Positive electrode composite, lithium-ion battery, and manufacturing method of lithium-ion battery

A composite material of plate-shaped and spherical O2 type active materials with a specific ratio improves the capacity of lithium ion batteries by optimizing the orientation and utilization of the plate-shaped material.

JP2024147981AActive Publication Date: 2024-10-17TOYOTA JIDOSHA KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023060793
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

Positive electrode active materials with an O2 type structure have limitations in capacity when used in lithium ion batteries.

Method used

A positive electrode composite material comprising a first active material with an O2 type structure in a plate shape and a second active material with an O2 type structure in a spherical shape, where the major axis to diameter ratio is between 0.1 and 1.5, and the ratio of the first active material to the total is 10% to 90% by mass, is used to form the positive electrode active material layer.

Benefits of technology

The composite material enhances the capacity of lithium ion batteries by increasing the utilization rate of the plate-shaped active material and contributing to the overall capacity through the spherical active material's contribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147981000001_ABST
    Figure 2024147981000001_ABST
Patent Text Reader

Abstract

To provide a positive electrode active material having an O2 type structure capable of improving the capacity when applied to a positive electrode active material layer of a lithium-ion battery.SOLUTION: A disclosed positive electrode composite includes a first active material and a second active material. The first active material has an O2-type structure and has a plate-like shape. The second active material has an O2-type structure and has a spherical shape. The ratio D1L / D2 of the major axis of the first active material D1L to the diameter of the second active material D2 is equal to or more than 0.1 and equal to or less than 1.5. The ratio of the first active material to the total of the first active material and the second active material is 10% by mass or more and 90% by mass or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses a cathode composite, a lithium-ion battery, and a method for making a lithium-ion battery. [Background technology]

[0002] A positive electrode active material having an O2 type structure is known for a lithium ion battery. As disclosed in Patent Document 1, a positive electrode active material having an O2 type structure is obtained by ion-exchanging at least a part of Na in a Na-containing transition metal oxide having a P2 type structure with Li. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-169365 A Summary of the Invention [Problem to be solved by the invention]

[0004] There is room for improvement in the capacity of a positive electrode active material having an O2 type structure when it is applied to a positive electrode active material layer of a lithium ion battery. [Means for solving the problem]

[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> a positive electrode mixture comprising a first active material and a second active material; The first active material has an O2 type structure and is plate-shaped; The second active material has an O2 type structure and is spherical, The major axis D of the first active material 1L and the diameter D2 of the second active material 1L / D2 is 0.1 or more and 1.5 or less, A ratio of the first active material to the total of the first active material and the second active material is 10% by mass or more and 90% by mass or less. Positive electrode mixture. <Aspect 2> 2. The positive electrode mixture of embodiment 1, The surface of the second active material has a plurality of crystallites. Positive electrode mixture. <Aspect 3> 3. The positive electrode mixture of Aspect 1 or 2, Including solid electrolytes, Positive electrode mixture. <Aspect 4> The positive electrode mixture of any one of Aspects 1 to 3, Containing one or both of a conductive assistant and a binder; Positive electrode mixture. <Aspect 5> A lithium ion battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The positive electrode active material layer has a positive electrode mixture according to any one of aspects 1 to 4. Lithium-ion battery. <Aspect 6> 6. The lithium ion battery of embodiment 5, One or both of the electrolyte layer and the negative electrode active material layer contain a solid electrolyte. Lithium-ion battery. <Aspect 7> A method for manufacturing a lithium ion battery, comprising: Obtaining a positive electrode active material layer using the positive electrode mixture according to any one of aspects 1 to 4; and obtaining a lithium ion battery using the positive electrode active material layer, the electrolyte layer, and the negative electrode active material layer; A manufacturing method comprising: Effect of the Invention

[0006] By using the positive electrode mixture of the present disclosure to form a positive electrode active material layer of a lithium ion battery, the capacity of the lithium ion battery is likely to be improved. [Brief description of the drawings]

[0007] [Figure 1] 1 shows a schematic diagram of a first active material and a second active material included in a positive electrode mixture of the present disclosure. [Diagram 2] FIG. 3 is a schematic diagram for explaining the major axis and minor axis of a first active material. [Diagram 3] FIG. 1 is a schematic diagram for explaining the problem of a plate-shaped O2 type active material. [Figure 4] 1 shows an example of a flow of a manufacturing method for a first active material and a second active material. [Diagram 5] 1 illustrates a schematic diagram of an example of the configuration of a lithium ion battery. [Figure 6] 1 shows an example of a flow of a manufacturing method for a lithium-ion battery. [Figure 7] An example of the calcination conditions for obtaining a P2 type compound is shown. [Figure 8A] FIG. 2 is an SEM photograph of a plate-shaped O2 type positive electrode active material particle. [Figure 8B] FIG. 2 is an SEM photograph of spherical O2 type positive electrode active material particles. [Figure 9] 4 shows the relationship between the plate-like particle ratio and the discharge capacity. [Figure 10A] 3 is a cross-sectional SEM photograph of a positive electrode active material layer of the evaluation cell according to Example 1. FIG. [Figure 10B] 4 is a cross-sectional SEM photograph of a positive electrode active material layer of an evaluation cell according to Example 2. FIG. [Figure 10C] 4 is a cross-sectional SEM photograph of a positive electrode active material layer of an evaluation cell according to Comparative Example 1. FIG. [Figure 10D] 13 is a cross-sectional SEM photograph of a positive electrode active material layer of an evaluation cell according to Comparative Example 2. FIG. [Figure 10E] 13 is a cross-sectional SEM photograph of a positive electrode active material layer of an evaluation cell according to Comparative Example 3. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1. Cathode mixture FIG. 1 shows a positive electrode composite 1 according to one embodiment. The positive electrode composite 1 includes a first active material 1a and a second active material 1b. The first active material 1a has an O2 type structure and is plate-like. The second active material 1b has an O2 type structure and is spherical. The major axis D of the first active material 1a is 1.0 mm. 1L and the diameter D2 of the second active material 1b. 1L / D2 is equal to or greater than 0.1 and equal to or less than 1.5. The proportion of the first active material 1a to the total of the first active material 1a and the second active material 1b is equal to or greater than 10 mass % and equal to or less than 90 mass %.

[0009] 1.1 First active material The first active material 1a has an O2 type structure and is plate-shaped.

[0010] 1.1.1 Crystal structure of the first active material The first active material 1a has at least an O2 type structure (belonging to space group P63mc) as a crystal structure. The first active material 1a may have an O2 type structure and a crystal structure other than the O2 type structure. Examples of crystal structures other than the O2 type structure include a T♯2 type structure (belonging to space group Cmca) formed when Li is deintercalated from the O2 type structure and an O6 type structure (belonging to space group R-3m, with a c-axis length of 2.5 nm to 3.5 nm, typically 2.9 nm to 3.0 nm, different from the O3 type structure also belonging to space group R-3m). The first active material 1a may have an O2 type structure as a main phase, or may have a crystal structure other than the O2 type structure as a main phase. The crystal structure of the first active material 1a as a main phase may change depending on the charge / discharge state.

[0011] The first active material 1a may be a single crystal consisting of one crystallite, or may be a polycrystal having a plurality of crystallites.

[0012] 1.1.2 Chemical composition of the first active material The chemical composition of the first active material 1a is not particularly limited as long as the O2-type structure is maintained. The first active material 1a may contain, as constituent elements, at least one transition metal element among at least Mn, Ni, and Co, Li, and O. In particular, when the constituent elements include at least Li, Mn, at least one of Ni and Co, and O, among others, especially when the constituent elements include at least Li, Mn, Ni, Co, and O, higher performance is more likely to be obtained. However, for the first active material 1a, for example, Li may be released upon charging, and the abundance of Li may approach 0.

[0013] The first active material 1a is Li a Na b Mn x-p Ni y-q Co z-r M p+q+r It may have a chemical composition represented by O2. Here, 0 < a ≤ 1.00, 0 ≤ b ≤ 0.20, x + y + z = 1, and 0 ≤ p + q + r ≤ 0.15. Also, M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. When the first active material 1a has such a chemical composition, the O2-type structure is more likely to be maintained.

[0014] In the above chemical composition, a may be greater than 0, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, or 0.70 or less. In the above chemical composition, b may be 0 or more, 0.01 or more, 0.02 or more, or 0.03 or more, and may be 0.20 or less, 0.15 or less, or 0.10 or less. In the above chemical composition, x may be 0 or more, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. In the above chemical composition, y may be 0 or more, 0.10 or more, or 0.20 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. In the above chemical composition, z may be 0 or more, 0.10 or more, 0.20 or more, or 0.30 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. Many M do not contribute to charge and discharge. In this respect, by having p+q+r be 0.15 or less, a high charge and discharge capacity is easily ensured. p+q+r may be 0.10 or less, or may be 0. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.

[0015] 1.1.3 Shape of the first active material 1, the first active material 1a is plate-shaped. Whether the active material contained in the positive electrode composite 1 is "plate-shaped" or not is determined by forming a positive electrode active material layer 20 (described later) using the positive electrode composite 1, and observing a cross section along the thickness direction of the positive electrode active material layer 20 with a scanning electron microscope (SEM), a transmission electron microscope (TEM), an optical microscope, or the like. In the cross section, the active material has a major diameter D 1L and minor axis D 1S and the aspect ratio of the major axis to the minor axis (major axis D 1L / minor diameter D 1S) is 2 or more, the active material is considered to be plate-shaped. 1L refers to the maximum length from one point to another point on the surface of the first active material 1a in the cross-sectional shape of the first active material 1a, and the minor axis D 1S In the cross-sectional shape of the first active material 1a, the major axis D 1L The maximum length of the line perpendicular to the surface of the first active material 1a from one point to another point on the surface of the first active material 1a is defined as the maximum length of the line from one point to another point on the surface of the first active material 1a. The plate-like first active material 1a is not limited to having a constant thickness, and may have different thicknesses in different parts. The plate-like first active material 1a is not limited to being flat, and may have curves or distortions.

[0016] 1.1.4 Size of the first active material Major axis D of the first active material 1a 1L The minor axis D of the first active material 1a may be, for example, 0.3 μm or more and 8.0 μm or less, 0.5 μm or more and 6.0 μm or less, or 1.0 μm or more and 4.0 μm or less. 1S For example, the major axis D of the first active material 1a in the case where the positive electrode composite 1 includes a plurality of first active materials 1a may be 0.1 μm or more and 4.0 μm or less, 0.3 μm or more and 3.0 μm or less, or 0.5 μm or more and 2.0 μm or less. 1L is the number average value of the major axis of each of the first active materials 1a contained in the positive electrode mixture 1, and 1S is the number average value of the minor axis of each of the first active materials 1 a contained in the positive electrode mixture 1 .

[0017] 1.2 Second active material The second active material 1b has an O2 type structure and is spherical.

[0018] 1.2.1 Crystal structure of the second active material The second active material 1b has at least an O2 type structure (belonging to space group P63mc) as a crystal structure. The second active material 1b may have an O2 type structure and a crystal structure other than the O2 type structure. Examples of crystal structures other than the O2 type structure include a T♯2 type structure (belonging to space group Cmca) formed when Li is deintercalated from the O2 type structure and an O6 type structure (belonging to space group R-3m, with a c-axis length of 2.5 nm to 3.5 nm, typically 2.9 nm to 3.0 nm, different from the O3 type structure also belonging to space group R-3m). The second active material 1b may have an O2 type structure as a main phase, or may have a crystal structure other than the O2 type structure as a main phase. The crystal structure of the second active material 1b as a main phase may change depending on the charge / discharge state.

[0019] The second active material 1b may be a single crystal consisting of one crystallite, or may be a polycrystal having multiple crystallites. The surface of the second active material 1b may have multiple crystallites. When the surface of the second active material 1b has multiple crystallites, a crystal grain boundary is present on the surface of the second active material 1b. Here, the crystal grain boundary may be an inlet and an outlet of intercalation. That is, when the second active material 1b has multiple crystallites on its surface, the effect of increasing the number of inlets and outlets for intercalation and reducing the reaction resistance, the effect of shortening the distance traveled by lithium ions and reducing the diffusion resistance, the absolute amount of expansion and contraction during charging and discharging is reduced, and the effect of making it difficult for cracks to occur can be expected.

[0020] The size of the crystallites constituting the second active material 1b may be large or small, but the smaller the crystallite size, the more grain boundaries there are, and the more likely the above-mentioned advantageous effects are to be exhibited. For example, if the diameter of the crystallites constituting the second active material 1b is less than 1 μm, higher performance is likely to be obtained. The "crystallites" and "diameter of the crystallites" can be obtained by observing the surface of the positive electrode active material particles with a scanning electron microscope (SEM) or a transmission electron microscope (TEM). That is, when the surface of the second active material 1b is observed and a closed region surrounded by grain boundaries is observed, the region is regarded as a "crystallite". The maximum Feret diameter of the crystallite is obtained and regarded as the "diameter of the crystallite". If the particle is composed of a single crystal, the particle itself can be said to be a single crystallite, and the maximum Feret diameter of the particle is the "diameter of the crystallite". Alternatively, the diameter of the crystallite can be obtained by EBSD or XRD. For example, the crystallite diameter can be determined from the half-width of the diffraction line in the XRD pattern based on Scherrer's formula. If the crystallite diameter of the second active material 1b determined by any method is less than 1 μm, higher performance is likely to be obtained.

[0021] The crystallites of the second active material 1b may have a first surface exposed on the particle surface, and the first surface may be planar. The surface of the second active material 1b may have a structure in which a plurality of planes are connected. When producing the second active material 1b, the crystallites are allowed to grow on the particle surface until one crystallite and another crystallite are connected to each other, whereby it is easy to obtain crystallites having a planar first surface.

[0022] 1.2.2 Chemical composition of the second active material The chemical composition of the second active material 1b is not particularly limited as long as the O2-type structure is maintained. The chemical composition of the second active material 1b may be the same as or different from the chemical composition of the first active material 1a. The second active material 1b may contain, as constituent elements, at least one transition metal element among at least Mn, Ni, and Co, Li, and O. In particular, when it contains, as constituent elements, at least Li, Mn, at least one of Ni and Co, and O, especially when it contains, as constituent elements, at least Li, Mn, Ni, Co, and O, higher performance is more likely to be obtained. However, in the second active material 1b, for example, Li may be released by charging and the abundance of Li may become close to 0.

[0023] The second active material 1b is Li a Na b Mn x-p Ni y-q Co z-r M p+q+r It may have a chemical composition represented by O2. Here, 0 < a ≤ 1.00, 0 ≤ b ≤ 0.20, x + y + z = 1, and 0 ≤ p + q + r ≤ 0.15. Also, M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. When the second active material 1b has such a chemical composition, the O2-type structure is more likely to be maintained.

[0024] In the above chemical composition, a may be greater than 0, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, or 0.70 or less. In the above chemical composition, b may be 0 or more, 0.01 or more, 0.02 or more, or 0.03 or more, and may be 0.20 or less, 0.15 or less, or 0.10 or less. In the above chemical composition, x may be 0 or more, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. In the above chemical composition, y may be 0 or more, 0.10 or more, or 0.20 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. In the above chemical composition, z may be 0 or more, 0.10 or more, 0.20 or more, or 0.30 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. Many M do not contribute to charge and discharge. In this respect, by having p+q+r be 0.15 or less, a high charge and discharge capacity is easily ensured. p+q+r may be 0.10 or less, or may be 0. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.

[0025] 1.2.3 Shape of the second active material The second active material 1b is spherical. "Spherical" means that the circularity is 0.80 or more. The circularity of the active material may be 0.81 or more, 0.82 or more, 0.83 or more, 0.84 or more, 0.85 or more, 0.86 or more, 0.87 or more, 0.88 or more, 0.89 or more, or 0.90 or more. The circularity of the active material is 4πS / L 2 Here, S is the orthogonal projected area of ​​the particle, and L is the perimeter of the orthogonal projected image of the particle. The circularity of the active material can be determined by observing the appearance or the above-mentioned cross-sectional shape of the particle using a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an optical microscope.

[0026] The second active material 1b may be a solid particle, a hollow particle, or a particle having a void. When the second active material 1b is a hollow particle or a particle having a void, it is considered possible to fill the hollow or void with a liquid. For example, the electrolyte is distributed not only on the outer surface of the active material but also inside, and the contact area between the particle and the electrolyte is likely to increase.

[0027] 1.2.4 Size of the second active material The size of the second active material 1b is the above D 1L As long as the relationship of / D2 is satisfied, there is no particular limitation. For example, the diameter D2 of the second active material 1b may be 0.5 μm or more and 10 μm or less, 1.0 μm or more and 8.0 μm or less, or 2.0 μm or more and 6.0 μm or less. The diameter D2 of the second active material 1b refers to the circle-equivalent diameter when the external appearance or cross-sectional shape of the second active material 1b is observed by SEM or the like. When the positive electrode composite 1 includes a plurality of second active materials 1b, the diameter D2 of the second active material 1b is the number average value of the circle-equivalent diameter of each of the second active materials 1b included in the positive electrode composite 1.

[0028] 1.3 Ratio of the major axis of the first active material to the diameter of the second active material In the positive electrode mixture 1, the major axis D of the first active material 1a 1L and the diameter D2 of the second active material 1b. 1L / D2 is 0.1 or more and 1.5 or less. 1L / D2 may be 0.2 to 1.5, 0.3 to 1.5, 0.4 to 1.5, 0.5 to 1.5, 0.6 to 1.5, 0.7 to 1.5, 0.8 to 1.5, 0.9 to 1.5, 1.0 to 1.5, or 1.1 to 1.5, or may be 0.1 to less than 1.5, 0.1 to 1.4, or 0.1 to 1.3. In this way, the second active material 1b has a predetermined size relative to the first active material 1a, so that the first active material 1a stands up due to the second active material 1b, as described later, and the amount of the first active material 1a that intersects with the surface direction of the positive electrode active material layer 20 increases, the degree of bending is reduced, and the utilization rate of the first active material 1a is easily increased. In addition, the second active material 1b itself can contribute to improving the capacity. As a result, the capacity of the positive electrode is easily increased.

[0029] 1.3 Ratio of first active material to second active material In the positive electrode composite 1, the ratio of the first active material 1a to the total of the first active material 1a and the second active material 1b is 10% by mass or more and 90% by mass or less. If the first active material 1a is too little or too much, the capacity tends to decrease. The mass ratio of the first active material 1a to the total of the first active material 1a and the second active material 1b may be lower or higher than the mass ratio of the second active material 1b. When combined with a solid electrolyte, the mass ratio of the first active material 1a to the total of the first active material 1a and the second active material 1b is higher than the mass ratio of the second active material 1b, which tends to exhibit better performance. On the other hand, when combined with a liquid electrolyte, the mass ratio of the first active material 1a to the total of the first active material 1a and the second active material 1b is lower than the mass ratio of the second active material 1b, which tends to exhibit better performance. The proportion of the first active material 1a may be 15% by mass or more and 85% by mass or less, and the lower limit may be 20% by mass or more, 25% by mass or more, 30% by mass or more, 35% by mass or more, 40% by mass or more, 45% by mass or more, 50% by mass or more, 55% by mass or more, 60% by mass or more, 65% by mass or more, or 70% by mass or more, and the upper limit may be 80% by mass or less, 75% by mass or less, 70% by mass or less, 65% by mass or less, 60% by mass or less, 55% by mass or less, 50% by mass or less, 45% by mass or less, 40% by mass or less, 35% by mass or less, 30% by mass or less, 25% by mass or less, 20% by mass or less, or 15% by mass or less.

[0030] 1.4 Other ingredients The positive electrode mixture 1 includes at least the first active material 1a and the second active material 1b as the positive electrode active material. The positive electrode mixture 1 may also include an electrolyte. The electrolyte may be a solid electrolyte, a liquid electrolyte, or a combination of a solid electrolyte and a liquid electrolyte. When the positive electrode mixture 1 includes a solid electrolyte, excellent effects are likely to be exhibited. The positive electrode mixture 1 may also include one or both of a conductive assistant and a binder. The positive electrode mixture 1 may also include an electrolyte, a conductive assistant, and a binder. The positive electrode mixture 1 may also include an electrolyte, a conductive assistant, and a binder. The positive electrode mixture 1 may also include various additives. The contents of the first active material 1a, the second active material 1b, the electrolyte, the conductive assistant, the binder, and the like in the positive electrode mixture 1 may be appropriately determined according to the desired performance. For example, assuming that the entire positive electrode composite 1 (total solid content) is 100 mass%, the content of the positive electrode active material (the total of the first active material 1a, the second active material 1b, and other positive electrode active materials) may be 40 mass% or more and 100 mass% or less, the lower limit may be 50 mass% or more or 60 mass% or more, and the upper limit may be 90 mass% or less.

[0031] 1.4.1 Other positive electrode active materials The positive electrode mixture 1 may contain only the first active material 1a and the second active material 1b as the positive electrode active material. Alternatively, the positive electrode mixture 1 may contain, in addition to the first active material 1a and the second active material 1b, a different type of positive electrode active material (another positive electrode active material). From the viewpoint of further enhancing the effect of the technology of the present disclosure, the content of the other positive electrode active material in the positive electrode mixture 1 may be small. For example, the content of the positive electrode active material derived from the first active material 1a and the second active material 1b may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less.

[0032] Any other positive electrode active material can be any of those known as positive electrode active materials for secondary batteries. Among the known active materials, a material with a relatively high potential (charge / discharge potential) for occluding and releasing a predetermined carrier ion can be used as the positive electrode active material, and a material with a relatively low potential can be used as the negative electrode active material. The other positive electrode active materials may be, for example, at least one selected from various lithium-containing compounds, elemental sulfur, sulfur compounds, etc. The lithium-containing compound as the positive electrode active material may be a lithium-containing oxide containing at least one element M, Li, and O. Element M may be, for example, at least one selected from Mn, Ni, Co, Al, Mg, Ca, Sc, V, Cr, Cu, Zn, Ga, Ge, Y, Zr, Sn, Sb, W, Pb, Bi, Fe, and Ti, or at least one selected from the group consisting of Mn, Ni, Co, Al, Fe, and Ti. More specifically, the lithium-containing oxide is lithium cobalt oxide, lithium nickel oxide, lithium manganate, lithium nickel cobalt oxide, lithium nickel manganate, lithium cobalt manganate, lithium nickel cobalt manganate (Li 1±α Ni x Co y Mn z O 2±δ (for example, 0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1)), spinel-type lithium compounds (Li 1+x Mn 2-x-y M y O4 (M is one or more selected from Al, Mg, Co, Fe, Ni, and Zn), such as hetero-element-substituted Li-Mn spinel with a composition represented by this formula), lithium nickel cobalt aluminum oxide (for example, Li 1±α Ni p Co q Al r O 2±δ(For example, p+q+r=1), lithium titanate, lithium metal phosphate (LiMPO4, etc., M is one or more selected from Fe, Mn, Co, and Ni), etc. The other positive electrode active material may contain a lithium-containing oxide containing at least one of Ni, Co, and Mn, Li, and O as a constituent element. Alternatively, the other positive electrode active material may contain a lithium-containing oxide containing at least one of Ni, Co, and Al, Li, and O as a constituent element. Only one type of the other positive electrode active material may be used alone, or two or more types may be used in combination.

[0033] The shape of the other positive electrode active material may be a general shape as a positive electrode active material for a secondary battery. The other positive electrode active material may be, for example, particulate. The other positive electrode active material may have voids, for example, may be porous or hollow. The other positive electrode active material may be primary particles or secondary particles formed by agglomeration of a plurality of primary particles. The average particle diameter D50 of the other positive electrode active material may be, for example, 1 nm or more and 500 μm or less, the lower limit may be 5 nm or more or 10 nm or more, and the upper limit may be 100 μm or less, 50 μm or less, or 30 μm or less. The average particle diameter D50 is the particle diameter (median diameter) at 50% cumulative value in the volume-based particle size distribution obtained by the laser diffraction / scattering method.

[0034] 1.4.2 Protective layer An ion-conductive protective layer may be formed on the surface of the positive electrode active material (first active material 1a, second active material 1b, other positive electrode active materials). That is, the positive electrode mixture 1 may include a complex of the positive electrode active material and the protective layer, and at least a part of the surface of the positive electrode active material in the complex may be covered with the protective layer. This makes it easier to suppress, for example, the reaction between the positive electrode active material and other battery materials (such as a sulfide solid electrolyte described later). The ion-conductive protective layer may include various ion-conductive compounds. The ion-conductive compound may be, for example, at least one selected from ion-conductive oxides and ion-conductive halides.

[0035] The ion conductive oxide may contain, for example, at least one element selected from B, C, Al, Si, P, S, Ti, La, Zr, Nb, Mo, Zn, and W, Li, and O. The ion conductive oxide may be an oxynitride containing N. More specifically, the ion conductive oxide may be Li3BO3, LiBO2, Li2CO3, LiAlO2, Li4SiO4, Li2SiO3, Li3PO4, Li2SO4, Li2TiO3, Li4Ti5O 12 , Li2Ti2O5, Li2ZrO3, LiNbO3, Li2MoO4, Li2WO4, LiPON, Li2O-LaO2, Li2O-ZnO2, etc. The ion-conductive oxide may be one in which some elements are substituted with various doping elements.

[0036] The ion conductive halide may be, for example, at least one of various compounds exemplified as the halide solid electrolyte described later. The ion conductive halide may include, for example, at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb and Sm, at least one halogen element selected from the group consisting of Cl, Br, I and F, and Li. The ion conductive halide may include at least one element selected from the group consisting of Ti, Al, Gd, Ca, Zr and Y, at least one element selected from the group consisting of Cl, Br, I and F, and Li. The ion conductive halide may also include at least one element selected from the group consisting of Ti and Al, at least one element selected from the group consisting of Cl, Br, I and F, and Li. The ion conductive halide may also be, for example, a complex halide of Li, Ti, Al and F.

[0037] The coverage (area ratio) of the protective layer with respect to the surface of the positive electrode active material may be, for example, 70% or more, 80% or more, or 90% or more. The thickness of the protective layer may be, for example, 0.1 nm or more and 100 nm or less, with a lower limit of 1 nm or more and an upper limit of 20 nm or less.

[0038] 1.4.3 Electrolytes The positive electrode mixture 1 may contain an electrolyte. The electrolyte that may be contained in the positive electrode mixture 1 may be a solid electrolyte, a liquid electrolyte, or a combination of a solid electrolyte and a liquid electrolyte. As described above, when the positive electrode mixture 1 contains a solid electrolyte, excellent effects are likely to be exhibited.

[0039] 1.4.3.1 Solid electrolyte As the solid electrolyte, a solid electrolyte known for lithium ion batteries may be used. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, the inorganic solid electrolyte has excellent ion conductivity and heat resistance. Examples of the inorganic solid electrolyte include an oxide solid electrolyte, a sulfide solid electrolyte, and an ion-bonded inorganic solid electrolyte. Among the inorganic solid electrolytes, the sulfide solid electrolyte, and among them, the sulfide solid electrolyte containing at least Li, S, and P as constituent elements, have high performance. Alternatively, among the inorganic solid electrolytes, the ion-bonded solid electrolyte, and among them, the solid electrolyte containing at least Li, Y, and a halogen (at least one of Cl, Br, I, and F) as constituent elements, have high performance. The solid electrolyte may be amorphous or crystalline. The solid electrolyte may be particulate. The average particle diameter (D50) of the solid electrolyte may be, for example, 10 nm or more and 10 μm or less. The average particle diameter D50 in the present application is the particle diameter (median diameter) at an integrated value of 50% in the volume-based particle size distribution obtained by a laser diffraction / scattering method. The ionic conductivity of the solid electrolyte at 25° C. is, for example, 1×10 -5 S / cm or more, 1×10 -4 S / cm or more, or 1×10 -3 The solid electrolyte may have a specific surface area of ​​100 nm or more and may have a specific surface area of ​​100 nm or more.

[0040] The oxide solid electrolyte is lithium lanthanum zirconate, LiPON, Li 1+X Al X Ge 2-X It may be one or more selected from (PO4)3, Li-SiO-based glass, Li-Al-SO-based glass, etc. In addition, when an oxide solid electrolyte is combined with a liquid electrolyte, ion conductivity can be improved.

[0041] The sulfide solid electrolyte may be a glass-based sulfide solid electrolyte (sulfide glass), a glass ceramic-based sulfide solid electrolyte, or a crystalline sulfide solid electrolyte. The sulfide glass is amorphous. The sulfide glass may have a glass transition temperature (Tg). In addition, when the sulfide solid electrolyte has a crystalline phase, examples of the crystalline phase include a Thio-LISICON type crystalline phase, a LGPS type crystalline phase, and an Argyrodite type crystalline phase.

[0042] The sulfide solid electrolyte may contain, for example, Li element, X element (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S element. The sulfide solid electrolyte may further contain at least one of O element and halogen element. The sulfide solid electrolyte may contain S element as a main component of anion element.

[0043] Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-GeS2, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-P2S5-LiI-LiBr, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-ZmSn (where m and n are positive numbers, and Z is Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, and Li2S-SiS2-Li x MO y (wherein x and y are positive numbers, and M is any one of P, Si, Ge, B, Al, Ga, and In).

[0044] The composition of the sulfide solid electrolyte is not particularly limited. For example, xLi2S·(100 - x)P2S5 (70 ≦ x ≦ 80), yLiI·zLiBr·(100 - y - z)(xLi2S·(1 - x)P2S5) (0.7 ≦ x ≦ 0.8, 0 ≦ y ≦ 30, 0 ≦ z ≦ 30), etc. may be mentioned. Alternatively, the sulfide solid electrolyte has a composition represented by the general formula: Li 4-x Ge 1-x P x S4 (0 < x < 1). In the above general formula, at least a part of Ge may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, at least a part of P may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, a part of Li may be substituted with at least one of Na, K, Mg, Ca, and Zn. In the above general formula, a part of S may be substituted with a halogen (at least one of F, Cl, Br, and I). Alternatively, the sulfide solid electrolyte is Li 7-a PS 6-a X a (X is at least one of Cl, Br, and I, and a is a number of 0 or more and 2 or less). a may be 0, or may be greater than 0. In the latter case, a may be 0.1 or more, may be 0.5 or more, and may be 1 or more. Also, a may be 1.8 or less, may be 1.5 or less.

[0045] The ion-bonded solid electrolyte may contain at least one element selected from the group consisting of, for example, Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb and Sm. These elements may generate cations in water. The ion-bonded solid electrolyte material may further contain, for example, at least one halogen element selected from the group consisting of Cl, Br, I and F. These elements may generate anions in water. The ion-bonded solid electrolyte may contain at least one element selected from the group consisting of Gd, Ca, Zr and Y, at least one element selected from the group consisting of Cl, Br, I and F, and Li. The ion-bonded solid electrolyte may contain Li and Y, and at least one element selected from the group consisting of Cl, Br, I and F. More specifically, the ionic solid electrolyte may contain Li, Y, Cl, and Br, or may contain Li, Ca, Y, Gd, Cl, and Br, or may contain Li, Zr, Y, and Cl. More specifically, the ionic solid electrolyte may be Li3YBr2Cl4, Li 2.8 Ca 0.1 Y 0.5 Gd 0.5 Br2Cl4 and Li 2.5 Y 0.5 Zr 0.5 Cl6.

[0046] The ionically bonded solid electrolyte may be a halide solid electrolyte. The halide solid electrolyte has excellent ion conductivity. Examples of the halide solid electrolyte include those represented by the formula (1): Li α M β X γ (A) It may have a composition represented by the following. Here, α, β, and γ are each independently a value greater than 0, M is at least one selected from the group consisting of metal elements other than Li and metalloid elements, and X is at least one selected from the group consisting of Cl, Br, and I. Note that the “metalloid element” may be at least one selected from the group consisting of B, Si, Ge, As, Sb, and Te. Also, the “metal element” may include (i) all elements contained in Groups 1 to 12 of the periodic table (excluding hydrogen) and (ii) all elements contained in Groups 13 to 16 of the periodic table (excluding B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se). The metal element can form an inorganic compound with a halide ion and become a cation.

[0047] In formula (A), M may contain Y (i.e., yttrium). The halide solid electrolyte containing Y is Li a Me b Y c It may have a composition represented by X6 (where a + mb + 3c = 6, c > 0, Me is at least one selected from the group consisting of metal elements and metalloid elements other than Li and Y, and m is the valence of Me). Me may be at least one selected from the group consisting of, for example, Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta, and Nb.

[0048] The halide solid electrolyte may have a composition represented by formula (A1): Li 6-3d Y d X6. In formula (A1), X is one or more elements selected from the group consisting of Cl, Br, and I. d may satisfy 0 < d < 2, or d = 1. The halide solid electrolyte may have a composition represented by formula (A2): Li 3-3δ Y 1+δ Cl6. In formula (A2), 0 < δ ≦ 0.15 may hold. The halide solid electrolyte may have a composition represented by formula (A3): Li 3-3δ Y 1+δIt may have a composition represented by Br6. In formula (A3), 0 < δ ≦ 0.25 may also be applicable. The halide solid electrolyte has the formula (A4): Li 3-3δ+a Y 1+δ-a Me a Cl 6-x-y Br x I y and may have a composition represented by this. In formula (A4), Me may be at least one selected from the group consisting of Mg, Ca, Sr, Ba, and Zn. In formula (A4), for example, -1 < δ < 2, 0 < a < 3, 0 < (3 - 3δ + a), 0 < (1 + δ - a), 0 ≦ x ≦ 6, 0 ≦ y ≦ 6, and (x + y) ≦ 6 are satisfied. The halide solid electrolyte has the formula (A5): Li 3-3δ Y 1+δ-a Me a Cl 6-x-y Br x I y and may have a composition represented by this. In formula (A5), Me may be at least one selected from the group consisting of Al, Sc, Ga, and Bi. In formula (A5), -1 < δ < 1, 0 < a < 2, 0 < (1 + δ - a), 0 ≦ x ≦ 6, 0 ≦ y ≦ 6, and (x + y) ≦ 6 may also be applicable. The halide solid electrolyte has the formula (A6): Li 3-3δ-a Y 1+δ-a Me a Cl 6-x-y Br x I y and may have a composition represented by this. In formula (A6), Me may be at least one selected from the group consisting of Zr, Hf, and Ti. In formula (A6), -1 < δ < 1, 0 < a < 1.5, 0 < (3 - 3δ - a), 0 < (1 + δ - a), 0 ≦ x ≦ 6, 0 ≦ y ≦ 6, and (x + y) ≦ 6 may also be applicable. The halide solid electrolyte has the formula (A7): Li 3-3δ-2a Y 1+δ-a Me a Cl 6-x-y Br x I yIn formula (A7), Me may be at least one selected from the group consisting of Ta and Nb. In formula (A7), -1<δ<1, 0 <a<1.2、0<(3-3δ-2a)、0<(1+δ-a)、0≦x≦6、0≦y≦6、かつ、(x+y)≦6であってもよい。

[0049] The ionically bonded solid electrolyte may be a complex hydride solid electrolyte. The complex hydride solid electrolyte may be composed of Li ions and complex ions containing H. The complex ion containing H may have, for example, an element M containing at least one of a nonmetallic element, a semimetallic element, and a metallic element, and H bonded to the element M. In addition, the complex ion containing H may have the element M as a central element and H surrounding the element M bonded to each other via a covalent bond. In addition, the complex ion containing H may be (M m H n ) α- In this case, m is any positive number, and n and α can be any positive number depending on m and the valence of the element M. The element M may be a nonmetallic element or a metallic element capable of forming a complex ion. For example, the element M may contain at least one of B, C, and N as a nonmetallic element, or may contain B. Also, for example, the element M may contain at least one of Al, Ni, and Fe as a metallic element. In particular, when the complex ion contains B or contains C and B, higher ionic conductivity is likely to be ensured. Specific examples of complex ions containing H include (CB9H 10 ) - , (C.B. 11 H 12 ) - , (B 10 H 10 ) 2- , (B 12 H 12 ) 2- , (BH4) - , (NH2) - , (AlH4) - , and combinations thereof. In particular, (CB9H 10 ) - , (C.B. 11H 12 ) - In other words, the complex hydride solid electrolyte may contain Li, C, B, and H.

[0050] 1.4.3.2 Liquid electrolyte The liquid electrolyte (electrolyte) is a liquid containing carrier ions. In the case of a positive electrode composite for a lithium ion battery, the electrolyte contains lithium ions. The electrolyte may be an aqueous electrolyte or a non-aqueous electrolyte. The composition of the electrolyte may be the same as that of the electrolyte of a lithium ion secondary battery known in the art. The electrolyte may be a solution of a lithium salt dissolved in water or a non-aqueous solvent. Examples of the non-aqueous solvent include carbonate-based solvents. Examples of the carbonate-based solvent include fluoroethylene carbonate (FEC), ethylene carbonate (EC), dimethyl carbonate (DMC), and the like. Examples of the lithium salt include LiPF6, LiTFSI, LiFSI, and the like.

[0051] 1.4.4 Conductive additives Examples of the conductive assistant that may be included in the positive electrode composite 1 include carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, titanium, aluminum, and stainless steel. The conductive assistant may be, for example, particulate or fibrous, and the size is not particularly limited. Only one type of conductive assistant may be used alone, or two or more types may be used in combination.

[0052] 1.4.5 Binders Examples of binders that can be included in the positive electrode mixture 1 include butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.

[0053] 1.4.6 Other In addition to the above components, the positive electrode mixture 1 may contain various additives, such as a dispersant and a lubricant.

[0054] 1.5 Effect of positive electrode mixture As described above, the positive electrode composite material 1 includes a predetermined first active material 1a and a predetermined second active material 1b. Here, the plate-shaped O2 type active material (first active material 1a) has an intercalation inlet and outlet at its end. Therefore, when a positive electrode active material layer is formed using a plate-shaped O2 type active material, it is preferable that the plate surface of the plate-shaped O2 type active material intersects (preferably perpendicular to) the surface direction of the positive electrode active material layer in the positive electrode active material layer. However, when a positive electrode active material layer is formed using only a plate-shaped O2 type active material as the positive electrode active material, the plate surface of the plate-shaped O2 type active material is aligned with the surface direction of the positive electrode active material layer (FIG. 3). Therefore, the capacity is likely to decrease due to an increase in the degree of bending and a decrease in the utilization rate of the plate-shaped O2 type active material. In contrast, according to the positive electrode composite 1, by mixing the spherical O2 type active material (second active material 1b) with the plate-shaped O2 type active material, the plate-shaped O2 type active material can be raised by the spherical O2 type active material, and the orientation of the plate surface of the plate-shaped O2 type active material can be easily randomized (FIG. 1). That is, the amount of the plate-shaped O2 type active material intersecting with the surface direction of the positive electrode active material layer 20 increases, and the capacity is easily increased due to a reduction in the degree of bending and an increase in the utilization rate of the plate-shaped O2 type active material. In addition, the spherical O2 type active material itself can contribute to improving the capacity, so that the capacity can be further increased.

[0055] 2. Manufacturing method of the positive electrode mixture The positive electrode mixture 1 is obtained by mixing at least a first active material 1a and a second active material 1b. Here, the first active material 1a and the second active material 1b can be produced, for example, as follows.

[0056] 2.1 Method for producing the first and second active materials As shown in FIG. 4, the first active material 1a and the second active material 1b are each produced by the following method: Obtaining precursor particles (step S1), Coating the surface of the precursor particles with a Na salt to obtain coated particles (step S2); The coated particles are calcined to obtain Na-containing transition metal oxide particles having a P2 type structure (step S3); and At least a portion of the Na in the Na-containing transition metal oxide particles is replaced with Li by ion exchange to obtain positive electrode active material particles having an O2 type structure (step S4); It may include.

[0057] 2.1.1 Process S1 In step S1, precursor particles are obtained. Here, the precursor particles may be a salt or a compound containing at least one transition metal element selected from Mn, Ni, and Co. The precursor particles may be, for example, at least one of carbonate, sulfate, nitrate, acetate, and hydroxide. Specifically, the precursor particles may be a salt represented by MeCO3 (Me is at least one transition metal element selected from Mn, Ni, and Co), a salt represented by MeSO4, a salt represented by Me(NO3)2, a salt represented by Me(CH3COO)2, or a compound represented by Me(OH)2. These may be hydrates. In addition to the transition metal element Me, the precursor particles may also contain at least one element M selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.

[0058] The precursor particles may be spherical. The definition of "spherical" is as described above. By using spherical precursor particles, the shape of the finally obtained active material may also be spherical. That is, the second active material 1b is easily obtained. The size of the spherical precursor particles is not particularly limited. The spherical precursor particles can be obtained by a solution method such as a coprecipitation method or a sol-gel method. Specifically, in the case of the coprecipitation method, an aqueous solution of MeSO4 and an aqueous solution of Na2CO3 are prepared, and each aqueous solution is dropped and mixed to obtain a precipitate. The precipitate is a spherical precursor particle represented by MeCO3. A carbonate containing Me and M may be obtained as the precursor particle by dissolving a sulfate of M in the aqueous solution of MeSO4.

[0059] 2.1.2 Process S2 In step S2, the surface of the precursor particle is coated with a Na salt to obtain a coated particle. When a spherical O2 type positive electrode active material (second active material 1b) is obtained, the coated particle may be obtained by coating 40% or more of the surface of the precursor particle with a Na salt. The coated particle may be obtained by coating 50% or more, 60% or more, or 70% or more of the surface of the precursor particle with a Na salt. Examples of the Na salt include carbonates and nitrates.

[0060] There are various methods for coating the surface of the precursor particles with a Na salt. When a spherical O2 type positive electrode active material (second active material 1b) is finally obtained, for example, a rolling fluidized coating method or a spray drying method may be adopted. That is, a coating solution in which a Na salt is dissolved is prepared, and the coating solution is brought into contact with the entire surface of the precursor particles, or the coating solution is dried at the same time as or after the contact. By adjusting the coating conditions (temperature, time, number of times, etc.), for example, 40 area % or more of the surface of the precursor particles can be coated with Na salt. According to the findings of the present inventor, if the coverage rate of the Na salt is small, when the coated particles are fired, P2 type crystals tend to grow abnormally on the surface of the coated particles, and while plate-shaped Na-containing transition metal oxide particles are obtained, it is difficult to obtain spherical Na-containing transition metal oxide particles. If the coverage rate of the Na salt is large, when the coated particles are fired, the crystallites of the P2 type crystals can be made small, and the shape of the coated particles tends to become spherical corresponding to the shape of the precursor particles. The amount of Na salt coated on the coated particles may be sufficient to obtain a P2 type structure (an amount sufficient for doping with Na).

[0061] 2.1.3 Process S3 In step S3, the coated particles are fired to obtain Na-containing transition metal oxide particles having a P2-type structure. Here, the Na-containing transition metal oxide particles may be plate-shaped or spherical. When the Na-containing transition metal oxide particles are plate-shaped, the O2-type positive electrode active material obtained thereafter is also plate-shaped. That is, a first active material 1a is obtained. On the other hand, when the Na-containing transition metal oxide particles are spherical, the O2-type positive electrode active material obtained thereafter is also spherical. That is, a second active material 1b is obtained.

[0062] The Na-containing transition metal oxide particles may contain, as constituent elements, at least one transition metal element selected from Mn, Ni, and Co, Na, and O. In particular, when the constituent elements contain at least Na, Mn, at least one of Ni and Co, and O, and especially when the constituent elements contain at least Na, Mn, Ni, Co, and O, the performance of the positive electrode active material particles is likely to be further improved. The Na-containing transition metal oxide particles may contain Na c Mn x-p Ni y-q Co z-r M p+q+rIt may have a chemical composition represented by O2. Here, 0 < c ≤ 1.00, x + y + z = 1, and 0 ≤ p + q + r ≤ 0.15. Also, M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. When the Na-containing transition metal oxide particles have such a chemical composition, the P2-type structure is more likely to be maintained. In the above chemical composition, c may be greater than 0, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, or 0.70 or less. In the above chemical composition, x may be 0 or more, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. In the above chemical composition, y may be 0 or more, 0.10 or more, or 0.20 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. In the above chemical composition, z may be 0 or more, 0.10 or more, 0.20 or more, or 0.30 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. Many of the M do not contribute to charge and discharge. In this regard, when p + q + r is 0.15 or less, it is easy to ensure a high charge and discharge capacity. p + q + r may be 0.10 or less, or may be 0. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.

[0063] The firing temperature may be a temperature at which the P2-type structure is formed. If the firing temperature is too low, Na doping is not performed and it is difficult to obtain the P2-type structure. On the other hand, if the firing temperature is too high, an O3-type structure is likely to be formed instead of the P2-type structure. The firing temperature may be, for example, 700°C or higher and 1100°C or lower, or may be 800°C or higher and 1000°C or lower.

[0064] The calcination time may be appropriately adjusted according to the shape of the desired Na-containing transition metal oxide particles. As described above, when the coverage rate of the Na salt in the coated particles is small, when the coated particles are calcined, P2 type crystals tend to grow abnormally on the surface of the coated particles, and plate-shaped Na-containing transition metal oxide particles are easily obtained. On the other hand, when the coverage rate of the Na salt in the coated particles is large, when the coated particles are calcined, small P2 type crystals tend to be formed on the surface of the particles, and one P2 type crystallite and another P2 type crystallite are connected to each other to grow the P2 type crystals along the surface of the particles, thereby obtaining spherical Na-containing transition metal oxide particles. If the calcination time is too short, Na doping is not performed and the desired P2 type structure is not obtained. On the other hand, if the calcination time is too long, the P2 type structure grows excessively, resulting in plate-shaped particles. As far as the inventors have confirmed, when the firing time is from 30 minutes to 3 hours, spherical Na-containing transition metal oxide particles are likely to be obtained, and when the firing time is longer than this, plate-shaped Na-containing transition metal oxide particles are likely to be obtained.

[0065] The firing atmosphere is not particularly limited, and may be, for example, an oxygen-containing atmosphere such as air atmosphere, or an inert gas atmosphere.

[0066] 2.1.4 Process S4 In step S4, at least a part of the Na in the Na-containing transition metal oxide particles is replaced with Li by ion exchange to obtain positive electrode active material particles having an O2 type structure. Here, a part of the Na in the plate-like P2 type particles is ion-exchanged with Li to obtain a plate-like O2 type active material (first active material 1a). On the other hand, a part of the Na in the spherical P2 type particles is ion-exchanged with Li to obtain a spherical O2 type active material (second active material 1b).

[0067] Ion exchange can be performed, for example, by using an aqueous solution containing lithium halide, or by using a mixture of lithium halide and other lithium salts (e.g., molten salt). From the viewpoint that the P2 type structure is easily broken by the intrusion of water and from the viewpoint of crystallinity, the method using the molten salt is preferred among the above two methods. That is, by mixing the Na-containing transition metal oxide particles having the above-mentioned P2 type structure with the molten salt and heating to a temperature equal to or higher than the melting point of the molten salt, at least a part of the Na in the Na-containing transition metal oxide particles can be replaced with Li by ion exchange.

[0068] The lithium halide constituting the molten salt is preferably at least one of lithium chloride, lithium bromide, and lithium iodide. The other lithium salt constituting the molten salt is preferably lithium nitrate. By using the molten salt, the melting point becomes lower than when the lithium halide or other lithium salt is used alone, and ion exchange can be performed at a lower temperature.

[0069] The temperature in the ion exchange may be, for example, above the melting point of the molten salt and below 600°C, below 500°C, below 400°C, or below 300°C. If the temperature in the ion exchange is too high, the stable O3 structure is likely to be formed instead of the O2 structure. On the other hand, from the viewpoint of shortening the time required for the ion exchange, it is preferable that the temperature in the ion exchange is as high as possible.

[0070] 2.2 Mixing with other ingredients The first active material 1a and the second active material 1b produced as described above are mixed with the above-mentioned solid electrolyte or the like to obtain the positive electrode composite material 1. The mixing means is not particularly limited, and the mixing may be performed using a known mixing device.

[0071] 3. Lithium-ion battery The positive electrode composite material 1 of the present disclosure may be employed as a positive electrode material for a lithium ion battery. FIG. 5 shows a schematic configuration of a lithium ion battery 100 according to an embodiment. As shown in FIG. 5, the lithium ion battery 100 has a positive electrode active material layer 20, an electrolyte layer 30, and a negative electrode active material layer 40. The positive electrode active material layer 20 has the positive electrode composite material 1 of the present disclosure. In the lithium ion battery 100, one or both of the electrolyte layer 30 and the negative electrode active material layer 40 may contain a solid electrolyte. In addition, in the lithium ion battery 100, all of the positive electrode active material layer 20, the electrolyte layer 30, and the negative electrode active material layer 40 may contain a solid electrolyte. Furthermore, the lithium ion battery 100 may be a solid-state battery. A solid-state battery refers to a battery in which an electrolyte having carrier ion conductivity is mainly composed of a solid electrolyte. However, a liquid component may be included in a part of the battery. Alternatively, the lithium ion battery 100 may be an all-solid-state battery that does not substantially contain a liquid component. 4, the lithium ion battery 100 may include a positive electrode current collector 10 in contact with the positive electrode active material layer 20. The lithium ion battery 100 may also include a negative electrode current collector 50 in contact with the negative electrode active material layer 40.

[0072] 3.1 Positive electrode current collector The positive electrode collector 10 may be any of those generally used as a positive electrode collector for lithium ion batteries. The positive electrode collector 10 may have at least one shape selected from a foil, a plate, a mesh, a punched metal, and a foam. The positive electrode collector 10 may be made of a metal foil or a metal mesh. In particular, a metal foil is excellent in terms of ease of handling. The positive electrode collector 10 may be made of a plurality of foils. Examples of metals constituting the positive electrode collector 10 include at least one selected from Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, V, Mg, Pb, Ge, In, Sn, Zr, and stainless steel. In particular, from the viewpoint of ensuring oxidation resistance, the positive electrode collector 10 may contain Al. The positive electrode collector 10 may have some kind of coating layer on its surface for the purpose of adjusting resistance, etc. For example, the positive electrode collector 10 may have a carbon coating layer. The positive electrode collector 10 may be a metal foil or a substrate plated or vapor-deposited with the above-mentioned metal. When the positive electrode collector 10 is made of a plurality of metal foils, some layer may be present between the plurality of metal foils. The thickness of the positive electrode collector 10 is not particularly limited. For example, it may be 0.1 μm or more and 1 mm or less, the lower limit may be 1 μm or more, and the upper limit may be 100 μm or less.

[0073] 3.2 Cathode active material layer The positive electrode active material layer 20 has the above-mentioned positive electrode composite material 1. The shape of the positive electrode active material layer 20 is not particularly limited, and may be, for example, a sheet-like positive electrode active material layer 20 having a substantially flat surface. The thickness of the positive electrode active material layer 20 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0074] The positive electrode active material layer 20 can be manufactured by applying a known method. For example, the positive electrode active material layer 20 can be easily formed by forming the positive electrode mixture 1 in a dry or wet manner. The positive electrode active material layer 20 may be formed together with the positive electrode current collector 10, or may be formed separately from the positive electrode current collector 10.

[0075] 3.3 Electrolyte layer The electrolyte layer 30 is disposed between the positive electrode active material layer 20 and the negative electrode active material layer 40. The electrolyte layer 30 includes at least an electrolyte. The electrolyte layer 30 may include one or both of a solid electrolyte and a liquid electrolyte (electrolytic solution), and may further include a binder and various additives. The content of the electrolyte and the binder in the electrolyte layer 30 is not particularly limited. Alternatively, the electrolyte layer 30 may have a separator or the like for holding the electrolytic solution and preventing contact between the positive electrode active material layer 20 and the negative electrode active material layer 40. The thickness of the electrolyte layer 30 is not particularly limited, and may be, for example, 0.1 μm or more and 2 mm or less, the lower limit may be 1 μm or more, and the upper limit may be 1 mm or less.

[0076] The electrolyte layer 30 may be composed of one layer or may be composed of multiple layers. For example, the electrolyte layer 30 may include a first layer arranged on the positive electrode active material layer 20 side and a second layer arranged on the negative electrode active material layer 40 side, and the first layer may include the first electrolyte, and the second layer may include the second electrolyte. The first electrolyte and the second electrolyte may be different from each other. The first electrolyte and the second electrolyte may each be at least one selected from the above-mentioned oxide solid electrolyte, sulfide solid electrolyte, and ionic solid electrolyte. For example, the first layer may include an ionic solid electrolyte, and the second layer may include at least one of an ionic solid electrolyte and a sulfide solid electrolyte.

[0077] The electrolyte contained in the electrolyte layer 30 may be appropriately selected from those exemplified as electrolytes that may be contained in the positive electrode active material layer 20 (solid electrolytes and / or liquid electrolytes). The binder that may be contained in the electrolyte layer 30 may also be appropriately selected from those exemplified as binders that may be contained in the positive electrode active material layer 20. Each of the electrolytes and binders may be used alone or in combination of two or more. The separator may be any separator that is normally used in secondary batteries, and examples of the separator include those made of resins such as polyethylene (PE), polypropylene (PP), polyester, and polyamide. The separator may have a single layer structure or a multilayer structure. Examples of the multilayer separator include a separator with a two-layer structure of PE / PP, or a separator with a three-layer structure of PP / PE / PP or PE / PP / PE. The separator may be made of a nonwoven fabric such as a cellulose nonwoven fabric, a resin nonwoven fabric, or a glass fiber nonwoven fabric.

[0078] 3.4 Negative electrode active material layer The negative electrode active material layer 40 includes at least a negative electrode active material. The negative electrode active material layer 40 may also include an electrolyte, a conductive assistant, a binder, various additives, and the like. The content of each component in the negative electrode active material layer 40 may be appropriately determined according to the target battery performance. For example, the content of the negative electrode active material may be 40 mass% or more, 50 mass% or more, 60 mass% or more, or 70 mass% or more, or 100 mass% or less, less than 100 mass%, 95 mass% or less, or 90 mass% or less, based on the entire solid content of the negative electrode active material layer 40 being 100 mass%. Alternatively, the negative electrode active material and optionally the electrolyte, the conductive assistant, and the binder may be included in a total amount of 85 volume% or more, 90 volume% or more, or 95 volume% or more, based on the entire negative electrode active material layer 40 being 100 volume%, and the remainder may be voids or other components. The shape of the negative electrode active material layer 40 is not particularly limited, and may be, for example, a sheet having a substantially flat surface. The thickness of the negative electrode active material layer 40 is not particularly limited, and may be, for example, 0.1 μm or more and 2 mm or less, with a lower limit of 1 μm or more, 10 μm or more, or 30 μm or more, and an upper limit of 1 mm or less, 500 μm or less, or 100 μm or less.

[0079] 3.4.1 Negative electrode active material The negative electrode active material contained in the negative electrode active material layer 40 can be any of those known as negative electrode active materials for lithium ion batteries. Of the known active materials, various materials can be used that have a potential (charge / discharge potential) at which a predetermined carrier ion is absorbed and released that is lower than the above-mentioned positive electrode active material. The negative electrode active material may be at least one selected from, for example, silicon-based active materials such as Si, Si alloys, and silicon oxide; carbon-based active materials such as graphite and hard carbon; various oxide-based active materials such as lithium titanate; metallic lithium, lithium alloys, and the like. Only one type of negative electrode active material may be used alone, or two or more types may be used in combination. The shape of the negative electrode active material may be any shape that is common as a negative electrode active material for lithium ion batteries. For example, the negative electrode active material may be in the form of particles. The negative electrode active material particles may be primary particles, or may be secondary particles formed by agglomeration of a plurality of primary particles. The average particle diameter (D50) of the negative electrode active material particles may be, for example, 1 nm or more and 500 μm or less, with a lower limit of 5 nm or more or 10 nm or more and an upper limit of 100 μm or less, 50 μm or less, or 30 μm or less. Alternatively, the negative electrode active material layer 40 may be made of a sheet-like (foil-like, film-like) active material such as lithium foil.

[0080] 3.4.2 Other The electrolyte that can be contained in the negative electrode active material layer 40 may be appropriately selected from those exemplified as the electrolyte that can be contained in the above-mentioned positive electrode active material layer 20 (solid electrolytes and / or liquid electrolytes). The conductive assistant that can be contained in the negative electrode active material layer 40 may be appropriately selected from those exemplified as the conductive assistant that can be contained in the above-mentioned positive electrode active material layer 20. The binder that can be contained in the negative electrode active material layer 40 may be appropriately selected from those exemplified as the binder that can be contained in the above-mentioned positive electrode active material layer 20. Each of the electrolyte, conductive assistant, and binder may be used alone or in combination of two or more kinds.

[0081] The negative electrode active material layer 40 may contain various additives in addition to the above-mentioned components, such as a dispersant and a lubricant.

[0082] The negative electrode active material layer 40 can be manufactured by applying a known method. For example, the negative electrode active material layer 40 can be easily formed by forming a negative electrode mixture containing the above-mentioned various components in a dry or wet manner. The negative electrode active material layer 40 may be formed together with the negative electrode current collector 50, or may be formed separately from the negative electrode current collector 50.

[0083] 3.5 Negative electrode current collector The negative electrode current collector 50 may be any of those generally used as negative electrode current collectors for lithium ion batteries. The negative electrode current collector 50 may be in the form of a foil, a plate, a mesh, a punched metal, or a foam. The negative electrode current collector 50 may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, metal foil is excellent in terms of ease of handling. The negative electrode current collector 50 may be made of a plurality of foils or sheets. Examples of metals constituting the negative electrode current collector 50 include at least one selected from Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, V, Mg, Pb, Ge, In, Sn, Zr, and stainless steel. In particular, from the viewpoint of ensuring reduction resistance and being difficult to alloy with lithium, the negative electrode current collector 50 may contain at least one metal selected from Cu, Ni, and stainless steel. The negative electrode collector 50 may have some kind of coating layer on its surface for the purpose of adjusting the resistance, etc. For example, the negative electrode collector 50 may have a carbon coating layer. The negative electrode collector 50 may be an aluminum foil having a carbon coating layer. The negative electrode collector 50 may also be a metal foil or a base material on which the above metal is plated or vapor-deposited. When the negative electrode collector 50 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the negative electrode collector 50 is not particularly limited. For example, it may be 0.1 μm or more and 1 mm or less, the lower limit may be 1 μm or more, and the upper limit may be 100 μm or less.

[0084] 3.6 Other configurations The lithium ion battery 100 may have a general configuration as a battery in addition to the above configuration. For example, a tab, a terminal, etc. The lithium ion battery 100 may have each of the above configurations housed inside an exterior body. Any known exterior body for a battery can be adopted as the exterior body. In addition, a plurality of lithium ion batteries 100 may be electrically connected and stacked in any manner to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case. The lithium ion battery 100 may have other obvious configurations such as necessary terminals. The shape of the lithium ion battery 100 may be, for example, a coin type, a laminate type, a cylindrical type, a square type, etc. The lithium ion battery 100 may be a secondary battery.

[0085] 4. Manufacturing method of lithium-ion batteries The lithium ion battery 100 can be manufactured by applying a known method. As shown in Fig. 6, the manufacturing method of the lithium ion battery 100 may include, for example, obtaining a positive electrode active material layer 20 using the positive electrode composite material 1 of the present disclosure (step S11), and obtaining a lithium ion battery 100 using the positive electrode active material layer 20, an electrolyte layer 30, and a negative electrode active material layer 40 (step S12). More specifically, for example, the lithium ion battery 100 may be manufactured as follows. However, the manufacturing method of the lithium ion battery 100 is not limited to the following method, and each layer may be formed by, for example, dry molding or the like. (1) A positive electrode mixture constituting a positive electrode active material layer is dispersed in a solvent to obtain a positive electrode slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. Thereafter, the positive electrode slurry is applied to the surface of a positive electrode current collector or an electrolyte layer described later using a doctor blade or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode current collector or the electrolyte layer, thereby forming a positive electrode. Here, the positive electrode active material layer may be press-molded. (2) The negative electrode mixture constituting the negative electrode active material layer is dispersed in a solvent to obtain a negative electrode slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. Thereafter, the negative electrode slurry is applied to the surface of the negative electrode current collector or the electrolyte layer described below using a doctor blade or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode current collector or the electrolyte layer, thereby forming a negative electrode. Here, the negative electrode active material layer may be press-molded. (3) The layers are laminated so as to sandwich the electrolyte layer between the negative electrode and the positive electrode, and a laminate having the negative electrode current collector, the negative electrode active material layer, the electrolyte layer, the positive electrode active material layer, and the positive electrode current collector in this order is obtained. The electrolyte layer may be obtained by, for example, molding an electrolyte mixture containing an electrolyte and a binder, or by press molding. Here, the laminate may be further press molded. Other members such as terminals are attached to the laminate as necessary. When an electrolytic solution is used, a separator may be used in the electrolyte layer. (4) The laminate is housed in a battery case and sealed to obtain a lithium-ion battery.

[0086] 5. How to increase the capacity of a lithium-ion battery The technology of the present disclosure also has an aspect of being a method for increasing the capacity of a lithium ion battery. That is, the method for increasing the capacity of a lithium ion battery of the present disclosure is characterized by using the positive electrode mixture of the present disclosure as a material constituting a positive electrode active material layer of the lithium ion battery.

[0087] 6. Vehicles equipped with lithium-ion secondary batteries As described above, when the positive electrode active material layer of a lithium ion battery is formed using the positive electrode composite of the present disclosure, an increase in the capacity of the lithium ion battery can be expected. Such a lithium ion battery can be suitably used in at least one vehicle selected from, for example, a hybrid vehicle (HEV), a plug-in hybrid vehicle (PHEV), and an electric vehicle (BEV). That is, the technology of the present disclosure also has an aspect of a vehicle having a lithium ion battery, the lithium ion battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, and the positive electrode active material layer having the positive electrode composite of the present disclosure. EXAMPLES

[0088] As described above, one embodiment of the positive electrode composite, the lithium ion secondary battery, and the manufacturing method thereof of the present disclosure has been described, but the technology of the present disclosure can be modified in various ways other than the above embodiment without departing from the gist of the technology. Below, the technology of the present disclosure will be described in more detail while showing examples, but the technology of the present disclosure is not limited to the following examples.

[0089] 1. Preparation of Precursor Particles MnSO4·5H2O, NiSO4·6H2O and CoSO4·7H2O were weighed out to obtain the desired composition ratio, and dissolved in distilled water to a concentration of 1.2 mol / L to obtain the first liquid. In a separate container, Na2CO3 was dissolved in distilled water to a concentration of 1.2 mol / L to obtain the second liquid. Next, 500 mL of the first and second liquids were dropped at a rate of about 4 mL / min into a reaction container that had already contained 1000 mL of pure water. After the dropwise addition, the mixture was stirred at room temperature for 1 h at a stirring speed of 150 rpm. The precipitate was washed with pure water and separated into solid and liquid using a centrifuge. The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and fine particles were removed by air classification to obtain mixed salt particles (precursor particles) containing Mn, Ni and Co. The precursor particles were spherical particles with a circularity of 0.98.

[0090] 2. Preparation of Na-containing transition metal oxide particles with P2-type structure 2.1 First P2-type platelet particles Na2CO3 and the above precursor particles were mixed with Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 The mixture was weighed in a dry atmosphere so as to have a composition of 02 and mixed in a mortar to obtain a mixture. The mixture was fired in an electric furnace using an alumina crucible in an air atmosphere. Specifically, the mixture was subjected to the "first heating step", "pre-firing step", "second heating step", "main firing step", "in-furnace cooling step" and "out-furnace cooling step" as shown in Table 1 below. The "in-furnace cooling step" refers to a cooling step in an electric furnace, and the "out-furnace cooling step" refers to a step of cooling in the air outside the electric furnace. Thereafter, the mixture was pulverized in a mortar in a dry atmosphere to obtain a Na-containing transition metal oxide (Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 The Na-containing transition metal oxide was a plate-like particle having an aspect ratio (major axis / minor axis) of 2.0 or more in a cross section along the thickness direction.

[0091] [Table 1]

[0092] 2.2 Second P2-type platelet particles The mixture was fired under the same conditions as the first plate-like particles, except that the heating time in the second heating step was 70 minutes, the end temperature was 950°C, the start and end temperatures in the firing step were 950°C, and the start temperature in the furnace cooling step was 950°C and the cooling time was 140 minutes. Thereafter, the mixture was pulverized in a mortar in a dry atmosphere to obtain a Na-containing transition metal oxide (Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 The Na-containing transition metal oxide was a plate-like particle having an aspect ratio (major axis / minor axis) of 2.0 or more in a cross section along the thickness direction.

[0093] 2.3 Spherical P2 type particles After weighing out Na2CO3 and distilled water so that the total amount was 1150 g / L, the mixture was stirred with a stirrer until completely dissolved to prepare an aqueous Na2CO3 solution. The above precursor particles were mixed into the aqueous Na2CO3 solution to prepare a slurry. The Na2CO3 and the above precursor particles were dried and then mixed with Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 The mixture was mixed so as to have a composition of 0.02. The obtained slurry was dried by spray drying. Specifically, a DL410 spray dryer was used, with a slurry delivery rate of 30 mL / min, an inlet temperature of 200°C, and a circulating air volume of 0.8 m 3 At a spray air pressure of 0.3 MPa, 77% by area of ​​the surface of the precursor particles was coated with Na2CO3 to obtain coated particles.

[0094] The coated particles were sintered in an electric furnace using an alumina crucible in an air atmosphere. Specifically, the coated particles were subjected to the "first heating step", "pre-firing step", "second heating step", "main firing step", "in-furnace cooling step" and "out-furnace cooling step" as shown in Table 2 and FIG. 7 below. Thereafter, the particles were pulverized in a mortar in a dry atmosphere to obtain a Na-containing transition metal oxide (Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 O2) was obtained. The Na-containing transition metal oxide was in the form of spherical particles.

[0095] [Table 2]

[0096] 3. Preparation of active material with O2 structure LiNO3 and LiCl were weighed out to a molar ratio of 50:50, and mixed with P2-type plate-like particles or P2-type spherical particles in a molar ratio that was 10 times the minimum Li amount required for ion exchange to obtain a mixture. The mixture was fired at 280°C for 1 hour in an air atmosphere using an alumina crucible to obtain a fired product. The salt remaining in the fired product was washed with pure water, and solid-liquid separation was performed by vacuum filtration to obtain a second precipitate. The second precipitate was dried overnight at 120°C to obtain positive electrode active material particles having an O2 structure.

[0097] In the case where the first P2 type plate-like particles are used, the positive electrode active material particles have an O2 type structure, and in the cross-sectional shape along the thickness direction, the aspect ratio of the major axis to the minor axis (major axis / minor axis) is 3.1, and the major axis D 1L The first O2 type plate-like particles having a diameter of 2.9 μm were obtained.

[0098] In the case where the second P2 type plate-like particles are used, the positive electrode active material particles have an O2 type structure, and in the cross-sectional shape along the thickness direction, the aspect ratio of the major axis to the minor axis (major axis / minor axis) is 3.2, and the major axis D 1L Secondary O2 type platelet particles were obtained having a diameter of 4.1 μm.

[0099] When spherical P2 type particles were used, spherical O2 type particles having a circularity of 0.85 and a diameter D2 of 2.3 μm were obtained as positive electrode active material particles having an O2 type structure.

[0100] The plate-shaped O2 type positive electrode active material particles were substantially composed of one crystallite. On the other hand, the surface of the spherical O2 type positive electrode active material particles was composed of multiple crystallites, and the diameter of the crystallites was less than 1 μm. The crystallites had a first surface exposed on the particle surface, and the first surface was flat. Furthermore, elemental analysis showed that both the plate-shaped O2 type positive electrode active material particles and the spherical O2 type positive electrode active material particles contained Li 0.63 Mn 0.5 Ni 0.2 Co 0.3It was confirmed that the positive electrode active material particles had a chemical composition represented by O2. Figures 8A and 8B show SEM images of the appearance of the positive electrode active material particles. Figure 8A shows a plate-shaped O2 type positive electrode active material particle, and Figure 8B shows a spherical O2 type positive electrode active material particle.

[0101] 4. Preparation of Evaluation Cell The above O2 type positive electrode active material particles, sulfide solid electrolyte A (Argyrodite type sulfide solid electrolyte), PVDF, and VGCF were weighed and mixed in a ratio of O2 type positive electrode active material particles:sulfide solid electrolyte A:PVDF:VGCF=82.1:14.9:0.6:2.4 (mass ratio) to obtain a positive electrode composite. 15 Si4 and Si alone), sulfide solid electrolyte B (Li2S-P2S5-LiI-LiBr), PVDF, and VGCF, 15 S4: Si simple substance: sulfide solid electrolyte B: PVDF: VGCF = 30.5: 50.7: 15.5: 0.9: 2.4 (mass ratio) was weighed and mixed to obtain a negative electrode composite. In addition, sulfide solid electrolyte B and acrylate butadiene rubber (ABR) were weighed and mixed to obtain sulfide solid electrolyte B: ABR = 99.4: 0.6 (mass ratio) to obtain an electrolyte composite. The above electrolyte composite was placed in a Macol cylinder and pressed at 9.8 kN for 1 minute to form an electrolyte layer. Then, the above positive electrode composite was placed on one side of the electrolyte layer and pressed at 19.6 kN for 1 minute to form a positive electrode active material layer. Then, the above negative electrode composite was placed on the other side of the electrolyte layer and pressed at 58 kN for 3 minutes to form a negative electrode active material layer. Finally, a current collector was placed on both ends of the stacking direction of each layer to obtain an evaluation cell.

[0102] 2.1 Example 1 As the O2 type positive electrode active material, a mixture of the first O2 type plate-like particles and the spherical O2 type particles in a plate-like:spherical ratio of 80:20 (mass ratio) was used. The major axis D of the first O2 type plate-like particles 1L and the diameter D2 of the spherical O2-type particle 1L / D2 was 1.26.

[0103] 2.2 Example 2 As the O2 type positive electrode active material, a mixture of the first O2 type plate-like particles and the spherical O2 type particles in a plate-like:spherical ratio of 20:80 (mass ratio) was used. The major axis D of the first O2 type plate-like particles 1L and the diameter D2 of the spherical O2-type particle 1L / D2 was 1.26.

[0104] 2.3 Comparative Example 1 As the O2 type positive electrode active material, a mixture of second O2 type plate-like particles and spherical O2 type particles in a plate-like:spherical ratio of 80:20 (mass ratio) was used. The major axis D of the second O2 type plate-like particles 1L and the diameter D2 of the spherical O2-type particle 1L / D2 was 1.78.

[0105] 2.4 Comparative Example 2 As the O2-type positive electrode active material, only spherical O2-type particles were used.

[0106] 2.5 Comparative Example 3 As the O2 type positive electrode active material, only the first O2 type plate-like particles were used.

[0107] 3. Evaluation conditions The above evaluation cell was charged and discharged in a thermostatic chamber maintained at 25° C. at a voltage range of 1.8-4.6 V and a 0.1 C rate (1 C=220 mA / g) to measure the discharge capacity. The results are shown in Table 3 below and FIG. 9.

[0108] [Table 3]

[0109] 4. Cross-section observation A cross section of the positive electrode active material layer of the evaluation cell taken along the thickness direction of the layer was observed by SEM, and the results are shown in Figures 10A to 10E.

[0110] 5. Evaluation Results As shown in Table 2 and FIG. 9, the cells according to Examples 1 and 2 obtained high discharge capacities. In particular, the cell according to Example 1 had a remarkably high discharge capacity. This is believed to be due to the following mechanism. First, the plate-shaped O2-type active material (first active material) has an inlet and outlet for intercalation at its end. Therefore, when a positive electrode active material layer is formed using a plate-shaped O2-type active material, it is preferable that the plate surface of the plate-shaped O2-type active material in the positive electrode active material layer intersects (preferably perpendicular to) the surface direction of the positive electrode active material layer. However, when a positive electrode active material layer is formed using only a plate-shaped O2-type active material as the positive electrode active material, the plate surface of the plate-shaped O2-type active material is aligned with the surface direction of the positive electrode (FIG. 10E, Comparative Example 3). Therefore, the capacity is likely to decrease due to an increase in the degree of bending, a decrease in the utilization rate of the plate-shaped O2-type active material, and the like. Even when a spherical O2-type active material is used together with a plate-shaped O2-type active material, the size of the spherical O2-type active material is small (D 1L When the ratio of D to D2 exceeds 1.5, this problem is not solved (FIG. 10C, Comparative Example 1). In contrast, when a spherical O2 type active material is used together with a plate-shaped O2 type active material and the size of the spherical O2 type active material is large (D 1L By setting the ratio of the diameter of the plate-shaped O2-type active material to the diameter of the plate-shaped O2-type active material (R / D2 is 1.5 or less), the plate-shaped O2-type active material can be raised by the spherical O2-type active material, and the orientation of the plate surface of the plate-shaped O2-type active material can be easily randomized (FIGS. 10A and 10B, Examples 1 and 2). That is, it is considered that the capacity is increased due to an increase in the amount of the plate-shaped O2-type active material intersecting with the surface direction of the positive electrode active material layer, a reduction in the degree of bending, and an increase in the utilization rate of the plate-shaped O2-type active material. It is also considered that the spherical O2-type active material itself can contribute to the improvement of the capacity, which further increases the capacity.

[0111] 6. Supplementary Information In the above examples, the positive electrode active material particles having a specific chemical composition are illustrated, but the chemical composition of the positive electrode active material particles of the present disclosure is not limited thereto. However, according to the knowledge of the present inventor, when the transition metal contains at least one of Mn, Ni, and Co, the P2 type structure crystal grows in a specific direction to become plate-like, and the O2 type particles finally obtained are also likely to become plate-like. It can be said that the problem solved by the technology of the present disclosure is particularly prominent when the transition metal contains at least one of Mn, Ni, and Co.

[0112] 7. Summary From the above examples, when a positive electrode active material layer of a lithium ion battery is formed using a positive electrode mixture having the following configurations (1) to (5), the capacity of the lithium ion battery is likely to be improved. (1) A positive electrode mixture comprising a first active material and a second active material. (2) The first active material has an O2 type structure and is plate-shaped. (3) The second active material has an O2 type structure and is spherical. (4) The major axis D of the first active material 1L and the diameter D2 of the second active material 1L / D2 is greater than or equal to 0.1 and less than or equal to 1.5. (5) The proportion of the first active material with respect to the total of the first active material and the second active material is 10% by mass or more and 90% by mass or less. [Explanation of symbols]

[0113] 1 Positive electrode mixture 1a First active material 1b Second active material 100 Lithium-ion batteries 10 Positive electrode current collector 20 Cathode active material layer 30 Electrolyte layer 40 Negative electrode active material layer 50 Negative electrode current collector

Claims

1. a positive electrode mixture comprising a first active material and a second active material; The first active material has an O2 structure and is plate-shaped, The second active material has an O2 structure and is spherical, The major axis D of the first active material 1L and the diameter D of the second active material 2 Compared to D 1L / D 2 is equal to or greater than 0.1 and equal to or less than 1.5, A ratio of the first active material to a total of the first active material and the second active material is 10% by mass or more and 90% by mass or less. Positive electrode mixture.

2. The positive electrode mixture according to claim 1 , The surface of the second active material has a plurality of crystallites. Positive electrode mixture.

3. The positive electrode mixture according to claim 1 , Including solid electrolytes, Positive electrode mixture.

4. The positive electrode mixture according to claim 1 , Containing one or both of a conductive assistant and a binder; Positive electrode mixture.

5. A lithium ion battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The positive electrode active material layer comprises the positive electrode mixture according to any one of claims 1 to 4. Lithium-ion battery.

6. 6. The lithium ion battery of claim 5, One or both of the electrolyte layer and the negative electrode active material layer contain a solid electrolyte. Lithium-ion battery.

7. A method for manufacturing a lithium ion battery, comprising: Obtaining a positive electrode active material layer using the positive electrode mixture according to any one of claims 1 to 4; and obtaining a lithium ion battery using the positive electrode active material layer, the electrolyte layer, and the negative electrode active material layer; A manufacturing method comprising:

Citation Information

Patent Citations

  • Electrode for all solid lithium secondary battery and all solid lithium secondary battery

    JP2008176981A

  • All-solid-state battery

    JP2022085829A

  • Positive electrode active material for secondary battery, and secondary battery

    WO2021085112A1

  • All-solid battery

    JP2019169365A