Steel material
A steel material with controlled composition and microstructure addresses the challenge of Sn segregation in Sn-added steel, achieving improved corrosion resistance, toughness, and strength for marine and bridge applications.
Patent Information
- Application Number
- JP2023062293
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
AI Technical Summary
Existing Sn-added steel materials face challenges in achieving balanced improvements in corrosion resistance, toughness, and strength, particularly in chloride environments, with Sn segregation at grain boundaries leading to embrittlement and reduced toughness.
A steel material with controlled chemical composition and microstructure, including specific ranges for elements like C, Mn, Sn, and S, along with a balanced ratio of Mn/Sn, is developed to enhance corrosion resistance, toughness, and strength by adjusting the ratio of C content to Sn content on grain boundaries and ensuring a predominantly ferrite and bainite microstructure.
The solution results in a steel material with improved corrosion resistance, toughness, and strength, suitable for large structures like marine structures and bridges, by minimizing Sn segregation and optimizing the microstructure for enhanced mechanical properties.
Smart Images

Figure 2024148822000001 
Figure 2024148822000002 
Figure 2024148822000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel material. [Background technology]
[0002] In recent years, there have been stricter demands for improved material properties for various steel materials, such as thick steel plates used in large structures such as marine structures and bridges installed in icy waters. There is a strong demand for improvements in not only corrosion resistance but also mechanical properties.
[0003] Conventionally, Sn-added steels have been proposed to improve corrosion resistance in seawater environments.
[0004] For example, Patent Document 1 discloses a steel material in which the contents of S and Sn are controlled and central segregation of Sn is suppressed, thereby improving corrosion resistance and lamellar tear resistance.
[0005] Furthermore, Patent Document 2 discloses a steel material in which the corrosion resistance, low-temperature toughness, and fatigue properties are improved by controlling the Sn concentration at the grain boundaries and within the grains. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2019 / 003856 [Patent Document 2] International Publication No. 2019 / 116520 Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, Sn-added steel has been proposed to improve corrosion resistance in seawater environments, etc. On the other hand, there is a demand for improving mechanical properties, particularly toughness and strength, while improving corrosion resistance by adding Sn.
[0008] For example, the invention described in Patent Document 1, which discloses that the addition of Sn improves corrosion resistance, requires improvement in toughness and strength.
[0009] In addition, the invention described in Patent Document 2 has excellent corrosion resistance, low-temperature toughness, and fatigue properties. However, as a result of further investigations by the inventors, it was found that there is still room for improvement in terms of further improving toughness and strength.
[0010] An object of the present invention is to solve the above problems and to provide a steel material having excellent corrosion resistance, toughness and strength. [Means for solving the problem]
[0011] The present invention has been made to solve the above problems, and the gist of the present invention is the following steel material.
[0012] (1) The chemical composition of the steel, in mass%, is C: 0.01-0.20%, Si: 0.01 to 1.00%, Mn: 0.01 to 2.00%, P: 0.010% or less, S: 0.005% or less, Sn: 0.010~0.20%, Al: 0.001 to 0.040%, N: 0.001 to 0.005%, O: 0.0001 to 0.010%, The balance is Fe and impurities. The following formula (i) is satisfied: In a cross section perpendicular to the rolling direction of the steel material, when the thickness of the steel material is t, the metal structure in a region from the 1 / 2t position to the 1 / 4t position of the steel material is, in terms of area%, The sum of ferrite and bainite is 90% or more, The area ratio of ferrite having a grain size of 20 μm or less is 50% or more of the total amount of ferrite, In the region from the 1 / 2t position to the 1 / 4t position of the steel material, The area ratio of MnS is 0.020% or less according to the point calculation method in JIS G 0555:2015, The ratio of the C content to the Sn content on the grain boundary between the MnS and a crystal grain in contact with the MnS is 0.04 to 6.00. Steel material. 10.0<(Mn / S)×Sn<175.0 (i) In the formula, each element symbol represents the content (mass%) of each element contained in the steel material.
[0013] (2) The chemical composition contains, in mass%, a part of the Fe replaced by Cu: 0.20% or less, Ni: 0.10% or less, W: 0.50% or less, Mo: 0.50% or less Cr: 0.10% or less, Nb: 0.010% or less, It contains one or more selected from The steel material described in (1) above. Effect of the Invention
[0014] According to the present invention, it is possible to provide a steel material excellent in corrosion resistance, toughness and strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] In order to achieve the above object, the present inventors have conducted detailed investigations into the corrosion resistance, toughness, and strength of steel materials, and have come to the following findings.
[0016] When Sn is contained in steel, the corrosion resistance is improved, but the toughness is reduced. Therefore, the inventors have repeatedly studied the cause of Sn reducing the toughness of steel. As a result, it has become clear that Sn segregates on the grain boundaries between MnS, which inevitably precipitates, and the surrounding crystal grains in steel. It has been found that the interface between MnS and Sn becomes a slip surface, which becomes the starting point of embrittlement and reduces the toughness.
[0017] However, in studying the relationship between Sn and toughness, it was difficult to measure the absolute amount of Sn content on the grain boundary. Therefore, the inventors conducted extensive research and found that it was possible to measure the Sn content based on the content of C that inevitably segregates on the grain boundary between MnS and the surrounding grains, that is, the ratio of the C content to the Sn content.
[0018] Therefore, first, the balance of Mn, S, and Sn contents in the steel material is appropriately adjusted. Then, by performing heat treatment under appropriate conditions and then cooling, it is possible to control the ratio of C content to Sn content on the grain boundary between MnS and the surrounding crystal grains. This makes it possible to improve toughness and strength while maintaining corrosion resistance.
[0019] Furthermore, it was found that toughness can be improved by making the metal structure primarily ferrite and bainite, while a decrease in strength can be suppressed by ensuring that the proportion of fine-grained ferrite is above a certain value.
[0020] The present invention has been made based on the above findings. Each of the features of the present invention will be described in detail below.
[0021] (A) Chemical composition The reasons for limiting the content of each element are as follows. In the following description, "%" for the content means "mass %."
[0022] C: 0.01 to 0.20% C is an element that improves the strength of steel. On the other hand, if the C content is excessive, the weldability is significantly reduced. In addition, with an increase in the C content, the amount of cementite that acts as a cathode in a low pH environment and promotes corrosion increases, and the corrosion resistance of the steel is reduced. Therefore, the C content is set to 0.01 to 0.20%. The C content is preferably 0.02% or more, more preferably 0.03% or more, and even more preferably 0.05% or more, 0.07% or more. In addition, the C content is preferably 0.18% or less, more preferably 0.16% or less, and even more preferably 0.15% or less, 0.13% or less.
[0023] Silicon: 0.01 to 1.00% Silicon is an element necessary for deoxidation. In order to obtain a sufficient deoxidation effect, it is contained in an amount of 0.01% or more. On the other hand, if the Si content is excessive, the toughness of the steel material, particularly the toughness of the base material and the welded heat affected zone when welding is performed, is impaired. Therefore, the Si content is set to 0.01 to 1.00%. The Si content is preferably 0.03% or more, more preferably 0.05% or more, and even more preferably 0.10% or more, 0.15% or more, or 0.20% or more. In addition, the Si content is preferably 0.80% or less, more preferably 0.60% or less, and even more preferably 0.50% or less, 0.40% or less, or 0.30% or less.
[0024] Mn: 0.01 to 2.00% Mn is a low-cost element that has the effect of increasing the strength of steel materials. On the other hand, if the Mn content is excessive, Mn segregation increases and toughness deteriorates. Therefore, the Mn content is set to 0.01 to 2.00%. The Mn content is preferably 0.05% or more, and more preferably 0.08% or more. In addition, the Mn content is preferably 1.50% or less, and more preferably 1.00% or less.
[0025] P:0.010% or less P is an element that exists as an impurity in steel. P is an element that reduces the acid resistance of steel, and in a chloride corrosion environment where the pH of the corrosion interface is reduced, it reduces the corrosion resistance of steel. P also reduces the weldability and toughness of steel. Therefore, the P content is set to 0.010% or less. The P content is preferably 0.008% or less, and more preferably 0.006% or less. To improve toughness, the upper limit of the P content may be set to 0.002% or 0.001%. Although it is not easy to completely remove P, it is not necessary to eliminate it, and the lower limit of the P content is 0%. Since the desulfurization cost for extremely low phosphorus is high, the lower limit of the P content may be set to 0.0005% or 0.0008%.
[0026] S: 0.005% or less S is an element that exists as an impurity in steel. When the S content is excessive, the precipitation of MnS increases, and Sn segregates on the interface between MnS and the surrounding crystal grains. As a result, the balance of segregation between Sn and C on the crystal grain interface is lost, and toughness deteriorates. Therefore, the S content is set to 0.005% or less. The S content is preferably 0.004% or less, and more preferably 0.003% or less. Although it is not easy to completely remove S, it is not necessary to eliminate it, and the lower limit of the S content is 0%. Since the refining cost for extremely low sulfurization is high, the lower limit of S may be set to 0.001% or 0.0020%.
[0027] Sn: 0.010~0.20% Sn significantly suppresses the anodic dissolution reaction of steel in a low pH chloride environment, and therefore significantly improves the corrosion resistance of steel in a chloride corrosion environment. On the other hand, when the Sn content becomes excessive, the MnS area ratio increases. Although the detailed mechanism is not clear, it is believed that this is because oxides or sulfides of Sn are generated, and MnS is generated from these. Therefore, Sn is likely to segregate on the interface between MnS and the surrounding crystal grains. In addition, not only does the above effect saturate, but the toughness of the steel, particularly the toughness of the base material and the high heat input welded joint when welding is performed, deteriorates. Therefore, the Sn content is set to 0.010 to 0.20%. The Sn content is preferably 0.050% or more, more preferably 0.080% or more, and even more preferably 0.100% or more. In addition, the Sn content is preferably 0.18% or less, more preferably 0.16% or less, and even more preferably 0.14% or less.
[0028] Al: 0.001 to 0.040% Al is an element effective for deoxidizing steel. On the other hand, if the Al content exceeds 0.040%, the corrosion resistance of the steel in a low pH environment decreases, and therefore the corrosion resistance of the steel in a chloride corrosion environment decreases. Furthermore, if the Al content exceeds 0.040%, the nitrides become coarse, causing a decrease in the toughness of the steel. Therefore, the Al content is set to 0.001 to 0.040%. The Al content is preferably 0.005% or more, more preferably 0.010% or more, and even more preferably 0.015% or more. Moreover, the Al content is preferably 0.035% or less, and more preferably 0.030% or less.
[0029] N: 0.001 to 0.005% N dissolves as ammonia, and in environments with high airborne salt content, Fe 3+By suppressing the decrease in pH due to hydrolysis of N, it has the effect of improving the corrosion resistance of steel sheets in salt environments. On the other hand, if the N content is excessive, not only will the effect saturate, but the toughness of the steel sheet will also deteriorate. In addition, there is a risk that coarse AlN will be formed, resulting in a decrease in toughness. Therefore, the N content is set to 0.001 to 0.005%. The N content is preferably 0.002% or more, and more preferably 0.003% or more. In addition, the N content is preferably 0.004% or less.
[0030] O: 0.0001 to 0.010% O (oxygen) improves the toughness of steel materials, especially the toughness of welded joints when welding is performed, when contained in a small amount. On the other hand, O forms oxides such as SnO and SnO2. Therefore, if the O content is excessive, the Sn concentration in the steel cannot be sufficiently secured. In addition, the above oxides become the starting point of corrosion, so the corrosion resistance of the steel material decreases. Therefore, the O content is set to 0.0001 to 0.010%. The O content is preferably 0.0002% or more, more preferably 0.0003% or more, and even more preferably 0.0005% or more, 0.0010% or more, or 0.0015% or more. In addition, the O content is preferably 0.009% or less, more preferably 0.008% or less, and even more preferably 0.006% or less, 0.004% or less, or 0.003% or less.
[0031] In the chemical composition of the steel material according to the present invention, in addition to the above elements, one or more elements selected from Cu, Ni, W, Mo, Cr, and Nb may be further contained in the ranges shown below in order to improve the corrosion resistance, etc., of the steel material. Note that these elements are not necessarily essential for the steel material according to the present invention, and therefore the lower limit of the content is 0%. The reasons for limiting each element will be explained.
[0032] Cu:0.20% or less Cu is an element that improves the corrosion resistance of steel materials, and therefore can be included as necessary. However, it has been found that excessive Cu content actually reduces corrosion resistance in a corrosive environment containing chlorides as envisaged in the present invention. Therefore, the Cu content is set to 0.20% or less. The Cu content is preferably set to 0.15% or less, and more preferably set to 0.10% or less. In order to stably obtain the above effects, the Cu content is preferably set to 0.01% or more, and more preferably set to 0.05% or more.
[0033] Ni: 0.10% or less Like Cu, Ni is an element that improves the corrosion resistance of steel materials, and can be included as necessary. However, it has been found that excessive Ni content actually reduces corrosion resistance in a corrosive environment containing chlorides as envisaged in the present invention. Therefore, the Ni content is set to 0.10% or less. The Ni content is preferably 0.08% or less, and more preferably 0.05% or less. In order to stably obtain the above effects, the Ni content is preferably 0.01% or more.
[0034] W: 0.50% or less Mo: 0.50% or less W and Mo can be added as necessary to improve properties such as strength or toughness (particularly low-temperature toughness). However, excessive addition reduces corrosion resistance. Therefore, the W and Mo contents are each set to 0.50% or less. The W and Mo contents are each preferably set to 0.40% or less, and more preferably set to 0.30% or less. In order to stably obtain the above effects, the W and Mo contents are each preferably set to 0.010% or more, and more preferably set to 0.020% or more.
[0035] Cr:0.10% or less Cr is an element that improves the corrosion resistance of steel materials, and can be included as necessary. However, it has been found that excessive Cr content actually reduces corrosion resistance in a corrosive environment containing chlorides as envisaged in the present invention. Therefore, the Cr content is set to 0.10% or less. The Cr content is preferably 0.07% or less, more preferably less than 0.05%, and even more preferably 0.03% or less. In order to stably obtain the above effects, the Cr content is preferably 0.01% or more.
[0036] Nb: 0.010% or less Nb is an element that produces precipitates and increases the strength of steel materials, so it can be added as necessary. However, if it is added in excess, toughness may decrease. Therefore, the Nb content is set to 0.010% or less. The Nb content is preferably set to 0.008% or less, more preferably set to 0.005% or less, and even more preferably set to 0.003% or less. In order to stably obtain the above effects, the Nb content is preferably set to 0.001% or more.
[0037] In the chemical composition of the steel material of the present invention, the balance is Fe and impurities. Here, the impurities refer to components that are mixed in due to various factors in raw materials such as ores and scraps and manufacturing processes during industrial production of steel material, and are permissible within a range that does not adversely affect the present invention.
[0038] In addition, in the chemical composition of the steel material according to the present invention, in addition to each element satisfying the above-mentioned range, the following formula (i) is satisfied. If the Sn content and Mn content are excessive, the amount of MnS precipitation increases, and the number of MnS with segregated Sn also increases. Therefore, toughness decreases. On the other hand, if the Sn content is insufficient, corrosion resistance deteriorates, and if the Mn content is insufficient, strength deteriorates. Furthermore, if the S content is excessive, the amount of MnS precipitation increases, and as a result, the number of MnS with segregated Sn also increases, and toughness deteriorates. Therefore, in order to obtain a steel material with excellent toughness and strength while maintaining corrosion resistance, it is important to balance the contents of Mn, S, and Sn, and the following formula (i) is satisfied. 10.0<(Mn / S)×Sn<175.0 (i) In the formula, each element symbol represents the content (mass%) of each element contained in the steel material.
[0039] The value in formula (i) is preferably 20.0 or more, and more preferably 30.0 or more, and the value in formula (i) is preferably 160.0 or less, and more preferably 140.0 or less.
[0040] (B) Metal structure In the metal structure of the steel material according to the present invention, in a cross section perpendicular to the rolling direction of the steel material, when the thickness of the steel material is t, the total area ratio of ferrite and bainite is 90% or more in the region from the 1 / 2t position to the 1 / 4t position of the steel material. Furthermore, in the region from the 1 / 2t position to the 1 / 4t position of the steel plate, the area ratio of ferrite having a grain size of 20 μm or less is 50% or more with respect to the total amount of ferrite in the steel material. The reasons for limiting each structure will be explained.
[0041] Total area ratio of ferrite and bainite: 90% or more Both ferrite and bainite are structures with excellent toughness. Therefore, by making the total area ratio of ferrite and bainite in the region from the 1 / 2t position to the 1 / 4t position of the steel material 90% or more, the toughness of the steel material can be ensured. The total area ratio of ferrite and bainite in the region from the 1 / 2t position to the 1 / 4t position of the steel material is preferably 95% or more.
[0042] Although there are no particular limitations on the area ratio of bainite, bainite is a structure that is hard and has high toughness. Therefore, when it is desired to improve the strength while maintaining the toughness of a steel material, the area ratio of bainite in the region from the 1 / 2t position to the 1 / 4t position of the steel material is preferably 10 to 70%. It is more preferable that the area ratio of bainite in the region from the 1 / 2t position to the 1 / 4t position of the steel material is 20 to 60%.
[0043] In addition, pearlite may be mixed in as the remaining structure, but pearlite is a hard structure and reduces the toughness of the steel material. Therefore, it is preferable that the area ratio of pearlite is small, and the area ratio of pearlite in the region from the 1 / 2t position to the 1 / 4t position of the steel material is 10% or less. It is preferable that the area ratio of pearlite in the region from the 1 / 2t position to the 1 / 4t position of the steel material is 5% or less.
[0044] Area ratio of ferrite with grain size of 20μm or less: 50% or more As described above, toughness can be improved by making the metal structure mainly composed of ferrite and bainite. Meanwhile, the mechanical properties of steel improve with the refinement of the grain size. Therefore, by making the area ratio of ferrite with a grain size of 20 μm or less 50% or more of the total amount of ferrite in the region from the 1 / 2t position to the 1 / 4t position of the steel, it is possible to suppress a decrease in the strength of the steel. It is preferable that the area ratio of ferrite with a grain size of 20 μm or less in the region from the 1 / 2t position to the 1 / 4t position of the steel is 60% or more.
[0045] In the present invention, the area ratios of ferrite, bainite, and pearlite, and the grain size of ferrite are measured by the following method.
[0046] First, a sample is taken so that the cross section perpendicular to the rolling direction of the steel material is the observation surface. The region from the 1 / 2t position to the 1 / 4t position of the steel material is then observed with an optical microscope, and ferrite, bainite, and pearlite are identified by image analysis of the obtained image. The area ratios of ferrite, bainite, and pearlite to the area of 100 observation fields are then calculated.
[0047] The minor axis and major axis of the ferrite grains identified as above are measured, and the grain size is calculated as half the sum of the minor axis and major axis. The grain size of the ferrite grains is calculated by arithmetically averaging the grain sizes of the individual grains obtained by observing 100 fields of view in the region from the 1 / 2t position to the 1 / 4t position of the steel material. The area ratio of ferrite grains with a grain size of 20 μm or less to the total amount of ferrite is then calculated.
[0048] (C) Inclusions In the steel material according to the present invention, in a cross section perpendicular to the rolling direction of the steel material, the area ratio of MnS in the region from the 1 / 2t position to the 1 / 4t position of the steel material is 0.020% or less by the point calculation method in JIS G 0555: 2015. Also, in the region from the 1 / 2t position to the 1 / 4t position of the steel material, the ratio of the C content to the Sn content on the interface between MnS and crystal grains in contact with MnS (hereinafter also referred to as "on the crystal grain interface") is 0.04 to 6.00. The reasons for limiting each inclusion will be explained.
[0049] Area ratio of MnS: 0.020% or less As described above, MnS is inevitably precipitated. However, if excessive MnS is precipitated in steel, the number of grain boundaries where Sn can segregate increases, which results in the starting point of embrittlement and deterioration of toughness. Therefore, the area ratio of MnS is set to 0.020% or less. The area ratio of MnS is preferably 0.010% or less. The lower the area ratio of MnS, the better, and the lower limit of the area ratio of MnS is 0%. However, it is not easy to completely remove S, and MnS is inevitably precipitated. Therefore, the lower limit of the area ratio of MnS may be set to 0.001%.
[0050] Ratio of C content to Sn content on grain boundaries: 0.04 to 6.00 Sn is easily segregated on the grain boundaries, and the Sn content on the grain boundaries increases in proportion to the Sn content in the steel material. If the ratio of the C content to the Sn content on the grain boundaries is less than 0.04, as described above, it becomes the starting point of embrittlement. However, if the ratio of the C content to the Sn content on the grain boundaries exceeds 6.00, the deterioration of toughness can be suppressed, but the Sn content in the steel material is insufficient to maintain good corrosion resistance. Therefore, the ratio of the C content to the Sn content on the grain boundaries is set to 0.04 to 6.00. The ratio of the C content to the Sn content on the grain boundaries is preferably 0.30 to 3.00.
[0051] In the present invention, the area ratio of MnS and the ratio of the C content to the Sn content on the grain boundary surface are measured by the following method.
[0052] The area ratio of MnS is measured by a microscope test method using the point counting method in accordance with JIS G 0555:2015. First, a sample is taken so that the cross section perpendicular to the rolling direction of the steel plate is the observation surface. Then, the observation surface is used as the inspection surface, and after polishing to a mirror finish, an eyepiece with 20 vertical and horizontal grid lines is used to randomly observe 60 fields of view from the 1 / 2t position to the 1 / 4t position of the steel material at 400x magnification in a non-etched state. Then, the number n of lattice point centers occupied by inclusions is counted, and the cleanliness d (%) calculated by the following formula is taken as the area ratio of MnS. d = {(n / (p × f)} × 100 Here, d is the cleanliness, p is the total number of lattice points in the field of view, f is the number of fields of view, and n is the number of lattice point centers occupied by inclusions in f fields of view.
[0053] The ratio of the C content to the Sn content on the grain boundary surface is determined by the following method. First, a cylindrical sample with a diameter of 3 mm and a length of 10 mm is prepared from the region between the 1 / 2t position and the 1 / 4t position of the steel material in a cross section perpendicular to the rolling direction of the steel material. The sample is then subjected to an ultra-high vacuum impact fracture mechanism attached to an Auger spectroscopy device (ULVAC-PHI, Inc. Model 670i) at a vacuum level (1.0×10 -9 The fracture surface was observed after fracture in an atmosphere of liquid nitrogen temperature (-150°C) at a pressure of 1000 MPa (below torr).
[0054] Comparing the two fractured samples, one has MnS present, and the other has a crater-like mark where the MnS was present. This crater-like mark is the grain boundary that was in contact with the MnS, and the C content relative to the Sn content at the grain boundary is measured using Auger spectroscopy. The C content relative to the Sn content is measured at 10 points on the same grain boundary, and the average value is calculated. Furthermore, five grain boundaries are identified in the same field of view, and the average value of the ratio of the C content to the Sn content is calculated. The relative sensitivity coefficient is calibrated with Au.
[0055] (D) Manufacturing method There is no particular limitation on the method for producing the steel material according to the present invention, but examples include steel plates and T-shaped steel produced by hot rolling.
[0056] When manufacturing steel plate, steel is melted by a conventional method, and after adjusting the components, the resulting slab is heated to 900 to 1200°C. Then, the steel is rolled in 4 to 8 rolling passes so that the cumulative rolling reduction is 50% or more. As described later, it is preferable to finish the finish rolling at a temperature of 750°C or higher and Ar3+25°C or higher, but considering the effect of processing heat generation, hot rolling may be performed at a temperature range where the surface temperature of the steel plate is 700 to 800°C.
[0057] When manufacturing T-shaped steel, steel is melted in a conventional manner, and after adjusting the components, the bloom obtained by casting is heated to 1100 to 1350° C. Then, it is rolled into a T-shape by reverse rolling.
[0058] Even when manufacturing steel plates, T-beams, and other products, the hot rolling end temperature is preferably set so that the surface temperature is 750°C or higher and Ar3+25°C or higher. If it is less than 750°C, it is not preferable because it puts a strain on the rolling machine. In addition, as described later, since the holding step is performed in the temperature range of Ar3 to Ar3+25°C, the hot rolling end temperature is preferably set to Ar3+25°C or higher.
[0059] Next, it is preferable to hold the surface temperature of the steel material in a temperature range of Ar3 to Ar3+25°C for 5 to 100 seconds. From various experimental results by the present inventors, it has been found that the following effects can be obtained by holding the steel material in a temperature range of Ar3 to Ar3+25°C, where the temperature calculated by the following formula is the Ar3 point. In hot rolling, the surface layer of the steel material is in contact with air compared to the inside of the steel material, so the temperature of the surface layer is lower. Therefore, by holding the steel material in a temperature range of Ar3 to Ar3+25°C, the temperature of the surface layer of the steel material is increased and the temperature difference between the inside and the surface layer is reduced. In this way, the ratio of fine ferrite can be increased by starting cooling, which will be described later, when the temperature in the thickness direction of the steel material reaches the austenite range of Ar3 to Ar3+25°C.
[0060] Here, the Ar3 point can be calculated using the following formula. Ar3(℃)=910-310×C+25×Si-80×(Mn+Cr+Cu+Mo+(Ni / 2)+10×(Nb-0.02)) In the above formula, each element symbol represents the content (mass%) of each element contained in the steel, and when no element is contained, the symbol is set to zero.
[0061] In addition, it was found that by holding the above temperature range for 5 seconds or more, it is possible to suppress the segregation of Sn on the grain boundaries when ferrite is formed from austenite in the cooling process described below, although the mechanism is not clear. If the temperature is held for 100 seconds or less, it is possible to suppress the coarsening of grains.
[0062] Thereafter, it is preferable to perform water cooling to a surface temperature in the range of 300 to 550°C under the condition that the average cooling rate up to 550°C is 5 to 60°C / s. By cooling to 550°C, it is possible to obtain a metal structure mainly composed of ferrite and bainite. In addition, by setting the cooling end temperature to 300°C or higher, it is possible to suppress the formation of martensite. By setting the cooling end temperature to 550°C or lower, it is possible to suppress the segregation of Sn. This is because by stopping cooling after passing through a high temperature range of 550°C or higher where Sn can move, it is possible to suppress the movement of Sn and suppress the segregation of Sn on the grain boundary surface.
[0063] By setting the average cooling rate to 5°C / s or more, it is possible to suppress the formation of pearlite. It is also possible to suppress the segregation of Sn on the grain boundaries. This is because the time spent in the high temperature range of 550°C or more, where Sn can move, can be shortened to suppress the segregation of Sn on the grain boundaries. On the other hand, by setting the average cooling rate to 60°C / s or less, it is possible to suppress the formation of martensite.
[0064] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. EXAMPLES
[0065] Steel having the chemical composition shown in Table 1 was melted in a furnace and then cast into a slab with a thickness of 300 mm. This slab was heated and hot rolled with six rolling passes, and then held under the conditions shown in Table 2. It was then water-cooled to form a steel plate with a thickness of 20 mm. The manufacturing conditions are shown in Table 2. In Table 1, the underlined values indicate values outside the range specified in the present invention. In Table 2, the underlined values indicate values outside the preferred manufacturing conditions.
[0066] [Table 1]
[0067] [Table 2]
[0068] For each steel sheet, the metal structure, the area ratio of MnS, and the ratio of the C content to the Sn content on the grain boundary surface were measured by the following methods.
[0069] First, a sample was taken so that the cross section perpendicular to the rolling direction of the steel material would be the observation surface. The region from the 1 / 2t position to the 1 / 4t position of the steel material was then observed using an optical microscope, and ferrite, bainite, and pearlite were identified by image analysis of the obtained images. The area ratios of ferrite, bainite, and pearlite to the area of 100 observation fields were then calculated.
[0070] The grain size of the ferrite grains identified as above was calculated by measuring the minor axis and major axis of the grains and dividing the minor axis and major axis by half the sum of the minor axis and major axis. The grain size of the ferrite grains was calculated by arithmetically averaging the grain sizes of the individual grains in the region from the 1 / 2t position to the 1 / 4t position of the steel material in 100 fields of view. The area ratio of the ferrite grains with a grain size of 20 μm or less to the total amount of ferrite in the steel material was then calculated.
[0071] The area ratio of MnS was measured by a microscope test method using the point counting method in accordance with JIS G 0555:2015. First, a sample was taken so that the cross section perpendicular to the rolling direction of the steel plate was the observation surface. Then, the observation surface was used as the inspection surface, and after polishing to a mirror finish, an eyepiece with 20 vertical and horizontal grid lines was used to randomly observe 60 fields of view from the 1 / 2t position to the 1 / 4t position of the steel material in a no-etching state at 400x magnification. Then, the number n of lattice point centers occupied by inclusions was counted, and the cleanliness d (%) calculated by the following formula was taken as the area ratio of MnS. d = {(n / (p × f)} × 100 Here, d is the cleanliness, p is the total number of lattice points in the field of view, f is the number of fields of view, and n is the number of lattice point centers occupied by inclusions in f fields of view.
[0072] The ratio of the C content to the Sn content on the grain boundary surface was determined by the following method. First, a cylindrical sample with a diameter of 3 mm and a length of 10 mm was prepared from the region between the 1 / 2t position and the 1 / 4t position of the steel material in a cross section perpendicular to the rolling direction of the steel material. The sample was then subjected to an ultra-high vacuum impact fracture mechanism attached to an Auger spectroscopy device (ULVAC-PHI, Inc. Model 670i) at a vacuum level (1.0×10 -9 The fracture surfaces prepared by fracture in an atmosphere of liquid nitrogen temperature (-150°C) at a pressure of 1000 MPa (below torr) were observed.
[0073] Comparing the two fractured samples, one had MnS, and the other had a crater-like mark at the position where the MnS had been. This crater-like mark was the grain boundary that had been in contact with the MnS, and the C content relative to the Sn content at the grain boundary was measured by Auger spectroscopy. Ten points on the same grain boundary were measured for the C content relative to the Sn content, and the average value was calculated. Furthermore, five grain boundaries were identified in the same field of view, and the average value of the ratio of the C content to the Sn content was calculated. The relative sensitivity coefficient was calibrated with Au.
[0074] Furthermore, a tensile test, a toughness test, and a corrosion resistance test were performed on each steel plate.
[0075] <Tensile test> JIS No. 4 tensile test pieces were taken from each steel plate at 1 / 2t of the plate thickness in a direction perpendicular to the rolling direction, and the tensile strength was investigated. Steel plates with a tensile strength of 350 MPa or more were deemed to have passed the test.
[0076] <Toughness test> JIS No. 4 test pieces were taken from each steel plate at 1 / 2t thickness in a direction parallel to the rolling direction and V-notched according to JIS Z 2242:2020. The absorbed energy (vE0) at 0°C was then calculated and evaluated. Toughness was evaluated as passing if the absorbed energy was 150J or more. If the toughness at the center of the plate thickness was good, it was determined that the toughness of the steel material was good.
[0077] <Corrosion resistance test> Test pieces measuring 60 mm in length, 100 mm in width, and 3 mm in thickness were cut out from each steel plate and subjected to the SAE J2334 test. Note that a corrosion protection film was formed on the surface of each test piece in advance. The SAE J2334 test is explained below.
[0078] The SAE J2334 test is an accelerated deterioration test in which repeated wet and dry conditions (wet → salt adhesion → dry) are repeated for one cycle (total of 24 hours), simulating a severe corrosive environment in which the amount of airborne salt exceeds 1mdd. The SAE J2334 test was conducted under the following conditions as one cycle. The corrosion pattern under the following conditions is similar to that in the atmospheric exposure test.
[0079] (Test conditions) Humidity: 50℃, 100%RH, 6 hours, Salt adhesion: Immersion in 0.5% by mass NaCl, 0.1% by mass CaCl2, and 0.075% by mass NaHCO3 aqueous solutions for 0.25 hours. Drying: 60℃, 50% RH, 17.75 hours
[0080] The surface of each test piece was shot blasted, and then the anticorrosive undercoat, undercoat, intermediate coat, and top coat were applied in that order to form an anticorrosive coating with a total thickness of 250 μm.
[0081] As the anticorrosive base, inorganic zinc-rich paint ("Shinto Zinc #2000" manufactured by Shinto Paint Co., Ltd.) was applied to a thickness of 75 μm, and as the mist coat, epoxy resin paint ("Neo Gosei #2300MC" manufactured by Shinto Paint Co., Ltd.) was applied. As the undercoat, epoxy resin paint ("Neo Gosei #2300PS" manufactured by Shinto Paint Co., Ltd.) was spray-applied to a thickness of 120 μm. As the intermediate coat, intermediate coat paint for fluororesin paint ("Shinto Flon #100 intermediate coat" manufactured by Shinto Paint Co., Ltd.) was applied to a thickness of 30 μm. Furthermore, as the top coat, fluororesin paint ("Shinto Flon #100" manufactured by Shinto Paint Co., Ltd.) was spray-applied to a thickness of 25 μm.
[0082] A cross-shaped scratch was then made in the anticorrosive coating to expose part of the steel material. The pass / fail criteria for the corrosion resistance test were as follows: The SAE J2334 test was performed 200 cycles using a test piece with the anticorrosive coating, and a test piece was deemed to have passed if the peeling area in the scratch was 20% or less and the maximum corrosion depth was 0.40 mm or less.
[0083] The results are shown in Table 3. In Table 3, the underlines indicate values outside the range defined by the present invention.
[0084] [Table 3]
[0085] Test Nos. 1 to 15 are examples of the present invention that satisfy all the requirements of the present invention. As can be seen from Table 3, the tensile strength was 350 MPa or more, and in the toughness test, the Charpy absorbed energy at 0°C was 150 J or more. Furthermore, the results of the corrosion resistance test were also good.
[0086] In contrast, the comparative examples, Test Nos. 16 and 17, had poor corrosion resistance because the Sn content in the steel was below the prescribed lower limit, and Test No. 18 had a high Sn content and a high median value in equation (i), resulting in a high MnS area ratio and poor toughness.
[0087] In test No. 19, the S content exceeded the prescribed upper limit and the median value of equation (i) was low, so MnS precipitated excessively in the steel, and the number of grain boundaries where Sn could segregate increased. As a result, Sn segregated on the grain boundaries, the balance of the C / Sn ratio value was lost, and toughness deteriorated. In test No. 20, the product of the Mn content and the Sn content was high, so the median value of equation (i) was high, and the MnS area ratio increased, and Sn segregated, resulting in a low C / Sn ratio value. As a result, toughness was poor.
[0088] In test No. 21, the holding time was long, so the percentage of ferrite with a grain size of 20 μm or less was low. As a result, the tensile strength was poor. In test No. 22, the holding time was short, so Sn segregated, the C / Sn ratio was low, and toughness was deteriorated. In addition, after hot rolling, cooling was started while the temperature in the center of the plate thickness was still high, so the percentage of ferrite with a grain size of 20 μm or less was low. As a result, the tensile strength was poor.
[0089] In test No. 23, the holding temperature was high, and cooling was started while the temperature in the center of the plate thickness was still high, which resulted in a low percentage of ferrite with a grain size of 20 μm or less, and poor tensile strength.In test No. 24, the holding temperature was below the Ar3 point, and coarse ferrite was formed, resulting in poor tensile strength.
[0090] In test No. 25, the average cooling rate was slow and the cooling stop temperature was over 550°C, so pearlite was generated and the total area ratio of ferrite and bainite was low. In addition, the C / Sn ratio was low. As a result, the toughness was poor. In test No. 26, the average cooling rate was fast, so 7% martensite was generated and the total area ratio of ferrite and bainite was low. As a result, the toughness was poor. [Industrial Applicability]
[0091] According to the present invention, it is possible to obtain a steel material having excellent corrosion resistance, toughness, and strength. Therefore, the steel material according to the present invention is suitable for use as a material for large structures such as marine structures and bridges.
Claims
1. The chemical composition of the steel is, in mass%, C: 0.01-0.20%, Si: 0.01-1.00%, Mn: 0.01 to 2.00%, P: 0.010% or less, S: 0.005% or less, Sn: 0.010-0.20%, Al: 0.001-0.040%, N: 0.001-0.005%, O: 0.0001 to 0.010%, The balance is Fe and impurities. The following formula (i) is satisfied: In a cross section perpendicular to the rolling direction of the steel material, when the thickness of the steel material is t, the metal structure in a region from the 1 / 2t position to the 1 / 4t position of the steel material is, in terms of area%, The sum of ferrite and bainite is 90% or more, The area ratio of ferrite having a crystal grain size of 20 μm or less is 50% or more with respect to the total amount of ferrite, In the region from the 1 / 2t position to the 1 / 4t position of the steel material, The area ratio of MnS is 0.020% or less by the point calculation method in JIS G 0555:2015, the ratio of the C content to the Sn content on the grain boundary between the MnS and a crystal grain in contact with the MnS is 0.04 to 6.00; Steel material. 10.0<(Mn / S)×Sn<175.0...(i) In the formula, each element symbol represents the content (mass %) of each element contained in the steel material.
2. The chemical composition is, in mass %, replacing a part of the Fe, Cu: 0.20% or less, Ni: 0.10% or less, W: 0.50% or less, Mo: 0.50% or less, Cr: 0.10% or less, Nb: 0.010% or less, It contains one or more selected from The steel material according to claim 1.
Citation Information
Patent Citations
Structural steel material and structure
WO2019003856A1
Steel material
WO2019116520A1