Granular carrier, granular medicine composition and absorbent article including the same and granular carrier production method

The reverse-phase suspension polymerization of carboxyalkyl cellulose salts in low-polarity solvents addresses shape and air flow issues in cellulose-based superabsorbent polymers, enhancing drug efficacy and reducing environmental impact.

JP2024148014APending Publication Date: 2024-10-17S T CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023060871
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional cellulose-based superabsorbent polymers used in gel formulations for stationary products have irregular shapes, poor air flow, and aesthetic issues, leading to inefficient drug volatilization and deodorization, and high environmental impact due to non-biodegradability.

Method used

A method involving reverse-phase suspension polymerization of carboxyalkyl cellulose salts in a low-polarity organic solvent to produce spherical, uniformly sized, and strong gel particles with reduced syneresis, using specific viscosity and crosslinking agents to enhance water absorption and biodegradability.

Benefits of technology

The method produces granular carriers with improved water absorption, biodegradability, and aesthetic appeal, ensuring efficient drug release and reduced environmental footprint.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148014000001_ABST
    Figure 2024148014000001_ABST
Patent Text Reader

Abstract

To provide a technique for producing a granular carrier which has both of high water absorptive property and bio-degradability, the granular carrier having a substantially spherical shape, uniform particle size, and is excellent in water separation suppression ability due to passing of time, and intensity and transparency.SOLUTION: There is provided a production method of granular carrier which is formed of gel particles including a cross linking body of carboxyalkyl cellulose salt, the production method comprising: a step for dissolving in an alkali aqueous solution, specific carboxyalkyl cellulose and / or a salt thereof, for preparing the carboxyalkyl cellulose salt solution; adjusting a mixture of the carboxyalkyl cellulose salt solution and a cross linking agent; dispersing the mixture in a specific low polarity organic solvent for forming suspension, advancing cross linkage and polymerization of the carboxyalkyl cellulose salt in the suspension, for forming dispersed particles formed of the gel particles including the cross linking body of the carboxyalkyl cellulose salt; filtering gel particles from the suspension; and warming the filtered gel particles.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a granular carrier, a granular pharmaceutical composition and an absorbent article containing the same, and a method for producing the granular carrier. [Background technology]

[0002] Superabsorbent polymers (SAP) absorb water upon contact with water and instantly become a transparent hydrated gel. This gel is one of the functional polymers that does not release water even when pressure is applied and retains water. Superabsorbent polymers have a wide range of uses, for example, in the field of sanitary products, they are used as highly absorbent substances in absorbent articles such as paper diapers and sanitary napkins for women. In addition, superabsorbent polymers are also used as carriers in gel preparations that absorb and support aqueous liquid compositions containing pharmaceuticals such as fragrances and deodorants. Gel preparations containing carriers made of such superabsorbent polymers are widely used in stationary air fresheners and deodorants because there is no risk of liquid spilling from the container and they have excellent design.

[0003] Currently, polyacrylic acid-based SAP is the mainstream of superabsorbent polymers (SAPs) from the viewpoints of ease of synthesis, cost, etc. However, because polyacrylic acid-based SAPs are made from petroleum, there is a problem that the production cost is affected by fluctuations and increases in crude oil prices, and the amount of CO emitted during production and disposal is also high. 2 In particular, when used for diapers, SAP is disposed of in a water-absorbed state, so incineration of acrylic acid-based SAP requires a large amount of energy and emits CO 2 In addition, when acrylic acid-based SAP is disposed of in landfills, problems such as soil contamination arise because it is not biodegradable.

[0004] The fact that polyacrylic acid-based SAPs are the mainstream of superabsorbent polymers (SAPs) may be a cause of environmental problems. As the demand for disposable diapers is expected to rapidly increase in emerging countries in the future, it is desirable to use biodegradable natural polymers as superabsorbent polymers. In this situation, superabsorbent polymers using plant-derived raw materials such as polysaccharides have been proposed.

[0005] For example, Patent Documents 1 to 3 propose a cellulose-based SAP consisting of a crosslinked polymer of carboxymethyl cellulose (CMC) or a CMC salt as a biodegradable, highly water-absorbent polymer to replace polyacrylic acid-based SAP. This CMC is a water-soluble cellulose derivative, and is synthesized by etherifying the hydroxyl groups of cellulose with chloroacetic acid or the like. Its aqueous solution exhibits anionic properties and has high viscosity and excellent dispersibility, and is therefore widely used as a thickener, dispersant, and stabilizer.

[0006] CMC is neither toxic nor allergenic, and is also used as a food additive and a pharmaceutical binder. Its physical properties depend strongly on the degree of substitution (DS), which is the average number of carboxymethyl groups substituted per glucose residue, and in one example, it is said to be water-soluble when DS>0.55. For example, Patent Document 1 uses CMC and CMC salts with a degree of substitution of 1.1 or more (see Claim 1, etc.), and Patent Document 2 uses CMC salts with a degree of substitution of 0.65 to 1.4 (see Claim 1, etc.). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2011-140534 A [Patent Document 2] International Publication No. 2012 / 147255 [Patent Document 3] JP 2008-285611 A Summary of the Invention [Problem to be solved by the invention]

[0008] Stationary products in which gel preparations such as fragrance compositions and deodorant compositions are filled in containers are on the market. Many of these products use granular gel preparations in which liquid compositions containing various chemicals are supported on gel carriers made of highly water-absorbent polymers. Many of these products are designed to have the surface of the granular gel preparation exposed to air to exert the functions of the various chemicals supported on the gel carriers. That is, when the chemical supported on the gel carrier is a volatile chemical such as a fragrance, the surface of the granular gel preparation is exposed to air to volatilize the volatile chemical. Also, when the chemical supported on the gel carrier is a non-volatile chemical, for example, a deodorant that uses a chemical reaction to deodorize, the surface of the granular gel preparation is exposed to air to bring the malodorous molecules into contact with the non-volatile deodorant, and the malodorous molecules are decomposed by a chemical reaction to deodorize.

[0009] Therefore, in order to make the drug carried by the gel carrier in the granular gel preparation function efficiently, it is desirable that air flow easily occurs when the granular gel preparation is filled in a container. In order to make air flow easily, it is preferable that the gaps between the granular gel preparations are uniform and have a certain size. Therefore, it is desirable that the granular gel preparations are uniform in size and have a shape close to a sphere. From the viewpoint of making the drug function efficiently, it is also important that the water separation rate over time is low. When the gel particles are immersed in a water-separating liquid, the area of ​​the gel particles that contacts the air is reduced, so that the volatilization efficiency of the volatile drug is reduced, and the contact efficiency with the malodorous molecules of the non-volatile drug is reduced.

[0010] In addition, considering that the granular gel preparation is distributed as a stationary product filled in a container, it is desirable that the granular gel preparation also has excellent gel strength. Furthermore, in such stationary products, the granular gel preparation is filled in a transparent or semitransparent container and is often in a form that can be seen from the outside. The fact that the granular gel preparation has a uniform size and a nearly spherical shape is preferable from the viewpoint of aesthetics as well as enabling the above-mentioned drug to function efficiently.

[0011] From the viewpoint of aesthetics, it is also important that the granular gel preparation has excellent transparency and exhibits little syneresis over time.

[0012] On the other hand, as a conventional method for producing cellulose-based SAP, a method of polymerizing CMC and / or a CMC salt in an aqueous solution using a crosslinking agent (hereinafter referred to as "aqueous solution polymerization") is known. For example, a crosslinking agent is added to a CMC salt aqueous solution in which CMC or a CMC salt is dissolved in a sodium hydroxide aqueous solution, and a crosslinking reaction is carried out to obtain a hydrogel in which the aqueous solution is uniformly gelled. The hydrogel is pulverized and undergoes a sorting process such as classification to form a cellulose-based SAP (for example, see paragraph 0035 of Patent Document 1, paragraph 0024 of Patent Document 2, and paragraph 0044 of Patent Document 3).

[0013] Crushed gel particles (crushed gel) finely granulated by crushing are typically fragmented with sharp edges, and most of them are irregularly shaped particles that are difficult to call spherical. When such cellulose-based SAP consisting of a collection of small, non-spherical, non-uniform gel fragments is filled in a container, the gel particles are in close contact with each other, making it difficult for air to flow. In addition, cellulose-based SAP consisting of a collection of such non-uniform small gel fragments is not preferable from the viewpoint of aesthetics.

[0014] The present invention aims to provide a technology for producing a granular carrier that combines high water absorbency and biodegradability, has a roughly spherical shape, uniform particle size, and excellent strength and ability to inhibit water separation over time. [Means for solving the problem]

[0015] According to one aspect of the present invention, there is provided a method for producing a granular carrier comprising gel particles containing a crosslinked product of a carboxyalkyl cellulose salt, comprising the steps of: preparing a carboxyalkyl cellulose salt aqueous solution by dissolving a carboxyalkyl cellulose and / or a salt thereof having a viscosity of 5 mPa·s or more and 300 mPa·s or less in a 1 mass% aqueous solution at 25°C in an alkaline aqueous solution; preparing a mixture of the aqueous carboxyalkyl cellulose salt and a crosslinking agent; dispersing the mixture in a low-polarity organic solvent to form a suspension, and proceeding with crosslinking polymerization of the carboxyalkyl cellulose salt in the suspension to form dispersed particles consisting of gel particles containing a crosslinked body of the carboxyalkyl cellulose salt; filtering the gel particles from the suspension; and Heating the gel particles that have been filtered out The low-polarity organic solvent has a relative dielectric constant of 10 or less at 25° C. and a kinetic viscosity of 10 mm at 37.8° C. 2 / s or more.

[0016] According to another aspect of the present invention, there is provided a method according to the above aspect, wherein the gel particles are heated at a temperature in the range of 40° C. to 110° C. for a period of 40 minutes to 24 hours.

[0017] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, further comprising washing the gel particles and / or cleaning the gel particles between filtering out the gel particles and heating the gel particles.

[0018] According to yet another aspect of the present invention, there is provided the production method according to any one of the above aspects, wherein the low-polarity organic solvent is liquid paraffin or silicone oil.

[0019] According to yet another aspect of the present invention, the low-polarity organic solvent has a kinetic viscosity of 10 mm at 37.8° C. 2 / s or more 100mm 2 / s or less.

[0020] According to yet another aspect of the present invention, there is provided a production method according to any of the above aspects, in which the cross-linking polymerization of the carboxyalkyl cellulose salt in the suspension is carried out under stirring at a rotation speed of 50 rpm or more and 500 rpm or less.

[0021] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the viscosity of the carboxyalkyl cellulose and / or salt thereof is 5 mPa·s or more and 100 mPa·s or less.

[0022] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the mass ratio (X / Y) of the carboxyalkyl cellulose and / or salt thereof (X) to the crosslinking agent (Y) in the mixture is in the range of 10 / 2 to 10 / 5.

[0023] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the crosslinking agent is a compound having two or more epoxy groups in the molecule.

[0024] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the granular carrier is used for carrying a drug.

[0025] According to yet another aspect of the present invention there is provided a method according to any of the above aspects, wherein the granular carrier is used as a water-absorbing material in an absorbent article.

[0026] According to yet another aspect of the present invention, there is provided a granular carrier consisting of gel particles containing a crosslinked salt of carboxyalkyl cellulose, wherein the carboxyalkyl cellulose is a carboxyalkyl cellulose having a viscosity of 5 mPa·s or more and 300 mPa·s or less in a 1 mass% aqueous solution at 25°C, and the gel particles are dry gel particles derived from dispersed particles in a reverse phase suspension, and the dry gel particles are saturated with water and the water separation rate when allowed to stand at 24°C for 96 hours is 10.5 mass% or less.

[0027] According to yet another aspect of the present invention, there is provided a granular carrier according to the above aspect, which is used for carrying a drug.

[0028] According to yet another aspect of the present invention, there is provided a granular drug composition comprising a granular carrier according to any of the above aspects and a liquid composition supported on the granular carrier and containing at least one drug selected from drugs having aromatic, deodorizing, odor eliminating, insect repellent, insecticidal or antifungal properties.

[0029] According to yet another aspect of the present invention, there is provided a granular pharmaceutical composition according to the above aspect, which is an air freshener composition or a deodorant composition.

[0030] According to yet another aspect of the present invention there is provided an absorbent article comprising a granular carrier according to any of the above aspects. Effect of the Invention

[0031] According to the present invention, a technology is provided for producing a granular carrier that combines high water absorption and biodegradability, has a roughly spherical shape, uniform particle size, and excellent strength and ability to inhibit water separation over time. [Brief description of the drawings]

[0032] [Figure 1] FIG. 1 is a flow diagram showing an example of a method for producing a granular carrier according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a photograph showing the water absorption state (water-absorbed gel particles) of each granular carrier produced in [Example]. [Diagram 3] FIG. 3 is a photograph showing the state of water release after 96 hours at 24° C. from the state in which each of the granular carriers produced in the [Examples] was saturated with water. [Figure 4] FIG. 4(a) is a photograph of the pulverized gel particles (in a dry state) produced in Comparative Example 2, and (b) is a photograph of the gel particles (in a dry state) of the granular carrier produced in Reference Example 1. [Diagram 5]FIG. 5(a) is a photograph of the water absorption state of the pulverized gel particles produced in Comparative Example 2, and (b) is a photograph of the water absorption state of the granular carrier produced in Reference Example 1 (water-absorbed gel particles). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. The preferred embodiments described below are embodiments in which any of the above aspects are more specifically embodied.

[0034] The granular carrier according to an embodiment of the present invention is a gel particle containing a crosslinked body of a carboxyalkyl cellulose salt, and is a gel particle derived from dispersed particles formed by suspension polymerization (i.e., reversed-phase suspension polymerization) in a suspension using a low-polarity organic solvent as a dispersion medium, as described below. The granular carrier derived from dispersed particles obtained through the formation of a crosslinked body of a carboxyalkyl cellulose salt by reversed-phase suspension polymerization has a substantially spherical shape, a uniform particle size, and excellent strength. According to the manufacturing method according to an embodiment of the present invention, a granular carrier having such characteristics can be easily obtained without going through the steps of crushing the gel body, classifying, etc., in the above-mentioned conventional manufacturing method.

[0035] In an embodiment of the present invention, the carboxyalkyl cellulose or its salt as the raw material is preferably a carboxyalkyl cellulose or its salt having an alkyl group having 1 to 3 carbon atoms, for example, from the viewpoint of production costs, etc., and specific examples thereof include carboxymethyl cellulose, carboxyethyl cellulose, carboxybutyl cellulose, or salts thereof. The carboxyalkyl cellulose and / or its salt may be used alone or in combination of two or more.

[0036] In an embodiment of the present invention, it is important to select carboxyalkyl cellulose and / or its salt as the raw material, which has a viscosity of 1% by mass aqueous solution within a predetermined range. The longer the polymer chain of carboxyalkyl cellulose, the higher the viscosity when dissolved, and the worse the handling property when injected into the low-polarity organic solvent, which is the dispersion medium. As a result, there is a possibility that the uniformity of the particle shape and particle size of the obtained granular carrier may be adversely affected. On the other hand, the longer the polymer chain of carboxyalkyl cellulose, the higher the water absorption amount, which means that when the granular carrier according to this embodiment is used as a drug carrier, it can carry a large amount of drug. However, if the water absorption amount becomes too large, problems such as a decrease in gel strength and an increase in water separation may occur. From these points of view, in an embodiment of the present invention, carboxyalkyl cellulose and / or its salt is used, which has a viscosity of 5 mPa·s to 300 mPa·s in a 1% by mass aqueous solution.

[0037] Here, the viscosity of a 1% by mass aqueous solution of carboxyalkyl cellulose and / or a salt thereof is the viscosity value measured by a B-type viscometer after preparing a 200 mL aqueous solution of carboxyalkyl cellulose so that the solid content is 1% by mass. Hereinafter, the viscosity of a 1% by mass aqueous solution of carboxyalkyl cellulose and / or a salt thereof measured under these conditions will be simply referred to as the "viscosity of carboxyalkyl cellulose." The viscosity of carboxyalkyl cellulose is preferably 10 mPa·s or more and 100 mPa·s or less, more preferably 20 mPa·s or more and 50 mPa·s or less.

[0038] In an embodiment of the present invention, the average degree of etherification (average degree of substitution, DS) of the raw carboxyalkyl cellulose may be, for example, 0.5 to 1.5. By using a carboxyalkyl cellulose having an average degree of etherification in this range, the water absorption and strength of the gel can be easily improved. The average degree of etherification (average degree of substitution) is the average of the degrees of substitution of hydroxyl groups at the 2-, 3-, and 6-positions of the glucose units constituting the cellulose.

[0039] Fig. 1 is a flow diagram showing an example of a method for producing a granular carrier according to an embodiment of the present invention. The production method shown in Fig. 1 includes a step S1 of dissolving carboxyalkyl cellulose and / or its salt in an alkaline aqueous solution to prepare a carboxyalkyl cellulose salt aqueous solution, a step S2 of preparing a mixture of the carboxyalkyl cellulose salt aqueous solution obtained in step S1 and a crosslinking agent, a step S3 of dispersing the mixture obtained in step S2 in a low-polarity organic solvent to form a suspension (reverse phase suspension), and proceeding with crosslinking polymerization of the carboxyalkyl cellulose salt in this suspension to form dispersed particles consisting of gel particles containing a crosslinked body of the carboxyalkyl cellulose salt, and a step S4 of filtering the dispersed particles consisting of the gel particles formed in step S3 from the suspension, and washing, drying, and heating the filtered gel particles.

[0040] As described above, the manufacturing method shown in Fig. 1 is one example. In other examples, the manufacturing method according to the embodiment of the present invention may further include other steps not shown in Fig. 1. In addition, in step S4 shown in Fig. 1, the cleaning step and drying step can be omitted, as described later.

[0041] In step S1, carboxyalkyl cellulose and / or its salt are added (injected) into the aqueous alkali solution and completely dissolved under stirring at room temperature to prepare an aqueous carboxyalkyl cellulose salt solution. In step S1, the time required to prepare the aqueous carboxyalkyl cellulose salt solution can be appropriately set, but according to one example, it can be 1 to 5 hours. After adding the carboxyalkyl cellulose to the aqueous alkali solution, a defoaming treatment can be performed by reducing pressure or by leaving it at normal pressure for a predetermined time, as necessary.

[0042] The carboxyalkyl cellulose and / or salt thereof used in step S1 may be one obtained by using cellulose such as pulp as a starting material and carboxyalkylating it in a conventional manner, or a commercially available carboxyalkyl cellulose and / or salt thereof may be used.

[0043] The carboxyalkylcellulose salt contained in the carboxyalkylcellulose salt aqueous solution obtained in step S1 may be, for example, an alkali metal salt or an alkaline earth metal salt of carboxyalkylcellulose, and in this case, an alkali aqueous solution containing an alkali metal or an alkaline earth metal is used as the alkali aqueous solution to which carboxyalkylcellulose and / or its salt is added. Examples of carboxyalkylcellulose salt include sodium salt, potassium salt, or calcium salt. In this case, an aqueous solution of sodium hydroxide, potassium hydroxide, or calcium hydroxide is used as the alkali aqueous solution to which carboxyalkylcellulose is added. According to one example, sodium carboxymethylcellulose (CMC-Na) is used as the carboxyalkylcellulose and / or its salt, and sodium hydroxide is used as the alkali aqueous solution to prepare a CMC-Na aqueous solution in step S1.

[0044] In step S2, the carboxyalkyl cellulose salt aqueous solution obtained in step S1 is mixed with a crosslinking agent to prepare a mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent. Hereinafter, when the term "mixture" is used simply, this refers to the mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent prepared in step S2.

[0045] The mixing of the aqueous carboxyalkyl cellulose salt solution and the crosslinking agent is preferably carried out at 10°C to 80°C, more preferably 20°C to 50°C, using, for example, a static mixer. If the temperature is higher than 80°C, the crosslinking reaction proceeds quickly, and it tends to be difficult to obtain uniform spherical gel particles in the next step S3. If the temperature is lower than 10°C, the viscosity of the mixture increases, and the handling properties when the mixture is added to the low-polarity organic solvent in the next step S3 tend to deteriorate. Immediately after the crosslinking agent is added to the aqueous carboxyalkyl cellulose salt solution in step S2, the crosslinking reaction of the carboxyalkyl cellulose salt starts, and the viscosity begins to increase. Therefore, from the viewpoint of handling properties when the mixture is added to the low-polarity organic solvent in the next step S3, the time from adding the crosslinking agent to the aqueous carboxyalkyl cellulose salt solution to adding the mixture to the low-polarity organic solvent can be appropriately set. According to one example, the reaction temperature can be adjusted within the above range and within 30 minutes as a guideline. After stirring, a degassing operation under reduced pressure may be performed as necessary.

[0046] The crosslinking agent used in the production method according to the embodiment of the present invention is not particularly limited, and known compounds such as polyepoxy compounds, polyglycidyl compounds, polyaldehyde compounds, polycarboxylic acids, vinyl ether compounds, methylol compounds, polyisocyanates, polyoxazoline compounds, polyvinyl compounds, polyacrylate compounds, polymethacrylate compounds, polyhalogen compounds, methylene bisacrylamide, epichlorohydrin, polyacid anhydrides, citric acid, methylene bisacrylamide, and glycidyl methacrylate can be used.

[0047] Preferred specific examples of the crosslinking agent include (a) a compound having two or more hydroxyl groups in the molecule, (b) a compound having two or more polymerizable double bonds, and (c) a compound having two or more epoxy groups.

[0048] (a) Examples of compounds having two or more hydroxyl groups in the molecule include ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, glycerin, polyglycerin, propylene glycol, diethanolamine, polyoxypropylene, sorbitan fatty acid esters, trimethylolpropane, pentaerythritol, 1,3-propanediol, and sorbitol.

[0049] (b) Examples of compounds having two or more polymerizable double bonds in the molecule include bis(meth)acrylamide, allyl(meth)acrylamide, diethylene glycol diacrylate, trimethylolpropane triacrylate, polyethylene glycol diacrylate, and ethoxylated trimethylolpropane triacrylate.

[0050] (c) Examples of compounds having two or more epoxy groups in the molecule include polyglycidyl ethers such as ethylene glycol diglycidyl ether (EGDE), polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerin triglycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, sorbitol polyglycidyl ether, pentaerythritol polyglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, and hydrogenated bisphenol A diglycidyl ether.

[0051] Among these, from the viewpoints of reactivity and the water absorption performance of the resulting granular carrier, (b) a compound having two or more polymerizable double bonds in its molecule, and (c) a compound having two or more epoxy groups in its molecule are preferred, (c) a compound having two or more epoxy groups in its molecule is more preferred, polyglycidyl ether is even more preferred, and ethylene glycol diglycidyl ether (EGDE) is particularly preferred.

[0052] The blending mass ratio of the carboxyalkyl cellulose and / or its salt to the crosslinking agent can be appropriately set. From the viewpoint of the shape, transparency and strength of the granular carrier, the blending mass ratio (X / Y) of the carboxyalkyl cellulose and / or its salt (X) to the crosslinking agent (Y) is preferably in the range of 10 / 2≧X / Y≧10 / 5, more preferably in the range of 10 / 2>X / Y≧10 / 4.

[0053] In step S3, the mixture obtained in step S2 is added (injected) into a low-polarity organic solvent and dispersed to form a suspension (reverse phase suspension), and dispersed particles consisting of gel particles containing crosslinked bodies of carboxyalkyl cellulose salt are formed by crosslinking polymerization in this suspension.

[0054] The low-polarity organic solvent used as the dispersion medium in step S3 is a low-polarity organic solvent having a relative dielectric constant of 10 or less at 25°C, and is less polar than the above mixture of dispersoids. Therefore, the suspension prepared in step S3 is a reversed-phase suspension, and the cross-linking polymerization of the carboxyalkyl cellulose salt is a reversed-phase suspension polymerization. Here, the relative dielectric constant is the relative dielectric constant at 25°C measured by a capacitance meter. According to one example, it is more preferable that the low-polarity organic solvent used as the dispersion medium has a relative dielectric constant of 3 or more and 6 or less.

[0055] Examples of low-polarity organic solvents having a relative dielectric constant of 10 or less include aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, liquid paraffin, silicone oil, etc., and these can be used alone or in combination of two or more.

[0056] The low polarity organic solvent used in step S3 has a kinetic viscosity of 10 mm at 37.8° C. 2 When the dispersion medium is a viscous fluid, the aggregation of the generated spherical gel particles can be suppressed, and the adhesion between the spherical gel particles can be suppressed, thereby suppressing the formation of clumps of the spherical gel particles. 2 / s or more is important in order to obtain high quality granular carriers which are spherical in shape and have a uniform particle size.

[0057] Here, the kinematic viscosity is the kinematic viscosity at 37.8° C. measured by a vibration viscometer. According to one example, the low polarity organic solvent used as the dispersion medium has a kinematic viscosity of 10 mm 2 / s or more 100mm 2 / s or less, and according to other examples, 15 mm 2 / s or more 80mm 2 / s or less, and according to another example, 20 mm 2 / s or more 50mm 2 / s or less.

[0058] Among the above-mentioned specific examples of low-polarity organic solvents having a relative dielectric constant of 10 or less, liquid paraffin and silicone oil are particularly preferable as the low-polarity organic solvent used in step S3 because they are viscous fluids.

[0059] The liquid paraffin is not particularly limited as long as it is a paraffin that is liquid at room temperature, and examples thereof include liquid saturated hydrocarbons having 12 to 50 carbon atoms, and may be any of n-paraffin, isoparaffin, and naphthene. In addition, examples of commercially available products that can be used include Moresco White, Moresco Bioless, and Smoil (registered trademark) (all trade names, manufactured by Matsumura Oil Research Institute), Stanol, Krystoll, Esso White Oil, and Purelex (all trade names, manufactured by Esso Oil Co., Ltd.). These may be used alone, or two or more of them may be used in combination.

[0060] The silicone oil is not particularly limited as long as it has a siloxane structure that is liquid at room temperature, and examples thereof include polysiloxane oils such as dimethyl silicone oil, and modified silicone oils having functional groups such as hydroxyl groups, carboxyl groups, amino groups, epoxy groups, cyano groups, mercapto groups, trifluoropropyl groups, chlorophenyl groups, long-chain alkyl groups, and the like, or modified with polyethers, alcohols, etc. These may be used alone or in combination of two or more kinds.

[0061] In step S3, the above-mentioned crosslinking agent may be further added to the low-polarity organic solvent to perform surface crosslinking (secondary crosslinking) to provide a portion with high crosslink density on the surface layer of the gel particles. By performing surface crosslinking (secondary crosslinking), it is possible to improve the gel strength while maintaining the water absorption amount.

[0062] In step S3, the low-polarity organic solvent to which the mixture obtained in step S2 is added is at room temperature or in a heated state. According to one example, the low-polarity organic solvent is preferably heated to 30° C. to 80° C., and according to another example, the low-polarity organic solvent is more preferably heated to 50° C. to 70° C.

[0063] In step S3, the low polarity organic solvent to which the mixture obtained in step S2 is added is stirred. Examples of the stirring device include a mechanical stirrer, and examples of the stirring blade include an anchor type, a propeller type, a paddle type, and the like, and can be appropriately selected and used. In one example, in step S3, the low polarity organic solvent is stirred at a rotation speed of 50 to 500 rpm, in another example, at a rotation speed of 200 to 500 rpm, and in yet another example, at a rotation speed of 250 to 400 rpm.

[0064] In step S3, the mixture obtained in step S2 is added (injected) into the low-polarity organic solvent, for example, by dripping the mixture drop by drop from the liquid surface of the low-polarity organic solvent using a pipette (hereinafter, sometimes referred to as the "drop injection method"). Another example is by continuously injecting the mixture while immersing a pipette in the low-polarity organic solvent (hereinafter, sometimes referred to as the "continuous injection method"). The drop injection method is preferred because it makes it easier to obtain uniform particle sizes for the dispersed particles. The continuous injection method is preferred because it can be easily performed in a short time.

[0065] In step S3, the time required for the cross-linking polymerization reaction of the carboxyalkyl cellulose salt can be appropriately set. According to one example, it can be set to 1 hour to 6 hours.

[0066] In step S4, the dispersed particles, which are gel particles containing crosslinked carboxyalkyl cellulose salts formed in the suspension (reverse phase suspension) in step S3, are removed from the suspension by filtration. The filtered gel particles are then washed, dried, and heated.

[0067] The gel particles that have been filtered out are washed, for example, by washing the surfaces of the gel particles with an aqueous detergent solution containing a surfactant. This removes low-polarity organic solvents and the like that have adhered to the surfaces of the gel particles. However, when a solvent with a low boiling point such as n-hexane is used as the low-polarity organic solvent, the solvent on the surfaces of the gel particles can be volatilized / removed without washing by using a method such as reduced pressure distillation.

[0068] The gel particles separated by filtration are washed, for example, by immersing the gel particles in ethanol to dehydrate and dealkalize them.

[0069] The washing of the filtered gel particles may include both washing by rinsing with the above-mentioned surfactant-containing detergent aqueous solution and washing by immersing in ethanol. Also, washing can be omitted.

[0070] In step S4, the washed gel particles are then dried to become dried gel particles. Drying can be performed, for example, by air drying. Air drying is performed by exposing the gel particles to air at ambient temperature. However, the drying step may be omitted, and the gel particles may be dried in the heating step described below. That is, the heating step may also serve as the drying step.

[0071] In step S4, the dry gel particles are then heated. Heating improves the ability of the dry gel particles to suppress water separation over time when they are in a water-absorbed state. This is presumably because the heating process advances a crosslinking reaction by the unreacted crosslinking agent remaining in the dry gel particles before heating, improving the water-retaining function of the gel particles. This effect of improving the water-separation suppression ability by heating is an effect that cannot be obtained by extending the time of the crosslinking polymerization reaction in the reversed-phase suspension of the carboxyalkyl cellulose salt in step S3 or by increasing the temperature of the crosslinking polymerization reaction to further advance the crosslinking reaction of the unreacted crosslinking agent.

[0072] The heating treatment can be carried out using a heating device such as an oven or a thermostatic bath. The time and temperature of the heating treatment can be appropriately set. In one example, the treatment temperature may be less than 150°C, may be in the range of 40°C to 110°C, or may be in the range of 40°C to 100°C. In another example, the treatment time may be in the range of 40 minutes to 24 hours, or may be in the range of 1 hour to 24 hours. In another example, when the treatment temperature is in the range of 40°C or more and less than 50°C, the treatment time may be in the range of more than 6 hours and less than 24 hours. When the treatment temperature is in the range of 50°C or more and less than 70°C, the treatment temperature may be in the range of 2 hours to 24 hours, or may be in the range of more than 6 hours and less than 24 hours. When the treatment temperature is in the range of 70°C or more and less than 110°C, the treatment time may be in the range of 40 minutes to 24 hours, or may be in the range of 2 hours to 15 hours. When the treatment temperature is within the range of 90° C. or more and 110° C. or less, the treatment time may be within the range of 40 minutes to 24 hours, or may be within the range of 40 minutes to 5 hours. If the temperature or time of the heating treatment is excessive, the water absorption rate of the dried gel particles decreases or the particles become yellow. Therefore, the temperature and time of the heating treatment can be appropriately set in consideration of the balance between the water syneresis rate, the water absorption rate, and the color depending on the application, etc.

[0073] As described above, the granular carrier made of the dry gel particles according to this embodiment obtained through the heating step in step S4 has an excellent ability to suppress water separation over time when in a water-absorbed state. This granular carrier has a water separation rate of 10.5% by mass or less, preferably 9.5% by mass or less, when saturated with water and left to stand at 24°C for 96 hours.

[0074] The particle diameter of the granular carrier according to the present embodiment is not particularly limited, but there is a preferred particle diameter depending on the purpose of use.For example, when the granular carrier according to the present embodiment is used for carrying medicine, the average particle diameter of the gel particles in the water-absorbed state may be 2 mm or more and 30 mm or less in one example, and 2 mm or more and 20 mm or less in another example.Here, the average particle diameter means the one measured by measuring the major axis of 30 randomly selected particles using a caliper and averaging them.

[0075] In addition, when the granular carrier according to the present embodiment is used for carrying drugs, the average particle size of the gel particles in a dry state may be, for example, 0.2 mm to 6 mm, and in another example, 0.5 mm to 4 mm. Here, the average particle size refers to the value measured by measuring the major axis of 30 randomly selected particles using a vernier caliper and averaging the measurements.

[0076] According to one example, the granular carrier of this embodiment can be used in a dry state as a highly absorbent material in absorbent articles such as disposable diapers, sanitary products (napkins, tampons, etc.), pads (sweat pads, breast milk pads, incontinence pads, etc.), and pet toilets.

[0077] In another example, the granular carrier according to the present embodiment is used as a drug carrier. That is, a liquid composition containing at least one drug selected from drugs having, for example, aromatic, deodorant, deodorizing, insect repellent, insecticidal, or antifungal properties is absorbed and carried by the granular carrier made of the dry gel particles according to the present embodiment. This makes it possible to provide gel formulations such as granular drug compositions, such as granular aromatic composition, granular deodorant composition, granular deodorant composition, granular insect repellent composition, granular insecticide composition, and granular antifungal composition.

[0078] In a gel preparation consisting of such a granular pharmaceutical composition, various commonly used drugs can be used as the pharmaceutical component contained in the liquid composition that is absorbed and carried by the granular carrier, depending on the purpose. Specific examples of aromatic drugs include animal fragrances such as musk, spirit cat fragrance, and dragon jasmine fragrance, and vegetable fragrances such as abies oil, acorn oil, almond oil, angelica root oil, page oil, bergamot oil, perch oil, boa bur rose oil, kayabuchi oil, gananga oil, capsicum oil, caraway oil, cardamom oil, cassia oil, celery oil, cinnamon oil, citronella oil, cognac oil, coriander oil, cumin oil, camphor oil, basil oil, estugoran oil, eucalyptus oil, fennel oil, garlic oil, ginger oil, grapefruit oil, hop oil, lemon oil, lemongrass oil, nutmeg oil, mandarin oil, peppermint oil, orange oil, sage oil, star anise oil, turpentine oil, rosemary oil, eucalyptus oil, anise oil, lavender oil, cumin oil, cinnamon oil, and hiba oil. In addition, artificial fragrances such as synthetic fragrances or extracted fragrances can also be used. Specific examples include hydrocarbon fragrances such as pinene and limonene, alcohol fragrances such as linalool, geraniol, citronellol, menthol, borneol, benzyl alcohol, anise alcohol, and β-phenethyl alcohol, phenol fragrances such as anethole and eugenol, aldehyde fragrances such as n-butyl aldehyde, isobutyraldehyde, hexyl aldehyde, citral, citronellal, benzaldehyde, and cinnamic aldehyde, ketone fragrances such as carvone, menthone, camphor, acetophenone, and ionone, lactone fragrances such as γ-butyrolactone, coumarin, and cineol, and ester fragrances such as octyl acetate, benzyl acetate, cinnamyl acetate, butyl propionate, and methyl benzoate. These may be used alone or in any combination of two or more.

[0079] The deodorizing agent may be either a volatile agent or a non-volatile agent, and specific examples include metal oxides such as titanium oxide and zinc oxide, flavonoid compounds, plant extracts such as catechin and polyphenol or derivatives thereof, cyclodextrin or derivatives thereof, amine compounds, etc. These may be used alone or in any combination of two or more.

[0080] Specific examples of deodorizing agents include activated carbon such as coconut shell activated carbon, charcoal such as binchotan charcoal, and other carbon-based adsorbents, as well as silica-based adsorbents such as zeolite, silica gel, and layered zinc aluminosilicate, etc. These may be used alone or in any combination of two or more.

[0081] Specific examples of agents having insect repellent or insecticidal properties include pyrethroid insecticidal components such as empenthrin, transfluthrin, allethrin, fenothrin, eminence, and profluthrin, and volatile insect repellent and insecticidal components such as paradichlorobenzene, naphthalene, camphor, 2-phenoxyethanol, hinokitiol, and allyl isothiocyanate. These can be used alone or in any combination of two or more.

[0082] In addition to the above-mentioned drugs, various additives can be used in the liquid composition, such as surfactants, colorants, preservatives, and pH adjusters.

[0083] The granular pharmaceutical composition according to this embodiment can be produced, for example, by impregnating dry gel particles into a liquid pharmaceutical composition.

[0084] As described above, the granular carrier according to the present embodiment, which is a gel particle derived from a dispersed particle formed by reversed-phase suspension polymerization using a low-polarity organic solvent as a dispersion medium, has a substantially spherical shape and a uniform particle size. Therefore, the granular drug composition obtained by carrying a liquid drug composition on the granular carrier according to the present embodiment is likely to cause air flow when filled in a container, and the drug carried on the granular carrier can function efficiently. In addition, the granular drug composition according to the present embodiment is also excellent in strength and ability to suppress water separation. Therefore, the granular carrier according to the present embodiment is suitably used for carrying a drug in a granular gel preparation filled in a container in stationary products such as air fresheners and deodorants. EXAMPLES

[0085] The results of tests carried out in relation to the present invention are described below. (1) Production of granular carriers (1.1) Example 1-1 The raw material used was sodium carboxymethylcellulose (CMC-Na) (Daicel 1120, manufactured by Daicel Miraize Co., Ltd.) with a viscosity in the range of 20 to 50 mPa s. The viscosity here was the viscosity of a 1% by mass aqueous solution of CMC-Na at 25°C measured by the method described above.

[0086] 6 g of sodium hydroxide was added to 300 g of deionized water to obtain an aqueous sodium hydroxide solution. 30 g of the above CMC-Na (Daicel 1120) was added to this aqueous sodium hydroxide solution, and completely dissolved while stirring at room temperature. The obtained aqueous CMC-Na solution was left to stand overnight to defoam. Next, 12 g of ethylene glycol diglycidyl ether (EGDE) (Denacol (registered trademark) EX-810, Nagase ChemteX Corporation) was dropped into this aqueous CMC-Na solution as a crosslinking agent, and the mixture was stirred for 30 minutes to obtain a mixture of the aqueous CMC-Na solution and EGDE. In this example, the blending mass ratio of CMC-Na to the crosslinking agent EGDE (CMC-Na / EGDE) was 10 / 4.

[0087] Next, the obtained mixture was poured into liquid paraffin (Sumoil P-100, manufactured by Matsumura Oil Co., Ltd.; kinematic viscosity 20.45 mm) heated to 55 to 60° C. and stirred at a stirring speed of 250 rpm. 2 The mixture was injected into a 900 g flask (100 ml / s). A high-viscosity pipette was used to inject the mixture, and the tip of the pipette was immersed in liquid paraffin while the mixture was injected. The mixture was allowed to react in the liquid paraffin for 4 hours while stirring.

[0088] After the reaction, the gel particles formed were filtered, and the liquid paraffin adhering to the surface of the gel particles was washed off with an appropriate amount of surfactant aqueous solution. The gel particles were then immersed in ethanol for dehydration and dealkalization, and then air-dried overnight at ambient temperature. The resulting dried gel particles were heated in an oven at 40°C for 1 hour to obtain a solid (granular carrier 1-1).

[0089] (1.2) Example 1-2 A solid material (granular carrier 1-2) was obtained in the same manner as in Example 1-1, except that the conditions of the heating treatment after air drying were changed from 40° C., 1 hour to 40° C., 24 hours.

[0090] (1.3) Example 2-1 A solid material (granular carrier 2-1) was obtained in the same manner as in Example 1-1, except that the conditions for the heating treatment after air drying were changed from 40° C., 1 hour to 60° C., 3 hours.

[0091] (1.4) Example 2-2 A solid material (granular carrier 2-2) was obtained in the same manner as in Example 2-1, except that the conditions for the heating treatment after air drying were changed from 60° C. for 3 hours to 60° C. for 6 hours.

[0092] (1.5) Example 2-3 A solid material (granular carrier 2-3) was obtained in the same manner as in Example 2-1, except that the conditions for the heating treatment after air drying were changed from 60° C. for 3 hours to 60° C. for 24 hours.

[0093] (1.6) Example 3-1 A solid material (granular carrier 3-1) was obtained in the same manner as in Example 1-1, except that the conditions for the heating treatment after air drying were changed from 40° C. for 1 hour to 80° C. for 1 hour.

[0094] (1.7) Example 3-2 A solid material (granular carrier 3-2) was obtained in the same manner as in Example 3-1, except that the heating treatment conditions after air drying were changed from 80° C. for 1 hour to 80° C. for 3 hours.

[0095] (1.8) Example 3-3 A solid material (granular carrier 3-3) was obtained in the same manner as in Example 3-1, except that the conditions for the heating treatment after air drying were changed from 80° C. for 1 hour to 80° C. for 6 hours.

[0096] (1.9) Example 3-4 A solid material (granular carrier 3-4) was obtained in the same manner as in Example 3-1, except that the conditions of the heating treatment after air drying were changed from 80° C. for 1 hour to 80° C. for 24 hours.

[0097] (1.10) Example 4-1 A solid material (granular carrier 4-1) was obtained in the same manner as in Example 1-1, except that the conditions of the heating treatment after air drying were changed from 40° C. for 1 hour to 100° C. for 1 hour.

[0098] (1.11) Example 4-2 A solid material (granular carrier 4-2) was obtained in the same manner as in Example 4-1, except that the conditions for the heating treatment after air drying were changed from 100° C. for 1 hour to 100° C. for 3 hours.

[0099] (1.12) Example 4-3 A solid material (granular carrier 4-3) was obtained in the same manner as in Example 4-1, except that the conditions for the heating treatment after air drying were changed from 100° C. for 1 hour to 100° C. for 6 hours.

[0100] (1.13) Example 4-4 A solid material (granular carrier 4-4) was obtained in the same manner as in Example 4-1, except that the conditions of the heating treatment after air drying were changed from 100° C. for 1 hour to 100° C. for 24 hours.

[0101] (1.14) Example 5-1 A solid material (granular carrier 5-1) was obtained in the same manner as in Example 1-1, except that the conditions of the heating treatment after air drying were changed from 40° C. and 1 hour to 150° C. and 1 hour.

[0102] (1.15) Reference example 1 A solid material (granular carrier 5) was produced in the same manner as in Example 1-1, except that the heating treatment was not carried out after air drying.

[0103] (1.16) Comparative Example 1 A solid material (granular carrier 6) was produced in the same manner as in Example 1-1, except that in Example 1-1, CMC-Na (Daicel 1120, viscosity 20 to 50 mPa·s) was changed to CMC-Na (Daicel 1190, viscosity 1300 to 2000 mPa·s) and no heating treatment was performed after air drying.

[0104] (1.17) Comparative Example 2 10.0 g of CMC-Na (Daicel 1120, Daicel Miraize Co., Ltd.) was dissolved in 100 mL of 0.5 mol / L aqueous sodium hydroxide solution. 4.0 g of EGDE (Denacol EX-810, Nagase ChemteX Co., Ltd.) was added dropwise and stirred for 20 minutes. After degassing for 5 minutes under reduced pressure, the mixture was reacted for 4 hours in a thermostatic bath at 60°C. After the reaction, the gel-like material formed was removed from the beaker and roughly crushed using a mixer. The crushed gel obtained was immersed in ethanol, dehydrated and dealkalized, and then air-dried to obtain a white to pale yellow solid (crushed gel).

[0105] (2) Evaluation method (2.1) Dried gel shape, transparency and strength The shape, transparency and strength of the dry gels obtained in Examples 1-1, 2-4, 3-2, 4-4, Reference Example 1, and Comparative Examples 1 and 2 were evaluated by the following methods.

[0106] (2.1.1) Dried gel shape The shape of each dry gel was visually evaluated according to the following criteria. A: Spherical dry gels make up the majority of the gel, and dry gels of other shapes are hardly found. B: Spherical dry gels make up the majority of the gel. Flat or thread-like dry gels are mixed in, but not noticeable. C: Most of the gel is thread-like, with few spherical gels.

[0107] (2.1.2) Transparency Each dry gel was immersed in ion-exchanged water to absorb the maximum amount of water that it could absorb, forming water-absorbed gel particles. The transparency of the gel particles was evaluated visually according to the following criteria. A: There is no cloudiness and the overall transparency is high. B: Some parts are cloudy, but more than 90% is transparent and the overall appearance is transparent. C: Approximately 30% of the sample is cloudy, but overall the sample appears transparent. D: The whole or most of the part is clouded or yellowed, and transparency is generally low.

[0108] (2.1.3) Strength 1 g of each dry gel was filled into a 200 mL beaker, 150 mL of ion-exchanged water was added, and the mixture was left to stand overnight to obtain water-absorbed gel particles that could absorb the maximum amount of water. The water-absorbed gel particles were filtered to remove excess water, and then filled into a 200 mL beaker again. At this time, the container was piled up with approximately six layers of particles from the bottom to the top. These were used as evaluation samples, and their strength was evaluated according to the following criteria.

[0109] A: The strength at which a particle located at the bottom of a container and bearing a weight approximately six times its own weight maintains its spherical shape and uniformly sized gaps form between particles throughout the packed structure. B: The strength at which at least some of the particles located at the bottom of the container and subjected to a weight approximately six times its own weight are unable to maintain their spherical shape, and there are areas at the bottom where no gaps exist between the particles. C: The strength at which a sphere cannot be maintained by its own weight alone.

[0110] (2.1.4) Results The results of the above evaluations are summarized in Table 1 below.

[0111] [Table 1]

[0112] The following can be seen from Table 1, Fig. 2, Fig. 4 and Fig. 5. Here, Fig. 2 is a photograph showing the water absorption state (water-absorbed gel particles) of each granular carrier produced in Examples 1-1 and 1-2, Examples 2-1 to 2-3, Examples 3-1 to 3-4, and Examples 4-1 to 4-4. Fig. 4(a) is a photograph of the crushed gel particles (crushed gel) in a dry state produced in Comparative Example 2, and Fig. 4(b) is a photograph of the granular carrier (dried gel particles) in a dry state produced in Reference Example 1. Fig. 5(a) is a photograph showing the water absorption state of the crushed gel particles (crushed gel) produced in Comparative Example 2, and Fig. 5(b) is a photograph showing the water absorption state (water-absorbed gel particles) of the granular carrier produced in Reference Example 1. The water-absorbent gel particles in Figures 2 and 5(a) and (b) are all photographs of water-absorbent gels loaded with a saturated amount of water, which were allowed to stand at 24°C for 96 hours (the conditions described in "(2) Syneresis-inhibiting ability" below).

[0113] From these, it can be seen that the crushed gel particles obtained by the conventional method of crushing the hydrogel formed by the aqueous polymerization of CMC-Na are in the form of fragments with sharp edges, and most of the particles are distorted in shape and cannot be said to be spherical. On the other hand, it can be seen that the granular carriers produced by the reversed-phase suspension polymerization of CMC-Na in Examples 1-1 and 1-2, Examples 2-1 to 2-3, Examples 3-1 to 3-4, Examples 4-1 to 4-4, and Reference Example 1 are spherical in shape and uniform in size both in the dry state and in the water-absorbed state, and are also excellent in transparency and strength.

[0114] Moreover, in Comparative Example 1, in which CMC with high viscosity was used, it is found that it is difficult to produce spherical gel particles by reverse phase suspension polymerization.

[0115] (2.2) Syneresis Inhibition Ability Water-absorbed gels carrying a saturated amount of water (maximum amount of water that can be absorbed) were obtained by immersing 1 g of each of the dry gels obtained in Examples 1-4, 2-1 to 2-3, 3-1 to 3-4, 4-1 to 4-4, and Reference Example 1 in ion-exchanged water. Each water-absorbed gel was filled into a 200 mL beaker and allowed to stand at 24° C. for 96 hours. Figure 3 is a photograph of each water-absorbed gel after standing, showing the state of water separation.

[0116] The water separation rate (mass%) of each water-absorbed gel after standing was calculated from the following formula (1). The results are shown in Tables 2 to 4. Water separation rate (%)=[(M1-M2) / M1]×100 (1) In the formula, M1 represents the mass (g) of the water-absorbed gel particles when 1 g of dry gel is saturated with water, and M2 represents the mass (g) of the water-absorbed gel particles after the water-absorbed gel particles are allowed to stand at 24°C for 96 hours.

[0117] [Table 2]

[0118] [Table 3]

[0119] [Table 4]

[0120] From Table 4 and FIG. 3, it was found that the water syneresis rate was reduced and the ability to suppress water syneresis was improved by performing a heating treatment after drying. It was also found that the water syneresis rate was reduced and the ability to suppress water syneresis was further improved as the temperature or time of the heating treatment increased. This tendency was particularly noticeable in Example 2-3 (60°C, 24 hours), Examples 3-2 to 3-4 (80°C, 3 to 24 hours), and Examples 4-1 to 4-4 (100°C, 1 to 24 hours). This is thought to be because the unreacted crosslinking agent was re-crosslinked by heating, strengthening the network and causing a decrease in the water syneresis rate. Among these, Examples 3-2 and 3-3 (80°C, 3 to 6 hours), Examples 4-1 and 4-2 (100°C, 1 to 3 hours) were particularly excellent in the ability to suppress water syneresis, and also had a particularly excellent balance of water absorption rate and color. On the other hand, in Example 4-4 (100°C, 24 hours), the dried gel particles after heating showed brown color. In addition, a decrease in water absorption was also observed. Therefore, it was found that it is possible to obtain a granular carrier having an excellent balance of water syneresis rate, water absorption rate, and color by optimizing the combination of temperature and time in the heating treatment.

[0121] The present invention is not limited to the above-mentioned embodiment, and can be modified in various ways without departing from the gist of the present invention. The embodiments may be combined as appropriate, and in that case, the combined effect can be obtained. Furthermore, the above-mentioned embodiment includes various inventions, and various inventions can be extracted by combinations selected from the multiple components disclosed. For example, if the problem can be solved and the effect can be obtained even if some components are deleted from all the components shown in the embodiment, the configuration from which the components are deleted can be extracted as an invention.

Claims

1. A method for producing a granular carrier comprising gel particles containing a crosslinked body of a carboxyalkyl cellulose salt, comprising the steps of: A carboxyalkyl cellulose and / or a salt thereof having a viscosity of 5 mPa·s or more and 300 mPa·s or less in a 1% by mass aqueous solution at 25°C is dissolved in an alkaline aqueous solution to prepare a carboxyalkyl cellulose salt aqueous solution; preparing a mixture of the aqueous carboxyalkyl cellulose salt and a crosslinking agent; dispersing the mixture in a low-polarity organic solvent to form a suspension, and proceeding with crosslinking polymerization of the carboxyalkyl cellulose salt in the suspension to form dispersed particles consisting of gel particles containing a crosslinked body of the carboxyalkyl cellulose salt; filtering the gel particles from the suspension; and Heating the filtered gel particles. The low-polarity organic solvent has a relative dielectric constant of 10 or less at 25° C. and a kinetic viscosity of 10 mm at 37.8° C. 2 / s or more.

2. The method according to claim 1 , wherein the gel particles are heated at a temperature in the range of 40° C. to 110° C. for a period of 40 minutes to 24 hours.

3. The method according to claim 1 , further comprising washing the gel particles and / or drying the gel particles between filtering the gel particles and heating the gel particles.

4. 2. The method according to claim 1, wherein the low-polarity organic solvent is liquid paraffin or silicone oil.

5. The kinetic viscosity of the low polarity organic solvent at 37.8° C. is 10 mm 2 / s or more 100mm 2 The method according to claim 1, wherein the β-amino acid value is in the range of 0.1 to 1.0 μm / s or less.

6. The method according to claim 1, wherein the cross-linking polymerization of the carboxyalkyl cellulose salt in the suspension is carried out under stirring at a rotation speed of 50 rpm or more and 500 rpm or less.

7. The method according to claim 1, wherein the viscosity of the carboxyalkyl cellulose and / or salt thereof is 5 mPa·s or more and 100 mPa·s or less.

8. The method according to claim 1, wherein the mass ratio (X / Y) of the carboxyalkyl cellulose and / or its salt (X) to the crosslinking agent (Y) in the mixture is in the range of 10 / 2 to 10 / 5.

9. 2. The method according to claim 1, wherein the crosslinking agent is a compound having two or more epoxy groups in the molecule.

10. The method according to claim 1, wherein the granular carrier is used for carrying a drug.

11. The method according to claim 1, wherein the granular carrier is used as a water-absorbent material in an absorbent article.

12. A granular carrier comprising gel particles containing a crosslinked salt of a carboxyalkyl cellulose, the carboxyalkyl cellulose being a carboxyalkyl cellulose having a viscosity of 5 mPa·s or more and 300 mPa·s or less in a 1% by mass aqueous solution at 25°C, the gel particles being dry gel particles derived from dispersed particles in a reverse phase suspension, the dry gel particles being saturated with water and having a water separation rate of 10.5% by mass or less when allowed to stand at 24°C for 96 hours.

13. The granular carrier according to claim 12, which is used for carrying a drug.

14. A granular drug composition comprising the granular carrier described in claim 12 and a liquid composition supported on the granular carrier and containing at least one drug selected from drugs having aromatic, deodorizing, odor eliminating, insect repellent, insecticidal or antifungal properties.

15. The granular pharmaceutical composition according to claim 14, which is an air freshener composition or a deodorant composition.

16. An absorbent article comprising the granular carrier according to claim 12.

Citation Information

Patent Citations

  • Production of fine particle

    JP1996027277A

  • Production of water-base gel base material and water-base gel base material produced thereby

    JP1998251447A

  • Method for producing crosslinked polymeric particle, and crosslinked polymeric particle

    JP2012126796A

  • Composite polymer presenting gel form by water absorption