Operation method of electric furnace
By introducing plastic material near the arc in electric furnaces to generate CO and H2O gases, the method addresses inefficiencies and costs associated with inert gas use, achieving nitrogen absorption suppression and cost savings.
Patent Information
- Application Number
- JP2023062924
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
AI Technical Summary
Conventional methods in electric furnaces that use inert gas to suppress nitrogen absorption are inefficient and costly due to continuous gas discharge, which can displace the forming slag and allow atmospheric nitrogen absorption, increasing heat loss and economic burden.
Introduce plastic material near the arc in the electric furnace at a rate of 0.03 kg/(min·ton of iron input) or more to generate CO and H2O gases that suppress nitrogen absorption by reacting with air, reducing the need for expensive inert gas.
Effectively suppresses nitrogen absorption in molten steel while minimizing inert gas usage, maintaining thermal efficiency and reducing operational costs.
Smart Images

Figure 2024149193000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for operating an electric furnace for producing molten steel by melting iron material with an arc from an electrode. [Background technology]
[0002] In general, in electric furnaces (arc furnaces), slag is foamed by blowing in carbonaceous material and oxygen, and the arc irradiated from the tip of the electrode onto the molten steel bath surface is covered with the foamed slag. This is intended to increase thermal efficiency by absorbing radiant heat generated from the arc into the slag, and to prevent contact between the arc and the atmosphere, thereby suppressing the nitrogen absorption reaction into the molten steel.
[0003] In the following Patent Document 1, focusing on the suppression of the nitrogen absorption reaction, a method is proposed in which an electrode having a gas flow passage therein is used and an inert gas is discharged from the tip of the electrode to suppress the nitrogen absorption reaction in the vicinity of the arc. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 61-276684 Summary of the Invention [Problem to be solved by the invention]
[0005] In the conventional method proposed in the above-mentioned Patent Document 1, the inert gas continues to be discharged even when the foaming slag covers the arc, so there is a risk that the inert gas will blow away the foaming slag near the arc. In that case, not only will heat loss from the arc increase, but nitrogen in the air accompanying the inert gas will be absorbed into the molten steel. In addition, inert gas is expensive, so continuing to discharge a large amount of inert gas as in this conventional method is a large economic burden.
[0006] The present invention has been made to solve the above-mentioned problems, and one of its objects is to provide a method for operating an electric furnace that can suppress nitrogen absorption during operation of the electric furnace while avoiding the use of a large amount of expensive inert gas. [Means for solving the problem]
[0007] In one embodiment, a method for operating an electric furnace according to the present invention is a method for producing molten steel by feeding iron material into a furnace body of the electric furnace and melting the iron material with an arc from an electrode, and includes continuously feeding plastic material from above the furnace body near the arc at a rate of 0.03 kg / (min·ton of iron fed into furnace) or more. Effect of the Invention
[0008] According to one embodiment of the electric furnace operating method of the present invention, plastic material is continuously fed from above the furnace body to the vicinity of the arc at a rate of 0.03 kg / (min / ton of iron fed into furnace) or more, so that the arc is prevented from coming into contact with air by a large amount of gas generated by the thermal decomposition of plastic due to the heat of the arc, and by CO2 and H2O generated by the reaction of the generated gas with the surrounding air. As a result, nitrogen absorption during the operation of the electric furnace can be suppressed while avoiding the use of a large amount of expensive inert gas. [Brief description of the drawings]
[0009] [Figure 1] 1 is an explanatory diagram showing an example of an electric furnace for carrying out a method for operating an electric furnace according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a plan view of the electric furnace of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments of the present invention will be described with reference to the drawings. The present invention is not limited to each embodiment, and the components can be modified without departing from the gist of the present invention. In addition, various inventions can be formed by appropriately combining multiple components disclosed in each embodiment. For example, some components may be deleted from all the components shown in the embodiments. Furthermore, components of different embodiments may be appropriately combined.
[0011] Fig. 1 is an explanatory diagram showing an example of an electric furnace 1 for carrying out a method for operating an electric furnace 1 according to an embodiment of the present invention, and Fig. 2 is a plan view of the electric furnace 1 in Fig. 1. In Fig. 2, illustration of some components such as a furnace lid 13 is omitted. The method for operating an electric furnace 1 according to an embodiment of the present invention can be carried out in the electric furnace 1 shown in Fig. 1. The configuration of this electric furnace 1 is merely an example for the purpose of explanation, and does not limit the configuration of the electric furnace 1 used in the method for operating an electric furnace 1 according to the present embodiment.
[0012] The electric furnace 1 includes a furnace body 10, an electrode 20, an oxygen blowing nozzle 30, a carbonaceous material blowing nozzle 35, an exhaust port 40, and a plastic material input section 50.
[0013] The furnace body 10 includes a furnace bottom 11, a side wall 12, and a furnace cover 13. Shaped and non-shaped furnace body refractories (not shown) are arranged on at least a portion of the furnace bottom 11 and the side wall 12. A portion of the furnace bottom 11 and the side wall 12 may be water-cooled.
[0014] The iron material can be charged into the furnace body 10. The iron material is typically scrap material, but may be other iron materials such as reduced iron obtained by reducing iron ore with carbon or natural gas. One Ch (charge) of iron material may be charged into the furnace body 10 at once, or the iron material may be continuously charged into the furnace body 10. In other words, the electric furnace 1 may be a batch furnace or a continuous charging furnace such as a Consteel type furnace. Auxiliary materials can be further charged into the furnace body 10. The auxiliary materials may include, but are not limited to, CaO, SiO2, and MgO. The auxiliary materials may be charged through a charging port (not shown) provided in the furnace lid 13.
[0015] The electrodes 20 generate an arc between the iron material charged into the furnace bottom 11 and molten steel in which the iron material is melted. Although FIG. 1 illustrates a case in which there are three electrodes 20, the number of electrodes 20 is arbitrary. The electric furnace 1 may be of either an AC type or a DC type. In the electric furnace 1, the iron material is melted by the arc from the electrodes 20 to produce molten steel.
[0016] The oxygen blowing nozzle 30 is for blowing oxygen into the furnace body 10. The carbonaceous material blowing nozzle 35 is for blowing carbonaceous material into the furnace body 10. The carbonaceous material may be blown using an inert gas such as Ar or CO2 as a carrier gas. Each of the oxygen blowing nozzle 30 and the carbonaceous material blowing nozzle 35 may be in contact with the slag S during melting, or may not be in contact with the slag S. In FIG. 1, one oxygen blowing nozzle 30 and one carbonaceous material blowing nozzle 35 are illustrated, but a plurality of oxygen blowing nozzles 30 and a plurality of carbonaceous material blowing nozzles 35 may be provided.
[0017] The exhaust port 40 is for exhausting gas from within the furnace body 10. In Fig. 1, it is shown to be provided in the furnace cover 13, but it may be provided in another position such as the side wall portion 12.
[0018] The plastic material input section 50 is for inputting the plastic material from above the furnace body 10 to the vicinity of the arc. The plastic material may be unused or a dedicated plastic material, but is preferably waste plastic, since waste plastic is relatively inexpensive. The type of plastic material may be mainly polyethylene, polypropylene and / or polystyrene, and its composition may be about 87% carbon and about 11% hydrogen.
[0019] Plastic materials are easily thermally decomposed at temperatures of about several hundred degrees Celsius. If there is high-temperature air in the vicinity, the gas generated by the thermal decomposition easily reacts with oxygen in the air to become harmless CO2 or water vapor (H2O). The inventors of the present invention have considered various methods for suppressing nitrogen absorption by the molten steel M during operation, and have come to the conclusion that if plastic materials are continuously fed near the arc of the electric furnace 1, the large amount of gas generated by the thermal decomposition of the plastic materials due to the heat of the arc, and furthermore, CO2 and H2O generated by the reaction of the generated gas with the surrounding air, can suppress contact between the arc and air, and thus suppress nitrogen absorption by the molten steel M from the contact point (spark) between the arc and the molten steel M.
[0020] The inventors investigated the nitrogen content of molten steel M before tapping while changing various conditions for feeding the plastic material, and found that nitrogen absorption during electric furnace operation can be suppressed by continuously feeding the plastic material at a rate of 0.03 kg / (min·ton of iron fed into furnace) or more. That is, the method of operating an electric furnace 1 according to an embodiment of the present invention includes continuously feeding the plastic material from above the furnace body 10 near the arc at a rate of 0.03 kg / (min·ton of iron fed into furnace) or more.
[0021] Here, "iron input into furnace" refers to the weight (ton) of iron newly input into furnace body 10 in 1Ch. When 1Ch is completed, tapping is terminated leaving some molten steel M in furnace body 10, and new iron material is input in the next Ch by adding it to the molten steel M remaining in furnace body 10. In such an operation method, "iron input into furnace" does not include the iron left in furnace body 10 in the previous Ch, but refers only to the iron newly input in that Ch, and "iron input into furnace ton" refers to its weight. For example, if 30 tons of molten steel M produced in the previous Ch is left in furnace body 10 and 100 tons of new iron material is input in that Ch, "iron input into furnace ton" is 100 tons. In this case, "plastic material input speed 0.03 kg / (min·iron input into furnace ton)" means that 3 kg of plastic material is input per minute.
[0022] The upper limit of the feeding speed of the plastic material is about 1.00 kg / (min·ton of iron fed into the furnace), but as will be shown later as an example, even if it is 0.50 kg / (min·ton of iron fed into the furnace), it was found that the increase in the effect of suppressing nitrogen absorption is limited compared to the case of 0.10 kg / (min·ton of iron fed into the furnace). For this reason, it is preferable that the feeding speed of the waste plastic is 0.50 kg / (min·ton of iron fed into the furnace) or less, and more preferably 0.10 kg / (min·ton of iron fed into the furnace) or less.
[0023] For example, when the electric furnace 1 is viewed in a plane as shown in Figure 2, the inner area of a circle 210 (the area shaded in Figure 2) that is concentric with a circumscribing circle 200 that touches the outer peripheral surfaces of all the electrodes 20 and has a radius 1 m larger than that of the circumscribing circle 200 can be understood to be the vicinity of the arc.
[0024] The plastic material may be charged during the arc application period. That is, the charging of the plastic material may start at the same time as the application of the arc to the furnace body 10, and the charging of the plastic material may end when the application of the arc ends.
[0025] The plastic material may be charged through the plastic material charging section 50 as described above. The plastic material charging section 50 shown in FIG. 1 is a cylindrical member inserted into the furnace body 10 from an opening provided in the furnace lid 13. The plastic material may be charged from the tip of the plastic material charging section 50. The plastic material may be blown in using an inert gas such as Ar or CO2 as a carrier gas, but it is preferable to allow the plastic material to fall naturally from the tip of the plastic material charging section 50. This is because equipment costs can be reduced.
[0026] Furthermore, when the shape of the plastic material was changed in various ways and the nitrogen content of the molten steel M was investigated, it was found that the effect of suppressing nitrogen absorption can be sufficiently ensured when the ratio of plastic material having a particle size of 4.75 mm or more to the entire plastic material is 70% or more. That is, in the method of operating the electric furnace 1 according to the embodiment of the present invention, it is preferable that the ratio of plastic material having a particle size of 4.75 mm or more to the entire plastic material is 70% or more.
[0027] It was also found that by making the ratio of plastic material with a particle size of 4.75 mm or more to the total plastic material 90% or more, the ratio of plastic material scattered by air currents in the furnace can be reduced, and a decrease in the efficiency of the introduced plastic material reaching the vicinity of the arc can be avoided. In other words, it is more preferable that the ratio of plastic material with a particle size of 4.75 mm or more to the total plastic material be 90% or more.
[0028] Incidentally, "total plastic material" may refer to the weight of all plastic material put into 1Ch. Plastic material with a particle size of 4.75mm or more can be selected by sieving the crushed plastic material through a 4.75mm sieve (JIS Z 8801 metal sieve). For example, when the ratio of plastic material with a particle size of 4.75mm or more is set to 90% or more, the plastic material on the sieve can be used at a weight ratio of 90% or more (plastic material under the sieve may be mixed with the plastic material on the sieve within a range of less than 10%).
[0029] There is no particular restriction on the maximum diameter of the plastic material as long as it can be fed into the furnace body 10, but it is preferable to set it to 200 mm or less. By setting the maximum diameter of the plastic material to 200 mm or less, it is possible to avoid the belt conveyor or air current conveying equipment for transporting the plastic material onto the furnace body 10 becoming large.
[0030] The plastic material input section 50 is preferably separated from the exhaust port 40 in the circumferential direction of the furnace body 10. This is to reduce the effect of exhaust on the plastic material input from the plastic material input section 50 and to more reliably input the plastic material near the arc. For example, when the electric furnace 1 is viewed in a plane as shown in FIG. 2, the angle between the first line segment L1 connecting the center C of the circumscribing circle 200 and the position of the plastic material input section 50 and the second line segment L2 connecting the center C of the circumscribing circle 200 and the exhaust port 40 is preferably 90 degrees or more, more preferably 135 degrees or more, and even more preferably 180 degrees. When the plastic material input section 50 is a cylindrical member as shown in FIG. 1, the first line segment L1 may be a line connecting the center C of the circumscribing circle 200 and the position of the tip of the plastic material input section 50. If the plastic material charging section 50 is an opening provided in the furnace lid 13, the first line segment L1 may be a line segment connecting the center C of the circumscribing circle 200 and the position of the opening in the furnace lid 13 corresponding to the plastic material charging section 50. The same applies to the exhaust port 40 and the second line segment L2.
[0031] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention. EXAMPLES
[0032] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0033] The inventors investigated the nitrogen content of molten steel M before tapping while changing the feeding conditions of the plastic material in various ways. First, 100 tons of scrap as an iron material and CaO, SiO2 and MgO as auxiliary materials were fed into the furnace body 10, and while oxygen and carbonaceous powder were blown into the slag S from the side wall 12, the scrap was melted by applying an arc from the electrode 20 installed above the center of the furnace to produce molten steel M. Even after the slag S was generated, oxygen (3000 Nm 3 While blowing in slag S at a flow rate of 1000 rpm (60 kg / hr) and carbonaceous powder (60 kg / min), an arc was applied to the molten steel M from an electrode 20 installed above the center of the furnace, and the molten steel temperature was raised to approximately 1650°C. The molten steel M was sampled at the time of tapping to measure the nitrogen concentration (hereinafter referred to as [%N], mass%). Operation was continued for 5 ch under the same conditions, and the average value of [%N] was calculated. The results are shown in the table below.
[0034] [Table 1]
[0035] [Comparative Example 1] Comparative Example 1 is an example in which no plastic material was added. The amount of slag S generated was about 70 kg / ton of molten steel, and the main components of the slag S were CaO, SiO2, MgO, and FeO. The component ratios of the slag S were CaO / SiO2=2, MgO=11%, and FeO=25%. After the scrap had melted down, i.e., after there was no unmelted scrap on the bath surface of the molten steel M, the operator observed the inside of the furnace and found that the forming height of the slag S near the electrode was unstable, and sometimes the arc was significantly exposed. The average value of [%N] obtained was 0.0103%.
[0036] [Comparative Example 2] In Comparative Example 2, waste plastics (maximum diameter 200 mm or less, with a particle size of 4.75 mm or more being 91% or more) were continuously fed near the arc for 45 minutes while the arc was being applied at a rate of 0.01 kg / (min·ton of iron fed into furnace). The feeding of the waste plastics began at the same time as the arc was applied. The amount of slag S generated was approximately 70 kg / ton of molten steel, and the composition of the slag S was CaO / SiO2=2, MgO=11%, and FeO=23%.
[0037] The average value of [%N] obtained was 0.0101%. When the waste plastic was fed at a rate of 0.01 kg / (min·ton of iron fed into furnace), the amount of gas generated by the thermal decomposition of the waste plastic was small, and contact between the arc and the atmosphere could not be suppressed very much, so it is considered that nitrogen absorption occurred at the same level as in Comparative Example 1, where no waste plastic was fed.
[0038] [Example 1] In Example 1, waste plastics (maximum diameter 200 mm or less, with a particle size of 4.75 mm or more being 92% or more) were continuously fed near the arc for 45 minutes while the arc was being applied at a rate of 0.03 kg / (min·ton of iron fed into furnace). The feeding of the waste plastics began at the same time as the arc was applied. The amount of slag S generated was approximately 70 kg / ton of molten steel, and the composition of the slag S was CaO / SiO2=2, MgO=11%, and FeO=23%.
[0039] The average value of [%N] obtained was 0.0088%. It was confirmed that by setting the waste plastic feeding rate at 0.03 kg / (min·ton of iron fed into furnace) or more, the amount of gas generated by the thermal decomposition of the waste plastic can be sufficiently secured, contact between the arc and the atmosphere can be suppressed, and nitrogen absorption can be suppressed.
[0040] [Example 2] In Example 2, the waste plastics feeding rate was changed to 0.10 kg / (min·ton of iron fed into furnace) from the conditions in Example 1. The amount of slag S generated was about 70 kg / ton of molten steel, and the composition ratio of slag S was CaO / SiO2=2, MgO=11%, and FeO=23%.
[0041] The average value of [%N] obtained was 0.0058%. It was confirmed that the nitrogen absorption suppression effect could be increased by increasing the waste plastic feeding rate to 0.10 kg / (min·ton of iron fed into furnace).
[0042] [Example 3] Example 3 is an example in which the ratio of waste plastics with a particle size of 4.75 mm or more to the total amount of waste plastics was changed to 70% from the conditions of Example 2. The amount of slag S generated was about 70 kg / ton of molten steel, and the composition ratio of slag S was CaO / SiO2=2, MgO=11%, and FeO=23%.
[0043] The average value of [%N] obtained was 0.0070%. In the case of Example 3, the nitrogen absorption suppression effect was sufficiently obtained compared to Comparative Examples 1 and 2, but it was confirmed that a higher nitrogen absorption suppression effect could be obtained when the ratio of waste plastics with a particle size of 4.75 mm or more was 90% or more as in Example 2.
[0044] [Example 4] Example 4 is an example in which the ratio of waste plastics with a particle size of 4.75 mm or more to the total amount of waste plastics was changed to 80% from the conditions of Example 2. The amount of slag S generated was about 70 kg / ton of molten steel, and the composition ratio of slag S was CaO / SiO2=2, MgO=11%, and FeO=23%.
[0045] The average value of [%N] obtained was 0.0065%. In the case of Example 4, the nitrogen absorption suppression effect was sufficient compared to Comparative Examples 1 and 2, but it was confirmed that a higher nitrogen absorption suppression effect could be obtained when the ratio of plastic material with a particle size of 4.75 mm or more was 90% or more, as in Example 2.
[0046] [Example 5] In Example 5, the waste plastics feeding rate was changed to 0.50 kg / (min·ton of iron fed into furnace) from the conditions in Example 2. The amount of slag S generated was about 70 kg / ton of molten steel, and the composition ratio of slag S was CaO / SiO2=2, MgO=11%, and FeO=24%.
[0047] The average value of [%N] obtained was 0.0051%. Comparing Example 2 with Example 5, it was confirmed that even if the waste plastic feeding rate was increased from 0.10 kg / (min·ton of iron fed into furnace) to 0.50 kg / (min·ton of iron fed into furnace), the increase in the effect of suppressing nitrogen absorption was limited (0.0058% → 0.0051%). From this result, it can be inferred that the effect will not change much even if the feeding rate of the waste plastic is increased further. For this reason, it is found that the feeding rate of the waste plastic is preferably 0.50 kg / (min·ton of iron fed into furnace) or less, and more preferably 0.10 kg / (min·ton of iron fed into furnace) or less. [Explanation of symbols]
[0048] 1: Electric furnace 10:Furnace body 20: Electrode M: Molten steel
Claims
1. A method for operating an electric furnace, comprising the steps of: charging an iron material into a furnace body of the electric furnace; and melting the iron material with an arc from an electrode to produce molten steel, comprising the steps of: The plastic material is continuously fed from the furnace body to the vicinity of the arc at a rate of 0.03 kg / (min / ton of iron fed into the furnace) or more. How to operate an electric furnace.
2. The proportion of the plastic material having a particle size of 4.75 mm or more in the entire plastic material is 90% or more; The method for operating an electric furnace according to claim 1.
Citation Information
Patent Citations
Method for judging slag foaming in electric furnace steel-making and operation of electric furnace
JP1998226812A
Manufacture of ferroalloys
JP2008511747A
Arc heating method of molten steel
JP1986276684A