.4.0]-7-undecene.
[0076] Examples of the solvent include ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, etc. From the viewpoint of the solubility of the gel-forming composition in the solvent, preferred solvents are ethyl acetate, methanol, ethanol, 1-propanol, 2-propanol, and 1-butanol, and more preferred solvents are ethyl acetate, 2-propanol, and methanol.
[0077] In the gel forming composition of the present invention, the weight of the room-temperature molten salt (B) is preferably 80% by weight or more and 95% by weight or less based on the total weight of the copolymer (A) and the room-temperature molten salt (B). In the gel-forming composition of the present invention, the weight of the copolymer (A) is preferably 1% by weight or more and 20% by weight or less based on the total weight of the copolymer (A), the room-temperature molten salt (B) and the other component (C). In the gel-forming composition of the present invention, the weight of the other component (C) is preferably 90% by weight or less based on the total weight of the copolymer (A), the room-temperature molten salt (B) and the other component (C).
[0078] The gel-forming composition of the present invention can be produced by mixing the copolymer (A), the room-temperature molten salt (B) and other components (C) at room temperature (preferably 10 to 40°C) using a stirrer such as a magnetic stirrer until a homogeneous liquid is formed.
[0079] [Carbon dioxide absorbing gel] The carbon dioxide absorbing gel of the present invention is a gel obtained by heating and reacting the carbon dioxide absorbing gel-forming composition, and is a complex having as its constituent components an ambient temperature molten salt (B) and a crosslinked polymer (D) obtained by heating a reaction between glycidyl groups possessed by the copolymer (A) contained in the gel-forming composition, or between a glycidyl group and a crosslinking agent. The method for heating the gel-forming composition may be a known method, and examples thereof include a method of heating the composition at a temperature of 60°C to 200°C for 1 minute to 3 hours using a known heating device (such as a hot air circulation type heating oven, a dryer, and a hot plate). From the viewpoint of operational simplicity, a method of applying the gel-forming composition to a desired thickness on an arbitrary substrate and then heating the composition using a hot air circulation type heating oven, a hot plate, or the like is preferred, and heating at a temperature of 80°C to 150°C for 3 minutes to 2 hours is preferred. From the viewpoint of heating time and film strength of the gel, the preferred film thickness to be applied to the substrate is 1 μm to 20 μm. A gel can also be produced by pouring the gel-forming composition into a mold of a desired shape and heating the composition. The fact that a gel has been produced can be determined by visually and tactilely confirming that no room-temperature molten salt (B) has oozed from the reaction product after heating, thereby judging that the carbon dioxide absorbing gel of the present invention has been obtained.
[0080] In the production of the gel of the present invention, the reaction of the gel-forming composition is preferably completed when the reaction rate of the glycidyl groups in the copolymer (A) is 70% to 100%. If the reaction rate is 70% or more, the room-temperature molten salt (B) is less likely to bleed out of the gel, which is preferable. The reaction rate of the glycidyl group can be calculated by measuring the FT-IR spectrum of the gel. -1 The peak intensity PIg appearing near 1625 cm decreases as the crosslinking reaction proceeds. -1 The intensity PIa of the peak derived from the glycidyl group does not change. Therefore, by comparing the ratio of the peak intensity derived from the amide group to the peak intensity derived from the glycidyl group before and after the crosslinking reaction, it is possible to calculate the extent to which the reaction has progressed. Specifically, 914 cm -1 The ratio of the peak intensity PIg1 of the glycidyl group to the peak intensity PIa1 of the amide group when the peak intensity of the glycidyl group that appears near the crosslinking reaction stops changing is defined as the peak intensity ratio R1 at a reaction rate of 100%. The ratio (PIg0 / PIa0) of the peak intensity PIg0 of the glycidyl group to the peak intensity PIa0 of the amide group before the crosslinking reaction is defined as the peak intensity ratio R0 at a reaction rate of 0%. The ratio (PIg / PIa) of the peak intensity PIg derived from the glycidyl group to the peak intensity PIa derived from the amide group, obtained by FT-IR spectrum measurement of the formed gel, is defined as Rx. The reaction rate can be calculated by applying each of the peak intensity ratios to the formula: 100 × (peak intensity ratio R0 at 0% reaction rate − peak intensity ratio Rx of the formed gel) / (peak intensity ratio R0 at 0% reaction rate − peak intensity ratio R1 at 100% reaction rate).
[0081] When the gel-forming composition used to produce the gel contains a solvent, it is preferable to remove the solvent by, for example, vaporizing the solvent by heating. When removing the solvent by heating, the removal may be performed during heating to form the gel, or by further heating the formed gel. The gel of the present invention may be obtained by cooling the gel after heating the gel-forming composition or heating for removing the solvent to room temperature by, for example, leaving it at room temperature.
[0082] In the gel of the present invention, the weight of the room-temperature molten salt (B) is preferably 80% by weight or more and 95% by weight or less with respect to the total weight of the gel. The weight of the room-temperature molten salt (B) with respect to the total weight of the gel can be measured by immersing the gel in a solvent (e.g., methanol) in which the room-temperature molten salt (B) dissolves at an arbitrary ratio, extracting the room-temperature molten salt (B) from the gel into the solvent, drying the extraction residue that did not dissolve in the solvent, and subtracting the dry weight of the extraction residue from the weight of the gel.
[0083] The gel of the present invention preferably has an initial (immediately after preparation) carbon dioxide absorption amount per gram of gel at 25° C. and under a carbon dioxide pressure of 100 kPa of 1.0 kPa / g or more, and more preferably 2.0 kPa / g or more. If the initial carbon dioxide absorption amount per gram of gel at 25° C. and under a carbon dioxide pressure of 100 kPa is 2.0 kPa / g or more, it can be determined that the gel has sufficient carbon dioxide absorption performance.
[0084] The amount of carbon dioxide absorbed can be measured, for example, by the following method. (1) Place 30 g of the gel-forming composition in a SUS container equipped with a needle valve, then place a lid capable of sealing the SUS container on the SUS container, and measure the total weight (the total weight of the SUS container, the lid, and the gel-forming composition in the SUS container). (2) The lid is removed from the SUS container, and the container is left open while being kept at 80°C for 60 minutes, and then heated at 150°C for 60 minutes to react with the gel-forming composition and form a gel. After a total of 120 minutes of heating, the container is cooled to room temperature, and the total weight of the gel and the SUS container contained in the container is measured. If the gel-forming composition contains a solvent, the heating operation at 80°C for 60 minutes and at 150°C for 60 minutes is repeated until all of the solvent contained therein has evaporated. The amount of solvent evaporated can be confirmed by calculating the difference between the total weight measured in (1) and the total weight measured after 120 minutes of heating. (3) Place the lid back on the SUS container containing the gel obtained in (2) to seal the container and adjust the temperature to 25°C. Insert the pressure sensor into the center of the lid and attach it with screws so that the pressure sensor is exposed inside the SUS container. Connect the tip of the needle valve to an oil rotary vacuum pump, open the valve to evacuate the air inside the SUS container, then close the valve and remove the oil rotary vacuum pump. Next, connect a gas collection balloon filled with carbon dioxide to the needle valve, open the valve to let carbon dioxide into the SUS container. Next, close the needle valve and immediately measure the initial pressure inside the SUS container. (4) With the pressure sensor still attached, leave the container stationary for 60 minutes after the initial pressure measurement, then read the pressure inside the container again. After that, read the pressure inside the container every 60 minutes, repeating this process until the pressure change in 60 minutes is 1 kPa or less, and record the final value as the final pressure. (5) The difference between the initial pressure and the final pressure is calculated as the amount of carbon dioxide absorbed by the gel. The greater this pressure difference, the greater the amount of carbon dioxide absorbed by the gel.
[0085] The gel of the present invention is capable of desorbing carbon dioxide from the gel under a heated environment, a reduced pressure environment, an environment in which a gas other than carbon dioxide is supplied, and the like.
[0086] The amount of carbon dioxide desorption can be measured by measuring the amount of carbon dioxide absorbed by the gel after desorbing carbon dioxide from the gel using the method for measuring the amount of carbon dioxide absorption described above, and calculating the difference from the initial amount of carbon dioxide absorbed (immediately after the gel was prepared). The smaller the difference from the initial amount of carbon dioxide absorbed (immediately after the gel was prepared), the greater the amount of carbon dioxide desorption.
[0087] Since the gel does not deteriorate due to absorption and desorption of carbon dioxide, it is possible to repeat the absorption and desorption of carbon dioxide many times.
[0088] [Carbon dioxide absorbent containing gel] The carbon dioxide absorbent of the present invention comprises the carbon dioxide absorbing gel.
[0089] The carbon dioxide absorber of the present invention is not particularly limited in shape, and can be formed into a sheet, particle, block, or other suitable shape that is easy to use, and may form an aggregate by combining several carbon dioxide absorbers.
[0090] [Carbon dioxide absorption device including a carbon dioxide absorber] The carbon dioxide absorbing device of the present invention is a device including the carbon dioxide absorbent.
[0091] The carbon dioxide absorption device of the present invention is not particularly limited as long as it contains the carbon dioxide absorbent and is a device used for absorbing and separating carbon dioxide, and includes devices installed at carbon dioxide generation sources such as gas fields, oil fields, factories and power plants, and devices installed in incineration facilities, etc. EXAMPLES
[0092] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples as long as they do not deviate from the gist of the present invention. In addition, unless otherwise specified, parts mean parts by weight.
[0093] <Production Example 1: Production of Copolymer (A-1)> A reaction vessel equipped with a thermometer, stirrer, reflux condenser, and nitrogen inlet was charged with 140 parts of ethyl acetate, and the air in the reaction vessel was replaced with nitrogen gas while stirring, and then the mixture was heated to reflux. Next, a mixture of 89.3 parts of N,N-dimethylacrylamide, 15.7 parts of glycidyl methacrylate, 112 parts of ethyl acetate, and 0.1 parts of 2,2'azobis(2-methylbutyronitrile) was added dropwise over a period of 3 hours to polymerize. The reaction was continued for another 2 hours while heating to reflux. The solvent was then removed under reduced pressure, and poly(N,N-dimethylacrylamide-co-glycidyl methacrylate) (weight average molecular weight: about 1 million) was obtained.
[0094] <Production Example 2: Production of Copolymer (A-2)> A reaction vessel equipped with a thermometer, stirrer, reflux condenser, and nitrogen inlet was charged with 140 parts of ethyl acetate, and the air in the reaction vessel was replaced with nitrogen gas while stirring, and then the mixture was heated to reflux. Next, a mixture of 84 parts of N,N-dimethylacrylamide, 21 parts of glycidyl methacrylate, 112 parts of ethyl acetate, and 0.1 parts of 2,2'azobis(2-methylbutyronitrile) was added dropwise over a period of 3 hours to polymerize. The reaction was continued for another 2 hours while heating to reflux. The solvent was then removed under reduced pressure to obtain poly(N,N-dimethylacrylamide-co-glycidyl methacrylate) (weight average molecular weight: about 1 million).
[0095] <Production Example 3: Production of Copolymer (A-3)> A reaction vessel equipped with a thermometer, stirrer, reflux condenser, and nitrogen inlet was charged with 140 parts of ethyl acetate, and the air in the reaction vessel was replaced with nitrogen gas while stirring, and then the mixture was heated to reflux. Next, a mixture of 95 parts of N,N-dimethylacrylamide, 10 parts of glycidyl methacrylate, 112 parts of ethyl acetate, and 0.1 parts of 2,2'azobis(2-methylbutyronitrile) was added dropwise over a period of 3 hours to polymerize. The reaction was continued for another 2 hours while heating to reflux. The solvent was then removed under reduced pressure to obtain poly(N,N-dimethylacrylamide-co-glycidyl methacrylate) (weight average molecular weight: approximately 1 million).
[0096] <Production Example 4: Production of Copolymer (A-4)> A reaction vessel equipped with a thermometer, stirrer, reflux condenser, and nitrogen inlet was charged with 140 parts of ethyl acetate, and the air in the reaction vessel was replaced with nitrogen gas while stirring, and then heated to reflux. Next, a mixture of 89.3 parts of N-isopropyl methacrylamide, 15.7 parts of glycidyl methacrylate, 112 parts of ethyl acetate, and 0.1 parts of 2,2'azobis(2-methylbutyronitrile) was added dropwise over 3 hours to polymerize. The reaction was continued for another 2 hours while heating to reflux. The solvent was then removed under reduced pressure, and poly(N-isopropyl methacrylamide-co-glycidyl methacrylate) (weight average molecular weight: about 1 million) was obtained.
[0097] <Production Example 5: Production of Copolymer (A-5)> A reaction vessel equipped with a thermometer, stirrer, reflux condenser, and nitrogen inlet was charged with 140 parts of ethyl acetate, and the air in the reaction vessel was replaced with nitrogen gas while stirring, and then heated to reflux. Next, a mixture of 89.3 parts of N-benzyl acrylamide, 15.7 parts of glycidyl methacrylate, 112 parts of ethyl acetate, and 0.1 parts of 2,2'azobis(2-methylbutyronitrile) was added dropwise over 3 hours to polymerize. The reaction was continued for another 2 hours while heating to reflux. The solvent was then removed under reduced pressure to obtain poly(N-benzyl acrylamide-co-glycidyl methacrylate) (weight average molecular weight: about 1 million).
[0098] <Production Example 6 Production of Copolymer (A-6)> A reaction vessel equipped with a thermometer, stirrer, reflux condenser, and nitrogen inlet was charged with 140 parts of ethyl acetate, and the air in the reaction vessel was replaced with nitrogen gas while stirring, and then the mixture was heated to reflux. Next, a mixture of 84 parts of N,N-dimethylacrylamide, 21 parts of 4-hydroxybutyl acrylate glycidyl ether, 112 parts of ethyl acetate, and 0.1 parts of 2,2'azobis(2-methylbutyronitrile) was added dropwise over a period of 3 hours to polymerize. The reaction was continued for another 2 hours while heating to reflux. The solvent was then removed under reduced pressure to obtain poly(N,N-dimethylacrylamide-co-4-hydroxybutyl acrylate glycidyl ether) (weight average molecular weight: about 1 million).
[0099] <Production Example 7 Production of Room Temperature Molten Salt (B-4)> A mixture of 18 parts by weight of glyoxal (40% by weight aqueous solution) and 10 parts by weight of formalin (37% by weight aqueous solution) was charged into a reaction flask equipped with a stirrer, a thermometer, a dropping funnel, a reflux condenser, and a nitrogen gas inlet tube, and the mixture was stirred to form a homogeneous solution, and heated to 40° C. while flowing a small amount of nitrogen gas. After that, a mixture of 64 parts by weight of ethylamine (70% by weight aqueous solution) and 61 parts by weight of ammonia (28% by weight aqueous solution) was dropped from the dropping funnel while maintaining the reaction temperature at 35 to 45° C. Next, 35 minutes after the start of the dropwise addition of the mixed solution of ethylamine and ammonia, a mixed solution of 127 parts by weight of glyoxal (40% by weight aqueous solution) and 71 parts by weight of formalin (37% by weight aqueous solution) was dropped from another dropping funnel over 4 hours. The mixed solution of ethylamine and ammonia was dropped over 4 hours and 35 minutes, and the drop start time was shifted so that the drop of the mixed solution of glyoxal and formalin was completed at the same time as the drop of the mixed solution of ethylamine and ammonia was completed. After the dropwise addition was completed, the reaction was continued for another hour at 40°C. Next, the pressure was gradually reduced from normal pressure to a reduced pressure of 5.3 kPa at a temperature of 80°C, and dehydration was performed to obtain crude 1-ethylimidazole. Subsequently, the mixture was purified by simple distillation at a temperature of 100°C and a reduced pressure of 0.7 kPa to obtain 1-ethylimidazole. Next, 96 parts by weight of the obtained 1-ethylimidazole, 135 parts by weight of dimethyl carbonate, and 192 parts by weight of methanol were charged into a stainless steel autoclave equipped with a reflux condenser and dissolved uniformly. The temperature was then raised to 150°C. The reaction was carried out at a pressure of about 0.8 MPa for 70 hours to obtain a reaction product. 1 H-NMR analysis revealed that 1-ethyl-3-methylimidazolium monomethyl carbonate was produced. 423 parts by weight of the resulting reaction product (salt purity 44% by weight) was placed in a flask, and 74 parts by weight of propionic acid was gradually added dropwise at room temperature over about 30 minutes while stirring. Carbon dioxide bubbles were generated during the dropwise addition. After the dropwise addition was completed and the generation of bubbles subsided, the reaction liquid was transferred to a rotary evaporator and the entire amount of the solvent was distilled off. 184 parts by weight of a colorless, transparent liquid was obtained in the flask. This liquid 1 H-NMR analysis revealed that the compound was 1-ethyl-3-methylimidazolium propionate.
[0100] <Examples 1 to 12 and Comparative Examples 1 to 2: Production and Evaluation of Gel-Forming Compositions and Gels> (Production of gel-forming composition) At room temperature, the copolymer (A), room temperature molten salt (B) and other components (C) shown in Tables 1 and 2 were placed in a 200 mL glass container in the ratios shown in Table 1, and stirred using a magnetic stirrer until a homogeneous liquid was formed, and gel-forming compositions according to Examples 1 to 12 and Comparative Examples 1 and 2 were obtained. Using a portion of the gel-forming composition of each example, a storage stability evaluation test was performed by the following method. For the remaining gel-forming compositions, a carbon dioxide absorbing gel was prepared by the method described below and an evaluation test was performed. The results are shown in Tables 1 and 2.
[0101] (Evaluation of storage stability of gel-forming composition) After preparing each gel-forming composition, the composition was allowed to stand at 25° C. for 3 weeks, and then the presence or absence of gelation in the composition was confirmed by the following method. (1) Immediately after preparation, 30 g of the gel-forming composition was placed in a 50 mL glass container, which was then sealed and allowed to stand at 25° C. in an incubator for 3 weeks. (2) After being left to stand, the gel-forming composition was visually observed every day from the next day onwards for the presence or absence of gelation, and evaluated according to the following evaluation criteria. ○: No gelation ×: gelation occurred
[0102] (Production of carbon dioxide absorbing gel and evaluation of leakage of room temperature molten salt from the gel) (1) After leaving 30 g of each gel-forming composition at room temperature for 12 hours, 1 g of the composition was applied to a 100 μm-thick PET (polyethylene terephthalate) film [Cosmoshine A4300, manufactured by Toyobo Co., Ltd.] using an applicator so that the film thickness was 100 μm, and the film was heated at 80° C. for 60 minutes, then heated at 150° C. for another 60 minutes, and cooled to room temperature to obtain a carbon dioxide absorbing gel. The gel had a thickness of 20 μm. (2) A 2 cm square PTFE (polytetrafluoroethylene) plate was placed on top of the gel coating. A load of 4080 g was applied to the top of the plate, compressing the gel with a pressure of 100 kPa for 5 minutes. (3) After compression, the presence or absence of leakage of the room-temperature molten salt from the gel was visually observed and evaluated according to the following criteria. 〇: No leakage ×: Leakage
[0103] (Calculation of the amount of carbon dioxide absorbed by gel under a carbon dioxide pressure of 100 kPa) (1) Each gel-forming composition was left to stand at room temperature for 12 hours. After that, 30 g of the gel-forming composition was weighed out and placed in a 40 mL SUS container equipped with a needle valve, and the total weight of the SUS container and the gel-forming composition contained therein (hereinafter referred to as the weight before heating) was measured. (2) The SUS container was heated at 80° C. for 60 minutes in an open state, and then heated at 150° C. for another 60 minutes to react the gel-forming composition. After that, it was cooled to room temperature, and the total weight of the SUS container and its contents (hereinafter referred to as the weight after heating) was measured. (3) The operation of (2) was repeated until the difference between the weight before heating measured in (1) and the weight after heating measured in (2) became equal to the amount of the solvent contained in the gel-forming composition (24 g), thereby obtaining a carbon dioxide absorbing gel. (4) A lid was placed on the SUS container containing the gel obtained in (3) to seal the SUS container, and the temperature was adjusted to 25°C. A pressure sensor (Kyowa Electric, PHL-A-5MP-B) was inserted into the center of the lid, and the pressure sensor was attached by fixing it with screws so that it was exposed inside the SUS container. An oil rotary vacuum pump was connected to the tip of the needle valve, the valve was opened to evacuate the air inside the SUS container, the valve was closed and the oil rotary vacuum pump was removed, and then a gas collection balloon filled with carbon dioxide was connected to the tip of the needle valve, and the valve was opened to introduce carbon dioxide into the SUS container. Next, the needle valve was closed and the gas collection balloon was removed. (5) The pressure inside the stainless steel container was immediately measured and set as the initial pressure. The initial pressure was 100 kPa. (6) With the pressure sensor still attached to the SUS container, the container was left to stand for 60 minutes after the initial pressure measurement, and the carbon dioxide pressure inside the container was then measured again. After that, the pressure inside the container was read every 60 minutes, and this procedure was repeated until the pressure change within 60 minutes was 1 kPa or less. (7) The difference between the initial pressure of carbon dioxide in the SUS container (100 kPa) and the final pressure in (6) was taken as the amount of carbon dioxide absorbed per 6 g of gel. The calculated amount of carbon dioxide absorbed was divided by the weight of the gel in the SUS container (6 g) to calculate the amount of carbon dioxide absorbed per 1 g of gel. A larger amount of carbon dioxide absorption is preferable.
[0104] [Table 1]
[0105] [Table 2]
[0106] In addition to Production Examples 1 to 7, the following materials were used in the examples and comparative examples. <Room temperature molten salt (B)> Room temperature molten salt (B-1): 1-ethyl-3-methylimidazolium tetrafluoroborate (Tokyo Chemical Industry Co., Ltd.) Room temperature molten salt (B-2): 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide (Kanto Chemical Co., Ltd.) Room temperature molten salt (B-3): 1-ethyl-3-methylimidazolium dicyanamide (Tokyo Chemical Industry Co., Ltd.) <Other ingredients (C)> Crosslinking agent: Pentaethylenehexamine (Tokyo Chemical Industry Co., Ltd.) Additive: Polyvinyl alcohol (Merck) Solvent: ethyl acetate (Tokyo Chemical Industry Co., Ltd.), methanol (Tokyo Chemical Industry Co., Ltd.), 2-propanol (Tokyo Chemical Industry Co., Ltd.), water (ion-exchanged water was used)
[0107] As shown in Tables 1 and 2, the gels according to the Examples did not leak room-temperature molten salt after the compression test, but the gels according to the Comparative Examples did leak. Also, the gels according to the Examples had a higher amount of carbon dioxide absorption by the gels under a carbon dioxide pressure environment of 100 kPa than the gels according to the Comparative Examples. [Industrial Applicability]
[0108] According to the carbon dioxide absorbent gel-forming composition, carbon dioxide absorbent gel, gel-containing carbon dioxide absorber, and carbon dioxide absorbing device of the present invention, a gel that does not leak ionic liquid can be formed by a simple procedure. In addition, according to the present invention, a carbon dioxide absorbent gel-forming composition with high storage stability can be provided. As a result, according to the present invention, a carbon dioxide absorber with excellent carbon dioxide absorption capacity can be efficiently provided. Therefore, the composition, carbon dioxide absorbent gel, and carbon dioxide absorber of the present invention can be suitably used for separation of acid gases such as carbon dioxide contained in exhaust gases from chemical plants and steelworks, production of energy resources (natural gas, biogas, synthetic gas) by carbon dioxide removal, and carbon dioxide removal from distributed emission sources such as automobiles. The applications of the composition, carbon dioxide absorbent gel, and carbon dioxide absorber of the present invention are not limited to the above-mentioned exemplary fields.
Claims
1. A copolymer (A) containing, as essential constituent monomers, a (meth)acrylic acid ester (a1) having a glycidyl group and a chemical formula weight of 500 or less, and a (meth)acrylamide-based monomer (a2) having a chemical formula weight of 500 or less; (B) a room-temperature molten salt composed of an anion and an organic cation; The (meth)acrylamide monomer (a2) is at least one amide selected from the group consisting of (meth)acrylamide, N-substituted (meth)acrylamide, and N,N-disubstituted (meth)acrylamide.
2. 2. The carbon dioxide absorbing gel forming composition according to claim 1, wherein the organic cation is a cation represented by general formula (1). 【Chemistry 1】 [In general formula (1), R 1 and R 3 each independently represents an alkyl group having 1 to 6 carbon atoms; R 2 , R 4 and R 5 represents a hydrogen atom.
3. The carbon dioxide absorbing gel forming composition according to claim 1, wherein the (meth)acrylic acid ester (a1) is one or more selected from the group consisting of glycidyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate glycidyl ether, and the (meth)acrylamide monomer (a2) is one or more selected from the group consisting of N,N-dimethyl(meth)acrylamide, N-isopropyl(meth)acrylamide and N-benzyl(meth)acrylamide.
4. The carbon dioxide absorbing gel forming composition according to claim 1, wherein the polymerization ratio of the (meth)acrylic acid ester (a1) is 5 to 30% by weight based on the total weight of the (meth)acrylic acid ester (a1) and the (meth)acrylamide monomer (a2).
5. 2. The carbon dioxide absorbent gel forming composition according to claim 1, wherein the weight of the room temperature molten salt (B) is 80% by weight or more and 95% by weight or less based on the total weight of the copolymer (A) and the room temperature molten salt (B).
6. A carbon dioxide absorbing gel obtained by reacting the carbon dioxide absorbing gel forming composition according to any one of claims 1 to 5.
7. A carbon dioxide absorbent comprising the carbon dioxide absorbing gel according to claim 6.
8. A carbon dioxide absorbing device comprising the carbon dioxide absorbent according to claim 7.
Citation Information
Patent Citations
V belt type stepless transmission
JP1983077961A
Ionic liquid-containing gelatinous composition, gelatinous thin film, and method for manufacturing the same
JP2013060504A